Solid electrolyte composition and method for producing solid electrolyte member
The use of an ionic bonding solid electrolyte material with specific organic solvents and solvent removal process addresses conductivity deterioration, resulting in high-performance solid electrolyte membranes for all-solid-state batteries.
Patent Information
- Application Number
- JP2020562892
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-17
- Filing Date
- 2019-11-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2039-11-08
AI Technical Summary
Existing solid electrolytes in all-solid-state batteries face issues with deterioration of ionic conductivity due to the use of organic solvents, which are necessary for preparing fluid compositions, and there is a need for a solid electrolyte material with high ionic conductivity that does not contain sulfur to avoid toxic hydrogen sulfide generation and improve safety.
A solid electrolyte composition comprising an ionic bonding solid electrolyte material without sulfur, combined with an organic solvent containing functional groups like ether, halogen, or Si-O-C groups, which is then processed to remove the solvent, resulting in a solid electrolyte member with enhanced lithium ion conductivity.
The method maintains high lithium ion conductivity and prevents deterioration, enabling the formation of dense, pinhole-free solid electrolyte membranes with improved charge/discharge efficiency in all-solid-state batteries.
Smart Images

Figure 0007576743000004 
Figure 0007576743000005 
Figure 0007576743000006
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a solid electrolyte composition for use in, for example, the manufacture of an all-solid-state battery, and a method for producing a solid electrolyte member. [Background technology]
[0002] Patent Document 1 discloses a halide solid electrolyte. Patent Document 2 discloses a sulfide solid electrolyte. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2018 / 025582 [Patent Document 2] International Publication No. 2018 / 168505 Summary of the Invention [Problem to be solved by the invention]
[0004] In the prior art, it is desirable to suppress the deterioration of the ionic conductivity of the solid electrolyte material in a solid electrolyte composition. [Means for solving the problem]
[0005] One aspect of the present disclosure is Halides A solid electrolyte material and an organic solvent are included, The halide solid electrolyte material has the composition formula Li α M β X γ wherein α, β, and γ are each independently a value greater than 0; M is at least one selected from the group consisting of metal elements and metalloid elements other than Li; and X is at least one selected from the group consisting of Cl, Br, and I; The present invention relates to a solid electrolyte composition, wherein the organic solvent contains at least one selected from the group consisting of a compound having a functional group and a hydrocarbon, and the functional group is at least one selected from the group consisting of an ether group, a halogen group, and a Si-OC group.
[0006] Another aspect of the present disclosure relates to a method for producing a solid electrolyte member, the method including a removal step of removing the organic solvent from the solid electrolyte composition. Effect of the Invention
[0007] By using the solid electrolyte composition according to the present disclosure, Halides This can suppress the deterioration of the ionic conductivity of the solid electrolyte material. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic diagram showing a method for evaluating the lithium ion conductivity of a solid electrolyte material. [Diagram 2] 1 is a graph showing the relationship between the polar term of the Hansen solubility parameter of an organic solvent and the lithium ion conductivity of LYBC after vacuum drying in embodiment 1. [Diagram 3] 1 is a graph showing the particle size distribution of LYBC in an organic solvent in embodiment 1. [Figure 4] 10 is a flowchart showing an example of a method for producing a solid electrolyte member according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. <Inventor's viewpoint> In the field of secondary batteries, where high energy density and large capacity are required, the mainstream approach has been to use an organic electrolyte solution in which an electrolyte salt is dissolved in an organic solvent. In secondary batteries using an organic electrolyte solution, there is a concern about leakage, and it has also been pointed out that the amount of heat generated may be large if a short circuit occurs.
[0010] On the other hand, all-solid-state secondary batteries that use inorganic solid electrolytes instead of organic electrolytes are gaining attention. All-solid-state secondary batteries do not leak and the inorganic solid electrolyte is not flammable, so it is expected that heat generation in the event of a short circuit or the like will be suppressed.
[0011] Inorganic solid electrolytes used in all-solid-state secondary batteries can be roughly divided into sulfide-based solid electrolytes containing sulfur as a main component and oxide-based solid electrolytes containing metal oxide as a main component. However, sulfide-based solid electrolytes have the disadvantage of generating toxic hydrogen sulfide when reacting with moisture, and oxide-based solid electrolytes have the disadvantage of low ionic conductivity. Therefore, there is a need to develop new solid electrolyte materials with high ionic conductivity.
[0012] As a new solid electrolyte material, for example, an ion-bonded solid electrolyte material consisting of lithium, yttrium, and at least one halogen element, and not containing sulfur, is expected. In order to put an all-solid-state secondary battery using an ion-bonded solid electrolyte material into practical use, a technique is required to prepare a composition having flowability containing the ion-bonded solid electrolyte material and coat it on the surface of an electrode or a current collector to form a solid electrolyte member.
[0013] To prepare a composition having fluidity, it is necessary to mix the ion-bonded solid electrolyte material with an organic solvent. Therefore, the inventors have investigated the resistance of the ion-bonded solid electrolyte material to various organic solvents using lithium ion conductivity as an index. As a result, it has been found that the lithium ion conductivity of the ion-bonded solid electrolyte material may decrease when an organic solvent is mixed with the ion-bonded solid electrolyte material. For example, even if an organic solvent can be used for a sulfide-based solid electrolyte, it may not be usable for an ion-bonded solid electrolyte material. From the above viewpoints, the configuration of the present disclosure has been obtained.
[0014] (Embodiment 1) The solid electrolyte composition in the first embodiment contains an ionically bonded solid electrolyte material that does not contain elemental sulfur and an organic solvent.
[0015] The ion-bonded solid electrolyte material may be a solid electrolyte material having ion-bonding and ion-conductivity. In general, a bond between atoms with a large difference in electronegativity is called an ionic bond. For example, the electronegativity of metal elements tends to be small, while the electronegativity of nonmetal elements tends to be large. Here, the ion-bonded solid electrolyte material may be, for example, a solid electrolyte material having a bond between a metal element other than lithium and a nonmetal element.
[0016] The organic solvent contains at least one selected from the group consisting of compounds having a functional group and hydrocarbons, provided that the functional group is at least one selected from the group consisting of an ether group, a halogen group, and a Si-OC group.
[0017] The hydrocarbon is a compound consisting of only carbon and hydrogen, and may be any of aliphatic hydrocarbons, alicyclic hydrocarbons, and aromatic hydrocarbons. From the viewpoint of increasing the dispersibility of the solid electrolyte material in the solid electrolyte composition, aromatic hydrocarbons are preferable. The hydrocarbon may be a saturated hydrocarbon or an unsaturated hydrocarbon. In addition, the compound having a functional group may be composed of only carbon and hydrogen in a portion other than the functional group. That is, the compound having a functional group may have a structure in which at least one hydrogen atom of the hydrocarbon is substituted with at least one selected from the group consisting of an ether group, a halogen group, and a Si-OC group.
[0018] More specifically, the organic solvent may contain at least one selected from the group consisting of hydrocarbons, halogenated hydrocarbons, ethers, and silyl ethers. The silyl ether may be an alkoxysilane. The number of ether groups contained in the organic solvent molecule is not particularly limited, but the number of ether groups contained in the organic solvent molecule may be, for example, one. The boiling point of the organic solvent is not particularly limited, but may be, for example, 200°C or higher. In addition, the organic solvent may be a liquid that can disperse the ion-bonded solid electrolyte material, and does not need to dissolve the ion-bonded solid electrolyte material.
