Pigment made of particles mainly composed of calcium titanium composite oxide, its manufacturing method and use

The calcium titanium composite oxide pigment addresses the unnatural white cast issue in cosmetics by transmitting light in the warm color range and offering high hiding power, serving as a titanium oxide substitute for natural skin tone coverage and UV protection.

JP7579567B2Active Publication Date: 2024-11-08TITAN IND INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020198705
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-30
Publication Date
2024-11-08
Estimated Expiration
2040-11-30

AI Technical Summary

Technical Problem

Existing cosmetics using titanium oxide pigments face issues with high hiding power leading to an unnatural white cast and the need for alternative materials that provide natural skin tone coverage without health hazards.

Method used

A pigment composed of calcium titanium composite oxide particles with a specific speckled pattern and true density within a certain range, which preferentially transmits light in the warm color range and offers high hiding power, serving as a substitute for titanium oxide.

Benefits of technology

The calcium titanium composite oxide pigment achieves a natural skin tone finish by scattering light in the warm color range, providing effective coverage and UV protection, while reducing the use of titanium oxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579567000005
    Figure 0007579567000005
  • Figure 0007579567000006
    Figure 0007579567000006
  • Figure 0007579567000007
    Figure 0007579567000007
Patent Text Reader

Abstract

To provide a pigment mainly used for cosmetic applications, which preferentially transmits light in a warm color region and has a large hiding power, and to provide a method for producing the same and a method of using the same.SOLUTION: A pigment comprises particles mainly composed of a calcium-titanium composite oxide, in which, when the particles of the calcium-titanium composite oxide in the pigment are observed by a transmission electron micrograph at a magnification of 100,000 times, the particles can be observed to have spots of lighter color than the surrounding, and which has a true density of 3500 kg / m3 to 3790 kg / m3.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pigment comprising particles containing calcium titanium composite oxide as a main component, and in particular to said pigment having a warm color light transmitting effect and further having a large hiding power. [Background technology]

[0002] Conventionally, makeup cosmetics such as foundations have been used as cosmetics that change the skin tone by adding colorants such as titanium dioxide pigments, which have high coloring power, and other inorganic pigments and organic pigments in order to cover redness, dullness, spots, freckles, and the like caused by the skin and to create a uniform and beautiful looking skin.

[0003] Regarding the titanium dioxide, pigments with high hiding power are generally used to make the skin tone uniform. If a pigment with low hiding power is used in a cosmetic, a large amount of the pigment must be blended to achieve sufficient hiding power, which deteriorates the usability of the cosmetic. Patent No. 2584562 (Patent Document 1) proposes a cosmetic with high hiding power that contains spherical or elliptical titanium dioxide.

[0004] However, when applying makeup to the skin using foundation or concealer containing titanium dioxide, which has a high hiding power, the intensity of the white scattered light tends to become too strong, causing the finished makeup to look pale and unnatural, which is a problem known as the white cast phenomenon.

[0005] One of the means for preventing the white cast phenomenon is to use rutile titanium dioxide of a specific shape to balance the coloring power, hiding power, and the intensity of the white scattered light. For example, Japanese Patent No. 4684970 (Patent Document 2) describes blending in cosmetics an aggregate of fan-shaped rutile titanium dioxide particles in which rod-shaped primary particles are aggregated and / or bonded. In addition, Japanese Patent No. 6258462 (Patent Document 3) describes blending in cosmetics a rutile titanium dioxide powder obtained by firing rutile titanium dioxide having needle-shaped protrusions on the particle surface.

[0006] Another method for preventing the white cast phenomenon is to utilize the scattering of light in the warm color region inside the skin. Patent No. 5363696 (Patent Document 4) describes that a study was conducted focusing on light propagating inside bare skin. Specifically, in a light scattering medium such as skin, a part of the light irradiated onto the skin is transmitted inside and reflected by the internal scatterers, so that it is emitted from a part different from the irradiated part. However, it describes that by using a coloring material with a low light absorption rate in the wavelength range of 630 nm to 700 nm in a skin cosmetic, the distribution of the above-mentioned emission parts becomes close to that of bare skin, and a natural texture can be obtained.

[0007] However, in recent years, the possibility of health damage from titanium dioxide (IV), including rutile-type titanium dioxide, cannot be denied, and there has been a growing trend, mainly in Europe, to reduce the amount of titanium dioxide used and to use alternative materials. JP-A-5-339121 (Patent Document 5) proposes the use of compounds having a perovskite crystal structure, such as calcium titanate, strontium titanate, barium titanate, calcium zirconate, and strontium zirconate, as pigments other than rutile-type titanium dioxide. Patent No. 3464564 (Patent Document 6) also describes an ultraviolet protection cosmetic composition using particles of a complex oxide having a perovskite structure or a solid solution thereof. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 2584562 [Patent Document 2] Patent No. 4684970 [Patent Document 3] Patent No. 6258462 [Patent Document 4] Patent No. 5363696 [Patent Document 5] Japanese Patent Application Publication No. 5-339121 [Patent Document 6] Patent No. 3464564 Summary of the Invention [Problem to be solved by the invention]

[0009] However, in Patent Document 5, only the smoothness, adhesion, and covering power are discussed, and the countermeasure against the white cast phenomenon is not considered. In addition, Patent Document 5 only describes blending a powder consisting of a compound having a perovskite crystal structure, an average particle size in the range of 0.05 to 15 μm, and particles having an equiaxed shape into a cosmetic, but does not describe a specific method for producing such a powder. In addition, Patent Document 6 describes the synthesis of a double oxide powder represented by CaTiO3, but does not describe a specific example of blending this powder into a cosmetic, and although it describes the UV protection effect, safety, and stability of a cosmetic containing a double oxide having a perovskite crystal structure, it does not consider the countermeasure against the white cast phenomenon and the hiding power.

[0010] Although progress is being made in the development of alternative materials to titanium dioxide, the development of cosmetics that provide a natural finish and have strong hiding power is still in its infancy.

[0011] An object of the present invention is to provide a pigment that realizes a natural finish by preferentially transmitting light in the warm color region, has a high hiding power, and can be used as an alternative material to titanium oxide. [Means for solving the problem]

[0012] The present inventors focused on calcium titanium composite oxide as an alternative material to titanium oxide, and as a result of extensive research, discovered that a pigment consisting of particles mainly composed of calcium titanium composite oxide, which shows a specific spotted pattern when observed under a transmission electron microscope, and which has a true density within a specific range, preferentially transmits light in the warm color range and has great hiding power.

[0013] The present invention includes, but is not limited to, the following: [1] A pigment consisting of particles mainly composed of calcium titanium composite oxide, When the calcium titanium composite oxide particles in the pigment were observed under a transmission electron microscope at a magnification of 100,000 times, it was confirmed that the particles contained dots of areas that were lighter in color than the surrounding area. True density is 3500kg / m 3 More than 3790kg / m 3 The pigment, which is: [2] The shape of the part that is lighter in color than the surrounding area is a circle with a diameter of 1.5 nm to 15.0 nm or an ellipse with a major axis length of 1.5 nm to 15.0 nm, and The area that is lighter in color than the surrounding area is 1.0×10 4 nm 2 The pigment according to [1], wherein the pigment is present in a range corresponding to 100 to 200 particles. [3] The pigment according to [1] or [2], wherein the number average diameter or major axis length of the part that is lighter in color than the surrounding area is 2.5 nm or more and 4.5 nm or less. [4] The pigment according to any one of [1] to [3], having a particle diameter of 200 nm or more and 500 nm or less. [5] A pigment according to any one of [1] to [4], wherein the particle size distribution width set in JIS Z 8825: 2013 is less than 10.00. [6] The pigment according to any one of [1] to [5], in which, in X-ray diffraction measurement, when the integrated diffraction intensity of the diffraction line of the (1 2 1) plane appearing in the diffraction angle range of 32.50° to 33.50° is taken as 100.0, the ratio of the integrated diffraction intensity of the diffraction line appearing in the diffraction angle range of 24.75° to 28.00° is 12.00 or less. [7] The pigment according to any one of [1] to [6], having an inorganic and / or organic coating layer on at least a portion of the surface of the particle. [8] Preparing an aqueous solution containing a titanium source and a calcium source; heating the aqueous solution to react the titanium source and the calcium source to form a reactant; The reaction product is subjected to a calcium removal treatment, and then subjected to solid-liquid separation to recover a solid content; and The resulting solid is heated. A method for producing the pigment according to any one of [1] to [7], comprising: [9] Mixing an acid peptized product of a hydrolysis product of a titanium compound, a water-soluble compound containing calcium, and an alkali, and heating the mixture to 70°C or higher and 100°C or lower under normal pressure to generate a reaction product; The reaction mixture is cooled and then maintained at a pH of 7.0 or less for 1 hour or more. The reaction product after the above retention is subjected to solid-liquid separation to recover a solid content, and The solid content is fired at 500°C or higher. A method for producing the pigment according to any one of [1] to [7], comprising:

[10] A cosmetic preparation comprising the pigment according to any one of [1] to [7].

[11] A resin composition comprising the pigment according to any one of [1] to [7].

[12] A paint comprising the pigment according to any one of [1] to [7].

[13] An ink comprising the pigment described in any one of [1] to [7]. Effect of the Invention

[0014] The pigment obtained by the present invention, which is composed of particles containing calcium titanium composite oxide as a main component, transmits light in the warm color region preferentially and has a large hiding power.

[0015] The pigment composed of particles containing the calcium titanium composite oxide as a main component obtained by the present invention, when used as an ingredient in cosmetics to be applied to the skin, such as foundation, can provide a cosmetic product with a natural finish and high hiding power, since the transmitted light in the warm color region is scattered inside the skin.

