Secondary battery manufacturing method and secondary battery manufacturing apparatus

By adjusting drying conditions based on the measured specific surface area of the electrode active material, the method stabilizes electrode plate surface area, addressing non-uniformity and ensuring consistent battery performance.

JP7577708B2Active Publication Date: 2024-11-05TOYOTA BATTERY CO LTD +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022080750
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-17
Publication Date
2024-11-05
Estimated Expiration
2042-05-17

AI Technical Summary

Technical Problem

Variations in the specific surface area of electrode active materials within the electrode composite material lead to non-uniform battery performance, which is not adequately addressed by existing manufacturing methods.

Method used

Adjust the drying conditions, such as temperature and time, based on the measured specific surface area of the electrode active material before drying to ensure uniformity of the electrode plate surface area, thereby stabilizing battery performance.

Benefits of technology

The method effectively suppresses variations in the specific surface area of electrode plates, ensuring consistent battery performance by precisely adjusting the drying conditions according to the initial surface area of the electrode active material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577708000001
    Figure 0007577708000001
  • Figure 0007577708000002
    Figure 0007577708000002
  • Figure 0007577708000003
    Figure 0007577708000003
Patent Text Reader

Abstract

To ensure the uniformity of battery performance by minimizing variations of an electrode plate specific surface area.SOLUTION: In manufacturing of an electrode sheet that forms a secondary battery electrode plate, a step of applying an electrode mixture that includes an electrode active material onto a substrate that becomes a current collector, and a step of drying the electrode mixture applied onto the substrate are performed. In a manufacturing process before the step of drying the electrode mixture applied onto the substrate, a specific surface area S of the electrode active material included in the electrode mixture is obtained. Furthermore, the obtained specific surface area S of the electrode active material is referred to as an obtained specific surface area Sd, and a specific surface area S of the electrode active material in a state where the electrode mixture applied onto the substrate forms an electrode plate is referred to as an electrode plate specific surface area Se. An electrode plate specific surface area Se2 after the drying of the applied electrode mixture is adjusted by setting a drying condition of the electrode mixture in accordance with the obtained specific surface area Sd.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for manufacturing a secondary battery. [Background technology]

[0002] Conventionally, for example, in secondary batteries such as lithium ion secondary batteries, the electrode plate is formed by applying an electrode mixture containing an electrode active material onto a substrate serving as a current collector. Furthermore, in such secondary batteries, the specific surface area of ​​the electrode active material contained in the electrode mixture has a large effect on the battery performance. In light of this, for example, Patent Document 1 describes a preferred range of the specific surface area for the electrode active material constituting the negative electrode. And, for example, Patent Document 2 describes the relationship between the firing temperature of the precursor and the specific surface area of ​​the electrode active material. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-19094 A [Patent Document 2] Japanese Patent Application Publication No. 9-175825 Summary of the Invention [Problem to be solved by the invention]

[0004] In addition, the electrode active material, which is the raw material of the electrode mixture, is usually allowed to have a variation in its specific surface area within a predetermined tolerance range. However, when considering the uniformity of battery performance, the specific surface area of ​​the electrode active material in a state in which the electrode mixture coated on the substrate forms an electrode plate is defined as the electrode plate specific surface area, and it is preferable that the variation in this electrode plate specific surface area is smaller. [Means for solving the problem]

[0005] A method for manufacturing a secondary battery that solves the above problem includes a step of applying an electrode mixture containing an electrode active material onto a substrate that serves as a current collector, and a step of drying the applied electrode mixture, in which a specific surface area of ​​the electrode active material is obtained during a manufacturing process prior to the step of drying the electrode mixture, and the obtained specific surface area of ​​the electrode active material is defined as an obtained specific surface area, and the specific surface area of ​​the electrode active material in a state in which the electrode mixture applied to the substrate forms an electrode plate is defined as an electrode plate specific surface area, and the drying conditions for the electrode mixture are set according to the obtained specific surface area to adjust the electrode plate specific surface area after drying.

[0006] That is, when the electrode mixture coated on the substrate is dried, the specific surface area of ​​the electrode plate after drying becomes larger than the specific surface area of ​​the electrode plate before drying. Furthermore, the amount of change in the specific surface area of ​​the electrode plate caused by this drying depends on the drying conditions of the electrode mixture coated on the substrate. This makes it possible to adjust the specific surface area of ​​the electrode plate after drying based on the setting of the drying conditions. Therefore, with the above configuration, it is possible to easily reduce the variation in the specific surface area of ​​the electrode plate with a simple configuration. This makes it possible to ensure uniformity in battery performance.

[0007] In the method for producing a secondary battery that solves the above problems, it is preferable that the drying temperature of the electrode mixture is set as the drying condition, and that the smaller the obtained specific surface area is, the higher the drying temperature is set.

[0008] That is, the amount of change in the specific surface area of ​​the electrode plate caused by drying increases as the drying temperature of the electrode mixture applied to the substrate increases. Therefore, according to the above configuration, the drying temperature of the electrode mixture can be set as a drying condition according to the specific surface area of ​​the electrode active material, and the specific surface area of ​​the electrode plate after drying can be easily adjusted. This makes it possible to suppress the variation in the specific surface area of ​​the electrode plate and ensure uniformity in battery performance.

[0009] In the method for producing a secondary battery that solves the above problems, it is preferable that the drying condition is a drying time for the electrode mixture, and that the smaller the obtained specific surface area is, the longer the drying time is set.

[0010] That is, the amount of change in the specific surface area of ​​the electrode plate caused by drying increases as the drying time of the electrode mixture applied to the substrate increases. Therefore, according to the above configuration, the drying time of the electrode mixture can be set as a drying condition corresponding to the specific surface area of ​​the electrode active material, and the specific surface area of ​​the electrode plate after drying can be easily adjusted. This makes it possible to suppress the variation in the specific surface area of ​​the electrode plate and ensure uniformity in battery performance.

[0011] In a method for manufacturing a secondary battery that solves the above problem, it is preferable to set the drying conditions so as to correct the difference between the acquired specific surface area and a predetermined standard specific surface area based on the amount of change in the plate specific surface area that changes depending on the drying conditions.

[0012] According to the above-mentioned configuration, the specific surface area of ​​the electrode plate after drying can be adjusted with high precision, and as a result, the variation in the specific surface area of ​​the electrode plate can be effectively suppressed to ensure uniformity in battery performance.

[0013] A method for manufacturing a secondary battery that solves the above problem includes a step of mixing raw materials for the electrode mixture, and a step of kneading the mixed electrode mixture, and the mixed electrode mixture is applied onto the substrate, and it is preferable that the specific surface area obtained for the electrode active material before the mixing is regarded as the obtained specific surface area.