[0019] According to the above-mentioned configuration, it is possible to provide a solid electrolyte composition with little deterioration in ion conductivity. That is, when the organic solvent is removed by drying from a solid electrolyte composition containing an ion-bonded solid electrolyte material (non-sulfide solid electrolyte material) not containing elemental sulfur and an organic solvent, a solid electrolyte member (e.g., a solid electrolyte membrane) having excellent ion conductivity can be obtained.
[0020] The ionically bonded solid electrolyte material may have, for example, lithium ion conductivity.
[0021] The ionically bonded solid electrolyte material may contain at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb, and Sm. These elements can generate cations in water.
[0022] The ion-bonded solid electrolyte material may further contain, for example, at least one halogen element selected from the group consisting of Cl, Br, I and F. These elements can generate anions in water.
[0023] The solid electrolyte composition having the above-mentioned structure is more likely to suppress the deterioration of lithium ion conductivity, and therefore a solid electrolyte member having higher lithium ion conductivity can be produced.
[0024] The ion-bonded solid electrolyte material contains Li and at least one selected from the group consisting of Gd, Ca, Zr, and Y, and may also contain at least one selected from the group consisting of Cl, Br, I, and F.
[0025] The solid electrolyte composition having the above-mentioned structure is more likely to suppress the deterioration of lithium ion conductivity, and therefore a solid electrolyte member having higher lithium ion conductivity can be produced.
[0026] The ion-bonded solid electrolyte material may be a material containing Li and Y and also containing at least one element selected from the group consisting of Cl, Br, I and F.
[0027] More specifically, the ion-bonded solid electrolyte material may be a material containing Li, Y, Cl, and Br, a material containing Li, Ca, Y, Gd, Cl, and Br, or a material containing Li, Zr, Y, and Cl.
[0028] More specifically, the ion-bonded solid electrolyte material is Li3YBr2Cl4, Li 2.8 Ca 0.1 Y 0.5 Gd 0.5 Br2Cl4, or Li 2.5 Y 0.5 Zr 0.5 It may also be Cl6.
[0029] In addition, the ion-bonded solid electrolyte material may be a material consisting essentially of Li, at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb, and Sm, and at least one element selected from the group consisting of Cl, Br, I, and F.
[0030] In this specification, "consisting essentially of Li, at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb, and Sm, and at least one element selected from the group consisting of Cl, Br, I, and F" means "containing only Li and an element selected from each group, excluding unavoidable impurities that are unintentionally mixed in." Therefore, for example, "consisting essentially of only Li, Y, Cl, and Br" means "containing only Li, Y, Cl, and Br, excluding unavoidable impurities that are unintentionally mixed in." Hereinafter, similar expressions shall have the same meaning. An example of an unavoidable impurity is the oxygen element.
[0031] The ion-bonded solid electrolyte material may be a material consisting essentially of Li, Y, Cl, and Br. The ion-bonded solid electrolyte material may be a material consisting essentially of Li, Ca, Y, Gd, Cl, and Br. The ion-bonded solid electrolyte material may be a material consisting essentially of Li, Zr, Y, and Cl.
[0032] When the organic solvent is a compound having a functional group, the compound having a functional group may not substantially contain functional groups other than ether groups and halogen groups. The dispersibility of the ion-bonded solid electrolyte material in such an organic solvent is good. In particular, the dispersibility of the ion-bonded solid electrolyte material, which is a halide (hereinafter also referred to as a halide solid electrolyte material), in the above organic solvent is good. By using a solid electrolyte composition having excellent dispersibility, a solid electrolyte member having excellent lithium ion conductivity and a denser structure can be formed. For example, a dense solid electrolyte film with few pinholes, irregularities, etc. can be easily formed.
[0033] The organic solvent may include a ring structure. The dispersibility of the ion-bonded solid electrolyte material in an organic solvent including a ring structure is good, and the dispersibility of the halide solid electrolyte material is particularly good. The ring structure may be an aromatic ring structure. That is, the organic solvent may be an aromatic compound. The dispersibility of the ion-bonded solid electrolyte material in an aromatic compound is good, and the dispersibility of the halide solid electrolyte material is particularly good.
[0034] More specifically, the organic solvent may include at least one selected from the group consisting of tetralin, ethylbenzene, mesitylene, pseudocumene, xylene, cumene, dibutyl ether, anisole, 1,2,4-trichlorobenzene, chlorobenzene, 2,4-dichlorobenzene, o-chlorotoluene, 1,3-dichlorobenzene, p-chlorotoluene, 1,2-dichlorobenzene, 1,4-dichlorobutane, 3,4-dichlorotoluene, and tetraethyl orthosilicate. The dispersibility of the ionic solid electrolyte material in these organic solvents is very good, and the dispersibility of the halide solid electrolyte material is particularly good.
[0035] The halide solid electrolyte material may be, for example, a material represented by the composition formula (1): Li α M β X γ Here, α, β, and γ are each independently a value greater than 0, M is at least one selected from the group consisting of metal elements and metalloid elements other than Li, and X is at least one selected from the group consisting of Cl, Br, and I.
[0036] The term "metalloid element" as used herein means at least one selected from the group consisting of B, Si, Ge, As, Sb and Te.
[0037] As used herein, the term "metal element" includes (i) all elements in Groups 1 to 12 of the periodic table (excluding hydrogen) and (ii) all elements in Groups 13 to 16 of the periodic table (excluding B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se). Metal elements form inorganic compounds with halide ions to become cations.
[0038] In the compositional formula (1), M may contain Y (i.e., yttrium). That is, the halide solid electrolyte material may contain Y as the metal element M. Since the halide solid electrolyte material has excellent ionic conductivity, all-solid-state batteries using the halide solid electrolyte material can exhibit excellent charge and discharge efficiency.
[0039] Specific examples of the halide solid electrolyte material containing Y include Li a Me b Y c Compounds represented by the compositional formula X6 (where a + mb + 3c = 6, c > 0, Me is at least one selected from the group consisting of metal elements and metalloid elements other than Li and Y, and m is the valence of Me) can be mentioned.
[0040] Me is, for example, at least one selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta, and Nb. In this case, the ionic conductivity of the halide solid electrolyte material can be further increased.
[0041] The halide solid electrolyte material may be a material represented by the compositional formula (A1): Li 6-3d Y d X6 Here, X is one or more elements selected from the group consisting of Cl, Br, and I. The compositional formula (A1) may satisfy 0 < d < 2.
[0042] The compositional formula (A1) may satisfy d = 1. That is, the halide solid electrolyte material may be a material represented by the compositional formula (A2): Li3YX6 Here, X is one or more elements selected from the group consisting of Cl, Br, and I. The compositional formula (A1) may satisfy 0 < d < 2.
[0043] The halide solid electrolyte material may be a material represented by the compositional formula (A3): Li 3-3δ Y 1+δ Cl6 It may be a material represented by. The compositional formula (A3) may satisfy 0 < δ ≦ 0.15.
[0044] The halide solid electrolyte material has a compositional formula (A4): Li 3-3δ Y 1+δ Br6 It may be a material represented by. The compositional formula (A4) may satisfy 0 < δ ≦ 0.25.
