High gamma prime nickel-base superalloys, their uses and methods for making turbine engine components - Patents.com
A new high gamma-prime nickel-based superalloy with optimized compositions and heat treatments addresses the durability issues of existing superalloys, offering crack-free welds and improved mechanical properties for turbine engine components.
Patent Information
- Application Number
- JP2019225403
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-01
- Filing Date
- 2019-12-13
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2039-12-13
AI Technical Summary
Turbine engine components made from existing high gamma-prime nickel-based superalloys suffer from cracks due to creep, thermomechanical fatigue, oxidation, and hot corrosion, limiting their durability and requiring costly weld repairs with materials like cobalt-based alloys that have poor weldability and creep properties at high temperatures.
Development of a new high gamma-prime nickel-based superalloy with optimized compositions of elements such as chromium, cobalt, molybdenum, tungsten, tantalum, niobium, aluminum, hafnium, and rhenium, combined with specific heat treatment processes, to enhance weldability, strength, and oxidation resistance, suitable for fusion welding, casting, and 3D additive manufacturing.
The new superalloy provides crack-free welds with excellent oxidation resistance, strength, and ductility, enabling effective repair and manufacturing of turbine engine components without premature failure, even at high temperatures.
Smart Images

Figure 0007575871000009 
Figure 0007575871000010 
Figure 0007575871000011
Abstract
Description
[Technical field]
[0001] The high gamma prime (γ') nickel-base superalloy of the present invention can be used for the production of turbine engine components and other articles by casting and hot forming, as well as laser beam (LBW), plasma (PAW), microplasma (MPW), gas tungsten arc welding (GTAW), electron beam (EBW) welding, and 3D additive manufacturing processes. [Background technology]
[0002] Most turbine blades in aircraft and industrial turbine engines are manufactured from nickel-base high gamma-prime (γ') superalloys, which have a unique combination of oxidation and creep properties. However, despite the outstanding properties of high γ' superalloys, engine components often require various weld repairs due to creep and thermo-mechanical fatigue cracking, oxidation, and high temperature corrosion damage that occurs during turbine engine operation. Dissimilar cobalt-based Merl 72 (M72), nickel-based Rene 142 (R142), and Rene 80 (R80) welding consumables have been used since the 1980s to repair high pressure turbine (HPT) and low pressure turbine (LPT) blades, see A. Gontcharov et al, GT2018-75862, “Advanced Welding Materials and Technologies for Repair of Turbine Engine Components manufactured of High Gamma Prime Nickel Based Superalloys”, Proceedings of ASME Turbo Expo 2018: Turbine Technical Conference and Exposition, GT2018, June 11-15, 2018, Oslo, Norway (further GT2018-75862).
[0003] Cobalt-based M72 has excellent weldability, ductility, and oxidation resistance, but as shown in GT2018-75862 and Example 1, oLow creep properties at temperatures above 2000°F (968.33°C) have resulted in premature HPT blade failures and unplanned engine withdrawals. Poor creep properties are typical of most cobalt-base alloys and nickel-base superalloys with high cobalt content. On the other hand, high gamma-prime nickel-base R142 welding wire, containing 6.8 wt% Cr-12 wt% Co-1.5 wt% Mo-4.9 wt% W-6.4 wt% Ta-6.1 wt% Hf-1.5 wt% Re, has been reported by Earl W. Ross and Kevin S. O'Hara ("Rene 142: High Strength, Oxidation Resistance DS Turbine Airfoil Alloy", Superalloys 1992, pp. 257 - 263). 265) and based on a high gamma prime nickel-base superalloy containing 10-13 wt.% Co, 3-10 wt.% Cr, 0.5-2 wt.% Mo, 3-7 wt.% W, 0.5-10 wt.% Re, 5-6 wt.% Al, 5-7 wt.% Ta, 0.5-2 wt.% Hf, 0.01-0.15 wt.% C, 0.005-0.05 wt.% B, 0-0.1 wt.% Zr, and balance nickel as per U.S. Pat. No. 4,169,742, which has excellent creep properties but extremely poor weldability.Limited weld repairs of turbine engine components using R142 have been performed by preheating the engine components to high temperatures, as shown by Dikran A. Barhanko et al., “Development of Blade Tip Repair for SGT-700 Turbine Blade Stage 1, With Oxidation Resistant Weld Alloy”, Proceedings of ASME Turbo Expo 2018, Turbomachinery Technical Conference and Exposition, GT2018, June 11-15, 2018, Oslo, Norway, and by Alexandre Gontcharov et al. in the previously cited paper GT2018-75862. However, even with preheat, R142 welds have poor ductility and are prone to microcracking, precluding the use of R142 in 3D additive manufacturing.
[0004] Nickel-base superalloy R80, with a chemistry as per U.S. Pat. No. 3,615,376, containing Ni-15%Cr-9.5%Co-5%Ti-4%W-4%Mo-3%Al-0.17%C, has better weldability but poorer oxidation resistance and cannot replace R142 and M72.
[0005] Nickel-base superalloys disclosed in Chinese Patent No. 105492639, Canadian Patent No. 28004402, U.S. Patent No. 4,288,247, U.S. Patent No. 7,014,723, U.S. Patent No. 8,992,669, and U.S. Patent No. 8,992,700, which have increased Co contents up to 20-30%, also have poor weldability at 1800°C, despite potentially better weldability. o Due to its inadequate mechanical properties above 2000°F (968.33°C), it cannot replace high gamma prime R142 superalloy. Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, there is a substantial need to develop new high gamma prime nickel-base superalloys with excellent oxidation resistance, strength, and ductility that can produce crack-free welds on single crystal (SX) materials at room temperature for the repair and 3D additive manufacturing of turbine engine components. [Means for solving the problem]
[0007] The inventors have determined that, in weight percent, Cr is 9.0 to 10.5%, Co is 16 to 22%, Mo is 1.0 to 1.4%, W is 5.0 to 5.8%, Ta is 2.0 to 6.0%, Nb is 1.0 to 4.0%, Al is 3.0 to 6.5%, Hf is 0.2 to 1.5%, C is 0.01 to 0.2%, Ge is 0 to 1.0%, and the total content of Ta and Nb is in the range of 3.0 to 7.0%, and the total content of Nb is in the range of 3.0 to 7.0%, respectively. We have found that a high gamma prime nickel-base superalloy containing up to 100% Si, 0 to 0.2 wt. % Y, 0 to 0.015 wt. % B, 1.5 to 3.5 wt. % Re, and the balance nickel and impurities, has excellent room temperature weldability, a good combination of mechanical and oxidation properties, and can be used for a variety of repairs of turbine engine components by fusion welding, and for the manufacture of turbine engine components by 3D additive manufacturing, casting, and hot forming.
