Copper-clad aluminum wire and its manufacturing method

The ion plating method for copper-coated aluminum wire addresses adhesion and weight reduction issues by removing the passive oxide film, enabling efficient production of ultra-fine wires with high adhesion and reduced copper content.

JP7576357B2Active Publication Date: 2024-10-31NAT INST FOR MATERIALS SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023505312
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-12
Filing Date
2022-02-28
Publication Date
2024-10-31
Estimated Expiration
2042-02-28

AI Technical Summary

Technical Problem

Existing copper/aluminum clad wires face challenges in achieving high adhesion and reducing weight due to the formation of a passive oxide film on aluminum surfaces, which affects the adhesion of copper coatings, and the use of electroplating methods is inefficient for long wires.

Method used

A copper-coated aluminum wire is manufactured using an ion plating method that removes the passive oxide film by controlled collision of copper ions with aluminum, ensuring a copper thin film with a space factor of 0.2% to 4% and adhesion of 10 mN or more, achieved by specific vacuum conditions and rotation speeds.

Benefits of technology

The method results in a copper-coated aluminum wire with excellent adhesion and reduced weight, allowing for high-purity aluminum wires to be processed into ultra-fine wires without breaking, while maintaining uniform copper coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576357000003
    Figure 0007576357000003
  • Figure 0007576357000004
    Figure 0007576357000004
  • Figure 0007576357000005
    Figure 0007576357000005
Patent Text Reader

Abstract

The problem addressed by the present invention is to provide a copper-coated aluminum wire material with a reduced weight and excellent adhesiveness, and a production method therefor. This copper-coated aluminum wire material is provided with an aluminum wire material comprising aluminum or an aluminum alloy and a thin copper film covering the aluminum wire material. The space factor of the thin copper film is in the range of 0.2% to 4% and the adhesiveness between the aluminum wire material and the thin copper film based on a scratch test compliant with JIS R 3255 is at least 10 mN.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copper-clad aluminum wire and a method for producing the same. [Background technology]

[0002] Aluminum is light, with a specific gravity of about 30% that of copper, and has a relatively high electrical conductivity. Currently, thin pure copper wires are used in wiring harnesses (multiple electric wires used for power supply and signal communication) installed in automobiles, but it is desirable to replace them with lightweight aluminum wires in order to improve fuel efficiency.

[0003] However, there are three major issues in putting aluminum wire into practical use. The first is that the strength drops significantly as the aluminum is purified to increase its electrical conductivity, the second is that the surface of aluminum is covered with a strong nanoscale passive oxide film, which makes soldering difficult, and the third is that aluminum, along with other metals with large potential differences, corrodes (electrolytic corrosion) when it comes into contact with moisture such as rainwater, making it difficult to use bare wire. To overcome these issues, a copper / aluminum clad wire has been developed in which an aluminum rod is inserted into a thick-diameter pure copper tube and then drawn, and is already on the market (see, for example, Patent Document 1).

[0004] However, according to Patent Document 1, in the case of copper / aluminum clad wire, pure copper is coated by a plastic processing method that ensures a large degree of processing, so it is difficult to reduce the space factor of pure copper per cross section of the wire. As a result, the advantage of aluminum, that is, its light weight, cannot be maximized, and therefore it has not become widely used.

[0005] There is a method of electroplating a thin layer of pure copper onto a thin aluminum wire, but since aluminum is a material that oxidizes very easily, even if the passive oxide film on the aluminum surface is removed by activation treatment, a film will form during subsequent water rinsing due to the small amount of dissolved oxygen in the water, and plating in this state will result in poor adhesion. To improve this, zincate treatment, which activates the aluminum surface while simultaneously displacing and depositing a zinc film, is commonly used to treat aluminum wires (see, for example, Patent Document 2). However, if the technology described in Patent Document 2 is adopted, it takes an enormous amount of time to treat long wires of several kilometers or more, making it unrealistic. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2011-194439 A [Patent Document 2] JP 2000-113730 A Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a copper-clad aluminum wire having excellent adhesion and reduced weight, and a method for producing the same. [Means for solving the problem]

