X-ray rotating anode with integral liquid metal bearing shell.

The X-ray rotating anode system with a liquid metal bearing shell addresses heat dissipation and mechanical support issues by using a Mo-based alloy anode and bush, enabling high-frequency operation and reduced fatigue.

JP7579870B2Active Publication Date: 2024-11-08PLANSEE SE
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2022549883
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-20
Filing Date
2021-01-28
Publication Date
2024-11-08
Estimated Expiration
2041-01-28

AI Technical Summary

Technical Problem

Existing X-ray rotating anodes face challenges in providing effective heat dissipation and mechanical support at high rotational frequencies, leading to material fatigue and overheating, particularly in high-power applications.

Method used

An X-ray rotating anode system with an integrated liquid metal bearing shell, featuring a Mo or Mo-based alloy anode disk and bearing bush, utilizing a liquid metal bearing running surface for frictionless rotation and enhanced heat dissipation, supported by a materially bonded connection such as friction welding or diffusion bonding.

Benefits of technology

The system achieves high operational reliability, effective heat dissipation, and mechanical stability, allowing rotational frequencies up to 300Hz with reduced material fatigue, suitable for high-power X-ray generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579870000001
    Figure 0007579870000001
  • Figure 0007579870000002
    Figure 0007579870000002
  • Figure 0007579870000003
    Figure 0007579870000003
Patent Text Reader

Abstract

The present invention relates to an X-ray rotary anode with an integrated liquid metal bearing shell, comprising an anode disk (5) made of Mo or a Mo-based alloy and having a hole (12) formed centrally in the region of the rotation axis (4) and extending axially through at least part of the anode disk (5), and a bearing bush (20) made of Mo or a Mo-based alloy. The bearing bush (20) is connected to the anode disk (5) via a materially bonded connection (21) so that an inner wall (22) of the bearing bush (20) continues into the hole (12) of the anode disk (5) and so that at least one axial section of the inner wall (14) of the hole (12) of the anode disk (5) and at least one axial section of the inner wall (22) of the bearing bush (20) are formed circumferentially as liquid metal bearing running surfaces and form at least part of the liquid metal bearing shell. The present invention also relates to a corresponding manufacturing method.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an X-ray rotating anode having an integrated liquid metal bearing outer shell according to the preamble of claim 1, an X-ray rotating anode system having an X-ray rotating anode having an integrated liquid metal bearing outer shell and an inner liquid metal bearing shell inserted therein, and a method for manufacturing such an X-ray rotating anode. [Background technology]

[0002] X-ray rotating anodes are used in X-ray tubes to generate X-rays. In use, electrons are emitted from the cathode of the X-ray tube and accelerated in the form of a focused electron beam towards the rotating X-ray rotating anode. Due to the rotational movement of the X-ray rotating anode, the electron beam scans a circular orbit (focal track). Most of the energy of the electron beam is converted into heat at the X-ray rotating anode, but a small part is emitted as X-rays. The locally released heat leads to strong heating of the X-ray rotating anode. The rotation of the X-ray rotating anode counters overheating of the anode material.

[0003] Especially in the high power region, a high radiation output (or dose output) is required, which can be generated by using a tightly focused electron beam of correspondingly high energy. To avoid material fatigue due to high temperatures and high temperature gradients, the X-ray rotating anode must be designed for high rotational frequencies and effective and uniform heat dissipation. Considering these requirements, it is advantageous to use liquid metal bearings for the support of the X-ray rotating anode.

[0004] X-ray rotating anode systems are known from US Pat. No. 5,399,623 and US Pat. No. 5,499,633, respectively, in which a liquid metal bearing shell is used as an insert in the central through-hole of the X-ray rotating anode. Furthermore, US Pat. No. 5,499,623 discloses a friction welding method with an intermediate piece introduced into the welding zone. Other X-ray rotating anode systems are known from US Pat. No. 5,499,623 and US Pat. No. 5,499,633. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] US Patent Application Publication No. 2016 / 0086760A1 [Patent Document 2] US Patent Application Publication No. 2017 / 0125199A1 [Patent Document 3] U.S. Patent No. 5,204,890A [Patent Document 4] U.S. Patent No. 6,198,805 B1 [Patent Document 5] German Patent Application Publication No. 102015215306A1 [Patent Document 6] JP 2012-084400 A [Patent Document 7] German Patent Application Publication No. 102015204488A1 [Patent Document 8] US Patent Application Publication No. 2017 / 0169984A1 Summary of the Invention [Problem to be solved by the invention]

[0006] The object of the present invention is to improve the X-ray rotating anode with respect to good support at high rotation frequencies and uniform and effective heat dissipation. Furthermore, it should enable a cost-effective and process stable production of the X-ray rotating anode. [Means for solving the problem]

[0007] This problem is solved according to the invention by an X-ray rotating anode according to claim 1, by an X-ray rotating anode system according to claim 10 and by a method for manufacturing an X-ray rotating anode according to claim 15. Advantageous developments of the invention are described in the dependent claims.

[0008] According to the invention, an X-ray rotating anode with an integrated liquid metal bearing shell is provided. The X-ray rotating anode comprises an anode disk made of Mo (Mo: molybdenum) or a Mo-based alloy and a bearing bush made of Mo or a Mo-based alloy, the anode disk having a hole formed centrally in the region of the rotation axis and extending axially through at least a part of the anode disk. The inner wall of the bearing bush is formed as a liquid metal bearing running surface at least over its entire axial section (i.e. in the circumferential direction with respect to the rotation axis) and forms a first subsection of the liquid metal bearing shell. In particular, the entire (typically cylindrical) inner wall of the bearing bush can be formed as a liquid metal bearing running surface. However, instead, only an axial section of the inner wall of the bearing bush, which is also typically formed cylindrically, can also be formed as a liquid metal bearing running surface, while another axial section can have, for example, a mechanical limiting element and / or a coating, whereby the liquid metal is retained in the liquid metal bearing during use. The liquid metal bearing shell is formed by a first subsection and an adjacent second subsection and has a continuous liquid metal bearing running surface. The bearing bush is connected to the anode disk via a materially bonded connection in such a way that the inner wall of the bearing bush continues into the hole in the anode disk. Furthermore, at least one axial section of the inner wall of the hole in the anode disk is formed as a running surface for the liquid metal bearing in a surrounding manner (i.e. in the circumferential direction relative to the rotation axis) and forms at least a part of the second subsection of the liquid metal bearing shell. Here too, the entire inner wall of the hole (typically formed cylindrically) can be formed as a running surface for the liquid bearing in a surrounding manner. In the case of a blind hole, the bottom of the hole can also form the liquid metal bearing running surface. However, instead, only an axial section of the inner wall of the hole, which is also usually formed cylindrically, can be formed as a liquid metal bearing running surface in the circumferential direction.

