Sulfide solid electrolyte, all-solid-state battery, and method for producing sulfide solid electrolyte
By controlling the Ge2+ to Ge4+ ratio through gas atmosphere adjustments during firing, the sulfide solid electrolyte achieves improved water resistance and maintains high Li ion conductivity in humid conditions, addressing the conductivity loss issue in LGPS-based electrolytes.
Patent Information
- Application Number
- JP2021165304
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-07
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-10-07
AI Technical Summary
LGPS-based sulfide solid electrolytes suffer from decreased Li ion conductivity due to moisture in the atmosphere, necessitating improved water resistance.
A sulfide solid electrolyte containing Li, Ge, and S with an LGPS type crystal phase, where the surface Ge2+ to total Ge ratio is controlled by adjusting the gas atmosphere during firing to form a Ge4+ reduction layer, enhancing water resistance.
The electrolyte maintains high Li ion conductivity even in high-humidity environments, ensuring stable battery performance.
Smart Images

Figure 0007578571000002 
Figure 0007578571000003 
Figure 0007578571000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to sulfide solid electrolytes. [Background technology]
[0002] All-solid-state batteries are batteries that have a solid electrolyte layer between a positive electrode active material layer and a negative electrode active material layer, and have the advantage that it is easier to simplify safety devices compared to liquid batteries that have an electrolyte solution containing a flammable organic solvent. Sulfide solid electrolytes are known as solid electrolytes used in all-solid-state batteries. Among sulfide solid electrolytes, LGPS-based sulfide solid electrolytes are known as materials with high Li-ion conductivity.
[0003] For example, Patent Document 1 discloses a method for producing a LGPS-based solid electrolyte, which includes a step of synthesizing a precursor by mixing Li3PS4 crystals and Li4MS4 crystals (M=Ge, Si, Sn) while the crystals are in the crystalline state, and a step of heat-treating the precursor at 300 to 700° C. Patent Documents 2 to 4 also disclose LGPS-based sulfide solid electrolytes. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2018 / 173939 [Patent Document 2] JP 2017-021965 A [Patent Document 3] JP 2019-501105 A [Patent Document 4] International Publication No. 2019 / 044517 Summary of the Invention [Problem to be solved by the invention]
[0005] Although the LGPS-based sulfide solid electrolyte is a material with high Li-ion conductivity, the Li-ion conductivity decreases due to moisture contained in the atmosphere. Therefore, improvement of water resistance is desired. The present disclosure has been made in view of the above-mentioned circumstances, and has as its main object to provide a sulfide solid electrolyte having good water resistance. [Means for solving the problem]
[0006] The present disclosure provides a sulfide solid electrolyte containing Li, Ge, P, and S and having an LGPS-type crystal phase, and when X-ray photoelectron spectroscopy is performed on the surface of the sulfide solid electrolyte, the ratio of Ge to the total amount of Ge is 2+ The sulfide solid electrolyte has a ratio of 20% or more.
[0007] According to the present disclosure, the amount of Ge relative to the total amount of Ge 2+ Since the ratio of is a predetermined ratio, it is possible to obtain a sulfide solid electrolyte having good water resistance.
[0008] In the above disclosure, the Ge 2+ The ratio may be 92% or less.
[0009] In the above disclosure, the Ge 2+ The proportion may be 49% or more.
[0010] In the above disclosure, the Ge 2+ The ratio may be 55% or more and 90% or less.
[0011] In the above disclosure, the Ge 2+ The proportion may be 94% or more.
[0012] In the above disclosure, the Ge 2+ The ratio may be 100%.
[0013] The present disclosure also provides an all-solid-state battery having a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, wherein at least one of the positive electrode active material layer, the negative electrode active material layer, and the solid electrolyte layer contains the sulfide solid electrolyte described above.
[0014] According to the present disclosure, by using the above-mentioned sulfide solid electrolyte, it is possible to obtain an all-solid-state battery that can maintain its output characteristics even in, for example, a high humidity environment.
[0015] The present disclosure also provides a method for producing the above-mentioned sulfide solid electrolyte, the method including a preparation step of preparing a precursor containing Li, Ge, P, and S, and a firing step of firing the precursor in an atmosphere of a gas containing at least one of nitrogen gas and a noble gas to form the above-mentioned LGPS-type crystal phase.
[0016] According to the present disclosure, a sulfide solid electrolyte having good water resistance can be obtained by performing firing in a predetermined gas atmosphere.
[0017] In the above disclosure, the gas may contain the nitrogen gas.
[0018] In the above disclosure, the gas may contain argon gas as the noble gas.
[0019] In the above disclosure, the gas may contain an oxidizing gas.
