Manufacturing method of electrode-embedded member

By laminating degreased aluminum nitride and tungsten bodies in electrode embedding members, the method addresses cracks and stress issues, ensuring durability and simplifying the manufacturing process for semiconductor equipment components.

JP7575864B2Active Publication Date: 2024-10-30NITERRA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2019077302
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-04-15
Publication Date
2024-10-30
Estimated Expiration
2039-04-15

AI Technical Summary

Technical Problem

Existing methods for manufacturing electrode embedding members with embedded metal electrodes in ceramic bases, such as those used in semiconductor manufacturing equipment, suffer from cracks and residual stress due to differences in thermal expansion coefficients and the application of high pressures during sintering, particularly when using metal-ceramic mixtures without binders, which complicates the process and deforms the electrodes.

Method used

The method involves laminating degreased bodies of aluminum nitride and tungsten, allowing them to shrink uniformly during pressure firing, thereby reducing stress and preventing cracks by using unfired connecting members with intermediate thermal expansion coefficients, and integrating them with ceramic materials without direct contact to avoid compressive forces.

Benefits of technology

This approach effectively suppresses cracks and residual stress, maintains electrode flatness, and simplifies the manufacturing process by eliminating the need for additional degreasing steps, ensuring durability under high-temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575864000001
    Figure 0007575864000001
  • Figure 0007575864000002
    Figure 0007575864000002
  • Figure 0007575864000003
    Figure 0007575864000003
Patent Text Reader

Abstract

To suppress generation of cracks or residual stress inside a material constituting an electrode embedded member and to suppress deformation of an electrode.SOLUTION: A manufacturing method of an electrode embedded member includes laminating a first degreased body 1 made of ceramics prepared by degreasing a ceramic molded body, an electrode 2, an unburned body of a connection member 3 made from ceramic powder and metal powder composed of at least one ceramic component constituting a substrate, and a second degreased body 4 made of ceramics, having a hole 5 in which the unburned body of the connecting member 3 is accommodated, made by degreasing the ceramic molded body, laminated in this order to constitute a laminated body 6, and pressurizing and sintering the laminated body 6 to produce an integrated electrode embedded member.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an electrode-embedded member having an electrode embedded in a ceramic base body. The electrode-embedded member is used, for example, as a ceramic heater or electrostatic chuck incorporated in a semiconductor manufacturing device. [Background technology]

[0002] Conventionally, there is known an electrode-embedded member that is configured by embedding a metal electrode (internal electrode) inside a plate-shaped base made of ceramics such as aluminum nitride (AlN), etc. In this electrode-embedded member, a hole (terminal hole) is formed in the ceramic base by machining, the metal electrode inside the base is exposed in the hole, a cylindrical metal terminal is inserted into the hole, and the tip face of the metal terminal is brazed to the metal electrode inside the base.

[0003] The electrode-embedded member is incorporated into, for example, semiconductor manufacturing equipment (etching equipment, CVD equipment, etc.) and used for electrostatic chucking and heating of semiconductor wafers, and may be repeatedly exposed to high temperatures in the usage environment.

[0004] According to Patent Document 1, when a conventional electrode-embedded member was subjected to a thermal cycle test between room temperature and 600°C, and a long-term holding test at 600°C, cracks were sometimes generated on the inner surface of the base that defines the hole for the metal terminal. As a measure against such crack generation, Patent Document 1 proposes a technology for reducing the stress remaining in the base during the manufacture of the electrode-embedded member, thereby suppressing the generation of cracks in the base.

[0005] Patent Document 2 discloses a conventional method for manufacturing a ceramic member (electrode-embedded member). Figures 9 and 10 are schematic diagrams showing this conventional manufacturing method, which includes the steps of placing a conductor 101 and a connecting conductor 102 made of a pellet of a mixture of tungsten and aluminum nitride powder on an aluminum nitride (AlN) sintered body 100, filling the aluminum nitride raw material powder that will form a base 103 after firing treatment on top of the conductor 101, and sintering the resulting body by hot pressing, and performing machining to form a hole (terminal hole) 104 that exposes the connecting conductor 102, and then connecting an external metal terminal 105 to the exposed part of the connecting conductor 102 by a brazing part 106. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 3776499 [Patent Document 2] Patent No. 4374096 Summary of the Invention [Problem to be solved by the invention]

[0007] However, when a ceramic member (electrode-embedded member) is manufactured by the manufacturing method of Patent Document 2, the aluminum nitride (AlN) sintered body 100 and the aluminum nitride raw material powder (which becomes the base 103 after firing) have different shrinkage rates during hot pressing, which can result in unexpected residual stress acting on the interface (particularly the edge of the connecting conductor 102) between the connecting conductor 102 and the base 103 formed by firing the aluminum nitride raw material powder, causing cracks to occur. These cracks can occur in the base 103 formed by sintering the aluminum nitride raw material powder, the aluminum nitride sintered body 100 prepared prior to the integration process by firing, and / or the connecting conductor 102.

