Metal-organic compound composite material

A metal-organic compound composite with specific organic particles on a metal substrate addresses the challenge of increased sliding frequency by reducing friction and enhancing wear resistance, offering improved lubricity and durability.

JP7577099B2Active Publication Date: 2024-11-01KOBE STEEL LTD
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
JP2022156907
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-09-29
Publication Date
2024-11-01
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

Existing metal materials used in sliding applications, such as those in electric vehicles, face challenges in achieving improved lubricity due to increased sliding frequency, necessitating better friction reduction and wear resistance.

Method used

A metal-organic compound composite is developed, comprising a metal material with over 50% by mass of Al, Ti, Cu, Au, Ni, Sn, or Cr, combined with organic compound particles that are either attached or buried on the surface, allowing for improved lubricity through decomposition and formation of a carbon-containing reaction film.

Benefits of technology

The composite material achieves reduced friction coefficients and improved wear resistance compared to conventional materials, with friction coefficients lowered by up to 50% and wear reduced by up to 1/10 after 500 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577099000007
    Figure 0007577099000007
  • Figure 0007577099000008
    Figure 0007577099000008
  • Figure 0007577099000009
    Figure 0007577099000009
Patent Text Reader

Abstract

To provide a metal composite having improved lubricity.SOLUTION: A metal-organic compound composite includes: a metal material including more than 50 mass% of one or more kinds of metals selected from a group consisting of Al, Ti, Cu, Au, Ni, Sn, Zn and Cr in total; and a plurality of organic compound particles. The plurality of organic compound particles having one or more states selected from a group consisting of a state of deposition on the surface of the metal material so as to be peeled with a cellophane adhesive tape and a state of implantation in the metal material so as to expose at least a part of the metal material to the surface includes one or more kinds selected from a group consisting of a compound A being an aliphatic compound including two or more kinds selected from H, C and O in a unit molecular structure, a compound B being an aliphatic compound including one or more amide bonds in a unit molecular structure, and a compound C being an aromatic compound including one or more amino groups in a unit molecular structure.SELECTED DRAWING: Figure 1B
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to metal-organic composites. [Background technology]

[0002] Metal materials can be used for sliding members such as machine parts, such as bearings, piston rings, and cylinders, as well as mold parts used in press working, etc. Sliding members are required to have lubricity (i.e., a low coefficient of friction) because they are subjected to repeated sliding on a daily basis.

[0003] Furthermore, in recent years, as CO2 emission regulations have become stricter, the number of electric vehicles (EVs) and plug-in hybrid vehicles (PHEVs), which are less dependent on fossil fuels, is increasing, and the number of parts that undergo repeated sliding, such as contact materials, used in EVs and PHEVs is also increasing.

[0004] For example, in Patent Document 1, a solid lubricant is brought into contact with a metal material (specifically, a solid lubricant is embedded in the metal material). Agent It is disclosed that the solid lubricant is preferably talc in terms of lubricity, etc. Patent Document 2 discloses that in order to impart lubricity to a metal material, an inorganic filler such as talc is brought into contact with the metal material (co-deposition). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 63-118047 [Patent Document 2] Japanese Patent Application Publication No. 11-241169 Summary of the Invention [Problem to be solved by the invention]

[0006] As described above, in recent years, the number of parts that are subjected to repeated sliding has been increasing, and there is a demand for metal materials (or composite materials thereof) with improved lubricity compared to conventional techniques.

[0007] The present invention has been made in view of the above circumstances, and one of its objects is to provide a metal material (or a composite material thereof) having improved lubricity compared to the prior art. [Means for solving the problem]

[0008] Aspect 1 of the present invention is A metal material containing more than 50 mass% in total of one or more metals selected from the group consisting of Al, Ti, Cu, Au, Ni, Sn, Zn, and Cr, and a plurality of organic compound particles, The organic compound particles include A state in which the adhesive tape is attached to the surface of the metal material so as to be peelable with cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405); and a state in which at least a portion of the metal material is embedded in the metal material so as to be exposed to the surface; the plurality of organic compound particles include at least one selected from the group consisting of compound A, compound B, and compound C; The compound A is an aliphatic compound containing two or more elements selected from the group consisting of hydrogen (H), carbon (C) and oxygen (O) in a unit molecular structure, The compound B is an aliphatic compound containing one or more amide bonds in a unit molecular structure, The compound C has a unit molecular structure NiA The compound is a metal-organic composite that is an aromatic compound containing one or more amino groups.

[0009] Aspect 2 of the present invention is The metal-organic compound composite according to aspect 1, wherein the plurality of organic compound particles includes the compound A.

[0010] Aspect 3 of the present invention is The metal material contains more than 50 mass% in total of one or more metals selected from the group consisting of Al, Ti, Cu, Au, Sn, Zn, and Cr, The metal-organic compound composite according to aspect 1, wherein the plurality of organic compound particles includes the compound B.

[0011] A fourth aspect of the present invention is The metal material contains more than 50 mass% in total of one or more metals selected from the group consisting of Al, Ti, Cu, Au, Ni, Sn, and Cr, The metal-organic compound composite according to embodiment 1, wherein the plurality of organic compound particles comprises compound C.

