Solution containing lithium, niobium complex, and hydrazine, method for producing same, and method for producing active material for lithium secondary battery
A solution of lithium, niobium complex, and hydrazine stabilizes the niobium complex, addressing sol formation issues and reducing storage costs, enabling efficient lithium niobate coating for lithium-ion secondary batteries.
Patent Information
- Application Number
- JP2021548842
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-26
- Filing Date
- 2020-09-16
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-09-16
AI Technical Summary
Existing aqueous solutions containing lithium and niobium complexes used for coating lithium-transition metal oxides in lithium-ion secondary batteries face issues such as sol formation, which affects the control of coating amounts and contaminates the lithium-transition metal oxides, and high niobium concentrations lead to increased transportation and storage costs.
A solution containing lithium, niobium complex, and hydrazine is developed, with specific concentration and pH ranges, to stabilize the niobium complex and suppress sol formation, allowing long-term storage and efficient production of a lithium niobate coating for lithium-ion secondary batteries.
The solution effectively suppresses sol formation, enabling stable storage and cost-effective production of lithium niobate coatings for lithium-ion secondary batteries, ensuring long-term stability and reduced contamination.
Smart Images

Figure 0007576557000003 
Figure 0007576557000004 
Figure 0007576557000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a solution containing lithium, a niobium complex, and hydrazine, a method for producing the same, and a method for producing an active material for lithium secondary batteries. [Background technology]
[0002] Recently, all-solid-state lithium-ion secondary batteries that are both high-performance and safe have been actively developed, and various lithium-transition metal oxides have been studied as positive electrode active materials for the all-solid-state lithium-ion secondary batteries.
[0003] Recently, it has been considered to form a coating layer containing lithium niobate on a part or all of the lithium-transition metal oxide particles, and an aqueous solution containing a niobium compound and a lithium compound for forming the coating layer has been researched.
[0004] For example, Patent Document 1 proposes an aqueous solution containing a niobium compound and a lithium compound, which is obtained by mixing an aqueous solution containing a water-soluble peroxo complex of niobic acid with a lithium compound.
[0005] Furthermore, for example, Patent Document 2 proposes an aqueous solution containing lithium and a niobium complex, the aqueous solution having a pH value of 8.0 to 9.9 and an ORP of 30 to 250 mV.
[0006] Furthermore, Non-Patent Document 1 describes an aqueous solution containing lithium and a niobium complex, which relates to a technical field substantially similar to that described in Patent Documents 1 and 2 above. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2012-074240 A [Patent Document 2] JP 2014-210701 A [Non-patent literature]
[0008] [Non-Patent Document 1] Journal of the Ceramic Society of Japan 2004, Vol. 112, No. 1307, p. 368-372 Summary of the Invention [Problem to be solved by the invention]
[0009] According to the study by the present inventors, the aqueous solution containing lithium and a niobium complex described in Patent Document 1 and Non-Patent Document 1 produced a sol containing niobium and oxygen as main components several hours after preparation. When a lithium-transition metal oxide such as lithium cobalt oxide coated with lithium niobate is produced using an aqueous solution containing lithium and a niobium complex from which such a sol has been produced, the amount of lithium niobate coated may decrease, the amount of coating may become difficult to control, and the sol may be mixed into the lithium-transition metal oxide such as lithium cobalt oxide coated with lithium niobate.
[0010] Furthermore, in the aqueous solution containing lithium and a niobium complex described in Patent Document 2, although the generation of precipitates (presumably the above-mentioned sol) is suppressed, the niobium concentration in the aqueous solution is only 1.14 wt %.
[0011] Here, the present inventors have conceived of the usefulness of a solution containing lithium and niobium complexes at high concentrations, from the viewpoint of reducing transportation / storage costs.
[0012] The present invention has been made under the above circumstances, and a problem to be solved by the present invention is to provide a solution containing lithium and a niobium complex, which has a high content of lithium and a niobium complex and can be stored for a long period of time while suppressing the generation of a sol, a method for producing the same, and a method for producing an active material for a lithium ion secondary battery. [Means for solving the problem]
[0013] As a result of intensive research, the present inventors have made the groundbreaking discovery that by adding hydrazine to a solution containing lithium and a niobium complex, the niobium complex can be stabilized, and the generation of a sol can be suppressed in a solution having a high concentration of lithium and niobium complex, thereby obtaining a solution containing lithium, niobium complex, and hydrazine that can be stored for a long period of time, and have completed the present invention.
