Multiaxial stitched substrate and method of manufacturing same
The multiaxial stitch base material addresses poor resin impregnation and productivity issues by forming continuous concave grooves along reinforcing fibers, enhancing impregnation efficiency and mechanical properties.
Patent Information
- Application Number
- JP2020114055
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-01
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-07-01
AI Technical Summary
Conventional multiaxial stitch base materials face challenges with poor resin impregnation properties and low productivity due to independent and elongated gaps between reinforcing fibers, leading to damage and reduced mechanical properties.
A multiaxial stitch base material with defined stitch length, interval, and orientation angle relationships, forming continuous concave grooves along reinforcing fibers to serve as resin flow paths, reducing fiber damage and enhancing impregnation efficiency.
The solution significantly improves resin impregnation speed and productivity while maintaining high mechanical properties by minimizing fiber bending and damage, ensuring reliable molded products.
Smart Images

Figure 0007578942000001 
Figure 0007578942000002 
Figure 0007578942000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a stitch base material made of reinforcing fibers, and more particularly to a multiaxial stitch base material that has excellent impregnation with a matrix resin and improves the production efficiency of molded products, and a method for producing the same. [Background technology]
[0002] Fiber-reinforced plastics, which use reinforcing fibers such as carbon fiber and glass fiber as reinforcement materials, exhibit high strength and elasticity in the direction of the reinforced fibers, but this rapidly decreases at angles away from the fiber direction.For this reason, they are laminated and molded so that the fiber axis direction is multiaxial, such as 0° / 90°, ±45°, or 0° / +45° / -45° / 90°, so that the mechanical properties become pseudo-isotropic.
[0003] However, stacking sheets while accurately aligning their fiber axes during molding is time-consuming and results in very low production efficiency. Therefore, as proposed in Patent Document 1 (Republished Publication No. 01-063033), multiaxial stitched base materials in which sheets arranged at a predetermined fiber orientation angle are integrated with stitch threads have come to be widely used.
[0004] Since the multiaxial stitch substrate is integrated with stitch threads, the orientation angle of the reinforcing fibers is not disturbed during molding operations, making it a substrate with excellent handleability. At the same time, the reinforcing fibers maintain a specified fiber orientation in the molded product, allowing the mechanical properties to be achieved as designed, resulting in a highly reliable molded product.
[0005] In addition, the orientation angle of the reinforcing fibers in the multiaxial stitched substrate is selected appropriately depending on the shape of the molded product and the required mechanical properties, such as biaxial orientation of 0° / 90° or ±45°, or 4-axial orientation of 0° / ±45° / 90°. In particular, a biaxially oriented stitched substrate at ±45° has excellent formability and is suitable for molded products with curved surfaces, and is therefore widely used as a substrate for the Resin Transfer Molding process (hereinafter referred to as the RTM method) and the Vacuum assisted Resin Transfer Molding process (hereinafter referred to as the VaRTM method).
[0006] In resin injection molding, ±45° oriented stitch substrates have gaps formed around the pinholes where the stitch threads are woven that penetrate the substrate in the thickness direction. This allows the matrix resin to flow easily in the thickness direction of the substrate. However, since the gaps do not continue in the planar direction, the resin does not flow well. This results in a long time for impregnation, which makes it difficult to achieve high productivity, and also leads to the occurrence of unimpregnated areas.
[0007] As a method for improving the resin impregnation of a ±45° biaxially oriented stitched substrate, for example, Patent Document 2 (JP Patent Publication No. 2016-078258) discloses a method for improving the density of pinholes generated when the substrate is woven into a reinforcing fiber layer by increasing the density of the pinholes to 80,000 / m 2 More than 180,000 pieces / m 2 The following proposals have been made to facilitate impregnation of the matrix resin into the fiber layer through the pinholes.
[0008] According to this proposal, by providing pinholes at a high density, the number of flow paths in the thickness direction of the laminated substrate increases, improving impregnation, but there is a problem that the reinforcing fibers may be damaged when pierced by the needle, or the reinforcing fibers may be bent more due to gaps between the reinforcing fibers caused by the pinholes, which may result in a decrease in the mechanical properties of the molded product. In addition, there are two ways to increase the pinhole density: shortening the stitch length to increase the pinhole density per unit length in the longitudinal direction of the substrate, and shortening the stitch interval to increase the pinhole density per unit length in the width direction of the substrate. In the method of shortening the stitch length, the length of substrate manufactured per one rotation in which the needle rises and falls once during manufacturing is shortened, resulting in a decrease in productivity. On the other hand, in the method of shortening the stitch interval, the number of stitch threads used per unit width of the substrate increases, which increases the volume ratio of the stitch threads contained in the substrate, resulting in a decrease in the strength of the molded product obtained by impregnating and curing the matrix resin.