[0012] A fifth aspect of the present invention is The metal-organic compound composite material according to any one of Aspects 1 to 4, wherein when the plurality of organic compound particles are subjected to a thermogravimetric differential thermal analysis from room temperature to a maximum of 1000°C at a heating rate of 10°C / min, if a melting point is exhibited, the melting point is 100°C or higher, or no melting point is exhibited.

[0013] A sixth aspect of the present invention is The metal-organic compound composite material according to any one of Aspects 1 to 5, wherein when the plurality of organic compound particles are subjected to thermogravimetric differential thermal analysis from room temperature to a maximum of 1000°C at a heating rate of 10°C / min, if a decomposition point is exhibited, the decomposition point is 500°C or lower, and if no decomposition point is exhibited but a combustion point is exhibited, the combustion point is 500°C or lower.

[0014] A seventh aspect of the present invention is The metal-organic compound composite material according to any one of aspects 1 to 6, wherein the plurality of organic compound particles does not contain fluorine.

[0015] Aspect 8 of the present invention is 8. The metal-organic compound composite according to any one of aspects 1 to 7, wherein the plurality of organic compound particles have an average particle size of less than 50 μm.

[0016] A ninth aspect of the present invention is The metal-organic compound composite material according to any one of aspects 1 to 8, wherein the plurality of organic compound particles are attached to the surface of the metal material so as to be peelable with cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405).

[0017] A tenth aspect of the present invention is The metal-organic compound composite material according to any one of Aspects 1 to 8, wherein the plurality of organic compound particles are embedded in the metal material such that at least a portion of the metal material is exposed on the surface. Effect of the Invention

[0018] According to embodiments of the present invention, it is possible to provide a metal composite having improved lubricity over the prior art. [Brief description of the drawings]

[0019] [Figure 1A] FIG. 1 is a schematic cross-sectional view of an example of a metal-organic compound composite material according to an embodiment of the present invention. [Figure 1B] FIG. 2 is a schematic cross-sectional view of another example of a metal-organic compound composite material according to an embodiment of the present invention. [Figure 2A] 1 shows a photograph of the surface of a metal-organic compound composite material in which polyethylene oxide particles are brought into contact (adhered) with the surface of the metal material (Ni-P plating layer) produced in Example 1. [Figure 2B] FIG. 2B shows a photograph of the metal-organic compound composite material after a cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405) was applied to the surface of the metal-organic compound composite material in FIG. 2A. [Figure 2C] A photograph of FIG. 2B after the tape was removed is shown. [Figure 3A] 1 shows a schematic diagram of the surface of a sample that was subjected to a reciprocating sliding test. [Figure 3B] After a reciprocating sliding test was performed on the metal material in Table 1: Ni-P (no particles), the center of the sliding mark 30 as shown in FIG. 3A was measured with a surface roughness meter in a direction perpendicular to the sliding direction to obtain a surface profile. [Figure 4]1 shows a photograph of the surface of a metal-organic compound composite material in which polyethylene oxide particles are brought into contact (adhered) with the surface of the metal material (Ni-P plating layer) produced in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present inventors have studied from various angles in order to realize a metal composite material with improved lubricity compared to the conventional technology described in Patent Document 1. In the conventional technology described in Patent Document 1, lubricity is imparted by contacting talc or the like having a solid lubricating effect with a metal material. As a result of the study conducted by the present inventors, it was found that, unlike talc, which is an inorganic particle having a solid lubricating effect, by contacting a specific organic compound particle, which does not necessarily have a solid lubricating effect, with a specific metal material under predetermined conditions, the friction coefficient can be reduced (i.e., lubricity can be improved) compared to contacting talc. This is thought to be because, when the metal material slides, a part of the specific organic compound decomposes, and a part of it forms a new reaction film containing carbon, etc., thereby reducing the friction coefficient near the surface of the metal material and improving lubricity. The reaction film may contain atomic components of the metal material that are thought to diffuse into the film or originate from wear powder. As a result, it is possible to realize a metal composite material having improved lubricity compared to the conventional technology. Note that the above mechanism does not limit the technical scope of the embodiment of the present invention. The following provides details of each requirement stipulated by the embodiment of the present invention.

[0021] The metal-organic compound composite according to an embodiment of the present invention is The present invention relates to a method for manufacturing a semiconductor device comprising: a metal material containing more than 50 mass% in total of one or more metals selected from the group consisting of Al, Ti, Cu, Au, Ni, Sn, Zn, and Cr; and a plurality of organic compound particles, the plurality of organic compound particles being attached to a surface of the metal material so as to be peelable with a cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405) and / or being embedded in the metal material so that at least a part of the metal material is exposed on the surface, the plurality of organic compound particles including one or more selected from the group consisting of Compound A, Compound B, and Compound C, Compound A being an aliphatic compound containing two or more selected from the group consisting of hydrogen (H), carbon (C), and oxygen (O) in its unit molecular structure, Compound B being an aliphatic compound containing one or more amide bonds in its unit molecular structure, and Compound C being a compound having at least one amide bond in its unit molecular structure. NiA It is an aromatic compound that contains one or more amino groups. This makes it possible to improve lubricity over the prior art (i.e., metal materials in contact with talc).

