Sealing material
A sealing member with a rubber base and surface treatment layer containing amines addresses the cost and efficacy issues of conventional corrosion prevention methods by effectively preventing corrosion and rust on aluminum housings through surface adhesion.
Patent Information
- Application Number
- JP2020086930
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-18
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2040-05-18
AI Technical Summary
Conventional corrosion prevention methods for aluminum housings, such as surface treatments, are costly and ineffective in preventing crevice corrosion and rust when exposed to salt water, especially in vehicles.
A sealing member with a rubber base material and a surface treatment layer containing a corrosion inhibitor, preferably amines, is applied to prevent corrosion and rust by adsorbing into minute gaps on the sealed surface.
The sealing member effectively prevents corrosion and rust on aluminum housings at a lower cost by ensuring the corrosion inhibitor adheres to and remains on the sealed surface, maintaining sealing performance even in saltwater environments.
Smart Images

Figure 0007580205000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a seal member. [Background technology]
[0002] In vehicles and general-purpose machines, such as automobiles, seal members are used to seal housings in engines, devices that house electronic components, etc. Such seal members are, for example, sandwiched in a compressed state between a pair of members that constitute the housing, and are elastically deformed to seal between the pair of members, thereby sealing the housing.
[0003] Automobiles may travel along coastal areas or in areas where snow-melting agents are sprayed. When this happens, if salt water or snow-melting agents adhere to the automobile's parts and there is a gap between the member that presses the seal member and the seal member, the salt water or snow-melting agent components may penetrate into the gap, causing corrosion (crevice corrosion) or rust in the member that presses the seal member. If this corroded portion penetrates beyond the seal line of the seal member and into the inside of the housing, it will lead to corrosion of the material that constitutes the housing.
[0004] In recent years, the automotive industry has been actively working to reduce weight in order to improve fuel efficiency, and aluminum, which is lighter than iron-based materials, is increasingly being used. Although aluminum generally has better corrosion resistance than iron, it tends to be susceptible to the above-mentioned crevice corrosion.
[0005] Conventionally, various methods of treating the surface of aluminum have been studied to prevent the corrosion of aluminum. Three methods are generally used for surface treatment of metal materials such as aluminum: anodizing (anodic oxidation), plating, and corrosion prevention coating.
[0006] For example, Patent Documents 1 and 2 disclose anodizing treatment. Specifically, Patent Document 1 discloses an anodized aluminum member in which an anodized coating and cobalt and / or chromium are present on the surface of an aluminum base material or an aluminum alloy base material. Patent Document 2 discloses a fuel pump in which an anodized aluminum layer is formed on the entire surface of the pump body.
[0007] A plating process is disclosed in Patent Document 3. Specifically, Patent Document 3 discloses a highly corrosion-resistant Ni-based composite plating film in which a Cu-based plating film is formed on the surface of a metal part, and a Ni-based plating film is formed thereon.
[0008] Patent Documents 4 to 9 disclose anti-corrosion coatings. Specifically, Patent Document 4 discloses a composition for coating a metal surface that contains water, an ion source such as aluminum, a chromium (III) cation source, and the like, and is substantially free of hexavalent chromium. Patent Document 5 discloses an apparatus that is coated with a coating that contains a cured binder and hydrophilic flakes whose surfaces contain metal oxides. Patent Document 6 discloses a steel plate on which a coating film is formed by applying an ultraviolet curing resin composition. Patent Document 7 discloses a corrosion-resistant magnetic material having a coating layer on the surface of a magnetic substrate that comes into contact with seawater, the coating layer being composed of at least one material selected from nitride-based materials composed of CrN, TiN, AlN, BN, BCN, and AlBN, and carbon-based materials composed of diamond-like carbon (DLC) containing hydrogen and TiC. Patent Document 8 discloses an aluminum alloy material for heat exchangers, the surface of which is directly provided with a fluororesin paint coating having an isocyanate group or a siloxane group. Patent Document 9 discloses an anti-corrosion composition comprising a polyamideimide (PAI) heat-resistant polymer binder, a liquid solvent, and inorganic filler particles. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2015-232155 A [Patent Document 2] JP 2008-261282 A [Patent Document 3] Patent No. 5365928 [Patent Document 4] Special Publication No. 2016-513755 [Patent Document 5] Special Publication No. 2015-509140 [Patent Document 6] Patent No. 5483296 [Patent Document 7] JP 2010-177326 A [Patent Document 8] Patent No. 5189823 [Patent Document 9] Patent No. 5319282