[0014] That is, the first invention for solving the above-mentioned problems is, A solution containing lithium, a niobium complex, and hydrazine, The solution contains lithium, a niobium complex, and hydrazine, and the niobium concentration in the solution is 2.0 mass % or more. The second invention is The solution according to the first aspect of the present invention is characterized in that the hydrazine content in the solution is 0.0005% by mass or more and 30% by mass or less. The third invention is The solution according to the first or second invention is characterized in that the niobium complex is a peroxo complex of niobic acid. The fourth invention is The solution according to any one of the first to third aspects of the present invention is characterized in that the pH value is 8.0 or more and 12.0 or less, and the redox potential is 0 mV or less and -700 mV or more. The fifth invention is In the solution according to any one of the first to fourth aspects of the present invention, the molar ratio of lithium to 1 mole of niobium (Li / Nb) is 0.9 or more and 1.4 or less. The sixth invention is A solution containing lithium, a niobium complex, and hydrazine, The solution is characterized by a pH value of 8.0 or more and 12.0 or less, and a redox potential of 0 mV or less and -700 mV or more. The seventh invention is The method includes a step of mixing lithium, a niobium complex, and hydrazine to obtain a solution containing lithium, a niobium complex, and hydrazine, The method for producing a solution containing lithium, a niobium complex, and hydrazine, wherein the niobium concentration in the solution is 2.0 mass % or more. The eighth invention is The step of obtaining a solution containing lithium, a niobium complex, and hydrazine includes: adding a lithium compound to a solution containing a niobium complex to obtain a solution containing lithium and a niobium complex; A method for producing a solution according to a seventh aspect of the present invention, further comprising the step of adding hydrazine to the solution containing lithium and a niobium complex. The ninth invention is A step of coating a surface of an active material for a lithium secondary battery with a solution containing the lithium and niobium complex according to any one of the first to sixth aspects of the present invention and hydrazine; and heat-treating the coated active material for lithium secondary batteries. Effect of the Invention
[0015] It was possible to obtain a solution containing lithium and a niobium complex, which has a high concentration of lithium and a niobium complex and can be stored for a long period of time because the formation of a sol is suppressed in the solution. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a plot of Comparative Example 1 and Examples 1 to 5, with the vertical axis representing the oxidation-reduction potential (ORP) [unit: mV] and the horizontal axis representing the pH value of a solution containing lithium and a niobium complex and hydrazine. [Diagram 2] FIG. 2 is a graph showing the results of FT-IR measurement according to Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, embodiments for carrying out the present invention will be described in the following order. In this specification, a solution containing a niobium complex is also called a "complex solution". In the case of an aqueous solution, it is also called an "aqueous complex solution". ·Complex solution containing lithium and niobium complex·Addition of hydrazine to a complex solution containing lithium and niobium complex·Solution containing lithium and niobium complex and hydrazine·pH value of a solution containing lithium and niobium complex and hydrazine·Redox potential of a solution containing lithium and niobium complex·Storage stability of a complex solution with added hydrazine·Coating of the surface of active material for lithium secondary batteries with a solution containing lithium and niobium complex and hydrazine·Heat treatment of the coated active material for lithium secondary batteries Note that "~" indicates a value greater than or equal to a specified value and less than or equal to a specified value.
[0018] (Complex solution containing lithium and niobium complexes) First, a complex solution containing lithium and a niobium complex is prepared by mixing a solution containing a niobium complex, a lithium compound, and an alkali.
[0019] The ligand of the niobium complex is not particularly limited as long as the niobium complex is water-soluble. Among them, the peroxo complex of niobic acid ([Nb(O2)4] 3- The peroxo complex of niobic acid is particularly suitable because it does not contain carbon in its chemical structure and therefore no carbon remains in the coating film of lithium niobate that is finally produced.