[0020] In the above disclosure, the gas may contain a reducing gas.
[0021] In the above disclosure, the calcination step may include a first calcination treatment in which the precursor is calcined under an atmosphere of a first gas containing argon gas, and a second calcination treatment in which the precursor after the first calcination treatment is calcined under an atmosphere of a second gas containing nitrogen gas.
[0022] In the above disclosure, the precursor may be a sulfide glass. Effect of the Invention
[0023] The present disclosure has an effect of providing a sulfide solid electrolyte having good water resistance. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating an all-solid-state battery according to the present disclosure. [Diagram 2] 1 is a flowchart illustrating a method for producing a sulfide solid electrolyte in the present disclosure. [Diagram 3] 1 shows the results of XPS measurement of the sulfide solid electrolyte produced in Reference Example 2. [Figure 4] 1 is a graph showing the relationship between the proportion of Ge2+ present and the Li ion conductivity after an exposure test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The sulfide solid electrolyte, the all-solid-state battery, and the method for producing the sulfide solid electrolyte according to the present disclosure will be described in detail below.
[0026] A. Sulfide solid electrolyte The sulfide solid electrolyte according to the present disclosure contains Li, Ge, P, and S and has an LGPS-type crystal phase. When X-ray photoelectron spectroscopy is performed on the surface of the sulfide solid electrolyte, the ratio of Ge to the total amount of Ge is 2+ The proportion of these is 20% or more.
[0027] According to the present disclosure, the amount of Ge relative to the total amount of Ge 2+Since the ratio of Ge to the total amount of Ge is a predetermined ratio, it is possible to obtain a sulfide solid electrolyte having good water resistance. Although the sulfide solid electrolyte having the LGPS type crystal phase is a material with high Li-ion conductivity, the Li-ion conductivity decreases due to moisture contained in the atmosphere. Therefore, improvement of water resistance is desired. In the present disclosure, 2+ Since the ratio of is a predetermined ratio, it is possible to obtain a sulfide solid electrolyte having good water resistance. Here, as described in the examples below, when sulfide glass is sintered in a vacuum, all of the Ge present on the particle surface is converted to Ge. 4+ That is, the ratio of Ge to the total amount of Ge 2+ Percentage of Ge 2+ In contrast, in the present disclosure, the presence rate of Ge is 0% by adjusting the type of gas used during firing. 2+ Specifically, the gas used during firing creates a highly water-resistant reduced layer (Ge 2+ By adjusting the type of gas, the reduced layer (Ge 2+ In this disclosure, the ratio of Ge 2+ By making the ratio of Ge equal to or greater than a certain ratio, a sulfide solid electrolyte having good water resistance can be obtained. The reason for the good water resistance is that 2+ Ge 4+ This is presumably because GeS has better water resistance than GeS2, which is also suggested by the fact that GeS has a lower solubility in water than GeS2.
[0028] The sulfide solid electrolyte of the present disclosure contains Li, Ge, P and S. The total ratio of Li, Ge, P and S to all elements contained in the sulfide solid electrolyte is, for example, 70 mol% or more, may be 80 mol% or more, or may be 90 mol% or more. In addition, the sulfide solid electrolyte may or may not contain a halogen. In the former case, the sulfide solid electrolyte may contain only one type of halogen, or may contain two or more types. Examples of halogen include Cl, Br and I.
[0029] The sulfide solid electrolyte of the present disclosure has a LGPS-type crystal phase. In the present disclosure, the LGPS-type crystal phase is a crystal phase containing Li, Ge, P, and S. The LGPS-type crystal phase has typical peaks at 20.18°±0.50°, 20.44°±0.50°, 26.96°±0.50°, and 29.58°±0.50° in X-ray diffraction measurement using CuKα radiation. The LGPS-type crystal phase may also have peaks at 2θ=17.38°±0.50°, 23.56°±0.50°, 23.96°±0.50°, 24.93°±0.50°, 29.07°±0.50°, 31.71°±0.50°, 32.66°±0.50°, and 33.39°±0.50°. Note that the positions of these peaks may vary depending on the composition of the sulfide solid electrolyte, for example, and are therefore defined within a range of ±0.50°. The positions of each peak may be within a range of ±0.30° or ±0.10°.
[0030] In addition, the LGPS type crystal phase is usually composed of an octahedron O (e.g., LiS6 octahedron) composed of Li and S elements, and M 2a Element (M 2a T1 is a tetrahedron composed of an element S (e.g., GeS4 and PS4), and M 2b Element (M 2b and a tetrahedron T2 (e.g., PS4) composed of an element T1 (which is at least one of P and Ge) and an element S, in which the tetrahedron T1 and the octahedron O share an edge, and the tetrahedron T2 and the octahedron O share a vertex.
