Woven carbon fiber reinforced steel matrix composites

By using steel nanoparticles to sinter around carbon fibers at lower temperatures, a composite material with reduced density and enhanced strength is formed, addressing the integration challenge of steel and carbon fibers in conventional methods.

JP7579064B2Active Publication Date: 2024-11-07TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020050206
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-21
Filing Date
2020-03-19
Publication Date
2024-11-07
Estimated Expiration
2040-03-19

AI Technical Summary

Technical Problem

The challenge lies in forming a composite material of steel and reinforcing carbon fibers, as conventional steel forging temperatures exceed the thermal decomposition temperatures of certain polymers, making it difficult to integrate carbon fibers into a steel framework without destruction.

Method used

A method involving the use of steel nanoparticles with a reduced melting point, allowing sintering around carbon fibers at temperatures below 450°C to create a composite material with a continuous steel matrix and integrated reinforcing carbon fibers, achieving a lower density and enhanced structural strength.

Benefits of technology

The resulting composite material achieves a significant reduction in density, reaching up to 61% of conventional steel density, while maintaining considerable structural strength, including tensile strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579064000001
    Figure 0007579064000001
  • Figure 0007579064000002
    Figure 0007579064000002
Patent Text Reader

Abstract

To provide a composite having reinforcing carbon fiber integrated into and bonded to a steel framework, and production methods thereof.SOLUTION: Composite materials include a steel matrix 110 with reinforcing carbon fiber 120 integrated into the matrix. The composite materials have substantially lower density than steel, and are expected to have appreciable strength. Methods for forming composite steel composites include combining a reinforcing carbon fiber component 120, such as a woven polymer, with steel nanoparticles, and sintering the steel nanoparticles in order to form a steel matrix 110 with reinforcing carbon fiber 120 integrated therein.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates generally to metal / polymer composites, and more particularly to lightweight steel and carbon fiber reinforced composites and methods for making same. [Background technology]

[0002] The discussion of the background art provided in this disclosure is intended to generally present the context of the disclosure, and the inventors' work is not expressly or impliedly admitted as prior art to the present technology to the extent that it is described in this background art section, or in the manner of description that does not qualify as prior art at the time of filing.

[0003] Lightweight steel has many uses. In automobiles and aircraft, it improves fuel economy by reducing the weight of the vehicle. Mild steel has a strength of 7.88 g / cm 3 and certain polymers such as aromatic polyamides have a density of about 2.1 g / cm 3 Thus, a composite of the two materials provides a lightweight material that has significant strength with an overall reduced weight versus steel alone. Summary of the Invention [Problem to be solved by the invention]

[0004] Steel is typically formed by conventional forging methods at temperatures in excess of 1000°C, while certain polymers, such as aromatic polyamides, undergo thermal decomposition at 450°C. Because steel is typically formed at temperatures much higher than the typical thermal decomposition temperatures of polymeric materials, it is difficult to form true composites with reinforcing carbon fibers integrated into and bonded with a steel skeleton. Methods that allow for the formation of such composites are desirable. [Means for solving the problem]

[0005] This section provides a general overview of the disclosure, and is not an exhaustive disclosure of its entire scope or all of its features.

[0006] In various aspects, the present teachings provide a composite material having a continuous steel matrix of sintered steel nanoparticles and at least one reinforcing carbon fiber at least partially encapsulated within the steel matrix. In some embodiments, the at least one reinforcing carbon fiber is fully encapsulated within the continuous steel matrix. In some embodiments, the composite material has a mass of 5 g / cm. 3 The density may be less than 100 nm.

[0007] In another aspect, the present teachings provide a composite material that includes at least one reinforcing carbon fiber and a continuous steel matrix of sintered steel nanoparticles disposed about the at least one reinforcing carbon fiber.

[0008] In yet another aspect, the present teachings provide a method for forming a composite steel, the method including providing steel nanoparticles and combining the steel nanoparticles with a reinforcing carbon fiber component to form a non-annealed combination, the method further including sintering the steel nanoparticles around the reinforcing carbon fiber component by applying an elevated temperature to the non-annealed combination.

[0009] Further applications and various methods of enhancing the above bonding techniques will become apparent from the description provided herein. The description and specific examples in this summary are for purposes of illustration only and are not intended to limit the scope of the disclosure.

