How to etch a metal hard mask
The metal hard mask etching method addresses particle and defect issues by controlling the hydrogen to fluorine ratio in the etching gas and using auxiliary gases to minimize hydrogen fluoride generation and associated particle formation.
Patent Information
- Application Number
- JP2023534136
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-17
- Filing Date
- 2021-12-15
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-12-15
AI Technical Summary
Conventional metal hard mask etching methods generate hydrogen fluoride by-products that react with chamber coatings, leading to particle and defect issues, particularly in advanced technology nodes like 28 nm and below.
A metal hard mask etching method that controls the ratio of hydrogen to fluorine elements in the etching gas below a threshold, uses auxiliary gases for ionization, and includes cleaning processes to remove reaction by-products, thereby reducing hydrogen fluoride generation and associated particle formation.
Reduces hydrogen fluoride by-products, minimizing particle generation and defects by controlling the hydrogen to fluorine ratio in the etching gas and employing auxiliary gases to promote ionization and cleaning, effectively suppressing yttrium-containing particle formation.
Smart Images

Figure 0007576176000001 
Figure 0007576176000002 
Figure 0007576176000003
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE
[0002] Embodiments of the present invention relate to the field of semiconductor manufacturing, and more particularly, to a method for etching a metal hardmask. [Background technology]
[0002] Particle control ability is an important index for evaluating device stability and process stability in the manufacturing process of integrated circuits, and as the requirements for particle control in current processes become higher and higher, it has become a greater challenge for integrated circuit devices.
[0003] The particle sources mainly include process generation and external introduction. Process generation refers to the generation of particles by the process during the process reaction, and external introduction mainly refers to the introduction of particles during the loading of silicon wafers. Although the particles introduced during the loading of wafers have been effectively suppressed so far, process generation particles have always been a major problem in the process of extending etch process technology to lower technology nodes.
[0004] For example, in processes below 28 nm, the particle requirements for the etching process of metal hard masks are very high. However, in the etching method of metal hard masks used in the prior art, during the long-term use of etching equipment in mass production, by-products such as hydrogen fluoride (HF) are generated, which leads to loss of materials (such as Y2O3 coating) on the inner surface of the chamber, and even damage to the coating, making the chamber unusable. In addition, the by-products such as HF react with the Y2O3 coating to form yttrium-containing particles, which causes particle problems and defect problems. Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art, and provides a method for etching a metal hard mask, which can reduce the generation of hydrogen fluoride by-products, thereby reducing particles generated due to loss of material (such as a Y2O3 coating) on the inner surface of the chamber. [Means for solving the problem]
[0006] In order to achieve the object of the present invention, there is provided a method for etching a metal hard mask, which comprises forming a metal hard mask layer and at least one functional film layer on a wafer surface in a direction away from the wafer surface, in that order; The method for etching the metal hard mask includes a plurality of etching processes for sequentially etching at least one of the functional film layer and the metal hard mask layer along a direction close to the wafer surface, Among all the etching processes for etching the functional film layer, an etching gas used in at least one etching process contains hydrogen and fluorine elements, and in order to reduce the generation of hydrogen fluoride by-products, the ratio of the content of the hydrogen element in the etching gas to the content of the fluorine element in the etching gas is less than a preset threshold value.
[0007] Optionally, the ratio is less than or equal to 1.
[0008] Optionally, the ratio is less than or equal to 0.5.
[0009] Optionally, in an etching process in which the etching gas includes hydrogen and fluorine elements, a first auxiliary gas is introduced into the process chamber simultaneously with introducing the etching gas into the process chamber to promote ionization of the etching gas and reduce generation of hydrogen fluoride by-products.
[0010] Optionally, the first auxiliary gas includes at least one of argon gas, helium gas, and oxygen gas.
[0011] Optionally, the method for etching the metal hard mask includes: performing at least one cleaning process on the process chamber after all of the etching processes are completed to remove at least one reaction by-product generated in the process chamber by the etching processes; The reaction by-products include silicon-containing by-products, and a cleaning gas used in the cleaning process to clean the silicon-containing by-products includes a fluorine-containing gas and a second auxiliary gas to reduce the generation of fluorine-containing particles in a plasma formed by ionization of the fluorine-containing gas.
