A testing method for evaluating the cell aggregation function of amorphous carbon films.

By measuring extinction coefficient, refractive index, and carbonyl group composition ratio, the method assesses amorphous carbon films' cell aggregation properties, addressing the limitations of existing evaluation methods and enhancing the suitability of carbon films for cell culture applications.

JP7576827B2Active Publication Date: 2024-11-01TOKYO DENKI UNIVERSITY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020188369
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-12
Publication Date
2024-11-01
Estimated Expiration
2040-11-12

AI Technical Summary

Technical Problem

Existing methods for evaluating amorphous carbon films for cell aggregation properties are inadequate, leading to low cell adhesion and excessive cell death due to the use of materials that are difficult for cells to adhere to, which is a barrier for practical applications in cell culture and biointerface technologies.

Method used

A method is developed to measure the extinction coefficient (k), refractive index (n), and carbonyl group composition ratio (CO) of amorphous carbon films using spectroscopic ellipsometry and X-ray photoelectron spectroscopy to determine the cell aggregation function, utilizing variables such as 1/k, n/k, and n/(k×CO) as criteria for quality assessment.

Benefits of technology

This method allows for easy and accurate evaluation of amorphous carbon films' cell aggregation properties, enabling the selection of films suitable for cell culture applications by providing a simple and rapid testing process that improves the reliability of products like culture vessels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576827000005
    Figure 0007576827000005
  • Figure 0007576827000006
    Figure 0007576827000006
  • Figure 0007576827000007
    Figure 0007576827000007
Patent Text Reader

Abstract

To realize an inspection method for measuring some physical characteristics of an amorphous carbon film to determine whether or not the carbon film may guide a cell aggregation based on the measurement value, and a method for manufacturing a product containing an amorphous carbon film as a part of its configuration, which uses the inspection method in an inspection process.SOLUTION: An amorphous carbon film inspection method comprises: measuring indexes of reflecting a basic structure of an amorphous carbon film, such as optical constants such as an extinction coefficient and a refractive index, and a carbonyl group composition ratio; and determining a cell aggregation function of the amorphous carbon film based on predetermined variables including the indexes. A method for manufacturing a product containing an amorphous carbon film as a part of its configuration has an inspection step of determining that an amorphous carbon film to be a target of the inspection method has a suitable cell aggregation function by using the inspection method.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for inspecting an amorphous carbon film, which comprises measuring an index that reflects the basic structure of the amorphous carbon film, and judging the cell aggregation function of the amorphous carbon film based on predetermined variables including the index. [Background technology]

[0002] Amorphous carbon films are also called diamond-like carbon (DLC) films, and have a sp 3 Carbon with bonds and sp corresponding to the graphite structure 2 It is an amorphous film in which carbon with bonds is randomly mixed. Because it has characteristics such as high hardness, low friction, and an inert surface, it is known that when used as a coating material for the surface of substrates made of inorganic materials such as metals and ceramics, or organic materials such as polymer resins, it provides the substrate surface with properties such as wear resistance, corrosion resistance, and sliding properties.

[0003] Since amorphous carbon films also have properties such as biocompatibility and chemical stability, they are expected to be used as a means of surface modification for medical devices. In addition to these properties, as mentioned above, coating various materials such as metals, ceramics, and polymer resins improves surface hardness and sliding properties, and their application to, for example, implants (Patent Document 1), stents (Patent Document 2), and catheters (Patent Document 3) has been proposed.

[0004] Although they are generally called amorphous carbon films, their basic physical properties (sp 3 Structure: Diamond structure derived, sp 2The characteristics of amorphous carbon films are different: structure: derived from graphite structure, H: hydrogen content). Specifically, they are classified into ta-C, ta-C:H, aC, aC:H, polymer, and graphitic based on the basic physical properties, and the surface functions are determined by these. In addition, amorphous carbon films have been evaluated by macroscopic analysis of the entire film, but it has become clear that the film properties of the surface layer, bulk layer, and substrate interface layer of each amorphous carbon film differ depending on the film formation method. Therefore, in order to bring out the properties of the amorphous carbon film as a biointerface in the interaction with biological substances, it is essential to understand the surface functions of the amorphous carbon film based on its basic physical properties. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2014-4166 [Patent Document 2] Patent Publication No. 2010-280636 [Patent Document 3] Patent Publication No. 2008-245883 [Patent Document 4] Patent Publication No. 2014-057578 [Patent Document 5] International Publication No. 2013 / 099901 Brochure [Patent Document 6] International Publication No. 2 0 1 3 / 0 2 2 0 8 5 Brochure [Non-patent literature]

[0006] [Non-Patent Document 1] Naoto Otake and 2 others, 2012, NEW DIAMOND Vol.28, No.3, pp.12-18 [Non-Patent Document 2] M. Hiratsuka et al., 2013, Journal of Solid Mechanics and Materials Engineering, Vol. 7, No. 2, pp. 187-198 [Non-Patent Document 3] Y. Nitta et al., 2012, IEEE Transactions on Plasma Science Vol. 40, pp. 2073-2078 [Non-Patent Document 4] S. Takabayashi, and T. Takahagi, 2015, Surf. Interface Anal. Vol. 47, pp. 345-349 [Non-Patent Document 5] MA Caro et al. and 4 others, 2018, Chemistry of Materials Vol.30, pp.7446-7455 [Non-Patent Document 6] A.Bagri, and R.Grantab, published in 2010, J.Phys.Chem.Vol.114, pp.12053-12061 Summary of the Invention [Problem to be solved by the invention]

[0007] Until now, the main indicators of the properties of amorphous carbon films as a biointerface have been biocompatibility and bioaffinity, which are the ability to allow good bonding and adhesion with biological substances. In particular, cell affinity, which indicates the property of cells adhering well to some kind of equipment or the like that exists outside the cells, is also strongly related to the control of cell proliferation on the surface (two-dimensional) of the equipment or the like, and therefore there have already been many reports on physical properties of amorphous carbon films that relate to cell affinity. For example, Patent Document 4 discloses the relationship between optical constants such as the refractive index (n) and the extinction coefficient (k) and the bioaffinity of amorphous carbon films, and Patent Document 3 shows the relationship between the introduction rate of carboxyl groups introduced into the surface of an amorphous carbon film formed on the surface of a substrate and the growth inhibitory effect of smooth muscle cells that are attached to the surface of the amorphous carbon film.

