Composite absorbent materials and sanitary products
The composite absorbent body with a hydrophilic continuous skeleton and pores addresses the inefficiencies of conventional absorbents by rapidly absorbing and transferring fluids to superabsorbent polymers for enhanced absorption and retention.
Patent Information
- Application Number
- JP2020219812
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-29
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2040-12-29
AI Technical Summary
Conventional absorbent materials in sanitary products face challenges in achieving high absorption performance, as porous materials quickly saturate and superabsorbent polymers have slow absorption rates, leading to inefficient fluid management.
A composite absorbent body comprising a polymer absorbent with a hydrophilic continuous skeleton and continuous pores, which rapidly absorbs fluids by osmotic pressure, expanding to incorporate large volumes, followed by transfer to superabsorbent polymers for steady retention.
The composite absorbent body achieves high absorption performance by instantly taking in large amounts of body fluids and steadily retaining them, combining rapid intake with long-term retention capabilities.
Smart Images

Figure 0007580270000001 
Figure 0007580270000002 
Figure 0007580270000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite absorbent body and a sanitary product having the same. [Background technology]
[0002] 2. Description of the Related Art Sanitary products such as disposable diapers and sanitary napkins are known to contain, as an absorbent, a porous material such as a sponge material or a superabsorbent polymer (so-called "SAP") having a high absorption capacity. For example, Patent Document 1 discloses an absorbent article containing a polymer foam material (porous material) consisting of a hydrophilic flexible structure of interconnected open cells, and Patent Document 2 discloses an absorbent article using an absorbent body formed by combining absorbent resin particles (superabsorbent polymer) with excellent absorption capacity and hydrophilic fibers such as pulp fibers with excellent absorption speed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 3231320 [Patent Document 2] International Publication No. 2013 / 018571 Summary of the Invention [Problem to be solved by the invention]
[0004] The absorbent materials used in such conventional absorbents have the following characteristics. For example, the porous material disclosed in Patent Document 1 absorbs moisture by taking it into a plurality of pores having a predetermined space, and therefore can instantly absorb moisture by utilizing capillary action. However, since the space that can absorb moisture is limited to the predetermined space formed by the plurality of pores, it is difficult to absorb large amounts of moisture. On the other hand, superabsorbent polymers (SAPs) as disclosed in Patent Document 2 absorb water while expanding the space equivalent to the volume of the absorbed water (i.e., expanding), and therefore can retain a large amount of water (i.e., have a high water retention capacity), but have a slow water absorption rate, making it difficult to instantly absorb water. In addition, it is possible to use these absorbent materials simultaneously to compensate for the shortcomings of each absorbent material. However, for example, when a large amount of body fluids such as urine or menstrual blood is discharged from the wearer of the sanitary product, the amount that can be absorbed by the porous material (absorption limit) may be exceeded in the early stages of absorption. Furthermore, body fluids that are not absorbed by the porous material will not be absorbed immediately by SAP, so that there is a risk that high absorption performance will not be achieved.
[0005] The present invention has been made in view of the above problems, and has an object to provide an absorbent body having high absorption performance capable of instantaneously absorbing a large amount of body fluid. [Means for solving the problem]
[0006] One aspect of the present invention (Aspect 1) is a composite absorbent for absorbing body fluids, The composite absorbent body includes a polymer absorbent having a hydrophilic continuous skeleton and continuous pores, and a superabsorbent polymer; The polymer absorbent is the composite absorbent characterized in that, when absorbing moisture, the polymer absorbent incorporates the moisture into the continuous framework and then into the continuous pores.
[0007] In the composite absorbent of this embodiment 1, when the polymer absorbent having a hydrophilic continuous skeleton and continuous pores absorbs body fluids such as urine or menstrual blood, the hydrophilic continuous skeleton instantaneously takes up the body fluid due to osmotic pressure and expands, expanding the volume of the continuous pores. This enables the body fluid to be further taken up into the expanded continuous pores, thereby enabling the composite absorbent to instantaneously absorb a large amount of body fluid, and the absorbed body fluid can then be transferred to a superabsorbent polymer (SAP) with high water retention capacity and steadily retained within the SAP. This allows the composite absorbent body of this embodiment to exhibit high absorption performance as an absorbent body.
[0008] In another aspect (Aspect 2) of the present invention, in the composite absorbent of Aspect 1 above, the polymer absorbent is characterized in that, at the time of water retention limit water absorption, the volume of the expanded polymer absorbent is larger than the volume of water absorbed.
[0009] The composite absorbent of this embodiment can exhibit higher absorption performance as an absorbent since the polymer absorbent can incorporate a larger amount of moisture into the open pores.
[0010] In still another aspect (Aspect 3) of the present invention, in the composite absorbent of Aspect 1 or 2 above, the polymer absorbent is characterized in that the water absorption capacity of the continuous pores is greater than the water absorption capacity of the continuous skeleton.
[0011] In the composite absorbent of this embodiment, the polymer absorbent can take in a larger amount of moisture into the open pores, and therefore the composite absorbent as an absorbent can exhibit even higher absorption performance.
[0012] In yet another aspect (Aspect 4) of the present invention, in the composite absorbent of any of Aspects 1 to 3 above, the polymer absorbent is characterized in that the mass ratio of the water absorption capacity of the continuous pores to the water absorption capacity of the continuous skeleton is 60:40 to 95:5.
[0013] In the composite absorbent of this embodiment, the mass ratio of the water absorption amount of the continuous pores of the polymer absorbent to the water absorption amount of the continuous skeleton is within the above-mentioned specific range, so that when the polymer absorbent absorbs moisture, the moisture can be more reliably absorbed into the continuous skeleton and then into the continuous pores.
[0014] In yet another aspect (Aspect 5) of the present invention, in the composite absorbent of any of Aspects 1 to 4 above, the polymer absorbent is characterized in that the absorption rate from immediately after the start of water absorption until the water retention limit is reached is relatively high, and the absorption rate after the water retention limit is relatively low.
[0015] In the composite absorbent of this embodiment, in the early stage of water absorption from immediately after the start of water absorption until the water retention limit is reached, the absorption rate of the polymer absorbent is relatively high and body fluids can be instantaneously taken up into the continuous skeleton, whereas in the later stage of water absorption after the water retention limit, the absorption rate of the polymer absorbent is relatively low and body fluids can be steadily taken up into the enlarged continuous pores due to the expansion of the continuous skeleton, so that the absorbent can more reliably exhibit its high absorption performance as an absorbent.
[0016] In still another aspect (aspect 6) of the present invention, in the composite absorbent of any one of aspects 1 to 5 above, the polymer absorbent is a monolithic absorbent.
[0017] In the composite absorbent of this embodiment, since the polymer absorbent is a monolithic absorbent, it is capable of swiftly absorbing body fluids and more reliably transferring the body fluid temporarily held in the polymer absorbent to the SAP.
[0018] In yet another aspect (Aspect 7) of the present invention, in the composite absorbent of any of Aspects 1 to 6 above, the polymer absorbent is a hydrolysate of a crosslinked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule, and is characterized in that it contains at least one -COONa group.
[0019] In the composite absorbent of this embodiment, since the polymer absorbent has the above-mentioned specific configuration, when absorbing body fluids, the hydrophilic continuous skeleton is easily elongated (i.e., easily expanded) and the continuous pores are easily expanded, so that a larger amount of body fluid can be taken up into the continuous pores more quickly, and the absorbent can exhibit even superior absorption performance.