[0031] The sulfide solid electrolyte of the present disclosure preferably contains an LGPS-type crystal phase as a main phase. "Containing as a main phase" means that the proportion of the LGPS-type crystal phase is the largest among all crystal phases contained in the sulfide solid electrolyte. The proportion of the LGPS-type crystal phase is, for example, 50% by weight or more, may be 70% by weight or more, or may be 90% by weight or more. The proportion of the above crystal phase can be measured, for example, by synchrotron radiation XRD.
[0032] In addition, in the present disclosure, when X-ray photoelectron spectroscopy was performed on the surface of the sulfide solid electrolyte, the ratio of Ge to the total amount of Ge was 2+ The ratio of Ge to the total amount of Ge is 20% or more. 2+ The ratio of Ge to the total amount of Ge may be 49% or more, 50% or more, 55% or more, or 60% or more. 2+ If the ratio of Ge is too small, the Li-ion conductivity after exposure to moisture may be low. 2+ The proportion of may be 92% or less, may be 90% or less, or may be 85% or less. 2+ By setting the ratio of Ge to the total amount of Ge in the above range, the Li ion conductivity after exposure to moisture is increased. 2+ When the ratio of Ge to the total amount of Ge is 49% or more and 92% or less (preferably, 55% or more and 90% or less), the Li ion conductivity after exposure to moisture is particularly high. 2+ The method for calculating the ratio will be described in the Examples below.
[0033] In addition, in the present disclosure, when X-ray photoelectron spectroscopy was performed on the surface of the sulfide solid electrolyte, the ratio of Ge to the total amount of Ge was 2+ The proportion of Ge may be 77% or more, 92% or more, 94% or more, 96% or more, or 100%. 2+ By increasing the proportion of, the retention rate of Li-ion conductivity before and after exposure to moisture is increased.
[0034] In addition, in the present disclosure, when X-ray photoelectron spectroscopy was performed on the surface of the sulfide solid electrolyte, the ratio of Ge to the total amount of Ge was 2+ The proportion of Ge may be 45% or less. 2+ By setting the ratio within the above range, the Li ion conductivity before exposure to moisture is increased.
[0035] The composition of the sulfide solid electrolyte in the present disclosure is not particularly limited. The sulfide solid electrolyte may have, for example, a composition represented by αLiX·(1-α)(Li 4-x Ge 1-x P x S4) (where X is one or more halogens, α satisfies 0≦α<1, and x satisfies 0<x<1). Examples of X include Cl, Br, and I. α may be 0 or may be greater than 0. In the latter case, α may be 0.1 or more, and may be 0.2 or more. Also, α may be 0.5 or less, and may be 0.4 or less. x may be 0.5 or more, and may be 0.6 or more. Also, x may be 0.8 or less, and may be 0.75 or less.
[0036] The sulfide solid electrolyte in the present disclosure preferably has a high Li ion conductivity. The Li ion conductivity (25°C) of the sulfide solid electrolyte is, for example, 1×10 -4 S / cm or more, and may be 1×10 -3 S / cm or more. Also, the sulfide solid electrolyte preferably has a high Li ion conductivity after a predetermined exposure test. The Li ion conductivity (25°C) after the exposure test is, for example, 1×10 -4 S / cm or more, and may be 1×10 -3 S / cm or more.
[0037] The exposure test is a test in which the sulfide solid electrolyte is left standing for 6 hours in a glove box with the dew point controlled to -30°C to expose the sulfide solid electrolyte to the moisture contained in the atmosphere, as described in the examples below. When the Li ion conductivity before the exposure test is IC1 and the Li ion conductivity after the exposure test is IC2, IC2 / IC1 (the retention rate of the Li ion conductivity before and after the exposure test) is, for example, 27% or more, may be 56% or more, and may be 95% or more.
[0038] Examples of the shape of the sulfide solid electrolyte include particulate form. The average particle size (D 50) is, for example, 0.1 μm or more, may be 0.5 μm or more, or may be 1 μm or more. On the other hand, the average particle diameter (D 50 ) is, for example, 50 μm or less, and may be 30 μm or less. 50 ) can be determined, for example, from the results of particle size distribution measurement by a laser diffraction scattering method.
[0039] The sulfide solid electrolyte of the present disclosure has good Li-ion conductivity and can be used in any application requiring Li-ion conductivity. In particular, the sulfide solid electrolyte of the present disclosure is preferably used in an all-solid-state battery. In addition, the method for producing the sulfide solid electrolyte of the present disclosure is not particularly limited, but may be the method described later in "C. Method for producing sulfide solid electrolyte."
