Radioactive iodine adsorbent, method for producing radioactive iodine adsorbent, and method for treating radioactive iodine
The development of a silver-supported high-silica zeolite adsorbent with altered hydroxyl nests addresses the challenge of removing iodine and iodate ions from nuclear waste under acidic conditions, ensuring high adsorption capacity and durability, thus preventing clogging and embrittlement.
Patent Information
- Application Number
- JP2021069835
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-16
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-04-16
AI Technical Summary
Conventional methods fail to effectively remove both iodine ions and iodate ions from nuclear waste under acidic conditions without causing brittleness or clogging issues, and existing iodine ion adsorbents lose adsorption capacity when a reducing agent is present.
A radioactive iodine adsorbent is developed by supporting silver on high-silica zeolites with altered hydroxyl nests to Si-O-Si bonds, specifically using chabasite, mordenite, or clinoptilolite zeolites, with a SiO2/Al2O3 molar ratio of 2 to 100 and 1-15% silver by mass, heat-treated at 500°C to 700°C, to maintain adsorption capacity and durability under acidic conditions.
The adsorbent maintains high iodine ion adsorption capacity and resistance to embrittlement, preventing clogging in acidic solutions with reducing agents, enabling efficient simultaneous removal of iodine and iodate ions from nuclear waste.
Smart Images

Figure 0007575990000005 
Figure 0007575990000006 
Figure 0007575990000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a radioactive iodine adsorbent suitable for use under acidic conditions, and more specifically to a radioactive iodine adsorbent suitable for adsorbing and removing radioactive iodine from waste liquid discharged from a nuclear facility that has been converted into an acidic solution by adding a reducing agent to the waste liquid, a method for producing the radioactive iodine adsorbent, and a method for treating radioactive iodine. [Background technology]
[0002] Wastewater generated at nuclear power plants and other nuclear facilities (hereafter referred to as nuclear facilities) contains various radioactive materials, which must be removed prior to discharge. Of these radioactive materials, radioactive iodine is essential to be completely removed, since one of its isotopes, iodine-129, has a long half-life of approximately 15.7 million years and tends to selectively accumulate in the thyroid gland and other organs of the human body.
[0003] The two main chemical species of radioactive iodine contained in the wastewater discharged from nuclear facilities are iodine ion (I-) and iodate ion (IO3-). Known adsorbents for iodine ions (hereinafter referred to as iodine ion adsorbents) include silver-impregnated activated carbon, which is activated carbon impregnated with silver, and silver zeolite, which is A-type zeolite or X-type zeolite impregnated with silver. However, none of these can remove iodate ions present in wastewater. On the other hand, cerium oxide is known as an adsorbent for iodate ions (hereinafter referred to as iodate ion adsorbent). However, cerium oxide has a small adsorption capacity and cannot remove iodine ions present in wastewater.
[0004] A method for removing iodine ions and iodate ions together has been proposed (Patent Document 1), in which a reducing agent is added to an aqueous solution containing iodine ions and iodate ions to reduce the iodate ions to iodine ions, and silver nitrate is further added to precipitate silver iodide (Patent Document 1). However, the method of Patent Document 1 generates sludge containing radioactive materials as a precipitate, which poses a problem in terms of waste disposal. When silver-impregnated activated carbon or silver zeolite obtained by impregnating A-type or X-type zeolite with silver, which have been conventionally used as an iodine ion adsorbent, are used instead of the silver nitrate, the generation of sludge containing radioactive substances can be avoided. However, problems arise such as a decrease in the ability of the iodine ion adsorbent to adsorb iodine ions in the presence of the reducing agent, and the iodine ion adsorbent becoming easily embrittled under acidic conditions in the presence of the reducing agent, which makes it more likely to cause clogging when a liquid is passed through an adsorption tower such as a column.