[0022] FIG. 1A shows a schematic cross-sectional view of a metal-organic compound composite according to an embodiment of the present invention. In FIG. 1A, the metal-organic compound composite 1 includes a metal material 2 and a plurality of particles 3, and the plurality of particles 3 are embedded in the metal material 2 so that at least a part 2a of the metal material 2 is exposed on the surface of the metal-organic compound composite 1 (so that the particles 3 do not cover the entire surface 2b of the metal material 2). Here, a part of each particle 3 is embedded in the metal material 2, and the remaining part is exposed on the surface of the metal-organic compound composite 1. By taking such a contact state, a part of a specific organic compound is decomposed during sliding of the metal material 2, and a part of the decomposition forms a new reaction film containing carbon, etc., thereby reducing the friction coefficient near the surface 2b of the metal material 2 and improving lubricity. In addition, by exposing at least a part 2a of the metal material 2 to the surface of the metal-organic compound composite 1, the initial contact resistance (electrical resistance) before sliding can be reduced when the metal-organic compound composite 1 is used as a contact material. Whether or not at least a portion 2a of the metal material 2 is exposed on the surface can be determined, for example, by visually checking whether or not there is metallic luster.

[0023] In the metal-organic compound composite 1 in FIG. 1A, each particle 3 may be entirely embedded in the metal material 2 before the start of sliding. By performing a sliding treatment so that the particles 3 are exposed, it is possible to reduce the friction coefficient as in the metal-organic compound composite 1. Also, as in the metal-organic compound composite 1, the initial contact resistance can be reduced. That is, in this specification, "particle 3 partly embedded in the metal material 2" includes an embodiment in which a single particle 3 is entirely embedded in the metal material 2 before the start of sliding, but part of it is exposed from the metal material 2 after the start of sliding, and the other part is embedded in the metal material 2.

[0024] FIG. 1B shows a schematic cross-sectional view of another example of the metal-organic compound composite according to the embodiment of the present invention. In FIG. 1B, the metal-organic compound composite 11 includes a metal material 2 and a plurality of particles 3, and the plurality of particles 3 are attached to the surface 2b of the metal material 2. Here, the particles 3 are attached to the surface 2b with such a weak force that they can be peeled off with a cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405). By adopting such a contact state, at least a part of the particles 3 in the sliding portion is immediately removed when the metal material 2 slides, and a state in which at least a part of the metal material 2 is exposed on the surface of the metal-organic compound composite 11 can be realized as in the metal-organic compound composite 1, and the friction coefficient in the vicinity of the surface 2b of the metal material 2 can be reduced as in the metal-organic compound composite 1. In addition, since the metal material 2 can be immediately exposed on the surface of the metal-organic compound composite 11 even when the contact resistance is measured, the initial contact resistance can be reduced as in the metal-organic compound composite 1.

[0025] FIG. 1B shows a state in which the multiple particles 3 are attached to the surface 2b of the metal material 2 so that the metal material 2 is not exposed on the surface of the metal-organic compound composite 1 between the multiple particles 3 (so as to cover the entire surface 2b of the metal material 2), but this state is not limited thereto, and for example, the metal material 2 may be attached to the surface 2b so that a portion of the metal material 2 is exposed on the surface of the metal-organic compound composite 1 between the multiple particles 3.

[0026] As described above, the contact state of the particles 3 with respect to the metal material 2 has been exemplified, but the contact state may be one type or two or more types. For example, in the embodiment of the present invention, among all the particles 3, a part of the particles 3 may be attached to the surface of the metal material 2, and the other particles 3 may be embedded in the metal material 2. In that case, it is sufficient that at least a part of the metal material is exposed on the surface of the metal-organic compound composite material on which the particles are attached, and even if it is not exposed, it is sufficient that the particles 3 attached to the surface can be peeled off by cellophane adhesive tape. In addition, as for the embedded state of the particles 3, a part of the particles 3 may be exposed from the surface of the metal material 2, and the other particles 3 may be entirely embedded in the metal material 2.

[0027] The metal material 2 contains more than 50 mass% in total of one or more metals selected from the group consisting of Al, Ti, Cu, Au, Ni, Sn, Zn, and Cr. The metal material 2 preferably contains 75 mass% or more of the metals in total, more preferably 85 mass% or more in total, and even more preferably 95 mass% or more in total. The metal material 2 may contain only one type of the metal, or two or more types.

[0028] The metal material 2 may be a bulk material or a surface-treated layer such as a plating layer. The thickness t of the metal material 2 is not particularly limited. If the metal material 2 is a surface-treated layer such as a plating layer, t may be 0.05 to 100 μm, preferably 0.07 to 50 μm, and more preferably 0.10 to 30 μm.

[0029] With regard to the organic compound particles 3, the term "organic compound" refers to compounds containing carbon, excluding compounds with simple structures such as carbon monoxide, carbon dioxide, carbonates, hydrocyanic acid, cyanates, thiocyanates, B4C, and SiC, etc. For example, a silicone resin having a siloxane bond (-Si-O-Si-) as the main chain and an organic group on the side chain is included in the "organic compound" in this specification.

[0030] As an organic compound constituting the particles 3, compound A is an aliphatic compound containing any two or more selected from the group consisting of hydrogen (H), carbon (C) and oxygen (O) in the unit molecular structure, and has the effect of further reducing the friction coefficient for all of the above metal types of the metal material 2. Therefore, it is preferable that the multiple particles 3 contain compound A. Examples of compound A include polyolefin resins such as polyethylene and polypropylene, resins obtained by oxidizing these resins (such as oxidized polyethylene), polymethacrylate resins, etc. Note that the "unit molecular structure" means one repeating unit in the case of a polymer, and an individual molecule in the case of a non-polymer.