[0008] However, in recent years, a new concept called cell aggregation has been proposed in addition to such cell affinity. Cell aggregation is the property of forming cell aggregates. A cell aggregate is a mass formed by the gathering of dispersed cells, in which the cells are adhered to each other. Cell aggregates also include those called cell aggregates, embryoid bodies, spheres, and spheroids. The function of inducing the formation of such cell aggregates is attracting attention as a new characteristic required for biointerfaces, which is different from the cell affinity that has been used in the past.

[0009] Recently, pluripotent stem cells such as ES cells and iPS cells have been attracting attention as a fundamental treatment for intractable diseases and lifestyle-related diseases in regenerative medicine because of their ability to proliferate indefinitely and differentiate into various cells, but the problem of cell production is a major obstacle to practical application. Generally, a large number of cells are required for organ regeneration, so conventional two-dimensional culture on the surface of a flat substrate is not a realistic method of cell supply. To solve this problem, methods and dedicated equipment have been developed for actively aggregating cells from two-dimensional culture and culturing them three-dimensionally in the form of cell aggregates. However, conventional equipment for forming cell aggregates is mainly made of molded products using materials to which cells simply do not adhere well (Patent Documents 5 and 6), and for this reason, problems such as cell death due to apoptosis caused by excessively low cell adhesion have been encountered.

[0010] Amorphous carbon films, which have biocompatibility and are used as surface materials for various two-dimensional culture ware, are known to be able to be endowed with various surface functions by changing the film formation technique. It was therefore hoped that an amorphous carbon film with the desired cell aggregation properties could be realized by some kind of film formation technique. However, it was not yet clear what properties of the amorphous carbon film are involved in determining whether the cell aggregation properties are good or bad.

[0011] In view of the above problems, an object of the present invention is to provide an inspection method for measuring some physical property of an amorphous carbon film and judging whether or not the carbon film is capable of inducing cell aggregation based on the measured value, and a manufacturing method for a product that includes an amorphous carbon film as part of its configuration, using the inspection method in the inspection process. [Means for solving the problem]

[0012] In order to establish an index of cell aggregation of an amorphous carbon film, the inventors used various kinds of amorphous carbon films formed by different film formation methods to evaluate the cell aggregation of each carbon film, and also measured indexes that may be related to cell aggregation among those reflecting the basic structure of the amorphous carbon film, and conducted intensive research into the correlation between the two. As a result, the inventors found a correlation between the quantitative characteristics of cell aggregation and optical constants represented by the extinction coefficient (k) and refractive index (n) and the carbonyl group composition ratio (CO) among the indexes. Furthermore, the inventors devised a new variable that combines these indexes, each of which indicates a different physical property of the amorphous carbon film, and established an inspection method for the amorphous carbon film that enables the determination of the cell aggregation function of the amorphous carbon film by using the new variable as a criterion for the quality of the cell aggregation of the amorphous carbon film.

[0013] Furthermore, the inspection method according to the present invention can be utilized as an inspection step in a manufacturing method of a product containing an amorphous carbon film as part of its configuration, in which the extinction coefficient and / or refractive index of the amorphous carbon film formed on the surface of the product is measured, for example, by spectroscopic ellipsometry, and the carbonyl group composition ratio is measured, for example, by X-ray photoelectric spectroscopy, and when predetermined variables based on these measured values ​​are equal to or greater than certain values, the amorphous carbon film of the product is determined to be good in terms of cell aggregation function.

[0014] Based on the above findings, the present invention has been completed. That is, the present invention relates to the following (1) to (10). (1) A method for inspecting an amorphous carbon film, comprising measuring an index that reflects the basic structure of the amorphous carbon film, and determining the cell aggregation function of the amorphous carbon film based on predetermined variables including the index. (2) The inspection method according to (1), wherein the index is an extinction coefficient k, and the specified variable is the reciprocal of the extinction coefficient k (1 / k). (3) The inspection method according to (2), wherein the amorphous carbon film is judged to have a suitable cell aggregation function when the value calculated by 1 / k is 7 or more. (4) The inspection method described in (1), characterized in that the indexes are an extinction coefficient k and a refractive index n, and the specified variable is n / k. (5) The inspection method according to (4), wherein the amorphous carbon film is judged to have a suitable cell aggregation function when the value calculated by n / k is 13 or more. (6) The inspection method described in (1), characterized in that the indices are the extinction coefficient k, the refractive index n, and the carbonyl group composition ratio CO, and the predetermined variable is n / (k×CO). (7) The inspection method according to (6), characterized in that when the value obtained by n / (k×CO) is 565 or more, the amorphous carbon film is determined to have a suitable cell aggregation function. (8) The inspection method according to any one of (2) to (7), wherein the extinction coefficient k and / or the refractive index n are measured by spectroscopic ellipsometry. (9) The inspection method according to any one of (6) to (8), wherein the carbonyl group composition ratio CO is measured by X-ray photoelectric spectroscopy. (10) A method for producing a product including an amorphous carbon film as a part of its configuration, comprising: an inspection step of determining, by the inspection method according to any one of (1) to (9), that the amorphous carbon film to be the subject of the inspection method has a suitable cell aggregation function. Effect of the Invention

[0015] According to the present invention, the extinction coefficient, refractive index, and carbonyl group composition ratio of an amorphous carbon film are measured using spectroscopic ellipsometry and / or X-ray photoelectric spectroscopy, which are relatively easy to measure, and a new variable combining these indices is used as a standard, so that the quality of the amorphous carbon film as a film having cell aggregation properties can be easily and numerically inspected. Furthermore, the measurement of the basic physical properties by spectroscopic ellipsometry and / or X-ray photoelectric spectroscopy is a non-destructive test for a product that includes an amorphous carbon film as a part of its composition, and can be performed while the product is kept at room temperature in the atmosphere, so that this inspection method can be easily incorporated into the manufacturing process. [Brief description of the drawings]

[0016] [Figure 1] Cultivation using cloning rings (top) and schematic diagram of the photographed and evaluation areas on an amorphous carbon film (DLC) (bottom). [Diagram 2] Optical constants (extinction coefficient and refractive index) of various amorphous carbon films. [Diagram 3] Raman spectra and extinction coefficients of various amorphous carbon films. [Figure 4] XPS analysis Carbon1s spectra of various amorphous carbon films. [Diagram 5] Cell adhesion / aggregation on various amorphous carbon films. [Figure 6] Total area of ​​aggregated cells after 24 hours of culture on various amorphous carbon films. [Figure 7] Number of two-dimensionally attached cells per unit area after 24 hours of culture on various amorphous carbon films. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] A first aspect of the present invention is a method for inspecting an amorphous carbon film, comprising measuring an index reflecting a basic structure of the amorphous carbon film and determining the cell aggregation function of the amorphous carbon film based on predetermined variables including the index.