[0016] The pigment obtained by the present invention can also be used as a substitute for titanium oxide. The calcium titanium composite oxide used in the pigment of the present invention has an ultraviolet ray shielding effect equivalent to that of titanium oxide, and can therefore be used in sun creams and the like.

[0017] The pigment obtained by the present invention can be used in a wide range of applications, including fields other than cosmetics, by taking advantage of its ability to transmit light in the warm color region and its high hiding power. Examples of such applications include, but are not limited to, adding the pigment to a resin to form a resin composition having a warm color light transmitting effect, adding the pigment to a paint to use in a paint for housing, etc. [Brief description of the drawings]

[0018] [Figure 1] 1 is a transmission electron microscope photograph of the pigment obtained in Example 5. [Diagram 2] 1 is a transmission electron microscope photograph of the pigment obtained in Example 3. [Diagram 3] 1 is a transmission electron microscope photograph of the pigment obtained in Comparative Example 3. [Figure 4] A rectangle with an area of ​​1.0×104 nm2 was drawn on a transmission electron microscope photograph of the pigment obtained in Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention relates to a pigment comprising particles containing calcium titanium composite oxide as a main component, and when the calcium titanium composite oxide particles in the pigment are observed under a transmission electron microscope at a magnification of 100,000 times, it can be confirmed that the particles have dotted areas that are lighter in color than the surrounding area, and the pigment has a true density of 3,500 kg / m 3 More than 3790kg / m 3 The following relates to pigments:

[0020] "A pigment composed of particles mainly composed of calcium titanium composite oxide" means that the individual particles constituting the pigment are mainly particles of calcium titanium composite oxide. Specifically, it means that 850 g / kg or more, preferably 900 g / kg or more of the individual particles constituting the pigment are particles of calcium titanium composite oxide. The individual particles constituting the pigment of the present invention may contain, in addition to calcium titanium composite oxide, unreacted materials during the synthesis reaction of calcium titanium composite oxide, unavoidable impurities derived from the raw materials, and inorganic and / or organic substances derived from the coating layer.

[0021] The calcium titanium composite oxide, which is the main component of the particles constituting the pigment of the present invention, is preferably an orthorhombic calcium titanium composite oxide. "Orthorhombic calcium titanium composite oxide" refers to a calcium titanium composite oxide in which the angles between the three different crystal axes are all 90°.

[0022] As shown in Figures 1 and 2, the calcium titanium composite oxide particles in the pigment of the present invention are characterized by the presence of dark and light colored areas within the particles in transmission electron micrographs. Specifically, when observed in a transmission electron micrograph at a magnification of 100,000 times, it can be confirmed that light colored areas are dotted like spots within the dark colored areas. The inventors have found that when this spotted pattern is observed in the calcium titanium composite oxide particles, the warm color light transmission effect of the pigment is improved. Although the relationship between this spotted pattern and the warm color light transmission effect has not been clarified, the reason for the above effect is speculated as follows: It is believed that voids are generated inside the particles during the synthesis process of the pigment of the present invention. When observed under a transmission electron microscope, the areas corresponding to the voids are lighter in color than the surrounding areas. Since light with a short wavelength is easily scattered and reflected by such voids, it is believed that light in the warm color range is preferentially transmitted through the pigment of the present invention. It is believed that these "voids" include both those that are connected to other voids or the outside, and those that are not connected. The present inventors have found for the first time that calcium titanium composite oxide particles that show the above-mentioned spotted pattern when observed in a transmission electron microscope photograph can be produced by the method described below. When a commercially available calcium titanium composite oxide was observed in a transmission electron microscope photograph, no spotted pattern was observed, as shown in Figure 3.

[0023] The above-mentioned spotted pattern in the calcium titanium composite oxide particles in the pigment of the present invention is preferably distributed uniformly throughout the particle. However, in a transmission electron microscope photograph, the particles may overlap, or the thickness of the particles may be specifically large in some areas, making it impossible to observe light-colored parts. If there is no overlap between the particles, the thickness of the particles will not be specifically large at the outer edge of the particles. Therefore, when the particles having a spotted pattern in the present invention are observed in a transmission electron microscope photograph at a magnification of 100,000 times, the spotted pattern can usually be observed at least at the outer edge. On the other hand, if there is no overlap between the particles and the spotted pattern cannot be observed even at the outer edge of the particles in a transmission electron microscope photograph at a magnification of 100,000 times, it can be determined that the particle does not have a spotted pattern.

[0024] The pigment of the present invention is also characterized by a small true density, as evaluated by the method described below. The true density of the pigment of the present invention is 3500 kg / m 3 More than 3790kg / m 3 The above spotted pattern can be observed and the true density is 3790 kg / m or less. 3When the particle size is less than 100,000, the hiding power is improved in addition to the warm color light transmission effect. The hiding power depends on the shape of the particle itself. Specifically, rectangular parallelepiped particles, which will be described later, tend to have a higher hiding power overall than roughly spherical particles. However, when comparing particles of the same shape, a spotted pattern can be observed in a transmission electron microscope photograph at a magnification of 100,000 times, and the true density is 3790 kg / m 3 It was found that the hiding power is greater when the density is 3,500 kg / m or less. The relationship between true density and the improvement of hiding power has not been clarified, but it is believed that when the true density is low, sufficient voids are formed inside the particles, making it easier for light to be scattered and reflected, and thus improving the hiding power in addition to the warm light transmission effect. 3 If it is smaller, the particles may easily disintegrate and the usability as a cosmetic material may deteriorate, so the true density is 3500 kg / m 3 The above is preferred.

[0025] The light-colored dots mentioned above have a circular shape with a diameter of 1.5 nm to 15 nm or an elliptical shape with a major axis length of 1.5 nm to 15 nm, and are smaller than 1.0 × 10 on a transmission electron microscope photograph at a magnification of 100,000 times. 4 nm 2 It is preferable that 100 to 200 particles are present in the range corresponding to the above, because the effect of further improving the hiding power is observed when comparing particles of the same shape. In addition, the number average value of the diameter or major axis length (hereinafter also referred to as "number average diameter") is preferably 2.5 nm to 4.5 nm, more preferably 2.5 nm to 4.2 nm, and even more preferably 3.0 nm to 4.2 nm. If the number average diameter of the particles is 2.5 nm or more, the hiding rate evaluated by the method described below is likely to be large, and if it is 4.5 nm or less, it is likely that the structural stability of the particles is easily obtained. Note that the above "circular" is not intended to be limited to only a perfect circle, but is intended to include shapes close to a circle. The same applies to "elliptical".

[0026] In addition, the 1.0×10 4 nm2 It is believed that the presence of 100 or more light-colored areas in the area corresponding to the number of light-colored areas is sufficient to cause the short-wavelength light to be sufficiently scattered in the voids inside the particle, resulting in preferential transmission of light in the warm color range and improving the hiding power of the pigment. On the other hand, if the number of light-colored areas is more than 200, the hiding power will not be further improved, and if the number of light-colored areas is more than 200, the particles will be prone to collapse due to the large number of voids inside the particles, which will deteriorate the usability as a cosmetic material. Therefore, it is preferable that the number of light-colored areas is 200 or less. A method for measuring the diameter or long axis length of a part that is lighter in color than the surrounding area on a 100,000x transmission electron micrograph, and a method for measuring the diameter or long axis length of a part that is lighter in color than the surrounding area on a 1.0 x 10 4 nm 2 A specific method for measuring the number of areas that are lighter in color than the surrounding areas in the area corresponding to the area will be described later.

[0027] The pigment obtained by the present invention has a particle shape of approximately spherical or rectangular. The term "approximately spherical" refers to a particle shape in which the primary particles or secondary particles grow isotropically in a crystallographic manner or form an aggregate isotropically, as shown in FIG. 1, and have an irregular or nearly spherical outer shape. For example, a rectangular shape as shown in FIG. 2, or a long and slender needle shape, or a shape with a protrusion as long as or longer than the diameter of the center like a sea urchin, are not included in the term "approximately spherical". The term "rectangular" refers to a particle shape in which the primary particles or secondary particles grow more in a crystallographic manner in a specific axial direction than in the other two axes, or form aggregates more in a specific axial direction, as shown in FIG. 2, and have an outer shape close to a rectangular parallelepiped. When referring to a "rectangular parallelepiped", it is not necessary for the particle to be a perfect rectangular parallelepiped (all six faces are formed as rectangles or squares). In addition, the shape of the particle cross section perpendicular to the long axis direction does not have to be rectangular or square, and all cross sections do not have to have the same shape. The phrase "particle shape is approximately spherical" or "particle shape is rectangular" means that 80% or more, and preferably 85% or more by number of the particles constituting the pigment of the present invention are approximately spherical or rectangular, respectively.

[0028] Although it is difficult to generalize, pigments made of roughly spherical particles are suitable for achieving a smooth feel when used in cosmetics, whereas pigments made of rectangular particles tend to have greater hiding power than roughly spherical particles, and are therefore suitable for obtaining cosmetics that require hiding power. The pigment of the present invention has the advantage that a rectangular parallelepiped shape provides greater hiding power than a roughly spherical shape, but the pigment of the present invention is not limited to a rectangular parallelepiped shape. For example, when it is desired to make the particle shape of the pigment roughly spherical in accordance with the desired texture of the cosmetic, the pigment according to the present invention can be produced by "observing particles of calcium titanium composite oxide in a transmission electron microscope photograph at a magnification of 100,000 times, it can be confirmed that there are dotted areas within the particles that are lighter in color than the surrounding area, and the true density is 3,500 kg / m 3 More than 3790kg / m 3 By using a pigment that uses approximately spherical particles having the characteristic that the hiding power is less than or equal to the pigment diameter, it is possible to obtain an advantage that a greater hiding power can be obtained compared to a pigment that uses approximately spherical particles that do not have such a characteristic.

