System and method for reducing refractory metal oxides using a liquid metal crucible

The use of a liquid metal crucible and eutectic phase reaction in the Kroll process addresses environmental and cost issues, enabling high-purity metal production with low oxygen content.

JP7580604B2Active Publication Date: 2024-11-11KSM TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023529926
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-17
Filing Date
2021-03-29
Publication Date
2024-11-11
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

The Kroll process for producing metals like titanium and zirconium is environmentally hazardous due to chlorine gas byproducts, costly due to equipment corrosion and replacement needs, and difficult to achieve high purity metals with controlled oxygen content.

Method used

A system and method using a liquid metal crucible with a eutectic phase reaction to reduce metal oxides without chlorides, employing a liquid metal alloy to form a eutectic phase with the metal oxide and reducing agent, allowing electrolytic reduction at lower temperatures and preventing oxygen contamination.

Benefits of technology

This approach achieves high purity metals with low oxygen content, reduces environmental hazards, and lowers operational costs by minimizing equipment corrosion and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580604000002
    Figure 0007580604000002
  • Figure 0007580604000003
    Figure 0007580604000003
  • Figure 0007580604000004
    Figure 0007580604000004
Patent Text Reader

Abstract

The present invention relates to a method for producing a metal M from a metal oxide. 1 The present invention provides a system and method for reducing
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a system and method for reducing refractory metal oxides using a liquid metal crucible. [Background technology]

[0002] When a metal typically known in the art is referred to as any metal "M", the metal M can be obtained by reducing a raw material such as an oxide or halide. Among the methods for producing a desired metal M, the relatively well-known method and the most widely and commonly used method in the art is the so-called Kroll process.

[0003] Typically, the Kroll process can be summarized as using molten magnesium as a reducing agent to reduce the chloride of the target metal M, such as titanium chloride or zirconium chloride, to titanium or zirconium. In this regard, more detailed information on the Kroll process can be found in U.S. Patent No. 5,035,404.

[0004] The Krol process uses chlorides as raw materials, and thus produces chlorine gas and magnesium chloride as by-products during the process. Among these by-products, chlorine gas is an environmental problem that can cause fatal problems to the human body and is considered to be a representative problem of the Krol process, while magnesium chloride causes process problems such as rapid corrosion of reaction vessels, such as electrolytic cells, melting furnaces, and crucibles.

[0005] Thus, the Kroll process has the disadvantages of requiring additional equipment to meet environmentally acceptable standards and of being expensive to operate due to the frequent changeover of reaction vessels.

[0006] In another aspect, the Kroll process produces metal in a sponge form containing many voids, making it very difficult to control oxygen that may be present in the metal, i.e., the Kroll process has limitations in obtaining high-purity metals.

[0007] Meanwhile, a method is being considered to overcome the shortcomings of the Kroll process by producing an alloy of the desired metals using CuCa or NiCa as a reducing agent and then electrolytically refining the alloy.

[0008] However, in this method, the reducing agent, which has a strong reducing power, comes into direct contact with parts of the reactor in the process system, which causes the problem of corrosion of the reactor, just like the Kroll process. There is also a method of minimizing the effect of the reducing agent by manufacturing the reactor from W or Mo metal, but the cost of such a reactor itself is very high, which increases the overall manufacturing cost. In addition, to continue the process continuously, CaO, a by-product generated in the reduction reaction, must be removed, and a large amount of electrolyte is required to remove it. This also causes a problem of increasing the overall manufacturing cost.

[0009] Therefore, there is a current demand for a completely new technology that can not only solve the problems of the Kroll process at once, but also easily operate the process to obtain the desired metal M and obtain a large amount of high-purity metal. Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide a technique capable of solving the above-mentioned problems.

[0011] The present invention provides a system optimized for obtaining desired metals from metal oxides without using any chlorides as metal chlorides or electrolytes, and a method for producing such metals. Therefore, the present invention can solve the environmental problems of the Kroll process and the cost problems associated with corrosion of the electrolytic cell.

[0012] Furthermore, the present invention provides a technology that can obtain a large amount of high-purity metal while easily operating the process due to the following aspects.

[0013] In one aspect of the present invention, the systems and methods provided herein include a method for preparing metals M that form a eutectic phase with each other. 1 and metal M 2 The present invention is characterized by the use of a liquid metal crucible containing a liquid metal alloy of the above formula.

[0014] The use of such a liquid metal crucible is advantageous in that it is possible to obtain a liquid metal M out of the metal oxides contained in the raw material module. 1 When is reduced, a eutectic reaction occurs to form metal M 1 Because of the low melting point of , the electrolytic reduction can be carried out effectively at relatively low temperatures, resulting in significant energy savings which can translate into cost savings.

[0015] In the above system and method, a liquid alloy (M 1 and M. 2 Since the metal alloy is obtained in a liquid state, the metal alloy itself can be used as the final product. The final product derived from such a liquid alloy has a significantly smaller specific surface area that can be exposed to oxygen than the sponge-like product of the Kroll process, so the system and method of the present invention can minimize the problem of the product being contaminated by oxygen.

[0016] Alternatively, the obtained metal alloy is electrolytically refined to produce metal M. 1The liquid alloy thus obtained can be thoroughly isolated from an environment in which oxygen may be present, and therefore contamination by oxygen can be significantly prevented. 1 It is possible to obtain the following.

[0017] In another aspect of the present invention, in the system and method provided by the present invention, the source material, for example, an oxide containing a target metal, a reducing agent, and a metal for alloying, form a module as one part, and such a source module is used. In a process in which a plurality of sources are continuously fed into an electrolytic cell, such as the Kroll process, the source material may be oxidized or contaminated with oxygen before being fed, but the source module according to the present invention has a structure that is treated to prevent oxidation, and therefore has a stronger oxygen blocking effect than the Kroll process. As a result, the metal alloy and metal obtained by the present invention can have a significantly lower oxygen content, in other words, the present invention can realize high-purity metal alloy and metal with almost no oxygen.

[0018] These aspects of the present invention overcome the problems of the prior art and at the same time make it possible to easily produce metal of excellent quality. The technical basis for the implementation of the present invention will be described in detail below. [Means for solving the problem]

[0019] In one embodiment of the present invention, a metal M is prepared from a metal oxide. 1 A system for refunding is provided.