[0008] Therefore, during firing processing using a hot press or the like, it was necessary to reduce the stress concentrated at the edge of the connecting member and suppress cracks by mitigating the difference in shrinkage rate between the connecting member (connecting conductor) and the surrounding ceramic material, such as aluminum nitride (AlN), while also mitigating the change in the difference in linear expansion coefficient (difference in thermal expansion coefficient).

[0009] In particular, when a connection member (connection conductor) is formed from a mixture of a metal material such as tungsten and a ceramic material such as aluminum nitride (AlN), cracks tend to occur more easily in the connection member during pressure firing than when the connection member is formed from only a metal material. This tendency (ease of cracks occurring in the connection member) is particularly noticeable when the connection member compact before pressure firing does not contain a binder. In addition, in consideration of the convenience of the manufacturing process, there is a demand to use a connection member compact without a binder. In other words, depending on the amount of binder contained in the connection member compact, an additional degreasing process in a N2 atmosphere may be required, which causes a problem of complicating the manufacturing process.

[0010] In addition, in the case of the manufacturing method of Patent Document 2, aluminum nitride (AlN) powder is filled on the connection member (connection conductor) and then hot-pressed, so that a relatively large pressure is applied to the connection member during the hot-press process. The pressure applied to the connection member is transmitted to the electrode by the deformation of the connection member, which causes the electrode to deform and deteriorates its flatness.

[0011] In view of the above, an object of the present invention is to provide a method for manufacturing an electrode-embedded member, which can suppress or prevent the occurrence of cracks or residual stress inside the material constituting the electrode-embedded member, or suppress or prevent deformation of the electrode, when manufacturing the electrode-embedded member by embedding an electrode and a connection member electrically connected to the electrode in a ceramic base such as aluminum nitride (AlN). [Means for solving the problem]

[0012] [1] In order to achieve the above object, the present invention provides a method for manufacturing an electrode-embedded member, comprising embedding an electrode and a connection member containing tungsten and aluminum nitride electrically connected to the electrode in an aluminum nitride substrate, the method comprising the steps of: a first degreased body made of aluminum nitride produced by degreasing an aluminum nitride molded body; The electrode; nitrogen Aluminum fluoride powder and tungsten An unsintered body of the connection member made from the powder of a second degreased body made of aluminum nitride, the second degreased body having a hole in which the unsintered body of the connection member is accommodated, the second degreased body being made by degreasing an aluminum nitride molded body; are laminated in order to form a laminate, The laminate is pressurized and sintered to produce an integrated electrode-embedded member.

[0013] According to the manufacturing method of the electrode-embedded member of the present invention having the above-mentioned features, the first degreased body and the second degreased body shrink simultaneously during pressure firing, which makes it possible to suppress or prevent the occurrence of cracks and residual stress caused by the difference in shrinkage rate and the difference in linear expansion coefficient (difference in thermal expansion coefficient) near the bonding interface between the first degreased body and the second degreased body during pressure firing.

[0014] In addition, since the connection member made of the unsintered body is made of ceramic powder made of at least one ceramic component constituting the base of the electrode-embedded member and metal powder, the linear expansion coefficient (thermal expansion coefficient) of the connection member made of the unsintered body is an intermediate value between the linear expansion coefficient (thermal expansion coefficient) of the electrode and the linear expansion coefficient (thermal expansion coefficient) of the ceramic material, and the change in the linear expansion coefficient (thermal expansion coefficient) of the interface between the connection member and the ceramic material is mitigated. This makes it possible to suppress or prevent the occurrence of cracks and residual stress.

[0015] Furthermore, the unsintered body of the connection member is inserted into a hole portion previously formed in the second degreased body. This causes the unsintered body of the connection member to shrink simultaneously with the ceramic material during pressure firing. When a bulk body made of sintered metal, which has been conventionally used as a connection member, is embedded, the stiffness of the bulk body is higher than that of its surroundings during pressure firing, so that compressive stress acts selectively on the bulk body. As a result, this causes cracks (damage) to occur in the connection member. Therefore, by using the unsintered body of the connection member, the sintering of the connection member progresses at the same time as the surrounding ceramic material during firing, while the unsintered body of the connection member is inserted into a hole portion previously formed in the second degreased body, so that the connection member can be prevented from being selectively subjected to strong compressive force, and the connection member can be integrated with the ceramic material while suppressing damage to the connection member itself. As a result, cracks that develop in the connection member and from the connection member to the ceramic material can be suppressed or prevented.

