Adhesive for pellicle, pellicle, exposed master plate with pellicle, manufacturing method for semiconductor device, manufacturing method for liquid crystal display panel, recycling method for exposed master plate, and method for reducing peeling residue

The use of a pellicle adhesive with specific acrylic polymers and ether bonds addresses the issue of adhesive residue on exposure masters, enabling efficient recycling and cleaning, thus enhancing production efficiency in semiconductor and liquid crystal display manufacturing.

JP7579648B2Active Publication Date: 2024-11-08SHIN ETSU CHEMICAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020122013
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-23
Filing Date
2020-07-16
Publication Date
2024-11-08
Estimated Expiration
2040-04-15

AI Technical Summary

Technical Problem

The challenge in semiconductor and liquid crystal display manufacturing is the difficulty in removing adhesive residue from exposure masters after pellicle peeling, particularly with advanced masks like phase shift films and negative type masks, which can lead to damage and hinder efficient recycling and cleaning.

Method used

A pellicle adhesive using an acrylic polymer with specific SP values and ether bonds in its monomer components, designed to minimize residue by enhancing hydrophilicity and degradability upon exposure light, facilitating easy removal with functional water cleaning.

Benefits of technology

The adhesive reduces peeling residue, allowing for efficient recycling of exposure masters with minimal damage, improving production efficiency in semiconductor and liquid crystal display manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579648000003
    Figure 0007579648000003
  • Figure 0007579648000001
    Figure 0007579648000001
  • Figure 0007579648000002
    Figure 0007579648000002
Patent Text Reader

Abstract

To provide an adhesive for pellicle, a pellicle, an exposure original plate with pellicle, a method for regenerating an exposure original plate, and a peeling residue reduction method which can reduce a residue stuck onto an exposure original plate after used in lithography, especially ArF lithography, when a pellicle is peeled from the exposure original plate.SOLUTION: An adhesive for pellicle for sticking a pellicle 10 onto an exposure original plate 1 has an acrylic polymer having an SP value of 10.0 or more and 12.0 or less as a base material.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive for a pellicle, a pellicle, an exposed master plate with a pellicle, a method for manufacturing a semiconductor device, a method for manufacturing a liquid crystal display panel, a method for recycling an exposed master plate, and a method for reducing peeling residue. [Background technology]

[0002] In the manufacture of semiconductor devices such as LSI and VLSI, or liquid crystal display panels, a pattern is created by irradiating a semiconductor wafer or a liquid crystal master with light, but if dust is attached to the exposure master used in this case, the dust absorbs or bends the light, causing problems such as deformation of the transferred pattern, rough edges, and black staining of the base, impairing dimensions, quality, appearance, etc. In this invention, "exposure master" is a general term for lithography masks and reticles.

[0003] These operations are usually carried out in a clean room. However, since it is difficult to keep the exposure master clean even in this clean room, a method is used in which a pellicle that allows exposure light to easily pass through is attached to the surface of the exposure master to keep out dirt. In this case, the dust does not adhere directly to the surface of the exposure master, but adheres to the pellicle film. Therefore, if the focus is aligned on the pattern of the exposure master during lithography, the dust on the pellicle film will not affect the transfer.

[0004] The basic structure of a pellicle is a pellicle frame and a pellicle film stretched over it. The pellicle film is made of nitrocellulose, cellulose acetate, fluoropolymer, etc., which transmits light used for exposure (g-line, i-line, 248 nm, 193 nm, 157 nm, etc.) well. The pellicle frame is made of aluminum alloys such as A7075, A6061, A5052, stainless steel, polyethylene, etc., which have been subjected to black anodizing treatment. A good solvent for the pellicle film is applied to the upper part of the pellicle frame, and the pellicle film is air-dried and bonded, or is bonded with an adhesive such as acrylic resin, epoxy resin, or fluororesin. In addition, since the exposure master plate is attached to the lower part of the pellicle frame, an adhesive layer made of polybutene resin, polyvinyl acetate resin, acrylic resin, silicone resin, etc., and a protective liner for protecting the adhesive layer are provided.

[0005] The pellicle is installed so as to surround the pattern area formed on the surface of the exposure master. The pellicle is provided to prevent dust from adhering to the exposure master, and therefore this pattern area is isolated from the outside of the pellicle so that dust outside the pellicle does not adhere to the pattern surface.

[0006] In recent years, LSI design rules have been miniaturized to the sub-quarter micron level, and as a result, exposure light sources are becoming shorter in wavelength, that is, they are shifting from the previously mainstream g-line (436 nm) and i-line (365 nm) from mercury lamps to KrF excimer lasers (248 nm), ArF excimer lasers (193 nm), F2 lasers (157 nm), etc. As a result of miniaturization, the allowable size of foreign matter and haze that may occur on the pattern surface of a mask substrate to which a pellicle is attached is becoming increasingly strict. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 5638693 [Patent Document 2] JP 2016-18008 A [Patent Document 3] JP 2006-146085 A [Patent Document 4] JP 2008-21182 A Summary of the Invention [Problem to be solved by the invention]

[0008] In recent years, phase shift films have become the norm for mask substrates in order to keep up with the miniaturization of design rules. However, phase shift films are very delicate, and mask cleaning under excessive conditions can cause damage such as corrosion or scraping. For this reason, there has been a trend in recent years to reconsider the chemicals used for mask cleaning and to weaken the cleaning conditions.

[0009] Furthermore, advanced masks are shifting from the previously mainstream positive type mask patterns to negative type mask patterns, and as a result, there are many cases where there is no light-shielding layer in the area where the pellicle is attached. Without the light-shielding layer, there is a possibility that the exposure light will be irradiated onto the pellicle adhesive through the mask substrate. This may result in more residue of the adhesive layer remaining on the mask substrate when the pellicle is peeled off.

[0010] When a pellicle is attached to a mask for use, if foreign matter or haze occurs or the pellicle film is damaged, the pellicle must be peeled off, the mask regenerated and cleaned, and replaced with a new pellicle (hereinafter, this will be referred to as a "repellicle"). The most important thing about a repellicle is to regenerate and clean the mask to a high degree of cleanliness, but in order to regenerate and clean the mask under recent weak cleaning conditions, it is important to minimize the residue remaining on the mask substrate when the pellicle is peeled off. This regeneration cleaning generally involves cleaning with chemicals such as sulfuric acid / hydrogen peroxide or ammonia / hydrogen peroxide, or physical cleaning using brushes, sponges, etc. However, in order to prevent damage to the photomask and to prevent sulfate ions from remaining on the photomask, regeneration cleaning using functional water has been considered.