[0045] The halide solid electrolyte material has a compositional formula (A5): Li 3-3δ+a Y 1+δ-a Me a Cl 6-x-y Br x I y It may be a material represented by. Here, Me may be at least one selected from the group consisting of Mg, Ca, Sr, Ba, and Zn. In the compositional formula (A5), for example, -1 < δ < 2, 0 < a < 3, 0 < (3 - 3δ + a), 0 < (1 + δ - a), 0 ≦ x ≦ 6, 0 ≦ y ≦ 6, and (x + y) ≦ 6 are satisfied.
[0046] The halide solid electrolyte material has a compositional formula (A6): Li 3-3δ Y 1+δ-a Me a Cl 6-x-y Br x I y It may be a material represented by. Here, Me may be at least one selected from the group consisting of Al, Sc, Ga, and Bi. In the compositional formula (A6), for example, -1 < δ < 1, 0 < a < 2, 0 < (1 + δ - a), 0 ≦ x ≦ 6, 0 ≦ y ≦ 6, and (x + y) ≦ 6 are satisfied.
[0047] The halide solid electrolyte material has a compositional formula (A7): Li 3-3δ-a Y 1+δ-a Me a Cl 6-x-y Br x I y It may be a material represented by the following. Here, Me may be at least one selected from the group consisting of Zr, Hf, and Ti. In the compositional formula (A7), for example, -1 < δ < 1, 0 < a < 1.5, 0 < (3 - 3δ - a), 0 < (1 + δ - a), 0 ≤ x ≤ 6, 0 ≤ y ≤ 6, and (x + y) ≤ 6 are satisfied.
[0048] The halide solid electrolyte material may be a material represented by the compositional formula (A8): Li 3-3δ-2a Y 1+δ-a Me a Cl 6-x-y Br x I y It may be a material represented by the following. Here, Me may be at least one selected from the group consisting of Ta and Nb. In the compositional formula (A8), for example, -1 < δ < 1, 0 < a < 1.2, 0 < (3 - 3δ - 2a), 0 < (1 + δ - a), 0 ≤ x ≤ 6, 0 ≤ y ≤ 6, and (x + y) ≤ 6 are satisfied.
[0049] The halide solid electrolyte materials of the compositional formulas (A1) to (A8) have high ionic conductivity. Therefore, an all-solid-state battery using the halide solid electrolyte materials of the compositional formulas (A1) to (A8) can exhibit excellent charge and discharge efficiency.
[0050] (Embodiment 2) Hereinafter, Embodiment 2 will be described. The same descriptions as those in Embodiment 1 described above will be omitted as appropriate. FIG. 4 is a flowchart showing an example of a method for manufacturing a solid electrolyte member in Embodiment 2.
[0051] The method for manufacturing a solid electrolyte member in Embodiment 2 includes a removal step S1000 of removing an organic solvent from the solid electrolyte composition in Embodiment 1 described above. Here, the solid electrolyte member is a member containing an ionically bonded solid electrolyte material. The solid electrolyte member may be, for example, a solid electrolyte layer or a solid electrolyte film containing an ionically bonded solid electrolyte material, an electrode layer containing an ionically bonded solid electrolyte material, or the like.
[0052] By removing the organic solvent from a solid electrolyte composition containing an ionically bonded solid electrolyte material not containing elemental sulfur and an organic solvent, a solid electrolyte member having high lithium ion conductivity, such as a homogeneous solid electrolyte membrane, can be produced.
[0053] In the removal step S1000, the organic solvent is removed from the solid electrolyte composition. At this time, the organic solvent may be removed by drying under reduced pressure. The solid electrolyte composition before the organic solvent is removed has fluidity, and therefore can form a coating film having excellent moldability and, for example, excellent thickness uniformity. By drying such a coating film, for example, a dense solid electrolyte film having few pinholes, unevenness, etc. can be easily obtained.
[0054] The vacuum drying refers to removing the organic solvent from the solid electrolyte composition in a pressure atmosphere lower than atmospheric pressure. The pressure atmosphere lower than atmospheric pressure may be, for example, -0.01 MPa or less in gauge pressure, and vacuum drying may be performed. The vacuum drying refers to removing the organic solvent from the solid electrolyte composition at a pressure equal to or lower than the vapor pressure at a temperature 20°C lower than the boiling point of the organic solvent. During the vacuum drying, the solid electrolyte composition or the solid electrolyte member may be heated to, for example, 50°C or higher and 250°C or lower.
[0055] The details of the present disclosure will be described below based on examples with reference to Tables 1, 2 and 3. Table 1 shows the results of measuring the lithium ion conductivity of a solid electrolyte member formed from a solid electrolyte composition containing an organic solvent and an ion-bonded solid electrolyte material represented by the composition formula Li3YBr2Cl4 (hereinafter referred to as LYBC) or a sulfide solid electrolyte material represented by the composition formula Li2S-P2S5 (hereinafter referred to as LPS). Table 2 shows the results of measuring the lithium ion conductivity of a solid electrolyte member formed from a solid electrolyte composition containing an organic solvent and an ion-bonded solid electrolyte material represented by the composition formula Li 2.8 Ca 0.1 Y 0.5 Gd 0.5Br2Cl4 (hereinafter referred to as LCYGBC) and an ion-bonded solid electrolyte material represented by the formula Li 2.5 Y 0.5 Zr 0.5 The results of measuring the lithium ion conductivity of a solid electrolyte member formed from a solid electrolyte composition containing an ion-bonded solid electrolyte material represented by Cl6 (hereinafter referred to as LYZC) are shown in Tables 1, 2, and 3. The names of the organic solvents contained in the solid electrolyte composition, the polarization terms of the Hansen solubility parameters δ p The skeletal structure, substituents, and boiling points, as well as the lithium ion conductivity of LYBC, LPS, and LCYGBC and LYZC are shown. In Table 1, the symbols A1 to A18 correspond to Examples 1 to 18, B1 to B14 correspond to Comparative Examples 1 to 14, and C1 corresponds to a reference example. In Table 2, the symbols A19 to A25 correspond to Examples 19 to 25, and C2 corresponds to a reference example. In Table 3, the symbol A26 corresponds to Example 26, and C3 corresponds to a reference example.
[0056] [Table 1]
[0057] [Table 2]
[0058] [Table 3]
[0059] (Preparation of Solid Electrolyte Composition) 300 mg of LYBC was weighed out in a commercially available glass screw tube. 150 mg of organic solvent was weighed out and added thereto, and the mixture was stirred and mixed with a spatula to prepare a solid electrolyte composition. 150 mg of LPS was weighed out and stirred and mixed in the same manner as for 150 mg of organic solvent to prepare a solid electrolyte composition. 300 mg of LCYGBC and LYZC were weighed out and stirred and mixed in the same manner as for 150 mg of organic solvent to prepare a solid electrolyte composition.
[0060] (Removal of organic solvents by vacuum drying) The lithium ion conductivity of the powder of the solid electrolyte material obtained by removing the organic solvent from the solid electrolyte composition by vacuum drying was evaluated. The temperature of the solid electrolyte material was kept at 150°C, and the pressure was reduced for one hour in an atmosphere at a pressure equal to or lower than the vapor pressure of each organic solvent at a temperature 20°C lower than the boiling point of the organic solvent.