[0008] Another preferred embodiment of the high gamma prime nickel-base superalloy comprises germanium and silicon in a combined amount ranging from 0.9 to 1.1 weight percent.
[0009] Preferred embodiments of the superalloys according to the present invention are selected from among welding wires, welding powders, equiaxed or directionally solidified turbine engine components, restored turbine engine components, and articles manufactured by hot forming.
[0010] Another embodiment of the present invention is a method of manufacturing a turbine engine component that includes using the high gamma prime nickel-base superalloy of the present invention.
[0011] As used herein, "manufacturing a turbine engine component" refers to producing it from raw materials and / or restoring an old turbine engine component so that it can be used as new.
[0012] Turbine engine components and other articles manufactured from the superalloys of this invention having the preferred chemistry are subjected to a heat treatment that differs from the heat treatment of R142 superalloy and is similar to that of 2190 o F (approximately 1198.89°C) to 2290 o Annealing for 1-2 hours at temperatures ranging from 1254.44°C to 1975°F o F (approximately 1079.44°C) to 2050 o Primary aging for 2 to 4 hours at temperatures ranging from 1300°F (approximately 1121.11°C), and o F (approximately 704.44°C) to 1500 o The aim of the study is to maximize the mechanical properties of the developed superalloy by aging treatments that involve secondary aging for 16 to 24 hours at temperatures ranging from 0.25 to 1.25°F (approximately 815.56°C), which results in the precipitation of γ'.
[0013] In a preferred embodiment of the present invention, the turbine engine component is manufactured by casting at a temperature of 2200 to 2290° C. prior to annealing. o The method includes the further step of hot isostatically pressing the ingot at a temperature of about 1204.44°F (about 1204.44°C to 1254.44°C) and a pressure of 15 to 20 KSI (about 103.45 to 137.93 MPa) for 2 to 6 hours.
[0014] According to another preferred embodiment, the manufacture of a turbine engine component includes a o F (approximately 1198.89°C) to 2290 o Annealing the ingot for 1-2 hours to 1500°F (approximately 1254.44°C) was then performed. oF (approximately 815.56°C) to 1800 o Hot forming with 5-80% plastic deformation using a temperature range of up to 1975-2050 F (approximately 968.33°C) and o Primary aging of turbine engine components at 1079.44 to 1121.11°C for 2 to 4 hours and 1300 to 1500°C o The method includes at least two subsequent steps, with a final heat treatment including a secondary aging treatment at 500°F (approximately 704.44°C to 815.56°C) for 16 to 24 hours.
[0015] In order to avoid recrystallization of turbine engine components manufactured by hot forming, the service temperatures of these turbine engine components are selected to be below the temperature of the primary ageing treatment.
[0016] According to another preferred embodiment, a method for manufacturing a turbine engine component comprises a fusion welding step, preferably selected from among laser beam, plasma arc, microplasma, and electron beam, and gas tungsten arc welding, by melting and solidifying depositing in a molten pool a powder mixture comprising at least two dissimilar powders, nickel-based and cobalt-based, in amounts of (70-80) wt.% and (20-30) wt.%, respectively, wherein the nickel-based powder comprises, in wt.%, - 6 to 8% chromium, - 6 to 12% cobalt, - 1.3 to 1.6% molybdenum, - 4.5 to 5% tungsten, - 2.0 to 6.0% tantalum, - from 1.0 to 4.0% niobium, - Tantalum and Niobium combined from 3.0 to 7.0% - 3.0 to 6.5% aluminum, - 0.2 to 1.5% hafnium, - 2.5 to 3% rhenium, - germanium from 0 to 1.0%; - 0 to 1% silicon, - 0 to 0.2% yttrium, - 0 to 0.015% boron, - 0.01 to 0.1% carbon and - the balance being nickel and impurities; and The cobalt-based powder comprises, by weight percent: - 10 to 18% nickel, - 19 to 21% chromium, - 8 to 10% tungsten, - 3 to 6.5% aluminium, - germanium from 0 to 1.0%; - from 0 to 1% silicon, - from 0 to 0.45% yttrium, - Hafnium from 0 to 1.5% - from 0 to 4% niobium, - 0.01 to 0.2% carbon and - balance cobalt and impurities; the steps of fusion welding, which includes a step of gradually moving and solidifying the molten pool according to a preprogrammed welding path, thereby forming a weld bead having the same chemical composition as the superalloy of the present invention; a step of post-weld heat treatment selected from high isostatic pressing, annealing, aging treatment, or a combination of annealing and aging treatment; and the steps of working to the required shape and non-destructive testing.