[0008] The copper-clad aluminum wire according to the present invention comprises an aluminum wire made of aluminum or an aluminum alloy, and a thin copper film coating the aluminum wire, the space factor of the thin copper film being in the range of 0.2% or more and 4% or less, and the adhesion between the aluminum wire and the thin copper film based on a scratch test in accordance with JIS R 3255 satisfies 10 mN or more, thereby solving the above-mentioned problems. The copper thin film may have a space factor in the range of 0.2% or more and less than 1%. The copper thin film may have a space factor in the range of 0.3% to 0.55%. The adhesion may be in the range of 20 mN or more and 100 mN or less. The adhesion may be in the range of 50 mN or more and 100 mN or less. The aluminium may have a purity in the range of 99.9% to 99.99999%. The aluminum alloy may be an alloy of aluminum (Al) and at least one element selected from the group consisting of magnesium (Mg), iron (Fe), zirconium (Zr), zinc (Zn), chromium (Cr), scandium (Sc), manganese (Mn), boron (B), titanium (Ti), copper (Cu), lithium (Li), and silicon (Si). The interface between the aluminum wire and the copper thin film may not have a passive oxide film. According to the present invention, a method for producing a copper-coated aluminum wire by coating an aluminum wire made of aluminum or an aluminum alloy with a thin copper film by an ion plating method is provided, which comprises: a step of winding an aluminum wire having an outer diameter of 0.1 mm to 1.5 mm from a first drum wound in a vacuum chamber equipped with a copper evaporation source, the aluminum wire being rotated crosswise through at least a pair of return rolls so that the aluminum wire can be wound onto a second drum; and the distance between the aluminum wire passing between the at least a pair of return rolls and the center of the copper evaporation source is 500 mm or more and 100 mm or less. the aluminum wire is placed so that its thickness is 0 mm or less; evaporating and ionizing copper from the copper evaporation source by electron beam heating; applying a negative voltage of a magnitude in the range of more than 10 V and less than 800 V to the first drum and the second drum; and winding the aluminum wire around the second drum while cross-rotating it from the first drum via the at least one pair of return rolls at a speed of 1 m / min or more and less than 15 m / min, causing the ionized copper ions to collide with the aluminum wire to form a copper thin film, thereby solving the above-mentioned problem. The applying of the negative voltage may be a negative voltage having a magnitude in the range of 50V to 700V. The applying of the negative voltage may be a negative voltage having a magnitude in the range of 200V or more and 700V or less. The copper thin film is formed on the aluminum wire. Material may be wound at a speed of 1 m / min or more and 5 m / min or less. The aluminium may have a purity in the range of 99.9% to 99.99999%. The aluminum alloy may be an alloy of aluminum (Al) and at least one element selected from the group consisting of magnesium (Mg), iron (Fe), zirconium (Zr), zinc (Zn), chromium (Cr), scandium (Sc), manganese (Mn), boron (B), titanium (Ti), copper (Cu), lithium (Li), and silicon (Si). Prior to evaporating and ionizing the copper, the aluminum wire was bombarded with argon ions. Material The method may further include washing the surface. The ion bombardment process may be carried out at a pressure in a vacuum chamber in the range of 1 Pa to 10 Pa. The method may further include repeating the step of forming the thin copper film. The method may further include subjecting the copper-clad aluminum wire obtained by forming the copper thin film to a wiredrawing process. The wire drawing process may be a drawing process using a carbide die or a diamond die. Before, after, or during the drawing process, the copper-clad aluminum wire may be annealed at a temperature in the range of 300° C. to 500° C. for a period of 1 second to 5 minutes. Effect of the Invention

[0009] The method for producing a copper-clad aluminum wire of the present invention can coat an aluminum wire made of aluminum or an aluminum alloy with a copper thin film by an ion plating method. As described above, by setting the region where copper ions are deposited on the aluminum wire to a predetermined range, sufficient collision energy is obtained, so that a copper thin film can be formed while removing a passive oxide film on the surface of the aluminum wire. As a result, a copper-clad aluminum wire having excellent adhesion between the copper thin film and the aluminum wire can be provided.

[0010] In addition, since deposition is performed while rotating crosswise using at least one pair of return rolls, a thin copper film can be uniformly and thinly coated on the surface of the aluminum wire. Therefore, a lightweight copper-clad aluminum wire with a small copper space factor can be provided. Furthermore, by setting the winding speed of the aluminum wire to the above-mentioned predetermined speed, the aluminum wire is not broken, and a copper-clad aluminum wire can be provided with a high yield even for long wires. Furthermore, since the manufacturing method of the present invention can be applied to soft aluminum of high purity, the yield strength of the entire aluminum wire can be improved by coating it with a thin copper film. Therefore, ultra-fine wire drawing is also possible. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic diagram showing a copper-clad aluminum wire of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of a manufacturing apparatus for manufacturing a copper-clad aluminum wire according to the present invention. [Diagram 3] 1 is a flowchart showing a process for producing a copper-clad aluminum wire according to the present invention. [Figure 4] FIG. 2 is a diagram showing a schematic diagram of a deposition region in an ion plating apparatus. [Diagram 5] FIG. 2 is a schematic diagram showing how a thin copper film is coated by an ion plating method. [Figure 6] FIG. 2 is a diagram showing a schematic diagram of a wire drawing process. [Figure 7]7A and 7B are diagrams showing the appearance of the copper-clad aluminum wire of Example 2. Here, Fig. 7A shows the copper-clad aluminum wire being wound around a second drum, and Fig. 7B shows the copper-clad aluminum wire after wiredrawing. [Figure 8] 8A and 8B are diagrams showing SEM images of the cross sections of the copper-clad aluminum wires of Examples 2 and 5. Here, Fig. 8A shows a SEM image of the cross section of the copper-clad aluminum wire of Example 2, and Fig. 8B shows a SEM image of the cross section of the copper-clad aluminum wire of Example 5. [Figure 9] FIG. 1 is a diagram showing the results of a scratch test of the copper-clad aluminum wires of Examples 2, 5, 10, 11, 12, and 14. [Figure 10] FIG. 2 is a diagram showing an optical microscope photograph of a cross section of the copper-clad aluminum wire of Example 2 during wiredrawing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that like elements are given like reference numerals and their description will be omitted.

