Synthesis and Use of Precursors for the ALD of Molybdenum- or Tungsten-Containing Thin Films
The use of Mo or W β-diketonate precursors in ALD processes addresses the challenges of toxicity and instability in conventional precursors, enabling precise and impurity-free deposition of Mo or W thin films, particularly MoS2, for 2D materials in electronic devices.
Patent Information
- Application Number
- JP2023064038
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-06-17
- Filing Date
- 2023-04-11
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2036-05-24
AI Technical Summary
Conventional precursors for atomic layer deposition (ALD) of molybdenum and tungsten thin films are toxic, unstable, and require high temperatures, leading to impurities and difficulty in handling, while existing methods for molybdenum(III) β-diketonate synthesis are cumbersome and inefficient.
The development of Mo or W-containing thin films using ALD processes with Mo or W β-diketonate precursors, such as Mo(thd)3 and W(thd)3, which are handled in an inert atmosphere and reacted with chalcogen precursors like H2S to form stable thin films at controlled temperatures, ensuring precise deposition and minimizing impurities.
This method allows for the formation of high-quality, impurity-free Mo or W thin films, particularly MoS2, with controlled growth rates and crystalline structures, suitable for 2D materials in electronic devices.
Smart Images

Figure 0007578748000001 
Figure 0007578748000002 
Figure 0007578748000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority under 35 U.S.C. §119 to U.S. Provisional Patent Application No. 62 / 167,220, filed May 27, 2015, and U.S. Provisional Patent Application No. 62 / 167,220, filed June 17, 2015, the entire contents of which are incorporated herein by reference.
[0002] Parties to the Joint Research Agreement The invention claimed in this application was made by, for, and / or in connection with a Joint Research Agreement between the University of Helsinki and ASM Microchemistry Oy, which was in effect on or before the date the claimed invention was made, and which was made as a result of activities undertaken within the scope of the Agreement. [Background technology]
[0003] This application relates generally to precursors and methods for forming thin films comprising molybdenum or tungsten by atomic layer deposition. Such films may find use, for example, as two-dimensional (2D) materials in electronic devices.
[0004] Related Technology Conventional processes for atomic layer deposition (ALD) of any type of thin film containing molybdenum rely on a select few known molybdenum precursors, such as MoCl5, Mo(CO)6, and Mo(N t Bu)2(NMe2)2 and Mo(N tPreviously, the deposition of MoS2 thin films has been limited to alkylamine precursors such as Mo(CO)6 and H2S, Mo(CO)6 and MeSSMe, and MoCl5 and H2S. However, these traditional molybdenum precursors may prove difficult to handle. For example, Mo(CO)6 is a highly toxic substance with a narrow deposition temperature range that would be too low to deposit crystalline thin films containing molybdenum. On the other hand, MoCl5 may require additional residence time to successfully deposit MoS2 films.
[0005] Some Mo alkylamine precursors may contain Mo with +VI oxidation state, which may cause problems during deposition of any type of thin film containing molybdenum. Mo alkylamine precursors with Mo's more preferred +IV oxidation state are generally unstable and difficult to use. In addition, Mo alkylamine precursors are relatively temperature sensitive and decompose at low temperatures. This may cause decomposition of Mo alkylamine precursors, since relatively high temperatures are usually required to promote the growth of crystalline films. This decomposition may produce impurities such as carbon, which may delay or even prevent the crystallization of any type of thin film containing molybdenum.
[0006] Molybdenum(III) β-diketonates have been utilized to deposit Mo-containing thin films using chemical vapor deposition (CVD) processes, but their use in ALD-type processes has not been extensively studied. Previously disclosed synthesis processes for molybdenum(III) β-diketonates use Mo(CO)6, K3MoCl6, and (NH4)2[MoCl5(H2O)]. Each of these compounds has significant drawbacks and can prove difficult to handle. For example, as discussed above, Mo(CO)6 is highly toxic and volatile, adding to the difficulties of the procedures used. Laboratory synthesis of K3MoCl6 is difficult and requires electrochemical or high temperature processes.
[0007] Transition metal dichalcogenide materials, especially 2D transition metal dichalcogenides such as Mo and W dichalcogenides, have desirable electrical properties for a variety of applications. Furthermore, unlike another 2D material, graphene, some 2D transition metal dichalcogenides have a direct band gap and are semiconducting. Therefore, 2D transition metal dichalcogenides such as Mo and W dichalcogenides are being explored for device miniaturization applications. Summary of the Invention
[0008] In some aspects, a process for forming a Mo or W-containing thin film is provided. In some embodiments, a Mo or W-containing thin film is formed on a substrate in a reaction chamber in a process that includes at least one cycle. The cycle includes contacting the substrate with a gas-phase Mo or W precursor such that up to a first monolayer of Mo or W precursor is formed on the substrate surface, removing excess Mo or W precursor and reaction by-products, if any, contacting the substrate with a gas-phase chalcogen precursor, removing excess chalcogen precursor and reaction by-products, if any, and optionally repeating the contacting and removing steps until a Mo or W-containing thin film of a desired thickness is formed. In some embodiments, Mo or W in the Mo or W precursor has an oxidation state of +IV or less but not 0. In some embodiments, the chalcogen precursor reacts with the Mo or W precursor on the substrate surface.
[0009] In some embodiments, the process is an atomic layer deposition (ALD) process. In some embodiments, the process includes two or more successive cycles. In some embodiments, the Mo or W-containing thin film is a Mo or W sulfide, selenide, or telluride thin film. In some embodiments, the oxidation state of Mo or W in the Mo or W precursor is +III. In some embodiments, the chalcogen precursor includes H2S, H2Se, H2Te, (CH3)2S, (CH3)2Se, or (CH3)2TSe.
[0010] In some aspects, an atomic layer deposition (ALD) process for forming Mo or W sulfide, selenide, or telluride thin films is provided. According to some embodiments, Mo or W sulfide, selenide, or telluride thin films are formed on a substrate in a reaction chamber in an ALD process that includes at least one cycle. The cycle includes contacting the substrate with a gas-phase Mo or W precursor such that up to a first monolayer of Mo or W precursor is formed on the substrate surface, removing excess Mo or W precursor and reaction by-products, if any, contacting the substrate with a gas-phase chalcogen precursor, removing excess chalcogen precursor and reaction by-products, if any, and repeating the contacting and removing steps until a Mo or W-containing thin film of a desired thickness is formed. In some embodiments, the Mo or W precursor may include at least one bidentate ligand. In some embodiments, the chalcogen precursor reacts with the Mo or W precursor on the substrate surface.
[0011] In some embodiments, the bidentate ligand is bonded to the Mo or W atom through an O, S, or N atom. In some embodiments, the bidentate ligand is bonded to the Mo or W atom through two O atoms. In some embodiments, the bidentate ligand is bonded to the Mo or W atom through an O atom and an N atom. In some embodiments, the bidentate ligand is bonded to the Mo or W atom through two N atoms. In some embodiments, the bidentate ligand is a β-diketonato ligand. In some embodiments, the β-diketonato ligand is an acetylacetonato (acac) ligand. In some embodiments, the β-diketonato ligand is a 2,2,6,6-tetramethyl-3,5-heptanedionato (thd) ligand. In some embodiments, the Mo or W precursor comprises at least two bidentate ligands. In some embodiments, the Mo or W precursor comprises three bidentate ligands.
[0012] In some aspects, an atomic layer deposition (ALD) process for forming Mo or W sulfide, selenide, or telluride 2D materials is provided. According to some embodiments, the Mo or W sulfide, selenide, or telluride 2D materials are formed on a substrate in a reaction chamber in an ALD process that includes at least one cycle. The cycle includes contacting the substrate with a gas-phase Mo or W precursor such that up to a first monolayer of the Mo or W precursor is formed on the substrate surface, removing excess Mo or W precursor and reaction by-products, if any, contacting the substrate with a gas-phase sulfur, selenium, or tellurium precursor, and removing excess sulfur, tellurium, or selenium precursor and reaction by-products, if any. In some embodiments, the Mo or W precursor is a Mo or W β-diketonate precursor. In some embodiments, the sulfur, selenium, or tellurium precursor reacts with the Mo or W precursor on the substrate surface.
[0013] In some aspects, a process for forming Mo or W sulfide, selenide, or telluride 2D materials is provided. According to some embodiments, Mo or W sulfide, selenide, or telluride 2D materials are formed on a substrate in a reaction chamber in a cyclic process including at least one cycle. The cycle includes contacting the substrate with a gas-phase Mo or W precursor such that a maximum of a monolayer of Mo or W-containing material is formed on the substrate surface, preferably about 50% or less of the monolayer, preferably about 25% or less of the monolayer, more preferably less than about 10% of the monolayer; exposing the substrate to a purge gas; and / or removing excess Mo or W precursor and reaction by-products, if any; contacting the substrate with a gas-phase sulfur, selenium, or tellurium precursor; exposing the substrate to a purge gas; and / or removing excess sulfur, tellurium, or selenium precursor and reaction by-products, if any. In some embodiments, the Mo or W precursor is a Mo or W β-diketonate precursor. In some embodiments, the sulfur, selenium or tellurium precursor reacts with a Mo or W containing material deposited on the substrate surface.
[0014] In some embodiments, the Mo or W-containing thin film is a Mo or W sulfide, selenide, or telluride thin film. In some embodiments, the oxidation state of the Mo or W atoms comprising the Mo or W precursor is +III. In some embodiments, the chalcogen precursor comprises H2S, H2Se, H2Te, (CH3)2S, (CH3)2Se, or (CH3)2Te. In some embodiments, the Mo or W precursor is Mo(thd)3 and the chalcogen precursor is H2S. In some embodiments, the Mo or W precursor is W(thd)3 and the chalcogen precursor is H2S. In some embodiments, the 2D material comprises MoS2.
[0015] In some aspects, a method for making Mo or W β-diketonate precursor is provided. According to some embodiments, the Mo or W β-diketonate precursor is formed by providing a first reactant having the formula MX3(R)n3, where n is a number between 0 and 4, M is Mo or W, X is a halide, and R is a solvent, reacting an alkali metal compound with a β-diketonate compound to form a first product, and then adding the first product to the first reactant. In some embodiments, the Mo or W β-diketonate precursor is formed having the formula ML3, where M is Mo or W, and L is a β-diketonate ligand.