[0040] B. All-solid-state battery Fig. 1 is a schematic cross-sectional view illustrating an all-solid-state battery according to the present disclosure. The all-solid-state battery 10 shown in Fig. 1 includes a positive electrode active material layer 1 containing a positive electrode active material, a negative electrode active material layer 2 containing a negative electrode active material, a solid electrolyte layer 3 disposed between the positive electrode active material layer 1 and the negative electrode active material layer 2, a positive electrode current collector 4 that collects current from the positive electrode active material layer 1, a negative electrode current collector 5 that collects current from the negative electrode active material layer 2, and a battery case 6 that houses these members. One feature of the present disclosure is that at least one of the positive electrode active material layer 1, the negative electrode active material layer 2, and the solid electrolyte layer 3 contains the sulfide solid electrolyte described above.
[0041] According to the present disclosure, by using the above-mentioned sulfide solid electrolyte, it is possible to obtain an all-solid-state battery that can maintain its output characteristics even in, for example, a high humidity environment.
[0042] 1.Cathode active material layer The positive electrode active material layer is a layer containing at least a positive electrode active material, and may contain at least one of a solid electrolyte, a conductive material, and a binder, as necessary. In particular, in the present disclosure, it is preferable that the positive electrode active material layer contains the above-mentioned sulfide solid electrolyte. The ratio of the sulfide solid electrolyte contained in the positive electrode active material layer is, for example, 0.1 vol.% or more, may be 1 vol.% or more, or may be 10 vol.% or more. On the other hand, the ratio of the sulfide solid electrolyte contained in the positive electrode active material layer is, for example, 80 vol.% or less, may be 60 vol.% or less, or may be 50 vol.% or less. In addition, examples of the positive electrode active material include LiCoO2, LiMnO2, LiNiO2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 Examples of oxide active materials include O2, LiVO2, LiCrO2, Li2NiMn3O8, LiFePO4, and LiCoPO4.
[0043] The positive electrode active material layer may contain a conductive material. The addition of the conductive material can improve the electronic conductivity of the positive electrode active material layer. Examples of the conductive material include carbon materials such as acetylene black, ketjen black, and carbon fiber. The positive electrode active material layer may also contain a binder. Examples of the binder include fluorine-based binders such as polyvinylidene fluoride (PVDF). The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.
[0044] 2.Negative electrode active material layer The negative electrode active material layer is a layer containing at least a negative electrode active material, and may contain at least one of a solid electrolyte, a conductive material, and a binder, as necessary. In particular, in the present disclosure, it is preferable that the negative electrode active material layer contains the above-mentioned sulfide solid electrolyte. The ratio of the sulfide solid electrolyte contained in the negative electrode active material layer is, for example, 0.1 vol.% or more, may be 1 vol.% or more, or may be 10 vol.% or more. On the other hand, the ratio of the sulfide solid electrolyte contained in the negative electrode active material layer is, for example, 80 vol.% or less, may be 60 vol.% or less, or may be 50 vol.% or less. In addition, examples of the negative electrode active material include metal active materials and carbon active materials. Examples of the metal active materials include In, Al, Si, and Sn. On the other hand, examples of the carbon active materials include mesocarbon microbeads (MCMB), highly oriented graphite (HOPG), hard carbon, and soft carbon.
[0045] The conductive material and binder used in the negative electrode active material layer are the same as those in the positive electrode active material layer described above. The thickness of the negative electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.
[0046] 3.Solid electrolyte layer The solid electrolyte layer is a layer disposed between the positive electrode active material layer and the negative electrode active material layer. The solid electrolyte layer is a layer containing at least a solid electrolyte, and may contain a binder as necessary. In particular, in the present disclosure, it is preferable that the solid electrolyte layer contains the above-mentioned sulfide solid electrolyte. The ratio of the sulfide solid electrolyte contained in the solid electrolyte layer is, for example, 50% by volume or more, may be 70% by volume or more, or may be 90% by volume or more. The binder used in the solid electrolyte layer is the same as that in the above-mentioned positive electrode active material layer. The thickness of the solid electrolyte layer is, for example, 0.1 μm or more and 1000 μm or less.
[0047] 4.Other configurations The all-solid-state battery in the present disclosure has at least the above-mentioned positive electrode active material layer, solid electrolyte layer, and negative electrode active material layer. In addition, it usually has a positive electrode current collector that collects the current of the positive electrode active material layer, and a negative electrode current collector that collects the current of the negative electrode active material layer. Examples of the material of the positive electrode current collector include SUS, aluminum, nickel, iron, titanium, and carbon. On the other hand, examples of the material of the negative electrode current collector include SUS, copper, nickel, and carbon.
