Low hydrogen type covered metal arc welding electrode
A low-hydrogen coated arc welding rod with optimized metal carbonate, fluoride, and oxide ratios stabilizes arcs and improves toughness and bead shape, addressing cost and performance issues of existing rods, ensuring effective welding across positions and temperatures.
Patent Information
- Application Number
- JP2021041843
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-15
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2041-03-15
AI Technical Summary
Existing low-hydrogen coated arc welding rods face issues with high costs due to the inclusion of expensive metals like Ni, unstable arcs, particularly with AC power sources, and poor weld metal toughness, especially at low temperatures, along with challenges in maintaining good bead shape and welding workability across various positions.
A low-hydrogen coated arc welding rod composition comprising specific ratios of metal carbonates, metal fluorides, oxides, and other components, excluding Ni, to stabilize the arc, improve toughness, and ensure good bead shape and workability, even at low temperatures, using either AC or DC power sources.
The welding rod achieves good weld metal toughness at -40°C, stable arcs, and excellent welding workability with a good bead shape, reducing costs by omitting Ni and enhancing productivity through controlled component ratios.
Smart Images

Figure 0007580312000004 
Figure 0007580312000005 
Figure 0007580312000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a low hydrogen-based covered electrode. [Background technology]
[0002] In recent years, as welded structures such as buildings, bridges, and ships have become larger, steel plates of 490 MPa class high tensile steel or higher have been used, and there is an increasing demand for improved low-temperature toughness of weld metal for pipelines and marine structures, which are used in low-temperature environments.
[0003] Low-hydrogen covered metal arc welding electrodes, whose main components are metal carbonate and metal fluoride, are easier to use for first-layer back-sand welding in all positions compared to non-low-hydrogen covered metal arc welding electrodes such as ilmenite-based covered metal arc welding electrodes and high-titanium oxide-based covered metal arc welding electrodes. The molten pool is shielded by CO2 gas from a gas generator, and the mechanical performance is excellent. The amount of diffusible hydrogen in the deposited metal is small, giving it excellent cracking resistance. For these reasons, low-hydrogen covered metal arc welding electrodes, which are primarily composed of metal carbonate and metal fluoride, are often used for first-layer back-sand welding in all positions, such as for circumferential welding of steel pipes. In order to form a uranami bead, low-hydrogen covered electrodes for uranami welding contain a higher SiO2 content in the coating than ordinary low-hydrogen electrodes. However, since SiO2 lowers the basicity of the molten slag, a relatively large amount of oxide remains in the weld metal, which tends to reduce the toughness of the weld metal.
[0004] As an example of a low-hydrogen covered metal arc welding electrode that can obtain a weld metal with good toughness, Patent Document 1 discloses a low-hydrogen covered metal arc welding electrode that ensures the toughness of the weld metal by adjusting the amounts of Si, Mn, Ni, Ti, and B in the coating material to appropriate amounts. Moreover, Patent Document 2 discloses a low-hydrogen covered metal arc welding rod that has improved toughness when an appropriate amount of Ni is contained therein. Furthermore, Patent Document 3 discloses a low-hydrogen covered metal arc welding rod in which the core wire contains 50 ppm or less N and appropriate amounts of Mn, Ni, Ti, and B, thereby promoting deoxidation and strengthening the ferritic structure and ensuring the low-temperature toughness of the weld metal. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-203253 A [Patent Document 2] Japanese Patent Application Publication No. 4-367393 [Patent Document 3] Japanese Patent Application Laid-open No. 63-144895 Summary of the Invention [Problem to be solved by the invention]
[0006] The low-hydrogen covered metal arc welding rod described in Patent Document 1 reduces the oxygen content of the weld metal with Si and Mn, and refines the microstructure with Ni, Ti, and B to improve low-temperature toughness, but on the other hand, the fluidity of the molten slag deteriorates, and depending on the welding position, the bead shape of the uranami welding tends to become distorted. In addition, Ni is expensive, and an increase in the cost of the welding rod is unavoidable. The low-hydrogen covered metal arc welding rod described in Patent Document 2 contains metallic Ni like the low-hydrogen covered metal arc welding rod in Patent Document 1, so the cost of the welding rod increases. In addition, depending on the particle size composition of the Ni powder, the coating of the welding rod is likely to crack when drying. The low-hydrogen covered metal arc welding rod described in Patent Document 3 does not contain CaO, so the arc becomes unstable and arc interruption is likely to occur, especially when an AC power source is used. In addition, the welding rod described in Patent Document 3 also contains Ni, which increases the cost.
