Optical Film
The optical film, with its tailored absorbance properties and high storage modulus, addresses the issue of deterioration in display devices by effectively shielding against short-wavelength visible light, ensuring durability and display quality.
Patent Information
- Application Number
- JP2023009463
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-06-27
- Filing Date
- 2023-01-25
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2038-06-25
AI Technical Summary
Display devices, particularly those with organic EL elements and liquid crystal retardation films, are susceptible to deterioration from both ultraviolet rays and short-wavelength visible light, with existing polarizing plates providing insufficient protection against visible light around 400 nm, leading to degradation issues.
An optical film composed of a resin and a photoselective absorption compound, specifically formulated to have high absorbance at 405 nm and low absorbance at 440 nm, with a storage modulus of 100 MPa or more, to effectively shield against short-wavelength visible light.
The optical film effectively suppresses deterioration of retardation films and organic EL elements by selectively absorbing short-wavelength visible light, maintaining display quality and durability even after weather resistance tests.
Smart Images

Figure 0007580504000026 
Figure 0007580504000027 
Figure 0007580504000028
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical film. [Background technology]
[0002] In display devices (FPD: flat panel displays) such as organic EL display devices and liquid crystal display devices, various components are used, such as display elements such as organic EL elements and liquid crystal cells, and optical films such as polarizing plates. Since the organic EL compounds and liquid crystal compounds used in these components are organic substances, degradation due to ultraviolet rays (UV) is likely to be a problem. In order to solve such problems, for example, Patent Document 1 describes a polarizing plate in which an ultraviolet absorbing agent with excellent ultraviolet absorbing ability in the wavelength range of 370 nm or less is added to the protective film of the polarizing plate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2006-308936 A Summary of the Invention [Problem to be solved by the invention]
[0004] In addition, as display devices have become thinner in recent years, liquid crystal retardation films obtained by aligning and photocuring polymerizable liquid crystal compounds have been developed. It has become clear that these liquid crystal retardation films and organic EL light-emitting devices tend to deteriorate not only due to ultraviolet light but also due to short-wavelength visible light. However, the polarizing plate described in Patent Document 1 has excellent ultraviolet light absorption ability in the wavelength range of 370 nm or less, but has low visible light absorption ability in the vicinity of 400 nm, and there are cases in which the deterioration of liquid crystal retardation films and organic EL light-emitting devices is not sufficiently suppressed. Furthermore, better display characteristics have been required for display devices in recent years.
[0005] An object of the present invention is to provide an optical film having an excellent function of suppressing deterioration of a retardation film or an organic EL light-emitting device caused by short-wavelength visible light. [Means for solving the problem]
[0006] The present invention includes the following inventions. [1] An optical film formed from a resin composition containing a resin (A) and a light selective absorbing compound (B), The resin (A) is at least one resin selected from the group consisting of a cellulose-based resin, a (meth)acrylic-based resin, a polyester-based resin, a polyamide-based resin, a polyimide-based resin, and a cycloolefin-based resin; An optical film satisfying the following formula (1): A(405)≧0.5 (1) [In formula (1), A(405) represents absorbance at a wavelength of 405 nm.] [2] The optical film according to [1], which satisfies the following formula (2): A(440)≦0.1 (2) [In formula (2), A(440) represents absorbance at a wavelength of 440 nm.] [3] The optical film according to [1] or [2], further satisfying the following formula (3): A(405) / A(440)≧5 (3) [In formula (3), A(405) represents the absorbance at a wavelength of 405 nm, and A(440) represents the absorbance at a wavelength of 440 nm.] [4] The optical film according to any one of [1] to [3], wherein the content of the light selective absorption compound (B) is 0.01 to 20 parts by mass per 100 parts by mass of the resin (A). [5] The optical film according to any one of [1] to [4], wherein the resin (A) has a storage modulus E at 23° C. of 100 MPa or more. [6] The optical film according to any one of [1] to [5], wherein the light selective absorption compound (B) is a compound satisfying formula (4). ε(405)≧20 (4) (In formula (4), ε(405) represents the gram absorption coefficient of the compound at a wavelength of 405 nm. The unit of the gram absorption coefficient is L / (g cm).) [7] The optical film according to [6], wherein the light selective absorption compound (B) is a compound satisfying formula (5): ε(405) / ε(440)≧20 (5) [In formula (6), ε(405) represents the gram absorbance coefficient of the compound at a wavelength of 405 nm, and ε(440) represents the gram absorbance coefficient at a wavelength of 440 nm.] [8] The optical film according to any one of [1] to [7], wherein the light selective absorption compound (B) is a compound having a merocyanine structure in the molecule. [9] An optical film with a pressure-sensitive adhesive, comprising the optical film according to any one of [1] to [8], and a pressure-sensitive adhesive layer on at least one surface of the optical film.
[10] A display device comprising the optical film according to [9]. Effect of the Invention
[0007] The optical film of the present invention exhibits high absorption selectivity for short-wavelength visible light around 405 nm, and thus has a good function of suppressing deterioration of retardation films and organic EL light-emitting devices caused by short-wavelength visible light. In addition, the optical film of the present invention exhibits high absorption selectivity for short-wavelength visible light around 405 nm even after a weather resistance test, and can maintain the suppression of deterioration caused by short-wavelength visible light even after a weather resistance test. When the optical film of the present invention is used in a display device, it can provide good display characteristics and durability. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic cross-sectional view showing an example of a pressure-sensitive adhesive layer-attached optical film according to the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of a laminate including an optical film according to the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional view showing an example of a laminate including an optical film according to the present invention. [Figure 4]FIG. 1 is a schematic cross-sectional view showing an example of a laminate including an optical film according to the present invention. [Diagram 5] FIG. 1 is a schematic cross-sectional view showing an example of a laminate including an optical film according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The optical film of the present invention is an optical film formed from a resin composition containing a resin (A) and a light selective absorption compound (B), Resin (A) is at least one resin selected from the group consisting of cellulose-based resins, (meth)acrylic-based resins, polyester-based resins, polyamide-based resins, polyimide-based resins, and cycloolefin-based resins, and is characterized by satisfying the following formula (1): A(405)≧0.5 (1) [In formula (1), A(405) represents absorbance at a wavelength of 405 nm.]
[0010] The larger the value of A(405), the higher the absorption at a wavelength of 405 nm. If the value of A(405) is less than 0.5, the absorption at a wavelength of 405 nm is low, and deterioration of displays such as organic EL elements and retardation films in short-wavelength visible light is likely to occur. The value of A(405) is preferably 0.6 or more, more preferably 0.8 or more, and particularly preferably 1.0 or more. There is no particular upper limit, but it is usually 10 or less.
[0011] It is preferable that the optical film of the present invention further satisfies the following formula (2). A(440)≦0.1 (2) [In formula (2), A(440) represents absorbance at a wavelength of 440 nm.] The smaller the value of A(440), the lower the absorption at a wavelength of 440 nm. If the value of A(440) exceeds 0.1, the better color expression in the display device tends to be impaired. In addition, the luminance is reduced because the luminance of the display device is inhibited. The value of A(440) is preferably 0.05 or less, more preferably 0.04 or less, and particularly preferably 0.03. There is no particular lower limit, but it is usually 0.00001 or more.
[0012] It is preferable that the optical film of the present invention further satisfies the following formula (3). A(405) / A(440)≧5 (3) [In formula (3), A(405) represents the absorbance at a wavelength of 405 nm, and A(440) represents the absorbance at a wavelength of 440 nm.] The value of A(405) / A(440) represents the magnitude of absorption at a wavelength of 405 nm relative to the magnitude of absorption at a wavelength of 440 nm, and the larger this value is, the more specific absorption there is in the wavelength region around 405 nm. The value of A(405) / A(440) is preferably 10 or more, more preferably 30 or more, and particularly preferably 60 or more.
[0013] The optical film of the present invention has a storage modulus E' at 23° C. of usually 100 MPa or more, preferably 300 MPa or more, more preferably 500 MPa or more, further preferably 1000 MPa or more, and particularly preferably 3500 MPa or more. There is no lower limit, but it is usually 100000 MPa or less. The storage modulus at 23° C. of the optical film of the present invention can be measured by the method described in the examples.
[0014] The optical film of the present invention is formed from a resin composition (hereinafter sometimes referred to as "resin composition (1)") containing a resin (A) and a selective light absorbing compound (B). The resin (A) is at least one resin selected from the group consisting of cellulose-based resins, (meth)acrylic-based resins, polyester-based resins, polyamide-based resins, polyimide-based resins, and cycloolefin-based resins.
[0015] The cellulose resin is preferably a cellulose ester resin, that is, a resin in which at least a part of the hydroxyl groups in cellulose are esterified with acetate, and may be a mixed ester in which a part is esterified with acetate and a part is esterified with another acid.The cellulose ester resin is preferably an acetyl cellulose resin.Specific examples of the acetyl cellulose resin include triacetyl cellulose, diacetyl cellulose, cellulose acetate propionate, and cellulose acetate butyrate. The raw cotton material for acetyl cellulose can be cellulose raw materials such as wood pulp and cotton linters, which are known in the Japan Institute of Invention and Innovation's Disclosure Techniques 2001-1745, etc. Acetyl cellulose can be synthesized by the method described in Wood Chemistry, pp. 180-190 (Kyoritsu Shuppan, Migita et al., 1968), etc. Commercially available triacetyl cellulose products include Fujifilm products under the trade names "UV-50," "UV-80," "SH-80," "TD-80U," "TD-TAC," and "UZ-TAC."
[0016] Examples of the (meth)acrylic resin include homopolymers of methacrylic acid alkyl esters or acrylic acid alkyl esters, and copolymers of methacrylic acid alkyl esters and acrylic acid alkyl esters. Specific examples of the methacrylic acid alkyl esters include methyl methacrylate, ethyl methacrylate, and propyl methacrylate, and specific examples of the acrylic acid alkyl esters include methyl acrylate, ethyl acrylate, and propyl acrylate. As such (meth)acrylic resins, those commercially available as general-purpose (meth)acrylic resins can be used. As the (meth)acrylic resins, those called impact-resistant (meth)acrylic resins may also be used. Specific examples of (meth)acrylic resins include "ACRYPET VH" and "ACRYPET VRL20A" manufactured by Mitsubishi Rayon Co., Ltd.
[0017] A polyester resin is a polymer resin having repeating units of ester bonds in the main chain, and is generally obtained by condensation polymerization of a polyvalent carboxylic acid or a derivative thereof and a polyhydric alcohol or a derivative thereof. Examples of polyvalent carboxylic acids or derivatives thereof that give polyesters include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, diphenyldicarboxylic acid, diphenylsulfonedicarboxylic acid, diphenoxyethanedicarboxylic acid, and 5-sodiumsulfonedicarboxylic acid, aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, dimer acid, maleic acid, and fumaric acid, alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, and oxycarboxylic acids such as paraoxybenzoic acid, as well as derivatives thereof. Examples of derivatives of dicarboxylic acids include esters of dimethyl terephthalate, diethyl terephthalate, 2-hydroxyethyl methyl terephthalate, dimethyl 2,6-naphthalenedicarboxylate, dimethyl isophthalate, dimethyl adipate, diethyl maleate, and dimethyl dimerate. Among these, from the viewpoints of moldability and handling, terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and esters thereof are preferably used. Examples of polyhydric alcohols or derivatives thereof that give polyesters include aliphatic dihydroxy compounds such as ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and neopentyl glycol, polyoxyalkylene glycols such as diethylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, alicyclic dihydroxy compounds such as 1,4-cyclohexanedimethanol and spiroglycol, aromatic dihydroxy compounds such as bisphenol A and bisphenol S, and derivatives thereof. Among these, ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, and 1,4-cyclohexanedimethanol are preferably used in terms of moldability and handling. Examples of polyester resins include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polytrimethylene terephthalate, polytrimethylene naphthalate, polycyclohexane dimethyl terephthalate, polycyclohexane dimethyl naphthalate, etc. Among these, polyethylene terephthalate or polyethylene naphthalate is preferred.
[0018] Polyamide resins are polymer resins containing amide bonds in the repeating units of the main chain, such as aromatic polyamides (aramids) in which aromatic ring structures are bonded by amide bonds, and aliphatic polyamides in which aliphatic structures are bonded by amide bonds, etc. Polyamide resins can generally be obtained by polymerization reactions between polyvalent carboxylic acids or their derivatives and polyvalent amines. Examples of polyvalent carboxylic acids or derivatives thereof which give polyamides include terephthalic acid chloride, 2-chloro-terephthalic acid chloride, isophthalic acid dichloride, naphthalene dicarbonyl chloride, biphenyl dicarbonyl chloride, and terphenyl dicarbonyl chloride. Examples of polyamines that give polyamides include 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 2,2'-ditrifluoromethyl-4,4'-diaminobiphenyl, 9,9-bis(4-aminophenyl)fluorene, 9,9-bis(4-amino-3-methylphenyl)fluorene, bis[4-(4-aminophenoxy)phenyl]sulfone, and bis[4-(3-aminophenoxy)phenyl]sulfone. Examples of suitable amines include 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 2,2'-ditrifluoromethyl-4,4'-diaminobiphenyl, 9,9-bis(4-aminophenyl)fluorene, 9,9-bis(4-amino-3-methylphenyl)fluorene, 1,4-cyclohexanediamine, and 1,4-norbornenediamine.