[0029] The pigment of the present invention preferably has a particle size of 200 nm or more and 500 nm or less. If the particle size is within this range, light scattering tends to occur, and a large hiding power tends to be obtained. The method for measuring the particle size of the pigment will be described later.

[0030] The pigment of the present invention preferably has a narrow particle size distribution. If the particle size distribution is wide, the particle size becomes non-uniform, and when used in cosmetics, the packing rate decreases, and the hiding power tends to decrease. The particle size distribution is preferably 10.00 or less, more preferably 8.00 or less, and even more preferably 5.00 or less. The method for measuring the particle size distribution of the pigment will be described later.

[0031] Since the pigment of the present invention may be used as an alternative material to cosmetics using titanium oxide, it is desirable that the content of titanium oxide is small. In order to calculate the exact content of titanium oxide in calcium titanium composite oxide, it is necessary to mix the pigment of the present invention with titanium oxide, perform X-ray diffraction measurement by powder method, and create a calibration curve, but this method requires a lot of time and cost. Therefore, as a method for confirming that the content of titanium oxide is small more simply, there is a method of comparing the integrated diffraction intensity ratio of the diffraction line of the (1 2 1) plane that appears in the range of 32.50° to 33.50°, which has the highest integrated diffraction intensity in calcium titanium composite oxide, and the diffraction line that appears in the range of 24.75° to 28.00°, which has the highest integrated diffraction intensity in rutile, anatase, and brookite titanium oxide, in X-ray diffraction measurement by powder method. In the present invention, when the integrated diffraction intensity of the (1 2 1) plane diffraction line appearing at angles of 32.50° to 33.50° is taken as 100.0, the ratio of the integrated diffraction intensity of the diffraction line appearing at angles of 24.75° to 28.00° (hereinafter referred to as "XRD titanium oxide integrated diffraction intensity") is preferably 12.00 or less. If such conditions are satisfied, the content of titanium oxide in the pigment can be considered to be low. The above-mentioned XRD titanium oxide integrated diffraction intensity is more preferably 11.00 or less, and even more preferably 8.50 or less. In addition, the diffraction line of the (1 1 1) plane of calcium titanium composite oxide exists in the range of 24.75° to 28.00°, and when the integrated diffraction intensity of the (1 2 1) plane diffraction line is taken as 100.0, the integrated diffraction intensity of the (1 1 1) plane diffraction line is about 3, so even if no titanium oxide is contained, the above-mentioned integrated diffraction intensity is not zero.

[0032] The color of the pigment of the present invention is not particularly limited, however, since it may be used as a substitute for titanium oxide, it is preferably white like titanium oxide.

[0033] The pigment of the present invention may have a coating layer made of an inorganic substance on the surface of the particle in order to impart hydrophobicity, optical properties, etc. Also, a coating layer made of an organic substance may be present. Two or more coating layers may be present, or the pigment may include both an inorganic layer and an organic layer.

[0034] The pigment of the present invention preferably has a warm color light transmission effect of 0.580 or more, calculated by the method described below. If the warm color light transmission effect is 0.580 or more, when used in a cosmetic, the warm color region is sufficiently reflected inside the skin, and a natural finish is obtained. There is no particular upper limit for the warm color light transmission effect, but the theoretical maximum value of the warm color light transmission effect calculated by the evaluation method used in the present invention is 1.000.

[0035] The pigment obtained by the present invention preferably has a large hiding power. When the hiding ratio, which is an index of hiding power, is evaluated by the method described below, the hiding ratio is preferably 0.690 or more for pigments having approximately spherical particles. A pigment having an approximately spherical particle shape and a hiding ratio within the above-mentioned range can impart a smooth feel and hiding power to cosmetics. A pigment having rectangular particles preferably has a hiding ratio of 0.730 or more. A pigment having a rectangular particle shape and a hiding ratio within the above-mentioned range can impart a very large hiding power to cosmetics. There is no particular upper limit for the hiding ratio, but the theoretical maximum value of the hiding ratio calculated by the evaluation method used in the present invention is 1.00.

[0036] An example of the method for producing the pigment of the present invention will be described below. However, the method for producing the pigment of the present invention is not limited to the following.

[0037] The pigment of the present invention, which is composed of particles mainly composed of calcium titanium composite oxide and has the above-mentioned characteristics, can be produced by heating an aqueous solution containing a titanium source and a calcium source to react the titanium source with the calcium source to generate a reaction product, subjecting the resulting reaction product to a decalcification treatment, then performing solid-liquid separation to recover the solid content, and heating (calcining) the resulting solid content. The titanium source is preferably an acid peptized product of a hydrolyzate of a titanium compound, typically a deflocculated product of metatitanic acid obtained by a method called the sulfuric acid method. When reacting the titanium source and the calcium source, it is preferable to mix an alkali and heat the mixture at normal pressure to 70°C or higher and 100°C or lower (normal pressure heating reaction method). When decalcification treatment is performed, it is preferable to cool the reaction product obtained by the normal pressure heating reaction method and then hold it at pH 7.0 or lower for 1 hour or more. The resulting solid content is preferably calcined at 500°C or higher.

[0038] (Sulfuric acid method) Ilmenite ore is dissolved in concentrated sulfuric acid, the resulting iron sulfate components are removed, and a hydrolysis process is carried out to obtain metatitanic acid, which has the chemical formula TiO(OH)2.

[0039] (Normal pressure heating reaction method) An example of the acid peptized product of the hydrolyzate of a titanium compound, which is a representative example of a titanium source, is an acid peptized product of metatitanic acid. As the metatitanic acid, it is preferable to use a compound having a sulfur content (SO3 equivalent) of 15 g / kg or less, preferably 10 g / kg or less, as the hydrolyzate of a titanium compound, and to use the hydrolyzate which is peptized by adjusting the pH of the hydrolyzate to 0.8 to 1.5 using hydrochloric acid. By using the peptized product of metatitanic acid thus obtained as the titanium source, it is possible to obtain calcium titanium composite oxide particles having a narrow particle size distribution. If the sulfur (SO3 equivalent) in the metatitanic acid exceeds 15 g / kg, peptization may not proceed. In addition to hydrochloric acid, nitric acid, hydrogen bromide, hydrogen iodide, formic acid, acetic acid, etc. can also be used. In addition, instead of the acid peptized product of the hydrolyzate of a titanium compound, the peptized product neutralized with an alkali can also be used.

[0040] The calcium source (water-soluble compound containing calcium) is not particularly limited, but examples thereof include calcium hydroxide and calcium carbonate. Factors that affect the crystallinity and particle size of the pigment composed of particles mainly composed of calcium titanium composite oxide obtained by the normal pressure heating reaction method include the concentration and mixing ratio of the raw materials, the concentration of the alkali, the reaction temperature, and additives. The mixing ratio of the titanium source and the water-soluble compound containing calcium is preferably such that the amount of calcium (Ca element) is 1.00 to 1.60 times the amount of titanium (Ti element), more preferably 1.10 to 1.50 times. Since the acid peptized product of the hydrolyzate of the titanium compound used as the titanium source has low solubility in water, when the amount of calcium is smaller than the amount of titanium, not only calcium titanium composite oxide particles but also unreacted titanium oxide tends to remain in the reaction product. The concentration of the acid peptized product of the hydrolyzate of the titanium compound in the mixture in the normal pressure heating reaction method is preferably 0.5 mol / L to 1.5 mol / L in terms of Ti, more preferably 0.7 mol / L to 1.4 mol / L.

[0041] During the normal pressure heating reaction, it is preferable to add an alkali in addition to the titanium source and calcium source. As the alkali, a caustic alkali can be used, and among them, sodium hydroxide is preferable. The concentration of the alkali in the mixture during the normal pressure heating reaction is preferably 0.1 mol / L or more, more preferably in the range of 0.5 mol / L or more and 3.6 mol / L or less.

[0042] The higher the reaction temperature, the better the crystallinity of the product. However, since a pressure vessel is required for a reaction at a temperature above 100°C, a practical range of 70°C to 100°C is appropriate, and a range of 70°C to less than 100°C is also acceptable.

[0043] When the shape of the calcium titanium composite oxide particles is approximately spherical, one or more sugars selected from monosaccharides and disaccharides such as glucose and maltose may be added as additives during normal pressure heating reaction. When adding such sugars, the total concentration of these is preferably 0.0115 mol / mol or more and 0.0195 mol / mol or less relative to the amount of calcium added during normal pressure heating reaction. If the concentration is less than 0.115 mol / mol, the particles will not be approximately spherical, and if it is more than 0.195 mol / mol, titanium oxide tends to remain. In addition, the particle size generally tends to become smaller when the amount of sugar added is large, but it is preferable that the particle size is not too small when used as a cosmetic, and from this point of view, the concentration of the sugar added is preferably 0.195 mol / mol or less.

[0044] During the normal pressure heating reaction, one or more compounds selected from aliphatic hydroxy acid compounds such as citric acid and isocitric acid may be added. When an aliphatic hydroxy acid compound is added, the aspect ratio of the calcium titanium composite oxide particles increases. When an aliphatic hydroxy acid is added, the amount of the added aliphatic hydroxy acid is preferably 0.0180 mol / mol or less relative to the amount of calcium added during the normal pressure heating reaction.