[0012] Optionally, the ratio of the flow rate of the second auxiliary gas to the flow rate of the fluorine-containing gas is in the range of 0.3-2.
[0013] Optionally, the second auxiliary gas includes at least one of argon gas, helium gas, and oxygen gas.
[0014] Optionally, the functional film layer is a two-layer structure, which is a dielectric material layer and an organic material mask layer disposed on the metal hard mask layer in sequence along a direction away from the wafer surface; The etching method for the metal hard mask includes three etching processes for sequentially etching the organic material mask layer, the dielectric material layer, and the metal hard mask layer along a direction close to the wafer surface; The etching gases used in the two etching processes for etching the organic material mask layer and the dielectric material layer, respectively, both contain hydrogen and fluorine elements.
[0015] Optionally, the etching gases used in the two etching processes for respectively etching the organic material mask layer and the dielectric material layer each contain CF4, CHF3 and CH2F2, and the gas flow rate ratio of CF4, CHF3 and CH2F2 is set so that the ratio of the content of hydrogen element in the CF4, CHF3 and CH2F2 in the etching gas to the content of fluorine element in the etching gas is smaller than the preset threshold value.
[0016] The embodiments of the present invention have the following beneficial effects: In the method for etching a metal hard mask according to the embodiment of the present invention, among all the etching processes for etching a functional film layer, an etching gas used in at least one etching process contains hydrogen and fluorine, and the ratio of the content of hydrogen in the etching gas to the content of fluorine in the etching gas is less than a preset threshold. By making the ratio of the content of hydrogen in the etching gas to the content of fluorine in the etching gas less than a preset threshold, the generation of hydrogen fluoride by-products can be reduced, thereby reducing the particles generated due to the loss of the material (such as Y2O3 coating) on the inner surface of the chamber, and further effectively suppressing the problems of particles and defects. [Brief description of the drawings]
[0017] [Figure 1] 1 is a flow chart of a method for etching a metal hard mask according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a process diagram of a method for etching a metal hard mask according to an embodiment of the present invention. [Diagram 3] 4 is another flow chart of the method for etching a metal hard mask in accordance with an embodiment of the present invention. [Figure 4] 4 is a further flow chart of a method for etching a metal hard mask in accordance with an embodiment of the present invention. [Diagram 5]1 is a line graph of chamber particles generated versus process time for a conventional metal hardmask etch method. [Figure 6] 1 is a line graph of chamber particles generated versus process time for a metal hard mask etching method according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, in order to enable those skilled in the art to better understand the technical solutions of the present invention, a method for etching a metal hard mask according to an embodiment of the present invention will be described in detail with reference to the accompanying drawings.
[0019] The embodiment of the present invention provides a method for etching a metal hard mask, which includes forming a metal hard mask layer and at least one functional film layer on a wafer surface in a direction away from the wafer surface (e.g., from bottom to top). In practical applications, the number and types of functional film layers vary according to technology generations, for example, in the 28 nm technology generation, the functional film layers are two layers, which are a dielectric material layer and an organic material mask layer, which are respectively disposed on the metal hard mask layer in a direction away from the wafer surface, but in the 14 nm technology generation, the functional film layers are at least three layers, for example, in addition to the above-mentioned dielectric material layer and organic material mask layer, an amorphous carbon layer or other organic material film layer is further disposed between the dielectric material layer and the organic material mask layer. In addition, before etching these functional film layers, a patterned photoresist layer needs to be formed on the top functional film layer to define the patterns of each functional film layer and the metal hard mask layer when performing the etching process of the functional film layers.
[0020] In practical applications, the wafer may be a normal semiconductor substrate such as a silicon substrate, or may be a laminated structure including a metal layer for wiring, an interlayer insulating layer, etc., where the metal hard mask layer includes, for example, a titanium nitride (TiN) layer, the dielectric material layer includes, for example, a silicon dioxide (SiO2) layer and a silicon nitride (SiN) layer, and the organic material mask layer includes, for example, a silicon anti-reflective layer (Si-arc layer) and a bottom anti-reflective layer (B-arc layer). The embodiments of the present invention do not particularly limit the types of functional film layers.
