Sheet
A glass fiber fabric impregnated with a cured resin layer containing brominated bisphenol A vinyl ester and a monofunctional (meth)acrylate with an alkylene oxide group addresses stickiness and bending durability issues, ensuring improved adhesiveness and fire-resistant transparency in smoke-proof hanging walls.
Patent Information
- Application Number
- JP2022203397
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-20
AI Technical Summary
Existing smoke-proof hanging walls made of transparent resin composites and polycarbonate sheets suffer from issues such as stickiness on cured resin layers, poor adhesiveness of thermoplastic resin layers, and poor bending durability, which affect their usability and performance in fire safety applications.
A sheet comprising a glass fiber fabric impregnated with a cured resin layer formed from a resin composition containing brominated bisphenol A type vinyl ester resin and a monofunctional (meth)acrylate with an alkylene oxide group and no aromatic ring, which suppresses stickiness and enhances bending durability.
The solution provides a sheet with improved adhesiveness, reduced stickiness, and enhanced bending durability, maintaining transparency and fire-resistant properties, making it suitable for smoke-proof applications.
Smart Images

Figure 0007576857000006 
Figure 0007576857000007 
Figure 0007576857000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a seat. [Background technology]
[0002] The Building Standards Act and its Enforcement Order prescribe that smoke exhaust systems must be installed to prevent the flow of smoke and toxic gases that are generated in the event of a fire in a building, and to facilitate evacuation and firefighting activities. Therefore, office buildings, commercial facilities, and other buildings often have smoke barriers and other equipment installed as smoke exhaust and smoke blocking systems.
[0003] Smoke barriers are usually installed on the ceilings of buildings to temporarily block the flow of smoke and toxic gases to corridors and upper floors in the event of a fire, thereby ensuring the time required for evacuation. For this reason, transparent plate glass, transparent resin composites of glass fiber and resin, etc. are used as smoke barriers so that the smoke barriers do not obstruct visibility or spoil the aesthetic appearance. Transparent resin composites of glass fiber and resin have the advantage of being less likely to break than transparent plate glass.
[0004] Known as the above-mentioned transparent resin composite is a sheet including at least one glass fiber fabric and a pair of cured resin layers sandwiching the glass fiber fabric, wherein the glass fiber fabric accounts for 20 to 70% by weight, the pair of cured resin layers accounts for 80 to 30% by weight, the difference in refractive index between a glass composition constituting the glass fibers in the glass fiber fabric and a resin composition constituting the pair of cured resin layers is 0.02 or less, and the difference in Abbe number between the glass composition constituting the glass fibers in the glass fiber fabric and the resin composition constituting the pair of cured resin layers is 30 or less (see, for example, Patent Document 1).
[0005] Also known is a non-flammable sheet having at least one glass fiber fabric and a photocurable resin impregnated into the glass fiber fabric, wherein the difference in refractive index between a glass composition constituting the glass fibers in the glass fiber fabric and the photocurable resin is 0.02 or less, the ratio of the glass fiber fabric to the non-flammable sheet is 20 to 70% by weight, the ratio of the photocurable resin to the non-flammable sheet is 80 to 30% by weight, and the photocurable resin is obtained by curing a composition containing at least brominated bisphenol A vinyl ester (see, for example, Patent Document 2).
[0006] A first polycarbonate sheet layer containing 5% by mass to 20% by mass of bromine and having a thickness of 100 μm to 150 μm and a laminated laminate having a basis weight of 30 g / m 2 ~80g / m 2 A transparent noncombustible sheet having a thickness of 300 μm to 400 μm is known, which is composed of a laminate including a cured resin composition layer containing a cured resin composition containing 10% by mass to 30% by mass of bromine impregnated into a glass fiber fabric, and a second polycarbonate sheet layer having a thickness of 100 μm to 150 μm and containing 5% by mass to 20% by mass of bromine laminated on the cured resin composition layer (see, for example, Patent Document 3). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent Publication No. 2005-319746 [Patent Document 2] Patent Publication No. 2014-213489 [Patent Document 3] Patent Publication No. 2020-1172 Summary of the Invention [Problem to be solved by the invention]
[0008] The present inventors have found that the sheet disclosed in Patent Document 1 may have a sticky surface on the cured resin layer after the cured resin layer is cured. If the sticky surface occurs, for example, when the sheet is made into a roll product, it may be difficult to pull out the sheet. In addition, the inventors have found that there is a problem in that when a thermoplastic resin layer such as a film layer is laminated on the cured resin layer for the purpose of improving the tear strength of the sheet, the adhesiveness of the thermoplastic resin layer is likely to be poor.
[0009] The present inventors also found that the noncombustible sheet disclosed in Patent Document 2 and the transparent noncombustible sheet disclosed in Patent Document 3 have a problem in that the cured resin layer impregnated in the glass fiber fabric may have poor folding resistance. Specifically, the inventors found that when the sheet is repeatedly bent, it is prone to breakage, resulting in poor folding resistance.
[0010] Therefore, a main object of the present invention is to solve the above problems and to provide a cured resin layer impregnated in a glass fiber fabric that is less sticky and has excellent folding resistance. [Means for solving the problem]
[0011] The present inventors have studied the above problem, and have found that, in Patent Document 1, only a so-called bisphenol A type vinyl ester resin made from a bisphenol A type epoxy resin is used as the curable resin for forming the cured resin layer. The inventors have found that when a bisphenol A type vinyl ester resin is used alone as the curable resin for forming the cured resin layer, the curing reaction proceeds relatively slowly, and the surface of the cured resin layer may become sticky.
[0012] On the other hand, the present inventors have found that when the cured resin layer contains a so-called brominated bisphenol A type vinyl ester resin, which is made from a brominated bisphenol A type epoxy resin among vinyl ester resins, the curing reaction proceeds relatively easily, and the stickiness occurring on the surface of the cured resin layer can be suppressed. However, the refractive index of the brominated bisphenol A type vinyl ester resin is considerably higher than that of the glass fiber fabric. Therefore, simply impregnating the glass fiber fabric with the brominated bisphenol A type vinyl ester resin does not have a similar refractive index to that of the glass fiber fabric, and the obtained sheet has poor transparency. Therefore, when the brominated bisphenol A type vinyl ester resin is contained, it is necessary to also contain a material with a relatively low refractive index in the cured resin composition in order to make the refractive index of the cured resin layer similar to that of the glass fiber fabric.
[0013] In this regard, Patent Document 2 discloses the use of neopentyl glycol dimethacrylate, which is a bifunctional methacrylate, as a refractive index modifier for brominated bisphenol A vinyl ester resin. Patent Document 3 discloses the use of phenoxyethyl acrylate and 2-ethylhexyl acrylate. However, the present inventors have found that when these refractive index modifiers are contained in the brominated bisphenol A vinyl ester resin, the folding resistance of the cured resin layer tends to deteriorate.
[0014] Therefore, the present inventors conducted extensive research and found that the above problems can be solved by forming the cured resin layer from a cured product of a resin composition containing (A) a brominated bisphenol A type vinyl ester resin and (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring. The present invention was completed based on this finding and through further extensive research.
[0015] That is, the present invention provides the following aspects. Item 1. A sheet comprising a glass fiber fabric and a cured resin layer impregnated in the glass fiber fabric, the cured resin layer being formed from a cured product of a resin composition comprising (A) a brominated bisphenol A type vinyl ester resin and (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring. Item 2. The sheet according to item 1, wherein the number of moles of the alkylene oxide groups added is 2 to 10. Item 3. The sheet according to item 1 or 2, wherein a thermoplastic resin layer is laminated on the cured resin layer. Item 4. The sheet according to any one of items 1 to 3, wherein the sheet has a total light transmittance of 80% or more and a haze of 20% or less. Term 5.50kW / m 2 When subjected to a heat generation test in which the material was irradiated with radiant heat of 8 MJ / m for 20 minutes after the start of heating, the total heat generation was 8 MJ / m 2 The sheet according to any one of claims 1 to 4, wherein: Item 6.50kW / m 2 When subjected to a heat generation test in which the material is irradiated with radiant heat of 200 kW / m for 20 minutes after heating begins, the heat generation rate continues for 10 seconds or more. 2 The sheet according to any one of items 1 to 5, wherein the sheet does not exceed 100 mm. Effect of the Invention
[0016] The sheet of the present invention comprises a glass fiber fabric and a cured resin layer impregnated in the glass fiber fabric, and the cured resin layer is formed from a cured product of a resin composition containing (A) a brominated bisphenol A type vinyl ester resin and (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring, and therefore the sheet is less sticky and has excellent folding resistance. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating one embodiment of a sheet of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view illustrating one embodiment of a sheet of the present invention. [Diagram 3] This is a diagram showing an overview of the test equipment used when conducting "4.9.2 Heat generation test" in the "Fire resistance performance test and evaluation procedure manual" (revised version on July 1, 2021) of the General Incorporated Foundation Building Materials Testing Center. [Figure 4] This is a schematic diagram of the test holder and holding frame included in the test equipment used to perform "4.9.2 Heat generation test" in the "Fire resistance test and evaluation procedure manual" (revised on July 1, 2021) of the General Incorporated Foundation Building Materials Testing Center. The units of values (dimensions) shown in Figure 4 are mm. [Diagram 5] FIG. 2 is a schematic plan view illustrating a method for measuring tear strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The sheet of the present invention is a sheet comprising a glass fiber fabric and a cured resin layer impregnated in the glass fiber fabric, wherein the cured resin layer is formed from a cured product of a resin composition comprising (A) a brominated bisphenol A type vinyl ester resin and (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring.