[0020] A further aspect (aspect 8) of the present invention is a sanitary article comprising the composite absorbent body according to any one of aspects 1 to 7 above.
[0021] The sanitary product of this embodiment has the composite absorbent body of any one of the above-mentioned embodiments 1 to 7, and therefore can exhibit excellent absorption performance as a sanitary product. Effect of the Invention
[0022] According to the present invention, it is possible to provide an absorbent body having high absorption performance, capable of instantaneously absorbing a large amount of body fluid. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a schematic plan view of a light incontinence pad 1 in an expanded state, as viewed in the thickness direction from the skin-facing surface side. [Diagram 2] FIG. 2 is a diagram illustrating a manufacturing process of absorbent A, which is an example of a polymer absorbent. [Diagram 3] FIG. 3 is an SEM photograph of absorbent A at a magnification of 50 times. [Figure 4] FIG. 4 is a SEM photograph of absorbent A at a magnification of 100 times. [Diagram 5] FIG. 5 is an SEM photograph of absorbent A at a magnification of 500 times. [Figure 6] FIG. 6 is a SEM photograph of absorbent A at a magnification of 1000 times. [Figure 7] FIG. 7 is a SEM photograph of absorbent A at a magnification of 1500 times. [Figure 8] FIG. 8 is a cross-sectional photograph taken by a scanning electron microscope, showing the state of absorbent A before and after water absorption. [Figure 9] FIG. 9 is a set of CT images showing the absorption state of absorbent A for each amount of distilled water dispensed. [Figure 10] FIG. 10 shows CT images showing the absorption state of two types of SAP at different drip amounts of distilled water. [Figure 11] FIG. 11 is a set of CT images showing the absorption state of Infinity particles for each drop of distilled water. [Figure 12] FIG. 12 is a graph showing the relationship between the absorbency and the amount of volume change of absorbent A, which is an example of the polymer absorbent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] A preferred embodiment of the composite absorbent body of the present invention will be described in detail below using a light incontinence pad 1, which is an example of a sanitary product to which the composite absorbent body can be applied. In this specification, unless otherwise specified, the term "planar view" simply refers to "viewing an object (e.g., a light incontinence pad, a composite absorbent, etc.) placed in an unfolded state on a horizontal surface from above in the vertical direction (from the top sheet side if the object is a sanitary product) in the thickness direction of the object."
[0025] In this specification, the "longitudinal direction" refers to the "longer direction of a vertically elongated object (e.g., a light incontinence pad, a composite absorbent, etc. in an unfolded state) when viewed in a plane", the "width direction" refers to the "shorter direction of a vertically elongated object when viewed in a plane", and the "thickness direction" refers to the "perpendicular direction to an object placed on a horizontal surface in an unfolded state", and these longitudinal, width and thickness directions are perpendicular to each other.
[0026] Furthermore, in this specification, unless otherwise specified, in the thickness direction of the light incontinence pad 1, the "proximal side relative to the wearer's skin when the light incontinence pad 1 is worn" is referred to as the "skin-facing side", and the "distal side relative to the wearer's skin when the light incontinence pad 1 is worn" is referred to as the "non-skin-facing side".
[0027] [Light incontinence pads] FIG. 1 is a schematic plan view of a light incontinence pad 1 in an expanded state to which a composite absorbent body 4 according to one embodiment of the present invention is applied. 1, the light incontinence pad 1 has a longitudinal direction L and a width direction W in plan view, and has a vertically elongated outer shape with two longitudinal end edges protruding outward in an arc shape in the longitudinal direction. Note that the outer shape of the light incontinence pad 1 is not limited to this, and any shape (e.g., oval, rectangular, hourglass, etc.) can be adopted as long as it is vertically elongated according to various applications and usage modes.
[0028] The light incontinence pad 1 basically comprises, in the thickness direction, a liquid-permeable top sheet 2 which forms the surface of the light incontinence pad 1 facing the skin, a back sheet 3 which forms the surface of the light incontinence pad 1 not facing the skin, and a composite absorbent 4 located between these sheets. The light incontinence pad 1 further includes an adhesive portion (not shown) that is disposed on the surface of the backsheet 3 that does not face the skin and that adhesively fixes the light incontinence pad 1 to the inner surface of the wearer's clothing, such as underwear.
[0029] It should be noted that the light incontinence pad 1 is not limited to this configuration, and may, for example, comprise a pair of side sheets for forming a leak-proof wall, which are positioned at both ends of the light incontinence pad 1 in the width direction W at a position closer to the skin-facing side than the top sheet 2 and extend in the longitudinal direction L, and a plurality of elastic members arranged along the longitudinal direction L on each of the pair of side sheets.
[0030] In the light incontinence pad 1, the composite absorbent 4 is located between the top sheet 2 and the back sheet 3, and is formed from an absorbent material capable of absorbing bodily fluids such as urine and menstrual blood that are discharged from the wearer and permeate the top sheet 2, and this composite absorbent 4 contains a polymer absorbent having a hydrophilic continuous skeleton and continuous pores, and a superabsorbent polymer (SAP). Furthermore, this polymer absorbent exhibits a unique water absorption behavior in which, when absorbing water, the water is incorporated into the above-mentioned continuous framework and then into the continuous pores.
[0031] In the composite absorbent 4, when the polymer absorbent having the above-mentioned hydrophilic continuous skeleton and continuous pores absorbs body fluids such as urine or menstrual blood, the hydrophilic continuous skeleton instantly takes up the body fluid due to osmotic pressure and expands, expanding the volume of the continuous pores. As a result, the body fluid can be further taken up into the expanded continuous pores, and therefore a large amount of body fluid can be instantly absorbed. The absorbed body fluid can then be transferred to the SAP, which has a high water retention capacity, and steadily retained within the SAP. This allows the composite absorbent body 4 to exhibit high absorption performance as an absorbent body.
[0032] Therefore, the light incontinence pad 1 including such a composite absorbent body 4 can also exhibit excellent absorption performance as a light incontinence pad.
[0033] Various constituent members of sanitary goods to which the composite absorbent body of the present invention is applied will be described in more detail below using the above-mentioned light incontinence pad 1.
[0034] (Surface sheet) 1, in the above-mentioned light incontinence pad 1, the top sheet 2 has a vertically elongated outer shape in a plan view, extending from one edge to the other edge in the longitudinal direction L of the light incontinence pad 1 and also extending from the vicinity of one edge to the vicinity of the other edge in the width direction W of the light incontinence pad 1. The top sheet 2 is arranged at a position on the skin-facing side in the thickness direction of the light incontinence pad 1 and is composed of a liquid-permeable sheet-like member that forms a contact surface that can come into contact with the wearer's skin, i.e., the surface of the light incontinence pad 1 facing the skin.
[0035] As shown in FIG. 1, the top sheet 2 is slightly larger in the longitudinal direction L and width direction W than the composite absorbent 4 arranged on the non-skin-facing side of the top sheet 2, and is joined at its peripheral portion to the back sheet 3 located on the non-skin-facing side.
[0036] In the present invention, the outer shape, various dimensions, basis weight, etc. of the top sheet are not particularly limited as long as they can be used as a top sheet for sanitary products, and any outer shape, various dimensions, basis weight, etc. can be adopted depending on the desired liquid permeability, feel to the skin, flexibility, strength, etc.