[0045] (Calcium removal treatment) After synthesizing calcium titanium composite oxide by normal pressure heating reaction, it is preferable to carry out calcium removal treatment to prevent unreacted calcium from remaining and interfering with surface treatment. The calcium removal treatment includes cooling the reaction product from the normal pressure heating reaction to 55°C or less, and then adjusting the pH to 7.0 or less using an acid. The pH is more preferably 6.0 or less. The lower limit of the pH is preferably 2.5 or more, more preferably 4.5 or more. Examples of the acid used to adjust the pH include hydrochloric acid, nitric acid, and acetic acid. If the pH is higher than 7.0, there is a risk that unreacted calcium cannot be completely removed. On the other hand, if the pH is lower than 2.5, the calcium in the calcium titanium composite oxide may flow out into the acid, and titanium oxide may be partially generated.

[0046] (Firing) After the calcium removal treatment, it is preferable to separate the solids from the solids and recover the solids, and then calcinate the solids. The higher the calcination temperature, the higher the hiding power of the pigment. However, calcination at a temperature higher than 900°C is not preferable because it may reduce the pores inside the pigment particles. The calcination temperature in the production of the pigment of the present invention is preferably 500°C or higher and 900°C or lower.

[0047] (Surface coating treatment) The pigment of the present invention may have an inorganic coating layer such as a hydrous oxide or oxide of metals such as aluminum, silicon, zinc, titanium, zirconium, iron, cerium, and tin on at least a part of the particle surface in order to improve the dispersion stability and durability in a dispersion medium when producing a cosmetic product. Metal salts other than those mentioned above may be used as the inorganic coating. In addition, an organic coating layer may be applied to at least a part of the particle surface in order to perform surface modification, typically hydrophobic treatment. Examples of organic coatings include silicone compounds such as dimethylpolysiloxane and methylhydrogenpolysiloxane, coupling agents such as silane-based, aluminum-based, titanium-based, and zirconium-based, fluorine compounds such as perfluoroalkyl phosphate compounds, hydrocarbons, lecithin, amino acids, polyethylene, wax, and metal soaps. A combination of these treatments may be performed, and the order of the treatments is not particularly limited.

[0048] (Pigment Uses) The pigment of the present invention can transmit light in the warm color region preferentially, and when used as an ingredient of a cosmetic to be applied to the skin, the transmitted light in the warm color region is scattered inside the skin, suppressing white cast and realizing a natural finish. In addition, since the pigment of the present invention strongly scatters light other than the warm color region, when used as an ingredient of a cosmetic to be applied to the skin, it can cover redness, dullness, spots, freckles, etc. caused by the skin, and can create a uniform and beautiful skin appearance. Therefore, the pigment of the present invention can be suitably used as an ingredient of a cosmetic. A cosmetic containing the pigment of the present invention is one aspect of the present invention. From another perspective, the use of the pigment of the present invention as a cosmetic is also one aspect of the present invention, and the use of the pigment of the present invention to suppress the white cast phenomenon in a cosmetic is also one aspect of the present invention. Here, the "white cast phenomenon" refers to a phenomenon in which the finish of makeup looks pale and unnatural when the intensity of white scattered light is strong when the cosmetic is applied to the skin. "Suppressing the white cast phenomenon" means that the pigment of the present invention blended into a cosmetic product preferentially transmits light in the warm color region, and the transmitted light in the warm color region is scattered inside the skin, thereby suppressing, reducing, or mitigating the above-mentioned white cast phenomenon, resulting in a natural-looking makeup finish. Note that "light in the warm color region" refers to light with a wavelength of 570 nm or more and 780 nm or less.

[0049] The pigment of the present invention can also be used in a wide range of applications outside of the field of cosmetics, taking advantage of its function of transmitting light in the warm color region. Examples of such applications include, but are not limited to, adding the pigment to resins to use in sunroofs, adding the pigment to paints to apply coatings that transmit light in the warm color region, etc. The pigment obtained by the present invention can also be used as a substitute for titanium oxide.

[0050] (Cosmetics) When the pigment of the present invention is used as a cosmetic, typically, the surface is coated as described above, and then the pigment may be mixed with inorganic pigments and / or organic pigments according to a known method. The content of the pigment of the present invention in the cosmetic varies depending on the type of cosmetic, and is not particularly limited. For example, the pigment may be used in an amount of about 1 g / kg to 900 g / kg for powder-type cosmetics, 1 g / kg to 500 g / kg for oil-based cosmetics, and 1 g / kg to 150 g / kg for emulsion-type or cream-type cosmetics, but is not limited to these ranges.

[0051] When the pigment of the present invention is used as a cosmetic, inorganic pigments and / or organic pigments that can be mixed with the pigment of the present invention may be inorganic pigments and organic pigments that are used in ordinary cosmetic products, as necessary. Examples of such inorganic pigments include titanium oxide, zinc oxide, iron oxide such as red iron oxide, cerium oxide, alumina, zirconium oxide, magnesium oxide, chromium oxide, magnesium silicate, aluminum magnesium silicate, calcium silicate, barium sulfate, magnesium sulfate, calcium sulfate, calcium carbonate, magnesium carbonate, talc, mica, surface-treated mica, micaceous synthetic pigments, sericite, zeolite, kaolin, bentonite, clay, silicic acid, boron nitride, bismuth oxychloride, hydroxyapatite, ultramarine, Prussian blue, and dehydrates and complexes thereof. Similarly, examples of organic pigments include silicone powder, silicone elastic powder, polyurethane powder, cellulose powder, nylon powder, urethane powder, silk powder, polymethyl methacrylate (hereinafter referred to as "PMMA") powder, polyethylene powder, starch, carbon black, metal soap such as zinc stearate, and complexes thereof. Tar dyes and various natural dyes can also be used.

[0052] The method for producing the cosmetic is not particularly limited, and a known method may be used. The formulation of the cosmetic is also not particularly limited, and may be, for example, any of powder, powder solid, cream, milky liquid, lotion, oily liquid, oily solid, paste, etc. For example, the cosmetic may be a makeup cosmetic, skin care cosmetic, hair care cosmetic, etc., such as a makeup base, foundation, concealer, face powder, control color, sunscreen cosmetic, lipstick, blusher, lip cream, lip color, lip gloss, eye shadow, eyeliner, mascara, cheek color, nail polish, body powder, perfume powder, baby powder, etc. In order to make the most of the light transmission effect and hiding power of the warm color region by the pigment of the present invention, it is preferable to use it in a makeup cosmetic to be applied to the skin.

[0053] In addition to the above-mentioned components, the cosmetic preparation of the present invention may contain other components in the quantitative and qualitative ranges that do not impair the effects of the present invention, depending on the purpose. For example, oily components, pigments, pH adjusters, moisturizers, thickeners, surfactants, dispersants, stabilizers, colorants, preservatives, antioxidants, sequestering agents, astringents, anti-inflammatory agents, UV absorbers, fragrances, some medicines, etc. may be appropriately blended depending on the purpose.

[0054] The pigment of the present invention can be used in fields other than cosmetics, such as resin compositions, paints, and inks. That is, a resin composition, paint, or ink containing the pigment of the present invention is one aspect of the present invention. From another perspective, the use of the pigment of the present invention in a resin composition, paint, or ink is also one aspect of the present invention. For example, the use of the pigment of the present invention for producing a resin composition, paint, or ink is also one aspect of the present invention.

[0055] The pigment of the present invention can be used as one of the materials of a resin composition. The resin composition containing the pigment of the present invention can be used for sunroofs, resin containers, etc., but is not limited thereto. As the resin, any of thermoplastic resins such as polyethylene and polypropylene, and thermosetting resins such as polycarbonate can be used. The resin composition is produced by a known method. For example, a monomer and the pigment of the present invention are dispersed in a solvent such as an organic solvent or water, a polymerization initiator is added, and the mixture is heated, washed, and dried to obtain a resin composition containing the pigment of the present invention. A flame retardant, a filler, etc. can be used in combination with the pigment of the present invention. The pigment of the present invention is not limited to this range, but it is preferable to add the pigment to the obtained resin composition so that the amount of the pigment is 1 g / kg or more and 350 g / kg or less. By using the pigment of the present invention, a white resin composition with a warm light can be obtained.

[0056] The pigment of the present invention can be used as one of the materials for paints. The paint containing the pigment of the present invention can be used for residential paints in cold regions, but is not limited thereto. The pigment of the present invention can be used for both water-based paints and oil-based paints. The paint can be obtained from a resin such as an acrylic resin, a urethane resin, or a polyvinyl alcohol, a solvent such as toluene, ethanol, or water, and a colorant such as the pigment of the present invention. The paint can be manufactured by a known method. For example, a paint containing the pigment of the present invention can be obtained by adding a hardener to a resin, and then adding the pigment obtained by the present invention and a solvent and stirring the mixture. An anti-settling agent, a preservative, other pigments, and the like can be used in combination as desired. The pigment of the present invention is not limited to this range, but is preferably added so that the amount of the pigment is 1 g / kg or more and 700 g / kg or less in the paint film dried after use. By using the pigment of the present invention, a residential paint that preferentially transmits light in the warm color region and easily raises the temperature inside the room can be obtained.

[0057] The pigment of the present invention can be used in ink. The ink containing the pigment of the present invention can be used in special inks for printing on films, glass surfaces, etc., but is not limited thereto. The ink can be obtained from a colorant, such as the pigment obtained in the present invention, a resin such as an acrylic resin, and a solvent such as a ketone, a hydrocarbon, or water. The ink is produced by a known method. For example, the ink can be obtained by dispersing and mixing the colorant, the resin, and the solvent. A pH adjuster, a surfactant, a preservative, a pigment other than the pigment obtained in the present invention, and the like can be used in combination. The pigment of the present invention is not limited to this range, but it is preferable to add it to the obtained ink so that it is 1 g / kg or more and 600 g / kg or less. By using the pigment of the present invention, it is possible to print on a transparent substrate such as vinyl or glass, and to give it a beauty that has not been achieved with white pigments in the past. In addition to the above, the pigment of the present invention can be used in applications such as paper, toner additives, coating tools, textile products, packaging materials, films, and coating materials.