[0009] Furthermore, Patent Document 3 (WO 2019-161926 A) proposes a method of inserting multiple monofilament yarns or twisted yarns between the +45° layer and the -45° layer in the length and width directions of the substrate, and using the gaps formed around the inserted yarns as flow paths for the resin. This proposed technology ensures a reliable resin flow path, which improves the resin impregnation speed and leads to a reduction in molding time.
[0010] However, while the technology proposed in Patent Document 3 ensures a flow path for the resin, the reinforcing fibers are pressed against the rigid insertion yarns by the molding pressure and are molded in a locally bent state. Therefore, when stress is generated in the molded product, the stress is concentrated at the bent points, which become the starting points for destruction, resulting in the problem that the high strength and elastic modulus of the reinforcing fibers are not fully utilized. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Republished Publication No. 01-063033 [Patent Document 2] JP 2016-078258 A [Patent Document 3] International Publication No. 2019-161926 Summary of the Invention [Problem to be solved by the invention]
[0012] The present invention has been made in consideration of the above-mentioned problems associated with conventional stitch base materials for FRP molding, and an object of the present invention is to provide a multiaxial stitch base material that has excellent resin impregnation properties, high productivity due to shortened molding time, and can produce FRP with excellent composite properties, and a method for manufacturing the same. [Means for solving the problem]
[0013] The means adopted by the present inventor to solve the above technical problems will be described below with reference to the accompanying drawings.
[0014] That is, the present invention provides a stitch base material in which reinforcing fiber sheets each having reinforcing fiber threads arranged in parallel to each other are laminated in different orientation directions and integrated with a stitch thread passing through these sheets, Carbon fiber yarn with 6,000 to 24,000 filaments and a degree of entanglement of 45 or less. The reinforcing fibers include two bias-oriented sheets oriented at angles +θ° and -θ°, which are not at least 0° and 90°, relative to the length direction of the stitched substrate; The weight of one layer of the bias orientation sheet is 75 to 400 g / m 2 and The relationship between the stitch length s of the stitch base material, the stitch interval w, and the orientation angle θ of the reinforcing fiber of the bias orientation sheet satisfies the following relational expression: The inclination line connecting a specific needle hole in a row of needle holes in the 0° direction and a needle hole n courses away from the same course in the adjacent needle hole row coincides with the inclination of the bias orientation of the reinforcing fiber, and the gaps caused by the needle holes in the woven part of the stitch thread are connected along the reinforcing fiber and formed on the surface of the base material. It becomes a resin flow path in the surface direction. The structure is completed by forming a plurality of recessed grooves. C = w / (n |tanθ|) C-0.1 / n <s<C+0.1 / n where C is the critical stitch length (mm), s is the stitch length (mm), w is the stitch spacing (mm), and n is 1, 2, or 3.
[0015] Also, technical means for setting the stitch interval at 4 to 7 mm can be adopted.
[0016] Furthermore, a technical means can be adopted in which the orientation angle of the reinforcing fibers is a lamination configuration of ±30 to ±60°.
[0017] Furthermore, a technical measure can be adopted in which the reinforcing fibers of the bias orientation sheet are carbon fibers.
[0019] Furthermore, the bending stiffness EI of the stitch yarn (tensile modulus of the fiber × (single yarn diameter) 4 x number of filaments x 4.9 x 10 -2 )(Pa·m 4 ) is the basis weight M (g / m 2 ) is 15×10 -10 ~60×10 -10 In accordance with the present invention, technical measures may be adopted.
[0020] Furthermore, the density of the pinholes in the woven portion of the stitch thread in the stitch base material is 35,000 to 80,000 pieces / m 2 In accordance with the present invention, technical measures may be adopted.
[0021] Furthermore, the method for producing a stitch base material of the present invention includes the steps of: The reinforcing fiber is a carbon fiber yarn with 6,000 to 24,000 filaments and a degree of entanglement of 45 or less. A plurality of reinforcing fiber yarns are arranged parallel to each other, Bias alignment sheet 1 layer Weight is 75~400g / m 2 These reinforcing fiber sheets are cross-laminated at an angle of ±30 to ±60°, so that the relationship between the stitch length s of the stitch base material, the stitch interval w, and the orientation angle θ of the reinforcing fibers of the bias orientation sheet satisfies the following relational expression, and the density of the pinholes in the woven part of the stitch thread is 35,000 to 80,000 pieces / m 2The fibers are stitched together using stitching threads with a fineness of 30 to 110 Dtex. By this, a plurality of concave grooves that become resin flow paths in the surface direction are formed on the surface of the base material. This is the method. C = w / (n |tanθ|) C-0.1 / n <s<C+0.1 / n where C is the critical stitch length (mm), s is the stitch length (mm), w is the stitch spacing (mm), and n is 1, 2, or 3.