[0020] The peroxo complex of niobic acid can be obtained, for example, by the following method. That is, niobic acid (Nb2O5·nH2O) is added to hydrogen peroxide water and mixed. Here, during the mixing, it is preferable that hydrogen peroxide is 8 moles or more per mole of niobic acid. Considering that hydrogen peroxide may decompose during the reaction, it is more preferable that hydrogen peroxide is 10 moles or more per mole of niobic acid. On the other hand, even if the molar ratio of hydrogen peroxide to 1 mole of niobic acid exceeds 20, the effect is considered to be saturated. Therefore, the molar ratio of hydrogen peroxide to 1 mole of niobic acid is preferably 20 or less, and more preferably 15 or less. In this mixing, niobic acid does not dissolve in hydrogen peroxide water, but a milky suspension solution can be obtained. Then, a transparent peroxo complex of niobic acid can be obtained by adding an alkali such as ammonia water to a suspension containing niobic acid and mixing it.
[0021] The amount of alkali to be added to the suspension is not particularly limited as long as it is an amount sufficient to obtain a transparent peroxo complex of niobic acid.
[0022] When ammonia water is added as an alkali to a suspension containing niobic acid, it is preferable to add it so that the molar ratio of ammonia to 1 mole of niobic acid (ammonia / Nb) is 1 or more. Furthermore, considering that ammonia volatilizes during the reaction, it is even more preferable to add it so that the molar ratio of ammonia to 1 mole of niobic acid is 2 or more. On the other hand, it is considered that the effect is saturated even if the molar ratio of ammonia to 1 mole of niobic acid exceeds 6. Therefore, it is preferable to set the molar ratio of ammonia to 1 mole of niobic acid to 6 or less. Furthermore, when an alkali such as ammonia water is added to and mixed with a suspension containing niobic acid, the liquid temperature of the ammonia water or the like is preferably 0° C. or more and 60° C. or less in order to avoid the volatilization of ammonia.
[0023] A complex solution containing lithium and a niobium complex can be obtained by adding a lithium compound to the aqueous solution containing the niobium complex obtained by the above-mentioned method. The amount (molar number) of the lithium compound to be added can be set arbitrarily based on the mole number of niobium contained in the aqueous solution. Suitable examples of the lithium compound to be added include lithium salts such as lithium hydroxide (LiOH), lithium nitrate (LiNO3), lithium sulfate (Li2SO4), and lithium carbonate (Li2CO3).
[0024] (Addition of hydrazine to a complex solution containing lithium and niobium complexes) Next, hydrazine (N2H4) is added to the obtained complex solution containing lithium and niobium complexes. The amount of hydrazine added can be adjusted depending on the desired storage period of the complex solution. The amount of hydrazine added can be adjusted according to the amount of the main component of the lithium and niobium complexes in the complex solution, or it can be determined in advance by adjusting the amount added experimentally.
[0025] Hydrazine may be added to the complex solution containing lithium and a niobium complex as described in the above paragraph. Alternatively, hydrazine may be added when preparing the raw material solution of the complex solution containing lithium and a niobium complex. That is, hydrazine may be added when mixing the solution containing the niobium complex with the lithium compound and the alkali. Hydrazine may also be added to the solution obtained after adding raw materials other than hydrazine. This method can suppress the decomposition of hydrazine to a minimum. That is, it is efficient because only a small amount of hydrazine is added.
[0026] The amount of hydrazine added is in the range of 0.003% by mass to 100% by mass, preferably 0.005% by mass to 50% by mass, and more preferably 0.1% by mass to 10% by mass. By setting the amount of hydrazine added within the above range, the storage stability of the complex solution containing the lithium and niobium complex described below can be improved.
[0027] The form of hydrazine to be added is not particularly limited as long as it is a compound having a hydrazine group, and examples thereof include anhydrous hydrazine, hydrazine hydrate, hydrazine sulfate, hydrazine hydrochloride, and hydrazine carbonate. In this embodiment, it is preferable to use hydrazine hydrate from the viewpoint of ease of handling. When using the above hydrazine compound, the amount of hydrazine to be added is based on the amount of hydrazine groups in the hydrazine compound. Hereinafter, "hydrazine" in this specification is a general term for the above compounds having a hydrazine group.