[0017] To implement the above preferred embodiment, the powder mixture is selected from a pre-alloyed powder blend containing different nickel-based and cobalt-based powders, or from nickel-based and cobalt-based powders that are mixed directly in the molten pool during welding. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a microstructure photograph of an annealed and aged cast superalloy according to the present invention, showing: a) the formation of zigzag grain boundaries during solidification; b) the precipitation of cubic γ' phase during the aging heat treatment. [Diagram 2] FIG. 2 is a microstructural photograph of the extruded bar in the aged condition, showing: a) the formation of equiaxed grains with straight grain boundaries during extrusion and primary recrystallization; b) the precipitation of the γ′ phase during the aging heat treatment. [Diagram 3] FIG. 3 is a micrograph of an LBW weld produced at room temperature showing: a) the formation of microcracks in Rene 142 weld produced using GTAW welding with a preheat of 1700-1800°F; b) a defect-free multi-layer weld overlay produced at room temperature using LBW with a welding powder made from the superalloy of the present invention. [Figure 4] Figure 4 is a micrograph of a defect-free multi-layer weld overlay produced using LBW at room temperature on a PWA1484 SX substrate (base metal) showing: a) crack-free fusion of the weld metal with the base metal in the as-welded condition; b) precipitation of γ' phase in the weld metal after the PWHT aging heat treatment. [Diagram 5] FIG. 5 shows the fracture surface of a tensile specimen produced from the weld metal and EDS mapping (distribution) of some alloying elements showing the interdendritic precipitation of fine cubic Ta-Hf based intermetallic particles: a) SEM image of ductile fracture of the weld metal tensile specimen; b) Tantalum distribution; c) Hafnium distribution. [Figure 6] FIG. 6 is a fractographic tensile test specimen produced from a germanium-free embodiment of a superalloy according to the present invention, showing: a) a fractograph showing a ductile dimple failure of the tensile test specimen and a cube-shaped Ta-Hf based intermetallic grain at the base of the dimple; b) a fractograph of the same fracture surface as in a) but at higher magnification showing representative grains selected and marked for EDS (spectrums 1 and 2); c) chemical analysis of the grain marked spectrum 1 and the chemical composition of the selected grain including 46.5% Ta-37.3% Hf-9.5% Ni-4.1% Co-1.8% Cr. [Figure 7]FIG. 7 is a microstructure photograph of a weld produced using a superalloy according to the present invention on a Rene 80 substrate, showing: a) dendrites formed in the weld in the "as-welded" condition; b) microstructure of the weld metal and base material adjacent the fusion line after annealing and aging PWHT as per the preferred embodiment. [Figure 8] FIG. 8 is a photograph of the fracture surface of a weld metal test specimen subjected to bending testing at room temperature, showing ductile fracture of the specimen. [Figure 9] FIG. 9 is a fractograph of a welded specimen made from an embodiment of a superalloy according to the present invention containing 0.85 wt.% germanium and tensile tested at 1800°F showing: a) the change in morphology of the Ta-Hf based intermetallic particles; b) the same fracture surface as in a) but at higher magnification with the typical Ta-Hf particle selected for EDS; c) the mapping of Ta and Hf on the surface of the particle marked map data 19 in FIG. 9a, showing that this particle is significantly enriched in Ta and Hf. [Figure 10] FIG. 10 is a micrograph of an LBW weld produced using a powder blend containing dissimilar nickel- and cobalt-based powders, showing: a) the formation of dendrites during solidification of the molten pool; b) the dissolution of dendrites during homogenization annealing followed by aging treatment as per the preferred embodiment. [Figure 11] FIG. 11 is a cross-sectional photograph of a welded specimen produced from 4285 material described in Example 6 using LBW and 3D additive manufacturing concepts, showing: a) manual butt gas tungsten arc weld of the test specimen produced by LBW; b) epitaxial growth of dendrites in multi-pass LBW welds and typical thickness of deposit of 795 μm per pass for LBW welds; c) precipitation of cubic gamma prime and double gamma prime phases during post-weld heat treatment of GTAW welded joints.
[0019] Standard Acronyms and Key Definitions ASTM – American Society for Testing and Materials HPT - High Pressure Turbine LPT – Low Pressure Turbine NDT – Non-Destructive Testing NGV - Nozzle Guide Vane PWHT - Post Weld Heat Treatment UTS - Maximum tensile strength SRT - Stress Rupture Test LBW - Laser Beam Welding MPW – Micro Plasma Welding GTAW – Gas Tungsten Arc Welding EBW - Electron Beam Welding PAW - Plasma Arc Welding SX - Single Crystal Materials BM - base material 3D AM – Three-dimensional Additive Manufacturing SEM - Scanning Electron Microscope EDS - Energy Dispersive X-ray Spectroscopy IPM - inches per minute FPI - Fluorescent Penetrant Inspection
[0020] Nickel-base superalloys - metallic materials used in the manufacture of turbine engine components and other articles that exhibit excellent mechanical strength and resistance to creep (the property of a solid material to move or deform slowly under stress) at high temperatures up to 0.9 times its melting temperature; good surface stability; and oxidation and corrosion resistance. Precipitation-strengthened superalloys have a matrix of an austenitic face-centered cubic crystal lattice with precipitation of the gamma prime phase, typically nickel-base-aluminum or titanium-aluminum. Superalloys are most often used in the manufacture of turbine engine components.
[0021] Hot forming - Hot forming, also known as hot working, is the process of shaping metals under pressure at sufficiently elevated temperatures that the material has sufficient ductility.
[0022] High Gamma Prime Nickel-Base Superalloy - A nickel-base superalloy containing from 3% to 12% by weight of either aluminum or titanium, or the total alloying elements aluminum and titanium.
[0023] Laser beam (electron beam, gas tungsten arc, and plasma arc) welding - a welding process that uses heat obtained from impinging a concentrated coherent light beam (electron beam, or electric arc, respectively) on a seam or base material with or without a weld material to produce a coalescence of materials. Weldability - The ability of a material to be welded under imposed conditions into a specific suitable structure and to perform satisfactorily for its intended use. Structural Turbine Engine Components – The various housings, frames, nozzle guide vane rings, and other stator parts that enable the engine to perform under operating conditions. Base Material - The material of the engine components and test specimens. Energy Dispersive X-ray Spectroscopy (EDS) - is an analytical technique used for elemental analysis or chemical characterization of samples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The material of the present invention belongs to the precipitation strengthened high gamma prime superalloys and contains a large amount of aluminum, a well-known gamma prime former.
[0025] The unique combination of strength, ductility, oxidation resistance, and weldability is due to the precipitation of large volumes of high strength intermetallic gamma prime (γ')Ni3Al phase, double gamma prime (γ'')Ni3Nb phase, and Ta-Hf-W-Si cubic intermetallic particles, as shown in Figures 1b, 9, 10, and 11, in an austenitic ductile γ phase matrix that is a solid solution of Co, Cr, Mo, W, and Re in nickel with optimized ratios of all alloying elements. The volume fraction of γ' and γ'' phases in the superalloy of the present invention was found to exceed 50 volume % in the aged condition.
[0026] Ingots for evaluating the mechanical properties of the superalloys of the present invention were produced by triple arc re-melt in argon, followed by annealing and aging heat treatments as per the preferred embodiment.
[0027] The welding wire is heated to a temperature of 1600~1800 o The alloy was produced by multi-step extrusion of an ingot at 1000 K (approximately 871.11 to 982.22 °C) followed by pickling to remove surface oxides.
[0028] Welding powder with a diameter of 45 μm was produced by gas atomizing the ingots in argon.
[0029] In order to maximize the mechanical properties of the precipitation-hardened superalloy of the present invention, o F (approximately 1198.89°C) to 2290 o Homogenization annealing at temperatures ranging from 1254.44°C to 1975°F for 1 to 2 hours, followed by o F (approximately 1079.44°C) to 2050 o Primary aging for 2 to 4 hours at temperatures ranging from 1300°F (approximately 1121.11°C), o F (approximately 704.44°C) to 1500 oA special heat treatment was developed that involves a secondary aging treatment for 16 to 24 hours at temperatures ranging from 1000 to 2000°F (approximately 815.56°C). This heat treatment differs from the heat treatments frequently used for the heat treatment of R142 superalloys (see W. Ross and Kevin S. O'Hara, "Rene 142: High Strength, Oxidation Resistance DS Turbine Airfoil Alloy", Superalloys 1992, pp. 257 - 265).