[0019] For example, as shown in FIGS. 1 and 2, a sheet 1 of the present invention comprises a glass fiber fabric 2 and a cured resin layer 3 impregnated in the glass fiber fabric 2, and the cured resin layer 3 is formed from a cured product of a resin composition containing (A) a brominated bisphenol A type vinyl ester resin and (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring.
[0020] The sheet 1 of the present invention may contain at least one glass fiber fabric 2, or may contain multiple glass fiber fabrics 2. As shown in Figs. 1 and 2, in the sheet 1 of the present invention, the cured resin layer 3 fills gaps between the glass fibers constituting the glass fiber fabric 2, and one surface side portion of the cured resin layer 3 communicates with the other surface side portion via the gaps. The sheet 1 of the present invention may contain multiple cured resin layers 3. One cured resin layer 3 may contain multiple glass fiber fabrics 2.
[0021] In the sheet 1 of the present invention, layers other than the cured resin layer 3 may be provided. For example, as shown in FIG. 2, the sheet 1 of the present invention may include a thermoplastic resin layer 4. It is preferable that the thermoplastic resin layer 4 is included on the outer side of the cured resin layer 3. In addition, when the thermoplastic resin layer 4 is provided, another layer may be provided between the cured resin layer 3 and the thermoplastic resin layer 4, and the other layer may be, for example, an adhesive layer. Each layer constituting the sheet 1 of the present invention will be described in detail below.
[0022] [Glass fiber fabric 2] In the sheet 1 of the present invention, the glass fiber fabric 2 is included in a state in which it is impregnated with the cured resin layer 3 described later. In the sheet 1 of the present invention, the glass fiber fabric 2 contributes to improving the fire retardancy of the sheet. The refractive index of the glass fiber fabric 2 can be set to be close to the refractive index of the cured resin layer 3 described later, and this allows the sheet 1 of the present invention to have a total light transmittance of 80% or more and a haze of 20% or less, which are preferable indexes of transparency, as described later. In other words, the total light transmittance of 80% or more and a haze of 20% or less, which are preferable indexes of transparency, of the sheet 1 of the present invention, at least indicates that the refractive index of the glass fiber fabric 2 and the refractive index of the cured resin layer 3 described later are sufficiently close (for example, the difference between the refractive index of the glass fiber fabric 2 and the refractive index of the cured resin layer 3 is 0.02 or less).
[0023] In the sheet 1 of the present invention, the weave of the glass fiber fabric 2 is not particularly limited, and examples thereof include plain weave, satin weave, twill weave, basket weave, and rib weave, with plain weave being preferred.
[0024] The glass material of the glass fibers constituting the glass fiber fabric 2 is not particularly limited, and for example, known glass materials can be used. Examples of glass materials include alkali-free glass (E glass), acid-resistant alkali-containing glass (C glass), high-strength, high-elasticity glass (S glass, T glass, etc.), and alkali-resistant glass (AR glass), and preferably includes highly versatile alkali-free glass (E glass). The glass fibers constituting the glass fiber fabric 2 may be made of one type of glass material, or may be a combination of two or more types of glass fibers made of different glass materials. In addition, from the viewpoint of improving transparency, it is preferable to select a glass material that is close to the refractive index of the cured resin layer 3 described later.
[0025] The count of the glass fibers constituting the glass fiber fabric 2 is not limited to a specific one as long as the glass fiber fabric 2 can be formed. From the viewpoint of further improving transparency, the count of the glass fibers is preferably 20 tex or less, more preferably 3 to 6 tex, and more preferably 3 to 5 tex. The count of the glass fibers may be one type alone or two or more types may be combined. The tex count of the glass fibers corresponds to the number of grams per 1000 m.
[0026] The glass fibers constituting the glass fiber fabric 2 are preferably glass yarns in which a plurality of single fibers, which are long glass fibers, are twisted together. The number of single fibers in the glass yarn is preferably about 30 to 400, and more preferably about 40 to 120. The diameter of the single fiber in the glass yarn is preferably about 3.0 to 6.0 μm, and more preferably about 3.0 to 5.0 μm, from the viewpoint of further improving the transparency of the sheet 1 while improving the non-combustibility of the sheet 1. The count of the glass yarn is preferably 2 to 30 tex, more preferably 2 to 12 tex, and even more preferably 2 to 6 tex, from the viewpoint of further improving the transparency of the sheet 1 while improving the non-combustibility of the sheet 1.
[0027] In the sheet 1, the total mass (g / m 2 ) and the total mass (g / m 2 , except for glass fiber fabric 2.) 2 The ratio (mass %) of the total mass of the glass fiber fabric 2 in the sheet 1 to the total mass (g / m2) of the sheet 1 is preferably 20 to 60 mass %, more preferably 30 to 60 mass %, from the viewpoint of further improving both transparency and non-combustibility when the resin weight in the sheet is increased. 2 ) to the total mass (g / m 2 The proportion (mass %) of 5 to 60 mass % is preferable from the viewpoint of achieving a further improvement in both transparency and non-combustibility.
[0028] The difference in refractive index between the glass fiber fabric 2 and the cured resin layer 3 described below is preferably 0.02 or less, and more preferably 0.01 or less. The refractive index of the glass fiber fabric 2 is preferably about 1.50 to 1.58, and more preferably about 1.53 to 1.57.
[0029] The refractive index of the glass fiber fabric 2 is measured in accordance with the B method of the Japanese Industrial Standard JIS K 7142:2008. Specifically, the glass fibers constituting the glass fiber fabric are crushed to an extent that the Becke lines can be observed when observed with an optical microscope at a magnification of 400 times. Then, a halogen lamp with an interference filter for D line is used as a light source, and the optical microscope is used to observe and measure under conditions of a magnification of 400 times and a temperature of 23°C, and the average value of three tests is taken as the refractive index value. The refractive index of the cured resin layer 3 is measured in accordance with the B method of the Japanese Industrial Standard JIS K 7142:2008. Specifically, the cured resin layer 3 is crushed to an extent that the Becke lines can be observed when observed with an optical microscope at a magnification of 400 times. Then, a halogen lamp with an interference filter for D line is used as a light source, and the optical microscope is used to observe and measure under conditions of a magnification of 400 times and a temperature of 23°C, and the average value of three tests is taken as the refractive index value.
[0030] The difference in Abbe number between the glass fiber fabric 2 and the cured resin layer 3 is preferably not more than 30, more preferably not more than 20, and even more preferably not more than 10. The Abbe number of the glass fiber fabric 2 is preferably from 30 to 80, more preferably from 40 to 70, and even more preferably from 50 to 65. The Abbe numbers of the cured resin layer 3 and the glass fiber fabric 2 are each measured as follows.
[0031] (Abbe number of cured resin layer 3) A sheet not including the glass fiber fabric 2 was prepared using the resin constituting the cured resin layer 3, with a width of 8 mm, a length of 20 mm, and a thickness of 1 mm, and measured in accordance with the Japanese Industrial Standard JIS K 7142A method using an Abbe refractometer manufactured by Atago Co., Ltd., DR-M2, diiodomethane as the contact liquid, and D-line (589 nm), F-line (486 nm), and C-line (656 nm) as interference filters at a measurement temperature of 23° C. The refractive indices of the D-line, F-line, and C-line were measured, and the Abbe number was calculated according to the following formula (I). Abbe number = (n D -1) / (n F -n C ) (I) n D : Refractive index at D line n F : Refractive index at F line n C : Refractive index at C line
[0032] (Abbe number of glass fiber fabric 2) A glass fiber was fabricated using the glass material constituting the glass fiber with a width of 8 mm, length of 20 mm, and thickness of 1 mm, and in accordance with the Japanese Industrial Standard JIS K 7142A method, an Abbe refractometer manufactured by Atago Co., Ltd., DR-M2 was used as the Abbe refractometer, diiodomethane was used as the contact liquid, and D line (589 nm), F line (486 nm), and C line (656 nm) were used as interference filters, and the measurement temperature was set at 23° C. The refractive indexes of the D line, F line, and C line were measured, and the Abbe number was calculated according to the following formula (I). Abbe number = (n D -1) / (n F -n C ) (I) n D : Refractive index at D line n F : Refractive index at F line n C : Refractive index at C line
[0033] The thickness of each sheet of the glass fiber fabric 2 is, for example, about 10 to 100 μm, preferably about 10 to 55 μm, and more preferably about 10 to 35 μm, from the viewpoint of improving the flame retardancy of the sheet 1 and further improving the transparency of the sheet 1. The thickness of each sheet of the glass fiber fabric 2 is a value measured in accordance with the method A specified in "7.10.1 Cloth thickness" of the Japanese Industrial Standard JIS R3420:2013 "General test method for glass fibers". The mass of each sheet of the glass fiber fabric 2 is, for example, 10 to 60 g / m 2 , preferably 25 to 50 g / m 2 , more preferably 25 to 35 g / m 2When the thickness of the glass fiber fabric 2 is 10 to 35 μm, it is particularly preferable that the glass fiber fabric 2 has a glass volume fraction of 38% or more, as calculated by the following formula (II). The glass fiber fabric 2 having a thickness of 10 to 35 μm and a glass volume fraction of 38% or more can be obtained, for example, by subjecting a glass fiber fabric to an opening treatment.