[0016] [2] In order to achieve the above object, the present invention provides a method for manufacturing an electrode-embedded member, comprising embedding an electrode and a connecting member containing tungsten and aluminum nitride electrically connected to the electrode in an aluminum nitride substrate, the method comprising the steps of: a first powder compact forming step of filling an aluminum nitride powder into a bottomed cylindrical mold having an opening and pressing the aluminum nitride powder to form a first powder compact; In the bottomed cylindrical mold, the first powder compact is , Nitrogen Aluminum fluoride powder and tungsten an electrode placement step of placing the green body of the connection member made from the powder and the electrode; a second green compact forming step of filling the aluminum nitride powder into the opening side of the unsintered body of the first green compact, the electrode, and the connection member in the bottomed cylindrical mold, and applying pressure to form a second green compact including the first green compact; and a sintering step of producing an electrode-embedded member by pressurizing and firing the second powder compact in which the unsintered bodies of the electrodes and the connecting members are embedded.

[0017] The manufacturing method of the electrode-embedded member of the present invention having the above-mentioned features can also achieve the above-mentioned unique effects.

[0018] [3] In the method for producing an electrode-embedded member of the present invention, the green body of the connection member is a molded body, a degreased body, or a calcined body. [4] Furthermore, in the manufacturing method of the electrode-embedded member of the present invention, a terminal hole having a diameter smaller than that of the connecting member and exposing only a part of the connecting member is formed on one surface of the electrode-embedded member after pressure sintering. This ensures that the above-mentioned unique effects can be achieved. [Brief description of the drawings]

[0019] [Figure 1A] 1A to 1C are schematic diagrams for explaining one embodiment of a method for producing an electrode-embedded member according to the present invention. [Figure 1B] 1A to 1C are schematic diagrams for explaining one embodiment of a method for producing an electrode-embedded member according to the present invention. [Figure 2A] 4A to 4C are other schematic diagrams for explaining an embodiment of the manufacturing method of an electrode-embedded member according to the present invention. [Figure 2B] 4 is another schematic diagram for explaining an embodiment of the manufacturing method of the electrode-embedded member according to the present invention. FIG. [Figure 3A] 10 is yet another schematic diagram for explaining an embodiment of the manufacturing method of an electrode-embedded member according to the present invention. FIG. [Figure 3B] 10 is yet another schematic diagram for explaining an embodiment of the manufacturing method of an electrode-embedded member according to the present invention. FIG. [Figure 4A] 1A to 1C are schematic diagrams for explaining an embodiment of a method for manufacturing an electrode-embedded member according to the present invention. [Figure 4B] 1A to 1C are schematic diagrams for explaining an embodiment of a method for manufacturing an electrode-embedded member according to the present invention. [Figure 4C] 1A to 1C are schematic diagrams for explaining an embodiment of a method for manufacturing an electrode-embedded member according to the present invention. [Figure 5A] 4A to 4C are other schematic diagrams for explaining an embodiment of the manufacturing method of an electrode-embedded member according to the present invention. [Figure 5B] 4A to 4C are other schematic diagrams for explaining an embodiment of the manufacturing method of an electrode-embedded member according to the present invention. [Figure 5C] 4A to 4C are other schematic diagrams for explaining an embodiment of the manufacturing method of an electrode-embedded member according to the present invention. [Figure 6A] 10A to 10C are still other schematic diagrams for explaining an embodiment of a method for manufacturing an electrode-embedded member according to the present invention. [Figure 6B] 10A to 10C are still other schematic diagrams for explaining an embodiment of a method for manufacturing an electrode-embedded member according to the present invention. [Figure 7A] 10A to 10C are still other schematic diagrams for explaining an embodiment of a method for manufacturing an electrode-embedded member according to the present invention. [Figure 7B] 10A to 10C are still other schematic diagrams for explaining an embodiment of a method for manufacturing an electrode-embedded member according to the present invention. [Figure 8] 10 is still another schematic diagram for explaining an embodiment of a manufacturing method for an electrode-embedded member according to the present invention. FIG. [Figure 9A] 1A to 1C are schematic diagrams for explaining an example of a conventional method for manufacturing an electrode-embedded member. [Figure 9B] 1A to 1C are schematic diagrams for explaining an example of a conventional method for manufacturing an electrode-embedded member. [Figure 10A] 11A and 11B are other schematic diagrams for explaining an example of a conventional method for manufacturing an electrode-embedded member. [Figure 10B] 11A and 11B are other schematic diagrams for explaining an example of a conventional method for manufacturing an electrode-embedded member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, a method for manufacturing an electrode-embedded member according to one embodiment of the present invention will be described with reference to the drawings. Note that the drawings are schematic (conceptual) views of the main parts of the electrode-embedded member, in particular the connection points between the internal electrodes and the external metal terminals.