[0010] The present teachings will become more fully understood from the detailed description and the accompanying drawings, wherein: [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a cross-sectional view of a composite steel having a steel matrix with two layers of reinforcing carbon fibers. [Diagram 2] FIG. 2 is a pictorial representation of a portion of a process for forming a composite material of the type shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] It should be noted that the diagrams described herein are intended to illustrate general features of the methods, algorithms, and devices within the technology for purposes of describing certain aspects. These diagrams may not precisely reflect the features of any given aspect, and are not necessarily intended to define or limit specific embodiments within the scope of the technology. Furthermore, an aspect may incorporate features from a combination of diagrams.

[0013] The present disclosure relates generally to a composite material comprising a steel matrix with reinforcing carbon fibers integrated into the matrix. The composite material has a substantially lower density than steel and has significant strength. A method for forming a polymer-steel composite includes combining a reinforcing carbon fiber component, such as an aromatic polyamide, with steel nanoparticles and sintering the steel nanoparticles to form a steel matrix with reinforcing carbon fibers integrated into the matrix.

[0014] Conventional steel melts at temperatures above about 1200°C. Such high temperatures instantly destroy on contact various reinforcing carbon fibers, which decompose at or below about 450°C. Therefore, the present technique for forming steel / polymer composites uses steel nanoparticles to reduce the melting point of steel to below about 450°C. This allows the steel nanoparticles to sinter around the reinforcing carbon fiber components when combined and heated without destroying the reinforcing carbon fiber components. The result is a layer or extension of reinforcing carbon fibers interpenetrated in a steel matrix.

[0015] The composite materials of the present disclosure can have a much lower density than conventional steel, as low as 60% in one example, and can provide significant structural strength, including tensile strength.

[0016] Referring to FIG. 1, a carbon fiber reinforced steel matrix composite (CF-SMC) 100 includes a continuous steel matrix 110 and at least one reinforcing carbon fiber 120 at least partially encapsulated within the steel matrix. As shown, the reinforcing carbon fiber 120 can be provided as a layer of cloth, fabric, weave, yarn, or the like. In other examples, the reinforcing carbon fiber 120 can be provided as a fiber, yarn, or multiple aligned fibers. In various embodiments, the placement or alignment of the fiber, fabric, weave, or the like may be asymmetric to coordinate with a structural design or to maximize mechanical performance for a particular task. This allows for organized layout of fiber patterns that may not be available with traditional metal matrix composite (MMC) technology.

[0017] The continuous steel matrix 110 generally comprises sintered steel nanoparticles and compositionally comprises an alloy of at least iron and carbon. The continuous steel matrix 110 may optionally include any, some, or all of manganese, nickel, chromium, molybdenum, boron, titanium, vanadium, tungsten, cobalt, niobium, phosphorus, sulfur, and silicon. The relative ratios of the various elemental components of the steel matrix 110 may depend on the desired application and may generally be selected based on the common sense of one of ordinary skill in the art. For example, an application requiring stainless steel may include chromium present at 11% or more by weight of the total weight. In one disclosed embodiment, the steel matrix is ​​comprised of iron, carbon, and manganese present at 99.08%, 0.17%, and 0.75%, respectively, by weight of the steel matrix. It will be understood that the term "weight" as used herein is interchangeable with the term "mass."

[0018] In some implementations, the continuous matrix 110 can be formed of another high melting point / high sintering temperature metal in addition to or instead of steel. Non-limiting examples of high sintering temperature metals from which the matrix can alternatively be formed include titanium, tungsten, tantalum, vanadium, zirconium, ruthenium, platinum, rhodium, and rhenium. It will be understood that as used herein, the phrase "continuous steel matrix 110" can alternatively refer to a continuous matrix of any of the above metals.

[0019] In some embodiments, the term "continuous," as used in the phrase "continuous steel matrix 110," can mean that the steel matrix is ​​formed or exists as a single, integral body. In such embodiments, as a negative example, a structure formed of two separate steel bodies held together, such as by an adhesive or a weld, is discontinuous. In some embodiments, the term "continuous," as used herein, can mean that the continuous steel matrix 110 is substantially compositionally and structurally uniform throughout its occupied volume. For simplicity, the continuous steel matrix 110 is alternatively referred to herein as "steel matrix 110," i.e., the term "continuous" is sometimes omitted without changing the meaning.

[0020] In some implementations of the CF-SMC 100, the at least one reinforcing carbon fiber 120 may be completely encapsulated within the continuous steel matrix 110. In various embodiments, the phrase "encapsulated within the continuous steel matrix 110" may mean that the at least one reinforcing carbon fiber 120 is partially or completely encapsulated, enclosed, wrapped, integrated, or otherwise contiguous and surrounded within the continuous steel matrix 110. In some embodiments, the phrase "encapsulated within the continuous steel matrix 110" may mean that at least a portion of the individual fibers comprising the at least one reinforcing carbon fiber 120 are contiguous and surrounded by the continuous steel matrix 110. In some embodiments, the phrase "encapsulated within the continuous steel matrix 110" may mean that the continuous steel matrix 110 is partially or completely formed around or otherwise contiguous and disposed around the at least one reinforcing carbon fiber 120.