[0021] As shown in FIG. 1, a method for etching a metal hard mask according to an embodiment of the present invention includes: The method includes step S1, which is a plurality of etching processes for sequentially etching at least one functional film layer and a metal hard mask layer along a direction close to the wafer surface, and among all the etching processes for etching the plurality of functional film layers, an etching gas used in at least one etching process contains hydrogen and fluorine elements.
[0022] For example, the etching method of the metal hard mask includes three etching processes for sequentially etching the organic material mask layer, the dielectric material layer, and the metal hard mask layer along the direction close to the wafer surface. Among them, the etching gases used in the two etching processes for etching the organic material mask layer and the dielectric material layer respectively include CF4, CHF3, and CH2F2, and the etching gases used in the etching process for etching the metal hard mask layer include Cl2, CH4, and BCl3, etc. In this case, the etching gases used in the two etching processes for etching the organic material mask layer and the dielectric material layer respectively include hydrogen and fluorine. Of course, in practical applications, the type of etching gas used in the etching process of each functional film layer can be freely selected according to specific process requirements, and the embodiment of the present invention does not particularly limit this.
[0023] During the etching process, when the etching gas contains hydrogen and fluorine, hydrogen fluoride by-products will be generated and react with the inner surface material of the chamber. Take the inner surface material of the chamber as an example, hydrogen fluoride by-products will react with the Y2O3 coating material to generate yttrium fluoride (YxFy), and since the molecular volume of yttrium fluoride is smaller than that of Y2O3, shallow cracks will occur in the Y2O3 coating, which is easy to form yttrium-containing particles. During the mass production process of using an etching device for a long time, the hydrogen fluoride by-products will cause the loss of the Y2O3 coating, and even the coating will be damaged, making the chamber unusable, and yttrium-containing particles will be formed, causing particle problems and defect problems.
[0024] In addition, after all the etching processes are completed, the chamber needs to undergo a cleaning process to remove the reaction by-products. Referring to Fig. 2, the process specifically includes: firstly, transferring the wafer into the process chamber, performing the etching process, and after the etching process is completed, taking the wafer out of the process chamber, and then performing a cleaning process on the process chamber.
[0025] During the cleaning process, the cleaning gas usually contains nitrogen fluoride (NF3) gas, and the plasma generated by this gas is highly corrosive and will penetrate the Y2O3 coating to produce yttrium fluoride (YxFy). If the cleaning gas contains O2, it will react with the Y2O3 coating to produce YOF, which will eventually fall off and produce particles.
[0026] In order to solve the above problems, for an etching process in which the etching gas contains hydrogen and fluorine elements, the ratio of the hydrogen content in the etching gas to the fluorine content in the etching gas can be controlled to be within a range smaller than a preset threshold value, thereby reducing the generation of hydrogen fluoride by-products, thereby reducing particles (such as yttrium fluoride particles) generated by the reaction between the hydrogen fluoride by-products and the material on the inner surface of the chamber, and reducing the loss of the material on the inner surface of the chamber (such as a Y2O3 coating), and further effectively suppressing particle problems and defect problems.
[0027] The above-mentioned hydrogen element content in the etching gas and fluorine element content in the etching gas specifically refer to the respective contents of hydrogen element and fluorine element contained in the etching gas in the process chamber.
[0028] In some alternative embodiments, the ratio of the content of hydrogen element in the etching gas to the content of fluorine element in the etching gas is less than 1, for example, less than 0.5. By controlling the ratio within this range, particles (such as yttrium fluoride particles) generated by the reaction between hydrogen fluoride by-products and the material on the inner surface of the chamber can be effectively reduced, and the loss of the material on the inner surface of the chamber (such as a Y2O3 coating) can be reduced.
[0029] In some alternative embodiments, the ratio can be adjusted by adjusting the flow rates of various gases contained in the etching gas. For example, if the etching gases used in the two etching processes for etching the organic material mask layer and the dielectric material layer respectively include CF4 and CHF3, the flow rates of both gases can be set to 20 sccm and 100 sccm, respectively, and the ratio of the content of hydrogen element in the etching gas to the content of fluorine element in the etching gas is 0.26, which is smaller than 1, and the particles generated by the reaction of hydrogen fluoride by-products with the material on the inner surface of the chamber can be effectively reduced. Also, if the etching gases used in the etching processes for etching the organic material mask layer and the dielectric material layer respectively include O2 and CH2F2, the flow rates of both gases can be set to 80 sccm and 100 sccm, respectively, and the ratio of the content of hydrogen element in the etching gas to the content of fluorine element in the etching gas is 1, and the particles generated by the reaction of hydrogen fluoride by-products with the material on the inner surface of the chamber can be effectively reduced.