[0028] (Solution containing lithium and niobium complex and hydrazine) The content of hydrazine in the solution containing lithium, niobium complex, and hydrazine can be measured by gas chromatography. In a solution containing a high concentration of lithium and niobium complex, the generation of sol is suppressed and the solution can be stored for a longer period of time, so the content of hydrazine in the complex solution is preferably in the range of 0.0005% by mass to 30% by mass. More preferably, the content of hydrazine in the complex solution is in the range of 0.0008% by mass to 10% by mass. It is more preferable that the content of hydrazine in the complex solution is 7% by mass or less.
[0029] When the content of hydrazine is 0.0005% by mass or more, the formation of a sol is suppressed in a solution having a high concentration of lithium and niobium complex, and a complex solution containing lithium and niobium complex that can be stored for a long period of time can be stably obtained, which is preferable. Also, even if the content of hydrazine is added in an amount exceeding 30% by mass, the effect is considered to be saturated.
[0030] In the solution containing lithium, a niobium complex, and hydrazine according to the present invention, the niobium concentration is preferably 10% by mass or less. When the niobium concentration is 10% by mass or less, the stability of the niobium complex in the solution containing lithium, a niobium complex, and hydrazine is ensured, and storage stability is also ensured. On the other hand, when the niobium concentration is 2% by mass or more, it is advantageous in terms of cost due to reduced transportation / storage costs.
[0031] In addition, when the niobium concentration is high (specifically, when it is 2.0 mass% or more), even if a large amount of hydrogen peroxide is present in the solution to improve the stability of the niobium complex, the present inventors have found that the large amount of hydrogen peroxide does not contribute much to improving the stability. On the other hand, by adopting the method of the present invention, the generation of a sol is suppressed in a solution containing a high concentration of lithium and a niobium complex without using a large amount of hydrogen peroxide, and long-term storage is possible.
[0032] In the present invention, the term "niobium concentration" means the concentration of niobium element in a solution containing lithium, a niobium complex, and hydrazine.
[0033] In the solution containing lithium, a niobium complex, and hydrazine according to the present invention, the molar ratio of lithium to 1 mole of niobium (Li / Nb) is preferably 0.9 or more and 1.4 or less. This is because, when the molar ratio of lithium to 1 mole of niobium (Li / Nb) is 0.9 or more, when lithium niobate represented by LiNbO3 is formed as a coating layer of the positive electrode active material, lithium is present in sufficient amount, which is preferable, and the lithium ion conductivity of the coating layer is ensured. In addition, when the molar ratio is 0.9 or more, the niobium complex is stabilized because the ratio of the number of moles of the niobium complex (-1 valence) to the number of moles of Li ions (+1 valence) does not require an excess of the niobium complex. On the other hand, when the molar ratio of lithium to 1 mole of niobium (Li / Nb) is 1.4 or less, non-conductive lithium hydroxide is not mixed into the lithium niobate, which is preferable, and the conductivity of lithium ions is ensured. In the solution containing lithium, a niobium complex, and hydrazine according to the present invention, the lithium concentration is preferably 0.13% by mass or more and 1.1% by mass or less.
[0034] (pH value of solution containing lithium and niobium complex and hydrazine) The pH value of the solution containing the lithium and niobium complex and hydrazine obtained by the above method is preferably 8.0 or more and 12.0 or less.
[0035] That is, if the pH value is 8.0 or more, the niobium complex is stable, and the formation of the sol is inhibited, and if the pH value is 12.0 or less, the ammonium niobium complex is not formed because there is no excess ammonia.
[0036] The pH value of the solution containing the lithium and niobium complexes and hydrazine can be adjusted by changing the ratio of the amounts of each substance added during the production of the solution, and in particular, can be adjusted by controlling the amount of alkali such as aqueous ammonia added.
[0037] (Oxidation-reduction potentials of solutions containing lithium and niobium complexes) FIG. 1 is a plot of Comparative Example 1 and Examples 1 to 5, with the vertical axis representing the oxidation-reduction potential (ORP) [unit: mV] and the horizontal axis representing the pH value of a solution containing lithium and a niobium complex and hydrazine.