[0005] Patent Document 2 discloses an iodine ion adsorbent obtained by subjecting silver zeolite particles, in which silver is supported on zeolite, to a reduction treatment using a reducing agent, and teaches that this iodine ion adsorbent makes it possible to avoid leaching of silver due to re-exchange of these ions with silver ions, even when polyvalent cationic atoms or cationic atoms having a larger atomic number than silver ions are present in an aqueous solution containing an adsorbed substance. Even when the iodine ion adsorbent described in Patent Document 2 is used instead of the silver nitrate, the iodine ion adsorbent tends to become embrittled under acidic conditions in the presence of the reducing agent, and problems such as clogging easily occur when passing a liquid through an adsorption tower such as a column occur.
[0006] For the reasons described above, in the past, in order to remove radioactive iodine contained in wastewater discharged from nuclear facilities, it was not possible to adopt a method in which iodate ions are reduced to iodine ions using a reducing agent and then the iodine ions are removed together, and it was necessary to use both an iodide ion adsorbent and an iodate ion adsorbent. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 05-126995 [Patent Document 2] JP 2016-107213 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in view of the above technical background, and an object of the present invention is to provide a radioactive iodine adsorbent suitable for applications in which iodate ions are reduced to iodine ions by adding a reducing agent to a solution containing radioactive iodine, and the iodine ions are removed collectively, the radioactive iodine adsorbent having high adsorption capacity without decreasing its ability to adsorb iodine ions even under acidic conditions in which a reducing agent coexists in the solution, and which is resistant to embrittlement, a method for producing the radioactive iodine adsorbent, and a method for treating radioactive iodine. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention provides the following means. <Radioactive iodine adsorbent> [1] A radioactive iodine adsorbent comprising a high-silica zeolite in which hydroxyl nests present inside the high-silica zeolite have been converted to Si-O-Si bonds, and silver is supported on the high-silica zeolite, the high-silica zeolite being at least one selected from the group consisting of chabazite (CHA)-type zeolite, mordenite (MOR)-type zeolite, and clinoptilolite (CLP)-type zeolite. [2] The radioactive iodine adsorbent according to [2], wherein the high-silica zeolite has a SiO2 / Al2O3 molar ratio of 2 to 100. [3] The radioactive iodine adsorbent according to [3] or [2], wherein the amount of the supported silver is 1 to 15 mass %. <Manufacturing method of radioactive iodine adsorbent> [4] A method for producing a radioactive iodine adsorbent, comprising supporting silver on a high-silica zeolite in which hydroxyl nests present inside the high-silica zeolite have been converted to Si-O-Si bonds, wherein the high-silica zeolite is at least one selected from the group consisting of chabazite (CHA)-type zeolite, mordenite (MOR)-type zeolite, and clinoptilolite (CLP)-type zeolite. [5] The method for producing a radioactive iodine adsorbent according to [4], wherein the hydroxyl nest is converted to the Si-O-Si bond by heat treatment at 500°C to 700°C. [6] The method for producing a radioactive iodine adsorbent according to [4] or [5], wherein the high-silica zeolite has a SiO2 / Al2O3 molar ratio of 2 to 100. [7] The method for producing a radioactive iodine adsorbent according to any one of [4] to [6], wherein the amount of the supported silver is 1 to 15 mass %. <How to dispose of radioactive iodine> [8] A method for treating radioactive iodine, comprising the steps of: adding a reducing agent to waste liquid discharged from a nuclear facility to prepare an acidic solution; and passing the acidic solution through the radioactive iodine adsorbent according to any one of claims 1 to 3. Effect of the Invention
[0010] According to the present invention, there is provided a radioactive iodine adsorbent suitable for applications in which iodate ions are reduced to iodine ions by adding a reducing agent to an aqueous solution containing radioactive iodine, and the iodine ions are removed collectively, the radioactive iodine adsorbent having high adsorption capacity without decreasing its ability to adsorb iodine ions even under acidic conditions in which a reducing agent coexists in a solution containing iodine ions, which are the adsorbed substance, and which is resistant to embrittlement, a method for producing the radioactive iodine adsorbent, and a method for treating radioactive iodine. [Brief description of the drawings]
[0011] [Figure 1] 13 is a photograph showing the vulnerability assessment results of sample 3. [Diagram 2]1 is a graph showing the results of evaluation of iodine adsorption characteristics using Samples 4, 5, 9, and 11. [Diagram 3] 1 is a graph showing the results of evaluation of iodine adsorption characteristics using Samples 11 and 19. [Figure 4] 1 is a graph showing the results of differential pressure evaluation using Samples 11 and 19. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below based on the embodiments. In the following description, the description of "A to B" indicating a numerical range indicates a numerical range including the endpoints A and B. Furthermore, parts by mass and % by mass are synonymous with parts by weight and % by weight, respectively.
