Layered iron rust and iron hydroxide nanoparticles containing the same
Layered ferric iron hydroxide nanoparticles with a novel crystal structure address the inefficiencies of existing arsenic removal methods by utilizing organic anions to enhance adsorption, providing a sustainable and economical solution for arsenic immobilization in soil.
Patent Information
- Application Number
- JP2023071586
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-04-29
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-25
AI Technical Summary
Existing methods for removing arsenic from contaminated soil are inefficient and pose environmental and economic challenges due to the complexity of nanomaterial synthesis and toxicity issues, necessitating a simpler and more effective adsorption technique.
The development of layered ferric iron hydroxide nanoparticles with a novel crystal structure, achieved by intercalating organic anions between nanoplatelets, which provides a wide interlayer spacing for enhanced arsenic adsorption through chemisorption and electrostatic intercalation.
This approach significantly enhances arsenic adsorption capacity, offering a sustainable and economical solution for immobilizing arsenic in soil, improving the efficiency of arsenic removal and maintaining ecosystem health.
Smart Images

Figure 0007580826000013 
Figure 0007580826000014 
Figure 0007580826000015
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0053803 dated April 29, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated as part of this specification.
[0002] The present invention relates to layered ferric iron hydroxide and iron hydroxide nanoparticles containing the same, and more particularly to layered ferric iron hydroxide having a new crystal structure due to an anionic organic substance inserted between the layered structure of iron oxide / ferric hydroxide, and iron hydroxide nanoparticles containing the same. [Background technology]
[0003] Iron hydroxides are abundant clay minerals that make up 4% of the earth's crust and play important roles in maintaining biogeochemical cycles and ecosystems, attracting attention in various fields such as metallurgy, water purification, and energy conversion and storage. Naturally occurring iron hydroxides include ferrihydrite, polymorphs of ferric hydroxide (FeOOH) (goethite, akaganeite, lepidocrocite, feroxyhyte), and green rust (type 1, type 2).
[0004] In particular, to obtain ceramic pigments with vivid hues, it is important to synthesize nanopigments that allow adjustment of the pigment shape and size. In the case of iron hydroxide, it can be adjusted to various shapes from rod to spindle, and is classified according to shape into α-FeOOH (goethite), β-FeOOH (akaganeite), and γ-FeOOH (lepidocrocite).
[0005] Therefore, there is a demand for a production method of iron hydroxide for such various applications that can be produced through simpler processes, that allows control of the shape and size, and that can impart diversity to the surface area characteristics.
[0006] In addition, naturally occurring iron hydroxides can be used as precursors for the formation of relatively thermodynamically stable iron oxides and play an important role in the crystallization process of iron oxides. Therefore, the iron hydroxide material with the new crystal structure can provide important information on the overall crystallization process of iron oxides, in addition to its fundamental understanding and technological impact.
[0007] Arsenic is a harmful substance to humans, and was once used as an ingredient in poisons. However, arsenic is more commonly found in our surroundings than we might think. Arsenic is not only produced by human activities such as mining and smelting, but can also be found naturally.
[0008] However, chronic exposure to arsenic can cause serious health problems, leading to the classification of inorganic arsenic as a carcinogen. Therefore, arsenic (As)-contaminated soils are inevitably present in natural systems and are known to be one of the global challenges for a sustainable future.
[0009] Therefore, although there have been attempts to remove arsenic using nanomaterials with increased adsorption capacity and affinity, there are problems with the use of nanomaterials in the soil ecosystem due to a combination of factors, including the large-scale synthesis of nanomaterials, toxicity of the soil environment, and environmental issues.
[0010] Specifically, the mechanical strength and arsenic adsorption efficiency are achieved through an adsorbent manufactured through a process of mixing iron oxide, iron oxyhydroxide, or a mixture thereof, which are known to be arsenic adsorbing materials, with a cation-selective binder resin.
[0011] Despite these conventional techniques, purification techniques are still ineffective against arsenic contamination, and there is a demand for an effective removal technique for arsenic contamination. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Republic of Korea Patent No. 10-1771005, "Method of manufacturing iron hydroxide powder" [Patent Document 2] Republic of Korea Patent Publication No. 10-2019-0085902, "Method for manufacturing hollow fiber-type arsenic adsorbent" Summary of the Invention [Problem to be solved by the invention]
[0013] One embodiment of the present invention provides layered ferric iron hydroxide, which is a new crystal structure having a relatively wide layer spacing relative to the size of the nanoparticles, by inserting an organic anion between the layers of the nanoplatelets, and iron hydroxide nanoparticles containing the same.
[0014] One embodiment of the present invention provides a layered ferric iron hydroxide in which an organic anion distorts the arrangement of FeO6 octahedra contained in the nanoplatelets and forms a stacked structure of the nanoplatelets, and an iron hydroxide nanoparticle comprising the same.
[0015] According to an embodiment of the present invention, there is provided iron hydroxide nanoparticles having a layered ferric iron hydroxide crystal structure in which the solvent molecules are involved in a dehydration process during a chemical reaction from ferrihydrite, which is a metastable phase, to magnetite, which is a stable phase, by adjusting the amount of a solvent together with an organic anion during the preparation of the iron hydroxide nanoparticles, thereby forming a layered structure of nanoplatelets, and a method for preparing the same.
[0016] One embodiment of the present invention provides an arsenic adsorbent comprising organic-inorganic composite iron hydroxide nanoparticles that can immobilize arsenic using iron hydroxide, a clay mineral that is abundant on Earth, and a method for producing the same, which is environmentally friendly and economical.
[0017] An embodiment of the present invention provides an arsenic adsorbent that can fix arsenic through a primary mechanism of adsorbing arsenic by chemical adsorption via the surface of nanoplatelets, and a secondary adsorption mechanism of inserting / fixing arsenic by electrostatic layer-by-layer insertion via layer spacing formed by organic ligands inserted between layers of nanoplatelets, and a method for manufacturing the same.
[0018] One embodiment of the present invention provides an arsenic adsorbent that can produce organic-inorganic composite iron hydroxide nanoparticles containing organic ligands intercalated between layers of nanoplatelets through colloidal assembly of nano-level building blocks through a particle-directed attachment process, and a method for producing the same. [Means for solving the problem]
[0019] Layered ferric rust according to one embodiment of the present invention has a novel crystal structure that satisfies the following conditions (a) to (c). (a) the crystal system is monoclinic; (b) the space group is Pn (No. 7); (c) the unit cell parameters are a = 3.854 ± 0.002 Å, b = 11.491 ± 0.007 Å, c = 9.818 ± 0.004 Å, and β = 88.47 ± 0.005° (where b is the distance between layers in the
[0010] axial direction).