[0016] In some embodiments, providing the first reactant may further include reducing a Mo or W halide with a reducing agent to form a first intermediate product, and then adding a solvent to the first product to form a second intermediate product, thereby forming the first reactant. In some embodiments, the Mo or W halide is MoCl5, the β-diketone compound is Hthd, and the formed Mo or W β-diketonate precursor is Mo(thd)3.
[0017] In some aspects, a method for forming a Mo or W β-diketonate compound is provided. According to some embodiments, the Mo or W β-diketonate compound is formed by providing a first reactant having the formula MX3(R)n3, where n is a number between 0 and 4, M is Mo or W, X is a halide, and R is a solvent, reacting an alkali metal compound with the β-diketonate compound to form a first product, and then reacting the first product with the first reactant. In some embodiments, a Mo or W β-diketonate compound is formed having the formula ML3, where M is Mo or W with an oxidation state of +III and L is a β-diketonate ligand. In some embodiments, the Mo or W in the Mo or W β-diketonate compound has an oxidation state of +III.
[0018] In some aspects, a process for forming a Mo or W containing material is provided. According to some embodiments, the Mo or W containing material is formed on a substrate in a reaction chamber in a process that includes at least one deposition cycle, the cycle including alternately and sequentially contacting the substrate with a gas phase Mo or W precursor and a second gas phase chalcogen precursor. In some embodiments, the Mo or W in the Mo or W precursor has an oxidation state that is equal to or lower than +IV but not equal to 0.
[0019] In some embodiments, the deposition is repeated two or more times. In some embodiments, excess Mo or W precursor and reaction by-products, if any, are removed after contacting the substrate with the gas-phase Mo or W precursor and before contacting the substrate with the gas-phase chalcogen precursor. In some embodiments, excess chalcogen precursor and reaction by-products, if any, are removed after contacting the substrate with the gas-phase chalcogen precursor and before starting another deposition cycle. In some embodiments, the substrate is contacted with a purge gas after contacting the substrate with the Mo or W gas-phase precursor and before contacting the substrate with the gas-phase chalcogen precursor. In some embodiments, the substrate is contacted with a purge gas after contacting the substrate with the chalcogen gas-phase precursor and before starting another deposition cycle. In some embodiments, the Mo or W containing material comprises elemental Mo or W. In some embodiments, the Mo or W containing material comprises an oxide material of Mo or W. In some embodiments, the Mo or W containing material comprises a nitride material of Mo or W. In some embodiments, the Mo or W containing material comprises a silicide material of Mo or W. [Brief description of the drawings]
[0020] The invention will be better understood from the detailed description and from the accompanying drawings which are intended to illustrate, but not to limit, the invention.
[0021] [Figure 1] FIG. 1 is a process flow diagram generally illustrating a method for depositing Mo- or W-containing thin films. [Diagram 2] FIG. 1 is a process flow diagram generally illustrating a method for synthesizing a metal β-diketonate precursor. [Diagram 3] 1 is a mass spectrum of a sample of Mo(thd)3 synthesized according to the procedures described herein. [Figure 4] Illustrates the molecular structure of Mo(thd)3 as determined by single crystal X-ray diffraction. [Diagram 5] Illustrates thermogravimetric curves of Mo(acac)3, Mo(hfac)3, and Mo(thd)3. [Figure 6] This is a field emission scanning electron microscope (FESEM) image of a MoS2 thin film. [Figure 7] 1 is a graph of MoS2 thin film growth rate per cycle versus Mo(thd)3 and H2S precursor pulse length. [Figure 8] 1 is a graph of film thickness versus number of film formation cycles. [Figure 9] A series of field emission scanning electron microscope (FESEM) images of MoS2 thin films deposited at 500 °C using various Mo(thd)3 precursor pulse lengths. [Figure 10] A series of field emission scanning electron microscope (FESEM) images of MoS2 thin films deposited at 500 °C using various H2S precursor pulse lengths. [Figure 11A] A series of field emission scanning electron microscope (FESEM) images of MoS2 thin films deposited at 500 °C through 10–50 deposition cycles. [Figure 11B] A series of field emission scanning electron microscope (FESEM) images of MoS2 thin films deposited at 500℃ through 100 to 2000 deposition cycles. [Figure 12A] 1 is a graph of the composition of MoS2 thin films deposited with varying Mo(thd)3 precursor pulse lengths as measured by energy dispersive X-ray (EDX) analysis. [Figure 12B] 1 is a graph of the composition of MoS 2 thin films deposited with varying H 2 S precursor pulse length as measured by energy dispersive X-ray (EDX) analysis. [Figure 13] The following shows an example of MoS2 film thickness versus the number of film-forming cycles, and the Mo and S element fraction versus the number of film-forming cycles. [Figure 14] Figure 1 shows grazing incidence X-ray diffraction (GIXRD) patterns of MoS2 thin films deposited with various chalcogen and Mo precursor pulse lengths. [Figure 15] This is a Raman spectrum of a MoS2 thin film. [Figure 16] 13 illustrates Raman spectra of MoS2 thin films deposited with various chalcogen and Mo precursor pulse lengths. [Figure 17] Illustrates the elemental composition of two MoS2 thin films analyzed by X-ray photoelectron spectroscopy (XPS). [Figure 18] 1 illustrates the surface roughness of MoS2 thin films analyzed using an atomic force microscope (AFM). [Figure 19] The growth rate of MoS2 thin films and the element ratio of Mo and S versus deposition temperature are illustrated. [Figure 20] A series of field emission scanning electron microscope (FESEM) images of MoS2 thin films deposited at 350℃~500℃. [Figure 21] AC-STEM image of a thin MoS2 film deposited on a silicon substrate containing native oxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] As described below, Mo and W containing thin films can be deposited on substrates by atomic layer deposition (ALD) type processes. In some embodiments, Mo or W chalcogenide thin films, particularly Mo or W sulfide or selenide thin films, can be deposited on substrates by ALD type processes. ALD type processes are based on controlled surface reactions of precursor chemicals. Gas phase reactions are avoided by contacting the substrate with precursors alternately and sequentially. Gas phase reactants are separated from each other on the substrate surface, for example, by removing excess reactant and / or reactant by-products from the reaction chamber between reactant pulses.
[0023] Suitable substrate materials may include insulating materials, dielectric materials, crystalline materials, epitaxial, heteroepitaxial, or single crystal materials such as oxides. For example, the substrate may include insulating nitrides such as A12O3, sapphire, silicon oxide, or AlN. Additionally, the substrate material and / or substrate surface may be selected by one skilled in the art to enhance, increase, or maximize two-dimensional crystal growth thereon. In some embodiments, the substrate surface on which the Mo and W containing thin film or material is deposited does not include semiconductor materials such as Si, Ge, III-V compounds, e.g., GaAs and InGaAs, and II-VI compounds. In some embodiments, the substrate surface on which the Mo and W containing thin film or material is deposited may include materials other than insulating materials. In some embodiments, after deposition of the Mo or W containing thin film, the Mo and W containing thin film is removed from at least a portion of the substrate that includes materials other than insulating materials. In some embodiments, the substrate surface onto which the Mo- and W-containing thin film or material, preferably a Mo or W-chalcogenide thin film or material, is deposited comprises a chalcogen, such as sulfur, selenium, or tellurium, most preferably sulfur. In some embodiments, the substrate surface onto which the Mo- and W-containing thin film or material is deposited comprises surface groups that include a chalcogen, preferably surface groups that have a chalcogen-hydrogen bond, such as -SH groups.
[0024] In summary, the substrate is heated to a suitable deposition temperature, typically under reduced pressure. The deposition temperature is typically maintained below the thermal decomposition temperature of the reactants, but at a high enough level to avoid condensation of the reactants and provide activation energy for the desired surface reaction. Of course, the appropriate temperature window for any given ALD reaction depends on the surface termination and reactant species involved. Here, the temperature varies depending on the type of film being deposited and the particular precursor, but is preferably about 650°C or less, more preferably less than about 500°C. The temperature window is preferably about 250°C to about 600°C, more preferably about 350°C to about 550°C, and most preferably about 375°C to about 500°C. In some cases, the reaction temperature is greater than about 250°C, preferably greater than about 350°C, and most preferably greater than about 375°C.
[0025] In some embodiments, the deposition temperature may be above the decomposition temperature of the reactants, but low enough to maintain reasonably surface-controlled growth of the film and a growth rate of about one monolayer of material or less per deposition cycle. In some embodiments, the deposition cycle growth rate can be about 50% or less, preferably less than about 25%, and more preferably less than about 10%, of about one monolayer of material deposited per cycle.
[0026] In some embodiments, the deposition process may not be a pure ALD process. In some embodiments, the chalcogen precursor may flow continuously or substantially continuously through the reaction space during the deposition process. For example, the flow rate of the chalcogen precursor through the reaction space may be reduced while the substrate is in contact with the metal precursor. In some embodiments, the chalcogen precursor may flow continuously, the growth rate of the film per pulse of the metal precursor is about one monolayer or less of the material being deposited. In some embodiments, where the chalcogen precursor flows continuously, the growth rate of the film per pulse of the metal precursor is about 50% or less of a monolayer of the material being deposited, preferably less than about 25%, more preferably less than about 10%.
[0027] In some embodiments, the growth rate of the Mo and W containing thin film is less than about 2 Å / cycle, less than about 1.5 Å / cycle, less than about 1 Å / cycle, or even less than about 0.5 Å / cycle. In some embodiments, the growth rate of the Mo and W containing dichalcogenide thin film can be from about 0.025 Å / cycle to about 0.5 Å / cycle. In other embodiments, the growth rate of the Mo and W containing dichalcogenide thin film, such as a MoS2 thin film, is from about 0.05 Å / cycle to about 0.3 Å / cycle.