[0011] Functional water is generally defined as an aqueous solution that has been given a reproducible and useful function by artificial processing, and the scientific basis of the processing and function has been clarified or is about to be clarified.Specific examples include ozone water, hydrogen water, fine bubble water such as microbubble water and nanobubble water, electrolytic water, supercritical water, and subcritical water, and ozone water and hydrogen water are often used to clean photomasks.In addition, the cleaning power can be improved by adding a small amount of ammonia.

[0012] However, the inventors have found that functional water has a weaker cleaning power than chemicals such as sulfuric acid / hydrogen peroxide, and therefore, when cleaning a photomask after peeling off a pellicle, the residue of the adhesive layer that fixed the pellicle and the photomask is difficult to remove by cleaning with functional water alone. In particular, in the case of a phase shift photomask, damage to the phase shift film leads to changes in transmittance and phase difference, so it is difficult to add physical cleaning in addition to cleaning with functional water.

[0013] Furthermore, when lithography is performed using exposure light such as an ArF excimer laser (193 nm) with a lithography pellicle in which a pellicle film is attached to the upper end surface of the pellicle frame via an adhesive layer for attaching the pellicle film, and an adhesive layer for attaching a mask is provided on the other end surface, the adhesive layer formed on the lower end surface of the pellicle frame is altered by the exposure light, and when it is peeled off from the exposed master, the altered parts of the adhesive layer remain on the exposed master as peeling residue, which is a problem.

[0014] To date, attempts have been made to reduce residue by adding a surface modifier or the like to the adhesive (see Patent Document 1 and Patent Document 2). 2Disclosed are a large pellicle having an adhesive layer having the above structure (Patent Document 3), and a pellicle having an adhesive for a pellicle having a ratio of peel strength to tensile strength of 0.10 or more and 0.33 or less (Patent Document 4).

[0015] The present invention has been made in view of the above circumstances, and aims to provide a pellicle adhesive, a pellicle, an exposed master with a pellicle, a method for regenerating an exposed master, and a method for reducing residues left behind after peeling, which are capable of reducing residues left on an exposed master when the pellicle is peeled off from the exposed master after use in lithography, particularly after use in ArF lithography, and thereby to provide a method for manufacturing a semiconductor device and a liquid crystal display panel that can improve production efficiency. [Means for solving the problem]

[0016] The above-mentioned problems of the present invention have been solved by the following means. [1] A pellicle adhesive for attaching a pellicle to an exposure master, comprising: An adhesive for pellicles, the base material of which is an acrylic polymer with an SP value of 10.0 or more and 12.0 or less. [2] A pellicle adhesive for attaching a pellicle to an exposure master, comprising: An adhesive for pellicles whose base material is an acrylic polymer whose monomer component is a (meth)acrylic acid ester having an ether bond. [3] The adhesive for pellicles according to [2] above, wherein the (meth)acrylic acid ester having an ether bond is a (meth)acrylic acid ester having an alkylene oxide group. [4] The adhesive for pellicles according to [3], wherein the (meth)acrylic acid ester having an ether bond is contained in an amount of 30 mass% or more based on the total monomer components. [5] The adhesive for pellicles according to [3] or [4] above, wherein the alkylene oxide group is an ethylene oxide group. [6] The pressure-sensitive adhesive for pellicles according to any one of [2] to [5] above, further comprising an unsaturated monomer having a carboxyl group or a hydroxyl group as a monomer component. [7] The pressure-sensitive adhesive for pellicles according to any one of [2] to [6] above, further comprising an alkyl (meth)acrylate ester as a monomer component. [8] A pellicle adhesive for attaching a pellicle to an exposure master, comprising: An adhesive for pellicles, the base material of which is an acrylic polymer having a side chain containing an ether bond. [9] The adhesive for pellicles according to [8], wherein the side chain containing an ether bond has an alkylene oxide group.

[10] The adhesive for pellicles according to [9], wherein the alkylene oxide group is an ethylene oxide group.

[11] A pellicle adhesive for attaching a pellicle to an exposure master, the pellicle adhesive comprising an acrylic polymer as a base material having side chains that are more decomposable than the main chain when irradiated with exposure light.

[12] A pellicle adhesive for attaching a pellicle to an exposure master, the pellicle adhesive comprising as a base material an acrylic polymer having a side chain that is selectively degraded by exposure to exposure light.

[13] A pellicle frame with an adhesive layer, comprising: a pellicle frame; and an adhesive layer obtained from the adhesive for a pellicle described in any one of [1] to

[12] provided on one end surface of the pellicle frame.

[14] A pellicle having a pellicle membrane, a pellicle frame having the pellicle membrane provided on one end surface thereof, and an adhesive layer obtained from the adhesive for a pellicle described in any one of [1] to

[12] provided on the other end surface of the pellicle frame.

[15] The pellicle according to

[14] , wherein the adhesive layer is irradiated with an exposure light beam.

[16] The pellicle according to

[14] above, which is attached to a phase shift photomask.

[17] The pellicle according to

[14] above, which is attached to a negative type exposure master.

[18] The pellicle according to

[14] above, which is attached to an exposure master having a non-light-shielding area or a semi-transparent light-shielding area in the area where the adhesive layer is attached.

[19] The pellicle according to

[14] above, which is attached to an exposure master having a transparent area at the attachment portion of the adhesive layer in the exposure master.

[20] The pellicle according to

[14] above, which is attached to a surface mainly composed of silicon oxide.

[21] The pellicle according to

[20] , wherein the surface mainly composed of silicon oxide is a quartz surface.

[22] The pellicle according to

[14] above, which is suitable for regeneration and cleaning using functional water.

[23] An exposure master with a pellicle, comprising the pellicle described in

[14] or

[15] attached to the exposure master.

[24] The exposure master with a pellicle according to the above

[23] , wherein the exposure master is a phase shift photomask.

[25] The exposure master with a pellicle according to the above

[23] , wherein the exposure master is of a negative type.

[26] The exposure master with a pellicle according to the above

[23] , wherein the adhesive layer of the exposure master has an area that is not light-shielded or a semi-transparent light-shielded area.

[27] The exposure master with a pellicle according to

[23] above, wherein the adhesive layer of the exposure master has a transparent area attached thereto.

[28] The exposure master with a pellicle according to

[23] , wherein the exposure master is mainly composed of silicon oxide.

[29] The exposure master with a pellicle according to

[23] above, wherein the exposure master is a quartz substrate.

[30] A method for manufacturing a semiconductor device, comprising a step of exposing using an exposure master with a pellicle according to any one of

[23] to

[29] above.

