Manufacturing method of tea waste fiber raw material and its use
The method transforms tea dregs into high-quality papermaking fibers by treating them with acids and alkalis, blending with additives, and integrating them with softwood pulp to produce eco-friendly, tough, and absorbent paper.
Patent Information
- Application Number
- JP2023071171
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-07-14
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2043-04-24
AI Technical Summary
China faces a shortage of papermaking fiber raw materials due to limited waste paper pulp resources and the environmental impact of tea dregs disposal, which are rich in organic matter and not effectively utilized in paper production.
A method is developed to process tea dregs into fiber raw materials through sun drying, boiling, ultrasonic treatment, acid and alkali treatments, and blending with additives to produce a pulp suitable for papermaking, reducing pollution and enhancing fiber properties.
The processed tea dregs fibers yield high-quality paper with improved toughness, texture, and water absorption, addressing the resource scarcity and environmental issues while maintaining eco-friendliness.
Abstract
Description
[Technical field]
[0001] The present invention relates to the papermaking technology field, in particular to the preparation method and use of tea residue fiber raw material. [Background technology]
[0002] China's papermaking fiber resources are relatively scarce, and the supply capacity is already unable to meet the demand for expansion, and fiber raw materials have become a bottleneck restricting the development of China's papermaking industry. Currently, the main raw material for papermaking used in China is waste paper pulp, but waste paper pulp has disadvantages such as uneven fiber length, unstable chemical composition, keratinized fiber, and high ink residue, which imposes many restrictions on the use of waste paper pulp, and if 100% waste paper pulp is used, it will be difficult to produce high-grade paper and special paper with high added value. Moreover, waste paper resources are not inexhaustible, and in particular waste paper recycling is already approaching its limit. Therefore, new papermaking raw materials are urgently needed to alleviate the problem of shortage of papermaking fiber raw materials.
[0003] China is a big agricultural country with a large annual production of tea biomass, but the main method of disposing of tea waste at present is incineration, and as the tea waste flows into rivers, a large amount of organic matter is dissolved in the water system, which makes the water system have a high organic matter content and deep color. Due to the consumption of a large amount of organic matter, the dissolved oxygen in the water is reduced, which directly affects the survival environment of aquatic organisms, and causes the death of many aquatic organisms.
[0004] The average length of tea stem fibers is 0.87mm and the average width is 0.017mm, which is not much different from that of Korean aspen, and compared to other high-quality pulp-making raw materials, it is finer and shorter, and the proportion of fine fibers (0.15-0.5mm) is higher, reaching an average of 32%. The arrangement of the large molecules in tea stem fibers is orderly and dense, and the crystallinity and orientation of the fibers are both high. The high content of hemicellulose and lignin gives it good paper-plastic properties and spinnability. Like other agricultural stalks, waste tea contains a large amount of fiber, so how to use tea waste in papermaking or spinning technology is currently an issue that needs to be resolved urgently. Summary of the Invention [Problem to be solved by the invention]
[0005] In response to the problems existing in the prior art, the present invention provides a manufacturing method and use of tea residue fiber raw material, in which the entire manufacturing process is less polluting and consumes less energy, and the obtained tea residue product is decomposable, has high toughness, is light, thin, and sound-absorbing, and is in line with the sustainability of the practice of ecological resource materials. [Means for solving the problem]
[0006] The technical solutions of the present invention are as follows: In a first aspect, the present invention provides a method for producing tea leaf fiber raw material,
[0007] Step 1: dry the tea leaves in the sun, crush them, blanch them in boiling water, add water and ultrasonicate them for a certain period of time, treat them with concentrated hydrochloric acid at 50-60℃ for 1-2 hours, filter and wash until neutral, treat them with sodium hydroxide liquid alkali with a mass concentration of 20-25% at 70-80℃ for 4-5 hours, filter and wash until neutral; Step 2 is to extract the treated tea residue with water to obtain tea polyphenols and a slurry, respectively, and then to cook the slurry and press-dehydrate it to obtain a crude pulp; Step 3: refining and screening the coarse pulp, and then beating it;
[0008] After beating, add β-cyclodextrin, sodium carboxymethylcellulose and reinforced starch, adjust the pH to 7-8, dilute and add the tea polyphenols obtained in step 2 and mix uniformly, squeeze and dehydrate, and then oven dry in step 4 to complete the process.