[0048] 5.All-solid-state battery The all-solid-state battery in the present disclosure is usually an all-solid-state lithium ion battery. The all-solid-state battery may be a primary battery or a secondary battery, but the latter is preferred because it can be repeatedly charged and discharged and is useful, for example, as an in-vehicle battery.
[0049] C. Method for producing sulfide solid electrolyte Fig. 2 is a flow chart illustrating a method for producing a sulfide solid electrolyte according to the present disclosure. In Fig. 2, first, a precursor containing Li, Ge, P, and S is prepared (preparation step). Next, the prepared precursor is fired under an atmosphere of a gas containing at least one of nitrogen gas and a noble gas to form an LGPS type crystal phase (firing step). In this way, the above-mentioned sulfide solid electrolyte is obtained.
[0050] According to the present disclosure, a sulfide solid electrolyte having good water resistance can be obtained by performing firing in a predetermined gas atmosphere.
[0051] 1. Preparation process The preparation step in the present disclosure is a step of preparing a precursor containing Li, Ge, P, and S. The precursor may be a raw material mixture, may be a sulfide glass, or may have an LGPS-type crystal phase.
[0052] First, the case where the precursor is a raw material mixture will be described. The precursor usually contains a Li source, a Ge source, a P source, and an S source. Examples of the Li source include elemental Li and lithium sulfide (e.g., Li2S). Examples of the Ge source include elemental Ge and germanium sulfide (e.g., GeS2). Examples of the P source include elemental P and phosphorus sulfide (e.g., P2S5). Examples of the S source include elemental S, lithium sulfide, germanium sulfide, and phosphorus sulfide. Further, the raw material mixture may or may not contain LiX (where X is a halogen).
[0053] The composition of the raw material mixture is not particularly limited. For example, the raw material mixture may have a composition represented by αLiX·(1-α)(Li 4-x Ge 1-x P x S4) (where X is one or more halogens, α satisfies 0≦α<1, and x satisfies 0<x<1). For X, α, and x, the same applies as the content described in "A. Sulfide solid electrolyte" above. Further, the raw material mixture can be obtained by mixing each raw material in a mixing device (e.g., an agate mortar).
[0054] Next, the case where the precursor is a sulfide glass will be described. The sulfide glass can be obtained, for example, by performing mechanical milling on the raw material mixture. Examples of mechanical milling include a ball mill, a vibration mill, a turbo mill, and a disk mill. Further, the sulfide glass can be obtained, for example, by performing melt quenching on the raw material mixture. The sulfide glass usually has amorphousness. That is, in X-ray diffraction measurement, a halo pattern is observed for the sulfide glass. Also, in X-ray diffraction measurement, the sulfide glass may or may not have peaks derived from the raw materials, but the latter is preferred because it has higher amorphousness.
[0055] Next, a case where the precursor has an LGPS type crystal phase will be described. Such a precursor can be obtained, for example, by heat treating a raw material mixture or sulfide glass. The heat treatment temperature is, for example, 300°C or higher, and may be 400°C or higher, or 500°C or higher. The heat treatment temperature is, for example, 1000°C or lower, and may be 700°C or lower. The heat treatment atmosphere can be, for example, a reduced pressure atmosphere such as a vacuum. The heat treatment time is, for example, 1 hour or more and 20 hours or less.
[0056] 2. Firing process The calcination step in the present disclosure is a step of calcining the precursor in an atmosphere containing at least one of nitrogen gas and noble gas to form the LGPS type crystal phase. 4+ Ge 2+ and Ge 2+ In addition, by adjusting the composition of the gas used during firing, the ratio of Ge to the total amount of Ge is 2+ The ratio can be adjusted.
[0057] The gas (atmospheric gas) used during firing contains at least one of nitrogen gas and noble gas. Examples of noble gases include argon gas and helium gas. Nitrogen gas has a higher concentration of Ge compared to noble gases. 4+ Ge 2+ In the present disclosure, nitrogen gas and noble gas are referred to as reference gases. The ratio of the reference gas in the atmospheric gas is, for example, 90% by volume or more, may be 95% by volume or more, or may be 99% by volume or more.
[0058] The atmospheric gas may contain an oxidizing gas. By adding the oxidizing gas, the reducing power of the reference gas can be suppressed. Examples of the oxidizing gas include oxygen gas, oxygen-containing gas such as dry air, and carbon dioxide gas. The ratio of the oxidizing gas in the atmospheric gas is, for example, 0.01% by volume or more and 1% by volume or less.
[0059] The atmosphere gas may contain a reducing gas. The reducing power of the reference gas can be enhanced by adding the reducing gas. Examples of the reducing gas include hydrogen gas, carbon monoxide gas, and hydrocarbon gases such as methane, propane, and butane. The ratio of the reducing gas in the atmosphere gas is, for example, 0.01% by volume or more and 1% by volume or less.