[0010] In conventional corrosion prevention methods, corrosion is prevented by performing a surface treatment on the sealed member. However, in such a method of directly performing a surface treatment on the sealed member, if there is a defect in the surface treatment, the corrosion prevention effect of the sealed member may not be fully achieved. In particular, in the case of an aluminum housing in which aluminum, which is prone to crevice corrosion and rust, is used as the material of the sealed member in an environment in contact with salt water, the corrosion prevention effect and rust prevention effect may be significantly reduced. In addition, when performing a surface treatment on the entire surface of the aluminum housing, the manufacturing cost is high, while in the case of partial surface treatment, masking etc. are required, so the number of steps increases, and as a result, the manufacturing cost increases. Therefore, a technology that prevents corrosion and rust of the sealed member by an approach different from the conventional method is desired. Summary of the Invention [Problem to be solved by the invention]
[0011] The present invention provides a sealing member that can effectively prevent corrosion and rust on the surface of a sealed member simply and at low cost.
[0012] As a result of intensive research into solving the above problems, the inventors have discovered that corrosion of the sealed member can be prevented simply, at low cost, and effectively by imparting anti-rust and anti-corrosion functions to the sealing member that comes into contact with the sealed member, rather than performing a surface treatment on the sealed member itself. [Means for solving the problem]
[0013] The sealing member of the present invention comprises a rubber base material and a surface treatment layer coated on a surface of the rubber base material, the surface treatment layer contains at least one corrosion inhibitor, the corrosion inhibitor contains at least one amine, the content of the corrosion inhibitor in the surface treatment layer is 0.5 mass% or more and 8 mass% or less, and the thickness of the surface treatment layer is greater than the maximum height roughness Rz (μm) of the sealed surface measured in accordance with JIS B 0601:2001.
[0014] In the sealing member of the present invention, the content of the corrosion inhibitor is preferably from 1% by mass to 5% by mass.
[0015] In the sealing member of the present invention, the amine is preferably selected from secondary amines and tertiary amines.
[0016] The seal of the present invention is preferably a seal for an aluminum housing. Effect of the Invention
[0017] According to the present invention, it is possible to provide a sealing member that can effectively prevent corrosion and rust on the surface of a sealed member simply and at low cost. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the present invention will be described. The sealing member according to this embodiment includes a rubber base material and a surface treatment layer coated on the surface of the rubber base material. The surface treatment layer as a coating layer contains at least one corrosion inhibitor in a content of 0.5 mass% or more and 8 mass% or less in the surface treatment layer, and the corrosion inhibitor contains at least one amine. Furthermore, the thickness of the surface treatment layer is larger than the maximum height roughness Rz (μm) measured in accordance with JIS B 0601:2001 on the sealed surface. When the surface of a sealed member such as an aluminum housing (contact surface between the sealing member and the sealed member) is sealed by such a sealing member, the surface of the sealing member adheres well to the surface of the sealed member, and the corrosion inhibitor contained in the surface treatment layer enters into fine gaps on the surface of the sealed member by volatilization. The corrosion inhibitor used has a corrosion prevention function in addition to a rust prevention function, so that the volatilized corrosion inhibitor is adsorbed on the surface of the sealed member to prevent initial corrosion. In addition, in the long term, the rust prevention function of the corrosion inhibitor prevents rust on the surface of the sealed member. Furthermore, since the contact surface between the seal member and the sealed member is an enclosed space, it is possible to prevent gap corrosion and rust on the seal surface due to salt water for a long period of time even in an environment where the seal surface comes into contact with salt water, and the sealing performance is maintained. This makes it possible to provide a seal member that can effectively prevent corrosion and rust on the surface of the sealed member simply and at low cost.