[0030] In some alternative embodiments, in an etching process in which the etching gas includes hydrogen and fluorine elements, a first auxiliary gas is introduced into the process chamber simultaneously with the introduction of the etching gas into the process chamber to promote ionization of the etching gas and further reduce the generation of hydrogen fluoride by-products. For example, when the etching gas includes CHF3 gas, the first auxiliary gas promotes further ionization of the CHF3 gas to reduce the generation of hydrogen fluoride by-products. + and CF3 + Fluorine and other free radicals and ions can be formed, thereby reducing the production of hydrogen fluoride by-products. Optionally, the first auxiliary gas includes at least one of argon gas, helium gas, and oxygen gas. Among them, oxygen gas can promote further ionization of CHF3 gas to produce CF2 + and CF3 +Not only can H react with H ions to produce HO, but also can form free radicals and ions such as HO, which can further reduce the production of hydrogen fluoride by-product.
[0031] In some alternative embodiments, as shown in FIG. 3, the method for etching the metal hard mask includes: After all the etching processes are completed, the method further includes a step S2 of performing at least one cleaning process on the process chamber to remove at least one reaction by-product generated in the process chamber by the etching processes.
[0032] In practical applications, the number of cleaning processes and the type of cleaning gas used in each cleaning process can be selected according to the type of reaction by-products generated in the process chamber.
[0033] When the reaction by-products include silicon-containing by-products, the cleaning gas used in the cleaning process for cleaning the silicon-containing by-products includes a fluorine-containing gas and a second auxiliary gas, where the fluorine-containing gas includes NF3 and SF6, etc., and the plasma generated by the fluorine-containing gas has high corrosiveness, and further penetrates the Y2O3 coating to generate yttrium fluoride (YxFy). To solve this problem, the second auxiliary gas can be introduced at the same time as the introduction of the fluorine-containing gas to reduce the generation of fluorine-containing particles (such as fluorine radicals) in the plasma formed by the ionization of the fluorine-containing gas, thereby reducing the yttrium-containing particles formed by the reaction of the fluorine-containing particles with the Y2O3 coating.
[0034] In some alternative embodiments, the ratio of the flow rate of the second auxiliary gas to the flow rate of the fluorine-containing gas can be controlled to control the components of the plasma formed by the ionization of the second auxiliary gas and the fluorine-containing gas, thereby ensuring that the plasma formed by the ionization of the second auxiliary gas can effectively reduce the generation of fluorine-containing particles (such as fluorine radicals) in the plasma formed by the ionization of the fluorine-containing gas while achieving the purpose of cleaning. Optionally, the ratio of the flow rate of the second auxiliary gas to the flow rate of the fluorine-containing gas is in the range of 0.3 to 2. Within this numerical range, it can be ensured that the generation of fluorine-containing particles (such as fluorine radicals) in the plasma formed by the ionization of the fluorine-containing gas can be effectively reduced.
[0035] In some alternative embodiments, the second auxiliary gas includes at least one of argon gas, helium gas, and oxygen gas.
[0036] Hereinafter, the method for etching a metal hard mask according to an embodiment of the present invention will be described in detail by taking as an example that the method for etching a metal hard mask includes three etching processes for sequentially etching an organic material mask layer, a dielectric material layer and a metal hard mask layer along a direction close to the wafer surface and corresponding cleaning processes.
[0037] Specifically, as shown in FIG. 4, the method for etching a metal hard mask includes the following steps S101 to S103.
[0038] S101, an etching process of an organic material mask layer is performed.