[31] A method for producing a liquid crystal display panel, comprising a step of exposing using an exposure master with a pellicle according to any one of

[23] to

[29] above.

[32] A method for regenerating an exposed master, comprising peeling off the pellicle from the pellicle-attached exposed master described in any one of

[23] to

[29] above, and washing off any adhesive residue remaining on the exposed master with functional water, thereby regenerating the exposed master.

[33] A method for reducing the residue of an adhesive layer of a pellicle remaining on an exposure master when the pellicle is peeled off from an exposure master to which the pellicle is affixed, the method using a pellicle described in any one of

[14] to

[22] as the pellicle.

[34] An application of a pellicle having a pellicle membrane, a pellicle frame having the pellicle membrane provided on one end surface thereof, and an adhesive layer obtained from the pellicle adhesive provided on the other end surface of the pellicle frame, wherein the adhesive layer is exposed to exposure light.

[35] An application of a pellicle having a pellicle membrane, a pellicle frame having the pellicle membrane provided on one end surface thereof, and an adhesive layer obtained from the pellicle adhesive provided on the other end surface of the pellicle frame, the application of the pellicle being attached to a phase shift photomask.

[36] An application of a pellicle having a pellicle membrane, a pellicle frame having the pellicle membrane provided on one end surface, and an adhesive layer obtained from the pellicle adhesive provided on the other end surface of the pellicle frame, the application of the pellicle being attached to a negative-type exposure master.

[37] An application of a pellicle having a pellicle membrane, a pellicle frame having the pellicle membrane provided on one end surface, and an adhesive layer obtained from the pellicle adhesive provided on the other end surface of the pellicle frame, wherein the pellicle is attached to an exposed master having a non-light-shielded area or a translucent light-shielded area in the adhesive layer attachment portion of the exposed master.

[38] An application of a pellicle having a pellicle membrane, a pellicle frame having the pellicle membrane provided on one end surface, and an adhesive layer obtained from the pellicle adhesive provided on the other end surface of the pellicle frame, wherein the pellicle is attached to an exposed master having a transparent area in the attachment portion of the adhesive layer on the exposed master.

[39] An application of a pellicle having a pellicle membrane, a pellicle frame having the pellicle membrane provided on one end surface, and an adhesive layer obtained from the pellicle adhesive provided on the other end surface of the pellicle frame, the application of the pellicle being attached to a surface primarily composed of silicon oxide (particularly a quartz surface).

[40] An application of a pellicle having a pellicle membrane, a pellicle frame having the pellicle membrane provided on one end surface, and an adhesive layer obtained from the pellicle adhesive provided on the other end surface of the pellicle frame, the application of the pellicle being compatible with regeneration and cleaning using functional water.

[41] A peeling residue-reducing pellicle comprising a pellicle film, a pellicle frame with the pellicle film attached to one end surface thereof, and an adhesive layer provided on the other end surface of the pellicle frame for attaching the pellicle to an exposure master, wherein the adhesive layer is made of an acrylic resin having an SP value of 10.0 or more and 12.0 or less as a base material.

[42] The pellicle having reduced peeling residue according to

[41] above, wherein the pressure-sensitive adhesive layer further contains a polyvinyl ether compound.

[43] The pellicle having reduced peeling residue according to

[41] or

[42] above, which is a pellicle having reduced peeling residue for ArF lithography.

[44] A method for producing a pellicle with reduced peeling residue, comprising the steps of: selecting an adhesive for attaching the pellicle to an exposure master; applying the adhesive to one end surface of a pellicle frame to form an adhesive layer; removably attaching a protective member to the adhesive layer; applying an adhesive to the other end surface of the pellicle frame; and attaching a pellicle film to the adhesive layer; A method for producing a pellicle with reduced peeling residue, characterized in that in selecting the adhesive, an adhesive having an acrylic resin base material with an SP value of 10.0 or more and 12.0 or less is selected.

[45] The method for producing a pellicle with reduced peeling residue described in

[44] above, wherein the pressure-sensitive adhesive layer further contains a polyvinyl ether compound.

[46] A method for reducing a peeling residue of an adhesive layer of a pellicle remaining on an exposure master when the pellicle is peeled off from the exposure master to which the pellicle is attached, comprising the steps of: A method, comprising using the pellicle according to any one of

[41] to

[43] above as the pellicle. Effect of the Invention

[0017] According to the present invention, when a pellicle is peeled off from an exposed master after lithography, particularly after ArF lithography, a pellicle, a method for regenerating an exposed master, and a method for reducing peeling residues can be provided, which can reduce the peeling residues of the adhesive layer of the pellicle remaining on the exposed master. The pellicle, the exposed master with a pellicle, the method for regenerating an exposed master, and the method for reducing peeling residues of the exposed master of the present invention can peel off the pellicle from the exposed master with very little peeling residues of the adhesive even if the exposure light is irradiated through the exposed master. As a result, the regeneration cleaning of the exposed master from which the pellicle has been peeled off can be carried out well, and the cleaning conditions can be relaxed, which is advantageous in terms of reducing damage to the exposed master surface during cleaning. In addition, the production efficiency can be improved in the manufacture of semiconductor devices and liquid crystal display panels. It is believed that the pellicle of the present invention uses a specific acrylic polymer (also known as acrylic resin) as the adhesive base material, which improves the intermolecular forces within the adhesive and maintains an appropriate adhesive force, thereby reducing not only large residues but also particulate residues when peeled off from the exposed master. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a conceptual diagram showing the basic structure of a pellicle of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The basic structure of the pellicle of the present invention will first be described with reference to FIG.

[0020] 1, the pellicle 10 of the present invention comprises a pellicle film 12 stretched over the upper end surface of a pellicle frame 11 via an adhesive layer 13 for attaching the pellicle film, and in this case, an adhesive layer 14 for adhering the pellicle 10 to an exposure master (mask substrate or reticle) 1 is usually formed on the lower end surface of the pellicle frame 11, and a liner (not shown) is releasably attached to the lower end surface of the adhesive layer 14. The pellicle frame 11 may also be provided with an air pressure adjustment hole (vent) 15, and may further be provided with a dust filter 16 for the purpose of removing particles.

[0021] In this case, the size of these pellicle components is similar to that of ordinary pellicles, such as pellicles used in semiconductor lithography and pellicles used in the lithography process of manufacturing large liquid crystal display panels, and the materials thereof can be the well-known materials as described above.

[0022] The type of pellicle film 12 is not particularly limited, and for example, an amorphous fluoropolymer that has been conventionally used for excimer lasers may be used. Examples of amorphous fluoropolymers include Cytop (trade name of Asahi Glass Co., Ltd.), Teflon (registered trademark) AF (trade name of DuPont Co., Ltd.), etc. These polymers may be dissolved in a solvent as necessary when preparing the pellicle film, and can be appropriately dissolved in, for example, a fluorine-based solvent.