[0028] In some embodiments, a pretreatment process can be performed on the substrate surface. In some embodiments, the pretreatment process includes exposing the substrate to a pretreatment reactant, either in situ or ex situ, prior to deposition of the Mo or W-containing thin film. In some embodiments, the pretreatment process can include exposing the substrate surface to at least one of the following pretreatment reactants: (NH4)2S, H2S, HCl, HBr, Cl2, and HF. In some embodiments, the pretreatment process can include exposing the substrate surface to a plasma, atoms, or radicals. In some embodiments, the pretreatment process can include exposing the substrate surface to a chalcogen-containing plasma, atoms, or radicals, such as sulfur, selenium, or tellurium, preferably a sulfur-containing plasma, atoms, or radicals. In some embodiments, the plasma, atoms, or radicals can include tellurium. In some embodiments, the plasma, atoms, or radicals can include selenium. In some embodiments, the pretreatment process can include exposing the substrate surface to a chalcogen-containing plasma, atoms, or radicals present in the subsequent deposition process. In some embodiments, the pretreatment process may include exposing the substrate surface to a plasma, atoms, or radicals formed from a chalcogen compound containing chalcogen-hydrogen bonds, such as a plasma, atoms, or radicals formed from H2S. In some embodiments, the pretreatment process may include exposing the substrate surface to at least one pretreatment reactant for about 1 second to about 600 seconds, preferably about 1 second to about 60 seconds. The pretreatment process may utilize a pretreatment reactant in vapor and / or liquid form. In some embodiments, the pretreatment process may be performed at the same temperature and / or pressure as the subsequent deposition process. In some embodiments, the pretreatment process may be similar to the subsequent deposition process, except that the pretreatment process requires a longer pulse or exposure time than is used in the subsequent deposition process. In some embodiments, the pretreatment process may include exposing the substrate surface to a pretreatment reactant to form a desired surface termination, such as an -SH surface termination. In some embodiments, forming a desired surface termination, such as an -SH surface termination, may promote two-dimensional growth of Mo- or W-containing thin films or materials.In some embodiments, the pretreatment process may include exposing the substrate to a plasma, atoms, or radicals that are free of S, Se, and Te, such as a plasma, atoms, or radicals that include hydrogen, such as a plasma formed from H2. In some embodiments, the pretreatment process may include exposing the substrate to an oxygen plasma, oxygen atoms, or oxygen radicals. In some embodiments, the pretreatment process may include exposing the substrate, such as a substrate that includes AlN, to a nitrogen plasma, nitrogen atoms, or nitrogen radicals. In some embodiments, the pretreatment process may be used to clean the substrate surface prior to deposition of a Mo- or W-containing thin film or material.
[0029] The substrate surface is contacted with the first reactant in the gas phase. In some embodiments, a pulse of the first reactant in the gas phase is provided to a reaction space containing the substrate. In some embodiments, the substrate is moved into a reaction space containing the first reactant in the gas phase. Preferably, conditions are selected such that about one or less monolayers of the first reactant are adsorbed on the substrate surface in a self-limiting manner. Appropriate contact times can be readily determined by one of skill in the art based on the particular circumstances. Excess first reactant and reaction by-products, if any, are removed from the substrate surface by purging with an inert gas or by removing the substrate from the presence of the first reactant.
[0030] Purging refers to removing gas phase precursor material and / or gas phase by-products from the substrate surface by evacuating the chamber using a vacuum pump and / or replacing the gas in the reactor with an inert gas such as argon or nitrogen. Typical purge times are about 0.05 to 20 seconds, more preferably about 0.2 to 10 seconds, and even more preferably about 0.5 to 5 seconds. However, other purge times can be utilized as needed, such as when very high aspect ratio structures or other structures with complex surface morphology are required, or when a high degree of conformal step coverage is required, or when a different reactor type is used, such as a batch reactor.
[0031] The substrate surface is contacted with the second gaseous reactant in the gas phase. In some embodiments, pulses of the second gaseous reactant are provided to the reaction space containing the substrate. The second gaseous reactant in the gas phase may be provided in the reaction chamber in a substantially continuous flow from the inlet to the outlet of the reaction chamber. In some embodiments, the outlet flow from the reaction chamber, e.g., the pump line, is not closed. In some embodiments, the outlet flow from the reaction chamber, e.g., the flow from the reaction chamber to the pump line and also through the pump line prior to the pump, is not substantially closed but may be restricted. In some embodiments, the substrate is moved to the reaction space containing the second reactant in the gas phase. Any excess second reactant and gaseous by-products of the surface reaction are removed from the substrate surface. In some embodiments, there is no residence time of the reactants. In some embodiments, the reactants in the gas phase are not static in the reaction space, and the reactants in the gas phase are in contact with the substrate. The reactants in the gas phase may be static if the reactants are not flowing relative to the substrate or if the reactants are flowing from one inlet into a reaction space with no open outlet.
[0032] The contacting and removing steps are repeated until a thin film of a desired thickness is selectively formed on the substrate, with each cycle depositing about a monolayer or less. The contacting and removing steps of the first gas phase Mo or W precursor can be referred to as the first precursor phase, the Mo or W precursor phase, or the Mo or W phase. The contacting and removing steps of the second gas phase precursor can be referred to as the second precursor phase, the chalcogen precursor phase, or the chalcogen phase. Together, these two phases can constitute a deposition cycle. Additional phases can be added, including alternating and sequential contact of the substrate surface with other reactants, to form more complex materials, such as ternary materials.
[0033] As mentioned above, each step of each cycle is preferably self-limiting. An excess of reactant precursor is provided at each step to saturate the structure surface undergoing reaction. Surface saturation ensures reactant occupation of all available reactive sites (subject to, for example, physical size or "steric hindrance" limitations), thus ensuring excellent step coverage and uniformity. Typically, less than one molecular layer of material is deposited in each cycle, although in some embodiments, more than one molecular layer is deposited during a cycle.
[0034] Removing excess reactants may include evacuating a portion of the contents of the reaction space and / or purging the reaction space with helium, nitrogen, or other inert gas. In some embodiments, purging may include stopping the flow of reactive gases while continuing to flow an inert carrier gas through the reaction space.
[0035] The precursors used in ALD type processes may be solid, liquid or gaseous materials under standard conditions (room temperature and atmospheric pressure), provided that the precursor is in the gas phase before contacting the substrate surface. Contacting the substrate surface with the vaporized precursor means that the precursor vapor is in contact with the substrate surface for a predetermined time. Typically, the contact time is about 0.05-20 seconds, more preferably about 0.2-10 seconds, and even more preferably about 0.5-5 seconds. In some embodiments, the second gas contact time in the gas phase is preferably on the same order of length as the first gas reactant contact time in the gas phase. In some embodiments, the second gas contact time in the gas phase is preferably about 100 times or less longer than the first gas reactant contact time in the gas phase.
[0036] However, depending on the type of substrate and its surface area, the contact time may be even longer than 20 seconds. The contact time may be on the order of a few minutes in some cases. Those skilled in the art can determine the optimal contact time based on the particular situation. In some embodiments, the contact time of the chalcogen precursor is less than about 60 seconds, preferably less than about 30 seconds, more preferably less than about 10 seconds, and most preferably less than about 5 seconds.
[0037] One skilled in the art can also determine the mass flow rate of the precursors. In some embodiments, the flow rate of the Mo or W precursor is preferably about 1-1000 sccm, more preferably about 100-500 sccm.
[0038] The pressure in the reaction chamber is typically from about 0.01 to about 50 mbar, more preferably from about 0.1 to about 10 mbar, although in some cases the pressure will be higher or lower than this range, as can be determined by one of skill in the art given the particular circumstances.
[0039] Before starting the deposition of the film, the substrate is typically heated to a suitable growth temperature. The growth temperature varies depending on the type of thin film to be formed, the physical properties of the precursor, etc. The growth temperature is preferably about 650°C or less, more preferably about 500°C or less. The growth temperature window is preferably about 250°C to about 600°C, more preferably about 350°C to about 550°C, and most preferably about 375°C to about 500°C. In some cases, the growth temperature is higher than about 250°C, preferably higher than about 350°C, and most preferably higher than about 375°C. The growth temperature can be below the crystallization temperature of the deposition material so that an amorphous thin film is formed, or it can be above the crystallization temperature so that a crystalline thin film is formed. The preferred deposition temperature can vary depending on many factors, including but not limited to the composition of the substrate, including the reactant precursors, pressure, flow rate, reactor configuration, crystallization temperature of the deposited thin film, and the nature of the material to be deposited. Those skilled in the art can select a particular growth temperature. It should be noted that the thermal budget, i.e., the reaction temperature and optionally the annealing temperature during deposition and at any point in further processing after deposition of the film of the present invention, is preferably less than about 800°C, more preferably less than about 650°C, most preferably less than about 600°C, and optionally less than about 500°C.
[0040] In some embodiments, the deposited Mo or W-containing thin film can be subjected to an optional post-deposition treatment process. In some embodiments, for example, the post-deposition treatment process can include an annealing process, such as a forming gas annealing process. In some embodiments, the post-deposition treatment process can include exposing the Mo or W-containing thin film or material surface to a plasma. In some other embodiments, the post-deposition treatment process does not include exposing the Mo or W-containing thin film or material surface to a plasma.
[0041] In some embodiments, the post-deposition treatment process may include exposing the deposited Mo or W-containing thin film or material to a post-deposition treatment reactant, either in situ or ex situ. In some embodiments, the post-deposition treatment process may include exposing the Mo or W-containing thin film or material surface to at least one of the following post-deposition treatment reactants: (NH4)2S or H2S. In some embodiments, the post-deposition treatment process may include exposing the Mo or W-containing thin film or material to a chalcogen-containing plasma, such as a sulfur-containing plasma. In some embodiments, the post-deposition treatment process may include exposing the Mo or W-containing thin film or material to a plasma formed from a chalcogen compound containing a chalcogen-hydrogen bond, such as a plasma formed from H2S. In some embodiments, the post-deposition treatment process may include exposing the Mo or W-containing thin film or material to a chalcogen-containing plasma, such as a sulfur-containing plasma. In some embodiments, the post-deposition treatment process may include exposing the Mo- or W-containing thin film or material to at least one post-deposition treatment reactant for about 1 second to about 600 seconds, preferably about 1 second to about 60 seconds. The post-deposition treatment process may utilize the post-deposition treatment reactant in vapor and / or liquid form. In some embodiments, the post-deposition treatment process may be performed at about the same temperature and / or pressure as the subsequent deposition process. In some embodiments, the post-deposition treatment process may be similar to the previous deposition process, except that it requires a longer pulse or exposure time than used in the previous deposition process. In some embodiments, the post-deposition treatment process includes exposing the Mo- or W-containing thin film or material to a plasma including hydrogen, atoms, or radicals, such as a plasma formed from H2.
