Plasma treatment method

The plasma processing method using a mixed gas and time-modulated power supply addresses the issue of protective film blockage in narrow mask patterns, ensuring effective etching and improved pattern processing in semiconductor devices.

JP7577865B2Active Publication Date: 2024-11-05HITACHI HIGH TECH CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023541019
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-04-18
Publication Date
2024-11-05
Estimated Expiration
2042-04-18

AI Technical Summary

Technical Problem

The miniaturization of semiconductor device features leads to narrower spacing between mask patterns, causing protective films to block mask openings during plasma etching, preventing adequate etching of the underlying film.

Method used

A plasma processing method using a mixed gas of oxygen, nitrogen, and hydrogen-containing gases to form a protective film on the mask, combined with time-modulated power supply, suppresses protective film deposition parallel to the substrate surface, allowing for improved pattern processing in narrow spaces.

Benefits of technology

The method effectively prevents protective film blockage in mask openings, enabling efficient etching of narrow spaces and improving pattern processing precision.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577865000001
    Figure 0007577865000001
  • Figure 0007577865000002
    Figure 0007577865000002
  • Figure 0007577865000003
    Figure 0007577865000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide a plasma processing method which inhibits the closing off of an opening of a mask pattern due to a protective film being deposited in a direction parallel to a substrate surface, and which improves pattern processing even in a narrow space. This plasma processing method plasma etches a film to be etched by using a protective film formed on a mask, the method having a step for forming the protective film on the mask by using plasma generated by a mixed gas composed of a silicon-containing gas, an oxygen-containing gas, a nitrogen-containing gas, and a hydrogen-containing gas. The hydrogen-containing gas is H2 gas, HBr gas, or CH4 gas. The oxygen-containing gas is O2 gas, CO gas, CO2 gas, COS gas, or SO2 gas.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a plasma processing method. [Background technology]

[0002] In the manufacturing process of semiconductor devices, a plasma processing method is known in which a film to be etched on a substrate is etched using a patterned mask made of an oxide film or a nitride film formed on the substrate. Since the patterned mask may be used for other purposes without being removed after the etching process, it is necessary not to damage the mask during etching. For this reason, a method is used in which a protective film is deposited on the patterned mask before etching. For this reason, such a plasma processing method includes a step of forming a protective film on the mask and a step of etching.

[0003] As a method for etching using a mask on which a protective film is deposited, an etching method disclosed in Patent Document 1 has been proposed. The invention disclosed in Patent Document 1 is an etching method for etching a silicon carbide substrate placed on a base in a processing chamber, in which the silicon carbide substrate is heated to 200° C. or higher, a processing gas containing at least a silicon-based gas containing SiF4 gas or SiCl4 gas, and oxygen gas or nitrogen gas is supplied into the processing chamber to generate plasma, and the silicon carbide substrate is etched while a silicon oxide film or silicon nitride film is formed on the silicon carbide substrate as a protective film. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-239757 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, as the cell size becomes smaller and the line and space becomes finer, the spacing between mask patterns becomes narrower, and it has been found that when a protective film is deposited using plasma, the protective film that grows in the lateral direction (surface direction) of the substrate blocks the opening of the mask pattern. Therefore, even if etching is performed using plasma, the protective film deposited in the opening prevents the plasma from entering the space, and the film to be etched cannot be sufficiently etched. The etching technology of Patent Document 1 also fails to recognize the problem that the spaces between mask patterns are blocked by a protective film.