[0021] In the manufacturing method of the electrode-embedded member according to the present embodiment, first, as shown in FIGS. 1A and 1B, there are prepared a first member 1 made of a first degreased ceramic body produced by degreasing a ceramic molded body, an electrode 2 made of a metal such as molybdenum (Mo) and functioning as a high-frequency electrode, a ground electrode, or an electrostatic attraction electrode, a connecting member 3 made of an unsintered body, and a second member 4 made of a second degreased ceramic body produced by degreasing a ceramic molded body.

[0022] More specifically, a first molded body (a plate that will become an insulating layer after firing) of a predetermined shape is produced by cutting out a CIP body made of a ceramic material such as aluminum nitride (AlN), and this first molded body is degreased to produce the first member 1 made of the first degreased body.

[0023] Similarly, a second molded body (a plate that will become the base after sintering) of a predetermined shape is produced by cutting out a CIP body made of a ceramic material such as aluminum nitride (AlN), and this second molded body is degreased to produce a second member 4 made of the second degreased body.

[0024] Next, the first member (first degreased body) 1 and the second member (second degreased body) 4 are processed to adjust their outer shapes and to form spaces for accommodating the electrodes 2 and the connecting members (green bodies) 3. As shown in Fig. 1A, the second member (second degreased body) 4 has holes 5 formed therein for accommodating the connecting members (green bodies) 3.

[0025] The connection member (unsintered body) 3 is made of a compact, degreased body, or calcined body made of a ceramic powder consisting of at least one ceramic component constituting the base (first member 1 and second member 4) of the electrode-embedded member and a metal powder. For example, a ceramic raw material powder such as aluminum nitride (AlN) and a metal powder such as tungsten (W) are mixed in a predetermined volume ratio, and then the unsintered body (such as a compact) of the connection member 3 is made. When the ceramic raw material powder contains aluminum nitride (AlN), a sintering aid such as yttria (Y2O3) may be added as necessary.

[0026] Next, an electrode 2 is placed on the first member (first degreased body) 1, and a connecting member (unfired body) 3 is placed thereon. Furthermore, a second member (second degreased body) 4 is placed thereon to form a laminate 6 as shown in Fig. 1B. Note that the order of lamination of the laminate 6 may be reversed from the order shown in Fig. 1B.

[0027] As can be seen from Fig. 1B, a gap is formed between the connection member (unsintered body) 3 housed in the hole 5 and the wall surface that defines the hole 5. In other words, the connection member (unsintered body) 3 and the ceramic material that forms the wall surface of the second member (second degreased body) 4 are not in contact with each other but are separated from each other. Note that Fig. 1B shows a state in which the two are entirely separated from each other (a state in which there is no contact), but they may be in partial contact with each other.

[0028] The dimensions of the gap formed around the connection member (unsintered body) 3 are typically 100 μm in the vertical direction of the connection member 3 and 300 μm in the horizontal direction.

[0029] Next, the laminate 6 shown in Fig. 1B is subjected to uniaxial pressure sintering (hot pressing). By pressure sintering the laminate 6 in this manner, the first member (first degreased body) 1, the second member (second degreased body) 4, and the connection member (unsintered body) 3 are sintered, and these members are integrated with the electrode 2 as shown in Fig. 2A. After sintering, the first member 1 and the second member 4 are integrated together to form the base 7 of the electrode-embedded member. The gaps that existed around the connection member 3 before pressure sintering have disappeared after sintering, and the connection member 3 is integrated with the second member 4.

[0030] 2B, one surface (the upper surface in the figure) of the sintered laminate 6 shown in Fig. 2A is machined to form a terminal hole 8. As a result, a part of the connection member 3 is exposed inside the terminal hole 8. Here, it is more desirable that the diameter of the terminal hole 8 is smaller than the representative dimension (e.g., diameter) of the connection member 3.