[0013] FIG. 1 is a schematic diagram showing a copper-clad aluminum wire according to the present invention.

[0014] The copper-clad aluminum wire 100 of the present invention includes an aluminum wire 110 made of aluminum or an aluminum alloy, and a copper thin film 120 that coats the aluminum wire 110. Since the aluminum wire 110 is coated with the copper thin film 120, it has environmental resistance.

[0015] In the copper-clad aluminum wire 100 of the present invention, the space factor (%) of the copper thin film 120 is 0.2% or more and 4% or less. This allows weight reduction. The space factor (%) of the copper thin film 120 is the percentage of the cross-sectional area of ​​the copper thin film 120 with respect to the total cross-sectional area of ​​the copper-clad aluminum wire 100. The space factor (%) of the copper thin film 120 is preferably in the range of 0.2% or more and less than 1%. This allows further weight reduction. The space factor (%) of the copper thin film 120 is more preferably in the range of 0.3% or more and 0.55% or less. Within this range, weight reduction is possible while maintaining adhesion. The cross-sectional area is the area of ​​a cross section in a direction perpendicular to the longitudinal direction of the copper-clad aluminum wire 100.

[0016] The copper-clad aluminum wire 100 of the present invention does not have a passive oxide film between the aluminum wire 110 and the copper thin film 120, and therefore the adhesion between the aluminum wire 110 and the copper thin film 120 based on a scratch test in accordance with JIS R 3255 satisfies 10 mN or more, and does not cause poor adhesion. Since there is no concern about poor adhesion if it is 10 mN or more, no upper limit is particularly set, but it may be 300 mN or less.

[0017] The adhesion preferably satisfies the range of 20 mN or more and 100 mN or less. Within this range, the adhesion is higher, the copper thin film 120 does not peel off, and the yield strength of the copper-clad aluminum wire 100 is further improved. The adhesion more preferably satisfies the range of 30 mN or more and 100 mN or less, and even more preferably, the range of 50 mN or more and 100 mN or less. Within this range, the yield strength of the copper-clad aluminum wire 100 is further improved.

[0018] The aluminum wire 110 may be aluminum or an aluminum alloy, but the aluminum preferably has a purity in the range of 99.9% to 99.99999%. In the case of the copper-clad aluminum wire of the present invention, even high-purity aluminum wire can be used without breakage.

[0019] In addition to pure aluminum, an aluminum alloy can also be used. The aluminum alloy may be an alloy containing aluminum (Al) as a main component and at least one element selected from the group consisting of magnesium (Mg), iron (Fe), zirconium (Zr), zinc (Zn), chromium (Cr), scandium (Sc), manganese (Mn), boron (B), titanium (Ti), copper (Cu), lithium (Li), and silicon (Si).

[0020] The content of elements other than aluminum constituting the aluminum alloy may be preferably 0.1 at% or more and 10 at% or less. In this case, even if two or more elements other than Al are selected, the total content of these elements may be within the above range. From this viewpoint, the amount of Al as the main component in the aluminum alloy may be 90 at% or more and less than 99.9 at%.

[0021] Next, a preferred method for producing the copper-clad aluminum wire 100 of the present invention will be described.

[0022] FIG. 2 is a schematic diagram of a manufacturing apparatus for manufacturing the copper-clad aluminum wire of the present invention. FIG. 3 is a flow chart showing the steps of producing a copper-clad aluminum wire according to the present invention.

[0023] The present inventors have discovered that by employing an ion plating method and setting various conditions, it is possible to remove the passive oxide film from an aluminum wire and at the same time form an extremely thin copper film.

[0024] In the method of the present invention, an ion plating apparatus shown in Fig. 2 is used, but it should be noted that the configuration shown in Fig. 2 is merely an example and is not limited to this configuration. The ion plating apparatus 200 may include a vacuum chamber 201, an electron gun 202 provided in the vacuum chamber 201, a thermionic filament 203, and an ionization electrode 204.

[0025] The vacuum chamber 201 can be evacuated via an exhaust port by a vacuum pump such as a diffusion pump, a turbo molecular pump, a cryopump, etc. A reactive gas, a discharge cleaning gas (a gas for ion bombardment processing), etc. are supplied to the vacuum chamber 201 via a gas supply pipe 205.

[0026] The electron gun 202 heats and evaporates an evaporation source (copper metal in this case) 207 housed in a hearth liner 206. The electron gun 202 generates an electron beam 208 by power supply from an electron gun power supply unit (not shown) provided outside the vacuum chamber 201. The electron beam 208 is deflected and irradiated onto the evaporation source in the hearth liner 206. The evaporation source 207 is heated and evaporated.