[0031] Compound B, an organic compound constituting particle 3, is an aliphatic compound containing one or more amide bonds in its unit molecular structure, and has the effect of sufficiently reducing the friction coefficient for all of the above metal types of metal material 2, and further reducing the friction coefficient for the above metal types except for Ni. Therefore, it is preferable that metal material 2 contains more than 50 mass% in total of one or more metals selected from the group consisting of Al, Ti, Cu, Au, Sn, Zn, and Cr, and that the multiple particles 3 contain compound B. Examples of compound B include nylon resins such as nylon 66 and nylon 12.

[0032] As an organic compound constituting particle 3, compound C has a unit molecular structure NiA Amino group (-NR 1 R 2 Where R 1 and R 2 is hydrogen or a hydrocarbon group, and R 1 and R 2 may be the same or different), and has the effect of sufficiently reducing the friction coefficient for all of the above metal types of the metal material 2, and further reducing the friction coefficient for the above metal types except for Zn. That is, it is preferable that the metal material 2 contains more than 50 mass% in total of one or more metals selected from the group consisting of Al, Ti, Cu, Au, Ni, Sn, and Cr, and the plurality of particles 3 contain the compound C. Examples of the compound C include melamine cyanurate, sulfanilic acid, etc.

[0033] The plurality of particles 3 preferably have a melting point of 100° C. or more or do not exhibit a melting point (i.e., decompose without melting). This can suppress the deterioration of the friction coefficient caused by melting of the organic compound when the metal-organic compound composites 1 and 11 are heated to a high temperature. More preferably, the plurality of particles 3 have a melting point of 110° C. or more or do not exhibit a melting point, and even more preferably have a melting point of 120° C. or more or do not exhibit a melting point. Here, the "melting point" is a melting point obtained by performing thermogravimetric differential thermal analysis (TG-DTA) from room temperature to a maximum of 1000° C. at a heating rate of 10° C. / min in air, for example. Specifically, the melting point can be a temperature within a temperature range in which the mass reduction in the TG curve is less than 1%, and a temperature at the intersection of the extrapolated line of the straight line up to the first inflection point where the heat flow rate starts to decrease with the temperature increase in the DTA curve and the extrapolated line of the straight line from the second inflection point onwards where the heat flow rate starts to decrease at a constant gradient (i.e., the straight line with the constant gradient) after the second inflection point where the heat flow rate starts to decrease at a constant gradient thereafter. In addition, when the particles 3 do not show a melting point (when the compound decomposes without melting), the decomposition point is preferably 100°C or higher, more preferably 110°C or higher, and even more preferably 120°C or higher. Here, the "decomposition point" is a decomposition point obtained by performing thermogravimetric differential thermal analysis (TG-DTA) from room temperature to a maximum of 1000°C at a heating rate of 10°C / min under air, for example. Specifically, the decomposition point can be a temperature within a temperature range where a mass reduction of 1% or more is confirmed in a TG curve, and a temperature at the intersection of an extrapolated line of a straight line up to a first inflection point where the heat flow rate starts to decrease with a temperature increase in a DTA curve and an extrapolated line of a straight line from a second inflection point onward where the heat flow rate starts to decrease at a constant gradient (i.e., the straight line with the constant gradient).

[0034] From the viewpoint of further reducing the friction coefficient of the metal-organic compound composites 1 and 11, the decomposition point of the particles 3 is preferably 500°C or less. More preferably, the decomposition point is 450°C or less, and even more preferably, 400°C or less. When the decomposition point is not shown but the combustion point is shown, the combustion point is preferably 500°C or less, more preferably 450°C or less, and even more preferably 400°C or less. Here, the "combustion point" is a combustion point obtained by performing thermogravimetric differential thermal analysis (TG-DTA) from room temperature to a maximum of 1000°C at a heating rate of 10°C / min in the atmosphere, for example. Specifically, the combustion point can be a temperature within a temperature range in which a mass reduction of 1% or more is confirmed in the TG curve, and a temperature at the intersection of an extrapolated line of a straight line up to the first inflection point where the heat flow rate starts to increase with the temperature increase in the DTA curve and an extrapolated line of a straight line from the second inflection point onwards where the heat flow rate starts to increase at a constant gradient (i.e., the straight line with the constant gradient) can be determined as the combustion point.

[0035] From the viewpoint of reducing costs, it is preferable that the plurality of particles 3 does not contain fluorine.

[0036] The average particle size (average circle equivalent diameter, median diameter (volume basis)) of the plurality of particles 3 is preferably less than 50 μm. This can, for example, promote a part of a specific organic compound to decompose and react with the vicinity of the surface 2b of the metal material 2. The average particle size of the plurality of particles 3 is more preferably 30 μm or less, and further preferably 10 μm or less. If the metal material 2 is a surface-treated layer such as a plating layer, the layer surface may become convex if the particle size of the particles 3 is large compared to the layer thickness. If the metal material 2 is a surface-treated layer such as a plating layer, it is preferable that the average particle size of the particles 3 is smaller than the layer thickness, and this makes it possible to improve the dispersion density of the particles 3 per volume in the metal material 2.