[0061] (Measurement of lithium ion conductivity) The lithium ion conductivity of the powder of the solid electrolyte material obtained by the above operation was measured using a pressure molding die 200. The pressure molding die 200 is composed of a frame 201 made of electronically insulating polycarbonate, and an upper punch 203 and a lower punch 202 made of stainless steel.
[0062] Using the pressure molding die shown in FIG. 1, the ionic conductivity was evaluated by the following method. A powder 100 of a solid electrolyte material obtained by vacuum drying a solid electrolyte composition in a dry atmosphere with a dew point of -30°C or less was filled into a pressure molding die 200 and uniaxially pressed at 400 MPa to prepare a conductivity measurement cell.
[0063] While still in the pressurized state, conductors were routed from each of the upper punch 203 and the lower punch 202 and connected to a potentiostat (Princeton Applied Research, VersaSTAT4) equipped with a frequency response analyzer, and the lithium ion conductivity at 25°C was measured by electrochemical impedance measurement.
[0064] <Example 1> A solid electrolyte composition was prepared by the above-mentioned method using tetralin, an aromatic hydrocarbon, as an organic solvent and LYBC or LPS as a solid electrolyte material. The organic solvent, tetralin, was then removed by the above-mentioned vacuum drying.
[0065] The lithium ion conductivity of LYBC and LPS from which tetralin had been removed was measured by the method described above. The lithium ion conductivity of LYBC was 1.7 × 10 -3 S / cm, LPS was 7.8 × 10 -4 S / cm.
[0066] The solid electrolyte materials of LYBC and LPS that had not been mixed with an organic solvent were dried in a vacuum as described above, and the lithium ion conductivity was measured by the method described above. The lithium ion conductivity of LYBC was 1.9 × 10 -3 S / cm, LPS was 8.0 × 10 -4 These are shown at the end of Table 1 as Reference Example (C1).
[0067] When the lithium ion conductivity of the LYBC of Example 1 was compared with that of the LYBC of the Reference Example, there was no deterioration of the LYBC due to tetralin, and the lithium ion conductivity was almost the same as that of the Reference Example.
[0068] <Example 2> The same procedure as in Example 1 was carried out except that ethylbenzene, an aromatic hydrocarbon, was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which ethylbenzene had been removed was measured. As a result, the lithium ion conductivity of LYBC was 1.9 × 10 -3 S / cm, LPS was 7.7 × 10 -4 There was no degradation of LYBC due to ethylbenzene, and the lithium ion conductivity was almost the same as that of the reference example.
[0069] <Example 3> The same procedure as in Example 1 was carried out except that mesitylene, an aromatic hydrocarbon, was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which mesitylene had been removed was measured. The lithium ion conductivity of LYBC was 1.9 × 10 -3 S / cm, LPS was 7.9 × 10 -4 There was no degradation of LYBC due to mesitylene, and the lithium ion conductivity was almost the same as that of the reference example.
[0070] <Example 4> The same procedure as in Example 1 was carried out except that pseudocumene, an aromatic hydrocarbon, was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which pseudocumene had been removed was measured. As a result, the lithium ion conductivity of LYBC was 1.3 × 10 -3 S / cm, LPS was 7.9 × 10 -4 There was no degradation of LYBC due to pseudocumene, and the lithium ion conductivity was almost the same as that of the reference example.
[0071] <Example 5> The same procedure as in Example 1 was carried out except that xylene, an aromatic hydrocarbon, was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which xylene had been removed was measured. As a result, the lithium ion conductivity of LYBC was 1.9 × 10 -3 S / cm, LPS was 7.9 × 10 -4 There was no degradation of LYBC due to xylene, and the lithium ion conductivity was almost the same as that of the reference example.
[0072] <Example 6> The same procedure as in Example 1 was carried out except that cumene, an aromatic hydrocarbon, was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which cumene had been removed was measured. As a result, the lithium ion conductivity of LYBC was 1.2 × 10 -3 S / cm, LPS was 7.4 × 10 -4 There was no degradation of LYBC by cumene, and the lithium ion conductivity was almost the same as that of the reference example.
[0073] As described in Examples 1 to 6, the solid electrolyte composition using an aromatic hydrocarbon organic solvent and LYBC can maintain high lithium ion conductivity.
[0074] The present invention can be carried out in the same manner as above, even when a hydrocarbon other than that shown in the examples is used as the organic solvent. However, in consideration of the application of the solid electrolyte composition and the removal of the organic solvent by vacuum drying, it is preferable to use a hydrocarbon that is liquid at room temperature and has a boiling point of 250° C. or less. The hydrocarbon may be used alone or in combination of two or more kinds.
[0075] Furthermore, although LYBC was used as the solid electrolyte material, other ionic solid electrolyte materials not containing sulfur element may be used.
[0076] Furthermore, other ion-bonded solid electrolyte materials can be similarly implemented as long as they have lithium ion conductivity, and contain at least one selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb, and Sm, and contain at least one selected from the group consisting of Cl, Br, I, and F, and do not contain sulfur element. One type of ion-bonded solid electrolyte material may be used alone, or multiple types may be used in combination.
[0077] <Example 7> The same procedure as in Example 1 was carried out except that dibutyl ether having an ether group was used as the organic solvent, and the lithium ion conductivity of LYBC and LPS from which dibutyl ether had been removed was measured. As a result, the lithium ion conductivity of LYBC was 1.4 × 10 -3 S / cm, LPS was 8.0 × 10 -4 There was no deterioration of LYBC due to dibutyl ether, and the lithium ion conductivity was almost the same as that of the reference example.
[0078] <Example 8> The same procedure as in Example 1 was carried out except that anisole, an aromatic compound having an ether group, was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which anisole had been removed was measured. The lithium ion conductivity of LYBC was 1.9 × 10 -3 S / cm, LPS was 8.0 × 10 -4 There was no degradation of LYBC due to anisole, and the lithium ion conductivity was almost the same as that of the reference example.
[0079] <Example 9> The same procedure as in Example 1 was carried out except that 1,2,4-trichlorobenzene, an aromatic compound having a chloro group, was used as the organic solvent. The lithium ion conductivity of LYBC from which 1,2,4-trichlorobenzene had been removed was measured. The lithium ion conductivity of LYBC was 1.7×10 -3 There was no degradation of the LYBC due to 1,2,4-trichlorobenzene, and the lithium ion conductivity was almost the same as that of the reference example.
[0080] <Example 10> The same procedure as in Example 1 was carried out except that chlorobenzene, an aromatic compound having a chloro group, was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which chlorobenzene had been removed was measured. As a result, the lithium ion conductivity of LYBC was 1.8 × 10 -3 S / cm, LPS was 7.9 × 10 -4 There was no degradation of the LYBC due to chlorobenzene, and the lithium ion conductivity was almost the same as that of the reference example.
[0081] <Example 11> The same procedure as in Example 1 was carried out except that 2,4-dichlorotoluene, an aromatic compound having a chloro group, was used as the organic solvent. The lithium ion conductivity of LYBC from which 2,4-dichlorotoluene had been removed was measured, and it was found to be 1.7×10 -3 There was no degradation of LYBC due to 2,4-dichlorotoluene, and the lithium ion conductivity was almost the same as that of the reference example.