[0027] The thermionic filament 203 is connected to a filament heating power supply device (not shown) and is supplied with AC power. The thermionic filament 203 is heated by the power supply and emits thermoelectrons. Such thermionic filament 203 is made of a metal such as tungsten, molybdenum, or tantalum.

[0028] A positive voltage is applied to the ionization electrode 204. The thermoelectrons from the thermionic filament 203 collide with evaporated particles (copper particles in this case) evaporated from the evaporation source 207 while traveling toward the ionization electrode 204, ionizing the evaporated particles. The ionized evaporated particles (copper ions in this case) adhere to the target to form a thin film. As shown in FIG. 2, a shutter 209 may be provided to control the timing of adhesion of the ionized evaporated particles to the target. Also, a film thickness meter 210 may be provided to measure the thickness of the formed thin film. Such an ion plating device 200 may be similar to an existing ion plating device.

[0029] The ion plating device 200 further contains a first drum 211 and a second drum 212. An aluminum wire 110 made of aluminum or an aluminum alloy is wound around the first drum 211, and is configured so as to be able to be wound from the first drum 211 onto the second drum 212. A voltage can be applied to the first drum 211 and the second drum 212, and the aluminum wire 110 becomes the target object.

[0030] The ion plating device 200 further contains at least one pair (one set) of return rolls 213 so that the aluminum wire 110 from the first drum 211 is wound around the second drum 212 while rotating in a crosswise direction. If there is one pair of return rolls, for example, a copper thin film is formed on one side of the aluminum wire while it moves from A to B, and a copper thin film is formed on the other side while it moves from C to D. By providing two or more pairs of return rolls, the thickness of the copper thin film coating the aluminum wire can be more efficiently controlled. To explain specifically with reference to FIG. 2, a combination of one return roll 213 moving from A to B and one return roll 213 moving from C to D is referred to as a pair (one set) of return rolls 213. Therefore, when there are five such combinations as shown in FIG. 4, it is referred to as having five pairs (five sets) of return rolls 213.

[0031] 2, an ion plating apparatus 200 is described in which the aluminum wire is wound from the first drum 211 onto the second drum 212 via at least a pair of return rolls 213, but the aluminum wire may be wound from the second drum 212 onto the first drum 211 via at least a pair of return rolls 213. Each step of the method of the present invention will be described using such an ion plating apparatus 200.

[0032] Step S310: In a vacuum chamber 201 equipped with a copper evaporation source 207, an aluminum wire 110 having an outer diameter of 0.1 mm to 1.5 mm is wound around a first drum 211, and the aluminum wire 110 is wound around the second drum 212 by cross-rotating (for example, in the order of A → B → C → D) via at least a pair of return rolls 213. The aluminum wire 110 is installed so that the distance between the aluminum wire 110 passing between at least a pair of return rolls 213 and the center of the copper evaporation source 207 is 500 mm to 1000 mm. The aluminum wire 110 is the same as the aluminum wire described with reference to FIG. 1, so a description thereof will be omitted. If two or more pairs (two sets) of return rolls are provided, the number of cross-rotations increases, which is advantageous for controlling the thickness of the copper thin film coated on the aluminum wire.

[0033] In step S310, when the aluminum wire 110 is set, the inside of the vacuum chamber 201 is evacuated. The degree of vacuum at this time is preferably 1×10 -9 Pa or more 1×10 -5 Pa or less, and more preferably 1×10 -7 Pa or more 1×10 -5 The range is below Pa.

[0034] FIG. 4 is a schematic diagram showing a deposition region in an ion plating apparatus. FIG. 5 is a schematic diagram showing how a thin copper film is coated by the ion plating method.

[0035] Figure 4 shows an enlarged view of the deposition area in an ion plating apparatus equipped with five sets of return rolls 213. The deposition area 410 obtained by the evaporation of the evaporation source 207 is indicated by hatching. Focusing on the deposition area 410 that can be formed by step S320 described later, there are three types of lengths: distance D1, distance D2, and distance D3 between the center P of the evaporation source 207 and the aluminum wire 110 spanning between the return rolls 213. Here, distance D1 is the shortest distance, and distance D2 is the longest distance. Such distances D1, D2, and D3 each satisfy the range of 500 mm or more and 1000 mm or less, and the distances are such that D1 < D3 < D2. The inventors of the present application have found that by thus limiting the deposition area 410, when copper ions 520 collide with the aluminum wire 110, the passive oxide film 510 on the surface of the aluminum wire 110 is removed by the collision energy, and at the same time, a copper thin film composed of copper particles 530 is formed. From this result, it was confirmed that high adhesion between the copper thin film and the aluminum wire can be achieved.

[0036] Step S320: Evaporate and ionize copper from the copper evaporation source 207 by heating with an electron beam 208. The evaporation and ionization of copper from the copper evaporation source 207 are performed by the electron gun 202, the thermionic filament 203, and the ionization electrode 204 of the ion plating apparatus 200.

