Microcrystalline glass, microcrystalline glass product and method for producing same

A tailored microcrystalline glass composition with specific components and a lithium monosilicate phase addresses the issues of poor chemical strength and haze in existing glasses, providing enhanced mechanical and optical performance for electronic and display applications.

JP7580603B2Active Publication Date: 2024-11-11CDGM OPTICAL GLASS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023528126
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-31
Filing Date
2021-09-26
Publication Date
2024-11-11
Estimated Expiration
2041-09-26

AI Technical Summary

Technical Problem

Commercially available microcrystalline glasses suffer from poor chemical strength, high haze, and large |B| value, making them unsuitable for high-performance display and electronic devices.

Method used

A microcrystalline glass composition comprising SiO2, Al2O3, Li2O, ZrO2, P2O5, and Y2O3, with optional additives like K2O, MgO, ZnO, Na2O, SrO, BaO, TiO2, B2O3, and Ln2O3, optimized to achieve a lithium monosilicate crystalline phase with specific component ratios and properties, enhancing mechanical and optical performance.

Benefits of technology

The optimized microcrystalline glass exhibits improved mechanical strength, reduced haze, and lower |B| value, suitable for use in electronic equipment and display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580603000001
    Figure 0007580603000001
  • Figure 0007580603000002
    Figure 0007580603000002
  • Figure 0007580603000003
    Figure 0007580603000003
Patent Text Reader

Abstract

The present invention provides a microcrystalline glass product, which contains the following components by weight: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, and Y2O3: greater than 0 and not greater than 8%. Thanks to a rational component design, the microcrystalline glass and microcrystalline glass product of the present invention have excellent mechanical and optical properties and are suitable for electronic devices and display devices.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to microcrystalline glass, a microcrystalline glass product, and a method for producing the same, and in particular to microcrystalline glass that has excellent mechanical properties and optical properties and is suitable for electronic devices or display devices, a microcrystalline glass product, and a method for producing the same. [Background technology]

[0002] Microcrystalline glass is a material in which crystals are precipitated inside the glass by heat-treating the glass, and has better mechanical properties than ordinary glass. Microcrystals are formed in the glass, and its bending resistance, wear resistance, drop resistance, and other properties are far superior to those of ordinary glass. On the other hand, the mechanical properties of microcrystalline glass can also be further improved by chemical strengthening.

[0003] Based on the above advantages, microcrystalline glass or the glass products obtained after its processing are currently applied to display devices and electronic devices that have high requirements for drop resistance, pressure resistance, scratch resistance, etc., and are especially popular for the front and rear covers of portable electronic devices (such as mobile phones, watches, PADs, etc.).

[0004] With the development of science and technology, the requirements for the optical performance of glass materials used in electronic devices or displays are becoming higher. Optical performance refers to the performance expressed when a material absorbs, reflects, and refracts light, and includes transmittance, haze, |B| value, and refractive index. However, microcrystalline glass currently on the market has problems such as poor chemical strength performance, high haze, and high |B| value, making it difficult to use it in displays and electronic devices with high performance requirements.

[0005] Therefore, the development of microcrystalline glass and microcrystalline glass products having excellent mechanical and optical properties and suitable for use in displays and electronic devices has become a goal pursued by scientists and engineers. Summary of the Invention [Problem to be solved by the invention]

[0006] The technical problem that the present invention seeks to solve is to provide a microcrystalline glass product having excellent mechanical and optical properties. [Means for solving the problem]

[0007] The technical solutions adopted in the present invention to solve the technical problems are as follows:

[0008] (1) A microcrystalline glass product containing the following components by weight: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, Y2O3: 0-8% or less.

[0009] (2) The microcrystalline glass product according to (1), further comprising the following components by weight: K2O: 0-5%, and / or MgO: 0-2%, and / or ZnO: 0-2%, and / or Na2O: 0-6%, and / or SrO: 0-5%, and / or BaO: 0-5%, and / or CaO: 0-5%, and / or TiO2: 0-5%, and / or B2O3: 0-5%, and / or Ln2O3: 0-5%, and / or a fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0010] (3) A microcrystalline glass product comprising SiO2, Al2O3, Li2O, ZrO2, P2O5, and Y2O3, wherein a crystalline phase of the microcrystalline glass product comprises lithium monosilicate, and the weight percentage of lithium monosilicate is greater than other crystalline phases.

[0011] (4) A microcrystalline glass product containing SiO2, Al2O3, Li2O, ZrO2 and P2O5, the microcrystalline glass product having a thickness of 1 mm or less and an average light |B| value of 400 to 800 nm of 0.6 or less.

[0012] (5) A microcrystalline glass product containing a lithium monosilicate crystalline phase, said microcrystalline glass product having a ball drop test height of 1300 mm or more.

[0013] (6) A microcrystalline glass product according to any one of (3) to (5), comprising the following components in weight percent: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, and Y2O3: more than 0 and not more than 8%.

[0014] (7) The microcrystalline glass product according to any one of (3) to (6), further comprising the following components in weight percent: K2O: 0-5%, and / or MgO: 0-2%, and / or ZnO: 0-2%, and / or Na2O: 0-6%, and / or SrO: 0-5%, and / or BaO: 0-5%, and / or CaO: 0-5%, and / or TiO2: 0-5%, and / or B2O3: 0-5%, and / or Ln2O3: 0-5%, and / or a fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0015] (8) A microcrystalline glass product comprising the following components by weight: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, Y2O3: more than 0 and not more than 8%, K2O: 0-5%, MgO: 0-2%, ZnO: 0-2%, Na2O: 0-6%, SrO: 0-5%, BaO: 0-5%, CaO: 0-5%, TiO2: 0-5%, B2O3: 0-5%, Ln2O3: 0-5%, and fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0016] (9) A microcrystalline glass product according to any one of (1) to (8), in which the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is greater than 0; 2) (Li2O+ZrO2+P2O5) / Y2O3 is 2.5~50.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.16~0.9; 4) Na2O / Y2O3 is 6.0 or less; 5) Y2O3 / (Al2O3+SiO2) is greater than 0 and less than 0.15.

[0017] (10) A microcrystalline glass product according to any one of (1) to (9), comprising the following components in weight percent: SiO2: 50-65%, and / or Al2O3: 8-15%, and / or Li2O: 13-22%, and / or ZrO2: 6-12%, and / or P2O5: 3.5-9%, and / or K2O: 0-4%, and / or MgO: 0-1%, and / or ZnO: 0-1%, and / or Na2O: 1-5%, and / or Y2O3: 1-7%, and / or SrO: 0-3%, and / or is BaO: 0-3%, and / or CaO: 0-3%, and / or TiO2: 0-3%, and / or B2O3: 0-3%, and / or Ln2O3: 0-4%, and / or fining agent: 0-1%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0018] (11) A microcrystalline glass product according to any one of (1) to (10), in which the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is 0.1~1.0; 2) (Li2O+ZrO2+P2O5) / Y2O3 is 3.0~40.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.18~0.6; 4) Na2O / Y2O3 is 0.1-5.0; 5) Y2O3 / (Al2O3+SiO2) is 0.01~0.12.

[0019] (12) A microcrystalline glass product according to any one of (1) to (11), comprising the following components in weight percent: SiO2: 53-63%, and / or Al2O3: 8-12%, and / or Li2O: 14-21%, and / or ZrO2: 7-12%, and / or P2O5: 4-8%, and / or K2O: 0-2%, and / or Y2O3: 2-6%, and / or B2O3: 0-2%, and / or Na2O: 1.5-4%. %, and / or SrO: 0-1%, and / or TiO2: 0-1%, and / or BaO: 0-1%, and / or CaO: 0-1%, and / or Ln2O3: 0-3%, and / or fining agent: 0-0.5%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0020] (13) A microcrystalline glass product according to any one of (1) to (12), in which the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is 0.2~0.6; 2) (Li2O+ZrO2+P2O5) / Y2O3 is 4.0~21.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.19~0.5; 4) Na2O / Y2O3 is 0.3~2.0; 5) Y2O3 / (Al2O3+SiO2) is 0.03~0.09.

[0021] (14) A microcrystalline glass product according to any one of (1) to (13), wherein the components do not contain SrO, and / or do not contain BaO, and / or do not contain CaO, and / or do not contain ZnO, and / or do not contain PbO, and / or do not contain As2O3, and / or do not contain TiO2, and / or do not contain B2O3, and / or do not contain Ln2O3, and / or do not contain F, and / or do not contain Ta2O5.

[0022] (15) A microcrystalline glass product according to any one of (1) to (14), wherein the crystalline phase of the microcrystalline glass product contains lithium monosilicate and / or lithium phosphate.

[0023] (16) A microcrystalline glass product according to any one of (1) to (15), wherein the crystalline phase of the microcrystalline glass product mainly comprises lithium monosilicate, the weight percentage of lithium monosilicate being higher than that of other crystalline phases, the lithium monosilicate comprising 10% to 63.5%, preferably 15 to 55%, of the microcrystalline glass product.

[0024] (17) The microcrystalline glass product according to any one of (1) to (16), wherein the microcrystalline glass product contains a lithium phosphate crystal phase, and the weight percentage of the lithium phosphate crystal phase in the microcrystalline glass product is 3 to 15%, preferably 5 to 12%.

[0025] (18) A microcrystalline glass product according to any one of (1) to (17), wherein the microcrystalline glass product has a surface stress of 600 MPa or more, preferably 650 MPa or more, and more preferably 700 MPa or more.

[0026] (19) A microcrystalline glass product according to any one of (1) to (18), wherein the microcrystalline glass product has a four-point bending strength of 600 MPa or more, preferably 650 MPa or more, and more preferably 700 MPa or more.

[0027] (20) A microcrystalline glass product according to any one of (1) to (19), wherein the depth of the ion exchange layer of the microcrystalline glass product is 20 μm or more, preferably 30 μm or more, more preferably 40 μm or more.

[0028] (21) A microcrystalline glass product according to any one of (1) to (20), wherein the microcrystalline glass product has a ball drop test height of 1300 mm or more, preferably 1400 mm or more, more preferably 1500 mm or more.

[0029] (22) The microcrystalline glass product has a fracture toughness of 1 MPa m 1 / 2More than 1.1 MPa m, preferably 1 / 2 More preferably, 1.2 MPa m 1 / 2 The microcrystalline glass product according to any one of (1) to (21) above.

[0030] (23) The Vickers hardness of the microcrystalline glass product is 700 kgf / mm 2 More than 720kgf / mm 2 More preferably, 730kgf / mm 2 The microcrystalline glass product according to any one of (1) to (22) above.

[0031] (24) A microcrystalline glass product according to any one of (1) to (23), wherein the crystallinity of the microcrystalline glass product is 50% or more, preferably 60% or more, and more preferably 70% or more.

[0032] (25) A microcrystalline glass product according to any one of (1) to (24), wherein the crystal grain size of the microcrystalline glass product is 50 nm or less, preferably 40 nm or less, more preferably 30 nm or less.

[0033] (26) A microcrystalline glass product according to any one of (1) to (15), in which the haze of the microcrystalline glass product having a thickness of 1 mm or less is 0.15% or less, preferably 0.12% or less, more preferably 0.1% or less.

[0034] (27) A microcrystalline glass product according to any one of (1) to (26), in which the microcrystalline glass product has a thickness of 1 mm or less and has an average transmittance of 89% or more at wavelengths of 400 to 800 nm.

[0035] (28) A microcrystalline glass product according to any one of (1) to (27), in which the microcrystalline glass product has a thickness of 1 mm or less and has a transmittance at a wavelength of 550 nm of 91% or more.

[0036] (29) A microcrystalline glass product according to any one of (1) to (28), in which the average light |B| value at 400 to 800 nm of the microcrystalline glass product having a thickness of 1 mm or less is 0.6 or less, preferably 0.55 or less, and more preferably 0.5 or less.

[0037] (30) A microcrystalline glass product according to any one of (26) to (29), wherein the thickness of the microcrystalline glass product is 0.2 to 1 mm, preferably 0.3 to 0.9 mm, more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.72 mm, or 0.75 mm.

[0038] (31) A microcrystalline glass product according to any one of (1) to (7), which contains a colorant.

[0039] (32) The microcrystalline glass product according to (31), wherein the coloring agent contains the following components by weight: NiO: 0-4%, and / or Ni2O3: 0-4%, and / or CoO: 0-2%, and / or Co2O3: 0-2%, and / or Fe2O3: 0-7%, and / or MnO2: 0-4%, and / or Er2O3: 0-8%, and / or Nd2O3: 0-8%, and / or Cu2O: 0-4%, and / or Pr2O3: 0-8%, and / or CeO2: 0-4%.

[0040] (33) A microcrystalline glass product according to any one of (31) or (32), wherein the coloring agent comprises, in weight percent, the following components: NiO: 0.1-4%, and / or Ni2O3: 0.1-4%, and / or CoO: 0.05-2%, and / or Co2O3: 0.05-2%, and / or Fe2O3: 0.2-7%, and / or MnO2: 0.1-4%, and / or Er2O3: 0.4-8%, and / or Nd2O3: 0.4-8%, and / or Cu2O: 0.5-4%, and / or Pr2O3: 0.4-8%, and / or CeO2: 0.5-4%.

[0041] (34) A microcrystalline glass product according to any one of (31) or (32), wherein the coloring agent comprises, in weight percent, the following components: NiO: 0.1-3%, and / or Ni2O3: 0.1-3%, and / or CoO: 0.05-1.8%, and / or Co2O3: 0.05-1.8%, and / or Fe2O3: 0.2-5%, and / or MnO2: 0.1-3%, and / or Er2O3: 0.4-6%, and / or Nd2O3: 0.4-6%, and / or Cu2O: 0.5-3%, and / or Pr2O3: 0.4-6%, and / or CeO2: 0.5-3%.

[0042] (35) The microcrystalline glass product according to any one of (31) or (32), wherein the colorant contains the following components in weight percent: NiO: 0.1-3%, and / or Ni2O3: 0.1-3%.

[0043] (36) The microcrystalline glass product according to any one of (31) or (32), wherein the colorant contains the following components in weight percent: CoO: 0.05-1.8%, and / or Co2O3: 0.05-1.8%.

[0044] (37) A microcrystalline glass product according to any one of (31) or (32), wherein the colorant contains the following components in weight percent: Cu2O: 0.5-3%, and / or CeO2: 0.5-3%.

[0045] (38) A microcrystalline glass product according to any one of (31) or (32), in which the colorant contains the following components by weight: Fe2O3: 0.2-5%, CoO: 0.05-0.3%, or Fe2O3: 0.2-5%, Co2O3: 0.05-0.3%, or Fe2O3: 0.2-5%, CoO: 0.05-0.3%, NiO: 0.1-1%, or Fe2O3: 0.2-5%, Co2O3: 0.05-0.3%, NiO: 0.1-1%.

[0046] (39) A microcrystalline glass product according to any one of (31) or (32), wherein the coloring agent contains the following components in weight percent: Pr2O3: 0.4-6%, or Fe2O3: 0.2-5%, or MnO2: 0.1-3%, or Er2O3: 0.4-6%, or Nd2O3: 0.4-6%.

[0047] (40) The microcrystalline glass product according to any one of (31) or (32), wherein the coloring agent contains the following components in weight percent: Er2O3: 0.4-6%, Nd2O3: 0.4-4%, MnO2: 0.1-2%.

[0048] The present invention also provides microcrystalline glasses that have excellent mechanical and optical properties.

[0049] The technical solutions adopted in the present invention to solve the technical problems are as follows:

[0050] (41) Microcrystalline glass containing the following components by weight: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, Y2O3: 0.0 to 8%.

[0051] (42) The microcrystalline glass according to (41), further comprising the following components by weight: K2O: 0-5%, and / or MgO: 0-2%, and / or ZnO: 0-2%, and / or Na2O: 0-6%, and / or SrO: 0-5%, and / or BaO: 0-5%, and / or TiO2: 0-5%, and / or CaO: 0-5%, and / or B2O3: 0-5%, and / or Ln2O3: 0-5%, and / or a fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0052] (43) A microcrystalline glass comprising SiO2, Al2O3, Li2O, ZrO2, P2O5, and Y2O3, wherein a crystalline phase of the microcrystalline glass comprises lithium monosilicate, and the weight percentage of the lithium monosilicate is higher than other crystalline phases.

[0053] (44) A microcrystalline glass containing SiO2, Al2O3, Li2O, ZrO2, and P2O5, the microcrystalline glass having a thickness of 1 mm or less and an average light |B| value of 0.6 or less from 400 to 800 nm.

[0054] (45) A microcrystalline glass containing a lithium monosilicate crystal phase, the microcrystalline glass having a ball drop test height of 1000 mm or more.