[0006] The present invention has been made to solve the above-mentioned problems, and has an object to provide a plasma processing method that prevents a protective film from being deposited in a direction parallel to the substrate surface and blocks openings in a mask pattern, thereby improving pattern processing even in a narrow space. [Means for solving the problem]

[0007] In order to solve the above problems, one representative plasma processing method of the present invention is a plasma processing method for plasma etching a film to be etched using a protective film formed on a mask, which includes a step of forming the protective film on the mask using plasma generated from a mixed gas of a silicon element-containing gas, an oxygen element-containing gas, a nitrogen element-containing gas, and a hydrogen element-containing gas. Effect of the Invention

[0008] According to the present invention, the deposition of a protective film in a direction parallel to the substrate surface and blocking of openings in a mask pattern is suppressed, and pattern processing is improved even in a narrow space. Problems, configurations and effects other than those described above will become apparent from the description of the following embodiments. [Brief description of the drawings]

[0009] [Figure 1]FIG. 1 is a schematic diagram of a plasma processing apparatus in which a plasma processing method according to a first embodiment of the present invention is performed. [Diagram 2] FIG. 2 is a schematic diagram of the formation of a protective film when a gas containing hydrogen elements is used in the first embodiment of the present invention. [Figure 3A] FIG. 3A is a schematic diagram of a cross section of a substrate to be processed on which a plasma processing method according to a second embodiment of the present invention is performed. [Figure 3B] FIG. 3B is a schematic diagram of a cross section of the target substrate after the protective film forming step in the plasma processing method according to the second embodiment of the present invention. [Figure 3C] FIG. 3C is a schematic diagram of a cross section of the target substrate after the etching step in the plasma processing method according to the second embodiment of the present invention. [Figure 3D] FIG. 3D is a conceptual diagram showing a mechanism for forming the protective film 204 in the second embodiment. [Figure 4] FIG. 4 is a diagram showing protective film formation conditions according to the second embodiment of the present invention. [Figure 5A] FIG. 5A is a schematic diagram of a cross section of a substrate to be processed after a protective film forming step in a plasma processing method according to a second embodiment of the present invention. [Figure 5B] FIG. 5B is a conceptual diagram showing a mechanism for forming the protective film 207 in the second embodiment. [Figure 6] FIG. 6 is a schematic diagram of a cross section of a substrate to be processed when a conventional protective film forming step is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that the present invention is not limited to the embodiment. In addition, in the description of the drawings, the same parts are denoted by the same reference numerals.

[0011] In an embodiment of the present invention, the mask is made of silicon nitride or silicon oxide, for example, and the mask pattern forms spaces spaced apart at predetermined intervals.

[0012] In an embodiment of the present invention, for example, a silicon nitride film is formed as a film to be etched on a substrate to be processed (hereinafter also referred to as a "sample"), and the above-mentioned mask is formed on the surface of the silicon nitride film. Therefore, the silicon nitride film to be etched is etched according to the pattern of the mask. Unless otherwise specified in this disclosure, the surface means a surface parallel to the surface of the film to be processed, such as a silicon nitride film. In the embodiment of the present invention, the time modulation of power means that the power output is periodically switched between an on state and an off state. Hereinafter, the time modulation is also referred to as "pulse modulation."

[0013] <Conventional example> A case where the conventional example is applied will be described with reference to Fig. 6. Fig. 6 is a schematic diagram of a cross section of a substrate to be processed when a conventional protective film forming step is applied. The substrate to be processed 209 has a silicon nitride film 203 formed on a wafer substrate 201 as a film to be etched, and a pattern of a mask 202 is formed on the surface of the silicon nitride film 203.

[0014] Next, in order to form a protective film 206 on the upper surface of the mask 202, SiCl4 gas, N2 gas, O2 gas, and He gas are used as process gases, and silicon oxides and nitrides are generated in plasma to deposit the protective film 206 on the upper surface of the mask 202. The He gas used here serves the function of adjusting the distribution so that the protective film 206 deposited on the wafer surface is uniformly distributed between the center and periphery of the wafer surface, and does not affect the properties of the protective film 206. In the conventional protective film formation step, the protective film 206 is deposited not only on the upper surface of the mask 202 but also in the openings 208, causing blockage of the pattern. Therefore, if an etching step is subsequently performed, it is not possible to perform the desired etching on the silicon nitride film 203. It has been confirmed that when the spacing d of the openings 208 in the pattern of the mask 202 is at least a space narrower than 15 nm, oxides and the like are deposited, causing clogging.