[0037] The plurality of particles 3 are preferably non-conductive. This makes it possible to suppress short-circuiting of the contacts due to the dropping off of conductive particles when the metal-organic compound composites 1 and 11 are used as contact materials.

[0038] The metal-organic compound composites 1 and 11 according to the embodiment of the present invention may contain other members in order to achieve the object of the present invention. For example, when the metal material 2 is a surface treatment layer, the metal-organic compound composites 1 and 11 may contain the substrate thereof. The substrate may be made of metals (or alloys thereof) such as copper, iron, aluminum, titanium, magnesium, etc. The substrate may be in the form of a wrought material such as a plate, strip, bar, shaped material, or wire, a casting, a sintered material, or a product made by processing them into a part. The metal-organic compound composites 1 and 11 may contain organic compound particles other than the specific organic compound particles 3 described above, or may contain inorganic particles. In this case, it is preferable that 50% by volume or more of the total particles are the specific organic compound particles 3, more preferably 60% by volume or more, 70% by volume or more, 80% by volume or more, or 90% by volume or more, and it is even more preferable that all (100% by volume) are the specific organic compound particles 3.

[0039] The metal-organic compound composite material 11 according to the embodiment of the present invention can be produced by applying a dispersion liquid containing a plurality of organic compound particles 3 to the surface 2 b of the metal material 2 .

[0040] The metal-organic compound composite material 1 according to the embodiment of the present invention is obtained by dispersing the particles 3 in a metal plating solution for the metal material 2, and performing an electroplating process on a substrate while stirring the solution, thereby obtaining the metal-organic compound composite material 1 on the substrate in which a plurality of particles 3 are embedded (co-deposited) in the metal material 2. Note that in order to suppress aggregation of the particles 3 in the metal plating solution for the metal material 2 and maintain a stable dispersion state, a surfactant (dispersant) may be used as appropriate.

[0041] In the process of dispersing the particles 3 in a metal plating solution and carrying out electroplating to codeposit the particles 3 into the metal material 2, the following reactions (A) and (B) proceed simultaneously. (A) A reaction in which dispersed particles in liquid are electrostatically or physically adsorbed (contacted) to the surface of a substrate. (B) Reaction in which metal material 2 deposits (grows) on the substrate surface "Eutectoid" occurs when the particles 3 adsorbed in (A) are incorporated into the metal material 2 in (B). Under conditions where eutectoid plating proceeds steadily, the particles 3 adsorbed in the early stages of the reaction are incorporated into the metal material 2, and at the same time, new particles 3 are adsorbed. For this reason, even when the plating process is stopped, in many cases the particles 3 are still exposed on the outermost surface, and in a typical eutectoid plating process, a metal-organic compound composite material 1 can be easily produced that contains particles 3 that are partly embedded in the metal material 2 and the remaining part exposed on the surface of the metal material 2. Here, the amount of the particles 3 co-deposited in the metal material 2 is determined by the balance between the frequency of adsorption of (A) and the plating film growth rate of (B). Therefore, it is possible to change the amount of co-deposition by changing plating conditions such as the amount of particles 3 dispersed in the plating solution. For example, at the end of the plating process, a plating solution that does not contain particles 3 dispersed in the plating solution is used, or the stirring speed of the plating solution is changed to reduce the frequency of adsorption of (A), thereby providing a layer on the outermost surface side of the plating that does not co-deposit the particles 3, and it is possible to manufacture a metal-organic compound composite material in which the particles 3 are all buried in the metal material 2.

[0042] The metal-organic compound composites 1 and 11 according to the embodiments of the present invention can improve lubricity (i.e., can reduce the friction coefficient) compared to the conventional technology. Specifically, the metal-organic compound composites 1 and 11 according to the embodiments of the present invention can reduce the average value of the friction coefficient (ratio of horizontal load to vertical load) after each cycle up to 50 cycles in the sliding test described below compared to a metal material in which conventional talc is contacted instead of the particles 3. <Sliding test (reciprocating sliding test)> A counter member, which is a φ6 mm high carbon chromium bearing steel ball (SUJ2), is slid for a predetermined number of cycles against the surface of the test subject metal-organic compound composite 1 or 11, with a normal load of 1 N applied, a sliding width (sliding stroke) of 10 mm, and an average sliding speed of 30 mm / sec, with one reciprocating motion being defined as one cycle. As the sliding tester, for example, a ball-on-disk testing device (Tribometer manufactured by CSM) can be used.