[0034] Glass volume ratio (%) = (A / (B×C))×100 (II) A: Mass of glass fiber fabric (g / m 2 ) B: Specific gravity of the glass material that composes the glass fiber fabric (g / m 3 ) C: Thickness of the glass fiber fabric (m)
[0035] [Cured resin layer 3] The sheet of the present invention comprises a cured resin layer impregnated in a glass fiber fabric, and the cured resin layer is formed from a cured product of a resin composition containing (A) a brominated bisphenol A type vinyl ester resin and (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring.
[0036] As described above, the present inventors have found that when the cured resin layer contains (A) brominated bisphenol A vinyl ester resin, the curing reaction proceeds relatively easily, and the stickiness occurring on the surface of the cured resin layer can be suppressed. Here, when the cured resin composition contains (A) brominated bisphenol A vinyl ester resin, it is necessary to contain a material having a relatively low refractive index in order to make the refractive index of the cured resin layer similar to that of a glass fiber fabric. Here, the present inventors have found that when the refractive index adjuster disclosed in Patent Documents 2 and 3 is used when the cured resin layer contains (A) brominated bisphenol A vinyl ester resin, the obtained cured resin layer has poor folding resistance. Then, as a result of the intensive research conducted by the present inventors, the present inventors have found that the obtained cured resin layer has excellent folding resistance by containing (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring as a refractive index adjuster when the cured resin layer contains (A).
[0037] The monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring is not particularly limited, and examples thereof include compounds represented by the following general formula (I).
[0038] R1-O-(R2O) n -R3···(I) (wherein R1 is an acryloyl group or a methacryloyl group, R2 is a divalent chain hydrocarbon group having 1 to 40 carbon atoms, R3 is a monovalent chain hydrocarbon group having 1 to 40 carbon atoms, and n is an integer of 2 to 50.)
[0039] In the compound represented by the general formula (I) described above, R2 is preferably a divalent chain hydrocarbon group having 1 to 5 carbon atoms. R3 is preferably a monovalent chain hydrocarbon group having 1 to 5 carbon atoms. n is preferably 2 to 10. From the viewpoint of further improving the folding resistance of the sheet, the compound represented by the general formula (I) described above is preferably one in which R2 in the general formula (I) is a divalent chain hydrocarbon group having 1 to 5 carbon atoms, R3 is a monovalent chain hydrocarbon group having 1 to 5 carbon atoms, and n is 2 to 10, and more preferably one in which R2 in the general formula (I) is a divalent chain hydrocarbon group having 1 to 5 carbon atoms, R3 is a monovalent chain hydrocarbon group having 1 to 5 carbon atoms, and n is 2 to 4 (i.e., the number of moles of alkylene oxide groups added is 2 to 4). From the viewpoint of more easily maintaining the transparency even after the sheet is left in a high-temperature environment, the above n is preferably 3 to 10, more preferably 2 to 9. In addition, from the viewpoint of more easily achieving both better folding resistance of the sheet and easier maintenance of transparency even after the sheet is left in a high-temperature environment, the above n is preferably 3 to 4.
[0040] Examples of monofunctional (meth)acrylates having an alkylene oxide group and no aromatic ring include ethoxy-diethylene glycol acrylate, methoxy-triethylene glycol acrylate, 2-ethylhexyl-diglycol acrylate, and methoxy-polyethylene glycol acrylate.
[0041] The cured resin layer 3 may be formed of a cured product of a resin composition containing (A) brominated bisphenol A vinyl ester resin and (B) monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring, as well as other components other than these. Examples of the other components include cured resins other than brominated bisphenol A vinyl ester resins. Examples of cured resins other than brominated bisphenol A vinyl ester resins include bisphenol A vinyl ester resins, novolac vinyl ester resins, urethane acrylate resins, fluorene acrylate resins, unsaturated polyester resins, curable acrylic resins, epoxy resins, etc., and bisphenol A vinyl ester resins are preferred from the viewpoint of making it easier to improve the transparency of the sheet. These cured resins may be used alone or in combination of two or more.
[0042] The other components include a polymerization initiator for curing the curable resin. The type of polymerization initiator may be appropriately selected according to the type of curable resin used. Examples of photopolymerization initiators include 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl ... Examples of the photopolymerization initiator include methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6,-trimethylbenzoyl-diphenyl-phosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. Among these photopolymerization initiators, 1-hydroxy-cyclohexyl-phenyl-ketone is preferred from the viewpoint of improving the transparency of the sheet. These photopolymerization initiators may be used alone or in combination of two or more. The content ratio of the polymerization initiator in the cured resin layer 3 may be 1 to 5 parts by mass of the polymerization initiator per 100 parts by mass of the total amount of the cured resin layer 3.
[0043] In the cured resin layer 3, the ratio of the mass of the brominated bisphenol A vinyl ester resin (A) to the mass of the resin composition containing the brominated bisphenol A vinyl ester resin and the monofunctional (meth)acrylate having an alkylene oxide group and not having an aromatic ring (mass excluding the glass fiber fabric 2) is, for example, 20 to 60 mass%, preferably 35 to 55 mass%. In addition, in the cured resin layer 3, the ratio of the mass of the monofunctional (meth)acrylate having an alkylene oxide group and not having an aromatic ring (B) to the mass of the resin composition containing the brominated bisphenol A vinyl ester resin and the monofunctional (meth)acrylate having an alkylene oxide group and not having an aromatic ring (mass excluding the glass fiber fabric 2) is, for example, 5 to 45 mass%, preferably 10 to 40 mass%. In the cured resin layer 3, in the resin composition containing (A) a brominated bisphenol A type vinyl ester resin and (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring, the ratio ((A) / (B)) of (A) the brominated bisphenol A type vinyl ester resin to (B) the monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring is, for example, 1 to 4, and preferably 1.5 to 2.0. In addition, in the cured resin layer 3, when the resin composition containing (A) a brominated bisphenol A type vinyl ester resin and (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring further contains a cured resin other than the brominated bisphenol A type vinyl ester resin, the proportion of the mass of the cured resin other than the brominated bisphenol A type vinyl ester to the mass of the resin composition (mass excluding the glass fiber fabric 2) is 15 to 45 mass%, and preferably 20 to 40 mass%.
[0044] In the present invention, in order to enhance the transparency of the sheet, it is desirable to set the refractive indexes of the glass fiber fabric 2 and the cured resin layer 3 to be close to each other. From this viewpoint, the refractive index of the cured resin layer 3 is preferably about 1.45 to 1.65, and more preferably about 1.50 to 1.60.
[0045] In the sheet of the present invention, the mass of each cured resin layer 3 (excluding the mass of the glass fiber fabric 2) is, for example, 10 to 100 g / m 2 In the sheet of the present invention, from the viewpoint of more suitably achieving both improved transparency and improved flame retardancy, the mass of each cured resin layer 3 (excluding the mass of the glass fiber fabric 2) is preferably 20 to 60 g / m 2 , more preferably 20 to 50 g / m 2 The thickness of each of the cured resin layers 3 is, for example, 10 to 120 μm, and from the viewpoint of more suitably achieving both improved transparency and improved non-flammability, it is preferably 20 to 100 μm, and more preferably 20 to 80 μm.
[0046] [Thermoplastic resin layer 4] In the sheet 1 of the present invention, the thermoplastic resin layer 4 is laminated on the cured resin layer 3 as necessary in order to improve the weather resistance, tear strength, folding resistance, etc. of the sheet 1. It is preferable that one thermoplastic resin layer 4 is included on the outer side of the cured resin layer 3.