[0038] As a result of carrying out the tests described in the Examples section below, it was found that as the pH value of a solution containing lithium and niobium complexes and hydrazine increases, the ORP of the solution tends to decrease, as shown in FIG.
[0039] The ORP of the solution containing the lithium-niobium complex and hydrazine obtained by the above method is preferably 0 mV or less and -700 mV or more. It is considered that when the ORP is 0 mV or less, the formation of the sol is suppressed because the colloids such as niobic acid formed are redissolved. When the ORP is -700 mV or more, the amount of hydrazine added is not large, which is economical.
[0040] It is further preferred that the ORP and pH of the solution containing lithium, a niobium complex, and hydrazine have the following relationship: ORP≦-175×pH+1400 (However, ORP must be 0mV or less, -700mV or more, pH must be 8 or more, 12 or less)
[0041] The outlines of various measurements in this embodiment and the examples described later are as follows.
[0042] <Measurement operation of niobium concentration> 0.1 g of the prepared solution containing lithium, niobium complex, and hydrazine was taken, 5 ml of hydrochloric acid and 15 ml of pure water were added, and then 2 ml of hydrogen peroxide solution was added to obtain a solution in which niobium was dissolved. Pure water was added to the obtained solution to make the volume up to 100 ml, and then the solution was diluted 20-fold by adding pure water. The niobium concentration was measured using ICP-AES (Agilent Technologies ICP-720).
[0043] <Measurement operation of lithium concentration> 0.1 g of the prepared solution containing lithium, niobium complex, and hydrazine was taken, 5 ml of hydrochloric acid and 15 ml of pure water were added, and then 2 ml of hydrogen peroxide solution was added to dissolve lithium to obtain a solution. Pure water was added to the obtained solution to make the volume up to 100 ml, and the lithium concentration was measured using ICP-AES (Agilent Technologies ICP-720).
[0044] <Measurement operation of pH and ORP> The pH value of the prepared solution containing lithium, niobium complex, and hydrazine was measured at a temperature of 25 °C using a pH meter (D-51, manufactured by Horiba, Ltd.).
[0045] Also, the oxidation-reduction potential (ORP) of the solution containing lithium, niobium complex, and hydrazine was measured at a temperature of 25 °C using an ORP meter (WM-32EP, manufactured by Toa DKK Corporation). However, for the internal electrode platinum - reference electrode silver chloride, the product name: platinum composite type ORP electrode 9300-10D was used, and the measurement was carried out using a 3.33 mol / L KCl aqueous solution as the internal solution of the reference electrode. Prior to the measurement, it was confirmed that when measuring the ORP standard solution (model number 160-22) manufactured by Horiba, Ltd., it was in the range of 258 mV ± 15 mV.
[0046] <Identification operation of peroxo complex> The peroxo complex in the solution containing the prepared lithium and niobium complexes and hydrazine was identified by FT-IR (NICOLET6700 manufactured by Thermo Fisher Scientific). Here, a single reflection ATR method was used, and the angle of incidence to the germanium prism was 45°. In order to remove the peak on the low wavenumber side of the solvent water, the background was measured using water.
[0047] FIG. 2 is a graph showing the results of FT-IR measurement according to Example 3. To state the results in advance, the measurement showed that the 850 cm -1 ±20cm -1 A peak in the vicinity was confirmed, and it is believed that the dissolved niobium is in the form of a peroxo complex.
[0048] <Quantitative analysis of hydrazine in solution> The amount of hydrazine (wt %) in the prepared solution containing the lithium and niobium complex and hydrazine was measured as follows.