[0022] The stitch interval can be set in the range of 4 to 7 mm. Effect of the Invention
[0024] The multiaxial stitched substrate of the present invention is a stitched substrate in which the relationship between the stitch length s of the stitched substrate, the stitch interval w, and the orientation angle θ of the reinforcing fibers of the bias orientation sheet is specified, so that the gap between the reinforcing fibers due to the needle holes of the woven part of the stitch yarn is equal to the gap between the adjacent needle hole rows. Connect with the gap Since a plurality of concave grooves that serve as resin flow paths are formed on the surface of the substrate, the grooves act as flow paths for the matrix resin in the planar direction, significantly shortening the resin impregnation time while reducing unimpregnated areas to obtain a highly reliable molded product.
[0025] As the stitch thread, the bending stiffness EI of the stitch thread (tensile modulus of fiber × (single thread diameter) 4 x number of filaments x 4.9 x 10 -2 )(Pa·m 4 ) is the basis weight M (g / m 2 ) and the exponent is 15×10 -10 ~60×10 -10 By doing so, even if the stitch base material has a high basis weight, the bending rigidity of the stitch thread strengthens the tightening, so that even if pressure is applied to the laminated material in the molding process, the formed concave groove portion is reliably maintained and there is no decrease in the resin impregnation rate.
[0026] In the manufacturing method of the present invention, in the manufacturing process in which the reinforcing fibers are stacked and stitched in different orientation directions relative to the length direction of the multiaxial stitch base material, by setting conditions that satisfy the relationship between the stitch length s, the stitch spacing w, and the orientation angle θ of the reinforcing fibers of the bias oriented sheet, the diagonal line connecting one needle hole in a row of needle holes in the 0° direction and a needle hole n courses away in an adjacent row of needle holes matches the inclination of the reinforcing fibers of the bias oriented sheet, so that the tip of the elongated gap created along the bias-oriented reinforcing fiber by the needle piercing extends to the position of the adjacent needle hole to be pierced in the next course, and the needle piercing is always repeated with low piercing resistance, thereby suppressing damage to the reinforcing fibers.
[0027] Furthermore, in conventional stitch substrates, the pinhole gap exists alone and partially bends the reinforcing fiber, but the elongated gap created by the manufacturing method of the present invention is continuously connected to adjacent gaps along the reinforcing fiber, and the reinforcing fiber is straightened, minimizing bending of the reinforcing fiber and allowing the high strength and high elastic modulus of the reinforcing fiber to be fully utilized.
[0028] Furthermore, by setting the stitch spacing of the stitch base material of the present invention in the range of 4 to 7 mm, a distance is ensured that adjacent gaps can be connected along the reinforcing fibers, and recessed groove portions that serve as resin paths are reliably obtained.
[0029] In addition, the density of pinholes is 35,000 to 80,000 pieces / m 2 By reducing the number of needle holes to 1, damage to the reinforcing fibers caused by needle puncture can be further reduced, and even if the density of the needle holes that serve as resin flow paths in the thickness direction is reduced, a fast resin impregnation speed can be maintained because concave grooves that serve as resin flow paths in the surface direction of the substrate are formed.
[0030] By using carbon fiber yarn with a filament count of 6,000 to 24,000 and a degree of entanglement of 45 or less as the reinforcing fiber, even a fiber bundle with a large number of fibers, which has low production costs, is easy to open due to the low degree of entanglement, and a reinforcing fiber sheet with a uniform fiber density and low basis weight can be obtained.Furthermore, the high openability allows the fibers to move easily when pierced with a needle, resulting in less fiber damage, and also makes it easy to form concave grooves by connecting gaps. [Brief description of the drawings]
[0031] [Figure 1] FIG. 2 is a front view of a stitched substrate according to an embodiment of the present invention. [Diagram 2] 1 is a cross-sectional schematic diagram of a stitched substrate of the present invention. [Diagram 3] FIG. 1 is a front view of a conventional stitched substrate. [Figure 4] 1 is a graph showing the resin impregnation of the stitched substrate of the present invention. [Diagram 5] 1 is a photograph of an example of a stitched substrate of the present invention. [Figure 6] 1 is a photograph of a comparative example of a stitched substrate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The embodiments of the present invention will be described in more detail below with reference to the drawings in which the embodiments are specifically illustrated.
[0033] An embodiment of the present invention will be described with reference to Fig. 1 to Fig. 6. The stitch base material of the present invention is formed by laminating two reinforcing fiber sheets each having reinforcing fibers arranged in parallel with one another, the reinforcing fibers being oriented at an angle of at least +θ° and -θ°, which are not 0° or 90°, relative to the length direction of the stitch base material, and the sheets are integrated with a stitch thread.
[0034] FIG. 1 is a front view of a stitched substrate 1 according to one embodiment of the present invention in which the reinforcing fibers are oriented at ±θ°. Reference numeral 2 denotes a reinforcing fiber 2 oriented at an angle of +θ° relative to the longitudinal direction of the stitched substrate 1, and reference numeral 11 denotes a reinforcing fiber 11 oriented at an angle of -θ°. The reinforcing fibers 2 and 11 are parallel to each other in a sheet-like shape and are integrated by a stitch thread 4 with a stitch length s and a stitch spacing w.