[0021] In some implementations, the phrase "encapsulated within the steel matrix" at least one reinforcing carbon fiber 120 means that the steel matrix 110 is formed around and with the reinforcing carbon fiber 120 with a sufficiently high degree of contact between the surface of the steel matrix 110 and the surface of the reinforcing carbon fiber 120 such that the reinforcing carbon fiber 120 is held in place relative to the steel matrix 110. In some implementations, the phrase "encapsulated within the steel matrix" means that the interacting surface of the steel matrix 110 is presented on all sides of the individual polymeric fibers that make up the reinforcing carbon fiber 120.

[0022] In some variations, the reinforcing carbon fiber 120 can include a combination of carbon fiber and ceramic fiber. In one non-limiting example, such ceramic fiber can include a basalt cloth or a silica cloth. In some such variations, the reinforcing carbon fiber 120 can include a weave or cloth formed from both carbon and ceramic fibers.

[0023] In various embodiments, the phrase "the reinforcing carbon fibers are held in place relative to the steel matrix with sufficiently high contact between the surface of the steel matrix and the surface of the reinforcing carbon fibers" can mean that at least 50%, or at least 60%, or at least 70%, or at least 80%, or at least 90% of the surface area of ​​the reinforcing carbon fibers 120 is in contact with the steel matrix.

[0024] Generally, the total density of CF-SMC100 is less than that of pure steel. For example, mild steel such as AISI grades 1005-1025 has a density of about 7.88 g / cm 3 In contrast, the exemplary CF-SMC 100 of the present disclosure has a density of 4.8 g / cm, which is about 61% of the density of mild steel. 3 In comparison, recently developed steel-aluminum alloys have a density of about 87% of that of mild steel.

[0025] Although FIG. 1 illustrates a CF-SMC 100 having two layers of reinforcing carbon fibers 120 encapsulated within a steel matrix 110, it can be understood that the composite can include any number of layers of reinforcing carbon fibers 120, one or more. In other words, at least one reinforcing carbon fiber 120 can, in some embodiments, include multiple mutually contacting or spatially separated layers of reinforcing carbon fibers. Furthermore, it is understood that the weight ratio of reinforcing carbon fibers 120 to steel matrix 110 in a CF-SMC 100 can vary significantly, and such variation can be achieved with the use of aromatic polyamide (approximately 2.1 g / cm 3 It will be appreciated that given the significantly different densities of various polymers, such as CF-SMC 100, and steel, this directly affects the density of the CF-SMC 100.

[0026] Thus, in some embodiments, the CF-SMC 100 of the present disclosure has a compressibility of 7 g / cm 3 In some embodiments, the density of the CF-SMC 100 of the present disclosure is less than 6 g / cm 3In some embodiments, the density of the CF-SMC 100 of the present disclosure is less than 5 g / cm 3 is less than.

[0027] Also disclosed is a method of forming a CF-SMC 100. With reference to FIG. 2, the method includes providing steel nanoparticles 210. The term "steel nanoparticles 210" generally refers to a sample consisting primarily of particles of steel having an average maximum dimension of less than 100 nm. The individual particles of steel nanoparticles 210 generally consist of any alloy, such as the compositions described above with respect to the steel matrix 110 of the CF-SMC 100. Thus, the individual particles of steel nanoparticles 210 generally include iron and carbon, and may optionally include any, some, or all of manganese, nickel, chromium, molybdenum, boron, titanium, vanadium, tungsten, cobalt, niobium, phosphorus, sulfur, and silicon.

[0028] As discussed above with respect to the steel matrix 110 of the CF-SMC 100, the relative proportions of the various elemental components of the steel nanoparticles 210 can depend on the desired application and are generally selectable based on the common sense of one of ordinary skill in the art. In the disclosed embodiment, the individual particles of the steel nanoparticles 210 are comprised of iron, carbon, and manganese present at 99.08%, 0.17%, and 0.75% by weight, respectively.