[0020] In one embodiment of the present invention, the system comprises:

[0021] An electrolytic cell;

[0022] The metals M are received from the bottom of the electrolytic cell and form a eutectic phase with each other. 1 and metal M 2 a liquid metal crucible containing a liquid metal alloy of

[0023] a liquid electrolyte contained in the electrolytic cell while forming an unmixed layer on the liquid metal crucible;

[0024] The metal oxide, metal M 2 , and a reducing agent metal M 3 and a solid source module including:

[0025] In the system, the solid source module reaches the liquid metal crucible and melts the metal oxide and the reducing agent metal M 3 In response, M 1 is reduced, and the reduced M 1 and M. 2 may be continuously mixed into the liquid metal crucible while forming a liquid metal alloy.

[0026] In one specific example, the system comprises a reduced M 1 and M. 2 The liquid metal alloy formed by the above is collected and electrolytically refined to obtain metal M. 1 The apparatus may further include an electrolytic refining unit for obtaining the above-mentioned.

[0027] In one specific example, the metal oxide is M 1 x O z and M. 1 x M 3 y O z wherein x, y are each a real number from 1 to 3, and z is a real number from 1 to 4.

[0028] In one specific example, the solid source module includes the metal oxide and the reducing agent metal M 3 A core layer including a core material and a core material covering the core layer, 2 and a shell layer composed of

[0029] In one specific example, the solid source module has a multi-layer structure including a core layer containing the metal oxide and a shell layer coated on the outer surface of the core layer, and the shell layer is a metal M 2 and the metal M 3 The alloy phase may include

[0030] In one specific example, the solid source module is configured to descend vertically from within the electrolytic cell through the electrolyte until it reaches the liquid metal crucible, and may descend at a rate of 0.1% to 10% of the distance per minute (min) relative to the depth of the electrolytic cell.

[0031] In one specific example, the solid source module is melted while the metal oxide and the reducing agent metal M 3 In response, M 1 When reducing the oxide M 3 a O b is generated, and 3 a O b may have a relatively low specific gravity compared to the electrolyte, where a and b are each real numbers from 1 to 3.

[0032] In one specific example, the M 3 a O b can float to the top of the electrolyte due to density differences and form a by-product layer.

[0033] In one specific example, the liquid metal alloy is continuously obtained through the lower part of the electrolytic cell and the by-product layer is continuously collected through the upper part of the electrolytic cell depending on the progress of the process, thereby enabling a continuous process.

[0034] In one specific example, the by-product layer is collected and 1 x O z Mixed with M 1 x M 3 y Oz The present invention may further include a recycling device for producing the above-mentioned.

[0035] In one specific example, the reaction of the metal oxide with the reductant metal can be carried out in an inert gas and / or in air.

[0036] In one specific example, the core layer is made of the metal oxide powder and the reducing agent metal M 3 It may consist of a mixture of powders including powder.

[0037] In one specific example, the core layer is coated to cover the first core made of the metal oxide and the outer shell surface of the first core, and the metal M 3 The second core may be a multi-layer structure including:

[0038] In one specific example, the solid source module may further include an anti-oxidation layer covering the shell layer to prevent oxidation of the metal contained in the core layer and / or the shell layer.

[0039] In one specific example, the antioxidant layer may include one or more selected from the group consisting of LiF, MgF2, CaF2, BaF2, CaCl2, MgCl2, MgO, CaO, BaO, Al2O3, and SiO2.

[0040] In one specific example, M 1 may be one selected from the group consisting of Ti, Zr, Hf, W, Fe, Ni, Zn, Co, Mn, Cr, Ta, Ga, Nb, Sn, Ag, La, Ce, Pr, Nd, Nb, Pm, Sm, Eu, Al, V, Mo, Gd, Tb, Dy, Ho, Er, Tm, Yb, Ac, Th, Pa, U, Np, Pu, Am, Cm, Bk, Cf, Es, Fm, Md, and No; 2 may be one or more selected from Cu, Ni, Fe, Sn, Zn, Pb, Bi, Cd, and alloys thereof; M 3 may be one or more selected from Ca, Mg, Al, and alloys thereof.

[0041] In one embodiment of the present invention, the metal oxide is a metal M 1 A method for reducing and refining the sintered material is provided.

[0042] In one embodiment of the present invention, the method comprises the steps of:

[0043] providing an electrolytic cell;

[0044] introducing a liquid electrolyte into the electrolytic cell;

[0045] In the electrolytic bath, metals M which form a eutectic phase with each other are added. 1 and metal M 2 a liquid metal crucible that has a relatively high specific gravity compared to the electrolyte and forms an unmixed layer under the electrolyte to be contained in the electrolytic cell;

[0046] The metal oxide and the metal M 2 , and a reducing agent metal M 3 moving a solid source module including the liquid metal crucible through the electrolyte until the liquid metal crucible is reached;

[0047] Metal M derived from the metal oxide of the solid source module 1 and M. 2 and obtaining a liquid metal alloy comprising:

[0048] In one specific example, in the step of moving the solid source module and / or the step of obtaining the liquid metal alloy in the method, a by-product oxide M 3 a O b is generated, and 3 a O b has a relatively low specific gravity compared to the electrolyte,

[0049] The method includes forming a layer on an electrolyte,3 a O b is continuously collected, and 3 a O b M 1 x O z and mixing to obtain the by-product M 3 a O b and added M 1 x O z M comes from 1 x M 3 y O z The method may further include the step of preparing a metal oxide represented by the formula:

[0050] In one embodiment of the present invention, a metal alloy or metal obtained by the method according to the above embodiment is provided, and the metal alloy is provided with a reducing agent metal M in comparison to its total weight. 3 The residual content may be less than or equal to 0.1 wt %, specifically less than or equal to 0.01 wt %, and more specifically less than or equal to 0.001 wt %, and the oxygen content may be less than or equal to 1,200 ppm, specifically less than or equal to 1,000 ppm, and more specifically less than or equal to 990 ppm. Effect of the Invention

[0051] The present invention provides a system and method for producing a desired metal from a metal oxide without using any chlorides, such as metal chlorides or electrolytes, that is optimized to obtain the desired metal from the metal oxide. Therefore, the present invention can eliminate the environmental problems of the Kroll process and the cost problems associated with corrosion of the electrolytic cell.

[0052] The system and method provided herein is directed to metals M that form a eutectic phase with each other. 1 and metal M 2 The liquid metal crucible is characterized by the use of a liquid metal alloy containing the above-mentioned liquid metal alloy. The use of such a liquid metal crucible is advantageous in that the metal M among the metal oxides contained in the raw material module is dissolved in the liquid metal alloy. 1When is reduced, a eutectic reaction occurs to form metal M 1 Because of the low melting point of , the electrolytic reduction can be carried out effectively at relatively low temperatures, resulting in significant energy savings which can translate into cost savings.

