Prussian blue-based transition metal cyanide, its manufacturing method, and related positive electrode plate, secondary battery, battery module, battery pack, and device
By optimizing the shape and production conditions of Prussian blue-based transition metal cyanides, the energy density and rate characteristics of sodium ion batteries are significantly improved, addressing the limitations of existing materials.
Patent Information
- Application Number
- JP2022558232
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-08
- Filing Date
- 2021-11-04
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-11-04
AI Technical Summary
Prussian blue-based transition metal cyanides used in sodium ion batteries suffer from low energy density and rate characteristics due to small granularity, low compaction density, and poor conductivity, limiting their commercial application.
The development of Prussian blue-based transition metal cyanides with spherical or nearly spherical primary particles that form secondary particles with specific internal angles and curvature, enhancing particle contact and compaction density, and optimizing production conditions such as concentration, mixing flow rate, and aging time to improve electrode performance.
The improved Prussian blue-based transition metal cyanides enhance energy density and rate characteristics of sodium ion batteries by increasing compaction density and conductivity, leading to higher capacity per gram and better ion transport performance.
Smart Images

Figure 0007577249000004 
Figure 0007577249000005 
Figure 0007577249000006
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims priority to Chinese Patent Application No. 202011423372.7, filed on December 8, 2020, entitled "Prussian blue-based transition metal cyanide, its manufacturing method, and related positive electrode plate, secondary battery, battery module, battery pack, and device," the entire contents of which are incorporated herein by reference.
[0002] The present application belongs to the technical field of energy storage devices, and in particular to Prussian blue-based transition metal cyanides, their manufacturing methods, and related positive electrodes, secondary batteries, battery modules, battery packs and devices. [Background technology]
[0003] In recent years, with the widespread use of lithium-ion batteries in new energy vehicles and electrochemical energy storage, the availability of lithium and other precious metal resources, such as cobalt and nickel, has gradually raised concerns. This is because the rapid increase in demand has led to a decline in the reserves of these resources and a significant increase in the cost of extraction and mining. Therefore, in order to achieve low energy storage costs, research into the development of new electrochemical energy storage systems with high availability of resources has become increasingly important.
[0004] The principle of energy storage in other secondary batteries, such as sodium-ion batteries, is similar to that of lithium-ion batteries, but the difference is that the ions that move back and forth between the positive and negative electrodes during the charge and discharge cycle change from lithium ions to active ions such as sodium ions. Due to the high abundance of sodium elements, they have a wide range of potential applications, and are particularly valuable in the fields of low-speed electric vehicles and large-scale energy storage.
[0005] Positive electrode materials are the most important components of secondary batteries such as sodium ion batteries. The alternative positive electrode materials for the industrialization of sodium ion batteries mainly include Prussian blue-based transition metal cyanides, layered transition metal oxides, polyanion-type oxides, etc. Compared with other positive electrode materials, Prussian blue-based transition metal cyanides have three core industrialization advantages: low cost, high specific capacity, and easy manufacturing, and have the highest industrialization prospects. However, compared with commonly used positive electrode materials for lithium ion batteries, there is still a problem that Prussian blue-based transition metal cyanides have a relatively low capacity per gram, which leads to a relatively low energy density of sodium ion batteries, which affects the commercial application of sodium ion batteries. Summary of the Invention
[0006] The Prussian blue based transition metal cyanide according to the first aspect of the present application comprises secondary particles, the secondary particles comprising a plurality of primary particles, of which the primary particles are spherical or near spherical in shape.
[0007] The Prussian blue-based transition metal cyanide of the present application contains secondary particles formed by an aggregation of a plurality of spherical or nearly spherical primary particles, and increases the granularity of the particles and the powder compaction density, and further improves the compaction density of the positive electrode plate, while improving the active ion transport performance and electronic conductivity of the positive electrode plate, thereby making it possible to improve the energy density and rate characteristics of a secondary battery employing the same.
[0008] In any embodiment of the present application, the interior angle of the secondary particles of the Prussian blue-based transition metal cyanide is 150° to 300°, and optionally 180° to 270°, or 200° to 250°. The Prussian blue-based transition metal cyanide having a relatively large number of obtuse angles on the particle surface is advantageous in increasing the contact area between particles, and improves the compaction density, thereby improving the energy density and rate characteristics of the battery.
[0009] In any embodiment of the present application, the curvature radius of the primary particle in the secondary particle of the Prussian blue-based transition metal cyanide is ≧0.2 μm, and optionally 0.5 μm to 100 μm, or 0.8 μm to 50 μm. A suitable curvature radius is advantageous for improving the compaction density, thereby improving the rate characteristics and energy density of the battery.
[0010] In any embodiment of the present application, the volume average particle diameter Dv50 of the Prussian blue-based transition metal cyanide is ≧1 μm, and optionally 2 μm to 50 μm, or 2 μm to 10 μm. The appropriate particle diameter range is advantageous for improving the compaction density, and therefore helps to improve the energy density and rate characteristics of the battery.
[0011] In any embodiment of the present application, the Prussian blue-based transition metal cyanide has a powder compaction density of 1.7 g / cm under a pressure of 600 MPa. 3 ~2.1g / cm 3 and optionally 1.8 g / cm 3 ~2.1g / cm 3 The powder compaction density of the Prussian blue-based transition metal cyanide is large, which is favorable for the contact between the particles and the conductive agent, and is also favorable for improving the compaction density of the electrode plate, thereby improving the energy density and rate characteristics of the battery.
[0012] In any embodiment of the present application, the Prussian blue-based transition metal cyanide is A x M 1 [M 2 (CN)6] y wherein A is selected from one or more of an alkali metal ion and an alkaline earth metal ion; 1 is selected from one or more of Mn, Ni, Cu, Co, Fe, Zn, and Cr; M 2 is selected from one or more of Mn, Ni, Cu, Co, Fe, Zn, and Cr, and 1.5≦x≦2, 0.6≦y≦1. The smaller the defect level of the Prussian blue-based transition metal cyanide, the higher the capacity per gram and the higher the energy density of the battery.
[0013] In any embodiment of the present application, the powder resistivity of the Prussian blue-based transition metal cyanide under a pressure of 12 MPa is 10 kΩ·cm to 100 kΩ·cm, and optionally 20 kΩ·cm to 90 kΩ·cm. The powder resistivity is within an appropriate range, and the rate characteristics of the battery can be improved.
[0014] In any embodiment of the present application, the capacity per gram of the Prussian blue-based transition metal cyanide is 140mAh / g to 170mAh / g, and optionally 150mAh / g to 165mAh / g. The Prussian blue-based transition metal cyanide has a relatively large capacity per gram, and can increase the energy density of the battery.
[0015] A method for producing a Prussian blue-based transition metal cyanide according to a second aspect of the present application comprises the steps of: Step S1: providing a first solution containing transition metal cations, wherein the concentration of the transition metal cations in the first solution is ≧0.1 mol / L; S2, providing a second solution containing a salt of a transition metal cyanate, the concentration of the transition metal cyanate anion in the second solution being ≧0.1 mol / L, and A being selected from one or more of an alkali metal ion and an alkaline earth metal ion; Step S3: adding and mixing one of the first solution and the second solution to the other under stirring conditions at a flow rate of 10 cm / s to 100 m / s within a time period of 0.5 h to 48 h to cause a co-precipitation chemical reaction to obtain a suspension, in which the temperature of one solution is 10° C. to 40° C. and the temperature of the other solution is 40° C. to 180° C.; Step S4 of aging the suspension under stirring and at 40°C to 180°C for ≥ 0.5 h; and (5) obtaining the Prussian blue-based transition metal cyanide through separation, washing and drying, in which the Prussian blue-based transition metal cyanide includes secondary particles, the secondary particles include a plurality of primary particles, and the primary particles are spherical or nearly spherical in shape.
[0016] If the concentrations of the transition metal cations and transition metal cyanate anions in the first and second solutions are relatively high, the yield of the Prussian blue-based transition metal cyanide can be improved and the production cost can be reduced.
[0017] In any embodiment of the present application, in S1, the concentration of the transition metal cation in the first solution is 0.2 mol / L to 4 mol / L, optionally 0.3 mol / L to 3 mol / L.
[0018] In any embodiment of the present application, in S2, the concentration of the transition metal cyanate anion in the second solution is 0.2 mol / L to 4 mol / L, optionally 0.3 mol / L to 3 mol / L.