[0015] [First embodiment] 1 is a schematic diagram of a plasma processing apparatus 100 for performing a plasma processing method according to an embodiment of the present invention. The plasma processing apparatus 100 is an apparatus for generating plasma by using microwave electron cyclotron resonance (ECR) and performing plasma processing by using the generated plasma.

[0016] <Device configuration> The processing chamber 101 is a space surrounded by a chamber 102 and a top plate 103. A shower plate 104 for introducing a processing gas is installed in the processing chamber 101. The shower plate 104 has holes, through which the processing gas is introduced. The shower plate 104 is made of, for example, quartz. The vacuum exhaust pump 105 is controlled by a control unit 107. The vacuum exhaust pump 105 exhausts the inside of the processing chamber 101 to a high vacuum. The sample stage 108 is provided with an electrode. The substrate 109 is electrostatically attracted to the electrode, whereby the substrate 109 is held. A bias power is supplied to the electrode of the sample stage 108, as described later. The sample stage 108 is made of, for example, aluminum or titanium.

[0017] The cavity resonator 110 is a space surrounded by the top plate 103 and the chamber 111. The top plate 103 can be made of, for example, quartz. A waveguide 112 is connected to the cavity resonator 110. The waveguide 112 is composed of a straight waveguide in which the waveguide is laid in a straight line and a corner waveguide in which the waveguide is bent by 90 degrees.

[0018] The central axes of the straight waveguide portion of the waveguide 112 connected to the opening of the cavity resonance portion 110, the processing chamber 101, the sample stage 108, and the substrate 109 to be processed are aligned. A magnetic field generating coil 113 for generating a magnetic field is disposed around the processing chamber 101 and the cavity resonance portion 110.

[0019] <Plasma generation> The control unit 114 controls the source power supply 115 and the bias power supply 116. The source power for generating plasma and the bias power supplied to the substrate 109 are set to etch the substrate 109. Hereinafter, the source power and the bias power are also simply referred to as high-frequency power.

[0020] The source power supply 115 generates an electromagnetic wave via a matching box 117. The source power supply 115 has a CW mode in which the power oscillation is continuously on [Continuous Wave] and a time modulation mode in which the power oscillation is periodically turned on and off on the order of milliseconds. In the present invention, the electromagnetic wave is a microwave of 2.45 GHz. In the first embodiment, the source power supply 115 outputs source power in the CW mode. The source power is power for generating plasma. The electromagnetic wave generated by the source power supply 115 propagates through the waveguide 112 and is introduced into the processing chamber 101 via the cavity resonator 110, the top plate 103, and the shower plate 104. Plasma 119 is generated from the processing gas present in the processing chamber 101 by the electric field generated by the electromagnetic wave and the magnetic field generated by the magnetic field generating coil 113.

[0021] A bias power Wv is supplied to the electrodes provided on the sample stage 108 from a bias power supply 116 via a matching box 118. The bias power supply 116 has a CW mode in which the bias power is continuously on [Continuous Wave] and a time modulation mode in which the bias is periodically turned on and off on the order of milliseconds.

[0022] <Examples of using hydrogen-containing gas> 2 is a schematic diagram of the formation of a protective film when a gas containing hydrogen element is used in the first embodiment. The process gas used in the first embodiment is SiCl4 gas, N2 gas, O2 gas, and HBr gas with a flow rate three times the total flow rate of N2 gas and O2 gas. The source power and bias power are in CW mode.

[0023] As a result, as shown in FIG. 2, the protective film 207 became thicker than 15 nm, causing tilting and contact between the protective films. It is considered that tilting occurs because the protective film is excessively attached due to the use of CW mode, and the formation of the protective film becomes uneven. Although etching of the silicon nitride film 203 can be performed in the step after the protective film formation step, the degree of processing of the silicon nitride film 203 varies due to the contact between the protective films at the opening 208. Although contact between the patterns can be prevented by reducing the deposition amount, the deposition of up to about 15 nm is the limit in order to avoid tilting of the protective film. The same result was obtained when CH4 was used as the gas containing hydrogen elements.