[0029] In various embodiments, the average largest dimension of the steel nanoparticles 210 can be determined by any suitable method, including but not limited to, x-ray diffraction (XRD), transmission electron microscopy, scanning electron microscopy, atomic force microscopy, photon correlation spectroscopy, nanoparticle surface area monitoring, condensation particle counter, differential mobility analysis, scanning mobility particle sizing, nanoparticle tracking analysis, aerosol time-of-flight mass spectrometry, or aerosol particle mass spectrometry.

[0030] In some embodiments, the average maximum dimension is an average by mass, and in some embodiments, an average by population. In some embodiments, the steel nanoparticles 210 can have an average maximum dimension of less than about 50 nm, less than about 40 nm, less than about 30 nm, less than about 20 nm, or less than about 10 nm.

[0031] In some embodiments, the average largest dimension can have a relative standard deviation, in some such embodiments, the relative standard deviation can be less than 0.1, and thus the steel nanoparticles 210 can be considered monodisperse.

[0032] 2, the method for forming the CF-SMC 100 additionally includes a step 215 of combining the steel nanoparticles 210 with a reinforcing carbon fiber component 220 to produce an unannealed combination. The reinforcing carbon fiber component 220 is identical to the reinforcing carbon fibers 120 described above for the CF-SMC 100 above, except that the reinforcing carbon fiber component 220 is not yet integrated into or encapsulated within the steel matrix 110 defined above. Thus, the reinforcing carbon fiber component 220 may include, for example, carbon fibers formed in any configuration designed to impart tensile strength in at least one dimension, and in some embodiments at least two dimensions.

[0033] In many embodiments, the combining step 215 involves sequentially combining at least one layer of steel nanoparticles 210 with at least one layer of reinforcing carbon fiber component 220, such that the unannealed combination consists of one or more layers of each of steel nanoparticles 210 and reinforcing carbon fiber component 220. Any number of layers of steel nanoparticles 210 and any number of layers of reinforcing carbon fiber component 220 can be used. It will be understood that in embodiments where reinforcing carbon fibers 120 are desired on the outer surfaces of the CF-SMC 100, the reinforcing carbon fiber component 220 will be the first and / or last consecutively layered component in the unannealed combination; and, in embodiments where reinforcing carbon fibers 120 are desired between the outer surfaces of the CF-SMC 100, a layer of reinforcing carbon fiber component 220 will precede, followed by a layer of steel nanoparticles 210.

[0034] The combining step 215 will generally involve combining the steel nanoparticles 210 and the reinforcing carbon fiber component 220 in a die, casting, mold, or other shaped structure having void spaces corresponding to the desired shape of the CF-SMC 100 to be formed. In some particular embodiments, at least one layer of steel nanoparticles 210 and at least one layer of reinforcing carbon fiber component 220 are combined in a heat press die 250.

[0035] In some embodiments, a method of forming a CF-SMC 100 can include manipulating steel nanoparticles 210 with one another in unlinked bonds within the reinforcing carbon fiber component 220. Such a manipulation step can be effective to maximize the surface area of ​​contact between the steel nanoparticles 210 and the reinforcing carbon fiber component 220 in the unannealed combination, improving the effectiveness of integration of the reinforcing carbon fibers 120 into the steel matrix 110 of the ultimately formed CF-SMC 100. Manipulating the steel nanoparticles 210 into the interstices of the reinforcing carbon fiber component 220 can be accomplished by any procedure effective to increase the surface area of ​​contact between the steel nanoparticles 210 and the reinforcing carbon fiber component 220, including, but not limited to, pressing, stirring, shaking, vibrating, sonicating, or any other suitable procedure.

[0036] The method for forming the CF-SMC 100 further includes sintering the steel nanoparticles 210 to convert the steel nanoparticles 210 to the steel matrix 110 such that the reinforcing carbon fiber components 220 become reinforcing carbon fibers 120 integrated into the steel matrix 110, thus converting the unannealed combination to the CF-SMC 100. The sintering step generally includes heating the unannealed combination to a temperature less than 450° C., a temperature high enough to sinter the steel nanoparticles 210. In some embodiments, the sintering step can include heating the unannealed combination to a temperature greater than 400° C. and less than 450° C. In some embodiments, the sintering step can include heating the unannealed combination to a temperature greater than 420° C. and less than 450° C.

[0037] In some embodiments, the sintering step can be accomplished by hot pressing, i.e., by applying high pressure 260 simultaneously with the application of high temperature. In some embodiments employing hot pressing, the high pressure can be at least 30 MPa, and in some embodiments, the high pressure can be at least 60 MPa. Depending on the sintering conditions of temperature and pressure, the duration of the sintering process can vary. In some embodiments, the sintering step can be carried out for a duration in the range of 2 to 10 hours, and in one disclosed embodiment, is carried out for a duration of 4 hours.