[0058] Before describing the examples, the test methods used in the present invention will be described.

[0059] (The diameter or major axis length of the part that is lighter in color than the surrounding area, and the number per area) The pigments were photographed using a JEOL JEM-1400plus transmission electron microscope (hereinafter referred to as "TEM") at an accelerating voltage of 100 kV and a magnification of 100,000 times. Among the particles in the photograph, those that overlapped with each other and those that were so thick that they were difficult to count due to their spotted patterns were selected, and photographed after focusing as much as possible on particles that had a similar appearance to the surrounding particles and increasing the contrast. As shown in Figure 4, the photograph of the selected particle was taken with a particle size of 1.0 x 10 4 nm 2A rectangular frame was drawn so that the diameter or major axis length of the light-colored areas with a roughly circular or roughly elliptical outer shape scattered like spots in the area within the frame was measured. The same procedure was carried out for 10 or more particles, and the number average value (number average diameter) and maximum value (maximum diameter) of the diameter or major axis length of the light-colored areas scattered like spots with a diameter or major axis length in the range of 1.5 nm to 15.0 nm were recorded. When the spots were connected to each other, the diameter was estimated from the particle outer diameter for spots where the outer diameter was 1 / 2 or more. In addition, the above 1.0 x 10 4 nm 2 The number of light-colored spots with a diameter or major axis length of 1.5 nm or more and 15.0 nm or less within the frame was visually counted. The "light-colored spots" referred to in this invention are generally widely distributed inside the calcium titanium composite oxide particles in the pigment of the present invention, and are lighter in color than the surroundings (usually appearing white or light gray against a dark gray or blackish surrounding). The light-colored spots can be observed to be scattered in the above particles of the present invention in the form of generally roughly circular or elliptical spots. The "light-colored spots" referred to in this invention do not include errors in the TEM photograph due to the device or instruments used for evaluation, or specific white spots in particles that have an appearance clearly different from the surrounding particles due to localized foreign matter and particle defects. When the entire particle was observed at a magnification of 100,000 times using the above method, if no light-colored spots were observed, it was determined that no spotted pattern was present inside the particle. (true density) Measurements were performed according to JIS K 5101-11-1:2004, Method A. A 50 mL pycnometer, model 055520-050, manufactured by Shibata Scientific Co., Ltd., was used as the pycnometer, and SAJ special grade kerosene, manufactured by Sigma-Aldrich Japan Co., Ltd., was used as the replacement liquid. 2 g of the dried product was used as the sample, and the true density was measured by adjusting the temperature to 25°C.

[0060] (Particle size distribution width) The width of the particle size distribution was measured using a Microtrac (registered trademark) MT3300EXII laser light diffraction scattering particle size analyzer manufactured by Microtrac Bell Co., Ltd., in accordance with a method conforming to JIS Z 8825:2013. Ion-exchanged water was used as the dispersion medium. After an appropriate amount of pigment was dropped into the ultrasonic dispersion tank of an automatic sample circulator attached to the measurement device, ultrasonic dispersion was performed for 360 seconds at an output of 40 W. After this, the measurement parameters were set to a refractive index of 1.33 for the ion-exchanged water, reflection of the light transmittance of the particles to be measured, and a measurement time of 30 seconds, and the particle size (X10) corresponding to 10% of the cumulative particle size distribution (volume basis) and the particle size (X90) corresponding to 90% of the cumulative particle size distribution (volume basis) were measured, and X90 / X10 was taken as the width of the particle size distribution.

[0061] (Particle size) The particle diameter is calculated by taking the area of ​​the particle when projected two-dimensionally as S and the diameter R of the circle equivalent to the same area as the particle. 0.5 The particle area S was calculated by photographing the particles at a magnification of 10,000 times using a TEM and using the image analysis software ImageJ. The average value of R for 200 or more particles was taken as the particle diameter.

[0062] (XRD titanium oxide integrated diffraction intensity) X-ray diffraction measurements were performed using the powder method with a Rigaku X-ray diffractometer RINT-TTR III. The sample was crushed in a mortar and packed in a cell at approximately 1.5g ± 0.2g, with a start angle of 5.0000°, end angle of 90.0000°, sampling width of 0.0100°, scan speed of 10.0000° / min, divergence slit of 0.5°, scattering slit of 0.5°, receiving slit width of 0.15mm, and characteristic X-rays were generated using copper as the cathode and a wavelength of 0.15418nm. The obtained X-ray diffraction pattern was subjected to background processing, smoothing and peak detection using powder X-ray analysis software PDXL2 manufactured by Rigaku Corporation. The integrated diffraction intensity of the diffraction line of the (1 2 1) plane appearing in the range of diffraction angle 2θ of 32.50° to 33.50° was taken as 100.0, and the ratio of the integrated diffraction intensity of the diffraction line appearing in the range of diffraction angle 2θ of 24.75° to 28.00° was calculated, and this was taken as the XRD titanium oxide integrated diffraction intensity.

[0063] (Warm light transmission effect) 3 mL of styrenated alkyd resin and 0.3 g of pigment were kneaded with an H3-type automatic Huber Marler manufactured by Toyo Seiki Seisakusho Co., Ltd. to prepare a paint, and the obtained dispersion was applied to a black and white hiding power test paper JIS-K5600-4-1 with a 3-mil doctor blade and baked at 130°C for 30 minutes to obtain a test sample. The reflectance at wavelengths of 380 nm to 780 nm was measured on the black background of the test sample using a spectrocolorimeter SQ-2000 manufactured by Nippon Denshoku Kogyo Co., Ltd. (hereinafter referred to as "colorimeter"). The measured value was subtracted from 100% to calculate the transmittance at each wavelength. The total value of the transmittances of 380 nm to 780 nm was taken as the total transmitted light amount, the total value of the transmittances of 570 nm to 780 nm was taken as the warm color transmitted light amount, and the value of the warm color transmitted light amount / total transmitted light amount was taken as the warm color transmission effect.

[0064] (Concealment rate) The hiding power of a pigment is measured using a color difference meter to determine the lightness index L of the test sample on a black background, which was prepared using the method described in the warm light transmission effect column above. b and the lightness index L on a white background w Measure L b / L w The value was taken as the concealment rate. EXAMPLES

[0065] The present invention will be described in detail below with reference to examples. However, the following examples are presented merely for illustrative purposes and are not intended to limit the scope of the invention.

[0066] In addition, in the stirring operations described in the Examples and Comparative Examples, the rotation speed is appropriately adjusted to ensure that the entire liquid is mixed uniformly and that droplets are not scattered around, taking into consideration the properties related to the behavior of the liquid during stirring, such as the liquid volume, viscosity of the liquid, and shape of the container. In addition, when the same effect can be obtained by using any company's product as long as it is a general commercially available product, such as sodium hydroxide, the names of the manufacturer and distributor are omitted.

[0067] [Example 1: Rectangular particles] Metatitanic acid obtained by the sulfuric acid method was bleached to remove iron, and then an aqueous sodium hydroxide solution was added to adjust the pH to 9.0, followed by desulfurization. The solution was then neutralized to pH 5.8 with hydrochloric acid, filtered, and washed to obtain a metatitanic acid cake (hydrolyzed titanium compound) with a sulfur content of 9.3 g / kg calculated as SO3. Water was added to the washed cake to make a slurry of 2.13 mol / L in terms of Ti, and hydrochloric acid was added to adjust the pH to 1.4, followed by peptization to obtain an acid peptized product of hydrolyzed titanium compound (metatitanic acid). 2.25 mol of the treated slurry was collected as TiO2 and placed in a reaction vessel with a capacity of 3000 mL. Calcium hydroxide was added to this so that the amount of calcium as Ca was 1.15 times the amount of titanium as Ti, 0.36 mol of sodium hydroxide was added, and water was added to make the total volume 2.0 L, and the mixed solution was stirred for 30 minutes using HEIDON600G manufactured by Shinto Scientific Co., Ltd.

[0068] The slurry was further stirred and mixed, and heated to 95°C using a BE-type mantle heater manufactured by Tokyo Technical Research Institute, and stirring was continued for 18 hours to complete the reaction (normal pressure heating reaction). The stirred slurry was allowed to cool to 50°C, hydrochloric acid was added until the pH reached 5.0, and stirring was continued for another hour (calcium removal treatment). The resulting precipitate was decanted and separated by filtration, and then dried in air at 120°C for 10 hours using a Perfect Oven PHH-202 manufactured by Espec Corporation. This dried material was fired in air for 1 hour in a SUPER-C C-2035D manufactured by Motoyama Co., Ltd. (hereinafter referred to as the "fired furnace") set at 500°C. This fired product was pulverized in an Ishikawa-type stirring and crushing machine AGA type manufactured by Ishikawa Factory Co., Ltd. (hereinafter referred to as the "automatic mortar") to obtain a white pigment. The shape of the particles constituting the pigment was mainly rectangular. When the pigment was evaluated using the above test method, it was confirmed in a transmission electron microscope photograph that there were spots inside the particle that were lighter in color than the surrounding area, and these lighter in color than the surrounding area were circular or elliptical, with a maximum diameter or major axis length of 10.0 nm and a number average value of 4.1 nm. The true density was 3760 kg / m 3 The area that is lighter in color than the surrounding area is 1.0×104 nm 2 There were 165 particles within the range. The particle size of the pigment was 294 nm, the width of the particle size distribution was 2.25, and the XRD titanium dioxide integrated diffraction intensity was 5.23. In addition, the warm light transmission effect was 0.586, and the hiding ratio was 0.731.