[0055] (46) The microcrystalline glass according to any one of (43) to (45), containing the following components in weight percent: SiO2: 45 to 70%, Al2O3: 8 to 18%, Li2O: 10 to 25%, ZrO2: 5 to 15%, P2O5: 2 to 10%, and Y2O3: more than 0 and not more than 8%.

[0056] (47) The microcrystalline glass according to any one of (43) to (46), further comprising the following components in weight percent: K2O: 0-5%, and / or MgO: 0-2%, and / or ZnO: 0-2%, and / or Na2O: 0-6%, and / or SrO: 0-5%, and / or BaO: 0-5%, and / or CaO: 0-5%, and / or TiO2: 0-5%, and / or B2O3: 0-5%, and / or Ln2O3: 0-5%, and / or a fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0057] (48) A microcrystalline glass comprising the following components by weight: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, Y2O3: more than 0 and not more than 8%, K2O: 0-5%, MgO: 0-2%, ZnO: 0-2%, Na2O: 0-6%, SrO: 0-5%, BaO: 0-5%, CaO: 0-5%, TiO2: 0-5%, B2O3: 0-5%, Ln2O3: 0-5%, and a fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0058] (49) A microcrystalline glass according to any one of (41) to (48), wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is greater than 0. 2) (Li2O+ZrO2+P2O5) / Y2O3 is 2.5~50.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.16~0.9; 4) Na2O / Y2O3 is 6.0 or less; 5) Y2O3 / (Al2O3+SiO2) is greater than 0 and less than 0.15.

[0059] (50) A microcrystalline glass according to any one of (41) to (49), comprising the following components in weight percent: SiO2: 50-65%, and / or Al2O3: 8-15%, and / or Li2O: 13-22%, and / or ZrO2: 6-12%, and / or P2O5: 3.5-9%, and / or K2O: 0-4%, and / or MgO: 0-1%, and / or ZnO: 0-1%, and / or Na2O: 1-5%, and / or Y2O3: 1-7%, and / or SrO: 0-3%, and / or is TiO2: 0-3%, and / or BaO: 0-3%, and / or CaO: 0-3%, and / or B2O3: 0-3%, and / or Ln2O3: 0-4%, and / or fining agent: 0-1%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0060] (51) A microcrystalline glass according to any one of (41) to (50), wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is 0.1~1.0; 2) (Li2O+ZrO2+P2O5) / Y2O3 is 3.0~40.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.18~0.6; 4) Na2O / Y2O3 is 0.1-5.0; 5) Y2O3 / (Al2O3+SiO2) is 0.01~0.12.

[0061] (52) A microcrystalline glass according to any one of (41) to (51), comprising the following components by weight: SiO2: 53-63%, and / or Al2O3: 8-12%, and / or Li2O: 14-21%, and / or ZrO2: 7-12%, and / or P2O5: 4-8%, and / or K2O: 0-2%, and / or Y2O3: 2-6%, and / or B2O3: 0-2%, and / or Na2O: 1.5-4%, and / or SrO: 0-1%, and / or is TiO2: 0-1%, and / or BaO: 0-1%, and / or CaO: 0-1%, and / or Ln2O3: 0-3%, and / or fining agent: 0-0.5%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0062] (53) A microcrystalline glass according to any one of (41) to (52), wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is 0.2~0.6; 2) (Li2O+ZrO2+P2O5) / Y2O3 is 4.0~21.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.19~0.5; 4) Na2O / Y2O3 is 0.3~2.0; 5) Y2O3 / (Al2O3+SiO2) is 0.03~0.09.

[0063] (54) The microcrystalline glass according to any one of (41) to (53), wherein the components do not contain SrO, and / or do not contain BaO, and / or do not contain CaO, and / or do not contain ZnO, and / or do not contain PbO, and / or do not contain As2O3, and / or do not contain TiO2, and / or do not contain B2O3, and / or do not contain Ln2O3, and / or do not contain F, and / or do not contain Ta2O5.

[0064] (55) The microcrystalline glass according to any one of (41) to (54), wherein the crystalline phase of the microcrystalline glass contains lithium monosilicate and / or lithium phosphate.

[0065] (56) Microcrystalline glass according to any one of (41) to (55), wherein the crystalline phase of the microcrystalline glass product mainly comprises lithium monosilicate, the weight percentage of lithium monosilicate being higher than that of other crystalline phases, the lithium monosilicate comprising 10% to 63.5%, preferably 15 to 55%, of the microcrystalline glass.

[0066] (57) The microcrystalline glass according to any one of (41) to (56), wherein the crystal phase of the microcrystalline glass contains a lithium phosphate crystal phase, and the weight percentage of the lithium phosphate crystal phase in the microcrystalline glass is 3 to 15%, preferably 5 to 12%.

[0067] (58) The microcrystalline glass according to any one of (41) to (57), wherein the degree of crystallinity of the microcrystalline glass is 50% or more, preferably 60% or more, and more preferably 70% or more.

[0068] (59) The microcrystalline glass according to any one of (41) to (58), wherein the crystal grain size of the microcrystalline glass is 50 nm or less, preferably 40 nm or less, and more preferably 30 nm or less.

[0069] (60) The thermal expansion coefficient of the microcrystalline glass is 75 to 95 × 10 -7 The microcrystalline glass according to any one of (41) to (59), wherein:

[0070] (61) The microcrystalline glass according to any one of (41) to (60), which has a refractive index of 1.5700 to 1.5800.

[0071] (62) The microcrystalline glass according to any one of (41) to (61), wherein the microcrystalline glass has a body drop ball test height of 1000 mm or more, preferably 1100 mm or more, and more preferably 1200 mm or more.

[0072] (63) The Vickers hardness of the microcrystalline glass is 650 kgf / mm 2 More than 680 kgf / mm 2 More preferably, 700kgf / mm 2 The microcrystalline glass according to any one of (41) to (62) above.

[0073] (64) The microcrystalline glass according to any one of (41) to (63), in which the haze of the microcrystalline glass having a thickness of 1 mm or less is 0.15% or less, preferably 0.12% or less, and more preferably 0.1% or less.

[0074] (65) The microcrystalline glass according to any one of (41) to (64), wherein the microcrystalline glass has a thickness of 1 mm or less and has an average transmittance of 89% or more at wavelengths of 400 to 800 nm.

[0075] (66) The microcrystalline glass according to any one of (41) to (65), which has a thickness of 1 mm or less and a transmittance at a wavelength of 550 nm of 91% or more.

[0076] (67) A microcrystalline glass product according to any one of (41) to (66), in which the average light |B| value at 400 to 800 nm of the microcrystalline glass having a thickness of 1 mm or less is 0.6 or less, preferably 0.55 or less, and more preferably 0.5 or less.

[0077] (68) The microcrystalline glass according to any one of (64) to (67), wherein the thickness of the microcrystalline glass is 0.2 to 1 mm, preferably 0.3 to 0.9 mm, more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.72 mm, or 0.75 mm.

[0078] (69) The microcrystalline glass according to any one of (41) to (47), which contains a colorant.

[0079] (70) The microcrystalline glass according to (69), wherein the colorant contains the following components by weight: NiO: 0-4%, and / or Ni2O3: 0-4%, and / or CoO: 0-2%, and / or Co2O3: 0-2%, and / or Fe2O3: 0-7%, and / or MnO2: 0-4%, and / or Er2O3: 0-8%, and / or Nd2O3: 0-8%, and / or Cu2O: 0-4%, and / or Pr2O3: 0-8%, and / or CeO2: 0-4%.

[0080] (71) The microcrystalline glass according to any one of (69) or (70), wherein the colorant contains the following components by weight: NiO: 0.1-4%, and / or Ni2O3: 0.1-4%, and / or CoO: 0.05-2%, and / or Co2O3: 0.05-2%, and / or Fe2O3: 0.2-7%, and / or MnO2: 0.1-4%, and / or Er2O3: 0.4-8%, and / or Nd2O3: 0.4-8%, and / or Cu2O: 0.5-4%, and / or Pr2O3: 0.4-8%, and / or CeO2: 0.5-4%.

[0081] (72) The microcrystalline glass according to any one of (69) or (70), wherein the colorant contains the following components by weight: NiO: 0.1-3%, and / or Ni2O3: 0.1-3%, and / or CoO: 0.05-1.8%, and / or Co2O3: 0.05-1.8%, and / or Fe2O3: 0.2-5%, and / or MnO2: 0.1-3%, and / or Er2O3: 0.4-6%, and / or Nd2O3: 0.4-6%, and / or Cu2O: 0.5-3%, and / or Pr2O3: 0.4-6%, and / or CeO2: 0.5-3%.

[0082] (73) The microcrystalline glass according to any one of (69) or (70), wherein the colorant contains the following components in weight percent: NiO: 0.1 to 3%, and / or Ni2O3: 0.1 to 3%.

[0083] (74) The microcrystalline glass according to either one of (69) or (70), wherein the colorant contains the following components in weight percent: CoO: 0.05 to 1.8%, and / or Co2O3: 0.05 to 1.8%.

[0084] (75) The microcrystalline glass according to any one of (69) or (70), wherein the colorant contains the following components in weight percent: Cu2O: 0.5 to 3%, and / or CeO2: 0.5 to 3%.

[0085] (76) The microcrystalline glass according to any one of (69) or (70), wherein the colorant contains the following components by weight: Fe2O3: 0.2-5%, CoO: 0.05-0.3%, or Fe2O3: 0.2-5%, Co2O3: 0.05-0.3%, or Fe2O3: 0.2-5%, CoO: 0.05-0.3%, NiO: 0.1-1%, or Fe2O3: 0.2-5%, Co2O3: 0.05-0.3%, NiO: 0.1-1%.

[0086] (77) The microcrystalline glass according to any one of (69) or (70), wherein the colorant contains the following components by weight: Pr2O3: 0.4-6%, or Fe2O3: 0.2-5%, or MnO2: 0.1-3%, or Er2O3: 0.4-6%, or Nd2O3: 0.4-6%.

[0087] (78) The microcrystalline glass according to either (69) or (70), wherein the colorant contains the following components by weight: Er2O3: 0.4 to 6%, Nd2O3: 0.4 to 4%, MnO2: 0.1 to 2%.

[0088] The present invention also provides a matrix glass.

[0089] The technical solutions adopted in the present invention to solve the technical problems are as follows:

[0090] (79) A matrix glass containing the following components by weight: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, Y2O3: 0.0 to 8%.

[0091] (80) The matrix glass according to (79), further comprising the following components in weight percent: K2O: 0-5%, and / or MgO: 0-2%, and / or ZnO: 0-2%, and / or Na2O: 0-6%, and / or SrO: 0-5%, and / or BaO: 0-5%, and / or CaO: 0-5%, and / or TiO2: 0-5%, and / or B2O3: 0-5%, and / or Ln2O3: 0-5%, and / or a fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0092] (81) A matrix glass comprising the following components by weight: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, Y2O3: more than 0 and 8% or less, K2O: 0-5%, MgO: 0-2%, ZnO: 0-2%, Na2O: 0-6%, SrO: 0-5%, BaO: 0-5%, CaO: 0-5%, TiO2: 0-5%, B2O3: 0-5%, Ln2O3: 0-5%, and a fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0093] (82) A matrix glass according to any one of (79) to (81), wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is greater than 0. 2) (Li2O+ZrO2+P2O5) / Y2O3 is 2.5~50.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.16~0.9; 4) Na2O / Y2O3 is 6.0 or less; 5) Y2O3 / (Al2O3+SiO2) is greater than 0 and less than 0.15. (83) A matrix glass according to any one of (79) to (82), comprising the following components in weight percent: SiO2: 50-65%, and / or Al2O3: 8-15%, and / or Li2O: 13-22%, and / or ZrO2: 6-12%, and / or P2O5: 3.5-9%, and / or K2O: 0-4%, and / or MgO: 0-1%, and / or ZnO: 0-1%, and / or Na2O: 1-5%, and / or Y2O3: 1-7%, and / or SrO: 0-3%, and / or is TiO2: 0-3%, and / or BaO: 0-3%, and / or CaO: 0-3%, and / or B2O3: 0-3%, and / or Ln2O3: 0-4%, and / or fining agent: 0-1%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0094] (84) A matrix glass according to any one of (79) to (83), wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is 0.1~1.0; 2) (Li2O+ZrO2+P2O5) / Y2O3 is 3.0~40.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.18~0.6; 4) Na2O / Y2O3 is 0.1-5.0; 5) Y2O3 / (Al2O3+SiO2) is 0.01~0.12.

[0095] (85) A matrix glass according to any one of (79) to (84), comprising the following components in weight percent: SiO2: 53-63%, and / or Al2O3: 8-12%, and / or Li2O: 14-21%, and / or ZrO2: 7-12%, and / or P2O5: 4-8%, and / or K2O: 0-2%, and / or Y2O3: 2-6%, and / or B2O3: 0-2%, and / or Na2O: 1.5-4%, and / or SrO: 0-1%, and / or is TiO2: 0-1%, and / or BaO: 0-1%, and / or CaO: 0-1%, and / or Ln2O3: 0-3%, and / or fining agent: 0-0.5%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0096] (86) A matrix glass according to any one of (79) to (85), wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is 0.2~0.6; 2) (Li2O+ZrO2+P2O5) / Y2O3 is 4.0~21.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.19~0.5; 4) Na2O / Y2O3 is 0.3~2.0; 5) Y2O3 / (Al2O3+SiO2) is 0.03~0.09.

[0097] (87) The matrix glass according to any one of (79) to (86), wherein the components do not contain SrO, and / or do not contain BaO, and / or do not contain CaO, and / or do not contain ZnO, and / or do not contain PbO, and / or do not contain As2O3, and / or do not contain TiO2, and / or do not contain B2O3, and / or do not contain Ln2O3, and / or do not contain F, and / or do not contain Ta2O5.

[0098] (88) The thermal expansion coefficient of the matrix glass is 50×10 -7 / K~70×10 -7 / K.

[0099] (89) The matrix glass according to any one of (79) to (88), which has a refractive index of 1.5600 to 1.5700.

[0100] (90) The matrix glass according to any one of (79) to (80), which contains a colorant.

[0101] (91) The matrix glass according to (90), wherein the colorant contains the following components by weight: NiO: 0-4%, and / or Ni2O3: 0-4%, and / or CoO: 0-2%, and / or Co2O3: 0-2%, and / or Fe2O3: 0-7%, and / or MnO2: 0-4%, and / or Er2O3: 0-8%, and / or Nd2O3: 0-8%, and / or Cu2O: 0-4%, and / or Pr2O3: 0-8%, and / or CeO2: 0-4%.

[0102] (92) The matrix glass according to (90) or (91), wherein the colorant contains the following components by weight: NiO: 0.1-4%, and / or Ni2O3: 0.1-4%, and / or CoO: 0.05-2%, and / or Co2O3: 0.05-2%, and / or Fe2O3: 0.2-7%, and / or MnO2: 0.1-4%, and / or Er2O3: 0.4-8%, and / or Nd2O3: 0.4-8%, and / or Cu2O: 0.5-4%, and / or Pr2O3: 0.4-8%, and / or CeO2: 0.5-4%.

[0103] (93) The matrix glass according to (90) or (91), wherein the colorant contains the following components by weight: NiO: 0.1-3%, and / or Ni2O3: 0.1-3%, and / or CoO: 0.05-1.8%, and / or Co2O3: 0.05-1.8%, and / or Fe2O3: 0.2-5%, and / or MnO2: 0.1-3%, and / or Er2O3: 0.4-6%, and / or Nd2O3: 0.4-6%, and / or Cu2O: 0.5-3%, and / or Pr2O3: 0.4-6%, and / or CeO2: 0.5-3%.

[0104] (94) The matrix glass according to (90) or (91), wherein the colorant contains the following components by weight: NiO: 0.1 to 3%, and / or Ni2O3: 0.1 to 3%.

[0105] (95) The matrix glass according to (90) or (91), wherein the colorant contains the following components by weight: CoO: 0.05 to 1.8%, and / or Co2O3: 0.05 to 1.8%.

[0106] (96) The matrix glass according to (90) or (91), wherein the colorant contains the following components by weight: Cu2O: 0.5 to 3%, and / or CeO2: 0.5 to 3%.

[0107] (97) The matrix glass according to (90) or (91), wherein the colorant contains the following components by weight: Fe2O3: 0.2 to 5%, CoO: 0.05 to 0.3%, or Fe2O3: 0.2 to 5%, Co2O3: 0.05 to 0.3%, or Fe2O3: 0.2 to 5%, CoO: 0.05 to 0.3%, NiO: 0.1 to 1%, or Fe2O3: 0.2 to 5%, Co2O3: 0.05 to 0.3%, NiO: 0.1 to 1%.