[0023] The base material of the pellicle frame 11 may be, for example, a conventionally used aluminum alloy material, preferably JIS A7075, JIS A6061, or JIS A5052 material, but there is no particular restriction on the aluminum alloy material as long as the strength of the pellicle frame is ensured. The surface of the pellicle frame is preferably roughened by sandblasting or chemical polishing, and a polymer coating may be provided after roughening. In the present invention, the method of roughening the frame surface may be a conventionally known method. A method of roughening the surface of an aluminum alloy material by blasting the surface with stainless steel, carborundum, glass beads, or the like, and then chemically polishing the surface with NaOH or the like is preferable.

[0024] Meanwhile, the inventors of the present invention have conducted extensive research and experiments in order to solve the above-mentioned problems of the present invention, focusing in particular on the characteristics of the adhesive that forms the adhesive layer, and have comparatively analyzed the experimental results, and have found that the following measures are effective. That is, the first aspect of the pellicle adhesive of the present invention is to use an acrylic polymer having an SP value of 10.0 or more and 12.0 or less as a base material. By setting the SP value of the acrylic polymer to 10.0 or more and 12.0 or less, when the pellicle is peeled off from the exposure master plate, the peeling residue of the adhesive layer remaining on the exposure master plate can be reduced. By setting the SP value to 10.0 or more, the residue that is difficult to remove by washing can be reduced. On the other hand, by setting the SP value to 12.0 or less, the volatility of the adhesive can be reduced, leading to the suppression of haze. The present inventors speculate that the effect of the present invention can be obtained by improving the hydrophilicity of the acrylic polymer by setting the SP value in a specific range.

[0025] The second aspect of the pellicle adhesive of the present invention is that the base material is an acrylic polymer having a (meth)acrylic acid ester having an ether bond as a monomer component. By including a (meth)acrylic acid ester having an ether bond as a monomer component of the acrylic polymer, it is possible to reduce the peeling residue of the adhesive layer remaining on the exposed master plate when the pellicle is peeled off from the exposed master plate. The introduction of an ether bond into the acrylic polymer makes it easier to control the hydrophilicity of the acrylic polymer. It is also presumed that the introduction of an ether bond into the side chain of the acrylic polymer suppresses photodegradation of the main chain.

[0026] In addition, the third aspect of the pellicle adhesive of the present invention is that the base material is an acrylic polymer having a side chain containing an ether bond. By including an ether bond in the side chain of the acrylic polymer, when the pellicle is peeled off from the exposure master, the peeling residue of the adhesive layer remaining on the exposure master can be reduced. By introducing an ether bond into the acrylic polymer, it becomes easier to control the hydrophilicity of the acrylic polymer. It is also presumed that by introducing an ether bond into the side chain of the acrylic polymer, photodegradation of the main chain can be suppressed.

[0027] The fourth aspect of the pellicle adhesive of the present invention is that the base material is an acrylic polymer having a side chain with higher decomposability by irradiation with exposure light than the main chain. By making the decomposability of the side chain of the acrylic polymer higher than that of the main chain by irradiation with exposure light, it is possible to reduce the peeling residue of the adhesive layer remaining on the exposed original plate when the pellicle is peeled off from the exposed original plate. It is presumed that by making the decomposability of the side chain higher than that of the main chain by exposure light, the decomposition of the side chain substantially precedes the decomposition of the main chain, and the peeling residue can be reduced. It is considered that the decomposition of the side chain has little effect on the deterioration of the adhesive, and even if the decomposition progresses, it is difficult to remain as a peeling residue at the time of peeling due to the cohesive force of the adhesive. On the other hand, it is considered that as the photodegradation of the main chain progresses, the main chain is decomposed into a lower molecular weight, and the decomposed adhesive is left on the substrate as a residue. Here, the difference in decomposability can be determined, for example, by comparing the decomposition products of the main chain and the decomposition products of the side chain before and after irradiation of the exposure light of the adhesive by IR, NMR, etc. More specifically, the change in the spectral intensity can be observed by comparing the IR chart of the adhesive before and after exposure to the exposure light. -1 COC (methoxy group), 1160cm -1 COC (ether group), 1727cm -1 C=O (ester group) and the like.

[0028] The fifth aspect of the pellicle adhesive of the present invention is that the base material is an acrylic polymer having a side chain that is selectively degraded by irradiation with exposure light. By selectively degrading the side chain of the acrylic polymer by irradiation with exposure light, it is possible to reduce the peeling residue of the adhesive layer remaining on the exposed original plate when the pellicle is peeled off from the exposed original plate. It is presumed that by selectively degrading the side chain by irradiation with exposure light, the decomposition of the side chain substantially precedes the decomposition of the main chain, and the peeling residue can be reduced. It is considered that the decomposition of the side chain has a relatively small effect on the deterioration of the adhesive, and even if the decomposition progresses, it is difficult to remain as a peeling residue at the time of peeling due to the cohesive force of the adhesive. On the other hand, it is considered that as the photodegradation of the main chain progresses, the main chain is degraded to a low molecular weight, and the degraded adhesive remains on the substrate as a residue. Here, the presence or absence of deterioration can be determined, for example, by comparing the decomposition products of the main chain and the decomposition products of the side chain before and after irradiation of the exposure light of the adhesive by IR, NMR, etc. More specifically, the change in the spectral intensity can be observed by comparing the IR chart of the adhesive before and after exposure to the exposure light. -1 COC (methoxy group), 1160cm -1 COC (ether group), 1727cm -1 C=O (ester group) and the like. In the present invention, the term "adhesive having an acrylic polymer as a base material" refers to an adhesive containing an acrylic polymer itself, or an adhesive containing a reaction product of an acrylic polymer and a curing agent or the like.

[0029] The inventors have discovered that in a pellicle provided with such an adhesive layer, the adhesive layer suppresses deterioration due to exposure light, and even if the pellicle does deteriorate, peeling residue is less likely to be left behind when the pellicle is peeled off from the mask substrate (exposure master). In the present invention, the acrylic polymer is, for example, a polymer having a (meth)acrylic acid ester as a monomer component, and can be copolymerized with a monomer component copolymerizable with the (meth)acrylic acid ester as necessary. Examples of the (meth)acrylic acid ester include a (meth)acrylic acid ester having an ether bond, a (meth)acrylic acid alkyl ester, and an unsaturated monomer having a carboxyl group or a hydroxyl group. By including a (meth)acrylic acid ester having an ether bond as a monomer component, an ether bond can be introduced into the side chain of the acrylic polymer.