[0031] Next, as shown in FIG. 3A, the brazing material (brazing portion 9) and the terminal (external connection terminal) 10 are inserted into the terminal hole 8, and as shown in FIG. 3B, the terminal 10 and the connection member 3 are brazed at the brazing portion 9. The brazing portion 9 includes an intermediate member 9a of tungsten (W) and an intermediate member 9b of kovar embedded in the brazing material. As the brazing material, gold brazing material represented by Au-Ni system and silver brazing material represented by Ag-Cu system are suitable. The diameter of the terminal hole 8 is, for example, 5 mm. The terminal 10 is, for example, 4.8 mm in diameter and 20 mm in length. A gap is formed between the terminal 10 and the inner surface of the base 7 that defines the terminal hole 8. The width of the gap is, for example, 0.1 mm. The metal material constituting the terminal 10 is typically nickel, and other low thermal expansion metal alloys such as kovar, and / or titanium, copper, or alloys mainly composed of these.

[0032] In this embodiment, the cylindrical terminal 10 and the disk-shaped connection member 3 are concentrically arranged and connected to each other, but the terminal 10 and the connection member 3 do not necessarily need to be concentrically arranged and may be shifted from the concentric position. The shape of the terminal 10 may be a rod shape other than a cylindrical shape. The brazing portion 9 may be in contact with the material of the base 7 present around it.

[0033] The above-mentioned configuration electrically connects the terminal (external metal terminal) 10 and the electrode 2 embedded inside the base 7. The shape of the connection member 3 is not necessarily limited to a disk shape, and any shape suitable for electrically connecting the electrode 2 and the terminal 10 can be appropriately selected. In addition, the form for ensuring the electrical connection between the electrode 2 and the connection member 3 can be a form in which they are directly contacted with each other, or a form in which they are bonded with a conductive paste, or the like.

[0034] The green body constituting the connection member (unsintered body) 3 can be subjected to CIP molding even if it does not contain a binder. A binder may be added to increase the strength of the green body, in which case degreasing in a N2 atmosphere is further performed depending on the amount of binder. In the case of this embodiment, since the first member 1 and the second member 4 are both degreased bodies before pressure sintering, it is preferable to use a connection member (unsintered body) 3 without a binder for the connection member (unsintered body) 3 to be placed between them.

[0035] In addition, in this embodiment, the manufacturing method of the electrode-embedded member when the electrode 2 is one layer has been described, but when electrodes of multiple layers are embedded, the electrode-embedded member can be manufactured in a similar process using multiple degreased bodies and multiple connecting members accordingly. This will be described later as an example of the present invention.

[0036] According to the manufacturing method of the electrode-embedded member of the present embodiment having the above configuration, the first degreased body (first member 1) and the second degreased body (second member 4) shrink simultaneously during pressure firing (hot press firing). Therefore, during pressure firing, it is possible to suppress or prevent the occurrence of cracks and residual stress caused by the difference in shrinkage rate and the difference in linear expansion coefficient (difference in thermal expansion coefficient) in the vicinity of the bonding interface between the first degreased body and the second degreased body.

[0037] In this embodiment, the connection member 3 made of an unsintered body is made of ceramic powder made of at least one ceramic component constituting the base 7 (first member 1 and second member 4) of the electrode-embedded member, and metal powder. Therefore, the linear expansion coefficient (thermal expansion coefficient) of the unsintered connection member 3 has an intermediate value between the linear expansion coefficient (thermal expansion coefficient) of the electrode 2 and the linear expansion coefficient (thermal expansion coefficient) of the ceramic material (AlN, etc.), and the change in the linear expansion coefficient (thermal expansion coefficient) of the interface between the connection member 3 and the ceramic material is mitigated. This makes it possible to suppress or prevent the occurrence of cracks and residual stress.

[0038] Furthermore, the unsintered body (such as a molded body) of the connection member 3 is inserted into a hole 5 formed in advance in the second member (second degreased body) 4, and a gap exists around the connection member (unsintered body) 3 before pressure firing. Furthermore, the unsintered body of the connection member 3 undergoes sintering and shrinks at the same time as the surrounding degreased body during pressure firing. This makes it possible to prevent the connection member 3 from receiving a strong compressive force due to shrinkage of the ceramic material during pressure firing, and the connection member 3 can be integrated with the ceramic material while suppressing damage to the connection member 3 itself. As a result, it is possible to suppress or prevent cracks inside the connection member 3 and cracks that progress from the connection member 3 to the ceramic material such as aluminum nitride (AlN).