[0069] [Example 2: Rectangular particles] Except for changing the set temperature of the calcination furnace to 700°C, normal pressure heating reaction, calcium removal treatment, washing, filtration, drying and pulverization were carried out under the same conditions as in Example 1 to obtain a white pigment. The shape of the particles constituting the pigment was mainly rectangular. Transmission electron microscope photographs of the pigment confirmed that there were spots inside the particles that were lighter in color than the surrounding area, and these lighter in color than the surrounding area were circular or elliptical. The measurement results are shown in Table 2.

[0070] [Example 3: Rectangular particles] Except for changing the set temperature of the calcination furnace to 900°C, normal pressure heating reaction, calcium removal treatment, washing, filtration, drying and pulverization were carried out under the same conditions as in Example 1 to obtain a white pigment. The shape of the particles constituting the pigment was mainly rectangular. Transmission electron microscope photographs of the pigment confirmed that there were spots inside the particles that were lighter in color than the surrounding area, and these lighter in color than the surrounding area were circular or elliptical. The measurement results are shown in Table 2.

[0071] [Comparative Example 1: Rectangular parallelepiped particles] A normal pressure heating reaction, calcium removal treatment, washing, filtration, drying and pulverization were carried out under the same conditions as in Example 1, except that no firing in a firing furnace was performed, to obtain a white pigment. The shape of the particles constituting the pigment was mainly rectangular. Transmission electron micrographs of the pigment confirmed that there were spots inside the particles that were lighter in color than the surrounding area, and these lighter in color than the surrounding area were circular or elliptical. The measurement results are shown in Table 2.

[0072] [Example 4: Nearly spherical particles] The amount of sodium hydroxide added after the addition of calcium hydroxide was changed to 3.60 mol, and 0.0193 mol of glucose was added per mol of Ca after the addition of sodium hydroxide. The normal pressure heating reaction, calcium removal treatment, washing, filtration, drying, calcination and pulverization were carried out under the same conditions as in Example 1 to obtain a white pigment. The shape of the particles constituting the pigment was mainly approximately spherical. In a transmission electron microscope photograph of the pigment, it was confirmed that there were spots inside the particles that were lighter in color than the surrounding area, and these lighter in color than the surrounding area were circular or elliptical. The measurement results are shown in Table 2.

[0073] [Example 5: Nearly spherical particles] Except for changing the set temperature of the calcination furnace to 700°C, normal pressure heating reaction, calcium removal treatment, washing, filtration, drying and pulverization were carried out under the same conditions as in Example 4 to obtain a white pigment. The shape of the particles constituting the pigment was mainly approximately spherical. Transmission electron microscope photographs of the pigment confirmed that there were spots inside the particles that were lighter in color than the surrounding area, and these lighter in color than the surrounding area were circular or elliptical. The measurement results are shown in Table 2.

[0074] [Example 6: Nearly spherical particles] Except for changing the set temperature of the calcination furnace to 900°C, normal pressure heating reaction, calcium removal treatment, washing, filtration, drying and pulverization were carried out under the same conditions as in Example 4 to obtain a white pigment. The shape of the particles constituting the pigment was mainly approximately spherical. Transmission electron microscope photographs of the pigment confirmed that there were spots inside the particles that were lighter in color than the surrounding area, and these lighter in color than the surrounding area were circular or elliptical. The measurement results are shown in Table 2.

[0075] [Comparative Example 2: Nearly spherical particles] A normal pressure heating reaction, calcium removal treatment, washing, filtration, drying and pulverization were carried out under the same conditions as in Example 4, except that no firing in a firing furnace was performed, to obtain a white pigment. The shape of the particles constituting the pigment was mainly approximately spherical. Transmission electron microscope photographs of the pigment confirmed that there were spots inside the particles that were lighter in color than the surrounding area, and these lighter in color than the surrounding area were circular or elliptical. The measurement results are shown in Table 2.

[0076] [Comparative Example 3: Commercially available product] The commercially available calcium titanium composite oxide reagent CAF04PB manufactured by Kojundo Chemical Laboratory was used as Comparative Example 3. The appearance of the reagent was pale pink, and in a transmission electron microscope photograph, the color of the inside of the particle was almost uniform, and no spotted pattern was observed. The measurement results are shown in Table 2.

[0077] Table 1 shows the production conditions for the pigments of the Examples and Comparative Examples, and Table 2 shows the measurement results for the properties of the pigments obtained in the Examples and Comparative Examples.

[0078] As shown in Table 2, the pigment made of particles mainly composed of calcium titanium composite oxide, in which the presence of dotted areas inside the particles that are lighter in color than the surrounding area can be confirmed in a transmission electron microscope photograph, has a greater warm color light transmission effect than the pigment (Comparative Example 3) in which no dotted patterns can be confirmed. Furthermore, the pigment with a true density of 3500 kg / m 3 More than 3790kg / m 3 It was found that the following pigments also had a large hiding power when pigments with the same particle shape were compared (comparison between Examples 1 to 3 and Comparative Example 1, and comparison between Examples 4 to 6 and Comparative Example 2). These pigments can be said to preferentially transmit light in the warm color region and have a large hiding power.

[0079] As described above, the pigment of the present invention can be said to preferentially transmit light in the warm color region and have a high hiding power. By using the pigment of the present invention as a raw material for cosmetics, it is possible to obtain cosmetics that realize a natural finish and have a high hiding power.

[0080] [Table 1]

[0081] [Table 2]

[0082] Next, the powder foundations prepared using the pigments obtained in the Examples and Comparative Examples were subjected to a sensory evaluation by the following method.

[0083] (Sensory evaluation of powder foundation) Each pigment obtained in the Examples and Comparative Examples was surface-treated with methylhydrogenpolysiloxane and uniformly mixed in a LAB.MIXER LM-110T (hereinafter referred to as "mixer") manufactured by HANIL Electric.Co.,Lid in the blending ratio shown in Table 3. The mixture was pulverized in a Sample Mill TASM-1 (hereinafter referred to as "sample mill") manufactured by Tokyo Atomizer Mfg. Co., Ltd., and then a predetermined amount was filled into a metal dish and compression molded to produce a powder foundation.

[0084] [Table 3]

[0085] Ten panelists were asked to apply each of the obtained powder foundations to areas of the arms and face, particularly areas with dullness or blemishes, and the natural finish and hiding power were evaluated.

[0086] (Natural finish) The impression of the area where foundation was not used was visually compared to that of an area where foundation was not used and evaluated according to the following criteria, and the "natural finish" was determined by the average score of the 10 panelists. The higher the score, the less the foundation looked "white and cast" and the more "natural finish" was achieved. The results of the sensory evaluation are shown in Table 4. (Evaluation Criteria) 4 points: Even when viewed from a close distance (30 cm), it is indistinguishable from an unpainted area. 3 points: When viewed up close, it is clear that paint has been applied, but the impression is natural. 2 points: When viewed from a close distance, it appears whitish. 1 point: Appears whitish even when viewed from a distance (1m).

[0087] (Concealment) The impression when applying foundation to spots or dullness was evaluated according to the following criteria, and the "concealing power" was judged based on the average score of 10 panelists. The higher the score, the better the concealing power of the foundation. The results of the sensory evaluation are shown in Table 4. (Evaluation Criteria) 4 points: Even when viewed up close (30 cm), no spots or dullness can be seen. 3 points: When viewed up close, spots or dullness are visible but not noticeable. 2 points: When viewed up close, spots and dullness are visible. 1 point: The distance at which blemishes or dullness can be seen is the same as when no cream is applied. (Comprehensive evaluation criteria) The sum of the natural finish score and hiding power score is 7 points or more: A, 5 points or more but less than 7 points: B, 3 points or more but less than 5 points: C, less than 3 points: D

[0088] [Table 4]

[0089] As a result of the sensory evaluation, it was found that the foundation prepared using the pigment mainly composed of particles having a spotted pattern had a natural finish with little white cast. In addition, when comparing pigments with the same particle shape (comparison between Examples 1 to 3 and Comparative Example 1, and comparison between Examples 4 to 6 and Comparative Examples 2 and 3), it was found that the pigment of the present invention had a greater hiding power than the pigment of the comparative example. In addition, the pigments of Examples 4 to 6, which have roughly spherical particles, had a smoother feel than those with rectangular parallelepiped particles. Thus, by blending the pigment of the present invention into cosmetics, it was possible to provide cosmetics that produce a natural finish and have excellent hiding power.

[0090] [Example 7] (Powder foundation manufacturing) Components 1 to 13 below were mixed and uniformly ground (Step A), and then components 15 to 17 were mixed uniformly and added to the mixed and ground product obtained in Step A and homogenized (Step B). Component 14 was then added and the mixture was press molded in a mold to obtain a powder foundation (Step C).