[0030] Examples of the (meth)acrylic acid ester having an ether bond (component (A)) include (meth)acrylic acid esters having an alkylene oxide group such as an ethylene oxide group, a propylene oxide group, and a butylene oxide group. Among these, (meth)acrylic acid esters having an ethylene oxide group (also referred to as (meth)acrylates containing an ethylene oxide group) are preferred, and examples thereof include 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, phenoxyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate such as methoxydiethylene glycol (meth)acrylate, ethoxypolyethylene glycol (meth)acrylate such as ethoxydiethylene glycol (meth)acrylate, butoxypolyethylene glycol (meth)acrylate such as butoxydiethylene glycol (meth)acrylate, and phenoxypolyethylene glycol (meth)acrylate such as phenoxydiethylene glycol (meth)acrylate. These may be used alone or in combination of two or more.

[0031] Examples of (meth)acrylic acid alkyl esters (component (B)) include (meth)acrylic acid alkyl esters having an alkyl group with 1 to 14 carbon atoms. Specific examples include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, and lauryl (meth)acrylate. Among these, (meth)acrylic acid alkyl esters having an alkyl group with 4 or 8 carbon atoms are preferred from the viewpoint of achieving both pressure-sensitive adhesive properties and release properties. These may be used alone or in combination of two or more.

[0032] Examples of unsaturated monomers having a carboxyl group or a hydroxyl group (component (C)) include α,β-unsaturated carboxylic acids such as (meth)acrylic acid, maleic acid, crotonic acid, itaconic acid, and fumaric acid, and hydroxyl group-containing methacrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate. These may be used alone or in combination of two or more.

[0033] In the acrylic polymer, the proportion of the (A) component used in the total monomer components is preferably 30% by mass or more, more preferably 35% by mass or more, particularly preferably 35 to 98% by mass, and extremely preferably 40 to 95% by mass. By setting the proportion of the (A) component within the above range, it becomes easy to control the peeling residue and light resistance.

[0034] In the acrylic polymer, the proportion of the (B) component used is preferably 0 to 70% by mass, more preferably 3 to 55% by mass, based on the total monomer components. By setting the proportion of the (B) component within the above range, it becomes easy to control the adhesion.

[0035] In the acrylic polymer, the proportion of the (C) component used is preferably 0 to 10% by mass, more preferably 2 to 8% by mass, of the total monomer components. By setting the proportion of the (C) component within the above range, it becomes easy to control the degree of crosslinking caused by the reaction with the peeling residue and the curing agent.

[0036] The acrylic polymer can be produced by appropriately selecting a known production method such as solution polymerization, bulk polymerization, emulsion polymerization, radical polymerization, etc. The obtained acrylic polymer may be any of a random copolymer, a block copolymer, a graft copolymer, etc. When the molecular weight of the acrylic polymer is within the range of 700,000 to 2,500,000 as the weight average molecular weight, the pressure-sensitive adhesive layer has an appropriate cohesive strength and adhesive strength, is less likely to leave adhesive residue, and has sufficient adhesive strength and load-bearing capacity, which is preferable.

[0037] The weight average molecular weight is a value measured by gel permeation chromatography (GPC) analysis and is expressed in terms of standard polystyrene. The GPC analysis can be performed using tetrahydrofuran (THF) as a solvent. In this embodiment, the adhesive of the adhesive layer preferably contains a reaction product of an acrylic polymer and a curing agent, but may contain an acrylic polymer that does not react with the curing agent in consideration of softness.

[0038] The curing agent is not particularly limited as long as it is a curing material used as a normal adhesive, and examples thereof include metal salts, metal alkoxides, aldehyde compounds, non-amino resin amino compounds, urea compounds, isocyanate compounds, polyfunctional epoxy compounds, metal chelate compounds, melamine compounds, aziridine compounds, etc. Among these, isocyanate compounds and epoxy compounds are preferred from the viewpoint of reactivity with carboxyl groups or hydroxyl groups.

[0039] Examples of the isocyanate compound include xylylene diisocyanate, hexamethylene diisocyanate, tolylene diisocyanate, and multimers, derivatives, polymers, etc. These may be used alone or in combination of two or more.

[0040] Examples of epoxy compounds include compounds having two or more epoxy groups in the molecule, and specific examples thereof include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, diglycidylaniline, diamine glycidylamine, N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N'-diamine glycidylaminomethyl), etc. These may be used alone or in combination of two or more.

[0041] In the present invention, the SP value is defined as follows. [How to calculate SP value] In the present invention, the SP value is a solubility parameter. This SP value can be calculated by the following formula 1 with reference to the Fedors calculation method [Polymer Engineering and Science, Vol. 14, No. 2 (1974), pp. 148-154].

[0042]

number

[0043] In the above formula 1, δ is the solubility parameter (SP value); Δei is the molar evaporation energy; Δvi is the molar volume. The unit of the solubility parameter is (cal / mol). 1 / 2 The characteristic values ​​of Δei and Δvi given to the main atoms or atomic groups for the above formula 1 are shown in Table 1.

[0044] [Table 1]

[0045] The SP value (solubility parameter) of the acrylic polymer is preferably from 10.0 to 12.0, and more preferably from 10.0 to 11.0. The SP value of an acrylic polymer can be controlled, for example, by changing the polar group concentration in the acrylic polymer. For example, when a relatively highly polar bond such as an ether bond is introduced into the side chain, the SP value increases. On the other hand, when a relatively less polar bond such as a long-chain alkylene bond is introduced into the side chain, the SP value decreases.

[0046] In addition, the adhesive in the present invention may be a combination of two or more acrylic polymers as a base material, such as two or more acrylic polymers with different weight average molecular weights, two or more acrylic polymers with different monomer components, and two or more acrylic polymers with different copolymerization ratios. In this case, as long as the effects of the present invention are achieved, the SP value of only one acrylic polymer may be within the range, or the SP values ​​of all acrylic polymers may be outside the range but the SP value of the entire acrylic polymer components may be within the range. Here, the SP value of the entire acrylic polymer components is calculated by apportioning the SP values ​​of the two or more acrylic polymers according to their respective blending amounts.

[0047] The shape of the adhesive layer 14 is preferably flattened to reduce deformation during pellicle attachment and to suppress residual stress due to pellicle attachment, thereby reducing the effects of distortion and the like on the mask substrate to which it is attached.