[0019] The shape of the sealing member is not particularly limited and may be any shape depending on the application. Examples of the sealing member include sheet-shaped sealing members such as square, rectangular, and disk-shaped sealing members, and annular sealing members such as O-rings and square rings.
[0020] Each element constituting the seal member according to this embodiment will be described in detail below.
[0021] <Rubber base material> The material of the rubber substrate is not particularly limited, but a water-resistant elastomer is preferable. Examples of such elastomers include rubber materials selected from the group consisting of cured ethylene-propylene-diene terpolymer rubber (EPDM), hydrogenated nitrile rubber (HNBR), acrylic rubber (ACM) and fluororubber (FKM). These rubber materials may be used alone or in combination of two or more. In addition, the rubber substrate may contain additives as necessary.
[0022] In addition, the rubber base material preferably has excellent water resistance. From this viewpoint, the material of the rubber base material is more preferably at least one rubber material selected from EPDM, HNBR, ACM and FKM.
[0023] The rubber base material preferably has a predetermined hardness in order to prevent the rubber member from being deformed by an external load. The hardness of the rubber base material can be expressed as a type A durometer hardness in accordance with JIS K 6253-3:2012. The type A durometer hardness of the rubber base material is preferably 40 to 90, more preferably 50 to 80, and even more preferably 60 to 70. When the type A durometer hardness of the rubber base material is within these ranges, a seal member having excellent adhesion and sealing properties can be obtained.
[0024] <Surface treatment layer> A surface treatment layer containing a corrosion inhibitor is provided on the surface of the rubber substrate. Specifically, the surface treatment layer as a coating layer is formed by applying a coating material containing a corrosion inhibitor to the surface of the rubber substrate and drying the coating under conditions such that the corrosion inhibitor does not volatilize (e.g., natural drying). Since the surface of the rubber substrate is surface-treated with the corrosion inhibitor, the surface treatment layer is endowed with the function of the corrosion inhibitor.
[0025] The surface treatment layer contains at least one corrosion inhibitor. The corrosion inhibitor contains a volatile component and therefore has a vaporizing action. When the surface treatment layer containing such a corrosion inhibitor adheres to the surface of the sealed member, the volatilized corrosion inhibitor penetrates into minute gaps on the surface of the sealed member through the contact surface and is adsorbed. In addition, since the corrosion inhibitor has a rust prevention function and a corrosion prevention function, the adsorbed corrosion inhibitor prevents rust and corrosion that may occur on the surface of the sealed member. This makes it possible to prevent corrosion and rust on the surface of the sealed member simply and at low cost with an approach different from conventional corrosion prevention methods. The corrosion inhibitor may be used alone or in combination of two or more types.
[0026] The corrosion inhibitor contains at least one amine as an active ingredient. By using an amine as an active ingredient of the corrosion inhibitor, it is possible to effectively impart rust prevention and corrosion prevention functions to the sealed member. The amine used is not particularly limited, but is preferably selected from secondary amines and tertiary amines. These amines may be any of aliphatic amines, alicyclic amines, and aromatic amines. Examples of secondary amines include diethanolamine, diisopropylamine, and dicyclohexylamine. Examples of tertiary amines include, for example, triethanolamine, a reaction product of dicyclohexylamine with a higher fatty acid, and an oligomer. These amines may be substituted with an alkyl group, a hydroxyl group, an alkoxyalkyl group, or the like, or may be unsubstituted amines. Examples of higher fatty acids include, but are not particularly limited to, saturated or unsaturated higher fatty acids such as oxidized paraffin, lauric acid, and oleic acid. The higher fatty acids may be substituted with a hydroxyl group, an ester group, or the like, or may be unsubstituted higher fatty acids. The amines as corrosion inhibitors may be used alone or in combination of two or more types.
[0027] Examples of commercially available corrosion inhibitors containing such amines include "Killeslite (registered trademark) T", "Killeslite (registered trademark) W-1", and "Killeslite (registered trademark) WR-5" from Chelesto Corporation, "Sanhibitor No. 50" from Sanyo Chemical Industries, and "NA-SUL (registered trademark) TEA / LB" from KING INDUSTRIES.