[0037] In step S320, preferably, the degree of vacuum is set in the range of 1×10 -4 Pa or more and 1×10 -2 Pa or less. Thereby, the amount of copper evaporation is controlled, and many copper particles are ionized, so that the formation of the copper thin film is further efficiently promoted.

[0038] Step S330: A negative voltage in the range of more than 10V and not more than 800V is applied to the first drum 211 and the second drum 212. This allows the positively charged copper ions ionized in step S320 to adhere to the aluminum wire 110 to which the negative voltage has been applied. Preferably, a negative voltage in the range of more than 50V and not more than 700V is applied. This allows the copper ions to adhere to the aluminum wire 110 more efficiently. More preferably, a negative voltage in the range of more than 200V and not more than 700V is applied. This allows the copper ions to adhere to the aluminum wire 110 more efficiently.

[0039] Step S340: The aluminum wire 110 is wound around the second drum 212 while being cross-rotated through at least one pair of return rolls 213 from the first drum 211 at a speed of 1 m / min or more and less than 15 m / min, and ionized copper ions are bombarded with the aluminum wire to form a copper thin film. As a result, a copper thin film is formed on the surface of the aluminum wire 110 while destroying and removing the passive oxide film on the surface of the aluminum wire 110, so that a copper-clad aluminum wire 100 (FIG. 1) is obtained. If the winding speed is slower than 1 m / min, the temperature of the aluminum wire increases due to the collision of copper ions, and there is a risk that the aluminum wire will break during the ion plating process. If the winding speed is 15 m / min or more, there may be an area of ​​the aluminum wire that is not copper-coated.

[0040] Preferably, aluminum wire Material 110 The copper-clad aluminum wire is wound at a speed of 1 m / min to 5 m / min. This allows efficient production of a copper-clad aluminum wire from which the passive oxide film has been removed. Material 110 The wire is wound at a speed of 2 m / min to 5 m / min. This makes it possible to more efficiently obtain a copper-clad aluminum wire that is free of a passive oxide film.

[0041] Step S3 4 The formation of the copper thin film of 0 may be repeated. For example, aluminum wire Material 110After the first drum 211 is wound onto the second drum 212, the second drum 212 is replaced with the first drum 211, and the first drum is replaced with the second drum 212, and step S3 is performed again. 4 0 may be performed. This allows the thickness of the copper thin film coated on the aluminum wire to be controlled. Material 110 After the aluminum wire 110 is wound from the first drum 211 onto the second drum 212, the aluminum wire 110 is wound from the second drum 212 onto the first drum 211 while being cross-rotated via at least a pair of return rolls 213, and then in step S3 in the reverse direction (for example, D→C→B→A in FIG. 4 ). 4 0 may be performed, or after winding, step S3 may be performed again in the forward direction (for example, A → B → C → D in FIG. 4). 4 0 may be performed. Such modifications are within the scope of the present specification. Thus, step S3 4 By repeating the winding of the return roll 213 and / or appropriately combining the number of pairs of return rolls 213 in step S310, the aluminum wire 110 can be more efficiently coated with a copper thin film having a thickness appropriate for the application.

[0042] Steps S320, S330 and S340 may be performed simultaneously, or step S340 may be performed first, followed by steps S320 and S330.

[0043] After step S310, and prior to step S320, an ion bombardment process using argon ions may be performed to clean the surface of the aluminum wire 110. In this case, while performing the ion bombardment process, the aluminum wire 110 may be wound around the second drum 212 while cross-rotating from the first drum 211 via at least a pair of return rolls 213, with a negative voltage being applied to the first drum 211 and the second drum 212. This allows the surface of the aluminum wire 110 to be cleaned.

[0044] In the ion bombardment process, the degree of vacuum is preferably set to a range of 1 Pa to 10 Pa. This promotes the generation of argon plasma more efficiently. After the ion bombardment process, the degree of vacuum is again set to 1×10 -9 Pa or more 1×10 -5 Pa or less, more preferably 1×10 -7 Pa or more 1×10 -5 After the pressure is adjusted to within the range of not more than Pa, step S320 may be performed. Furthermore, there is no particular limitation on the winding speed, and it may be, for example, 5 m / min to 15 m / min.

[0045] In the ion bombardment process, a negative voltage having a magnitude in the range of 100 V to 400 V may be applied to the first drum 211 and the second drum 212. This promotes cleaning by argon plasma more efficiently.

[0046] FIG. 6 is a diagram showing a schematic diagram of the wire drawing process.