[0108] (98) The matrix glass according to (90) or (91), wherein the colorant contains the following components by weight: Pr2O3: 0.4 to 6%, or Fe2O3: 0.2 to 5%, or MnO2: 0.1 to 3%, or Er2O3: 0.4 to 6%, or Nd2O3: 0.4 to 6%.

[0109] (99) The matrix glass according to (90) or (91), wherein the colorant contains the following components by weight: Er2O3: 0.4 to 6%, Nd2O3: 0.4 to 4%, MnO2: 0.1 to 2%.

[0110] The present invention also provides a glass cover plate.

[0111] (100) A glass cover plate comprising a microcrystalline glass product according to any one of (1) to (40), and / or a microcrystalline glass according to any one of (41) to (78), and / or a matrix glass according to any one of (79) to (99).

[0112] The present invention also provides a glass element.

[0113] (101) A glass element comprising a microcrystalline glass product according to any one of (1) to (40), and / or a microcrystalline glass according to any one of (41) to (78), and / or a matrix glass according to any one of (79) to (99).

[0114] The present invention also provides a display device.

[0115] (102) A display device comprising a microcrystalline glass product according to any one of (1) to (40), and / or a microcrystalline glass according to any one of (41) to (78), and / or a matrix glass according to any one of (79) to (99), and / or a glass cover plate according to (100), and / or a glass element according to (101).

[0116] The present invention also provides an electronic device.

[0117] (103) An electronic device comprising a microcrystalline glass product according to any one of (1) to (40), and / or a microcrystalline glass according to any one of (41) to (78), and / or a matrix glass according to any one of (79) to (99), and / or a glass cover plate according to (100), and / or a glass element according to (101).

[0118] The present invention also provides a method for making a microcrystalline glass article.

[0119] (104) A method for producing a microcrystalline glass product, said method comprising the steps of: A matrix glass is formed, and the matrix glass contains the following components by weight: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, Y2O3: more than 0 and 8% or less. The matrix glass is subjected to a crystallization process to form a microcrystalline glass, and the microcrystalline glass is further subjected to a chemical strengthening process to form a microcrystalline glass product.

[0120] (105) A method for producing a microcrystalline glass product according to (104), wherein the matrix glass further comprises the following components by weight: K2O: 0-5%, and / or MgO: 0-2%, and / or ZnO: 0-2%, and / or Na2O: 0-6%, and / or SrO: 0-5%, and / or TiO2: 0-5%, and / or BaO: 0-5%, and / or CaO: 0-5%, and / or B2O3: 0-5%, and / or Ln2O3: 0-5%, and / or a fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0121] (106) A method for producing a microcrystalline glass product, said method comprising the steps of: A matrix glass is formed, and the matrix glass is composed of the following components by weight: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, Y2O3: more than 0 and 8% or less, K2O: 0-5%, MgO: 0-2%, ZnO: 0-2%, Na2O: 0-6%, SrO: 0-5%, TiO2: 0-5%, BaO: 0-5%, CaO: 0-5%, B2O3: 0-5%, Ln2O3: 0-5%, and a fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br. The matrix glass is subjected to a crystallization process to form a microcrystalline glass, and the microcrystalline glass is further subjected to a chemical strengthening process to form a microcrystalline glass product.

[0122] (107) A method for producing a microcrystalline glass product according to any one of (104) to (106), wherein the components of the matrix glass are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is greater than 0. 2) (Li2O+ZrO2+P2O5) / Y2O3 is 2.5~50.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.16~0.9; 4) Na2O / Y2O3 is 6.0 or less; 5) Y2O3 / (Al2O3+SiO2) is greater than 0 and less than 0.15.

[0123] (108) A method for producing a microcrystalline glass product according to any one of (104) to (107), wherein the matrix glass contains the following components by weight: SiO2: 50-65%, and / or Al2O3: 8-15%, and / or Li2O: 13-22%, and / or ZrO2: 6-12%, and / or P2O5: 3.5-9%, and / or K2O: 0-4%, and / or MgO: 0-1%, and / or ZnO: 0-1%, and / or Na2O: 1-5%, and / or Y2O3: 1-7%, and / or SrO: 0-3%, and / or is TiO2: 0-3%, and / or BaO: 0-3%, and / or CaO: 0-3%, and / or B2O3: 0-3%, and / or Ln2O3: 0-4%, and / or fining agent: 0-1%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0124] (109) A method for producing a microcrystalline glass product according to any one of (104) to (108), wherein the components of the matrix glass, expressed in weight percent, satisfy one or more of the following five conditions: 1) Y2O3 / ZrO2 is 0.1~1.0; 2) (Li2O+ZrO2+P2O5) / Y2O3 is 3.0~40.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.18~0.6; 4) Na2O / Y2O3 is 0.1-5.0; 5) Y2O3 / (Al2O3+SiO2) is 0.01~0.12.

[0125] (110) A method for producing a microcrystalline glass product according to any one of (104) to (109), wherein the matrix glass contains the following components by weight: SiO2: 53-63%, and / or Al2O3: 8-12%, and / or Li2O: 14-21%, and / or ZrO2: 7-12%, and / or P2O5: 4-8%, and / or K2O: 0-2%, and / or Y2O3: 2-6%, and / or B2O3: 0-2%, and / or Na2O: 1.5-4%, and / or SrO: 0-1%, and / or is TiO2: 0-1%, and / or BaO: 0-1%, and / or CaO: 0-1%, and / or Ln2O3: 0-3%, and / or fining agent: 0-0.5%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0126] (111) A method for producing a microcrystalline glass product according to any one of (104) to (110), wherein the components of the matrix glass, expressed in weight percent, satisfy one or more of the following five conditions: 1) Y2O3 / ZrO2 is 0.2~0.6; 2) (Li2O+ZrO2+P2O5) / Y2O3 is 4.0~21.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.19~0.5; 4) Na2O / Y2O3 is 0.3~2.0; 5) Y2O3 / (Al2O3+SiO2) is 0.03~0.09.

[0127] (112) A method for producing a microcrystalline glass product according to any one of (104) to (111), wherein the matrix glass components do not contain SrO, and / or do not contain BaO, and / or do not contain CaO, and / or do not contain ZnO, and / or do not contain PbO, and / or do not contain As2O3, and / or do not contain TiO2, and / or do not contain B2O3, and / or do not contain Ln2O3, and / or do not contain F, and / or do not contain Ta2O5.

[0128] (113) The method for producing microcrystalline glass according to any one of (104) to (105), wherein the matrix glass contains a colorant.

[0129] (114) A method for producing microcrystalline glass according to (113), wherein the colorant contains the following components by weight: NiO: 0-4%, and / or Ni2O3: 0-4%, and / or CoO: 0-2%, and / or Co2O3: 0-2%, and / or Fe2O3: 0-7%, and / or MnO2: 0-4%, and / or Er2O3: 0-8%, and / or Nd2O3: 0-8%, and / or Cu2O: 0-4%, and / or Pr2O3: 0-8%, and / or CeO2: 0-4%.

[0130] (115) A method for producing microcrystalline glass according to any one of (113) or (114), wherein the colorant contains the following components by weight: NiO: 0.1-4%, and / or Ni2O3: 0.1-4%, and / or CoO: 0.05-2%, and / or Co2O3: 0.05-2%, and / or Fe2O3: 0.2-7%, and / or MnO2: 0.1-4%, and / or Er2O3: 0.4-8%, and / or Nd2O3: 0.4-8%, and / or Cu2O: 0.5-4%, and / or Pr2O3: 0.4-8%, and / or CeO2: 0.5-4%.

[0131] (116) A method for producing microcrystalline glass according to any one of (113) or (114), wherein the colorant contains the following components by weight: NiO: 0.1-3%, and / or Ni2O3: 0.1-3%, and / or CoO: 0.05-1.8%, and / or Co2O3: 0.05-1.8%, and / or Fe2O3: 0.2-5%, and / or MnO2: 0.1-3%, and / or Er2O3: 0.4-6%, and / or Nd2O3: 0.4-6%, and / or Cu2O: 0.5-3%, and / or Pr2O3: 0.4-6%, and / or CeO2: 0.5-3%.

[0132] (117) The method for producing microcrystalline glass according to any one of (113) or (114), wherein the colorant contains the following components in weight percent: NiO: 0.1 to 3%, and / or Ni2O3: 0.1 to 3%.

[0133] (118) The method for producing microcrystalline glass according to any one of (113) or (114), wherein the colorant contains the following components in weight percent: CoO: 0.05 to 1.8%, and / or Co2O3: 0.05 to 1.8%.

[0134] (119) The method for producing microcrystalline glass according to any one of (113) or (114), wherein the colorant contains the following components in weight percent: Cu2O: 0.5 to 3%, and / or CeO2: 0.5 to 3%.

[0135] (120) A method for producing microcrystalline glass according to any one of (113) or (114), wherein the colorant contains the following components by weight: Fe2O3: 0.2-5%, CoO: 0.05-0.3%, or Fe2O3: 0.2-5%, Co2O3: 0.05-0.3%, or Fe2O3: 0.2-5%, CoO: 0.05-0.3%, NiO: 0.1-1%, or Fe2O3: 0.2-5%, Co2O3: 0.05-0.3%, NiO: 0.1-1%.

[0136] (121) A method for producing microcrystalline glass according to any one of (113) or (114), wherein the colorant contains the following components by weight: Pr2O3: 0.4-6%, or Fe2O3: 0.2-5%, or MnO2: 0.1-3%, or Er2O3: 0.4-6%, or Nd2O3: 0.4-6%.

[0137] (122) The method for producing microcrystalline glass according to any one of (113) or (114), wherein the colorant contains the following components in weight percent: Er2O3: 0.4 to 6%, Nd2O3: 0.4 to 4%, MnO2: 0.1 to 2%.

[0138] (123) A method for producing a microcrystalline glass product according to any one of (104) to (122), wherein the crystallization step comprises the steps of: raising the temperature to a predetermined crystallization temperature, maintaining the temperature for a certain period of time after the crystallization temperature is reached, and then lowering the temperature. The crystallization temperature is 600 to 750°C, preferably 650 to 700°C, and the maintenance time at the crystallization temperature is 0 to 8 hours, preferably 1 to 6 hours.

[0139] (124) A method for producing a microcrystalline glass product according to any one of (104) to (122), wherein the crystallization step comprises the steps of: carrying out a nucleation step at a first temperature, and then carrying out a crystal growth step at a second temperature higher than the temperature of the nucleation step.

[0140] (125) A method for producing a microcrystalline glass product according to (124), wherein the crystallization step comprises the following steps: a first temperature of 470-630°C, a second temperature of 650-750°C, a holding time at the first temperature of 0-24 hours, preferably 2-15 hours, and a holding time at the second temperature of 0-10 hours, preferably 0.5-6 hours.

[0141] (126) A method for producing a microcrystalline glass product according to any one of (104) to (125), wherein the chemical strengthening step comprises the steps of: immersing the microcrystalline glass in a salt bath containing molten Na salt at a temperature of 430°C to 470°C for 6 to 20 hours, the temperature range being preferably 435°C to 460°C, for a time range being preferably 8 to 13 hours, and / or immersing the microcrystalline glass in a salt bath containing molten K salt at a temperature of 400°C to 450°C for 1 to 8 hours, the time range being preferably 2 to 4 hours.

[0142] (127) A method for producing a microcrystalline glass product according to any one of (104) to (126), wherein the crystalline phase of the microcrystalline glass product contains lithium monosilicate and / or lithium phosphate.

[0143] (128) A method for producing a microcrystalline glass product according to any one of (104) to (127), wherein the crystalline phase of the microcrystalline glass product mainly comprises lithium monosilicate, the weight percentage of lithium monosilicate is higher than that of other crystalline phases, and the lithium monosilicate accounts for 10% to 63.5%, preferably 15 to 55%, of the microcrystalline glass product.

[0144] (129) A method for producing a microcrystalline glass product according to any one of (104) to (128), wherein the microcrystalline glass product contains a lithium phosphate crystal phase, and the weight percentage of the lithium phosphate crystal phase in the microcrystalline glass product is 3 to 15%, preferably 5 to 12%.

[0145] (130) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the microcrystalline glass product has a surface stress of 600 MPa or more, preferably 650 MPa or more, and more preferably 700 MPa or more.

[0146] (131) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the microcrystalline glass product has a four-point bending strength of 600 MPa or more, preferably 650 MPa or more, and more preferably 700 MPa or more.

[0147] (132) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the microcrystalline glass product has an ion exchange layer depth of 20 μm or more, preferably 30 μm or more, more preferably 40 μm or more.

[0148] (133) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the microcrystalline glass product has a ball drop test height of 1300 mm or more, preferably 1400 mm or more, and more preferably 1500 mm or more.

[0149] (134) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the microcrystalline glass product has a fracture toughness of 1 MPa m 1 / 2More than 1.1 MPa m 1 / 2 More preferably, 1.2 MPa m 1 / 2 That's all.

[0150] (135) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the microcrystalline glass product has a Vickers hardness of 700 kgf / mm 2 More than 720 kgf / mm 2 More preferably, 730 kgf / mm 2 That's all.

[0151] (136) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the microcrystalline glass product has a crystallinity of 50% or more, preferably 60% or more, and more preferably 70% or more.

[0152] (137) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the crystal grain size of the microcrystalline glass product is 50 nm or less, preferably 40 nm or less, more preferably 30 nm or less.

[0153] (138) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the haze of the microcrystalline glass product having a thickness of 1 mm or less is 0.15% or less, preferably 0.12% or less, and more preferably 0.1% or less.

[0154] (139) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the microcrystalline glass product has a thickness of 1 mm or less and has an average transmittance of 89% or more at wavelengths of 400 to 800 nm.

[0155] (140) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the microcrystalline glass product having a thickness of 1 mm or less has a transmittance of 91% or more at a wavelength of 550 nm.

[0156] (141) A method for producing a microcrystalline glass product according to any one of (104) to (112), wherein the microcrystalline glass product has a thickness of 1 mm or less and an average light |B| value at 400 to 800 nm of 0.6 or less, preferably 0.55 or less, more preferably 0.5 or less.

[0157] (142) A method for producing a microcrystalline glass product according to any one of (138) to (141), wherein the microcrystalline glass product has a thickness of 0.2 to 1 mm, preferably 0.3 to 0.9 mm, more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.72 mm, or 0.75 mm.

[0158] The present invention also provides a method for making a microcrystalline glass.

[0159] (143) A method for producing a microcrystalline glass, said method comprising the steps of: A matrix glass is formed, and the matrix glass contains the following components by weight: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, Y2O3: more than 0 and 8% or less. A crystallization process processes the matrix glass into a microcrystalline glass.

[0160] (144) A method for producing microcrystalline glass according to (143), wherein the matrix glass further contains the following components by weight: K2O: 0-5%, and / or MgO: 0-2%, and / or ZnO: 0-2%, and / or Na2O: 0-6%, and / or SrO: 0-5%, and / or TiO2: 0-5%, and / or BaO: 0-5%, and / or CaO: 0-5%, and / or B2O3: 0-5%, and / or Ln2O3: 0-5%, and / or a fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0161] (145) A method for producing a microcrystalline glass, said method comprising the steps of: A matrix glass is formed, and the matrix glass is composed of the following components by weight: SiO2: 45-70%, Al2O3: 8-18%, Li2O: 10-25%, ZrO2: 5-15%, P2O5: 2-10%, Y2O3: more than 0 and 8% or less, K2O: 0-5%, MgO: 0-2%, ZnO: 0-2%, Na2O: 0-6%, SrO: 0-5%, TiO2: 0-5%, BaO: 0-5%, CaO: 0-5%, B2O3: 0-5%, Ln2O3: 0-5%, and a fining agent: 0-2%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br. A crystallization process processes the matrix glass into a microcrystalline glass.

[0162] (146) A method for producing a microcrystalline glass according to any one of (143) to (145), wherein the components of the matrix glass are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is greater than 0. 2) (Li2O+ZrO2+P2O5) / Y2O3 is 2.5~50.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.16~0.9; 4) Na2O / Y2O3 is 6.0 or less; 5) Y2O3 / (Al2O3+SiO2) is greater than 0 and less than 0.15.