[0035] When the relationship between the stitch length s of the stitch substrate, the stitch spacing w, and the orientation angle θ of the reinforcing fibers satisfies the following relational expression, the gap between the reinforcing fibers caused by the needle holes 5 in the woven portion of the stitch thread 4 is such that the diagonal line connecting one needle hole 5 in a row of needle holes arranged in the 0° direction and a needle hole 5 n courses apart in an adjacent needle hole row is parallel to the reinforcing fibers of the bias orientation sheet. For example, in the stitch substrate 1 of Figure 1, when the stitch spacing w is 5 mm, the orientation angle of the reinforcing fibers is ±45°, and n = 1, the stitch length s is 4.9 to 5.1 mm from the relational expression, and the line connecting the pin hole 5a and the pin hole 5b in the adjacent pin hole row arranged in the 0° direction approximately coincides with the orientation angle of the reinforcing fibers, which is +45°, and similarly coincides on the back side. Relation: C=w / (n·|tanθ|) C-0.1 / n <s<C+0.1 / n where C is the critical stitch length (mm), s is the stitch length (mm), w is the stitch spacing (mm), and n is 1, 2, or 3.
[0036] The range of the critical stitch length C has the following technical significance. (1) Precision of the knitting machine The equipment factor that determines the stitch length is the distance that the sheets stacked on the equipment advance during one cycle of the needle rising and lowering. Small distortions of each part related to these movements and gaps between parts affect the stitch length, and an error occurs from the target value, so this error is within the allowable range. (2) Continuity of the grooves When the stitch length s is the same as the critical stitch length C, the orientation direction of the reinforcing fibers and the direction of the gaps are perfectly aligned, and adjacent gaps in the fiber orientation direction are aligned in a straight line, forming a concave groove portion when the gaps connect to each other, so s = C is ideal. However, even if the stitch length s deviates slightly from the critical stitch length C, the gaps connect slightly to form a concave groove portion, and higher impregnation is obtained compared to the substrate of the conventional technology. The results of the experiment confirmed that a deviation of 0.1 / n (mm) in the critical stitch length C results in a significant loss of impregnation, while a deviation of 0.09 / n (mm) results in marginally high impregnation. In other words, although the continuity of the concave grooves is significantly lost in appearance, continuity remains in three dimensions (part of the thickness direction), or even if there is no continuity, there are only a few interrupted parts of the concave grooves, and if the resin moves to the adjacent gap, impregnation progresses within the gap.
[0037] In the needle hole 5, a long and narrow gap 6 is created along the reinforcing fibers 2·11 due to the piercing action of the needle into the sheet-like reinforcing fibers and the tightening action of the stitch thread being fed into the needle to form a loop and tightening the reinforcing fibers 2·11, as shown in the conventional stitch base material 7 in Figure 3 described below.
[0038] In FIG. 1, the tip of the elongated gap formed at the pinhole 5a extends to the pinhole 5b of the next course or its vicinity, and a similar elongated gap is also formed at the pinhole 5b of the next course. Therefore, two adjacent elongated gaps are connected to each other to form a concave groove portion 3 along the reinforcing fibers.
[0039] The stitch interval w affects whether the elongated gaps formed along the reinforcing fibers 2·11 can be connected to each other. The smaller the stitch interval w, the easier it is to connect them. However, if the stitch interval w is smaller than 4 mm, the density of the pinholes in the stitch base material 1 increases, which increases the damage to the reinforcing fibers. In addition, the number of stitch threads used per unit width of the base material increases, which increases the volume ratio of the stitch threads contained in the base material, and the strength of the molded product obtained by impregnating and curing the matrix resin decreases. On the other hand, if the stitch interval w is larger than 7 mm, the gaps do not connect to each other, and the concave groove portion 3 that serves as the resin path cannot be formed. For this reason, it is most preferable that the stitch interval w is 4 to 7 mm.
[0040] The formation of multiple grooves 3 along the reinforcing fibers 2·11 on the surface of the stitch substrate 1 of the present invention serves as a resin flow path when performing resin injection molding. In particular, with conventional bias-oriented substrates, the resin flowed quickly from the pinholes in the thickness direction, but there was no resin flow path in the surface direction, so resin impregnation took time. However, the formation of the grooves 3 ensures a resin flow path in the surface direction, allowing resin impregnation in a short time and achieving high productivity.
[0041] The shape of the concave groove portion 3 differs in size between the loop side (the back side in Figure 1) and the sinker loop side (the front side in Figure 1). As can be seen from the schematic cross-sectional view of the substrate in Figure 2, the collection of reinforcing fibers 2·11 is restrained by the sinker loops 23 and the needle loops 22. However, since the needle loops 22 are connected to each other and are in a state of tension in the longitudinal direction, it is the sinker loops 23 that restrain the reinforcing fibers 2 in a bent state, and as a result, the concave groove portion 3 is formed on the sinker loop 23 side.