[0047] The material constituting the thermoplastic resin layer 4 is not particularly limited. Examples include polyester resin (including polyethylene terephthalate), polycarbonate resin, polyolefin resin, fluororesin, acrylic resin, polyamide resin, and polyvinyl chloride resin. From the viewpoint of achieving a good balance between the flame retardancy and tear strength of the sheet, polyvinyl chloride resin is preferred. Furthermore, the thermoplastic resin layer 4 is preferably a film layer made of the above resin. Furthermore, an inorganic filler can be added to the thermoplastic resin layer 4. Examples of the inorganic filler include glass beads.
[0048] The thickness of each thermoplastic resin layer 4 is, for example, 50 to 200 μm, and from the viewpoint of achieving both flame retardancy and folding resistance, is preferably 60 to 150 μm, and more preferably 80 to 140 μm. The mass of each thermoplastic resin layer 4 is, for example, 60 to 280 g / m 2 From the viewpoint of achieving both flame retardancy and folding resistance, a preferred range is 70 to 200 g / m 2 is preferable, and 95 to 190 g / m 2 are more preferred.
[0049] When the thermoplastic resin layer 4 is laminated, another layer, for example, an adhesive layer, may be provided between the cured resin layer 3 and the thermoplastic resin layer 4. When an adhesive layer is provided, the mass of each adhesive layer is 3 to 20 g / m 2 and 5 to 15 g / m 2 are preferred.
[0050] [Sheet characteristics] The sheet 1 of the present invention preferably has high transparency in order to suppress obstruction of visibility or damage to aesthetics when used, for example, as a smoke barrier, partition, or daylight tent film. From the viewpoint of ensuring high transparency, the total light transmittance of the sheet 1 of the present invention is 80% or more, preferably 85% or more, and more preferably 90% or more. The haze of the sheet 1 of the present invention is, for example, 20% or less, preferably 10% or less, more preferably 5% or less, and even more preferably 2% or less. In this specification, the total light transmittance of the sheet 1 is a value measured according to the Japanese Industrial Standard JIS K 7361-1:1997 "Test method for total light transmittance of plastic transparent materials - Part 1: Single beam method". The haze of the sheet 1 is a value measured according to the Japanese Industrial Standard JIS K7136 2000 "Determination of haze of plastic transparent materials".
[0051] The sheet of the present invention has a total light transmittance of 80% or more, preferably 85% or more, before and after being left in a high-temperature environment at a temperature of 40° C. and a relative humidity of 65% for three days. The sheet of the present invention has a haze of 20% or less, preferably 10% or less, more preferably 5% or less, before and after being left in a high-temperature environment at a temperature of 40° C. and a relative humidity of 65% for three days. The total light transmittance and haze can be measured by the same measuring method as described above.
[0052] The sheet 1 of the present invention has a property of being difficult to burn (hard to generate heat) in the event of a fire, since the cured resin layer 3 contains a brominated bisphenol A type vinyl ester resin. As an index of the property of the sheet 1 of the present invention, a thermal shock resistance of 50 kW / m 2 In a heat generation test in which the material is irradiated with radiant heat, the total heat generation amount for 20 minutes after the start of heating is, for example, 8 MJ / m 2 Less than 6MJ / m, preferably 2 Less than or equal to 5MJ / m 2 The following can be mentioned. In addition, other indexes of the properties of the sheet 1 of the present invention include a thermal conductivity of 50 kW / m 2 In a heat generation test in which radiation heat is irradiated, the heat generation rate is 200 kW / m for 10 seconds or more continuously for 20 minutes after heating starts. 2 Preferably, the heat generation rate does not exceed 200 kW / m for 3 seconds or more for 20 minutes after the start of heating. 2 More preferably, the heat generation rate does not exceed 200 kW / m for 1 second or more for 20 minutes after the start of heating. 2 The main points to note are that the maximum power consumption is not to exceed 50kW / m 2 The total heat generation amount and the heat generation rate per unit area in the heat generation test in which radiant heat is irradiated are values obtained according to "4.9.2 Heat Generation Test" in the "Fire Resistance Test and Evaluation Procedure Manual" (revised version as of July 1, 2021) of the General Incorporated Foundation Building Materials Testing Center (Japan). In order to make it easier for the sheet of the present invention to have the above properties, the mass of the cured resin layer 3, the mass of the thermoplastic resin layer 4, etc. can be adjusted.
[0053] In the sheet 1 of the present invention, the folding resistance of the cured resin layer impregnated in the glass fiber fabric is preferably 30,000 times or more, and more preferably 35,000 times or more. The folding resistance is measured as follows. That is, using an MIT folding resistance tester, the load is set to 1 kg, the folding angle of the folding device is set to 135°, and the folding speed is set to 175±10 times / min, and the number of reciprocating foldings until the test piece breaks is measured. The size of the sheet is 15 mm×110 mm per piece. The number of reciprocating foldings can be measured in accordance with the method specified in 7.14 “Cloth folding resistance” of the Japanese Industrial Standard JIS R 3420:2013 “General test method for glass fibers”. The measurement is performed in the warp and weft directions of the glass fiber fabric, and the average value of the number of reciprocating foldings in the warp direction and the number of reciprocating foldings in the weft direction (=(number of reciprocating foldings in the warp direction+number of reciprocating foldings in the weft direction) / 2) is used to evaluate.
[0054] In the sheet 1 of the present invention, the tear strength of the cured resin layer impregnated in the glass fiber fabric is preferably 1N or more, more preferably 1 to 3N. The tear strength is measured by performing a tensile test using a constant-speed load tensile tester under the conditions of a grip interval of 25 mm and a tensile speed of 200 mm / min in accordance with the C method (trapezoid method) of 7.16 of the Japanese Industrial Standards JIS R 3420:2013. Specifically, a test piece of 75 mm x 150 mm is taken from the sheet 1 in the warp direction of the glass fiber fabric and the weft direction of the glass fiber fabric, and an isosceles trapezoid with a short side of 25 mm, a long side of 100 mm, and a height of 75 mm is marked on the test piece as shown in the figure, and a tape for preventing slipping (product name "600S", manufactured by Sekisui Chemical Co., Ltd.) is applied to both sides of the area other than the isosceles trapezoid (i.e., two trapezoidal parts including a right angle; corresponding to the trapezoid A part illustrated in FIG. 2). Also, make a 10 mm cut at a right angle to the center of the short side of the isosceles trapezoid mark. Using a constant-rate load tensile tester (product name "RTC-1310A", manufactured by Orientec Co., Ltd.), the test piece is clamped with the short side of the isosceles trapezoid tensed and the long side of the isosceles trapezoid loosened, with the test piece gripped at a distance of 25 mm, and a tensile test is performed at a tensile speed of 200 mm / min to measure the maximum load shown when the test piece is torn. The maximum load in the warp direction of the glass fiber fabric and the maximum load in the weft direction of the glass fiber fabric are measured, and the average value of the maximum load in the warp direction of the glass fiber fabric and the maximum load in the weft direction of the glass fiber fabric (= (maximum load in the warp direction of the glass fiber fabric (N) + maximum load in the weft direction (N)) / 2) is calculated as the tear strength (N).
[0055] The mass of the sheet 1 of the present invention is not particularly limited. From the viewpoint of more suitably imparting the property of being difficult to burn (hard to generate heat) in the event of a fire and excellent folding resistance, the mass of the sheet 1 of the present invention is preferably 30 to 450 g / m 2 , more preferably 40 to 430 g / m 2 In particular, when the sheet 1 of the present invention includes the thermoplastic resin layer 4, the mass is preferably 200 to 450 g / m 2 , more preferably 250 to 430 g / m 2 Examples include:
[0056] The thickness of the sheet 1 of the present invention is not particularly limited, but from the viewpoint of more suitably imparting the property of being difficult to burn (hard to generate heat) in the event of a fire and excellent folding resistance, the thickness of the sheet 1 of the present invention is preferably 30 to 400 μm, more preferably 40 to 350 μm. In particular, when the sheet 1 of the present invention has a thermoplastic resin layer 4, the thickness is preferably 150 to 400 μm, more preferably 200 to 350 μm.
[0057] When the sheet 1 of the present invention comprises a thermoplastic resin layer 4, the ratio of the thickness per layer of the cured resin layer 3 to the thickness of the sheet 1 (thickness of the cured resin layer 3 / thickness of the sheet 1) is, from the viewpoint of more suitably imparting the property of being difficult to burn (hard to generate heat) in the event of a fire and excellent folding resistance, for example, 0.01 to 0.8, preferably 0.03 to 0.3, and more preferably 0.05 to 0.25.
[0058] (Method of manufacturing sheet 1 of the present invention) The method for producing the sheet 1 of the present invention is not particularly limited. For example, first, the resin composition constituting the glass fiber fabric 2 and the cured resin layer 3 is prepared. Next, the glass fiber fabric 2 is coated with the resin composition and impregnated, and then the thickness and content of the resin composition are adjusted using a squeeze roller or the like. Next, the resin composition is cured by heating or applying light energy, etc., to obtain a sheet 1 in which the glass fiber fabric 2 is impregnated with the cured resin layer 3. In addition, a process film such as polyethylene terephthalate coated with the resin composition is prepared, and the film is pressed against both sides of the glass fiber fabric 2 to impregnate both sides of the glass fiber fabric 2 with the resin composition, and the resin composition is cured, and then the process film is peeled off to obtain a sheet 1 in which the glass fiber fabric 2 is impregnated with the cured resin layer 3.