[0028] The corrosion inhibitor may also contain other rust inhibitors than the amines, such as inorganic compounds such as chromates, nitrites, silicates, and polyphosphates, and organic compounds such as carboxylic acids, metal soaps, sulfonic acids, esters, and phosphates.
[0029] The content of the corrosion inhibitor contained in the surface treatment layer is 0.5% by mass or more and 8% by mass or less. By having the content of the corrosion inhibitor be 0.5% by mass or more and 8% by mass or less, the corrosion inhibitor can be added without other components such as binders agglomerating, and the corrosion inhibitor is gradually released after the surface treatment layer is formed, so that the desired function can be effectively imparted to the sealed member. In addition, the lower limit of the content of the corrosion inhibitor is preferably 1% by mass or more, and the upper limit is preferably 5% by mass or less.
[0030] The thickness of the surface treatment layer is controlled to be larger than the maximum height roughness Rz (μm) of the sealed surface measured in accordance with JIS B 0601:2001. In particular, when the seal member is used as a seal member for an aluminum housing described later, the thickness of the surface treatment layer is preferably larger than the maximum height roughness Rz (μm) of the sealed surface of the aluminum housing measured in accordance with JIS B 0601:2001. By making the thickness of the surface treatment layer larger than the maximum height roughness Rz of the sealed surface, it is possible to provide a seal member with good sealing properties, and as a result, rust and corrosion that may occur on the surface of the sealed member can be effectively prevented. The thickness of the surface treatment layer can be designed according to the maximum height roughness Rz of the sealed member, and is not particularly limited, but is preferably 6 μm or more, and more preferably 10 μm or more. In addition, the upper limit of the thickness of the surface treatment layer is preferably 30 μm or less.
[0031] The thickness of the surface treatment layer can be measured by the following method (a) or (b). It has been confirmed that the thickness of the surface treatment layer is the same regardless of whether the method (a) or (b) is used.
[0032] (a) A method in which a coating material for forming a surface treatment layer is applied to a film of known thickness, and then cured, the total thickness of the resulting sheet is measured with a micrometer, and the thickness of the surface treatment layer is calculated by subtracting the total thickness of the sheet from the thickness of the film. (b) A method in which a cross section of the obtained sealing member is photographed with a FE-SEM (field emission scanning electron microscope) and then the thickness of the surface treatment layer in the obtained photograph is measured.
[0033] The surface treatment layer further contains a binder. By containing the binder in the surface treatment layer, the corrosion inhibitor is uniformly dispersed in the coating material, and a surface treatment layer of uniform thickness can be formed. Examples of binders include aqueous emulsion of emulsion-polymerized polydimethylsiloxane containing hydroxyl groups at both ends, hydrazides, aqueous emulsion of urethane resin containing carbonyl groups, aqueous emulsion of silanol-modified polyurethane resin, and cured silicone rubber. When a binder is used to form the surface treatment layer, the content of the corrosion inhibitor contained in the surface treatment layer is calculated as the ratio of the corrosion inhibitor to the binder converted into solid content.
[0034] The surface treatment layer may contain other additives as necessary. Examples of such additives include thickeners, flow aids, defoamers, fillers, leveling agents, adhesion promoters, etc. These additives may be used alone or in any combination and ratio of two or more.
[0035] <Applications of sealing materials> The sealing member according to the present embodiment can provide the member to be sealed with rust prevention and corrosion prevention functions, and can therefore be used for various members including metal materials that are easily corroded in the sealed portion. In particular, from the viewpoint of the influence of salt water, the sealing member is suitable for use as a sealing member for aluminum housings, and examples of aluminum housings include aluminum housings for vehicles. Examples of products including aluminum housings for vehicles include fuel cells (FCs), forward discharge (FDC) converters, electric power steering (EPS) such as electric power steering for hybrid electric vehicles (HEVs), electronic control units (ECUs) such as electronic control units for hybrid electric vehicles, continuously variable transmissions (CVT) such as continuously variable transmissions for hybrid electric vehicles, electric water pumps (electric W / Ps), stroke sensors, thermo housings, V-pumps, brakes, and other automotive products. In addition to the above applications, the sealing member is also effective for use in general parts where corrosion by salt water or seawater is a concern.