[0018] Amorphous carbon films are produced by various deposition methods and have a wide range of applications. However, the physical properties of amorphous carbon films have not been defined, and there are no quantitative evaluation indices, which is an obstacle to their production and use. Therefore, in order to appropriately utilize amorphous carbon films suited to their applications, it has been necessary to classify and standardize the applications and physical properties of the carbon films. To date, more than 75 types of amorphous carbon films have been classified, and 2 / sp 3 A total of 14 analyses were carried out, including the bond ratio, hydrogen content, and film density. 2 / sp 3 Based on the bond ratio and hydrogen content, they are classified into ta-C, ta-C:H, aC, and aC:H film types with a tolerance of ±5% (Non-Patent Document 1). In addition to the above, amorphous carbon films are also classified into PLC (polymer like carbon), which has a high hydrogen content and exhibits polymeric properties, and GLC (graphite like carbon), which exhibits graphite-like properties, and these are collectively classified as amorphous carbon films. The amorphous carbon film according to the present invention is a graphite structure-derived sp 2 and sp from the diamond structure 3 Any carbon film having a mixed hybrid orbital and a hydrogenated structure may be used, and may belong to any of the above categories, without any particular limitation.

[0019] The method for forming the amorphous carbon film according to the present invention is not particularly limited and may be any existing film forming method and / or a new method. In examining amorphous carbon films having different basic structures, the inventors formed a total of five types of amorphous carbon films on Si substrates using a High Power Impulse Magnetron Sputtering method (HiPIMS), an ionization deposition method (Ionization), a DC Pulse Plasma Chemical Vapor Deposition method (DC pulse CVD), and an rf Plasma CVD method (RF CVD), respectively, and conducted the examination, but the present invention is not limited to amorphous carbon films formed by these film forming methods.

[0020] The basic structure of an amorphous carbon film refers to the basic structure of the carbon film, and can be defined by various physical properties of the carbon film. Although not particularly limited, in the present invention, it is a structure defined by at least the basic physical properties and surface state of the amorphous carbon film.

[0021] The basic physical property of the amorphous carbon film is that the carbon film has a diamond structure. 3 Structure and graphite structure origin sp 2 It is a physical property represented by the bond ratio and hydrogen content of the structure. However, the sp 2 / sp 3 Quantitative measurement of the bond ratio and hydrogen content is not easy, and as a quality control method for amorphous carbon films, a simple and inexpensive evaluation index is required at the production sites of coating manufacturers, etc. For this reason, a classification method for amorphous carbon films using optical constants (refractive index n and extinction coefficient k) that can be easily obtained by spectroscopic ellipsometry as indexes has been proposed at present (Non-Patent Document 2).

[0022] Spectroscopic ellipsometry is a technique for analyzing film thickness and optical constants by irradiating a sample with light and measuring the change in polarization between the incident light and the reflected light. The refractive index (n) reflects the hardness and film density, and the extinction coefficient (k) reflects the sp 2 Since the optical constants obtained by spectroscopic ellipsometry reflect the content rate and hydrogen content of the amorphous carbon film, the optical constants reflect the basic physical properties of the amorphous carbon film.

[0023] For this reason, as an index reflecting a basic physical property, which is one of the characteristics that defines the basic structure of the amorphous carbon film according to the present invention, the sp 2 / sp 3 There is no particular limitation as long as it is a quantitative index capable of indicating the bond ratio and hydrogen content, but the extinction coefficient and / or refractive index are preferable. In addition, the method for measuring the indexes reflecting the fundamental physical properties is not particularly limited, but may be spectroscopic ellipsometry, laser Raman spectroscopy (RAMAN), Rutherford backscattering analysis (RBS) / elastic recoil detection analysis (ERDA), near edge X-ray absorption fine structure (NEXAFS), etc., preferably laser Raman spectroscopy or spectroscopic ellipsometry, and particularly preferably measurement by spectroscopic ellipsometry.

[0024] The surface state of an amorphous carbon film is another characteristic that determines the basic structure of the film. In recent years, the medical applications of amorphous carbon films have expanded rapidly due to their tissue compatibility and cell affinity, which are suggested to be due to the surface state of the carbon film, and the diversification of amorphous carbon films has progressed accordingly. For this reason, an index for the amorphous carbon film as a biointerface is required, and it has been reported that in particular, in affinity evaluation at the cellular level, the cell adhesion function is greatly affected by oxygen functional groups (mainly carbonyl groups) formed on the surface. In other words, it has been suggested that the carbonyl group composition ratio on the surface of an amorphous carbon film may be one of the indexes that reflect the surface state in evaluating cell affinity.

[0025] The cell aggregation property of the amorphous carbon film according to the present invention is a biological property different from cell affinity. In order to investigate whether there is any correlation between the carbonyl group composition ratio and cell aggregation property, the inventors formed and evaluated amorphous carbon films with different properties by five different film formation methods as described above, and found a strong correlation between the two.

[0026] In view of the above, as an index reflecting the surface state, which is another characteristic that defines the basic structure of the amorphous carbon film according to the present invention, although there are no particular limitations, an index that quantitatively indicates the amount of oxygen functional groups formed on the surface is preferable, and the carbonyl group composition ratio on the surface of the amorphous carbon film is particularly preferable. The method for measuring the index reflecting the surface state is not particularly limited, but may be X-ray photoelectron spectroscopy (XPS) or near edge X-ray absorption fine structure (NEXAFS), and is preferably measurement by X-ray photoelectron spectroscopy.

[0027] The cell aggregation function of the amorphous carbon film according to the present invention refers to the ability to induce the formation of a cell aggregate from cells cultured on the carbon film. As described in

[0007] , a cell aggregate is a mass formed by the aggregation of dispersed cells, in which the cells are adhered to each other. In some embodiments, the cell aggregate according to the present invention may have cells that are surface-adhered to each other, and in some embodiments, the cells may form cell-cell junctions and / or cell adhesions, such as adhesion junctions, in a part or the whole of the aggregate, but the cell aggregates according to the present invention include various embodiments of cell aggregates without being limited to a specific embodiment. Thus, the cell aggregation ability of the amorphous carbon film according to the present invention refers to the characteristics of the surface of the amorphous carbon film that, when cells are cultured on the carbon film, the cells that were cultured in a two-dimensionally dispersed state on the surface of the substrate immediately after the start of the culture can be aggregated over time to induce the formation of the cell aggregate.