[0009] Furthermore, the tea residue may be any one or a combination of tea stems, tea leaves, tea residue, tea residue after drinking, or any defective product generated during any tea manufacturing process. Furthermore, the screen residue obtained from step 3 is combined with the next coarse pulp for refining. Furthermore, in step 3, the degree of beating is controlled to 30-40°SR.
[0010] Furthermore, the total amount of the β-cyclodextrin, sodium carboxymethylcellulose and reinforced starch is 10-20% of the bone-dry tea residue fiber raw material, and the mass ratio of the β-cyclodextrin, sodium carboxymethylcellulose and reinforced starch is 1:1-3:1-5. In a second aspect, the present invention provides a method for producing tea leaf fiber raw material,
[0011] Step 1: dry the tea leaves in the sun, crush them, blanch them in boiling water, add water and ultrasonicate them for a certain period of time, treat them with concentrated hydrochloric acid at 50-60℃ for 1-2 hours, filter and wash until neutral, treat them with sodium hydroxide liquid alkali with a mass concentration of 20-25% at 70-80℃ for 4-5 hours, filter and wash until neutral; Step 2: adding sodium alginate-gelatin aqueous solution to the treated tea leaves, leaving it at room temperature for a certain period of time, filtering it, and washing the filter cake; and step 3 of adding distilled water to the filter cake and shaking for 30 min-1 h, followed by filtering and oven drying.
[0012] Furthermore, the tea residue may be any one or a combination of tea stems, tea leaves, tea residue, tea residue after drinking, or any defective product generated during any tea manufacturing process.
[0013] Furthermore, the mass concentration of sodium alginate in the sodium alginate-gelatin aqueous solution is 10 to 20%, and the mass concentration of gelatin is 5 to 10%. In a third aspect, the present invention provides the use of tea residue raw material in papermaking.
[0014] In a fourth aspect, the present invention provides a method for producing writing paper, which comprises the steps of processing the above-mentioned tea residue raw material into 50-60 mesh powder, then blending it with bleached sulfate softwood pulp based on a weight ratio composition of 10-20%:90-80%, uniformly mixing it, refining and beating it, forming it into a paper, squeezing it, drying it in an oven, and sequentially winding and cutting it to complete the process. Effect of the Invention
[0015] Compared with the prior art, the advantages of the present invention are as follows:
[0016] The present invention chooses chemical pulp production, and through acid treatment, starch, pectin and other substances can be hydrolyzed, improving the pulp yield. Some sugars can be removed by acid treatment, and at the same time, it prepares the paper for the subsequent alkaline treatment. In order to highlight the characteristics of tea, chemical treatment is used in the papermaking process to moderately maintain the texture of tea leaf fiber. The tea residue paper produced by the method of the present invention has a light color, fine fiber, uniform paper, strong toughness, smooth texture, matte color, excellent water absorption, and good writing feel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] In describing the present invention, it should be noted that unless specific conditions are specified in the examples, they are carried out according to normal conditions or conditions suggested by the manufacturer. The reagents or equipment used are normal products that can be purchased and obtained commercially unless the manufacturer is specified.