[0049] First, 1.0 g of the solution was weighed out, and hydrazine was converted into a Schiff base using acetone according to the following reaction formula. [ka] The standard sample for quantification was also derivatized in the same manner, a standard solution was prepared, and a calibration curve for the substance on the right side of [Chemical formula 1] was obtained. A chromatogram was obtained using a gas chromatograph (GC-2110, manufactured by Shimadzu Corporation). The calibration curve was used for this chromatogram to quantify the substance on the right side of [Chemical formula 1]. Note that He gas (flow rate 10 mL / min) was used as the carrier gas for the gas chromatograph, the inlet temperature was set to 240°C, and the oven temperature was raised from 40°C at a rate of 10°C / min and maintained at 190°C. The concentration value in the solution of the substance on the right side of [Chemical formula 1] obtained above was taken as the hydrazine content value in the solution containing the lithium and niobium complex and hydrazine.
[0050] (Storage stability of complex solution containing hydrazine) The storage stability of a solution containing lithium, a niobium complex, and hydrazine can be objectively evaluated by measuring the maximum absorbance value in the wavelength range of 400 nm to 700 nm (sometimes referred to as "maximum absorbance" in the present invention).
[0051] That is, if storage stability is guaranteed, the generation of sol is suppressed, and therefore the increase in the maximum absorbance value is suppressed. On the other hand, if there is a problem with storage stability, sol is generated and the maximum absorbance value increases. Therefore, by leaving the solution containing lithium, a niobium complex, and hydrazine to be measured under a predetermined environment for a predetermined period of time and measuring the increase rate of the maximum absorbance value at the beginning and end of the standing, the storage stability of the solution containing lithium, a niobium complex, and hydrazine can be objectively evaluated.
[0052] The inventors have considered the state of use in the market of the solution containing lithium, a niobium complex, and hydrazine and have determined that the storage stability of the solution containing lithium, a niobium complex, and hydrazine is sufficient if the rate of increase in the maximum absorbance value after leaving the solution undisturbed for a predetermined time (60 days) at room temperature of 25° C. in a dark place, “[(maximum absorbance after 60 days of leaving the solution-maximum absorbance at the beginning of leaving the solution) / (maximum absorbance at the beginning of leaving the solution)]×100” is 100% or less.
[0053] <Storage stability of complex solution (absorbance)> 3.5 ml of 100 ml of the solution containing lithium, niobium complex, and hydrazine was dispensed into a quartz cell, and the absorbance was measured in the wavelength range of 400 nm to 700 nm using an ultraviolet-visible spectrophotometer (UV-1800, manufactured by SHIMADZU CORPORATION). The maximum absorbance value was taken as the initial absorbance after standing.
[0054] Next, 100 ml of the solution containing lithium, niobium complex, and hydrazine was left to stand in a dark place at room temperature of 25° C. for a predetermined time (60 days). After that, 3.5 ml of the solution containing lithium, niobium complex, and hydrazine after storage was taken into the quartz cell in which it was stored, and the maximum value of absorbance (maximum absorbance) in the wavelength range of 400 nm to 700 nm was measured, and it was confirmed that the storage stability was sufficient. If there was a precipitate in the solution containing lithium, niobium complex, and hydrazine after storage, it was shaken three times back and forth for one second to disperse the precipitate, and then 3.5 ml was taken into the quartz cell and the maximum value of absorbance (maximum absorbance) in the wavelength range of 400 nm to 700 nm was measured.
[0055] The increase rate (%) of maximum absorbance was calculated using the following formula. "(Maximum absorbance after 60 days of standing - Maximum absorbance at the beginning of standing) / (Maximum absorbance at the beginning of standing) x 100%"
[0056] The initial absorbance of the solution containing lithium, a niobium complex, and hydrazine after standing was the absorbance measured within 2 hours after the preparation of the solution containing lithium, a niobium complex, and hydrazine, because it was confirmed that the absorbance does not change substantially within 2 hours after the preparation of the solution containing lithium, a niobium complex, and hydrazine.
[0057] Furthermore, the storage conditions of the solution containing the lithium, niobium complex, and hydrazine were determined according to the actual storage method, and 50 ml of the solution containing the lithium, niobium complex, and hydrazine was left in a dark place at room temperature of 25°C for a predetermined time (60 days) using a glass container. After that, 3.5 ml of the solution containing the lithium, niobium complex, and hydrazine after storage was taken into a quartz cell, and the maximum value of the absorbance (maximum absorbance) in the wavelength range of 400 nm to 700 nm was measured. The results confirmed that the storage stability was sufficient.