[0030] The parameters for PWHT heat treatment of turbine engine components are application dependent. The optimal heat treatment parameters for HPT, LPT, NGV, and other non-rotating turbine engine components produced by casting and 3D additive manufacturing methods are 2250-2290 o Annealing for 2 hours at a temperature range of 1232.22 to 1254.44 °C (approximately 1232.22 to 1254.44 °C), followed by annealing at 1100 to 1120 o F (approximately 593.33 to 604.44°C) for 2 hours, and then 1480 to 1500 o The study found that the secondary aging treatment included a 24-hour treatment at a temperature of 204.44°F (approximately 804.44°C to 815.56°C).
[0031] The PWHT parameters for the heat treatment of HPT and LPT turbine blades made from single crystal superalloys and / or repaired by welding using the welding wire or welding powder according to the present invention are set forth in the 1975 Annex 1 and 1976 Annex 2 parameters for the primary and secondary aging treatments, respectively, in order to avoid recrystallization of the base material. o F (approximately 1079.44°C) since 1995 o F (approximately 1090.56°C) for 4 hours and 1300 o F (approximately 704.44°C) to 1325 o The heat treatment of turbine engine components manufactured by hot forming from the superalloys of the present invention also includes only primary and secondary aging treatments using the parameters disclosed above to prevent recrystallization of the base material.
[0032] The service temperatures of turbine engine components manufactured by hot forming from the superalloys of the present invention were selected to be below the primary aging temperature in order to eliminate recrystallization and degradation of the mechanical properties of the base material under service conditions.
[0033] Annealing of the ingot prior to extrusion or after the production of the turbine engine component by casting as in the preferred embodiment results in homogenization, while aging plays a vital role in the development of superior strength due to the precipitation of the γ′ phase. Further examples are provided to explain the preferred embodiments in more detail. EXAMPLES
[0034] Example 1 To demonstrate the unique combination of high strength and ductility of the developed superalloys, samples made from Rene (R142) and Marl 72 (M72), the superalloys of the present invention using the preferred embodiment (samples marked 4275A, 4275B, 4275C, and 4275D), and a superalloy having a chemistry deviating from the preferred embodiment (sample marked 427X) shown in Table 1 were subjected to triple arc remelt in argon followed by 2215-2230 sintering. o Homogenization annealing at 2035-2050°F (approximately 1212.78-1221.11°C) for 2 hours, o First aging at 1155 to 1170°F (approximately 1112.78 to 1121.11°C) for 2 hours, and then o F (approximately 623.89-632.22℃) for 24 hours.
[0035] Test specimens of 0.255 to 0.275 inches in diameter were machined from the ingots and subjected to radiographic testing as per ASTM E192-04. Linear defects and holes greater than 0.002 inches in size were not permitted. Smaller test specimens of 0.176 to 0.180 inches in gauge diameter and 1.8 inches in length were machined as per ASTM E-8. Tensile tests were performed at temperatures up to 1800°C.o The test was performed as per ASTM E-21 at a temperature of 250°F (968.33°C).
[0036] [Table 1]
[0037] Solidification of the ingot resulted in the formation of zigzag grain boundaries shown in Figure 1a, which enhances the mechanical properties of the developed superalloy. Post-weld (PWHT) aging heat treatment resulted in the precipitation of a high volume of γ' phase shown in Figure 1b.
[0038] The precipitation of a large volume of high strength γ' phase in a ductile austenitic matrix results in a desirable combination of high strength and ductility, as shown in Table 2. The ductility of the superalloy of the present invention is superior to that of the standard R142 specimen, while the strength is superior to that of M72.
[0039] [Table 2]
[0040] Example 2 Low gamma prime wrought AMS 5664 Inconel 718 (IN718) and AMS 5704 Waspaloy superalloys are 1200 o Due to its high strength at temperatures up to 1800°F (648.89°C) and good workability, it has been used to manufacture structural turbine engine components. o Upon further heating to 2000°F (approximately 968.33°C), the strength and stress rupture properties (SRT) of these superalloys decrease dramatically, as shown in Table 3.
[0041] Developed high gamma prime superalloy 1800 oDue to the favorable combination of strength and workability at temperatures up to 1950° F., the developed high gamma prime superalloys have been found to be most suitable to replace standard wrought superalloys for the manufacture of structural turbine engine components utilizing hot forming processes. To evaluate the mechanical properties of the superalloys of the present invention in the wrought (hot formed) condition, ingots were extruded as per the preferred embodiment to produce 0.225 inch diameter bars which were further extruded in the 1950° F. o Primary aging at 1300°F (approximately 1065.56°C) for 4 hours and o The specimens were subjected to a secondary aging treatment at 24°C (approximately 704.44°F) for 24 hours.
[0042] Standard undersized test specimens measuring 1.8 inches in length with gauge diameters of 0.158 to 0.162 inches were fabricated as per ASTM E-8. Tensile tests were performed at 70 o F (approximately 21.11°C) as per ASTM E-8, and 1200 o F (approximately 648.89°C) and 1800 o F (approximately 968.33°C) as per ASTM E-21. Stress rupture tests were performed at 1200 o F (about 648.89℃), 1350 o F (approximately 732.22°C), and 1800 o The experiment was carried out at a temperature of 100°F (968.33°C).
[0043] Extrusion of the superalloy of the present invention at elevated temperatures resulted in the formation of equiaxed grains with straight grain boundaries as shown in Figure 2a, which differed from the zigzag grain boundaries formed during solidification of the ingot as shown in Figure 1a. A primary aging heat treatment resulted in the precipitation of the γ' phase as shown in Figure 2b.
[0044] As found by the experiment, the UTS and SRT properties of the developed superalloy are oF (approximately 968.33°C), outperformed the UTS and SRT of Inconel 718 and Waspaloy, as shown in Tables 3 and 4, respectively.
[0045] [Table 3]
[0046] [Table 4]
[0047] The combination of high strength, ductility, and workability of the superalloys of the present invention makes them outstanding for the manufacture of turbine engine components by hot forming.