[0053] In the above system and method, a liquid alloy (M 1 and M. 2 Since the metal alloy is obtained in a liquid state, the metal alloy itself can be used as the final product. The final product derived from such a liquid alloy has a significantly smaller specific surface area that can be exposed to oxygen than the sponge-like product of the Kroll process, so the system and method of the present invention can minimize the problem of the product being contaminated by oxygen.

[0054] The liquid alloy thus obtained can be thoroughly isolated from an environment in which oxygen may be present, and therefore contamination by oxygen can be significantly prevented. 1 It is possible to obtain the following.

[0055] In the system and method provided by the present invention, the raw material is formed as a module in which, for example, an oxide containing a target metal, a reducing agent, and a metal for alloying are integrated into one component, and such a raw material module is used. In a process in which a plurality of raw materials are continuously fed into an electrolytic cell, such as the Kroll process, the raw materials may be oxidized or contaminated with oxygen before being fed, but the raw material module according to the present invention includes a structure that is treated to prevent oxidation, and therefore has a stronger oxygen blocking effect than the Kroll process. As a result, the metal alloy and metal obtained by the present invention can have a significantly lower oxygen content, in other words, the present invention can realize high-purity metal alloy and metal with almost no oxygen. [Brief description of the drawings]

[0056] [Figure 1] FIG. 1 is a schematic diagram of a system according to one embodiment of the present invention. [Diagram 2] 1 is a photograph showing a process of manufacturing a source module including a metal oxide, MgTiO3, according to one embodiment of the present invention. [Diagram 3] 3 is a graph showing the results of XRD analysis of the raw material produced in FIG. 2. [Figure 4] FIG. 2 is a schematic vertical cross-sectional view of a feedstock module according to one embodiment of the present invention. [Diagram 5] FIG. 2 is a schematic vertical cross-sectional view of a raw material module according to another embodiment of the present invention. [Figure 6] FIG. 2 is a schematic vertical cross-sectional view of a raw material module according to yet another embodiment of the present invention. [Figure 7] This is a photograph of the raw material module. [Figure 8] 13 is yet another photograph of the raw material module. [Figure 9] 4 is a photograph showing a weight comparison before and after removing an electrolyte from an alloy ingot manufactured in accordance with an embodiment. [Figure 10] 1 is a table showing the results of elemental analysis of the inside of an alloy by an energy dispersive spectrometer (EDS) after cutting the alloy manufactured in the examples. [Figure 11] This is a table showing the results of measuring the oxygen content present in the alloy using an ELTRA ONH2000. Specific Modes for Carrying Out the Invention

[0057] Hereinafter, the intention, action, and effect of the present invention will be described in detail through specific explanations and examples for carrying out the present invention, which will help understand the embodiments of the present invention. However, the following explanations and examples are presented as examples for helping understand the present invention as described above, and are not intended to define or limit the scope of the invention.

[0058] Before describing the present invention in detail, the terms and words used in the specification and claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term in order to best describe his / her invention.

[0059] Therefore, it should be understood that the configuration of the embodiment described in this specification is merely one of the most preferred embodiments of the present invention and does not represent the entire technical idea of ​​the present invention, and therefore, at the time of this application, there may be various equivalents and modifications that can replace these.

[0060] In this specification, the singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, the terms "comprise", "provide", "have", and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the possibility of the presence or addition of one or more different features, numbers, steps, components, or combinations thereof.

[0061] The term "charging" as used herein may be used interchangeably with "introducing," "introducing," "injecting," and "injecting" herein and may be understood to mean delivering or putting any substance, such as a raw material, into a required location.

[0062] In the following, metal M 1 The present invention will be described in detail in the order of the reduction system, the reduction method, and examples.

[0063] 1.Metal M 1 Rebate system

[0064] In one specific example, the metal M is produced from the metal oxide according to the present invention. 1A system for reducing is shown diagrammatically in Figure 1. Referring to Figure 1, the system according to the present invention comprises:

[0065] An electrolytic cell 400;

[0066] The metals M are received from the bottom of the electrolytic cell 400 and form a eutectic phase with each other. 1 and metal M 2 a liquid metal crucible 100 containing a liquid metal alloy of

[0067] a liquid electrolyte 200 contained in an electrolytic cell, the liquid electrolyte 200 forming an unmixed layer on the liquid metal crucible 100 to block the inflow of oxygen and reaction by-products into the liquid metal crucible 100;

[0068] The metal oxide, the metal M 2 , and a reducing agent metal M 3 A solid source module 300 including:

[0069] Here, the solid source module 300 is melted by reaching the liquid metal crucible 100 and melting the metal oxide and the reducing metal M 3 In response, M 1 is reduced, and the reduced M 1 and M. 2 may be continuously mixed into the liquid metal crucible 100 while forming a liquid metal alloy.

[0070] In the system of the present invention, the target metal M 1is not particularly limited, and specifically may be one selected from the group consisting of Ti, Zr, Hf, W, Fe, Ni, Zn, Co, Mn, Cr, Ta, Ga, Nb, Sn, Ag, La, Ce, Pr, Nd, Nb, Pm, Sm, Eu, Al, V, Mo, Gd, Tb, Dy, Ho, Er, Tm, Yb, Ac, Th, Pa, U, Np, Pu, Am, Cm, Bk, Cf, Es, Fm, Md, and No, more specifically may be one selected from the group consisting of Ti, Zr, W, Fe, Ni, Zn, Co, Mn, Cr, Ta, Er, and No, even more specifically may be one selected from the group consisting of Ti, Zr, W, Fe, Ni, Zn, Co, Mn, and Cr, and particularly specifically may be Ti, Zr, or W.

[0071] In the system of the present invention, the metal M 2 is metal M 1 The metal is not particularly limited as long as it can form a liquid metal alloy through a eutectic reaction with the metal, and specifically, the metal may be one or more selected from Cu, Ni, Fe, Sn, Zn, Pb, Bi, Cd, and alloys thereof, and more specifically, the metal may be Cu, Ni, or an alloy thereof.

[0072] In the system of the present invention, the metal M 3 The metal oxide is M. 1 As long as it can be reduced to the above, there is no particular limitation, but among such substances, one or more selected from Ca, Mg, Al, and alloys thereof may be preferable, more specifically Ca or Mg, and particularly specifically Mg.

[0073] In the system of the present invention, the metal oxide is M 1 x O z and M. 1 x M 3 y O z wherein x, y are each a real number from 1 to 3, and z is a real number from 1 to 4.