[0091] The obtained powder foundation did not produce a white cast when applied to the skin, gave a natural, bare skin finish, and was confirmed to have good hiding power. (Ingredients) Mixing ratio (g / kg) 1. Caprylylsilane-treated mica (note 1) 400 2. Caprylylsilane-treated pigment described in Example 6 (Note 1) 50 3. Silicone-treated talc (Note 2) Residual 4. Silicone-treated pigment-grade titanium dioxide (Note 2) 50 5. Silicone-treated titanium dioxide microparticles (Note 2) 50 6. Silicone-treated barium sulfate (Note 2) 100 7. Silicone-treated red iron oxide (Note 2) 4 8. Silicone-treated yellow iron oxide (Note 2) 20 9. Silicone-treated amber (Note 2) 4 10. Silicone-treated black iron oxide (Note 2) 1 11. Phenyl-modified hybrid silicone composite powder (Note 3) 20 12. Spherical polymethylsilsesquioxane powder (Note 4) 5 13. Preservatives (appropriate amount) 14.Fragrance (appropriate amount) 15. Crosslinked dimethylpolysiloxane (Note 5) 40 16. Glyceryl trioctanoate 20 17. Squalane 10 (Note 1) Surface treated with Shin-Etsu Chemical Co., Ltd.'s AES-3083 (Note 2) Surface treated with Shin-Etsu Chemical Co., Ltd.'s KF-9909 (Note 3) Shin-Etsu Chemical Co., Ltd. KSP-300 (Note 4) Shin-Etsu Chemical Co., Ltd. KMP-590 (Note 5) Shin-Etsu Chemical Co., Ltd. KSG-16

[0092] [Example 8] (Pressed powder manufacturing) After mixing and grinding components 1 to 7 below (step A), the mixture was transferred to a mixer, components 8 to 12 were added, and the mixture was stirred and mixed uniformly (step B). The mixture was then ground in a sample mill and press-molded into an aluminum dish to obtain a pressed powder (step C).

[0093] The obtained pressed powder did not cast a white cast when applied to the skin, gave a natural, bare skin finish, and was confirmed to have good hiding power. (Ingredients) Mixing ratio (g / kg) 1. Talc Residue 2.PMMA (Note 1) 100 3. Sericite 300 4. Scaly silica (Note 2) 30 5. Pigment described in Example 4 60 6. Preservatives: appropriate amount 7.Color material appropriate amount 8. Octyl methoxycinnamate 30 9. Squalane 20 10. Preservatives (appropriate amount) 11. Antioxidants (appropriate amount) 12.Fragrance (appropriate amount) (Note 1) Matsumoto Microsphere M-100, 7 μm, manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd. (Note 2) Sun Lovely C manufactured by Dokai Chemical Industry Co., Ltd.

[0094] [Example 9] (Loose powder manufacturing) After mixing and grinding the following components 1 to 7 (step A), the mixed and ground product was transferred to a mixer, and components 8 to 10 were added and stirred and mixed to be uniform (step B). Furthermore, the mixture obtained in step B was ground in a sample mill, and this was filled to obtain a loose powder (step C).

[0095] The obtained loose powder did not produce a white cast when applied to the skin, gave a natural, bare skin finish, and was confirmed to have good hiding power. (Ingredients) Mixing ratio (g / kg) 1. Talc Residue 2. Pigment described in Example 3 10 3. Amihope LL 30 4.PMMA (Note 1) 80 5. Preservatives (appropriate amount) 6. Appropriate amount of coloring material 7. Squalane 10 8. Preservatives (appropriate amount) 9. Antioxidants (appropriate amount) 10.Fragrance (appropriate amount) (Note 1) Matsumoto Microsphere S-100, 10 μm, manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd.

[0096] [Example 10] (Manufacture of oil-based foundation) Components 1 to 6 below were mixed in a mixer and pulverized uniformly (Step A). ​​Components 7 to 16 were then heated to 85°C to dissolve, and the mixed and pulverized product obtained in Step A was added and stirred uniformly (Step B). After degassing, the solids were poured into a tray and slowly cooled to room temperature to obtain an oil-based foundation (Step C).

[0097] The obtained oil-based foundation did not produce a white cast when applied to the skin, gave a natural, bare-skin-like finish, and was confirmed to have good hiding power. (Ingredients) Mixing ratio (g / kg) 1. Silicone-treated talc (Note 1) 53 2. Silicone treatment Pigment described in Example 4 (Note 1) 150 3. Silicone-treated sericite (Note 1) 282 4. Silicone-treated red iron oxide (Note 1) 5 5. Silicone-treated yellow iron oxide (Note 1) 18 6. Silicone-treated black iron oxide (Note 1) 2 7. Candelilla Row 10 8. Carnauba Wax 10 9. Ceresin 15 10. Decamethylcyclopentasiloxane 140 11. Isononyl isononanoate residue 12. Polyglyceryl diisostearate 20 13. Dextrin Palmitate 10 14. Octyl methoxycinnamate 30 15. Preservatives (appropriate amount) 16. Antioxidants (appropriate amount) (Note 1) Surface treated with Shin-Etsu Chemical's KF-96A-50cs

[0098] [Example 11] (Stick foundation manufacturing) Components 12 to 16 below were mixed in a mixer (Step A). ​​Components 1 to 11 were weighed out in a container that could hold the entire amount, heated to 85°C, and dissolved (Step B). Components 17 to 21 were weighed out in a separate container and dissolved (Step C). Thereafter, the mixture obtained in Step A was added to the heated and dissolved product obtained in Step B, dispersed with a stirrer until visually uniform, and the heated and dissolved product obtained in Step C was further added to emulsify (Step D). After degassing, the solids were poured into a mold and slowly cooled to room temperature to obtain a stick foundation (Step E).

[0099] The obtained stick foundation did not produce a white cast when applied to the skin, gave a natural, bare skin finish, and was confirmed to have good hiding power. (Ingredients) Mixing ratio (g / kg) 1. Dimethylpolysiloxane 180 2. Decamethylcyclopentasiloxane 300 3. Octyl methoxycinnamate 50 4. Diisostearyl malate 40 5. Candelilla Wax 60 6. Hydrogenated Jojoba Esters 40 7. Cetyl Dimethicone Copolyol 20 8. Sorbitan Sesquiisostearate 5 9. Antioxidants (appropriate amount) 10. Preservatives (appropriate amount) 11.Fragrance (appropriate amount) 12. Silicone-treated coloring agent (Note 1) 5 13. Silicone treatment Pigment described in Example 1 (Note 1) 85 14. Silicone-treated talc (Note 1) 60 15. Silicone-treated mica (Note 1) 20 16. Polymethylmethacrylate 20 17.Purified water remainder 18. Sodium Citrate 3 19.1,3-Butylene glycol 30 20. Glycerin 20 21. Preservatives (appropriate amount) (Note 1) Surface treated with Shin-Etsu Chemical's KF-99P

[0100] [Example 12] (Manufacture of W / O emulsion foundation) After mixing components 12 to 14 below with a mixer (step A), components 1 to 11 were added and dispersed using a stirrer until visually uniform (step B). Meanwhile, components 15 to 19 were heated and dissolved in a separate container (step C). After that, the heated and dissolved product obtained in step C was added to the dispersion obtained in step B to emulsify, and the mixture was cooled to room temperature to obtain a W / O emulsion foundation (step D).

[0101] The obtained W / O emulsion foundation did not cast a white cast when applied to the skin, gave a natural, bare-skin-like finish, and was confirmed to have good hiding power. (Ingredients) Mixing ratio (g / kg) 1. POE modified silicone (Note 1) 8 2. Polyglyceryl Polyricinoleate 5 3. Neopentyl glycol dicaprylate 30 4. Squalane 10 5. Pentaerythrityl tetraisopropyl ester 20 6. Inulin stearate (Note 2) 10 7. Octyl methoxycinnamate 40 8. Decamethylcyclopentasiloxane 154 9. Preservatives (appropriate amount) 10. Antioxidants (appropriate amount) 11.Fragrance (appropriate amount) 12. Silicone treatment Pigment described in Example 5 (Note 3) 80 13. Silicone-treated talc (Note 3) 57 14. Silicone-treated coloring agent (Note 3) 10 15.Purified water remainder 16.1,3-Butylene glycol 60 17. Glycerin 10 18. Sodium Chloride 10 19. Preservatives (appropriate amount) (Note 1) HLB value 4.5 (Note 2) Leopearl (registered trademark) ISK manufactured by Chiba Flour Mills (Note 3) Surface treated with Shin-Etsu Chemical Co., Ltd.'s KF-9901

[0102] [Example 13] (Manufacture of O / W emulsion foundation) Components 1 to 7 below were heated and dissolved at 85°C (Step A). ​​Components 8 to 10 were mixed and ground (Step B). Components 11 to 15 were heated to 85°C and mixed (Step C). The ground mixture obtained in Step B was then added to the heated and dissolved product obtained in Step A, and dispersed using a stirrer until visually uniform. The dissolved mixture obtained in Step C was gradually added thereto to emulsify, and the mixture was stirred and cooled to room temperature. The mixture was then filled into a suitable container to obtain an O / W emulsion foundation (Step D).

[0103] The obtained O / W emulsion foundation did not cast a white cast when applied to the skin, gave a natural, bare-skin-like finish, and was confirmed to have good hiding power. (Ingredients) Mixing ratio (g / kg) 1. Stearic acid 4 2. Isostearic acid 3 3. Cetyl 2-ethylhexanoate 40 4. Liquid Paraffin 110 5. Polyoxyethylene (10) stearyl ether 20 6. Cetyl Alcohol 3 7. Preservatives 2 8. Talc 150 9. Coloring agent 40 10. Pigment described in Example 1 30 11. Triethanolamine 4 12. Propylene glycol 50 13.Purified water 541 14. Preservatives 2 15. Antioxidants 1

[0104] [Example 14] (W / O liquid foundation manufacturing) After components 8 to 12 below were mixed uniformly (step A), a part of component 4 and component 13 were mixed, and the mixture obtained in step A was added and dispersed using a stirrer until it was visually uniform (step B). Components 1 to 3, the remainder of component 4, and components 5 to 7 were mixed and dispersed using a stirrer until it was visually uniform (step C). Furthermore, components 14 to 18 and component 20 were mixed and dispersed using a stirrer until it was visually uniform (step D). Under stirring, the mixture obtained in step D was gradually added to the mixture obtained in step C to emulsify, and the dispersion obtained in step B and component 19 were further added to obtain a W / O liquid foundation (step E).