[0013] <Radioactive iodine adsorbent and its manufacturing method> The radioactive iodine adsorbent of the present invention is formed by supporting silver on a high-silica zeolite in which hydroxyl nests present inside the high-silica zeolite have been converted to Si-O-Si bonds, and the high-silica zeolite is at least any one selected from the group consisting of chabazite (CHA)-type zeolite, mordenite (MOR)-type zeolite, and clinoptilolite (CLP)-type zeolite. In the present invention, high-silica zeolite means a zeolite having a SiO2 / Al2O3 molar ratio of more than 2.0. In the crystal lattice of a zeolite with a SiO2 / Al2O3 molar ratio of 2.0, Si and Al are arranged alternately, with Al present between each pair of Si, but in the crystal lattice of a zeolite with a SiO2 / Al2O3 molar ratio of more than 2.0, there are positions between Si and Si where no Al is present (hereinafter referred to as hydroxyl nests). Hydroxyl nests are lattice defects that reduce the durability of high-silica zeolites.
[0014] As a result of extensive investigations, the inventors have found that by subjecting high-silica zeolite containing hydroxyl nests therein to heat treatment, the hydroxyl nests can be converted to Si-O-Si bonds, thereby improving durability, and that a radioactive iodine adsorbent obtained by supporting silver after converting the hydroxyl nests to Si-O-Si bonds by this heat treatment has high adsorption capacity without decreasing its ability to adsorb iodine ions even under acidic conditions in which a reducing agent coexists in a solution containing iodine ions, the adsorbed substance, and is also resistant to embrittlement, thereby completing the present invention. The heat treatment is preferably performed at 500°C to 700°C for 20 to 90 minutes, more preferably at 550°C to 650°C for 20 to 60 minutes, and even more preferably at 600°C to 650°C for 30 to 50 minutes.
[0015] The high silica zeolite used as the base material of the radioactive iodine adsorbent preferably has a SiO2 / Al2O3 molar ratio of 2 to 100, more preferably 2 to 50, and even more preferably 2 to 20. The lower the SiO2 / Al2O3 molar ratio, the more the amount of silver that can be supported and the higher the ability to adsorb iodine ions, but on the other hand, the lower the acid resistance and the more likely it is to become embrittled under acidic conditions in which a reducing agent coexists in the aqueous solution. By setting the SiO2 / Al2O3 molar ratio within the above range, it is possible to realize a radioactive iodine adsorbent that has a high adsorption capacity without decreasing its ability to adsorb iodine ions even under acidic conditions in which a reducing agent coexists in the aqueous solution, and is less likely to become embrittled.
[0016] The high-silica zeolite used as the base material for the radioactive iodine adsorbent is not limited to synthetic products, but may be a natural product.
[0017] In the radioactive iodine adsorbent, the amount of silver supported on the high silica zeolite (hereinafter also referred to as the supported amount) is preferably 1 to 15 mass % and more preferably 3 to 12 mass % based on the total mass of the radioactive iodine adsorbent. The greater the supported amount of silver, the higher the ability to adsorb iodine ions can be, but on the other hand, when a solution containing iodine ions, which is an adsorbed substance, is passed through the adsorbent, liberated silver iodide is more likely to be generated, which is likely to cause clogging in an adsorption tower such as a column during the passage of the solution. By setting the supported amount of silver within the above range, it is possible to ensure a sufficient level of ability to adsorb iodine ions while avoiding the clogging.