[0020] The atomic coordinates and equivalent isotropic displacement parameters of the elements in the lattice of the layered ferric rust can satisfy Table 1 below.
[0021] [Table 1]
[0022] The layered ferric rust may be represented by the following Chemical Formula 1.
[0023] FeO x C y H z (chemical formula 1) (In the above Chemical Formula 1, x is a number between 3 and 3.5 (3≦x≦3.5), y is a number between 0.67 and 1 (0.67≦y≦1), and z is a number between 1.94 and 3.5 (1.94≦z≦3.5).)
[0024] The layered ferric rust includes at least two layers of nanoplatelets each including at least one FeO6 octahedral structure; and an organic anion inserted between the at least two layers of nanoplatelets, and the at least two layers of nanoplatelets may have a distance between the layers determined by the organic anion.
[0025] The nanoplatelets and the organic anions may be linked by bidentate bridging.
[0026] The nanoplatelets may include zigzag corner sharing and edge sharing between adjacent FeO6 octahedral structures due to the organic anions.
[0027] The number of nanoplatelets in the at least two layers may be 2 to 16.
[0028] The nanoplatelets can include FeOOH (Iron(III) oxide-hydroxide).
[0029] The organic anion is acetate (CH3COO - ) type compounds.
[0030] The iron hydroxide nanoparticles according to one embodiment of the present invention include layered ferric rust according to one embodiment of the present invention.
[0031] The iron hydroxide nanoparticles may be included in at least one of a pollutant adsorbent, a battery catalyst, an OER (oxygen evolution reaction) catalyst, a thermotherapy material, a bioplastic, a construction material, a pigment, and a dye.
[0032] An arsenic adsorbent according to one embodiment of the present invention comprises organic-inorganic composite iron hydroxide nanoparticles, the organic-inorganic composite iron hydroxide nanoparticles comprising at least two or more layers of nanoplatelets each having at least one FeO6 octahedral structure; and an organic ligand intercalated between the at least two or more layers of nanoplatelets. The organic-inorganic composite iron hydroxide nanoparticles adsorb arsenic by chemisorption through the surfaces of the nanoplatelets and electrostatic intercalation through the layer-like spaces between the nanoplatelets.
[0033] The layer spacing of the at least two layers of nanoplatelets may be 1.14 nm to 1.19 nm.
[0034] The nanoplatelets and the organic ligands may be linked by bidentate bridging.
[0035] The nanoplatelets may have adjacent FeO6 octahedral structures that are corner-shared and edge-shared in a zigzag manner by the organic ligands.
[0036] The number of nanoplatelets in the at least two layers may be 2 to 16.
[0037] The nanoplatelets can include FeOOH (Iron(III) oxide-hydroxide).
[0038] The organic ligand is acetate (CH3COO - ) type compounds.
[0039] The arsenic may be contained in soil. Effect of the Invention
[0040] According to one embodiment of the present invention, it is possible to provide layered ferric iron hydroxide, which is a new crystal structure having a relatively wide layer spacing compared to the size of the nanoparticles, by inserting an organic anion between the layers of the nanoplatelets, and iron hydroxide nanoparticles including the same.
[0041] According to one embodiment of the present invention, a layered ferric iron hydroxide in which an organic anion distorts the arrangement of FeO6 octahedra contained in the nanoplatelets and forms a stacked structure of the nanoplatelets, and an iron hydroxide nanoparticle including the same can be provided.
[0042] According to an embodiment of the present invention, by adjusting the amount of solvent together with the organic anion during the preparation of iron hydroxide nanoparticles, it is possible to provide iron hydroxide nanoparticles having a layered ferric iron hydroxide crystal structure in which the solvent molecules are involved in a dehydration process during a chemical reaction from ferrihydrite, which is a metastable phase, to magnetite, which is a stable phase, to form a layered structure of nanoplatelets, and a method for preparing the same.
[0043] According to one embodiment of the present invention, it is possible to provide an arsenic adsorbent comprising environmentally friendly and economical organic-inorganic composite iron hydroxide nanoparticles that can immobilize arsenic using iron hydroxide, a clay mineral that is abundant on Earth, and a method for producing the same.
[0044] According to an embodiment of the present invention, there is provided an arsenic adsorbent that can fix arsenic through a primary mechanism of adsorbing arsenic by chemical adsorption via the surface of nanoplatelets and a secondary adsorption mechanism of inserting / fixing arsenic by electrostatic layer-by-layer insertion via layer spaces formed by organic ligands inserted between layers of nanoplatelets, and a method for manufacturing the same.