[0043] The metal-organic compound composites 1 and 11 according to the embodiment of the present invention can have even better wear resistance. Specifically, the metal-organic compound composites 1 and 11 according to the embodiment of the present invention can significantly reduce the amount of wear after 500 cycles of the sliding test (for example, to 1 / 2 or less, preferably to 1 / 5 or less, more preferably to 1 / 10 or less) compared to the case where the particles 3 are not in contact. EXAMPLES

[0044] The following examples are provided to more specifically describe the embodiments of the present invention. The embodiments of the present invention are not limited to the following examples, and may be modified as appropriate within the scope of the above and below-described aims, and all of these are included in the technical scope of the embodiments of the present invention. EXAMPLES

[0045] Commercially available substrates were prepared using Fe plate (thickness t: 0.2 mm), Al plate (thickness t: 0.2 mm), Ti plate (thickness t: 0.2 mm) and Cu plate (thickness t: 0.3 mm) as metal materials (each metal had a purity of 95% by mass or more). On one surface perpendicular to the thickness direction of the metal materials, 0.5 ml / cm of a liquid containing various particles shown in Table 1 suspended in alcohol at a ratio of 20 mg / ml was applied. 2 Metal-organic compound composites in which various particles were in contact with (attached to) the metal surface were obtained by dropping and drying the particles. In addition, plating layers of Au, Sn, Zn, Ni, Ni-P (Ni content: 85 mass% or more) and Cr were formed by known methods on the above-mentioned Cu plate as a substrate (plating thickness t: 5 μm, purity of each plating layer was 95 mass% or more), and a liquid in which various particles (or particle dispersions) shown in Table 1 were suspended in alcohol at a rate of 20 mg / ml was applied thereon at 0.5 ml / cm. 2By dropping and drying, a metal-organic compound composite material in which various particles contacted (adhered) to the metal material surface was obtained. In addition, a thermogravimetric differential thermal analysis (TG-DTA) was performed on various particles shown in Table 1 using a differential thermobalance (Rigaku Corporation, Thermo plus EVOII) at a heating rate of 10°C / min in air from room temperature to a maximum of 1000°C, and the melting point, decomposition point, and combustion point of each particle were obtained. The results are also shown in Table 1. In Table 1, "-" in the "Compound type" column means that it does not correspond to any of the compounds A to C in the embodiment of the present invention, "-" in the "Melting point (°C)", "Decomposition point (°C)", and "Combustion point (°C)" columns means that the corresponding temperature was not shown in the thermogravimetric differential thermal analysis, and "-" in the "Average particle size (μm)" column means that the corresponding average particle size was not investigated.

[0046] [Table 1]

[0047] As a result of visually observing the metal-organic compound composites prepared as described above, in all composites, the plurality of particles were in contact (attached) with the surface of the metal material without the metal material being exposed between the plurality of particles on the surface of the metal-organic compound composite (i.e., the surface of the metal material was covered with the plurality of particles). In addition, in all of the metal-organic compound composites prepared as described above, the particles in contact (attached) with the metal material can be peeled off by, for example, pressing the adhesive side of cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405) with a finger against the surface of the metal-organic compound composite on the side where the particles were in contact, and peeling it off in a direction perpendicular to the surface. As an example, Figure 2A shows a photograph of the surface of a metal-organic compound composite in which polyethylene oxide particles have been brought into contact with (attached to) the surface of a metal material (Ni-P plating layer). As shown in Figure 2A, the part where the particles were attached (the part surrounded by the dashed line) had no metallic luster, and no exposed metal material was observed. FIG. 2B shows a photograph of the metal-organic compound composite of FIG. 2A after cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405) has been applied to the surface (the tape is applied to the area surrounded by the dashed line), and FIG. 2C shows a photograph of the metal-organic compound composite of FIG. 2A after the tape has been peeled off in a direction perpendicular to the surface to which it was applied. In FIG. 2B, the cellophane adhesive tape is applied by pressing its adhesive side with a finger against the surface of the metal-organic compound composite that has been in contact with the particles. As shown in FIG. 2C, a new metallic luster is seen in the area where the tape was applied (area surrounded by the dashed line), indicating that the particles have been peeled off by the cellophane adhesive tape.

[0048] The metal-organic compound composite material prepared as described above was subjected to the following lubricity evaluation. The following lubricity evaluation was performed using a separately prepared sample set in which the cellophane adhesive tape was not attached or peeled off. <Lubricity evaluation> In a reciprocating sliding test using a ball-on-disk testing device (Tribometer, manufactured by CSM), a counter material, a φ6 mm high carbon chromium bearing steel (SUJ2) ball, was slid against the metal-organic compound composite material under test for 50 cycles, with one reciprocating movement being counted as one cycle, with a vertical load of 1 N, a sliding width (sliding stroke) of 10 mm, and an average sliding speed of 30 mm / sec. To judge the lubricity evaluation, the average friction coefficient (ratio of horizontal load to vertical load) after each cycle was calculated, and those in which the average friction coefficient was lower than when no particles were in contact and when talc was in contact were rated as sufficient (◯), those in which the average friction coefficient was not lower than when no particles were in contact and / or when talc was in contact were rated as insufficient (×), and those in which the average friction coefficient was lower by 50% or less than when no particles were in contact were rated as excellent (◎). The above results are summarized in Table 2.

[0049] [Table 2]

[0050] From the results in Table 2, the following can be considered: In Table 2, when the metal material is Al, Ti, Cu, Au, Ni, Ni-P, Sn, Zn or Cr, and the contacted particles are polyethylene oxide (meeting the requirements of compound A according to the embodiment of the present invention), polypropylene (meeting the requirements of compound A according to the embodiment of the present invention), nylon 12 (meeting the requirements of compound B according to the embodiment of the present invention), or melamine cyanurate (meeting the requirements of compound C according to the embodiment of the present invention), all of them satisfy the requirements stipulated in the embodiment of the present invention, and the friction coefficient is lower and lubricity is improved compared to the case where no particles are contacted and the conventional technology (i.e., the case where talc is contacted with the metal material).