[0024] [Second embodiment] In the second embodiment, the plasma 119 is generated from a mixed gas of a silicon element-containing gas, an oxygen element-containing gas, a nitrogen element-containing gas, and a hydrogen element-containing gas. With respect to the mixed gas (hereinafter also referred to as a "processing gas") from which the plasma 119 is generated, charged particles and neutral particles of ions and electrons emitted from the plasma 119 can be used as etching species. For example, the reactive gas can be selected from Cl2, HBr, O2, N2, He, Ar, SiCl4, CH4, and the like. In the second embodiment, the bias power supply 116 is different from the first embodiment in that it outputs bias power in the TM mode. The ions contained in the plasma contribute to the etching reaction together with the radicals attached to the substrate 109 to be processed while the energy thereof is controlled according to the power supplied to the wafer. In the description of the second embodiment, the same reference numerals are used for the same or equivalent components as those in the first embodiment, and the description thereof will be simplified or omitted.

[0025] Next, a plasma processing method according to a second embodiment of the present invention using the plasma processing apparatus 100 will be described with reference to FIGS. 3A to 3C. FIG. 3A is a schematic cross-sectional view of a substrate 109 to be processed, on which a plasma processing method according to a second embodiment of the present invention is performed. The substrate 109 to be processed is formed by depositing a silicon nitride film 203, which is a film to be etched, on a wafer substrate 201, and further forming a mask 202 of silicon nitride. The pattern of the mask 202 is formed in advance by a process before the substrate 109 to be processed is formed. In the embodiment of the present invention, the interval d between the openings 208 in the pattern of the mask 202 is about 15 nm. In the second embodiment, the protective film 204 is silicon oxide or silicon nitride, and silicon contained in the processing gas becomes a deposition component of the protective film 204.

[0026] The plasma processing method according to the present invention is performed in a state where a mask is formed on the film to be etched. FIG. 3A shows an example where the film to be etched and the mask are formed on the surface of the wafer substrate 201, but the plasma processing method according to the present invention can be applied in a state where the film to be etched and the mask are present. In the second embodiment, the film to be etched and the mask are made of the same material, but the present invention is not limited to this. For example, the material of the film to be etched can be silicon oxide and the material of the mask can be silicon nitride. Alternatively, the material of the film to be etched can be silicon nitride and the material of the mask can be silicon oxide.

[0027] FIG. 3B is a schematic diagram of a cross section of the substrate 109 to be processed after a protective film forming step in the plasma processing method according to the second embodiment of the present invention. In the protective film forming step, a protective film is formed on the mask using plasma. In the protective film forming step, a protective film is formed while a high frequency power is supplied from the bias power supply 116 to the sample. As shown in FIG. 3B, a protective film 204 having a thickness w1 of approximately 15 nm is deposited on the surface of the mask 202. Here, the surface refers to a surface parallel to the surface of the wafer substrate 201. On the side of the mask 202, in other words, on a surface parallel to the creeping surface (slope) of the wafer substrate 201, the protective film 204 is hardly formed. Here, the processing gas is SiCl4 gas, N2 gas, and a gas containing an oxygen element and a gas containing a hydrogen element. The gas containing a hydrogen element is H2 gas, HBr gas, or CH4 gas, and may contain at least one of H2 gas, HBr gas, or CH4 gas. The gas containing oxygen element is O2 gas, CO gas, CO2 gas, COS gas or SO2 gas, and may contain at least one of O2 gas, CO gas, CO2 gas, COS gas and SO2 gas. Reason The gas may be, for example, a mixture of SiCl4 gas, O2 gas, HBr gas, and N2 gas.

[0028] 3C is a schematic diagram of a cross section of the substrate 109 to be processed after an etching step in the plasma processing method according to the second embodiment of the present invention. The etching step is plasma etching performed after a protective film 204 of a predetermined thickness is formed. As shown in FIG. 3C, a trench 205 having a predetermined depth is formed in the silicon nitride film 203, which is the film to be etched. In the second embodiment, CHF3 gas and O2 gas are used as processing gases for the plasma etching. The protective film 204 is also removed by the etching step, but since the protective film 204 is formed, etching of the mask 202 below the protective film 204 is suppressed.