[0037] (Back sheet) In the above-mentioned light incontinence pad 1, the back sheet 3 has a vertically elongated outer shape in a plan view, extending from one side edge to the other side edge in the longitudinal direction L of the light incontinence pad 1 and also from one side edge to the other side edge in the width direction W of the light incontinence pad 1. The back sheet 3 is disposed at a position on the non-skin-facing side in the thickness direction of the light incontinence pad 1 to form the non-skin-facing surface of the light incontinence pad 1, and is composed of a liquid-impermeable sheet-like member that prevents body fluids such as urine and menstrual blood that have permeated the composite absorbent 4 from leaking out of the light incontinence pad 1.
[0038] In the present invention, the outer shape, various dimensions, basis weight, etc. of the back sheet are not particularly limited as long as they can be used as a back sheet of a sanitary product, and any outer shape, various dimensions, basis weight, etc. can be adopted according to the desired leak prevention performance, breathability, strength, etc.
[0039] (Composite absorber) In the above-mentioned light incontinence pad 1, as shown in Figure 1, when viewed in a plane, the composite absorbent 4 extends over a wide area in the longitudinal direction L from near one edge in the longitudinal direction L to near the other edge, centered on the center of the light incontinence pad 1 in the longitudinal direction L and width direction W, and also extends over a wide area in the width direction W from near one edge in the width direction W to near the other edge, and further has a vertically elongated outer shape in which the two longitudinal edges protrude in an arc shape toward the outward longitudinal direction.
[0040] More specifically, the composite absorbent body 4 has a constricted portion in the longitudinal center when viewed in a plane, the constricted portion having a widthwise length relatively smaller than other portions, and further has a minimum width portion in this constricted portion having the minimum width of the composite absorbent body 4, and a maximum width portion on the longitudinal outer side of the constricted portion having the maximum width of the composite absorbent body 4.
[0041] The composite absorbent 4 is disposed between the top sheet 2 and the back sheet 3 in the thickness direction of the light incontinence pad 1, and is formed from a predetermined absorbent member capable of absorbing and retaining bodily fluids such as urine and menstrual blood that have permeated the top sheet 2, and this absorbent member is composed of absorbent materials such as polymer absorbents, hydrophilic fibers, and highly absorbent polymers, which will be described later, and a sheet such as tissue that retains it. In other words, the composite absorbent means an absorbent member composed of an absorbent material capable of absorbing and retaining bodily fluids, and a sheet that retains it.
[0042] In the light incontinence pad 1, the composite absorbent body 4 is bonded to each of the top sheet 2 and the back sheet 3 by any adhesive such as a hot melt adhesive.
[0043] The composite absorbent 4 contains a polymer absorbent having a hydrophilic continuous skeleton and continuous pores and exhibiting the above-mentioned unique water absorption behavior, and a superabsorbent polymer. The polymer absorbent will be described later, and the superabsorbent polymer is a powder or granular material made of a highly absorbent polymer such as a sodium acrylate copolymer known in the art, and is called SAP (Super Absorbent Polymer).
[0044] The composite absorbent 4 may contain only the above-mentioned polymer absorbent and superabsorbent polymer as the water-absorbing material, or may further contain a water-absorbing material known in the art in addition to these. Examples of such water-absorbing materials include hydrophilic fibers, and more specifically, pulp fibers (e.g., ground pulp, etc.), and cellulosic fibers such as cotton, rayon, and acetate.
[0045] The composite absorbent body 4 may have a configuration in which such a polymer absorbent, a highly absorbent polymer, and any water-absorbent material are covered with a wrap sheet such as a hydrophilic tissue.
[0046] In the present invention, the outer shape, various dimensions, basis weight, etc. of the composite absorbent body are not particularly limited as long as they do not impair the effects of the present invention, and any outer shape, various dimensions, basis weight, etc. can be adopted according to the desired water absorbency, flexibility, strength, etc.
[0047] The polymer absorbent used in the composite absorbent of the present invention will be described in more detail below.
[0048] [Polymer absorbent] In the present invention, the polymer absorbent is not particularly limited as long as it has a hydrophilic continuous skeleton and continuous pores, and exhibits a unique water absorption behavior in which, when absorbing moisture, the moisture is taken into the above-mentioned continuous skeleton and then into the continuous pores. Such a polymer absorbent is, for example, a hydrolyzate of a crosslinked polymer of two or more monomers including at least a (meth)acrylic acid ester, and a polymer compound having at least one hydrophilic group in the functional group. More specifically, a polymer compound is a hydrolyzate of a crosslinked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule, and has at least a -COONa group. Such a polymer absorbent is an organic porous body having at least one or more -COONa groups in one molecule, and may further have a -COOH group. The -COONa groups are distributed approximately uniformly in the skeleton of the porous body.
[0049] When the polymer absorbent is a hydrolysate of a crosslinked polymer of such a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule and contains at least one -COONa group, as described below, the hydrophilic continuous skeleton becomes easier to extend (i.e., expand) when absorbing body fluids such as urine and menstrual blood, and the continuous pores also become easier to expand, so that a larger amount of body fluid can be taken in the continuous pores more quickly, and the absorbent can exhibit even better absorption performance.
[0050] In this specification, the (meth)acrylic acid ester refers to an acrylic acid ester or a methacrylic acid ester.
[0051] In such a polymer absorbent formed by a hydrolysis product of a cross-linked polymer of a (meth)acrylic acid ester and divinylbenzene, a hydrophilic continuous skeleton is formed by an organic polymer having at least -COONa groups, and the skeleton has communicating holes (interconnected pores) that serve as absorption sites for the liquid to be absorbed (i.e., body fluids such as urine and menstrual blood). In addition, since the hydrolysis treatment converts the -COOR groups (that is, carboxylate groups) of the crosslinked polymer into -COONa groups or -COOH groups (see FIG. 2), the polymer absorbent may have -COOR groups.
[0052] The presence of --COOH groups and --COONa groups in the organic polymer forming the hydrophilic continuous skeleton can be confirmed by analysis using infrared spectroscopy and a method for quantifying weakly acidic ion-exchange groups.
[0053] Here, Fig. 2 is a diagram for explaining the manufacturing process of absorbent A, which is an example of a polymer absorbent. In this Fig. 2, the upper diagram shows the constituent raw materials for polymerization, the middle diagram shows monolith A, which is a crosslinked polymer of (meth)acrylic acid ester and divinylbenzene, and the lower diagram shows absorbent A obtained by subjecting monolith A in the middle diagram to hydrolysis and drying treatment.
[0054] Hereinafter, an explanation will be given using absorbent A, which is an example of a polymer absorbent and is formed from a hydrolysate of a crosslinked polymer of a (meth)acrylic acid ester and divinylbenzene.
[0055] The polymer absorbent is not limited to the absorbent A, but may be a hydrolysate of a cross-linked polymer of a (meth)acrylic acid ester and a compound having two or more vinyl groups in one molecule, or a hydrolysate of a cross-linked polymer of two or more monomers including at least a (meth)acrylic acid ester. However, when the polymer absorbent is a monolithic absorbent, it has the advantage that it can quickly absorb body fluids and that the body fluid temporarily held in the polymer absorbent can be more steadily transferred to the SAP.