[0082] <Example 12> The same procedure as in Example 1 was carried out except that o-chlorotoluene, an aromatic compound having a chloro group, was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which o-chlorotoluene had been removed was measured. The lithium ion conductivity of LYBC was 1.6 × 10 -3 S / cm, LPS was 7.9 × 10 -4 There was no degradation of LYBC due to o-chlorotoluene, and the lithium ion conductivity was almost the same as that of the reference example.
[0083] <Example 13> The same procedure as in Example 1 was carried out except that 1,3-dichlorobenzene, an aromatic compound having a chloro group, was used as the organic solvent. The lithium ion conductivity of LYBC from which 1,3-dichlorobenzene had been removed was measured. The lithium ion conductivity of LYBC was 1.7 × 10 -3 There was no degradation of the LYBC due to 1,3-dichlorobenzene, and the lithium ion conductivity was almost the same as that of the reference example.
[0084] <Example 14> The same procedure as in Example 1 was carried out except that p-chlorotoluene, an aromatic compound having a chloro group, was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which p-chlorotoluene had been removed was measured, and the result was 1.6×10 -3 S / cm, LPS was 7.7 × 10 -4 There was no degradation of LYBC due to p-chlorotoluene, and the lithium ion conductivity was almost the same as that of the reference example.
[0085] <Example 15> The same procedure as in Example 1 was carried out except that 1,2-dichlorobenzene, an aromatic compound having a chloro group, was used as the organic solvent. The lithium ion conductivity of LYBC from which 1,2-dichlorobenzene had been removed was measured. The lithium ion conductivity of LYBC was 1.6×10 -3 There was no degradation of the LYBC due to 1,2-dichlorobenzene, and the lithium ion conductivity was almost the same as that of the reference example.
[0086] <Example 16> The same procedure as in Example 1 was carried out except that 1,4-dichlorobutane, a non-aromatic compound having a chloro group, was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which 1,4-dichlorobutane had been removed was measured. The lithium ion conductivity of LYBC was 1.6 × 10 -3 S / cm, LPS was 7.6 × 10 -4 There was no degradation of the LYBC due to 1,4-dichlorobutane, and the lithium ion conductivity was almost the same as that of the reference example.
[0087] <Example 17> The same procedure as in Example 1 was carried out except that 3,4-dichlorotoluene, an aromatic compound having a chloro group, was used as the organic solvent. The lithium ion conductivity of LYBC from which 3,4-dichlorotoluene had been removed was measured, and it was found to be 1.7×10 -3 There was no degradation of LYBC due to 3,4-dichlorotoluene, and the lithium ion conductivity was almost the same as that of the reference example.
[0088] In Examples 9 to 17, examples of organic solvents into which a chloro group, which is a halogen element, has been introduced are shown, but organic solvents into which functional groups, such as a bromo group, an iodine group, or a fluoro group, which is another halogen element, have been introduced may also be used.
[0089] Alternatively, an organic solvent into which multiple types of halogen groups selected from the group consisting of a chloro group, a bromo group, an iodo group, and a fluoro group have been introduced may be used.
[0090] <Example 18> The same procedure as in Example 1 was carried out except that tetraethyl orthosilicate having Si-OC groups was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which tetraethyl orthosilicate had been removed was measured. The lithium ion conductivity of LYBC was 1.0×10 -3 S / cm, LPS was 7.9 × 10 -4The degradation of LYBC by tetraethyl orthosilicate was within the acceptable range.
[0091] As described in Examples 7 to 18, the solid electrolyte composition using an organic solvent having an ether group, a halogen group, or a Si-OC group and LYBC as the solid electrolyte material can maintain high lithium ion conductivity.
[0092] <Example 19> A solid electrolyte composition was prepared by the above-mentioned method using tetralin, which is an aromatic hydrocarbon, as an organic solvent and LCYGBC as a solid electrolyte material. The organic solvent, tetralin, was then removed by the above-mentioned vacuum drying.
[0093] The lithium ion conductivity of LCYGBC from which tetralin had been removed was measured by the method described above, and was found to be 8.8 × 10 -4 S / cm.
[0094] The solid electrolyte material of LCYGBC that had not been mixed with an organic solvent was dried in a vacuum as described above, and the lithium ion conductivity was measured by the method described above. It was 1.0 × 10 -3 This is shown at the end of Table 2 as Reference Example (C2).
[0095] Comparing the lithium ion conductivity of LCYGBC of Example 1 with that of the Reference Example, there was no degradation of LCYGBC due to tetralin, and the lithium ion conductivity was almost the same as that of the Reference Example.
[0096] <Example 20> The same procedure as in Example 1 was carried out except that mesitylene, an aromatic hydrocarbon, was used as the organic solvent. The lithium ion conductivity of LCYGBC from which mesitylene had been removed was measured, and it was found to be 9.4×10 -4 There was no degradation of LCYGBC due to mesitylene, and the lithium ion conductivity was almost the same as that of the reference example.
[0097] <Example 21> The same procedure as in Example 1 was carried out except that cumene, an aromatic hydrocarbon, was used as the organic solvent. The lithium ion conductivity of LCYGBC from which cumene had been removed was measured, and it was found to be 1.0×10 -3 There was no degradation of LCYGBC due to cumene, and the lithium ion conductivity was almost the same as that of the reference example.
[0098] As described in Examples 19 to 21, the solid electrolyte composition using an aromatic hydrocarbon organic solvent and LCYGBC can maintain high lithium ion conductivity.
[0099] The present invention can be carried out in the same manner as above, even when a hydrocarbon other than that shown in the examples is used as the organic solvent. However, in consideration of the application of the solid electrolyte composition and the removal of the organic solvent by vacuum drying, it is preferable to use a hydrocarbon that is liquid at room temperature and has a boiling point of 250° C. or less. The hydrocarbon may be used alone or in combination of two or more kinds.
[0100] <Example 22> The same procedure as in Example 1 was carried out except that dibutyl ether having an ether group was used as the organic solvent. The lithium ion conductivity of LCYGBC from which dibutyl ether had been removed was measured, and it was found to be 1.2×10 -3 There was no degradation of LCYGBC due to dibutyl ether, and the lithium ion conductivity was almost the same as that of the reference example.
[0101] <Example 23> The same procedure as in Example 1 was carried out except that anisole, an aromatic compound having an ether group, was used as the organic solvent. The lithium ion conductivity of LCYGBC from which anisole had been removed was measured, and it was 9.2×10 -4 There was no degradation of LCYGBC due to anisole, and the lithium ion conductivity was almost the same as that of the reference example.
[0102] <Example 24> The same procedure as in Example 1 was carried out except that p-chlorotoluene, an aromatic compound having a chloro group, was used as the organic solvent. The lithium ion conductivity of LCYGBC from which p-chlorotoluene had been removed was measured, and it was found to be 1.1×10 -3 There was no degradation of LCYGBC due to p-chlorotoluene, and the lithium ion conductivity was almost the same as that of the reference example.
[0103] <Example 25> The same procedure as in Example 1 was carried out except that 3,4-dichlorotoluene, an aromatic compound having a chloro group, was used as the organic solvent. The lithium ion conductivity of LCYGBC from which 3,4-dichlorotoluene had been removed was measured, and it was found to be 1.0×10 -3 There was no degradation of LCYGBC due to 3,4-dichlorotoluene, and the lithium ion conductivity was almost the same as that of the reference example.