[0105] The obtained W / O liquid foundation did not cast a white cast when applied to the skin, gave a natural, bare-skin-like finish, and was confirmed to have good hiding power. (Ingredients) Mixing ratio (g / kg) 1. Cross-linked polyether modified silicone (Note 1) 30 2. Crosslinked dimethylpolysiloxane (Note 2) 50 3. Branched polyether modified silicone (Note 3) 20 4. Decamethylcyclopentasiloxane 211 5. Cetyl isooctanoate 50 6. Dimethylpolysiloxane (Note 4) 65 7. Dimethyl distearyl ammonium hectorite 12 8. Silicone-treated pigment described in Example 1 (Note 5) 50 9. Silicone-treated pigment-grade titanium dioxide (Note 5) 50 10. Silicone-treated red iron oxide (Note 5) 4 11. Silicone-treated yellow iron oxide (Note 5) 10 12. Silicone-treated black iron oxide (Note 5) 1 13. Acrylic silicone resin solution (Note 6) 20 14. 1,3-Butylene glycol 50 15. Xanthan gum (note 7) 50 16. Sodium Citrate 2 17. Sodium Chloride 5 18. Preservatives (appropriate amount) 19.Fragrance (appropriate amount) 20.Purified water 320 (Note 1) Shin-Etsu Chemical Co., Ltd. KSG-210 (Note 2) Shin-Etsu Chemical Co., Ltd. KSG-15 (Note 3) Shin-Etsu Chemical Co., Ltd. KF-6028P (Note 4) 6mm 2 / second (25℃) product (Note 5) Surface treated with Shin-Etsu Chemical's KF-9909 (Note 6) Shin-Etsu Chemical Co., Ltd. KP-575 (Note 7) 20g / kg aqueous solution

[0106] [Example 15] (Manufacture of Sun Cut Cream) In order to confirm the ultraviolet shielding ability of the pigment of the present invention, a sun-cut cream was prepared. Component 7 was added to a part of component 5 below to make it uniform, and components 8 and 9 were added and dispersed with a bead mill (step A). ​​Components 1 to 4, the remainder of component 5, and component 6 were mixed uniformly (step B). Furthermore, components 10 to 12 and component 14 were dispersed with a stirrer until they were visually uniform (step C). Next, the mixture obtained in step C was added to the mixture obtained in step B and emulsified, and the dispersion obtained in step A and component 13 were added to obtain a sun-cut cream (step D).

[0107] It was confirmed that the obtained sun cream had the same UV blocking ability as titanium oxide, did not produce a whitish cast when applied to the skin, and gave a natural, bare-skin finish. (Ingredients) Mixing ratio (g / kg) 1. Cross-linked polyether modified silicone (Note 1) 30 2. Crosslinked dimethylpolysiloxane (Note 2) 20 3. Alkyl-modified branched polyether-modified silicone (Note 3) 10 4. Neopentyl glycol dioctanoate 50 5. Decamethylcyclopentasiloxane 175 6. Octyl methoxycinnamate 60 7. Acrylic silicone resin solution (Note 4) 100 8. Caprylylsilane-treated fine zinc oxide (note 5) 200 9. Caprylylsilane-treated pigment described in Example 2 (Note 5) 30 10. 1,3-Butylene glycol 20 11. Sodium Citrate 2 12. Sodium Chloride 5 13.Fragrance (appropriate amount) 14.Purified water 298 (Note 1) Shin-Etsu Chemical Co., Ltd. KSG-240 (Note 2) Shin-Etsu Chemical Co., Ltd. KSG-15 (Note 3) Shin-Etsu Chemical Co., Ltd. KF-6038 (Note 4) Shin-Etsu Chemical Co., Ltd. KP-575 (Note 5) Surface treated with Shin-Etsu Chemical Co., Ltd.'s AES-3083

[0108] [Example 16] (Production of resin composition) A resin composition containing the pigment of the present invention was prepared. Component 1 was distilled and then bubbled with nitrogen for 30 minutes (step A). ​​Component 5 and component 6 were mixed and dispersed using a bead mill (step B). The liquid obtained in step A and components 2 to 4 were added to component 7 and heated with stirring. Five minutes after the temperature reached 65°C, the dispersion obtained in step B was added and stirring was continued while maintaining the temperature at 65°C (step C). After 10 hours, component 8 was added to neutralize (step D), and the mixture was filtered and washed to obtain a resin composition (step E).

[0109] When the obtained resin composition was held up to sunlight, the proportion of warm color region in the transmitted light was significantly large, and it was confirmed that the resin composition had a warm color light transmitting effect. (Ingredients) Mixing ratio (g / kg) 1. Methyl methacrylate 600 2. Azoisobutyronitrile 0.3 3. Sodium chloride 1 4. Calcium phosphate 6 5. Methylhydrogenpolysiloxane surface treatment Pigment described in Example 4 200 6. Toluene 140 7. Purified water (appropriate amount) 8. Hydrochloric acid (appropriate amount)

[0110] [Example 17] (Paint manufacturing) A paint containing the pigment of the present invention was prepared by mixing components 1 to 4 in a mixer for 30 to 120 minutes (step A) and then dispersing the mixture in a bead mill (step B).

[0111] When the obtained paint was applied onto a transparent glass substrate and held up to the light, the proportion of warm color regions in the transmitted light was significantly large, confirming that the paint has a warm color light transmitting effect. (Ingredients) Mixing ratio (g / kg) 1. Acrylic resin (Note 1) 300 2. Methylhydrogenpolysiloxane surface treatment Pigment described in Example 4 300 3. Toluene 200 4. Isophorone 200 (Note 1) Includes polymerization initiator

[0112] [Example 18] (Ink manufacturing) An ink containing the pigment of the present invention was prepared by mixing components 1 to 4 in a mixer for 30 to 120 minutes (step A) and then dispersing the mixture in a bead mill for 24 hours (step B).

[0113] When the obtained ink was applied to a glass plate and held up to the light, the proportion of warm color areas in the transmitted light was significantly large, confirming that the ink had a warm color light transmission effect. (Ingredients) Mixing ratio (g / kg) 1. Acrylic resin 75 2. Methylhydrogenpolysiloxane surface treatment Pigment described in Example 4 495 3. Methylcyclohexane 400 4. Dispersant (Note 1) 10 5. Gelling agent (note 2) 20 (Note 1) Homogenol (registered trademark) L-18 manufactured by Kao Corporation (Note 2) Organite (registered trademark)-T manufactured by Japan Organic Clay Co., Ltd.

Claims

1. A pigment comprising particles mainly composed of calcium titanium composite oxide, When the calcium titanium composite oxide particles in the pigment were observed under a transmission electron microscope at a magnification of 100,000 times, it was confirmed that the particles contained dots of areas that were lighter in color than the surrounding area. True density is 3500 kg / m 3 More than 3790kg / m 3 The pigment, which is:

2. The shape of the portion that is lighter in color than the surrounding area is a circle with a diameter of 1.5 nm to 15.0 nm or an ellipse with a major axis length of 1.5 nm to 15.0 nm, and The area that is lighter in color than the surrounding area is 1.0×10 4 nm 2 The pigment according to claim 1 , wherein 100 to 200 of the pigments are present in the range corresponding to

3. 3. The pigment according to claim 1, wherein the number average diameter or major axis length of the portion that is lighter in color than the surrounding area is 2.5 nm or more and 4.5 nm or less.

4. The pigment according to claim 1 , wherein the particle size is from 200 nm to 500 nm.

5. The pigment according to claim 1 , wherein the particle size distribution width set in JIS Z8825:2013 is smaller than 10.

00.

6. 6. The pigment according to claim 1, wherein, in an X-ray diffraction measurement, when the integrated diffraction intensity of the diffraction line of the (1 2 1) plane appearing in the diffraction angle range of 32.50° to 33.50° is taken as 100.0, the ratio of the integrated diffraction intensity of the diffraction line appearing in the diffraction angle range of 24.75° to 28.00° is 12.00 or less.

7. The pigment according to claim 1 , which has an inorganic and / or organic coating layer on at least a portion of the surface of the particle.

8. providing an aqueous solution containing a titanium source and a calcium source; heating the aqueous solution to react the titanium source and the calcium source to form a reactant; The reaction product is subjected to a calcium removal treatment, and then subjected to solid-liquid separation to recover a solid content; and The resulting solid is heated. A method for producing the pigment according to any one of claims 1 to 7, comprising:

9. mixing an acid peptized product of a hydrolysis product of a titanium compound, a water-soluble compound containing calcium, and an alkali, and heating the mixture to 70° C. or higher and 100° C. or lower under normal pressure to generate a reaction product; The resulting reaction mixture is cooled and then maintained at a pH of 7.0 or less for 1 hour or more. The reaction product after the above retention is subjected to solid-liquid separation to recover a solid content, and The solid is baked at 500°C or higher. A method for producing the pigment according to any one of claims 1 to 7, comprising:

10. A cosmetic preparation comprising the pigment according to any one of claims 1 to 7.

11. A resin composition comprising the pigment according to claim 1 .

12. A paint comprising the pigment according to any one of claims 1 to 7.

13. An ink comprising the pigment according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Method of and device for lap finishing surface of work

    JP1978063696A

  • Noise eliminating circuit

    JP1987058462A

  • Cosmetic

    JP1993339121A

  • Amber-white pigment particulate compounded cosmetic

    JP1998167929A

  • Effect pigment

    JP2007327059A