[0048] Example 3 Test specimens were generated to simulate the repair of turbine engine components manufactured from single crystal materials using manual GTAW and automated LBW welding, using the developed superalloy in the form of welding wire and welding powder, respectively, and standard Rene 142 welding wire at 1700-1800. o It is made by preheating it to 200°F (approximately 926.67 to 968.33°C) for GTAW and at room temperature for LBW.
[0049] The Rene 142 welding wire used for GTAW was preheated to produce specimens for tensile and SRT tests because welding at room temperature resulted in extensive cracking in the Rene 142 weld, as shown in Figure 3a.
[0050] Multi pass LBW with welding powder made from the superalloy of the present invention and GTAW with welding wire made from the superalloy of the present invention were carried out at room temperature to produce welded specimens marked LBW4275 and GTAW4275. The welds were crack free. Typical microstructures of these specimens are shown in Figures 3b and 4a.
[0051] Post-weld heat treatment of the welds is required at 2200 to eliminate recrystallization of HPT blades manufactured from PWA1484 SX material. o F (approximately 1204.44°C) for 2 hours, followed by homogenization annealing at 1975-1995 o First aging at 1079.44 to 1090.56°C for 4 hours, and then 1300 to 1320°C. o F (approximately 704.44–715.56 °C) for 16 h, which resulted in the precipitation of the γ′ phase shown in Fig. 4b with a volume fraction of 49.2 vol.%.
[0052] Flat substandard "all weld metal" specimens 0.050 inches thick were produced per ASTM E-8 and 1800 mm thick per ASTM E-21. o F (approximately 968.33°C) for tensile testing, and 1800 o The specimen was subjected to SRT at 22 KSI (approximately 151.72 MPa) and 20 F (approximately 968.33°C).
[0053] [Table 5]
[0054] As can be seen from Table 5 below, the ductility and SRT properties of the LBW and GTAW welds produced from the superalloys of the present invention were superior to the properties of the welds made from the standard material, Rene 142.
[0055] The poor tensile and SRT properties of the Rene 142 welds were attributed to the formation of microcracks shown in Figure 3a.
[0056] The high tensile and creep properties as well as the good ductility and weldability of the developed superalloy were attributed to the precipitation of a high volume of high strength cubic γ' phase in the gamma matrix, a ductile Ni-Cr-Co-Re-W-Mo solid solution, and the interdendritic precipitation of fine cubic Ta-Hf based intermetallic particles, as shown in Figures 5 and 6.
[0057] Example 4 Germanium has not been used in the manufacture of Ni-base superalloys, even though nickel-base brazing materials containing Ni-(5-40) wt.% Cr-(15-40) wt.% Ge were invented in 1954, as per US Patent No. 2,901,374. Although germanium is a melting point depressant that should affect strength at high temperatures, we have found that the addition of up to 0.85 wt.% germanium to the superalloy of the present invention, marked 4275C in Table 1, improved weldability, producing defect-free welds on Rene 80, as shown in Figure 7.
[0058] The test specimens were manually welded at a welding current of 75-80A, a voltage of 9-10V, and a welding speed of 1-1.2 ipm (inches per minute). After welding, the specimens were 2190 o Annealing at 1198.89°C for 2 hours, 1975 o First aging at 1079.44°C for 2 hours, followed by 1550°F o The specimens were subjected to heat treatment including a secondary aging treatment at 1800°F (about 843.33°C) for 16 hours. Tensile specimens for testing were fabricated from the base material and the welds as per ASTM E-8 and subjected to tensile tests at 1800°F (about 843.33°C) for 16 hours. o The specimens were subjected to tensile testing at 200°F (approximately 968.33°C).
[0059] The weld metal was also subjected to half-form bend testing as per ASTM E-190 at room temperature.
[0060] In addition to the above, cylindrical samples made from Rene 80 and the superalloy of the present invention were subjected to 2050 o The alloys were subjected to cyclic oxidation tests at 2050°F (about 1121.11°C) for 500 hours. The duration of each cycle was 2050°F (about 1121.11°C). o F (approximately 1121.11°C), for 50 minutes, followed by 10 minutes of exposure to approximately 700 o F (approximately 371.11°C) and 2050 o The time taken to heat the oven was 1 hour, including reheating to 250°F.
[0061] As found by experiment, the strength and oxidation resistance of the welded joints and weld metal were superior to that of the Rene 80 base material, as shown in Tables 6A and 6B.
[0062] [Table 6A]
[0063] [Table 6B]
[0064] The bend test specimens produced from the weld metal fractured at approximately 90° and showed the ductility characteristic of the superalloy of the present invention shown in FIG. 8, which has not been reported for any welds produced on known high γ′ superalloys. As found by experiment, germanium enhances the bonding between the Ta-Hf intermetallic particles and changes the morphology of these particles, as shown in FIGS. 6a and 9a, respectively. EDS analysis confirmed that the particles were produced by Ta-Hf based intermetallic compounds, see FIGS. 9b and 9c. This effect was not known because, in contrast to Si, which belongs to the same IVA group of chemical elements, germanium in the specified range does not result in the formation of interparticle and interdendritic Ni-Ge based eutectic that affects the mechanical properties of Si-bearing nickel-based superalloys.
[0065] Therefore, the combination of high gamma prime content and grain and dendritic boundary reinforcement by fine Ta-Hf based intermetallic particles with coherent bonding to the ductile Ni-Cr-Co-Re-Mo-W based matrix shown in Figure 9a results in superior mechanical properties of the Ge-bearing embodiment of the superalloy of the present invention, and furthermore, the uniqueness of the solidification of the molten pool produced by melting dissimilar nickel and cobalt based powders together in the molten pool prior to solidification produces weld properties superior to those produced using homogeneous welding powder and wire. The oxidation resistance was enhanced by optimizing the Cr, Al, and Si contents in combination with Ge and all other alloying elements in the superalloy of the present invention.
[0066] Based on the test results, it was found that the welding wire and powder made from the superalloy of the present invention are most outstanding for HPT and LPT blade tip restoration, ensuring optimal play between the blade tips and the stator of the turbine engine, low fuel consumption, and high efficiency throughout the entire engine cycle between overhauls.
[0067] Example 5 To demonstrate the 3D additive manufacturing process for producing turbine engine components, samples measuring 4 inches in length, 1 inch in height, and 0.125 inches in thickness were produced using a LAWS1000 laser welding system equipped with a 1 kW IPG laser and two powder feeders that can not only perform welding using pre-alloyed powder blends, but also mix two types of powders, nickel-based and cobalt-based, directly in the molten pool.