[0019] Polyimide resins are polymer resins containing imide bonds in the repeating units as the main chain, and are generally condensation-type polyimides obtained by polycondensation using diamines and tetracarboxylic dianhydrides as starting materials. As diamines, aromatic diamines, alicyclic diamines, aliphatic diamines, etc. can be used. As tetracarboxylic dianhydrides, aromatic tetracarboxylic dianhydrides, alicyclic tetracarboxylic dianhydrides, acyclic aliphatic tetracarboxylic dianhydrides, etc. can be used. The diamines and tetracarboxylic dianhydrides may be used alone or in combination of two or more. Instead of tetracarboxylic dianhydrides, tetracarboxylic acid compounds selected from tetracarboxylic acid compound analogs such as acid chloride compounds may be used as starting materials.
[0020] Cycloolefin resins are thermoplastic resins having monomer units made of cyclic olefins (cycloolefins) such as norbornene and polycyclic norbornene monomers, and are also called thermoplastic cycloolefin resins. The cycloolefin resins may be ring-opening polymers of the above cycloolefins or hydrogenated ring-opening copolymers using two or more cycloolefins, or may be addition polymers of cycloolefins and chain olefins or aromatic compounds having polymerizable double bonds such as vinyl groups. A polar group may be introduced into the cycloolefin resin.
[0021] When the first protective film is formed using a copolymer of a cycloolefin and a linear olefin and / or an aromatic compound having a vinyl group, examples of the linear olefin include ethylene and propylene, and examples of the aromatic compound having a vinyl group include styrene, α-methylstyrene, and styrene substituted with a nuclear alkyl group. In such a copolymer, the monomer unit consisting of the cycloolefin may be 50 mol% or less, but is preferably about 15 to 50 mol%. In particular, when the first protective film is formed using a ternary copolymer of a cycloolefin, a linear olefin, and an aromatic compound having a vinyl group, the monomer unit consisting of the cycloolefin can be relatively small as described above. In such a ternary copolymer, the monomer unit consisting of the linear olefin is usually 5 to 80 mol%, and the monomer unit consisting of an aromatic compound having a vinyl group is usually 5 to 80 mol%.
[0022] As the cycloolefin resin, an appropriate commercially available product can be used. For example, "TOPAS" sold by Polyplastics Co., Ltd., "ARTON" sold by JSR Corporation, "ZEONOR" and "ZEONEX" sold by Zeon Corporation, and "APEL" sold by Mitsui Chemicals, Inc. (all of the above are trade names) can be mentioned.
[0023] The storage modulus E of the resin (A) at 23° C. is usually 100 MPa or more, preferably 300 MPa or more, more preferably 500 MPa or more, and particularly preferably 1000 MPa or more. There is no lower limit, but it is usually 100000 MPa or less.
[0024] The light selective absorption compound (B) is a compound that selectively absorbs light with a wavelength of 405 nm, and is preferably a compound that satisfies the following formula (4), and more preferably a compound that satisfies formula (5). ε(405)≧20 (4) (In formula (4), ε(405) represents the gram absorption coefficient of the compound at a wavelength of 405 nm. The unit of the gram absorption coefficient is L / (g cm).) ε(405) / ε(440)≧20 (5) [In formula (6), ε(405) represents the gram absorbance coefficient of the compound at a wavelength of 405 nm, and ε(440) represents the gram absorbance coefficient at a wavelength of 440 nm.] The gram absorbance coefficient is measured by the method described in the Examples.
[0025] The larger the value of ε(405), the easier it is for the compound to absorb light with a wavelength of 405 nm, and the easier it is for the compound to exhibit a function of suppressing deterioration caused by ultraviolet light or short-wavelength visible light. If the value of ε(405) is less than 20 L / (g·cm), the content of the light-selective absorbing compound (B) in the resin composition of the present invention is increased in order to exhibit a function of suppressing deterioration caused by ultraviolet light or short-wavelength visible light in retardation films and organic EL light-emitting devices. If the content of the light-selective absorbing compound (B) is increased, the light-selective absorbing compound (B) may bleed out or disperse unevenly, resulting in insufficient light absorption function. The value of ε(405) is preferably 20 L / (g·cm) or more, more preferably 30 L / (g·cm) or more, even more preferably 40 L / (g·cm) or more, and is usually 500 L / (g·cm) or less.
[0026] A compound having a larger value of ε(405) / ε(440) is able to absorb light in the vicinity of 405 nm without impairing the color expression of the display device, and suppress photodegradation of the display device such as a retardation film or an organic EL element. The value of ε(405) / ε(440) is preferably 20 or more, more preferably 40 or more, even more preferably 70 or more, and particularly preferably 80 or more.
[0027] In addition, the light selective absorption compound (B) is preferably a compound containing a merocyanine structure in the molecule. The compound containing a merocyanine structure in the molecule is a compound containing a partial structure represented by -(NC=CC=C)- in the molecule, and examples thereof include merocyanine-based compounds, cyanine-based compounds, indole-based compounds, and benzotriazole-based compounds. Merocyanine-based compounds, cyanine-based compounds, and benzotriazole-based compounds are preferred, and compounds represented by formula (I) are more preferred. [ka] [In the formula, R 1 and R 5 each independently represents a hydrogen atom, an alkyl group having 1 to 25 carbon atoms which may have a substituent, an aralkyl group having 7 to 15 carbon atoms which may have a substituent, an aryl group having 6 to 15 carbon atoms, or a heterocyclic group, and -CH- contained in the alkyl group or aralkyl group is -NR 1A It may be substituted by -, -CO-, -SO2-, -O- or -S-. R 1A represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. R 2 , R 3 and R 4 each independently represents a hydrogen atom, an optionally substituted alkyl group having 1 to 6 carbon atoms, an optionally substituted aromatic hydrocarbon group, or an optionally substituted aromatic heterocyclic group, and -CH2- contained in the alkyl group is -NR 1B It may be substituted by -, -CO-, -SO2-, -O- or -S-. R 1Brepresents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. R 6 and R 7 each independently represents a hydrogen atom, an alkyl group having 1 to 25 carbon atoms, or an electron-withdrawing group, or R 6 and R 7 may be linked to each other to form a ring structure. R 1 and R 2 may be linked together to form a ring structure, R 2 and R 3 may be linked together to form a ring structure, R 2 and R 4 may be linked together to form a ring structure, R 3 and R 6 may be linked to each other to form a ring structure.
[0028] R 1 and R 5 Examples of the alkyl group having 1 to 25 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, a 2-cyanopropyl group, an n-butyl group, a tert-butyl group, a sec-butyl group, an n-pentyl group, an n-hexyl group, a 1-methylbutyl group, a 3-methylbutyl group, an n-octyl group, an n-decyl group, and a 2-hexyl-octyl group. R 1 and R 5 Examples of the substituent that the alkyl group having 1 to 25 carbon atoms represented by the following formula (I) may have include the groups described in group A below. Group A: a nitro group, a hydroxy group, a carboxy group, a sulfo group, a cyano group, an amino group, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, an alkylsilyl group having 1 to 12 carbon atoms, an alkylcarbonyl group having 2 to 8 carbon atoms, *-R a1 -(OR a2 ) t1 -R a3 (R a1 and R a2 each independently represents an alkanediyl group having 1 to 6 carbon atoms; R a3 represents an alkyl group having 1 to 6 carbon atoms, and s1 represents an integer of 1 to 3. Examples of the alkylsilyl group having 1 to 12 carbon atoms include monoalkylsilyl groups such as methylsilyl group, ethylsilyl group, and propylsilyl group; dialkylsilyl groups such as dimethylsilyl group, diethylsilyl group, and methylethylsilyl group; and trialkylsilyl groups such as trimethylsilyl group, triethylsilyl group, and tripropylsilyl group. Examples of the alkylcarbonyl group having 2 to 8 carbon atoms include a methylcarbonyl group and an ethylcarbonyl group. Examples of the halogen atom include a fluorine atom, a chlorine atom, and a bromine atom.
[0029] R 1 and R 5 Examples of the aralkyl group having 7 to 15 carbon atoms represented by the formula (I) include a benzyl group, a phenylethyl group, etc. Examples of the group in which -CH2- contained in the aralkyl group is replaced with -SO2- or -COO- include 2-phenylethyl acetate. R 1 and R 5 Examples of the substituent that the aralkyl group having 7 to 15 carbon atoms represented by the following formula (I) may have include the groups described in group A below. R 1 and R 5 Examples of the aryl group having 6 to 15 carbon atoms represented by the following formula include a phenyl group, a naphthyl group, and anthracenyl group. R 1 and R 5 Examples of the substituent that the aryl group having 6 to 15 carbon atoms represented by the following formula (1) may have include the groups described in group A above. R 1 and R 5 Examples of the heterocyclic group having 6 to 15 carbon atoms represented by the formula (I) include aromatic heterocyclic groups having 3 to 9 carbon atoms such as a pyridyl group, a pyrrolidyl group, a quinolyl group, a thiophene group, an imidazolyl group, an oxazolyl group, a pyrrole group, a thiazolyl group and a furanyl group.
[0030] R 1A and R 1BExamples of the alkyl group having 1 to 6 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, a sec-butyl group, an n-pentyl group, and an n-hexyl group.
[0031] R 2 , R 3 and R 4 As the alkyl group having 1 to 6 carbon atoms represented by the formula: 1B Examples of the alkyl group include the alkyl group having 1 to 6 carbon atoms represented by the following formula: R 2 , R 3 and R 4 Examples of the substituent that the alkyl group having 1 to 6 carbon atoms represented by the following formula (I) may have include the groups described in group A above. R 2 , R 3 and R 4 Examples of the aromatic hydrocarbon group represented by the formula (I) include aryl groups having 6 to 15 carbon atoms, such as a phenyl group, a naphthyl group, and an anthracenyl group; and aralkyl groups having 7 to 15 carbon atoms, such as a benzyl group and a phenylethyl group. R 2 , R 3 and R 4 Examples of the substituent that the aromatic hydrocarbon group represented by the following formula (1) may have include the groups described in Group A above. R 2 , R 3 and R 4 Examples of the aromatic heterocyclic ring represented by the formula (I) include aromatic heterocyclic groups having 3 to 9 carbon atoms, such as a pyridyl group, a pyrrolidyl group, a quinolyl group, a thiophene group, an imidazolyl group, an oxazolyl group, a pyrrole group, a thiazolyl group, and a furanyl group. R 2 , R 3 and R 4 Examples of the substituent that the aromatic heterocycle represented by the following formula (I) may have include the groups described in Group A above.
[0032] R 6 and R 7 As the alkyl group having 1 to 25 carbon atoms represented by the formula: 1 and R 5Examples of the alkyl group include the same alkyl groups having 1 to 25 carbon atoms as those represented by the following formula: R 6 and R 7 Examples of the substituent that the alkyl group having 1 to 25 carbon atoms represented by the following formula (I) may have include the groups described in group A above.
[0033] R 6 and R 7 As the alkyl group having 1 to 25 carbon atoms represented by the formula: 1 and R 5 Examples of the alkyl group include the same alkyl groups having 1 to 25 carbon atoms as those represented by the following formula: R 6 and R 7 Examples of the electron-withdrawing group represented by the formula (I-1) include a cyano group, a nitro group, a halogen atom, an alkyl group substituted with a halogen atom, and a group represented by the formula (I-1). [ka] [In the formula, R 11 represents a hydrogen atom or an alkyl group having 1 to 25 carbon atoms, and at least one methylene group contained in the alkyl group may be substituted with an oxygen atom. X 1 -CO-, -COO-, -OCO-, -CS-, -CSO-, -CSS-, -NR 12 CO- or CONR 13 - represents. R 12 and R 13 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a phenyl group.]
[0034] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Examples of the alkyl group substituted with a halogen atom include perfluoroalkyl groups such as a trifluoromethyl group, a perfluoroethyl group, a perfluoropropyl group, a perfluoroisopropyl group, a perfluorobutyl group, a perfluorosec-butyl group, a perfluorotert-butyl group, a perfluoropentyl group, and a perfluorohexyl group. The number of carbon atoms of the alkyl group substituted with a halogen atom is usually 1 to 25.
[0035] R 6 and R 7 may be linked together to form a ring structure, R 6 and R 7 Examples of the ring structure formed by this include a Meldrum's acid structure, a barbituric acid structure, and a dimedone structure. R 11 As the alkyl group having 1 to 25 carbon atoms represented by the formula: 1 and R 5 The alkyl group may be the same as the alkyl group represented by the following formula:
[0036] R 2 and R 3 The ring structure formed by bonding with each other is R 2 R is a nitrogen-containing ring structure containing a nitrogen atom bonded to R, and examples of the nitrogen-containing ring include 4- to 14-membered nitrogen-containing heterocycles. 2 and R 3 The ring structure formed by linking together may be a single ring or multiple rings. Specific examples include a pyrrolidine ring, a pyrroline ring, an imidazolidine ring, an imidazoline ring, an oxazoline ring, a thiazoline ring, a piperidine ring, a morpholine ring, a piperazine ring, an indole ring, and an isoindole ring.