[0039] The etching process of the organic material mask layer may, for example, use the following process parameters:
[0040] The etching gas may be a gas containing hydrogen and fluorine, such as CF4, CHF3, and CH2F2, or a gas not containing hydrogen and fluorine, such as Cl2 and O2, or Cl2, O2, and CH4. The process pressure is in the range of 3mT to 40mT, preferably 5mT to 20mT, the excitation power is in the range of 200W to 2000W, preferably 400W to 1200W, and the bias power is in the range of 20W to 500W, preferably 60W to 200W. When the etching gas contains Cl2 and O2, or contains Cl2, O2, and CH4, the gas flow rate of Cl2 is 50sccm to 200sccm, the gas flow rate of O2 is 10sccm to 35sccm, and the gas flow rate of CH4 is 0sccm to 20sccm. When the etching gas contains CF4, CHF3 and CH2F2, the gas flow rate of CF4 is 0sccm-200sccm, the gas flow rate of CHF3 is 0sccm-200sccm, and the gas flow rate of CH2F2 is 0sccm-200sccm. When the etching gas contains CF4, CHF3 and CH2F2, a first auxiliary gas containing at least one of Ar, He and O2 can be selectively introduced, in which the gas flow rate of Ar is 0sccm-200sccm, the gas flow rate of He is 0sccm-300sccm, and the gas flow rate of O2 is 0sccm-150sccm.
[0041] After the etching process of the organic material mask layer is completed, carbon-containing by-products are formed in the chamber.
[0042] S102, performing an etching process for the dielectric material layer.
[0043] The etching process for the dielectric material layer may, for example, use the following process parameters:
[0044] The etching gas may be a gas containing hydrogen and fluorine, such as CF4, CHF3, and CH2F2, in which the gas flow rate of CF4 is 0sccm-200sccm, the gas flow rate of CHF3 is 0sccm-200sccm, and the gas flow rate of CH2F2 is 0sccm-200sccm. The total flow rate of the etching gas used in the etching process of the dielectric material layer is the same as the total flow rate of the etching gas used in the etching process of the organic material mask layer, the process pressure is in the range of 3mT-80mT, preferably 5mT-50mT, the excitation power is in the range of 200W-2000W, preferably 400W-1600W, and the bias power is in the range of 20W-500W, preferably 60W-400W.
[0045] After the etching process of the dielectric material layer is completed, silicon-containing by-products are formed in the chamber.
[0046] S103, an etching process of the metal hard mask layer is performed.
[0047] The etching process for the metal hardmask layer may, for example, use the following process parameters:
[0048] The etching gas includes Cl2, CH4 and BCl3, of which the gas flow rate of Cl2 is 0sccm-200sccm, the gas flow rate of CH4 is 0sccm-30sccm, and the gas flow rate of BCl3 is 0sccm-200sccm. Optionally, according to the needs of a specific process, shape modification gas or auxiliary gas for realizing other functions (such as gas that can promote plasma dispersion) can be introduced at the same time as introducing the etching gas. The shape modification gas is, for example, NF3 and SiCl4, and the gas flow rate of NF3 is 0sccm-200sccm, and the gas flow rate of SiCl4 is 0sccm-100sccm. The auxiliary gas for other functions is, for example, Ar, He and O2, and the gas flow rate of Ar is 0sccm-200sccm, the gas flow rate of He is 0sccm-300sccm, and the gas flow rate of O2 is 0sccm-150sccm. The process pressure ranges from 3mT to 40mT, preferably from 5mT to 20mT, the excitation power ranges from 200W to 2000W, preferably from 400W to 1200W, and the bias power ranges from 20W to 300W, preferably from 60W to 200W.
[0049] After the etching process of the metal hardmask layer is completed, metal by-products are formed in the chamber.
[0050] In the above two etching processes of step 1 and step 3, when the etching gas uses a gas containing hydrogen and fluorine, such as CF4, CHF3 and CH2F2, the ratio of the hydrogen content to the fluorine content in the etching gas is controlled within a range smaller than a preset threshold, for example, the range of the ratio is 0 to 1, preferably 0 to 0.5, thus reducing the generation of hydrogen fluoride by-products, thereby reducing particles (such as yttrium fluoride particles) generated by the reaction between the hydrogen fluoride by-products and the material on the inner surface of the chamber, and at the same time reducing the loss of the material on the inner surface of the chamber (such as Y2O3 coating), and further effectively suppressing particle problems and defect problems.
[0051] Furthermore, in the two etching processes of steps 1 and 3, when the etching gas uses a gas containing hydrogen and fluorine, such as CF4, CHF3, and CH2F2, a first auxiliary gas can be introduced at the same time as introducing the etching gas to promote ionization of the etching gas and further reduce the generation of hydrogen fluoride by-products.