[0014] That is, for the electrode active material as a raw material before mixing, the variation in its initial specific surface area is usually allowed within a predetermined tolerance range. As a result, the electrode active material as a raw material has a variation in its initial specific surface area for each production unit, that is, for each lot. Therefore, according to the above configuration, the electrode plate specific surface area after drying can be adjusted efficiently and highly accurately by setting the drying conditions according to the obtained specific surface area of ​​the electrode active material. As a result, the variation in the electrode plate specific surface area can be effectively suppressed to ensure uniformity in electrical performance.

[0015] Furthermore, the initial specific surface area of ​​the electrode active material is often indicated as a measured value in the form of, for example, a specification or a label. Therefore, according to the above configuration, the specific surface area of ​​the electrode active material contained in the electrode mixture can be easily obtained in the manufacturing process prior to the step of drying the electrode mixture applied to the substrate without performing any special measurement work. This allows efficient setting of drying conditions according to the obtained specific surface area of ​​the electrode active material.

[0016] The manufacturing apparatus for a secondary battery that solves the above-mentioned problem is a manufacturing apparatus for a secondary battery that coats an electrode mixture containing an electrode active material on a substrate that serves as a current collector and dries the coated electrode mixture, and is equipped with an acquired specific surface area input unit that accepts input of the acquired specific surface area, where the specific surface area of ​​the electrode active material acquired in the manufacturing process before drying the electrode mixture is defined as an acquired specific surface area, and the specific surface area of ​​the electrode active material in a state in which the electrode mixture coated on the substrate forms an electrode plate is defined as an electrode plate specific surface area, and a drying condition calculation unit that calculates drying conditions for the electrode mixture according to the input acquired specific surface area in order to adjust the electrode plate specific surface area after drying.

[0017] According to the above-mentioned configuration, with a simple structure, it is possible to easily suppress the variation in the specific surface area of ​​the electrode plates and ensure uniformity in the battery performance. Effect of the Invention

[0018] According to the present invention, the variation in the specific surface area of ​​the electrode plates can be suppressed, and uniformity in the battery performance can be ensured. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is a perspective view of a secondary battery. [Diagram 2] FIG. [Diagram 3] FIG. 2 is a side view of the secondary battery. [Figure 4] 4 is a flowchart showing a manufacturing process of an electrode sheet that forms an electrode plate of a secondary battery. [Diagram 5] 1 is a graph showing the relationship between the manufacturing process of an electrode sheet and the specific surface area of ​​an electrode active material. [Figure 6] FIG. 2 is a diagram showing a state of an electrode mixture applied onto a substrate before drying. [Figure 7] FIG. 1 is a diagram showing a state after an electrode mixture applied to a substrate is dried. [Figure 8] 1 is a graph showing the relationship between the specific surface area of ​​the pressed electrode plate and the battery performance. [Figure 9] 10 is a flowchart showing a procedure for setting drying conditions according to an acquired specific surface area of ​​an electrode active material. [Figure 10] 4 is a graph showing the relationship between the amount of change in specific surface area of ​​a plate caused by drying and the drying temperature. [Figure 11] FIG. 11 is an explanatory diagram of a method for adjusting the specific surface area of ​​a dried electrode plate by setting drying conditions according to the obtained specific surface area. [Figure 12] 1 is a table showing the relationship between the difference between the acquired specific surface area and the standard specific surface area, the target change in the specific surface area of ​​the plate during drying, and the drying temperature set as a drying condition. [Figure 13] FIG. 2 is a schematic diagram of a drying condition setting device. [Figure 14] 5 is a flowchart showing a processing procedure for setting a drying temperature by the drying condition setting device. [Figure 15] FIG. 11 is an explanatory diagram showing another example of setting the drying temperature according to the obtained specific surface area. [Figure 16] FIG. 11 is a schematic diagram of a drying condition setting device according to another embodiment of the present invention. [Figure 17] FIG. 4 is an explanatory diagram showing the relationship between the amount of change in the specific surface area of ​​a plate caused by drying and the drying time. [Figure 18] FIG. 13 is an explanatory diagram of setting a drying time according to an acquired specific surface area. [Figure 19] FIG. 11 is a schematic configuration diagram of a drying condition setting device according to another example. [Figure 20] FIG. 11 is an explanatory diagram showing another example of setting drying conditions according to an acquired specific surface area. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, an embodiment relating to the manufacturing direction of a secondary battery will be described with reference to the drawings. 1, the secondary battery 1 includes an electrode assembly 10 in which a positive electrode 3, a negative electrode 4, and a separator 5 are integrated, and a case 20 that houses the electrode assembly 10. The secondary battery 1 of this embodiment has a configuration as a lithium ion secondary battery in which the electrode assembly 10 in the case 20 is impregnated with a non-aqueous electrolyte solution (not shown).

[0021] More specifically, in the secondary battery 1 of this embodiment, the positive electrode 3, the negative electrode 4, and the separator 5 are laminated with a sheet-like outer shape. Then, by winding up the laminate of the positive electrode 3, the negative electrode 4, and the separator 5, an electrode body 10 is formed in which the positive and negative electrodes and the separators 5 are alternately arranged in the radial direction with the separator 5 sandwiched between the positive electrode 3 and the negative electrode 4.

[0022] The case 20 of this embodiment includes a case body 21 having a flat, substantially rectangular box shape, and a lid member 22 that closes an open end 21x of the case body 21. The electrode body 10 of this embodiment has a flat outer shape that corresponds to the box shape of the case 20.

[0023] More specifically, as shown in FIG. 2, in the secondary battery 1 of this embodiment, the positive electrode 3 and the negative electrode 4 each have a configuration as an electrode sheet 35 including a current collector 31 having a sheet-like outer shape and an electrode active material layer 32 laminated on this current collector 31.

[0024] Specifically, for the electrode sheet 35P for the positive electrode 3, a composite paste 37P containing a lithium transition metal oxide serving as a positive electrode active material is applied onto a substrate 36P made of aluminum or the like that constitutes the positive electrode current collector 31P. For the electrode sheet 35N for the negative electrode 4, a composite paste 37N containing a carbon-based material serving as a negative electrode active material is applied onto a substrate 36N made of copper or the like that constitutes the negative electrode current collector 31N. Furthermore, each of these composite pastes 37P and 37N contains a binder. In the secondary battery 1 of this embodiment, the composite pastes 37P and 37N are dried to form the corresponding positive electrode active material layer 32P and negative electrode active material layer 32N on the positive and negative electrode sheets 35P and 35N, respectively.

[0025] Furthermore, in the secondary battery 1 of this embodiment, the positive and negative electrode sheets 35P, 35N are each shaped into a belt-like shape. The electrode body 10 of this embodiment is configured such that the positive and negative electrode sheets 35P, 35N, which are stacked with the separator 5 sandwiched therebetween, are wound around a winding axis L that extends in the width direction of the belt-like shape (the left-right direction in FIG. 2).