[0037] R 1 and R 2 The ring structure formed by bonding with each other is R 1 and R 2 R is a nitrogen-containing ring structure containing a nitrogen atom to which R is bonded, and examples of such structures include nitrogen-containing heterocycles having 4 to 14 members (preferably 4 to 8 members). 1 and R 2The ring structure formed by linking together may be a monocyclic ring or a polycyclic ring. 2 and R 3 are the same as those formed by linking together.
[0038] R 2 and R 4 Examples of the ring structure formed by bonding with each other include 4- to 14-membered nitrogen-containing ring structures, and 5- to 9-membered nitrogen-containing ring structures are preferred. 2 and R 4 The ring structure formed by bonding together may be a monocyclic ring or a polycyclic ring. These rings may have a substituent. Examples of such a ring structure include the above-mentioned R 2 and R 3 Examples of the ring structure formed by the formula include the same as those exemplified above.
[0039] R 3 and R 6 The ring structure formed by linking together is R 3 -C=CC=CR 6 is a ring structure that forms the backbone of the ring. For example, a phenyl group can be mentioned.
[0040] R 2 and R 3 The compound represented by formula (I) in which R is linked to each other to form a ring structure includes a compound represented by formula (IA), 2 and R 4 Examples of the compound represented by formula (I) in which are linked to each other to form a ring structure include a compound represented by formula (IB). [ka] [In formula (IA) and formula (IB), R 1 , R 3 , R 4 , R 5 , R 6 and R 7 have the same meanings as above. Ring W 1and Ring W 2 each independently represents a nitrogen-containing ring.
[0041] Ring W 1 and Ring W 2 represents a nitrogen-containing ring containing a nitrogen atom as a ring constituent unit. Ring W 1 and Ring W 2 may each independently be a monocyclic ring or a polycyclic ring, and may contain a heteroatom other than nitrogen as a ring constituent unit. 1 and Ring W 2 are preferably each independently a 5- to 9-membered ring.
[0042] The compound represented by formula (IA) is preferably a compound represented by formula (IA-1). [ka] [In formula (IA-1), R 1 , R 4 , R 5 , R 6 and R 7 have the same meanings as above. A 1 is -CH2-, -O-, -S- or -NR 1D - represents. R 14 and R 15 each independently represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms. R 1D represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.]
[0043] The compound represented by formula (IB) is preferably a compound represented by formula (IB-1) or a compound represented by formula (IB-2). [ka] [In formula (IB-1), R 1 , R 6 and R 7have the same meanings as above. R 16 each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group.]
[0044] [ka] [In formula (IB-2), R 3 , R 5 , R 6 and R 7 have the same meanings as above. R 30 represents a hydrogen atom, a cyano group, a nitro group, a halogen atom, a mercapto group, an amino group, an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aromatic hydrocarbon group having 6 to 18 carbon atoms, an acyl group having 2 to 13 carbon atoms, an acyloxy group having 2 to 13 carbon atoms, or an alkoxycarbonyl group having 2 to 13 carbon atoms. R 31 represents an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, a mercapto group, an alkylthio group having 1 to 12 carbon atoms, an amino group which may have a substituent, or a heterocyclic group.]
[0045] R 30 Examples of the halogen atom represented by the formula (I) include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. R 30 R represented by 30 Examples of the acyl group having 2 to 13 carbon atoms represented by the following formula include an acetyl group, a propionyl group, and a butyryl group. R 30 Examples of the acyloxy group having 2 to 13 carbon atoms represented by the following formula include a methylcarbonyloxy group, an ethylcarbonyloxy group, a propylcarbonyloxy group, and a butylcarbonyloxy group. R 30 Examples of the alkoxycarbonyl group having 2 to 13 carbon atoms represented by the formula (I) include a methoxycarbonyl group, an ethoxycarbonyl group, a propoxycarbonyl group, and a butoxycarbonyl group. R 30Examples of the aromatic hydrocarbon group having 6 to 18 carbon atoms represented by the formula (I) include aryl groups having 6 to 18 carbon atoms, such as a phenyl group, a naphthyl group, and a biphenyl group; and aralkyl groups having 7 to 18 carbon atoms, such as a benzyl group and a phenylethyl group. R 30 As the alkyl group having 1 to 12 carbon atoms represented by the formula: 14 Examples of the alkyl group include the alkyl group having 1 to 12 carbon atoms represented by the following formula: R 30 Examples of the alkyl group having 1 to 12 carbon atoms represented by the formula (I) include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, and a pentoxy group. R 30 is preferably an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an amino group, or a mercapto group.
[0046] R 31 As the alkyl group having 1 to 12 carbon atoms represented by the formula: 14 Examples of the alkyl group include the alkyl group having 1 to 12 carbon atoms represented by the following formula: R 31 The alkoxy group having 1 to 12 carbon atoms represented by the formula: 30 Examples of the alkoxy group include the same alkoxy groups having 1 to 12 carbon atoms as those represented by the following formula: R 31 Examples of the alkylthio group having 1 to 12 carbon atoms represented by the following formula include a methylthio group, an ethylthio group, a propylthio group, a butylthio group, a pentylthio group, and a hexylthio group. R 31 Examples of the amino group which may have a substituent represented by the formula (I) include an amino group; an amino group substituted with one alkyl group having 1 to 8 carbon atoms, such as an N-methylamino group or an N-ethylamino group; and an amino group substituted with two alkyl groups having 1 to 8 carbon atoms, such as an N,N-dimethylamino group, an N,N-diethylamino group, or an N,N-methylethylamino group. R 31 Examples of the heterocycle represented by the following formula include nitrogen-containing heterocycles having 4 to 9 carbon atoms, such as a pyrrolidinyl group, a piperidinyl group, and a morpholinyl group.
[0047] R 3and R 6 are linked together to form a ring structure, and R 2 and R 4 Examples of the compound represented by formula (I) in which are bonded to each other to form a ring structure include a compound represented by formula (IC). [ka] [In formula (IC), R 1 、 R 5 and R 7 has the same meaning as above. R 21 , R 22 each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a hydroxy group. X 2 and X 3 are each independently -CH2- or -N(R 25A )=. R 25A represents a hydrogen atom, an alkyl group having 1 to 25 carbon atoms, or an aromatic hydrocarbon group which may have a substituent.]
[0048] R 25A As the alkyl group having 1 to 25 carbon atoms represented by the formula: 1 Examples of the alkyl group include the same alkyl groups having 1 to 25 carbon atoms as those represented by the following formula: R 25A Examples of the aromatic hydrocarbon group represented by the formula (I) include aryl groups such as a phenyl group and a naphthyl group, aralkyl groups such as a benzyl group and a phenylethyl group, and biphenyl groups, and are preferably aromatic hydrocarbon groups having 6 to 20 carbon atoms. 25A Examples of the substituent that the aromatic hydrocarbon group represented by the following formula may have include a hydroxy group.
[0049] R 3 and R 6 is preferably each independently an electron-withdrawing group.
[0050] R 1 and R 2are linked together to form a ring structure, and R 3 and R 6 Examples of the compound represented by formula (I) in which are bonded to each other to form a ring structure include a compound represented by formula (ID). [ka] [In formula (ID), R 4 , R 5 , R 7 has the same meaning as above. R 25 , R 26 , R 27 and R 28 each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may have a substituent, a hydroxyl group, or an aralkyl group.]
[0051] R 25 , R 26 , R 27 and R 28 As the alkyl group having 1 to 12 carbon atoms represented by the formula: 1A and R 1B The alkyl group having 1 to 12 carbon atoms represented by the formula R 25 , R 26 , R 27 and R 28 Examples of the substituent that the alkyl group having 1 to 12 carbon atoms represented by the following formula may have include a hydroxy group. R 25 , R 26 , R 27 and R 28 Examples of the aralkyl group represented by the formula (I) include aralkyl groups having 7 to 15 carbon atoms, such as a benzyl group and a phenylethyl group.
[0052] R 6 and R 7 Examples of compound (I) in which are linked to each other to form a ring structure include compounds represented by formula (IE). [ka] [In formula (IE), R 1 , R 2 , R 3 , R 4 , R 5 have the same meanings as above. Ring W 3 represents a cyclic compound] Ring W 3 is a 5- to 9-membered ring, which may contain a heteroatom such as a nitrogen atom, an oxygen atom or a sulfur atom as a constituent unit of the ring.
[0053] The compound represented by formula (IE) is preferably a compound represented by formula (IE-1). [ka] [In formula (IC-1), R 1 , R 2 , R 3 and R 5 have the same meanings as above. R 17 , R 18 , R 19 , R q each independently represents a hydrogen atom or an alkyl group, an aralkyl group, or an aryl group having 1 to 12 carbon atoms which may have a substituent, and a -CH2- group contained in the alkyl group or the aralkyl group is -NR 1D may be substituted with -, -C(=O)-, -C(=S)-, -O-, or -S-; R 17 and R 18 may be linked together to form a ring structure, R 18 and R 19 may be linked together to form a ring structure, R 19 and R q may be linked to each other to form a ring structure. m, p, and q each independently represent an integer of 0 to 3.]
[0054] Examples of the compound represented by formula (I) include the following compounds. [ka]
[0055] [ka]
[0056] [ka]
[0057] [ka] [ka]
[0058] [ka]
[0059] [ka] [ka]
[0060] [ka]
[0061] [ka]
[0062] The content of the light selective absorption compound (B) is usually 0.01 to 20 parts by mass, preferably 0.05 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the resin (A).
[0063] The resin composition (1) may further contain a plasticizer, an organic acid, a dye, an antistatic agent, a surfactant, a lubricant, a flame retardant, a filler, rubber particles, a retardation adjuster, an ultraviolet absorbing agent, and the like.
[0064] As the method for producing the optical film of the present invention, any suitable molding method can be adopted. Specifically, compression molding, transfer molding, injection molding, extrusion molding, blow molding, powder molding, FRP molding, cast coating (for example, casting), calendar molding, heat pressing, etc. can be mentioned. Since the smoothness of the obtained film can be improved and good optical uniformity can be obtained, the extrusion molding method or cast coating method is preferable. The molding conditions can be appropriately set according to the composition and type of the resin used, the properties desired for the retardation film, etc.
[0065] The thickness of the optical film of the present invention is usually from 1 to 500 μm, preferably from 5 to 300 μm, more preferably from 10 to 150 μm, and particularly preferably from 10 to 75 μm. The optical film of the present invention may be unstretched or stretched. When the optical film of the present invention is stretched, it may be uniaxially stretched or biaxially stretched. The stretching ratio is usually 1.01 to 10 times, preferably 1.01 to 6 times. The stretching direction may be various directions or dimensions such as the length direction, width direction, thickness direction, and oblique direction.
[0066] The pressure-sensitive adhesive layer-attached optical film of the present invention is a film having a pressure-sensitive adhesive layer on at least one side of the optical film of the present invention. The pressure-sensitive adhesive layer is formed from a known pressure-sensitive adhesive. The known pressure-sensitive adhesive may be any pressure-sensitive adhesive having a base polymer such as an acrylic, rubber, urethane, silicone, or polyvinyl ether, but is preferably an acrylic pressure-sensitive adhesive composition containing a (meth)acrylic resin (A) as a base polymer.
[0067] The (meth)acrylic resin (A) is preferably a polymer containing a structural unit derived from a (meth)acrylic acid ester as a main component (preferably 50% by mass or more). The structural unit derived from a (meth)acrylic acid ester may contain one or more structural units derived from a monomer other than a (meth)acrylic acid ester (for example, a structural unit derived from a monomer having a polar functional group). In this specification, (meth)acrylic acid means either acrylic acid or methacrylic acid, and the "(meth)" in (meth)acrylate and the like has the same meaning.
[0068] Examples of the (meth)acrylic acid ester include (meth)acrylic acid esters represented by the following formula (I): [ka] [In formula (I), R1 represents a hydrogen atom or a methyl group, R2 represents an alkyl group having 1 to 14 carbon atoms or an aralkyl group having 7 to 20 carbon atoms, and the hydrogen atom of the alkyl group or the aralkyl group may be replaced by an alkoxy group having 1 to 10 carbon atoms.]
[0069] In formula (I), R2 is preferably an alkyl group having 1 to 14 carbon atoms, and more preferably an alkyl group having 1 to 8 carbon atoms.
[0070] The (meth)acrylic acid ester represented by formula (I) is linear alkyl esters of (meth)acrylic acid, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate; Branched alkyl esters of (meth)acrylic acid, such as i-propyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, i-pentyl (meth)acrylate, i-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, i-octyl (meth)acrylate, i-nonyl (meth)acrylate, i-stearyl (meth)acrylate, and i-amyl (meth)acrylate; alicyclic skeleton-containing alkyl esters of (meth)acrylic acid, such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dicyclopentanyl (meth)acrylate, cyclododecyl (meth)acrylate, methylcyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, and cyclohexyl α-ethoxyacrylate; Aromatic ring skeleton-containing esters of (meth)acrylic acid such as phenyl (meth)acrylate; etc. In addition, examples of the substituent-containing (meth)acrylic acid alkyl ester include an alkyl group in which a substituent has been introduced into the alkyl group of the (meth)acrylic acid alkyl ester. The substituent of the substituent-containing (meth)acrylic acid alkyl ester is a group that replaces the hydrogen atom of the alkyl group, and specific examples thereof include a phenyl group, an alkoxy group, and a phenoxy group. Specific examples of the substituent-containing (meth)acrylic acid alkyl ester include 2-methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-(2-phenoxyethoxy)ethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, and phenoxypoly(ethylene glycol) (meth)acrylate.