[0039] Furthermore, by forming the connecting member (unsintered body) 3 as a calcined body obtained by calcining a molded body, the strength can be further increased, and damage to the connecting member 3 during the pressure sintering step can be more reliably prevented.

[0040] Next, another embodiment of the method for producing an electrode-embedded member according to the present invention will be described. In the above-described embodiment, the compact pressing method is used, but in this embodiment, a powder hot pressing method is used.

[0041] That is, the manufacturing method of the electrode-embedded member according to the present embodiment includes a first green compact forming step of filling a bottomed cylindrical mold having an opening with ceramic raw material powder and pressing it to form a first green compact (corresponding to the first member 1 in Figs. 1A and 1B). In addition, the method includes an electrode placing step of placing an unfired body of a connection member (corresponding to the connection member 3 in Figs. 1A and 1B) made of ceramic powder consisting of at least one ceramic component constituting a base (corresponding to the base 7 in Figs. 2A and 2B) and a metal powder, and an electrode (corresponding to the electrode 2 in Figs. 1A and 1B) on the opening side of the bottomed cylindrical mold of the first green compact. In addition, the method includes a second green compact forming step of filling a ceramic raw material powder on the opening side of the first green compact, the electrode, and the unfired body of the connection member in the bottomed cylindrical mold and pressing it to form a second green compact including the first green compact. In addition, the method includes a sintering step of pressurizing and firing the second green compact in which the electrode and the unfired body of the connection member are embedded.

[0042] In this embodiment as well, it is possible to obtain the same effects as those of the above-described embodiment (FIGS. 1A to 3B).

[0043] (Example) Various examples of the manufacturing method of the electrode-embedded member of the above embodiment will be described below. The conditions of degreasing, firing, and brazing described in the following examples are based on the conventional manufacturing method of the ceramic sintered body, and include appropriate changes to the conditions.

[0044] [Example 1] First, as Example 1, an example in which an electrode-embedded member was manufactured using a compact pressing method will be described with reference to FIGS. 4A to 8. FIG.

[0045] (1) First, a powder mixture consisting of 95% aluminum nitride powder and 5% yttrium oxide powder was molded using CIP (pressure 1 ton / cm 2 ) to obtain an ingot of a compact, which was then machined and degreased to produce the following compacts. (i) Disc-shaped body (first degreased body) 21 (plate that will become an insulating layer after firing) (FIG. 4A) Diameter 340mm, thickness 5mm (ii) A disk-shaped body (second degreased body) 22 (a plate that becomes an intermediate base after firing) (FIG. 4B) Diameter 340mm, thickness 10mm A recess 24 having a diameter of 300 mm and a depth of 0.1 mm is provided on one surface of the disk-shaped molded body 22, sharing the center of the molded body, for accommodating an electrode. Furthermore, a recess 25 having a diameter of 8.5 mm and a depth of 1.1 mm is provided at a predetermined position where the terminal is to be formed, for accommodating a connecting member. (iii) A disk-shaped body (third degreased body) 23 (a plate that becomes a base after firing) (FIG. 4C) Diameter 340mm, thickness 20mm A recess 26 having a diameter of 300 mm and a depth of 0.1 mm is provided on one surface of the disk-shaped molded body 23, sharing the center of the molded body, for accommodating an electrode. Furthermore, a recess 27 having a diameter of 8.5 mm and a depth of 1.1 mm for accommodating the connecting member molded body is provided at a predetermined position where the terminal is to be formed.

[0046] (2) Preparation of connection member molded body A powder mixture consisting of 95% by mass of tungsten (W) powder, aluminum nitride (AlN) powder, and 5% by mass of yttrium oxide powder was mixed so that the volume ratio of W was 90%, 80%, 70%, and 60%, and this was uniaxially press molded and then CIP molded to produce a connecting member molded body 3 with a dimension of φ8 mm x 0.8 mmt.