[0009] In the case of liquid metal bearings, a defined bearing gap is formed between the outer liquid metal bearing shell and the inner liquid metal bearing shell, which are adapted to one another, one formed on the stationary part and the other formed on the rotating part. Here, the outer liquid metal bearing shell is formed integrally with the X-ray rotating anode and thus as the rotating part. The inner liquid metal bearing shell can be formed integrally, for example, on a pin (stationary part) inserted in the outer liquid metal bearing shell. In use, the bearing gap is filled with liquid metal (for example gallium, a gallium alloy such as a eutectic gallium-indium-tin alloy, etc.). The gap width is typically from a few micrometers to 500 μm (at least ≦1 mm), in particular 5-500 μm, preferably 7-40 μm, and the gap width can vary over the length of the bearing gap. In particular, the outer and / or inner liquid metal bearing shells may be provided with at least one circumferential recess and / or step or rib, in the region of which the gap width may also be formed differently with respect to the remaining part of the bearing gap (see, for example, US Pat. No. 5,399,313). In particular, at least one circumferential rib on one component together with (at least) one corresponding groove on the other component may fix the two components to each other in the axial direction. The liquid metal bearing running surfaces are referred to as sections of the outer and inner liquid metal bearing shells which are wetted with liquid metal during use on both the outer and inner liquid metal bearing shells, thereby allowing frictionless rotation. The liquid metal prevents direct contact between the outer and inner liquid metal bearing shells and at the same time acts as a lubricant, thereby resulting in good running properties. To drive the X-ray rotating anode, the outer liquid metal bearing shell is equipped with a rotor or is (mechanically) connected to a rotor and is rotated in a known manner in cooperation with a stator.

[0010] It is advantageous to use liquid metal bearings to support the X-ray rotating anode, since liquid metal bearings are designed for high loads and high rotational speeds and at the same time have a high level of operational reliability and a long service life. One advantage (for example compared to ball bearings) is that the increased pressure of the liquid metal in the bearing gap is built up over a larger surface section (especially the axial extent), thus increasing the mechanical stability. In particular, ball bearings are typically designed for rotational frequencies well below 200 Hz (for example 140 Hz), while liquid metal bearings allow rotational frequencies up to 300 Hz (Hertz). Furthermore, liquid metal bearings are quieter compared to ball bearings and allow effective heat dissipation over a large area due to the increased contact area (through the bearing gap filled with liquid metal). In this way, heat is effectively dissipated to stationary components (for example pins inserted inside the outer shell of the liquid metal bearing). Heat can then be effectively dissipated from the stationary parts via internal cooling (by coolant conducted in at least one cooling channel), making thermal management very effective and therefore suitable for high power ranges. On the other hand, ball bearings are not designed for effective heat dissipation through the bearings due to the use of heat sensitive coatings, which could damage the respective coatings.

[0011] Mo or Mo-based alloys are particularly advantageous as anode disk material and as bearing bush material, since they have high strength (even at high service temperatures) and allow good heat dissipation. Furthermore, Mo or Mo-based alloys have good wettability with the liquid metals typically used. Therefore, since already good wettability is provided by the substrate, it is advantageous further that the inner walls of the holes of the anode disk and the inner walls of the bearing bush are formed as liquid metal bearing running surfaces. In some cases, a coating (typically less than 10 μm thick) can be provided completely or only partially on the inner walls of the bearing bush and / or on the inner walls of the holes, respectively. However, no separate insert with an inner liquid metal bearing shell is provided, which would have to be inserted into the holes of the anode disk and connected to it. This would make the manufacture more complicated and could be a barrier to heat dissipation. Furthermore, a high level of mechanical stability is achieved between the anode disk and the liquid metal bearing shell, which is advantageous for the running properties. The inner wall of the bearing bush continues to the inner wall of the hole in the anode disk, providing a liquid metal bearing running surface with a correspondingly long axial extension, thereby ensuring mechanically stable and accurate guidance when the anode disk rotates.

[0012] Mo-based alloys are understood here to mean alloys containing more than 50% by weight of Mo. In particular, Mo-based alloys contain at least 80% by weight of Mo, more preferably at least 98% by weight of Mo, which is particularly advantageous in view of the above-mentioned properties of Mo. In this case, the anode disk and the bearing bush do not have to be entirely made of Mo or a Mo-based alloy, but particular reference is made here to the substrate. In particular, the substrate may comprise a coating (for example a blackening layer for increasing the radiant heat output), a carbon-based body (for example a graphite body) attached to the anode disk as a heat accumulator, a mounting part such as a flange on the bearing bush, or a coating, for example a circumferential focal track coating applied in the area of ​​the focal track. As explained at the beginning, the "focal track" refers to the section of the anode disk that surrounds the rotation axis in an annular manner, which section is scanned by the electron beam during use. Typically, the focal track coating is applied on the anode disk in the area of ​​the focal track (having a certain radial extent). The focal track coating is in particular formed by W or a W-Re alloy with a Re content of 1-15% by weight, in particular 5-10% by weight (W: tungsten, Re: rhenium). Furthermore, the anode disk typically has an inclined focal track surface in the region of the focal track, which preferably forms a frustoconical peripheral surface. In particular, the focal track surface is angled with respect to a reference plane extending perpendicular to the rotation axis, so that the exit of the generated X-ray radiation is possible via a lateral exit window of the respective X-ray device. For example, a focal track angle in the range of 2° to 16.25°, in particular 7° to 13°, is formed with respect to this reference plane.

[0013] The "axis of rotation" referred to is given by the rotationally symmetric basic shape of the X-ray rotating anode and the liquid metal bearing shell. This axis of rotation simultaneously designates the "axial" direction (running parallel to it) and the "radial" direction (running perpendicular to it). The "reference plane" of the X-ray rotating anode (which typically also forms its main extension plane) extends in particular perpendicular to the axis of rotation. It should be noted that the X-ray rotating anode does not have to be designed to be rotationally symmetric in all details, so that for example circumferentially formed slots, periodically arranged projections, recesses, mounting parts, etc. can break the exact rotational symmetry. A bearing bush is here understood to be a part with a (through) hole whose inner wall is formed at least partially as a liquid metal bearing running surface, and the bearing bush can have various (in particular external) contours and mounting parts. In a preferred variant, the bearing bush (and the corresponding mechanical holder of the X-ray rotating anode) is arranged on the side of the anode disk opposite the focal track. Alternatively, the bearing bush (and the corresponding mechanical holder of the rotating X-ray anode) can be arranged on the side of the anode disc on which the focal track is provided.

[0014] According to the invention, the first subsection of the liquid metal bearing shell is monolithically formed with the bearing bush, and at least a part of the second subsection of the liquid metal bearing shell is monolithically formed with the anode disk. "Monolithic" means that the component is produced in one piece in a metallurgical production (preferably by powder metallurgy or alternatively by molten metallurgy) and is capable of subsequent mechanical processing and / or formation of at least one layer, for example to form pores and / or surface structures. A monolithic formation can be recognized by the expert from a uniform and continuous microstructure (of the substrate made of Mo or a Mo-based alloy). Powder metallurgical production of the anode disk and / or the bearing bush is preferred, which includes the steps of compression and sintering of the corresponding starting powders and preferably a subsequent shaping step (for example rolling, forging, extrusion, etc.) of the resulting shaped article. Powder metallurgical production results in a typical and expert-recognizable microstructure, which can be clearly distinguished from, for example, a molten structure (obtained in a molten metallurgical production). The inner wall of the bearing bush is therefore formed, at least in the region of the liquid metal bearing running surface, from the base material of the bearing bush (Mo or Mo-based alloy) and the inner wall of the hole of the anode disk is formed, at least in the region of the liquid metal bearing running surface, from the base material of the anode disk (Mo or Mo-based alloy). Furthermore, the inner wall of the bearing bush and / or the inner wall of the hole of the anode disk can be provided with a coating (typically less than 10 μm thick) and / or a surface structure.