[0104] <Example 26> A solid electrolyte composition was prepared by the above-mentioned method using p-chlorotoluene, which is an aromatic hydrocarbon, as an organic solvent and LYZC as a solid electrolyte material. Furthermore, the organic solvent p-chlorotoluene was removed by the above-mentioned vacuum drying.
[0105] The lithium ion conductivity of LYZC from which p-chlorotoluene had been removed was measured by the method described above, and was found to be 1.2 × 10 -3 S / cm.
[0106] The solid electrolyte material of LYZC that had not been mixed with an organic solvent was dried in a vacuum as described above, and the lithium ion conductivity was measured by the method described above. The result was 1.2 × 10 -3 This is shown at the end of Table 3 as a reference example (C3).
[0107] When the lithium ion conductivity of LYZC of Example 26 was compared with that of the LYZC of the Reference Example, there was no deterioration of LYZC due to p-chlorotoluene, and the lithium ion conductivity was almost the same as that of the Reference Example.
[0108] Although examples 24 to 26 show organic solvents into which a halogen element, a chloro group, has been introduced, organic solvents into which functional groups such as other halogen elements, such as a bromo group, an iodine group, or a fluoro group, have been introduced, may also be used.
[0109] Alternatively, an organic solvent into which multiple types of halogen groups selected from the group consisting of a chloro group, a bromo group, an iodo group, and a fluoro group have been introduced may be used.
[0110] As described in Examples 19 to 26, the solid electrolyte composition using an organic solvent having an ether group or a halogen group and LCYGBC or LYZC as the solid electrolyte material can maintain high lithium ion conductivity.
[0111] Organic solvents having an ether group, a halogen group, or a Si-OC group other than those shown in the examples may be used. However, in consideration of coating the solid electrolyte composition and removing the organic solvent by vacuum drying, it is preferable to use a hydrocarbon that is liquid at room temperature, has a boiling point of 250° C. or less, and has a hydrogen atom substituted with the above functional group. These organic solvents may be used alone or in combination.
[0112] Furthermore, although LCYGBC and LYZC were used as the solid electrolyte material, other ionic solid electrolyte materials not containing sulfur element may be used.
[0113] Furthermore, other ion-bonded solid electrolyte materials can be similarly implemented as long as they have lithium ion conductivity, and contain at least one selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb, and Sm, and contain at least one selected from the group consisting of Cl, Br, I, and F, and do not contain sulfur element. One type of ion-bonded solid electrolyte material may be used alone, or multiple types may be used in combination.
[0114] <Comparative Example 1> The same procedure as in Example 1 was carried out except that butyl butyrate, a non-aromatic compound having an ester group, was used as the organic solvent. An attempt was made to measure the lithium ion conductivity of LYBC from which the butyl butyrate had been removed, but the butyl butyrate could not be removed. Considering the application of the solid electrolyte composition and the removal of the organic solvent by vacuum drying, it was found that butyl butyrate was inappropriate. The same procedure was carried out for LPS, and the lithium ion conductivity of LPS from which the butyl butyrate had been removed was measured, resulting in a value of 7.9×10 -4 There was no degradation of LPS due to butyl butyrate, and the lithium ion conductivity was almost the same as that of the reference example.
[0115] <Comparative Example 2> The same procedure as in Example 1 was carried out, except that ethyl 3-ethoxypropionate, a non-aromatic compound having an ester group, was used as the organic solvent. When an attempt was made to measure the lithium ion conductivity of LYBC from which ethyl 3-ethoxypropionate had been removed, the resistance was too high and the measurement was not possible. It is believed that ethyl 3-ethoxypropionate has significantly deteriorated LYBC. The same procedure was carried out for LPS, and the lithium ion conductivity of LPS from which ethyl 3-ethoxypropionate had been removed was measured, resulting in a value of 8.1×10 -4 There was no degradation of LPS due to ethyl 3-ethoxypropionate, and the lithium ion conductivity was almost the same as that of the reference example.
[0116] <Comparative Example 3> The same procedure as in Example 1 was carried out except that butyl acetate, a non-aromatic compound having an ester group, was used as the organic solvent. The lithium ion conductivity of LYBC and LPS from which butyl acetate had been removed was measured. As a result, the lithium ion conductivity of LYBC was 1.1 × 10 -9 S / cm, LPS was 8.2 × 10 -4 S / cm. Compared to the lithium ion conductivity of the reference LYBC, the value is significantly lower, suggesting that LYBC has been degraded by butyl acetate. There was no degradation of LPS by butyl acetate, and the lithium ion conductivity was almost the same as that of the reference.
[0117] <Comparative Example 4> The same procedure as in Example 1 was carried out, except that 2-ethylhexyl acrylate, a non-aromatic compound having an ester group, was used as the organic solvent. When an attempt was made to measure the lithium ion conductivity of LYBC from which 2-ethylhexyl acrylate had been removed, it was found that 2-ethylhexyl acrylate could not be removed. Considering the application of the solid electrolyte composition and the removal of the organic solvent by vacuum drying, it was found that 2-ethylhexyl acrylate was inappropriate. The same procedure was carried out for LPS, and the lithium ion conductivity of LPS from which butyl butyrate had been removed was measured, resulting in a value of 7.9×10 -4 There was no degradation of LPS due to 2-ethylhexyl acrylate, and the lithium ion conductivity was almost the same as that of the reference example.
[0118] <Comparative Example 5> The same procedure as in Example 1 was carried out except that 2-ethoxyethyl acetate, a non-aromatic compound having an ester group, was used as the organic solvent. When an attempt was made to measure the lithium ion conductivity of LYBC from which 2-ethoxyethyl acetate had been removed, it was found that 2-ethoxyethyl acetate could not be removed. Considering the application of the solid electrolyte composition and the removal of the organic solvent by vacuum drying, it was found that 2-ethoxyethyl acetate was inappropriate. The same procedure was carried out for LPS, and the lithium ion conductivity of LPS from which 2-ethoxyethyl acetate had been removed was measured, resulting in a value of 8.2×10 -4 There was no degradation of LPS due to 2-ethoxyethyl acetate, and the lithium ion conductivity was almost the same as in the reference example.
[0119] <Comparative Example 6> The same procedure as in Example 1 was carried out, except that ethyl benzoate, an aromatic compound having an ester group, was used as the organic solvent. When an attempt was made to measure the lithium ion conductivity of LYBC and LPS from which the ethyl benzoate had been removed, the resistance was too high and measurements were not possible. It is believed that the ethyl benzoate has significantly deteriorated the LYBC. The same procedure was carried out for LPS, and the lithium ion conductivity of LPS from which the ethyl benzoate had been removed was measured, resulting in a value of 8.1 x 10 -4 There was no degradation of LPS due to ethyl benzoate, and the lithium ion conductivity was almost the same as that of the reference example.
[0120] It was found that the organic solvents having an ester group described in Comparative Examples 1 to 6 deteriorate the ionic solid electrolyte material LYBC, but do not deteriorate the covalent solid electrolyte material LPS. It is considered that it is inappropriate to use an organic solvent having an ester group for an ionic solid electrolyte material that does not contain sulfur element.