[0042] Examples of suitable reactors that may be used include commercially available ALD equipment, such as the F-120® reactor, Eagle® XP8, Pulsar® reactor, and Advance® 400 Series reactors available from ASM America, Inc., Phoenix, Arizona; ASM Japan KK, Tokyo, Japan; and Almere ASM Europe BV, The Netherlands. In addition to these ALD reactors, many other types of reactors capable of ALD growth of thin films can be used, including CVD reactors with appropriate equipment and means for pulsing precursors. In some embodiments, a flow-type ALD reactor is used. Preferably, the reactants are kept separate until they reach the reaction chamber, such that shared lines for the precursors are minimized. However, other configurations are possible, such as the use of a pre-reaction chamber as described in U.S. Patent Application Nos. 10 / 929,348, filed August 30, 2004, and 09 / 836,674, filed April 16, 2001, the disclosures of which are incorporated herein by reference.
[0043] In some embodiments, a suitable reactor may be a batch reactor and may contain greater than about 25 substrates, greater than about 50 substrates, or greater than about 100 substrates. In some embodiments, a suitable reactor may be a mini-batch reactor and may contain from about 2 to about 20 substrates, from about 3 to about 15 substrates, or from about 4 to about 10 substrates.
[0044] The growth process can optionally be carried out in reactors or reaction spaces connected to a cluster tool, where each reaction space is dedicated to one type of process, so the temperature of the reaction space in each module can be kept constant, improving throughput compared to reactors where the substrate is heated to the process temperature before each run.
[0045] A stand-alone reactor is equipped with a load lock, in which case there is no need to cool the reaction space between each run.
[0046] According to a preferred embodiment, as shown in FIG. 1, a Mo or W-containing thin film is formed on a substrate by an ALD-type process including at least one deposition cycle 10, the deposition cycle comprising:
[0047] In step 12, contacting the substrate surface with a vaporized Mo or W precursor to form up to a monolayer of the Mo or W precursor on the substrate; In step 13, removing excess Mo or W precursor and reaction by-products, if any, from the surface; In step 14, contacting the substrate surface with a vaporized chalcogen precursor; Step 15 includes removing excess chalcogen precursor and any gaseous by-products formed in the reaction between the Mo or W precursor layer and the chalcogen precursor from the surface.
[0048] The contacting and removing steps 16 can be repeated until a Mo- or W-containing thin film of the desired thickness is formed.
[0049] Although the illustrated deposition cycle begins with contacting the substrate surface with a Mo or W precursor, in other embodiments, the deposition cycle begins with contacting the substrate surface with a chalcogen precursor. Those skilled in the art will appreciate that if the substrate surface is contacted with a first precursor and the precursor does not react, the process begins when the next precursor is provided. In some embodiments, reactants and reaction by-products can be removed from the substrate surface by stopping the flow of the Mo or W precursor while continuing to flow an inert carrier gas such as nitrogen or argon.
[0050] In some embodiments, reactants and reaction by-products can be removed from the substrate surface by stopping the flow of the second reactant while continuing to flow the inert carrier gas. In some embodiments, the substrate is moved so that different reactants alternately and sequentially contact the substrate surface in a desired order for a desired time. In some embodiments, no removing step is performed. In some embodiments, reactants may not be removed from various parts of the chamber. In some embodiments, the substrate is moved from one part of the chamber containing the first precursor to another part of the chamber containing the second precursor. In some embodiments, the substrate is moved from a first reaction chamber to a second, different reaction chamber.
[0051] In some embodiments, the deposited Mo or W-containing film may include a dichalcogenide thin film. In some embodiments, the deposited thin film may include a molybdenum dichalcogenide or a tungsten dichalcogenide. In some embodiments, the deposited thin film may include MoS2, WS2, MoSe2, WSe2, MoTe2, or WTe2. For simplicity, these dichalcogenides are represented as having their general stoichiometry. However, it will be understood that the exact stoichiometry of any Mo or W-containing film or material will vary based on the oxidation state of the elements involved. Thus, other stoichiometries are expressly contemplated.
[0052] The term "dichalcogenides" is used herein and these dichalcogenides are shown to have a typical stoichiometry of 1:2 ratio of metal atoms, such as Mo or W, to chalcogen atoms, such as S, Se, or Te, although the stoichiometry of the film may vary. For example, the ratio of metal atoms to chalcogen atoms may vary depending on the analytical technique and / or process conditions used. In some embodiments, the ratio of metal atoms to chalcogen atoms may be about 1:3 to about 2:1, preferably about 1:2.5 to about 1:1, more preferably about 1:2. In some embodiments, the dichalcogenide film may include about 20 at% to about 50 at%, preferably about 25 at% to about 40 at% Mo or W. In some embodiments, the dichalcogenide film may include about 30 at% to about 75 at%, preferably about 35 at% to about 70 at% chalcogen (S, Se, or Te).
[0053] In some embodiments, the Mo or W-containing dichalcogenide film may contain less than about 35 at% in total, and more preferably less than about 25 at% in total, of elements other than Mo, W, and chalcogens, preferably Mo, W, and elements other than chalcogens, including hydrogen. In some embodiments, the film may contain less than about 20 at% carbon, preferably less than about 15 at% carbon, and most preferably less than about 10 at% carbon. In some embodiments, the film may contain less than about 15 at% hydrogen, preferably less than about 10 at% hydrogen, and most preferably less than about 5 at% hydrogen. In some embodiments, the film may contain less than about 10 at% oxygen, preferably less than about 5 at% oxygen, and most preferably less than about 3 at% oxygen. In some embodiments, the film may contain less than about 10 at% elements other than Mo or W, chalcogens, hydrogen, carbon, or oxygen, preferably less than about 5 at% and most preferably less than about 3 at%. It is noted that the Mo or W-containing film containing the above elements is also suitable for different applications, such as 2D materials.
[0054] In some embodiments, the deposited Mo or W containing films are described herein as including Mo or W for simplicity, but may include both Mo and W. In some embodiments, the deposited Mo or W containing films may include additional elements other than Mo, W, chalcogens (S, Te, or Se), oxygen, nitrogen, or silicon. In some embodiments, the deposited Mo or W containing films may include dopants. In some embodiments, the deposited Mo or W containing films may include two or more elements from the group of chalcogens (S, Te, or Se), oxygen, nitrogen, or silicon. In some embodiments, the deposited Mo or W chalcogenide containing films may include two or more elements from the group of chalcogens (S, Te, or Se). In some embodiments, the thin films of the present disclosure may include any number of metals. According to some embodiments, the Mo or W containing films may include two or more metals. In some embodiments, additional deposition phases are added to one or more deposition cycles to incorporate additional metal or metals into the Mo or W containing thin films. The additional metal phase or metal phases may follow the first metal phase, or may follow the chalcogen phase, or may follow both phases. In some embodiments, two or more different metal precursors may be simultaneously delivered to the same metal phase of a deposition cycle. In some embodiments, metal precursors containing different metals may be used in different deposition cycles. For example, a first metal precursor may be the only metal precursor used in one or more deposition cycles, and a second metal precursor containing a second, different metal may be used in one or more other deposition cycles.
[0055] Referring again to FIG. 1, some embodiments may include an optional pretreatment process in step 11 applied to the substrate surface. The pretreatment process may include one or more steps. In the pretreatment, the substrate surface on which the Mo or W-containing thin film is to be deposited may be exposed to one or more pretreatment reactants and / or specific conditions, such as temperature or pressure. Pretreatment may be used for a number of reasons, including cleaning the substrate surface, removing impurities, removing native oxides, and providing a desired surface termination. In some embodiments, the pretreatment includes exposing the substrate surface to one or more pretreatment reactants, such as (NH4)2S, H2S, HCl, HBr, Cl2, or HF. In some embodiments, the pretreatment process is performed at approximately the same temperature as the subsequent deposition process.
[0056] Many different precursors can be used to deposit Mo or W containing thin films, as described below. Preferably, the Mo or W precursor has the formula M(thd)3, where M is one of Mo or W, and thd is 2,2,6,6-tetramethyl-3,5-heptanedionato. Preferably, the chalcogen precursor is either H2S or H2Se. In a preferred embodiment, the Mo or W precursor is Mo(thd)3, the chalcogen precursor is H2S, and the resulting Mo or W containing thin film is a MoS2 thin film.
[0057] In some embodiments, the MoS thin film is formed on a substrate by an ALD type process that includes at least one deposition cycle, the at least one deposition cycle comprising:
[0058] contacting the substrate surface with vaporized Mo(thd)3 to form up to a monolayer of Mo(thd)3 on the substrate; removing excess Mo(thd)3 and reaction by-products, if any, from the surface; and contacting a substrate surface with vaporized H2S; and removing from the surface excess H2S and any gaseous by-products formed in the reaction between the Mo(thd)3 layer and H2S.
[0059] The contacting and removing steps can be repeated until a MoS2 thin film of desired thickness is formed.
[0060] In some embodiments, the MoSe thin film is formed on a substrate by an ALD type process that includes at least one deposition cycle, the at least one deposition cycle comprising: contacting the substrate surface with vaporized Mo(thd)3 to form up to a monolayer of Mo(thd)3 on the substrate; removing excess Mo(thd)3 and reaction by-products, if any, from the surface; and contacting a substrate surface with vaporized H2Se; and removing from the surface excess H2Se and any gaseous by-products formed in the reaction between the Mo(thd)3 layer and H2Se.
[0061] The contacting and removing steps can be repeated until a MoSe2 thin film of desired thickness is formed.
[0062] In some embodiments, the WS2 thin film is formed on the substrate by an ALD type process that includes at least one deposition cycle, the at least one deposition cycle comprising: contacting a substrate surface with vaporized W(thd) to form up to a monolayer of W(thd) on the substrate; removing excess W(thd)3 and reaction by-products, if any, from the surface; and contacting a substrate surface with vaporized H2S; and removing from the surface excess H2S and gaseous by-products formed in the reaction between the W(thd)3 layer and H2S.
[0063] The contacting and removing steps can be repeated until a WS2 film of the desired thickness is formed.
[0064] In some embodiments, the WSe thin film is formed on a substrate by an ALD type process comprising at least one deposition cycle, the at least one deposition cycle comprising: contacting a substrate surface with vaporized W(thd) to form up to a monolayer of W(thd) on the substrate; removing excess W(thd)3 and reaction by-products, if any, from the surface; and contacting a substrate surface with vaporized H2Se; and removing from the surface excess H2Se and any gaseous by-products formed in the reaction between the W(thd)3 layer and H2Se.