[0019] The concentrations of the first solution transition metal cation and the second solution transition metal cyanate anion are within an appropriate range, and the crystal concentration can be thermodynamically less than the saturated solubility and is represented as a liquid phase, thereby maintaining a stable concentration and reacting to obtain the Prussian blue-based transition metal cyanide described in the present application.
[0020] In any embodiment of the present application, the first solution in S1 or the second solution in S2 further comprises an A source, wherein the A source is selected from one or more of a chloride salt of A, a nitrate salt of A, a sulfate salt of A, a hydroxide salt of A, a formate salt of A, an acetate salt of A, an oxalate salt of A, a phosphate salt of A, a perchlorate salt of A, a benzoate salt of A, and a citrate salt of A; optionally, the A source is selected from one or more of a chloride salt of A, a nitrate salt of A, and a sulfate salt of A.
[0021] The addition of an A source can promote the migration of A into the frame of the Prussian blue-based transition metal cyanide, which is favorable for the completion of the product structure, thereby improving the capacity per gram of the Prussian blue-based transition metal cyanide, thereby improving the energy density of the battery.
[0022] In any embodiment of the present application, the first solution in S1 or the second solution in S2 includes an antioxidant, which can inhibit the transition metal from being oxidized in the reaction solution and reduce the probability of the product being doped with oxidized impurities, thereby improving the capacity per gram of the Prussian blue-based transition metal cyanide, thereby improving the energy density of the battery.
[0023] In any embodiment of the present application, in S3, the flow rate of the mixing is 50 cm / s to 10 m / s, and optionally 1 m / s to 5 m / s. The Prussian blue-based transition metal cyanide produced by mixing and reacting within this flow rate range has relatively high dispersibility, and the particles are unlikely to excessively aggregate with each other, but are not excessively dispersed, and secondary particles are formed while the primary particles maintain their spherical shape, thereby reducing the resistivity of the electrode plate and improving the compaction density of the electrode plate, thereby improving the energy density and rate characteristics of the battery.
[0024] In any embodiment of the present application, in S3, the mixing time is 1h-24h, and optionally 2h-12h. By mixing within this time range, the Prussian blue-based transition metal cyanide can have a relatively large particle size, which reduces the resistivity of the electrode plate and improves the compaction density of the electrode plate, which is favorable for improving the energy density and rate characteristics of the battery.
[0025] In any embodiment of the present application, in S3, the temperature of the other solution is 60° C. to 140° C., and optionally 70° C. to 110° C. By controlling the solution temperature, the content of metal A and transition metal M2 in the product formula can be improved, making the crystal structure more perfect and less defective, so that the Prussian blue-based transition metal cyanide can exhibit a higher capacity per gram, and thereby improve the energy density of the battery.
[0026] In any embodiment of the present application, in S4, the aging temperature is 60° C. to 140° C., and optionally 70° C. to 110° C. By performing the aging within this temperature range, the capacity per gram of the Prussian blue-based transition metal cyanide and the energy density of the battery can be further improved. Furthermore, the rate characteristics of the battery can be improved.
[0027] In any embodiment of the present application, in S4, the aging time is 1h to 24h, and optionally 2h to 12h. By carrying out the aging within this time range, the Na content ratio in the chemical formula of the product can be improved, and the capacity per gram of the Prussian blue-based transition metal cyanide and the energy density of the battery can be further improved.
[0028] A positive electrode plate according to a third aspect of the present application comprises a positive electrode material, the positive electrode material comprising the Prussian blue-based transition metal cyanide according to the first aspect of the present application or the Prussian blue-based transition metal cyanide obtained by the manufacturing method according to the second aspect of the present application.
[0029] The positive plate of the present application employs the positive electrode material of the present application, so that a sodium ion battery employing it can have a relatively high energy density.
[0030] A secondary battery according to a fourth aspect of the present application includes a positive plate, the positive plate being the positive plate according to the third aspect of the present application. Optionally, the secondary battery is a sodium ion battery.
[0031] The secondary battery of the present application can have a relatively high energy density because it employs the positive electrode plate of the present application.
[0032] A battery module according to a fifth aspect of the present application includes the secondary battery according to the fourth aspect of the present application.
[0033] A battery pack according to a sixth aspect of the present application includes the secondary battery according to the fourth aspect of the present application or the battery module according to the fifth aspect of the present application.
[0034] An apparatus according to a seventh aspect of the present application includes at least one of the secondary battery described in the fourth aspect of the present application, the battery module described in the fifth aspect of the present application, or the battery pack described in the sixth aspect of the present application.
[0035] The battery modules, battery packs and devices of the present application include the secondary batteries described in the present application, and therefore have at least the same or similar technical effects as said secondary batteries. [Brief description of the drawings]
[0036] In order to more clearly describe the technical solutions of the embodiments of the present application, the following will briefly describe the drawings that need to be used in the embodiments of the present application. It is obvious that the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on the drawings without paying creative efforts.
[0037] [Figure 1] FIG. 2 is a scanning electron microscope (SEM) image of the Prussian blue-based transition metal cyanide obtained in Comparative Example 1. [Diagram 2] FIG. 2 is a scanning electron microscope (SEM) image of the Prussian blue-based transition metal cyanide obtained in Example 1. [Diagram 3] FIG. 2 is an ion-polished cross-sectional scanning electron microscope (SEM) image of the Prussian blue-based transition metal cyanide obtained in (a) Comparative Example 1 and (b) Example 1. [Figure 4] FIG. 2 is a schematic diagram of the internal angles of secondary particles. [Diagram 5] FIG. 1 is an X-ray diffraction (XRD) diagram of the Prussian blue-based transition metal cyanide obtained in Example 1. The results show that the material is a typical monoclinic phase. [Figure 6] FIG. 1 is a schematic diagram of one embodiment of a secondary battery. [Figure 7]FIG. 7 is an exploded view of FIG. [Figure 8] FIG. 1 is a schematic diagram of one embodiment of a battery module. [Figure 9] FIG. 1 is a schematic diagram of one embodiment of a battery pack. [Figure 10] FIG. 10 is an exploded view of FIG. [Figure 11] FIG. 1 is a schematic diagram of one embodiment of a device in which a secondary battery is used as a power source. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] In order to make the objectives, technical solutions and beneficial technical effects of the present application clearer, the present application will be described in detail below with reference to specific examples, which are provided for illustrative purposes only and are not intended to limit the present application.
[0039] For the sake of brevity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form a range not expressly described, and any lower limit can be combined with another lower limit to form a range not expressly described, and similarly any upper limit can be combined with any other upper limit to form a range not expressly described. Also, although not expressly described, each point or single value between the endpoints of a range is included within this range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit, or with any other lower limit or upper limit to form a range not expressly described.
[0040] In the description of this specification, unless otherwise specified, the terms "more than" and "less than" are inclusive, and it is necessary to explain that the meaning of "multiple" in "one or more" is two or more.
[0041] In the description of this specification, the term "or" is inclusive unless otherwise stated. For example, the term "A or B" means "A, B, or both A and B." More specifically, any one of the following conditions satisfies the condition "A or B," where A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), or both A and B are true (or exist).
[0042] The above Summary of the Invention of this application is not intended to describe each disclosed embodiment or every implementation in this application. The following examples more particularly describe exemplary embodiments. Guidance is provided in several places throughout the application by a series of examples that can be used in various combinations. In each example, the listing is provided only as a representative group and should not be construed as exhaustive.
[0043] According to the inventor's research, existing Prussian blue-based transition metal cyanides have problems such as small granularity, low powder compaction density, and low electrical conductivity, which results in a relatively low energy density of secondary batteries, making secondary battery production more difficult and requiring high equipment. The main reason for this phenomenon is that the shape of the product obtained in the co-precipitation reaction step is generally a regular cube, so the gaps between the active material particles in the electrode plate are large and difficult to fill, and the connection between the active material particles and the conductive agent particles is not tight. Therefore, how to reinforce the contact between the particles and reduce the gaps is the key to improving the energy density of secondary batteries such as sodium ion batteries.
[0044] Therefore, the present inventors have conducted further research and found that the Prussian blue-based transition metal cyanide according to the first aspect of the present application comprises secondary particles, the secondary particles comprising a plurality of primary particles, among which the primary particles are spherical or nearly spherical, as shown in Figures 1 and 2.
[0045] In this application, primary particles and secondary particles have the meanings known in the art. Primary particles are particles that do not form an aggregated state. Secondary particles are particles in an aggregated state in which two or more primary particles are aggregated. Primary particles, secondary particles, and particle shapes can be easily distinguished by taking SEM images with a scanning electron microscope.