[0068] The following examples demonstrate welding with a pre-alloyed powder blend containing 75 wt.% nickel-based powder and 25 wt.% cobalt-based powder. The nickel-based powder contains 6.8 wt.% Cr, 12 wt.% Co, 1.5 wt.% Mo, 4.9 wt.% W, 6.3 wt.% Ta, 6.1 wt.% Al, 1.2 wt.% Hf, 2.8 wt.% Re, 0.1 wt.% Si, 0.12 wt.% C, 0.015 wt.% B, 0.1 wt.% Si, and balance Ni. The cobalt-based powder contains 17 wt.% Ni, 20 wt.% Cr, 3 wt.% Ta, 9 wt.% W, 4.4 wt.% Al, 0.45 wt.% Y, 0.1 wt.% Si, and balance Co.
[0069] The welding parameters used to generate the samples are provided below: - Laser beam power - 480W (watts) - Coagulation deposition rate - 3.8g / min (grams per minute) - Welding speed - 3.5 ipm (inches per minute) (approximately 8.89 cm / min) - Beam speed across the weld line - 40 imp (approximately 101.6 cm / min) - Inert gas - Argon
[0070] During solidification deposition of the multi-pass weld, the molten pool was moved gradually along a preprogrammed path at a speed of 3.5 ipm (8.89 cm / min), resulting in the formation of a weld bead upon solidification having the same preferred chemical composition as the superalloy of the present invention. The chemical composition of the weld metal sample marked 4275E is provided in Table 1.
[0071] After the welding test, the specimens were o First aging at 1155 to 1170°F (approximately 1112.78 to 1121.11°C) for 2 hours, and then oThe welds were subjected to a secondary aging treatment at 623.89°F for 24 hours, fabricated into the required shapes, and then subjected to non-destructive testing including FPI per AMS 2647 and radiographic examination per ASTM E192-04. Weld discontinuities exceeding 0.002 inches in size were not permitted.
[0072] Smaller than standard test specimens were prepared from welds as per ASTM E-8 and 1775 as per ASTM E-21. o The specimens were subjected to tensile testing at 200°F (approximately 968.33°C).
[0073] The weld resulted in the formation of dendrites with epitaxial grain growth, as shown in Figure 10a. The weld was free of cracks and other weld discontinuities.
[0074] The post-weld homogenization and aging heat treatment resulted in the precipitation of a large volume of gamma phase, as shown in Fig. 10b.
[0075] [Table 7]
[0076] From Table 7, as shown below, the welded sample had a bulk Al content of 5.7 wt% in the weld metal, but the 1775 o It exhibits excellent strength and good ductility at temperatures up to 968.33°C (approximately 1000°F).
[0077] The superior weldability, strength, and ductility of the 5.7 weight percent aluminum containing superalloy of the present invention are achieved through the peculiarities of solidification of the molten pool produced by the dissimilar nickel-base and cobalt-base powders.
[0078] Known nickel-base superalloys containing 5.7 wt. % Al are not cold weldable, whereas LBW welding using dissimilar powder mixtures and / or powder blends produces a weld having a bulk chemistry corresponding to that of the superalloy of the present invention due to solidification of the molten pool, producing a robust weld with high mechanical properties.
[0079] Example 6 To simulate the repair of a turbine engine component manufactured from Rene N5 single crystal (SX) material, LBW welds were made at room temperature onto the SX substrate using a powder blend of 78-80% Ni-based powder 'A' and 20-22% Co-based powder 'B' containing: Powder A: Ni-8%Cr-8%Co-1.5%Mo-4.5%W-3.5%Ta-6%Al-0.75%Hf-0.15%Si-3.5%Re-1.2%Nb-0.012%B-0.1%C Powder B: Co-18%Cr-15%Ni-10%W-0.05%Hf-3.5%Al-0.15%Si-0.1%C
[0080] Dissimilar powders, Ni-based Powder A and Co-based Powder B, were melted by a laser beam in a molten pool to produce a homogeneous alloy. Upon solidification of the molten pool, a weld bead was formed with the following bulk chemical composition (4285 material): 4285 Material: Ni-10%Cr-16%Co-1.2%Mo-5.6%W-2.8%Ta-1%Nb-5.5%Al-0.5%Hf-0.15%Si-0.01%B-0.1%C-2.2%Re
[0081] After welding, the test specimens manufactured by LBW using the 3D additive manufacturing concept were subjected to a primary aging treatment at 1975°F (about 1079.44°C) for 4 hours, followed by a secondary aging treatment at 1650°F (about 898.89°C) for 4 hours.
[0082] After welding and heat treatment, the samples were subjected to metallographic and radiographic examination.
[0083] Smaller than standard tensile specimens were machined from the weld samples and tensile tested at room temperature, demonstrating the high ductility of the developed material, as per ASTM E-8 alloy. Tensile properties of all weld metal specimens of 4285 material are as follows: ·UTS=187.2KSI ·0.2% yield strength=173.4SKI Elongation = 11.2%
[0084] Additional testing was done to evaluate the weldability of the 4285 material.
[0085] As found by experiment, the GTAW weld produced using manual welding at room temperature on the 4285 material produced by automatic LBW had no weld discontinuity, as shown in Fig. 11a.
[0086] As a result of multi-pass LBW welding, dendrites and epitaxial grain growth were formed, as shown in Fig. 11b.
[0087] As a result of post-weld heat treatment, fine γ' Ni3Al, double gamma prime γ'' Ni3Nb and intermetallic Ta-Hf-W-Si strengthening phases are formed and precipitated in the ductile austenite matrix of the GTAW weld metal, as shown in Fig. 11c, which enhances the ductility, weldability and high strength of the invented superalloy.
[0088] GTAW butt welded joint shown in Figure 11a demonstrated high strength at 1400°F: ·UTS=142.1KSI ·0.2% proof stress=132.9KSI Elongation = 5.2%
[0089] The good weldability, high ductility and enhanced strength of 4285 material were attributed to the optimized total content of Ta and Nb in the invented superalloy ranging from 3 to 7 wt%.