[0015] A connection by a material bond is understood to mean that a continuous material bond is produced, but does not mean that only a mechanical connection is present (e.g. via a screw or clamp connection, via mechanical fixing elements, etc.). In particular, the connection by a material bond between the bearing bush and the anode disk is produced by welding, by soldering or by diffusion bonding (diffusion connection). When examining the connection zones microscopically on a polished surface, an expert can distinguish a welded joint via a corresponding weld zone (melted or at least plasticized base material), a soldered connection via a corresponding solder zone (molten structure of the solder) and a diffusion connection via a corresponding diffusion zone (diffusion area of ​​the base material joined to one another).

[0016] A structure as a liquid metal bearing shell can be recognized by a specialist by its shape, in particular the inner contour which allows the introduction of a pin (or other component) with the liquid metal bearing running surface and the corresponding liquid metal bearing inner shell, which are arranged rotationally symmetrically with respect to the rotation axis therein. Furthermore, the inner contour is not provided with running grooves for ball bearings (even if the running surface of the liquid metal bearing can in principle be provided with steps and / or with ribs or recesses). In the region of the ends of the liquid metal bearing shell and / or the inner liquid metal bearing shell, surface structures, coatings and / or mechanical limiting elements can be provided to keep the liquid metal in the region of the liquid metal bearing.

[0017] According to one development, the materially bonded connection is a connection produced by diffusion bonding, a friction welded connection or a beam welded connection (by laser or electron beam). The advantage of the abovementioned connection techniques is that a materially bonded connection with high strength can be achieved even at high application temperatures. In particular, in the region of the connection zone, it is possible to dispense with additional materials (solder, welding additional materials, etc.) which may form troublesome impurities (e.g. in the liquid metal) in the region of the liquid metal bearing, which may be dangerous for the vacuum stability (application takes place in high vacuum) and / or which may have a lower melting point (compared to the base material of the connected components). This is particularly advantageous compared to soldered connections using solders which typically have a low melting point and a lower strength than the base material (of the connected components) at least at high temperatures.

[0018] In diffusion bonding, the (typically appropriately prepared) surfaces of the parts to be connected are joined together and the application of pressure and temperature causes a diffusion of atoms in the region of the connection zone, which results in a connection by material bonding (diffusion connection). According to the (more detailed) understanding of diffusion bonding used here, in the region of the connection zone, no melting of the substrates of the parts to be connected occurs. As already explained above, the diffusion bond can be recognized by the expert through a microscopic examination of the connection area in a micrograph on the basis of the corresponding diffusion zone (diffusion area of ​​the substrates joined together) in which no melt structure occurs. If parts made of the same material are connected to each other by diffusion bonding, the diffusion connection may not be recognizable in a micrograph. This is because in the region of the connection zone a homogeneous structure is obtained that reaches to each substrate. In these cases, the presence of a diffusion connection can be inferred only from the external geometric shape of the connected parts (here the anode disk and the bearing bush). This is because, for example, they would not be able to be manufactured in one piece (for example by powder metallurgy) with their respective overall shape. Beam welded connections can be recognized by an expert on the basis of microscopic examination of the connection zone in a micrograph on the basis of the weld zone, in which the corresponding fusion structure (of the base material and possibly additionally used weld add-on material) appears, and on the basis of the root and position of the fusion zone. Beam welded connections, in particular beam welded connections by electron beam welding, are advantageous due to the small heat-affected zone. Furthermore, beam welding processes are more suitable for Mo-based alloys than for pure molybdenum.

[0019] In friction welding, one part is in contact with the other part to be joined and moved (e.g. rotated) relative to the other part, whereby heat is generated at the abutment surface. The welding is completed by applying a force during or after the relative motion (e.g. rotational motion), but there are several forms of energy supply and relative motion. In this case, the connection of parts that are almost rotationally symmetrical is important, since in order to generate frictional heat, preferably one part (e.g. a bearing bush or a cutting piece) is rotated and then brought into contact with the other part (e.g. an anode disk). Friction welding, which also allows the connection of parts with thicker walls (especially 20-130 mm), requires only relatively low joining temperatures at the joining cross section and is therefore often suitable for materials and material combinations that are difficult to weld otherwise (see also DIN EN ISO 15620 in this regard). This applies in particular to pure Mo, but also to Mo-based alloys. Friction welded connections can be recognized by experts from microscopic examination of the connection zone in micrographs on the basis of the typical microstructure. In particular, no molten structure is recognized, since the base material is only in a plasticized state during friction welding. Typically, the weld is relatively narrow and has a fine grain structure. In particular, in the case of friction welded connections between a bearing bush and an anode disk, each made of Mo and / or Mo-based alloys, several subzones can be recognized in the area of ​​the weld zone with a slightly different structure (between the base materials of the bearing bush and the anode disk). This applies in particular to the grain size distribution and the grain orientation. Typically, the grains are elongated in the direction of the material flow, which occurs in particular when the weld bead is formed. Zones of different grain aspect ratios (high grain aspect ratio near the bearing bush and low grain aspect ratio near the anode disk) occur in particular when the bearing bush has a high grain aspect ratio and the anode disk has a lower grain aspect ratio, which is brought about by the respective manufacturing processes for these components. Macroscopically, a friction welded connection is indicated when protruding connection parts are used on the anode disc to allow the formation of a weld bead (due to the flow of material during the compression phase during friction welding).This can be noticed in particular in the weld zone between the connecting part and the bearing bush, away from the anode disk.

[0020] According to one development, the Mo-based alloy (of the anode disk and / or the bearing bush) is MHC and / or TZM. In particular, the substrate of the bearing bush (i.e. excluding the coating, mounting parts, etc.) is made of MHC and / or TZM (preferably only from MHC or only from TZM). In particular, the substrate of the anode disk (i.e. excluding the coating, mounting parts, etc.) is made of MHC and / or TZM (preferably only from MHC or only from TZM). Both alloys (MHC, TZM) have high strength and hardness. Their mechanical properties are largely retained at high temperatures, which means that higher process temperatures during manufacture and higher operating temperatures of the X-ray rotating anode are possible. This applies for temperatures up to 1,250 ° C for MHC and for temperatures up to 1,100 ° C for TZM. MHC is therefore particularly suitable for the high power range and high operating temperatures in particular.