[0052] After completing the etching process of the current wafer by the above-mentioned metal hard mask etching method, various by-products, i.e., carbon-containing by-products, silicon-containing by-products, and metal by-products, formed in the process chamber can be cleaned by the following cleaning method before performing the etching process of the next wafer, which specifically includes the following steps S104 to S106.
[0053] S104, performing a cleaning process on the metal by-products generated by the etching process of the metal hard mask layer.
[0054] The specific process parameters used are as follows:
[0055] The cleaning gas contains Cl2, and the gas flow rate is 0 sccm to 500 sccm, the process pressure is in the range of 3 mT to 40 mT, preferably 5 mT to 20 mT, and the excitation power is in the range of 200 W to 2000 W, preferably 400 W to 1200 W.
[0056] S105, performing a cleaning process on the silicon-containing by-products generated by the etching process of the dielectric material layer.
[0057] The specific process parameters used are as follows:
[0058] The cleaning gas includes NF3 and SF6, in which the gas flow rate of NF3 is 0sccm-300sccm and the gas flow rate of SF6 is 0sccm-100sccm. The cleaning gas includes a fluorine-containing gas, and the plasma generated by the fluorine-containing gas has a very high corrosiveness and further penetrates the Y2O3 coating to generate yttrium fluoride (YxFy). To solve this problem, a second auxiliary gas can be introduced at the same time as the introduction of the fluorine-containing gas to reduce the generation of fluorine-containing particles (such as fluorine radicals) in the plasma formed by the ionization of the fluorine-containing gas, thereby reducing the yttrium-containing particles formed by the reaction of the fluorine-containing particles with the Y2O3 coating. The second auxiliary gas includes at least one of Ar, He, and O2, in which the gas flow rate of O2 is 0sccm-500sccm, the gas flow rate of Ar is 0sccm-500sccm, and the gas flow rate of He is 0sccm-500sccm. Furthermore, the ratio of the flow rate of the second auxiliary gas to the flow rate of the fluorine-containing gas is in the range of 0.3 to 2. Within this numerical range, it is possible to ensure that the generation of fluorine-containing particles (such as fluorine radicals) in the plasma formed by ionization of the fluorine-containing gas can be effectively reduced. The process pressure is in the range of 5mT to 250mT, preferably 20mT to 90mT, and the excitation power is in the range of 200W to 2000W, preferably 800W to 1800W.
[0059] S106, performing a cleaning process on the carbon-containing by-products generated by the etching process of the organic material mask layer.
[0060] The specific process parameters used are as follows:
[0061] The cleaning gas contains O2, the gas flow rate is 0sccm to 500sccm, the process pressure is in the range of 3mT to 40mT, preferably 5mT to 20mT, and the excitation power is in the range of 200W to 2000W, preferably 400W to 1200W.
[0062] The present application is not limited to performing the cleaning in the order of steps S104 to S106, and steps S104 to S106 may be performed in other orders in order to achieve cleaning of the various by-products, and the present application is not limited thereto.
[0063] FIG. 5 is a line graph of chamber particles generated in a conventional metal hard mask etching method versus process time, and FIG. 6 is a line graph of chamber particles generated in a metal hard mask etching method according to an embodiment of the present invention versus process time. As shown in FIG. 5 and FIG. 6, PA is the total particle number in the process chamber, and Y2O3 is the Y2O3 particle number in the process chamber. As can be seen by comparing FIG. 5 and FIG. 6, in the conventional metal hard mask etching method, the total particle number generated in the process chamber gradually increases to 70 with the passage of process time, and the Y2O3 particle number gradually increases to 60 with the passage of process time. In comparison, in the metal hard mask etching method according to an embodiment of the present invention, the total particle number and the Y2O3 particle number generated in the process chamber are both controlled to less than 10 at different process times (0 to 100 h), thereby significantly reducing the particles generated due to the loss of material (such as Y2O3 coating) on the inner surface of the chamber, and further effectively suppressing particle problems and defect problems.
[0064] The method for etching a metal hard mask according to an embodiment of the present invention is applied to the manufacture of logic chip products such as central processing units (CPUs), graphics processing units (GPUs), and microprocessors (MPUs).