[0007] An object of the present disclosure is to provide a low-hydrogen covered metal arc welding rod that does not contain Ni and that has excellent welding workability, such as producing a weld metal with good toughness at a low temperature of -40°C, producing a stable arc even at a low current, and producing a good uranami weld bead shape, regardless of whether an AC or DC power source is used for uranami welding in all positions, such as circumferential welding of steel pipes. [Means for solving the problem]
[0008] The gist of the present disclosure for solving the above problems is as follows. <1> The steel core wire includes a coating material that coats the steel core wire, The mass ratio of the coating material to the total mass of the welding rod is 25% or more and 35% or less, The coating agent is, in mass % based on the total mass of the coating agent, C: 0.01-0.20%, Total metal carbonates: 32-52%, Total metal fluorides: 4-14%, Total TiO2 equivalent value of Ti oxides: 3~10%, Total of silicon oxides converted into SiO2: 8-22% Total Al oxides converted into Al2O3: 0.5-3.0% Total Ca oxides converted into CaO: 0.5-3.0% Total of metal Si and Si alloy converted into Si: 2.0 to 6.0% Total of metallic Mn and Mn alloy converted into Mn: 3.0 to 6.0% The sum of the B-converted values of B alloys and B oxides: 0.05 to 0.25%, and A low-hydrogen covered metal arc welding electrode containing 1.0 to 3.5% of sodium oxide converted into Na2O and 1.0 to 3.5% of potassium oxide converted into K2O, with the remainder being a coating material, Fe and impurities. <2> The coating agent contains, in mass % relative to the total mass of the coating agent, one or both of the following (A) and (B) in place of a portion of the components constituting the coating agent: <1> The low hydrogen type covered metal arc welding rod according to claim 1. (A) The total of the Al-equivalent value of metallic Al and Al alloys and the Mg-equivalent value of metallic Mg and Mg alloys: 3.0% or less (B) The total of the Ti-equivalent value of metallic Ti and Ti alloys: 2.5% or less Effect of the Invention
[0009] According to the present disclosure, a low-hydrogen covered metal arc welding rod that does not contain Ni is provided, which has excellent welding workability, such as producing a weld metal with good toughness at a low temperature of -40°C, producing a stable arc even at a low current, and producing a good uranami weld bead shape, regardless of whether an AC or DC power source is used for uranami welding in all positions, such as circumferential welding of steel pipes. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a schematic diagram showing the shape of a steel plate used for groove welding in the examples. [Diagram 2] FIG. 2 is a schematic diagram showing the bead height and bead width on the bead surface immediately after reverse welding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment that is an example of the present disclosure will be described. In this specification, when a numerical range is expressed using "~", unless "more than" or "less than" is added to the numerical values before and after "~", it means a range that includes these numerical values as the lower and upper limits. In addition, when "more than" or "less than" is added to the numerical values before and after "~", it means a range that does not include these numerical values as the lower and upper limits. In the present specification, the upper limit of a certain numerical range may be replaced by the upper limit of another numerical range, or may be replaced by a value shown in an example. The lower limit of a certain numerical range may be replaced by the lower limit of another numerical range, or may be replaced by a value shown in an example. With respect to the content, "%" means "mass %" unless otherwise specified. In addition, when the content (%) is specified with only an upper limit as "not more than __%" without specifying a lower limit, it means that the content may be in the range from more than 0% to the upper limit.
[0012] As a result of intensive research into improving the low-temperature toughness of the weld metal of low-hydrogen covered metal arc welding electrodes, the inventors have found that the low-temperature toughness of the weld metal can be improved by including B alloy and B oxide in the coating material, and have completed the present invention through further investigation. The details are described below.
[0013] Usually, low-hydrogen covered metal arc welding rods contain Si, Mn, and strong deoxidizers such as Al and Mg, in order to secure a good weld metal at low temperatures. Among these, Mn dissolves in the weld metal, increasing the carbon equivalent, making the ferrite grains finer, and contributing to improving toughness. Therefore, the inventors investigated whether the Mn content in the coating material could be increased stepwise to increase the yield of Mn in the weld metal and improve low-temperature toughness, but the results showed that the low-temperature toughness was not improved, and rather decreased in the reheated part. One of the factors that deteriorate the reheated part of the weld metal is island martensite. Even in the case of adding Mn, the low-temperature toughness was not improved because it affected the formation of island martensite to a certain extent. In addition, the increase in the Mn content in the coating material lowers the melting point of the molten slag, which causes the shape of the uranami weld bead to become distorted and makes it easier for the slag to be peeled off.
[0014] The present inventors have studied alloy elements effective for low-temperature toughness, and have found that by setting the content of B alloy and B oxide to an appropriate amount, the formation of acicular ferrite in the weld metal structure is promoted, the crystal grains are refined, and low-temperature toughness can be improved. In addition, since the content of B alloy and B oxide is small, it does not significantly affect the uranami welding workability, and good welding workability can be maintained. In addition to the above, it has been found that the low-temperature toughness can be further improved by adding an appropriate amount of strong deoxidizers of Al, Mg, and Ti in addition to the deoxidizers of Si and Mn.