[0121] <Comparative Example 7> The same procedure as in Example 1 was carried out except that diisobutyl ketone, a non-aromatic compound having a ketone group, was used as the organic solvent. When an attempt was made to measure the lithium ion conductivity of LYBC from which diisobutyl ketone had been removed, the resistance was too high and the measurement was not possible. It is believed that LYBC has been significantly deteriorated by diisobutyl ketone. The same procedure was carried out for LPS, and the lithium ion conductivity of LPS from which diisobutyl ketone had been removed was measured, resulting in a value of 7.2×10 -4 There was no degradation of LPS due to diisobutyl ketone, and the lithium ion conductivity was almost the same as that of the reference example.
[0122] <Comparative Example 8> The same procedure as in Example 1 was carried out except that isophorone, a cyclic non-aromatic compound having a ketone group, was used as the organic solvent. When an attempt was made to measure the lithium ion conductivity of LYBC from which isophorone had been removed, it was found that isophorone could not be removed. Considering the application of the solid electrolyte composition and the removal of the organic solvent by vacuum drying, it was found that isophorone was inappropriate. The same procedure was carried out for LPS, and the lithium ion conductivity of the LPS from which isophorone had been removed was measured, resulting in a value of 7.6×10 -4 There was no degradation of LPS due to isophorone, and the lithium ion conductivity was almost the same as that of the reference example.
[0123] <Comparative Example 9> The same procedure as in Example 1 was carried out except that N-methylpyrrolidone, a cyclic non-aromatic compound having a ketone group, was used as the organic solvent. The lithium ion conductivity of LYBC from which N-methylpyrrolidone had been removed was measured, and it was found to be 1.8×10 -7S / cm. Compared to the reference example, the value is significantly lower, and it is believed that LYBC is degraded by N-methylpyrrolidone. The same procedure was performed for LPS, and an attempt was made to measure the lithium ion conductivity of LPS from which N-methylpyrrolidone had been removed, but the resistance was too high and measurement was not possible. It was found that N-methylpyrrolidone cannot be used because it degrades both LYBC and LPS.
[0124] It was found from Comparative Examples 7 to 9 that an organic solvent having a ketone group deteriorates LYBC. It is considered that it is inappropriate to use an organic solvent having a ketone group for an ionic solid electrolyte material not containing elemental sulfur.
[0125] <Comparative Example 10> The same procedure as in Example 1 was carried out, except that N,N-dimethyldodecylamine, a non-aromatic compound having an amino group, was used as the organic solvent. When an attempt was made to measure the lithium ion conductivity of LYBC from which N,N-dimethyldodecylamine had been removed, it was found that N,N-dimethyldodecylamine could not be removed. Considering the application of the solid electrolyte composition and the removal of the organic solvent by vacuum drying, it was found that N,N-dimethyldodecylamine was inappropriate. The same procedure was carried out for LPS, and the lithium ion conductivity of LPS from which N,N-dimethyldodecylamine had been removed was measured, resulting in a value of 7.6×10 -4 There was no degradation of LPS due to N,N-dimethyldodecylamine, and the lithium ion conductivity was almost the same as that of the reference example.
[0126] <Comparative Example 11> The same procedure as in Example 1 was carried out except that N,N-dimethylaniline, an aromatic compound having an amino group, was used as the organic solvent. The lithium ion conductivity of LYBC from which N,N-dimethylaniline had been removed was measured, and it was found to be 7.5×10 -4S / cm. Compared to the reference example, the value is significantly lower, and it is believed that the LYBC is degraded by N,N-dimethylaniline. The same procedure was performed on LPS, and the lithium ion conductivity of the LPS from which N,N-dimethylaniline had been removed was measured, resulting in a value of 7.7×10 -4 There was no degradation of LPS due to N,N-dimethylaniline, and the lithium ion conductivity was almost the same as that of the reference example.
[0127] <Comparative Example 12> The same procedure as in Example 1 was carried out except that N-methylaniline, an aromatic compound having an amino group, was used as the organic solvent. The lithium ion conductivity of LYBC from which N-methylaniline had been removed was measured, and it was found to be 1.1×10 -7 S / cm. Compared to the reference example, the value is significantly lower, and it is believed that the LYBC is degraded by N-methylaniline. The same procedure was performed on LPS, and the lithium ion conductivity of the LPS from which N,N-dimethylaniline had been removed was measured, resulting in a value of 7.9×10 -4 There was no degradation of LPS due to N-methylaniline, and the lithium ion conductivity was almost the same as that of the reference example.
[0128] It was found from Comparative Examples 10 to 12 that an organic solvent having an amino group does not deteriorate LPS but deteriorates LYBC. It is considered that it is inappropriate to use an organic solvent having an amino group for an ion-bonded solid electrolyte material not containing sulfur element.
[0129] <Comparative Example 13> The same procedure as in Example 1 was carried out except that 2-ethyl-1-hexanol, a non-aromatic compound having a hydroxyl group, was used as the organic solvent. The lithium ion conductivity of LYBC from which 2-ethyl-1-hexanol had been removed was measured, and it was found to be 9.8×10 -6S / cm. Compared to the reference example, the value is significantly lower, and it is believed that LYBC is degraded by 2-ethyl-1-hexanol. The same procedure was performed for LPS, and the lithium ion conductivity of LPS from which 2-ethyl-1-hexanol had been removed was measured, resulting in a value of 7.9 x 10 -4 There was no degradation of LPS due to 2-ethyl-1-hexanol, and the lithium ion conductivity was almost the same as that of the reference example.
[0130] It was found from Comparative Example 13 that an organic solvent having a hydroxyl group does not deteriorate LPS but deteriorates LYBC. It is considered that it is inappropriate to use an organic solvent having a hydroxyl group for an ionic solid electrolyte material not containing sulfur element.
[0131] <Comparative Example 14> The same procedure as in Example 1 was carried out except that benzaldehyde, an aromatic compound having an aldehyde group, was used as the organic solvent. When an attempt was made to measure the lithium ion conductivity of LYBC from which benzaldehyde had been removed, it was found that benzaldehyde could not be removed. Considering the application of the solid electrolyte composition and the removal of the organic solvent by vacuum drying, it was found that benzaldehyde was inappropriate. The same procedure was carried out for LPS, and the lithium ion conductivity of LPS from which benzaldehyde had been removed was measured, resulting in a value of 7.5×10 -4 There was no degradation of LPS due to benzaldehyde, and the lithium ion conductivity was almost the same as that of the reference example.
[0132] It was found that organic solvents containing aldehyde groups do not degrade LPS but do degrade LYBC. It is therefore considered inappropriate to use organic solvents containing aldehyde groups with ionic solid electrolyte materials that do not contain sulfur elements.
[0133] 2 plots the polar term values (arbitrary units) of the Hansen solubility parameters of LYBC in organic solvents listed in Table 1 on the horizontal axis and the lithium ion conductivity (mS / cm) of LYBC after vacuum drying on the vertical axis, with the values of Examples 1 to 18 and Comparative Examples 1 to 14 plotted. For organic solvents that had high resistance and could not measure the lithium ion conductivity or could not be dried, the values were plotted on the graph as 0 mS / cm.