[0018] The present invention will be described in more detail below in light of the embodiments for carrying out the invention, thereby helping those skilled in the art to have a more complete, accurate and in-depth understanding of the ideas and technical solutions of the invention. The scope of protection of the present invention includes but is not limited to the following examples. Any modifications made to the details and forms of the technical solutions of the present invention without departing from the spirit and scope of the present application will also fall within the scope of protection of the present invention. The specific embodiment of the present invention provides two methods for producing tea residue fiber raw materials, which are as follows: The first type is a method for producing tea leaves fiber raw material,
[0019] Step 1: The tea residue is dried in the sun, crushed, blanched in boiling water, then sonicated in water for a certain period of time, treated with concentrated hydrochloric acid at 55°C for 2 hours, filtered and washed until neutral, further treated with sodium hydroxide liquid alkali of 20% by mass at 75°C for 4 hours, filtered and washed until neutral, the tea residue being any one or a combination of tea stems, tea leaves, tea residue, tea residue after drinking, or any defective product generated during any tea manufacturing process; Step 2 is to extract the treated tea residue with water to obtain tea polyphenols and a slurry, respectively, and then to cook the slurry and press-dehydrate it to obtain a crude pulp; Step 3: the coarse pulp is successively refined and screened, and then beaten to a degree of beating of 30-40°SR;
[0020] Step 4: after beating, add β-cyclodextrin, sodium carboxymethylcellulose and reinforced starch, the total amount of β-cyclodextrin, sodium carboxymethylcellulose and reinforced starch is 20% of the bone-dry tea residue fiber raw material, and the mass ratio of β-cyclodextrin, sodium carboxymethylcellulose and reinforced starch is 1:2:5, and adjust the pH to 8. After dilution, add the tea polyphenol obtained from step 2 and mix uniformly, squeeze dehydration and oven dry. In the above process, the screen residue from step 3 is combined with the next coarse pulp for refining. The second type is a method for producing tea leaves fiber raw material,
[0021] Step 1: The tea residue is dried in the sun, crushed, blanched in boiling water, then sonicated in water for a certain period of time, treated with concentrated hydrochloric acid at 55°C for 2 hours, filtered and washed until neutral, further treated with sodium hydroxide liquid alkali of 20% by mass at 75°C for 4 hours, filtered and washed until neutral, the tea residue being any one or a combination of tea stems, tea leaves, tea residue, tea residue after drinking, or any defective product generated during any tea manufacturing process;
[0022] Step 2: adding sodium alginate-gelatin aqueous solution to the treated tea leaves, leaving it at room temperature for a certain period of time, filtering and washing the filter cake, so that the mass concentration of sodium alginate in the sodium alginate-gelatin aqueous solution is 10% and the mass concentration of gelatin is 5%; and step 3, shaking the filter cake in distilled water for 30 minutes, then filtering and oven drying.
[0023] The present invention further provides a method for producing writing paper, which is completed by the steps of processing the above-mentioned tea waste raw material into 50-60 mesh powder, then blending it with bleached sulfate softwood pulp based on the weight ratio composition: 10-20%:90-80%, uniformly mixing, refining and beating, forming into paper, squeezing, drying in an oven, winding and cutting in sequence. The paper-making process is performed based on the existing process, and will not be described in detail here. Example 1: In this embodiment, the first type of tea residue fiber raw material was used, and the weight ratio of the tea residue raw material for papermaking to the bleached sulfate softwood pulp was 10%:90%. The technical indicators of the tea waste paper described in Example 1 are as shown in Table 1: Table 1: Color Fiber Edge Toughness Feel Absorbency Ease of writing Shallow Fine Uniform Strong Smooth and matte color Good Good writing feel Example 2: In this embodiment, the first type of tea residue fiber raw material was used, and the weight ratio of the tea residue raw material for papermaking to the bleached sulfate softwood pulp was 20%:80%. The technical indicators of the tea waste paper described in Example 2 are as shown in Table 2: Table 2: Color Fiber Edge Toughness Feel Absorbency Ease of writing Shallow Fine Uniform Strong Smooth and slightly matte color Good Relatively good writing feel Example 3: In this embodiment, the second type of tea residue fiber raw material was used, and the weight ratio of the tea residue raw material for papermaking to the bleached sulfate softwood pulp was 10%:90%. The technical indicators of the tea waste paper described in Example 3 are as shown in Table 3: Table 3: Color Fiber Edge Toughness Feel Absorbency Ease of writing Slightly deep Fine Slightly shrunk Strong Flat and smooth Good Good writing feel Example 4: In this embodiment, the second type of tea residue fiber raw material was used, and the weight ratio of the tea residue raw material for papermaking to the bleached sulfate softwood pulp was 20%:80%. The technical indicators of the tea waste paper described in Example 4 are as shown in Table 4: Table 4: Color Fiber Edge Toughness Feel Absorbency Ease of writing Somewhat deep Fine Somewhat shrunken Brittle Flat and smooth Good Good writing experience
[0024] The above-mentioned examples only represent some embodiments of the present invention, and the description is specific and detailed, but should not be understood as a limitation on the patent scope of the present invention. It should be noted that those skilled in the art can make some modifications and improvements without departing from the idea of the present invention, all of which are within the scope of protection of the present invention. Therefore, the scope of protection of the patent of the present invention shall be subject to the appended claims.