[0018] The shape of the radioactive iodine adsorbent is not particularly limited, but since it is used by being packed into an adsorption tower such as a column, it is preferably in the form of a granular or rod-shaped molded body.
[0019] The particle size of the radioactive iodine adsorbent is preferably 0.1 mm or more and 5.0 mm or less, and more preferably 0.2 mm or more and 2.0 mm or less. By making the particle size of the radioactive iodine adsorbent 0.1 mm or more, the resistance when filled in the adsorption tower and water is passed through is not excessively large, and high liquid permeability can be ensured. By making the particle size of the radioactive iodine adsorbent 5.0 mm or less, it is possible to avoid a decrease in the adsorption rate caused by an increase in the external surface area of the radioactive iodine adsorbent filled in the adsorption tower, and it is possible to ensure a sufficient level of ability to adsorb iodine ions.
[0020] <How to dispose of radioactive iodine> The radioactive iodine adsorbent of the present invention can be suitably used for adsorbing and removing iodine ions and iodate ions, which are radioactive iodine contained in wastewater discharged from nuclear facilities. The method for treating radioactive iodine using the radioactive iodine adsorbent of the present invention includes a step of adding a reducing agent to waste liquid discharged from a nuclear facility to convert it into an acidic solution (hereinafter referred to as the reducing agent adding step), and a step of passing the waste liquid converted into the acidic solution through the radioactive iodine adsorbent (hereinafter referred to as the liquid passing step).
[0021] In the reducing agent addition process, the reducing agent converts iodate ions (IO3 - ) is reduced to iodide ions (I - ) The reducing agent used in the reducing agent addition step may be any reducing agent capable of reducing iodate ions, and examples thereof include formaldehyde, acetaldehyde, sodium sulfite, sodium pyrosulfite (SMBS), L-ascorbic acid (vitamin C), etc. Among these, L-ascorbic acid is preferred from the viewpoints of iodine adsorption amount and waste liquid treatment due to harmfulness.
[0022] In the liquid passing step, iodine ions contained in the acidic solution are adsorbed and removed by the radioactive iodine adsorbent. EXAMPLES
[0023] <Preparation of Test Samples: Samples 1 to 15 (Comparative Examples), Samples 16 to 19 (Examples)> Test samples were prepared under the conditions shown in Table 1 below. For the samples with "heat treatment before silver loading" the zeolite before silver loading was heat treated for 30 minutes at 600° C. This heat treatment is hereinafter referred to as "heat treatment before silver loading" to distinguish it from the heat treatment before each measurement described below (heat treatment after silver loading). The amount of supported silver was measured using a fluorescent X-ray measuring device (Shimadzu Corporation, XRF-1700). As a pretreatment before measuring the amount of supported silver, all samples (samples 1 to 19) were subjected to a heat treatment at 550° C. for 1 hour.
[0024] [Table 1]
[0025] <Vulnerability assessment using samples 1 to 3> i. Solution preparation Potassium iodate, L-ascorbic acid, and hydrochloric acid were added to neutral artificial seawater (Tomita Pharmaceutical's Marine Art SF-1 dissolved in ion-exchanged water) to the following concentrations. Cl = 900 ppm by mass (solution for vulnerability assessment of samples 1 to 3) L-ascorbic acid = 0 ppm by mass (vulnerability assessment solution for sample 1), 5000 ppm by mass (vulnerability assessment solutions for samples 2 and 3) pH=3~4 ii. Vulnerability assessment 0.5 g of each sample was added to 250 g of each solution prepared in i. After 6 days had passed, the appearance of each sample was observed and its composition was analyzed to evaluate its fragility. The results of the vulnerability assessment are shown in Table 2 below.