[0026] 2, the separator 5 and each electrode sheet 35 are wound in such a manner that the electrode sheet 35P constituting the positive electrode 3 is wound inward. However, this figure is one example showing the structure of the electrode body 10, and the separator 5 and each electrode sheet 35 may be wound in such a manner that the electrode sheet 35N constituting the negative electrode 4 is wound inward. This determines whether the electrode sheet 35 arranged on the outermost shell of the electrode body 10 is the electrode sheet 35P constituting the positive electrode 3 or the electrode sheet 35N constituting the negative electrode 4.

[0027] 1 to 3, the cover member 22 of the case 20 is provided with a positive electrode terminal 38P and a negative electrode terminal 38N that protrude to the outside of the case 20. Furthermore, each electrode sheet 35 has an uncoated portion 39 in which the electrode active material layer 32 is not formed on the current collector 31. The secondary battery 1 of this embodiment is configured such that the electrode sheet 35P constituting the positive electrode 3 and the positive electrode terminal 38P are electrically connected, and the electrode sheet 35N constituting the negative electrode 4 and the negative electrode terminal 38N are electrically connected, utilizing the uncoated portion 39.

[0028] Specifically, the electrode body 10 of this embodiment is housed in the case 20 with its winding axis L aligned along the longitudinal direction (left-right direction in FIG. 1) of the cover member 22, which is an elongated, generally rectangular plate. Furthermore, in this state, an uncoated portion 39P of an electrode sheet 35P constituting the positive electrode 3 is connected to a positive electrode terminal 38P via a connecting member 40P. Similarly, an uncoated portion 39N of an electrode sheet 35N constituting the negative electrode 4 is connected to a negative electrode terminal 38N via a connecting member 40N.

[0029] Furthermore, an electrolyte solution 41 is poured into the case 20. In the secondary battery 1 of this embodiment, a fluorine-based electrolyte solution 41 in which a lithium salt serving as a supporting salt is dissolved in an organic solvent is used. Thus, the secondary battery 1 of this embodiment is configured such that the electrolyte solution 41 is impregnated into the electrode body 10 sealed in the case 20.

[0030] (Electrode sheet manufacturing process) 4, in the process of manufacturing the electrode sheet 35 that forms the secondary battery 1 of this embodiment, first, the electrode active material, binder, thickener, and the like that are the raw materials of the electrode mixture 50 are mixed (step 101). Then, the mixed electrode mixture 50 is kneaded (step 102).

[0031] Next, the electrode mixture 50 kneaded in the step 102 is applied to the corresponding substrates 36P and 36N in the state of the above-mentioned mixture pastes 37P and 37N (step 103, see FIG. 2). Next, the electrode mixture 50 applied in the step 103 is dried (step 104). In this embodiment, the application process in the step 102 and the drying process in the step 103 are continuously performed. Furthermore, in a state in which the electrode mixture 50 applied on the substrate 36 forms the corresponding positive and negative electrodes, that is, the electrode plates 51, these are pressed to increase the adhesive strength of the electrode mixture 50 to the substrate 36 (step 105). Then, in the secondary battery 1 of this embodiment, the electrode sheet 35 shaped into a foil extending in a strip shape as described above is manufactured through a cutting process (step 106) performed after the pressing process.

[0032] (Electrode sheet manufacturing process and specific surface area of ​​electrode active material) As shown in FIG. 5, the specific surface area of ​​the electrode active material used in the secondary battery 1 changes during the manufacturing process of the electrode sheet 35.

[0033] In more detail, if the specific surface area S of the electrode active material before mixing the raw materials (see FIG. 4, step 101) is defined as an initial specific surface area S0, the specific surface area S of the electrode active material becomes smaller than the initial specific surface area S0 by performing the kneading step (step 102). In addition, the general term "specific surface area of ​​the electrode active material" often refers to this initial specific surface area S0. In addition, if the specific surface area S of the electrode active material in a state in which the electrode mixture 50 applied to the substrate 36 forms the electrode plate 51 is defined as the electrode plate specific surface area Se, the value immediately after application to the substrate 36 (step 103), that is, the electrode plate specific surface area Se1 before drying, is equal to the value after kneading. Furthermore, the value of the specific surface area S of the electrode active material after performing the drying step (step 104), that is, the electrode plate specific surface area Se2 after drying, becomes larger than the electrode plate specific surface area Se1 before drying. If the specific surface area S of the electrode active material after the pressing step (step 105) is taken as the specific surface area Se3 of the pressed electrode plate, this specific surface area Se3 of the pressed electrode plate will be greater than the specific surface area Se2 of the dried electrode plate.

[0034] The specific surface area of ​​a porous powder such as an electrode active material is measured, for example, by a gas adsorption measurement method using the BET method, that is, the BET method. The unit is "square meters / gram." The specific surface area measured by the BET method is called the "BET specific surface area." In this embodiment, the specific surface area S of the electrode active material is measured by the BET method using nitrogen as the adsorption gas.

[0035] 6, by carrying out the kneading step, a binder 56 adheres to the electrode active material 55 in the electrode mixture 50. This reduces the specific surface area S of the electrode mixture 50, so that even when the electrode mixture 50 forms an electrode plate 51 together with the substrate 36, the electrode plate specific surface area Se1 before drying becomes smaller than the value before kneading, i.e., the initial specific surface area S0 (see FIG. 5, S0>Se1).

[0036] As shown in FIG. 7, when the electrode mixture 50 applied on the substrate 36 dries, the binder 56 contained in the electrode mixture 50 moves, that is, so-called migration occurs, with the evaporation of the solvent (not shown). That is, the solvent in the electrode mixture 50 evaporates from the surface 50s (upper side in FIG. 7) of the electrode mixture 50 applied on the substrate 36. Furthermore, at this time, together with the solvent moving in the electrode mixture 50, the binder 56 also contained in the electrode mixture 50 is detached from the attached electrode active material 55 and moves from a position close to the substrate 36 to a position close to the surface 50s of the electrode mixture 50 (upper side in FIG. 7). Then, due to the detachment of the binder 56 caused by the occurrence of this migration, the specific surface area S of the electrode mixture 50 contained in the electrode mixture 50 increases, and the electrode plate specific surface area Se2 after drying becomes larger than the electrode plate specific surface area Se1 before drying (see FIG. 5, Se1 <Se2)。

[0037] Incidentally, the binder 56 that has migrated to the surface 50s side due to migration usually aggregates in gaps between the electrode active materials 55. Then, the segregation state of the binder 56 caused by such migration is sometimes expressed as a "migration index" and as a "ratio (surface side / substrate side)" when the electrode mixture 50 applied on the substrate 36 is divided into the surface 50s side and the substrate 36 side.