[0051] From the results in Table 2, the following cases (1) to (3) had lower friction coefficients and were preferable embodiments. (1) The metal material is Al, Ti, Cu, Au, Ni, Ni-P, Sn, Zn or Cr, and the particles in contact are compound A (polyethylene oxide or polypropylene). (2) The metal material is Al, Ti, Cu, Au, Ni-P, Sn, Zn or Cr, and the contacted particles are compound B (nylon 12). (3) The metal material is Al, Ti, Cu, Au, Ni, Ni-P, Sn or Cr, and the contacted particles are compound C (melamine cyanurate).

[0052] On the other hand, when the metal material was Fe and the contacted particles were PEEK, the requirements of the embodiment of the present invention were not met, and the friction coefficient could not be sufficiently reduced.

[0053] Furthermore, the following abrasion resistance evaluation was performed on some of the above metal-organic compound composites. The following abrasion resistance evaluation was performed by separately preparing a sample set that was not subjected to the above cellophane adhesive tape attachment and peeling, and lubricity evaluation. <Wear resistance evaluation> In a reciprocating sliding test using a ball-on-disk testing device (Tribometer, manufactured by CSM), a counter material, a φ6 mm high carbon chromium bearing steel (SUJ2) ball, was slid against the metal-organic compound composite material under test for 500 cycles, with one reciprocating movement being defined as one cycle, with a vertical load of 1 N, a sliding width (sliding stroke) of 10 mm, and an average sliding speed of 30 mm / sec. round trip After the sliding test, a surface profile was obtained using a surface shape measuring device (DEKTAK6M, manufactured by ULVAC, Inc.) to calculate the amount of wear.

[0054] FIG. 3A shows a schematic diagram of the surface of a sample that has been subjected to a reciprocating sliding test, and FIG. 3B shows, as an example, the result of measuring the center of the sliding mark 30 shown in FIG. 3A in a direction perpendicular to the sliding direction using a surface roughness meter after a reciprocating sliding test on the metal material: Ni-P (without particles) in Table 1. Here, the amount of wear (μm 2 ) was obtained by subtracting the area of ​​the raised portion 31b, which is considered to have protruded upward due to plastic deformation, from the area of ​​the worn portion 31a, which was scraped downward from the average line 32a of the non-sliding portion 32 (other than the sliding portion 31) in the surface profile result of FIG. 3B. The wear amount calculation results are shown in Table 3.

[0055] [Table 3]

[0056] The results in Table 3 show that when the requirements of the embodiment of the present invention are met, the amount of wear can be significantly reduced compared to when particles are not in contact with the metal material (when no particles are present). EXAMPLES

[0057] The same Cu plate as used in Example 1 was used as a substrate, and a plating layer of Ni-P (Ni content: 85% by mass or more) was formed by a known method (plating thickness t: 5 μm, plating layer purity: 95% by mass or more). On top of that, a liquid in which oxidized polyethylene particles shown in Table 1 were suspended in alcohol at a ratio of 2 mg / ml was applied at a rate of 0.5 ml / cm. 2 By dripping the mixture and drying it, a metal-organic compound composite material was obtained in which polyethylene oxide particles were in contact with (adhered to) the surface of the metal material (Ni-P plating layer).

[0058] Fig. 4 shows a photograph of the surface of a metal-organic compound composite in which polyethylene oxide particles were contacted (adhered) to the surface of the metal material (Ni-P plating layer) prepared as described above. As shown in Fig. 4, metallic luster (e.g., the area surrounded by the dashed line) was confirmed between the multiple polyethylene oxide particles, and a part of the Ni-P plating layer was exposed on the surface of the metal-organic compound composite. In addition, since the above metal-organic compound composite was prepared (coated) in the same manner as in Example 1, it is considered that the polyethylene oxide particles can be peeled off with cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405) in the same manner as in Example 1.

[0059] The metal-organic compound composite material prepared as described above, in which oxidized polyethylene particles were brought into contact with the metal material (Ni-P plating layer), was evaluated for lubricity in the same manner as in Example 1. As a result, the average friction coefficient was an excellent value of 0.17. EXAMPLES

[0060] A pure copper plate with a thickness of 0.3 mm was used as the plating substrate, and the surface was degreased by washing with acetone. Then, a sulfuric acid-based Sn plating solution was used, and organic compound particles (addition amount 30 g / L) and a surfactant (AGX Seimi Chemical, Surflon S231, addition amount 5 g / L) shown in Table 4 were dispersed in the plating solution. The solution was stirred and then subjected to a current of 1 A / dm with the Sn plate as the counter electrode. 2A current was passed through the sample for 10 minutes at a current density of 1000 Ω / s, yielding a metal-organic compound composite in which a number of organic compound particles were co-deposited (embedded) in a Sn plating layer approximately 5 μm thick, with at least a portion of the metal material exposed to the surface. For comparison, a metal material (Sn plating layer) was also produced that was plated without dispersing organic compound particles and surfactants. Thermogravimetric differential thermal analysis (TG-DTA) was also performed on the particles shown in Table 4 using a differential thermobalance (Rigaku Thermo plus EVOII) in air at a heating rate of 10°C / min from room temperature to a maximum of 1000°C, to determine the melting point, decomposition point, and combustion point of the particles. These results are also shown in Table 4. 4 In the table, "-" in the "Melting point (°C)", "Decomposition point (°C)" and "Combustion point (°C)" columns means that the corresponding temperature was not observed in thermogravimetric differential thermal analysis.