[0026] [Table 2]
[0027] Sample 1: When silver was supported on A-type zeolite without adding L-ascorbic acid to the acidic solution, no change occurred in the appearance of the A-type zeolite, and no embrittlement was confirmed. Sample 2: When L-ascorbic acid was added to the acidic solution and no silver was supported on the A-type zeolite, no change occurred in the appearance of the A-type zeolite, and no embrittlement was confirmed. Sample 3: When L-ascorbic acid was added to an acidic solution and silver was supported on A-type zeolite, embrittlement such as holes, cracks, and powdering was confirmed in the A-type zeolite, as shown in Figure 1.
[0028] <SiO2 / Al2O3 molar ratio measurement and fragility evaluation using samples 4-11> The SiO2 / Al2O3 molar ratio of each sample was calculated by quantifying the mass ratio of Si and Al measured by a fluorescent X-ray measurement device (Shimadzu XRF-1700) using a calibration curve. As a pretreatment before measurement by the fluorescent X-ray measurement device (Shimadzu XRF-1700), all samples (samples 4 to 11) were heated at 575°C for 1 hour. i. Solution preparation Potassium iodate, L-ascorbic acid, and hydrochloric acid were added to neutral artificial seawater (Tomita Pharmaceutical's Marine Art SF-1 dissolved in ion-exchanged water) to the following concentrations. Cl = 900 ppm by mass (solution for vulnerability assessment of samples 4 to 11) L-ascorbic acid = 5000 ppm by mass (vulnerability assessment solution for samples 4 to 11) pH=3~4 ii. Vulnerability assessment 0.5 g of each sample was added to 250 g of each solution prepared in i. Six days after the addition, the appearance of each sample was observed and its composition was analyzed to evaluate its fragility. The results of the SiO2 / Al2O3 molar ratio measurement and the fragility assessment are shown in Table 3 below.
[0029] [Table 3]
[0030] In all of Samples 4 to 11, 6 days after the addition of a solution containing a reducing agent (L-ascorbic acid), the SiO2 / Al2O3 molar ratio increased, and it was confirmed that dealuminization occurred in the solution. The higher the SiO2 / Al2O3 molar ratio before evaluation, the less the composition changed, and it was confirmed that high-silica zeolites were relatively more durable in the acidic region, but the same holes, cracks, powdering, and other embrittlement as shown in Figure 1 were confirmed on the surface of the molded bodies of all zeolites. From the results in Table 3, it can be confirmed that Samples 4 to 11 are not suitable for use in an acidic solution containing an added reducing agent.
[0031] <SiO2 / Al2O3 molar ratio measurement and fragility evaluation using samples 12-19> The SiO2 / Al2O3 molar ratio of each sample was calculated by quantifying the mass ratio of Si and Al measured by a fluorescent X-ray measurement device (Shimadzu XRF-1700) using a calibration curve. As a pretreatment before measurement by the fluorescent X-ray measurement device (Shimadzu XRF-1700), all samples (samples 12 to 19) were heated at 575°C for 1 hour. i. Solution preparation Potassium iodate, L-ascorbic acid, and hydrochloric acid were added to neutral artificial seawater (Tomita Pharmaceutical's Marine Art SF-1 dissolved in ion-exchanged water) to the following concentrations. Cl = 900 ppm by mass (solution for vulnerability assessment of samples 4 to 11) L-ascorbic acid = 5000 ppm by mass (vulnerability assessment solution for samples 4 to 11) pH=3~4 ii. Vulnerability assessment 0.5 g of each sample was added to 250 g of each solution prepared in i. Six days after the addition, the appearance of each sample was observed and its composition was analyzed to evaluate its fragility. The results of the SiO2 / Al2O3 molar ratio measurement and the fragility assessment are shown in Table 4 below.