[0038] Furthermore, the electrode active material 55 in the electrode mixture 50 is crushed by the pressing process, and the specific surface area S of the electrode active material 55 is increased. As a result, the specific surface area Se3 of the electrode plate after pressing becomes larger than the specific surface area Se2 of the electrode plate after drying (see FIG. 5, Se2 <Se3)。

[0039] 5, in the secondary battery 1 of this embodiment, a standardized specific surface area Sc is set in advance during the manufacture of the electrode sheet 35 as a value for standardizing the specific surface area S of the electrode active material 55. Specifically, in the secondary battery 1 of this embodiment, this standardized specific surface area Sc is a prescribed value set for the initial specific surface area S0, which is the specific surface area S of the electrode active material 55 before the raw materials are mixed. In the secondary battery 1 of this embodiment, the standardized specific surface area Sc is set as the standard center value, and variation in the initial specific surface area S0 is allowed within a predetermined tolerance α (S0=Sc±α).

[0040] 5 is a graph showing the specific surface area S of the electrode active material 55 that changes during the manufacturing process of the electrode sheet 35 when the initial specific surface area S0 is equal to the standard specific surface area Sc. Waveform 62 in the same figure is a graph showing the specific surface area S of the electrode active material 55 that changes during the manufacturing process of the electrode sheet 35 when the initial specific surface area S0 corresponds to the lower limit of the allowable range (S0=Sc-α). Waveform 63 in the same figure is a graph showing the specific surface area S of the electrode active material 55 that changes during the manufacturing process of the electrode sheet 35 when the initial specific surface area S0 corresponds to the upper limit of the allowable range (S0=Sc+α).

[0041] 8, in the secondary battery 1 of this embodiment, the specific surface area Se3 of the electrode plate after pressing becomes the specific surface area S of the electrode active material 55 in a state in which the electrode mixture 50 applied on the substrate 36 forms a substantially completed electrode plate 51. The specific surface area Se3 of the electrode plate after pressing determines the battery performance.

[0042] That is, in the graph of Fig. 8, the "battery resistance" shown on the vertical axis is one of the indicators representing the battery performance. This "battery resistance" is a value measured in the battery state by the so-called "AC impedance method."

[0043] 5, when there is a discrepancy between the initial specific surface area S0, which is the specific surface area S of the electrode active material 55 before the raw materials are mixed, and the predetermined standard specific surface area Sc, the difference δ is likely to be maintained even after the above-mentioned manufacturing processes are performed under the same manufacturing conditions. For this reason, it is common to set a tolerance α for the initial specific surface area S0 of the electrode active material 55, which is the raw material of the secondary battery 1.

[0044] However, when considering the uniformity of the battery performance, it is preferable that the variation in the specific surface area S of the electrode active material 55 contained in the electrode mixture 50 is smaller. In consideration of this point, in the secondary battery 1 of this embodiment, in the manufacturing process of the electrode sheet 35, manufacturing conditions are set based on the specific surface area S of the electrode active material 55. Specifically, in this embodiment, the drying temperature T is set as the drying condition of the electrode mixture 50, and the smaller the acquired specific surface area Sd, the higher the drying temperature T is set. This makes it possible to ensure the uniformity of the battery performance by adjusting the specific surface area S of the electrode active material 55 in a state in which the electrode mixture 50 applied on the substrate 36 forms the electrode plate 51.

[0045] In the secondary battery 1 of this embodiment having a configuration as a lithium ion secondary battery, the battery performance is easily affected by variations in the specific surface area S of the electrode active material 55 on the negative electrode 4 side that receives lithium ions moving from the positive electrode 3 side during charging. For this reason, in this embodiment, in the manufacturing process of the electrode sheet 35N constituting the negative electrode 4, manufacturing conditions are set based on the specific surface area S of the electrode active material 55.

[0046] (Setting drying conditions according to the specific surface area obtained) Next, the setting of drying conditions according to the obtained specific surface area of ​​the electrode active material 55 executed when manufacturing the secondary battery 1 of this embodiment will be described.

[0047] As shown in FIG. 9, when manufacturing the secondary battery 1 of the present embodiment, the specific surface area S of the electrode active material 55 is obtained (step 201) in the manufacturing process before the step of drying the electrode mixture 50 applied on the base material 36 (see FIG. 4, step 104). Specifically, in the present embodiment, the acquisition of the specific surface area S is performed on the initial specific surface area S0 of the electrode active material 55 in the step of preparing the raw materials of the electrode mixture 50 (see FIG. 4, step 101). Further, in the present embodiment, the specific surface area S of the electrode active material 55 obtained in step 201, that is, the initial specific surface area S0, is set as the acquired specific surface area Sd of the electrode active material 55 (see FIG. 5). Then, according to this acquired specific surface area Sd, the drying temperature T is set as the drying condition of the electrode mixture 50 applied on the base material 36 (step 202).

[0048] That is, as shown in FIGS. 5 to 7, by drying the electrode mixture 50 applied on the base material 36, the specific surface area Se2 of the electrode plate after drying becomes larger than the specific surface area Se1 of the electrode plate before drying (Se1 < Se2). Further, as described above, the change in the specific surface area Se of the electrode plate before and after drying is caused by the migration that occurs during the drying, so the degree of its progress depends on the drying conditions of the electrode mixture 50 applied on the base material 36. And thereby, the change amount ΔS of the specific surface area Se of the electrode plate caused by the drying also depends on the drying conditions of this electrode mixture 50.

[0049] For example, as shown in FIG. 10, when a plurality of different drying temperatures T are set while keeping other drying conditions such as the drying time the same, the change amount ΔS of the specific surface area Se of the electrode plate before and after drying is substantially proportional to the drying temperature T. In the example shown in FIG. 10, drying tests of the electrode mixture 50 applied on the base material 36 are performed multiple times when the drying temperature T is set to "175°C" and when it is set to "180°C", respectively. From the test results, when the change amount ΔS of the specific surface area Se of the electrode plate caused by drying is "y" and the drying temperature T is "x", it can be confirmed that there is a correlation expressed by a linear approximation formula "y = ax - b, (where "a" and "b" are coefficients)" between them.

[0050] In consideration of this, in the secondary battery 1 of this embodiment, the drying temperature T is set according to the acquired specific surface area Sd, thereby adjusting the post-drying specific surface area Se2 of the electrode plate. This reduces the variation in the specific surface area S of the electrode active material 55 contained in the electrode mixture 50 applied to the substrate 36.