[0045] According to one embodiment of the present invention, an arsenic adsorbent can be provided that can produce organic-inorganic composite iron hydroxide nanoparticles containing organic ligands intercalated between layers of nanoplatelets through colloidal assembly of nano-unit building blocks through a particle-directed attachment process, and a method for producing the same. [Brief description of the drawings]
[0046] [Figure 1A] FIG. 1 is a schematic diagram showing the crystal structures of layered ferric rust (LFR), which is a new crystal structure of iron hydroxide, according to one embodiment of the present invention, and conventional iron hydroxide. [Figure 1B]FIG. 1 is a schematic diagram showing the crystal structures of layered ferric rust (LFR), which is a new crystal structure of iron hydroxide according to an embodiment of the present invention, and conventional iron hydroxide. [Diagram 2] FIG. 1 is a schematic diagram showing layered ferric rust according to one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram illustrating an example of nanoplatelets and organic anions contained in layered ferric rust according to an embodiment of the present invention. [Figure 4] FIG. 1 is a schematic diagram showing a bonding structure of nanoplatelets and organic anions contained in layered ferric rust according to one embodiment of the present invention. [Diagram 5] FIG. 1 is a bright-field transmission electron microscope image of layered ferric rust according to Example 1 of the present invention. [Figure 6] FIG. 2 is a diagram showing a scanning transmission electron microscopy image of layered ferric rust according to Example 1 of the present invention measured at a low voltage (80 kV). [Figure 7] FIG. 1 is a diagram showing a selected area electron diffraction analysis image of layered ferric rust according to Example 1 of the present invention. [Figure 8] 1 is an intensity profile showing the layer spacing of layered ferric rust according to Example 1 of the present invention. [Figure 9] 1 is a graph showing the surface characteristics of layered ferric rust according to Example 1 of the present invention. [Figure 10]1 is a graph showing an analysis of the components of layered ferric rust according to Example 1 of the present invention. [Figure 11] 1 is a graph showing an analysis of the components of layered ferric rust according to Example 1 of the present invention. [Figure 12] 1 is a graph showing an analysis of the components of layered ferric rust according to Example 1 of the present invention. [Figure 13] 1 is a graph showing an analysis of the components of layered ferric rust according to Example 1 of the present invention. [Figure 14] 1 is a graph showing an analysis of the components of layered ferric rust according to Example 1 of the present invention. [Figure 15] FIG. 1 is a diagram showing a Fourier transform infrared spectrum in which the coordination of acetate in layered ferric rust according to Example 1 of the present invention was measured. [Figure 16] FIG. 1 is a diagram showing Raman analysis spectra of layered ferric rust and ferric hydroxide polymorphs according to Example 1 of the present invention. [Figure 17] FIG. 1 shows a Rietveld analysis of a synchrotron high-resolution powder neutron diffraction analysis for analyzing the crystal structure of layered ferric rust according to Example 1 of the present invention, and a photograph of the crystal structure of LFR. [Figure 18] 1 is a graph showing the results of Rietveld analysis of synchrotron high-resolution powder neutron diffraction analysis of layered ferric rust according to Example 1 of the present invention compared with an existing crystal structure. [Figure 19A] 1 is a flowchart showing a method for producing layered ferric rust according to an embodiment of the present invention. [Figure 19B]FIG. 1 is a schematic diagram showing the formation process of the crystal structure of LFR. [Figure 20] 1 is a transmission electron microscope image of a powder containing a high concentration of layered ferric rust according to an embodiment of the present invention on a glass substrate. [Figure 21] 1 is a transmission electron microscope image obtained by measuring a powder containing a medium concentration of layered ferric rust according to an embodiment of the present invention on a glass substrate. [Figure 22] 1 is a transmission electron microscope image obtained by measuring a powder containing a low concentration of layered ferric rust according to an embodiment of the present invention on a glass substrate. [Figure 23] 1 is a graph showing a Gaussian distribution of the average length of the width and thickness in the lamination direction of layered ferric rust according to an embodiment of the present invention, measured for n=200 particles obtained through a transmission electron microscope. [Figure 24] 1 is a graph showing growth kinetics of layered ferric rust according to an embodiment of the present invention in the lateral and axial directions. [Diagram 25] FIG. 1 is a schematic diagram showing the growth mode observed by a scanning transmission electron microscope. [Figure 26] FIG. 1 is a schematic diagram of the lateral and axial alignment observed by scanning transmission electron microscopy. [Figure 27] 1 is a graph showing in situ thermal XRD patterns for a powder including layered ferric rust according to an embodiment of the present invention in air (oxidizing), Ar+H2 (reducing), and Ar (inert) atmospheres. [Figure 28] 28 is a graph showing a phase change diagram for FIG. 27. [Figure 29] FIG. 1 shows a transmission electron microscopy image and a selected area electron diffraction pattern showing a change over time (reaction time) of a second heat treatment step of layered ferric rust according to an embodiment of the present invention. [Diagram 30] FIG. 2 shows transmission electron microscope (TEM) images of layered ferric rust according to an embodiment of the present invention depending on the content of a solvent (H2O). [Diagram 31] FIG. 2 is a diagram showing a powder X-ray diffraction (XRPD) graph of layered ferric rust according to an embodiment of the present invention according to the content of a solvent (H2O). [Diagram 32] 1 is a graph showing a ratio of a phase that changes from magnetite to layered ferric rust according to an embodiment of the present invention depending on the content of a solvent (H2O). [Diagram 33] FIG. 1 is a schematic diagram illustrating an arsenic adsorbent according to one embodiment of the present invention. [Diagram 34] FIG. 1 is a schematic diagram showing the adsorption mechanism of arsenic in soil (As in soil) using an arsenic adsorbent according to one embodiment of the present invention. [Diagram 35] FIG. 1 is a schematic diagram illustrating a method for producing an arsenic adsorbent according to one embodiment of the present invention. [Diagram 36] FIG. 1 is a schematic diagram illustrating a method for producing an arsenic adsorbent according to an embodiment of the present invention. [Figure 37] 1 is an image showing a manufacturing process of an arsenic adsorbent according to Example 2 of the present invention. [Figure 38] 4 is a scanning electron microscopy (SEM) and a transmission electron microscopy (TEM) image showing a hierarchical structure of an arsenic adsorbent according to Example 2 of the present invention. [Figure 39] 1 is an image showing a selected area electron diffraction (SAED) pattern of an arsenic adsorbent according to Example 2 of the present invention, and a graph showing a result of powder X-ray diffraction (XRPD). [Diagram 40] FIG. 1 is a schematic diagram showing the arsenic (As) adsorption mechanism. [Diagram 41] 1 is a graph showing the results of inductively coupled plasma mass spectrometry (ICP-MS) illustrating the adsorption capacity of the arsenic adsorbent according to Comparative Example 1 and the arsenic adsorbent according to Example 2 of the present invention. [Diagram 42] 1 is a graph showing electrokinetic potential before and after arsenic adsorption. [Diagram 43] 1 is a graph showing the results of X-ray Photoelectron Spectroscopy (XPS) of the arsenic adsorbent according to Comparative Example 1 before arsenic adsorption. [Diagram 44] 1 is a graph showing the results of X-ray photoelectron spectroscopy