[0038] Carbon fiber reinforced steel matrix composites (CF-SMC) are made by charging alternating layers of steel powder and carbon fiber cloth into a die. The steel powder used can be nanoparticles, <45 micron powder, or a mixture of the two size regimes. The weave of the carbon fiber cloth is loose enough to allow interpenetration between the fibers so that the steel matrix around the reinforcement can be continuous after consolidation.

[0039] The carbon fiber cloth and steel powder are assembled in a die under an inert atmosphere (in an argon glove box) to prevent the formation of oxidized surfaces, and the final punch and die assembly is then compressed at 800 °C for 1 h at a pressure of 60 MPa under argon flow.

[0040] Carbon fibers have a lower density (~3.75 times) and higher tensile strength than steel. The addition of multiple carbon fiber layers to a steel matrix lowers the weight of the final composite (as a function of the lower carbon fiber density) and increases the tensile strength as a function of their contribution to the mechanical strength of the composite.

[0041] It will be appreciated that in some instances, providing steel nanoparticles 210 with a desired composition, average maximum dimension, and / or relative standard deviation of the average maximum dimension may be difficult to achieve by conventional methods. For example, "top-down" approaches involving fragmenting bulk steel into granular steel via milling, arc detonation, or other known procedures often provide steel particles that are too large and / or too non-uniform for effective sintering into a uniform and robust steel matrix 110. "Bottom-up" approaches, such as those involving chemical reduction of dissolved cations, are often inappropriate for various alloy nanoparticles due to incompatibility, or even unavailability, of the cations involved. For example, cationic carbon suitable for chemical co-reduction with cationic iron to form steel may be difficult to obtain. Moreover, even if these or other techniques may be effective in producing steel nanoparticles 210 of a given composition on a laboratory scale, scaling up may prove to be infeasible or uneconomical.

[0042] For these reasons, the step of providing steel nanoparticles 210 can in many embodiments be performed by a novel steel nanoparticle 210 synthesis using anionic elemental reagent complexes (AERCs). AERCs are generally reagents consisting of one or more elements that form complexes with hydride molecules and have the following formula I:

[0043] Formula:Q 0X y (Formula I)

[0044] In the formula, Q 0 represents a combination of one or more elements, each formally in oxidation state zero, not necessarily in equimolar ratio with respect to each other; X represents a hydride molecule, and y is an integer or fractional value greater than zero. AERCs of formula I can be formed by ball milling a mixture containing (i) a powder of each of the one or more elements present in the desired molar ratio, and (ii) a powder of a hydride molecule present in a molar ratio to the combined one or more elements corresponding to y. In many embodiments, the hydride molecule is borohydride, and in some particular embodiments, the hydride molecule is lithium borohydride.

[0045] Contacting the AERC of formula I with a suitable solvent and / or ligand molecules results in the formation of nanoparticles consisting essentially of one or more elements, the one or more elements being present in the nanoparticles in the same proportions as they are present in the AERC.

[0046] Thus, AERC suitable for use in the synthesis of steel nanoparticles 210 generally has the formula:

[0047] Fe a C b M d X y (Formula II)

[0048] where Fe is elemental iron, formally in oxidation state zero, C is elemental carbon, formally in oxidation state zero, M represents one or more elements in oxidation state zero, M represents one or more elements selected from the group including Mn, Ni, Cr, Mo, B, Ti, V, W, Co, Nb, P, S, and Si, X is a hydride molecule as defined with respect to formula I, a is a fraction or integer greater than zero, b is a fraction or integer greater than zero, d is a fraction or integer greater than zero, and y is a fraction or integer greater than zero. It will be understood that the values ​​of a, b, and c generally correspond to the molar ratios of the various components in the desired composition of the steel. Furthermore, it will be understood that M and d are shown as singular values ​​only for simplicity and can correspond to multiple elements present in non-equimolar amounts relative to each other. The AERC of formula II can alternatively be referred to as Steel-AERC.

[0049] The formation of steel-AERC can be accomplished by ball milling a pre-steel mixture containing (I) a powder of a hydride molecule, such as lithium borohydride, and (II) (i) iron powder, (ii) carbon powder, and (iii) optionally, a powder(s) of one or more elements selected from the group including Mn, Ni, Cr, Mo, B, Ti, V, W, Co, Nb, P, S, and Si. The mixture should contain iron powder, carbon powder, and any powder of one or more selected elements in the same weight ratios as the weight ratios of these various components in the desired steel product. For example, to synthesize a stainless steel type 316 product having 12 wt.% Ni, 17 wt.% Cr, 2.5 wt.% Mo, 1 wt.% Si, 2 wt.% Mn, 0.08 wt.% C, 0.045 wt.% P, and 0.03 wt.% S, the pre-steel mixture to be mixed with the powder of the hydride molecule for ball milling should contain the powders of each of these elements present in the weight percentages listed.