[0015] Regarding welding workability, it was found that the arc spray and arc stability can be improved by adding appropriate amounts of C, Ti oxide, Ca oxide, Na oxide, and K oxide. It was also found that the slag encapsulation and slag removability can be improved by adding appropriate amounts of metal fluoride and Si oxide, and the bead shape can be improved by adding appropriate amounts of Ti oxide, Si oxide, and Al oxide.
[0016] They also discovered that welding defects such as blowholes can be prevented by adding appropriate amounts of metal carbonates, metal fluorides, and deoxidizers such as Si and Mn, which react with the oxygen in the molten pool and sufficiently deoxidize it.
[0017] <Low hydrogen type covered metal arc welding electrode> The low-hydrogen covered metal arc welding rod according to the present disclosure (which may be referred to as a "covered metal arc welding rod" or simply a "welding rod" in the present disclosure) includes a steel core wire and a coating material that coats the steel core wire.
[0018] (steel core wire) The steel core wire may be a steel core wire used in a known low-hydrogen covered metal arc welding rod. For example, it is preferable to use a core wire manufactured from wire of SWRY11 specified in JIS G 3503:2006.
[0019] (Coating material) The coating material that coats the outer surface of the steel core wire is, in mass %, based on the total mass of the coating material. C: 0.01-0.20%, Total metal carbonates: 32-52%, Total metal fluorides: 4-14%, Total TiO2 equivalent value of Ti oxides: 3~10%, Total of silicon oxides converted into SiO2: 8-22% Total Al oxides converted into Al2O3: 0.5-3.0% Total Ca oxides converted into CaO: 0.5-3.0% Total of metal Si and Si alloy converted into Si: 2.0 to 6.0% Total of metallic Mn and Mn alloy converted into Mn: 3.0 to 6.0% The sum of the B-converted values of B alloys and B oxides: 0.05 to 0.25%, and The total of Na oxides converted into Na2O and K oxides converted into K2O is 1.0 to 3.5%, with the remainder consisting of coating agents, Fe, and impurities. The composition of the coating material of the covered electrode according to the present disclosure and the reasons for limiting the composition of the coating material will be described in detail below. The content of each component is expressed as mass% relative to the total mass of the coating material, and when expressing the mass%, it is simply written as %.
[0020] In addition, with regard to the components constituting the coating material of the welding rod according to the present disclosure, for example, "total of metal carbonates" may include only one type of metal carbonate, or may include two or more types, and when two or more types are included, it means the total content thereof. In addition, for example, "total of Mn-equivalent values of metal Mn and Mn alloy: 3.0-6.0%" means that only metal Mn may be included, only Mn alloy may be included, metal Mn and Mn alloy may be included, and when Mn alloy is included, it may include one or two or more types of Mn alloy, but in any case, the total of Mn-equivalent values is 3.0-6.0%. The same applies to components other than metal Mn and Mn alloy. Regarding oxides, for example, "the TiO2 equivalent value of Ti oxide" means a value calculated by assuming that all Ti contained as Ti oxide is contained as TiO2, including Ti oxides other than TiO2.
[0021] [C: 0.01~0.20%] C is contained in metal powder and alloy powder contained in the coating agent, and has the effect of ensuring the arc blow strength when welding is performed with AC and DC power sources. It is also an important component for ensuring the strength of the weld metal. If C is less than 0.01%, the arc blow is weak, the penetration into the base metal is insufficient, and the quality of the welded part is reduced. In addition, the strength of the weld metal is reduced. On the other hand, if C exceeds 0.20%, the arc blow strength becomes excessive, making undercuts more likely to occur. In addition, the strength of the weld metal becomes excessive, and the low-temperature toughness is reduced. Therefore, C is set to 0.01 to 0.20%.
[0022] [Total metal carbonates: 32-52%] Metal carbonates are contained as magnesium carbonate, calcium carbonate, barium carbonate, manganese carbonate, etc., and have the effect of protecting against gas components such as oxygen, nitrogen, and hydrogen that decompose in the arc atmosphere to generate carbon dioxide gas and invade the molten pool, thereby preventing welding defects such as pits and blow holes. If the total of metal carbonates is less than 32%, the shielding effect of the molten pool is insufficient, and welding defects such as pits and blow holes are likely to occur. On the other hand, if the total of metal carbonates exceeds 52%, the arc blowing becomes weak and the arc in the low current range becomes unstable due to the endothermic reaction during carbonate decomposition, especially when an AC power source is used, making it difficult to form a good back bead. Therefore, the total of metal carbonates is 32 to 52%.
[0023] [Total metal fluorides: 4-14%] Metal fluorides are added as fluorite, magnesium fluoride, aluminum fluoride, etc., and adjust the fluidity of the molten slag, and because the vapor pressure of fluorine is high, they have the effect of protecting the molten pool from gas components such as oxygen, nitrogen, and hydrogen. If the total amount of metal fluorides is less than 4%, the shielding ability of the molten pool due to fluorine deteriorates, and welding defects such as pits and blowholes are likely to occur. On the other hand, if the total amount of metal fluorides exceeds 14%, the melting point of the molten slag decreases and the slag removability becomes poor. Therefore, the total amount of metal fluorides is set to 4 to 14%.