[0065] As described above, in the method for etching a metal hard mask according to the embodiment of the present invention, the etching gas used in at least one of all etching processes for etching a functional film layer contains hydrogen and fluorine, and the ratio of the content of hydrogen in the etching gas to the content of fluorine in the etching gas is less than a preset threshold. By making the ratio of the content of hydrogen in the etching gas to the content of fluorine in the etching gas less than a preset threshold, the generation of hydrogen fluoride by-products can be reduced, thereby reducing the particles generated by the loss of the material (such as Y2O3 coating) on the inner surface of the chamber, and further effectively suppressing the problems of particles and defects.
[0066] It is understood that the above embodiments are merely exemplary embodiments used to explain the principles of the present application, but the present application is not limited thereto. Those skilled in the art can make various modifications and improvements without departing from the spirit and essence of the present application, and these modifications and improvements are also considered to be within the protection scope of the present application.
Claims
1. A method for etching a metal hard mask, comprising forming a metal hard mask layer and at least one functional film layer on a wafer surface in a direction away from the wafer surface, the method comprising the steps of: A method for manufacturing a semiconductor device comprising the steps of: etching at least one of the functional film layer and the metal hard mask layer in a direction close to the wafer surface; Among all the etching processes for etching the functional film layer, an etching gas used in at least one etching process contains hydrogen and fluorine, and in order to reduce the generation of hydrogen fluoride by-products, a ratio of the content of the hydrogen element to the content of the fluorine element in the etching gas is smaller than a preset threshold value; The ratio can be adjusted by adjusting the flow rates of the gases contained in the etching gas, thereby reducing particles generated by reaction of the hydrogen fluoride by-products with materials on the interior surfaces of the chamber; The functional film layer includes a dielectric material layer and an organic material mask layer, which are disposed on the metal hard mask layer in sequence along a direction away from the wafer surface, Three etching processes are included to sequentially etch the organic material mask layer, the dielectric material layer, and the metal hard mask layer along a direction approaching the wafer surface; the etching gases used in the two etching processes for etching the organic material mask layer and the dielectric material layer, respectively, both contain hydrogen and fluorine; A method for etching a metal hard mask, characterized in that the etching gases used in the two etching processes for etching the organic material mask layer and the dielectric material layer, respectively, both contain CF4, CHF3 and CH2F2, and the gas flow rate ratio of CF4, CHF3 and CH2F2 is set so that the ratio of the hydrogen element content to the fluorine element content in the CF4, CHF3 and CH2F2 in the etching gas is smaller than the predetermined threshold value.
2. 2. The method for etching a metal hard mask according to claim 1, wherein the preset threshold value is 1 or less.
3. 3. The method for etching a metal hard mask according to claim 2, wherein the preset threshold is 0.5 or less.
4. 2. The method for etching a metal hard mask according to claim 1, wherein in the etching process, the etching gas contains hydrogen and fluorine, a first auxiliary gas is introduced into the process chamber at the same time as the etching gas is introduced into the process chamber to promote ionization of the etching gas and reduce generation of hydrogen fluoride by-products.
5. 5. The method for etching a metal hard mask according to claim 4, wherein the first auxiliary gas contains at least one of argon gas, helium gas, and oxygen gas.
6. The method for etching the metal hard mask includes the steps of: performing at least one cleaning process on the process chamber after all of the etching processes are completed to remove at least one reaction by-product generated in the process chamber by the etching processes; 2. The method of claim 1, wherein the reaction by-products include silicon-containing by-products, and a cleaning gas used in the cleaning process to clean the silicon-containing by-products includes a fluorine-containing gas and a second auxiliary gas for reducing generation of fluorine-containing particles in a plasma formed by ionization of the fluorine-containing gas.
7. 7. The method for etching a metal hard mask according to claim 6, wherein the second auxiliary gas contains at least one of argon gas, helium gas, and oxygen gas.
Citation Information
Patent Citations
Process for manufacturing contact hole
CN101866876A
Dry etching method
CN101937832A
Manufacturing method of graphs with small size
CN103903972A
Method of etching silicon oxide by carbon dioxide
JP1998189555A
Method for etching silicon nitride film and method for manufacturing semiconductor device
JP2001176842A