[0071] These (meth)acrylic acid esters may be used alone or in combination of two or more different ones.
[0072] The (meth)acrylic resin (A) preferably contains a structural unit derived from a (meth)acrylic acid alkyl ester (a1) having a homopolymer glass transition temperature Tg of less than 0° C., and a structural unit derived from a (meth)acrylic acid alkyl ester (a2) having a homopolymer Tg of 0° C. or higher. The inclusion of a structural unit derived from an acrylic acid alkyl ester (a1) and a structural unit derived from an acrylic acid alkyl ester (a2) is advantageous in terms of enhancing the high temperature durability of the pressure-sensitive adhesive layer. The Tg of the homopolymer of the (meth)acrylic acid alkyl ester can be, for example, a literature value such as POLYMER HANDBOOK (Wiley-Interscience).
[0073] Specific examples of the (meth)acrylic acid alkyl ester (a1) include (meth)acrylic acid alkyl esters in which the alkyl group has about 2 to 12 carbon atoms, such as ethyl acrylate, n- and i-propyl acrylate, n- and i-butyl acrylate, n-pentyl acrylate, n- and i-hexyl acrylate, n-heptyl acrylate, n- and i-octyl acrylate, 2-ethylhexyl acrylate, n- and i-nonyl acrylate, n- and i-decyl acrylate, and n-dodecyl acrylate.
[0074] The (meth)acrylic acid alkyl ester (a1) may be used alone or in combination of two or more. Among them, n-butyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, etc. are preferred from the viewpoint of followability and reworkability when laminated on an optical film.
[0075] The (meth)acrylic acid alkyl ester (a2) is a (meth)acrylic acid alkyl ester other than the (meth)acrylic acid alkyl ester (a1). Specific examples of the (meth)acrylic acid alkyl ester (a2) include methyl acrylate, cyclohexyl acrylate, isobornyl acrylate, stearyl acrylate, t-butyl acrylate, and the like.
[0076] The (meth)acrylic acid alkyl ester (a2) may be used alone or in combination of two or more kinds. Among them, from the viewpoint of high temperature durability, the (meth)acrylic acid alkyl ester (a2) preferably contains methyl acrylate, cyclohexyl acrylate, isobornyl acrylate, or the like, and more preferably contains methyl acrylate.
[0077] The structural units derived from the (meth)acrylic acid ester represented by formula (I) preferably account for 50 mass % or more of all structural units contained in the (meth)acrylic resin, preferably from 60 to 95 mass %, and more preferably from 65 to 95 mass % or more.
[0078] As the structural unit derived from a monomer other than a (meth)acrylic acid ester, a structural unit derived from a monomer having a polar functional group is preferred, and a structural unit derived from a (meth)acrylic acid ester having a polar functional group is more preferred. Examples of the polar functional group include a hydroxyl group, a carboxyl group, a substituted or unsubstituted amino group, and a heterocyclic group such as an epoxy group. Examples of the monomer having a polar functional group include: 1-Hydroxymethyl (meth)acrylate, 1-hydroxyethyl (meth)acrylate, 1-hydroxyheptyl (meth)acrylate, 1-hydroxybutyl (meth)acrylate, 1-hydroxypentyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxypentyl (meth)acrylate, 2-hydroxyhexyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, p) 3-hydroxypentyl acrylate, 3-hydroxyhexyl (meth)acrylate, 3-hydroxyheptyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-hydroxypentyl (meth)acrylate, 4-hydroxyhexyl (meth)acrylate, 4-hydroxyheptyl (meth)acrylate, 4-hydroxyoctyl (meth)acrylate, 2-chloro-2-hydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 5-hydroxyhexyl (meth)acrylate, 5-hydroxyheptyl (meth)acrylate, 5-hydroxyoctyl (meth)acrylate, 5-hydroxynonyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 6-hydroxyheptyl (meth)acrylate, 6-hydroxyoctyl (meth)acrylate, 6-hydroxynonyl (meth)acrylate, 6-hydroxydecyl (meth)acrylate, 7-hydroxyheptyl (meth)acrylate, 7-hydroxyoctyl (meth)acrylate, 7-hydroxynonyl (meth)acrylate, 7-hydroxydecyl (meth)acrylate, 7-hydroxyundecyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 8-hydroxynonyl (meth)acrylate, 8-hydroxydecyl (meth)acrylate, 8-hydroxyundecyl (meth)acrylate, 8-hydroxydodecyl (meth)acrylate, 9-hydroxynonyl (meth)acrylate, 9-hydroxydecyl (meth)acrylate, 9-hydroxyundecyl (meth)acrylate, 9-hydroxydodecyl (meth)acrylate,9-Hydroxytridecyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 10-hydroxyundecyl (meth)acrylate, 10-hydroxydodecyl (meth)acrylate, 10-hydroxytridecyl acrylate, 10-hydroxytetradecyl (meth)acrylate, 11-hydroxyundecyl (meth)acrylate, 11-hydroxydodecyl (meth)acrylate, 11-hydroxytridecyl (meth)acrylate, 11-hydroxytetradecyl (meth)acrylate, 11-hydroxypentadecyl (meth)acrylate, ) monomers having a hydroxy group, such as 12-hydroxydodecyl acrylate, 12-hydroxytridecyl (meth)acrylate, 12-hydroxytetradecyl (meth)acrylate, 13-hydroxypentadecyl (meth)acrylate, 13-hydroxytetradecyl (meth)acrylate, 13-hydroxypentadecyl (meth)acrylate, 14-hydroxytetradecyl (meth)acrylate, 14-hydroxypentadecyl (meth)acrylate, 15-hydroxypentadecyl (meth)acrylate, and 15-hydroxyheptadecyl (meth)acrylate; Monomers having a carboxyl group, such as (meth)acrylic acid, carboxyalkyl (meth)acrylates (for example, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate), maleic acid, maleic anhydride, fumaric acid, and crotonic acid; Monomers having a heterocyclic group, such as acryloylmorpholine, vinylcaprolactam, N-vinyl-2-pyrrolidone, vinylpyridine, tetrahydrofurfuryl (meth)acrylate, caprolactone-modified tetrahydrofurfuryl acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, glycidyl (meth)acrylate, and 2,5-dihydrofuran; Examples of the monomer include monomers having a substituted or unsubstituted amino group, such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and dimethylaminopropyl (meth)acrylate. Among these, from the viewpoint of reactivity between the (meth)acrylic acid ester polymer and the crosslinking agent, a monomer having a hydroxy group or a monomer having a carboxyl group is preferred, and it is more preferred to include both a monomer having a hydroxy group and a monomer having a carboxyl group.
[0079] As the monomer having a hydroxy group, 2-hydroxyethyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 5-hydroxypentyl acrylate, and 6-hydroxyhexyl acrylate are preferred. In particular, good durability can be obtained by using 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, and 5-hydroxypentyl acrylate. As the monomer having a carboxyl group, it is preferable to use acrylic acid.
[0080] From the viewpoint of preventing an increase in the peel strength of a separation film that can be laminated on the outer surface of the pressure-sensitive adhesive layer, it is preferable that the resin is substantially free of a monomer having an amino group, which means that the amount of the monomer is 0.1 part by weight or less in 100 parts by weight of all the constituent units constituting the (meth)acrylic resin (A).
[0081] The content of the structural units derived from the monomer having a polar functional group is preferably 20 parts by mass or less, more preferably 0.5 parts by mass or more and 15 parts by mass or less, even more preferably 0.5 parts by mass or more and 10 parts by mass or less, and particularly preferably 1 part by mass or more and 7 parts by mass or less, relative to 100 parts by mass of all structural units of the (meth)acrylic resin (A).
[0082] The content of the structural units derived from the monomer having an aromatic group is preferably 20 parts by mass or less, more preferably 4 parts by mass or more and 20 parts by mass or less, and even more preferably 4 parts by mass or more and 16 parts by mass or less, relative to 100 parts by mass of all structural units of the (meth)acrylic resin (A).
[0083] Examples of structural units derived from monomers other than (meth)acrylic acid esters include structural units derived from styrene-based monomers, structural units derived from vinyl-based monomers, structural units derived from monomers having multiple (meth)acryloyl groups in the molecule, and structural units derived from (meth)acrylamide-based monomers.
[0084] Examples of styrene-based monomers include styrene; alkyl styrenes such as methylstyrene, dimethylstyrene, trimethylstyrene, ethylstyrene, diethylstyrene, triethylstyrene, propylstyrene, butylstyrene, hexylstyrene, heptylstyrene, and octylstyrene; halogenated styrenes such as fluorostyrene, chlorostyrene, bromostyrene, dibromostyrene, and iodostyrene; nitrostyrene; acetylstyrene; methoxystyrene; and divinylbenzene.
[0085] Examples of vinyl monomers include fatty acid vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, vinyl 2-ethylhexanoate, and vinyl laurate; vinyl halides such as vinyl chloride and vinyl bromide; vinylidene halides such as vinylidene chloride; nitrogen-containing heteroaromatic vinyls such as vinylpyridine, vinylpyrrolidone, and vinylcarbazole; conjugated dienes such as butadiene, isoprene, and chloroprene; and unsaturated nitriles such as acrylonitrile and methacrylonitrile.
[0086] Examples of monomers having multiple (meth)acryloyl groups in the molecule include monomers having two (meth)acryloyl groups in the molecule, such as 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate; and monomers having three (meth)acryloyl groups in the molecule, such as trimethylolpropane tri(meth)acrylate.
[0087] Examples of (meth)acrylamide monomers include N-methylol (meth)acrylamide, N-(2-hydroxyethyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(4-hydroxybutyl) (meth)acrylamide, N-(5-hydroxypentyl) (meth)acrylamide, N-(6-hydroxyhexyl) (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-(3-dimethylaminopropyl) (meth)acrylamide, N-(1,1-dimethyl-3-oxobutyl) (meth)acrylamide, N-[2-(2-oxo-1-imidazolidinyl)ethyl] (meth)acrylamide, 2-acryloylamino-2-methyl-1-propanesulfonic acid, N-(methoxymethyl)acrylamide, N-(ethoxymethyl) (meth)acrylamide, N-(propoxymethyl)(meth)acrylamide, N-(1-methylethoxymethyl)(meth)acrylamide, N-(1-methylpropoxymethyl)(meth)acrylamide, N-(2-methylpropoxymethyl)(meth)acrylamide, N-(butoxymethyl)(meth)acrylamide, N-(1,1-dimethylethoxymethyl)(meth)acrylamide, N-(2-methoxyethyl)(meth)acrylamide, N-(2-ethoxyethyl)(meth)acrylamide Examples of such acrylamide include N-(2-propoxyethyl)acrylamide, N-[2-(1-methylethoxy)ethyl]acrylamide, N-[2-(1-methylpropoxy)ethyl]acrylamide, N-[2-(2-methylpropoxy)ethyl]acrylamide, N-(2-butoxyethyl)acrylamide, and N-[2-(1,1-dimethylethoxy)ethyl]acrylamide. Among these, N-(methoxymethyl)acrylamide, N-(ethoxymethyl)acrylamide, N-(propoxymethyl)acrylamide, N-(butoxymethyl)acrylamide, and N-(2-methylpropoxymethyl)acrylamide are preferred.
[0088] The weight average molecular weight (Mw) of the (meth)acrylic resin (A) is preferably 500,000 to 2,500,000. When the weight average molecular weight is 500,000 or more, the durability of the adhesive layer in a high temperature environment is improved, and defects such as peeling between the adherend and the adhesive layer and cohesive failure of the adhesive layer are easily suppressed. When the weight average molecular weight is 2,500,000 or less, it is advantageous in terms of coatability when the adhesive composition is processed into a sheet (applied to a substrate). From the viewpoint of achieving both the durability of the adhesive layer and the coatability of the adhesive composition, the weight average molecular weight is preferably 600,000 to 1,800,000, more preferably 700,000 to 1,700,000, and particularly preferably 1,000,000 to 1,600,000. In addition, the molecular weight distribution (Mw / Mn), which is expressed as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn), is usually 2 to 10, preferably 3 to 8, and more preferably 3 to 6. The weight average molecular weight can be analyzed by gel permeation chromatography and is expressed as a value converted into standard polystyrene.
[0089] When the (meth)acrylic resin (A) is dissolved in ethyl acetate to prepare a solution having a concentration of 20% by mass, the viscosity at 25°C is preferably 20 Pa·s or less, and more preferably 0.1 to 15 Pa·s. A viscosity in this range is advantageous from the viewpoint of coatability when the pressure-sensitive adhesive composition is applied to a substrate. The viscosity can be measured by a Brookfield viscometer.