[0163] (147) A method for producing a microcrystalline glass according to any one of (143) to (146), wherein the matrix glass contains the following components by weight: SiO2: 50-65%, and / or Al2O3: 8-15%, and / or Li2O: 13-22%, and / or ZrO2: 6-12%, and / or P2O5: 3.5-9%, and / or K2O: 0-4%, and / or MgO: 0-1%, and / or ZnO: 0-1%, and / or Na2O: 1-5%, and / or Y2O3: 1-7%, and / or SrO: 0-3%, and / or is TiO2: 0-3%, and / or BaO: 0-3%, and / or CaO: 0-3%, and / or B2O3: 0-3%, and / or Ln2O3: 0-4%, and / or fining agent: 0-1%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0164] (148) A method for producing a microcrystalline glass according to any one of (143) to (147), wherein the components of the matrix glass are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is 0.1~1.0; 2) (Li2O+ZrO2+P2O5) / Y2O3 is 3.0~40.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.18~0.6; 4) Na2O / Y2O3 is 0.1-5.0; 5) Y2O3 / (Al2O3+SiO2) is 0.01~0.12.

[0165] (149) A method for producing a microcrystalline glass according to any one of (143) to (148), wherein the matrix glass contains the following components by weight: SiO2: 53-63%, and / or Al2O3: 8-12%, and / or Li2O: 14-21%, and / or ZrO2: 7-12%, and / or P2O5: 4-8%, and / or K2O: 0-2%, and / or Y2O3: 2-6%, and / or B2O3: 0-2%, and / or Na2O: 1.5-4%, and / or SrO: 0-1%, and / or is TiO2: 0-1%, and / or BaO: 0-1%, and / or CaO: 0-1%, and / or Ln2O3: 0-3%, and / or fining agent: 0-0.5%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3, and the fining agent is one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br.

[0166] (150) A method for producing a microcrystalline glass according to any one of (143) to (149), wherein the components of the matrix glass are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y2O3 / ZrO2 is 0.2~0.6; 2) (Li2O+ZrO2+P2O5) / Y2O3 is 4.0~21.0; 3) Al2O3 / (Li2O+ZrO2+P2O5) is 0.19~0.5; 4) Na2O / Y2O3 is 0.3~2.0; 5) Y2O3 / (Al2O3+SiO2) is 0.03~0.09.

[0167] (151) A method for producing a microcrystalline glass according to any one of (143) to (150), wherein the components of the matrix glass do not contain SrO, and / or do not contain BaO, and / or do not contain CaO, and / or do not contain ZnO, and / or do not contain PbO, and / or do not contain As2O3, and / or do not contain TiO2, and / or do not contain B2O3, and / or do not contain Ln2O3, and / or do not contain F, and / or do not contain Ta2O5.

[0168] (152) A method for producing microcrystalline glass according to any one of (143) to (144), wherein the matrix glass contains a colorant.

[0169] (153) A method for producing microcrystalline glass according to (152), wherein the colorant contains the following components by weight: NiO: 0-4%, and / or Ni2O3: 0-4%, and / or CoO: 0-2%, and / or Co2O3: 0-2%, and / or Fe2O3: 0-7%, and / or MnO2: 0-4%, and / or Er2O3: 0-8%, and / or Nd2O3: 0-8%, and / or Cu2O: 0-4%, and / or Pr2O3: 0-8%, and / or CeO2: 0-4%.

[0170] (154) A method for producing microcrystalline glass according to any one of (152) or (153), wherein the colorant contains the following components by weight: NiO: 0.1-4%, and / or Ni2O3: 0.1-4%, and / or CoO: 0.05-2%, and / or Co2O3: 0.05-2%, and / or Fe2O3: 0.2-7%, and / or MnO2: 0.1-4%, and / or Er2O3: 0.4-8%, and / or Nd2O3: 0.4-8%, and / or Cu2O: 0.5-4%, and / or Pr2O3: 0.4-8%, and / or CeO2: 0.5-4%.

[0171] (155) A method for producing microcrystalline glass according to any one of (152) or (153), wherein the colorant contains the following components by weight: NiO: 0.1-3%, and / or Ni2O3: 0.1-3%, and / or CoO: 0.05-1.8%, and / or Co2O3: 0.05-1.8%, and / or Fe2O3: 0.2-5%, and / or MnO2: 0.1-3%, and / or Er2O3: 0.4-6%, and / or Nd2O3: 0.4-6%, and / or Cu2O: 0.5-3%, and / or Pr2O3: 0.4-6%, and / or CeO2: 0.5-3%.

[0172] (156) A method for producing microcrystalline glass according to any one of (152) or (153), wherein the colorant contains the following components by weight: NiO: 0.1 to 3%, and / or Ni2O3: 0.1 to 3%.

[0173] (157) A method for producing microcrystalline glass according to any one of (152) or (153), wherein the colorant contains the following components by weight: CoO: 0.05 to 1.8%, and / or Co2O3: 0.05 to 1.8%.

[0174] (158) A method for producing microcrystalline glass according to any one of (152) or (153), wherein the colorant contains the following components by weight: Cu2O: 0.5-3%, and / or CeO2: 0.5-3%.

[0175] (159) A method for producing microcrystalline glass according to any one of (152) and (153), wherein the colorant contains the following components by weight: Fe2O3: 0.2-5%, CoO: 0.05-0.3%, or Fe2O3: 0.2-5%, Co2O3: 0.05-0.3%, or Fe2O3: 0.2-5%, CoO: 0.05-0.3%, NiO: 0.1-1%, or Fe2O3: 0.2-5%, Co2O3: 0.05-0.3%, NiO: 0.1-1%.

[0176] (160) A method for producing microcrystalline glass according to any one of (152) or (153), wherein the colorant contains the following components by weight: Pr2O3: 0.4-6%, or Fe2O3: 0.2-5%, or MnO2: 0.1-3%, or Er2O3: 0.4-6%, or Nd2O3: 0.4-6%.

[0177] (161) A method for producing microcrystalline glass according to any one of (152) or (153), wherein the colorant contains the following components by weight: Er2O3: 0.4-6%, Nd2O3: 0.4-4%, MnO2: 0.1-2%.

[0178] (162) A method for producing microcrystalline glass according to any one of (143) to (161), wherein the crystallization step comprises the steps of: raising the temperature to a predetermined crystallization temperature, maintaining the temperature for a certain period of time after the crystallization temperature is reached, and then lowering the temperature. The crystallization temperature is 600 to 750°C, preferably 650 to 700°C, and the crystallization temperature is maintained for 0 to 8 hours, preferably 1 to 6 hours.

[0179] (163) A method for producing microcrystalline glass according to any one of (143) to (161), wherein the crystallization step includes the following steps: a nucleation step is performed at a first temperature, and then a crystal growth step is performed at a second temperature higher than the temperature of the nucleation step.

[0180] (164) A method for producing microcrystalline glass according to (163), wherein the crystallization step includes the following steps: a first temperature of 470 to 630°C, a second temperature of 650 to 750°C, a holding time at the first temperature of 0 to 24 hours, preferably 2 to 15 hours, and a holding time at the second temperature of 0 to 10 hours, preferably 0.5 to 6 hours.

[0181] (165) A method for producing microcrystalline glass according to any one of (143) to (164), wherein the crystal phase of the microcrystalline glass contains lithium monosilicate and / or lithium phosphate.

[0182] (166) A method for producing microcrystalline glass according to any one of (143) to (165), wherein the crystalline phase of the microcrystalline glass mainly contains lithium monosilicate, the weight percentage of lithium monosilicate is higher than that of other crystalline phases, and the lithium monosilicate accounts for 10% to 63.5%, preferably 15 to 55%, of the microcrystalline glass product.

[0183] (167) A method for producing microcrystalline glass according to any one of (143) to (166), wherein the microcrystalline glass contains a lithium phosphate crystal phase, and the weight percentage of the lithium phosphate crystal phase in the microcrystalline glass is 3 to 15%, preferably 5 to 12%.

[0184] (168) A method for producing microcrystalline glass according to any one of (143) to (151), wherein the microcrystalline glass has a crystallinity of 50% or more, preferably 60% or more, and more preferably 70% or more.

[0185] (169) A method for producing microcrystalline glass according to any one of (143) to (151), wherein the crystal grain size of the microcrystalline glass is 50 nm or less, preferably 40 nm or less, more preferably 30 nm or less, and / or the thermal expansion coefficient is 75 to 95×10 -7 / K.

[0186] (170) A method for producing microcrystalline glass according to any one of (143) to (151), wherein the microcrystalline glass has a refractive index of 1.5700 to 1.5800.

[0187] (171) A method for producing microcrystalline glass according to any one of (143) to (151), wherein the main body falling ball height of the microcrystalline glass is 1000 mm or more, preferably 1100 mm or more, and more preferably 1200 mm or more.

[0188] (172) A method for producing microcrystalline glass according to any one of (143) to (151), wherein the microcrystalline glass has a Vickers hardness of 650 kgf / mm 2 More than 680kgf / mm 2 More preferably, 700kgf / mm 2 That's all.

[0189] (173) A method for producing microcrystalline glass according to any one of (143) to (151), wherein the haze of the microcrystalline glass having a thickness of 1 mm or less is 0.15% or less, preferably 0.12% or less, and more preferably 0.1% or less.

[0190] (174) A method for producing microcrystalline glass according to any one of (143) to (151), wherein the microcrystalline glass having a thickness of 1 mm or less has an average transmittance of 89% or more at wavelengths of 400 to 800 nm.

[0191] (175) A method for producing microcrystalline glass according to any one of (143) to (151), wherein the microcrystalline glass having a thickness of 1 mm or less has a transmittance of 91% or more at a wavelength of 550 nm.

[0192] (176) A method for producing microcrystalline glass according to any one of (143) to (151), wherein the microcrystalline glass has a thickness of 1 mm or less and an average light |B| value at 400 to 800 nm of 0.6 or less, preferably 0.55 or less, and more preferably 0.5 or less.

[0193] (177) The method for producing microcrystalline glass according to any one of (173) to (176), wherein the thickness of the microcrystalline glass is 0.2 to 1 mm, preferably 0.3 to 0.9 mm, more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.72 mm, or 0.75 mm. Effect of the Invention

[0194] The beneficial effects of the present invention are as follows: Due to the rational component design, the microcrystalline glass and microcrystalline glass products obtained by the present invention have excellent mechanical and optical properties, and are suitable for electronic devices and display devices. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0195] The microcrystalline glass and microcrystalline glass products of the present invention are materials having a crystalline phase and a glass phase different from an amorphous solid. The crystalline phase of the microcrystalline glass and microcrystalline glass products can be identified by the peak angle appearing in the X-ray diffraction pattern of X-ray diffraction analysis and / or measured by TEMEDX.

[0196] As a result of extensive testing and research, the inventors have been able to obtain the microcrystalline glass or microcrystalline glass product of the present invention at lower cost by precipitating a specific crystalline phase by specifying the content and content ratio of specific components that make up the microcrystalline glass and microcrystalline glass product to specific values.

[0197] The range of components (ingredients) of the matrix glass, microcrystalline glass, and microcrystalline glass product of the present invention will be described below. In this specification, the content of each component is expressed in weight percent (wt%) of the matrix glass, microcrystalline glass, or microcrystalline glass product converted into an oxide composition, unless otherwise specified. "Converted into an oxide composition" here means that the total weight of oxide substances when oxides, complex salts, hydroxides, etc. used as raw materials for the composition of the matrix glass, microcrystalline glass, or microcrystalline glass product of the present invention are decomposed and converted into oxides during melting is taken as 100%. In this specification, glass refers to matrix glass before microcrystallization, microcrystallized matrix glass is called microcrystalline glass, and microcrystalline glass product refers to microcrystalline glass that has been chemically strengthened.

[0198] Specifically, numerical ranges described herein include upper and lower limits, and "greater than" and "less than" include the endpoints, as well as all integers and fractions contained within the range, and are not limited to the specific values ​​set forth when the range is limited. As used herein, the term "about" indicates that recipes, parameters and other quantities and characteristics are not, and need not be, precise and can be approximated and / or greater or lesser as necessary, to reflect tolerances, conversion factors, measurement errors, and the like. References to "and / or" herein are inclusive, e.g., "A and / or B" means A only, B only, or both A and B.

[0199] In the microcrystalline glasses and microcrystalline glass products of the present invention, the crystalline phase comprises lithium monosilicate and / or lithium phosphate.

[0200] In some embodiments of the invention, the crystalline phase of the microcrystalline glass or microcrystalline glass product comprises primarily lithium monosilicate crystalline phase, the weight percentage of lithium monosilicate is higher than other crystalline phases, and the lithium monosilicate comprises between 10% and 63.5% of the microcrystalline glass or microcrystalline glass product, and in some embodiments the weight percentage range is between 15 and 55%.

[0201] In some embodiments of the present invention, the crystalline phase of the microcrystalline glass or microcrystalline glass product comprises a lithium phosphate crystalline phase, and the weight percent range of the lithium phosphate crystalline phase in the microcrystalline glass or microcrystalline glass product is 3-15%, and in some embodiments the weight percent range is 5-12%.

[0202] SiO2 is an essential component of the glass of the present invention, and is one of the main components that form crystals after heat treatment. If the content of SiO2 is 45% or less, it is difficult to form crystals in the glass. Therefore, the lower limit of the content of SiO2 is 45%, preferably 50%, and more preferably 53%, and if the content of SiO2 is 70% or more, it is disadvantageous to the molding of glass and affects the haze and |B| value of microcrystalline glass and microcrystalline glass products. Therefore, the upper limit of the content of SiO2 is 70%, preferably 65%, and more preferably 63%. In some embodiments, it can contain about 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, and 70% of SiO2.

[0203] As a glass network structure, Al2O3 is advantageous for glass forming, and can lower the crystallization temperature of glass, which is favorable for glass crystallization. Al2O3 is one of the components that form crystals of microcrystalline glass, which is advantageous for chemical strengthening of microcrystalline glass, and can increase the ion exchange layer depth of microcrystalline glass products. However, if its content is less than 8%, the above effect is low, so the lower limit of the content of Al2O3 is 8%. On the other hand, if the content of Al2O3 exceeds 18%, it will affect the size of the fragments after chemical strengthening of microcrystalline glass, so the upper limit of the content of Al2O3 is 18%, preferably 15%, and more preferably 12%. In some embodiments, the Al2O3 may include about 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, or 18% Al2O3.

[0204] Li2O can promote the melting of glass and reduce the melting temperature. It is the main component of crystal formation, and is also a component that mainly replaces sodium and potassium ions in chemical strengthening treatment. It can increase the surface stress of microcrystalline glass products after chemical strengthening and improve the falling height of microcrystalline glass products. However, if its content is less than 10%, the formation effect of lithium monosilicate crystal phase is poor, which affects the falling height and the size of the fragments of the microcrystalline glass products. Therefore, the lower limit of the Li2O content is 10%, preferably 13%, and more preferably 14%. On the other hand, if the Li2O content is too high, the glass is easily phase-separated during microcrystallization, which affects the transmittance of the microcrystalline glass and the microcrystalline glass products. Therefore, the upper limit of the Li2O content is 25%, preferably 22%, and more preferably 21%. Some embodiments can include about 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, or 25% LiO.

[0205] Na2O is an optional component, which can reduce the melting temperature of glass and is advantageous for adjusting the chemical strengthening process of glass or microcrystalline glass. Therefore, the lower limit of the content of Na2O in the present invention is preferably 1%, more preferably 1.5%. On the other hand, if the content of Na2O in glass is too high, it promotes phase separation of glass, and the transmittance of microcrystalline glass and microcrystalline glass products after crystallization decreases. Therefore, the upper limit of the content of Na2O is 6%, preferably 5%, and more preferably 4%. In some embodiments, it can contain about 0%, more than 0%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, or 6% Na2O.

[0206] Although K2O is advantageous for forming glass and reduces the viscosity of glass, if the content of K2O is too high, the chemical stability and hardness of glass will decrease. Therefore, the upper limit of the content of K2O is 5%, preferably 4%, and more preferably 2%. In some embodiments, it can contain about 0%, more than 0%, 0.1%, 0.5%, 1%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, or 5.0% K2O.

[0207] P2O5 can form crystal nuclei in the glass crystallization process, promote the formation of crystals, increase the crystallinity of microcrystalline glass or microcrystalline glass products, and be favorable for chemical strengthening, and can increase the hardness, drop height and bending strength of microcrystalline glass products. Therefore, the lower limit of the content of P2O5 is 2%, preferably 3.5%, and more preferably 4%. However, if the content of P2O5 is too high, the phase separation of glass and the chemical stability of glass will be reduced. Therefore, the upper limit of the content of P2O5 is 10%, preferably 9%, and more preferably 8%. In some embodiments, it can contain about 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, or 10% P2O5.