[0047] (3) The electrodes and connection member molded bodies were fitted inside the disk-shaped degreased body 23 (FIG. 5A). (iv) Heater electrode Molybdenum wire mesh (wire diameter 0.1 mm, plain weave, mesh size #50) This is cut into a specified shape to make heater electrode 2A. The maximum outer diameter is 294 mm. (v) Arrangement of electrodes, etc. The connection member molded body 3 is placed in a recess 27 having a diameter of 8.5 mm in the disk-shaped degreased body 23 (FIG. 5A). On top of that, the heater electrode 2A is placed in a 300 mm recess (Figure 5B). (vi) Stacking of disk-shaped degreased bodies 22 A disk-shaped degreased body 22 is layered on the side of the disk-shaped degreased body 23 where the heater electrode 2A is embedded (FIG. 5C). (vii) Stacking of disk-shaped degreased bodies 21 (FIGS. 6 and 6B) The above-mentioned connection member molded body 3 is placed in a recess 25 having a diameter of 8.5 mm in the disk-shaped degreased body 22 (FIG. 6A). The high-frequency electrode 2B, which is made of a mesh of molybdenum wire similar to that of the heater electrode and cut to have a maximum outer diameter of 300 mm, is placed in the 300 mm recess 24 above (FIG. 6A). A disk-shaped degreased body 21 is laminated thereon to complete a laminate (degreased body) 28 (FIG. 6B).

[0048] (4) The laminate 26 was placed in a hot press furnace and hot press sintered (FIG. 7A). The hot press firing was carried out at a pressure of 10 MPa, a firing temperature of 1800°C, and a firing time of 2 hours.

[0049] (5) Post-firing processing (Figure 7B) Thereafter, the entire surface was ground and polished to form a wafer-mounting surface with a total thickness of 25 mm, an insulating layer thickness of 1.0 mm, and a surface roughness of Ra 0.4 μm. A flat-bottom hole having a diameter of φ5.5 mm is drilled from the rear surface of the ceramic substrate to the terminal position, reaching the connecting member 3, to form a terminal hole 8.

[0050] (6) External metal terminal connection (Fig. 8) A buffer member (intermediate members 9a, 9b) made of tungsten and Kovar with a diameter of 5 mm and a thickness of 2 mm and a cylindrical Ni power supply terminal 10 with a diameter of 5 mm and a length of 30 mm were placed on the exposed bottom surface of the connection member via a solder material (soldering part 9), and the terminals were soldered in a vacuum furnace at 1050°C using a Au-Ni solder material to complete the electrode-embedded member (Fig. 8).

[0051] [Example 2] Next, as Example 2, an example will be described in which an electrode-embedded member was similarly produced by using a degreased connecting member body prepared by the following process instead of the connecting member molded body laminated in Example 1.

[0052] W powder, aluminum nitride powder 95 mass%, yttrium oxide powder 5 mass%, and PVA 3 mass% were added, and this was uniaxially press molded and then CIP molded to produce a connection member molded body of φ8 mm x 1.1 mmt. The volume ratio of W was mixed to be 60%. This was degreased in an N2 atmosphere at 500°C to produce a degreased connection member.

[0053] [Example 3] Next, as Example 3, an example will be described in which an electrode-embedded member was produced in the same manner as in Example 1, except that a calcined connecting member body produced by the following process was used instead of the connecting member compacts laminated in Example 1.

[0054] A powder mixture consisting of W powder, 95% by mass of aluminum nitride powder, and 5% by mass of yttrium oxide powder was uniaxially press molded and then CIP molded to produce a connection member molded body having a diameter of 8 mm and a thickness of 0.8 mm. The volume ratio of W was mixed to be 60%. This was calcined in an Ar atmosphere at 1500° C. to prepare a calcined body for the connection member.

[0055] [Example 4] Next, as Example 4, an example in which an electrode-embedded member was manufactured by using a powder hot pressing method will be described.

[0056] (1) A powder mixture of 95% by mass of aluminum nitride powder and 5% by mass of yttrium oxide powder is filled into a bottomed carbon mold and uniaxially pressed to produce a first disk-shaped green compact. (i) First circular compact (the plate that will become the insulating layer after firing) Diameter 340mm, thickness 5mm. (ii) The same high-frequency electrode as in Example 1 is placed at a predetermined position on the first circular powder compact. (iii) Connection members The same connecting member molded article as in Example 1 is placed at a predetermined position on the high-frequency electrode.

[0057] (2) The same powder mixture is further filled into a bottomed carbon mold and uniaxially pressed to produce a second disk-shaped green compact. Diameter 340mm, thickness 10mm (iv) A heater electrode is placed on the second disk-shaped compact. (v) Connection members The same connection member molded body as in Example 1 is placed at a predetermined position on the heater electrode.

[0058] (3) The same powder mixture is further packed into a bottomed carbon mold and uniaxially pressed to produce a third disk-shaped green compact. (vi) Third circular compact (the plate that will become the base after firing) Diameter 340mm, thickness 20mm

[0059] (4) Hot press firing The hot press firing was carried out at a pressure of 10 MPa, a firing temperature of 1800°C, and a firing time of 2 hours.