[0090] Example 7 To simulate the repair of a turbine engine component manufactured from Rene N5 SX material, LBW welds were made at room temperature on the SX substrate using a powder blend of 70-72% Ni-based powder 'C' and 28-30% Co-based powder 'D' containing: Powder C: Ni-6%Cr-6%Co-1.7%Mo-5.6%W-3.4%Ta-4%Nb-6.2%Al-0.3%Hf-0.5%Si-3%Re-0.02%B-0.1%C Powder D: Co-21%Cr-5.6%W-4%Nb-6.2%Al-0.3%Hf-0.5%Si-0.1%C
[0091] Upon solidification of the molten pool, a weld bead was formed having the following bulk chemical composition of 4287 material: 4287 Material Composition: Ni-10%Cr-18%Co-1.2%Mo-5.6%W-2%Ta-4%Nb-6.2%Al-0.3%Hf-0.5%Si-0.015%B-0.1%C-2.2%Re
[0092] Post-weld heat treatment of the welds includes a primary aging treatment at 1975°F (approximately 1079.44°C) for four hours, followed by a secondary aging treatment at 1650°F (approximately 898.89°C) for four hours.
[0093] After welding and heat treatment, the specimens were subjected to metallographic and radiographic examination and were free of cracks and other weld discontinuities.
[0094] Standard undersized tensile specimens were machined from the weld samples per ASTM E-8 alloy and tensile tested at 1800°F per ASTM E-21. Tensile properties of all weld metal specimens of 4287 material are provided below: ·UTS=63.6KSI ·0.2% yield strength=49.3SKI Elongation = 14.5%
[0095] While the present invention has been described in terms of preferred embodiments, it is apparent that other forms of the invention could be adopted by those skilled in the art. Accordingly, the scope of the present invention is intended to be limited only by the scope of the claims which follow. The present invention can be embodied in the following manner. (Appendix 1) By weight: - 9.0 to 10.5% chromium, - about 16 to 22% cobalt, - from 1.0 to 1.4% molybdenum, - 5.0 to 5.8% tungsten, - tantalum from 2.0 to 6.0%; - 1.0 to 4.0% niobium, - Tantalum and Niobium combined from 3.0 to 7.0% - 3.0 to 6.5% aluminium, - from 0.2 to 1.5% hafnium, - Germanium from 0 to 1.0% - yttrium from 0 to 0.2%; - from 0 to 1.0% silicon, - from 0 to 0.015% boron, - 0.01 to 0.2% carbon, - 1.5 to 3.5% rhenium, and - a high gamma prime nickel-base superalloy containing the balance nickel and impurities. (Appendix 2) 2. The high gamma prime nickel-base superalloy of claim 1, wherein the total germanium and silicon content is in the range of 0.9 to 1.1 weight percent. (Appendix 3) 13. Use of the high gamma prime nickel-base superalloy of any one of claims 1 or 2 as a welding wire, a welding powder, or a material for a turbine engine component. (Appendix 4) 13. A method of manufacturing a turbine engine component comprising using the high gamma prime nickel-base superalloy of any one of claims 1 or 2. (Appendix 5) a) Casting, b) 2190~2290 o Annealing at 1198.89 to 1254.44°C for 1 to 2 hours. c) 1500~1800 o Hot forming by plastic deformation at F (approximately 815.56 to 982.22 °C), d) 1975~2050 o F (approximately 1079.44 to 1121.11°C) for 2 to 4 hours, and e) 1300~1500 o and a secondary aging treatment at about 704.44°C to 815.56°C for 16 to 24 hours. (Appendix 6) 2190 o F (approximately 1198.89°C) to 2290 o Annealing for 1-2 hours at temperatures ranging from 1254.44°C to 1975°F o F (approximately 1079.44°C) to 2050 o Primary aging for 2 to 4 hours at temperatures ranging from 1300°F (approximately 1121.11°C), and o F (approximately 704.44°C) to 1500 o 6. A method for manufacturing the turbine engine component of claim 5, comprising a heat treatment selected from the group consisting of a secondary aging treatment at a temperature range of up to about 815° C. (about 815.56° C.) for 16 to 24 hours. (Appendix 7) 1500~1800 o Prior to the step of hot forming at a temperature of 2200 to 2290° F. o 6. A method for manufacturing a turbine engine component as described in claim 5, comprising the further step of hot isostatic pressing at a temperature of about 1204.44° C. to 1254.44° C. and a pressure of 15 to 20 KSI for 2 to 6 hours. (Appendix 8) 6. A method of manufacturing the turbine engine component of claim 5, comprising hot forming with a plastic deformation of 5-80%. (Appendix 9) 6. The method of manufacturing a turbine engine component as described in claim 5, wherein the primary aging temperature is selected above a service temperature of the turbine engine component. (Appendix 10) 5. A method for manufacturing the turbine engine component according to claim 4, comprising the steps of: a) forming a first portion of a first sintered body by a second sintering agent; a) a fusion welding step in which a powder mixture containing at least two different powders, the following nickel-based powder and cobalt-based powder, in amounts of (70-80) wt% and (20-30) wt%, respectively, is melted in a molten pool and solidified and deposited: The nickel-based powder comprises, in weight percent: - 6 to 8% chromium, - 6 to 12% cobalt, - 1.3 to 1.6% molybdenum, - 4.5 to 5% tungsten, - 2.0 to 6.0% tantalum, - from 1.0 to 4.0% niobium, - Tantalum and Niobium combined from 3.0 to 7.0% - 3.0 to 6.5% aluminum, - 0.2 to 1.5% hafnium, - 2.5 to 3% rhenium, - germanium from 0 to 1.0%; - from 0 to 1% silicon, - 0 to 0.2% yttrium, - 0 to 0.015% boron, - 0.01 to 0.1% carbon, and - the balance being nickel and impurities; and The cobalt-based powder comprises, in weight percent: - from 10 to 18% nickel, - 19 to 21% chromium, - 8 to 10% tungsten, - 3 to 6.5% aluminium, - germanium from 0 to 1.0%; - from 0 to 1% silicon, - from 0 to 0.45% yttrium, - Hafnium from 0 to 1.5% - from 0 to 4% niobium, - 0.01 to 0.2% carbon, and - balance includes cobalt and impurities; b) gradually moving and solidifying the molten pool according to a preprogrammed weld path to form a weld bead having the same chemical composition as the high gamma prime nickel-base superalloy described in Appendix 1. (Appendix 11) 11. The method of manufacturing a turbine engine component as described in claim 10, wherein the fusion welding is selected from the group consisting of laser beam, plasma arc, microplasma, electron beam, and gas tungsten arc welding. (Appendix 12) 11. The method of manufacturing the turbine engine component of claim 10, further comprising a post-weld heat treatment selected from the group consisting of the high isostatic pressing, annealing, aging, or a combination of the annealing and aging. (Appendix 13) 13. The method of manufacturing the turbine engine component of claim 12, further comprising the step of machining to a required shape after a post-weld heat treatment. (Appendix 14) 14. A method of manufacturing a turbine engine component as described in claim 13, further comprising the step of non-destructive testing. (Appendix 15) 11. The method of manufacturing a turbine engine component as described in claim 10, wherein the powder mixture is in the form of a pre-alloyed powder blend including nickel-base powder and cobalt-base powder, or in the form of heterogeneous powders of nickel-base powder and cobalt-base powder that are mixed directly in the molten pool during welding. (Appendix 16) 16. A method for manufacturing a turbine engine component according to any one of claims 4 to 15, wherein the turbine engine component is manufactured by 3D additive manufacturing. (Appendix 17) A turbine engine component obtainable by the method according to any one of claims 4 to 16.