Claims
1. Step 1: dry the tea leaves in the sun, crush them, blanch them in boiling water, add water and ultrasonicate them for a certain period of time, treat them with concentrated hydrochloric acid at 50-60°C for 1-2 hours, filter and wash them until they are neutral, treat them with sodium hydroxide liquid alkali with a mass concentration of 20-25% at 70-80°C for 4-5 hours, filter and wash them until they are neutral; Step 2: extracting the treated tea residue with water to obtain tea polyphenols and a slurry, respectively, and cooking the slurry, followed by squeezing and dehydrating to obtain a crude pulp; Step 3 of sequentially refining and screening the coarse pulp and then beating it; After beating, add β-cyclodextrin, sodium carboxymethylcellulose and reinforced starch, adjust pH to 7-8, dilute and add tea polyphenol obtained from step 2, mix uniformly, squeeze and dehydrate, and oven dry. A method for producing tea residue fiber raw material, comprising the steps of:
2. The tea residue is any one or a combination of tea stems, tea leaves, tea residue, tea residue after drinking, or any defective product generated during any tea manufacturing process; The method for producing tea residue fiber raw material according to claim 1.
3. The screen residue from step 3 is combined with the next coarse pulp for refining. The method for producing tea residue fiber raw material according to claim 1.
4. In step 3, the degree of beating is controlled to 30 to 40°SR. The method for producing tea residue fiber raw material according to claim 1.
5. the total amount of said β-cyclodextrin, sodium carboxymethylcellulose and reinforced starch is 10-20% of the bone-dry tea residue fiber raw material, and the mass ratio of said β-cyclodextrin, sodium carboxymethylcellulose and reinforced starch is 1:1-3:1-5; The method for producing tea residue fiber raw material according to claim 1.
6. Step 1: drying tea leaves in the sun, crushing them, blanching them in boiling water, adding water and ultrasonicating them for a certain period of time, treating them with concentrated hydrochloric acid at 50-60°C for 1-2 hours, filtering and washing until neutral, treating them with sodium hydroxide liquid alkali having a mass concentration of 20-25% at 70-80°C for 4-5 hours, filtering and washing until neutral; Step 2: adding an aqueous solution of sodium alginate and gelatin to the treated tea leaves, leaving the mixture at room temperature for a certain period of time, filtering the mixture, and washing the filter cake; Step 3 includes adding distilled water to the filter cake, shaking the mixture for 30 min-1 h, and then filtering and oven drying the mixture. A method for producing tea residue fiber raw material, comprising the steps of:
7. The tea residue is any one or a combination of tea stems, tea leaves, tea residue, tea residue after drinking, or any defective product generated during any tea manufacturing process; The method for producing tea residue fiber raw material according to claim 6.
8. The mass concentration of sodium alginate in the sodium alginate-gelatin aqueous solution is 10 to 20%, and the mass concentration of gelatin is 5 to 10%. The method for producing tea residue fiber raw material according to claim 6.
9. 9. Use of tea leaves raw material obtained by the manufacturing method according to any one of claims 1 to 8 in papermaking.
10. The tea leaves raw material obtained by the manufacturing method according to any one of claims 1 to 8 is processed into a powder of 50 to 60 mesh, and then the raw materials are blended with bleached sulfate softwood pulp based on a weight ratio composition of 10 to 20%:90 to 80%, and the raw materials are uniformly mixed, refined, beaten, molded into paper, pressed, dried in an oven, and sequentially wound and cut to complete the process. A method for producing writing paper comprising the steps of:
Citation Information
Patent Citations
Method for recycling tea leaf residues and tea paper for writing
CN106522019A
Papermaking method taking waste tea stems as raw materials
CN107287968A
Paper containing tea leaf residues and manufacturing method thereof
CN112064414A
Tea residue paper support and preparation method thereof
CN112111994A
Paper mixed with used tea leaf
JP2004143640A