[0047] The copper-clad aluminum wire 100 is obtained by step S340, but the obtained copper-clad aluminum wire 100 may be further subjected to wire drawing. According to the method of the present invention, even a high-purity soft aluminum wire 110 can be coated with a copper thin film, so that the overall yield strength of the obtained copper-clad aluminum wire 100 is increased. Therefore, even a high-purity aluminum wire 110 can be made into an ultra-thin wire by wire drawing. There is no particular restriction on such wire drawing, but it is preferably a drawing process using a superhard die or a diamond die as shown in FIG. 6. This allows an aluminum wire 110 having an outer diameter in the range of 0.1 mm or more and 1.5 mm or less to be made into an ultra-thin wire to an outer diameter in the range of 0.05 mm or more and less than 0.1 mm.

[0048] Before drawing, after drawing, or during drawing, the copper-clad aluminum wire 100 may be annealed at a temperature range of 300° C. to 500° C. for 1 second to 5 minutes. This removes the strain generated during drawing, and can more efficiently suppress cracks and microcracks in the aluminum wire 110. The drawing and annealing may be performed multiple times until the desired outer diameter is obtained, as shown in FIG. 6.

[0049] The present invention will now be described in detail with reference to specific examples, but it should be noted that the present invention is not limited to these examples. EXAMPLES

[0050] [Example 1 to Example 24] An ion plating apparatus 200 (FIG. 2) equipped with five sets of return rolls 213 (FIG. 4) and housing a copper evaporation source 207 (FIG. 2) (copper purity 99.999%) was used to coat an aluminum wire 110 (FIG. 1) made of aluminum or an aluminum alloy shown in Table 1 with a thin copper film to produce a copper-coated aluminum wire.

[0051] An aluminum wire was placed in the vacuum chamber 201 (FIG. 2) so that the distances D1, D2, and D3 were 500 mm, 1000 mm, and 700 mm, respectively, as shown in FIG. 4 (step S310 in FIG. 3). Here, the aluminum wire (FIG. 1) was wound around the first drum 211 (FIG. 2), and the aluminum wire was wound around five return rolls. 213 The aluminum wire 110 is wound around the second drum 212 (FIG. 2) by rotating the aluminum wire 110 in a crosswise direction 10 times through the five return rolls 213, and the distance between the aluminum wire 110 passing between the five return rolls 213 and the center P of the copper evaporation source 207 is in the range of 500 mm to 1000 mm. Next, the vacuum degree in the vacuum chamber 201 is set to 1×10 -6 The pressure was then reduced to 1 Pa using a vacuum pump.

[0052] Next, in some examples as shown in Table 1, argon ion bombardment treatment was performed to clean the aluminum wire. In detail, argon gas was introduced into the vacuum chamber 201 so that the pressure was in the range of 1 Pa or more and 10 Pa or less. A negative voltage of 240 V was applied to the first drum 211 and the second drum 212 to generate argon plasma. Next, the aluminum wire was wound (rewound) from the first drum 211 to the second drum 212 via five sets of return rolls. The rewinding speed of the aluminum wire at this time was 10 m / min.

[0053] After the argon ion bombardment process is completed, the voltage application is stopped and the vacuum degree of the vacuum chamber 201 is reduced to 1×10 -6 The vacuum was drawn until the pressure reached 1 Pa. Then, the film was taken up again from the second drum 212 onto the first drum 211.

[0054] Next, the copper evaporation source 207 was evaporated and ionized by heating with the electron beam 208 (step S320 in FIG. 3). In detail, the thermionic voltage was 14 V, thermionic current was 80 A, the emission current was 450 mA, the ionization voltage was 50 V, and the ionization current was 90 A. The degree of vacuum in the vacuum chamber 201 was 1×10 -3 The evaporation rate of copper was controlled by adjusting the pressure in the vacuum chamber to 100 Pa.

[0055] Next, a negative voltage having a magnitude shown in Table 1 was applied to the first drum 211 and the second drum 212 (step S330 in FIG. 3). The aluminum wire 110 was rotated 10 times crosswise from the first drum 211 through five sets of return rolls 213 at the speed shown in Table 1 and wound around the second drum 212, and ionized copper ions were collided with the aluminum wire 110 to form a copper thin film (step S340 in FIG. 3).

[0056] Next, in some examples, the formation of a thin copper film was repeated as shown in Table 1. In Table 1, a repetition number of 0 means that the formation of a thin copper film (step S340 in FIG. 3) was performed once, and a repetition number of 1 means that the formation of a thin copper film was performed twice.

[0057] The repeated copper thin film formation was carried out in detail as follows. After the first copper thin film formation was completed, the electron beam heating and the voltage application to the first drum 211 and the second drum 212 were stopped, and the degree of vacuum in the vacuum chamber 201 was reduced to 1×10 -6 The film was then evacuated to 10 Pa. The film was then rewound from the second drum 212 onto the first drum 211, and again subjected to electron beam heating under the above-mentioned conditions, a negative voltage was applied, and the film was rewound at the speed shown in Table 1 to form a thin copper film.

[0058] Next, some of the samples were subjected to a wire drawing process, as shown in Table 1. The wire drawing process was a drawing process using a diamond die multiple times, as shown in Figure 6. After the drawing process, the samples were annealed at 300°C for 30 seconds.