of the arsenic adsorbent according to Comparative Example 1 after arsenic adsorption. [Diagram 45] 1 is a graph showing the results of X-ray photoelectron spectroscopy of the arsenic adsorbent according to Example 2 of the present invention before arsenic adsorption. [Diagram 46] 1 is a graph showing the results of X-ray photoelectron spectroscopy of the arsenic adsorbent according to Example 2 of the present invention after arsenic adsorption. [Figure 47] 1 is a graph showing the results of Fourier Transform Infrared Spectroscopy (FT-IR) of the arsenic adsorbent according to Example 2 of the present invention before and after arsenic adsorption. [Figure 48] 1 is a graph showing the results of Fourier transform infrared spectroscopy of the arsenic adsorbent according to Comparative Example 1 before and after arsenic adsorption. [Figure 49] 1 is a graph showing the results of a bioassay of A. kimi in artificial soil in the absence of arsenic. [Figure 50]1 is a graph showing the results of a bioassay of B. juncea in artificial soil that was not treated with arsenic. [Figure 51] This is a graph showing the results of a bioassay of A. kimi in artificial soil treated with arsenic (circles are adults, bars are larvae). [Figure 52] 1 is a graph showing the content of each arsenic in arsenic-treated artificial soil. [Figure 53] FIG. 1 shows an image of A. kimi in arsenic-treated artificial soil. [Figure 54] 1 is a graph showing B. juncea in artificial soil. [Figure 55] 1 is a graph showing the arsenic content of B. juncea in artificial soil. [Figure 56] 1 is a graph showing an image of B. juncea in artificial soil. [Figure 57] 1 is a graph showing the number of surviving A. kimi adults (circles) and larvae (bars) after 28 days of exposure to As-contaminated mine soil. [Figure 58] 1 is a graph showing the mean As concentration (mg / kg) of surviving adults after exposure to arsenic. [Figure 59] 1 is an image of a larval specimen produced after exposure to arsenic. [Figure 60] 1 is a graph showing the weight (g) of root and shoot of B. juncea after exposure to arsenic. [Figure 61] 1 is a graph showing the average As concentration (mg / kg) of B. juncea after exposure to arsenic. [Figure 62] The growth images of B. juncea after exposure to arsenic. [Figure 63] 1 is an image showing the morphological characteristics of the arsenic adsorbent according to Example 2 of the present invention in artificial soil (a) and arsenic-contaminated soil (b). [Figure 64]FIG. 1 is a graph showing Olsen extraction results for arsenic-contaminated artificial soil (a) and arsenic-contaminated mine soil (b) treated with the arsenic adsorbent according to Comparative Example 1 (Gt), Comparative Example 2 (Control), and the arsenic adsorbent according to Example 2 of the present invention (r-FAN). [Figure 65] 1 is a graph showing the average percentage of arsenic by form in artificial soils. [Figure 66] 1 is a graph showing the average percentage of arsenic by form in actual mine soils. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0047] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings and the contents described in the accompanying drawings. However, the present invention is not limited or restricted by the embodiments.
[0048] The terms used in the present specification are for the purpose of describing the embodiments and are not intended to limit the present invention. In the present specification, the singular form includes the plural form unless otherwise specified in the phrase. The words "comprises" and / or "comprising" used in the specification do not exclude the presence or addition of one or more other components or steps other than the components or steps mentioned.
[0049] As used herein, words such as "embodiment," "example," "aspect," "exemplary," and "illustrative" are not meant to construe any described aspect or design as better or advantageous over other aspects or designs.
[0050] Additionally, the term "or" refers to the inclusive or rather than the exclusive or. That is, unless otherwise specified or clear from the context, the phrase "x uses a or b" refers to any one of the natural inclusive permutations.
[0051] Additionally, the singular terms "a" or "an" as used in the specification and claims should generally be construed to mean "one or more" unless otherwise noted or unless it is clear from the context that the singular form is intended.
[0052] The terms used in the following description are selected to be common and universal in the relevant technical field, but other terms may exist depending on the development and / or change of technology, customs, preferences of engineers, etc. Therefore, the terms used in the following description should not be understood as limiting the technical idea, but should be understood as exemplary terms for describing the embodiments.
[0053] In addition, in certain cases, the applicant may arbitrarily select certain terms, and in such cases, the meanings of those terms will be described in detail in the relevant description. Therefore, the terms used in the following description should be understood based on the meanings of those terms and the contents of the entire specification, rather than simply the names of those terms.
[0054] Unless otherwise defined, all terms (including technical and scientific terms) used herein may be used as commonly understood by those having ordinary skill in the art to which the present invention belongs. Furthermore, terms defined in commonly used dictionaries are not to be interpreted ideally or excessively unless clearly defined otherwise.
[0055] Meanwhile, in describing the present invention, if a detailed description of related known functions or configurations is deemed to unnecessarily obscure the gist of the present invention, the detailed description will be omitted. Furthermore, the terminology used in this specification is used to appropriately express the embodiments of the present invention, and may vary depending on the intention of the user or operator, or the practice of the field to which the present invention belongs. Therefore, the definition of the terminology should be based on the contents of this specification as a whole.
[0056] Hydroxides are primarily formed through a particle-directed deposition process and grow via the colloidal assembly of nano-scale building blocks. The particle-directed deposition process is known to be a new growth model related to the formation of anisotropic and organic-composite structures.
[0057] 1A and 1B are schematic diagrams showing the crystal structures of layered ferric rust (LFR), which is a new crystal structure of iron hydroxide according to one embodiment of the present invention, and conventional iron hydroxide.
[0058] Layered ferric rust according to one embodiment of the present invention is a material with a new crystal structure in which acetate is inserted between layers of ferric hydroxide, with the spacing being relatively wide compared to the particle size. Acetate, an organic anion, distorts the arrangement of FeO6 octahedra and creates layered stacks of hydroxide, thereby forming a layered ferric rust (LFR) structure.
[0059] Excess water molecules that enter into the hydroxide synthesis also participate in the dehydration process in the chemical reaction that transforms the metastable phase ferrihydrite into the stable phase magnetite, and together with acetate, can play a crucial role in the formation of a new crystal structure.
[0060] Layered ferric rust according to one embodiment of the present invention has a new crystal structure that is completely different from currently known layered structures of ferric hydroxide such as lepidocrocite and green rust.
[0061] Layered ferric rust according to an embodiment of the present invention has a novel crystal structure that satisfies the following conditions (a) to (c). (a) the crystal system is monoclinic, (b) the space group is Pn (No. 7), and (c) the unit cell parameters are a = 3.854 ± 0.002 Å, b = 11.491 ± 0.007 Å, c = 9.818 ± 0.004 Å, and β = 88.47 ± 0.005° (where b is the distance between layers in the
[0010] axial direction).
[0062] a means one side of a unit cell in the
[0100] axial direction, c means one side of a unit cell in the
[0001] axial direction, and β means the angle between the ac plane and the b axis.