[0028] In order to clarify the cell aggregation properties of the amorphous carbon film, the inventors attempted cell culture on amorphous carbon films formed by different film formation methods. An environment suitable for culture was prepared by placing a cloning ring on the surface of an amorphous carbon film (prepared by five types of film formation methods: HiPIMS, ionization, DC pulse CVD, and RFCVD (10 and 30 Pa)) formed on a Si substrate together with a PS-dish (a culture dish made of polystyrene) as a positive control, and NIH-3T3 cells (mouse-derived fibroblasts) were seeded therein, and the cell morphology (cell adhesion state and cell aggregation state) and the number of attached cells were evaluated after 24 hours of culture (Figure 1).

[0029] First, looking at the state of cell adhesion, which reflects cell affinity, it was confirmed that cells were uniformly attached to the amorphous carbon films formed using HiPIMS, ionization, DC pulse CVD, and RF CVD at 10 Pa. However, on the surface of the amorphous carbon film formed using RF CVD at 30 Pa, there were few cells adhering individually, and aggregations of two or more cells were clearly observed, with such aggregated cells occupying most of the culture area (Figure 5). When the total area of ​​aggregated cells observed on the positive control and the surfaces of various amorphous carbon films was compared, the area was 0.15 mm on average for the amorphous carbon film formed using RF CVD at 30 Pa. 2 As a result, at a p-value of 0.01, statistically significant differences were observed compared to all other groups (Figure 6).

[0030] On the other hand, the number of adherent cells, which quantitatively reflects the cell affinity of each amorphous carbon film, was the lowest for the amorphous carbon film deposited at 30 Pa RF CVD, and a statistically significant difference was observed only with the amorphous carbon film deposited by ionization, which had the highest number of counts, under the condition of p-value 0.01 (Fig. 7). However, there was no significant difference with the other three groups, and a large difference was confirmed between these three groups (amorphous carbon films deposited by HiPIMS, ionization, and DC pulse CVD), although the difference was not significant (Fig. 7). This is different in nature from the total area of ​​aggregated cells, which showed very little difference among groups other than the amorphous carbon film deposited at 30 Pa RF CVD (five groups including the positive control group) (Fig. 6).

[0031] This suggests that the cell aggregation ability of amorphous carbon films is not simply a phenomenon caused by poor cell affinity, but is a characteristic of the amorphous carbon film as a biointerface separate from cell affinity, and that since amorphous carbon films formed by different methods each have their own unique cell aggregation ability, it may be possible to determine the cell aggregation ability of an amorphous carbon film by measuring some index that reflects the basic structure of the amorphous carbon film and determining the cell aggregation ability of the amorphous carbon film based on a specified variable including the index.

[0032] Next, in order to find some index that reflects the basic structure of an amorphous carbon film and enables the determination of the cell aggregation ability of the amorphous carbon film, the inventors first measured the optical constants (refractive index and extinction coefficient), which are one of the candidates, for the above five types of amorphous carbon films that were formed. Figure 2 and Table 2 show the optical constants of various amorphous carbon films obtained by spectroscopic ellipsometry. The amorphous carbon film deposited by HiPIMS had the smallest refractive index of less than 2.0 compared to the other amorphous carbon films, but showed the largest extinction coefficient of 0.6 or more. On the other hand, the amorphous carbon film deposited by ionization tended to have the highest refractive index of 2.4 or more, but had a smaller extinction coefficient than HiPIMS. The extinction coefficient of DLC deposited by RF CVD 30 Pa was the smallest, less than 0.1.

[0033] Summarizing these, it was found that the extinction coefficient was greatest for the amorphous carbon film deposited by the PVD method (HiPIMS), followed by ionization, a deposition method that is intermediate between the PVD and CVD methods, and then DLC deposited by the CVD method (DC pulse CVD, RF CVD), with the order being HiPIMS > Ionization > DC pulse CVD > RF CVD 10 Pa > RF CVD 30 Pa (Table 2).

[0034] The difference in the optical constants of amorphous carbon films is due to the hydrogen content and sp 2 In addition to the content, it depends on the hardness and film density. 2 The hydrogen content is low, and there is a tendency for there to be a large number of electrons from the graphite structure. Amorphous carbon films formed by ionization, DC pulse CVD, and RF CVD use hydrocarbon gases, which contain hydrogen in the film, resulting in a smaller extinction coefficient than amorphous carbon films formed by HiPIMS. In addition, when CH is used as the source gas, 4 DLC films formed by RF CVD using HF are generally considered to have a high hydrogen content, and the source gas is C. 6 H 6It is considered that the extinction coefficient is smaller than that of amorphous carbon films formed by ionization using ionization and DC pulse CVD. In particular, it is considered that the hydrogen content was higher in the 30 Pa film formed by RF CVD than in the 10 Pa film, and the value of the extinction coefficient was the smallest. On the other hand, it has been reported that the film hardness and film density increase with increasing substrate bias voltage, and the hydrogen content is smaller than that of amorphous carbon films formed by general CVD methods. From these facts, it is considered that the refractive index and extinction coefficient of amorphous carbon films formed by ionization are larger than those of amorphous carbon films formed by DC pulse CVD and RF CVD. In addition, DC pulse CVD forms amorphous carbon films with higher hardness and lower hydrogen content than RF CVD, and therefore the refractive index and extinction coefficient values ​​are considered to be larger than those of RF CVD.

[0035] From the above, it was confirmed that the results of spectroscopic ellipsometry measurements show that the optical constants of various amorphous carbon films indicate the basic characteristics of amorphous carbon films formed by each individual film formation method, and in particular, the extinction coefficient is a value that reflects the difference in relative hydrogen content resulting from the film formation method.

[0036] In order to further investigate what kind of index the extinction coefficient serves as for the carbon film structure, the inventors performed Raman spectrum analysis on the above five types of amorphous carbon films and examined the relationship with the extinction coefficient (FIG. 3). -1 In the region of 1350 cm, a broad peak due to the amorphous structure was obtained. -1 Nearby are Dband and 1520~1580cm -1The Gband appears near the center of the Dband. In the amorphous carbon film (deposited by HiPIMS) with the largest extinction coefficient, the Dband peak appears prominently, and the Gband peak shifts to the higher wavenumber side. On the other hand, for the other amorphous carbon films, the Dband peak intensity decreases in the order of ionization, DC pulse CVD, and RF CVD (10 Pa, 30 Pa). It was also confirmed that the extinction coefficient of each amorphous carbon film decreases in this order, and that the central peak of the Gband shifts to the lower wavenumber side accordingly. In particular, it was confirmed that the amorphous carbon film deposited at 30 Pa with RF CVD, which has the smallest extinction coefficient, shifts to the lowest wavenumber side.