[0021] MHC is a Mo-based alloy provided by the applicant, Plansee SA, having the following composition: - Hf content of 1.00 to 1.30% by weight (wt%: weight percent), - C content of 500 to 1,200 μg / g (μg: microgram), the balance being Mo (typically a Mo content of at least 97.0% by weight, preferably at least 98.0% by weight, which may correspondingly be at least 98.5% by weight in the case of low proportions of impurities).

[0022] TZM is a Mo-based alloy specified in the ASTM B387 (364) standard and provided by the applicant, Plansee SA, and has the following composition for use herein: - a Ti content of 0.40-0.55% by weight, - Zr content of 0.06-0.12% by weight, - C content of 50-500 μg / g (this range, which is particularly well suited to the application area of ​​X-ray rotating anodes, is somewhat wider than the range of 100-400 μg / g specified in the ASTM B387(364) standard), The balance is Mo (typically a Mo content of at least 98.0% by weight, preferably at least 99.0% by weight, and correspondingly may even be at least 99.3% by weight if the proportion of impurities is low).

[0023] Possible or permissible contents of impurities that may be present are typically not specified for all elements, but in particular for those that are typically present and / or whose too high contents would be important for the advantageous properties of the alloy. Against this background, the following permissible ranges of impurities are particularly advantageous: in particular the total content of metallic impurities in MHC and TZM is less than or equal to 5,000 μg / g. In particular, the Al (aluminum) and Ni (nickel) contents of MHC and TZM are, according to particularly advantageous specifications of Plansee SA, less than or equal to 10 μg / g, the Cr (chromium), Cu (copper), Fe (iron), K (potassium) and Si (silicon) contents are each less than or equal to 20 μg / g, the W (tungsten) content is less than or equal to 300 μg / g, the Cd (cadmium) and Pb (lead) contents are each less than or equal to 5 μg / g, and the Hg (mercury) content is less than or equal to 1 μg / g. The total content of impurities from H (hydrogen), N (nitrogen) and O (oxygen) present in MHC is less than or equal to 1,000 μg / g. In particular, according to Plansee SA's specifications, the H and N contents of MHC are less than or equal to 10 μg / g and the O content is less than or equal to 600 μg / g. The total content of any impurities from H, N, O and C (carbon) that may be present in TZM is less than or equal to 1,500 μg / g. In particular, according to Plansee SA's specifications, the H and N contents of TZM are less than or equal to 10 μg / g each and the O content is less than or equal to 500 μg / g. Depending on the manufacturing process, contamination with Cr(VI) and organic contamination is possible, each of which is permissible up to a maximum of 1,000 μg / g, but is usually not detectable in the alloys offered by Plansee SA. The sum S of all impurities is advantageously in the range 0≦S≦6,000 μg / g for both MHC and TZM, with W (tungsten) as a typical impurity preferably having a proportion of 300 μg / g or less.

[0024] In principle, the anode disk and the bearing bush can be made of different materials. According to one development, the anode disk and the bearing bush are both made of molybdenum or of the same molybdenum-based alloy. This is particularly advantageous for connections with material bonding (especially in the case of friction-welded or beam-welded connections), since the material properties of both parts (e.g. both made of MHC or both made of TZM) are the same. If there are slight differences in composition, as is clear to the expert, the term "same" molybdenum-based alloy is still used. If both compositions are within the specifications of the Mo-based alloy in question (e.g. in the case of TZM or MHC as indicated above), then in particular only "slight differences" are given. Even if there is no specification for the alloy, there will usually only be a "minor difference" if the difference in Mo content is ≦2% by weight, the non-metallic alloying elements (e.g. C, N) total ≦0.2% by weight, the total of the metallic alloying elements total ≦1% by weight, and W total ≦0.05% by weight (with respect to impurities, the ranges given above apply in particular to TZM and MHC).

[0025] According to one development, the connection by material bonding is a friction welded connection. This is advantageous with regard to achieving high strength and heat resistance of the connection. Furthermore, the friction welding technique is highly reproducible and has a high degree of automation. It is preferable that no additional material (such as, for example, welding additional material, inserts inserted between the parts to be connected, etc.) is used during friction welding, i.e. no foreign bodies or different compositions different from the base material of the connected parts are detected, especially in the area of ​​the connection by material bonding. For friction welding, Mo-based alloys are preferred over pure Mo. It is even more preferable that the two components (anode disk, bearing bush) are made from the same Mo-based alloy (for example both from MHC, both from TZM, etc.), since this allows a particularly high stability and quality of the friction welded connection to be achieved. A particular advantage of friction welding (for example compared to beam welding processes) is that no melt is formed in the connection zone and the base material of the parts to be connected is only plasticized. As a result, a favorable structure is established in the region of the connection zone, preserving a homogeneous distribution of the contained elements / compounds (eg Mo-based alloys).

[0026] According to one development, the anode disk has a connecting piece on the bearing bush side, the inner wall of which extends through the hole in the anode disk and projects from the surface surrounding the outside of the anode disk. At least one axial section of the inner wall of the connecting piece is configured as a running surface of the liquid metal bearing in the circumferential direction and forms part of a second subsection of the liquid metal bearing shell (along with the inner wall of the hole in the anode disk and possibly other sections). Furthermore, a materially bonded connection is formed between the protruding connecting piece of the anode disk and the bearing bush. By means of the protruding connecting piece, which can have in particular a tubular or hollow-cylindrical basic shape, the materially bonded connection between the anode disk and the bearing bush can be produced more easily. This is particularly true in the case of friction-welded connections (but also in the case of beam-welded connections), since this essentially provides two similarly designed sections (in particular the circumferential wall and the annular end face) that are connected to one another. Furthermore, the materially bonded connection is thus arranged at a distance of, for example, 2-50 mm, preferably 5-30 mm, from the outer surrounding surface of the anode disc (ranges apply to the finished material connection). This provides sufficient space for the formation of a weld bead, which is formed by the material flow during the compression stage, particularly in the case of friction welded connections (the weld bead is subsequently removed by reworking). The original axial length of the connection piece (before the materially bonded connection is made) should be chosen, for example, 3-8 mm longer than the desired position after the materially bonded connection, due to the compression that occurs during friction welding, particularly when using friction welding processes. The connection piece is preferably formed monolithically with the anode disc, which is advantageous in terms of stability and running properties. The connection piece is preferably formed monolithically from the material of the anode disc as part of the forging process. Alternatively, the connection piece can also be connected to the anode disc by material bonding.

[0027] According to one development, the hole in the anode disk is designed as a through hole, and the anode disk has an extension piece on the side facing away from the bearing bush, which extends the through hole in the anode disk with its inner wall and projects forward from the outer surrounding surface of the anode disk. At least one axial section of the inner wall of the extension piece is formed in the circumferential direction as a running surface for the liquid metal bearing and forms part of a second subsection of the shell of the liquid metal bearing (adjacent to the inner wall of the hole in the anode disk, possibly the connecting piece and possibly the other section). The provision of such an extension piece is advantageous in terms of the stability and running properties of the shell of the liquid metal bearing (in particular because the extension of the running surface of the liquid metal bearing is provided on both sides of the anode disk). Accordingly, as in the connecting piece, the extension piece can also be preferably formed monolithically with the anode disk (for example formed by forging) or alternatively can be connected to the anode disk by a connection by material bonding. Preferably, the extension piece and possibly other components then form a closure for the shell of the liquid metal bearing, or, depending on the design of the liquid metal bearing, the extension piece can once again be connected to the bearing bush by a material connection, thereby further extending the shell of the liquid metal bearing, whereby the variants described for the connection of the connecting piece to the bearing bush are also possible.