[0046] The inventors have found through research that, compared with the independently dispersed primary particles, the secondary particles have increased granularity, and the primary particles in the secondary particles are in direct contact with the solid phase, resulting in closer contact. The curved surface provided by the spherical or nearly spherical primary particles increases the contact surface between each independently dispersed active material particle, reduces the porosity under pressing conditions, and improves the space utilization rate, as shown in FIG. 3. Therefore, by adopting the Prussian blue-based transition metal cyanide of the present application, a relatively high powder compaction density and compaction density of the electrode plate can be obtained, thereby improving the mass energy density and volume energy density of the secondary battery. In addition, the close contact between the active material particles can improve the solid phase transport performance of the active ions, and the curved surface provided by the primary particles can bring the active material particles and the conductive agent particles (such as Super P, etc.) into close contact with each other, improving the electrode plate conductivity, thereby allowing the secondary battery to obtain a relatively high energy density and improve the rate characteristics.
[0047] In some embodiments, the interior angle of the secondary particles of the Prussian blue-based transition metal cyanide is 150° to 300°, and may be, for example, 170° to 270°, 180° to 270°, 200° to 270°, 210° to 265°, 215° to 250°, 215° to 240°, or 200° to 250°.
[0048] As shown in FIG. 4, the interior angle is the angle range of the surface inside of the secondary particle, including the surface inside angle of the primary particle that is not adjacent to other primary particles in the secondary particle, and the interior angle formed by the adjacent primary particles. An exemplary test method for the interior angle of the secondary particle is as follows: Using a ZEISS Gemini SEM 300 scanning electron microscope (SEM), select the backscattered electron mode at a magnification of 10k, take three randomly different positions of photos, randomly find two secondary particles from each photo, and both of these secondary particles are composed of primary particles with a particle size of Prussian blue transition metal cyanide Dv50 or more, and measure the maximum interior angle of each secondary particle. The average value of the maximum interior angle measurements of the six secondary particles in the three photos is taken, that is, the interior angle of the secondary particle.
[0049] The Prussian blue transition metal cyanide with a relatively large number of obtuse angles on the particle surface has a cell structure formed by a relatively long coordinate bond, so the particles have elasticity. The obtuse angles on the particle surface are also advantageous in increasing the mutual contact area between particles. Therefore, the use of this Prussian blue transition metal cyanide can improve the compaction density of the electrode plate and facilitate the construction of the conductive network, thereby improving the energy density and rate characteristics of the battery.
[0050] In some embodiments, the secondary particles of the Prussian blue-based transition metal cyanide have a radius of curvature of the primary particles of ≧0.2 μm. Within the 100 micron scale, the larger the radius of curvature of the primary particles, the closer their shape is to a sphere. Alternatively, the radius of curvature of the primary particles of the Prussian blue-based transition metal cyanide may be 0.2 μm to 100 μm, 0.5 μm to 100 μm, 0.8 μm to 70 μm, 0.8 μm to 50 μm, 0.8 μm to 20 μm, 0.8 μm to 15 μm, 0.8 μm to 10 μm, 0.8 μm to 8 μm, 0.8 μm to 5 μm, 1.5 μm to 50 μm, 1.5 μm to 18 μm, 1.5 μm to 12 μm, 1.5 μm to 7 μm, 1 μm to 70 μm, 2 μm to 50 μm, 2 μm to 20 μm, 5 μm to 50 μm, 3 μm to 30 μm, 3 μm to 20 μm, 5 μm to 20 μm, or 2 μm to 10 μm.
[0051] The radius of curvature is fitted using a circle with a certain diameter, and the radius of the fitted circle is the radius of curvature of the measured object. An exemplary test method for the radius of curvature of the primary particles of Prussian blue-based transition metal cyanide is as follows: using a ZEISS Gemini SEM 300 scanning electron microscope (SEM), selecting the backscattered electron mode at a magnification of 10k, taking three randomly different positions of photos, randomly finding two secondary particles from each photo, the two secondary particles being composed of primary particles with a particle size of Prussian blue-based transition metal cyanide Dv50 or more, measuring the radius of curvature of any point of the primary particles in the secondary particles, and taking the average value of the measured radius of curvature of the primary particles in the six secondary particles in the three photos, i.e. the radius of curvature of the primary particles.
[0052] The appropriate radius of curvature is favorable for tight wrapping between the Prussian blue particles, which is favorable for improving the plate compaction density and smooth transport of ions and electrons, thereby improving the rate characteristics and energy density of the battery.
[0053] In some embodiments, the volume average particle size Dv50 of the Prussian blue-based transition metal cyanide is ≧1 μm. Alternatively, the Dv50 of the Prussian blue-based transition metal cyanide may be 1 μm to 50 μm, 2 μm to 50 μm, 2 μm to 40 μm, 10 μm to 40 μm, 5 μm to 20 μm, 8 μm to 25 μm, 5 μm to 45 μm, 5 μm to 30 μm, 5 μm to 20 μm, 5 μm to 15 μm, 4 μm to 30 μm, 8 μm to 20 μm, 1 μm to 10 μm, or 2 μm to 10 μm. The appropriate particle size range is advantageous for improving the compaction density of the electrode plate, and the transfer of ions and electrons is relatively fast, which helps to improve the energy density and rate characteristics of the battery.
[0054] In some embodiments, the Prussian blue-based transition metal cyanide has a powder compaction density of 1.7 g / cm under 600 MPa pressure. 3 ~2.1g / cm 3 Alternatively, the powder compaction density of the Prussian blue transition metal cyanide under 600 MPa pressure is 1.8 g / cm 3 ~2.1g / cm 3 , 1.74g / cm 3 ~2.02g / cm 3 , 1.8g / cm 3 ~1.95g / cm 3 , 1.85g / cm 3 ~1.9g / cm 3 , 1.71g / cm 3 ~1.9g / cm 3 , or 1.71 g / cm 3 ~1.85g / cm 3 may be also possible.
[0055] The powder compaction density of the Prussian blue-based transition metal cyanide is large, which is favorable for the contact between the particles and the conductive agent, thereby improving the rate characteristics of the battery. In addition, the powder compaction density of the Prussian blue-based transition metal cyanide is also favorable for improving the compaction density of the electrode plate, thereby improving the energy density of the battery.
[0056] In some embodiments, the Prussian blue-based transition metal cyanide is A x M1 [M 2 (CN)6] y wherein A is selected from one or more of an alkali metal ion and an alkaline earth metal ion; 1 is selected from one or more of Mn, Ni, Cu, Co, Fe, Zn, and Cr; M 2 is selected from one or more of Mn, Ni, Cu, Co, Fe, Zn, and Cr, and is 1.5≦x≦2, 0.6≦y≦1, where x represents the content of A, and y represents the degree of defects in the Prussian blue-based transition metal cyanide. The higher the content of A and the lower the degree of defects, the higher the capacity per gram of the Prussian blue-based transition metal cyanide.
[0057] In some embodiments, A may be selected from one or more of Na, K, Zn, Li. In one example, A is selected from Na.
[0058] In some embodiments, M 1 is selected from one or more of Mn, Ni, Co, and Fe. 1 is selected from Mn.
[0059] In some embodiments, M 2 is selected from one or more of Mn, Ni, Co, and Fe. 2 is selected from Fe.
[0060] In some embodiments, 1.7≦x≦2, 1.8≦x≦2, or 1.9≦x≦2.
[0061] In some embodiments, 0.8≦y≦1, 0.9≦y≦1, or 0.95≦y≦1.
[0062] Higher values of x and y result in lower element valences and an increased ratio of elements whose valences can increase during the charging process, thereby improving the capacity per gram of the Prussian blue transition metal cyanide and thereby improving the energy density of the battery.
[0063] In some embodiments, the powder resistivity of the Prussian blue-based transition metal cyanide under 12 MPa pressure is 10 kΩ·cm to 100 kΩ·cm. Alternatively, the powder resistivity of the Prussian blue-based transition metal cyanide under 12 MPa pressure is 10 kΩ·cm to 90 kΩ·cm, 10 kΩ·cm to 70 kΩ·cm, 20 kΩ·cm to 90 kΩ·cm, 20 kΩ·cm to 80 kΩ·cm, 30 kΩ·cm to 80 kΩ·cm, 30 kΩ·cm to 70 kΩ·cm, 20 kΩ·cm to 60 kΩ·cm, or 40 kΩ·cm to 60 kΩ·cm. The powder resistivity being within the appropriate range indicates that the wrap between the Prussian blue-based transition metal cyanide particles is tight, and helps the plate obtain a relatively high ionic conductivity, thereby improving the rate characteristics of the battery.