[0058] (Coating treatment of the surface of active material for lithium secondary batteries with a solution containing lithium, niobium complex and hydrazine) The method of coating the surface of the active material for lithium secondary batteries made of lithium-transition metal oxide with the solution containing lithium, a niobium complex, and hydrazine according to the present invention is not particularly limited. However, a preferred coating method is to spray and apply a solution containing lithium, a niobium complex, and hydrazine to the active material powder for lithium secondary batteries while heating the active material powder to about 100°C to 120°C. There is also a method of immersing the active material powder for lithium secondary batteries in a solution containing lithium, a niobium complex, and hydrazine to perform coating. The active material for lithium secondary batteries is not particularly limited, but may be, in addition to lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2) or an active material in which a part of the transition metal of the active material is replaced with Al, Ti, Cr, Fe, Zr, Y, W, Ta, Nb, Mn, or the like, as the same layered rock salt type compound (LiNi 0.95 Al 0.05 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2), and spinel-type compounds such as lithium manganese oxide (LiMnO4) and those in which part of the Mn is replaced by Al, Ti, Cr, Fe, Zr, Y, W, Ta, Nb, Ni, Co, Fe, etc. (LiAl 0.1 Mn 0.9 O4, LiNi 0.5 Mn 1.5 O4, etc.) can be preferably used.
[0059] (Heat treatment of coated active material for lithium secondary batteries) When the above-mentioned coated active material for lithium secondary batteries is used as a positive electrode material for a lithium ion battery, in order to avoid adverse effects on the battery characteristics, the coated active material for lithium secondary batteries is subjected to an appropriate heat treatment for the purpose of decomposing and removing components containing elements such as N (nitrogen) present in the coating layer. Specifically, for example, heat treatment may be performed in air at 120° C. to 350° C. for 1 hour to 10 hours. By this heat treatment, the active material for lithium secondary batteries having a coating layer containing lithium niobate according to the present invention can be produced.
[0060] Therefore, an active material for lithium secondary batteries having a coating film of lithium-metal oxide such as lithium niobate produced by coating the surface of the active material for lithium secondary batteries with a solution containing lithium, a niobium complex, and hydrazine according to the present invention and baking the resulting material is considered to be suitable as a positive electrode active material for all-solid-state lithium batteries.
[0061] Although an embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the spirit of the present invention. EXAMPLES
[0062] The present invention will be described below with reference to more detailed examples, but the present invention is not limited to these examples.
[0063] Example 1 142 g of hydrogen peroxide solution with a concentration of 30 mass% was prepared. 19.3 g of niobic acid (Nb2O5·5.5H2O (Nb2O5 content 68.2%)) was added to this hydrogen peroxide solution. After adding niobic acid, the temperature of the liquid with added niobic acid was adjusted so that it was in the range of 20℃ to 30℃. 29 g of ammonia water with a concentration of 28 mass% was added to this liquid with added niobic acid, and the mixture was thoroughly stirred to obtain a transparent solution.
[0064] Next, 4.35 g of lithium hydroxide monohydrate (LiOH·H2O) was added to the obtained transparent solution in a nitrogen gas atmosphere to obtain a transparent aqueous solution containing lithium and niobium complexes. Finally, pure water was added to adjust the concentration so that the total weight became 145 g. The pH value and redox potential of the aqueous solution were measured, and the pH value was 8.9 and the redox potential was 320 mV (this value corresponds to Comparative Example 1 described later).
[0065] 100 g of the resulting aqueous complex solution containing lithium and a niobium complex was taken, and 0.0125 g of hydrazine hydrate (N2H4 concentration: 51.1 wt%) was added with stirring to obtain an aqueous complex solution containing lithium, a niobium complex, and hydrazine.
[0066] Table 1 shows the niobium concentration, amount of hydrazine added, pH value, redox potential, amount of hydrazine in the solution, and storage stability (maximum absorbance) of the complex aqueous solution containing lithium, niobium complex, and hydrazine in each of the Examples and Comparative Examples.