[0050] Thus, in some embodiments, the disclosed process for synthesizing steel nanoparticles includes contacting a steel-AERC as defined by Formula I or II with a solvent. In some embodiments, the disclosed process for synthesizing steel nanoparticles includes contacting a steel-AERC as defined by Formula I or II with a ligand. In some embodiments, the disclosed process for synthesizing steel nanoparticles includes contacting a steel-AERC as defined by Formula I or II with a solvent and a ligand. Contacting the steel-AERC with a suitable solvent or ligand forms steel nanoparticles 210 having an alloy composition determined by the composition of the steel-AERC, i.e., the composition of the pre-steel mix that forms the steel-AERC.

[0051] Non-limiting examples of suitable ligands include nonionic, cationic, anionic, amphoteric, zwitterionic, and polymeric ligands, and combinations thereof. Such ligands typically have a hydrocarbon-based, organosilane-based, or fluorocarbon-based lipophilic moiety. Without being limited thereto, examples of types of ligands that may be suitable include alkyl sulfates and sulfonates, petroleum and lignin sulfonates, phosphate esters, sulfosuccinate esters, carboxylates, alcohols, ethoxylated alcohols and alkylphenols, fatty acid esters, ethoxylated acids, alkanolamides, ethoxylated amines, amine oxides, nitriles, alkylamines, quaternary ammonium salts, carboxybetaines, sulfobetaines, or polymeric ligands. In some particular embodiments, the ligand may be at least one of a nitrile, an amine, and a carboxylate.

[0052] Non-limiting examples of suitable solvents may include any molecular species or combination of molecular species that can interact with the components of the AERC by means of non-bonded or transient bonded interactions. In different embodiments, solvents suitable for the synthesis of iron nanoparticles 210 from steel-AERC may be hydrocarbon or aromatic species, including but not limited to linear, branched, or cyclic alkyl, or alkoxy; or monocyclic or polycyclic aryl or heteraryl. In some embodiments, the solvent is a non-coordinating or sterically hindered ether. The solvent terms described may include deuterated or tritiated forms in some variations. In some embodiments, the solvent may be an ether, such as THF.

[0053] The present invention will be further described with reference to the following examples. It should be understood that these examples are provided to illustrate certain embodiments of the invention and should not be construed as limiting the scope of the invention. EXAMPLES

[0054] Example 1: Synthesis of steel nanoparticles Into a ball mill jar, add 0.0136 g carbon, 0.06 g manganese, 7.9264 g iron, and 6.28 g lithium borohydride. This is ball milled for 4 hours under inert atmosphere. The steel-AERC product is washed with THF to form steel nanoparticles with a composition of 99.08% Fe, 0.17% C, 0.75% Mn. The resulting steel nanoparticles are isolated.

[0055] Example 2: Formation of composite steel The steel nanoparticles of Example I are loaded into a punch and die having a dispersed layer of woven carbon fiber. The steel nanoparticle powder is encouraged to penetrate into the interstices between the fibers of the woven carbon fiber during the loading process. The material is then sintered at 430°C and 60 MPa for 4 hours. The product is a composite steel with reinforcing carbon fibers integrated into a steel matrix, as shown in Figures 1 and 2.

[0056] The foregoing description is merely exemplary in nature and is not intended to limit the disclosure, its application, or uses in any way. It should be understood that, as used herein, the phrases A, B, and at least one of C should be interpreted to mean the logic (A, B, or C) using the non-exclusive logic "or". Various steps within the method may be performed in different orders without changing the principles of the disclosure, and various steps may be performed independently or simultaneously unless otherwise stated. The disclosure of a range includes the disclosure of all ranges and subranges within the entire range.

[0057] The headings (such as "Background" and "Summary") and subheadings used herein are intended only for a general organization of topics within the disclosure and are not intended to limit the disclosure or any aspect thereof. The description of multiple embodiments having described features is not intended to exclude other embodiments having additional features or other embodiments incorporating different combinations of the described features.