[0037] The Raman spectrum in Fig. 3 shows the sp 2 The cluster size determines the intensity of the Dband and the peak position of the Gband. Looking at the peak positions of the Gband for various amorphous carbon films, the Gband peak is at 1520 cm for RF CVD 30 Pa, which deposits aC:H films with a high hydrogen content, compared to HiPIMS. -1 The Gband shifts to the low wavenumber side to around 1000 nm. At this time, the intensity of the Dband also decreases. From these facts, it can be said that the amorphous carbon film with the Gband shifted to the low wavenumber side is sp 2 Cluster size and sp 2 It is considered that the bond ratio is low and the hydrogen content is high. That is, from Fig. 3, the amorphous carbon film formed by HiPIMS has sp 2 Cluster size and sp 2 The bond ratio was the highest, and the amorphous carbon film deposited at 30 Pa with RF CVD had sp 2 Cluster size and sp 2 It can be said that this is a structure with a low bonding ratio. In addition, the amorphous carbon films deposited by ionization, DC pulse CVD, and RF CVD at 10 Pa are considered to have an intermediate structure between those deposited by HiPIMS and RF CVD at 30 Pa, based on the peak position of Gband. From the above, and combining the results of the previous spectroscopic ellipsometry, the value of the extinction coefficient (k) and the sp2 Cluster size and sp 2 The ratio of hydrogen to the center frequency of the G band and the intensity of the D band of the Raman spectrum were correlated with each other. 2 Structural indicators, especially sp 2 It was confirmed that this is an index positively correlated with cluster size.

[0038] From the above evaluation, it was found that the extinction coefficient reflects the difference in the hydrogen content of the amorphous carbon film, and that the sp 2 It was found that the sp of the amorphous carbon film was positively correlated with the cluster size. 2 When the cluster size decreases and the number of CH terminations in the unbonded species increases, the inactivation of the film surface progresses and the cell aggregation on the film surface is expected to increase, so that the smaller the extinction coefficient (k) of the amorphous carbon film, the higher the cell aggregation ability is expected to be. Furthermore, when comparing the extinction coefficients of various amorphous carbon films and the total area of ​​aggregated cells showing cell aggregation ability (Figure 6), a correlation is found between the reciprocal of the extinction coefficient (k) (1 / k) and the total area, so the extinction coefficient is considered to be an index reflecting the basic structure of the amorphous carbon film, which enables the cell aggregation ability of the amorphous carbon film to be determined.

[0039] Here, the predetermined variable including an index reflecting the basic structure of the amorphous carbon film according to the first embodiment of the present invention will be described as a variable having the index as one or more terms in a mathematical and / or logical formula, and defined by a mathematical and / or logical formula composed of one or more of the terms. For example, in the above case, the extinction coefficient (k) is an index reflecting the basic structure of the amorphous carbon film, and the variable includes the index k as one term and is defined by the mathematical formula (1 / k), but is not limited thereto.

[0040] By spectroscopic ellipsometry, the refractive index (n) as well as the extinction coefficient (k) are measured as optical constants of the amorphous carbon film. Like the extinction coefficient, the refractive index of the amorphous carbon film is also an index that reflects the basic structure of the carbon film. The basic physical properties of the carbon film include the sp 3It indicates the amount of structure present (Non-Patent Document 2). That is, the higher the measured refractive index, the more inactivation of the film formation surface progresses and the greater the aggregability is expected to be, so the refractive index can be an index that reflects a basic structure different from the extinction coefficient and can be used to determine the cell aggregability of an amorphous carbon film. Therefore, when determining the cell aggregability of an amorphous carbon film, using the refractive index, in addition to the extinction coefficient, as an index that reflects the basic structure of the carbon film leads to improved accuracy of determination, and further, the refractive index can be analyzed together with the extinction coefficient by simultaneous measurement using spectroscopic ellipsometry, which is useful because it enables simple and rapid testing. In view of the above, another example of the first aspect of the present invention is a method for inspecting an amorphous carbon film, characterized in that the extinction coefficient (k) and the refractive index (n) are used as indices reflecting the basic structure of the amorphous carbon film, and the indices k and n are each considered as one term, and the cell aggregation function of the amorphous carbon film is determined based on a variable defined by the formula (n / k).

[0041] In order to search for an index reflecting the surface state, which is another characteristic that defines the basic structure of the amorphous carbon film according to the present invention, the inventors performed XPS analysis as a surface composition analysis of various amorphous carbon films. Figure 4 shows the XPS Carbon1s (C1s) spectrum. Table 3 shows the sp 2 The bond ratio and oxygen functional group ratio are shown. 2 The bond ratio was 54.8-67.3% for the amorphous carbon films formed by HiPIMS, ionization, and DC pulse CVD, which had relatively large extinction coefficients, and 43.3-48.2% for the RF CVD film. In addition, the full width at half maximum of the C1s peak was 1.64 eV, which was a relatively large value, for the amorphous carbon films formed by RF CVD. Table 3 shows the sp 2 The coupling ratio and full width at half maximum are shown.

[0042] Regarding the oxygen functional groups on the surface of various amorphous carbon films, the peak intensity due to oxygen functional groups in the vicinity of 286-289 eV tended to increase in the amorphous carbon films deposited by HiPIMS and ionization, which have relatively large extinction coefficients, and the composition ratio of carbonyl groups (C=O groups) and OC=O groups was high. On the other hand, as the extinction coefficient value decreased, the peak intensity due to oxygen functional groups in the vicinity of 286-289 eV tended to decrease, and in the amorphous carbon film deposited by RF CVD 30 Pa, the composition ratio of C=O groups and OC=O groups was the smallest compared to other amorphous carbon films.

[0043] In surface analysis by XPS, the depth region is about 5 nm at maximum. The sp 2 The ratio of the D band and the G band center peak value obtained by Raman spectroscopy showed a tendency to be high and low, respectively. 2 Cluster size and sp 2 The results of the XPS analysis show the same tendency as the relationship between the ratio of sp 2 It is shown that the higher the ratio, the larger the value of the extinction coefficient.