[0074] To aid in understanding, non-limiting examples of the metal oxides can include one or a combination of two or more selected from the group consisting of ZrO2, TiO2, MgTiO3, HfO2, Nb2O5, Dy2O3, Tb4O7, WO3, Co3O4, MnO, Cr2O3, MgO, CaO, Al2O3, Ta2O5, Ga2O3, Pb3O4, SnO, NbO, and Ag2O.

[0075] The system of the present invention differs from the conventional Kroll process in that it uses metal oxides instead of metal chlorides as raw materials. Typically, raw materials found in nature are M 1 However, in order to use it in the Kroll process, a pretreatment process is required to convert these metal oxides to chlorides. The pretreatment process itself increases the process cost. Furthermore, hydrochloric acid is used in the pretreatment process to convert metal oxides to chlorides, but the strong acidity promotes corrosion of the manufacturing equipment and may generate toxic chlorine gas during the process, which may cause environmental problems. The other system of the present invention does not require a pretreatment process to convert metal oxides to chlorides, so it has the advantage of being lower in process cost than the Kroll process and not causing environmental problems.

[0076] In terms of durability, the electrolytic cell 400 is preferably made of a material that has a high melting point and does not induce side reactions with the electrolyte and the liquid metal crucible. The material of the electrolytic cell may include, but is not limited to, one or more selected from the group consisting of MgO, Cr2O3, Al2O3, SiO2, CaO, SiC, WO3, W, C, and Mo.

[0077] The electrolytic cell 400 may include a tapping port 410 at the bottom thereof for continuously tapping the produced liquid metal alloy.

[0078] As used in the present invention, the term "liquid metal crucible" may mean a reaction region in which at least one metal is in a molten and fluid state and is contained, for example, in an electrolytic cell of the present invention to form a layer, and in which, and on the surface of the layer, a raw material module of the present invention is melted to create an environment in which metal oxides can be reduced.

[0079] The system of the present invention has advantages associated with the use of such liquid metal crucibles.

[0080] Specifically, the system of the present invention comprises metals M 1 and metal M 2 By using a liquid metal crucible containing a liquid metal alloy of 1 is reduced and at the same time, metal M 1 Since the melting point of the metal M is low, electrolytic reduction can be effectively performed at a relatively low temperature. That is, the system of the present invention is capable of operating a liquid metal crucible in which the metal is molten and liquid, and obtaining a liquid metal alloy. 1 The process can be run at temperatures below the melting point of M, resulting in significant energy savings. 1 and M. 2 The temperature may vary depending on the type of material, but is preferably 900°C to 1600°C.

[0081] Also of note with respect to the liquid metal crucible is that the liquid alloy (M 1 and M. 2 Since the product is obtained in the form of a liquid metal alloy, the metal alloy itself can be used as the final product. 1 is often used industrially in the form of an alloy, but as in the conventional Kroll process, M 1 If M can only be produced as a single metal, a post-processing step of alloying with other metals may be required. However, the present invention provides the ability to simultaneously produce M without such a post-processing step.1 and M. 2 In addition, when forming the liquid metal crucible, the M 1 and M. 2 The ratio of metal oxide and M can be adjusted in the module. 2 The ratio of M can be adjusted so that the final product, the metal alloy, 1 and M. 2 If necessary, the obtained metal alloy can be electrolytically refined to obtain metal M. 1 can be obtained, and such electrolytic refining can be carried out by any method known in the art.

[0082] The liquid alloy obtained by the present invention can be thoroughly isolated from an environment in which oxygen may be present, and therefore contamination by oxygen can be significantly prevented. 1 It is possible to obtain the following.

[0083] Furthermore, metals M that form a eutectic phase with each other 1 and metal M 2 The use of a liquid metal crucible containing the liquid metal alloy of the present invention allows the liquid metal alloy to be mixed with the desired metal M even if the metal oxide contained in the raw material is a substance that is difficult to electrolytically reduce to a metal. 1 This has the advantage that the metal oxide of the raw material module can be more easily reduced using the standard redox potential difference of 1. 1 Metal M having a standard reduction potential more positive than that of 2 When using a liquid metal crucible, 1 Since the standard reduction potential value of isopropanol is shifted in the positive direction, electrolytic reduction of metals can be achieved more easily.

[0084] In one main aspect of the present invention, the system of the present invention does not input a metal oxide as a raw material, another metal as a reducing agent, and other different additive metals, but rather forms a raw material module as a single component, and based on such a raw material module, metal alloys and metals of higher quality can be obtained.

[0085] For example, in a process in which multiple raw materials are continuously fed into an electrolytic cell, such as the Kroll process, the raw materials may be oxidized before being fed, but the raw material module according to the present invention includes a structure that is treated to prevent oxidation, and therefore has a stronger oxygen blocking effect than the Kroll process. As a result, the metal alloy and metal obtained according to the present invention can have a significantly lower oxygen content.

[0086] In addition, the system of the present invention includes a structure in which oxygen is blocked doubly, since the electrolyte serves as a blocking film for blocking oxygen as described above, and the module itself, which is the raw material, can also block oxygen. As a result, the system of the present invention has a considerable advantage in that it can operate the reaction between metal oxide and reducing metal not only in an inert gas atmosphere, which is commonly recognized in the art, but also in the air. Even if the system of the present invention is operated in the air, the metal alloy and metal produced thereby are highly pure with almost no oxygen. This will be clearly demonstrated through the examples described below. In some cases, the system of the present invention can be used to operate the reaction between metal oxide and reducing metal in both an inert gas atmosphere and an air atmosphere.

[0087] In addition, the system of the present invention uses a raw material module in which the raw materials necessary for the reaction are collected in one place, which has the advantage that the reaction can be easily induced at the optimal position in the electrolytic cell.

[0088] Photographs of the process of manufacturing the raw material module according to the present invention are shown in Fig. 2, and a schematic diagram of the raw material module according to one embodiment of the present invention is shown in Fig. 4. It should be noted that the photographs shown in Fig. 2 are merely intended to facilitate understanding of the manufacturing of the raw material module as a non-limiting example, and are not intended to limit the scope of the present invention.

[0089] Referring to FIG. 4, the solid source module 300 includes a metal oxide 10 and a reducing agent metal M 3 A core layer 310 including 30 and a core layer 310 covering the core layer 310, 2 4, the core layer 310 is coated to cover the first core 311 made of the metal oxide 10 and the outer surface of the first core 311, and the reducing agent metal M 3 The second core 312 may be a multi-layer structure including a second core 312 made of 30 .