[0065] The contacting and removing steps can be repeated until a WSe2 thin film of a desired thickness is formed.
[0066] Mo or W precursor Any of the following precursors can be used in the various ALD processes disclosed herein. In some embodiments, the Mo or W precursor is a metal organic compound. In some embodiments, the Mo or W precursor can include at least one multidentate ligand. In some embodiments, the Mo or W precursor can include at least one bidentate ligand. In some embodiments, the Mo or W precursor has three bidentate ligands and no other ligands. In some embodiments, the Mo or W precursor has at least one multidentate ligand bonded to Mo or W through an O, N, or S atom, more preferably through at least one O atom. In some embodiments, the Mo or W precursor has at least one multidentate ligand bonded to Mo or W through both O and N atoms. More preferably, a β-diketonate compound is used. In some embodiments, a ketoiminate compound is used. In some embodiments, M(acac), M(thd), M(tfac), M(bac), M(hfac), or M(fod) compounds are used, where M is Mo or W, acac is acetylacetonate or 2,4-pentanedionato, thd is 2,2,6,6-tetramethyl-3,5-heptanedionato, and tfac is trifluoroacetylacetonate or 1,1,1-trifluoroacetylacetonate. fluoro-2,4-pentanedionato, bac is benzoylacetonato, CHCOCHCOCH3, or 1-phenyl-1,3-butanedionato, hfac is hexafluoroacetylacetonato or 1,1,1,5,5,5-hexafluoro-2,4-pentanedionato, and fod is 2,2-dimethyl-6,6,7,7,8,8,8-heptafluorooctane-3,5-dionato. In some embodiments, the Mo or W precursor does not include a metal halide. In some embodiments, the Mo or W precursor has two or more Mo or W atoms. In some embodiments, the Mo or W precursor has two or more Mo or W atoms, and the two or more Mo or W atoms are bonded to each other. In some embodiments, the organometallic Mo or W precursor has at least one coordinated organic ligand and Mo or W bonded directly to oxygen that is not bonded to any other element or compound.In some embodiments, the Mo or W precursor may have at least one ligand bound to Mo or W through an O, N or S atom, preferably through at least one O atom.
[0067] In some embodiments, the Mo or W precursor may be selected from the group consisting of Mo or W β-diketonate compounds, Mo or W cyclopentadienyl compounds, Mo or W carbonyl compounds, and combinations thereof. In some embodiments, the Mo or W precursor does not contain one or more metal halides. In some embodiments, the Mo or W precursor does not contain one or more metal halides directly bonded to Mo or W. In some embodiments, the Mo or W precursor does not contain one or more halogen ligands that are not directly bonded to Mo or W. In preferred embodiments, the Mo or W precursor is Mo(thd)3 or W(thd)3. In some embodiments, the Mo or W precursor does not contain a carbonyl (CO) ligand. In some embodiments, the Mo or W precursor does not contain 6 carbonyl (CO) ligands. In some embodiments, the Mo or W precursor has 1, 2, 3, 4, or 5 carbonyl (CO) ligands. In some embodiments, the Mo or W precursor is a β-diketonate and is not Mo(thd)3 or W(thd)3.
[0068] Mo has several oxidation states including +VI, +V, +IV, +III, +II, +I, 0, -I, and -II. W has several oxidation states including +VI, +V, +IV, +III, +II, +I, 0, -I, and -II. In some embodiments, Mo or W in the Mo or W precursor has an oxidation state of +III, e.g., Mo has an oxidation state of +III in Mo(thd). In some embodiments, Mo or W in the Mo or W precursor has an oxidation state of +II, e.g., Mo has an oxidation state of +I in Mo(CO)Cl, Me2Mo(PMe3)4, CpW(CO)Cl, and Me2W(PMe3)4. In some embodiments, Mo or W in the Mo or W precursor has an oxidation state of +I, e.g., Mo has an oxidation state of +I in Mo(hfac). In some embodiments, Mo or W in the resulting thin film has an oxidation state of +IV. In some embodiments, Mo or W from the Mo or W precursor is oxidized during the formation of the resulting thin film. In some embodiments, the Mo or W precursor may be, for example, Cp2MoH2, Mo(NMe2)4, Mo(S t Bu)4, and Mo(S2CNMe2)4, or Cp2WH2, W(NMe2)4, W(S t It can be beneficial for Mo or W in, for example, W(S2CNMe2)4 to have an oxidation state of +IV.
[0069] The appropriate or desired oxidation state of Mo or W in a Mo or W precursor may depend on the particular conditions and circumstances, and the optimal oxidation state of Mo or W in a Mo or W precursor for a particular situation can be determined by one skilled in the art.
[0070] In some embodiments, Mo or W in the Mo or W precursor does not have an oxidation state higher than +III. In some embodiments, Mo or W in the Mo or W precursor does not have an oxidation state of +IV. In some embodiments, Mo or W in the Mo or W precursor has an oxidation state of +I to +III. In some embodiments, Mo or W in the Mo or W precursor does not have an oxidation state from +IV to +VI. In some embodiments, Mo or W in the Mo or W precursor does not have an oxidation state of +V. In some embodiments, Mo or W in the Mo or W precursor does not have an oxidation state of +VI. In some embodiments, Mo or W in the Mo or W precursor does not have an oxidation state of +II. In some embodiments, Mo or W in the Mo or W precursor has an oxidation state of +III. In some embodiments, Mo or W in the Mo or W precursor does not have an oxidation state of -II.
[0071] Thus, in some embodiments, Mo or W in the Mo or W precursor can include oxidation states from +I to +III, and when oxidized during formation of the resulting thin film, Mo or W has an oxidation state of +IV.
[0072] Without wishing to be bound by any particular theory, it is believed that the closer the oxidation state of the precursor metal is to the oxidation state of the deposited film metal, the less energy and / or time is required to deposit a film of the desired phase, crystal structure, crystallinity, or orientation. Furthermore, it is believed that if the precursor metal has a lower oxidation state relative to the oxidation state of the deposited film metal, less energy or time is required to deposit a film of the desired phase, crystal structure, crystallinity, or orientation. For example, if the deposited film metal has an oxidation state of +IV, it may be desirable for the precursor metal to have an oxidation state below +IV, such as +III, and thus undergo oxidation during deposition of the film, unlike in typical ALD processes.
[0073] In some embodiments, the Mo or W precursor comprises at least one ligand that binds to Mo or W through two atoms, referred to herein as a bidentate ligand. In some embodiments, the Mo or W precursor comprises at least one bidentate ligand that binds to Mo or W through at least an O, N or S atom. In some embodiments, the Mo or W precursor comprises at least one bidentate ligand that binds to Mo or W through an O atom at a first site and a second O atom at a second site. In some embodiments, the Mo or W precursor comprises at least one bidentate ligand that binds to Mo or W through an O atom at a first site and a N atom at a second site. In some embodiments, the Mo or W precursor comprises at least one bidentate ligand where the ligand binds to Mo or W through an N atom at a first site and a second N atom at a second site. In some embodiments, the Mo or W precursor comprises at least two bidentate ligands. In some embodiments, the Mo or W precursor comprises three bidentate ligands.
[0074] In some embodiments, the Mo or W precursor comprises at least one bidentate ligand that is a β-diketonato ligand. In some embodiments, the at least one bidentate ligand is an acac ligand. In some embodiments, the at least one bidentate ligand is a thd ligand. In some embodiments, the Mo or W precursor may comprise at least two β-diketonato ligands. In some embodiments, the Mo or W precursor may comprise three β-diketonato ligands. In some embodiments, the Mo or W precursor may comprise at least two thd ligands. In some embodiments, the Mo or W precursor may comprise at least two acac ligands. In some embodiments, the Mo or W precursor may comprise three thd ligands. In some embodiments, the Mo or W precursor may comprise three acac ligands.
[0075] In some embodiments, the Mo or W precursor is vaporized without a solvent, in a preferred embodiment, the Mo or W precursor is not mixed with a solvent, such as an organic solvent.
[0076] In some embodiments, Mo or W β-diketonates can be used in ALD type processes to deposit any type of Mo or W containing thin film. In some embodiments, Mo or W β-diketonates can be used to deposit elemental Mo or W films, Mo or W oxide films, Mo or W nitride films, or Mo or W silicide films. In particular, Mo(thd)3 and W(thd)3 can be used in ALD type processes to deposit any type of Mo or W containing thin film.
[0077] In some embodiments, Mo or W elemental thin films can be formed on a substrate by an ALD type process that includes at least one deposition cycle, the at least one deposition cycle comprising: contacting the substrate surface with vaporized Mo or W β-diketonate precursor to form up to one monolayer of Mo or W β-diketonate precursor on the substrate; removing excess Mo or W β-diketonate precursor and reaction by-products, if any, from the surface; contacting the substrate surface with a second reactant, such as H2 or hydrogen plasma, radicals, or atoms; and removing from the surface any excess second reactant and any gaseous by-products formed in the reaction between the Mo or W β-diketonate precursor layer and the second reactant.
[0078] The contacting and removing steps can be repeated until a Mo or W elemental thin film of a desired thickness is formed.
[0079] In some embodiments, Mo or W oxide thin films can be formed on a substrate by an ALD type process that includes at least one deposition cycle, the at least one deposition cycle comprising: contacting the substrate surface with vaporized Mo or W β-diketonate precursor to form up to one monolayer of Mo or W β-diketonate precursor on the substrate; removing excess Mo or W β-diketonate precursor and reaction by-products, if any, from the surface; contacting the substrate surface with water, ozone, or an oxygen precursor, such as oxygen plasma, radicals, or atoms; removing excess oxygen precursor and any gaseous by-products formed in the reaction between the Mo or W β-diketonate precursor layer and the oxygen precursor from the surface.
[0080] The contacting and removing steps can be repeated until a Mo or W oxide thin film of the desired thickness is formed.
[0081] In some embodiments, Mo or W nitride thin films can be formed on a substrate by an ALD type process that includes at least one deposition cycle, the at least one deposition cycle comprising: contacting the substrate surface with vaporized Mo or W β-diketonate precursor to form up to one monolayer of Mo or W β-diketonate precursor on the substrate; removing excess Mo or W β-diketonate precursor and reaction by-products, if any, from the surface; contacting a substrate surface with a precursor comprising nitrogen; removing excess oxygen precursor and any gaseous by-products formed in the reaction between the Mo or W β-diketonate precursor layer and the nitrogen-containing precursor from the surface.