[0208] ZrO2 and P2O5 can dissolve each other, reduce the phase separation of P2O5 during glass molding, increase the crystallization temperature of glass during crystallization, ensure the completeness of the lithium monosilicate crystal phase in microcrystalline glass and microcrystalline glass products, reduce the haze and |B| value of microcrystalline glass and microcrystalline glass products, and improve the drop resistance of microcrystalline glass products. Therefore, the lower limit of the content of ZrO2 is 5%, preferably 6%, and more preferably 7%. On the other hand, if the content of ZrO2 is too high, it becomes difficult to melt the glass, so the upper limit of the content of ZrO2 is 15%, preferably 12%. Some embodiments may include about 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 10.0%, 10.5%, 11.0%, 11.5%, 12%, 12.5%, 13.0%, 13.5%, 14.0%, 14.5%, or 15.0% ZrO2.

[0209] Y2O3 can promote the melting of ZrO2, reduce the melting difficulty of glass, reduce phase separation in glass, and reduce the haze and |B| value of microcrystalline glass and microcrystalline glass products. Therefore, the lower limit of the content of Y2O3 is more than 0%, preferably 1%, and more preferably 2%. On the other hand, if the content of Y2O3 is too high, it becomes difficult to form crystals during glass crystallization, and the crystallinity of microcrystalline glass and microcrystalline glass products decreases. Therefore, the upper limit of the content of Y2O3 is 8%, preferably 7%, and more preferably 6%. In some embodiments, it can contain about 0% or more, 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, or 8.0% Y2O3.

[0210] After extensive testing and research, the inventors have found that in some embodiments, the relative content of Y2O3 and ZrO2 has an important effect on the haze and |B| value of microcrystalline glass and microcrystalline glass products, and especially when Y2O3 / ZrO2 is greater than 0, it can reduce the haze and |B| value of microcrystalline glass and microcrystalline glass products, and improve the photography and photographic effect of terminal products. Therefore, it is preferred that Y2O3 / ZrO2 is greater than 0, more preferably Y2O3 / ZrO2 is 0.1-1.0, and even more preferably Y2O3 / ZrO2 is 0.2-0.6. In some embodiments, the value of Y2O3 / ZrO2 can be greater than 0, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0.

[0211] In some embodiments of the present invention, (Li2O+ZrO2+P2O5) / Y2O3 is set in the range of 2.5-50.0, which can refine the crystal grains of the matrix glass in the crystallization process, enable the microcrystalline glass and the microcrystalline glass product to obtain finer crystal grains, and reduce the haze of the microcrystalline glass and the microcrystalline glass product. Therefore, it is preferable that (Li2O+ZrO2+P2O5) / Y2O3 is 2.5-50.0, more preferably (Li2O+ZrO2+P2O5) / Y2O3 is 3.0-40.0, and even more preferably (Li2O+ZrO2+P2O5) / Y2O3 is 4.0-21.0. In some embodiments, the value of (Li2O+ZrO2+P2O5) / Y2O3 is 2.5, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0, 12.0, 13.0, 14.0, 15.0, 16.0, 17.0, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, 40.0, 41.0, 42.0, 43.0, 44.0, 45.0, 46.0, 47.0, 48.0, 49.0, 50.0, 51.0, 52.0, 53.0, 54.0, 55.0, 56.0, 57.0, 58.0, 59.0, 60.0, 61.0, 62.0, 63.0, 64.0, 65.0, 66.0, 67.0, 68.0, 69.0, 70.0, 71.0, 72.0, 73.0, 74.0, 75.0, 76.0, 77.0, 78.0, 79.0, 80.0, 81.0, 82.0, 83.0 It can be 4.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, 40.0, 41.0, 42.0, 43.0, 44.0, 45.0, 46.0, 47.0, 48.0, 49.0, 50.0.

[0212] As a result of extensive testing and research, the inventors have found that by controlling the ratio of Al2O3 / (Li2O+ZrO2+P2O5), the total content of Al2O3, P2O5, Li2O and ZrO2, Li2O+ZrO2+P2O5, to within the range of 0.16 to 0.9, the microcrystalline glass product can withstand the impact of a falling ball of 1300 mm or more, and more preferably, by controlling Al2O3 / (Li2O+ZrO2+P2O5) to within the range of 0.18 to 0.6. Furthermore, in some embodiments, it is even more preferable to control Al2O3 / (Li2O+ZrO2+P2O5) to within the range of 0.19 to 0.5, in which case the lithium monosilicate crystal phase is easily formed and the microcrystalline glass product can have excellent fracture toughness, with a fracture toughness of 1 MPa m 1 / 2 More than 1.1 MPa m, preferably 1.1 MPa m 1 / 2 More preferably, 1.2 MPa m 1 / 2 That is all. Furthermore, since the ability to withstand the height of the ball drop test can be further optimized, it is more preferable that Al2O3 / (Li2O+ZrO2+P2O5) is 0.19 to 0.5. In some embodiments, Al2O3 / (Li2O+ZrO2+P2O5) can be 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90.

[0213] After extensive testing and research, the inventors have found that the relative content of Na2O and Y2O3 has an important effect on the surface stress and ion exchange layer depth of the microcrystalline glass product, and especially when Na2O / Y2O3 is less than 6.0, it can increase the surface stress and ion exchange layer depth of the microcrystalline glass product, and more preferably Na2O / Y2O3 is 0.1-5.0. In some embodiments, it is more preferable that Na2O / Y2O3 is 0.3-2.0, and it can also improve the size of the fragments of the microcrystalline glass product, and in some embodiments, the surface stress of the microcrystalline glass product is 600 MPa or more, preferably 650 MPa or more, more preferably 700 MPa or more, and the ion exchange layer depth of the microcrystalline glass product is 20 μm or more, preferably 30 μm or more, more preferably 40 μm or more. In some embodiments, the value of Na2O / Y2O3 can be 0, greater than 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.3, 2.5, 2.7, 3.0, 3.3, 3.5, 3.7, 4.0, 4.3, 4.5, 4.7, 5.0, 5.3, 5.5, 5.7, 6.0.

[0214] In some embodiments of the present invention, when the ratio Y2O3 / (Al2O3+SiO2) of the content of Y2O3 to the total content of Al2O3 and SiO2 (Al2O3+SiO2) is controlled to be more than 0 and less than 0.15, the microcrystalline performance of glass can be optimized, so that microcrystalline glass and microcrystalline glass products have appropriate microcrystallinity and excellent performance. Therefore, Y2O3 / (Al2O3+SiO2) is preferably 0.01-0.12, more preferably 0.03-0.09, and the ball drop test height of microcrystalline glass and microcrystalline glass products is large. In some embodiments, the ball drop test height of microcrystalline glass products is preferably 1300mm or more, more preferably 1400mm or more, and even more preferably 1500mm or more. In some embodiments, the value of Y2O3 / (Al2O3+SiO2) can be greater than 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15.

[0215] B2O3 can improve the network structure of glass, optimize the chemical strengthening performance of glass and microcrystalline glass, and improve the falling height of microcrystalline glass products, but if the content of B2O3 exceeds 5%, it is disadvantageous to glass molding and is prone to crystallization during molding. Therefore, the upper limit of the content of B2O3 is 5%, preferably 3%, more preferably 2%, and even more preferably no B2O3. In some embodiments, it can contain about 0%, more than 0%, 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, or 5.0% B2O3.

[0216] Although ZnO can reduce the melting difficulty of glass, a high content of ZnO promotes low-temperature crystallization of glass, reduces the crystallinity and transmittance of microcrystalline glass and microcrystalline glass products, and increases the haze of microcrystalline glass and microcrystalline glass products, so the upper limit of the content is 2%, preferably 1%, and more preferably does not contain ZnO. In some embodiments, ZnO can be contained in an amount of about 0%, more than 0%, 0.1%, 0.5%, 1.0%, 1.5%, or 2.0%.

[0217] MgO is advantageous in lowering the melting difficulty of glass and increasing the drop height of microcrystalline glass and microcrystalline glass products, but promotes low-temperature crystallization of glass and reduces the crystallinity and transmittance of microcrystalline glass and microcrystalline glass products, so the upper limit of its content is 2%, preferably 1%. In some embodiments, it can contain about 0%, more than 0%, 0.1%, 0.5%, 1.0%, 1.5%, or 2.0% MgO.

[0218] SrO is an optional component that enhances the low-temperature melting property of glass and suppresses crystal precipitation during glass molding. If the content is too high, it affects the molding of glass and crystals are likely to precipitate during molding. Therefore, the content range of SrO in the present invention is 0 to 5%, preferably 0 to 3%, more preferably 0 to 1%, and further preferably does not contain SrO. In some embodiments, it can contain about 0%, more than 0%, 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, or 5.0% SrO.

[0219] BaO is an optional component that helps improve the glass forming performance of glass, and if the content is too high, it is disadvantageous to glass forming. Therefore, the BaO content range in the present invention is 0 to 5%, preferably 0 to 3%, more preferably 0 to 1%, and even more preferably does not contain BaO. In some embodiments, BaO can be contained in an amount of about 0%, more than 0%, 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, or 5.0%.

[0220] CaO can increase the hardness of glass, but if the content is too high, it is easy to emulsify during glass molding. Therefore, the CaO content in the present invention is in the range of 0 to 5%, preferably 0 to 3%, more preferably 0 to 1%, and even more preferably does not contain CaO. In some embodiments, it can contain about 0%, more than 0%, 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, or 5.0% CaO.

[0221] TiO2 is an optional component that helps to lower the melting temperature of the matrix glass and increase its chemical stability, and the present invention includes up to 5% TiO2 to facilitate control of the crystallization process of the matrix glass, preferably up to 3%, more preferably up to 1%. In some embodiments, it is even more preferred to have no TiO2. In some embodiments, it can include about 0%, greater than 0%, 0.1%, 0.3%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5% TiO2.

[0222] Ln2O3 (Ln2O3 is one or more of La2O3, Gd2O3, and Yb2O3) is an optional component that increases the hardness and chemical stability of microcrystalline glass and controls crystallization during glass molding. If the content is too high, it affects the chemical strengthening performance of glass and reduces the strength of the microcrystalline glass product. Therefore, the content of Ln2O3 in the present invention is in the range of 0 to 5%, preferably 0 to 4%, more preferably 0 to 3%, and even more preferably does not contain Ln2O3. In some embodiments, it can contain about 0%, more than 0%, 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, or 5.0% Ln2O3.

[0223] In some embodiments, the glass, microcrystalline glass, or microcrystalline glass product may also contain 0-2% of a fining agent to enhance the defoaming ability of the glass, microcrystalline glass, or microcrystalline glass product. Such fining agents include, but are not limited to, one or more of Sb2O3, SnO2, SnO, CeO2, F, Cl, and Br, and preferably Sb2O3 is used as the fining agent. When the above fining agents are used alone or in combination, the upper limit of their content is preferably 1%, more preferably 0.5%. In some embodiments, the content of one or more of the above fining agents is about 0%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, or 2.0%.

[0224] In order to obtain the excellent performance, such as mechanical performance, optical performance, manufacturability, and chemical strengthening performance, expected from the glass, microcrystalline glass, or microcrystalline glass product of the present invention, in some embodiments of the present invention, it is preferable that the glass, microcrystalline glass, or microcrystalline glass product does not contain F and / or does not contain Ta2O5.

[0225] Some embodiments of the present invention preferably do not contain PbO and As2O3, because PbO and As2O3 are toxic substances and even small amounts added do not meet the requirements of environmental protection.

[0226] In some embodiments of the present invention, colorants are added to produce colored matrix glasses, microcrystalline glasses, or microcrystalline glass products, so that the matrix glasses, microcrystalline glasses, or microcrystalline glass products can have different colors. The colorants include: NiO: 0-4%, and / or Ni2O3: 0-4%, and / or CoO: 0-2%, and / or Co2O3: 0-2%, and / or Fe2O3: 0-7%, and / or MnO2: 0-4%, and / or Er2O3: 0-8%, and / or Nd2O3: 0-8%, and / or Cu2O: 0-4%, and / or Pr2O5: 0-8%, and / or CeO2: 0-4%. The weight percentages of the colorants and their roles are explained in detail below:

[0227] The brown or green matrix glass, microcrystalline glass or microcrystalline glass product produced by the present invention uses NiO, Ni2O3 and Pr2O5 as colorants. NiO and Ni2O3 are colorants used to produce brown or green matrix glass, microcrystalline glass or microcrystalline glass products. The two components can be used alone or mixed, and the respective contents are generally below 4%, preferably below 3%. If the content exceeds 4%, the colorant cannot be well dissolved in the matrix glass, microcrystalline glass or microcrystalline glass product. Therefore, the lower limit of each content is above 0.1%, and if it is less than 0.1%, the color of the matrix glass, microcrystalline glass or microcrystalline glass product is not obvious. In some embodiments, NiO and Ni2O3 may be present at about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%. When used in combination, the total content of NiO and Ni2O3 is generally 4% or less, with the lower limit of the total content being 0.1% or more. In some embodiments, the NiO and Ni2O3 may include about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% NiO and Ni2O3. Pr2O5 is used as a coloring agent for green matrix glass, microcrystalline glass or microcrystalline glass products, and is used alone. The content is generally not more than 8%, preferably not more than 6%, and the lower limit of the content is not less than 0.4%.Below 0.4%, the color of the matrix glass, microcrystalline glass, or microcrystalline glass product is not obvious. In some embodiments, the PrO5 may be about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, 8.0%.

[0228] The blue matrix glass, microcrystalline glass or microcrystalline glass product produced by the present invention uses CoO and Co2O3 as colorants, and the two colorant components can be used alone or mixed, and the respective contents are generally below 2%, preferably below 1.8%, and if the content exceeds 2%, the colorant cannot be well dissolved in the matrix glass, microcrystalline glass or microcrystalline glass product. Therefore, the lower limit of the respective contents is above 0.05%, and if it is less than 0.05%, the color of the matrix glass, microcrystalline glass or microcrystalline glass product is not obvious. In some embodiments, it may contain about 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0% CoO or Co2O3. When used in combination, the total content of CoO and Co2O3 does not exceed 2%, with the lower limit of the total content being 0.05% or more. Some embodiments may include about 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, or 2.0% CoO and Co2O3.

[0229] The yellow matrix glass, microcrystalline glass or microcrystalline glass product produced by the present invention uses Cu2O and CeO2 as colorants, and the two colorant components can be used alone or mixed, and the lower limit of each content is 0.5% or more, and if the content is less than 0.5%, the color of the matrix glass, microcrystalline glass or microcrystalline glass product is not obvious. Therefore, when Cu2O is used alone, it should be 4% or less, preferably 3% or less, and if the content exceeds 4%, the matrix glass is prone to crystallization. In some embodiments, it may contain about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% Cu2O. When CeO2 is used alone, its content is generally 4% or less, preferably 3% or less, and if the content exceeds 4%, the gloss of the matrix glass, microcrystalline glass or microcrystalline glass product will be poor. In some embodiments, it can contain about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% CeO2. At the same time, adding a small amount of CeO2 to glass can have a bubble removing effect, and CeO2 can also be used as a fining agent in glass. When two colorants are used in combination, their total content is generally 4% or less, with the lower limit of the total content being 0.5% or more.In some embodiments, the composition may include about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, or 4.0% CeO2 and Cu2O.

[0230] The black or smoke gray matrix glass, microcrystalline glass or microcrystalline glass product produced by the present invention uses Fe2O3 alone as a colorant, or uses two colorants, Fe2O3 and CoO, or two colorants, Fe2O3 and Co2O3, or three colorants, Fe2O3, CoO and NiO, or three colorants, Fe2O3, Co2O3 and NiO, in combination. The colorant used in producing the black or smoke gray matrix glass, microcrystalline glass or microcrystalline glass product is mainly colored by Fe2O3, and its content is 7% or less, preferably 5% or less, with the lower limit of its content being 0.2% or more, and in some embodiments, it is about 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 3.1%, 3.2%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 3.1%, 3.2%, 3.3 ...4%, 3.5%, It can contain Fe2O3 of 0.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0%. CoO and Co2O3 can absorb visible light and deepen the coloring of matrix glass, microcrystalline glass or microcrystalline glass products. When mixed with Fe2O3, the respective contents are generally not more than 0.6%, with the lower limit being not less than 0.2%. In some embodiments, it can contain about 0.2%, 0.3%, 0.4%, 0.5%, 0.6% CoO and / or Co2O3. NiO absorbs visible light and can deepen the coloring of matrix glass, microcrystalline glass or microcrystalline glass product, and when used in a mixture, its content is 1% or less, and the lower limit of the total content is 0.2% or more. In some embodiments, it can contain about 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0% NiO.