[0056] In the following description, "Monolith A" refers to an organic porous material consisting of a crosslinked polymer of (meth)acrylic acid ester and divinylbenzene before hydrolysis treatment, and may be referred to as a "monolithic organic porous material." In addition, "absorbent A" is a hydrolyzate of a crosslinked polymer (monolith A) of (meth)acrylic acid ester and divinylbenzene after hydrolysis and drying. In the following description, absorbent A refers to the absorbent in a dry state.
[0057] First, the structure of absorbent A will be described. As described above, absorbent A has a hydrophilic continuous skeleton and continuous pores. As shown in Figure 2, absorbent A, which is an organic polymer having a hydrophilic continuous skeleton, is obtained by cross-linking polymerizing (meth)acrylic acid ester, which is a polymerization monomer, and divinylbenzene, which is a cross-linking monomer, and further hydrolyzing the obtained cross-linked polymer (monolith A).
[0058] The organic polymer that forms a hydrophilic continuous skeleton has, as structural units, a polymerized residue of an ethylene group (hereinafter referred to as "structural unit X") and a cross-linked polymerized residue of divinylbenzene (hereinafter referred to as "structural unit Y"). Furthermore, the polymerized residue of the ethylene group (structural unit X) in the organic polymer forming the hydrophilic continuous skeleton has a -COONa group generated by hydrolysis of the carboxylate group, or both a -COOH group and a -COONa group. When the polymerized monomer is a (meth)acrylic acid ester, the polymerized residue of the ethylene group (structural unit X) has a -COONa group, a -COOH group, and an ester group.
[0059] In the absorbent A, the ratio of the crosslinked polymer residue of divinylbenzene (structural unit Y) in the organic polymer forming the hydrophilic continuous skeleton is, for example, 0.1 to 30 mol %, preferably 0.1 to 20 mol %, based on the total structural units. For example, in the absorbent A in which butyl methacrylate is used as the polymerization monomer and divinylbenzene is used as the crosslinked monomer, the ratio of the crosslinked polymer residue of divinylbenzene (structural unit Y) in the organic polymer forming the hydrophilic continuous skeleton is, for example, about 3 mol %, preferably 0.1 to 10 mol %, more preferably 0.3 to 8 mol %, based on the total structural units. Furthermore, when the ratio of cross-linked polymerized residues of divinylbenzene in the organic polymer forming the hydrophilic continuous skeleton is 0.1 mol % or more, the strength of absorbent A is less likely to decrease, and when the ratio of cross-linked polymerized residues of divinylbenzene is 30 mol % or less, the absorption amount of the liquid to be absorbed is less likely to decrease.
[0060] In addition, in the absorbent A, the organic polymer forming the hydrophilic continuous skeleton may be composed only of the structural unit X and the structural unit Y, or may have, in addition to the structural unit X and the structural unit Y, a structural unit other than the structural unit X and the structural unit Y, that is, a polymerized residue of a monomer other than a (meth)acrylic acid ester and divinylbenzene.
[0061] Examples of structural units other than the structural unit X and the structural unit Y include polymerized residues of monomers such as styrene, α-methylstyrene, vinyltoluene, vinylbenzyl chloride, glycidyl (meth)acrylate, isobutene, butadiene, isoprene, chloroprene, vinyl chloride, vinyl bromide, vinylidene chloride, tetrafluoroethylene, (meth)acrylonitrile, vinyl acetate, ethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate.
[0062] The proportion of structural units other than the structural unit X and the structural unit Y in the organic polymer that forms the hydrophilic continuous skeleton is, for example, 0 to 50 mol %, and preferably 0 to 30 mol %, relative to all structural units.
[0063] In addition, the thickness of the hydrophilic continuous skeleton of the absorbent A is preferably 0.1 to 100 μm. When the thickness of the hydrophilic continuous skeleton of the absorbent A is 0.1 μm or more, the spaces (pores) for taking in the liquid to be absorbed (body fluid) in the porous body are less likely to collapse during absorption, and the absorption amount is less likely to decrease. On the other hand, when the thickness of the hydrophilic continuous skeleton is 100 μm or less, an excellent absorption speed is easily obtained.
[0064] In addition, since the pore structure of the hydrophilic continuous skeleton of absorbent A is an open-cell structure, the thickness of the continuous skeleton is measured by evaluating the cross section of the skeleton that appears on the test piece for electron microscope measurement. The continuous skeleton is often polygonal in shape because it is formed by the gaps between water (water droplets) removed by the dehydration and drying process after hydrolysis. Therefore, the thickness of the continuous skeleton is the average value of the diameter (μm) of the circle circumscribing the polygonal cross section. In rare cases, there may be small holes in the polygon, in which case the circumscribing circle of the polygonal cross section surrounding the small holes is measured.
[0065] Furthermore, the absorbent A preferably has an average diameter of interconnected pores of 1 to 1000 μm. When the average diameter of interconnected pores in the absorbent A is 1 μm or more, the spaces (pores) for taking in the liquid to be absorbed (body fluid) in the porous body are less likely to collapse during absorption, and the absorption rate is less likely to decrease. On the other hand, when the average diameter of interconnected pores is 1000 μm or less, an excellent absorption rate is more likely to be obtained.
[0066] The average diameter (μm) of the interconnected pores of absorbent A can be measured by mercury intrusion porosimetry, and the maximum value of the pore distribution curve obtained by the mercury intrusion porosimetry is used. Regardless of the ionic form of absorbent A, samples for measuring the average diameter of interconnected pores are those dried for 18 hours or more in a reduced pressure dryer set at a temperature of 50°C. The final pressure reached is 0 Torr.
[0067] Here, FIG. 3 is an SEM photograph of absorbent A at a magnification of 50 times, FIG. 4 is an SEM photograph of absorbent A at a magnification of 100 times, FIG. 5 is an SEM photograph of absorbent A at a magnification of 500 times, FIG. 6 is an SEM photograph of absorbent A at a magnification of 1000 times, and further, FIG. 7 is an SEM photograph of absorbent A at a magnification of 1500 times. The absorbents A shown in these Figs. 3 to 7 are examples of absorbents that use butyl methacrylate as a polymerization monomer and divinylbenzene as a cross-linking monomer, and each has a cubic structure with a side length of 2 mm.
[0068] 3 to 7 has a large number of cellular macropores and further has portions where these cellular macropores overlap. Absorbent A has an open cell structure in which the overlapping portions of the macropores form common openings (mesopores), i.e., it has an open cell structure (open macropore structure).
[0069] The overlapping portions of the macropores form common openings (mesopores) having an average diameter in a dry state of 1 to 1000 μm, preferably 10 to 200 μm, and particularly preferably 20 to 100 μm, and most of them have an open pore structure. When the average diameter of the mesopores in a dry state is 1 μm or more, the absorption rate of the liquid to be absorbed is improved. On the other hand, when the average diameter of the mesopores in a dry state is 1000 μm or less, the absorbent A is less likely to become embrittled. The number of overlapping macropores in each macropore is about 1 to 12, and in most cases, about 3 to 10.
[0070] In addition, since absorbent A has such an open cell structure, macropores and mesopores can be uniformly formed, and there is an advantage in that the pore volume and specific surface area can be significantly increased compared to the particle agglomeration type porous bodies as described in JP-A-8-252579 and the like.