[0036] <Aluminum housing> The seal member according to the present embodiment is elastically deformed by being sandwiched in a compressed state between a pair of components constituting the aluminum housing, thereby achieving a seal between the pair of components. In this way, the seal member can hermetically seal the aluminum housing.
[0037] When the seal member is used as a seal member for an aluminum housing, the thickness of the surface treatment layer is controlled to be greater than the maximum height roughness Rz of the sealed surface of the aluminum housing (the surface in contact with the seal member) as specified in JIS B 0601:2001. By making the thickness of the surface treatment layer greater than the maximum height roughness Rz of the sealed surface of the aluminum housing, the adhesion between the seal member and the sealed surface of the aluminum housing is improved, making it possible to provide a seal member for an aluminum housing with good sealing properties, and as a result, the corrosion inhibitor can also remain on the seal surface, making it possible to effectively prevent rust and corrosion that may occur on the surface of the aluminum housing that is the sealed member.
[0038] The material for the aluminum housing may be aluminum or an aluminum-based alloy. An aluminum-based alloy is an alloy whose main component (the component with the largest content among the constituent components) is aluminum, and examples of alloy components other than aluminum include copper (Cu), silicon (Si), zinc (Zn), iron (Fe), and magnesium (Mg).
[0039] In the aluminum housing, at least one of the members that press the seal member may be the above aluminum or aluminum-based alloy, and the other pressing members may be metal members other than aluminum-based members or resin members. The shape, size, and properties of the pressing surface of the seal member are not particularly limited, and can be appropriately selected depending on the location and purpose of the seal member. The type of aluminum housing is not particularly limited, but it is preferable to use an aluminum housing that is used in an environment where it comes into contact with salt water.
[0040] (Method of manufacturing the sealing member) The method for producing the sealing member of this embodiment is described below. First, a rubber base material is prepared. The rubber base material may be a rubber base material having a desired shape and made of already cured rubber, or may be a rubber material obtained by curing and molding.
[0041] Next, a surface treatment layer is formed on the rubber substrate. The method of forming the surface treatment layer is not particularly limited, but includes a method of applying a coating material (liquid material) containing a corrosion inhibitor onto the rubber substrate, and then drying the coating material for a predetermined time to harden the coating film. The method of applying the coating material is not particularly limited, and includes methods such as wire bar coater, film applicator, spray, air knife coating, die coating, and inkjet printing. From the viewpoint of obtaining a surface treatment layer with a uniform thickness, spray application is preferred.
[0042] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and includes all aspects encompassed by the concept of the present invention and the scope of the claims, and can be modified in various ways within the scope of the present invention. EXAMPLES
[0043] Examples of the present invention will be described below, but the present invention is not limited to these examples as long as they do not depart from the spirit of the present invention.
[0044] Example 1 As the rubber substrate, a cured ethylene-propylene-diene terpolymer rubber (EPDM) O-ring with a type A durometer hardness of 70 was prepared and degreased with methyl methyl ketone. Then, corrosion inhibitor A (a triethanolamine-containing composition) was added to the urethane binder (Daiichi Yakuhin Kogyo Co., Ltd.'s "Superflex 740") at a ratio of 1% by mass to the solid content to obtain a coating material (liquid material). The obtained coating material was stirred and passed through a 100M filter to check for residues. In addition, the coating material was sprayed onto the surface of the O-ring, and then naturally dried to harden the coating material, forming a surface treatment layer with a thickness of 12 μm on the surface of the O-ring.
[0045] The O-ring (sealing member) on which the surface treatment layer was formed was sandwiched between a pair of aluminum substrates (maximum height roughness Rz=6 μm; ADC12 (product name)) and compressed to a compression ratio of 17% using a resin jig. Next, the sealing member in close contact with the aluminum substrate was immersed in salt water with a salt concentration of 5% by mass at 50° C. for 2000 hours. Thereafter, the sealing member sandwiched between the aluminum substrates was taken out of the salt water, and the sealing member was removed from between the aluminum substrates.
[0046] <Salt water immersion test> The presence or absence of rust on the surface (sealing surface) of the aluminum base material that contacts the sealing member was confirmed by visual inspection. When rust was confirmed by visual inspection, it was evaluated as "x", and when no rust was confirmed, it was evaluated as "○".