[0029] <Actions and Effects> FIG. 3D is a conceptual diagram showing a mechanism for forming the protective film 204 in the second embodiment. With reference to FIG. 3D(1), a first expected phenomenon will be described. First, silicon contained in the processing gas is bonded with oxygen or nitrogen, and the protective film 204 begins to deposit on the surface of the mask 202. On the other hand, in the space between the patterns of the mask 202, hydrogen, which has a smaller atomic radius than the atomic radius of other elements contained in the plasma, is likely to enter, and it is considered that a large amount of hydrogen remains there. The hydrogen remaining in such a space combines with N or O, and the N or O bonded to the silicon is dissociated. Due to such a reduction action of hydrogen, the growth of the protective film is suppressed in the space of the mask 202, while the deposition of the protective film progresses on the surface of the mask 202. With reference to FIG. 3D(2), a second expected phenomenon will be described. N or O that has bonded with H and dissociated recombines with H or the like to become stable molecules, making it difficult for them to adhere to the surface of the protective film. It is believed that the growth of the protective film in the space portion is suppressed by the synergistic effect of the first and second phenomena.

[0030] <Source power and bias power time modulation mode> The second embodiment also allows the source power and bias power to be in a time modulation mode.

[0031] FIG. 4 is a diagram showing the protective film forming conditions according to the second embodiment of the present invention. The bias power is time-modulated in association with the time modulation of the source power. FIG. 4 shows the relationship between the on (ON) state and the off (OFF) state of the source power Ws and the bias power Wv. The source power Ws is supplied periodically in a pulsed manner. As shown in FIG. 4, at time t s1 From time t s2 is the on-state period (hereinafter also referred to as the "on period"), and the time t s2 From time t s3 is an off-state period (hereinafter also referred to as the "off period"), and the time t s3 From time t s4 The duty ratio Ds of the source power is Ds = (t s2 -ts1 ) / (t s3 -t s1 ) The bias power is also supplied periodically in a pulsed manner, with the time t v1 From time t v2 is the on-period, and time t v2 Hours since t v3 During off Period and time t v3 Hours since t v4 During On Period The duty ratio Dv of the bias power is Dv=(t v2 -t v1 ) / (t v3 -t v1 4, the ON period of the bias power is included in the ON period of the source power, and the duty ratio Dv of the bias power is set to be smaller than the duty ratio Ds of the source power.

[0032] 4, during the ON period of the source power Ws, the bias power Wv is turned on. The frequency of the source power and the frequency of the bias power are set to be the same.

[0033] 5A is a schematic diagram of a cross section of a substrate 109 to be processed after a protective film forming step in a plasma processing method according to a second embodiment of the present invention. A thickness w2 of the protective film 207 is larger than a thickness w1 of the protective film 204 in the first embodiment, and a protective film with no inclination up to a thickness of approximately 30 nm can be formed.

[0034] <Actions and Effects> FIG. 5B is a conceptual diagram showing a mechanism for forming the protective film 207 in the second embodiment. FIG. 5B(1) shows a case where the bias power is also turned on during a period in which the source power is turned on and plasma is generated (for example, t in FIG. 4). v1 From v2FIG. 5B(2) shows a state in which the surface of the protective film 207 is flattened by physical collision of ions with the protective film 207. v2 From s2 FIG. 5B(3) shows how the protective film is isotropically deposited when the bias power is also turned off during the source power off period (for example, during t s2 From s3 This shows how the reaction for forming the protective film is suppressed while the excess reaction products are exhausted and removed to prevent them from adhering to the substrate and causing the growth direction to deviate from the vertical. By repeating these three processes, the protective film 207 is formed without any tilt. At this time, the time modulation of the source power and the time modulation of the bias power are related to each other as shown in Fig. 4. In particular, the duty ratio Ds of the source power is set to be larger than the duty ratio Dv of the bias power.