[0090] In some cases, a raw material module 300a as shown in FIG. 5 may be used in which the core layer is another example of the present invention. The core layer 310a of such a raw material module 300a is made of a metal oxide powder 10a and a reducing agent metal M. 3 It may consist of a mixture of powders including powder 30a.

[0091] Alternatively, the structure shown in Fig. 6 may also be preferred as a source module. Referring to Fig. 6, a source module 300b is similar to the above-mentioned example in that it is a multi-layer structure, but includes a core layer 310b containing a metal oxide 10b and a shell layer 320b coated on the outer surface of the core layer 310b. The shell layer 320b is made of a metal M. 2 20b and the metal M 3 The difference is that it is a coating layer containing an alloy phase 330b of 30b.

[0092] The solid source module may further include an anti-oxidation layer (330 in FIG. 4) that covers the shell layer and prevents the metal contained in the core layer and / or the shell layer from contacting with oxygen to prevent oxidation. The anti-oxidation layer 330 may include at least one selected from the group consisting of LiF, MgF2, CaF2, BaF2, CaCl2, MgCl2, MgO, CaO, BaO, Al2O3, and SiO2, but the scope of the present invention is not limited thereto. Although the anti-oxidation layer is only illustrated in FIG. 4, it is obvious that it can be applied to FIG. 5 and FIG. 6 according to other embodiments.

[0093] Such a solid source module is configured to descend vertically from within the electrolytic cell through the electrolyte until it reaches the liquid metal crucible, and can descend at a rate of 0.1% to 10% of the distance per minute of the electrolytic cell depth.

[0094] When the solid raw material module is set to have a descending direction as a virtual axis, it may be preferable to rotate the solid raw material module around the virtual axis in terms of stirring the liquid metal crucible and thereby improving the reactivity. The rotation may be performed while the solid raw material module is being lowered after being introduced into the electrolytic cell and / or after the module has completed its descent and is no longer being lowered.

[0095] Therefore, the system according to the present invention may further include a rotation unit to which the solid source module is attached and which rotates the solid source module.

[0096] Meanwhile, the solid source module is lowered to the liquid metal crucible and melted, and simultaneously or partially melted with the metal oxide and the reducing agent metal M 3 reacts to form metal oxide M 1 is reduced, and the reduced M 1 is the M contained in the solid source module 2 and forms a liquid metal alloy.

[0097] In one example, M 1 is Ti, metal oxide (M 1x O z ) is TiO2, M 2 Ni, M 3 When Mg is used, Ti metal is reduced according to the following reaction formula 1-1 and reaction formula 1-2, and then liquid metal alloy TiNi is obtained while M 3 Oxide (M 3 a O b ) can be separated.

[0098] (Reaction Scheme 1-1) 2Mg+TiO2 → Ti+2MgO

[0099] (Reaction Scheme 1-2) Ti+Ni+2MgO→TiNi(alloy)+2MgO(separated)

[0100] In yet another example, M 1 is Ti, metal oxide (M 1 x M 3 y O z ) is MgTiO3, M 2 Ni, M 3 When Mg is used, Ti metal is reduced according to the following reaction formula 2-1 and reaction formula 2-2, and then liquid metal alloy TiNi is obtained while M 3 Oxide (M 3 a O b ) can be separated.

[0101] (Reaction Scheme 2-1) 2Mg+MgTiO3→Ti+3MgO

[0102] (Reaction Scheme 2-2) Ti+Ni+3MgO→TiNi(alloy)+3MgO(separated)

[0103] The M produced by the above reaction 3 a O b may have a relatively low specific gravity as a by-product compared to the electrolyte of the present invention. 3 a Ob Due to the density difference with the electrolyte, the by-product M can float on the electrolyte and form a by-product layer. 3 a O b The by-product layer forms a layer below the electrolyte and is not mixed with the liquid metal crucible and the liquid metal alloy formed. In addition, this by-product layer is located on top of the electrolyte and prevents the electrolyte from evaporating and flowing away, and can prevent oxygen from the atmosphere from penetrating into the reactor.

[0104] Meanwhile, since the by-products rise to the top of the electrolytic bath as liquid metal alloy is produced, in order to continuously carry out processes in an electrolytic bath with a limited volume, the by-products must be continuously removed from the electrolytic bath. In this regard, the system according to the present invention may be configured to enable continuous processes by utilizing such by-products. Specifically, the system according to the present invention continuously collects the by-products that have risen to the top of the electrolyte and formed a layer through the upper part of the electrolytic bath, and performs, for example, M 1 x O z and mixed with metal oxide M 1 x M 3 y O z The recycling device may further include a recycling device for producing the M 1 x M 3 y O z When using M 1 x O z The reduction reaction rate can be further improved as compared with the case where

[0105] The electrolyte is a liquid metal crucible and a by-product, M 3 a O b It is preferable that the specific gravity of the by-product M 3 a O bThe electrolyte is preferably insoluble in the liquid metal crucible and the desired metal M. 1 Preferably, the liquid metal alloy containing the metal oxide can be prevented from being permeated by oxygen, but does not pose environmental problems, for example, is not a chlorine-based material.

[0106] Such electrolytes may include molten salts of halides of one or more metals selected from the group consisting of alkali metals and alkaline earth metals, but not chlorides. More specifically, in the system of the present invention, the electrolyte may be a molten salt of halides of one or more metals selected from the group consisting of alkali metals including Li, Na, K, Rb, and Cs, and alkaline earth metals including Mg, Ca, Sr, and Ba. In this case, the halides may include fluorides, bromides, iodides, or mixtures thereof.

[0107] In the system of the present invention, the electrolyte is also a metal oxide involved in the overall reduction reaction, i.e., a target metal M 1 % to 50% by weight, specifically 10% to 20% by weight, more specifically 10% to 15% by weight, and even more specifically 12% to 13% by weight, based on the metal oxide that can be reduced to the metal oxide.

[0108] The electrolyte may further include an oxide of one or more metals selected from the group consisting of alkali metals and alkaline earth metals as an additive. The content of the additive may be 0.1 to 25 wt % based on the total weight of the electrolyte. The additive may include, but is not limited to, Li2O, Na2O, SrO, Cs2O, KO, CaO, BaO, or a mixture thereof. The additive contained in the electrolyte may enable easier reduction of the metal oxide contained in the raw material module.

[0109] The system according to the present invention is configured to perform M 1 and M. 2 The liquid metal alloy formed by the above is continuously obtained and recovered, and is then electrolytically refined to produce metal M.1 The apparatus may further include an electrolytic refining unit for obtaining the above-mentioned.