[0090] The glass transition temperature (Tg) of the (meth)acrylic resin (A) may be, for example, -60 to 20°C, preferably -50 to 15°C, more preferably -45 to 10°C, and particularly preferably -40 to 0°C. If the Tg is equal to or lower than the upper limit, it is advantageous for improving the wettability of the pressure-sensitive adhesive layer to the adherend substrate, and if it is equal to or higher than the lower limit, it is advantageous for improving the durability of the pressure-sensitive adhesive layer. The glass transition temperature can be measured by a differential scanning calorimeter (DSC).
[0091] The (meth)acrylic acid resin (A) can be produced by known methods such as solution polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization, and the solution polymerization is particularly preferred. As the solution polymerization, for example, a method of mixing a monomer and an organic solvent, adding a thermal polymerization initiator under a nitrogen atmosphere, and stirring for about 3 to 15 hours at a temperature of 40 to 90°C, preferably about 50 to 80°C, may be mentioned. In order to control the reaction, the monomer or the thermal polymerization initiator may be added continuously or intermittently during polymerization. The monomer or the thermal initiator may be in a state of being added to the organic solvent.
[0092] As the polymerization initiator, a thermal polymerization initiator or a photopolymerization initiator is used. As the photopolymerization initiator, 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone and the like can be mentioned. As the thermal polymerization initiator, azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl-2,2'-azobis(2-methylpropionate), and 2,2'-azobis(2-hydroxymethylpropionitrile); lauryl Examples of the peroxide initiator include organic peroxides such as peroxide, t-butyl hydroperoxide, benzoyl peroxide, t-butyl peroxybenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, dipropyl peroxydicarbonate, t-butyl peroxyneodecanoate, t-butyl peroxypivalate, and (3,5,5-trimethylhexanoyl) peroxide; and inorganic peroxides such as potassium persulfate, ammonium persulfate, and hydrogen peroxide. Redox initiators using a peroxide in combination with a reducing agent can also be used.
[0093] The proportion of the polymerization initiator is about 0.001 to 5 parts by mass relative to 100 parts by mass of the total amount of the monomers constituting the (meth)acrylic resin. The polymerization of the (meth)acrylic resin may be carried out using a polymerization method using active energy rays (for example, ultraviolet rays).
[0094] Examples of the organic solvent include aromatic hydrocarbons such as toluene and xylene; esters such as ethyl acetate and butyl acetate; aliphatic alcohols such as propyl alcohol and isopropyl alcohol; and ketones such as acetone, methyl ethyl ketone and methyl isobutyl ketone.
[0095] The content of the (meth)acrylic resin (A) is usually 60% by mass to 99.9% by mass, preferably 70% by mass to 99.5% by mass, and more preferably 80% by mass to 99% by mass, in 100% by mass of the pressure-sensitive adhesive composition.
[0096] The pressure-sensitive adhesive composition may contain a crosslinking agent (b). The crosslinking agent (b) reacts with a polar functional group (e.g., a hydroxyl group, an amino group, a carboxyl group, a heterocyclic group, etc.) in the (meth)acrylic resin (A). The crosslinking agent (B) forms a crosslinked structure with the (meth)acrylic resin, etc., and forms a crosslinked structure that is advantageous in durability and reworkability.
[0097] Examples of the crosslinking agent (b) include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, metal chelate-based crosslinking agents, etc., and from the viewpoints of the pot life of the pressure-sensitive adhesive composition, the durability of the pressure-sensitive adhesive layer, the crosslinking rate, etc., it is particularly preferable to use an isocyanate-based crosslinking agent.
[0098] As the isocyanate compound, a compound having at least two isocyanato groups (-NCO) in the molecule is preferable, and examples thereof include aliphatic isocyanate compounds (e.g., hexamethylene diisocyanate, etc.), alicyclic isocyanate compounds (e.g., isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate), aromatic isocyanate compounds (e.g., tolylene diisocyanate, xylylene diisocyanate diphenylmethane diisocyanate, naphthalene diisocyanate, triphenylmethane triisocyanate, etc.), and the like. The crosslinking agent (B) may be an adduct of the isocyanate compound with a polyhydric alcohol compound (e.g., an adduct with glycerol, trimethylolpropane, etc.), an isocyanurate, a biuret-type compound, a urethane prepolymer-type isocyanate compound obtained by addition reaction with a polyether polyol, a polyester polyol, an acrylic polyol, a polybutadiene polyol, a polyisoprene polyol, etc. The crosslinking agent (B) may be used alone or in combination of two or more. Among these, representative examples include an aromatic isocyanate compound (e.g., tolylene diisocyanate, xylylene diisocyanate), an aliphatic isocyanate compound (e.g., hexamethylene diisocyanate), or an adduct of these with a polyhydric alcohol compound (e.g., glycerol, trimethylolpropane), or an isocyanurate. When the crosslinking agent (B) is an aromatic isocyanate-based compound and / or an adduct thereof with a polyhydric alcohol compound or an isocyanurate, the durability of the pressure-sensitive adhesive layer can be improved, possibly because it is advantageous for forming an optimal crosslink density (or crosslinked structure). In particular, when the crosslinking agent (B) is a tolylene diisocyanate-based compound and / or an adduct thereof with a polyhydric alcohol compound, the durability can be improved even when the pressure-sensitive adhesive layer is applied to a polarizing plate, for example.
[0099] The content of the crosslinking agent (b) is usually 0.01 to 15 parts by weight, preferably 0.05 to 10 parts by weight, and more preferably 0.1 to 5 parts by weight, based on 100 parts by weight of the (meth)acrylic resin (A).
[0100] The resin composition may further contain a silane compound (D). Examples of the silane compound (D) include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylethoxydimethylsilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane. The silane compound (D) may be a silicone oligomer. Specific examples of the silicone oligomer, expressed in the form of a combination of monomers, are as follows:
[0101] Oligomers containing mercaptopropyl groups, such as 3-mercaptopropyltrimethoxysilane-tetramethoxysilane oligomer, 3-mercaptopropyltrimethoxysilane-tetraethoxysilane oligomer, 3-mercaptopropyltriethoxysilane-tetramethoxysilane oligomer, 3-mercaptopropyltriethoxysilane-tetraethoxysilane oligomer; oligomers containing mercaptomethyl groups, such as mercaptomethyltrimethoxysilane-tetramethoxysilane oligomer, mercaptomethyltrimethoxysilane-tetraethoxysilane oligomer, mercaptomethyltriethoxysilane-tetramethoxysilane oligomer, mercaptomethyltriethoxysilane-tetraethoxysilane oligomer; 3-glycidyloxysilane copolymers containing 3-glycidoxypropyl groups, such as propyltrimethoxysilane-tetramethoxysilane copolymer, 3-glycidoxypropyltrimethoxysilane-tetraethoxysilane copolymer, 3-glycidoxypropyltriethoxysilane-tetramethoxysilane copolymer, 3-glycidoxypropyltriethoxysilane-tetraethoxysilane copolymer, 3-glycidoxypropylmethyldimethoxysilane-tetramethoxysilane copolymer, 3-glycidoxypropylmethyldimethoxysilane-tetraethoxysilane copolymer, 3-glycidoxypropylmethyldiethoxysilane-tetramethoxysilane copolymer, and 3-glycidoxypropylmethyldiethoxysilane-tetraethoxysilane copolymer;3-Methacryloyloxypropyltrimethoxysilane-tetramethoxysilane oligomer, 3-Methacryloyloxypropyltrimethoxysilane-tetraethoxysilane oligomer, 3-Methacryloyloxypropyltriethoxysilane-tetramethoxysilane oligomer, 3-Methacryloyloxypropyltriethoxysilane-tetraethoxysilane oligomer, 3-Methacryloyloxypropylmethyldimethoxysilane-tetramethoxysilane oligomer, 3-Methacryloyloxypropylmethyldimethoxysilane-tetraethoxysilane oligomer Methacryloyloxypropyl group-containing oligomers such as methacryloyloxypropyl methyldiethoxysilane-tetramethoxysilane oligomer, 3-methacryloyloxypropyl methyldiethoxysilane-tetraethoxysilane oligomer; 3-acryloyloxypropyl trimethoxysilane-tetramethoxysilane oligomer, 3-acryloyloxypropyl trimethoxysilane-tetraethoxysilane oligomer, 3-acryloyloxypropyl triethoxysilane-tetramethoxysilane oligomer , acryloyloxypropyl group-containing oligomers such as 3-acryloyloxypropyltriethoxysilane-tetraethoxysilane oligomer, 3-acryloyloxypropylmethyldimethoxysilane-tetramethoxysilane oligomer, 3-acryloyloxypropylmethyldimethoxysilane-tetraethoxysilane oligomer, 3-acryloyloxypropylmethyldiethoxysilane-tetramethoxysilane oligomer, 3-acryloyloxypropylmethyldiethoxysilane-tetraethoxysilane oligomer, and 3-acryloyloxypropylmethyldiethoxysilane-tetraethoxysilane oligomer; Vinyl group-containing oligomers such as silane-tetramethoxysilane oligomer, vinyltrimethoxysilane-tetraethoxysilane oligomer, vinyltriethoxysilane-tetramethoxysilane oligomer, vinyltriethoxysilane-tetraethoxysilane oligomer, vinylmethyldimethoxysilane-tetramethoxysilane oligomer, vinylmethyldimethoxysilane-tetraethoxysilane oligomer, vinylmethyldiethoxysilane-tetramethoxysilane oligomer, and vinylmethyldiethoxysilane-tetraethoxysilane oligomer;Amino group-containing copolymers such as 3-aminopropyltrimethoxysilane-tetramethoxysilane copolymer, 3-aminopropyltrimethoxysilane-tetraethoxysilane copolymer, 3-aminopropyltriethoxysilane-tetramethoxysilane copolymer, 3-aminopropyltriethoxysilane-tetraethoxysilane copolymer, 3-aminopropylmethyldimethoxysilane-tetramethoxysilane copolymer, 3-aminopropylmethyldimethoxysilane-tetraethoxysilane copolymer, 3-aminopropylmethyldiethoxysilane-tetramethoxysilane copolymer, 3-aminopropylmethyldiethoxysilane-tetramethoxysilane copolymer, 3-aminopropylmethyldiethoxysilane-tetraethoxysilane copolymer, and the like;
[0102] The silane compound (D) may be a silane compound represented by the following formula (d1). When the pressure-sensitive adhesive composition contains the silane compound represented by the following formula (d1), the adhesiveness (or bonding property) can be further improved, so that an adhesive layer having good peel resistance can be formed. In particular, even when the adhesive layer is applied (or laminated) to a transparent electrode or glass in a high-temperature environment, the adhesiveness (or bonding property) can be maintained and high durability can be exhibited.
[0103] [ka] (In the formula, B represents an alkanediyl group having 1 to 20 carbon atoms or a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, and -CH- constituting the alkanediyl group and the alicyclic hydrocarbon group may be substituted with -O- or -CO-; R d7 represents an alkyl group having 1 to 5 carbon atoms, and R d8 , R d9 , R d10 , R d11 and R d12 each independently represents an alkyl group having 1 to 5 carbon atoms or an alkoxy group having 1 to 5 carbon atoms.
[0104] In formula (d1), B represents an alkanediyl group having 1 to 20 carbon atoms, such as a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a hexamethylene group, a heptamethylene group, or an octamethylene group; a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, such as a cyclobutylene group (e.g., a 1,2-cyclobutylene group), a cyclopentylene group (e.g., a 1,2-cyclopentylene group), a cyclohexylene group (e.g., a 1,2-cyclohexylene group), or a cyclooctylene group (e.g., a 1,2-cyclooctylene group), or these alkanediyl groups and groups in which -CH2- constituting the alicyclic hydrocarbon group is replaced with -O- or -CO-. Preferred B is an alkanediyl group having 1 to 10 carbon atoms. R d7 represents an alkyl group having 1 to 5 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a s-butyl group, a t-butyl group, or a pentyl group, and R d8 , R d9 , R d10 , R d11 and R d12 Each independently represents the R d7 or an alkoxy group having 1 to 5 carbon atoms, such as a methoxy group, an ethoxy group, a propoxy group, an i-propoxy group, a butoxy group, a s-butoxy group, or a t-butoxy group. d8 , R d9 , R d10 , R d11 and R d12 each independently represents an alkoxy group having a carbon number of 1 to 5. These silane compounds (D) can be used alone or in combination of two or more kinds.