[0028] According to one development, the thickness of the anode disk (measured in the axial direction) increases in the radial direction towards the rotation axis. This increase in thickness can occur continuously (with a constant gradient or with a changing thickness profile) or in one or more steps. In this way, heat generated in the region of the focal track is distributed over an increasingly larger material cross-sectional area towards the rotation axis and can then be effectively dissipated over a large area of ​​the liquid metal bearing outer shell (through the liquid metal arranged in the bearing gap, then through the liquid metal inner shell and its adjacent parts, such as, for example, pins with coolant cooling). Due to this material cross-sectional area increasing radially inwards, temperature peaks and excessively high temperatures occurring locally in the region of the liquid metal bearing, which could damage the liquid metal bearing and lead to stresses in the anode disk, are avoided. According to one development, the thickness increase from the reference thickness measured at the radial center in the region of the inclined focal track surface to the thickness in the region of the bore is 30-300%, in particular 50-260%, more preferably 70-230% (a thickness increase of 100% corresponds to a doubling of the thickness). This is particularly advantageous with regard to the heat dissipation of the liquid metal bearing and the stability and running properties of the shell. The term "thickness in the region of the bore" refers to the thickness of the anode disk just in the region of the inner wall of the bore, the thickness measurement also including sections that are possibly monolithically formed together with the anode disk, such as for example monolithically formed connecting pieces and / or monolithically formed extension pieces, but not only parts that are connected to the anode disk by a material bond (for example bearing bushes). However, the thickness of the anode disk also preferably increases radially inwards, without including possibly monolithically formed connecting pieces and / or extension pieces. In particular, the latter thickness increase is between 20 and 150%, preferably between 30 and 100%, and in case of providing a monolithic connecting piece and / or an extension piece, instead of the "area of ​​the hole" a reference area is used which is located directly (radially) outside this connecting piece and / or extension piece.

[0029] According to one development, the anode disk has a number of slits that are uniformly arranged in the circumferential direction and that penetrate the thickness of the anode disk, each of which extends over one radial section in the region between the outer periphery of the anode disk and the hole in the anode disk. Such slits allow the material of the anode disk to be stretched at the high temperatures that occur during use without the anode disk being plastically deformed, so that stresses in the material and thus material fatigue or material destruction are avoided. Such slits can extend exactly in the radial direction. Alternatively, the slits can also run slightly obliquely to the radial direction (for example at an angle of more than 0° and up to 5°). The path of the radial direction, the path of the axial direction (here they can also be inclined only by a small angle to the axial direction, for example in the range of 1° to 10°) and / or the width of the slits can vary according to a given contour. Furthermore, at least one end of the slits (preferably the radially inner end) can be provided with end holes and / or circumferential passages, each of which preferably extends through the thickness of the anode disk and has a diameter greater than the width of the opening slit. Preferably, the slits extend completely to the outer periphery, i.e. they open out to the outer periphery but end radially outside the holes in the anode disk. Preferably, all the slits are formed symmetrically with respect to one another with respect to the axis of rotation. The provision of such slits is particularly advantageous if the thickness of the anode disk increases towards the axis of rotation.

[0030] The present invention also relates to an X-ray rotating anode system comprising an X-ray rotating anode according to the present invention having an integrated liquid metal bearing outer shell, which may possibly also be configured according to one or more of the above-mentioned developments, and an inner liquid metal bearing shell integrated into said outer liquid metal bearing shell and having a liquid metal bearing running surface, wherein the outer liquid metal bearing shell and the inner liquid metal bearing shell are adjusted to one another in such a way that a defined bearing gap (in particular the gap width defined above) is formed between them.

[0031] According to one development, at least one circumferential mechanical limiting element is provided in the region of at least one axial end (axial: relative to the axis of rotation) of the liquid metal bearing running surface on the outer liquid metal bearing shell and / or of the liquid metal bearing running surface on the inner liquid metal bearing shell, which mechanical limiting element limits the axial flow of liquid metal in the bearing gap during use. The mechanical limiting element thus serves to keep the liquid metal in the (axial) inner region of the liquid metal bearing, where the liquid metal is required to achieve the gliding effect. The mechanical limiting element can in particular be formed by one or more of the following variants: - a series of bearing gaps formed in several stages to form a labyrinth seal (see, for example, US Pat. No. 5,399,313); - one or more circumferential ribs (continuous or interrupted over short circumferential sections) on one (e.g. stationary, inner) part of the liquid metal bearing and corresponding grooves on the other (e.g. rotating, outer) part, which at the same time provide an axial fixation of the liquid metal bearing. In the case of several ribs, these can also be provided alternately on one part and on the other; - A sealing ring made of a material (e.g. an alloy containing iron, nickel and cobalt) which interacts with the liquid metal present in the bearing gap (e.g. US Pat. No. 5,399,323).

[0032] According to one development, a circumferential coating is provided in the region of at least one axial end of the liquid metal bearing running surface on the outer liquid metal bearing shell and / or the liquid metal bearing running surface on the inner liquid metal bearing shell, which coating prevents wetting by the liquid metal located in the bearing gap during use. As a result, the liquid metal is retained in the (axial) inner region of the liquid metal bearing, where it is required to achieve a gliding effect. Suitable coatings are, inter alia, titanium oxide, aluminum oxide, titanium nitride and mixtures thereof, in particular CrN (chromium nitride), Cr2N (dichromium nitride), Cr2O3 (chromium(III) oxide), TiAlN (titanium aluminum nitride) (see, for example, US Pat. No. 5,399,313). The coating can be provided both on the inner shell of the liquid metal bearing and on the outer shell of the liquid metal bearing. However, if necessary, it can also be provided only on one (for example only on the inner shell of the liquid metal bearing). Furthermore, it can also be provided in the region of at least one mechanical limiting element.

[0033] According to one development, the inner shell of the liquid metal bearing is formed on a pin, which is led through the bearing bush at least into a hole in the anode disk. The pin preferably has at least one coolant channel for guiding the coolant. If the hole is formed as a through hole, the pin preferably extends completely through this through hole as well. The pin is preferably formed from one piece (integrally), since this is advantageous with regard to its stability and the robustness of the coolant channel. Alternatively, it can also be formed from several components which are connected to one another by a geometric and / or material bond, which can be advantageous in particular in the case of complex structures of the liquid metal bearing. The at least one coolant channel, which preferably extends over at least 80% of the length of the pin, can effectively dissipate heat during use.