[0110] The electrolytic refining unit solidifies the obtained liquid metal alloy to obtain a solid phase metal alloy, and electrolytically refines the solid phase metal alloy to obtain a metal M 1 can be recovered.

[0111] In some cases, electrolytes that may remain in the liquid metal alloy may be removed before the solidified alloy is electrolytically refined, which may be achieved, for example, by heat treating the liquid metal alloy in a vacuum or inert gas atmosphere to induce the electrolyte to be distilled and removed. The distillation temperature (heat treatment temperature) is not particularly limited as long as it is a temperature equal to or higher than the melting point of the electrolyte used in the system of the present invention, and may be, for example, 780 to 1,000° C. In order to effectively prevent the liquid metal alloy from being re-oxidized, it may be advantageous to carry out the distillation under a vacuum atmosphere or an inert gas.

[0112] The electrolytic refining unit may include an electrolyte containing a molten salt in which a halide of one or more metals selected from an alkali metal and an alkaline earth metal group is dissolved, independently of the electrolyte used in the reduction reaction.

[0113] 2. Manufacturing method

[0114] The method according to the present invention comprises the steps of:

[0115] providing an electrolytic cell;

[0116] introducing a liquid electrolyte into the electrolytic cell;

[0117] In the electrolytic bath, metals M which form a eutectic phase with each other are added. 1 and metal M 2 a liquid metal crucible that has a relatively high specific gravity compared to the electrolyte and forms an unmixed layer under the electrolyte to be contained in the electrolytic cell;

[0118] The metal oxide and the metal M 2 , and a reducing agent metal M 3 moving a solid source module including the liquid metal crucible through the electrolyte until the liquid metal crucible is reached;

[0119] Metal M derived from the metal oxide of the solid source module 1 and M. 2 and obtaining a liquid metal alloy comprising:

[0120] In the step of moving the solid source module, when the solid source module reaches the liquid metal crucible, it is melted. At this time, the metal oxide and the reducing agent metal M 3 In response, M 1 is reduced, and the reduced M 1 and M. 2 may be continuously mixed into the liquid metal crucible while forming a liquid metal alloy.

[0121] In the method of the present invention, the target metal M 1 is not particularly limited, and specifically may be one selected from the group consisting of Ti, Zr, Hf, W, Fe, Ni, Zn, Co, Mn, Cr, Ta, Ga, Nb, Sn, Ag, La, Ce, Pr, Nd, Nb, Pm, Sm, Eu, Al, V, Mo, Gd, Tb, Dy, Ho, Er, Tm, Yb, Ac, Th, Pa, U, Np, Pu, Am, Cm, Bk, Cf, Es, Fm, Md, and No, more specifically may be one selected from the group consisting of Ti, Zr, W, Fe, Ni, Zn, Co, Mn, Cr, Ta, Er, and No, even more specifically may be one selected from the group consisting of Ti, Zr, W, Fe, Ni, Zn, Co, Mn, and Cr, and particularly specifically may be Ti, Zr, or W.

[0122] In the method of the present invention, the metal M 2 is metal M 1The metal is not particularly limited as long as it can form a liquid metal alloy through a eutectic reaction with the metal, and specifically, the metal may be one or more selected from Cu, Ni, Fe, Sn, Zn, Pb, Bi, Cd, and alloys thereof, and more specifically, the metal may be Cu, Ni, or an alloy thereof.

[0123] In the method of the present invention, the metal M 3 The metal oxide is M. 1 However, among such substances, one or more selected from Ca, Mg, Al, and alloys thereof may be preferable, more specifically Ca or Mg, and particularly specifically Mg.

[0124] In the method of the present invention, the metal oxide is 1 x O z and M. 1 x M 3 y O z wherein x, y are each a real number from 1 to 3, and z is a real number from 1 to 4.

[0125] To aid in understanding, non-limiting examples of the metal oxides can include one or a combination of two or more selected from the group consisting of ZrO2, TiO2, MgTiO3, HfO2, Nb2O5, Dy2O3, Tb4O7, WO3, Co3O4, MnO, Cr2O3, MgO, CaO, Al2O3, Ta2O5, Ga2O3, Pb3O4, SnO, NbO, and Ag2O.

[0126] The method of the present invention differs from the conventional Kroll process in that it uses metal oxides instead of metal chlorides as raw materials. 1However, in order to use it in the Kroll process, a pretreatment process is required to convert the metal oxides to chlorides. The pretreatment process itself increases the process cost. Furthermore, hydrochloric acid is used in the pretreatment process to convert the metal oxides to chlorides, but the strong acidity promotes corrosion of the manufacturing equipment and may generate toxic chlorine gas during the process, which may cause environmental problems. The method of the present invention does not require a pretreatment process to convert the metal oxides to chlorides, and therefore has the advantages of lower process cost and no environmental problems compared to the Kroll process.

[0127] The raw material module used in the method of the present invention contains metal oxide and reducing agent metal M 3 A core layer including a 2 As shown in FIG. 4, the core layer is coated on the first core and the outer shell surface of the first core, and the reducing agent metal M 3 In some cases, the core layer may be a multi-layer structure including a second core made of a metal oxide powder and a reducing agent metal M, as shown in FIG. 5 as yet another example of the present invention. 3 It may consist of a mixture of powders including powder.

[0128] Alternatively, a source module as shown in FIG. 6 may be used, which includes a core layer containing a metal oxide and a shell layer coated on the outer surface of the core layer, the shell layer being made of a metal M. 2 and the metal M 3 The coating layer may include an alloy phase of

[0129] The solid source module may further include an anti-oxidation layer covering the shell layer to prevent the metal contained in the core layer and / or the shell layer from contacting with oxygen to prevent oxidation. The anti-oxidation layer may include at least one selected from the group consisting of LiF, MgF2, CaF2, BaF2, CaCl2, MgCl2, MgO, CaO, BaO, Al2O3, and SiO2, but the scope of the present invention is not limited thereto.

[0130] The step of moving the solid source module may involve lowering the solid source module through the electrolyte at a speed of 0.1% to 10% of the distance / min of the depth of the electrolytic cell until the solid source module reaches the liquid metal crucible.

[0131] metal M 1 and M. 2 The step of obtaining an alloy containing metal oxide and reducing agent metal M when the solid source module reaches a liquid metal crucible and is melted is performed. 3 reacts to form metal oxide M 1 is reduced, and the reduced M 1 is the M contained in the solid source module 2 forming a liquid metallic alloy with the metal.