[0024] [Total of Ti oxides converted into TiO2: 3~10%] Ti oxides are contained as rutile, titanium oxide, titanium slag, ilmenite, etc., and act as an arc stabilizer and slag viscosity adjuster, stabilizing the arc and improving the bead shape. If the total of Ti oxides in terms of TiO2 is less than 3%, the arc becomes unstable and the bead shape becomes poor. On the other hand, if the total of Ti oxides in terms of TiO2 exceeds 10%, the slag becomes dense and the slag removability becomes poor. Therefore, the total of Ti oxides in terms of TiO2 is set to 3-10%.
[0025] [Total of silicon oxides converted into SiO2: 8-22%] Silicon oxides are contained in the form of silica sand, feldspar, wollastonite, water glass, etc., and have the effect of adjusting the viscosity of the slag and improving the encapsulation of the slag. If the total of the SiO2-equivalent values of silicon oxides is less than 8%, the viscosity of the molten slag is insufficient, making it difficult to form a uranami welding bead and resulting in a poor bead shape. On the other hand, if the total of the SiO2-equivalent values of silicon oxides exceeds 22%, the viscosity of the slag becomes excessive, and the distance between the molten pool and the molten slag becomes short, resulting in poor encapsulation of the slag. Therefore, the total of the SiO2-equivalent values of silicon oxides is set to 8-22%.
[0026] [Total of Al oxides converted into Al2O3: 0.5-3.0%] Aluminum oxides are contained as alumina, feldspar, mica, etc., and have the effect of adjusting the viscosity of the molten slag and improving the bead shape. If the total of the aluminum oxides in terms of Al2O3 is less than 0.5%, the viscosity of the slag is insufficient, resulting in poor bead shape in the vertical and upward positions. On the other hand, if the total of the aluminum oxides in terms of Al2O3 exceeds 3.0%, the viscosity of the molten slag becomes excessive, and the distance between the molten pool and the molten slag becomes short, resulting in poor slag encapsulation. Therefore, the total of the aluminum oxides in terms of Al2O3 is set to 0.5-3.0%.
[0027] [Total of Ca oxides converted into CaO: 0.5-3.0%] Ca oxides are contained as wollastonite, etc., and are effective as an arc stabilizer. If the total of Ca oxides converted into CaO is less than 0.5%, the arc becomes unstable and arc interruption is likely to occur, especially when an AC power source is used. On the other hand, if the total of Ca oxides converted into CaO exceeds 3.0%, the melting point of the molten slag increases and the encapsulation of the slag becomes poor. Therefore, the total of Ca oxides converted into CaO is set to 0.5-3.0%.
[0028] [Total of Si-equivalent value of metal Si and Si alloy: 2.0~6.0%] Si is contained as Fe-Si, metal Si, Fe-Si-Mn, etc., and is added for the purpose of deoxidizing oxygen that has entered the molten pool. If the total of the Si-equivalent values of metal Si and Si alloy is less than 2.0%, deoxidation is insufficient, and welding defects such as pits and blowholes are likely to occur in the weld metal. On the other hand, if the total of the Si-equivalent values of metal Si and Si alloy exceeds 6.0%, island martensite is likely to be generated with an increase in Si, especially in the reheated part of multi-layer weld metal, and toughness is reduced. Therefore, the total of the Si-equivalent values of metal Si and Si alloy is set to 2.0 to 6.0%.
[0029] [Total of metal Mn and Mn alloy converted into Mn: 3.0-6.0%] Mn is contained as metal Mn, Fe-Mn alloy powder, etc., and acts as a deoxidizer, and has the effect of improving the strength and toughness of the weld metal. If the total of the Mn-equivalent values of metal Mn and Mn alloy is less than 3.0%, deoxidation is insufficient, the strength and toughness of the weld metal are reduced, and welding defects such as pits and blowholes are likely to occur. On the other hand, if the total of the Mn-equivalent values of metal Mn and Mn alloy exceeds 6.0%, the strength of the weld metal becomes excessively high. Therefore, the total of the Mn-equivalent values of metal Mn and Mn alloy is set to 3.0 to 6.0%.
[0030] [Total of B alloy and B oxide converted to B: 0.05~0.25%] B is contained in alloys and oxides such as Fe-B, borax, and colemanite, and has the effect of forming acicular ferrite by dissolving in the weld metal and improving toughness. If the total B equivalent value of B alloys and B oxides is less than 0.05%, the amount of B dissolved in the weld metal is insufficient, and the toughness is reduced. On the other hand, if the total B equivalent value of B alloys and B oxides exceeds 0.25%, B segregates in the final solidification region of the weld metal, making it easier for cracks to occur. Therefore, the total B equivalent value of B alloys and B oxides is set to 0.05 to 0.25%.