[0060] (5) Post-firing processing Thereafter, the entire surface was ground and polished to form a wafer-mounting surface with a total thickness of 25 mm, an insulating layer thickness of 1.0 mm, and a surface roughness of Ra 0.4 μm. A flat-bottom hole with a diameter of φ5.5 mm is drilled from the back side of the ceramic base to the terminal position until it reaches the connecting member.

[0061] (6) External metal terminal connection A buffer member made of tungsten and Kovar with a diameter of 5 mm and a thickness of 2 mm and a cylindrical Ni power supply terminal with a diameter of 5 mm and a length of 30 mm were installed on the exposed bottom surface of the connecting member via solder, and the electrode-embedded member was completed by brazing using a Au-Ni solder at 1050°C in a vacuum furnace.

[0062] [Comparative Example] In Example 1, an electrode-embedded member was produced by a conventional manufacturing method in which the connecting member was a bulk body (sintered metal) of tungsten (W).

[0063] (evaluation) The electrode-embedded members produced in Examples 1 to 4 and the Comparative Example were used in a semiconductor manufacturing process in which the process temperature was 600°C. Three months after the start of use, the cross section of the terminal was observed using a SEM. As a result, no cracks were observed in any of Examples 1 to 4, but in the comparative example, the progress of cracks from the edge of the connection member toward the surface of the electrode-embedded member was observed. In addition, a 4mm Ni terminal was brazed to the connection member and then a tensile test was performed. After the strength test, all of the connection members were broken inside. As the volume ratio of W increased, the strength tended to decrease slightly, but this was not enough to cause any problems in use. [Explanation of symbols]

[0064] 1 First member (first degreased body) 2, 2A, 2B electrode (internal electrode) 3 Connection parts 4 Second component (second degreased body) 5, 25, 27 holes 6 Laminate 7 Base 8 Terminal Hole 9 Brazed part 10 Terminals 21 Disc-shaped body (first degreased body) 22 Disc-shaped body (second degreased body) 23 Disc-shaped body (third degreased body)

Claims

1. A method for manufacturing an electrode-embedded member, comprising embedding an electrode and a connection member containing tungsten and aluminum nitride electrically connected to the electrode in an aluminum nitride substrate, comprising: a first degreased body made of aluminum nitride produced by degreasing an aluminum nitride molded body; The electrode; an unsintered body of the connection member made of aluminum nitride powder and tungsten powder; a second degreased body made of aluminum nitride and having a hole in which the unsintered body of the connection member is accommodated, the second degreased body being produced by degreasing an aluminum nitride molded body; are laminated in order to form a laminate, The method for producing an electrode-embedded member comprises pressurizing and sintering the laminate to produce an integrated electrode-embedded member.

2. A method for manufacturing an electrode-embedded member, comprising embedding an electrode and a connection member containing tungsten and aluminum nitride electrically connected to the electrode in an aluminum nitride substrate, comprising: a first powder compact forming step of filling an aluminum nitride powder into a bottomed cylindrical mold having an opening and pressing the aluminum nitride powder to form a first powder compact; an electrode placement step of placing the green body of the connection member made of aluminum nitride powder and tungsten powder and the electrode on an opening side of the bottomed cylindrical mold of the first powder compact in the bottomed cylindrical mold; a second green compact forming step of filling the aluminum nitride powder into the opening side of the unsintered body of the first green compact, the electrode, and the connection member in the bottomed cylindrical mold, and applying pressure to form a second green compact including the first green compact; a sintering step of pressurizing and firing the second powder compact in which the unsintered bodies of the electrodes and the connecting members are embedded; A method for manufacturing an electrode-embedded member comprising the steps of:

3. The method for producing an electrode-embedded member according to claim 1 or 2, wherein the green body of the connection member is a compact, a degreased body, or a calcined body.

4. 2. The method for manufacturing an electrode-embedded member according to claim 1, characterized in that a terminal hole having a diameter smaller than that of the connection member and exposing only a portion of the connection member is formed by machining on one surface of the laminate after pressure sintering.

Citation Information

Patent Citations

  • Wafer holder for semiconductor manufacturing apparatus and semiconductor manufacturing apparatus carrying the same

    JP2004288887A

  • Manufacturing method for ceramic heater

    JP2004362933A

  • Heating apparatus

    JP2008130609A

  • Bonding structure, and manufacturing method thereof

    JP2009060103A

  • Bonding structure and semiconductor production apparatus using the same

    JP2015002300A