[0071] The total pore volume of the pores (voids) of the absorbent A is preferably 0.5 to 50 mL / g, more preferably 2 to 30 mL / g. When the total pore volume of the absorbent A is 0.5 mL / g or more, the spaces (voids) for taking in the liquid to be absorbed (body fluid) of the porous body are less likely to collapse during absorption, and the absorption amount and absorption rate are less likely to decrease. On the other hand, when the total pore volume of the absorbent A is 50 mL / g or less, the strength of the absorbent A is less likely to decrease.
[0072] The total pore volume can be measured by mercury intrusion porosimetry. The sample for measuring the total pore volume is dried for 18 hours or more in a vacuum dryer set at a temperature of 50°C, regardless of the ion form of absorbent A. The final pressure is 0 Torr.
[0073] Hereinafter, the state when the absorbent A comes into contact with a liquid such as a body fluid (hereinafter simply referred to as "body fluid") will be described, but the same applies to the state when the composite absorbent 4 containing the absorbent A comes into contact with a body fluid. Furthermore, since the mass of absorbed body fluid is approximately proportional to the amount of body fluid, in the following description, the mass of body fluid may be simply referred to as the "amount of body fluid".
[0074] First, the continuous pores of absorbent A shown in Figures 3 to 7 are pores in which a plurality of pores (voids) are interconnected, and the presence of a large number of voids can be visually confirmed by the naked eye from the outside. When body fluids such as urine or menstrual blood come into contact with absorbent A having such a large number of pores, first, the hydrophilic continuous skeleton instantly absorbs a portion of the body fluid due to osmotic pressure and elongates (i.e., expands). This elongation of the continuous skeleton occurs in almost all directions. Here, Fig. 8 is a cross-sectional photograph taken with a scanning electron microscope (SEM) showing the state of absorbent A before and after water absorption. In this Fig. 8, the SEM photograph (a) on the left side is absorbent A before water absorption, and the SEM photograph (b) on the right side is absorbent A after water absorption. As shown in Figure 8, the size of each pore of absorbent A increases as the external shape of absorbent A increases due to the extension of the continuous skeleton during water absorption. When the size of the pores increases in this way, the volume of the pores increases, and the amount of body fluid that can be retained in the pores also increases. In other words, absorbent A, which has increased in size by absorbing a certain amount of body fluid in this way, is able to absorb a further predetermined amount of body fluid into the enlarged pores due to capillary action. In this way, absorbent A exhibits a unique water absorption behavior in which, when absorbing water (body fluid), the water is first incorporated into the hydrophilic continuous framework and then absorbed by the continuous pores.
[0075] Furthermore, body fluids absorbed into the hydrophilic continuous skeleton of absorbent A are not easily released from the continuous skeleton (i.e., are not easily synergized), whereas body fluids absorbed into the continuous pores are easily synergized. Therefore, within the composite absorbent, the body fluids absorbed into the continuous pores are synergized and transferred to the superabsorbent polymer (SAP) with high water retention capacity, and are steadily retained within the SAP. Here, the amount of body fluid absorbed into the continuous skeleton of absorbent A and the amount of body fluid absorbed into the continuous pores are determined as follows: out of the total amount of fluid absorbed by absorbent A, the amount of body fluid that is separated from absorbent A during centrifugation (150G / 90 seconds) (amount of separated water) is the amount of body fluid absorbed into the continuous pores, and the remaining amount of body fluid (i.e. the amount of body fluid that is not separated from absorbent A during centrifugation) is the amount of body fluid absorbed into the continuous skeleton.
[0076] Furthermore, more of the body fluid absorbed by absorbent A remains in the pores than in the hydrophilic continuous skeleton. Most of the body fluid is absorbed by absorbent A by retaining the body fluid in the pores through capillary action, so the greater the porosity (the volume of the pores relative to the volume of absorbent A), which is the ratio of the volume of the voids in the pores (total pore volume), the more body fluid can be absorbed. It is preferable that this porosity is 85% or more.
[0077] For example, when the porosity of the absorbent A shown in the above-mentioned Figs. 3 to 7 is calculated, it is as follows. First, the specific surface area of absorbent A obtained by mercury porosimetry is 400 m 2 / g, and the pore volume is 15.5 mL / g. This pore volume of 15.5 mL / g means that the volume of the pores in 1 g of absorbent A is 15.5 mL. Here, assuming that the specific gravity of absorbent A is 1 g / mL, the volume occupied by pores in 1 g of absorbent A, i.e., the pore volume, is 15.5 mL, and the volume of 1 g of absorbent A is 1 mL. In this case, the total volume (volume) of 1 g of absorbent A is 15.5 + 1 (mL), and the ratio of the pore volume to that is the porosity, so the porosity of absorbent A is 15.5 / (15.5 + 1) × 100 ≒ 94%.
[0078] Such an absorbent A having a hydrophilic continuous skeleton and continuous pores, i.e., a polymer absorbent, is applied in the form of, for example, particles or a sheet to a composite absorbent for absorbing body fluids such as urine and menstrual blood, such as the composite absorbent 4 of the light incontinence pad 1 described above. As described above, this polymer absorbent exhibits a unique water-absorbing behavior in which, when absorbing water, the water is first incorporated into the hydrophilic continuous skeleton and then into the continuous pores, so that it can instantly absorb a large amount of body fluid and can transfer the absorbed body fluid (mainly the body fluid absorbed into the continuous pores) to the SAP with high water-retaining capacity and steadily retain it within the SAP. Therefore, a composite absorbent using such a polymer absorbent can exhibit high absorption performance as an absorbent.
[0079] Here, a polymer absorbent as an example of the present invention, two types of superabsorbent polymers (SAP(A) and SAP(B)) as comparative examples, and an Infinity particle as a comparative example were prepared, and the absorption state when a predetermined amount of distilled water was dropped on each was observed by photographing it using a 3D micro X-ray CT device (CosmoScan FX (manufactured by Rigaku Corporation)). In this photographing, a sample of the polymer absorbent or the like was fixed to the bed of the device with double-sided tape, and distilled water was added from above. The photographing conditions were tube voltage: 90 kV, tube current: 88 μA, irradiation time: 2 minutes, resolution: 20 μm, matrix: 512 x 512 x 512. These observation results are shown in Figures 9 to 11. Fig. 9 is a CT image showing the absorption state of absorbent A for each drop amount of distilled water, Fig. 10 is a CT image showing the absorption state of two types of SAP for each drop amount of distilled water, and Fig. 11 is a CT image showing the absorption state of Infinity particles for each drop amount of distilled water. In Figs. 9 to 11, the white parts of each CT image correspond to the parts that have absorbed water, and each drop amount of distilled water is shown by the water absorption amount (mass) per unit mass of the absorbent such as a polymer absorbent, i.e., the water absorption ratio (g / g). The Infinity particles mentioned above are absorbents manufactured by P&G, and have a structure (foam structure) similar to that of polymer absorbents. However, unlike polymer absorbents, they do not have the ability to absorb water and expand.
[0080] As shown in FIG. 9, in the absorbent A of the present invention, as the amount of distilled water dropped (absorption capacity) increases, the hydrophilic continuous skeleton absorbs water and the continuous skeleton extends, causing the outer shape of the absorbent A to become larger. H After the water absorption capacity reaches 10 g / g (i.e., 25% water absorption), the water absorption in the interconnected pores progresses, and it becomes possible to absorb more water. A After the absorbency reaches 60 g / g, it becomes difficult to absorb moisture, and at a water absorption capacity of 90 g / g, moisture begins to overflow, as shown in FIG.