[0031] [The total of Na oxide converted into Na2O and K oxide converted into K2O is 1.0-3.5%] Na oxide and K oxide are contained as sodium silicate and potassium silicate in water glass, potassium feldspar, potassium glass and soda feldspar, etc., and have the effect of stabilizing the arc and reducing the amount of spatter generation. If the total of the Na2O equivalent value of Na oxide and the K2O equivalent value of K oxide is less than 1%, the arc becomes unstable and the amount of spatter generation increases. On the other hand, if the total of the Na2O equivalent value of Na oxide and the K2O equivalent value of K oxide exceeds 3.5%, the arc blow becomes excessively strong, undercutting is likely to occur, and the bead shape becomes poor. Therefore, the total of the Na2O equivalent value of Na oxide and the K2O equivalent value of K oxide is 1.0 to 3.5%.
[0032] [Total of Al metal and Al alloys converted into Al, and Mg metal and Mg alloys converted into Mg: 3.0% or less] Al is contained by alloy powder such as metal Al, Fe-Al, Al-Mg, etc., and Mg is contained and added by alloy powder such as metal Mg, Al-Mg, Ni-Mg, etc. These act as strong deoxidizers, and have the effect of preventing welding defects such as pits and blowholes, and further improving the toughness of the weld metal. Therefore, the coating may contain metal Al, Al alloy, metal Mg, and / or Mg alloy. However, if the total of the Al equivalent value of metal Al and Al alloy and the Mg equivalent value of metal Mg and Mg alloy exceeds 3.0%, Al and Mg react with water in the binder during the production of the welding rod, and drying cracks are likely to occur. Therefore, one or more of metal Al, Al alloy, metal Mg, and Mg alloy are set to be 3.0% or less in terms of the total of the Al equivalent value and the Mg equivalent value, that is, the total of the Al equivalent value of metal Al and Al alloy and the Mg equivalent value of metal Mg and Mg alloy is set to be 3.0% or less. In order to prevent welding defects such as blowholes and to obtain the effect of further improving the toughness of the weld metal, it is preferable that the total of the Al converted value of metallic Al and Al alloys and the Mg converted value of metallic Mg and Mg alloys be 0.4% or more.
[0033] [Total of Ti-equivalent value of metallic Ti and Ti alloys: 2.5% or less] Ti is contained as metallic Ti, alloy powder such as Fe-Ti, etc., and acts as a strong deoxidizer to prevent welding defects such as blowholes. It also has the effect of further improving the toughness of the weld metal. For this reason, the coating material may contain metallic Ti and / or a Ti alloy. However, if the total of metallic Ti and Ti alloy exceeds 2.5% in terms of Ti, inclusions such as TiC and TiN are generated in the weld metal, lowering the toughness. Therefore, the total of metallic Ti and Ti alloy is set to 2.5% or less in terms of Ti. In order to prevent welding defects such as blowholes and to obtain the effect of further improving the toughness of the weld metal, it is preferable that the total of metallic Ti and Ti alloy is set to 0.10% or more in terms of Ti.
[0034] [others] The coating material for the welding rod according to the present disclosure is a coating material other than the above components. outfit Contains agents, Fe, and impurities. coating outfitFrom the viewpoint of productivity, the coating agent is included, and examples thereof include sodium alginate and hectorite. outfit The content of the agent is, for example, 0.1 to 3.0%. Iron is found in iron alloys such as Fe-Si, Fe-Mn, Fe-Si-Mn, Fe-B, Fe-Al, and Fe-Ti. Impurities are components contained in raw materials or components mixed in during the manufacturing process, but are not intentionally contained in the coating. Impurities contained in the coating include organic matter and P and S contained in alloy powder. The total amount of impurities is preferably 2% or less, and more preferably 1% or less.
[0035] [Ratio of coating agent, etc.] From the viewpoint of obtaining good mechanical performance by uranami welding using the welding rod according to the present disclosure, the mass ratio of the coating material to the total mass of the welding rod is set to 25 to 35%. The mass ratio of the coating material to the total mass of the welding rod (coverage rate: %) is a value calculated by the following formula. Coverage % = coating mass / total mass of welding rod x 100
[0036] [Welded metal] The weld metal formed using the welding rod according to the present disclosure preferably has a tensile strength of 520 to 620 MPa and a Charpy absorbed energy of 40 J or more at −40° C. in the Charpy impact test specified in JIS Z 3111:2005.
[0037] (Tensile strength) A weld metal test specimen produced using the welding rod according to the present disclosure can have a tensile strength of the weld metal in the range of 520 to 620 MPa. A high joint strength can be ensured by setting the tensile strength of the weld metal to 520 MPa or more. On the other hand, a tensile strength of the weld metal to 620 MPa or less can suppress the occurrence of cracks in the weld metal formed by uranami welding. The tensile strength of the weld metal is measured by a tensile test using an A2 test piece in accordance with JIS Z 3111:2005. Specific measurement methods, such as the positions at which the sample pieces are taken, will be described in the examples.