Claims
1. In % by weight: - from 9.0 to 10.5% chromium, - from 16 to 22% cobalt, - from 1.0 to 1.4% molybdenum, - 5.0 to 5.8% tungsten, - tantalum from 2.0 to 6.0%; from 0 to 4.0% niobium, - Tantalum and Niobium combined from 2.0 to 7.0%; - from 3.0 to 6.5% aluminium, - from 0.2 to 1.5% hafnium, - germanium from 0 to 1.0%; - from 0 to 0.2% yttrium, from 0 to 1.0% silicon, - from 0 to 0.015% boron, - from 0.01 to 0.2% carbon, - from 1.5 to 3.5% rhenium, and - a high gamma prime nickel-base superalloy, the balance being nickel and impurities.
2. The high gamma prime nickel-base superalloy of claim 1, wherein the total germanium and silicon content is in the range of 0.9 to 1.1 weight percent.
3. 3. Use of the high gamma prime nickel-base superalloy of claim 1 or 2 as a welding wire, a welding powder, or a material for a turbine engine component.
4. A method of manufacturing a turbine engine component comprising the step of using the high gamma prime nickel-base superalloy of claim 1 or 2.
5. For the high gamma prime nickel-base superalloy of any one of claims 1 or 2, b) 2190-2290 o F (about 1198.89-1254.44°C) for 1-2 hours; d) 1975-2050 o F (approximately 1079.44 to 1121.11 °C) for 2 to 4 hours; and e) 1300-1500 o 5. The method of claim 4, further comprising the step of performing a secondary aging treatment at about 704.44-815.56°C for 16-24 hours.
6. For the high gamma prime nickel-base superalloy of any one of claims 1 or 2, a) Casting, and c) 1500-1800 o 6. The method of claim 5, further comprising performing one or more steps selected from: hot forming by plastic deformation at about 815.56-982.22°C.
7. 1500-1800 o and (c) hot forming the mixture at a temperature of 2200 to 2290° F. (about 815.56 to 982.22° C.), and prior to said step (c), o 7. The method of claim 6, further comprising the step of hot isostatic pressing at a temperature of 1204.44-1254.44° C. and a pressure of 15-20 KSI for 2-6 hours.
8. 1500-1800 o 7. The method of claim 6, further comprising said step c) of hot forming at a temperature of about 815.56-982.22°C, said hot forming causing a plastic deformation of 5-80%.
9. The method of manufacturing a turbine engine component according to claim 5 , wherein the primary aging temperature is selected above a service temperature of the turbine engine component.
10. 5. A method for manufacturing a turbine engine component according to claim 4, comprising the steps of: a) forming a first portion of said first and second dies; a) a fusion welding step in which a powder mixture containing at least two different powders, the following nickel-based powder and cobalt-based powder, in amounts of (70-80) wt % and (20-30) wt %, respectively, is melted in a molten pool and solidified and deposited: The nickel-based powder comprises, in weight percent: - 6 to 8% chromium, - from 6 to 12% cobalt, - from 1.3 to 1.6% molybdenum, - 4.5 to 5% tungsten, - from 2.0 to 6.0% tantalum, from 1.0 to 4.0% niobium, - Tantalum and Niobium combined from 3.0 to 7.0%; - from 3.0 to 6.5% aluminium, - from 0.2 to 1.5% hafnium, - 2.5 to 3% rhenium, - from 0 to 1.0% germanium, from 0 to 1% silicon, - from 0 to 0.2% yttrium, from 0 to 0.015% boron, - 0.01 to 0.1% carbon, and the balance consisting of nickel and impurities, and The cobalt-based powder comprises, in weight percent: - from 10 to 18% nickel, - 19 to 21% chromium, - 8 to 10% tungsten, - from 3 to 6.5% aluminium, - from 0 to 1.0% germanium, from 0 to 1% silicon, from 0 to 0.45% yttrium, from 0 to 1.5% hafnium, - from 0 to 4% niobium, - 0.01 to 0.2% carbon, and - the balance consisting of cobalt and impurities; b) gradually moving and solidifying the molten pool according to a preprogrammed welding path to form a weld bead having the same chemical composition as the high gamma prime nickel-base superalloy of any one of claims 1 or 2.
11. The method of manufacturing a turbine engine component according to claim 10 , wherein said fusion welding is selected from the group consisting of laser beam, plasma arc, microplasma, electron beam, and gas tungsten arc welding.
12. The method of manufacturing a turbine engine component according to claim 10 , further comprising a post-weld heat treatment selected from high isostatic pressing, annealing, aging, or a combination of annealing and aging.
13. The method of manufacturing a turbine engine component according to claim 12 , further comprising the step of machining to a required shape after post weld heat treatment.
14. The method of manufacturing a turbine engine component according to claim 13 , further comprising the step of non-destructive testing.
15. 11. The method of manufacturing a turbine engine component according to claim 10, wherein the powder mixture is in the form of a pre-alloyed powder blend including nickel-base powder and cobalt-base powder, or in the form of heterogeneous powders of nickel-base powder and cobalt-base powder mixed directly in the molten pool during welding.
16. A method for manufacturing a turbine engine component according to any one of claims 4, 5 and 9-15, wherein said turbine engine component is manufactured by 3D additive manufacturing.
Citation Information
Patent Citations
Powder alloy and production technique thereof
CN104561662A
Cast product of nickellbased alloy
JP1978076122A
Production of preform for forging nickel base superalloy
JP1997310162A
Ni-BASED SUPERALLOY FOR UNIDIRECTIONAL SOLIDIFICATION HAVING SUPERIOR STRENGTHS IN SOLIDIFICATION DIRECTION AND OF GRAIN BOUNDARY, CASTING, AND HOT PARTS FOR GAS TURBINE