[0105] Specific examples of the silane compound represented by the formula (d1) include bis(triC1) compounds such as (trimethoxysilyl)methane, 1,2-bis(trimethoxysilyl)ethane, 1,2-bis(triethoxysilyl)ethane, 1,3-bis(trimethoxysilyl)propane, 1,3-bis(triethoxysilyl)propane, 1,4-bis(trimethoxysilyl)butane, 1,4-bis(triethoxysilyl)butane, 1,5-bis(trimethoxysilyl)pentane, 1,5-bis(triethoxysilyl)pentane, 1,6-bis(trimethoxysilyl)hexane, 1,6-bis(triethoxysilyl)hexane, 1,6-bis(tripropoxysilyl)hexane, 1,8-bis(trimethoxysilyl)octane, 1,8-bis(triethoxysilyl)octane, and 1,8-bis(tripropoxysilyl)octane. bis(diC1-5 alkoxyC1-5 alkylsilyl) C1-10 alkanes such as bis(dimethoxymethylsilyl)methane, 1,2-bis(dimethoxymethylsilyl)ethane, 1,2-bis(dimethoxyethylsilyl)ethane, 1,4-bis(dimethoxymethylsilyl)butane, 1,4-bis(dimethoxyethylsilyl)butane, 1,6-bis(dimethoxymethylsilyl)hexane, 1,6-bis(dimethoxyethylsilyl)hexane, 1,8-bis(dimethoxymethylsilyl)octane, and 1,8-bis(dimethoxyethylsilyl)octane; and bis(monoC1-5 alkoxy-diC1-5 alkylsilyl) C1-10 alkanes such as 1,6-bis(methoxydimethylsilyl)hexane and 1,8-bis(methoxydimethylsilyl)octane. Of these, bis(triC1-3 alkoxysilyl)C1-10 alkanes such as 1,2-bis(trimethoxysilyl)ethane, 1,3-bis(trimethoxysilyl)propane, 1,4-bis(trimethoxysilyl)butane, 1,5-bis(trimethoxysilyl)pentane, 1,6-bis(trimethoxysilyl)hexane, and 1,8-bis(trimethoxysilyl)octane are preferred, and 1,6-bis(trimethoxysilyl)hexane and 1,8-bis(trimethoxysilyl)octane are particularly preferred.
[0106] The content of the silane compound (D) is usually 0.01 to 10 parts by weight, preferably 0.03 to 5 parts by weight, more preferably 0.05 to 2 parts by weight, and even more preferably 0.1 to 1 part by weight, based on 100 parts by weight of the (meth)acrylic resin (A). When the content is equal to or less than the upper limit, it is advantageous for suppressing the bleeding out of the silane compound (D) from the pressure-sensitive adhesive layer, and when the content is equal to or more than the lower limit, it is easier to improve the adhesion (or adhesiveness) between the pressure-sensitive adhesive layer and a metal layer or a glass substrate, etc., and is advantageous for improving peel resistance, etc.
[0107] The pressure-sensitive adhesive composition may further contain an antistatic agent. Examples of the antistatic agent include surfactants, siloxane compounds, conductive polymers, ionic compounds, etc., and ionic compounds are preferred. Examples of the ionic compounds include conventional ones. Examples of the cationic components constituting the ionic compounds include organic cations and inorganic cations. Examples of the organic cations include pyridinium cations, pyrrolidinium cations, piperidinium cations, imidazolium cations, ammonium cations, sulfonium cations, phosphonium cations, etc. Examples of the inorganic cations include alkali metal cations such as lithium cations, potassium cations, sodium cations, and cesium cations, and alkaline earth metal cations such as magnesium cations and calcium cations. In particular, from the viewpoint of compatibility with (meth)acrylic resins, pyridinium cations, imidazolium cations, pyrrolidinium cations, lithium cations, and potassium cations are preferred. Examples of the anionic components constituting the ionic compounds may be either inorganic anions or organic anions, but from the viewpoint of antistatic performance, an anionic component containing a fluorine atom is preferred. Examples of anion components containing fluorine atoms include hexafluorophosphate anion (PF6-), bis(trifluoromethanesulfonyl)imide anion [(CF3SO2)2N-], bis(fluorosulfonyl)imide anion [(FSO2)2N-], and tetra(pentafluorophenyl)borate anion [(C6F5)4B-]. These ionic compounds can be used alone or in combination of two or more. In particular, bis(trifluoromethanesulfonyl)imide anion [(CF3SO2)2N-], bis(fluorosulfonyl)imide anion [(FSO2)2N-], and tetra(pentafluorophenyl)borate anion [(C6F5)4B-] are preferred. In terms of the stability over time of the antistatic performance of the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition, an ionic compound that is solid at room temperature is preferred.
[0108] The content of the antistatic agent is, for example, 0.01 to 20 parts by mass, preferably 0.1 to 10 parts by mass, and more preferably 1 to 7 parts by mass, relative to 100 parts by mass of the (meth)acrylic resin (A).
[0109] The pressure-sensitive adhesive composition may contain one or more additives such as a solvent, a crosslinking catalyst, a tackifier, a plasticizer, a softener, a pigment, a rust inhibitor, an inorganic filler, and light-scattering fine particles.
[0110] An example of the pressure-sensitive adhesive layer-attached optical film according to the present invention is shown in FIG. As shown in Fig. 1, the pressure-sensitive adhesive layer-attached optical film of the present invention having a pressure-sensitive adhesive layer 2 on at least one surface of an optical film 1 may have a separate film (release film) 3 laminated on the surface opposite to the surface where the optical film and the pressure-sensitive adhesive layer are attached. This separate film 3 is usually peeled off and removed when the pressure-sensitive adhesive layer-attached optical film is used (for example, when it is laminated on a liquid crystal cell, a retardation film, etc.). The separate film may be, for example, a film made of various resins such as polyethylene terephthalate, polybutylene terephthalate, polycarbonate, polyarene, etc., with a release treatment such as silicone treatment applied to the surface on which the pressure-sensitive adhesive layer is formed.
[0111] 2 to 5 show an example of the layer structure of an optical laminate including the optical film according to the present invention. The optical laminate 10A shown in FIG. 2 is an optical laminate including a protective film 4, an adhesive layer 5, a polarizing film 6, an adhesive layer 5, the optical film 1 of the present invention, and a pressure-sensitive adhesive layer . The optical laminate 10B shown in FIG. 3 is an optical laminate including the optical film 1 of the present invention, an adhesive layer 5, a polarizing film 6, an adhesive layer 5, a protective film 4, and a pressure-sensitive adhesive layer . The optical film 10C shown in FIG. 4 and the optical laminate 10D shown in FIG. 5 are optical laminates including a protective film 4, an adhesive layer 5, a polarizing film 6, an adhesive layer 5, the optical film 1 of the present invention, a pressure-sensitive adhesive layer 7, an optical film 40, a pressure-sensitive adhesive layer 7a, and a light-emitting element 30 (liquid crystal cell, OLED cell).
[0112] As shown in Figs. 2 to 5, an optical film such as a retardation film, a polarizing film, a window film, a light collecting film, or a brightness enhancing film may be laminated on the pressure-sensitive adhesive layer surface of the pressure-sensitive adhesive layer-attached optical film of the present invention.
[0113] The retardation film is an optical film exhibiting optical anisotropy, and examples thereof include stretched films obtained by stretching polymer films made of polyvinyl alcohol, polycarbonate, polyester, polyarylate, polyimide, polyolefin, polycycloolefin, polystyrene, polysulfone, polyethersulfone, polyvinylidene fluoride / polymethyl methacrylate, acetyl cellulose, saponified ethylene-vinyl acetate copolymer, polyvinyl chloride, etc., to about 1.01 to 6 times. Among them, a polymer film obtained by uniaxially or biaxially stretching a polycarbonate film or a cycloolefin-based resin film is preferable. In this specification, the retardation film includes a zero retardation film, and also includes films called uniaxial retardation film, low photoelasticity retardation film, wide viewing angle retardation film, etc.
[0114] Examples of films that exhibit optical anisotropy by coating and orienting a liquid crystal compound or films that exhibit optical anisotropy by coating an inorganic layer compound include films called temperature-compensated retardation films, such as "NH film" (product name: film with inclined alignment of rod-shaped liquid crystals) sold by JX Nippon Oil & Energy Corporation, "WV film" (product name: film with inclined alignment of discotic liquid crystals) sold by Fujifilm Corporation, "VAC film" (product name: fully biaxially oriented film) sold by Sumitomo Chemical Co., Ltd., and "new VAC film" (product name: biaxially oriented film) sold by Sumitomo Chemical Co., Ltd.
[0115] Zero retardation film means a front retardation R e and retardation R thThe zero retardation film refers to an optically isotropic film in which both of the retardation and retardation values are -15 to 15 nm. Examples of the zero retardation film include resin films made of cellulose resins, polyolefin resins (chain polyolefin resins, polycycloolefin resins, etc.), or polyethylene terephthalate resins, and cellulose resins or polyolefin resins are preferred because the retardation value is easily controlled and they are easily available. The zero retardation film can also be used as a protective film. Examples of the zero retardation film include "Z-TAC" (trade name) sold by Fujifilm Corporation, "Zerotack (registered trademark)" sold by Konica Minolta Opto Co., Ltd., and "ZF-14" (trade name) sold by Zeon Corporation.
[0116] In the present invention, the retardation film is preferably a retardation film obtained by curing a polymerizable liquid crystal compound.
[0117] Examples of films that exhibit optical anisotropy by coating and orienting liquid crystal compounds include a first form: a retardation film in which rod-shaped liquid crystal compounds are oriented horizontally to the supporting substrate; a second form: a retardation film in which rod-shaped liquid crystal compounds are oriented vertically to the supporting substrate; a third form: a retardation film in which the orientation direction of rod-shaped liquid crystal compounds changes helically in the plane; a fourth form: a retardation film in which discotic liquid crystal compounds are oriented at an inclination; and a fifth form: a biaxial retardation film in which discotic liquid crystal compounds are oriented vertically to the supporting substrate.
[0118] For example, as an optical film used in an organic electroluminescence display, the first, second and fifth embodiments are preferably used, or these may be laminated and used.
[0119] When the retardation film is a layer made of a polymer in an oriented state of a polymerizable liquid crystal compound (hereinafter, sometimes referred to as an "optically anisotropic layer"), the retardation film preferably has reverse wavelength dispersion. Reverse wavelength dispersion is an optical property in which the liquid crystal alignment in-plane retardation value at a short wavelength is smaller than the liquid crystal alignment in-plane retardation value at a long wavelength, and preferably, the retardation film satisfies the following formulas (7) and (8). Note that Re(λ) represents the in-plane retardation value for light with a wavelength of λ nm. Re(450) / Re(550)≦1 (7) 1≦Re(630) / Re(550) (8) In the optical film of the present invention, when the retardation film is in the first form and has reverse wavelength dispersion, coloring during black display on a display device is reduced, which is preferable, and in the formula (7), 0.82≦Re(450) / Re(550)≦0.93 is more preferable. Furthermore, 120≦Re(550)≦150 is more preferable.
[0120] When the retardation film is a film having an optically anisotropic layer, examples of the polymerizable liquid crystal compound include compounds having a polymerizable group among the compounds described in "3.8.6 Network (completely crosslinked type)" and "6.5.1 Liquid crystal material b. Polymerizable nematic liquid crystal material" in Liquid Crystal Handbook (edited by Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 2000), as well as the polymerizable liquid crystal compounds described in JP 2010-31223 A, JP 2010-270108 A, JP 2011-6360 A, JP 2011-207765 A, JP 2011-162678 A, JP 2016-81035 A, WO 2017 / 043438 A and JP 2011-207765 A.
[0121] Examples of a method for producing a retardation film from a polymer in an aligned state of a polymerizable liquid crystal compound include the method described in JP-A-2010-31223.
[0122] In the second embodiment, the front retardation value Re(550) may be adjusted to a range of 0 to 10 nm, preferably 0 to 5 nm, and the thickness retardation value Rth The retardation value R in the thickness direction, which means the refractive index anisotropy in the thickness direction, may be adjusted to the range of -10 to -300 nm, preferably -20 to -200 nm. th is the phase difference value R measured by tilting the in-plane fast axis by 50 degrees. 50 and the in-plane retardation value R0. That is, the retardation value R th is the in-plane retardation value R0, and the retardation value R measured at a 50 degree inclination with the fast axis as the tilt axis. 50 From the thickness d of the retardation film and the average refractive index n0 of the retardation film, n is calculated by the following formulas (10) to (12). x , n y and n z and then substituting these values into equation (9) to perform the calculation.
[0123] R th =[(n x +n y ) / 2-n z ]×d (9) R0=(n x -n y )×d (10) R 50 =(n x -n y ')×d / cos(φ) (11) (n x +n y +n z ) / 3=n0(12) Where: φ=sin -1 [sin(40°) / n0] n y '=n y ×n z / 〔n y 2 ×sin 2 (φ)+n z 2 ×cos 2 (φ) 1 / 2
[0124] The retardation film may be a multilayer film having two or more layers. For example, a retardation film having a protective film laminated on one or both sides thereof, or a retardation film having two or more retardation films laminated via a pressure-sensitive adhesive or adhesive may be mentioned.
[0125] When the optical film 40 is a multilayer film in which two or more retardation films are laminated, the optical laminate including the optical film of the present invention may have a configuration including an optical film 40 in which a ¼ wavelength retardation layer 50 that imparts a ¼ wavelength retardation to transmitted light and a ½ wavelength retardation layer 70 that imparts a ½ wavelength retardation to transmitted light are laminated via an adhesive or pressure-sensitive adhesive 60, as shown in Fig. 4. In addition, as shown in Fig. 5, a configuration including an optical film 40 in which a ¼ wavelength retardation layer 50a and a positive C layer 80 are laminated via an adhesive layer or pressure-sensitive adhesive layer may also be used.