[0082] The contacting and removing steps can be repeated until a Mo or W nitride thin film of the desired thickness is formed.
[0083] In some embodiments, suitable nitrogen-containing precursors may include NH3. In some embodiments, suitable nitrogen-containing precursors may include nitrogen-containing plasmas, such as N plasma, N atoms, or N radicals, or N and H-containing plasmas, N and H-containing atoms, or N and H-containing radicals.
[0084] In some embodiments, Mo or W silicide thin films can be formed on a substrate by an ALD type process that includes at least one deposition cycle, the at least one deposition cycle comprising: contacting the substrate surface with vaporized Mo or W β-diketonate precursor to form up to one monolayer of Mo or W β-diketonate precursor on the substrate; removing excess Mo or W β-diketonate precursor and reaction by-products, if any, from the surface; contacting a substrate surface with a precursor comprising silicon; and removing from the surface any excess silicon-containing precursor and any gaseous by-products formed in the reaction between the Mo or W β-diketonate precursor layer and the silicon-containing precursor.
[0085] The contacting and removing steps can be repeated until a Mo or W silicide film of the desired thickness is formed.
[0086] In some embodiments, the Mo or W-containing material is formed in a process that includes at least one deposition cycle on a substrate, the deposition cycle including contacting the substrate alternately and sequentially with a gas phase Mo or W precursor and a second gas phase chalcogen precursor. In some embodiments, the deposition cycle may be repeated two or more times. In some embodiments, the deposition cycle may be repeated sequentially two or more times. In some embodiments, after contacting the substrate with the gas phase Mo or W precursor and before contacting the substrate with the gas phase chalcogen precursor, excess Mo or W precursor and reaction by-products, if any, may be removed. In some embodiments, after contacting the substrate with the gas phase chalcogen precursor and before starting another deposition cycle, excess chalcogen precursor and reaction by-products, if any, may be removed. In some embodiments, after contacting the substrate with the Mo or W gas phase precursor and before contacting the substrate with the gas phase chalcogen precursor, the substrate may be contacted with a purge gas. In some embodiments, after contacting the substrate with the chalcogen gas phase precursor and before starting another deposition cycle, the substrate may be contacted with a purge gas.
[0087] Synthesis of Mo or W β-diketonate precursors Methods for producing some of the Mo or W precursors used in the ALD processes described herein are also provided. In some embodiments, a precursor having a formula of M(L)3 is synthesized, where M is Mo or W, and L is preferably a β-diketonato ligand, most preferably acac, hfac, or thd. In some embodiments, the Mo or W precursor synthesized has a formula of M(thd)3, where M is Mo or W. In some embodiments, the precursor synthesized is Mo(thd)3, and in other embodiments, it is W(thd)3.
[0088] In some embodiments, all handling and manipulation may be performed in an air, oxygen and moisture free atmosphere, hi some embodiments, all handling and manipulation may be performed in an inert gas atmosphere, such as N2 or Ar atmosphere.
[0089] 2 is a process flow diagram generally illustrating a method of forming a Mo or W β-diketonate precursor 20. In some embodiments, the method of making a Mo or W β-diketonate precursor includes:
[0090] forming a first product by reducing a Mo or W halide with a reducing agent in step 21;
[0091] Subsequently, a second product is formed in step 22 by adding a solvent to the first product, thereby forming the second product MX3 (R 1 ) n , n=0-4, where M is Mo or W, X is a halide, and R 1 is a solvent), forming a third product in step 23 by reacting an alkali metal compound, e.g., BuLi, MeLi, NaH, or KH, with the β-diketone; Then, in step 24, the third product is added to the second product, thereby forming a Mo or W β-diketonate precursor having the formula M(L)3, where M is Mo or W and L is a β-diketonate ligand, in step 25.
[0092] In some embodiments, the Mo or W halide of step 21 is preferably anhydrous Mo or W halide. In some embodiments, the Mo or W halide of step 21 has the formula MX5, where M is Mo or W and X is a halide, preferably Cl. In some embodiments, the metal halide of step 21 can have the formula MX4 or MX6, where M is W and X is a halide. In some embodiments, the Mo or W halide of step 21 is added to a solvent before reduction with a reducing agent, preferably an organic solvent, such as an ether. In a preferred embodiment, the solvent is EtO.
[0093] In some embodiments, the reducing agent comprises a metal, such as metallic Sn. In some embodiments, the reducing agent comprises an organic species, preferably a bis(trialkylsilyl) six-membered ring system or related compounds, such as 1,4-bis(trimethylsilyl)-1,4-dihydropyrazine (DHP). Preferably, the reducing agent is provided in the form of a powder or pellets, such as Sn pellets. In some embodiments, reducing the Mo or W halide comprises adding the reducing agent to a solution comprising the Mo or W halide to form a first product. In a preferred embodiment, reducing the Mo or W halide comprises adding Sn pellets to a solution of MCl5 in Et2O to form MCl4(Et2O)2, where M is Mo or W.
[0094] In some embodiments, the mixture of Mo or W halide and reducing agent is stirred for a first duration. In some embodiments, the mixture is stirred until the reaction is complete. After the desired first product is formed, comprising MCl4(Et2O)2, where M is Mo or W, the mixture can be allowed to settle. In some embodiments, after the reaction is complete, the first product can be separated and isolated from any solvent, by-products, excess reactants, or any other compounds that are undesired in the first product.
[0095] In some embodiments, a second product is formed by adding a solvent to the first product. In a preferred embodiment, the solvent is THF. In some embodiments, the mixture is stirred for a second duration. In some embodiments, the mixture is stirred until the reaction is complete. After the desired second product is formed, the mixture can be allowed to settle. In some embodiments, after the reaction is complete, the second product can be separated and isolated from any solvent, by-products, excess reactants, or any other compounds that are undesirable in the second product. In a preferred embodiment, forming the second product can include adding THF to the first product to form MCl3(THF)3, where M is Mo or W.
[0096] In some embodiments, the second product, MoCl3(THF)3, is formed according to the methods disclosed in Stoffelbach et al., "Improved Preparations of Molybdenum Coordination Compounds from Tetrachlorobis(diethyl ether)molybdenum(IV).", Eur. J. Inorg. Chem. 10 / 2001: 2699-2703, which is incorporated herein by reference in its entirety.
[0097] In some embodiments, the third product is formed by reacting an alkali metal compound with a β-diketone. In a preferred embodiment, the alkali metal compound includes butyllithium. In some embodiments, the alkali metal compound may include, for example, KH, NaH, or MeLi. In some embodiments, the alkali metal compound may be provided as an alkane solution, preferably a hexane solution. In some embodiments, the alkali metal compound may be added to a solvent. In some embodiments, the solvent may include a heterocyclic solvent. In a preferred embodiment, the solvent is THF.
[0098] In some embodiments, the β-diketone compound can include Hthd, Hacac, Htfac (wherein Htfac is trifluoroacetylacetone), Hfod (wherein fod is 2,2-dimethyl-6,6,7,7,8,8,8-heptafluoro-3,5-octanedione), or Hhfac, preferably Hthd. In some embodiments, reacting the alkali metal compound with the β-diketone compound can include reacting the alkali metal compound with the β-diketone compound of formula M by adding the β-diketone compound to a solution containing the alkali metal compound. 1 L (where M 1 and forming a third product having Lithd (wherein L is an alkali metal and L is a β-diketonato ligand). In a preferred embodiment, butyllithium in hexane is added to THF to form a solution. Hthd is then added to the solution to react with the butyllithium, thereby forming a third product comprising Lithd.
[0099] In some embodiments, the solution is optionally cooled before, during, and / or after the reaction is complete. In some embodiments, the β-diketone compound may be cooled before adding the alkali metal compound. In some embodiments, the solution may be stirred until the reaction is complete. In some embodiments, any gaseous by-products produced by the reaction may be vented, for example, via a bubbler.
[0100] In some embodiments, the third product is added to the second product, thereby forming a Mo or W β-diketonate precursor having the formula ML3, where M is Mo or W and L is a β-diketonate ligand. In some embodiments, the second product may be added to a solvent before adding the third product. In a preferred embodiment, the solvent is THF. In some embodiments, the third product is added to the mixture to form a Mo or W β-diketonate precursor. In some embodiments, the third product is added to the mixture to form a Mo or W β-diketonate precursor having the formula M 1 L (where M 1 In some embodiments, the third product can include a solution comprising the third product. In a preferred embodiment, Lithd is added to a suspension of MCl3(THF)3 in THF, thereby forming M(thd)3, where M is Mo or W.
[0101] In some embodiments, the second product may be cooled before the third product is added. In some embodiments, after the third product is added, the mixture is allowed to warm to room temperature. In some embodiments, the mixture is stirred for a second duration. In some embodiments, the mixture is stirred until the reaction is complete.
[0102] After the reaction is nearly complete, the final product may be separated and isolated from any solvent, by-products, excess reactants, or any other compounds that are undesirable in the final product.
[0103] In some embodiments, the method of making a Mo or W β-diketonate precursor comprises: In step 21, forming a first product by reducing anhydrous MoCl5 with Sn; Subsequently, forming a second product MoCl3(THF)3 in step 22 by adding a solvent comprising tetrahydrofuran (THF) to the first product, thereby forming a second product MoCl3(THF)3; reacting butyllithium with Hthd to form a third product Lithd in step 23; Subsequently, in step 24, the third product Lithd is added to the second product MoCl3(THF)3, thereby forming the precursor Mo(thd)3 in process 25. EXAMPLES
[0104] Example 1 Mo(thd)3 was synthesized by the following process: All handling and manipulations were performed with rigorous exclusion of air and moisture using standard Schlenk techniques and an inert gas (N2 or Ar) glove box.
[0105] First, 5.00 g (18.3 mmol) of anhydrous MoCl5 and 10 g (84 mmol) of Sn pellets were suspended in 50 ml of Et2O. The mixture was stirred at room temperature for 1 h to form a solution and a solid. The solid was allowed to settle to the bottom of the Schlenk flask, and most of the Et2O solution was removed using Ar pressure and a Teflon capillary tube.