[0064] In some embodiments, the capacity per gram of the Prussian blue-based transition metal cyanide is 120 mAh / g to 170 mAh / g. Optionally, the capacity per gram of the Prussian blue-based transition metal cyanide is 140 mAh / g to 170 mAh / g, 145 mAh / g to 165 mAh / g, 150 mAh / g to 165 mAh / g, 155 mAh / g to 165 mAh / g, or 155 mAh / g to 160 mAh / g. The Prussian blue-based transition metal cyanide has a relatively large capacity per gram, which can increase the energy density of the battery.
[0065] In this application, the volume average particle size Dv50 of the Prussian blue-based transition metal cyanide has a meaning known in the art, and can be tested by adopting a method known in the art. For example, the laser diffraction particle size analysis method. For example, refer to the standard GB / T 19077.1-2016, and measure with a laser particle size analyzer (for example, Malvern Master Size 3000). In the test, the medium is, for example, water, and the absorptivity is, for example, 1.567. Wherein, Dv50 is the particle size corresponding to when the cumulative volume distribution percentage of the Prussian blue-based transition metal cyanide reaches 50%.
[0066] In this application, the powder compaction density of the Prussian blue-based transition metal cyanide has a meaning known in the art, and can be tested by adopting a method known in the art, for example, see standard GB / T24533-2009, and measured by an electronic pressure tester (for example, UTM7305 type). An exemplary test method is as follows: 1 g of a sample of the Prussian blue-based transition metal cyanide is weighed and found to have a base area of 1.327 cm 2 The mold is then pressed to 600 MPa, held for 30 seconds, then released and held for 10 seconds, and the powder compaction density of the Prussian blue transition metal cyanide powder under a pressure of 600 MPa is recorded and calculated. Specifically, the height (H1) of the roof pillar exposed outside the sleeve after pressing is measured with a caliper, and the compaction density of the sample can be calculated as m / (S×(H1-H0)), of which: m: mass of the sample, H1: the height of the roof pillar exposed outside the sleeve after the sample is pressed, H0: The height of the roof pillar exposed outside the sleeve when no sample is inserted. S: Cross-sectional area of roof pillar.
[0067] In the present application, the chemical composition of Prussian blue-based transition metal cyanides can be tested using methods known in the art, such as an inductively coupled plasma spectrometer ICP (e.g., Spectroblue type) to measure the percentage of each element in the sample material.
[0068] In this application, the powder resistivity of Prussian blue-based transition metal cyanides has the meaning known in the art, and can be tested by adopting methods known in the art, for example, see GB / T 30835-2014, and can be tested by a PRCD1100 powder resistivity meter.
[0069] In this application, the capacity per gram of Prussian blue-based transition metal cyanide has a meaning known in the art, and can be tested by adopting a method known in the art. An exemplary test method is as follows: The prepared Prussian blue-based transition metal cyanide, a conductive agent (e.g., acetylene black (Denka, Denka Black)), and a binder (e.g., polyvinylidene fluoride (Arkema, HSV 900)) are uniformly mixed with a solvent N-methylpyrrolidone (NMP) in a mass ratio of 7:2:1 to prepare a slurry, and the prepared slurry is coated on an aluminum foil current collector and dried in an oven for use. A 2025-type coin battery is assembled in an argon-protected glove box with a sodium metal sheet as the counter electrode, a ceramic separator, and a propylene carbonate (PC) electrolyte of 1 mol / L NaPF6. The resulting coin battery is left to stand for 12 hours, then charged at a constant current of 0.1 C to 4 V at 25° C. in a land tester, then charged at a constant voltage of ≦0.05 C, left to stand for 5 minutes, and then discharged at a constant current of 0.1 C to 2 V, and the discharge capacity is recorded. The ratio of the discharge capacity to the mass of the Prussian blue transition metal cyanide is the capacity per gram of the produced Prussian blue transition metal cyanide.
[0070] The method for producing a Prussian blue-based transition metal cyanide according to the second aspect of the present application can produce the above-mentioned Prussian blue-based transition metal cyanide based on this production method. The method for producing a Prussian blue-based transition metal cyanide includes the steps of: Step S1: providing a first solution containing transition metal cations, wherein the concentration of the transition metal cations in the first solution is ≧0.1 mol / L; S2, providing a second solution containing a salt of a transition metal cyanate, the concentration of the transition metal cyanate anion in the second solution being ≧0.1 mol / L, and A being selected from one or more of an alkali metal ion and an alkaline earth metal ion; Step S3: adding and mixing one of the first solution and the second solution to the other under stirring conditions at a flow rate of 10 cm / s to 100 m / s within a time period of 0.5 h to 48 h to cause a co-precipitation chemical reaction to obtain a suspension, in which the temperature of one solution is 10° C. to 40° C. and the temperature of the other solution is 40° C. to 180° C.; Step S4 of aging the suspension under stirring and at 40°C to 180°C for ≥ 0.5 h; and (5) obtaining the Prussian blue-based transition metal cyanide through separation, washing and drying, in which the Prussian blue-based transition metal cyanide includes secondary particles, the secondary particles include a plurality of primary particles, and the primary particles are spherical or nearly spherical in shape.
[0071] In S1, the transition metal cation providing material may be selected from one or more of transition metal chlorides, transition metal nitrates, transition metal sulfates, transition metal hydroxides, transition metal formates, transition metal acetates, transition metal oxalates, transition metal phosphates, transition metal phosphites, transition metal sulfites, transition metal thiosulfates, transition metal perchlorates, transition metal benzoates, and transition metal citrates. Optionally, the transition metal source is selected from one or more of transition metal chlorides, transition metal nitrates, and transition metal sulfates, wherein the transition metal is M 1 As a specific example, the transition metal cation providing agent may be selected from one or more of manganese chloride, manganese sulfate, manganese nitrate, nickel chloride, nickel sulfate, nickel nitrate, cobalt chloride, cobalt sulfate, and cobalt nitrate.
[0072] In some embodiments, the concentration of the transition metal cations in the first solution is between 0.2 mol / L and 4 mol / L. Optionally, the concentration of the transition metal cations in the first solution is between 0.25 mol / L and 3.5 mol / L, between 0.3 mol / L and 3 mol / L, between 0.2 mol / L and 2 mol / L, between 0.35 mol / L and 2 mol / L, or between 0.4 mol / L and 1 mol / L.
[0073] In S2, the transition metal in the transition metal cyanate is M 2 For example, the transition metal cyanate may be selected from one or more of ferrocyanate, manganese cyanate, cobalt cyanate, nickel cyanate, copper cyanate. A may be a metal as described herein. By way of example, the A salt of the transition metal cyanate may be selected from one or more of sodium ferricyanide, potassium ferricyanide, sodium ferrocyanide, lithium ferrocyanide, sodium nickel cyanide, zinc cobalt cyanide, potassium cobalt cyanide.
[0074] In some embodiments, the concentration of the transition metal cyanate anion in the second solution is between 0.2 mol / L and 4 mol / L. Optionally, the concentration of the transition metal cyanate anion in the second solution is between 0.25 mol / L and 3.5 mol / L, between 0.3 mol / L and 3 mol / L, between 0.2 mol / L and 2 mol / L, between 0.35 mol / L and 2 mol / L, or between 0.4 mol / L and 1 mol / L.
[0075] The solvent of the first solution and the second solution may be independently selected from one or more of water, deuterium oxide, acetonitrile, adiponitrile, methanol, ethanol, ethylene glycol, diethylene glycol, acetone, glycerin, dimethylformamide, N-methylpyrrolidone, For example, the solvent of the first solution and the second solution may be selected from water, e.g., deionized water.
[0076] If the concentrations of the transition metal cations and the transition metal cyanate anions are relatively high, the yield of the Prussian blue-based transition metal cyanide can be improved and the production cost can be reduced. In particular, if the concentrations of the first solution transition metal cations and the second solution transition metal cyanate anions are within an appropriate range, the concentration of the crystals generated by the reaction can be thermodynamically smaller than the saturated solubility, and the crystals are expressed as a liquid phase, so that the reaction can be maintained at a stable concentration to obtain the Prussian blue-based transition metal cyanide described in the present application.