[0034] According to one development, the liquid metal bearing running surface on the outer liquid metal bearing shell and / or the liquid metal bearing running surface on the inner liquid metal bearing shell have at least two surface-structured circumferential running sections, which are spaced apart from one another in the axial direction. At least one non-surface-structured section is preferably provided between the at least two surface-structured running sections. When the rotating part rotates in use, the liquid metal collects and builds up an increased pressure in the region of the surface-structured running sections. This results in a particularly good gliding effect. At the same time, the rotating part and the stationary part are fixed relative to one another in the radial direction. The provision of at least two such running sections also makes it possible to prevent tilting and vibrations of the X-ray rotating anode in use. It is particularly advantageous if the surface-structured running section is formed in a region that is arranged completely within the anode disk or at least overlaps this region. The surface structuring can be formed, for example, as a groove pattern (for example with one or more partial regions, each with parallel grooves). The surface-structured running sections can in principle be provided both on the inner and on the outer shell of the liquid metal bearing. In principle, the surface-structured running sections can also be formed opposite each other (relative to the bearing gap), however, it is preferred that in the region of a surface-structured running section on one component (e.g. on a liquid metal bearing inner shell) the other component in the opposite region does not have a surface-patterned running section.

[0035] The invention also relates to a method for manufacturing an X-ray rotating anode according to the invention, which may also be designed according to one or more of the developments and variants described above, wherein the method comprises the following steps: Providing an anode disk made of Mo or a Mo-based alloy; Preparing a cut piece made of Mo or a Mo-based alloy; - connecting the cut piece to the anode disc by material bonding so that the cut piece is centrally located with respect to the axis of rotation of the anode disc; A step of mechanically machining the anode disk and the cut piece to form an X-ray rotating anode having an integrated liquid metal bearing shell, the cut piece forming a bearing bushing having a liquid metal bearing running surface, the anode disk having a hole, and at least a portion of the axial direction of the inner wall being formed as the liquid metal running surface in the circumferential direction.

[0036] This method provides a cost-effective and process-reliable manufacturing means for producing the rotating X-ray anode of the invention.Furthermore, the above-mentioned developments and embodiments are also possible in the method according to the invention by providing appropriate method steps, and the above-mentioned advantages are achieved.

[0037] The anode disks and / or the cut pieces are preferably provided as part of a powder metallurgical production. This includes, in particular, pressing and sintering, preferably also shaping (e.g. rolling, forging, round rolling, round forging, etc.) of the corresponding starting powders. The holes in the anode disks and / or the through-holes in the bearing bushes can already be preformed before the connection by material bonding, so that the mechanical post-processing is less complicated. Alternatively, they can also be solved as part of the mechanical processing (i.e. the anode disks and / or the cut pieces do not yet have holes or through-holes before the connection by material bonding). The connection by material bonding is preferably performed by friction welding. The focal track coating can already be applied to the anode disks before the connection by material bonding (e.g. as part of a powder metallurgical production in composite materials), but can also be applied afterwards, for example by thermal spraying (e.g. vacuum plasma spraying), chemical vapor deposition (CVD) or physical vapor deposition (PVD). Other fittings, coatings, linings, etc., as mentioned at the beginning, can also be added during the production.

[0038] Other advantages and benefits of the present invention will become apparent from the following detailed description of the preferred embodiments with reference to the accompanying drawings. [Brief description of the drawings]

[0039] [Figure 1]FIG. 1 is a cross-sectional perspective view of a rotating X-ray anode according to a first embodiment of the present invention. [Figure 2A] FIG. 2A is a cross-sectional view of the X-ray rotating anode from FIG. 1 to illustrate fabrication. [Figure 2B] FIG. 2B is a cross-sectional view of the X-ray rotating anode from FIG. 1 to illustrate fabrication. [Diagram 3] FIG. 3 is a cross-sectional view of a rotating X-ray anode according to the present invention in accordance with a second embodiment. [Figure 4] FIG. 4 is a cross-sectional view of a rotating X-ray anode according to the present invention in accordance with the third embodiment. [Diagram 5] FIG. 5 is a cross-sectional view of a rotating X-ray anode according to the present invention in accordance with the fourth embodiment. [Figure 6] FIG. 6 is a cross-sectional view of a rotating X-ray anode according to the present invention in accordance with the fifth embodiment. [Figure 7] FIG. 7 is a cross-sectional view of a rotating X-ray anode according to the present invention in accordance with the sixth embodiment. [Figure 8] FIG. 8 is a cross-sectional view of a rotating X-ray anode according to the seventh embodiment of the present invention. [Figure 9] FIG. 9 is a cross-sectional view of an X-ray rotating anode system according to the present invention with a pin inserted, and two variants of the pin A and B are shown above the cross-sectional view, one in plan view and one in cross-section. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0040] 1 to 9 are schematic views which are not drawn to scale and do not show the details of the liquid metal bearing shell or the axial end termination of the liquid metal bearing. As is known in the art, various configurations of the axial end termination of the liquid metal bearing are possible, examples of which are shown, inter alia, in US Pat. No. 5,399,633, US Pat. No. 5,493,366, US Pat. No. 5,493,621 and US Pat. No. 5,529,111. In the views of Figs. 1 to 9, the bearing bush, the anode disk and the pin can extend further in the axial direction and / or be connected to other components, possibly with a different course or configuration.

[0041] In the following, a first embodiment of an X-ray rotating anode 2 according to the invention will be described with the aid of FIGS. 1, 2A and 2B. In its basic form, this first embodiment has an anode disk 5 made of MHC, which is rotationally symmetrically formed with respect to the axis of rotation 4 (axial direction). On one side of the anode disk 5 there is a circumferential focal track 6 with a focal track coating made of a W-Re alloy (W: 95% by weight; Re: 5% by weight). In the region of the focal track 6, the anode disk 5 has a circumferential focal track surface 10 inclined at an angle (angle α) with respect to a reference plane 8 extending perpendicularly to the axis of rotation 4. A hole 12 extends through the anode disk 5, the inner wall 14 of which is formed as a running surface for a liquid metal bearing. On the opposite side to the focal track 6, the anode disk has a tubular connecting piece 16 which is monolithically formed and forged from the material of the anode disk 5, which protrudes with respect to the surface of the anode disk 5 surrounding the outside. Its inner wall 18 extends the bore 12 of the anode disk 5 and is also designed as a liquid metal bearing running surface. A tubular bearing bush 20, also made of MHC, is connected with its axial (annular) end face to the correspondingly formed axial (annular) end face of the connecting piece 16 via a materially bonded connection 21. An inner wall 22 of the bearing bush 20 is designed as a liquid metal bearing running surface in the circumferential direction. The liquid metal bearing running surfaces of the anode disk 5, the connecting piece 16 and the bearing bush 20 together form a continuous liquid metal bearing running surface, which here extends linearly in the form of a cylindrical outer peripheral surface and forms part of the liquid metal bearing shell. The bearing bush 20 and the anode disk 5 are still shown as separate components in FIG. 2A and after the final materially bonded connection 21 has been produced by friction welding (and mechanical post-processing). As explained, axial friction welding leads to a shortening of the connecting piece 16 and the bearing bush 20 in the region of the connection zone.