[0063] A substance having one or more crystal structures is called polymorphism, and the crystal structure is an internal structure of six types of crystal systems, which changes the properties of the substance. The layered ferric rust according to one embodiment of the present invention has a new crystal structure different from the crystal structure of existing FeOOH polymorphs through synchrotron HRPD and Raman analysis, and preferably, the layered ferric rust according to one embodiment of the present invention has a monoclinic crystal system, a space group Pn(No.7), and unit cell parameters a=3.854(2)Å, b=11.491(7)Å, c=9.818(4)Å, and β=88.47(5)° (where b is the distance between layers in the 0010 axis direction).
[0064] More specifically, the crystallographic data of the layered ferric rust according to one embodiment of the present invention is as shown in Table 2 below.
[0065] [Table 2]
[0066] In Table 2, volume means the volume of a unit cell, Z means the proton number, formula weight means the sum of the atomic weights of the elements included in the (chemical formula) composition formula, density means the value obtained through weight / volume-TGA measurement, temperature means the measurement temperature of synchrotron high-resolution powder neutron diffraction analysis, and wavelength means the wavelength of the X-ray used in synchrotron high-resolution powder neutron diffraction analysis.
[0067] XRD is measured by scanning the diffraction angle (2θ) while the X-ray source and detector move along the circumference. At this time, the 2θ range means the range to be scanned, the step scan increment means the increase in the incident angle, and the R-factor is a reliable factor for the refinement result, and is the difference between the calculated value and the measured value expressed as a percentage, indicating the reliability of the calculated value.
[0068] R p can be calculated by the following formula 1, R wp can be calculated using the following formula 2, R exp can be calculated using the following formula 3, R bragg can be calculated using Equation 4 below.
[0069]
number
number
number
number
[0070] When measuring the electron density of a sample with XRD, the electron density is not spherical but distorted in three dimensions due to the atomic bonds and arrangement. In powder XRD, the electron density is assumed to be spherical and the extent to which it spreads from the original is calculated, where B is the thermal factor and eq is a variable that assumes a spherical shape.
[0071] GOF is the good of fitness, a reduced chi-square test that tests whether the observed ratio values are the same as the expected values.
[0072] Table 2 shows the crystallographic data of LFR obtained from synchrotron high-resolution powder neutron diffraction analysis, including the crystal system, space group, unit cell side lengths, angles, volume, molecular weight, density, and information used in the analysis, and indicates the reliability of the analysis.
[0073] The atomic coordinates and equivalent isotropic displacement parameters of elements in the lattice of the layered ferric rust according to the embodiment of the present invention may satisfy Table 3 below.
[0074] [Table 3]
[0075] In Table 1, x, y, and z represent the coordinates of each atom within the unit cell, Occ. represents the site occupancy, which is the fraction of the atom present at the atomic site within the unit cell (e.g., the presence of 1 atom means 1), and the numbers in parentheses in Table 1 represent the standard deviation of the result, and 0.4096(19) can mean 0.4096±0.019.
[0076] Also, B eqWhen measuring electron density by XRD, the thermal factor is calculated for each three-dimensional direction. In reality, atoms are not spherical but have a distorted shape due to bonds and arrangements. However, this is the calculated thermal factor (thermal factor B) assuming that the atoms are spherical (eq).
[0077] Also, Occ. is the occupancy (fraction), which is a value that indicates the degree to which atoms occupy a unit cell when one oxygen atom is assumed to be 1.
[0078] Table 1 shows the coordinates in three-dimensional space of all the atoms in the unit cell.
[0079] Layered ferric rust according to an embodiment of the present invention may be represented by the following Chemical Formula 1.
[0080] FeO x C y H z (chemical formula 1) (In the above Chemical Formula 1, x is a number between 3 and 3.5 (3≦x≦3.5), y is a number between 0.67 and 1 (0.67≦y≦1), and z is a number between 1.94 and 3.5 (1.94≦z≦3.5).)
[0081] For example, layered ferric rust according to one embodiment of the present invention is FeO 3.5 CH 3.5 Or it may be Fe2O4H2·(CH3COO)·H2O.
[0082] Layered ferric rust according to embodiments of the present invention can be synthesized by a particle-directed deposition process and can have a novel crystal structure with organic anions intercalated between at least two layers of nanoplatelets (e.g., ferric hydroxide).
[0083] In particular, the organic anion molecules grafted onto the building blocks (at least two layers of nanoplatelets) are closely related to the intermolecular interactions during the assembly process, so that by adjusting the organic anion (e.g., acetate), which is an organic molecule, the crystal structure of the hydroxide (e.g., ferric hydroxide) can be adjusted in various ranges from atomic units to micrometers.
[0084] For example, γ-FeOOH and green rust (GR-2) can have boehmite arranged in a zigzag arrangement along the ac plane, and brucite with a planar FeO3(OH)3 arrangement along the ab plane, respectively.
[0085] However, in the layered ferric rust according to one embodiment of the present invention, the FeO6 octahedral structure is connected in the a-axis direction by edge sharing through the organic anions, and in the c-axis direction, the edge sharing is broken by the organic anions 121, and corner sharing occurs, resulting in a completely different crystal structure.
[0086] Hereinafter, layered ferric rust according to one embodiment of the present invention will be described in more detail with reference to FIG.
[0087] FIG. 2 is a schematic diagram showing layered ferric rust according to one embodiment of the present invention, and FIG. 3 is a schematic diagram showing examples of nanoplatelets and organic anions contained in layered ferric rust according to one embodiment of the present invention.
[0088] Layered ferric rust according to one embodiment of the present invention includes at least two or more layers of nanoplatelets 110 each including at least one FeO6 octahedral structure 111, and organic anions 121 intercalated between the at least two or more layers of nanoplatelets 110, and the at least two or more layers of nanoplatelets 110 have a layer spacing 120 that is the distance between the layers separated by the organic anions 121.
[0089] Therefore, in the layered ferric rust according to the embodiment of the present invention, the organic anion 121 is inserted between the layers of the nanoplatelets 110, and the layer spacing 120 can be relatively wide compared to the size of the nanoparticles.
[0090] Since it has a different crystal structure from other FeOOH (Green Rust, Lepidocrocite) materials with existing layered structures, a new pathway and intermediate phase for forming Fe3O4 have been discovered, making it possible to adsorb and remove pollutants using the wide layer spacing 120, and it can be used as a battery catalyst.
[0091] The nanoplatelets 110 and the organic anions 121 can be connected by bidentate bridging. Thus, the nanoplatelets 110 can have a zigzag structure due to edge sharing and corner sharing by the organic anions 121 between the adjacent FeO6 octahedral structures 111.