[0081] On the other hand, in the SAPs of the comparative examples, as shown in FIG. 10, both types of SAP absorbed water uniformly while diffusing it into the SAP as the amount of distilled water dropped (absorption ratio) increased, and did not show a stepwise water absorption behavior as in absorbent A of the invention example. Furthermore, in the Infinity particle body of the comparative example, as shown in Figure 11, as the amount of distilled water dripped increases, water absorption progresses from the upper side of the Infinity particle body, and this Infinity particle body also does not show a stepwise water absorption behavior like absorbent A of the present invention example.
[0082] As described above, absorbent A of the present invention exhibits the above-mentioned unique water absorption behavior not found in conventional SAP or Infinity particles, and is capable of instantly absorbing large amounts of body fluids and further transferring the absorbed body fluid to the SAP with high water retention capacity, demonstrating excellent absorption performance.
[0083] In the present invention, the polymer absorbent has a water retention limit L H It is preferable that the volume of the expanded polymer absorbent is larger than the volume of the absorbed water when absorbing water. Since such a polymer absorbent can absorb a larger amount of water into the interconnected pores, a composite absorbent containing such a polymer absorbent can exhibit higher absorption performance as an absorbent. Note that such characteristics of the polymer absorbent can be realized, for example, by appropriately adjusting the total pore volume of the interconnected pores and the porosity of the polymer absorbent. Here, the water retention limit L H The volume of the polymer absorbent that expands when absorbing water, and the water retention limit L H The volume of water taken up by the polymer absorbent during water absorption can be measured as follows.
[0084] <Water retention limit L H How to measure the volume of polymer absorbents that expand when absorbing water> (1) 1 g of the sample (polymer absorbent) for measurement is placed in a mesh bag (NBC Meshtec Co., Ltd., N-No. 255HD 115) cut to a size of 10 cm square. The mass (g) of the mesh bag is measured in advance. (2) The mesh bag containing the sample is immersed in saline (0.9% sodium chloride solution) for one hour. (3) Hang the mesh bag for 5 minutes and drain, then measure its mass (g). (4) After draining the water, the mesh bag is centrifuged at 150 G for 90 seconds, and the mass (g) of the mesh bag after centrifugation is measured. (5) The water retention capacity (g) of the sample is calculated by subtracting the total mass of the sample (=1g) and the mesh bag from the mass of the mesh bag after centrifugation, and then this water retention capacity is divided by the mass of the sample (=1g) to obtain the water retention capacity (g / g) per unit mass of the sample (polymer absorbent). This water retention capacity per unit mass is the water retention limit L H (g / g). (6) Separately, take out 30 particles of the measurement sample (polymer absorbent), measure their mass, and further divide the mass by the number of particles (30 particles) to calculate the average mass (g) per sample particle. (7) From the 30 samples, one sample that best matches the average mass value is selected, and that sample is fixed to the bed of a 3D micro X-ray CT device (CosmoScan FX, Rigaku Corporation) with double-sided tape. (8) From above the fixed grain sample, the water retention limit L obtained in (5) above H Add an amount (g) of distilled water equivalent to the amount of water added, and soak the single grain of sample in distilled water. (9) A single sample containing distilled water was observed using the above-mentioned 3D micro X-ray CT device (tube voltage: 90 kV, tube current: 88 μA, exposure time: 2 min, resolution: 20 μm, matrix: 512 x 512 x 512), and the water retention limit L was determined from the obtained CT images. H The volume (cm) of a single sample expanded at 3 ) is calculated.
[0085] In addition, the water retention limit L HThe volume of water absorbed by the polymer absorbent during water absorption is 1g = 1cm of distilled water. 3 As the water retention limit L H Amount (g) of volume (cm 3 ) is calculated.
[0086] In addition, when the measurement sample (polymer absorbent) is recovered from a sanitary product, it can be obtained according to the following <Recovery method of measurement sample (polymer absorbent)>.
[0087] <How to collect the measurement sample (polymer absorbent)> (1) Peel off the top sheet or other covering from the sanitary product to expose the absorbent core. (2) The object to be measured (polymer absorbent) is dropped from the exposed absorbent, and anything other than the (particulate) object to be measured (e.g., pulp, synthetic resin fibers, etc.) is removed using tweezers or the like. (3) A microscope or a simple magnifying glass is used as a magnifying observation means, and the measurement object is collected using tweezers or the like while observing at a magnification at which the difference from SAP can be recognized or at which the pores of the porous body can be visually recognized. The magnification of the simple magnifying glass is not particularly limited as long as the pores of the porous body can be visually recognized, and may be, for example, 25 to 50 times. (4) The objects to be measured thus collected are used as samples for measurement in various measurement methods.
[0088] Furthermore, it is preferable that the polymer absorbent has a water absorption capacity of the interconnected pores that is greater than that of the interconnected skeleton. Since such a polymer absorbent can incorporate a larger amount of water into the interconnected pores, a composite absorbent containing such a polymer absorbent can exhibit even higher absorption performance as an absorbent. The characteristics of such a polymer absorbent can be realized, for example, by appropriately adjusting the total pore volume of the interconnected pores or the porosity of the polymer absorbent. Here, the water absorption amount of the interconnected pores and the water absorption amount of the interconnected skeleton of the polymer absorbent can be measured as follows.
[0089] <Method for measuring the amount of water absorption of the interconnected pores and the interconnected skeleton of a polymer absorbent> (1) 1 g of the sample (polymer absorbent) for measurement is placed in a mesh bag (NBC Meshtec Co., Ltd., N-No. 255HD 115) cut to a size of 10 cm square. The mass (g) of the mesh bag is measured in advance. (2) The mesh bag containing the sample is immersed in saline (0.9% sodium chloride solution) for one hour. (3) Hang the mesh bag for 5 minutes and drain, then measure its mass (g). (4) The amount of water absorption (g) of the sample is calculated by subtracting the total mass of the sample (=1g) and the mesh bag from the mass of the mesh bag after draining measured in (3) above, and this amount of water absorption is further divided by the mass of the sample (=1g) to obtain the amount of water absorption (g / g) per unit mass of the sample (polymer absorbent). This amount of water absorption per unit mass is the water absorption limit L A (g / g). (5) Furthermore, the mesh bag after draining in (3) above is centrifuged at 150 G for 90 seconds, and the mass (g) of the mesh bag after the centrifugation is measured. (6) The water retention capacity (g) of the sample is calculated by subtracting the mass of the sample (=1g) and the total mass of the mesh bag from the mass of the mesh bag after centrifugation measured in (5) above, and this water retention capacity is then divided by the mass of the sample (=1g) to obtain the water retention capacity (g / g) per unit mass of the sample (polymer absorbent). This water retention capacity per unit mass is the water retention limit L H (g / g), and this water retention limit L H is defined as the "water absorption capacity of the continuous skeleton." (7) And the water absorption limit L obtained in (4) above A Water retention limit L H The amount (g / g) obtained by subtracting this is the "water absorption amount of the interconnected pores."
[0090] In addition, the polymer absorbent preferably has a mass ratio of the water absorption amount of the continuous pores to the water absorption amount of the continuous skeleton of 60:40 to 95:5. When the mass ratio of the water absorption amount of the continuous pores to the water absorption amount of the continuous skeleton of the polymer absorbent is within such a specific range, when the polymer absorbent absorbs moisture, the moisture can be more reliably absorbed into the continuous skeleton and then into the continuous pores. In addition, such properties of the polymer absorbent can also be realized by appropriately adjusting, for example, the total pore volume of the above-mentioned continuous pores or the porosity of the polymer absorbent.