[0077] In some embodiments, the first solution or the second solution optionally further comprises a source of A. The source of A is selected from one or more of a chloride salt of A, a nitrate salt of A, a sulfate salt of A, a hydroxide salt of A, a formate salt of A, an acetate salt of A, an oxalate salt of A, a phosphate salt of A, a perchlorate salt of A, a benzoate salt of A, and a citrate salt of A. Optionally, the source of A is selected from one or more of a chloride salt of A, a nitrate salt of A, and a sulfate salt of A.
[0078] In some embodiments, the concentration of the A source added to the first solution or the second solution is between 0.05 mol / L and 10 mol / L, optionally between 0.05 mol / L and 5 mol / L, between 1 mol / L and 5 mol / L, between 3 mol / L and 8 mol / L, between 2 mol / L and 6 mol / L, between 4 mol / L and 9 mol / L, or between 4 mol / L and 7 mol / L.
[0079] The addition of an A source can promote the migration of A into the frame of the Prussian blue-based transition metal cyanide, which is favorable for the completion of the product structure, thereby improving the capacity per gram of the Prussian blue-based transition metal cyanide, thereby improving the energy density of the battery.
[0080] In some embodiments, the first solution or the second solution includes an antioxidant. For example, the antioxidant may be selected from ascorbic acid, sodium ascorbate, thiosulfuric acid, sodium thiosulfate, citric acid, and sodium citrate. The antioxidant can inhibit the transition metal from oxidizing in the reaction solution, reduce the probability of doping the product with oxidized impurities, and thereby improve the capacity per gram of the Prussian blue-based transition metal cyanide, thereby improving the energy density of the battery.
[0081] In S3, any device and method can be employed to adjust the flow rate and time for adding one of the first solution and the second solution to the other. For example, a syringe with a diameter of 0.3 mm to 2 mm, a peristaltic pump, or an autosampler can be used. By calculating the relationship between the mixing time, the flow rate, and the diameter of the sample introduction tube, the solution mixing is performed under a specific flow rate and a specific time condition.
[0082] The order of mixing the solutions affects the physical properties of the product; for example, adding a first solution to a second solution reduces the internal angle of the resulting secondary particles compared to adding the second solution to the first, but increases the radius of curvature of the primary particles and the Dv50 of the material, as well as improving the powder resistivity.
[0083] In some embodiments, the flow rate of the mixing in S3 is 10 cm / s to 20 m / s. Optionally, the flow rate of the mixing in S3 is 50 cm / s to 20 m / s, 10 cm / s to 10 m / s, 50 cm / s to 10 m / s, 50 cm / s to 5 m / s, 1 m / s to 8 m / s, 1 m / s to 5 m / s, 2 m / s to 5 m / s, or 50 cm / s to 2 m / s. Within a suitable flow rate range, the transition metal cation or transition metal cyanate anion added to the liquid can form a certain local concentration in the mixed liquid. At the mixing interface, the transition metal cation or transition metal cyanate anion concentration of the adding liquid and the receiving liquid exceeds the saturation degree of the Prussian blue-based transition metal cyanide, and the degree of supersaturation is relatively large, so that nucleation is likely to occur. The moment nucleation occurs, the mixture is rapidly dispersed into the crystal nuclei at a relatively high flow rate, improving the dispersibility of the final particles, making it difficult for the particles to aggregate excessively, but also preventing excessive dispersion, and allowing the primary particles to form secondary particles while maintaining their spherical shape. The resulting Prussian blue transition metal cyanide has an appropriate particle size distribution and shape, which is advantageous in improving the compaction density of the electrode plate and reducing the electrode plate resistivity, thereby helping to improve the energy density of the battery.
[0084] In some embodiments, the mixing time in S3 is 1h to 24h. Optionally, the mixing time in S3 is 4h to 20h, 6h to 12h, 2h to 12h, 0.5h to 10h, 5h to 15h, 8h to 24h, 10h to 48h, or 1h to 4h. Within the appropriate mixing time range, the crystal grains can further grow in a supersaturated state to obtain a relatively large grain size, thereby reducing the resistivity of the plate, improving the capacity per gram of the battery, and improving the packing density of the plate and the energy density of the battery.
[0085] In some embodiments, in S3, the temperature of the other solution is 60° C. to 140° C. Optionally, in S3, the temperature of the other solution is 60° C. to 120° C., 70° C. to 110° C., or 80° C. to 100° C. Controlling the solution temperature can improve the content of metal A and transition metal M2 in the product's chemical formula, making the crystal structure more perfect and less defective, so that the Prussian blue-based transition metal cyanide exhibits a higher capacity per gram, and thereby improves the energy density of the battery.
[0086] In some embodiments, in S4, the aging temperature is 60° C. to 140° C. Optionally, in S4, the aging temperature is 60° C. to 120° C., 70° C. to 110° C., or 80° C. to 100° C.
[0087] In some embodiments, in S4, the aging time is 1 h to 24 h. Optionally, in S4, the aging time is 2 h to 12 h, 5 h to 15 h, 8 h to 20 h, 10 h to 15 h, or 6 h to 12 h.
[0088] Within the appropriate aging temperature and time range, the precipitation product can undergo modification, and more Na element can be introduced into the structure of the Prussian blue-based transition metal cyanide, improving the Na ratio in the product, and further improving the capacity per gram of the Prussian blue-based transition metal cyanide and the energy density of the battery.
[0089] The separation, washing, and drying of S5 may be performed by any method known in the art. For example, the Prussian blue-based transition metal cyanide product may be separated from the reaction solution by suction filtration. The washing may involve washing the Prussian blue-based transition metal cyanide product with deionized water 3-5 times and with absolute ethanol 1-5 times. The drying may involve drying in a vacuum drying box at 120°C to 180°C for 12-48 hours.
[0090] The Prussian blue transition metal cyanides that were successfully synthesized are typical monoclinic phases, as shown in Figure 5.
[0091] A positive electrode plate according to a third aspect of the present application comprises a positive electrode material, said positive electrode material comprising any one or more of the Prussian blue based transition metal cyanides of the present application.
[0092] The positive electrode plate of the present application adopts the positive electrode material of the present application, so that the sodium ion battery adopting it can have a relatively high energy density, and further, the sodium ion battery can also have a relatively high rate characteristic.
[0093] The positive electrode plate of the present application includes a positive electrode current collector and a positive electrode film layer including a positive electrode material and provided on at least one surface of the positive electrode current collector. In one example of the positive electrode plate, the positive electrode current collector has two surfaces facing each other in the thickness direction of the positive electrode current collector, and the positive electrode film layer may be laminated on either one or both of the two facing surfaces of the positive electrode current collector.
[0094] In the positive electrode plate of the present application, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymer substrate.
[0095] In the positive electrode plate of the present application, the positive electrode film layer includes a positive electrode material, and the positive electrode material includes any one or more of the Prussian blue-based transition metal cyanides of the present application.
[0096] In some embodiments, the positive electrode material may further include other positive electrode active materials for a sodium ion battery positive electrode. Examples of other positive electrode active materials include, for example, Na 0.9 Fe 0.5 Mn 0.5 O2, NaMnO2, NaFeO2, NaCoO2, NaFe 0.33 Mn 0.33 Ni 0.33 O2, e.g., Na3V2(PO4)3, NaFePO 4 , Na4Fe3(PO4)2P2O7 and other polyanion-type positive electrode materials.
[0097] In the secondary battery of the present application, the positive electrode film layer typically includes a positive electrode material, an optional binder, and an optional conductive agent, and is typically coated with a positive electrode slurry, which is then dried and cold pressed to form the positive electrode slurry. The positive electrode slurry is typically formed by dispersing the positive electrode active material, the optional conductive agent, the binder, etc. in a solvent and uniformly stirring the mixture. The solvent may be N-methylpyrrolidone (NMP).
[0098] The binder of the positive electrode membrane layer may be any binder known in the art for positive electrodes. For example, the binder for the positive electrode membrane layer may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and acrylonitrile multipolymer (LA133).
[0099] In some embodiments, the mass percentage of the binder in the positive electrode membrane layer is 1%-20%, optionally 1%-10%, 2%-5%, 2%-12%, 3%-8%, 5%-10%, 5%-15%, 10%-20%, etc. In the present application, the granularity of the Prussian blue-based transition metal cyanide is increased, the processing performance of the positive electrode slurry can be improved, and the electrode plate can obtain a relatively high adhesive force while the amount of binder used can be reduced, thereby further improving the energy density of the secondary battery.