[0058] As used herein, the terms "having" and "including," and variations thereof, are intended to be non-limiting, such that the recitation of a succession of items or lists is not an exclusion of other similar items that may also be useful in the devices and methods of the technology. Similarly, the terms "can" and "may be," and variations thereof, are intended to be non-limiting, such that a recitation that an embodiment can or may include particular elements or features does not exclude other embodiments of the technology that do not include those elements or features.

[0059] The broad teachings of the present disclosure can be implemented in various forms. Thus, while the present disclosure includes specific examples, the true scope of the present disclosure should not be so limited, since other modifications will become apparent to those skilled in the art upon review of this specification and the following claims. In this specification, reference to an aspect or various aspects means that a particular feature, configuration, or characteristic described in connection with an embodiment is included in at least one embodiment or aspect. The appearance of the phrase "in one aspect" (or variations thereof) does not necessarily refer to the same aspect or embodiment.

[0060] While particular embodiments have been described, presently unanticipated alternatives, modifications, variations, improvements, and substantial equivalents may occur to applicant or others skilled in the art. Accordingly, the appended claims, as filed and amended, are intended to cover all such alternatives, modifications, improvements, and substantial equivalents. Some of the embodiments of the invention related to the present invention are given below. [Embodiment 1] A composite material comprising a continuous matrix of sintered metal nanoparticles selected from the group consisting of steel and titanium, and at least one reinforcing carbon fiber at least partially encapsulated within the steel matrix. [Embodiment 2] 2. The composite material of embodiment 1, wherein the at least one reinforcing carbon fiber is completely encapsulated within the continuous matrix. [Embodiment 3] 2. The composite material of embodiment 1, wherein the at least one reinforcing carbon fiber is partially encapsulated within the continuous matrix. [Embodiment 4] 2. The composite material of embodiment 1, wherein the at least one reinforcing carbon fiber comprises a plurality of spatially separated layers of reinforcing carbon fiber. [Embodiment 5] 7g / cm 3 2. The composite material of claim 1 having a density of less than 1000 nm. [Embodiment 6] 6g / cm 3 2. The composite material of claim 1 having a density of less than 1000 nm. [Embodiment 7] 5g / cm 3 2. The composite material of embodiment 1, having a density of less than 1000 nm. [Embodiment 8] 2. The composite material of embodiment 1, wherein the continuous matrix comprises an alloy of iron and carbon and at least one element selected from the group including Mn, Ni, Cr, Mo, B, Ti, V, W, Co, Nb, P, S, and Si. [Embodiment 9] A composite material comprising: at least one reinforcing fiber structure comprising a combination of carbon fibers and ceramic fibers; and a continuous steel matrix of sintered steel nanoparticles disposed about said at least one reinforcing fiber structure. [Embodiment 10] 7g / cm 3 10. The composite material of embodiment 9, having a density of less than [Embodiment 11] 6g / cm 3 10. The composite material of embodiment 9, having a density of less than [Embodiment 12] 5g / cm 3 10. The composite material of embodiment 9, having a density of less than [Embodiment 13] 10. The composite of embodiment 9, wherein the continuous steel matrix comprises an alloy of iron and carbon and at least one element selected from the group including Mn, Ni, Cr, Mo, B, Ti, V, W, Co, Nb, P, S, and Si. [Embodiment 14] providing steel nanoparticles; combining the steel nanoparticles with a reinforcing carbon fiber component to form an unannealed combination; and sintering the steel nanoparticles to create a steel matrix; A method for producing a composite material, comprising: [Embodiment 15] 15. The method of claim 14, wherein the steel nanoparticles have an average largest dimension of less than about 20 nm. [Embodiment 16] synthesizing said steel nanoparticles by contacting an anionic elemental reagent complex (AERC) with a solvent; The process of embodiment 15, wherein the AERC has the formula: Fe a C b M d ·X y where Fe is elemental iron, formally in the oxidation state zero; C is elemental carbon, formally in the oxidation state zero; M represents one or more elements in the oxidation state zero, where M represents each of one or more elements selected from the group including Mn, Ni, Cr, Mo, B, Ti, V, W, Co, Nb, P, S, and Si; X is a hydride molecule; a is a fractional or integer value greater than zero; b is a fractional or integer value greater than zero; d is a fractional or integer value greater than zero; and y is a fractional or integer value greater than zero. [Embodiment 17] 17. The method of claim 16, comprising forming an AERC by ball milling a pre-steel mixture comprising a powder of hydride molecules, and iron and carbon powders. [Embodiment 18] 18. The method of claim 17, wherein the pre-steel mixture comprises a powder of one or more elements selected from the group including Mn, Ni, Cr, Mo, B, Ti, V, W, Co, Nb, P, S, and Si. [Embodiment 19] Providing steel nanoparticles includes synthesizing steel nanoparticles by a process including contacting steel-AERC with a ligand; The method of claim 14, wherein Steel-AERC has the formula: Fe a C b M d·X y where Fe is elemental iron, formally with an oxidation state of zero; C is elemental carbon, formally with an oxidation state of zero; M represents one or more elements with an oxidation state of zero, where M is one or more elements selected from the group including Mn, Ni, Cr, Mo, B, Ti, V, W, Co, Nb, P, S, and Si, each of which is a hydride molecule; a is a fractional or integer value greater than zero; b is a fractional or integer value greater than zero; d is a fractional or integer value greater than zero; d is a fractional or integer value greater than zero; and y is a fractional or integer value greater than zero.