[0038] (Low temperature toughness) The weld metal specimens produced using the welding rods according to the present disclosure can have an average Charpy absorbed energy of the weld metal at -40°C of 40 J or more. Preferably, it is 60 J or more, and more preferably, it is 80 J or more. The Charpy impact test conforms to JIS Z 3111:2005, and is repeated three times at a test temperature of -40°C, and the average absorbed energy (arithmetic mean) is obtained. Specific measurement methods, such as the positions at which the sample pieces are taken, will be described in the Examples.
[0039] (Welding defects) It is preferable that the weld metal specimens produced using the welding rod according to the present disclosure have suppressed weld defects such as blowholes. Specifically, when a radiographic photograph of the weld metal is used to determine which of the first to fourth types of defects in "Annex 4, Table 1, Types of Defects" corresponds to a defect according to JIS Z 3104:1995 "Radiation Transmission Testing Method for Steel Welded Joints," and defects in "6. Classification of Defects" are divided into types 1 to 4, it is preferable that the defect is classified into type 1 or type 2, and more preferably type 1.
[0040] [Welded joint] The welding rod according to the present disclosure is used for shielded arc welding of steel materials. For example, when performing uranami welding of steel materials such as steel pipes and steel plates, by performing shielded arc welding using the welding rod according to the present disclosure, a welded joint having excellent welding workability, strength of the weld metal, and toughness at low temperatures can be produced. Note that normal conditions can be adopted except for using the welding rod according to the present disclosure. The welding workability of the welding rod according to the present disclosure is evaluated by producing a welded joint and performing uranami welding in a vertical upward advance position.
[0041] (Arc spraying) The welding rod according to the present disclosure preferably provides a consistent arc blow with moderate strength.
[0042] (Arc Stability) In the welding rod according to the present disclosure, it is preferable that the arc is stable and no arc interruption occurs.
[0043] (Bead shape) The welded joint produced using the welding rod according to the present disclosure preferably has a bead shape excellent in uniformity of the weld metal reinforcement height and bead width. Specifically, on the bead surface of the first layer immediately after uranami welding of the weld metal, when a portion having a reinforcement height of 1 to 3 mm and a bead width of 6 to 8 mm is defined as a good bead portion and a portion other than the good bead portion is defined as a defective bead portion, it is preferable that the defective bead portion is 20% or less of the total weld length.
[0044] (Slag encapsulation) It is preferable that the welding rod according to the present disclosure has high uniformity of slag encapsulation and can suppress the intrusion of molten slag into the molten pool during welding.
[0045] (Slag removability) In the welding rod according to the present disclosure, it is preferable that the solidified slag after welding is easily peeled off when it is removed. EXAMPLES
[0046] The effects of the present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to the following examples.
[0047] <Manufacture of covered electrodes> Various prototype welding rods were produced by applying a coating agent having the composition shown in Tables 1 and 2 to a steel core wire of SWRY11 specified in JIS G 3503:2006 (C: 0.07 mass%, Si: 0.10 mass%, Mn: 0.45 mass%, P: 0.010 mass%, S: 0.003 mass% based on the total mass of the steel core wire) having a diameter of 3.2 mm and a length of 400 mm, at a coverage rate of 25 to 35 mass% based on the total mass of the welding rod, and then firing at 400°C. Note that the notation "-" for the coating agent components in Tables 1 and 2 means that the component is not intentionally included. Also, underlines indicate that the component is outside the scope of this disclosure. The productivity, welding workability, welding defects and mechanical properties of the produced welding rods were investigated.
[0048] [Table 1]
[0049] [Table 2]
[0050] [Productivity] When manufacturing the welding rod, drying cracks may occur, which are cracks that form on the coating surface after the welding rod is dried. Drying cracks have a negative effect on welding workability, such as preventing the protective tube from being formed uniformly during welding and causing the arc to deflect. Productivity was evaluated by checking the presence or absence of cracks in the coating after drying when the welding rod was manufactured. A was given for no drying cracks, B for individual drying cracks smaller than 1 mm in size, and C for individual drying cracks 1 mm or larger in size, with A and B being considered pass and C being considered fail.
[0051] <Production of weld metal test specimens> The weld metal test specimens were prepared using 12 mm thick JIS G 3106:2017 SM490A steel plate and DC in accordance with JIS Z 3211:2008. The mechanical properties were evaluated by taking specimens for tensile tests (A2 type) and Charpy impact tests to investigate the mechanical properties. Weld defects (blowholes, etc.) were evaluated by X-ray transmission tests in accordance with JIS Z 3104:1995.