[0092] For example, the a-axis direction is similar to other FeOOH having an existing layered structure due to edge sharing of Fe atoms in the FeO6 octahedron, but the c-axis direction is different from other FeOOH having an existing layered structure because LFR has a wide layer spacing due to distortion caused by organic anions 121, edge sharing is cut, and Fe atoms are attached to each other by corner sharing. The bonding structure is described in more detail in Figure 3.
[0093] The layer spacing 120 of the at least two or more layers of nanoplatelets 110 may be 1.14 nm to 1.19 nm.
[0094] The number of layers of the at least two or more nanoplatelets 110 is not particularly limited, but preferably the number of layers of the at least two or more nanoplatelets 110 may be 2 to 16.
[0095] In addition, the layer spacing 120 of the at least two layers of nanoplatelets 110 and the number of layers of the at least two layers of nanoplatelets 110 are proportional to the synthesis time of the LFR, so the longer the time for heating the synthesis solution, the more the number of layers increases, and after 8 hours, the rate at which the particle size increases gradually slows down, and the critical point can be reached in about 8 hours (average number of layers: 16).
[0096] The nanoplatelets 110 may be disk-shaped.
[0097] The nanoplatelets 110 can include FeOOH (Iron(III) oxide-hydroxide).
[0098] The organic anion 121 is not particularly limited, but preferably, the organic anion 121 is acetate (CHCOO - ) type compounds.
[0099] For example, the acetate-based compound may include at least one of sodium acetate, potassium acetate, and ammonium acetate.
[0100] In one embodiment, the layered ferric rust according to one embodiment of the present invention may be included in the iron hydroxide nanoparticles according to one embodiment of the present invention.
[0101] The iron hydroxide nanoparticles according to one embodiment of the present invention may be included in at least one of a pollutant adsorbent, a battery catalyst, an oxygen evolution reaction (OER) catalyst, a thermotherapy material, a bioplastic, a construction material, a pigment, and a dye.
[0102] For example, when used as a pollutant adsorbent, the iron hydroxide nanoparticles according to one embodiment of the present invention have wide layer spacing 120 because the nanoplatelets 110 are stacked in the b-axis direction with the octahedrons distorted by the organic anions 121. Therefore, pollutants can more easily flow into the wide layer spacing 120, thereby improving the pollutant removal efficiency.
[0103] In addition, when used as a battery catalyst, the iron hydroxide nanoparticles according to one embodiment of the present invention have a wide layer spacing 120 because the nanoplatelets 110 are stacked in the b-axis direction with the octahedrons distorted by the organic anions 121, allowing more ions to be stored and transported in Na and Li batteries.
[0104] In addition, when used as an OER (oxygen evolution reaction) catalyst, the iron hydroxide nanoparticles according to one embodiment of the present invention have nanoplatelets 110 stacked in the b-axis direction with the octahedron distorted by the organic anion 121, so that the current density is higher than that of other FeOOH nanoparticles, thereby improving efficiency.
[0105] FIG. 4 is a schematic diagram showing a bonding structure of nanoplatelets and organic anions contained in layered ferric rust according to one embodiment of the present invention.
[0106] Referring to FIG. 4, it can be seen that the FeO6 octahedral structures 111 of the layered ferric rust according to one embodiment of the present invention are connected by edge sharing in the a-axis direction, and the edge sharing is broken by the organic anions 121 in the c-axis direction, resulting in corner sharing.
[0107] In this manner, nanoplatelets 110 including FeO6 octahedral structures 111 can be formed in the ac plane and stacked with a large layer spacing 120 along the b-axis direction.
[0108]
[0100] When viewed from the domain direction, the corner sharing FeO6 octahedral structures 111 pairs can form a zigzag layer arrangement together with edge sharing.
[0109] The organic anion 121 can form a pair of FeO6 octahedral structures 111 through bidentate bridging, and can also participate as a component of the FeO6 octahedral structure 111 together with a carboxylate.
[0110] The zigzag arrangement of FeO6 octahedral structures111 pairs and the b-axis stacking induced by organic anions121 can determine the crystal structure of iron oxyhydroxide.
[0111] Therefore, the layered ferric rust according to one embodiment of the present invention may have an atomic arrangement that is completely different from other iron hydroxides having a layered structure.
[0112] [Example 1: Synthesis of layered ferric rust with a new crystal structure] LFR was carried out via the polyol method. FeCl3·6H2O (iron chloride hexahydrate) was used as the iron ion precursor, EG (ethylene glycol) acted as both a reducing agent and a solvent, and CH3COONa (sodium acetate) and H2O acted as the hydroxyl (OH) groups. - ) was used as an adjuvant to impart
[0113] 3mmol of FeCl3·6H2O was dissolved in 400mmol of H2O and 15mmol of CH3HOONa was dissolved in 50mL of EG using an ultrasonic generator, and the solution was placed in a three-neck flask and mechanically stirred for 15 minutes until the color changed from yellow-brown to red-brown. The solution was then rapidly heated to 200°C for 15 minutes and reacted for 8 hours while maintaining the temperature. After the reaction was completed, the solution was cooled and washed at least three times with ethanol.
[0114] FIG. 5 shows a bright field transmission electron microscope image of the layered ferric rust according to Example 1 of the present invention, FIG. 6 shows a scanning transmission electron microscopy image of the layered ferric rust according to Example 1 of the present invention measured at a low voltage (80 kV), and FIG. 7 shows a selected area electron diffraction analysis image of the layered ferric rust according to Example 1 of the present invention.
[0115] 5 to 7, it can be seen that the layered ferric rust according to Example 1 of the present invention has a ring pattern at d=1.14 nm.
[0116] At this time, a strong pattern appeared at d=1.134nm through electron diffraction analysis, which means that the stacking of the disk-shaped 2D layers has crystallographic regularity, and the wide gap between the layers was formed through acetate.Fourier transform infrared analysis showed strong vibration of acetate molecules, confirming that acetate and iron are bonded by bidentate bridging, and then confirmed the coordination number of acetate and iron.
[0117] FIG. 8 is an intensity profile showing the layer spacing of layered ferric rust according to Example 1 of the present invention, FIG. 9 is a graph showing the surface characteristics of layered ferric rust according to Example 1 of the present invention, FIGS. 10 to 14 are graphs showing an analysis of the components of layered ferric rust according to Example 1 of the present invention, FIG. 15 is a Fourier transform infrared spectrum measuring the coordination of acetate in layered ferric rust according to Example 1 of the present invention, and FIG. 16 is a Raman analysis spectrum of layered ferric rust and a polymorph of ferric hydroxide according to Example 1 of the present invention.