[0091] In addition, it is preferable that the polymer absorbent has a relatively high absorption rate from immediately after the start of water absorption until the water retention limit is reached, and a relatively low absorption rate after the water retention limit. Here, FIG. 12 is a graph showing the relationship between the water absorption capacity and the volume change of absorbent A, which is an example of the polymer absorbent of the present invention. As shown in FIG. 12, after the start of water absorption, the volume change of absorbent A increases rapidly with an increase in water absorption capacity (i.e., the water absorption rate R1 is high). However, when the water absorption capacity is close to the water retention limit L H It can be seen that after the volume change reaches 10 g / g, the volume change increases slowly (i.e., the water absorption rate R2 is small). In this way, absorbent A reaches its water retention limit L immediately after it starts absorbing water. H In the initial stage of water absorption, the absorption rate is relatively high, so body fluids can be instantly absorbed into the continuous skeleton. H In the later stage of water absorption, the absorption rate is relatively slow, so that the body fluid can be steadily taken into the open pores expanded by the expansion of the open skeleton. This allows absorbent A to more reliably demonstrate its high absorption performance as an absorbent.
[0092] The volume change of the polymer absorbent is the water retention limit L H The volume of the polymer absorbent swelled at each water absorption capacity is measured according to the method for measuring the volume of the polymer absorbent swelled upon water absorption, and the volume is divided by the volume of the polymer absorbent before water absorption and multiplied by 100 to obtain the volume.
[0093] Hereinafter, the method for producing such a polymer absorbent will be described in detail using the above-mentioned absorbent A as an example.
[0094] [Method of manufacturing polymer absorbent] The above-mentioned absorbent A can be obtained through a cross-linking polymerization step and a hydrolysis step, as shown in Fig. 2. Each of these steps will be described below.
[0095] (Crosslinking polymerization process) First, an oil-soluble monomer for crosslinking polymerization, a crosslinkable monomer, a surfactant, water, and optionally a polymerization initiator are mixed to obtain a water-in-oil emulsion, which is an emulsion in which the oil phase is the continuous phase and water droplets are dispersed within it.
[0096] In the above-mentioned absorbent A, as shown in the upper diagram of Figure 2, butyl methacrylate, which is a (meth)acrylic acid ester, is used as the oil-soluble monomer, divinylbenzene is used as the cross-linking monomer, sorbitan monooleate is used as the surfactant, and isobutyronitrile is used as the polymerization initiator to cause cross-linking polymerization to obtain monolith A.
[0097] Specifically, for absorbent A, as shown in the upper diagram of Figure 2, first, 9.2 g of t-butyl methacrylate as an oil-soluble monomer, 0.28 g of divinylbenzene as a cross-linking monomer, 1.0 g of sorbitan monooleate (hereinafter abbreviated as "SMO") as a surfactant, and 0.4 g of 2,2'-azobis(isobutyronitrile) as a polymerization initiator are mixed and dissolved uniformly. Next, the mixture of t-butyl methacrylate / divinylbenzene / SMO / 2,2'-azobis(isobutyronitrile) is added to 180 g of pure water and stirred under reduced pressure using a planetary stirring device, a vacuum stirring and degassing mixer (manufactured by EME), to obtain a water-in-oil emulsion.
[0098] Furthermore, this emulsion is quickly transferred to a reaction vessel, sealed, and polymerized at 60°C for 24 hours under stationary conditions. After the polymerization is completed, the contents are removed, extracted with methanol, and then dried under reduced pressure to obtain Monolith A, which has a continuous macropore structure. The internal structure of Monolith A was observed by SEM, and it was found that Monolith A had a continuous cell structure and the thickness of the continuous skeleton was 5.4 μm. The average diameter of the continuous pores measured by mercury intrusion porosimetry was 36.2 μm, and the total pore volume was 15.5 mL / g.
[0099] The content of divinylbenzene in the total monomers is preferably 0.3 to 10 mol%, more preferably 0.3 to 5 mol%. The ratio of divinylbenzene to the total of butyl methacrylate and divinylbenzene is preferably 0.1 to 10 mol%, more preferably 0.3 to 8 mol%. In the above-mentioned absorbent A, the ratio of butyl methacrylate to the total of butyl methacrylate and divinylbenzene is 97.0 mol%, and the ratio of divinylbenzene is 3.0 mol%.
[0100] The amount of surfactant added can be set depending on the type of oil-soluble monomer and the desired size of emulsion particles (macropores), and is preferably in the range of about 2 to 70% of the total amount of the oil-soluble monomer and surfactant.
[0101] In order to control the shape and size of the bubbles in Monolith A, alcohols such as methanol and stearyl alcohol; carboxylic acids such as stearic acid; hydrocarbons such as octane, dodecane, and toluene; cyclic ethers such as tetrahydrofuran and dioxane, etc. may be allowed to coexist in the polymerization system.
[0102] In addition, the mixing method for forming the water-in-oil emulsion is not particularly limited, and any mixing method can be used, such as a method of mixing all the components at once, or a method of separately and uniformly dissolving oil-soluble components such as the oil-soluble monomer, surfactant, and oil-soluble polymerization initiator, and water-soluble components such as water and the water-soluble polymerization initiator, and then mixing the respective components.
[0103] Furthermore, the mixing device for forming the emulsion is not particularly limited, and any device such as a normal mixer, homogenizer, or high-pressure homogenizer can be used depending on the desired emulsion particle size. Furthermore, a so-called planetary mixing device can also be used in which the material to be treated is placed in a mixing container and rotated while revolving around the revolution axis while tilting the mixing container, thereby stirring and mixing the material to be treated.
[0104] In addition, there are no particular limitations on the mixing conditions, and the stirring rotation speed, stirring time, etc. can be set as desired according to the desired emulsion particle size. Note that, with the above planetary stirring device, water droplets in the W / O emulsion can be uniformly generated, and the average diameter can be set as desired within a wide range.
[0105] The polymerization conditions for the water-in-oil emulsion can be various, depending on the type of monomer and initiator, etc. For example, when azobisisobutyronitrile, benzoyl peroxide, potassium persulfate, etc. are used as the polymerization initiator, the polymerization can be carried out by heating in a sealed container under an inert atmosphere at a temperature of 30 to 100°C for 1 to 48 hours, and when hydrogen peroxide-ferrous chloride, sodium persulfate-acidic sodium sulfite, etc. are used as the polymerization initiator, the polymerization can be carried out in a sealed container under an inert atmosphere at a temperature of 0 to 30°C for 1 to 48 hours.
[0106] After the polymerization is completed, the contents are taken out and subjected to Soxhlet extraction with a solvent such as isopropanol to remove unreacted monomers and residual surfactants, thereby obtaining monolith A shown in the center diagram of Figure 2.
[0107] (Hydrolysis process) Next, the step of hydrolyzing the monolith A (crosslinked polymer) to obtain the absorbent A (hydrolysis step) will be described.
[0108] First, monolith A is immersed in dichloroethane containing zinc bromide and stirred at 40° C. for 24 hours, then contacted with methanol, 4% hydrochloric acid, 4% aqueous sodium hydroxide solution, and water in that order to carry out hydrolysis, and then dried to obtain a block-shaped absorbent A. Furthermore, this block-shaped absorbent A is crushed to a predetermined size to obtain a particulate absorbent A. The form of this absorbent A is not limited to particulate, and for example, it may be formed into a sheet during or after drying.