[0052] <Welded joint manufacturing> As shown in Figure 1, the weld joint was made by butting together steel plates 12A and 12B of SS400 conforming to JIS G 3101:2017, having a plate thickness of 9 mm, width of 125 mm, length of 160 mm, and a groove angle of 30° on one side, with a gap of 2 mm and a groove shape 14 of 1.5 mm on the root face. The evaluation of welding workability was carried out using various prototype welding rods in the vertical upward welding position, which is the most problematic position for welding workability in all positions, and using alternating current (hereinafter referred to as AC) and direct current (hereinafter referred to as DC) welding power sources to perform back-strip welding with a welding current of 85A.
[0053] [Welding workability] (Arc spraying) After welding, the occurrence of undercuts at the toes of the welds was checked. If there was no undercut of 0.5 mm or more, it was rated as good, and if even one undercut of 0.5 mm or more occurred, it was rated as bad.
[0054] (Arc Stability) If the arc was stable during welding and did not disappear, it was rated as good, and if the arc disappeared even once, it was rated as poor.
[0055] (Bead shape) The bead shape of the above-mentioned uranami welding was visually evaluated. The bead shape of the weld metal was evaluated according to the following criteria.
[0056] As shown in Figure 2, on the bead surface immediately after uranami welding (the surface opposite the uranami bead), if the portion with the reinforcement height H of 1 to 3 mm and the bead width W of 6 to 8 mm is considered good, and the remaining portion is considered defective, then a portion with less than 20% of the defective portion relative to the total weld length is considered good, and a portion with more than 20% is considered defective.
[0057] (Slag encapsulation) A good welding result was obtained when the molten slag did not enter the weld pool during welding, and a bad welding result was obtained when the molten slag entered the weld pool and the arc direction was disturbed.
[0058] (Slag removability) After welding, the solidified slag on the uranami weld surface was struck with a chipping hammer (total length 300 mm, weight 350 g) by lightly swinging it down in an arc around the handle. If the slag cracked and could then be easily removed, it was rated as good, and if the slag did not crack, it was rated as poor.
[0059] [Welding defects] Specifically, defects in the weld metal were judged according to JIS Z 3104:1995 "Radiation Testing Method for Steel Welded Joints." From the radiographic photographs, it was determined which of the defects fell under "Annex 4 Table 1: Types of Defects," from Type 1 to Type 4, and defects in "6. Classification of Defects" were classified into Classes 1 to 4. Of these, Class 1 was A, Class 2 was B, Class 3, and Class 4 was C, with A and B being considered pass and C being a fail.
[0060] [Mechanical properties] To evaluate the mechanical properties, 12 mm thick steel plate of JIS G 3106:2017 SM490A was used, and weld metal test specimens were prepared by DC in accordance with JIS Z 3211:2008. Test specimens were then taken for tensile tests (A2 type) and Charpy impact tests to investigate the mechanical performance. In the tensile test, a tensile strength of 520 to 620 MPa was considered good, and in the Charpy impact test, an average absorbed energy of 40 J or more after three repeated tests at a test temperature of -40°C was considered good. The criteria for low temperature toughness were as follows: A:50J or more B: 40J or more but less than 50J C: Less than 40J
[0061] These analysis results and survey findings are summarized in Table 3.
[0062] [Table 3]
[0063] In Tables 1, 2 and 3, welding rods No. 1 to No. 14 are examples of the present invention, and welding rods No. 15, No. 16, No. 18 to No. 20, and No. 22 to No. 28 are comparative examples. In welding rods No. 1 to No. 14, which are examples of the present invention, the coating agent contains appropriate amounts of C, the total of metal carbonates, the total of metal fluorides, the total of TiO2 equivalent values, the total of SiO2 equivalent values, the total of Al2O3 equivalent values, the total of CaO equivalent values, the total of Si equivalent values, the total of Mn equivalent values, the total of B equivalent values, the total of Na2O equivalent values and the total of K2O equivalent values, so that the productivity is good, the welding workability is good in terms of arc spraying, the arc is stable, the bead shape is good, and the slag encapsulation and slag detachment are good. In addition, there was no occurrence of blowholes in the deposited metal in the deposited metal test, and the tensile strength and absorbed energy of the deposited metal were both good. In addition, since welding rods No. 1, No. 2, No. 3, No. 8 and No. 14 have an appropriate amount of Al-equivalent value and Mg-equivalent value or Ti-equivalent value added, the absorbed energy of the deposited metal was 60 J or more. Furthermore, since welding rods No. 4, No. 7, and No. 9 contain appropriate amounts of Al-equivalent value, Mg-equivalent value, and Ti-equivalent value, the absorbed energy of the deposited metal was 80 J or more, which was an extremely satisfactory result. For welding rods No. 6 and No. 10, the total of the Al-equivalent value and the Mg-equivalent value or the total of the Ti-equivalent value was added in an appropriate amount, but since the amount added was small, the effect of increasing the absorbed energy of the weld metal to 60 J or more was not obtained.