[0059] When the resin composition is cured by applying thermal energy, the heating temperature is not particularly limited and can be, for example, about 50 to 200° C. When the resin composition is cured by applying light energy, the resin composition is cured by irradiating it with light. The light irradiation conditions are, for example, an integrated light amount of 100 to 500 mJ / cm. 2 It can be said that:
[0060] When the sheet 1 of the present invention has a thermoplastic resin layer 4, the thermoplastic resin layer 4 can be laminated on the cured resin layer 3 obtained above. EXAMPLES
[0061] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the examples.
[0062] 1. Measurement and evaluation methods 1-1. Average diameter of single fiber of glass yarn (μm) and number of single fibers (pieces) Two pieces of glass fiber fabric were cut into 30 cm squares, one for observing the warp yarns and the other for observing the weft yarns, and each was embedded in epoxy resin (product name "3091", manufactured by Marumoto Struers K.K.) and cured. Next, the glass cloth embedded in epoxy resin was polished to such an extent that the cross section of the single fibers constituting the warp yarns or weft yarns could be observed, and the average single fiber diameter (μm) and the number of single fibers (number of fibers) of the glass yarns were measured by observing them at a magnification of 500 times using a scanning electron microscope (SEM) (product name "JSM-6390A", manufactured by JEOL Ltd.). (1) Average single fiber diameter of long glass fibers (μm) Twenty warp and weft yarns were randomly selected, and the cross sections of all the single fibers contained in each of the 20 glass yarns were observed, the diameters were measured, and the average value was calculated to obtain the average single fiber diameter of the warp and weft yarns. (2) Number of single fibers (pieces) Twenty warp and weft yarns were randomly selected, and the total number of single fibers contained in each of the 20 glass yarns was measured and the average value was calculated to obtain the number of single fibers in the warp and weft yarns.
[0063] 1-2.Glass yarn count The count of the glass yarn was measured according to the method specified in "7.1 Count" of the Japanese Industrial Standard JIS R 3420 2013 "General Test Method for Glass Fibers". Specifically, 500 m of glass yarn was first taken from the yarn winding device and used as a test piece. The test piece was placed flat and placed in a muffle furnace, baked at 625°C for 25 minutes, then cooled in a desiccator, and the mass of the test piece was measured. The count was calculated according to the following formula. t = (m / 500) x 1000 t: count m: mass of test piece (g)
[0064] 1-3.Weave density of glass fiber fabric 2 (threads / 25mm) The weave density of the glass fiber fabric 2 was measured by measuring the weave density of the warp and weft threads according to the method specified in "7.9 Density (weave density)" of the Japanese Industrial Standard JIS R 3420:2013 "General test method for glass fibers". Specifically, the measurement targets were positions 50 mm or more away from the ends and selvages of the glass fiber fabric 2, the measurement interval was set to 10 mm or more and 200 mm or less, and the total number of threads within the set measurement interval was measured. This was counted as one measurement, and the measurement was moved to another position that did not include the previously measured thread, and the total number of threads within the measurement interval was measured two more times in the same manner. For each of the three measurements, the number of threads per 25 mm was calculated according to the following formula, and the average value of the three measurements was calculated. Mi = (ni / ai) x 25 Mi: Number of threads per 25mm ni: Number of yarns measured ai: the exact distance at which the measurement was taken (mm)
[0065] 1-4. Thickness of glass fiber fabric 2 (μm) The thickness of the glass fiber fabric 2 was measured in accordance with the A method stipulated in "7.10.1 Cloth thickness" of the Japanese Industrial Standard JIS R3420:2013 "General test method for glass fiber". Specifically, the thickness of the glass fiber fabric 2 was measured by gently rotating the spindle using a micrometer to lightly contact the measurement surface parallel to it, and reading the scale after the ratchet makes three noises. The thickness of the glass fiber fabric 2 was measured at the intersection of the warp and weft threads.
[0066] 1-5. Refractive index of the glass fiber fabric 2 and the cured resin layer 3 The refractive index of the glass fiber fabric 2 and the cured resin layer 3 was measured according to the "B method" specified in the Japanese Industrial Standard JIS K 7142:2008 "Plastics - Determination of refractive index". Specifically, the glass fibers constituting the glass fiber fabric 2 and the cured resin layer 3 were first crushed to such an extent that the Becke line could be observed when observed with an optical microscope at a magnification of 400 times, and used as a measurement sample. Separately, a plurality of immersion liquids with refractive indices differing by 0.002 were prepared. A small amount of the immersion liquid was placed on a slide glass, and several grains of the measurement sample were placed on the immersion liquid on the slide glass, and a cover glass was placed on it. Then, a halogen lamp equipped with an interference filter for D-line was used as a light source, and the measurement sample was focused at a magnification of 400 times using an optical microscope, and the focus was slightly shifted by moving the stage of the microscope away from the objective lens. By this operation, if the refractive index of the measurement sample does not match the refractive index of the immersion liquid, the Becke lines (i.e., the bright halo seen around or inside the powder) will move to the side with a larger refractive index, and if the refractive index of the measurement sample matches the refractive index of the immersion liquid, the Becke lines will not appear. The refractive index was measured by repeating the measurement until the refractive index of the measurement sample matches the refractive index of the immersion liquid or falls between two adjacent refractive indices in the series of immersion liquids. The refractive index was measured three times at a temperature of 23°C, and the average value of the three measurements was taken as the refractive index value.
[0067] 1-6. Mass (g / m) of glass fiber fabric 2 2 ) The mass of the glass fiber fabric 2 was measured in accordance with the method specified in "7.2 Mass (mass) of cloths and mats" of the Japanese Industrial Standard JIS R 3420:2013 "General test method for glass fibers". Specifically, a sample of 100 cm2 of glass fiber fabric 2 was measured from a point 50 mm or more away from the edge of the glass fiber fabric 2. 2 A square test piece was taken and dried at 105°C for 1 hour, after which the mass of the test piece was measured and the mass of 1m was calculated according to the following formula: 2 The mass per unit was calculated. ρA=(ms / 100)×10 4 ρA:1m 2 Mass per unit (g / m 2 ) ms: mass of test piece (g)
[0068] 1-7. Total light transmittance (%) and haze (%) immediately after manufacturing, and total light transmittance (%) and haze (%) after being left in a high-temperature environment after manufacturing The total light transmittance of the sheet 1 was measured according to the Japanese Industrial Standard JIS K 7361-1:1997 "Test method for total light transmittance of plastic transparent materials - Part 1: Single beam method". The haze of the sheet 1 was measured according to the Japanese Industrial Standard JIS K 7136:2000 "Determination of haze of plastic transparent materials". The total light transmittance and haze of the sheet 1 were measured. First, the measurement was performed immediately after production, and then the sheet was left in a high temperature environment of 40°C and 65% relative humidity for 3 days, and then the measurement was performed again.
[0069] 1-8. Total heat generation in heat generation test (MJ / m 2 ), and a heat generation rate per unit area of 200 kW / m 2 Exceeded duration (seconds) Sheet 1: 50kW / m 2 The total heat generation amount in the heat generation test in which radiant heat is irradiated is 200kW / m2, and the heat generation rate per unit area is 200kW / m2. 2 The excess duration was measured in accordance with "4.9.2 Heat Generation Test" in the "Fire Resistance Testing and Evaluation Procedures" (revised on July 1, 2021) of the Japan Construction Materials Testing Center. The specific method is as follows. The total heat generation in the heat generation test was 8 MJ / m 2 Pass the following (〇), heat generation rate per unit area 200kW / m 2The excess duration is 20 minutes after the start of heating, and the heat generation rate exceeds 200 kW / m for 10 seconds or more. 2 Those that did not exceed this were marked as passing (O).