[0106] Then, 50 ml of THF was added and the mixture was stirred at room temperature for 3 h to form solid MoCl3(THF)3. MoCl3(THF)3 was separated from the excess Sn by transferring the THF / MoCl3(THF)3 suspension to another Schlenk flask using Ar pressure and a Teflon capillary tube. The solid MoCl3(THF)3 was then filtered from the suspension using a Schlenk sinter and washed with Et2O.
[0107] Next, a Lithd solution was prepared. 30 ml of THF was cooled in a CO2 / acetone bath and 4.48 ml of a hexane solution of 1.6BuLi was added. 1.321 g (7.168 mmol) of Hthd was then added slowly to the solution using a syringe. The solution was then stirred at room temperature for 2 hours. The gaseous by-products were evacuated from the Schlenk flask containing the solution through a mercury bubbler.
[0108] Solid MoCl3(THF)3 was then suspended in 20 ml of THF. The suspension was then cooled in a CO2 / acetone bath and the previously prepared Lithd solution was added using a Teflon capillary and Ar pressure. The resulting solution was allowed to warm to room temperature and stirred overnight.
[0109] The THF solvent was then evaporated using a water bath and vacuum. The resulting solid product was transferred to a sublimation apparatus and sublimed at 160°C-180°C and 0.5 mbar. The resulting Mo(thd)3 sublimate was collected in a glove box.
[0110] The synthesized compounds were analyzed using mass spectrometry. As shown in Figure 3, a molecular ion with an isotopic pattern corresponding to Mo(thd)3 is seen at m / z 647. In addition to Mo(thd)3, fragment ions with oxygen, e.g., [Mo(thd)2O2] + , [Mo(thd)O] + , [Mo(thd)2O2-Bu] + , and [Mo(thd)O2] + However, these peaks are likely due to the exposure of the Mo(thd)3 compound to air during sample introduction into the mass spectrometer.
[0111] The molecular structure of the synthesized compound was analyzed using single crystal X-ray diffraction (SCXRD). The structure of the synthesized Mo(thd)3 compound is illustrated in Figure 4.
[0112] Mo(acac)3 and Mo(hfac)3 were also synthesized using a procedure similar to that used to synthesize Mo(thd)3. Hacac and Hhfac were used instead of Hthd to synthesize Mo(acac)3 and Mo(hfac)3, respectively. Thermogravimetric analysis (TGA) was used to investigate the thermal properties of the three Mo β-diketonate compounds. As shown in Figure 5, the thermogravimetric curves of Mo(thd)3 and Mo(hfac)3 indicate the evaporation of these compounds as the temperature increases, while the thermogravimetric curve of Mo(acac)3 indicates that this compound is primarily decomposed as the temperature increases.
[0113] Chalcogen Precursors It will be appreciated by those skilled in the art that many chalcogen precursors can be used in the ALD processes disclosed herein. In some embodiments, the chalcogen precursor is selected from the following list: H2S, H2Se, H2Te, (CH3)2S, (NH4)2S, dimethylsulfoxide ((CH3)2SO), (CH3)2Se, (CH3)2Te, elemental or atomic S, Se, Te, other precursors containing chalcogen-hydrogen bonds, such as H2S2, H2Se2, H2Te2, or chalcogenols having the formula RYH, where R is a substituted or unsubstituted hydrocarbon, preferably a C1-C8 alkyl or substituted alkyl, such as an alkylsilyl group, more preferably a linear or branched C1-C5 alkyl group, and Y can be S, Se, or Te. In some embodiments, the chalcogen precursor is a thiol having the formula RSH, where R can be a substituted or unsubstituted hydrocarbon, preferably a C1-C8 alkyl group, more preferably a linear or branched C1-C5 alkyl group. In some embodiments, the chalcogen precursor has the formula (R3Si)2Y, where R3Si is an alkylsilyl group and Y can be Se or Te. In some embodiments, the chalcogen precursor comprises S or Se. In some preferred embodiments, the chalcogen precursor comprises S. In some embodiments, the chalcogen precursor may comprise a chalcogen element, such as elemental sulfur. In some embodiments, the chalcogen precursor does not comprise Te. In some embodiments, the chalcogen precursor comprises Se. In some embodiments, the chalcogen precursor is selected from precursors comprising S, Se, or Te. In some embodiments, the chalcogen precursor comprises H2S n (wherein n is 4 to 10).
[0114] Suitable chalcogen precursors may include many chalcogen-containing compounds, so long as they contain at least one chalcogen-hydrogen bond. In some embodiments, the chalcogen precursor may include a chalcogen plasma, a chalcogen atom, or a chalcogen radical. In some embodiments where an excited chalcogen precursor is desired, a plasma may be generated in the reaction chamber or upstream of the reaction chamber. In some embodiments, the chalcogen precursor does not include an excited chalcogen precursor, such as a plasma, an atom, or a radical. In some embodiments, the chalcogen precursor may include a chalcogen plasma, a chalcogen atom, or a chalcogen radical formed from a chalcogen precursor containing a chalcogen-hydrogen bond, such as H2S. In some embodiments, the chalcogen precursor may include a chalcogen plasma, a chalcogen atom, or a chalcogen radical, such as a plasma containing sulfur, selenium, or tellurium, preferably a plasma containing sulfur. In some embodiments, the plasma, atom, or radical includes tellurium. In some embodiments, the plasma, atom, or radical includes selenium.
[0115] Example 2 Various deposition experiments were performed using MoCl5 and H2S as precursors in a flow-type reactor (ASM America F-120 reactor) with no residence time for the precursors, at reaction temperatures between 150°C and 500°C. Various substrates were used, such as Al2O3, ZnS, soda-lime glass, Si, and Ir. After the deposition experiments were performed, neither Mo nor S was detected on the substrate in amounts that would indicate film growth. EDX was performed on the samples, showing only trace amounts of Mo. No S was detected on the samples at all. This process is reported by Browning et al. in "Atomic layer deposition of MoS2 thin films," which is incorporated herein by reference in its entirety. The inventors have performed similar experiments under reasonably similar conditions with respect to the process conditions described in the Browning paper, but the tests were unsuccessful, possibly indicating the non-robustness of the process disclosed therein.
[0116] Example 3 MoS2 thin films were deposited according to the ALD process disclosed herein utilizing Mo(thd)3 as the Mo precursor and H2S as the chalcogen precursor. MoS2 was deposited on silicon, titanium disulfide, alumina, and soda-lime glass substrates. The substrates were contacted with alternating pulses of Mo(thd)3 and H2S at deposition temperatures ranging from about 175°C to about 500°C.
[0117] At deposition temperatures between 175°C and 350°C, no MoS2 film formation was observed. The amount of film on the substrate seemed to increase at deposition temperatures higher than about 375°C. The highest growth rate was achieved at a deposition temperature of about 500°C. At this deposition temperature, the substrate was covered with a purple or brown MoS2 film.
[0118] The resulting MoS2 films were characterized by FESEM, and the morphology of the films was found to be virtually identical regardless of the substrate on which they were deposited. Although a flaky structure was observed on the surface of some of the films, cross-sectional FESEM images revealed that the films were dense and free of cracks and pinholes, as shown in Figure 6.
[0119] The growth rate of ALD MoS2 films saturated at about 0.2 Å / cycle for pulse lengths of about 0.5–1 s for both Mo(thd)3 and H2S, as shown in Figure 7. The film thickness was observed to increase substantially linearly, as shown in Figure 8, although there may be an incubation period, as indicated by the slightly steeper slope after 500 deposition cycles.
[0120] Increasing the Mo(thd)3 pulse length did not affect the growth rate, but the morphology of the film was affected. Figure 9 illustrates that the films deposited with 0.2 and 0.5 second pulses have almost identical surfaces containing sharp flaky structures. No difference in film thickness was observed, but Mo(thd)3 pulse lengths of 1 second or more resulted in surfaces containing grains. The resulting films were deposited using 1000 deposition cycles, but similar surface structures were observed with a Mo(thd)3 pulse length of 4 seconds, as compared to films deposited with 2000 cycles using Mo(thd)3 pulse lengths of 0.2, 0.5, and 1 second. Thus, the film thickness may affect the structural differences of the surface, as the Mo(thd)3 pulse length is also likely to affect it.
[0121] Varying the H2S pulse length resulted in similar differences in the membrane surface structure, but now shorter H2S pulse lengths resulted in flake-free surfaces. As shown in Figure 10, a 0.2 second H2S pulse length resulted in a membrane with a particle-containing surface. Longer pulses resulted in a surface containing sharp-edged flakes.
[0122] The growth of MoS2 films was visually analyzed for MoS2 films deposited from 10 to 2000 deposition cycles. Mo(thd)3 was used as the Mo precursor with a pulse time of 0.5 seconds and a purge time of 1 second, while H2S was used as the chalcogen precursor with a pulse time of 0.5 seconds and a purge time of 1 second. The deposition temperature for all samples was 500 °C. Figure 11A illustrates MoS2 films deposited from 10 to 50 cycles, and Figure 11B shows MoS2 films deposited from 100 to 2000 cycles. The surface structure of the film is crystalline, and the presence of sharp flakes on the film surface appears to be nearly flat up to approximately 1500 deposition cycles, which seems to be thickness dependent. After 2000 deposition cycles, the raised flake structure covers the entire surface of the film.
[0123] The composition of the MoS2 film was analyzed by EDX. 35 S 65The theoretical film composition of was obtained by synthesizing the spectra of theoretical samples consisting of MoS2 films on silicon substrates using Oxford INCA software. The composition of MoS2 films deposited at 500 °C was analyzed by EDX while varying the Mo(thd)3 pulse length as shown in Figure 12A. The composition of MoS2 films deposited at 500 °C was analyzed by EDX while varying the H2S pulse length as shown in Figure 12B. In both cases, the measured MoS2 film composition was determined to be similar to the theoretical composition.
[0124] The elemental ratios of MoS2 film samples deposited at 500°C by the ALD process were also measured and are illustrated in FIG. 13. The MoS2 films were deposited by the ALD process with 250 to 2000 deposition cycles. As the number of deposition cycles increased, the measured elemental ratios of the MoS2 films became Mo-rich to S-rich. The MoS2 sample deposited by the ALD process with 2000 deposition cycles had a high elemental ratio of Mo. 42 S 58 Although there may be an incubation period, the deposited film thickness was observed to increase approximately linearly, as illustrated in FIG.