[0048] It was also found that if the adhesive layer contains a polyvinyl ether compound, more favorable results tend to be obtained. Specifically, when vinyl ether groups are mixed in the adhesive layer so as to be uniformly dispersed throughout, the peelability of the adhesive is further improved, and there is almost no residue in visual inspection. The adhesive layer in which the vinyl ether groups are uniformly dispersed and mixed is less likely to generate dust even when exposed to 193 nm ultraviolet light after being attached to a mask substrate, and the probability of good peeling without leaving any peeling residue on the mask substrate is significantly improved.

[0049] That is, in the best mode of the present invention, the pellicle uses an acrylic polymer having an SP value of 10.0 or more and 12.0 or less as the base material constituting the mask adhesive layer, and contains a polyvinyl ether compound, so that even if the exposure light is irradiated through the mask substrate, surface deterioration is reduced, and fine particulate residues are also reduced when the pellicle is peeled off from the mask substrate. As a result, not only does the regeneration and cleaning of the mask substrate from which the pellicle has been peeled off proceed smoothly, but it also becomes possible to ease the cleaning conditions, which is advantageous in reducing damage to the mask surface during cleaning.

[0050] Examples of polyvinyl ether compounds include homopolymers of vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, butyl vinyl ether, isobutyl vinyl ether, and (2-methoxyethyl) vinyl ether, copolymers of two or more vinyl ethers, copolymers of these vinyl ethers with other monomers, etc. Among these, polyvinyl ether compounds containing methyl vinyl ether as a raw material monomer are preferred from the viewpoint of controlling peeling residues.

[0051] In the adhesive forming the adhesive layer 14, the blending ratio of the acrylic polymer and the polyvinyl ether compound is 90:10 to 99:1, preferably 92:8 to 98:2, and particularly preferably 94:6 to 96:4, on a mass basis, from the viewpoint of reducing peeling residue.

[0052] In addition, the adhesive forming the adhesive layer of the pellicle may contain other components such as crosslinkers, tackifiers, plasticizers, stabilizers, viscosity regulators, antistatic agents, lubricants, electrical conductivity imparting agents, flame retardant agents, thermal conductivity improvers, heat resistance improvers, weather resistance improvers, thixotropy imparting agents, antioxidants, antibacterial agents, antifungal agents, and colorants, depending on the purpose, within the scope of the present invention.

[0053] The adhesive layer 14 is formed by applying an uncured liquid or paste adhesive to the lower end surface of the pellicle frame 11, and then performing a curing process to form an adhesive layer. The adhesive may be applied once, or may be applied several times in order to obtain a predetermined thickness of the adhesive layer. In this case, it is preferable to leave the adhesive between each application until the shape of the adhesive after application is stabilized. In addition, if the viscosity of the adhesive is high and application is difficult, the adhesive may be diluted with an organic solvent, alcohol, water, etc. as necessary to reduce the viscosity of the adhesive before application. The adhesive can be applied by, for example, dipping, spraying, brushing, or using an application device such as a dispenser, but application using an application device such as a dispenser is preferable in terms of stability, workability, yield, etc.

[0054] In the manufacture of pellicle 10, normally, the adhesive layer 14 is applied and formed first, and then the pellicle film 12 is stretched, but the order may be reversed. The pellicle film 12 is stretched, for example, by applying an adhesive to the upper end surface of pellicle frame 11, then heating pellicle frame 11 to harden the adhesive, and finally attaching the upper end surface of pellicle frame 11 on which the adhesive layer 13 for attaching the pellicle film has been formed, to a pellicle film mounted on an aluminum frame larger than pellicle frame 11, and removing any excess of the pellicle film that protrudes outside pellicle frame 11 to complete the pellicle.

[0055] By using the pellicle of the present invention having the above-described configuration, it is possible to reduce the amount of adhesive residue when the pellicle is peeled off from the exposure master after use in lithography. In addition, according to the present invention, a method for reducing the peeling residue of the adhesive layer of the pellicle is provided by using the pellicle of the present invention. Therefore, the pellicle of the present invention is useful as a pellicle that can be attached to a phase shift photomask having the above-mentioned delicate phase shift film or a surface mainly composed of silicon oxide such as quartz.

[0056] It is also useful as a pellicle applied to an exposure master in which the pressure-sensitive adhesive layer is irradiated with exposure light during exposure, such as a negative-type exposure master, an exposure master having a non-light-shielded area or a semi-transparent light-shielded area in the adhesive-attached area, an exposure master having a transparent area in the adhesive-attached area, etc. The pressure-sensitive adhesive layer of the pellicle used in such an exposure master is exposed to exposure light through the exposure master from the side opposite to the side of the exposure master on which the pellicle is provided.

[0057] The pellicle of the present invention may be used not only as a protective member for preventing foreign matter from adhering to an exposed master in an exposure device, but also as a protective member for protecting the exposed master during storage or transportation of the exposed master. An exposed master with a pellicle can be manufactured by attaching the above-mentioned pellicle to an exposed master such as a photomask.

[0058] The manufacturing method of a semiconductor device or liquid crystal display panel according to this embodiment includes a step of exposing a substrate (semiconductor wafer or liquid crystal original plate) using the above-mentioned exposure master with pellicle. For example, in a lithography process, which is one of the manufacturing processes of a semiconductor device or liquid crystal display panel, the above-mentioned exposure master with pellicle is placed on a stepper and exposed to light in order to form a photoresist pattern corresponding to an integrated circuit or the like on the substrate. As a result, even if foreign matter adheres to the pellicle in the lithography process, the foreign matter is not imaged on the wafer coated with photoresist, so that short circuits or breaks in the integrated circuits or the like due to the image of the foreign matter can be prevented. Therefore, the use of the exposure master with pellicle can improve the yield in the lithography process.

[0059] In general, when a desired number of lithography steps are performed, when foreign matter or haze occurs, or when the pellicle film is damaged, the pellicle may be peeled off from the exposure master plate and the exposure master plate may be regenerated and cleaned.By using the pellicle of the present invention, even if the exposure master plate has a surface mainly composed of silicon oxide that is likely to cause peeling residue of the adhesive layer, a negative type exposure master plate in which the adhesive layer is irradiated with more exposure light than before, an exposure master plate having a non-shielded area or a semi-transparent light-shielded area in the adhesive attachment part in which the exposure light is irradiated with more exposure light than before, or an exposure master plate having a transparent area in the adhesive attachment part in which the exposure light is irradiated with more exposure light than before, the exposure master plate in which the adhesive layer is irradiated with more exposure light than before, the exposure master plate in which the adhesive layer is irradiated with more exposure light than before, etc., the peeling residue during repellicle can be reduced. In addition, by using the pellicle of the present invention, the amount of peeled off residue of the adhesive layer is reduced, making it easier to apply cleaning with functional water, and improving the cleaning properties of delicate exposure masters such as phase shift photomasks. In addition, cleaning with functional water can contribute to reducing the environmental load. EXAMPLES

[0060] The present invention will be specifically illustrated and described below with reference to examples. Note that the "mask" in the examples and comparative examples is described as an example of an "exposure master", and it goes without saying that the present invention can also be applied to a reticle in the same manner.