[0047] <Thickness of surface treatment layer> In addition, when the liquid material for coating was applied, the liquid material was also applied onto a 0.52 mm polyimide film at the same time, and the thickness of the entire sheet obtained after the liquid material was cured was measured with a digital micrometer. Next, the total thickness of the sheet, which was (thickness of the surface treatment layer + thickness of the polyimide film), was measured, and then the thickness of the surface treatment layer was calculated by calculating (total thickness of the sheet - thickness of the polyimide film).
[0048] Example 2 A sealing member was produced in the same manner as in Example 1, except that a corrosion inhibitor B (a mixture of dicyclohexylamine and oleic acid) previously dissolved in isopropyl alcohol was used instead of the corrosion inhibitor A. The obtained sealing member was evaluated in the same manner as in Example 1.
[0049] Example 3 A sealing member was prepared in the same manner as in Example 1, except that a corrosion inhibitor C (a reactant of dicyclohexylamine and oleic acid substituted with -(CHO)-H) previously dissolved in isopropyl alcohol was used instead of the corrosion inhibitor A. The obtained sealing member was evaluated in the same manner as in Example 1.
[0050] Example 4 A sealing member was produced in the same manner as in Example 1, except that in Example 3, the corrosion inhibitor C was added to the urethane binder ("Superflex 740" manufactured by Daiichi Pharmaceutical Co., Ltd.) at a ratio of 5 mass % based on the solid content. The obtained sealing member was evaluated in the same manner as in Example 1.
[0051] Example 5 A sealing member was produced in the same manner as in Example 1, except that in Example 1, instead of the corrosion inhibitor A, a corrosion inhibitor D (an oligomer of dicyclohexylamine, oleic acid, and dicyclohexylamine substituted with -(C2H4O)2-CH3) dissolved in advance in isopropyl alcohol was used, and the corrosion inhibitor D was added to a urethane binder ("Superflex 740" manufactured by Daiichi Pharmaceutical Co., Ltd.) at a ratio of 5 mass % relative to the solid content. The obtained sealing member was evaluated in the same manner as in Example 1.
[0052] Example 6 A sealing member was produced in the same manner as in Example 1, except that in Example 5, an O-ring made of cured ethylene-propylene-diene terpolymer rubber (EPDM) having a type A durometer hardness of 60 was used as the O-ring. The obtained sealing member was evaluated in the same manner as in Example 1.
[0053] Comparative Example 1 A sealing member was produced in the same manner as in Example 1, except that no surface treatment layer was formed in Example 1. The obtained sealing member was evaluated in the same manner as in Example 1.
[0054] Comparative Example 2 A sealing member was produced in the same manner as in Example 1, except that the corrosion inhibitor A was not added and the surface treatment layer was formed with a urethane binder. The obtained sealing member was evaluated in the same manner as in Example 1.
[0055] Comparative Example 3 A sealing member was produced in the same manner as in Example 1, except that a corrosion inhibitor E (calcium sulfonate) was added in a proportion of 5 mass % relative to the solid content of a urethane binder ("Superflex 740" manufactured by Daiichi Pharmaceutical Co., Ltd.) instead of the corrosion inhibitor A in Example 1. The obtained sealing member was evaluated in the same manner as in Example 1.
[0056] Comparative Example 4 A sealing member was produced in the same manner as in Example 1, except that in Example 3, the corrosion inhibitor C was added to the urethane binder ("Superflex 740" manufactured by Daiichi Pharmaceutical Co., Ltd.) so that the ratio of the solid content was 10 mass %. The obtained sealing member was evaluated in the same manner as in Example 1.
[0057] Comparative Example 5 In Example 5, a sealing member was produced in the same manner as in Example 1, except that the thickness of the surface treatment film was formed to be 5 μm. The obtained sealing member was evaluated in the same manner as in Example 1.
[0058] The results of the "salt water immersion test" for Examples 1 to 6 and Comparative Examples 1 to 5 are shown in Table 1.