[0035] In this manner, according to the second embodiment, deposition of the protective film in a direction parallel to the substrate surface is suppressed, thereby improving blockage of the openings 208 in the mask pattern and enabling processing of patterns with narrow spaces with good selectivity.

[0036] In the first and second embodiments, the mask pattern spacing d is 15 nm. When the spacing d is 15 nm or less, the plasma processing method according to the present invention is preferably applied.

[0037] The above-mentioned embodiments have been described in order to explain the present invention in an easy-to-understand manner, and are not necessarily limited to those having all the configurations described above. In addition, it is possible to replace the configuration of one embodiment. In addition, it is possible to add, delete, or replace part of the configuration of each embodiment with another configuration.

[0038] Although an embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and various modifications are possible without departing from the gist of the present invention.

[0039] For example, in the first and second embodiments, the microwave ECR type plasma processing apparatus shown in FIG. 1 is used, but similar effects can be obtained in plasma processing apparatuses using other plasma sources such as CCP (Capacitively Coupled Plasma) type and ICP (Inductively Coupled Plasma) type by adjusting the pressure, gas flow rate, gas ratio, bias power, frequency, etc. [Explanation of symbols]

[0040] 100: plasma processing apparatus, 101: processing chamber, 102: chamber, 103: top plate 104...shower plate, 105...vacuum exhaust pump, 107...control unit 108: sample stage, 109: substrate to be processed 110: cavity resonator, 111: chamber, 112: waveguide 113: magnetic field generating coil, 114: control unit 115... source power supply, 116... bias power supply 117, 118...matching box, 119...plasma 201...wafer substrate, 202...mask, 203...silicon nitride film 204, 206, 207...protective film, 205...trench 208: opening, 209: substrate to be processed

Claims

1. 1. A plasma processing method for plasma etching a film to be etched using a protective film formed on a mask, comprising: forming the protective film on the mask using plasma generated by a mixed gas of a silicon element-containing gas, an oxygen element-containing gas, a nitrogen element-containing gas, and a hydrogen element-containing gas; The step of forming the protective film while supplying high frequency power to the sample on which the etched film is formed, The high frequency power for generating the plasma and the high frequency power supplied to the sample are pulse modulated; a duty ratio of the high frequency power supplied to the sample is smaller than a duty ratio of the high frequency power for generating the plasma; a first period during which the high frequency power supplied to the sample is turned on; a second period during which the high frequency power is turned on for generating the plasma;

2. 1. A plasma processing method for plasma etching a film to be etched using a protective film formed on a mask, comprising:

1. A plasma processing method comprising the step of forming the protective film on the mask using plasma generated from a mixed gas of SiCl 4 gas, O 2 gas, HBr gas, and N 2 gas.

3. 2. The plasma processing method according to claim 1, The hydrogen-containing gas is H 2 gas, HBr gas or CH 4 2. A plasma processing method comprising the steps of:

4. 2. The plasma processing method according to claim 1, The oxygen-containing gas is O 2 Gas, CO gas, CO 2 Gas, COS gas or SO 2 2. A plasma processing method comprising the steps of:

5. 3. The plasma processing method according to claim 2, The step of forming the protective film while supplying high frequency power to the sample on which the etched film is formed, The plasma processing method according to claim 1, wherein the high frequency power for generating the plasma and the high frequency power supplied to the sample are pulse modulated.

6. 6. The plasma processing method according to claim 5, a duty ratio of the high frequency power supplied to the sample is smaller than a duty ratio of the high frequency power for generating the plasma; a period during which high frequency power is supplied to the sample and which is included in a period during which high frequency power is supplied to the sample for generating the plasma;

7. 3. The plasma processing method according to claim 1, The plasma processing method according to claim 1, wherein the mask patterns are spaced apart at intervals of 15 nm or less.

Citation Information

Patent Citations

  • Etching method

    JP2013239757A

  • Plasma processing method

    JP2018160689A

  • Plasma etching method

    JP2019087626A

  • Etching method and substrate processing apparatus

    JP2021034483A

  • Methods for etching a hardmask layer

    US20190221441A1