[0118] Table 3 shows the peak parameters of the Fourier transform infrared spectrum.
[0119] [Table 4]
[0120] Referring to Table 3 and FIGS. 8 to 16, the spectrum for each element (Fe, C, O) was measured by X-ray-photoelectron spectroscopy analysis, and it was confirmed that LFR was a type of ferric hydroxide.
[0121] Through Raman analysis, it is shown that LFR has a different crystal structure by comparing the Raman peaks of existing ferric hydroxide polymorphs with those of LFR. After that, by analyzing the crystal structure of LFR through synchrotron high resolution powder diffraction measurement, it is found that the crystal structure is different from that of lepidocrocite and green rust, which have layered structures among existing ferric hydroxides.
[0122] FIG. 17 shows a Rietveld analysis of synchrotron high-resolution powder neutron diffraction analysis of the crystal structure of layered ferric rust in accordance with Example 1 of the present invention, and a photograph of the crystal structure of LFR. FIG. 18 is a graph showing the results of a Rietveld analysis of synchrotron high-resolution powder neutron diffraction analysis of the layered ferric rust in accordance with Example 1 of the present invention, in comparison with an existing crystal structure.
[0123] Referring to Figures 17 and 18, the composition of the LFR was analyzed by in-situ X-ray Diffraction, Thermogravimetric Analysis / Differential Thermal Analysis, and Rutherford Backscattering Spectrometry / Time of Flight / Elastic Recoil Detecion.
[0124] In the above mentioned composition analysis, the elemental composition is FeOOH·0.5CH3COO, which proves that LFR is a polymorph of ferric hydroxide.
[0125] Moreover, the layered ferric rust according to Example 1 of the present invention has a completely different crystal structure, as it does not match the graph line of the existing crystal structure.
[0126] When the crystal structure of LFR is explained by the ab-initio method based on the HRPD data, as shown in Tables 1 and 2, it is found that the layered ferric rust according to Example 1 of the present invention (a) belongs to the monoclinic crystal system, (b) belongs to the space group Pn (No. 7), and (c) has unit cell parameters of a = 3.854(2) Å, b = 11.491(7) Å, c = 9.818(4) Å, and β = 88.47(5)° (where b is the distance between layers in the
[0010] axial direction).
[0127] FIG. 19A is a flow chart showing a method for producing layered ferric rust according to one embodiment of the present invention, and FIG. 19B is a schematic diagram showing the process of forming the crystal structure of LFR.
[0128] In one embodiment, layered ferric rust according to one embodiment of the present invention can be prepared as follows.
[0129] The method for producing layered ferric rust according to one embodiment of the present invention includes the same components as those of layered ferric rust according to one embodiment of the present invention, and therefore a description of the same components will be omitted.
[0130] First, in a method for producing layered ferric rust according to an embodiment of the present invention, a step of preparing a mixed solution by mixing an iron ion precursor, a reducing agent, and a solvent (S110) is performed.
[0131] The iron ion precursor is not particularly limited, but may be preferably FeCl3·6H2O (iron chloride hexahydrate).
[0132] The reducing agent can function not only as a reducing agent but also as a solvent. The reducing agent is not particularly limited, but may be preferably ethylene glycol (EG), and specifically may include at least one of ethylene glycol, diethylene glycol, triethylene glycol, and tetraethylene glycol.
[0133] The solvent may be water (H2O).
[0134] In one embodiment, a hydrolysis aid may be further included, and the hydrolysis aid may be CH3COONa (sodium acetate).
[0135] Thereafter, a step (S120) of growing layered ferric rust by heating the mixed solution is performed.
[0136] The step of growing layered ferric rust by heating the mixed solution may include a first heat treatment step (S121) of heating the mixed solution to 200° C. for 15 minutes, and a second heat treatment step (S122) of heating the mixed solution at 200° C. for 8 hours.
[0137] The first heat treatment step (S121) is a process for reaching the temperature of the second heat treatment step (S122), and the mixed solution can be heated up to 200° C. for 15 minutes.
[0138] The second heat treatment step (S122) is a process for forming iron hydroxide FeOOH from ferrihydrite, and the mixed solution can be heated at 200° C. for 8 hours to grow crystals.
[0139] Referring to FIG. 19B, in general, the synthesis process of iron hydroxide is initiated by a heat treatment reaction, and thermodynamically stable iron oxides such as hematite and magnetite are formed by iron ion precursors, and metastable iron hydroxide phases such as green rust and ferrihydrite may be formed.
[0140] However, in the method for producing layered ferric rust according to an embodiment of the present invention, an iron ion precursor reacts with acetate (organic anion) provided from ethylene glycol, which is a reducing agent, and hydroxide ions provided from a solvent (water), to form ferrihydrite.
[0141] Then, ferrihydrite and magnetite are formed through a dehydration and reduction reaction using ethylene glycol. At this time, the content of the solvent is adjusted to produce layered ferric rust according to an embodiment of the present invention, which is an intermediate phase.
[0142] For example, the iron ion precursor reacts with acetate and the hydroxyl group (OH - ) to form ferrihydrite, then it changes from iron hydroxide (FeOOH) to magnetite through dehydration and reduction processes, but if too much water is added, it will hinder the dehydration and reduction processes that lead to magnetite, and the material will remain in the FeOOH phase instead of going to magnetite. For example, even if hydroxyl groups are released as water during the dehydration process, you can add a sufficient amount of water to replenish the hydroxyl groups that disappear.
[0143] That is, in the method for producing layered ferric rust according to one embodiment of the present invention, the excessive water molecules that enter into the synthesis of hydroxide are involved in the dehydration process in the chemical reaction from the metastable phase of ferrihydrite to the stable phase of magnetite, and play a crucial role in the formation of a new crystal structure together with acetate. Therefore, the layered ferric rust according to one embodiment of the present invention can have a completely new crystal structure that is different from lepidocrocite and green rust, which are currently known layered structures of ferric hydroxide.
[0144] Therefore, in the method for producing layered ferric rust according to an embodiment of the present invention, the ratio of hydroxyl groups / iron (OH) is determined according to the content of the solvent contained in the mixed solution. - / Fe) ratio can be adjusted.