[0032] [Table 4]
[0033] Samples 12 to 19 differ from Samples 4 to 11 only in the presence or absence of heat treatment before silver loading (heat treatment at 600 ° C for 30 minutes before silver loading). As described above, in all Samples 4 to 11, embrittlement such as holes, cracks, and powdering was confirmed on the surface of the zeolite molded body, and similar results were observed in Samples 12 to 15. However, in Samples 16 to 19 using zeolite "at least one selected from the group consisting of chabazite (CHA) type zeolite, mordenite (MOR) type zeolite, and clinoptilolite (CLP) type zeolite," the SiO2 / Al2O3 molar ratio was almost unchanged, and it was confirmed that dealuminization did not occur in the solution. In Samples 12 to 15, embrittlement such as holes, cracks, and powdering was not confirmed on the surface of any of the zeolites or molded bodies. From the results in Table 3, it can be confirmed that none of Samples 12 to 15 is suitable for use in an acidic solution to which a reducing agent has been added, and that none of Samples 12 to 15 is suitable for use in an acidic solution to which a reducing agent has been added.
[0034] <Evaluation of iodine adsorption characteristics using samples 4, 5, 9, and 11> i. Solution preparation Sodium iodide, L-ascorbic acid, and hydrochloric acid were added to artificial seawater (Tomita Pharmaceutical's Marine Art SF-1 dissolved in ion-exchanged water) to the following concentrations. Cl=900 mass ppm I=0.2 mass ppm L-ascorbic acid = 30 ppm by mass pH=3.5 ii. Iodine adsorption test Each sample was placed in a 1 cm diameter column with 5 cm of each solution. 3 The solution prepared in step i was then pumped through the column at a spatial velocity of 15 m / hr using a tube pump. The liquid at the outlet of the column was sampled at appropriate times, and the iodine content in the liquid was quantified by ICP-MS. The ratio C / C0 of the I concentration in the solution before passing through the column (C0) to the I concentration at the column outlet (C) was used to calculate C / C0 versus the passage time. The evaluation results are shown in Figure 2.
[0035] The sample with silver supported on mordenite (Sample 9) and the sample with silver supported on chabazite (Sample 11) maintained a C / C0 of 0.03 or less for a long period of time compared to the sample with silver supported on A-type zeolite (Sample 4) and the sample with silver supported on X-type zeolite (Sample 5), confirming that they have a long iodine adsorption life. However, after 20 days, the C / C0 of Sample 9 and Sample 11 increased, indicating a decrease in adsorption performance.
[0036] <Evaluation of iodine adsorption characteristics and differential pressure using samples 11 and 19> i. Solution preparation Sodium iodide, L-ascorbic acid, and hydrochloric acid were added to artificial seawater (Tomita Pharmaceutical's Marine Art SF-1 dissolved in ion-exchanged water) to the following concentrations. Cl=900 mass ppm I=0.2 mass ppm L-ascorbic acid = 30 ppm by mass pH=3.5 ii. Iodine adsorption characteristics evaluation and differential pressure evaluation A column with a diameter of 1 cm was filled with 80 cm of each sample, and a pressure gauge was installed at the inlet side of the column. Next, the solution prepared in i was passed through the column using a tube pump at a spatial velocity of 45 m / hr (flow rate 2.83 L / h), and the pressure on the pressure gauge was read at appropriate times. Furthermore, the liquid at the outlet side of the column was sampled at appropriate times, and the iodine content in the liquid was quantified by ICP-MS. Figure 3 shows the ratio C / C0 of the I concentration in the solution before passing through the column (C0) to the I concentration at the column outlet (C). FIG. 4 shows the results of calculating the difference (P-P0) between the pressure during liquid passage (P) and the pressure at the start of liquid passage (P0) as the differential pressure increase.
[0037] As shown in FIG. 3, for both Samples 11 and 19, no increase in C / C0 was observed within the 20-day liquid passage period, and the C / C0 was maintained at 0.1 or less, confirming that the samples have excellent iodine adsorption performance. After the 20th day, in sample 11, which had not been heat-treated before silver loading (a sample in which the zeolite was not heat-treated for 30 minutes at 600°C before silver loading), the C / C0 increased and a decrease in adsorption performance was observed. However, in sample 19, which had been heat-treated before silver loading (a sample in which the zeolite was heat-treated for 30 minutes at 600°C before silver loading), no increase in C / C0 was observed even after the liquid was passed through for 60 days, confirming that there was no decrease in iodine adsorption performance.