[0070] [Test specimen] (1) The number of test specimens (sheets 1) shall be three. (2) The shape and dimensions of the test specimen shall be a square with each side measuring 99 mm ± 1 mm. (3) Before the test, the test specimen is cured at a temperature of 23°C ± 2°C and a relative humidity of 50% ± 5% to a constant mass. [Test equipment] (1) A schematic diagram of the test equipment used is shown in Figure 3. The test equipment consists of a cone-shaped radiant electric heater, a spark plug, a radiant heat shield, a test specimen holder, a gas sampling device, an exhaust system capable of measuring gas flow rate, a heat flow meter, etc. (2) Radiant electric heater: 50 kW / m 2 The radiant heat must be able to be irradiated uniformly and stably onto the surface of the test piece. (3) The radiant heat shield shall be capable of protecting the test specimen from radiant heat before the test begins. (4) A schematic diagram of the test holder and presser frame included in the test equipment is shown in Figure 4. The specimen holder shall be made of stainless steel and be a square with outer dimensions of 106 mm ± 1 mm on each side, 25 mm ± 1 mm in depth, and 2.4 mm ± 0.15 mm in thickness. The presser frame shall be made of stainless steel and be a square with inner dimensions of 111 mm ± 1 mm on each side, 54 mm ± 1 mm in height, and 1.9 mm ± 0.1 mm in thickness, with a square opening at the top with sides of 94.0 mm ± 0.5 mm. (5) The exhaust system shall be equipped with a centrifugal exhaust fan, hood, fan intake and exhaust ducts, an orifice plate flow meter, etc. that function effectively at the test temperature. The distance between the bottom end of the hood and the surface of the test specimen shall be 210 mm ± 50 mm. In that state, the exhaust device of the exhaust system shall have a flow rate of 0.024 m when converted to standard temperature and standard pressure. 3 / s. For exhaust gas flow measurement, an orifice plate with an inner diameter of 57 mm ± 3 mm and a thickness of 1.6 mm ± 0.3 mm is placed in the exhaust duct at a distance of at least 350 mm ± 15 mm downstream from the fan. For exhaust gas sampling, a ring sampler with 12 holes of 2.2 mm ± 0.1 mm diameter is attached 685 mm ± 15 mm from the hood with the holes facing in the opposite direction to the flow. Exhaust gas temperature is measured at the centre of the exhaust duct 100 mm ± 5 mm upstream from the orifice plate. (6) The gas sampling device shall be capable of continuously and accurately measuring the concentrations of oxygen, carbon monoxide, and carbon dioxide in the exhaust gas. (7) The spark plug shall be capable of receiving power from a 10kV transformer or induction coil system, etc. The distance between the electrodes of the spark plug shall be 3mm±0.5mm, and the position of the electrodes shall, in principle, be 13mm±2mm on the central axis of the test specimen. (8) The heat flow meter is 100kW / m 2 ±10kW / m 2 The heat flow meter is a Schmidt-Boelter type that can measure up to 12.5 mm in diameter. The heat sensing part of the heat flow meter is a circle with a diameter of 12.5 mm, and the surface emissivity is 0.95 ± 0.05.
[0071] [Test conditions] (1) The test time shall be 20 minutes from the time when radiant heat is applied to the surface of the test specimen and an electric spark is generated at the same time. (2) The test specimen is wrapped on the sides and back with aluminum foil of 0.025 mm or more and 0.04 mm or less in thickness, placed in a press frame, and then coated with inorganic fiber (nominal density 64-128 kg / m) on the back side. 3 ) and then pressed into the specimen holder. (3) During the test, a radiant electric heater applied 50 kW / m to the surface of the test specimen. 2 It emits radiant heat. (4) Exhaust gas flow rate of 0.024 m 3 Adjust to / s. (5) Until the start of the test, a radiant heat shield is used to protect the test specimen from radiant heat. (6) Set the spark plug in the designated position before moving the radiation heat shield.
[0072] [measurement] (1) Measure the oxygen concentration at intervals of not more than 5 seconds. (2) The heat generation rate per unit area (kW / m) was calculated using the following method: 2 ) and the heat generation rate per unit area is calculated as 200 kW / m 2 The duration of the ultra-high heat generation rate per unit area is 200 kW / m 2 The total heat generation rate per unit area (MJ / m) was calculated by trapezoidal integration of the heat generation rate per unit area with respect to time. 2 Here, the trapezoidal integration is performed by dividing the integration interval equally over the measurement interval with the test time as the integration interval, setting negative heat generation rates to 0, and integrating only positive heat generation rates.
number
number
number
number
[0073] 1-9. Resistance to deformation during fire For sheet 1, the total heat generation amount (MJ / m 2 ), and a heat generation rate per unit area of 200 kW / m 2 The heat generation test shown in the "Excess duration (seconds)" column was conducted, and the condition of the test specimen was observed after 20 minutes of exposure to radiant heat, and the "resistance to deformation in the event of a fire" was evaluated according to the following criteria. <Evaluation criteria for resistance to deformation during fire> A: After 20 minutes of exposure to radiant heat, the deformation of the test specimen was suppressed and the test specimen was contained within the holding frame. B: After 20 minutes of exposure to radiant heat, the specimen was deformed and did not fit within the frame.
[0074] 1-10.Folding resistance Using an MIT folding endurance tester, the load was set to 1 kg, the bending angle of the bending device was set to 135°, and the bending speed was set to 175±10 times / min, and the number of times the test piece was folded back and forth until it broke was measured. The size of the sheet was 15 mm × 110 mm per piece. The number of times the test piece was folded back and forth was measured in accordance with the method specified in 7.14 "Folding endurance of cloth" of the Japanese Industrial Standard JIS R 3420:2013 "General test method for glass fiber". The measurement was performed in the warp and weft directions of the glass fiber fabric, and the average value of the number of times the test piece was folded back and forth in the warp direction and the number of times the test piece was folded back and forth in the weft direction (=(number of times the test piece was folded back and forth in the warp direction + number of times the test piece was folded back and forth in the weft direction) / 2) was used for evaluation.
[0075] 1-11. Evaluation of stickiness The obtained sheet was wound around a paper tube with a fixed tension for 5 revolutions, and left to stand for 20 hours in an environment of 20°C temperature and 65% relative humidity, after which it was rewound. When rewinding, sheets that felt stuck due to adhesion between the wound sheets were rated as failing (×), and sheets that could be rewound smoothly without any sticking were rated as passing (○).
[0076] 1-12.Tear strength (N) The tear strength of the sheet 1 was measured by performing a tensile test under the conditions of a gripping distance of 25 mm and a tensile speed of 200 mm / min using a constant-speed load tensile tester in accordance with the C method (trapezoid method) of 7.16 of the Japanese Industrial Standards JIS R 3420:2013. Specifically, a test piece of 75 mm x 150 mm was taken from the sheet 1 in the warp direction of the glass fiber fabric and the weft direction of the glass fiber fabric, respectively, and an isosceles trapezoid mark with a short side of 25 mm, a long side of 100 mm, and a height of 75 mm was made on the test piece as shown in the figure, and a tape for preventing slipping (product name "600S", manufactured by Sekisui Chemical Co., Ltd.) was attached to both sides of the area other than the isosceles trapezoid (i.e., two trapezoidal parts including a right angle; corresponding to the trapezoid A part illustrated in FIG. 2). In addition, a 10 mm cut was made at a right angle to the short side in the center of the isosceles trapezoid mark. A constant-rate-load tensile tester (product name "RTC-1310A", manufactured by Orientec Co., Ltd.) was used to clamp the test piece with a gripping distance of 25 mm, with the short side of the isosceles trapezoid of the test piece tensed and the long side of the isosceles trapezoid loosened, and a tensile test was performed at a tensile speed of 200 mm / min to measure the maximum load shown when tearing. The maximum load in the warp direction of the glass fiber fabric and the maximum load in the weft direction of the glass fiber fabric were measured, and the average value of the maximum load in the warp direction of the glass fiber fabric and the maximum load in the weft direction of the glass fiber fabric (= (maximum load in the warp direction of the glass fiber fabric (N) + maximum load in the weft direction (N)) / 2) was calculated as the tear strength (N).
[0077] <Example 1> (Preparation of glass fiber fabric 2) Glass yarns (product name "ECC1200 1 / 0 1.0Z", manufactured by Unitika Glass Fiber Co., Ltd.; average single fiber diameter 4.5 μm, number of single fibers 100, twist number 1.0Z, count 4.2 tex) were used as warp and weft yarns, and woven with an air jet loom to obtain a plain weave glass fiber fabric with a warp density of 90 / 25 mm and a weft density of 90 / 25 mm. Next, the spinning bundling agent and weaving bundling agent attached to the obtained glass fiber fabric were removed by heating at 400°C for 30 hours. Thereafter, the glass fiber fabric was treated with a surface treatment agent adjusted to a concentration of 15 g / L using a silane coupling agent (S-350: N-vinylbenzyl-aminoethyl-γ-aminopropyltrimethoxysilane (hydrochloride) Chisso Corporation), squeezed with a padder roll, and then dried at 120°C for 1 minute to be cured. The glass fiber fabric was then subjected to a water flow process at a pressure of 1.5 MPa, with the warp tension of the fabric set to 100 N / m, and a width-widening process was carried out once to obtain a glass fiber fabric 2 (glass fiber fabric). The obtained glass fiber fabric 2 had a warp density of 90 threads / 25 mm, a weft density of 90 threads / 25 mm, a thickness of 30 μm, and a mass of 30 g / m 2 The refractive index was 1.561. The average single fiber diameter and the number of single fibers of the glass yarn were measured using the glass fiber fabric 2.