[0044] The formation of oxygen functional groups on the surface of the amorphous carbon film is believed to be the result of the surface being oxygen-terminated by exposure to the atmosphere after the amorphous carbon film is formed. 2 , CH sp 3 ) and CC sp 3 The following has been reported regarding the formation of oxygen functional groups and oxygen terminations for bonds. First, the bond energy of C-H bonds is greater than that of C-C bonds, so oxygen functional groups are less likely to be formed (Non-Patent Document 3). In an experiment on oxidation reactions by wet processing, CC sp 3 The bonds are difficult to oxidize and are chemically inactive (Non-Patent Document 4). In aC film with few hydrogen terminations, sp 2Due to the strain and geometrical relationship present in the bonds, many carbonyl groups (C=O groups) are formed (Non-Patent Document 5). From the above, the formation of oxygen functional groups on the surface of amorphous carbon films is as follows: 1) During film formation, the dangling bonds of carbon atoms are terminated with hydrogen (CH sp 2 , CH sp 3 1) In the case of the amorphous carbon film, oxygen termination does not progress after exposure to the atmosphere, and oxygen functional groups are not easily formed on the surface of the amorphous carbon film. 3 The bond is chemically inert and therefore stable against oxygen. 3) The hydrogen content is low and sp 2 It is assumed that in an amorphous carbon film with many bonds, oxygen termination progresses due to exposure to the atmosphere, and carbonyl groups (C=O groups) are easily formed on the surface of the amorphous carbon film.

[0045] From the above 1) to 3), like the aC membrane, sp 2 On the surface of amorphous carbon films with high bond ratio and low hydrogen content, many carbonyl groups (C=O groups) are formed, and sp 2 It is estimated that the formation of carbonyl groups (C=O groups) is small on the surface of an amorphous carbon film with a low bond ratio and a high hydrogen content. Therefore, in the amorphous carbon film formed at 30 Pa with RF CVD, which has the smallest extinction coefficient, sp 2 The carbonyl group (C=O group) composition ratio is the smallest due to the low bond ratio and high hydrogen content. On the other hand, the amorphous carbon films formed by HiPIMS and ionization have relatively large extinction coefficients. 2 The high bond ratio and low hydrogen content also suggest that the carbonyl group (C=O group) composition ratio is large. In addition, in carbon materials such as graphite, sp 2It has been reported that on the surface of six-membered ring clusters derived from bonds (C=C), oxygen functional groups such as CO, C=O, and -COC- groups are formed by oxygen termination, and in particular, carbonyl groups (C=O groups) are formed by stabilization of -COC- groups due to strain relaxation of six-membered ring clusters (Non-Patent Document 6). From these findings, it is believed that the formation process of carbonyl groups (C=O groups) on the surfaces of various amorphous carbon films is sp 2 It is considered that the extinction coefficient reflects the cluster size and the state of hydrogen content. 2 The bond size increases with the number of π electrons contained in the bond, and the formation of a carbonyl group (C=O group) is thought to be induced by the stabilization of the -COC group formed by the destruction of the π electron conjugated system by oxidation.

[0046] From the above, it is expected that the lower the measured value of the carbonyl group (C=O group) composition ratio (CO), the more inactivation of the film formation surface progresses and the more coagulable the film is, so the carbonyl group (C=O group) composition ratio can be an index reflecting the basic structure other than the optical constants, which can be used to determine the cell coagulation ability of an amorphous carbon film. Therefore, in addition to the extinction coefficient and refractive index, using the carbonyl group (C=O group) as an index reflecting the basic structure of the carbon film when determining the cell coagulation ability of an amorphous carbon film will lead to further improvement in the accuracy of the determination. Thus, yet another example of the first aspect of the present invention is a method for inspecting an amorphous carbon film, characterized in that the extinction coefficient (k), refractive index (n) and carbonyl group (C=O group) composition ratio (CO) are used as indexes reflecting the basic structure of the amorphous carbon film, and the indexes k, n and CO are each considered as one term, and the cell aggregation function of the amorphous carbon film is determined based on a variable defined by the formula (n / (k×CO)).

[0047] Table 4 shows the calculated values ​​of (1 / k), (n / k) and (n / (k×CO)) for the amorphous carbon films formed by various film forming methods. In all three variables, the only amorphous carbon film having significant cell aggregation ability is the amorphous carbon film formed at RF CVD 30 Pa. Therefore, the boundary value at which it can be determined that the amorphous carbon film has a suitable cell aggregation function is a numerical value located between the calculated value for the amorphous carbon film formed at RF CVD 30 Pa and the calculated value for the amorphous carbon film formed at RF CVD 10 Pa, which has the next cell aggregation ability, although it is not significant. That is, as long as each is a numerical value located between the calculated values, it is not particularly limited, but the variable (1 / k) is preferably 7 or more, particularly preferably 11 or more, the variable (n / k) is preferably 13 or more, particularly preferably 23 or more, and the variable (n / (k×CO)) is preferably 565 or more, particularly preferably 2573 or more. However, since a person skilled in the art can determine appropriate boundary values ​​according to the present invention by examining in preliminary experiments the extinction coefficient, refractive index, and carbonyl group composition ratio of the amorphous carbon film to be inspected, which is formed under various film formation conditions, and the cell aggregation property on the amorphous carbon film, the appropriate boundary values ​​according to the present invention are not necessarily limited to the above-mentioned boundary values.

[0048] A second aspect of the present invention is a method for producing a product including an amorphous carbon film as a part of its configuration, characterized by comprising an inspection step of determining that the amorphous carbon film that is the subject of the inspection method according to the first aspect and / or an inspection method in which the inspection method according to the first aspect is limited to any one of the conditions described above has a suitable cell aggregation function.

[0049] Here, "having suitable cell aggregation ability" means that a person skilled in the art can set a boundary value between "suitable" and "unsuitable" in the above-mentioned inspection method for each product that contains as part of its composition the amorphous carbon film that is the subject of the present invention, and so there is no particular limitation to this. For example, the boundary value of the inspection method may be set based on the presence or absence of a statistically significant difference, and a product having an evaluation value exceeding this boundary value may be defined as having suitable cell aggregation ability.