[0109] In addition, the method of hydrolysis of monolith A is not particularly limited, and various methods can be adopted. For example, aromatic solvents such as toluene and xylene, halogen-based solvents such as chloroform and dichloroethane, ether-based solvents such as tetrahydrofuran and isopropyl ether, amide-based solvents such as dimethylformamide and dimethylacetamide, alcohol-based solvents such as methanol and ethanol, carboxylic acid-based solvents such as acetic acid and propionic acid, or water as a solvent are contacted with a strong base such as sodium hydroxide, or a hydrohalic acid such as hydrochloric acid, a Bronsted acid such as sulfuric acid, nitric acid, trifluoroacetic acid, methanesulfonic acid, and p-toluenesulfonic acid, or a Lewis acid such as zinc bromide, aluminum chloride, aluminum bromide, titanium (IV) chloride, cerium chloride / sodium iodide, and magnesium iodide.
[0110] Furthermore, among the polymerization raw materials of the organic polymer that forms the hydrophilic continuous skeleton of the absorbent A, the (meth)acrylic acid ester is not particularly limited, but is preferably a C1 to C10 (i.e., carbon number 1 to 10) alkyl ester of (meth)acrylic acid, and more preferably a C4 (i.e., carbon number 4) alkyl ester of (meth)acrylic acid. Examples of C4 alkyl esters of (meth)acrylic acid include t-butyl (meth)acrylic acid ester, n-butyl (meth)acrylic acid ester, and iso-butyl (meth)acrylic acid ester.
[0111] Furthermore, the monomers used in the crosslinking polymerization may be only (meth)acrylic acid esters and divinylbenzene, or may contain, in addition to (meth)acrylic acid esters and divinylbenzene, other monomers other than (meth)acrylic acid esters and divinylbenzene. In the latter case, the other monomers are not particularly limited, but examples thereof include styrene, α-methylstyrene, vinyltoluene, vinylbenzyl chloride, glycidyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobutene, butadiene, isoprene, chloroprene, vinyl chloride, vinyl bromide, vinylidene chloride, tetrafluoroethylene, (meth)acrylonitrile, vinyl acetate, ethylene glycol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. The proportion of monomers other than (meth)acrylic acid ester and divinylbenzene in all monomers used in the crosslinking polymerization is preferably from 0 to 80 mol %, more preferably from 0 to 50 mol %.
[0112] The surfactant is not limited to the above-mentioned sorbitan monooleate, and may be any surfactant capable of forming a water-in-oil type (W / O) emulsion when the monomer for crosslinking polymerization is mixed with water. Examples of such surfactants include nonionic surfactants such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan trioleate, polyoxyethylene nonylphenyl ether, polyoxyethylene stearyl ether, and polyoxyethylene sorbitan monooleate, anionic surfactants such as potassium oleate, sodium dodecylbenzenesulfonate, and dioctyl sodium sulfosuccinate, cationic surfactants such as distearyl dimethyl ammonium chloride, and amphoteric surfactants such as lauryl dimethyl betaine. These surfactants may be used alone or in combination of two or more.
[0113] In addition, the polymerization initiator is preferably a compound that generates radicals by heat and light irradiation. Furthermore, the polymerization initiator may be water-soluble or oil-soluble, and examples thereof include azobis(4-methoxy-2,4-dimethylvaleronitrile), azobisisobutyronitrile, azobisdimethylvaleronitrile, azobiscyclohexanenitrile, azobiscyclohexanecarbonitrile, azobis(2-methylpropionamidine)dihydrochloride, benzoyl peroxide, potassium persulfate, ammonium persulfate, hydrogen peroxide-ferrous chloride, sodium persulfate-acidic sodium sulfite, and tetramethylthiuram disulfide. However, in some cases, there are systems in which polymerization proceeds only by heating or light irradiation without the addition of a polymerization initiator, and in such systems, the addition of a polymerization initiator is not necessary.
[0114] In addition to the light incontinence pads of the above-mentioned embodiments, the composite absorbent of the present invention can be applied to various sanitary products, such as pants-type disposable diapers, tape-type disposable diapers, sanitary napkins, absorbent liners, absorbent pads (e.g., bedsore pads and postpartum pads), absorbent sheets, breast milk pads, disposable diapers for pets, absorbent pads for pets, pet waste disposal sheets, wet sheets, wet tissues, cosmetic wipes, masks, etc. Therefore, the body fluids to be absorbed by the composite absorbent are liquids discharged from the wearer of the sanitary product, such as urine, sweat, feces, menstrual blood, vaginal discharge, breast milk, blood, exudates, etc.
[0115] Furthermore, the present invention is not limited to the above-described embodiments, and appropriate combinations, substitutions, modifications, etc. are possible without departing from the scope and spirit of the present invention. [Explanation of symbols]
[0116] 1. Light incontinence pads 2 Surface sheet 3 Back sheet 4. Composite absorber
Claims
1. 1. A composite absorbent for absorbing body fluids, comprising: The composite absorbent body includes a polymer absorbent having a hydrophilic continuous skeleton and continuous pores, and a superabsorbent polymer; The polymer absorbent is a hydrolyzate of a crosslinked polymer of a (meth)acrylic acid ester and divinylbenzene, which is a compound containing two or more vinyl groups in one molecule; a ratio of crosslinked polymer residues of the divinylbenzene in the organic polymer forming the hydrophilic continuous skeleton to all constitutional units is 0.1 to 30 mol %; The composite absorbent body as described above is characterized in that, when absorbing moisture, the polymer absorbent incorporates the moisture into the continuous skeleton and then into the continuous pores.
2. 2. The composite absorbent according to claim 1, wherein the volume of the expanded polymer absorbent is greater than the volume of the absorbed water at the water retention limit.
3. 3. The composite absorbent according to claim 1, wherein the polymer absorbent has a water absorption capacity of the interconnected pores greater than a water absorption capacity of the interconnected skeleton.
4. The composite absorbent according to any one of claims 1 to 3, characterized in that the mass ratio of the water absorption amount of the continuous pores to the water absorption amount of the continuous skeleton of the polymer absorbent is 60:40 to 95:
5.
5. The composite absorbent according to any one of claims 1 to 4, characterized in that the polymer absorbent has a relatively high absorption rate from immediately after the start of water absorption until it reaches its water retention limit, and has a relatively low absorption rate after the water retention limit.
6. The composite absorbent according to any one of claims 1 to 5, wherein the polymer absorbent is a monolithic absorbent.
7. A composite absorbent described in any one of claims 1 to 6, characterized in that it contains at least one -COONa group.
8. A sanitary product comprising the composite absorbent body according to any one of claims 1 to 7.
Citation Information
Patent Citations
Absorbent material structures, methods of manufacture and uses thereof, and disposable absorbent articles containing such material structures
JP2002505702A
Particle-agglomerated type monolithic organic porous article, its manufacturing process, particle-agglomerated type monolithic organic porous ion exchanger and chemical filter
JP2009007550A
Absorbent article
JP2017164356A
Absorbent foam materials for aqueous body fluids and absorbent articles containing such materials
JP3231320B2
Water absorbing resin particles, method for manufacturing water absorbing resin particles, absorption body, absorptive article, and water-sealing material
WO2013018571A1