[0051] In more detail, for example, as shown in Fig. 11, when the initial specific surface area S0 as the acquired specific surface area Sd coincides with the standard specific surface area Sc, the specific surface area Se1 of the electrode plate before drying is designated as "Se1C" and the specific surface area Se2 of the electrode plate after drying is designated as "Se2C" (see Fig. 5). When the acquired specific surface area Sd is smaller than the standard specific surface area Sc, the specific surface area Se1 of the electrode plate before drying is designated as "Se1L" and the specific surface area Se2 of the electrode plate after drying is designated as "Se2L".

[0052] Even in such a case, if the manufacturing conditions, including the drying conditions, are the same, the change amount ΔS in the electrode plate specific surface area Se caused by the drying will be substantially the same in all of these cases (see FIG. 5). When the acquired specific surface area Sd is smaller than the standard specific surface area Sc, the difference ΔL between the electrode plate specific surface area Se1L before drying and Se1C corresponding to its standard center value is substantially equal to the difference δ between the acquired specific surface area Sd and the standard specific surface area Sc.

[0053] Furthermore, from these relationships, it is possible to calculate a target change during drying ΔST for correcting the difference δ between the acquired specific surface area Sd and the standard specific surface area Sc for the change ΔS in the electrode plate specific surface area Se caused by drying of the electrode mixture 50 applied on the substrate 36. This makes it possible to set a drying temperature T for reducing variation in the electrode plate specific surface area Se2 after drying caused by the difference in the initial specific surface area S0, which is the acquired specific surface area Sd.

[0054] That is, under predetermined drying conditions, the change amount ΔS in the plate specific surface area Se caused by the drying is set as the reference change amount ΔSC. Furthermore, for example, the difference δ between the acquired specific surface area Sd and the standard specific surface area Sc is set as "δ=Sd-Sc", and the difference δ between the acquired specific surface area Sd and the standard specific surface area Sc is subtracted from the reference change amount ΔSC to set the target change amount ΔST during drying (ΔST=ΔSC-δ). Then, based on the target change amount ΔST during drying, the drying temperature T for correcting the difference δ between the acquired specific surface area Sd and the standard specific surface area Sc can be set.

[0055] Specifically, for example, in the example shown in FIG. 10, the approximation formula showing the relationship between the change amount ΔS of the electrode plate specific surface area Se caused by drying the electrode mixture 50 applied on the substrate 36 and the drying temperature T is "y=0.0429x-7.4072". Furthermore, when the acquired specific surface area Sd coincides with the standard specific surface area Sc, that is, when the initial specific surface area S0 is at the standard center value, the standard drying temperature T is "175°C". In this example, the value of the standard specific surface area Sc is "4.2". Then, by substituting this "175°C" into the above approximation formula, approximately "0.1" is derived as the reference change amount ΔSC of the electrode plate specific surface area Se caused by the drying.

[0056] In this example, a tolerance α of the initial specific surface area S0 that results in the acquired specific surface area Sd is allowed to have a variation of ±0.4. For this reason, for example, when the variation of the initial specific surface area S0 corresponds to the lower limit of the allowable range (δ=-0.4), the target change amount ΔST during drying is ΔST=0.5 (see FIG. 5). In this case, the value of the acquired specific surface area Sd is 3.8. Furthermore, the value of the target change amount ΔST during drying, 0.5, is substituted into the above approximation formula. This allows the drying temperature T to be derived as approximately 184° C. to correct the difference δ=-0.4 between the acquired specific surface area Sd and the standard specific surface area Sc.

[0057] In this manner, in this embodiment, the drying temperature T as the drying condition is set in order to correct the difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc based on the amount of change ΔS in the plate specific surface area Se, which changes depending on the drying conditions.

[0058] (Drying condition setting device) Next, a drying condition setting device used in manufacturing the secondary battery 1 will be described. 13, when manufacturing the secondary battery 1 of this embodiment, a drying condition setting device 71 constituting a manufacturing device 70 thereof includes an acquired specific surface area input unit 73 that receives an input of an acquired specific surface area Sd of the electrode active material 55 included in the electrode mixture 50. The drying condition setting device 71 of this embodiment also includes a drying temperature calculation unit 76 as a drying condition calculation unit 75 that calculates a drying temperature T of the electrode mixture 50 according to the acquired specific surface area Sd of the electrode active material 55 that has been input in order to adjust the plate specific surface area Se2 after drying.

[0059] More specifically, the initial specific surface area S0 of the electrode active material 55 acquired in the preparation step (see FIG. 4, step 201) is input to the drying condition setting device 71 of this embodiment as the acquired specific surface area Sd. Furthermore, the drying condition setting device 71 of this embodiment stores the relationship between the difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc, the target change amount during drying ΔST, and the drying temperature T set as the drying condition in the form of a data table 77 in a storage area 78 (see FIG. 12). The drying temperature calculation unit 76 of this embodiment is configured to calculate the drying temperature T of the electrode mixture 50 according to the acquired specific surface area Sd input by referring to this data table 77.

[0060] Specifically, as shown in Fig. 14, when the acquired specific surface area Sd is inputted (step 301), the drying condition setting device 71 of this embodiment reads out the standardized specific surface area Sc stored in the memory area 78 (step 302). Next, the drying condition setting device 71 calculates the difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc (step 303, δ = Sd - Sc). Furthermore, the drying condition setting device 71 reads out the reference change amount ΔSC stored in the memory area 78 (step 304). Then, the drying condition setting device 71 of this embodiment calculates the target change amount ΔST during drying based on this reference change amount ΔSC and the difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc calculated in the above step 303 (step 305, ΔST = ΔSC - δ).

[0061] Next, the drying condition setting device 71 refers to the data table 77 stored in the memory area 78 to calculate a drying temperature T for correcting the difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc (step 306). The drying condition setting device 71 of this embodiment is configured to execute setting output of the drying temperature T calculated in step 306 (step 307).

[0062] (action) That is, when the electrode mixture 50 applied on the substrate 36 is dried, the plate specific surface area Se2 after drying becomes larger than the plate specific surface area Se1 before drying. Furthermore, the change amount ΔS in the plate specific surface area Se caused by this drying depends on the drying conditions of the electrode mixture 50 applied on the substrate 36. This makes it possible to adjust the plate specific surface area Se2 after drying based on the setting of the drying conditions.

[0063] Next, the effects of this embodiment will be described. (1) When manufacturing the electrode sheet 35 that forms the electrode plate 51 of the secondary battery 1, a step of applying an electrode mixture 50 containing an electrode active material 55 onto a substrate 36 that becomes the current collector 31, and a step of drying the electrode mixture 50 applied onto the substrate 36 are performed. In addition, in a manufacturing process prior to the step of drying the electrode mixture 50 applied onto the substrate 36, a specific surface area S of the electrode active material 55 contained in the electrode mixture 50 is acquired. Furthermore, the acquired specific surface area S of the electrode active material 55 is set as an acquired specific surface area Sd, and the specific surface area S of the electrode active material 55 in a state in which the electrode mixture 50 applied onto the substrate 36 forms the electrode plate 51 is set as an electrode plate specific surface area Se. Then, by setting drying conditions for the electrode mixture 50 according to the acquired specific surface area Sd, the electrode plate specific surface area Se2 after drying is adjusted.