[0050] The product containing the amorphous carbon film according to the present invention as a part of its configuration may be any product that has an amorphous carbon film as a part of its configuration and exhibits the cell aggregation ability of the amorphous carbon film as a function of the product, but may be a product that is used particularly when culturing cells due to its cell aggregation property. Examples of such products include flasks, tissue culture flasks, culture dishes, tissue culture dishes, multi-dishes, microplates, microwell plates, multi-plates, multi-well plates, chamber slides, petri dishes, tubes, trays, culture bags, microcarriers, beads, stack plates, spinner flasks, and roller bottles, but are not limited thereto. In addition, a person skilled in the art can appropriately select a product according to the scale of culture, culture conditions, and culture period. Furthermore, it is preferable that these products have a certain degree of cell adhesiveness in order to enable adhesion culture in a two-dimensional state necessary for ultimately inducing cell aggregates.

[0051] In the manufacturing method according to the present invention, the inspection step for determining the cell aggregation function of a product containing an amorphous carbon film as a part of its configuration may be carried out after the completion of all steps of the manufacturing process, or may be carried out after the film formation step during the manufacturing process. In either manufacturing method, the cell aggregation ability of the amorphous carbon film is inspected by measurement using spectroscopic ellipsometry and / or photoelectric spectroscopy, which improves the reliability of the product and allows feedback to be provided to the film formation step of the amorphous carbon film. EXAMPLES

[0052] Examples are shown below. These are merely illustrative and do not limit the scope of the present invention, and various improvements and design changes may be made without departing from the spirit of the present invention.

[0053] 1. Experiments on the deposition of amorphous carbon films using various deposition methods 1-1. Overview A total of five types of amorphous carbon films with different basic structures were deposited on Si substrates using the High Power Impulse Magnetron Sputtering method (HiPIMS), the ionization deposition method (Ionization), the DC Pulse Plasma Chemical Vapor Deposition method (DC pulse CVD), and the radio frequency (rf) Plasma CVD method (RF CVD).

[0054] 1-2. Experimental method In the HiPMS method, a graphite target was used as the raw material. In the ionization method and DC pulse CVD method, benzene (C 6 H 6 ) was used, and CH 4 The DLC film was formed using the gas as the source material. For RF CVD, the source gas was deposited at 10 Pa and 30 Pa (hereinafter referred to as RF CVD 10 Pa and RF CVD 30 Pa). Table 1 shows the deposition conditions for the amorphous carbon film used in this experiment. [Table 1] Table 1. Deposition conditions for various amorphous carbon films

[0055] 1-3.Results Various amorphous carbon films were formed by five different film formation methods. The carbon films were used in the following experiments.

[0056] 2. Measurement of optical constants of various amorphous carbon films using spectroscopic ellipsometry 2-1. Overview As a fundamental structural analysis of the five types of amorphous carbon films formed in the above 1, the optical constants were measured by spectroscopic ellipsometry.

[0057] 2-2. Experimental method The optical constants of the amorphous carbon film were measured from the wavelength change of the amplitude reflectance and phase difference using a spectroscopic ellipsometer (AutoSE, HORIBA). Spectroscopic ellipsometry is a method for calculating the film thickness and optical constants of films consisting of single and multilayers based on polarization measurement. The measurement conditions were an incidence angle of 70 degrees, a wavelength range of 450 to 1000 nm, and a step width of 2.2 nm, and the extinction coefficient k and refractive index n were evaluated by fitting the amplitude reflectance and phase difference to an optical model of the amorphous carbon film.

[0058] 2-3.Results The optical constants (extinction coefficient k and refractive index n) of five types of amorphous carbon films were measured by spectroscopic ellipsometry (Figure 2 and Table 2). [Table 2] Table 2 Optical constants (extinction coefficient k and refractive index n) of various amorphous carbon films

[0059] 3. Structural analysis of various amorphous carbon films using Raman spectroscopy 3-1. Overview As a basic structural analysis of the five types of amorphous carbon films formed in the above 1, structural analysis was carried out by Raman spectroscopy.

[0060] 3-2. Experimental method The amorphous carbon film was subjected to Raman spectroscopy for structural analysis. The analysis conditions were: excitation source: Ar, excitation wavelength: 532 nm, aperture: 25 μm, irradiation intensity: 12.5 mW, measurement range: 800–2000 cm -1 The number of measurements was three. That is, the surface of the amorphous carbon film was irradiated with a 532 nm laser with an Ar excitation source, and the scattered light was detected at 1000 to 1800 cm -1 Six-membered ring clusters (sp 2 The film structures of various amorphous carbon films were evaluated from the relationship between the peak position of the G band, which reflects the size of carbon, and the intensity of the D band, which indicates defects of six-membered ring clusters.

[0061] 3-3.Results The Raman spectra of five types of amorphous carbon films were measured by Raman spectroscopy (Figure 3). All of the amorphous carbon films had a peak in the range of 1000 to 1800 cm -1 In the region, a broad peak due to the amorphous structure was observed, and a peak at 1350 cm -1 Nearby and 1520~1580cm -1 D band and G band were confirmed nearby.

[0062] 4. Surface composition analysis of various amorphous carbon films using XPS analysis 4-1. Overview As a basic structural analysis of the five types of amorphous carbon films formed in the above 1, surface composition analysis was performed by XPS analysis.

[0063] 4-2. Experimental method The surface composition was analyzed by X-ray photoelectron spectroscopy (XPS, JPS-9000MC, JEOL) to obtain the Carbon 1s (C1s) spectrum and perform waveform separation. The analysis conditions were: radiation source; Mg Kalpha, acceleration voltage; 10 kV, acceleration current; 10 mA, number of scans; 20. The C1s spectrum was corrected for charging and sp 2 Bond(284.0±0.35eV),sp 3 Waveform separation was performed for bonds (284.7±0.2 eV), CO (285.8 eV), C=O (287.1 eV), and OC=O (289.0 eV), and the sp 2 Bonding ratio (sp 2 / (sp 2 +sp 3 )) and the composition ratio of oxygen functional groups were evaluated.

[0064] 4-3.Results The C1s spectra of five types of amorphous carbon films were measured by XPS analysis (Figure 4). In addition, the sp 2 The bond ratio, oxygen functional group composition ratio and full width at half maximum were calculated (Table 3). [Table 3] Table 3 sp of various amorphous carbon films 2 Bond ratio, oxygen functional group ratio and full width at half maximum

[0065] 5. Cell aggregation and adhesion properties of various amorphous carbon films 5-1. Overview In order to investigate the cell aggregation and cell adhesion properties of various amorphous carbon films, the five types of amorphous carbon films described in 1 above were formed on a Si substrate, and cells were cultured on the surface of each carbon film. After 24 hours, the cell morphology was observed, and the total area of ​​aggregated cells and the number of adherent cells were measured.