[0060] In the present disclosure, it is preferable to flow a gas during firing. 4+ Ge 2+ This is because the firing temperature is, for example, 300° C. or higher, and may be 400° C. or higher, or 500° C. or higher. The firing temperature is, for example, 1000° C. or lower, and may be 700° C. or lower. The firing time is, for example, 1 hour or longer and 20 hours or shorter.
[0061] In the present disclosure, the firing step may include a first firing process in which the precursor is fired under an atmosphere of a first gas containing argon gas, and a second firing process in which the precursor after the first firing process is fired under an atmosphere of a second gas containing nitrogen gas. By performing the first firing process and the second firing process, a sulfide solid electrolyte having high Li-ion conductivity after the exposure test and high retention rate before and after the exposure test can be obtained. The first firing process and the second firing process may be performed continuously, or cooling may be performed after the first firing process, and then the second firing process may be performed. In the latter case, cooling to room temperature may be performed after the first firing process. The firing temperature and firing time in the first firing process and the second firing process are the same as those described above.
[0062] 3.Sulfide solid electrolyte The sulfide solid electrolyte obtained by each of the above-mentioned steps is similar to that described in "A. Sulfide solid electrolyte", and therefore will not be described here.
[0063] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0064] [Comparative Example 1] Li2S, P2S5 and GeS2 were prepared as raw materials, and these were mixed with Li 10 GeP2S 12 The mixture was weighed out to obtain the composition and placed in a zirconia pot together with zirconia balls. Then, mechanical milling (mechanical alloying) was performed using a planetary ball mill at 380 rpm for 40 hours to obtain sulfide glass. The obtained sulfide glass was pelletized, vacuum sealed in a quartz tube, and fired at 550°C for 8 hours to obtain a sulfide solid electrolyte.
[0065] [Example 1] A sulfide glass was obtained in the same manner as in Comparative Example 1. The obtained sulfide glass was placed on an alumina board and fired in a tubular furnace at 550° C. for 8 hours while flowing nitrogen gas containing 0.2 vol % oxygen gas, to obtain a sulfide solid electrolyte.
[0066] [ Reference example 2] A sulfide glass was obtained in the same manner as in Comparative Example 1. The obtained sulfide glass was placed on an alumina board and fired in a tubular furnace at 550° C. for 8 hours while flowing nitrogen gas, to obtain a sulfide solid electrolyte.
[0067] [Example 3] A sulfide glass was obtained in the same manner as in Comparative Example 1. The obtained sulfide glass was placed on an alumina board and fired in a tubular furnace at 550°C for 8 hours while flowing argon gas. After cooling to room temperature, the glass was fired again in a tubular furnace at 550°C for 8 hours while flowing nitrogen gas, to obtain a sulfide solid electrolyte.
[0068] [ Reference example 4] A sulfide glass was obtained in the same manner as in Comparative Example 1. The obtained sulfide glass was placed on an alumina board and fired in a tubular furnace at 550° C. for 8 hours while flowing argon gas, to obtain a sulfide solid electrolyte.
[0069] [Example 5] A sulfide glass was obtained in the same manner as in Comparative Example 1. The obtained sulfide glass was placed on an alumina board and fired in a tubular furnace at 550° C. for 8 hours while flowing argon gas to which 0.2 volume % of hydrogen gas was added, to obtain a sulfide solid electrolyte.
[0070] [evaluation] (XRD measurement) Example 1 , 3, 5, Reference examples 2, 4 X-ray diffraction (XRD) measurements were performed on the sulfide solid electrolytes obtained in Example 1 and Comparative Example 1. , 3, 5, Reference examples 2, 4 It was confirmed that the sulfide solid electrolyte obtained in Comparative Example 1 and Comparative Example 2 both had an LGPS type crystal phase.
[0071] (XPS measurement) Example 1 , 3, 5, Reference examples 2, 4 X-ray photoelectron spectroscopy (XPS) was performed on the sulfide solid electrolyte obtained in Comparative Example 1 and Comparative Example 2 to evaluate the structure of the sulfide solid electrolyte. The XPS device PHI-5800 manufactured by ULVAC-PHI was used as the X-ray photoelectron spectroscopy measurement device. The sample was placed in a holder for XPS measurement in a glove box with an argon atmosphere, and the holder was evacuated in a preliminary exhaust chamber for 30 minutes or more and introduced into the analysis chamber. For the measurement, a monochromatic AlKα (1487 eV) X-ray source was used to obtain information on the outermost surface of the sample. The measurement area was about 100 μmΦ, and a neutralization gun for Ar+ electron beam was used for charge neutralization.