[0100] The conductive agent for the positive electrode film layer may be any conductive agent for a positive electrode known in the art. For example, the conductive agent for the positive electrode film layer may include one or more of superconducting carbon, carbon black (e.g., Super P, acetylene black, ketjen black), carbon spots, carbon nanotubes, graphene, and carbon nanofibers.
[0101] In some embodiments, the mass percentage of the conductive agent in the positive electrode membrane layer is 1%-20%, and optionally 1%-10%, 2%-5%, 2%-12%, 3%-8%, 5%-10%, 5%-15%, 10%-20%, etc. In the present application, the Prussian blue-based transition metal cyanide particles can be intimately contacted with the conductive agent, and the electrode plate can obtain a relatively high conductivity while reducing the amount of the conductive agent used, thereby improving the rate characteristics and energy density of the secondary battery.
[0102] In some embodiments, the positive electrode membrane layer has a packed density of 1.2 to 1.6 g / cm 3 For example, 1.25 to 1.55 g / cm 3 , 1.3~1.5g / cm 3 , or 1.35 to 1.45 g / cm 3 The positive electrode film layer may have a relatively large compaction density, which can improve the energy density of the battery.
[0103] The compaction density of the positive electrode film layer has a meaning known in the art, and can be tested by using a method known in the art. For example, take a positive electrode plate after one side is coated and cold pressed (if the plate is coated on both sides, the positive electrode film layer on one side can be wiped off first), test the thickness of the positive electrode film layer, and further test the surface density of the positive electrode film layer by the following method, where the compaction density of the positive electrode film layer=the surface density of the positive electrode film layer / the thickness of the positive electrode film layer.
[0104] The areal density of the positive electrode film layer has a meaning known in the art and can be tested by adopting a method known in the art. For example, take a positive electrode plate after one side is coated and cold pressed (if the plate is coated on both sides, the positive electrode film layer on one side can be wiped off first), punch it into a small wafer with an area of S1, and weigh it and record it as M1. Then, wipe off the positive electrode film layer of the positive electrode plate after the above weighing, weigh the weight of the positive electrode current collector and record it as M0, and the areal density of the positive electrode film layer = (the mass of the positive electrode plate M1 - the weight of the positive electrode current collector M0) / S1.
[0105] A secondary battery according to a fourth aspect of the present application includes a positive plate, said positive plate being any positive plate of the present application.
[0106] The secondary batteries of the present application can be classified into different types of secondary batteries, such as sodium ion batteries, magnesium ion batteries, potassium ion batteries, zinc ion batteries, lithium ion batteries, etc., according to the difference in active ions (A).
[0107] The secondary battery of the present application can have a relatively high energy density because it employs the positive electrode plate of the present application.
[0108] The secondary battery of the present application further includes a negative plate and an electrolyte. During the charge and discharge process of the battery, active ions shuttle between the positive plate and the negative plate to absorb and release. The electrolyte plays the role of transmitting ions between the positive plate and the negative plate.
[0109] In the secondary battery of the present application, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector.
[0110] In the secondary battery of the present application, the negative electrode current collector may be a metal foil piece or a composite current collector. For example, aluminum foil or copper foil may be used. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymer substrate.
[0111] The negative electrode film layer includes a negative electrode material. The secondary battery of the present application may employ a negative electrode material that can be used in a secondary battery known in the art. For example, the negative electrode material may include one or more of natural graphite, artificial graphite, soft carbon, hard carbon, a silicon-based material, and a tin-based material. The silicon-based material may be selected from one or more of elemental silicon, silicon oxide, and silicon carbon composite. The tin-based material may be selected from one or more of elemental tin, stannate, and tin alloy.
[0112] In the secondary battery of the present application, the negative electrode film layer typically includes a negative electrode material, an optional binder, an optional conductive agent, and other optional auxiliary agents, and is typically formed by coating and drying a negative electrode slurry. The negative electrode slurry is typically formed by dispersing the negative electrode active material, the optional conductive agent, the binder, etc. in a solvent and stirring the mixture uniformly. The solvent may be N-methylpyrrolidone (NMP) or deionized water.
[0113] By way of example, the conductive agent may include one or more of superconducting carbon, carbon black (eg, Super P, acetylene black, ketjen black), carbon spots, carbon nanotubes, graphene, and carbon nanofibers.
[0114] By way of example, the binder may include one or more of styrene butadiene rubber (SBR), polyvinylidene fluoride, and acrylonitrile copolymers.
[0115] Other optional auxiliary agents are, for example, thickeners (eg, sodium carboxymethylcellulose CMC-Na), PTC thermistor materials, and the like.
[0116] The type of electrolyte in the secondary battery of the present application is not specifically limited and can be selected according to need. For example, the electrolyte may be selected from at least one of a solid electrolyte and a liquid electrolyte (i.e., an electrolytic solution).
[0117] In some embodiments, the electrolyte employs an electrolyte solution, which includes an electrolyte salt and a solvent.
[0118] In some embodiments, the electrolyte salt may be selected from one or more of NaPF6, NaClO4, NaBF4, KPF6, KClO4, KBF4, LiPF6, LiClO4, LiBF4, Zn(PF6)2, Zn(ClO4)2, Zn(BF4)2. For example, the electrolyte salt may be selected from one or more of NaPF6, NaClO4, and NaBF4.
[0119] In some embodiments, the solvent may be selected from one or more of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl acetate (EA).
[0120] In some embodiments, the electrolyte solution may further include an additive, for example, an additive may include a negative electrode film-forming additive, a positive electrode film-forming additive, and an additive that can improve some performance of the battery, such as an additive that improves the overcharge performance of the battery, an additive that improves the high temperature performance of the battery, or an additive that improves the low temperature performance of the battery.
[0121] In some embodiments, the secondary battery of the present application further includes a separator. The separator is provided between the positive electrode plate and the negative electrode plate and can play a role of separation. The present application has no particular limitation on the type of separator, and any known porous structure separator having good chemical stability and mechanical stability can be selected. For example, the separator may be selected from one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride single layer or multi-layer composite film.
[0122] In some embodiments, the positive and negative plates and the separator can be formed into an electrode assembly by a winding or lamination process.
[0123] In some embodiments, the secondary battery may include an exterior body. The exterior body may be a hard case, such as a hard plastic case, an aluminum case, a steel case, etc. The exterior body may be a soft bag, such as a pouch-type soft bag. The material of the soft bag may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.
[0124] The present application does not particularly limit the shape of the secondary battery, which may be cylindrical, rectangular, or any other shape. Figure 6 shows a secondary battery 5 with a rectangular structure as an example.
[0125] In some embodiments, referring to FIG. 7, the exterior body may include a housing 51 and a cover plate 53. The housing 51 includes a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate are surrounded to form a receiving chamber. The housing 51 has an opening communicating with the receiving chamber, and the cover plate 53 may be installed to cover the opening to close the receiving chamber. The positive electrode plate, the negative electrode plate and the separator may form an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is packaged in the receiving chamber. The electrolyte may be infiltrated into the electrode assembly 52. The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and may be adjusted according to needs.
[0126] A battery module according to a fifth aspect of the present application includes the secondary battery according to the fourth aspect of the present application. In some embodiments, the secondary battery can be assembled into a battery module, and the number of secondary batteries included in the battery module can be multiple, and the specific number can be adjusted based on the application and capacity of the battery module.
[0127] Fig. 8 shows an example of a battery module 4. Referring to Fig. 8, in the battery module 4, the multiple secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 are fixed in place by a fastener.
[0128] Optionally, the battery module 4 may further include a housing having an accommodating space, in which the multiple secondary batteries 5 are accommodated.
[0129] A battery pack according to a sixth aspect of the present application includes the secondary battery according to the fourth aspect of the present application or the battery module according to the fifth aspect of the present application. In some embodiments, the battery module can be further assembled into a battery pack, and the number of battery modules included in the battery pack can be adjusted based on the application and capacity of the battery pack.
[0130] 9 and 10 show an example of a battery pack 1. Referring to Fig. 9 and 10, the battery pack 1 may include a battery box and a plurality of battery modules 4 provided in the battery box. The battery box includes an upper case 2 and a lower case 3, and the upper case 2 can be installed on the lower case 3 as a lid, and forms a closed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.
[0131] The device according to the seventh aspect of the present application includes at least one of the secondary battery according to the fourth aspect of the present application, the battery module according to the fifth aspect of the present application, or the battery pack according to the sixth aspect of the present application. The secondary battery can be used as a power source for the device, and can also be used as an energy storage unit for the device. Since the device according to the present application employs the secondary battery according to the present application, it has at least the same advantages as the secondary battery.