[0231] The purple matrix glass, microcrystalline glass or microcrystalline glass product produced in the present invention uses MnO2 as a colorant, and its content is generally not more than 4%, preferably not more than 3%, and the lower limit of the content is not less than 0.1%. If it is less than 0.1%, the color of the matrix glass, microcrystalline glass or microcrystalline glass product will not be obvious. In some embodiments, the MnO2 may include about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% MnO2.

[0232] The pink matrix glass, microcrystalline glass or microcrystalline glass product produced by the present invention uses Er2O3 as a colorant, and its content is generally less than 8%, preferably less than 6%. The coloring efficiency of Er2O3, which is a rare earth element, is low, so even if the content exceeds 8%, the color of the matrix glass, microcrystalline glass or microcrystalline glass product cannot be deepened, but rather increases the cost. Therefore, the lower limit of the content is 0.4% or more, and if it is less than 0.4%, the color of the matrix glass, microcrystalline glass or microcrystalline glass product is not obvious. Some embodiments can include about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, or 8.0% Er2O3.

[0233] The magenta matrix glass, microcrystalline glass or microcrystalline glass product produced by the present invention uses Nd2O3 as a colorant, and its content is generally less than 8%, preferably less than 6%. Since the coloring efficiency of rare earth element Nd2O3 is low, even if the content exceeds 8%, the color of the matrix glass, microcrystalline glass or microcrystalline glass product cannot be deepened, but rather increases the cost. Therefore, the lower limit of the content is 0.4% or more, and if it is less than 0.4%, the color of the matrix glass, microcrystalline glass or microcrystalline glass product is not obvious. In some embodiments, the Nd2O3 may include about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, or 8.0% Nd2O3.

[0234] The red matrix glass, microcrystalline glass or microcrystalline glass product produced by the present invention uses a mixed colorant color of Er2O3, Nd2O3 and MnO2, Er ions in the glass absorb at 400-500nm, Mn ions mainly absorb at 500nm, and Nd ions mainly strongly absorb at 580nm, and by mixing three kinds of substances, red matrix glass, microcrystalline glass or microcrystalline glass product can be produced. Er2O3 and Nd2O3 are rare earth colorants, and their coloring ability is relatively weak, so the amount of Er2O3 used is within 6%, the amount of Nd2O3 used is within 4%, and MnO2 has a strong coloring ability, so its amount is within 2%, and the lower limit of the total content of the mixed colorants is above 0.9%.

[0235] The terms "free" and "0%" used herein mean that no compounds, molecules, elements, etc. were intentionally added as raw materials for the matrix glass, microcrystalline glass, or microcrystalline glass product of the present invention. However, impurities or components that are not intentionally added as raw materials and / or equipment for producing the matrix glass, microcrystalline glass, or microcrystalline glass product may be present in small or trace amounts in the final matrix glass, microcrystalline glass, or microcrystalline glass product, and are also covered by the patent of the present invention.

[0236] In some embodiments of the present invention, the crystalline phase in the microcrystalline glass and microcrystalline glass product comprises lithium monosilicate crystals, which imparts high strength to the microcrystalline glass and microcrystalline glass product of the present invention, and the microcrystalline glass and microcrystalline glass product have high fracture toughness, and high ball drop test height and four-point bending strength. The microcrystalline glass of the present invention has excellent chemical strengthening performance, and additional mechanical strength can be obtained by chemical strengthening. Through rational component design, the crystal grain size of the microcrystalline glass and microcrystalline glass product obtained by the present invention is appropriate, and the microcrystalline glass and microcrystalline glass product of the present invention has high strength. Since the microcrystalline glass and microcrystalline glass product of the present invention have good crystallinity, the microcrystalline glass and microcrystalline glass product of the present invention have excellent mechanical performance. The crystallinity described in this specification refers to the perfection of the crystal, and the arrangement of the mass points inside the crystal of a perfect crystal is relatively regular, the diffraction line is strong, sharp and symmetrical, and the half-width of the diffraction peak is close to the width measured by instrument measurement, while a crystal with poor crystallinity has outlying defects and the peak shape of the diffraction line is broad and dispersed. The poorer the crystallinity, the weaker the diffraction ability and the broader the diffraction peaks become until they disappear into the background. In some embodiments, the crystallinity of the microcrystalline glass product or microcrystalline glass is 50% or more, preferably 60% or more, and more preferably 70% or more.

[0237] The grain size and type of the microcrystalline glass or microcrystalline glass product of the present invention affect the haze and transmittance of the microcrystalline glass or microcrystalline glass product, with smaller grains resulting in higher transmittance and smaller haze resulting in higher transmittance. In some embodiments, the haze of a microcrystalline glass product or microcrystalline glass having a thickness of 1 mm or less is 0.15% or less, preferably 0.12% or less, more preferably 0.1% or less. In some embodiments, the grain size of the microcrystalline glass product or microcrystalline glass is 50 nm or less, preferably 40 nm or less, more preferably 30 nm or less.

[0238] In some embodiments, the crystalline phase content and refractive index in the microcrystalline glass or microcrystalline glass product of the present invention affect the |B| value of the microcrystalline glass or microcrystalline glass product, causing the microcrystalline glass or microcrystalline glass product to appear blue or yellow in the visible light range, affecting the optical performance of the product, and using the |B| value to display the LAB (chromaticity value of material color). The microcrystalline glass or microcrystalline glass product exhibits a low |B| value in the visible light range, and in some embodiments, the average light |B| value of the microcrystalline glass product or microcrystalline glass 400-800 nm with a thickness of 1 mm or less is 0.6 or less, preferably 0.55 or less, more preferably 0.5 or less.

[0239] In some embodiments, the microcrystalline glass or microcrystalline glass product of the present invention exhibits high transparency in the visible light range (i.e., the microcrystalline glass or microcrystalline glass product is transparent). The microcrystalline glass or microcrystalline glass product exhibits high transmittance in the visible light range, and in some embodiments, the average light transmittance of the microcrystalline glass product or microcrystalline glass at 400-800 nm with a thickness of 1 mm or less is preferably 89% or more. In some preferred embodiments, the light transmittance of the microcrystalline glass product or microcrystalline glass at 550 nm with a thickness of 1 mm or less is preferably 91% or more.

[0240] In some embodiments, antimicrobial components can be added to the matrix glass, microcrystalline glass, or microcrystalline glass product. The microcrystalline glass or microcrystalline glass product described herein can be used in applications such as kitchen or dining tables where there is a high probability of exposure to harmful bacteria. Antimicrobial components that can be added to the matrix glass, microcrystalline glass, or microcrystalline glass product include, but are not limited to, Ag, AgO, Cu, CuO, Cu2O, etc. In some embodiments, the single or mixed content of the above antimicrobial components is 2% or less, preferably 1% or less.

[0241] The matrix glass, microcrystalline glass and microcrystalline glass products of the present invention can be produced and manufactured by the following methods:

[0242] Formation of matrix glass: The raw materials are mixed uniformly according to the composition ratio, and the uniformly mixed mixture is placed in a platinum or quartz crucible and melted for 5 to 24 hours at a temperature range of 1250 to 1650°C in an electric furnace or gas furnace depending on the degree of difficulty of melting the glass composition. After melting and stirring uniformly, the temperature is lowered to an appropriate level and the mixture is poured into a mold and slowly cooled to form the matrix glass.

[0243] The matrix glass of the present invention can be formed by known methods.

[0244] The matrix glass of the present invention is subjected to a microcrystallization process after molding or processing, in which crystals are uniformly precipitated inside the glass. This microcrystallization process can be performed in one or two stages, and is preferably performed in two stages. The nucleation process is performed at a first temperature, and then the crystal growth process is performed at a second temperature higher than the temperature of the nucleation process. The microcrystallization process performed at the first temperature is called the first microcrystallization process, and the microcrystallization process performed at the second temperature is called the second microcrystallization process.

[0245] In order to obtain the expected physical properties of the microcrystalline glass, the crystallization process is preferably as follows:

[0246] By carrying out the microcrystallization treatment in one step, the nucleation step and the crystal growth step can be carried out continuously. That is, the temperature is raised to a predetermined crystallization treatment temperature, and after reaching the crystallization treatment temperature, the temperature is maintained for a certain period of time, and then the temperature is lowered. The crystallization treatment temperature is preferably 600 to 750°C, and more preferably 650 to 700°C in order to precipitate the expected crystal phase, and the holding time at the crystallization treatment temperature is preferably 0 to 8 hours, more preferably 1 to 6 hours.

[0247] When the microcrystallization treatment is carried out in the above two stages, the first temperature is preferably 470 to 630° C., and the second temperature is preferably 650 to 750° C. The holding time at the first temperature is preferably 0 to 24 hours, more preferably 2 to 15 hours. The holding time at the second temperature is preferably 0 to 10 hours, more preferably 0.5 to 6 hours.

[0248] The above-mentioned holding time of 0 hours means that the temperature starts to be lowered or raised again within one minute after the temperature is reached.

[0249] In some embodiments, the matrix glasses or microcrystalline glasses described herein can be fabricated into bodies by a variety of techniques, including, but not limited to, sheets, processes including, but not limited to, slit drawing, float, roll rolling, and other sheet forming techniques known in the art, or the matrix glasses or microcrystalline glasses can be formed by float or roll rolling techniques known in the art.

[0250] The matrix glass or microcrystalline glass of the present invention can be used to produce a sheet-like glass molded body by polishing or polishing, but the method for producing the glass molded body is not limited to these methods.

[0251] The matrix glass or microcrystalline glass molded body of the present invention can be manufactured into various shapes by using methods such as hot bending or pressing at a certain temperature, but is not limited to these methods.

[0252] The matrix glasses, microcrystalline glasses, and microcrystalline glass articles according to the present invention can have any reasonable and useful thickness.

[0253] The microcrystalline glass of the present invention not only improves mechanical properties by precipitating crystals, but also provides higher strength by forming a compressive stress layer, and can be used to produce microcrystalline glass products.

[0254] In some embodiments, the matrix glass or microcrystalline glass can be processed into a sheet and / or shaped (e.g., punched, hot bent, etc.), polished and / or polished after shaping, and chemically strengthened using a chemical strengthening process.

[0255] The chemical strengthening described in the present invention is namely an ion exchange method. Both the matrix glass and the microcrystalline glass of the present invention can be ion exchanged by methods known in the art. In ion exchange, smaller metal ions in the matrix glass or microcrystalline glass are replaced or "exchanged" by larger metal ions that have the same valence state close to that of the matrix glass or microcrystalline glass. The replacement of the smaller ions with the larger ions creates a compressive stress in the matrix glass or microcrystalline glass, forming a compressive stress layer.

[0256] In some embodiments, the metal ion is a monovalent alkali metal ion (e.g., Na + , K + , Rb + , Cs + ion exchange is carried out by immersing the matrix glass or the microcrystalline glass in a salt bath of at least one molten salt containing smaller metal ions, which are used to replace the smaller metal ions in the matrix glass. + , Tl + , Cu +The monovalent ions can also be exchanged with other monovalent metal ions such as ZnO, ZnS, ZnO ...

[0257] In some embodiments, the matrix glass or microcrystalline glass can be ion-exchanged by immersion in a salt bath containing molten Na salts (e.g., NaNO3) at a temperature of about 430°C to 470°C for about 6 to 20 hours, preferably in the temperature range of 435°C to 460°C, and for a time range of 8 to 13 hours. In this embodiment, the Na ions replace some of the Li ions in the matrix glass or microcrystalline glass, thereby forming a surface compression layer and exhibiting high mechanical properties. In some embodiments, the matrix glass or microcrystalline glass can be ion-exchanged by immersion in a salt bath containing molten K salts (e.g., KNO3) at a temperature of about 400°C to 450°C for 1 to 8 hours, preferably in the time range of 2 to 4 hours.

[0258] In some embodiments, there is also an ion implantation method in which ions are implanted into the surface layer of the matrix glass or microcrystalline glass, and a thermal strengthening method in which the matrix glass or microcrystalline glass is heated and then rapidly cooled.

[0259] The performance indicators of the microcrystalline glass and / or the microcrystalline glass product and / or the matrix glass of the present invention have been tested according to the following methods.

[0260] [Haze degree] Using a haze meter EEL57 D, samples of less than 1 mm are prepared and measured according to GB 2410-80.

[0261] [Crystal grain size] The measurement is carried out using a SEM scanning electron microscope. The microcrystalline glass is surface-treated in HF acid, and then the surface of the microcrystalline glass is sprayed with molten metal. The surface is scanned using a SEM scanning electron microscope to determine the crystal grain size.

[0262] [Light transmittance] The light transmittance described in this specification is the external transmittance, and may be abbreviated to transmittance. The sample is cut to a thickness of 1 mm or less, and the opposing surfaces are polished parallel to each other. The average light transmittance from 400 to 800 nm is measured using a Hitachi U-41000 spectrophotometer. The sample is processed to a thickness of 1 mm or less, the opposing surfaces are parallelly polished, and the light transmittance at 550 nm is measured using a Hitachi U-41000 spectrophotometer.

[0263] [Crystallization] The XRD diffraction peaks are compared with database spectra, and the crystallinity is calculated by calculating the ratio of the diffraction intensity of the crystalline phase to the total spectral intensity, and internal orientation is performed using a pure quartz crystal. [Surface stress] and [Ion exchange layer depth] The surface stress is measured using a glass surface stress meter FSM-6000 LEUV. The ion-exchange layer depth is measured using a glass surface stress meter SLP-2000. The measurement conditions are a refractive index of 1.54 for the sample and an optical elastic constant of 25.3 [(nm / cm) / Mpa].

[0264] [Ball drop test height] A microcrystalline glass product sample of 150 x 57 x 0.55 mm is placed on a glass fixture, and a steel ball of 132 g is dropped from a specified height. The maximum impact that the sample can withstand without breaking is the drop ball test height. Specifically, the test is performed from a drop ball test height of 800 mm, and if no breakage occurs, the height is changed in the order of 850 mm, 900 mm, 950 mm, and 1000 mm or more. For specific examples of the "drop ball test height", microcrystalline glass products are the test subjects. Test data recorded as 1000 mm in the examples indicates that the microcrystalline glass product can withstand the impact without breaking even when a steel ball is dropped from a height of 1000 mm onto the microcrystalline glass product. The drop ball test height of the present invention may be abbreviated to the drop ball height.

[0265] [Ball drop height] A microcrystalline glass sample of 150 x 57 x 0.55 mm is placed on a glass fixture, and a 32 g steel ball is dropped from a specified height. The maximum ball drop test height at which the sample can withstand the impact without breaking is the main ball drop height. Specifically, the test is performed from a ball drop test height of 500 mm, and if no breakage occurs, the height is changed in the order of 550 mm, 600 mm, 650 mm, and 700 mm or more. For specific examples of the "main ball drop height", microcrystalline glass is the test subject. The test data recorded as 1000 mm in the examples indicates that the microcrystalline glass can withstand the impact without breaking even when a steel ball is dropped from a height of 1000 mm onto the microcrystalline glass.

[0266] [Fracture toughness] A method is used to directly measure the dimensions of the indentation expansion crack. The sample dimensions are 2mm x 4mm x 20mm, and are chamfered, polished, and polished. After the sample is manufactured, a Vickers hardness indenter is used to apply a force of 49N to the sample and hold it for 30 seconds to create an indentation, and then the breaking strength is measured using a three-point bending method.

[0267] [4-point bending strength] The microcomputer-controlled electronic universal testing machine CMT 6502 is used, the specimens have a thickness of 1 mm or less, and are tested according to ASTM C 158-2002. The thickness of the sample is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, even more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.72 mm, or 0.75 mm.

[0268] [Vickers hardness] The surface area (mm2) was calculated by calculating the load (N) when a pyramidal indenter with a square diamond indenter having an angle of 136° formed by the mating surfaces was used to indent a pyramidal indentation on the test surface, based on the length of the indentation. 2 The test is performed with a test load of 100 (N) and a holding time of 15 (seconds). In the present invention, Vickers hardness may be abbreviated to hardness.

[0269] [|B|value] Measure the B value using a Minolta CM-700d. Use the attached calibration tube and short tube to perform zero calibration and white board calibration of the meter, respectively. After calibration, perform a blank test with the long tube to determine the calibration stability and reliability of the meter (B≦0.05). After the meter calibration, place the product on the zero tube and measure it. The |B| value is the absolute value of the B value.

[0270] [Thermal expansion coefficient] Thermal expansion coefficient (α 20℃-120℃ ) is tested in accordance with the method specified in GB / T7962.16-2010.

[0271] [Refractive index] The refractive index (nd) is tested according to the method specified in GB / T7962.1-2010.