Claims

1. a continuous matrix of sintered metal nanoparticles selected from the group consisting of steel and titanium; at least one of a carbon fiber cloth and a plurality of layers of woven carbon fiber fabric at least partially encapsulated within the continuous matrix.

2. The composite material of claim 1 , wherein at least one of said layers of carbon fiber cloth and woven carbon fiber fabric is completely encapsulated within said continuous matrix.

3. The composite material of claim 1 , wherein at least one of the layers of carbon fiber cloth and woven carbon fiber fabric is partially encapsulated within the continuous matrix.

4. 10. The composite material of claim 1, wherein the layers of woven carbon fiber fabric are spatially separated.

5. 7 g / cm 3 2. The composite material of claim 1 having a density of less than 1000 nm.

6. 6 g / cm 3 2. The composite material of claim 1 having a density of less than 1000 nm.

7. 5 g / cm 3 2. The composite material of claim 1 having a density of less than 1000 nm.

8. 2. The composite material of claim 1, wherein the continuous matrix comprises an alloy of iron and carbon and at least one element selected from the group including Mn, Ni, Cr, Mo, B, Ti, V, W, Co, Nb, P, S, and Si. (i) providing steel nanoparticles; (ii) combining the steel nanoparticles with a component comprising at least one of a carbon fiber cloth and a plurality of layers of a carbon fiber fabric to form an unannealed combination; and (iii) sintering the steel nanoparticles to create a steel matrix; A method for producing a composite material, comprising:

10. The method of claim 9, wherein the steel nanoparticles provided in step (i) have an average maximum dimension of less than 20 nm.

11. The steel nanoparticles provided in step (i) are synthesized by a process comprising contacting an anionic elemental reagent complex (AERC) with a solvent; The method of claim 10, wherein the AERC has the formula: Fe a C b M d X y where Fe is elemental iron, formally in an oxidation state of zero; C is elemental carbon, formally in an oxidation state of zero; M represents one or more elements in an oxidation state of zero, where M represents each of one or more elements selected from the group including Mn, Ni, Cr, Mo, B, Ti, V, W, Co, Nb, P, S, and Si; X is a hydride molecule; a is a fractional or integer value greater than zero; b is a fractional or integer value greater than zero; d is a fractional or integer value greater than zero; and y is a fractional or integer value greater than zero.

12. The method of claim 11, wherein the AERC is formed by ball milling a pre-steel mixture containing a powder of hydride molecules, as well as iron and carbon powders.

13. 13. The method of claim 12, wherein the pre-steel mix comprises powders of one or more elements selected from the group including Mn, Ni, Cr, Mo, B, Ti, V, W, Co, Nb, P, S, and Si.

14. The method of claim 13, wherein step (i) comprises synthesizing steel nanoparticles by a process comprising contacting a steel-AERC with a ligand; The method of claim 9, wherein the Steel-AERC has the following formula: Fe a C b M d X y where Fe is elemental iron, formally in an oxidation state of zero; C is elemental carbon, formally in an oxidation state of zero; M represents one or more elements in an oxidation state of zero, where M represents each of one or more elements selected from the group including Mn, Ni, Cr, Mo, B, Ti, V, W, Co, Nb, P, S, and Si; X is a hydride molecule; a is a fractional or integer value greater than zero; b is a fractional or integer value greater than zero; d is a fractional or integer value greater than zero; d is a fractional or integer value greater than zero; and y is a fractional or integer value greater than zero.

Citation Information

Patent Citations

  • Fiber-reinforced composite material

    JP2016151031A

  • carbon composite

    JP2017535499A

  • Reinforced structural element

    US20040086701A1

  • Composite metal foam and methods of preparation thereof

    US20120196147A1

  • Light weight composite of steel and polymer

    US20180079884A1