[0061] Example 1 After precision cleaning of an aluminum alloy pellicle frame (outer dimensions 149mm x 115mm x 3.5mm, thickness 2mm, flatness of the end surface coated with the adhesive for attaching the mask: 15um), an acrylic adhesive manufactured by Soken Chemical Industries, Ltd. (product name: SK Dyne SN-70A, containing an acrylic polymer as a base material in which 95% of the monomer component is ethylene oxide group-containing (meth)acrylate, SP value of the base material is 10.2) was applied to the end surface on the side with a flatness of 15um, and left to stand at room temperature for 60 minutes. After that, a separator was placed on an aluminum plate with a flatness of 5um, and the pellicle frame coated with the adhesive was placed so that the adhesive was facing downwards. As a result, the adhesive came into contact with the flat separator and was flattened. Next, the pellicle on the aluminum plate was placed in a 60°C oven for 60 minutes to harden the adhesive. Then, the pellicle was taken out together with the aluminum plate, and the separator was peeled off.

[0062] Then, an adhesive (product name: Cytop CTX-A) manufactured by Asahi Glass Co., Ltd. was applied to the end surface opposite to the adhesive coating. The pellicle frame was then heated to 130°C to harden the adhesive. Finally, the adhesive-coated end face of the pellicle frame was attached to a pellicle film mounted on an aluminum frame larger than the pellicle frame, and the portion outside the pellicle frame was removed to complete the pellicle.

[0063] Next, the 6025 mask substrate (6 inches) and the pellicle prepared above were set in the attachment device, and the pellicle was attached to the mask substrate by applying a pressure of 50 N for a loading time of 30 seconds.

[0064] The mask substrate with the pellicle attached was left at room temperature for 24 hours, and then ultraviolet light was applied from the back of the mask at 10 mJ / cm using a 193 nm ultraviolet lamp so that the light hit the pellicle adhesive. 2 Irradiated. After the ultraviolet irradiation, the mask was left at room temperature for 1 hour, and then the pellicle was slowly peeled upward from the mask substrate at a speed of 0.1 mm / sec.

[0065] When the mask substrate was visually inspected after peeling, only a few thin opaque streaks were observed at the outline where the pellicle had been attached, which were thought to be solute residues of the adhesive, and the surface of the mask substrate was clearly cleaner than that of the comparative example described below.The above residues could be removed in 5 minutes by immersing the mask substrate in a cleaning tank (with functional water overflowing) using ultrasonic waves and functional water (ultrapure water with hydrogen and ammonia added).

[0066] Example 2 A pellicle was completed using the same method and materials as in Example 1, except that an acrylic adhesive manufactured by Soken Chemical Industries, Ltd. (product name: SN-25B, containing an acrylic polymer as a base material in which 40% by mass of the monomer component is an ethylene oxide group-containing (meth)acrylate, SP value of the base material is 10.5) was used as the adhesive. Furthermore, the pellicle was attached to a mask substrate and peeled off under the same conditions as in Example 1.

[0067] When the mask substrate after peeling was visually observed, only a thin opaque streak was observed at the outline where the pellicle had been attached, which was thought to be a solute residue of the adhesive, and the surface of the mask substrate was clearly clean compared to that of the comparative example described below. In addition, the above residues could be removed by washing the mask substrate twice for 5 minutes in a cleaning tank (with functional water overflowing) using ultrasonic waves and functional water (ultrapure water with hydrogen and ammonia added) in the same manner as in Example 1.

[0068] Example 3 Except for the fact that 100 parts by mass of SK Dyne SN-70A was used as the adhesive and 3 parts by mass of a polyvinyl ether compound was used, a pellicle was completed using the same method and materials as in Example 1. Furthermore, the pellicle was attached to a mask substrate and peeled off under the same conditions as in Example 1.

[0069] When the mask substrate after peeling was visually observed, only a thin glossy transparent streak was seen on the outline where the pellicle had been attached, which was thought to be a solvent residue of the adhesive, and the mask substrate was clean with almost no trace of solute residue of the adhesive. Subsequent cleaning was possible with a 3-minute cleaning using the same equipment as in Example 1.

[0070] Comparative Example 1 A pellicle was completed using the same method and materials as in Example 1, except that an acrylic adhesive manufactured by Soken Chemical & Engineering Co., Ltd. (product name: SK Dyne SK-1425S, containing an acrylic polymer as a base material that does not contain a (meth)acrylic acid ester having an ether bond as a monomer component, SP value of the base material 9.8) was used as the adhesive. Furthermore, the pellicle was attached to a mask substrate and peeled off under the same conditions as in Example 1.

[0071] When the mask substrate after peeling was visually observed, a thin solute residue of the adhesive was found in the area where the pellicle had been attached. The peeling residue was removed by washing twice for 5 minutes using the same equipment as in Example 1, but it could not be completely removed, so it was necessary to lightly rub the residue with a polyvinyl alcohol foam before the washing.

[0072] Comparative Example 2 A pellicle was completed using the same method and materials as in Example 1, except that an acrylic adhesive manufactured by Soken Chemical & Engineering Co., Ltd. (product name: SK Dyne SK-1495S, containing an acrylic polymer as a base material that does not contain a (meth)acrylic acid ester having an ether bond as a monomer component, SP value of the base material 9.2) was used as the adhesive. Furthermore, the pellicle was attached to a mask substrate and peeled off under the same conditions as in Example 1.

[0073] When the mask substrate after peeling was visually observed, a thin solute residue of the adhesive was found in the area where the pellicle had been attached. As in Comparative Example 1, the peeling residue could not be removed by ultrasonic cleaning with functional water alone, but could be removed by combining it with scrubbing cleaning with polyvinyl alcohol foam before the above cleaning.

[0074] (Synthesis Example 1) In a 5L flask equipped with a stirrer, reflux condenser, thermometer and gas inlet, 320g of butyl acrylate, 550g of 2-methoxyethyl acrylate, 80g of acrylic acid, 50g of 2-hydroxyethyl acrylate, 1500g of ethyl acetate and 2g of azobisisobutyronitrile as a polymerization initiator were charged and solution polymerization was carried out for 8 hours at 68°C in a nitrogen gas stream. After the reaction was completed, 830g of ethyl acetate was added to the mixture to obtain a solution of an acrylic polymer (SP value 10.6) with a solid content of 30%. A solution of polyisocyanate was added to the obtained acrylic polymer solution and mixed by stirring to obtain an adhesive.