[0078] (Preparation of Resin Composition Solution Used to Form Cured Resin Layer 3) As the resin composition solution used to form the cured resin layer 3, brominated bisphenol A type vinyl ester (product name "Neopol 8197", manufactured by Japan U-PICA Corporation), bisphenol A type vinyl ester resin (product name "Neopol 8126", manufactured by Japan U-PICA Corporation), methoxytriethylene glycol acrylate (product name "Light Acrylate MTG-A", manufactured by Kyoeisha Chemical Co., Ltd.), and a photopolymerization initiator (product name "Omnirad 184", manufactured by IGM) were prepared and mixed to the mass ratio shown in Table 1 to prepare a resin composition solution.
[0079] (Preparation of process film) As a processing film, a PET film (thickness 75 μm, total light transmittance (JIS K7361-1 1997) 93%, haze (JIS K7136 2000) 4%) was prepared. Two sheets of the processing film were prepared.
[0080] A sheet was manufactured using the prepared glass fiber fabric 2, resin composition solution, and processing film. Specifically, the resin composition solution was first applied to one side of one processing film and one side of the other processing film. Then, the glass fiber fabric 2 was sandwiched between the two processing films to which the resin composition solution was applied so that the side to which the resin composition solution was applied faced the glass fiber fabric 2, and pressure was applied with a roller so that the mass of the cured resin layer 3 satisfied the value shown in Table 1, and the glass fiber fabric 2 was impregnated with the resin composition solution from both sides. Thereafter, while the processing film was still laminated, the resin composition solution was irradiated with light (light irradiation conditions: cumulative light amount 200 mJ / cm 2 ) using a black light fluorescent lamp (product name "FL15BLB", manufactured by Toshiba Corporation). 2 ) to cure the resin composition solution, forming a cured resin layer 3, and the process film was peeled off to obtain a sheet having the laminated structure illustrated in FIG. 1 , which includes a glass fiber fabric and a cured resin layer contained in a state of being impregnated into the glass fiber fabric.
[0081] <Example 2> (Preparation of glass fiber fabric 2) The same glass fiber fabric 2 as in Example 1 was prepared.
[0082] (Preparation of Resin Composition Solution Used to Form Cured Resin Layer 3) As the resin composition solution used to form the cured resin layer 3, brominated bisphenol A type vinyl ester (product name "Neopol 8197", manufactured by Japan U-PICA Corporation), bisphenol A type vinyl ester resin (product name "Neopol 8126", manufactured by Japan U-PICA Corporation), ethoxy-diethylene glycol acrylate (product name "Light Acrylate EC-A", manufactured by Kyoeisha Chemical Co., Ltd.), and photopolymerization initiator (product name "Omnirad 184", manufactured by IGM) were prepared and mixed to the mass ratio shown in Table 1 to prepare a resin composition solution.
[0083] (Preparation of process film) As a processing film, a PET film (thickness 75 μm, total light transmittance (JIS K7361-1 1997) 93%, haze (JIS K7136 2000) 4%) was prepared. Two sheets of the processing film were prepared.
[0084] A sheet was manufactured using the prepared glass fiber fabric 2, resin composition solution, and processing film. Specifically, the resin composition solution was first applied to one side of one processing film and one side of the other processing film. Then, the glass fiber fabric 2 was sandwiched between the two processing films to which the resin composition solution was applied so that the side to which the resin composition solution was applied faced the glass fiber fabric 2, and pressure was applied with a roller so that the mass of the cured resin layer 3 satisfied the value shown in Table 1, and the glass fiber fabric 2 was impregnated with the resin composition solution from both sides. Thereafter, while the processing film was still laminated, the resin composition solution was irradiated with light (light irradiation conditions: cumulative light amount 200 mJ / cm 2 ) using a black light fluorescent lamp (product name "FL15BLB", manufactured by Toshiba Corporation). 2 ) to cure the resin composition solution, forming a cured resin layer 3, and the process film was peeled off to obtain a sheet having the laminated structure illustrated in FIG. 1 , which includes a glass fiber fabric and a cured resin layer contained in a state of being impregnated into the glass fiber fabric.
[0085] <Example 3> (Preparation of glass fiber fabric 2) The same glass fiber fabric 2 as in Example 1 was prepared.
[0086] (Preparation of Resin Composition Solution Used to Form Cured Resin Layer 3) As the resin composition solution used to form the cured resin layer 3, brominated bisphenol A type vinyl ester (product name "Neopol 8197", manufactured by Japan U-PICA Corporation), bisphenol A type vinyl ester resin (product name "Neopol 8126", manufactured by Japan U-PICA Corporation), methoxy-polyethylene glycol acrylate (n=9) (product name "Light Acrylate 130A", manufactured by Kyoeisha Chemical Co., Ltd.), and photopolymerization initiator (product name "Omnirad 184", manufactured by IGM) were prepared and mixed to the mass ratio shown in Table 1 to prepare a resin composition solution.
[0087] (Preparation of process film) As a processing film, a PET film (thickness 75 μm, total light transmittance (JIS K7361-1 1997) 93%, haze (JIS K7136 2000) 4%) was prepared. Two sheets of the processing film were prepared.
[0088] A sheet was manufactured using the prepared glass fiber fabric 2, resin composition solution, and processing film. Specifically, the resin composition solution was first applied to one side of one processing film and one side of the other processing film. Then, the glass fiber fabric 2 was sandwiched between the two processing films to which the resin composition solution was applied so that the side to which the resin composition solution was applied faced the glass fiber fabric 2, and pressure was applied with a roller so that the mass of the cured resin layer 3 satisfied the value shown in Table 1, and the glass fiber fabric 2 was impregnated with the resin composition solution from both sides. Thereafter, while the processing film was still laminated, the resin composition solution was irradiated with light (light irradiation conditions: cumulative light amount 200 mJ / cm 2 ) using a black light fluorescent lamp (product name "FL15BLB", manufactured by Toshiba Corporation). 2 ) to cure the resin composition solution, forming a cured resin layer 3, and the process film was peeled off to obtain a sheet having the laminated structure illustrated in FIG. 1 , which includes a glass fiber fabric and a cured resin layer contained in a state of being impregnated into the glass fiber fabric.
[0089] <Comparative Example 1> (Preparation of glass fiber fabric 2) The same glass fiber fabric 2 as in Example 1 was prepared.
[0090] (Preparation of Resin Composition Solution Used to Form Cured Resin Layer 3) As the resin composition solution used to form the cured resin layer 3, brominated bisphenol A type vinyl ester (product name "Neopol 8197", manufactured by Japan U-PICA Corporation), bisphenol A type vinyl ester resin (product name "Neopol 8126", manufactured by Japan U-PICA Corporation), 2-hydroxyethyl acrylate (product name "Light Ester HOA (N)", manufactured by Kyoeisha Chemical Co., Ltd.), and a photopolymerization initiator (product name "Omnirad 184", manufactured by IGM) were prepared and mixed to the mass ratio shown in Table 1 to prepare a resin composition solution.
[0091] (Preparation of process film) As a processing film, a PET film (thickness 75 μm, total light transmittance (JIS K7361-1 1997) 93%, haze (JIS K7136 2000) 4%) was prepared. Two sheets of the processing film were prepared.
[0092] A sheet was manufactured using the prepared glass fiber fabric 2, resin composition solution, and processing film. Specifically, the resin composition solution was first applied to one side of one processing film and one side of the other processing film. Then, the glass fiber fabric 2 was sandwiched between the two processing films to which the resin composition solution was applied so that the side to which the resin composition solution was applied faced the glass fiber fabric 2, and pressure was applied with a roller so that the mass of the cured resin layer 3 satisfied the value shown in Table 1, and the glass fiber fabric 2 was impregnated with the resin composition solution from both sides. Thereafter, while the processing film was still laminated, the resin composition solution was irradiated with light (light irradiation conditions: cumulative light amount 200 mJ / cm 2 ) using a black light fluorescent lamp (product name "FL15BLB", manufactured by Toshiba Corporation). 2 ) to cure the resin composition solution, forming a cured resin layer 3, and the process film was peeled off to obtain a sheet having the laminated structure illustrated in FIG. 1 , which includes a glass fiber fabric and a cured resin layer contained in a state of being impregnated into the glass fiber fabric.
[0093] <Comparative Example 2> (Preparation of glass fiber fabric 2) The same glass fiber fabric 2 as in Example 1 was prepared.
[0094] (Preparation of Resin Composition Solution Used to Form Cured Resin Layer 3) As the resin composition solution to be used for forming the cured resin layer 3, bisphenol A type vinyl ester resin (product name "Neopol 8126", manufactured by Japan U-Pica Corporation) was prepared and mixed to obtain the mass ratio shown in Table 1 to prepare a resin composition solution.
[0095] (Preparation of process film) As a processing film, a PET film (thickness 75 μm, total light transmittance (JIS K7361-1 1997) 93%, haze (JIS K7136 2000) 4%) was prepared. Two sheets of the processing film were prepared.