[0042] When the stitch base material 1 has a low basis weight, the amount of reinforcing fibers 2·11 is small, so the recessed groove portion 3 can be maintained even when pressure is applied without being tightly fastened with the sinker loop 23. However, as the basis weight increases, the amount of fiber increases and the thickness of the recessed groove portion 3 increases, so that when pressure is applied in the layered state, the reinforcing fibers 2·11 will flow toward the recessed groove portion 3, causing the recessed groove portion 3 to be easily crushed.
[0043] Therefore, the stitch yarn 4 used in the present invention has a bending stiffness EI (tensile modulus of fiber × (single yarn diameter) 4 x number of filaments x 4.9 x 10 -2 )(Pa·m 4 ) is the basis weight M (g / m 2 ) is 15×10 -10 ~60×10 -10 By setting the range as described above, as the stitch base material 1 has a higher basis weight, a stitch thread 4 with higher bending rigidity can be used, and in particular, the sinker loop 23 can be used to strengthen the pressure applied to the reinforcing fibers 2·11 in the upper part of the side wall of the concave groove portion 3, so that the concave groove portion 3 can be maintained without being crushed even when pressure is applied.
[0044] On the other hand, when the stitch base material 1 has a low basis weight, the amount of reinforcing fibers 2 / 11 is small, so even when pressure is applied, there is almost no movement toward the concave groove portion 3, and therefore the pressing force applied by the sinker loop 23 to the reinforcing fibers 2 / 11 at the upper part of the side wall of the concave groove portion 3 can be small.
[0045] In addition, the index is 60 x 10 -10 If the index is larger than 60×10, the pressure on the sinker loop 23 becomes stronger and the concave groove portion 3 is maintained. However, if the pressure is too strong, the strength will decrease due to bending of the reinforcing fiber, and if the concave groove portion 3 is too large, a resin-rich portion will be formed. -10 It is preferable that:
[0046] On the other hand, if the exponent is 15×10 -10 If the index is smaller than 15×10, the sinker loop 23 is not pressed against the side wall of the concave groove 3, and when pressure is applied by stacking the stitch base material 1, the reinforcing fibers 2·11 tend to move toward the concave groove 3, making it difficult to maintain the concave groove 3 that has been created. -10 More preferably, it is equal to or greater than this.
[0047] In addition, since the bending rigidity EI of the stitch 4 is proportional to the fourth power of the single yarn diameter, by using a filament yarn with a large single yarn diameter, the fineness of the stitch thread 4 itself can be made finer. Furthermore, in terms of yarn type, polyester yarn has a high tensile modulus of elasticity, so the stitch thread 4 can be made finer, which is preferable in that it reduces the unevenness of the substrate surface caused by the stitch thread 4 and also leads to cost reduction, but in the present invention, the index can be appropriately determined within the range of the above index based on the stitch processability and the substrate surface condition, etc.
[0048] The concave groove portion 3 formed on the sinker loop 23 side (+45° sheet side) extends to the bias oriented sheet surface on the needle loop 22 side of the lower layer (-45° sheet side), so that resin impregnation is performed at the same speed into the bias oriented sheet of the lower layer through the resin flow in the concave groove portion 3 on the sinker loop 23 side.
[0049] The stitch substrate 1 shown in FIG. 1 is a case where n=1 in the above-mentioned relational expression, but the number n can be appropriately selected to 2 or 3 by controlling the size of the stitch spacing w and the resin impregnation speed, and the present invention includes angles of the reinforcing fibers relative to the longitudinal direction of the substrate that are not 0° or 90°. Generally, when pseudo-isotropy is required, a substrate arranged in the ±45° direction as described above is most stable and preferable, but similar effects can be obtained with an arrangement angle in the range of ±30 to ±60°.
[0050] <Conventional multi-axis stitched substrate> Fig. 3 shows a conventional stitch substrate 7 in which the reinforcing fibers are oriented at ±45°. The needle piercing forms the pinhole 5 and the long and narrow gap 6 along the reinforcing fiber 2 in the same manner as in the embodiment of the present invention. However, the gaps formed by the pinhole 5a and the pinhole 5b in Fig. 3 are separated by a distance a in their extensions along the reinforcing fiber 2, so they are not continuous and exist independently, and no groove is formed to become a resin flow path. In addition, the needle pierces each pinhole 5 at a place where the reinforcing fiber 2 is not separated, so that the reinforcing fiber is easily damaged and there is a concern that fuzzing may occur. In addition, the reinforcing fiber around the gap 6 is bent along the gap shape, which has a problem of adversely affecting the mechanical properties of the molded product.
[0051] As the reinforcing fibers 2-11 in this embodiment, high strength and high modulus fibers such as carbon fibers, glass fibers, and aramid fibers can be used. Among them, polyacrylonitrile- or pitch-based carbon fibers with a tensile strength of 2.5 GPa or more and a tensile modulus of 200 GPa or more are preferred because they can achieve a large reinforcing effect with a small amount of fiber.