[0132] The devices include, but are not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid vehicles, plug-in hybrid vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), trains, ships and satellites, energy storage systems, etc.
[0133] The device can select a secondary battery, a battery module or a battery pack according to its usage needs.
[0134] An example device is shown in Figure 11. The device may be a pure electric vehicle, a hybrid vehicle, or a plug-in hybrid vehicle. To meet the high power and high energy density demands for the secondary battery of the device, a battery pack or a battery module may be employed.
[0135] Other examples of the device may be a mobile phone, a tablet computer, a notebook computer, etc. These devices are generally required to be lightweight and thin, and may employ a secondary battery as a power source.
[0136] Working Example In order to make the objectives, technical solutions and beneficial technical effects of the present invention clearer, the present application will be described in more detail below with reference to examples. However, it should be understood that the examples of the present application are only for illustrating the present application, and are not intended to limit the present application, and the examples of the present application are not limited to the examples given herein. Those that do not specify specific experimental conditions or operating conditions in the examples are made under normal conditions or under conditions recommended by material suppliers.
[0137] Example 1 S1, under the condition of 25°C, 6.292 g of manganese chloride, 35 g of sodium chloride, and 2.48 g of sodium thiosulfate (antioxidant) are dispersed in 100 mL of deionized water to obtain a first solution. S2, 19.203 g of sodium ferrocyanide is dispersed in 100 mL of deionized water at 25° C. to obtain a second solution. S3, after heating the first solution to 80℃, inject the second solution at 25℃ into the first solution within 10h with a 0.6mm inner diameter syringe at a flow rate of 2m / s to generate a coprecipitation chemical reaction, and perform magnetic stirring at a speed of 800rpm / min. The tip of the syringe needle is inserted below the liquid surface to ensure the mixing effect. S4. The obtained suspension is kept at 80° C. and aged for 24 hours under stirring conditions, during which the small crystal grains dissolve and the large crystal grains grow continuously. After S5, suction filtration, washing with water, washing with ethanol, and drying, a white, nearly spherical Prussian blue-based transition metal cyanide material, Na2Mn[Fe(CN)6], is obtained.
[0138] Examples 2 and 11 Similar to Example 1, except that the antioxidant in the first solution was 1 g of ascorbic acid, and the remaining parameters were as shown in Table 1.
[0139] Example 3 Similar to Example 1, except that the antioxidant in the first solution was 0.5 g ascorbic acid, and the remaining parameters were as shown in Table 1.
[0140] Example 4 Similar to Example 1, except that the antioxidant in the first solution was 1 g of ascorbic acid, and the remaining parameters were as shown in Table 1.
[0141] Example 5 Similar to Example 1, except that the antioxidant in the first solution was 2 g of ascorbic acid, and the remaining parameters were as shown in Table 1.
[0142] Example 6 Similar to Example 1, except that the antioxidant in the first solution was 0.5 g ascorbic acid, and the remaining parameters were as shown in Table 1.
[0143] Example 7 Similar to Example 1, except that the antioxidants in the first solution were 0.1 g sodium ascorbate and 0.48 g sodium thiosulfate, and the remaining parameters were as shown in Table 1.
[0144] Example 8 Similar to Example 1, except that the antioxidants in the first solution were 0.1 g sodium ascorbate and 0.48 g sodium thiosulfate, and the remaining parameters were as shown in Table 1.
[0145] Examples 9-10 Similar to Example 1, except that the antioxidant in the first solution was 0.2 g of ascorbic acid, and the remaining parameters were as shown in Table 1.
[0146] Example 12 This is the same as Example 1, except that the antioxidant in the first solution is 0.5 g of ascorbic acid, and in S3, the second solution is heated to 80° C., and then the first solution at 25° C. is injected into the second solution using a 0.6 mm inner diameter syringe, and the remaining parameters are as shown in Table 1.
[0147] Example 13 This is the same as Example 1, except that the antioxidant in the first solution is 0.5 g of ascorbic acid, the first solution is heated to 95° C., and the diameter of the injection needle is 0.4 mm. The remaining parameters are as shown in Table 1.
[0148] Example 14 Similar to Example 13, except that the antioxidants in the first solution were 0.3 g sodium ascorbate and 0.48 g sodium thiosulfate, and the remaining parameters were as shown in Table 1.
[0149] Example 15 Similar to Example 13, except that the antioxidant in the first solution was 1 g of ascorbic acid, and the remaining parameters were as shown in Table 1.
[0150] Examples 16-17 Similar to Example 13, except that the antioxidant in the first solution was 1 g of ascorbic acid, and the remaining parameters were as shown in Table 1.
[0151] Examples 18 to 21, Comparative Examples 1 to 6 and 8 Similar to Example 1, the different parameters are as shown in Table 1.
[0152] Comparative Example 7 Similar to Example 13, with different parameters as shown in Table 1.
[0153] Test part (1) Mixing flow velocity (m / s): The fluid ejection velocity at the syringe outlet is measured using a high-speed camera (CCD).
[0154] (2) Mixing time (h): The time required for the syringe to start and finish spraying liquid.
[0155] (3) Solution temperature during heating (°C): Measurement is performed by inserting a thermocouple into the bottom of the solution.
[0156] (4) Aging time (h): Time measurement begins when the syringe finishes spraying liquid.
[0157] (5)Energy density (Wh / kg): S1, the positive electrode material (Prussian blue transition metal cyanide), conductive agent acetylene black (Denka, Denka Black), and binder polyvinylidene fluoride (Arkema, HSV 900) in each embodiment or comparative example are dispersed in N-methylpyrrolidone solvent in a weight ratio of 90:5:5, and thoroughly stirred to mix uniformly to obtain a positive electrode slurry with a solid content of 30%. The positive electrode slurry is coated on both sides of an aluminum foil with a thickness of 12 μm with a blade to form a wet coating layer with a thickness of 120 μm each. The mixture is transferred to an oven and dried at a temperature of 150 ° C for 60 minutes, and cold pressed with a pressure of 60 tons in a cold press machine to obtain a positive electrode film layer with a thickness of 130 μm each on both sides of the aluminum foil, and a compaction density of 1.3 g / cm each. 3 A positive electrode plate having the formula: S2, the negative electrode material hard carbon, conductive agent acetylene black, binder styrene butadiene rubber, thickener sodium carboxymethylcellulose are dispersed in deionized water solvent in a weight ratio of 95:2:2:1, and thoroughly stirred to mix uniformly to obtain a negative electrode slurry with a solid content of 15%, and the negative electrode slurry is coated on both sides of an aluminum foil with a thickness of 12 μm by a blade to form a wet coating with a thickness of 120 μm each. Transfer to an oven and dry at a temperature of 150 ° C for 60 minutes, and cold press with a pressure of 50 tons in a cold press machine to obtain a negative electrode film layer with a thickness of 60 μm each on both sides of the aluminum foil, and a compaction density of 0.95 g / cm each. 3 A negative electrode plate having a thickness of 1000 nm is obtained. S3, the positive electrode plate, the separator, and the negative electrode plate are wound in order to form a bare cell with a wound laminated structure measuring 16 cm x 10 cm x 2.8 cm. The bare cell is placed in a steel case exterior, and 150 grams of electrolyte is injected into the steel case. After packaging, a secondary battery can be obtained. The electrolyte is a propylene carbonate (PC) solution with a composition of 1 mol / L NaPF6. At 25°C, the battery is constant current charged at a rate of 0.1C to a rated voltage of 4.0V, constant voltage charged for 30 minutes, and then constant current discharged at a rate of 0.1C to 1.5V. The energy released by the constant current discharge is recorded and divided by the mass of the whole battery, i.e., the energy density of the battery.
[0158] (6) Rate characteristics (%): At 25° C., the battery is constant current charged at a rate of 0.1 C to a rated voltage of 4.0 V, constant voltage charged for 30 minutes, and then constant current discharged at a rate of 0.1 C to 1.5 V, and the capacity C1 discharged by the constant current discharge is recorded. At 25° C., the battery is constant current charged at a rate of 0.1 C to a rated voltage of 4.0 V, constant voltage charged for 30 minutes, and then constant current discharged at a rate of 1 C to 1.5 V, and the capacity C2 discharged by the constant current discharge is recorded. C2 divided by C1 multiplied by 100% is the rate characteristic of the battery.