[0042] In the following description of other embodiments, the same reference symbols are used to indicate that the same or nearly identical components are involved, and differences relative to the first embodiment will be primarily discussed.

[0043] In the second embodiment shown in FIG. 3, the thickness (measured axially) of the anode disc 5′ increases continuously radially inwards. In particular, the thickness increases from a reference thickness d R Starting from the radial center (measured in the area of ​​the inclined focal track surface 10), the maximum thickness d II (including all components monolithically connected to the anode disk 5', i.e., in this case including the connection piece 16) increases by 30 to 300%. Furthermore, the reference thickness d R Starting from the thickness increases by 20-150% radially inwards without including the monolithic connecting piece 16, and then the associated thickness d I is measured directly on the (radial) outside of the connecting piece 16.

[0044] In the third embodiment shown in Fig. 4, in comparison with the first embodiment, the anode disc 5 has an extension piece 24 on the side facing away from the bearing bush 20, the inner wall 26 of which extends the (through) hole 12 of the anode disc 5 and projects forward from the outer face of the anode disc 5. The inner wall 26 of the extension piece 24 is also formed on the periphery as a liquid metal bearing running surface and therefore forms part of the outer shell of the liquid metal bearing. Furthermore, Fig. 4 shows that the nominal thickness d R Starting from the maximum thickness d II (including all components monolithically connected to the anode disc 5, i.e. in this case including the connection piece 16 and the extension piece 24). In the fourth embodiment shown in FIG. 5, the anode disc 5″ does not have a connection piece as compared to the first embodiment, rather the bearing bush 20 is directly connected to the plane of the anode disc 5″ via a diffusion bond.

[0045] In the embodiments shown in Figures 6 to 9, the bearing bush 20 is arranged on the same side as the focal track 6. Compared to the first embodiment, in the fifth embodiment shown in Figure 6, the connection piece 16' on the anode disc 5''' is also arranged on the side of the focal track 6. In the sixth embodiment shown in Figure 7, the anode disc 5'' does not have a connection piece, as in the fourth embodiment (Figure 5). Rather, the bearing bush 20 is directly connected to a flat surface of the anode disc 5'' via diffusion bonding, and the seventh embodiment shown in Figure 8 differs from the sixth embodiment in that the thickness of the anode disc 5'''' increases continuously radially inwards.

[0046] FIG. 9 shows an X-ray rotating anode system 27, in which the X-ray rotating anode 2 with the anode disk 5"', the connecting piece 16' and the bearing bush 20 is constructed according to the fifth embodiment (see FIG. 6). Furthermore, an internally inserted pin 28 is shown, on which an inner liquid metal bearing shell is formed. Between the inner and outer liquid metal bearing shells of the pin 28 a bearing gap 30 is formed, which is filled with liquid metal (not shown) during use. Two variants for the design of the pin 28 are shown above the rotating X-ray anode. According to a first variant A (shown above in FIG. 9, on the left in plan view and on the right in cross section through the interior of the X-ray rotating anode 2), the pin 28 is a tubular It has a basic shape and has a smooth surface on the outside. According to a second variant B (shown above in FIG. 9 as the third view, in plan view on the left and in section on the right), the pin 28' has two surface-structured running sections 32, 34 spaced apart from each other in the axial direction. Furthermore, the pin 28' has a coolant channel 36 running on the inside, which has a coolant tube 40 inserted in a blind hole 38, the diameter of which is selected to be correspondingly smaller than the diameter of the blind hole 38, so that, for example, the coolant can be made to flow in through the coolant tube 40 and can flow back outwards via the annular channel formed between the coolant tube 40 and the blind hole 38.

[0047] Example of production: Example 1: A method for manufacturing an X-ray rotating anode according to the invention, in which the anode disc and the bearing bush are made of MHC and connected to each other by friction welding, is described below. First, the anode disc and the cut pieces having a cylindrical basic shape are manufactured by powder metallurgy. This includes the steps of providing a suitable starting powder (for the MHC), pressing and sintering, and then shaping (forging of the anode disc; radial forging of the cut pieces). The cut pieces are machined to have a tubular basic shape in order to form the later bearing bush. Furthermore, as part of the shaping (forging), a protruding tubular connecting piece (with an axial length of 40 mm) is forged in the center of one side of the anode disc, i.e. the connecting piece is monolithically formed from the material of the anode disc. The end faces of the tubular cut pieces and the end faces of the connecting pieces are both welded to a surface area of ​​2,000 mm. 2 , with an inner diameter of 44 mm (the outer diameter is determined by this). Here, a friction welding machine with direct spindle drive is used. The tubular cut pieces are clamped in the (non-rotating) fixture of the friction welding machine, and the anode disk is clamped in the (rotating) spindle fixture. The anode disk is then rotated (2,000 revolutions per minute) and pressed against the cut pieces with a friction pressure of 30 bar. The anode disk drive is then stopped and the pressing pressure is increased to 65 bar. The total friction time during which the relative rotational movement between the anode disk and the cut pieces occurs is 3 seconds. Then still mechanical processing to generate the final geometric shape is performed, during which the tubular cut pieces form the bearing bushes. Other fittings, coatings, coverings, etc. can still be added, as described at the beginning. Depending on the part geometry and the process, a stress relief anneal (for example at a temperature in the range of 1,100 ° C to 1,300 ° C) can be inserted once or several times during the manufacturing process.

[0048] Example 2: A method for manufacturing an X-ray rotating anode according to the invention is described below, in which the anode disk and the bearing bush are made of TZM and are connected to each other by friction welding. The same steps and parameters as in example 1 apply, with the following difference: the starting powder for manufacturing the anode disk and the cutting pieces from TZM (and not from MHC) is prepared. The applied friction pressure is only 25 bar, the pressing force increases to only 60 bar after the end of the drive of the anode disk.

[0049] Example 3: A method for manufacturing an X-ray rotating anode according to the invention, in which the anode disk and the bearing bush are made of TZM and are connected to each other via diffusion bonding, is described below. First, the anode disk and the tubular cut piece are manufactured from TZM as in example 2. Both the (joined) end faces of the tubular cut piece and the (joined) end faces of the connecting piece are machined and then ground and / or polished to provide smooth flat surfaces. Then, diffusion bonding of the contacting end faces of the two components is performed at a temperature of 1,700°C, a pressure of 10 MPa and a duration of at least 5 minutes (preferably in the range of 6-15 minutes).