[0072] The Ge3d spectrum obtained by XPS measurement was peak-separated, and the high-energy Ge 4+The peak area A of Ge corresponding to low energy 2+ The peak area B of Ge was calculated using the calculated peak area. 2+ The ratio of Ge to the total amount of Ge (B / (A+B)) is calculated. 2+ Peak separation was performed using the analysis software (MULTI PACK (ULVAC-PHI)) attached to the X-ray photoelectron spectroscopy measurement device. Background processing was performed using the Shirley method, and peak separation was performed using curve fitting by the nonlinear least squares method. A typical result is shown in Figure 3. Reference example Specifically, as shown in FIG. 3, the Ge3d spectrum obtained by XPS measurement is 4+ The peak of Ge 2+ The area of each peak was used to determine the Ge 2+ The proportions were calculated, and the results are shown in Table 1.
[0073] (Li ion conductivity measurement) Example 1 , 3, 5, Reference examples 2, 4 The Li-ion conductivity was measured for the sulfide solid electrolyte obtained in Comparative Example 1 and Comparative Example 2. Specifically, 100 mg of the sulfide solid electrolyte was weighed out in a glove box with a dew point of -80°C, placed in a Macol cylinder, and heated to 4 ton / cm. 2 The pellet was pressed at a pressure of 10 ...
[0074] (Exposure test) Example 1 , 3, 5, Reference examples 2, 4An exposure test was performed on the sulfide solid electrolyte obtained in Comparative Example 1 and Comparative Example 2. Specifically, the sulfide solid electrolyte was left to stand for 6 hours in a glove box in which the dew point was controlled at -30°C, and the sulfide solid electrolyte was exposed to moisture contained in the atmosphere. The Li-ion conductivity after the exposure test was measured in the same manner as above. The results are shown in Table 1 and FIG. 4.
[0075] [Table 1]
[0076] As shown in Table 1, when sintering was performed in a vacuum as in Comparative Example 1, Ge 2+ The proportion of Ge was 0%. In other words, all of the Ge present on the particle surface of the sulfide solid electrolyte was Ge. 4+ In contrast, in Example 1 , 3, 5, Reference examples 2, 4 So, both are Ge 2+ The proportion of the fluorine-containing fluoride was 20% or more. , 3, 5, Reference examples 2, 4 The Li ion conductivity after the exposure test was higher in Example 1 than in Comparative Example 1. 3 and Reference Examples 2 and 4 The Li ion conductivity after the exposure test was high, and in particular, Example 3 was the highest. Reference example 2 and Reference example It was suggested that there is a maximum value between 4.
[0077] In addition, from the viewpoint of the maintenance rate of Li-ion conductivity before and after the exposure test, Reference example 2 is higher than that of Example 1, Reference example 2 to Example 3 , 5 and Reference Example 4 was significantly increased. and reference examples Comparing Example 4 with Example 5, the Li ion conductivity after the exposure test was and reference examples 4 is higher than Example 5, and the retention rate of Li ion conductivity before and after the exposure test is Example 3. , 5 and Reference Example 4 The results were the same as in Example 1. , 3, 5, Reference examples 2, 4 From the results of Comparative Example 1, Ge 2+It is clear that the ratio of the sulfide to the sulfide solid electrolyte affects the water resistance of the sulfide solid electrolyte. Therefore, it was suggested that Example 5 was superior in terms of water resistance over time.
[0078] In addition, Example 1 , 3, 5 and Reference Examples 2, 4 We will consider the results in detail. First, Reference example 2 and Reference example 4. Nitrogen gas has a higher concentration of Ge than argon gas. 4+ Ge 2+ Nitrogen gas and argon gas are generally known to be gases with low reactivity, but the reduction power of Ge was confirmed to be weak when nitrogen gas was used and when argon gas was used. 2+ The unexpected result was that there was a large difference in the abundance ratio. The reason for this large difference is not entirely clear, but since nitrogen gas itself is classified as a neutral gas, it may have been less reactive than argon gas. In addition, since it is assumed that the sulfur contained in the precursor volatilizes during firing, it is assumed that some kind of interaction occurs between the volatilized sulfur and the nitrogen and argon gases, and that the large difference may have occurred depending on the strength of this interaction.
[0079] next, Reference example Comparing Example 2 and Example 1, the addition of oxygen gas, which is an oxidizing gas, to nitrogen gas increases the amount of Ge 4+ Ge 2+ It was confirmed that the reducing power of the Reference example Comparing Example 4 and Example 5, the addition of hydrogen gas, which is a reducing gas, to argon gas resulted in the formation of Ge 4+ Ge 2+ It was confirmed that the reduction power of Ge was enhanced by using an oxidizing gas and a reducing gas. 2+ It was confirmed that the ratio of Ge was controllable. Although no specific experiments were conducted, it was confirmed that Ge was 2+ It is expected that the proportion of Ge will be similar to that in Example 3. Similarly, when a reducing gas is added to nitrogen gas,2+ The proportion of the elements present is expected to be similar to that in Example 3.