[0272] The microcrystalline glass product of the present invention has the following properties: 1) In some embodiments, the surface stress of the microcrystalline glass article is 600 MPa or more, preferably 650 MPa or more, and more preferably 700 MPa or more. 2) In some embodiments, the microcrystalline glass article has a four-point bending strength of 600 MPa or more, preferably 650 MPa or more, and more preferably 700 MPa or more. 3) In some embodiments, the microcrystalline glass article has an ion exchange layer depth of 20 μm or more, preferably 30 μm or more, more preferably 40 μm or more. 4) In some embodiments, the microcrystalline glass product has a ball drop test height of 1300 mm or more, preferably 1400 mm or more, more preferably 1500 mm or more. 5) In some embodiments, the microcrystalline glass article has a fracture toughness of 1 MPa m 1 / 2 More than 1.1 MPa m, preferably 1.1 MPa m 1 / 2 More preferably, 1.2 MPa m 1 / 2 That's all. 6) In some embodiments, the microcrystalline glass product has a Vickers hardness (Hv) of 700 kgf / mm 2 More than 720kgf / mm 2 More preferably, 730kgf / mm 2 That's all. 7) In some embodiments, the crystallinity of the microcrystalline glass article is 50% or more, preferably 60% or more, and more preferably 70% or more. 8) In some embodiments, the microcrystalline glass product has a grain size of 50 nm or less, preferably 40 nm or less, and more preferably 30 nm or less. 9) In some embodiments, the haze of a microcrystalline glass product having a thickness of 1 mm or less is 0.15% or less, preferably 0.12% or less, more preferably 0.1% or less, and the thickness is preferably 0.2-1 mm, more preferably 0.3-0.9 mm, even more preferably 0.5-0.8 mm, and even more preferably 0.55 mm or 0.6 mm or 0.68 mm or 0.72 mm or 0.75 mm. 10) In some embodiments, a microcrystalline glass product having a thickness of 1 mm or less has an average transmittance of 89% or more at wavelengths of 400 to 800 nm, preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, even more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.72 mm, or 0.75 mm. 11) In some embodiments, the transmittance at 550 nm of a microcrystalline glass product having a thickness of 1 mm or less is 91% or more, preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, even more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.72 mm, or 0.75 mm. 12) In some embodiments, the average optical |B| value at 400-800 nm of a microcrystalline glass product having a thickness of 1 mm or less is 0.6 or less, preferably 0.55 or less, more preferably 0.5 or less. This thickness is preferably 0.2-1 mm, more preferably 0.3-0.9 mm, even more preferably 0.5-0.8 mm, and even more preferably 0.55 mm or 0.6 mm or 0.68 mm or 0.72 mm or 0.75 mm.

[0273] The microcrystalline glass of the present invention has the following properties: 1) In some embodiments, the crystallinity of the microcrystalline glass is 50% or more, preferably 60% or more, and more preferably 70% or more. 2) In some embodiments, the crystal grain size of the microcrystalline glass is 50 nm or less, preferably 40 nm or less, and more preferably 30 nm or less. 3) In some embodiments, the haze of the microcrystalline glass having a thickness of 1 mm or less is 0.15% or less, preferably 0.12% or less, more preferably 0.1% or less, and the thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, even more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.72 mm, or 0.75 mm. 4) In some embodiments, the average transmittance of a 400-800 nm wavelength microcrystalline glass product having a thickness of 1 mm or less is 89% or more, and the thickness is preferably 0.2-1 mm, more preferably 0.3-0.9 mm, even more preferably 0.5-0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.72 mm, or 0.75 mm. 5) In some embodiments, the transmittance at 550 nm of a microcrystalline glass product having a thickness of 1 mm or less is 91% or more, preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, even more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.72 mm, or 0.75 mm. 6) In some embodiments, the microcrystalline glass body has a falling ball height of 1000 mm or more, preferably 1100 mm or more, more preferably 1200 mm or more. 7) In some embodiments, the average light |B| value at 400 to 800 nm of the microcrystalline glass having a thickness of 1 mm or less is 0.6 or less, preferably 0.55 or less, more preferably 0.5 or less. This thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, even more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.72 mm, or 0.75 mm. 8) In some embodiments, the microcrystalline glass has a Vickers hardness (Hv) of 650 kgf / mm 2 More than 680kgf / mm 2 More preferably, 700kgf / mm 2 That's all. 9) In some embodiments, the thermal expansion coefficient (α 20℃-120℃ ) is 75~95×10 -7 / K. 10) In some embodiments, the refractive index (n d ) is 1.5700~1.5800.

[0274] The matrix glass of the present invention has the following properties: 1) In some embodiments, the thermal expansion coefficient of the matrix glass (α 20℃-120℃ ) is 50 x 10 -7 / K~70×10 -7 / K. 2) In some embodiments, the refractive index of the matrix glass (n d ) is between 1.5600 and 1.5700.

[0275] The microcrystalline glass, microcrystalline glass product and matrix glass of the present invention have the above-mentioned excellent properties, and therefore can be widely produced as glass cover plates or glass elements.In addition, the microcrystalline glass, microcrystalline glass product and matrix glass of the present invention are applied to electronic devices or display devices such as mobile phones, watches, computers and touch screens, and are used in the manufacture of mobile phones, smartphones, tablets, notebook computers, PDAs, televisions, personal computers, MTA devices or industrial displays, or in the manufacture of touch screens, protective windows, automobile windows, train windows, aviation device windows, touch screen protective glass, or in the manufacture of hard disk substrates, solar cell substrates, and white goods such as refrigerator parts and cooking utensils.

[0276] Working Example In order to more clearly illustrate the technical solution of the present invention, the following non-limiting examples are provided. The examples of the present invention make every effort to ensure the accuracy of the values ​​(e.g., amounts, temperatures, etc.), but some errors and deviations should be considered. The compositions themselves are assigned by weight % based on the oxides and normalized to 100%.

[0277] <Example of matrix glass> In this example, the above-mentioned method for producing matrix glass is used to obtain matrix glass having the composition shown in Tables 1 to 4. In addition, the properties of the matrix glass are measured by the test methods described in the present invention, and the measurement results are shown in Tables 1 to 4.

[0278] [Table 1]

[0279] [Table 2]

[0280] [Table 3]

[0281] [Table 4]

[0282] <Examples of microcrystalline glass> In this example, the above-mentioned manufacturing method for microcrystalline glass is used to obtain microcrystalline glass having the composition shown in Tables 5 to 8. In addition, the properties of the microcrystalline glass are measured by the test methods described in the present invention, and the measurement results are shown in Tables 5 to 8.

[0283] [Table 5]

[0284] [Table 66]

[0285] [Table 7]

[0286] [Table 8]

[0287] <Examples of microcrystalline glass products> In this example, the microcrystalline glass product having the composition shown in Tables 9 to 12 is obtained by using the above-mentioned manufacturing method of the microcrystalline glass product. In addition, the properties of the microcrystalline glass product are measured by the test method described in the present invention, and the measurement results are shown in Tables 9 to 12.

[0288] [Table 9]

[0289] [Table 10]

[0290]

Table 11

[0291]

Table 12

Claims

1. A microcrystalline glass product containing, by weight, the following components: SiO 2 : 53-70%, Al 2 O 3 : 8-18%, Li 2 O: 13.5-25%, ZrO 2 : 7.5-15%, P 2 O 5 : 2-10%, Y 2 O 3 : greater than 0 and less than 8%, K 2 O: 0-4.5%, BaO: 0-1.5%, TiO 2 : 0-1.5%, (Li 2 O+ZrO 2 +P 2 O 5 ) / Y 2 O 3 is 9.0-50.

0.

2. 2. The microcrystalline glass product according to claim 1, further comprising the following components in weight percent: MgO: 0-2%, and / or ZnO: 0-2%, and / or Na 2 O: 0-6%, and / or SrO: 0-5%, and / or CaO: 0-5%, and / or B 2 O 3 : 0 to 5%, and / or Ln 2 O 3 : 0 to 5%, and / or clarifier: 0 to 2%, and the Ln 2 O 3 La 2 O 3 , Gd 2 O 3 , Yb 2 O 3 One or more of the above, and the fining agent is Sb 2 O 3 , SnO 2 , SnO, CeO 2 , F, Cl and Br.

3. 3. The microcrystalline glass product according to claim 1 or 2, wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following four conditions: 1) Y 2 O 3 / ZrO 2 is greater than 0; 2) Al 2 O 3 / (Li 2 O+ZrO 2 +P 2 O 5 ) is between 0.16 and 0.9; 3) Na 2 O / Y 2 O 3 is less than or equal to 6.0; 4) Y 2 O 3 / (Al 2 O 3 +SiO 2 ) is greater than 0 and less than or equal to 0.

15.

4. 3. The microcrystalline glass product according to claim 1 or 2, comprising the following components in weight percent: SiO 2 : 53-65% and / or Al 2 O 3 : 8-15% and / or Li 2 O: 13.5-22% and / or P 2 O 5 : 3.5-9% and / or K 2 O: 0-4%, and / or MgO: 0-1%, and / or ZnO: 0-1%, and / or Na 2 O: 1-5% and / or Y 2 O 3 : 1-7%, and / or SrO: 0-3%, and / or CaO: 0-3%, and / or B 2 O 3 : 0 to 3%, and / or Ln 2 O 3 : 0 to 4%, and / or fining agent: 0 to 1%, and the Ln 2 O 3 La 2 O 3 , Gd 2 O 3 , Yb 2 O 3 One or more of the above, and the fining agent is Sb 2 O 3 , SnO 2 , SnO, CeO 2 , F, Cl and Br.

5. 3. The microcrystalline glass product according to claim 1 or 2, wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y 2 O 3 / ZrO 2 is between 0.1 and 1.0; 2) (Li 2 O+ZrO 2 +P 2 O 5 ) / Y 2 O 3 is between 9.0 and 40.0; 3) Al 2 O 3 / (Li 2 O+ZrO 2 +P 2 O 5 ) is between 0.18 and 0.6; 4) Na 2 O / Y 2 O 3 is between 0.1 and 5.0; 5) Y 2 O 3 / (Al 2 O 3 +SiO 2 ) is between 0.01 and 0.

12.

6. 3. The microcrystalline glass product according to claim 1 or 2, comprising the following components in weight percent: SiO 2 : 53-63% and / or Al 2 O 3 : 8-12% and / or Li 2 O: 14-21% and / or ZrO 2 : 7.5-12% and / or P 2 O 5 : 4-8% and / or K 2 O: 0-2% and / or Y 2 O 3 : 2-6%, and / or B 2 O 3 : 0-2% and / or Na 2 O: 1.5-4%, and / or SrO: 0-1%, and / or TiO 2: 0-1%, and / or BaO: 0-1%, and / or CaO: 0-1%, and / or Ln 2 O 3 : 0 to 3%, and / or fining agent: 0 to 0.5%, and the Ln 2 O 3 La 2 O 3 , Gd 2 O 3 , Yb 2 O 3 One or more of the above, and the fining agent is Sb 2 O 3 , SnO 2 , SnO, CeO 2 , F, Cl and Br.

7. 3. The microcrystalline glass product according to claim 1 or 2, wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y 2 O 3 / ZrO 2 is between 0.2 and 0.6; 2) (Li 2 O+ZrO 2 +P 2 O 5 ) / Y 2 O 3 is between 9.0 and 21.0; 3) Al 2 O 3 / (Li 2 O+ZrO 2 +P 2 O 5 ) is between 0.19 and 0.5; 4) Na 2 O / Y 2 O 3 is between 0.3 and 2.0; 5) Y 2 O 3 / (Al 2 O 3 +SiO 2 ) is between 0.03 and 0.

09.

8. 3. The microcrystalline glass product of claim 1 or 2, wherein the crystalline phase of the microcrystalline glass product comprises predominantly lithium monosilicate, the weight percentage of lithium monosilicate is higher than other crystalline phases, and lithium monosilicate constitutes 10% to 63.5% of the microcrystalline glass product.

9. 3. The microcrystalline glass product of claim 1 or 2, wherein the crystalline phase of the microcrystalline glass product comprises predominantly lithium monosilicate, the weight percentage of lithium monosilicate is higher than other crystalline phases, and lithium monosilicate constitutes 15-55% of the microcrystalline glass product.

10. 3. The microcrystalline glass product according to claim 1 or 2, wherein the microcrystalline glass product comprises a lithium phosphate crystalline phase, and the weight percentage of the lithium phosphate crystalline phase in the microcrystalline glass product is between 3 and 15%.

11. The microcrystalline glass product has a surface stress of 600 MPa or more, and / or a four-point bending strength of 600 MPa or more, and / or an ion exchange layer depth of 20 μm or more, and / or a drop ball test height of 1300 mm or more, and / or a fracture toughness of 1 MPa m 1 / 2 and / or Vickers hardness is 700kgf / mm 2 3. The microcrystalline glass product according to claim 1 or 2, wherein the average transmittance at wavelengths from 400 to 800 nm of the microcrystalline glass product is 89% or more, and / or the average transmittance at wavelengths from 550 nm of the microcrystalline glass product is 91% or more, and / or the average light |B| value at 400 to 800 nm of the microcrystalline glass product is 0.6 or less, and / or the crystallinity is 50% or more, and / or the crystal grain size is 50 nm or less, and / or the haze of the microcrystalline glass product having a thickness of 1 mm or less is 0.15% or less, and / or the average transmittance at wavelengths from 400 to 800 nm of the microcrystalline glass product having a thickness of 1 mm or less is 89% or more, and / or the average transmittance at wavelengths from 550 nm of the microcrystalline glass product having a thickness of 1 mm or less is 91% or more, and / or the average light |B| value at 400 to 800 nm of the microcrystalline glass product having a thickness of 1 mm or less is 0.6 or less.

12. The microcrystalline glass product has a surface stress of 700 MPa or more, and / or a four-point bending strength of 700 MPa or more, and / or an ion exchange layer depth of 40 μm or more, and / or a ball drop test height of 1500 mm or more, and / or a fracture toughness of 1.2 MPa m 1 / 2 and / or Vickers hardness is 730kgf / mm 2 3. The microcrystalline glass product according to claim 1 or 2, wherein the crystallinity is 70% or more, and / or the crystal grain size is 30 nm or less, and / or the haze of the microcrystalline glass product having a thickness of 1 mm or less is 0.1% or less, and / or the average light |B| value at 400 to 800 nm of the microcrystalline glass product having a thickness of 1 mm or less is 0.5 or less.

13. 12. The microcrystalline glass product according to claim 11, wherein the thickness of the microcrystalline glass product is between 0.2 and 1 mm.

14. The microcrystalline glass product includes a colorant, the colorant including the following components in weight percent: NiO: 0-4%; and / or Ni 2 O 3 : 0-4%, and / or CoO: 0-2%, and / or Co 2 O 3 : 0-2% and / or Fe 2 O 3 : 0 to 7% and / or MnO 2 : 0-4%, and / or Er 2 O 3 : 0-8% and / or Nd 2 O 3 : 0-8% and / or Cu 2 O: 0-4% and / or Pr 2 O 3 : 0-8% and / or CeO 2 : 0 to 4%, in the microcrystalline glass product according to claim 1 or 2.

15. A microcrystalline glass containing, by weight, the following components: SiO 2 : 53-70%, Al 2 O 3 : 8-18%, Li 2 O: 13.5-25%, ZrO 2 : 7.5-15%, P 2 O 5 : 2-10%, Y 2 O 3 : greater than 0 and less than 8%, K 2 O: 0-4.5%, BaO: 0-1.5%, TiO 2 : 0-1.5%, (Li 2 O+ZrO 2 +P 2 O 5 ) / Y 2 O 3 is 9.0-50.

0.

16. 16. The microcrystalline glass according to claim 15, further comprising the following components in weight percent: MgO: 0-2%, and / or ZnO: 0-2%, and / or Na 2 O: 0-6%, and / or SrO: 0-5%, and / or CaO: 0-5%, and / or B 2 O 3 : 0 to 5%, and / or Ln 2 O 3 : 0 to 5%, and / or clarifier: 0 to 2%, and the Ln 2 O 3 La 2 O 3 , Gd 2 O 3 , Yb 2 O 3 One or more of the above, and the fining agent is Sb 2 O 3 , SnO 2 , SnO, CeO 2 , F, Cl and Br.

17. 17. The microcrystalline glass according to claim 15 or 16, wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following four conditions: 1) Y 2 O 3 / ZrO 2 is greater than 0; 2) Al 2 O 3 / (Li 2 O+ZrO 2 +P 2 O 5 ) is between 0.16 and 0.9; 3) Na 2 O / Y 2 O 3 is 6.0 or less; 4) Y 2 O 3 / (Al 2 O 3 +SiO 2 ) is greater than 0 and less than or equal to 0.

15.