[0067] [Table 1]
[0068] In addition, Fig. 1 shows the relationship between the oxidation-reduction potential (ORP) [unit: mV] on the vertical axis and the pH value of the solution containing lithium, a niobium complex, and hydrazine on the horizontal axis for Comparative Example 1 and Examples 1 to 5. As shown in Fig. 1, as the pH value of the solution containing lithium, a niobium complex, and hydrazine increases, the ORP of the solution decreases. All of the examples fall within the range of the preferred relationship between the ORP and the pH value described in this embodiment.
[0069] Example 2 An aqueous complex solution containing a lithium and niobium complex and hydrazine was obtained in the same manner as in Example 1, except that the amount of hydrazine hydrate added was 0.125 g.
[0070] Example 3 An aqueous complex solution containing a lithium and niobium complex and hydrazine was obtained in the same manner as in Example 1, except that the amount of hydrazine hydrate added was 1.25 g.
[0071] Example 4 An aqueous complex solution containing a lithium and niobium complex and hydrazine was obtained in the same manner as in Example 1, except that the amount of hydrazine hydrate added was 6.25 g.
[0072] Example 5 An aqueous complex solution containing a lithium and niobium complex and hydrazine was obtained in the same manner as in Example 1, except that the amount of hydrazine hydrate added was 12.5 g.
[0073] Comparative Example 1 An aqueous complex solution containing lithium and a niobium complex was obtained in the same manner as in Example 1, except that hydrazine hydrate was not added.
[0074] (result) In Comparative Example 1, the increase rate of the maximum absorbance exceeded 100%, while in each Example, the increase rate could be kept low. In other words, in each Example, the formation of a sol was suppressed in a solution containing a high concentration of lithium and niobium complex, and a complex solution containing lithium and niobium complexes was obtained that could be stored for a long period of time.
Claims
1. A solution containing lithium, a niobium complex which is a peroxo complex of niobic acid, and hydrazine, A solution containing lithium, a niobium complex, and hydrazine, the solution having a niobium concentration of 2.0 mass% or more.
2. 2. The solution according to claim 1, wherein the hydrazine content in the solution is from 0.0005% by mass to 30% by mass.
3. 3. The solution according to claim 1, wherein the pH value is 8.0 or more and 12.0 or less, and the redox potential is 0 mV or less and -700 mV or more.
4. 4. The solution according to claim 1, wherein the molar ratio of lithium to 1 mole of niobium (Li / Nb) is 0.9 or more and 1.4 or less.
5. A solution containing lithium, a niobium complex which is a peroxo complex of niobic acid, and hydrazine, A solution having a pH value of 8.0 or more and 12.0 or less, and an oxidation-reduction potential of 0 mV or less and -700 mV or more.
6. The method includes a step of mixing a niobium complex, which is a peroxo complex of lithium and niobic acid, with hydrazine to obtain a solution containing lithium, the niobium complex, and hydrazine; A method for producing a solution containing lithium, a niobium complex, and hydrazine, the solution having a niobium concentration of 2.0 mass% or more.
7. The step of obtaining a solution containing lithium, a niobium complex which is a peroxo complex of niobic acid, and hydrazine includes the steps of: adding a lithium compound to a solution containing a niobium complex to obtain a solution containing lithium and a niobium complex; 7. The method of claim 6, further comprising the step of adding hydrazine to the solution containing the lithium and niobium complex.
8. A step of coating a surface of an active material for a lithium secondary battery with a solution containing a niobium complex which is a peroxo complex of lithium and niobic acid according to any one of claims 1 to 5 and hydrazine; and heat-treating the coated active material for lithium secondary batteries.
Citation Information
Patent Citations
Method for preparing niobium-tungsten-tantalum doped lithium cobalt oxide
CN108682848A
Lithium-transition metal oxide powder and manufacturing method thereof, cathode active material for lithium ion battery, and lithium ion secondary battery
JP2012074240A
Active material, method for manufacturing active material, electrode, and lithium ion secondary battery
JP2012212636A
Solution containing lithium and niobium complex, and method of producing the same
JP2014210701A
Solution containing lithium and niobium complex, method for producing the same, and lithium ion battery
JP2015103321A