[0052] In addition, when carbon fibers have a single fiber diameter of 5 μ or more and a tensile modulus of elasticity of 200 GPa or more, they exhibit high bending rigidity in the single fiber state, so that the elongated gap of the needle hole caused by the needle piercing becomes longer and the resistance to the next needle piercing becomes lower, which has the effect of further suppressing damage to the reinforcing fibers.
[0053] In this embodiment, the fineness of the carbon fiber yarn used for the reinforcing fibers 2 and 11 is set to 400 to 1650 tex, and the weight per layer of the bias orientation sheet is set to 75 to 400 g / m 2 Since it is particularly difficult to impregnate a high basis weight product with resin, the technique of the present invention for forming the concave grooves 3 on the sheet surface can be highly effective.
[0054] The fineness of the carbon fiber yarn and the basis weight of the substrate should be determined appropriately based on the required characteristics, such as the performance and cost of the desired molded product. However, when reliability is required, such as for aircraft components, it is also necessary to take into account that a high-quality substrate must be steadily supplied, with properties such as resin impregnation that are difficult to determine from appearance alone. The stitch substrate of the present invention is provided with a resin flow path, which allows for reliable resin impregnation and makes it possible to supply highly reliable molded products.
[0055] The mechanism of resin impregnation in the resin injection molding method of the ±45° laminated stitch base material 1 of the present invention shown in Figure 1 is that the injected resin flows along the concave groove portion 3, spreading the impregnation to the reinforcing fibers 2 lateral to the concave groove portion 3 and to the reinforcing fibers 11 in the -45° layer below the concave groove portion 3, so that resin impregnation progresses throughout the entire material.
[0056] Therefore, in the ±45° laminated stitch base material 1 of the present invention, the resin in the concave grooves 3 simultaneously impregnates the upper and lower sheets, so even if there are few flow paths in the thickness direction due to the pinholes, there is no effect on the impregnation speed. Therefore, the minimum pinhole density that maintains the shape stability of the base material is sufficient, and the preferred pinhole density is 35,000 to 80,000 pcs / m 2 The pinhole density is 80,000 / m 2 If the thickness is larger, the base material will be strongly clamped in the thickness direction by the stitch threads, making it hard, and there will be problems with the resin flow paths being crushed and the resin impregnation performance being reduced. There will also be problems with the number of needle punctures increasing, which will increase damage to the reinforcing fibers. Therefore, a thickness of 35,000 to 45,000 pieces / m is more preferable. 2 It is.
[0057] The manufacturing method of the present invention includes arranging a plurality of reinforcing fiber yarns parallel to each other and at equal intervals, Between threads Spread it out so that there are no gaps, and the basis weight is 75 to 400 g / m 2Then, these reinforcing fiber sheets are laminated together, including at least two sheets with an orientation angle of ±θ° other than 0° and 90°, so that the relationship between the stitch length s of the stitch base material, the stitch interval w, and the orientation angle θ of the reinforcing fiber of the bias orientation sheet satisfies the following relational expression, and the density of the pinholes in the woven part of the stitch thread is 35,000 to 80,000 pieces / m 2 The fibers are stitched together using stitching thread with a fineness of 30 to 110 Dtex. C = w / (n |tanθ|) C-0.1 / n <s<C+0.1 / n where C is the critical stitch length (mm), s is the stitch length (mm), w is the stitch spacing (mm), and n is 1, 2, or 3.
[0058] By stitching with a stitch length s and stitch spacing w that satisfy the above relationship, the diagonal line connecting one needle hole in a row of needle holes in the 0° direction to a needle hole n courses away in an adjacent row of needle holes becomes parallel to the reinforcing fibers of the bias oriented sheet, and the tip of the long, thin gap created along the bias-oriented reinforcing fibers by the needle piercing reaches the position of the adjacent needle hole to be pierced in the next course.Since the needle piercing is repeated with low piercing resistance, damage to the reinforcing fibers can be reduced.
[0059] In addition, because the gaps along the reinforcing fibers are connected to each other, multiple grooves are formed on the surface of the substrate. These grooves act as resin flow paths in the resin injection molding process, significantly improving the low resin impregnation rate that has been a problem with bias stitch substrates.
[0060] In addition, the pinhole density is set to 35,000 to 80,000 pieces / m 2 By reducing the number of needle holes to 1, damage to the reinforcing fibers caused by needle puncture can be further reduced, and even if the density of the needle holes that serve as resin flow paths in the thickness direction is reduced, a fast resin impregnation speed can be maintained because grooves that serve as resin flow paths in the surface direction of the substrate are formed.