[0126] The 1 / 4 wavelength retardation layer 50 that imparts a phase difference of 1 / 4 wavelength and the 1 / 2 wavelength retardation layer 70 that imparts a phase difference of 1 / 2 wavelength to transmitted light in Fig. 4 may be the optical film of the first embodiment or the optical film of the fifth embodiment. In the case of the configuration of Fig. 4, it is more preferable that at least one of them is the fifth embodiment.
[0127] In the case of the configuration of FIG. 5, the quarter-wave retardation layer 50a is preferably the optical film of the first embodiment, and more preferably satisfies formulas (7) and (8).
[0128] A polarizing film is a film that has the property of absorbing linearly polarized light with a vibration plane parallel to its absorption axis and transmitting linearly polarized light with a vibration plane perpendicular to its absorption axis (parallel to its transmission axis), and can be, for example, a film in which a dichroic dye is adsorbed and oriented on a polyvinyl alcohol-based resin film. Examples of dichroic dyes include iodine and dichroic organic dyes.
[0129] Usually, a film of a polyvinyl alcohol-based resin is used as the raw film of the polarizing film. The polyvinyl alcohol-based resin can be formed into a film by a known method. The thickness of the raw film is usually 1 to 150 μm, and is preferably 10 μm or more in consideration of ease of stretching.
[0130] A polarizing film is produced, for example, by subjecting a raw film to a process of uniaxially stretching, a process of dyeing the film with a dichroic dye to adsorb the dichroic dye, a process of treating the film with an aqueous boric acid solution, a process of washing the film with water, and finally drying. The thickness of the polarizing film is usually 1 to 30 μm, and from the viewpoint of thinning, it is preferably 20 μm or less, more preferably 15 μm or less, and particularly preferably 10 μm or less.
[0131] The polarizing film obtained by adsorbing and orienting a dichroic dye on a polyvinyl alcohol-based resin film can be obtained by a method (referred to as method (1)) in which a single film of a polyvinyl alcohol-based resin film is used as a raw film and the film is subjected to uniaxial stretching and dyeing with a dichroic dye, and also by a method (referred to as method (2)) in which a coating liquid (such as an aqueous solution) containing a polyvinyl alcohol-based resin is applied to a substrate film and dried to obtain a substrate film having a polyvinyl alcohol-based resin layer, and then the substrate film is uniaxially stretched with each substrate film, the stretched polyvinyl alcohol-based resin layer is subjected to dyeing with a dichroic dye, and then the substrate film is peeled off. As the substrate film, a film made of a thermoplastic resin can be used, and preferably a film made of a polyester-based resin such as polyethylene terephthalate, a polycarbonate-based resin, a cellulose-based resin such as triacetyl cellulose, a cyclic polyolefin-based resin such as norbornene-based resin, a polystyrene-based resin, or the like. By using the above method (2), it is easy to prepare a thin polarizing film, and even a polarizer 2 having a thickness of, for example, 7 μm or less can be easily prepared.
[0132] At least one surface of the polarizing film is preferably provided with a protective film via an adhesive. As the adhesive, a known adhesive is used, and it may be a water-based adhesive or an active energy ray curable adhesive.
[0133] Examples of the aqueous adhesive include conventional aqueous adhesives (for example, an adhesive made of an aqueous polyvinyl alcohol resin solution, an aqueous two-liquid urethane emulsion adhesive, an aldehyde compound, an epoxy compound, a melamine compound, a methylol compound, an isocyanate compound, an amine compound, a crosslinking agent such as a polyvalent metal salt, etc.). Of these, an aqueous adhesive made of an aqueous polyvinyl alcohol resin solution can be preferably used. When an aqueous adhesive is used, it is preferable to carry out a drying step to remove water contained in the aqueous adhesive after laminating the polarizing film and the protective film. After the drying step, a curing step of curing at a temperature of, for example, about 20 to 45°C may be provided.
[0134] The active energy ray-curable adhesive refers to an adhesive that is cured by irradiation with active energy rays such as ultraviolet rays or electron beams. Examples of the active energy ray-curable adhesive include a curable composition containing a polymerizable compound and a photopolymerization initiator, a curable composition containing a photoreactive resin, and a curable composition containing a binder resin and a photoreactive crosslinking agent. An ultraviolet ray-curable adhesive is preferred.
[0135] When an active energy ray curable adhesive is used, a drying step is performed as necessary after laminating the polarizing film and the protective film, and then a curing step is performed in which the active energy ray curable adhesive is cured by irradiating the active energy ray. The light source of the active energy ray is not particularly limited, but ultraviolet light having an emission distribution of a wavelength of 400 nm or less is preferable.
[0136] Examples of a method for laminating a polarizing film and a protective film include a method of performing a surface activation treatment such as a saponification treatment, a corona treatment, a plasma treatment, etc., on at least one of the laminating surfaces of the polarizing film. When resin films are laminated to both sides of the polarizing film, the adhesives for laminating these resin films may be the same or different.
[0137] A preferred configuration of the polarizing plate is a polarizing plate in which a protective film is laminated on at least one surface of the polarizing film via an adhesive layer. When the protective film is laminated on only one surface of the polarizing film, it is more preferable that the protective film is laminated on the viewing side. The protective film laminated on the viewing side is preferably a protective film made of a triacetyl cellulose resin or a cycloolefin resin. The protective film may be an unstretched film, or may be stretched in any direction and have a phase difference. A surface treatment layer such as a hard coat layer or an anti-glare layer may be provided on the surface of the protective film laminated on the viewing side. When the protective film is laminated on both sides of the polarizing film, the protective film on the panel side (opposite the viewing side) is preferably a protective film or a retardation film made of a triacetyl cellulose resin, a cycloolefin resin, or an acrylic resin. The retardation film may be a zero retardation film described later. Other layers or films may be laminated between the polarizing plate and the panel. When used as a circular polarizing plate for an organic EL display, it is preferable that a retardation layer having a 1 / 4 wavelength retardation layer and a 1 / 2 wavelength retardation layer, and a 1 / 4 wavelength layer having reverse wavelength dispersion described later are laminated. From the viewpoint of thinning, it is preferable that the retardation layer is a liquid crystal retardation film.
[0138] The light-condensing film is used for the purpose of controlling the light path, and can be a prism array sheet, a lens array sheet, a dot-applied sheet, or the like.
[0139] Brightness enhancing films are used for the purpose of improving the brightness of liquid crystal displays to which polarizing plates are applied. Specific examples include a reflective polarizing separation sheet designed to generate anisotropy in reflectance by laminating a plurality of thin films having mutually different anisotropies in refractive index, and a circular polarizing separation sheet in which an oriented film of a cholesteric liquid crystal polymer or an oriented liquid crystal layer of the cholesteric liquid crystal polymer is supported on a substrate film.
[0140] The window film means a front panel in a flexible display device such as a flexible display, and is generally disposed on the outermost surface of the display device. The window film may be, for example, a resin film made of polyimide resin. The window film may be, for example, a hybrid film of an organic material and an inorganic material, such as a resin film containing polyimide and silica. In addition, the window film may have a hard coat layer disposed on its surface to provide surface hardness, antifouling properties, and fingerprint resistance. For example, the film described in JP 2017-94488 A may be mentioned.
[0141] The optical film of the present invention may be used as a protective film for a polarizing plate. As described above, the polarizing plate has a protective film laminated on one or both sides of the polarizing film via an adhesive layer. In a polarizing plate having a protective film laminated on both sides of a polarizer, the optical film of the present invention may be used as the protective film on one side of the polarizer, or the optical film of the present invention may be used as the protective film on both sides. In addition, a polarizing plate using the optical film of the present invention as a protective film of the polarizing plate may be laminated with another optical film via an adhesive layer or a pressure-sensitive adhesive layer. Figures 2 and 3 show an example in which the optical film of the present invention is used as a protective film of a polarizing plate.
[0142] The adhesive layer 5 is a layer formed from a known adhesive. The known adhesive may be a water-based adhesive or an active energy ray curable adhesive. The pressure-sensitive adhesive layer 6 may be a layer formed from the above-mentioned pressure-sensitive adhesive or a layer formed from another known pressure-sensitive adhesive.
[0143] The protective film 4 may be a known thermoplastic resin film. The protective film 4 may be the optical film of the present invention.
[0144] The optical film of the present invention can be suitably used in a liquid crystal display device. EXAMPLES
[0145] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. In the examples, % and parts representing the content or amount used are based on mass unless otherwise specified.
[0146] <Synthesis of light-selective absorbing compounds> [Synthesis Example 1] Synthesis of light selective absorption compound (1) [ka] A 200mL-four-neck flask equipped with a Dimroth condenser and a thermometer was filled with nitrogen, and 10 g of the compound represented by formula (aa) synthesized with reference to patent document (JP 2014-194508), 3.6 g of acetic anhydride (manufactured by Wako Pure Chemical Industries, Ltd.), 6.9 g of 2-ethylhexyl cyanoacetate (manufactured by Tokyo Chemical Industry Co., Ltd.), and 60 g of acetonitrile (manufactured by Wako Pure Chemical Industries, Ltd.) were charged and stirred with a magnetic stirrer. At an internal temperature of 25°C, 4.5 g of DIPEA (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise from the dropping funnel over 1 hour, and after the end of the dropwise addition, the internal temperature was kept at 25°C for another 2 hours. After the reaction was completed, acetonitrile was removed using a reduced pressure evaporator, and the mixture was purified by column chromatography (silica gel), and the effluent containing the light-selective absorbing compound (1) represented by formula (aa1) was used to remove the solvent using a reduced pressure evaporator to obtain yellow crystals. The crystals were dried under reduced pressure at 60° C. to obtain 4.6 g of light selective absorbing compound (1) as a yellow powder. The yield was 50%.
[0147] 1 When H-NMR analysis was performed, the following peaks were observed, confirming that light selective absorbing compound (1) was produced. 1 H-NMR(CDCl3)δ:0.87-0.94(m, 6H), 1.32-1.67(m, 8H), 1.59-1.66(m, 2H), 2.0 9(quin, 2H), 3.00(m, 5H), 3.64(t, 2H), 4.10(dd, 2H), 5.52(d, 2H), 7.87(d, 2H)
[0148] <Gram absorption coefficient ε measurement> In order to measure the gram absorption coefficient of the obtained light-selective absorbing compound (1), the light-selective absorbing compound (1) was dissolved in 2-butanone. The obtained solution (concentration: 0.007 g / L) was placed in a 1 cm quartz cell, and the quartz cell was set in a spectrophotometer UV-2450 (manufactured by Shimadzu Corporation), and the absorbance was measured in the wavelength range of 300 to 800 nm in 1 nm steps by the double beam method. The gram absorption coefficient for each wavelength was calculated using the following formula from the obtained absorbance value, the concentration of the light-absorbing compound in the solution, and the optical path length of the quartz cell. ε(λ)=A(λ) / CL (where ε(λ) is the gram absorption coefficient L / (g cm) of the compound at a wavelength of λ nm, A(λ) is the absorbance at a wavelength of λ nm, C is the concentration g / L, and L is the optical path length of the quartz cell cm.) The gram absorbance coefficient of the photoselective absorbing compound (1) was ε(405)=47 L / (g·cm), ε(440)=0.1 L / (g·cm) or less, and ε(405) / ε(440)=80 or more.
[0149] [Synthesis Example 2] Synthesis of light selective absorption compound (1) [ka] In a 200mL-four-neck flask equipped with a Dimroth condenser and a thermometer, 10g of the compound represented by formula (aa) synthesized with reference to JP 2014-194508, 3.6g of acetic anhydride (manufactured by Wako Pure Chemical Industries, Ltd.), 10g of 2-butyloctyl cyanoacetate (manufactured by Tokyo Chemical Industry Co., Ltd.), and 60g of acetonitrile (manufactured by Wako Pure Chemical Industries, Ltd.) were charged in a nitrogen atmosphere and stirred with a magnetic stirrer. At an internal temperature of 25°C, 4.5g of DIPEA (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise to the resulting mixture over 1 hour, and the mixture was then kept at an internal temperature of 25°C for another 2 hours. Thereafter, acetonitrile was removed using a reduced pressure evaporator, and the mixture was purified by column chromatography (silica gel), and the solvent was removed from the effluent containing the compound represented by formula (aa2) using a reduced pressure evaporator to obtain yellow crystals. The crystals were dried under reduced pressure at 60° C. to obtain 4.6 g of a compound represented by formula (aa2) (light selective absorption compound (2)) as a yellow powder. The yield was 56%. When the gram absorptivity coefficient was calculated using the same method as above, the ε(405) value of the compound represented by formula (aa4) was 45 L / (g·cm) and the ε(420) value was 2.1 L / (g·cm).
[0150] <Preparation of optical film> [Example 1] Preparation of optical film (1) A cellulose acylate solution (solid concentration: 10% by mass) consisting of cellulose triacetate (acetyl substitution degree: 2.87; Fujifilm Wako Pure Chemical Industries, Ltd., product name "Cellulose triacetate"), light selective absorption compound (1) (3 parts by mass per 100 parts by mass of cellulose triacetate), and a solvent (a mixture of methylene chloride and ethanol, mass ratio 87:13) was placed in a mixing tank and stirred to dissolve each component. The obtained solution was uniformly cast onto a glass support using an applicator, dried in an oven at 40° C. for 10 minutes, and then further dried in an oven at 80° C. for 10 minutes. After drying, the optical film (1) was peeled off from the glass support to obtain an optical film (1) having selective light absorption ability. The film thickness of the optical film (1) after drying was 30 μm.