[0125] The composition of two sets of deposited MoS2 film samples was analyzed by grazing incidence X-ray diffraction (GIXRD), as illustrated in FIG. 14. One set of sample MoS2 films was deposited by an ALD process in which the Mo precursor pulse time was varied from 0.2 to 4 seconds while the sulfur precursor pulse was kept constant at 0.5 seconds. A second set of sample MoS2 films was deposited by an ALD process in which the sulfur precursor pulse time was varied from 0.2 to 2 seconds while the Mo precursor pulse was kept constant at 0.5 seconds. The samples were deposited at 500°C. The intensity of the (002) peak shown in FIG. 14 increased as the Mo precursor pulse time decreased and increased as the sulfur precursor pulse time increased.
[0126] The phase of the deposited film was identified using Raman spectroscopy. MoS2 has a peak at 383 cm for the in-plane vibration of Mo and S atoms. -1 , and 406 cm for the out-of-plane vibration of S atoms.-1 As shown in Figure 15, both of these peaks are clearly visible in the as-deposited MoS2 thin film.
[0127] The phases of two sets of deposited MoS2 film samples were analyzed using Raman spectroscopy, as illustrated in FIG. 16. One set of sample MoS2 films was deposited by an ALD process in which the Mo precursor pulse time was varied from 0.2 to 4 seconds while the sulfur precursor pulse was kept constant at 0.5 seconds. A second set of sample MoS2 films was deposited by an ALD process in which the sulfur precursor pulse time was varied from 0.2 to 2 seconds while the Mo precursor pulse was kept constant at 0.5 seconds. The samples were deposited at 500°C. The intensity of the in-plane and out-of-plane MoS2 peaks was observed to increase with decreasing Mo precursor pulse time and increasing with increasing sulfur precursor pulse time.
[0128] The elemental composition of two MoS2 thin film samples deposited by the ALD process was investigated using X-ray photoelectron spectroscopy (XPS), as illustrated in Figure 17. One sample was deposited by the ALD process with a 0.2 second Mo precursor pulse, while the second sample was deposited by the ALD process with a 4 second Mo precursor pulse time.
[0129] The surface roughness of MoS2 film samples deposited by an ALD process using Mo(thd)3 as the Mo precursor and having 10 to 50 deposition cycles was also examined using atomic force microscopy (AFM), as illustrated in Figure 18. The roughness of the samples deposited by 10 and 50 cycles was found to be 0.41 nm, while the roughness of the sample deposited by 25 cycles was found to be 0.44 nm. The surface features of the films were less than 10 nm in size for all samples, although the size of the surface features appeared to increase with the number of deposition cycles.
[0130] Figure 19 illustrates the growth rate and elemental ratios of MoS2 films deposited by an ALD process at temperatures between 425°C and 500°C using Mo(thd)3 as the Mo precursor. The growth rate was observed to increase with increasing deposition temperature, with the highest growth rate observed at a deposition temperature of 500°C. The composition of the deposited films varied with deposition temperature.
[0131] The growth of MoS2 films was visually analyzed for MoS2 films deposited by ALD, as illustrated in Figure 20. Mo(thd)3 was used as the Mo precursor with a pulse time of 0.5 seconds and a purge time of 1 second, while H2S was used as the chalcogen precursor with a pulse time of 0.5 seconds and a purge time of 1 second. The deposition temperature was varied from 350°C to 500°C.
[0132] 2D materials The ALD processes described herein can be used to deposit 2D materials containing Mo or W, such as Mo or W dichalcogenides, such as MoS2, WS2, MoSe2, or WSe22D materials. 2D materials, also called monolayer materials, are materials that consist of a single connected monolayer. Although 2D materials form a single connected monolayer, multiple monolayers can be deposited by the deposition processes disclosed herein. For example, in the case of 2D MoS2, the 2D material comprises a single layer of covalently bonded MoS2 molecules arranged such that one layer of Mo atoms is sandwiched between two layers of S atoms. The basic atomic structure of MoS2 will be familiar to those skilled in the art.
[0133] Such special features make 2D materials useful for a wide range of promising applications, such as, for example, as lubricants in optoelectronics, spintronics, and valleytronics, for use as catalysts, chemical and biological sensors in THz generation and detection, in supercapacitors, LEDs, solar cells, lithium-ion batteries, and MOSFET channel materials.
[0134] Unlike other 2D materials such as graphene, 2D Mo or W dichalcogenides have unique electronic properties that make them useful for miniaturizing semiconductor devices. For example, unlike graphene, 2D Mo or W dichalcogenides have a direct band gap and are semiconducting. Therefore, Mo or W dichalcogenides are useful in electronic devices, for example, Mo or W dichalcogenides can be used as channel materials in gate stacks or transistors.
[0135] According to some embodiments, 2D materials comprising Mo or W may be deposited by ALD according to the methods disclosed herein. In some embodiments, the 2D materials comprising Mo or W may comprise no more than 10 monolayers, preferably less than 5 monolayers, and most preferably no more than 3 monolayers of a compound comprising Mo or W.
[0136] In some embodiments, the 2D material comprising Mo or W may comprise no more than 10 monolayers, preferably less than 5 monolayers, and most preferably no more than 3 monolayers of a Mo or W dichalcogenide. In some embodiments, the 2D material comprising Mo or W may comprise no more than 10 monolayers, preferably less than 5 monolayers, and most preferably no more than 3 monolayers of MoS2, WS2, MoSe2, WSe2, MoTe2, or WTe2.
[0137] In some embodiments, the method of depositing a 2D material comprising Mo or W on a substrate can include an ALD process comprising multiple cycles as disclosed herein. In some embodiments, the method of depositing a 2D material comprising Mo or W can include an ALD process comprising 500 deposition cycles or less, preferably 200 deposition cycles or less, and most preferably 100 deposition cycles or less, as disclosed herein. As can be selected by one of skill in the art depending on the particular precursors, substrate, and process conditions, the method of depositing a 2D material comprising Mo or W on a substrate can include an ALD process comprising 50 cycles or less, 25 cycles or less, 15 cycles or less, or 10 cycles or less, as disclosed herein.
[0138] In some embodiments, the deposited 2D material comprising Mo or W can be less than 10 nm, more preferably less than 5 nm, more preferably less than 3 nm, more preferably less than 2 nm, more preferably less than 1.5 nm, and most preferably less than 1.0 nm.
[0139] In some embodiments, the deposited 2D material has a roughness (R q ). Roughness can be measured, for example, by atomic force microscopy (AFM) or X-ray reflectometry (XRR). For ultra-thin 2D material films, AFM can be the preferred method.
[0140] In some embodiments, the 2D material comprising Mo or W can be used as a channel material in an electronic device, such as a gate stack. In some embodiments, the 2D material comprising Mo or W can be deposited after the gate dielectric, i.e., channel last. In some embodiments, the 2D material comprising Mo or W can be deposited before the gate dielectric, i.e., channel first. In some embodiments, the gate stack can be fabricated upside down, such that the channel is above the gate in the gate stack.
[0141] FIG. 21 is an aberration-corrected scanning tunneling electron microscope (AC-STEM) image of a MoS2 thin film 1420 deposited on a silicon substrate 1400 containing a native oxide 1410. The silicon atoms 1401 of the substrate 1400 are seen as white dots in the bottom half of the image, while the native oxide 1410 is the darker layer between the MoS2 thin film 1420 and the silicon substrate 1400. The MoS2 shown here is about 2-3 monolayers, with a thickness of about 10-15 Å. The spacing between monolayers is about 6-8 Å, which is within the expected range for MoS2.
[0142] The terms "film" and "thin film" are used herein for simplicity. "Film" and "thin film" are intended to mean any continuous or non-continuous structures and materials deposited by the methods disclosed herein. "Films" and "thin films" can include, for example, 2D materials, nanorods, nanotubes, or nanoparticles, or flat single partial or complete molecular layers, or partial or complete atomic layers, or clusters of atoms and / or molecules. "Films" and "thin films" can include materials or layers that have pinholes, but are still at least partially continuous.
[0143] The term chalcogen as used herein is intended to refer primarily to the chemical elements sulfur, selenium, and tellurium, although in some cases, as will be apparent to those skilled in the art, the term may also refer to oxygen. Similarly, the terms chalcogenide and dichalcogenide are intended to refer primarily to sulfides, selenides, and tellurides, although in some cases, as will be apparent to those skilled in the art, such terms may also refer to oxides.
[0144] Although the foregoing invention has been described with respect to certain preferred embodiments, other embodiments will be apparent to those skilled in the art. Furthermore, other combinations, omissions, substitutions and modifications will be apparent to those skilled in the art in view of the disclosure herein. Thus, the present invention is not intended to be limited by the recitation of preferred embodiments, but is instead defined by reference to the appended claims.
Claims
1. Formula ML 3 wherein M is Mo or W and L is a β-diketonato ligand, and an inert carrier gas; A composition for an atomic layer deposition (ALD) process, wherein M is Mo or W, and L is selected from the group consisting of thd (2,2,6,6-tetramethyl-3,5-heptanedionato), acac (acetylacetonato[2,4-pentanedionato]), hfac (hexafluoroacetylacetonato[1,1,1,5,5,5-hexafluoro-2,4-pentanedionato]), tfac (trifluoroacetylacetonato[1,1,1-trifluoro-2,4-pentanedionato]), and fod (2,2-dimethyl-6,6,7,7,8,8,8-heptafluoro-3,5-octanedionato).
2. The composition of claim 1, wherein the β-diketonato ligand is bonded to a Mo or W atom via two O atoms.
3. The Mo or W β-diketonate precursor is Mo(thd) 3 2. The composition of claim 1 ,
4. The Mo or W β-diketonate precursor is Mo(acac) 3 2. The composition of claim 1 ,
5. The Mo or W β-diketonate precursor is W(thd) 3 2. The composition of claim 1 ,
6. The Mo or W β-diketonate precursor is W(acac) 3 2. The composition of claim 1 ,
Citation Information
Patent Citations
Method for preparing pyrochlore type Nd2Mo2O7 cushioning layer
CN101337828A
Porous carbon material used for anode of lithium-air cell
CN103855412A
Apparatus and method for delivering non-volatile reactants
JP1995503759A
Reagents made from metal complexes
JP1999507629A
Production of carbon nanotube
JP2000086217A