[0050] The invention is not limited to the embodiment shown in the figures. In particular, the liquid metal bearing running surface of the outer liquid metal bearing shell does not necessarily have a straight contour in the form of a cylindrical flank, but can also have a stepped contour, circumferential ribs, etc., as explained at the beginning. In this case, the liquid metal bearing typically has an inner shell with a correspondingly adapted contour. [Explanation of symbols]

[0051] 2. Rotating X-ray anode 4 Rotation axis 5 Anode disc 6 focal trajectory 8 Reference plane 10 Focal orbital plane 12 Anode disc hole 14 Inner wall of hole in anode disk 16 Connection piece 18 Inner wall of connecting piece 20 Bearing bush 21 Materially bonded connections 22 Inner wall of bearing bush 24 Extension piece 26 Inner wall of extension piece 27 X-ray rotating anode system 28-pin 30 Bearing gap 32 Running Section 34 Running Section 36 Coolant flow path 38 Non-through hole 40 Coolant tube

Claims

1. a liquid metal bearing shell having an anode disc (5; 5'; 5"') made of Mo or a Mo-based alloy and a bearing bush (20) made of Mo or a Mo-based alloy, said anode disc (5; 5'; 5"') has a hole (12) formed centrally in the region of the axis of rotation (4) and which hole extends axially through at least a portion of said anode disc (5; 5'; 5"'); an inner wall (22) of the bearing bush (20) is formed as a liquid metal bearing running surface in the circumferential direction at least over its axial section and forms a first subsection of the liquid metal bearing shell, the liquid metal bearing shell being formed by the first subsection and a second subsection adjacent the first subsection and having a continuous liquid metal bearing running surface, the anode disk (5; 5'; 5"') has a connecting piece (16; 16') on the side of the bearing bush (20), the inner wall (18) of which extends the hole (12) in the anode disk (5; 5'; 5"') and projects outwardly from the outer surrounding surface of the anode disk (5; 5'; 5"'); at least an axial section of the inner wall (18) of the connecting piece (16; 16') is formed as a liquid metal bearing running surface in the circumferential direction and forms part of a second subsection of the liquid metal bearing shell; and a materially bonded connection (21) is formed between the protruding connecting piece (16; 16') of the anode disk (5; 5'; 5"') and the bearing bush (20), the materially bonded connection (21) being a friction welded connection or a beam welded connection. A rotating X-ray anode comprising:

2. The Mo-based alloy is MHC and / or TZM, MHC has the following composition: - a Hf content of 1.00 to 1.30% by weight, - a C content of 500 to 1,200 μg / g, - Remainder Mo The content of any metal impurities that may be present is 5,000 μg / g or less, and the total content of any impurities from H, N and O that may be present is 1,000 μg / g or less, and TZM has the following composition: - a Ti content between 0.40 and 0.55% by weight, - a Zr content of 0.06 to 0.12% by weight, - C content of 50-500 μg / g - Remainder Mo The content of any metal impurities that may be present is 5,000 μg / g or less, and the total content of any impurities from H, C, N and O that may be present is 1,500 μg / g or less.

2. The X-ray rotating anode according to claim 1 .

3. 3. An X-ray rotating anode according to claim 1 or 2, characterized in that the anode disk (5; 5'; 5''') and the bearing bush (20) are both made from molybdenum or both made from a molybdenum-based alloy.

4. 4. The X-ray rotating anode according to claim 1, wherein the connection (21) by material bonding is a friction welded connection.

5. 5. The X-ray rotating anode according to claim 1, characterized in that the hole (12) of the anode disk (5) is formed as a through hole, the anode disk (5) has an extension piece (24) on its side opposite the bearing bush (20), the extension piece (24) extending the through hole (12) of the anode disk (5) by its inner wall (26) and protruding outward from the outer surrounding surface of the anode disk (5), and at least an axial section of the inner wall (26) of the extension piece (24) is formed as a liquid metal bearing running surface in the circumferential direction and forms part of the second subsection of the liquid metal bearing shell.

6. The thickness of the anode disk (5') increases radially towards the axis of rotation (4), where a reference thickness (d R ) starting from the thickness (d II 6. The X-ray rotating anode according to claim 1, wherein the increase in thickness from the first to the second electrode is 30 to 300%.

7. 7. The X-ray rotating anode according to claim 1, characterized in that the anode disk (5;5';5"') has a plurality of through slits uniformly distributed in the circumferential direction and passing through the thickness of the anode disk (5;5';5"'), each of which extends over a radial section in the area between the outer periphery of the anode disk (5;5';5"') and a hole (12) in the anode disk (5;5';5"').

8. 8. An X-ray rotating anode system comprising an X-ray rotating anode having an integrated liquid metal bearing outer shell according to any one of claims 1 to 7, and a liquid metal bearing inner shell inserted into said liquid metal bearing outer shell and having a liquid metal bearing running surface, wherein said liquid metal bearing outer shell and said liquid metal bearing inner shell are adjusted to each other such that a defined bearing gap (30) is formed between them.

9. 9. An X-ray rotating anode system as claimed in claim 8, characterized in that at least one circumferential mechanical limiting element is provided in the region of at least one axial end section of the liquid metal bearing running surface on the outer liquid metal bearing shell and / or the liquid metal bearing running surface on the inner liquid metal bearing shell, which limit the axial flow of liquid metal in the bearing gap (30) in use.

10. 10. An X-ray rotating anode system as claimed in claim 8 or 9, characterized in that the liquid metal bearing running surface on the outer liquid metal bearing shell and / or the liquid metal bearing running surface on the inner liquid metal bearing shell are provided with a circumferential coating in the region of at least one axial end section, which prevents wetting by liquid metal present in the bearing gap (30) during use.

11. 11. An X-ray rotating anode system according to claim 8, characterized in that the liquid metal bearing inner shell is formed on a pin (28') which passes through the bearing bush (20) and is guided at least as far as the hole (12) of the anode disk (5"').

12. 12. An X-ray rotating anode system according to claim 8, characterized in that the liquid metal bearing running surface on the outer liquid metal bearing shell and / or the liquid metal bearing running surface on the inner liquid metal bearing shell has at least two circumferential surface structured running sections (32, 34) spaced apart from each other in the axial direction.

13. A method for manufacturing an X-ray rotating anode according to any one of claims 1 to 9, characterized by the steps of: - providing an anode disk (5; 5'; 5"') with a connecting piece (16; 16') made of Mo or a Mo-based alloy, - preparing a cutting piece from Mo or a Mo-based alloy, - connecting said cut piece to said connection piece (16; 16') of said anode disc (5; 5'; 5"') by material bonding, in such a way that said cut piece is centrally located with respect to the axis of rotation (4) of said anode disc (5; 5'; 5"'; 5""); and - mechanically machining the anode disk (5; 5'; 5"') with the connecting piece (16; 16') and the cut piece to form the X-ray rotating anode (2) with an integrated liquid metal bearing shell, in which the cut piece forms a bearing bush (20) with the liquid metal bearing running surface, the anode disk (5; 5'; 5"') having the hole (12) in which at least an axial section of the inner wall (14) is formed in the circumferential direction as a liquid metal bearing running surface.

Citation Information

Patent Citations

  • Rotary anode target for X-ray tube, preparation method and target assembly

    CN110556278A

  • Liquid metal sliding bearing

    DE102015204488A1

  • liquid metal plain bearing

    DE102015215306A1

  • Composite member manufacturing method

    JP2007512959A

  • Rotating anode x-ray tube and rotating anode x-ray tube assembly

    JP2011060517A