[0064] According to the above-mentioned configuration, it is possible to easily reduce the variation in the specific surface area S of the electrode active material 55, i.e., the electrode plate specific surface area Se, in a state in which the electrode mixture 50 applied to the substrate 36 forms the electrode plate 51, with a simple configuration. This makes it possible to ensure uniformity in the battery performance.

[0065] (2) When drying the electrode mixture 50, the smaller the obtained specific surface area Sd, the higher the drying temperature T that is set. That is, the change ΔS in the plate specific surface area Se caused by drying increases as the drying temperature T of the electrode mixture 50 applied to the substrate 36 increases. Therefore, according to the above configuration, the drying temperature T of the electrode mixture 50 can be set as a drying condition setting subject to the acquired specific surface area Sd of the electrode active material 55, and the plate specific surface area Se2 after drying can be easily adjusted. This makes it possible to suppress the variation in the plate specific surface area Se and ensure uniformity in battery performance.

[0066] (3) When drying the electrode mixture 50, the drying temperature T is set to correct the difference δ between the acquired specific surface area Sd and the standard specific surface area Sc based on the amount of change ΔS in the electrode plate specific surface area Se, which changes depending on the drying conditions.

[0067] According to the above-mentioned configuration, the specific surface area Se2 of the electrode plate after drying can be adjusted with high precision, and this effectively reduces the variation in the specific surface area Se of the electrode plate, thereby ensuring uniformity in the battery performance.

[0068] (4) When manufacturing the electrode sheet 35, a step of mixing the raw materials of the electrode mixture 50 and a step of kneading the mixed electrode mixture 50 are performed. Furthermore, in a coating step, the kneaded electrode mixture 50 is coated on the substrate 36. When setting the drying temperature T, the initial specific surface area S0 obtained for the electrode active material 55 before mixing is used as the obtained specific surface area Sd.

[0069] That is, for the electrode active material 55 as a raw material before mixing, the variation of its initial specific surface area S0 is usually allowed within a predetermined tolerance α. As a result, the initial specific surface area S0 varies for each production unit as a raw material, that is, for each lot. Therefore, according to the above configuration, the electrode plate specific surface area Se2 after drying can be adjusted efficiently and highly accurately by setting the drying conditions according to the obtained specific surface area Sd of the electrode active material 55. As a result, the variation of the electrode plate specific surface area Se can be effectively suppressed to ensure uniformity of battery performance.

[0070] Furthermore, the initial specific surface area S0 of the electrode active material 55 is often indicated as a measured value in the form of, for example, a specification or a label. Therefore, according to the above configuration, the specific surface area S of the electrode active material 55 contained in the electrode mixture 50 can be easily obtained in the manufacturing process prior to the step of drying the electrode mixture 50 applied on the substrate 36 without performing any special measurement work. This makes it possible to efficiently set drying conditions according to the obtained specific surface area Sd of the electrode active material 55.

[0071] The above embodiment can be modified as follows: The above embodiment and the following modifications can be combined with each other to the extent that no technical contradiction occurs.

[0072] In the above embodiment, in the preparation process of the electrode mixture 50, an initial specific surface area S0, which is the specific surface area S of the electrode active material 55 as the raw material, is acquired. Then, this initial specific surface area S0 is set as the acquired specific surface area Sd, and the drying conditions according to the acquired specific surface area Sd are set. However, the acquired specific surface area Sd is not limited to this, and may be the specific surface area S of the electrode active material 55 acquired in the manufacturing process before the process of drying the electrode mixture 50 applied on the substrate 36. For example, the electrode plate specific surface area Se1 before drying may be measured, and the value may be the acquired specific surface area Sd. Also, the specific surface area S after kneading may be measured before application to the substrate 36, and the value may be the acquired specific surface area Sd. The standardized specific surface area Sc may also be specified as a value at the time of acquisition.

[0073] The value of the standard specific surface area Sc may be set arbitrarily, and the value of the tolerance α may also be set arbitrarily. For example, the value of the tolerance α may be different above and below the standard specific surface area Sc. In other words, the standard specific surface area Sc does not necessarily have to be the standard center value.

[0074] In the above embodiment, as an example, the standardized specific surface area Sc, which is the standard center value, is set to "4.2", the standard drying temperature T corresponding to the case where the acquired specific surface area Sd coincides with this standardized specific surface area Sc is set to "175°C", and the value of the reference change amount ΔSC is determined to be "0.1". However, the present invention is not limited to this, and the reference change amount ΔSC may be any value that indicates the change amount ΔS in the plate specific surface area Se caused by the drying under predetermined drying conditions. In other words, the drying conditions when setting the reference change amount ΔSC may be arbitrarily changed, including the standard drying temperature T.

[0075] In the above embodiment, the drying condition setting device 71 calculates the drying temperature T for correcting the difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc by referring to the data table 77 stored in the memory area 78. In addition, this data table 77 is assumed to have recorded in advance the relationship between the difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc, the target change amount during drying ΔST, and the drying temperature T set as the drying condition.

[0076] However, the present invention is not limited to this, and for example, as shown in Fig. 15, a data table 77B is used in which the relationship between the acquired specific surface area Sd and the drying temperature T set as the drying condition is recorded. Then, by referring to this data table 77B, the drying temperature T corresponding to the acquired specific surface area Sd can be calculated. That is, the relationship between the acquired specific surface area Sd and the drying temperature T set as the drying condition can also be grasped in advance based on the amount of change ΔS in the plate specific surface area Se that changes according to the drying temperature T, through experiments, simulations, or the like. This can simplify the configuration.

[0077] Also, for example, a data table 77 may be used in which the relationship between the difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc and the drying temperature T set as the drying condition is recorded. Also, a data table 77 may be used in which the relationship between the target change amount during drying ΔST and the drying temperature T set as the drying condition is recorded. In other words, as long as it is possible to ultimately calculate the drying temperature T set as the environmental condition according to the acquired specific surface area Sd, the calculation process using a formula before referring to the data table 77 is optional.

[0078] Furthermore, the drying condition setting device 71 holds in advance a formula showing the relationship between the amount of change ΔS in the plate specific surface area Se caused by the drying and the drying temperature T. Note that the formula in this case does not necessarily have to be the linear approximation formula expressed as "y=ax-b" as described above. Then, as shown in the above example, the drying temperature T corresponding to the acquired specific surface area Sd may be calculated by using such a formula without using the data table 77.