[0080] Next, in Example 3, a first baking process was performed in which argon gas was made to flow, and a second baking process was performed in which nitrogen gas was made to flow. Reference example 4 as well as Ge 2+ The proportion of Ge is estimated to be 92%, but if a second firing process is performed after that, 2+ The proportion of Ge in the particles decreased to 77%. The reason for this is unclear, but it is thought that the amount of Ge diffused from inside the particles was 4+ The amount of Ge is 4+ From Ge 2+ It is possible that the amount of waste generated was greater than the amount of waste that was returned to the environment. [Explanation of symbols]
[0081] 1...Cathode active material layer 2...Negative electrode active material layer 3...Solid electrolyte layer 4...Positive electrode current collector 5...Negative electrode current collector 6. Battery case 10...All-solid-state battery
Claims
1. A sulfide solid electrolyte containing Li, Ge, P, and S and having an LGPS-type crystal phase, When X-ray photoelectron spectroscopy was performed on the surface of the sulfide solid electrolyte, the ratio of Ge to the total amount of Ge was 2+ The sulfide solid electrolyte,
2. A sulfide solid electrolyte containing Li, Ge, P, and S and having an LGPS-type crystal phase, When X-ray photoelectron spectroscopy was performed on the surface of the sulfide solid electrolyte, the ratio of Ge to the total amount of Ge was 2+ The sulfide solid electrolyte has a ratio of 94% or more.
3. The Ge 2+ The sulfide solid electrolyte according to claim 2, wherein the ratio of is 100%.
4. An all-solid-state battery having a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, An all-solid-state battery, wherein at least one of the positive electrode active material layer, the negative electrode active material layer, and the solid electrolyte layer contains the sulfide solid electrolyte according to any one of claims 1 to 3.
5. A method for producing a sulfide solid electrolyte containing Li, Ge, P, and S and having an LGPS-type crystal phase, comprising: When X-ray photoelectron spectroscopy is performed on the surface of the sulfide solid electrolyte, the ratio of Ge 2+ to the total amount of Ge is 20% or more, The manufacturing method includes: A preparation step of preparing a precursor containing Li, Ge, P, and S; a calcination step of calcining the precursor in an atmosphere of a gas containing at least one of nitrogen gas and a noble gas to form the LGPS-type crystal phase; having The method for producing a sulfide solid electrolyte, wherein the gas contains an oxidizing gas.
6. A method for producing a sulfide solid electrolyte containing Li, Ge, P, and S and having an LGPS-type crystal phase, comprising: When X-ray photoelectron spectroscopy is performed on the surface of the sulfide solid electrolyte, the ratio of Ge 2+ to the total amount of Ge is 20% or more, The manufacturing method includes: A preparation step of preparing a precursor containing Li, Ge, P, and S; a calcination step of calcining the precursor in an atmosphere of a gas containing at least one of nitrogen gas and a noble gas to form the LGPS-type crystal phase; having The method for producing a sulfide solid electrolyte, wherein the gas contains a reducing gas.
7. A method for producing a sulfide solid electrolyte containing Li, Ge, P, and S and having an LGPS-type crystal phase, comprising: When X-ray photoelectron spectroscopy is performed on the surface of the sulfide solid electrolyte, the ratio of Ge 2+ to the total amount of Ge is 20% or more, The manufacturing method includes: A preparation step of preparing a precursor containing Li, Ge, P, and S; a calcination step of calcining the precursor in an atmosphere of a gas containing at least one of nitrogen gas and a noble gas to form the LGPS-type crystal phase; having The firing step comprises: a first firing treatment in which the precursor is fired under an atmosphere of a first gas containing argon gas; A second firing treatment is performed in which the precursor after the first firing treatment is fired under an atmosphere of a second gas containing nitrogen gas; The present invention relates to a method for producing a sulfide solid electrolyte.
8. The method for producing a sulfide solid electrolyte according to any one of claims 5 to 7, wherein the precursor is a sulfide glass.
Citation Information
Patent Citations
Lithium solid electrolyte
JP2017021965A
Materials for solid electrolytes
JP2019501105A
Method of producing LGPS-based solid electrolyte
JP2020027780A
Production method for LGPS-based solid electrolyte
WO2018173939A1
Method for producing LGPS-based solid electrolyte
WO2019044517A1