[0132] In one example, M 1 is Ti, metal oxide (M 1 x O z ) is TiO2, M 2 Ni, M 3 When Mg is used, Ti metal is reduced according to the following reaction formula 1-1 and reaction formula 1-2, and then liquid metal alloy TiNi is obtained while M 3 Oxide (M 3 a O b ) can be separated.

[0133] (Reaction Scheme 1-1) 2Mg+TiO2 → Ti+2MgO

[0134] (Reaction Scheme 1-2) Ti+Ni+2MgO→TiNi(alloy)+2MgO(separated)

[0135] In yet another example, M 1 is Ti, metal oxide (M 1 x M 3 y O z ) is MgTiO3, M 2 Ni, M 3 When Mg is used, Ti metal is reduced according to the following reaction formula 2-1 and reaction formula 2-2, and then liquid metal alloy TiNi is obtained while M 3 Oxide (M 3 a O b ) can be separated.

[0136] (Reaction Scheme 2-1) 2Mg+MgTiO3→Ti+3MgO

[0137] (Reaction Scheme 2-2) Ti+Ni+3MgO→TiNi(alloy)+3MgO(separated)

[0138] The M produced by the above reaction 3 a O b may have a relatively low specific gravity as a by-product compared to the electrolyte of the present invention. 3 a O b Due to the density difference with the electrolyte, the by-product M can float on the electrolyte and form a by-product layer. 3 a O b The by-product layer forms a layer below the electrolyte and is not mixed with the liquid metal crucible and the liquid metal alloy formed. In addition, this by-product layer is located on top of the electrolyte and prevents the electrolyte from evaporating and flowing away, and can prevent oxygen from the atmosphere from penetrating into the reactor.

[0139] Meanwhile, since the by-products rise to the top of the electrolytic bath as liquid metal alloy is produced, in order to continuously carry out processes in an electrolytic bath with a limited volume, the by-products must be continuously removed from the electrolytic bath. In this regard, the method according to the present invention can be configured to utilize such by-products. Specifically, the method according to the present invention removes the by-products, i.e., M, which have risen to the top of the electrolytic bath and formed a layer on the electrolyte. 3 a O b is continuously collected, and 3 a O b For example, M 1 x O z and mixing to obtain the by-product M 3 a O b and added M 1 x O z M is a metal oxide derived from 1 x M 3 y O z The method may further include the step of manufacturing the

[0140] The M obtained in this way 1 x M 3 y O z In some cases, using 1 x O z The reduction reaction rate can be further improved compared to when the M 1 x M 3 y O z may be carried out at a temperature of 1,000°C to 1,500°C, particularly 1,200°C to 1,400°C, more particularly 1,250°C to 1,350°C.

[0141] The electrolyte is not particularly limited as long as it is not a chlorine-based substance, and is preferably as defined in the above embodiment.

[0142] The method according to the invention comprises the step of: 1 and M. 2 The metal M obtained after the step of obtaining the alloy containing 1 and M. 2 Metal M is produced by electrolytic refining of an alloy containing 1 The method may further include the step of obtaining.

[0143] The electrolytic refining of metal M 1 The step of obtaining the metal M includes solidifying the obtained liquid metal alloy to obtain a solid phase alloy, and then electrolytically refining the solid phase alloy to obtain a metal M from the alloy. 1 The step may include recovering the

[0144] 3. Working Example

[0145] The following examples are provided to demonstrate the functions and effects of the present invention, but are merely provided as examples of the present invention and are not intended to define the scope of the invention.

[0146] <Example>

[0147] A system as shown in Figure 1 was used. The electrolyte MgF2 (0.2 kg)-BaF2 (1.5 kg) was weighed and placed in an electrolytic cell in a resistance heating furnace, and then heated to about 1,200°C to form an electrolyte layer.

[0148] Cu (20 g) and Ti (200 g) were weighed and placed in the electrolytic cell and melted to produce a liquid metal crucible that was positioned at the bottom of the cell and formed a layer below the cell.

[0149] As shown in FIG. 2, 630 g of MgTiO3 (average particle size 300 μm) was used as the metal oxide, and 100 g of metal M 3 The raw material module was manufactured by mixing 250 g of Mg powder as the raw material and placing it in a cylindrical copper container (250 g) and drying it. In addition, photographs of the raw material module that was actually manufactured are shown in Figures 7 and 8.

[0150] The manufactured raw material module was inserted into the electrolytic cell and vertically lowered at a speed of about 6 cm / min until it reached the layer of the liquid metal crucible, and the module was rotated for 10 minutes to stir the electrolyte and the liquid metal crucible, and the melting and reduction reaction of the raw material module was carried out for 2 hours, and the reaction product, CuTi liquid metal alloy, was collected through an outlet provided at the bottom of the electrolytic cell and solidified to finally obtain the CuTi alloy as shown in Figure 9. After the reaction was completed, the crucible was cooled at -10°C / min to prevent damage to the crucible.

[0151] <Experimental Example>

[0152] The alloy obtained in Example 1 was evaluated for its properties using the following methods.

[0153] - Recovery rate: 100-{(1st weight-2nd weight) / 2nd weight x 100%}

[0154] - Residual impurity content: The produced alloy was cut and the inside of the alloy was confirmed by energy dispersive spectroscopy.

[0155] - Oxygen Content: The oxygen content present in the alloy was measured using an ELTRA ONH2000.

[0156] [Table 1] * First weight: The total amount of CuTi liquid metal crucibles put into the initial electrolysis cell + the theoretical chemical reduction amount of Ti contained in the metal oxide **Second weight: total amount of CuTi obtained

[0157] From the results in Table 1, it can be seen that the alloys of the examples produced according to the present invention showed a high recovery rate far exceeding 90%, and contained an extremely small amount of oxygen, which is a cause of contamination. The results for such low oxygen content are clearly demonstrated in Figure 11.

[0158] In addition, the alloy produced in the example was cut, and the remaining impurity content was confirmed by using an energy dispersive spectrum inside the alloy, which is shown in Figure 10. From Figure 10, it can be seen that the alloy is composed only of the desired metals Ti and Cu, and that Mg, which was used as a reducing agent, is not present at all.

[0159] These experimental results suggest that the present invention can realize high purity alloys with very low oxygen content and without other impurities used in the process.