[0096] A sheet was manufactured using the prepared glass fiber fabric 2, resin composition solution, and processing film. Specifically, the resin composition solution was first applied to one side of one processing film and one side of the other processing film. Then, the glass fiber fabric 2 was sandwiched between the two processing films to which the resin composition solution was applied so that the side to which the resin composition solution was applied faced the glass fiber fabric 2, and pressure was applied with a roller so that the mass of the cured resin layer 3 satisfied the value shown in Table 1, and the glass fiber fabric 2 was impregnated with the resin composition solution from both sides. Thereafter, while the processing film was still laminated, the resin composition solution was irradiated with light (light irradiation conditions: cumulative light amount 200 mJ / cm 2 ) using a black light fluorescent lamp (product name "FL15BLB", manufactured by Toshiba Corporation). 2 ) to cure the resin composition solution, forming a cured resin layer 3, and the process film was peeled off to obtain a sheet having the laminated structure illustrated in FIG. 1 , which includes a glass fiber fabric and a cured resin layer contained in a state of being impregnated into the glass fiber fabric.
[0097] <Comparative Example 3> (Preparation of glass fiber fabric 2) The same glass fiber fabric 2 as in Example 1 was prepared.
[0098] (Preparation of Resin Composition Solution Used to Form Cured Resin Layer 3) As the resin composition solution used to form the cured resin layer 3, brominated bisphenol A type vinyl ester (product name "Neopol 8197", manufactured by Japan U-PICA Corporation), bisphenol A type vinyl ester resin (product name "Neopol 8126", manufactured by Japan U-PICA Corporation), neopentyl glycol diacrylate (product name "NK Ester A-NPG", manufactured by Shin-Nakamura Chemical Co., Ltd.), and a photopolymerization initiator (product name "Omnirad 184", manufactured by IGM) were prepared and mixed in the mass ratio shown in Table 1 to prepare a resin composition solution.
[0099] (Preparation of process film) As a processing film, a PET film (thickness 75 μm, total light transmittance (JIS K7361-1 1997) 93%, haze (JIS K7136 2000) 4%) was prepared. Two sheets of the processing film were prepared.
[0100] A sheet was manufactured using the prepared glass fiber fabric 2, resin composition solution, and processing film. Specifically, the resin composition solution was first applied to one side of one processing film and one side of the other processing film. Then, the glass fiber fabric 2 was sandwiched between the two processing films to which the resin composition solution was applied so that the side to which the resin composition solution was applied faced the glass fiber fabric 2, and pressure was applied with a roller so that the mass of the cured resin layer 3 satisfied the value shown in Table 1, and the glass fiber fabric 2 was impregnated with the resin composition solution from both sides. Thereafter, while the processing film was still laminated, the resin composition solution was irradiated with light (light irradiation conditions: cumulative light amount 200 mJ / cm 2 ) using a black light fluorescent lamp (product name "FL15BLB", manufactured by Toshiba Corporation). 2 ) to cure the resin composition solution, forming a cured resin layer 3, and the process film was peeled off to obtain a sheet having the laminated structure illustrated in FIG. 1 , which includes a glass fiber fabric and a cured resin layer contained in a state of being impregnated into the glass fiber fabric.
[0101] <Comparative Example 4> (Preparation of glass fiber fabric 2) The same glass fiber fabric 2 as in Example 1 was prepared.
[0102] (Preparation of Resin Composition Solution Used to Form Cured Resin Layer 3) As the resin composition solution used to form the cured resin layer 3, brominated bisphenol A type vinyl ester (product name "Neopol 8197", manufactured by Japan U-PICA Corporation), bisphenol A type vinyl ester resin (product name "Neopol 8126", manufactured by Japan U-PICA Corporation), 3-phenoxybenzyl acrylate (product name "Light Acrylate POB-A", manufactured by Shin-Nakamura Chemical Co., Ltd.), and a photopolymerization initiator (product name "Omnirad 184", manufactured by IGM) were prepared and mixed to the mass ratio shown in Table 1 to prepare a resin composition solution.
[0103] (Preparation of process film) As a processing film, a PET film (thickness 75 μm, total light transmittance (JIS K7361-1 1997) 93%, haze (JIS K7136 2000) 4%) was prepared. Two sheets of the processing film were prepared.
[0104] A nonflammable sheet was manufactured using the prepared glass fiber fabric 2, resin composition solution, and processing film. Specifically, the resin composition solution was first applied to one side of one processing film and one side of the other processing film. Then, the glass fiber fabric 2 was sandwiched between the two processing films to which the resin composition solution was applied so that the side to which the resin composition solution was applied faced the glass fiber fabric 2, and pressure was applied with a roller so that the mass of the cured resin layer 3 satisfied the value shown in Table 1, and the glass fiber fabric 2 was impregnated with the resin composition solution from both sides. Thereafter, while the processing film was still laminated, the resin composition solution was irradiated with light (light irradiation conditions: cumulative light amount 200 mJ / cm 2 ) using a black light fluorescent lamp (product name "FL15BLB", manufactured by Toshiba Corporation). 2 ) to cure the resin composition solution, forming a cured resin layer 3, and the process film was peeled off to obtain a nonflammable sheet having the laminated structure illustrated in FIG. 1 , which includes a glass fiber fabric and a cured resin layer contained in a state of being impregnated into the glass fiber fabric.
[0105] The results are shown in Table 1.
[0106] [Table 1]
[0107] The sheets of Examples 1 to 3 were sheets including a glass fiber fabric and a cured resin layer impregnated in the glass fiber fabric, and the cured resin layer was formed from a cured product of a resin composition including (A) a brominated bisphenol A type vinyl ester resin and (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring, and therefore were less sticky and had excellent folding resistance.
[0108] Among them, the sheets of Examples 1 and 2 had better folding resistance because the number of moles of the alkylene oxide groups added of the monofunctional (meth)acrylate (B) having an alkylene oxide group and not having an aromatic ring was 2 to 4. Also, the sheets of Examples 1 and 3 had a number of moles of the alkylene oxide groups added of the monofunctional (meth)acrylate (B) having an alkylene oxide group and not having an aromatic ring was 3 to 10, so that the transparency was more easily maintained even after being left in a high-temperature environment. In particular, the sheet of Example 1 had a number of moles of the alkylene oxide groups added of the monofunctional (meth)acrylate (B) having an alkylene oxide group and not having an aromatic ring was 3 to 4, so that the folding resistance of the sheet was more excellent and the transparency was more easily maintained even after being left in a high-temperature environment.
[0109] On the other hand, the sheet of Comparative Example 1 had poor folding resistance because the 2-hydroxyethyl acrylate did not have an alkylene oxide group and did not contain (B) a monofunctional (meth)acrylate that had an alkylene oxide group and no aromatic ring.
[0110] Moreover, the sheet of Comparative Example 2 did not contain brominated bisphenol A vinyl ester, and therefore was unable to suppress stickiness.
[0111] In addition, the sheet of Comparative Example 3 had poor folding resistance because the neopentyl glycol diacrylate was polyfunctional and did not contain (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring.
[0112] In addition, the sheet of Comparative Example 4 had poor folding resistance because the 3-phenoxybenzyl acrylate had an aromatic ring and did not contain (B) a monofunctional (meth)acrylate that had an alkylene oxide group and no aromatic ring.
Claims
1. A sheet comprising a glass fiber fabric and a cured resin layer impregnated in the glass fiber fabric, the cured resin layer is formed from a cured product of a resin composition containing (A) a brominated bisphenol A type vinyl ester resin and (B) a monofunctional (meth)acrylate having an alkylene oxide group and no aromatic ring, A sheet comprising a thermoplastic resin layer laminated on the cured resin layer.
2. 2. The sheet according to claim 1, wherein the number of moles of the alkylene oxide group added is 2 to 10.
3. 3. The sheet according to claim 1, wherein the sheet has a total light transmittance of 80% or more and a haze of 20% or less.
4. 50kW / m 2 When subjected to a heat generation test in which the material was irradiated with radiant heat of 8 MJ / m for 20 minutes after the start of heating, the total heat generation amount was 8 MJ / m 2 3. A sheet according to claim 1 or 2, wherein:
5. 50kW / m 2 When subjected to a heat generation test in which the material was irradiated with radiant heat of 200 kW / m for 20 minutes after the start of heating, the heat generation rate was 200 kW / m for 10 seconds or more. 2 3. The sheet according to claim 1 or 2, wherein the thickness of said sheet is not more than 1 mm.
Citation Information
Patent Citations
Welding curtain material
JP1993123869A
Transparent nonflammable sheet and its manufacturing method
JP2005319746A
Incombustible sheet and method for producing the same
JP2014213489A
Non-flammable sheet
JP2017210712A
Transparent nonflammable sheet, Anti-smoke vertical wall, and manufacturing method of transparent nonflammable sheet
JP2020001172A