[0064] The welding rod No. 15 in the comparative example had a high C content, which caused the arc to blow too strongly and undercut. In addition, the tensile strength of the weld metal was high and the absorbed energy was low. Furthermore, the total Al2O3 equivalent value was high, so the encapsulation of the slag was poor. Welding rod No. 16 had a low carbon content, which resulted in weak arc blowing and poor penetration. Also, because it had a low carbon content, the tensile strength of the weld metal was low. Furthermore, because the total TiO2 equivalent value was low, the coating had poor conductivity, which resulted in an unstable arc and poor bead shape. Welding rod No. 18 had a high total metal carbonate content, which resulted in a weak arc and poor bead shape when an AC power source was used. In addition, the total Al and Mg converted values were high, so the rod reacted with moisture during manufacturing, causing drying cracks. Welding rod No. 19 had a low total amount of metal carbonate, which resulted in insufficient shielding of the molten pool and the occurrence of blowholes in the deposited metal. In addition, the total amount of CaO was high, which resulted in poor encapsulation of the slag. Welding rod No. 20 had a high total metal fluoride content, which lowered the melting point of the molten slag, and especially when using DC, the slag removability was poor. Also, because the total Mn equivalent value was low, the deoxidation of the molten metal was insufficient, which caused blowholes. Furthermore, because the total Mn equivalent value was low, the solid solution strengthening of the deposited metal was insufficient, which resulted in low tensile strength and low absorbed energy. Welding rod No. 22 had a high total TiO2 equivalent value, which resulted in dense slag and poor slag removability. Also, because it had a high total B equivalent value, B segregated at the final solidification point, causing hot cracking. Welding rod No. 23 had a high total SiO2 equivalent value, which resulted in high viscosity of the molten slag and poor encapsulation of the slag. Also, because the total Ti equivalent value was high, TiC, TiN, etc. were precipitated in the weld metal, resulting in low absorbed energy. Welding rod No. 24 had a low total SiO2 equivalent value, which made it difficult to form a back-strip weld bead, resulting in a poor bead shape. Also, the total of the Na2O equivalent value and the K2O equivalent value was low, resulting in poor arc stability. The welding rod No. 25 had a low total Al2O3 equivalent value, so the molten slag did not have sufficient viscosity, resulting in a poor bead shape. Also, the total Na2O equivalent value and K2O equivalent value were high, so the arc was blown excessively, resulting in undercut. Welding rod No. 26 had a low total CaO equivalent value, so the arc was unstable with AC. Also, the total Mn equivalent value was high, so the tensile strength was high. Welding rod No. 27 had a high total SiO2 equivalent value, which resulted in high viscosity of the molten slag and poor encapsulation of the slag. Also, because it had a high total Si equivalent value, island martensite was formed in the reheated part of the weld metal, resulting in low absorbed energy. Welding rod No. 28 had a low total TiO2 equivalent value, which resulted in poor coating conductivity, an unstable arc, and poor bead shape. Also, because the total B equivalent value was low, sufficient acicular ferrite was not obtained in the deposited metal, resulting in low absorbed energy. [Explanation of symbols]
[0065] 12A,12B steel plate 14 Groove opening 16A First layer (Uranami welding)
Claims
1. The steel core wire includes a coating material that coats the steel core wire, The mass ratio of the coating material to the total mass of the welding rod is 25% or more and 35% or less, The coating agent is, in mass % based on the total mass of the coating agent, C: 0.01-0.20%, Sum of metal carbonates: 32-52%, Total metal fluorides: 4-14%, Ti oxide TiO 2 Total conversion value: 3-10%, Silicon oxide SiO 2 Total conversion value: 8-22%, Al oxide Al 2 O 3 Total conversion value: 0.5-3.0%, Sum of Ca oxides converted into CaO: 0.5 to 3.0%, Sum of metal Si and Si alloy converted into Si: 2.0 to 6.0%, Sum of metal Mn and Mn alloy converted into Mn: 3.0 to 6.0%, The sum of the B-converted values of B alloy and B oxide: 0.05 to 0.25%, and Na oxide 2 O equivalent value and K oxide K 2 A low hydrogen type covered metal arc welding rod comprising: a total of 1.0 to 3.5% converted into O; and the remainder consisting of a coating material, Fe, and impurities.
2. 2. The low-hydrogen covered metal arc welding rod according to claim 1, wherein the coating material contains, in mass % with respect to the total mass of the coating material, one or both of the following (A) and (B) in place of a part of the components constituting the coating material: (A) The sum of the Al value of metal Al and Al alloys and the Mg value of metal Mg and Mg alloys: 3.0% or less (B) The total of the Ti-equivalent value of metal Ti and Ti alloys: 2.5% or less
Citation Information
Patent Citations
Low hydrogen type covered electrode
JP1982152396A
Covered arc welding rod generating low hydrogen atmosphere
JP1983053393A
Consumable nozzle for electroslag welding
JP1984107790A
Low hydrogen type coated electrode
JP1988144895A
Low hydrogen type coated electrode
JP1992367393A