[0151] <Measurement of storage modulus> The obtained optical film (1) was cut into a size of 5 mm x 30 mm. The cut light selective absorption layer (A-1) was held with a gripping distance of 2 cm using a dynamic viscoelasticity measuring device "DVA-220" manufactured by IT Measurement and Control Co., Ltd. so that the long side of the cut light selective absorption layer (A-1) was in the tensile direction, and the storage modulus E' at temperatures of 23°C to 200°C was determined by setting the tensile and contraction frequency to 10 Hz and the heating rate to 10°C / min. The storage modulus E' at 23°C was 4100 MPa.
[0152] [Example 2] Preparation of optical film (2) A cellulose acylate solution (solid concentration: 5% by mass) consisting of cellulose triacetate (acetyl substitution degree: 2.87; Fujifilm Wako Pure Chemical Industries, Ltd., product name "Cellulose triacetate"), light selective absorption compound (2) (2 parts by mass per 100 parts by mass of cellulose triacetate), and a solvent (a mixture of methylene chloride and ethanol, mass ratio 90:10) was placed in a mixing tank and stirred to dissolve each component. The obtained solution was uniformly cast onto a glass support using an applicator, dried in an oven at 40°C for 10 minutes, and then further dried in an oven at 80°C for 10 minutes. After drying, the optical film (2) was peeled off from the glass support to obtain an optical film (2) having light selective absorption ability. The film thickness of the optical film (2) after drying was 20 μm. The storage modulus of the obtained optical film (2) was measured in the same manner as above, and the storage modulus E' at 23°C was 3800 MPa.
[0153] <Synthesis of (meth)acrylic resin> [Synthesis Example 3] A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer was charged with 81.8 parts of ethyl acetate as a solvent, 70.4 parts of butyl acrylate, 20.0 parts of methyl acrylate as monomers, and 8.0 parts of 2-phenoxyethyl acrylate, 1.0 parts of 2-hydroxyethyl acrylate and 0.6 parts of acrylic acid. The air in the reaction vessel was replaced with nitrogen gas, and the internal temperature was then adjusted to 60°C. Then, a solution in which 0.12 parts of azobisisobutyronitrile was dissolved in 10 parts of ethyl acetate was added. After maintaining the temperature at the same temperature for 1 hour, ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / Hr while maintaining the internal temperature at 54-56°C so that the polymer concentration was approximately 35%. The internal temperature was maintained at 54-56°C until 12 hours had elapsed since the start of the addition of ethyl acetate, and then ethyl acetate was added to adjust the polymer concentration to 20%, to obtain an ethyl acetate solution (1) of a (meth)acrylic resin. The (meth)acrylic resin had a weight average molecular weight Mw of 1.39 million, and a ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn of 5.32.
[0154] The weight-average molecular weight and number-average molecular weight were measured using a GPC apparatus with four "TSK gel XL (Tosoh Corporation)" columns and one "Shodex GPC KF-802 (Showa Denko K.K.)" columns connected in series, a total of five columns, and tetrahydrofuran as the eluent under the conditions of a sample concentration of 5 mg / mL, a sample introduction amount of 100 μL, a temperature of 40° C., and a flow rate of 1 mL / min, and were calculated in terms of standard polystyrene.
[0155] <Synthesis of (meth)acrylic resin pressure-sensitive adhesive composition (1)> [Production Example 1] The ethyl acetate solution (1) of the (meth)acrylic resin obtained above (resin concentration: 20%) was mixed with 0.4 parts of a crosslinking agent (Coronate L, solid content 75%: manufactured by Tosoh Corporation) and 0.4 parts of a silane compound (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) per 100 parts of solid content of the solution, and ethyl acetate was further added to give a solid content concentration of 14%, thereby obtaining a pressure-sensitive adhesive composition (1). Note that the amount of the crosslinking agent is the number of parts by mass as an active ingredient.
[0156] The crosslinking agent and silane compound used in Production Example 1 are as follows. Crosslinking agent: an ethyl acetate solution (solids concentration 75%) of a trimethylolpropane adduct of tolylene diisocyanate, trade name "Coronate L" obtained from Tosoh Corporation. Silane compound: 3-glycidoxypropyltrimethoxysilane, trade name "KBM403" obtained from Shin-Etsu Chemical Co., Ltd.
[0157] <Preparation of adhesive layer> [Production Example 2] The adhesive composition (1) prepared in Production Example 1 was applied to the release-treated surface of a separate film made of a release-treated polyethylene terephthalate film (product name "PLR-382190" available from Lintec Corporation) using an applicator so that the thickness after drying would be 20 μm, and the coating was dried at 100° C. for 1 minute to produce an adhesive layer (1).
[0158] <Synthesis of (meth)acrylic pressure-sensitive adhesive composition (2)> [Production Example 3] An ethyl acetate solution (1) (resin concentration: 20%) of the (meth)acrylic resin obtained in Synthesis Example 3 was mixed with 0.4 parts of a crosslinker (Coronate L, solid content 75%: manufactured by Tosoh), 0.4 parts of a silane compound (KBM-403: manufactured by Shin-Etsu Chemical Co., Ltd.), and 2 parts of the light selective absorbing compound (1) synthesized in Synthesis Example 1 relative to 100 parts of the solid content of the solution, and ethyl acetate was further added to give a solid content concentration of 14%, to obtain a pressure-sensitive adhesive composition (2). The blending amount of the crosslinker (Coronate L) is the number of parts by mass as an active ingredient.
[0159] <Preparation of Pressure-Sensitive Adhesive Layer (2)> The pressure-sensitive adhesive composition (2) prepared above was applied to the release-treated surface of a separate film made of a release-treated polyethylene terephthalate film (product name "PLR-382190" available from Lintec Corporation) using an applicator so that the thickness after drying would be 20 μm, and the coating was dried at 100° C. for 1 minute to produce a pressure-sensitive adhesive layer (2).
[0160] <Synthesis of (meth)acrylic pressure-sensitive adhesive composition (3)> [Production Example 4] A pressure-sensitive adhesive composition (3) was obtained in the same manner as in Synthesis Example 6, except that the light selective absorption compound was changed to the light selective absorption compound (2). The obtained pressure-sensitive adhesive composition (3) was applied to the release-treated surface of a separate film made of a release-treated polyethylene terephthalate film (product name "PLR-382190" available from Lintec Corporation) using an applicator so that the thickness after drying would be 20 μm, and the coating was dried at 100° C. for 1 minute to produce a pressure-sensitive adhesive layer (3).
[0161] <Evaluation> Example 3 After a corona discharge treatment was performed on one side of the optical film (1) obtained in Example 1, the acrylic adhesive produced in Production Example 1 was laminated using a laminator, and the laminate was aged for 7 days under conditions of a temperature of 23°C and a relative humidity of 65%, to obtain an optical film with an adhesive. Next, the optical film with the adhesive was cut into a size of 30 mm x 30 mm and laminated to an alkali-free glass (trade name "EAGLE XG" manufactured by Corning Incorporated) to prepare a sample. The absorbance of the prepared sample in the wavelength range of 300 to 800 nm was measured using a spectrophotometer (UV-2450: manufactured by Shimadzu Corporation). The sample after the measurement was placed in a weather resistance tester (Sunshine Weather Meter: manufactured by Suga Test Instruments Co., Ltd.) and subjected to a weather resistance test for 24 hours, after which the absorbance of the sample taken out was measured again. From the measured absorbance, the absorbance retention rate of the sample at 405 nm was calculated based on the following formula. The results are shown in Table 1. The closer the absorbance retention rate is to 100, the less the selective light absorption function deteriorates and the better the weather resistance is. Note that the absorption of non-alkali glass at wavelengths of 405 nm and 440 nm is almost zero. Absorbance retention rate = A(405) after durability test / A(405) before durability test × 100
[0162] Example 4 The optical film (2) was evaluated in the same manner as in Example 3, except that the optical film was replaced with the optical film (2) obtained in Example 2. The results are shown in Table 1.
[0163] <Comparative Example 1> The evaluation was carried out in the same manner as in Example 3, except that a corona discharge treatment was performed on one side of a 40 μm-thick triacetyl cellulose film (trade name "KC4CW" obtained from Konica) and then the adhesive layer (2) was attached using a laminator.
[0164] <Comparative Example 2> The evaluation was carried out in the same manner as in Example 3, except that a corona discharge treatment was performed on one side of a 40 μm-thick triacetyl cellulose film (trade name "KC4CW" available from Konica) and then the adhesive layer (3) was attached using a laminator.
[0165] [Table 1]
[0166] The optical film of the present invention has a good light absorption ability (A(405)) at a wavelength of about 405 nm. Therefore, when the optical film of the present invention is laminated on a retardation film or an organic EL element, the optical film of the present invention absorbs short-wavelength visible light at a wavelength of about 405 nm, and can block short-wavelength visible light to the retardation film or the organic EL element, thereby suppressing deterioration of the retardation film or the organic EL element from short-wavelength visible light. The optical film of the present invention has good light absorption function (good absorbance retention) at a wavelength of about 405 nm even after weather resistance testing, and has good weather resistance (durability). Therefore, the optical film of the present invention can maintain the function of suppressing deterioration of a retardation film or an organic EL element caused by short-wavelength visible light. In addition, the optical film of the present invention has low light absorption performance at a wavelength of about 440 nm, does not inhibit the light emission of a liquid crystal display device, and is capable of good color expression. [Industrial Applicability]
[0167] The optical film of the present invention is suitably used in liquid crystal panels and liquid crystal display devices. [Explanation of symbols]
[0168] 1. Optical film of the present invention 2 Adhesive layer 3 Separate film 4 Protective film 5 Adhesive layer 6 Polarizing Film 7, 7a Adhesive layer 8 Protective Film 30 Light emitting element 40 Optical Film 50, 50a 1 / 4 wavelength retardation layer 60 Adhesive layer 70 1 / 2 wavelength retardation layer 80 Positive C Layer 10 Optical film with adhesive layer 100 Polarizing Plate 10A, 10B, 10C, 10D Optical laminate
Claims
1. An optical film formed from a resin composition containing a resin (A) and a light selective absorbing compound (B) (excluding cases where the light selective absorbing compound (B) is an indole-based compound or a benzotriazole-based compound), The resin (A) is at least one resin selected from the group consisting of a cellulose-based resin, a (meth)acrylic-based resin, a polyester-based resin, a polyamide-based resin, a polyimide-based resin, and a cycloolefin-based resin; An optical film satisfying the following formula (1) and formula (2') (excluding the case where the optical film contains a fluorescent whitening agent): A(405)≧0.5 (1) A(440)≦0.04 (2') [In formula (1), A(405) represents absorbance at a wavelength of 405 nm. In formula (2'), A(440) represents absorbance at a wavelength of 440 nm.
2. The optical film according to claim 1 , which satisfies the following formula (2″): A(440)≦0.03 (2'') [In formula (2″), A(440) represents the absorbance at a wavelength of 440 nm.]
3. The optical film according to claim 1 or 2, further satisfying the following formula (3): A(405) / A(440)≧5 (3) [In formula (3), A(405) represents the absorbance at a wavelength of 405 nm, and A(440) represents the absorbance at a wavelength of 440 nm.]
4. 4. The optical film according to claim 1, wherein the storage modulus E at 23° C. is 100 MPa or more.
5. 5. The optical film according to claim 1, wherein the content of the light selective absorption compound (B) is 0.01 to 20 parts by mass based on 100 parts by mass of the resin (A).
6. 6. The optical film according to claim 1, wherein the light selective absorption compound (B) is a compound satisfying formula (4). ε(405)≧20 (4) (In formula (5), ε(405) represents the gram absorption coefficient of the compound at a wavelength of 405 nm. The unit of the gram absorption coefficient is L / (g cm).)
7. 7. The optical film according to claim 6, wherein the light selective absorption compound (B) is a compound satisfying formula (5). ε(405) / ε(440)≧20 (5) [In formula (6), ε(405) represents the gram absorbance coefficient of the compound at a wavelength of 405 nm, and ε(440) represents the gram absorbance coefficient at a wavelength of 440 nm.]
8. 8. The optical film according to claim 1, wherein the light selective absorption compound (B) is a compound having a merocyanine structure in the molecule.
9. The optical film according to claim 1 , which satisfies the following formula (2′″): A(440)≦0.018 (2''') [In formula (2'''), A(440) represents the absorbance at a wavelength of 440 nm.]
10. 10. An optical film with adhesive, comprising the optical film according to claim 1, and an adhesive layer on at least one surface of the optical film.
11. A display device comprising the pressure-sensitive adhesive optical film according to claim 10.
Citation Information
Patent Citations
Ultraviolet-ray shielding film
JP1996287715A
Filter for organic electroluminescent display element
JP2004102223A
Polarizing plate and liquid crystal display device
JP2006308936A
Optical filter, and lighting fixture using same
JP2007180040A
Outdoor display device
JP2014115524A