[0059] The appearance and cross section of the copper-clad aluminum wires of Examples 1 to 24 obtained in this manner were observed. A scanning electron microscope (Hitachi High-Tech Corporation, TM3030Plus) or an optical microscope (Nikon Corporation, ECLIPSE LV150) was used to observe the cross sections. The thickness of the copper thin film and the copper space factor were determined from the SEM images. The adhesion between the copper thin film and the aluminum wire was evaluated by a scratch test in accordance with JIS R 3255. These results are shown in Figures 7 to 10 and Table 2.

[0060] [Table 1]

[0061] [Table 2]

[0062] FIG. 7 is a diagram showing the appearance of the copper-clad aluminum wire of Example 2.

[0063] Fig. 7(A) shows the copper-clad aluminum wire being wound around the second drum 212, and Fig. 7(B) shows the copper-clad aluminum wire after the wire drawing process. Although shown in grayscale in Fig. 7, the wire surface in both cases exhibited a copper luster.

[0064] FIG. 8 is a diagram showing SEM images of the cross sections of the copper-clad aluminum wires of Examples 2 and 5.

[0065] FIG. 8(A) is a cross-sectional SEM image of the copper-clad aluminum wire of Example 2, and FIG. 8(B) is a cross-sectional SEM image of the copper-clad aluminum wire of Example 5. FIG. 8(A) shows that there is no passive oxide film at the interface between the aluminum wire and the copper thin film. On the other hand, FIG. 8(B) shows that a passive oxide film with a thickness of about 10 nm was observed at the interface between the aluminum wire and the copper thin film. Although not shown, no passive oxide film was observed at the interface between the aluminum wire and the copper thin film in the copper-clad aluminum wires of Examples 1 to 4, 6 to 10, 12 to 14, and 16 to 24.

[0066] Furthermore, referring to the results of the scratch test of the copper-clad aluminum wires of Examples 2 and 5 in Table 2, the adhesion of the copper-clad aluminum wire of Example 2 was significantly higher than that of Example 5. From these results, it was demonstrated that the method of the present invention is a suitable method for coating a thin copper film while removing the passive oxide film on the surface of an aluminum wire, and that high adhesion can be obtained between the aluminum wire and the thin copper film.

[0067] According to Examples 1 to 3, 6 to 10, 12 to 14, and 16 to 24 in Table 2, it was shown that by carrying out the method of the present invention, a copper-clad aluminum wire can be obtained in which the space factor of the copper thin film is in the range of 0.2% or more and 4% or less, preferably in the range of 0.3% or more and 0.55% or less, and the adhesion between the aluminum wire and the copper thin film based on a scratch test in accordance with JIS R 3255 is 10 mN or more, preferably in the range of 20 mN or more and 100 mN or less, more preferably in the range of 30 mN or more and 100 mN or less, and even more preferably in the range of 50 mN or more and 100 mN or less.

[0068] Focusing on the results of the copper-clad aluminum wires of Examples 4, 8, and 13 in Table 2, although they had adhesion, the aluminum wires were broken during production. This shows that it is necessary to wind the aluminum wires at a speed of 1 m / min or more and less than 15 m / min.

[0069] Looking at the results of the copper-clad aluminum wires of Examples 5, 11, and 15 in Table 2, it was shown that in order to remove the passive oxide film and maintain adhesion, it was necessary to apply a negative voltage of at least 10 V to the first drum and the second drum.

[0070] FIG. 9 is a diagram showing the results of a scratch test of the copper-clad aluminum wires of Examples 2, 5, 10, 11, 12 and 14.

[0071] According to the adhesion results in Table 2 and FIG. 9, it is found that it is preferable to apply a negative voltage in the range of 200 V to 700 V and wind the aluminum wire at a speed of 1 m / min to 5 m / min.

[0072] FIG. 10 is a diagram showing an optical microscope photograph of a cross section of the copper-clad aluminum wire of Example 2 during wire drawing.

[0073] 10 shows the change in cross section during drawing of the copper-clad aluminum wire of Example 2, with the outer diameters being 1.004 mm, 0.920 mm, and 0.837 mm from the left. It was confirmed that the copper thin film remained firmly attached without peeling even after multiple drawing processes using a die. [Industrial Applicability]

[0074] According to the present invention, a copper-clad aluminum wire having excellent adhesion and reduced weight is provided, and therefore the wire can be used for electronic devices, cable conductors, braided wires, various motor coils, and the like. [Explanation of symbols]

[0075] 100 Copper-clad aluminum wire 110 Aluminum wire 120 Copper thin film 200 Ion plating equipment 201 Vacuum Chamber 202 Electron Gun 203 Thermionic Filament 204 Ionization Electrode 205 Gas supply pipe 206 Hearthliner 207 Evaporation Source 208 Electron Beam 209 Shutter 210 Film Thickness Gauge 211 First Drum 212 Second Drum 213 Return Roll 410 Deposition area 510 Passive oxide film 520 Copper ion 530 Copper particles

Claims

1. An aluminum wire made of aluminum or an aluminum alloy; A copper thin film covering the surface of the aluminum wire; Equipped with The copper thin film has a space factor of 0.2% or more and 4% or less. A copper-clad aluminum wire, wherein the adhesion between the aluminum wire and the copper thin film based on a scratch test in accordance with JIS R 3255 is 10 mN or more.