[0079] In the above embodiment, in order to adjust the dried specific surface area Se2 of the electrode mixture 50, the drying temperature T is set according to the acquired specific surface area Sd of the electrode mixture 50. However, the present invention is not limited to this, and the dried specific surface area Se2 of the electrode mixture 50 may be adjusted by changing the drying conditions other than the drying temperature T.

[0080] For example, a drying condition setting device 71C shown in Fig. 16 includes a drying time calculation unit 79 as a drying condition calculation unit 75C, which may be configured to set the drying time t according to the obtained specific surface area Sd.

[0081] That is, as shown in FIG. 17, the change in the electrode plate specific surface area Se caused by drying the electrode mixture 50 is due to migration that occurs during drying (see FIG. 6 and FIG. 7), and thus the drying time t, like the drying temperature T, is also a factor that affects the progress of migration. Note that FIG. 17 is an explanatory diagram for showing that there is a correlation between the electrode plate specific surface area Se caused by the drying and the drying time t, and is not a graph showing actual measurement data. However, in the actual electrode mixture 50, as in the model shown in the figure, the longer the drying time t, the more the migration progresses. This also increases the amount of change ΔS in the electrode plate specific surface area Se caused by the drying.

[0082] Therefore, when drying the electrode mixture 50, the smaller the obtained specific surface area Sd, the longer the drying time t should be set. Even with this configuration, the electrode plate specific surface area Se2 after drying can be easily adjusted. This makes it possible to suppress the variation in the electrode plate specific surface area Se and ensure uniformity in battery performance.

[0083] 18, for example, a data table 77C in which the acquired specific surface area Sd is associated with the drying time t set as the drying condition may be used for the calculation of the drying time t according to the acquired specific surface area Sd by the drying time calculation unit 79. Also, in this way, when the drying time t is set as the drying condition according to the acquired specific surface area Sd of the electrode active material 55, the design of the data table 77C may be changed as desired.

[0084] For example, data table 77C may correlate the difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc, the target change during drying ΔST, and the drying time t set as a drying condition. Also, data table 77C may correlate the difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc and the drying time t set as a drying condition. Data table 77C may also correlate the target change during drying ΔST and the drying time t set as a drying condition.

[0085] That is, in this case as well, as long as it is possible to calculate the drying time t to be set as an environmental condition according to the acquired specific surface area Sd, the calculation process using the formula before referring to the data table 77C is optional. And, instead of the data table 77C, an approximation formula showing the relationship between the amount of change ΔS in the electrode plate specific surface area Se caused by the drying and the drying time t may be stored.

[0086] 19 and 20, a drying condition setting device 71D may be provided with a drying condition calculation unit 75D that calculates the drying temperature T and drying time t according to the acquired specific surface area Sd. For example, a data table 77D may be used in which the acquired specific surface area Sd is associated with the drying temperature T and drying time t set as the drying conditions. In this case, too, as long as it is possible to calculate the drying temperature T and drying time t set as the environmental conditions according to the acquired specific surface area Sd, the calculation process using a formula before referring to the data table 77D is optional. By adopting such a configuration, the plate specific surface area Se2 after drying can be adjusted with higher accuracy.

[0087] In the above embodiment, a method for calculating the drying temperature T according to the obtained specific surface area Sd in order to correct the difference δ between the obtained specific surface area Sd and the standardized specific surface area Sc has been described by taking as an example a case in which the obtained specific surface area Sd is smaller than the standardized specific surface area Sc. However, the present invention is not limited to this, and a drying temperature T for correcting the difference δ between the obtained specific surface area Sd and the standardized specific surface area Sc may also be calculated in the same manner in a case in which the obtained specific surface area Sd is larger than the standardized specific surface area Sc.

[0088] For example, in the case of the above embodiment, even if the drying temperature T is in a temperature range lower than the standard value of "175°C", within the range in which the approximation formula is valid, it is possible to calculate the drying temperature T corresponding to an obtained specific surface area Sd larger than the standard specific surface area Sc by using a similar procedure (see Figures 10 to 12).

[0089] Here, the adjustment limit of the plate specific surface area Se by changing the setting of the drying temperature T utilizing the migration phenomenon during drying is the range in which this plate specific surface area Se increases during drying (see FIG. 11). For example, in the above embodiment, when the acquired specific surface area Sd matches the standard specific surface area Sc, the change amount ΔS of the plate specific surface area Se caused by the drying, i.e., the reference change amount ΔSC, is "0.1". Therefore, in the above embodiment, the adjustment limit of the plate specific surface area Se by changing the setting of the drying temperature T, i.e., the lower limit of the target change amount ΔST during drying, is "-0.1".

[0090] In the above embodiment, in a region where the target change amount ΔST during drying is close to the adjustment limit, the relationship between the change amount ΔS of the specific surface area Se of the plate caused by the drying and the drying temperature T may deviate from the above approximation formula. However, even in such a case, it is possible to deal with it by grasping in advance the relationship between the change amount ΔS of the specific surface area Se of the plate during drying, including the region close to the adjustment limit, and the drying temperature T, through the execution of experiments, simulations, etc.

[0091] That is, in this case as well, it is advisable to prepare an approximation formula or data table 77 including a region close to the adjustment limit, for example, by experiments, simulations, etc. in advance. The approximation formula in this case is not necessarily limited to the linear approximation formula shown in "y=ax-b" as described above. And, in the data table 77, the acquired specific surface area Sd and the drying conditions to be set do not necessarily have to have a linear relationship. By adopting such a configuration, it is possible to expand the range in which the specific surface area Se2 of the electrode plate after drying can be appropriately adjusted.

[0092] The adjustment limit of the electrode plate specific surface area Se by changing the drying conditions, i.e., the lower limit of the target change amount ΔST during drying, depends on the specifications of the electrode sheet 35 to be manufactured. That is, the adjustment limit does not necessarily match the lower limit of the target change amount ΔST during drying, "-0.1," in the above embodiment. Therefore, even when the obtained specific surface area Sd is larger than the standard specific surface area Sc, it may be possible to correct the difference δ between the obtained specific surface area Sd and the standard specific surface area Sc within the entire range of the allowable tolerance α, as long as the adjustment limit by changing the drying conditions is not exceeded.

[0093] In the above embodiment, when drying the electrode mixture 50, the drying temperature T for the acquired specific surface area Sd is set to correct the difference δ between the acquired specific surface area Sd and the standard specific surface area Sc based on the change amount ΔS of the plate specific surface area Se that changes according to the drying conditions. However, this is not limited to this, and the setting of the acquired specific surface area Sd according to the acquired specific surface area Sd does not necessarily have to completely correct the difference δ between the acquired specific surface area Sd and the standard specific surface area Sc. In other words, it is sufficient to suppress the variation in the plate specific surface area Se2 after drying, and the degree of the correction is not important. And the standard specific surface area Sc does not necessarily have to be determined.