[0159] JPEG0007577249000001.jpg196150
[0160] In Table 1, the heated solution temperature means that when one of the first solution and the second solution is added to the other and mixed, the other solution is heated, and the temperature of this solution is the heated solution temperature.
[0161] JPEG0007577249000002.jpg212156
[0162] In Table 2, the main particle type is the particle type of more than 50% of the particles in the viewing area of 10k magnification of an electron microscope (ZEISS Gemini SEM 300). The radius of curvature of the rectangular particle of the comparative example is tested from the angle between two adjacent faces.
[0163] JPEG0007577249000003.jpg108154
[0164] As can be seen from the comparison of Examples 1-5 and Comparative Examples 1-2, the mixing flow rate affects the interior angle of the secondary particles, the radius of curvature of the primary particles, and the particle size of the material. Except for the method of directly mixing the solution during sample injection, the interior angle of the secondary particles, the radius of curvature of the primary particles, and the particle size of the material all show a phenomenon of increasing with an increase in the mixing flow rate. In the method of directly mixing the solution, the particle state during mixing is not consistent, so the radius of curvature of the primary particles and the particle size of the material are too small. When a relatively large mixing flow rate is used, the content of Na in the chemical formula of the Prussian blue transition metal cyanide is greatly increased, which improves the capacity and particle size per gram of the Prussian blue transition metal cyanide, and improves the compaction density of the electrode plate, thereby improving the energy density of the battery.
[0165] As can be seen from the comparison of Examples 1, 6-8 and Comparative Examples 3-4, the mixing time affects the chemical composition of the product, the interior angle of the secondary particles, the radius of curvature of the primary particles, and the particle size of the material. As can be seen from Comparative Example 3, if the mixing time is too short, the primary particles will aggregate in large quantities, resulting in secondary particles with large particle sizes. And if the mixing time is too short, the radius of curvature of the primary particles will be too small, resulting in quadrangular particles. In the mixing time range of 0.5h to 48h, the particles will first aggregate and then gradually decompose, so the particle size will increase and then decrease, and in the mixing time range of 0.5h to 48h, the radius of curvature will also increase and then decrease. As can be seen from the chemical formula and capacity per gram of Comparative Example 4, if the reaction time is too long, the transition metal elements will oxidize, the particles will decompose violently, and the radius of curvature of the primary particles and the particle size of the material will decrease. Therefore, an appropriate mixing time can effectively control the particle size and shape of the particles, thereby significantly improving the energy density of the battery.
[0166] As can be seen from the comparison between Examples 1, 9-10 and Comparative Example 5, the concentration of transition metal cations and transition metal cyanate anions has a large effect on the interior angle of secondary particles and the radius of curvature of primary particles. When the concentration of transition metal cations or transition metal cyanate anions is too low, the interior angle of secondary particles and the radius of curvature of primary particles become relatively small, resulting in quadrangular primary particles. When the concentrations of transition metal cations and transition metal cyanate anions are both 0.1 mol / L or more, but the concentration difference between the transition metal cations and transition metal cyanate anions increases, the interior angle of secondary particles increases and the material particle size decreases. Therefore, appropriate transition metal cation and transition metal cyanate anion concentrations can improve the energy density of the battery.
[0167] As can be seen from the comparison of Examples 1 and 11 with Comparative Example 6, the temperature of the heated solution affects the radius of curvature and the particle size of the material of the primary particles. When the temperature of the solution is too low, the degree of supersaturation of the Prussian blue-based transition metal cyanide is greatly improved, so that the crystals are rapidly nucleated to form small particles. When the temperature of the solution is too low, it causes the formation of square particles. When the temperature of the solution is relatively high, the secondary particles of the crystals are easily decomposed, so that relatively small secondary particles are obtained. However, a relatively high solution temperature is also favorable for increasing the radius of curvature of the primary particles, and the sphericity is relatively high. The increase in the solution temperature can further increase the content of Na in the Prussian blue-based transition metal cyanide, thereby improving the capacity and particle size per gram of the Prussian blue-based transition metal cyanide, and improving the compaction density, so as to improve the energy density of the battery.
[0168] As can be seen from the comparison with Examples 1 and 12, the order of addition affects the radius of curvature of the primary particles and the particle size of the material. By adopting the method of adding the first solution to the second solution, relatively large secondary particles are obtained, but the ratio of the radius of curvature of the primary particles to the total particle size is reduced, and the capacity per gram of the obtained Prussian blue-based transition metal cyanide is higher, which is favorable for the battery to have a relatively high energy density.
[0169] As can be seen from the comparison of Examples 1, 18-21 and Comparative Example 8, the aging time affects the structural integrity of the Prussian blue-based transition metal cyanide. The appropriate aging time can improve the structural integrity of the Prussian blue-based transition metal cyanide, thereby increasing the Na content and forming Fe(CN)6 4- The defects in the Prussian blue transition metal cyanide are reduced, and the active Na ions are increased, which can reduce the powder resistivity of the Prussian blue transition metal cyanide, thereby improving the rate characteristics and cycle performance of the battery.
[0170] It should be noted that, based on the disclosure and guidance of the above specification, a person skilled in the art of the present application may also appropriately change and modify the above embodiment. Therefore, the present application is not limited to the specific embodiments disclosed and described above, and some modifications and changes of the present application will also fall within the scope of protection of the claims of the present application. Although some specific terms are used in this specification, these terms are merely for ease of description and do not limit the present application.
Claims
1. A method for producing a Prussian blue-based transition metal cyanide, comprising the steps of: Step S1 of providing a first solution containing transition metal cations, the concentration of the transition metal cations in the first solution being ≧0.1 mol / L, the transition metal cations being selected from one or more of Mn, Ni, Cu, Co, Fe, Zn, and Cr; S2, providing a second solution containing an A salt of a transition metal cyanate, wherein the concentration of the transition metal cyanate anion in the second solution is ≧0.1 mol / L, A is Na, and the transition metal cyanate is selected from one or more of ferrocyanate, manganese cyanate, cobalt cyanate, nickel cyanate, and copper cyanate; Step S3: adding and mixing one of the first solution and the second solution to the other under stirring conditions at a flow rate of 10 cm / s to 100 m / s within a time period of 0.5 h to 48 h to cause a co-precipitation chemical reaction to obtain a suspension, the temperature of one solution being 10° C. to 40° C. and the temperature of the other solution being 40° C. to 180° C.; Step S4 of aging the suspension under stirring and at 40° C. to 180° C. for ≧0.5 h; and step S5 of obtaining the Prussian blue-based transition metal cyanide through separation, washing and drying, the Prussian blue-based transition metal cyanide comprising secondary particles, the secondary particles comprising a plurality of primary particles, the primary particles being spherical or near-spherical, and the interior angles of the secondary particles being 150° to 300°.
2. 2. The method according to claim 1, wherein in step S1, the concentration of the transition metal cation in the first solution is 0.2 mol / L to 4 mol / L.
3. 2. The method according to claim 1, wherein in step S2, the concentration of the transition metal cyanate anion in the second solution is 0.2 mol / L to 4 mol / L.
4. The first solution in step S1 or the second solution in step S2 further includes an A source; 2. The method of claim 1, wherein the A source is selected from one or more of a chloride salt of A, a nitrate salt of A, a sulfate salt of A, a hydroxide salt of A, a formate salt of A, an acetate salt of A, an oxalate salt of A, a phosphate salt of A, a perchlorate salt of A, a benzoate salt of A, and a citrate salt of A.
5. The method according to claim 1 , wherein the first solution in step S1 or the second solution in step S2 contains an antioxidant.
6. The method according to claim 1, wherein in step S3, the flow rate of the mixing is 50 cm / s to 10 m / s.
7. The method according to claim 1, wherein in step S3, the mixing time is 1 hour to 24 hours.
8. The method according to claim 1, wherein in step S3, the temperature of the other solution is 60°C to 140°C.
9. In step S4, the aging temperature is 60° C. to 140° C.; and / or The manufacturing method according to claim 1 , wherein in step S4, the aging time is 1 hour to 24 hours.
Citation Information
Patent Citations
Preparation method and use of graphite / Prussian blue composite material
CN106469828A
Prussian blue positive pole material and preparation method thereof, and electrochemical energy storage device
CN109698345A
Positive plate and electrochemical battery
CN109841832A
Prussian blue material and preparation method thereof
CN110078096A
Method for quickly preparing Prussian blue analog with monoclinic structure
CN110451525A