18. 17. The microcrystalline glass according to claim 15 or 16, comprising the following components in weight percent: SiO 2 : 53-65% and / or Al 2 O 3 : 8-15% and / or Li 2 O: 13.5-22% and / or P 2 O 5 : 3.5-9% and / or K 2 O: 0-4%, and / or MgO: 0-1%, and / or ZnO: 0-1%, and / or Na 2 O: 1-5% and / or Y 2 O 3 : 1-7%, and / or SrO: 0-3%, and / or CaO: 0-3%, and / or B 2 O 3 : 0 to 3%, and / or Ln 2 O 3 : 0 to 4%, and / or fining agent: 0 to 1%, and the Ln 2 O 3 La 2 O 3 , Gd 2 O 3 , Yb 2 O 3 One or more of the above, and the fining agent is Sb 2 O 3 , SnO 2 , SnO, CeO 2 , F, Cl and Br.

19. 17. The microcrystalline glass according to claim 15 or 16, wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y 2 O 3 / ZrO 2 is between 0.1 and 1.0; 2) (Li 2 O+ZrO 2 +P 2 O 5 ) / Y 2 O 3 is between 9.0 and 40.0; 3) Al 2 O 3 / (Li 2 O+ZrO 2 +P 2 O 5 ) is between 0.18 and 0.6; 4) Na 2 O / Y 2 O 3 is between 0.1 and 5.0; 5) Y 2 O 3 / (Al 2 O 3 +SiO 2 ) is between 0.01 and 0.

12.

20. 17. The microcrystalline glass according to claim 15 or 16, comprising the following components in weight percent: SiO 2 : 53-63% and / or Al 2 O 3 : 8-12% and / or Li 2 O: 14-21% and / or ZrO 2 : 7.5-12% and / or P 2 O 5 : 4-8% and / or K 2 O: 0-2% and / or Y 2 O 3 : 2-6%, and / or B 2 O 3 : 0-2% and / or Na 2 O: 1.5-4%, and / or SrO: 0-1%, and / or TiO 2 : 0-1%, and / or BaO: 0-1%, and / or CaO: 0-1%, and / or Ln 2 O 3 : 0 to 3%, and / or fining agent: 0 to 0.5%, and the Ln 2 O 3 La 2 O 3 , Gd 2 O 3 , Yb 2 O 3 One or more of the above, and the fining agent is Sb 2 O 3 , SnO 2 , SnO, CeO 2 , F, Cl and Br.

21. 17. The microcrystalline glass according to claim 15 or 16, wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y 2 O 3 / ZrO 2 is between 0.2 and 0.6; 2) (Li 2 O+ZrO 2 +P 2 O 5 ) / Y 2 O 3 is between 9.0 and 21.0; 3) Al 2 O 3 / (Li 2 O+ZrO 2 +P 2 O 5 ) is between 0.19 and 0.5; 4) Na 2 O / Y 2 O 3 is between 0.3 and 2.0; 5) Y 2 O 3 / (Al 2 O 3 +SiO 2 ) is between 0.03 and 0.

09.

22. 17. The microcrystalline glass of claim 15 or 16, wherein the crystalline phase of the microcrystalline glass comprises predominantly lithium monosilicate, the weight percentage of lithium monosilicate is higher than other crystalline phases, and lithium monosilicate constitutes 10% to 63.5% of the microcrystalline glass.

23. 17. The microcrystalline glass of claim 15 or 16, wherein the crystalline phase of the microcrystalline glass comprises predominantly lithium monosilicate, the weight percentage of lithium monosilicate is higher than other crystalline phases, and lithium monosilicate constitutes 15% to 55% of the microcrystalline glass.

24. 17. The microcrystalline glass according to claim 15, wherein the crystal phase of the microcrystalline glass comprises a lithium phosphate crystal phase, and the weight percentage of the lithium phosphate crystal phase in the microcrystalline glass is 3 to 15%.

25. The crystallinity of the microcrystalline glass is 50% or more, and / or the crystal grain size is 50 nm or less, and / or the thermal expansion coefficient is 75 to 95×10 -7 / K, and / or the refractive index is 1.5700 to 1.5800, and / or the body drop test height is 1000 mm or more, and / or the Vickers hardness is 650 kgf / mm 2 and / or the haze degree of the microcrystalline glass having a thickness of 1 mm or less is 0.15% or less, and / or the average transmittance of the microcrystalline glass having a thickness of 1 mm or less at a wavelength of 400 to 800 nm is 89% or more, and / or the average transmittance of the microcrystalline glass having a thickness of 1 mm or less at a wavelength of 550 nm is 91% or more, and / or the average light |B| value of the microcrystalline glass having a thickness of 1 mm or less at a wavelength of 400 to 800 nm is 0.6 or less.

26. The crystallinity of the microcrystalline glass is 70% or more, and / or the crystal grain size is 30 nm or less, and / or the body drop ball test height is 1200 mm or more, and / or the Vickers hardness is 700 kgf / mm 2 17. The microcrystalline glass according to claim 15 or 16, wherein the haze of the microcrystalline glass having a thickness of 1 mm or less is 0.1% or less, and / or the average light |B| value from 400 to 800 nm of the microcrystalline glass having a thickness of 1 mm or less is 0.5 or less.

27. 26. The microcrystalline glass according to claim 25, wherein the thickness of the microcrystalline glass is 0.2 to 1 mm.

28. The microcrystalline glass contains a colorant, and the colorant contains the following components in weight percent: NiO: 0 to 4%, and / or Ni 2 O 3 : 0-4%, and / or CoO: 0-2%, and / or Co 2 O 3 : 0-2% and / or Fe 2 O 3 : 0 to 7% and / or MnO 2 : 0-4%, and / or Er 2 O 3 : 0-8% and / or Nd 2 O 3 : 0-8% and / or Cu 2 O: 0-4% and / or Pr 2 O 3 : 0-8% and / or CeO 2 : 0 to 4%, the microcrystalline glass according to claim 15 or 16.

29. A matrix glass containing the following components in weight percent: SiO 2 : 53-70%, Al 2 O 3 : 8-18%, Li 2 O: 13.5-25%, ZrO 2 : 7.5-15%, P 2 O 5 : 2-10%, Y 2 O 3 : greater than 0 and less than 8%, K 2 O: 0-4.5%, BaO: 0-1.5%, TiO 2 : 0-1.5%, (Li 2 O+ZrO 2 +P 2 O 5 ) / Y 2 O 3 is 9.0-50.

0.

30. 30. The matrix glass according to claim 29, further comprising the following components in weight percent: MgO: 0-2%, and / or ZnO: 0-2%, and / or Na. 2 O: 0-6%, and / or SrO: 0-5%, and / or CaO: 0-5%, and / or B 2 O 3 : 0 to 5%, and / or Ln 2 O 3 : 0 to 5%, and / or clarifier: 0 to 2%, and the Ln 2 O 3 La 2 O 3 , Gd 2 O 3 , Yb 2 O 3 One or more of the above, and the fining agent is Sb 2 O 3 , SnO 2 , SnO, CeO 2 , F, Cl and Br.

31. 31. The matrix glass according to claim 29 or 30, wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following four conditions: 1) Y 2 O 3 / ZrO 2 is greater than 0; 2) Al 2 O 3 / (Li 2 O+ZrO 2 +P 2 O 5 ) is between 0.16 and 0.9; 3) Na 2 O / Y 2 O 3 is 6.0 or less; 4) Y 2 O 3 / (Al 2 O 3 +SiO 2 ) is greater than 0 and less than or equal to 0.

15.

32. 31. The matrix glass according to claim 29 or 30, wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y 2 O 3 / ZrO 2 is between 0.1 and 1.0; 2) (Li 2 O+ZrO 2 +P 2 O 5 ) / Y 2 O 3 is between 9.0 and 40.0; 3) Al 2 O 3 / (Li 2 O+ZrO 2 +P 2 O 5 ) is between 0.18 and 0.6; 4) Na 2 O / Y 2 O 3 is between 0.1 and 5.0; 5) Y 2 O 3 / (Al 2 O 3 +SiO 2 ) is between 0.01 and 0.

12.

33. 31. The matrix glass according to claim 29 or 30, wherein the components are expressed in weight percent and the content of each component satisfies one or more of the following five conditions: 1) Y 2 O 3 / ZrO 2 is between 0.2 and 0.6; 2) (Li 2 O+ZrO 2 +P 2 O 5 ) / Y 2 O 3 is between 9.0 and 21.0; 3) Al 2 O 3 / (Li 2 O+ZrO 2 +P 2 O 5 ) is between 0.19 and 0.5; 4) Na 2 O / Y 2 O 3 is between 0.3 and 2.0; 5) Y 2 O 3 / (Al 2 O 3 +SiO 2 ) is between 0.03 and 0.

09.

34. 31. A matrix glass according to claim 29 or 30, comprising the following components in weight percent: SiO 2 : 53-65% and / or Al 2 O 3 : 8-15% and / or Li 2 O: 13.5-22% and / or P 2 O 5 : 3.5-9% and / or K 2 O: 0-4%, and / or MgO: 0-1%, and / or ZnO: 0-1%, and / or Na 2 O: 1-5% and / or Y 2 O 3 : 1-7%, and / or SrO: 0-3%, and / or CaO: 0-3%, and / or B 2 O 3 : 0 to 3%, and / or Ln 2 O 3 : 0 to 4%, and / or fining agent: 0 to 1%, and said Ln 2 O 3 La 2 O 3 , Gd 2 O 3 , Yb 2 O 3 One or more of the above, and the fining agent is Sb 2 O 3 , SnO 2 , SnO, CeO 2 , F, Cl and Br.

35. 31. A matrix glass according to claim 29 or 30, comprising the following components in % by weight: SiO 2 : 53-63% and / or Al 2 O 3 : 8-12% and / or Li 2 O: 14-21% and / or ZrO 2 : 7.5-12% and / or P 2 O 5 : 4-8% and / or K 2 O: 0-2% and / or Na 2 O: 1.5-4% and / or Y 2 O 3 : 2-6%, and / or SrO: 0-1%, and / or BaO: 0-1%, and / or TiO 2 : 0-1%, and / or CaO: 0-1%, and / or B 2 O 3 : 0-2%, and / or Ln 2 O 3 : 0 to 3%, and / or fining agent: 0 to 0.5%, and the Ln 2 O 3 La 2 O 3 , Gd 2 O 3 , Yb 2 O 3One or more of the above, and the fining agent is Sb 2 O 3 , SnO 2 , SnO, CeO 2 , F, Cl and Br.

36. The thermal expansion coefficient of the matrix glass is 50×10 -7 / K~70×10 -7 31. The matrix glass according to claim 29 or 30, wherein the refractive index of the matrix glass is 1.5600 to 1.5700.

37. The matrix glass contains a colorant, and the colorant contains the following components in weight percent: NiO: 0 to 4%, and / or Ni 2 O 3 : 0-4%, and / or CoO: 0-2%, and / or Co 2 O 3 : 0-2% and / or Fe 2 O 3 : 0 to 7% and / or MnO 2 : 0-4%, and / or Er 2 O 3 : 0-8% and / or Nd 2 O 3 : 0-8% and / or Cu 2 O: 0-4% and / or Pr 2 O 3 : 0-8% and / or CeO 2 : 0 to 4%, the matrix glass according to claim 29 or 30.

38. A glass cover plate comprising a microcrystalline glass product according to any one of claims 1 to 14, and / or a microcrystalline glass according to any one of claims 15 to 28, and / or a matrix glass according to any one of claims 29 to 37.

39. A glass element comprising a microcrystalline glass product according to any one of claims 1 to 14, and / or a microcrystalline glass according to any one of claims 15 to 28, and / or a matrix glass according to any one of claims 29 to 37.

40. A display device comprising a microcrystalline glass product according to any one of claims 1 to 14, and / or a microcrystalline glass according to any one of claims 15 to 28, and / or a matrix glass according to any one of claims 29 to 37, and / or a glass cover plate according to claim 38, and / or a glass element according to claim 39.

41. 38. An electronic device comprising a microcrystalline glass product according to any one of claims 1 to 14, and / or a microcrystalline glass according to any one of claims 15 to 28, and / or a matrix glass according to any one of claims 29 to 37, and / or a glass cover plate according to claim 38, and / or a glass element according to claim 39.

42. A method for producing a microcrystalline glass product according to any one of claims 1 to 14, said method comprising the steps of: A matrix glass is formed, a microcrystalline glass is formed from the matrix glass by a crystallization process, and a microcrystalline glass product is formed from the microcrystalline glass by a chemical strengthening process.

43. The method for producing a microcrystalline glass product according to claim 42, wherein the crystallization step includes the steps of: increasing the temperature to a predetermined crystallization temperature, and after reaching the crystallization temperature, maintaining the temperature for a certain period of time, and then decreasing the temperature; the crystallization temperature is 600-750°C, and the maintaining time of the crystallization temperature is 0-8 hours.

44. The method for producing a microcrystalline glass product according to claim 42, wherein the crystallization step includes the steps of: raising the temperature to a predetermined crystallization temperature, and after reaching the crystallization temperature, maintaining the temperature for a certain period of time, and then lowering the temperature; the crystallization temperature is 650-700°C, and the maintaining time of the crystallization temperature is 1-6 hours.

45. The method for producing a microcrystalline glass product according to claim 42, wherein the crystallization step comprises the steps of: performing a nucleation step at a first temperature, followed by a crystal growth step at a second temperature higher than the temperature of the nucleation step, the first temperature being 470-630°C, the second temperature being 650-750°C, the holding time at the first temperature being 0-24 hours, and the holding time at the second temperature being 0-10 hours.

46. The method for producing a microcrystalline glass product according to claim 42, wherein the crystallization step comprises the steps of: performing a nucleation step at a first temperature, followed by a crystal growth step at a second temperature higher than the temperature of the nucleation step, the first temperature being 470-630°C, the second temperature being 650-750°C, the holding time at the first temperature being 2-15 hours, and the holding time at the second temperature being 0.5-6 hours.

47. The method for producing a microcrystalline glass product according to claim 42, wherein the chemical strengthening step comprises the steps of: immersing the microcrystalline glass in a salt bath containing molten Na salt at a temperature of 430°C to 470°C for 6 to 20 hours, and / or immersing the microcrystalline glass in a salt bath containing molten K salt at a temperature of 400°C to 450°C for 1 to 8 hours.

48. The method for producing a microcrystalline glass product according to claim 42, wherein the chemical strengthening step comprises the steps of: immersing the microcrystalline glass in a salt bath containing molten Na salt at a temperature of 435°C to 460°C for 8 to 13 hours, and / or immersing the microcrystalline glass in a salt bath containing molten K salt at a temperature of 400°C to 450°C for 2 to 4 hours.

49. A method for producing microcrystalline glass according to any one of claims 15 to 28, said method comprising the steps of: A matrix glass is formed and then processed into a microcrystalline glass by a crystallization process.

50. The crystallization process includes the following steps: heating to a predetermined crystallization temperature, and after the crystallization temperature is reached, maintaining the temperature for a certain period of time, and then lowering the temperature, the crystallization temperature being 600-750°C, and the crystallization temperature maintaining time being 0-8 hours.

51. The crystallization process includes the following steps: the manufacturing method of the microcrystalline glass according to claim 49, the temperature is raised to a predetermined crystallization temperature, and after the crystallization temperature is reached, the temperature is maintained for a certain period of time, and then the temperature is lowered, the crystallization temperature is 650-700°C, and the crystallization temperature is maintained for 1-6 hours.

52. The method for producing microcrystalline glass according to claim 49, wherein the crystallization step includes the steps of: performing a nucleation step at a first temperature, and then performing a crystal growth step at a second temperature higher than the temperature of the nucleation step, the first temperature being 470-630°C, the second temperature being 650-750°C, the holding time at the first temperature being 0-24 hours, and the holding time at the second temperature being 0-10 hours.

53. The method for producing microcrystalline glass according to claim 49, wherein the crystallization step includes the steps of: performing a nucleation step at a first temperature, and then performing a crystal growth step at a second temperature higher than the temperature of the nucleation step, the first temperature being 470-630°C, the second temperature being 650-750°C, the holding time at the first temperature being 2-15 hours, and the holding time at the second temperature being 0.5-6 hours.

Citation Information

Patent Citations

  • Surface treated solder ball and surface treatment method of solder ball

    JP2008272779A

  • Crystallized glass of three-dimensional shape, chemically strengthened glass of three-dimensional shape, and method for producing crystallized glass of three-dimensional shape and chemically strengthened glass of three-dimensional shape

    WO2019167850A1

  • Crystallized glass, chemically strengthened glass, and semiconductor substrate

    WO2020161949A1