2. 2. The copper-clad aluminum wire according to claim 1, wherein the copper thin film has a space factor of 0.2% or more and less than 1%.

3. 3. The copper-clad aluminum wire according to claim 2, wherein the copper thin film has a space factor of 0.3% or more and 0.55% or less.

4. The copper-clad aluminum wire according to any one of claims 1 to 3, wherein the adhesion satisfies the range of 20 mN or more and 100 mN or less.

5. The copper-clad aluminum wire according to claim 4, wherein the adhesion satisfies the range of 50 mN or more and 100 mN or less.

6. The copper-clad aluminum wire according to any one of claims 1 to 5, wherein the aluminum has a purity in the range of 99.9% or more and 99.99999% or less.

7. The aluminum alloy is an alloy of aluminum (Al) and at least one element selected from the group consisting of magnesium (Mg), iron (Fe), zirconium (Zr), zinc (Zn), chromium (Cr), scandium (Sc), manganese (Mn), boron (B), titanium (Ti), copper (Cu), lithium (Li) and silicon (Si). The copper-clad aluminum wire according to any one of claims 1 to 5.

8. The copper-clad aluminum wire according to any one of claims 1 to 7, wherein the aluminum wire does not have a passive oxide film at the interface between the aluminum wire and the copper thin film.

9. A method for producing a copper-clad aluminum wire by coating an aluminum wire made of aluminum or an aluminum alloy with a copper thin film by an ion plating method, comprising the steps of: In a vacuum chamber equipped with a copper evaporation source, an aluminum wire having an outer diameter of 0.1 mm to 1.5 mm is wound around a first drum, and the aluminum wire is wound around a second drum by cross-rotating through at least a pair of return rolls, and the aluminum wire is placed so that the distance between the aluminum wire passing between the at least a pair of return rolls and the center of the copper evaporation source is 500 mm to 1000 mm; evaporating and ionizing copper from the copper evaporation source by electron beam heating; applying a negative voltage to the first drum and the second drum, the voltage having a magnitude in the range of greater than 10 V to 800 V; the aluminum wire is wound around the second drum while being cross-rotated at a speed of 1 m / min or more and less than 15 m / min via the at least one pair of return rolls from the first drum, and ionized copper ions are caused to collide with the aluminum wire to form a copper thin film; The method includes:

10. 10. The method of claim 9, wherein applying the negative voltage comprises applying a negative voltage having a magnitude in the range of 50V to 700V.

11. 11. The method of claim 10, wherein applying the negative voltage comprises applying a negative voltage having a magnitude in the range of 200V to 700V.

12. The method according to any one of claims 9 to 11, wherein the forming of the copper thin film comprises winding the aluminum wire at a speed of 1 m / min or more and 5 m / min or less.

13. The method according to any one of claims 9 to 12, wherein the aluminium has a purity in the range of 99.9% to 99.99999%.

14. The method according to any one of claims 9 to 12, wherein the aluminum alloy is an alloy of aluminum (Al) and at least one element selected from the group consisting of magnesium (Mg), iron (Fe), zirconium (Zr), zinc (Zn), chromium (Cr), scandium (Sc), manganese (Mn), boron (B), titanium (Ti), copper (Cu), lithium (Li) and silicon (Si).

15. The method according to any one of claims 9 to 14, further comprising cleaning the surface of the aluminum wire by ion bombardment treatment using argon ions prior to evaporating and ionizing the copper.

16. The method according to claim 15 , wherein the ion bombardment process is carried out at a pressure in a vacuum chamber in the range of 1 Pa to 10 Pa.

17. The method of any one of claims 9 to 16, further comprising repeating the forming of the copper thin film.

18. The method according to any one of claims 9 to 17, further comprising drawing the copper-clad aluminum wire obtained by forming the copper thin film.

19. The method according to claim 18, wherein the wire drawing is a drawing process using a carbide die or a diamond die.

20. The method according to claim 19, wherein the copper-clad aluminum wire is annealed at a temperature range of 300° C. to 500° C. for a time period of 1 second to 5 minutes before, after or during the drawing process.

Citation Information

Patent Citations

  • Method and apparatus for manufacturing composite wiry body

    JP1987001850A

  • Composite material for welding and its production

    JP1993285690A

  • Compound lightweight ribbon wire, insulated compound lightweight ribbon wire, and manufacture thereof

    JP2000113730A

  • Lightweight conductor for automobile

    JP2004039477A

  • Wire rod for acoustic purpose, IC, keyless entry system, miniature motor winding, speaker voice coil, transmission line, and electrical machinery component

    JP2005248318A