[0059] [Table 1]
[0060] The components shown in Table 1 above are as follows. ·EPDM: Ethylene-propylene-diene terpolymer rubber Corrosion inhibitor A: A composition containing triethanolamine and calcium sulfonate Corrosion inhibitor B: A mixture of dicyclohexylamine and oleic acid Corrosion inhibitor C: -(C2H4O)2-H substituted dicyclohexylamine reacted with oleic acid Corrosion inhibitor D: Oligomeric compound of dicyclohexylamine, oleic acid, and dicyclohexylamine substituted with -(C2H4O)2-CH3 Corrosion inhibitor E: Calcium sulfonate
[0061] From the results in Table 1, in Examples 1 to 6, in which a sealing member was used in which a surface treatment layer containing an amine-containing corrosion inhibitor in an amount of 0.5% by mass or more and 8% by mass or less was formed on the sealed surface with a thickness greater than the maximum height roughness Rz, the salt water immersion test results were all "○". In addition, no residue was found on the 100M filter, and coating without clogging during spray application was possible. Therefore, it was possible to provide a sealing member that can effectively prevent corrosion and rust on the surface of the sealed member simply and at low cost.
[0062] On the other hand, from the results of Table 1, no surface treatment layer was formed on the rubber base material of the sealing material in Comparative Example 1. Therefore, the result of the salt water immersion test was "X", and the occurrence of rust could not be prevented.
[0063] In Comparative Example 2, the surface treatment layer formed with the urethane binder did not contain a corrosion inhibitor, and therefore the result of the salt water immersion test was "X", meaning that the occurrence of rust could not be prevented.
[0064] In Comparative Example 3, the result of the salt water immersion test was "good", and although the occurrence of rust was prevented, calcium sulfonate was used in the formation of the surface treatment layer instead of the corrosion inhibitor containing amine. Therefore, residue was confirmed on the 100M filter. Such residue caused clogging during the subsequent spray application of the coating material, so it was not possible to effectively prevent the occurrence of rust at low cost.
[0065] In Comparative Example 4, the result of the salt water immersion test was "good", and the occurrence of rust could be prevented, but the content of the corrosion inhibitor containing amine in the formation of the surface treatment layer was 10 mass%, and an excessive amount of the corrosion inhibitor was used. Therefore, the excess corrosion inhibitor aggregated with other components, and residue was confirmed on the 100M filter. Such residue caused clogging during the subsequent spray application of the coating material, so it was not possible to effectively prevent the occurrence of rust at low cost.
[0066] In Comparative Example 5, the thickness of the surface treatment layer is equal to or less than the maximum height roughness Rz of the sealed surface of the aluminum substrate, which is the sealed member, so the surface treatment layer cannot completely seal the sealed surface, and the corrosion inhibitor easily escapes from the gaps in the aluminum substrate and cannot remain on the sealed surface. Therefore, the result of the salt water immersion test was "X", and rust generation could not be prevented.
Claims
1. A rubber substrate and a surface treatment layer coated on a surface of the rubber substrate, the surface treatment layer contains at least one volatile corrosion inhibitor; the corrosion inhibitor comprises at least one amine; the amine is a tertiary amine selected from the group consisting of triethanolamine, a reaction product of dicyclohexylamine with a higher fatty acid, and an oligomer of dicyclohexylamine with a higher fatty acid; The tertiary amine may be substituted with an alkyl group, a hydroxyl group, or an alkoxyalkyl group, or may be an unsubstituted amine; The content of the corrosion inhibitor in the surface treatment layer is 0.5% by mass or more and 8% by mass or less. and The thickness of the surface treatment layer on the sealed surface conforms to JIS B 0601:2001. The seal member is characterized in that the maximum height roughness Rz (μm) measured by
2. 2. The seal according to claim 1, wherein the content of the corrosion inhibitor is 1% by mass or more and 5% by mass or less. Parts.
3. 3. The seal member according to claim 1, which is a seal member for an aluminum housing.
Citation Information
Patent Citations
Daikasutomashinnoshashutsusochi
JP1976089823A
Storage box producing method
JP1978019282A
Alkaline primary battery
JP1978065928A
Boarding bridge
JP1979083296A
Joint sheet
JP1987101680A