[0061] In addition, as the reinforcing fiber in the production of the stitch base material of the present invention, it is preferable to use a carbon fiber yarn having a filament count of 6,000 to 24,000 and an entanglement degree of 45 or less. 2 In order to obtain a thin sheet with a uniform fiber density, the spreading action of the yarn bundle is essential, and this action improves the opening property, thereby reducing the resistance to needle piercing. At the same time, the gaps caused by the needle piercing tend to become longer, making it easier to form concave grooves on the surface of the substrate by connecting the gaps.
[0062] In addition, by using carbon fiber yarns with a degree of entanglement of 45 or less, the carbon fiber yarns themselves have sufficient fiber opening, so that a sheet with a uniform fiber density can be obtained as described above, and since the gaps caused by needle piercing tend to be long, it becomes easy to form concave grooves on the surface of the substrate by connecting the gaps.
[0063] On the other hand, carbon fiber yarns with a degree of entanglement of more than 45 have poor opening properties and a high filament count, so the basis weight is 75 to 400 g / m 2 When producing a thin sheet of this type, gaps will form between the yarn bundles, making it impossible to obtain a sheet with a uniform fiber density. In addition, the needle piercing resistance will increase, and it will be difficult to connect the gaps. Therefore, it is preferable that the degree of entanglement is 45 or less.
[0064] The degree of entanglement was measured according to the JIS L 1013 (2010) "Testing method for chemical fiber filament yarn". One end of the reinforced fiber bundle was attached to the upper grip of the hanging device, and a load (100 g) was hung from the position of the fiber bundle 1 m below the grip, and the sample was hung vertically. A hook with a diameter of 1 mm and a weight was inserted at a point 1 cm below the upper grip of the sample so as to divide the fiber bundle in two, and the hook was lowered at a speed of about 2 cm / sec. The descent distance L [mm] of the hook to the point where the hook stopped due to entanglement of the yarn was measured, and the degree of entanglement was calculated by the following formula. The above operation was repeated 50 times (1 time / m x 50), and the average value was used. Intertwining degree = 1000 / LL: Hook drop distance [mm].
[0065] While the angles of ±θ° shown in Figure 1 have been described above as a lamination of ±45°, the present invention is not limited to this lamination and includes a stitch base material 1 laminated containing at least two sheets with bias orientations of +θ° and -θ°, with orientation angles other than 0° and 90°, such as a three-layer lamination of 0° / +45° / 90° / -45°, 0° / +45 / -45° / 90°, or 0° / +45 / -45°. EXAMPLES
[0066] The stitch base material is made of carbon fiber thread with a tensile strength of 4900 MPa, a tensile modulus of 235 GPa, a fineness of 800 tex (12,000 filaments), and an entanglement degree of 14. The weight per layer is 150 g / m. 2 The sheets were arranged parallel to each other so as to form a laminate at an angle of ±45° to the direction in which the stitch yarn was woven.
[0067] Then, a multi-axis knitting machine was used to knit polyester fibers of 33 dtex and 36 filaments (flexural stiffness / weight index 17×10 -10 The stitching was performed under the manufacturing conditions of a chain stitch structure with stitch interval w = 5.08 mm, n = 1, and θ = 45°, resulting in a stitch length s of 5.08 mm calculated from the relational expression of the present invention. The needle hole density was 38,750 pieces / m 2 It was.
[0068] The resulting stitched material had a bending stiffness / basis weight index of 17×10 -10 Even though the value was relatively low, it was confirmed that the gaps caused by the pinholes in the stitching yarn weaving part on the sinker loop surface were continuously connected along the reinforcing fibers, and multiple concave grooves were formed. In addition, the appearance was free of fluff caused by damage to the carbon fibers.
[0069] In order to investigate the resin impregnation, the obtained stitch substrate of the present invention was cut to a size of 290 mm wide x 350 mm long, one substrate was placed on a mold, and a transparent cowl plate of 0.1 mm thick x 280 mm wide x 340 mm long was placed on top of it. The periphery of these was covered with a bag film, and the inside of the bag sealed with a sealant tape was vacuum-suctioned to perform resin impregnation by the VaRTM method. Resin was injected from the end of the stitch substrate of the present invention using an epoxy resin with a resin viscosity of 190 mPa·s, the resin was impregnated in the longitudinal direction of the substrate, and the time from the start of impregnation and the impregnation distance (the distance from the resin injection port to the tip of the resin flow) were measured. These results are plotted on a graph in Figure 4 with the impregnation distance on the vertical axis and the time on the horizontal axis. It was confirmed that the resin had impregnated the entire substrate when it reached 350 mm 46 minutes after the start of impregnation.
[0070] <Comparative Example 1> As a comparative example, a base material stitched under the conditions of Example 1 with only the stitch length set to 2.80 mm, which does not satisfy the relational expression of the present invention, had a single gap caused by the pinhole in the woven stitch thread, and the reinforcing fibers around it were bent, as shown in the photograph in Figure 6. The resulting stitch base material was impregnated with resin under the same conditions as in the examples, and as shown in Figure 4, it took 164 minutes to reach 350 mm, which was about 3.7 times longer than in the examples.