[0038] As shown in Figure 4, in sample 11, which was not heat-treated before silver loading, when liquid was passed through it under the differential pressure evaluation conditions (2.83 L / h), it was confirmed that the differential pressure gradually increased after 10 days, and further increased after 40 days. On the other hand, in sample 19, which was heat-treated before silver loading, no increase in differential pressure was observed even after 60 days, confirming that it can withstand long-term use under acidic conditions with the addition of a reducing agent.
[0039] It was confirmed that Sample 19, an embodiment of the present invention, did not develop embrittlement such as holes, cracks, or powdering even when used under acidic conditions with the addition of a reducing agent, and the differential pressure was less likely to increase during liquid passage, and the number of days during which liquid could be passed was longer, compared to Sample 11, a comparative example. This is thought to be due to the fact that Sample 19, an embodiment of the present invention, suppressed embrittlement of the agent and excessive precipitation of AgI, which are factors that cause clogging during liquid passage. [Industrial Applicability]
[0040] The radioactive iodine adsorbent of the present invention can stably adsorb iodine ions from waste liquid that has been converted into an acidic solution by the addition of a reducing agent, and can therefore be suitably used in the treatment of radioactive waste liquid in which iodate ions and iodine ions coexist, by adding a reducing agent to an aqueous solution containing radioactive iodine to reduce iodate ions to iodine ions and remove them together as iodine ions.
Claims
1. The zeolite is made by loading silver on a high-silica zeolite in which hydroxyl nests present inside the high-silica zeolite have been converted to Si-O-Si bonds, A radioactive iodine adsorbent, wherein the high silica zeolite is at least any one selected from the group consisting of chabazite (CHA) type zeolite, mordenite (MOR) type zeolite, and clinoptilolite (CLP) type zeolite.
2. The SiO of the high silica zeolite 2 / Al 2 O 3 The radioactive iodine adsorbent according to claim 1, wherein the molar ratio is 2 to 100.
3. The radioactive iodine adsorbent according to claim 1 or 2, wherein the amount of silver supported is 1 to 15 mass %.
4. A method for producing a radioactive iodine adsorbent, comprising the steps of: supporting silver on high-silica zeolite in which hydroxyl nests present inside the high-silica zeolite are converted to Si—O—Si bonds; A method for producing a radioactive iodine adsorbent, wherein the high silica zeolite is at least any one selected from the group consisting of chabazite (CHA) type zeolite, mordenite (MOR) type zeolite, and clinoptilolite (CLP) type zeolite.
5. 5. The method for producing a radioactive iodine adsorbent according to claim 4, wherein the hydroxyl nests are converted to the Si-O-Si bonds by heat treatment at 500° C. to 700° C.
6. The SiO of the high silica zeolite 2 / Al 2 O 3 The method for producing a radioactive iodine adsorbent according to claim 4 or 5, wherein the molar ratio is 2 to 100.
7. The method for producing a radioactive iodine adsorbent according to any one of claims 4 to 6, wherein the amount of silver supported is 1 to 15 mass%.
8. A process of adding a reducing agent to wastewater discharged from a nuclear facility to produce an acidic solution; A method for treating radioactive iodine, comprising a step of passing the acidic solution through the radioactive iodine adsorbent according to any one of claims 1 to 3.
Citation Information
Patent Citations
Iodine adsorbent
JP1985225638A
Separation by precipitation of radioactive iodine compound
JP1993126995A
Removal of iodide from organic liquid stream contaminated with iodide
JP2000334206A
Waste water treatment device and waste water treatment method for nuclear facility
JP2013104727A
Iodine adsorbent and production method thereof
JP2016107213A