[0094] In the above embodiment, the specific surface area S of the electrode active material 55 is measured by the BET method using nitrogen as the adsorption gas. However, this is not limited to this, and a value measured using an adsorption gas other than nitrogen may be used. Furthermore, the specific surface area S of the electrode active material 55 measured using other methods may be used, not limited to the BET specific surface area.

[0095] In the above embodiment, the drying conditions are set in accordance with the acquired specific surface area Sd of the electrode active material 55 in the manufacturing process of the electrode sheet 35N constituting the negative electrode 4. However, the present invention is not limited to this, and the drying conditions may be set in accordance with the acquired specific surface area Sd in the manufacturing process of the electrode sheet 35P constituting the positive electrode 3.

[0096] In the above embodiment, the electrode body 10 of the secondary battery 1 is formed in a wound state of the positive and negative electrode sheets 35P, 35N stacked with the separator 5 sandwiched therebetween. However, the present invention is not limited to this, and may be applied to, for example, a secondary battery 1 including an electrode body 10 in a planar laminated state.

[0097] In the above embodiment, the method for manufacturing the secondary battery 1 having a configuration as a lithium ion secondary battery is embodied. However, the present invention is not limited to this, and may be applied to a method for manufacturing a secondary battery 1 other than a lithium ion secondary battery.

[0098] The terminal shapes of the positive electrode terminal 38P and the negative electrode terminal 38N are not limited to the shapes shown in Fig. 1 and may be changed as desired. The shape of the case 20 that defines the outer shape of the secondary battery 1 is also not necessarily limited to a flat rectangular box shape and may be changed as desired, for example, to a cylindrical shape.

[0099] Next, the technical ideas that can be understood from the above embodiment and modified examples will be described. (a) The BET specific surface area is used as the specific surface area. (b) A formula showing the relationship between the amount of change in the specific surface area of ​​the electrode plate caused by the drying and the drying conditions is stored.

[0100] (c) A data table is maintained in which the acquired specific surface area is associated with the drying conditions to be set. (iv) A data table is maintained in which the difference between the acquired specific surface area and the standard specific surface area is associated with the drying conditions to be set. [Explanation of symbols]

[0101] 1…Secondary battery 31...Current collector 36...Base material 50...Electrode composite material 51...Pole plate 55...electrode active material S…Specific surface area Sd...obtained specific surface area Se,Se1,Se2…electrode plate specific surface area

Claims

1. A method for producing a secondary battery, comprising: applying an electrode mixture containing an electrode active material, a binder, and a solvent onto a substrate serving as a current collector; and drying the applied electrode mixture, The specific surface area of ​​the electrode active material is obtained in a manufacturing process prior to the step of drying the electrode mixture, The specific surface area of ​​the electrode active material obtained is designated as an obtained specific surface area Sd, The specific surface area of ​​the electrode active material in a state in which the electrode mixture applied to the substrate forms an electrode plate is defined as an electrode plate specific surface area Se, In advance, when the change amount ΔS of the specific surface area Se of the plate caused by drying is y and the drying temperature T is x, the relationship between them is obtained as a linear approximation equation y=ax-b (where "a" and "b" are coefficients), and A change amount ΔS in the specific surface area Se of the plate caused by drying under a predetermined drying condition is defined as a reference change amount ΔSC. The difference between the acquired specific surface area Sd and the standard specific surface area Sc is δ, A value obtained by subtracting the difference δ between the acquired specific surface area Sd and the standard specific surface area Sc from the reference change amount ΔSC is set as a target change amount ΔST during drying. A drying temperature T for correcting the difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc is set by the approximation formula based on the target change amount ΔST during drying; A method for manufacturing a secondary battery, comprising: setting drying conditions for the electrode mixture according to the obtained specific surface area, thereby adjusting the specific surface area of ​​the electrode plate after drying.

2. The drying temperature of the electrode mixture is set as the drying condition, The smaller the obtained specific surface area, the higher the drying temperature is set. The method for producing the secondary battery according to claim 1 .

3. The drying time of the electrode mixture is set as the drying condition, The smaller the acquired specific surface area, the longer the drying time is set. The method for producing the secondary battery according to claim 1 .

4. The drying conditions are set so as to reduce a difference between the acquired specific surface area and a predetermined standard specific surface area based on an amount of change in the specific surface area of ​​the electrode plate that changes depending on the drying conditions. The method for producing the secondary battery according to claim 1 .

5. The electrode mixture is applied to the substrate by a process comprising the steps of: preparing raw materials for the electrode mixture; and kneading the prepared electrode mixture. The electrode mixture is applied to the substrate by a process comprising the steps of: The method for producing a secondary battery according to claim 1 , wherein the specific surface area obtained for the electrode active material before the mixing is defined as the obtained specific surface area.

6. An apparatus for manufacturing a secondary battery, comprising: applying an electrode mixture containing an electrode active material, a binder, and a solvent onto a substrate serving as a current collector; and drying the applied electrode mixture, The specific surface area of ​​the electrode active material obtained during the manufacturing process before drying the electrode mixture is defined as an obtained specific surface area Sd; The specific surface area of ​​the electrode active material in a state in which the electrode mixture applied to the substrate forms an electrode plate is defined as an electrode plate specific surface area Se, an acquired specific surface area input unit that receives an input of the acquired specific surface area Sd; a drying condition calculation unit that calculates drying conditions for the electrode mixture according to the acquired specific surface area Sd input in order to adjust the electrode plate specific surface area Se after the drying; Equipped with The drying condition calculation unit calculates a relationship between the change amount ΔS of the electrode plate specific surface area Se caused by drying in advance as y and the drying temperature T as x, as a linear approximation equation y=ax-b (where "a" and "b" are coefficients), and A change amount ΔS in the specific surface area Se of the plate caused by drying under a predetermined drying condition is defined as a reference change amount ΔSC. The difference between the acquired specific surface area Sd and the standard specific surface area Sc is δ, A value obtained by subtracting the difference δ between the acquired specific surface area Sd and the standard specific surface area Sc from the reference change amount ΔSC is set as a target change amount ΔST during drying. The secondary battery manufacturing device calculates a drying temperature T for correcting a difference δ between the acquired specific surface area Sd and the standardized specific surface area Sc based on the target change ΔST during drying using the approximation formula.

Citation Information

Patent Citations

  • Production of compound oxide using sol-gel method

    JP1997175825A

  • Nonaqueous electrolyte secondary battery negative electrode and nonaqueous electrolyte secondary battery using it

    JP1998116604A

  • Nonaqueous secondary battery

    JP2005019094A

  • Method for manufacturing nonaqueous electrolyte secondary battery

    JP2017091943A

  • Apparatus for managing electrode drying oven

    KR1020160047748A