[0071] As can be seen from the above-mentioned Examples and Comparative Examples, the resin impregnation speed of the technology proposed by the present invention is clearly faster than that of the conventional technology, and high productivity can be obtained by shortening the molding time, which is expected to result in a significant reduction in manufacturing costs. It is therefore anticipated that the technology will be applied to applications in which manufacturing costs have been a bottleneck in the development of carbon fiber composite materials up until now. [Explanation of symbols]
[0072] 1:Stitching material 2: Reinforced fiber 3: Concave groove 4: Stitching thread 5, 5a, 5b: Needle hole 6: Gap 7: Conventional multi-axis stitched substrate 11: Reinforced fiber 12: Concave groove 22: Needle loop 23: Sinker Loop
Claims
1. A stitch base material in which reinforcing fiber sheets each having reinforcing fiber yarns arranged in parallel to each other are laminated in different orientation directions and integrated by a stitch thread penetrating these sheets, The reinforcing fibers are carbon fiber yarns having a filament count of 6,000 to 24,000 and an entanglement degree of 45 or less, and the reinforcing fibers are oriented at angles +θ° and −θ°, which are not 0° or 90°, relative to the length direction of the stitch base material. and the weight per layer of the bias orientation sheet is 75 to 400 g / m 2 ; The relationship between the stitch length s of the stitch base material, the stitch interval w, and the orientation angle θ of the reinforcing fibers of the bias orientation sheet satisfies the following relational expression: A multiaxial stitched substrate characterized in that a line of inclination connecting a specific needle hole in a row of needle holes arranged in the 0° direction to a needle hole in an adjacent row of needle holes that is n courses away from the same course matches the inclination of the bias orientation of the reinforcing fibers, and gaps created by the needle holes in the woven portion of the stitch thread are connected along the reinforcing fibers to form a plurality of concave grooves on the surface of the substrate that serve as resin flow paths in the planar direction. C=w / (n・|tanθ|) C-0.1 / n<s<C+0.1 / n where C is the critical stitch length (mm), s is the stitch length (mm), w is the stitch spacing (mm), and n is 1, 2, or 3.
2. 2. The multi-axial stitched substrate of claim 1, wherein the stitch spacing is 4 to 7 mm.
3. 3. The multiaxial stitched substrate according to claim 1, characterized in that the reinforcing fibers have a layered structure in which the orientation angle of the reinforcing fibers is within a range of ±30 to ±60 degrees.
4. The bending stiffness EI of the stitch yarn (tensile modulus of fiber x (single yarn diameter) 4 x number of filaments x 4.9 x 10 -2 ) (P a m 4 ) is the basis weight M (g / m 2 ) is 15 x 10 -10~60 x 10 -10 The multiaxial stitched substrate according to any one of claims 1 to 3,
5. The density of the pinholes in the woven portion of the stitch thread in the stitch base material is 35,000 to 80,000 pinholes / m 2 The multiaxial stitched substrate according to any one of claims 1 to 4, characterized in that
6. In the manufacture of a multiaxially stitched substrate, (A) A carbon fiber yarn having a filament count of 6,000 to 24,000 and an entanglement degree of 45 or less is used as the reinforcing fiber, and a plurality of reinforcing fiber yarns are arranged in parallel to each other, so that the weight of one layer of the bias oriented sheet is 75 to 400 g / m 2 A plurality of reinforcing fiber sheets are prepared, (B) These reinforcing fiber sheets are laminated together, including at least two sheets having an orientation angle other than 0° and 90°; (C) The relationship between the stitch length s of the stitch base material, the stitch interval w, and the orientation angle ±θ° of the reinforcing fibers of the bias orientation sheet satisfies the following relational expression: C=w / (n・|tanθ|) C-0.1 / n<s<C+0.1 / n where C is the critical stitch length (mm), s is the stitch length (mm), w is the stitch spacing (mm), and n is 1, 2, or 3. (D) And the density of the pinholes in the woven part of the stitch thread is 35,000 to 80,000 pieces / m 2 A method for manufacturing a multiaxial stitched substrate, characterized in that a plurality of concave grooves that serve as resin flow paths in the planar direction are formed on the surface of the substrate by stitching and integrating the substrate with a stitch thread having a fineness of 30 to 110 Dtex within the range of 100 to 150 Dtex.
7. The method for producing a multi-axis stitched material according to claim 6, characterized in that the stitch spacing is 4 to 7 mm.
Citation Information
Patent Citations
Reinforcing woven fabric and method and device for producing the same
JP1995300739A
Composite reinforced fiber base and preform
JP2002113802A
Multilayer substrate and preform
JP2008132775A
Fiber sheet for fiber-reinforced resin and molding using the same
JP2016078258A
A stitched multi-axial reinforcement and a method of producing the same
WO2019161926A1