[0061] [Table 4]

[0062] The metal-organic compound composite material prepared as above was subjected to a lubricity evaluation and a wear resistance evaluation in the same manner as in Example 1. The results are shown in Tables 5 and 6, respectively.

[0063] [Table 5]

[0064] [Table 6]

[0065] As shown in the results in Table 5, the above metal-organic compound composite was a preferred embodiment in which the metal material was Al, Ti, Cu, Au, Ni, Ni-P, Sn, Zn or Cr and the particles in contact (embedded) were compound A (crosslinked PMMA), and therefore showed excellent results in that the average friction coefficient was reduced to 50% or less compared to the case in which no particles were in contact (embedded) compared to the case in which no particles were in contact (embedded). Furthermore, the results in Table 6 show that when the requirements of the embodiment of the present invention are met, the amount of wear can be significantly reduced compared to when particles are not in contact with the metal material (when no particles are present). [Explanation of symbols]

[0066] 1, 11 Metal-organic compound composites 2 Metal material 2a Part of metal material 2 exposed on the surface 2b Surface of metal material 2 3 Organic compound particles 30 Sliding marks 31 Sliding part 31a Wear part 31b Ridge 32 Non-sliding part 32a Average line

Claims

1. The present invention is composed of a metal material containing more than 50 mass% in total of one or more metals selected from the group consisting of Al, Ti, Cu, Au, Ni, Sn, Zn, and Cr, and a plurality of organic compound particles (excluding capsules containing a lubricant), The plurality of organic compound particles include A state in which the adhesive tape is attached to the surface of the metal material so as to be peelable with cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405); and a state in which at least a portion of the metal material is embedded in the metal material so as to be exposed to the surface; The plurality of organic compound particles include a compound A, The compound A is an aliphatic compound containing, in a unit molecular structure, two or more selected from the group consisting of hydrogen (H), carbon (C) and oxygen (O), The metal-organic compound composite material, wherein the plurality of organic compound particles does not contain fluorine.

2. The present invention is made up of a metal material containing more than 50 mass% in total of one or more metals selected from the group consisting of Al, Ti, Cu, Au, Sn, Zn, and Cr, and a plurality of organic compound particles (excluding capsules containing a lubricant), The plurality of organic compound particles include A state in which the adhesive is attached to the surface of the metal material so as to be peelable with cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405); and a state in which at least a portion of the metal material is embedded in the metal material so as to be exposed to the surface; The organic compound particles include a compound B, The compound B is an aliphatic compound containing one or more amide bonds in a unit molecular structure, The metal-organic compound composite material, wherein the plurality of organic compound particles does not contain fluorine.

3. The present invention is made up of a metal material containing more than 50 mass% in total of one or more metals selected from the group consisting of Al, Ti, Cu, Au, Ni, Sn, and Cr, and a plurality of organic compound particles (excluding capsules containing a lubricant), The plurality of organic compound particles include A state in which the adhesive tape is attached to the surface of the metal material so as to be peelable with cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405); and a state in which at least a portion of the metal material is embedded in the metal material so as to be exposed to the surface; The organic compound particles include a compound C, The compound C is an aromatic compound containing one or more amino groups in a unit molecular structure, The plurality of organic compound particles does not contain fluorine, and the metal-organic compound composite material (excluding those in which the metal material is a porous plating layer having a large number of pores on the surface and the plurality of organic compound particles are filled into the pores by blasting) is used.

4. The metal-organic compound composite material according to any one of claims 1 to 3, wherein when the plurality of organic compound particles are subjected to a thermogravimetric differential thermal analysis at a heating rate of 10°C / min from room temperature to a maximum of 1000°C, if a melting point is exhibited, the melting point is 100°C or higher, or no melting point is exhibited.

5. The metal-organic compound composite material according to any one of claims 1 to 3, wherein, when the plurality of organic compound particles are subjected to a thermogravimetric differential thermal analysis from room temperature to a maximum of 1000°C at a heating rate of 10°C / min, if a decomposition point is exhibited, the decomposition point is 500°C or less, and if a combustion point is exhibited but no decomposition point is exhibited, the combustion point is 500°C or less.

6. 4. The metal-organic compound composite according to claim 1, wherein the average particle size of the organic compound particles is less than 50 μm.

7. The metal-organic compound composite material according to any one of claims 1 to 3, wherein the plurality of organic compound particles are attached to the surface of the metal material so as to be peelable with a cellophane adhesive tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) No. 405).

8. 4. The metal-organic compound composite material according to claim 1, wherein the plurality of organic compound particles are embedded in the metal material such that at least a portion of the metal material is exposed on the surface.

Citation Information

Patent Citations

  • JP1975032244A

  • Aqueous lubricant

    JP1980104395A

  • Powder metal parts and production thereof

    JP1988118047A

  • Production of composite plated al sheet excellent in moldability

    JP1994017296A

  • Inorganic filler reinforced metallic composite coating film forming material

    JP1999241169A