Claims

1. Metal oxide to metal M 1 A system for returning An electrolytic cell; The metal M is received from the bottom of the electrolytic cell and forms a eutectic phase with each other. 1 and Metal M 2 a liquid metal crucible containing a liquid metal alloy of a liquid electrolyte contained in the electrolytic cell while forming an unmixed layer on the liquid metal crucible; The metal oxide, the metal M 2 , and a reducing agent metal M 3 a solid source module including: The solid source module reaches the liquid metal crucible and melts while mixing the metal oxide and the reducing agent metal M 3 In response, M 1 is reduced, and the reduced M 1 and M. 2 is continuously mixed into the liquid metal crucible while forming a liquid metal alloy; M 1 is one selected from the group consisting of Ti, Zr, Hf, W, Fe, Ni, Zn, Co, Mn, Cr, Ta, Ga, Nb, Sn, Ag, La, Ce, Pr, Nd, Nb, Pm, Sm, Eu, Al, V, Mo, Gd, Tb, Dy, Ho, Er, Tm, Yb, Ac, Th, Pa, U, Np, Pu, Am, Cm, Bk, Cf, Es, Fm, Md, and No; M 2 is at least one selected from Cu, Ni, Fe, Sn, Zn, Pb, Bi, Cd, and alloys thereof; The system, wherein M 3 is one or more selected from Ca, Mg, Al, and alloys thereof.

2. The reduced M 1 and M. 2 The liquid metal alloy formed by the above is recovered and electrolytically refined to obtain metal M. 1 10. The system of claim 1, further comprising an electrorefining section for obtaining

3. The metal oxide is M 1 x O z and M. 1 x M 3 y O z The system of claim 1 , comprising at least one selected from the group consisting of: Here, x and y are each a real number from 1 to 3, and z is a real number from 1 to 4.

4. The solid source module includes the metal oxide and the reducing agent metal M 3 A core layer including a core material covering the core layer and a 2 and a shell layer comprised of:

5. The solid source module has a multi-layer structure including a core layer containing the metal oxide and a shell layer that covers and coats an outer surface of the core layer, The shell layer is made of the metal M 2 and the metal M 3 The system of claim 1 , comprising an alloy phase of

6. the solid source module is configured to descend vertically from within the electrolytic cell through an electrolyte until it reaches the liquid metal crucible; 10. The system of claim 1, wherein the system descends at a rate of between 0.1% and 10% of the distance per minute (min) relative to the depth of the electrolytic bath.

7. The solid source module is melted while the metal oxide and the reducing agent metal M 3 In response, M 1 When reducing the oxide M 3 a O b is generated, and the M 3 a O b The system of claim 1 , wherein the electrolyte has a relatively low specific gravity compared to the electrolyte. Here, a and b are real numbers from 1 to 3.

8. Said M 3 a O b The system of claim 7 , wherein the electrolyte is heated to a temperature of 100° C. and ... temperature of the electrolyte is increased to 150° C.

9. 9. The system according to claim 8, wherein the liquid metal alloy is continuously obtained through a lower portion of the electrolytic cell and the by-product layer is continuously collected through an upper portion of the electrolytic cell according to the progress of the process, thereby enabling a continuous process.

10. The by-product layer is collected and M 1 x O z Mix with M 1 x M 3 y O z 10. The system of claim 9, further comprising a recycling device for producing:

11. The system of claim 1 , wherein the reaction of the metal oxide with the reductant metal is carried out in an inert gas and / or in air.

12. The core layer is made of the metal oxide powder and the reducing agent metal M 3 5. The system of claim 4, comprising a mixture of powders including powder.

13. The core layer is a coating that covers the first core made of the metal oxide and the outer shell surface of the first core, and the metal M 3 5. The system of claim 4, which is a multi-layer structure including a second core consisting of:

14. 5. The system of claim 4, wherein the solid source module further comprises an anti-oxidation layer covering the shell layer to prevent oxidation of metals contained in the core layer and / or the shell layer.

15. The oxidation prevention layer is LiF, MgF 2 , CaF 2 , BaF 2 , CaCl 2 , MgCl 2 , MgO, CaO, BaO, Al 2 O 3 , and SiO 2 The system of claim 14, comprising one or more selected from the group consisting of:

16. 10. The system of claim 1, wherein the electrolyte comprises a molten salt of a halide of one or more metals selected from the group consisting of alkali metals and alkaline earth metals.

17. Metal oxide to metal M 1 A method for reducing providing an electrolytic cell; introducing a liquid electrolyte into the electrolytic cell; The electrolytic bath contains metals M that form a eutectic phase with each other. 1 and Metal M 2 a liquid metal crucible that has a relatively high specific gravity compared to the electrolyte and forms an unmixed layer under the electrolyte to be contained in the electrolytic cell; The metal oxide and the metal M 2 , and a reducing agent metal M 3 moving a solid source module including: The metal M derived from the metal oxide of the solid source module 1 and M. 2 obtaining a liquid metal alloy comprising: M 1 is one selected from the group consisting of Ti, Zr, Hf, W, Fe, Ni, Zn, Co, Mn, Cr, Ta, Ga, Nb, Sn, Ag, La, Ce, Pr, Nd, Nb, Pm, Sm, Eu, Al, V, Mo, Gd, Tb, Dy, Ho, Er, Tm, Yb, Ac, Th, Pa, U, Np, Pu, Am, Cm, Bk, Cf, Es, Fm, Md, and No; M 2 is at least one selected from Cu, Ni, Fe, Sn, Zn, Pb, Bi, Cd, and alloys thereof; The method, wherein M 3 is one or more selected from Ca, Mg, Al, and alloys thereof.

18. The obtained metal M 1 and M. 2 Metal alloy containing metal M is electrolytically refined. 1 The method of claim 17 , further comprising the step of obtaining:

19. In the step of moving the solid source module and / or the step of obtaining the liquid metal alloy, the by-product oxide M 3 a O b is generated, and the M 3 a O b has a relatively low specific gravity compared to the electrolyte, M forming a layer on the electrolyte 3 a O b is continuously collected, and 3 a O b To M 1 x O z and mixing to obtain the by-product M 3 a O b and added M 1 x O z M comes from 1 x M 3 y O z 20. The method of claim 17, further comprising the step of producing a metal oxide represented by

20. The weight of the reducing agent metal M 3 18. The method of claim 17, wherein the residual content is 0.1 wt. % or less and the oxygen content is 1,000 ppm or less.

Citation Information

Patent Citations

  • Utilize device of liquid alloy as pure titanium of electrode preparation

    CN207525356U

  • Method and apparatus for producing metal

    JP2005068539A

  • Method for producing titanium

    JP2014133939A

  • Porous sintered compact of titanium oxide for production of metallic titanium through direct electrolytic process and process for producing the same

    WO2004024995A1