[0134] From Figure 2, we can see that the lithium ion conductivity of LYBC after vacuum drying is more affected by the substituted functional groups than by the polarity term of the organic solvent. Although the detailed mechanism of action is unknown, it is presumed that when functional groups that cause localization of electron density in the organic solvent molecule, such as ester groups, ketone groups, amino groups, and hydroxyl groups, are introduced, the localized sites and the ionic constituent elements of LYBC cause interactions such as solvation, which causes the structure of LYBC to collapse, resulting in a decrease in the lithium ion conductivity of LYBC after vacuum drying. This can be considered to be a common tendency for ionic solid electrolyte materials that do not contain sulfur elements.
[0135] Figure 3 shows the particle size distribution of LYBC in a solid electrolyte composition containing an organic solvent and LYBC. Measurements were performed for five types of organic solvent: n-heptane, anisole, tetralin, o-chlorotoluene, and p-chlorotoluene. The horizontal axis shows the particle size (μm) measured using an image analysis type particle analysis system, and the vertical axis shows the probability of existence (arbitrary units).
[0136] The details of the measurement method are described below. (Preparation of Solid Electrolyte Composition) In a glove box controlled under an argon atmosphere, 30 ml of organic solvent was weighed out, and 0.006 g of LYBC was weighed out and mixed by stirring. The organic solvent was thoroughly dried in advance using molecular sieves. Furthermore, to prevent the intrusion of moisture, oxygen, etc., the container for stirring and mixing was double-walled, and a non-polar solvent (specifically, heptane) was poured into the outer container and sealed. In this state, dispersion was performed for 30 minutes using ultrasonic waves.
[0137] (Particle size distribution measurement) Measurement was carried out using an image analysis particle size distribution measuring device (model: XPT-C, manufactured by PS Prozesstechnik GmbH) while stirring with a stirrer.
[0138] Looking at the peak values of the particle size distribution in Figure 3, it is in the order of p-chlorotoluene < o-chlorotoluene = tetralin < anisole < n-heptane. Here, "=" means substantially equal, and the same meaning applies to the following "=". This indicates the dispersibility in the organic solvent, and the dispersibility is good in the order of p-chlorotoluene, o-chlorotoluene = tetralin, anisole, n-heptane, resulting in a solid electrolyte composition with less aggregation of LYBC. From the above, it is desirable that the organic solvent is an aromatic compound, and particularly when preparing a solid electrolyte composition containing an electrode active material, it is desirable to use an aromatic compound as the organic solvent.
Industrial applicability
[0139] The solid electrolyte composition according to the present invention is useful, for example, when used in the manufacture of all-solid-state lithium secondary batteries.
Explanation of symbols
[0140] 100 Solid electrolyte material 200 Die for pressure molding 201 Frame type made of polycarbonate 202 Lower punch made of stainless steel 203 Upper punch made of stainless steel
Claims
1. A solid electrolyte material having a halide and an organic solvent, The halide solid electrolyte material has the composition formula Li α M β X γ is represented by In the formula, α, β, and γ are each independently a value greater than 0, M is at least one selected from the group consisting of metal elements and metalloid elements other than Li, and X is at least one selected from the group consisting of Cl, Br, and I. the organic solvent contains at least one selected from the group consisting of a compound having a functional group and a hydrocarbon, The solid electrolyte composition, wherein the functional group is at least one selected from the group consisting of an ether group, a halogen group, and a Si—O—C group.
2. 2. The solid electrolyte composition according to claim 1, wherein the halide solid electrolyte material has lithium ion conductivity and contains at least one selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb, and Sm, and also contains at least one selected from the group consisting of Cl, Br, and I.
3. The halide solid electrolyte material is Li and The solid electrolyte composition according to claim 2, further comprising at least one selected from the group consisting of Gd, Ca, Zr, and Y, and at least one selected from the group consisting of Cl, Br, and I.
4. The solid electrolyte composition according to claim 2 or 3, wherein the halide solid electrolyte material contains Li and Y, and also contains at least one selected from the group consisting of Cl, Br, and I.
5. The solid electrolyte composition according to any one of claims 1 to 4, wherein the halide solid electrolyte material is a material containing Li, Y, Cl, and Br, a material containing Li, Ca, Y, Gd, Cl, and Br, or a material containing Li, Zr, Y, and Cl.
6. The halide solid electrolyte material is Li 3 YBr 2 C 4 , Li 2.8 Ca 0.1 Y 0.5 G.D. 0.5 B 2 C 4 , or Li 2.5 Y 0.5 Zr 0.5 C 6 The solid electrolyte composition according to claim 1 ,
7. The halide solid electrolyte material is substantially Li and At least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb and Sm; 3. The solid electrolyte composition according to claim 1, which is a material consisting of at least one element selected from the group consisting of Cl, Br and I.
8. The solid electrolyte composition according to claim 1 , wherein the compound having a functional group is substantially free of functional groups other than an ether group and a halogen group.
9. The solid electrolyte composition according to claim 1 , wherein the organic solvent includes a ring structure.
10. The solid electrolyte composition according to claim 9 , wherein the organic solvent is an aromatic compound.
11. The solid electrolyte composition according to any one of claims 1 to 10, wherein the organic solvent includes at least one selected from the group consisting of tetralin, ethylbenzene, mesitylene, pseudocumene, xylene, cumene, dibutyl ether, anisole, 1,2,4-trichlorobenzene, chlorobenzene, 2,4-dichlorobenzene, o-chlorotoluene, 1,3-dichlorobenzene, p-chlorotoluene, 1,2-dichlorobenzene, 1,4-dichlorobutane, 3,4-dichlorotoluene, and tetraethyl orthosilicate.
12. The solid electrolyte composition according to claim 1 , wherein the halide solid electrolyte material is dispersed in the organic solvent.
13. 13. The solid electrolyte composition according to claim 1, wherein the halide solid electrolyte material is not dissolved in the organic solvent.
14. The present invention includes an ionically bonded solid electrolyte material that does not contain elemental sulfur and an organic solvent, the ion-bonded solid electrolyte material is a material containing Li, Y, Cl, and Br, a material containing Li, Ca, Y, Gd, Cl, and Br, or a material containing Li, Zr, Y, and Cl; the organic solvent contains at least one selected from the group consisting of a compound having a functional group and a hydrocarbon, The solid electrolyte composition, wherein the functional group is at least one selected from the group consisting of an ether group, a halogen group, and a Si—O—C group.
15. A method for producing a solid electrolyte member, comprising: a removing step of removing the organic solvent from the solid electrolyte composition according to claim 1 .
16. The method for producing a solid electrolyte member according to claim 15 , wherein in the removing step, the organic solvent is removed by drying under reduced pressure.
Citation Information
Patent Citations
Nonaqueous secondary battery
JP2001006745A
Solid electrolyte, method for manufacturing the same, and lithium ion battery
JP2017162728A
Solid electrolyte composition, electrode sheet for all-solid-state secondary cell, all-solid-state secondary cell, and method for manufacturing electrode sheet for all-solid-state secondary cell and all-solid-state secondary cell
WO2016194705A1
Solid electrolyte material, and cell
WO2018025582A1
Solid electrolyte composition, solid electrolyte-containing sheet, all-solid-state secondary battery, method for producing solid electrolyte composition, method for producing solid electrolyte-containing sheet, and method for producing all-solid-state secondary battery
WO2018168505A1