[0066] 5-2. Experimental method 5-2-1.Culture method A cloning ring (RING 07, IWAKI) with a diameter of 5 mm was placed on the surface of an amorphous carbon film (HiPIMS, Ionization, DC pulse CVD, RF CVD (10, 30 Pa)) formed on a Si substrate, and 3000 NIH-3T3 cells (mouse-derived fibroblasts) were seeded in it. The cell morphology, total area of ​​aggregated cells, and number of attached cells were evaluated after 24 hours of culture. Other culture conditions were medium type and amount: DMEM (High Glucose) 0.1 mL, CO 2 The cells were cultured at a concentration of 5%, at a temperature of 37°C, and at a humidity of 100%. The state of the culture is shown in Figure 1. As a positive control, a cloning ring was also placed on a PS-dish (VTC-D60, VIOLAMO) and cultured in the same manner.

[0067] 5-2-2. Observation of cell morphology The cloning ring was removed, and a cover glass was placed on the ring to observe the cells. The cells were observed using a metallurgical microscope (BX51M, Olympus), and the four corners of the cloning ring were photographed using a digital camera (COOLPIX A9000, Nikon), and the images (1202 × 934 pixels) were saved. The images were then cropped to 710 × 600 pixels using ImageJ (Ver. ImageJ 2.0.-rc-69 / 1.52p / Java 1.8.0_172). The photographing conditions were: microscope magnification: 10x, focus: 3.5, mode: close-up (macro). Figure 1 shows a schematic diagram of the photographing and evaluation ranges. In this evaluation, the center was deliberately excluded from the evaluation target, taking into account the distribution of seeded cells due to the surface tension (meniscus) inside the cloning ring. It was confirmed that the number of cells in the center tends to be lower due to the meniscus.

[0068] 5-2-3. Measurement of total area of ​​aggregated cells and number of adherent cells Within the images obtained using ImageJ, areas with a gray value of 170 or more were regarded as the amorphous carbon film surface, and image processing was used to separate cells into single adherent cells and aggregated cells. Aggregated cells were considered to be areas where two or more cells were densely packed together, and their area was calculated. Furthermore, the number of adherent cells was determined by counting the single cells on the DLC surface other than aggregated cells using ImageJ's Cell counter. The measurement range was pixel count: horizontal 710, vertical 600, actual area: 1.58 x 1.33 mm 2 The evaluation range was four regions, top, bottom, left and right, as shown in Figure 1. The area of ​​aggregated cells and the number of adherent cells were measured, and the average values ​​were calculated from three trials, and a significance test was performed using the Tukey-Kramer method (critical value p = 0.01, number of trials n = 3).

[0069] 5-3.Results The total area of ​​aggregated cells (FIG. 6) and the number of adherent cells (FIG. 7) in cultured cells on the five types of amorphous carbon films and the positive control were measured.

[0070] 6. Examination of variables including indices reflecting the basic structure of amorphous carbon films 6-1. Overview From the indices (extinction coefficient k, refractive index n, and carbonyl group composition ratio CO) reflecting the basic structure of each amorphous carbon film and the cell aggregation ability obtained from the above experiments, variables including the indices that are suitable for determining the cell aggregation ability of an amorphous carbon film were examined.

[0071] 6-2.Results Taking into consideration the physical properties and cell aggregation ability (indicated by ○, △, and ×) of each amorphous carbon film, i.e., the extinction coefficient k, refractive index n, and carbonyl group composition ratio CO, we investigated variables suitable for determining the cell aggregation ability of amorphous carbon films, including these indicators (Table 4). [Table 4] Table 4. Consideration of variables including indicators reflecting the basic structure of amorphous carbon films [Industrial Applicability]

[0072] The method for inspecting an amorphous carbon film according to the present invention, which is characterized by measuring an index reflecting the basic structure of the amorphous carbon film and determining the cell aggregation function of the amorphous carbon film based on a predetermined variable including the index, makes it possible to non-destructively determine the presence or absence and / or strength of the cell aggregation ability of the amorphous carbon film, which is a property of the amorphous carbon film as a biointerface that is distinct from cell affinity, by simple and rapid measurements such as spectroscopic ellipsometry and / or photoelectric spectroscopy. Furthermore, in a second embodiment of the present invention, a method for producing a product including an amorphous carbon film as a part of its configuration, characterized in that it includes an inspection step of determining by the inspection method that the amorphous carbon film that is the subject of the inspection method has a suitable cell aggregation function, the cell aggregation ability of the amorphous carbon film is inspected by measurement using spectroscopic ellipsometry and / or photoelectric spectroscopy, thereby improving the reliability of the product and enabling feedback to the film formation step of the amorphous carbon film.

Claims

1. An inspection method for an amorphous carbon film, characterized in that an index reflecting the basic structure of the amorphous carbon film is an extinction coefficient k, the index is measured, a variable including the index is the reciprocal of the extinction coefficient k (1 / k), and the cell aggregation function of the amorphous carbon film is determined based on the variable.

2. 2. The inspection method according to claim 1, wherein the amorphous carbon film is determined to have a suitable cell aggregation function when the value obtained by 1 / k is 7 or more.

3. 2. The inspection method according to claim 1, wherein the indices are an extinction coefficient k and a refractive index n, and the variable is n / k.

4. 4. The inspection method according to claim 3, wherein the amorphous carbon film is judged to have a suitable cell aggregation function when the value obtained by n / k is 13 or more.

5. 2. The inspection method according to claim 1, wherein the indices are an extinction coefficient k, a refractive index n, and a carbonyl group composition ratio CO, and the variable is n / (k×CO).

6. 6. The inspection method according to claim 5, wherein the amorphous carbon film is determined to have a suitable cell aggregation function when the value obtained by n / (k×CO) is 565 or more.

7. An inspection method according to claim 1, wherein k is measured by spectroscopic ellipsometry.

8. An inspection method according to claim 3, wherein n is measured by spectroscopic ellipsometry.

9. The inspection method described in claim 5 or 6, characterized in that the CO is measured by X-ray photoelectron spectroscopy.

10. A method for producing a product including an amorphous carbon film as a part of its configuration, comprising an inspection step of determining, by the inspection method according to any one of claims 1 to 9, that the amorphous carbon film to be inspected has a suitable cell aggregation function.

Citation Information

Patent Citations

  • Balloon catheter

    JP2008245883A

  • Proliferation inhibiting material of smooth muscle cell

    JP2010280636A

  • Implant, method of manufacturing the same, and bone metabolism control method

    JP2014004166A

  • Program, information processing apparatus, and information processing method