[0075] (Synthesis Example 2) 400g of 2-ethylhexyl acrylate, 500g of 2-ethoxyethyl acrylate, 100g of acrylic acid, 1200g of ethyl acetate, and 2g of azobisisobutyronitrile as a polymerization initiator were charged into a 5L flask equipped with a stirrer, reflux condenser, thermometer, and gas inlet, and solution polymerization was carried out at 68°C for 8 hours in a nitrogen gas stream. After the reaction was completed, 1130g of ethyl acetate was added to the mixture to obtain a solution of an acrylic polymer (SP value 10.1) with a solid content of 30%. A solution of polyisocyanate was added to the obtained acrylic polymer solution, and the mixture was stirred and mixed to obtain an adhesive.

[0076] (Synthesis Example 3) In a 5L flask equipped with a stirrer, reflux condenser, thermometer and gas inlet, 350g of 2-ethylhexyl acrylate, 550g of 2-methoxyethyl acrylate, 50g of methacrylic acid, 50g of 2-hydroxyethyl methacrylate, 1400g of ethyl acetate and 2g of azobisisobutyronitrile as a polymerization initiator were charged and solution polymerization was carried out at 68°C for 8 hours in a nitrogen gas stream. After the reaction was completed, 930g of ethyl acetate was added to the mixture to obtain a solution of an acrylic polymer (SP value 10.2) with a solid content of 30%. A solution of polyisocyanate was added to the obtained acrylic polymer solution and mixed by stirring to obtain an adhesive.

[0077] (Synthesis Example 4) In a 5L flask equipped with a stirrer, reflux condenser, thermometer and gas inlet, 300g of butyl acrylate, 550g of 2-methoxyethyl acrylate, 100g of propyloxybutyl acrylate, 50g of itaconic acid, 1500g of ethyl acetate and 2g of azobisisobutyronitrile as a polymerization initiator were charged and solution polymerization was carried out at 68°C for 8 hours in a nitrogen gas stream. After the reaction was completed, 830g of ethyl acetate was added to the mixture to obtain an acrylic polymer solution with a solid content of 30%. A polyisocyanate solution was added to the obtained acrylic polymer solution (SP value about 10.7) and mixed by stirring to obtain an adhesive.

[0078] (Synthesis Example 5) In a 5L flask equipped with a stirrer, reflux condenser, thermometer, and gas inlet, 300g of butyl acrylate, 600g of methoxypolyethylene glycol acrylate, 100g of acrylic acid, 1400g of ethyl acetate, and 2g of azobisisobutyronitrile as a polymerization initiator were charged, and solution polymerization was carried out at 68°C for 8 hours in a nitrogen gas stream. After the reaction was completed, 930g of ethyl acetate was added to the mixture to obtain a solution of an acrylic polymer with a solid content of 30% (SP value of about 10). A solution of polyisocyanate was added to the obtained acrylic polymer solution, and the mixture was stirred and mixed to obtain an adhesive.

[0079] (Examples 4 to 8) Pellicles were prepared in the same manner as in Example 1, except that the adhesives obtained in Synthesis Examples 1 to 5 were used as the adhesives, and peeling tests were carried out. As a result, in the pellicles using any of the adhesives, the amount of peeling residue was reduced compared to the comparative examples, and the cleaning removability was improved. [Explanation of symbols]

[0080] 1 Exposure master 10 Pellicle 11 Pellicle frame 12 Pellicle membrane 13 Adhesive layer for attaching pellicle membrane 14 Adhesive layer 15 Air pressure adjustment hole (vent) 16 Dust removal filter

Claims

1. A pellicle adhesive for attaching a pellicle to an exposure master plate, It is used to form an adhesive layer provided on one end surface of a pellicle frame constituting the pellicle, When the pellicle is peeled off after being attached to the exposure master, the adhesive layer is peeled off from the exposure master together with the pellicle frame, An adhesive for pellicles, comprising as a base material an acrylic polymer having an SP value of 10.0 or more and 12.0 or less.

2. An adhesive for pellicles as described in claim 1, which has an acrylic polymer as a base material having a (meth)acrylic acid ester having an ether bond as a monomer component.

3. An adhesive for pellicles as described in claim 2, wherein the (meth)acrylic acid ester having an ether bond is a (meth)acrylic acid ester having an alkylene oxide group.

4. An adhesive for pellicles as described in claim 3, wherein the alkylene oxide group is an ethylene oxide group.

5. The pressure-sensitive adhesive for a pellicle according to any one of claims 2 to 4, further comprising an unsaturated monomer having a carboxyl group or a hydroxyl group as a monomer component.

6. The adhesive for a pellicle according to any one of claims 2 to 5, further comprising an alkyl (meth)acrylate ester as a monomer component.

7. A pellicle frame with an adhesive layer, comprising: a pellicle frame; and an adhesive layer obtained from the adhesive for a pellicle according to any one of claims 1 to 6 provided on one end surface of the pellicle frame.

8. A pellicle having a pellicle frame and a pellicle membrane, and an adhesive layer obtained from the pellicle adhesive described in any one of claims 1 to 6 on one end surface of the pellicle frame.

9. 9. The pellicle of claim 8, wherein the adhesive layer is exposed to an exposure light beam.

10. 9. The pellicle according to claim 8, which is attached to an exposure master having a non-light-shielding area or a semi-transparent light-shielding area in the area where the adhesive layer is attached.

11. The pellicle according to claim 8, which is attached to an exposure master having a transparent area in the area where the adhesive layer is attached.

12. An exposure master with a pellicle, comprising the pellicle according to any one of claims 8 to 11 attached to the exposure master.

13. An exposure method comprising exposing using an exposure master with a pellicle as described in claim 12.

14. A method for manufacturing a semiconductor device, comprising a step of exposing using the pellicle-attached exposure master according to claim 12.

15. A method for manufacturing a liquid crystal display panel, comprising a step of exposing using the pellicle-attached exposure master according to claim 12.

Citation Information

Patent Citations

  • Semiconductor differential pressure transmitter

    JP1981038693A

  • Large pellicle

    JP2006146085A

  • Photomask

    JP2007310175A

  • Adjustment request support device, delivery date reply / shipment adjustment system, and delivery date reply / shipment adjustment method

    JP2008021182A

  • Pellicle

    JP2011128605A