[0145] For example, hydroxyl group / iron (OH - The ratio of hydroxyl groups / iron (OH / Fe) is an important factor in the transformation process from iron hydroxide to magnetite, but as the solvent content increases, the ratio of hydroxyl groups / iron (OH / Fe) - The increase in the ratio of OH / Fe hinders the dehydration and reduction reactions required to convert ferric oxyhydroxide to magnetite, resulting in the formation of layered ferric rust (OH / Fe) according to one embodiment of the present invention. - / Fe=1) is magnetite (OH - / Fe=0).
[0146] The content of the solvent may be 150 mmol to 400 mmol. If it is outside the above range, there is a problem that the LFR is not produced.
[0147] Also, depending on the solvent content, the amount of LFR produced can be adjusted.
[0148] The second heat treatment step (S122) may include a step (S122-1) of forming ferrihydrite nanocrystals in the mixed solution, a step (S122-2) of forming nanoplatelets on the surfaces of the ferrihydrite nanocrystals, and a step (S122-3) of growing at least two layers of nanoplatelets attached at different angles to each other into a layered ferric rust (LFR) crystal structure.
[0149] For example, when the time for the second heat treatment step (S122) reaches 30 minutes, ferrihydrite crystals having low crystallinity, which are an intermediate phase before magnetite, may be produced (S122-1).
[0150] When the time of the second heat treatment step (S122) reaches 1 hour, nanoplatelets of 7 nm size begin to be generated on the surface of the ferrihydrite and grow through an alignment and attachment process with other adjacent nanoplatelets, thereby forming LFR (S122-2).
[0151] When the time of the second heat treatment step (S122) reaches 3 to 5 hours, all the ferrihydrite present in the mixed solution is converted into nanoplatelets, which are attached to adjacent nanoplatelets and spread in the a-axis and c-axis directions while being stacked in the b-axis direction, thereby growing into LFR (S122-3).
[0152] When the time of the second heat treatment step (S122) reaches 8 hours, the size of the LFR can be stabilized. At this time, the attachment methods of the nanoplatelets can be roughly divided into three types: axial, lateral, and axial+lateral.
[0153] Therefore, in the method for producing layered ferric rust according to an embodiment of the present invention, even if the mixing ratio of the synthesis solution is the same, the synthesis can be controlled by the second heat treatment time.
[0154] Thereafter, in the method for producing layered ferric rust according to an embodiment of the present invention, a step of cooling the heated mixed solution (S130) is performed.
[0155] In the method for producing layered ferric rust according to an embodiment of the present invention, the process of producing LFR can be terminated by cooling the mixed solution.
[0156] Finally, the method for producing layered ferric rust according to an embodiment of the present invention includes a step of washing the cooled mixed solution to obtain layered ferric rust according to an embodiment of the present invention (S140).
[0157] That is, referring to FIG. 19B, LFR is synthesized through an intermediate phase with stepwise transformation.
[0158] For example, thermodynamically stable iron oxide is generally not synthesized directly from ions in solution, but through a metastable phase. After 30 minutes of heating the synthesis solution, ferrihydrite with low crystallinity is formed as an intermediate phase before the formation of LFR, and after 1 hour, 7 nm-sized nanoplatelets (nanodisks) in the form of particles with layer spacing of 1.2 nm begin to form in the intermediate phase, and adjacent nanoplatelets are observed to be attached at different angles.
[0159] After 3 to 5 hours, the ferrihydrite mesophase is completely consumed to grow LFR, and the SAED pattern shows a strong diffraction pattern at d = 1.2 nm due to the wide layer spacing of LFR.
[0160] The nanoplatelets grow as building blocks on the LFR, growing over time in both thickness and stacking directions and reaching a stable size after about 8 hours.
[0161] FIG. 20 is a transmission electron microscope image obtained by measuring a powder containing a high concentration of layered ferric rust according to one embodiment of the present invention on a glass substrate, FIG. 21 is a transmission electron microscope image obtained by measuring a powder containing a medium concentration of layered ferric rust according to one embodiment of the present invention on a glass substrate, FIG. 22 is a transmission electron microscope image obtained by measuring a powder containing a low concentration of layered ferric rust according to one embodiment of the present invention on a glass substrate, and FIG. 23 is a graph showing Gaussian distribution of the average length of the width and thickness in the layering direction of layered ferric rust according to one embodiment of the present invention measured for n=200 particles obtained through a transmission electron microscope.
[0162] 20 to 23, the shape of the LFR was analyzed by a transmission electron microscope and a scanning electron microscope and found to have a structure in which disk-shaped 2D layers were stacked, and the LFR was uniformly synthesized as a particle in which approximately 16 layers were stacked, with a diameter of 26.1±3.3 nm and a thickness of 18.3±2.7 nm in the stacking direction, and the average spacing between the layers was measured to be approximately 1.19 nm.
[0163] FIG. 24 is a graph showing growth kinetics of layered ferric rust according to an embodiment of the present invention in the lateral and axial directions, FIG. 25 is a schematic diagram showing the growth mode observed by scanning transmission electron microscopy, and FIG. 26 is a schematic diagram of the lateral and axial alignment observed by scanning transmission electron microscopy.
[0164] 24 to 26, it can be seen that the growth of layered ferric rust according to the embodiment of the present invention progresses mainly in the axial and lateral directions, and the size stabilizes within 8 hours.
[0165] FIG. 27 is a graph showing in situ thermal XRD patterns for a powder including layered ferric rust according to an embodiment of the present invention in air (oxidizing), Ar+H2 (reducing), and Ar (inert) atmospheres, and FIG. 28 is a graph showing a phase change diagram for FIG. 27.
[0166] 25 and 26, it can be seen that layered ferric rust according to an embodiment of the present invention is produced by carrying out a second heat treatment step at 300° C. or less to cause a reaction.
[0167] FIG. 29 shows a transmission electron microscopy image and a selected area electron diffraction pattern showing a change over time (reaction time) of a second heat treatment step of layered ferric rust according to an embodiment of the present invention.
[0168] Referring to FIG. 29, the LFR is synthesized through an intermediate phase by a stepwise transformation, as a result of analysis by ex-situ transmission electron microscope. Thermodynamically stable iron oxide is generally not synthesized directly from ions in a solution, but is synthesized through a metastable phase. After 30 minutes of heating the synthesis solution, ferrihydrite with low crystallinity is generated as an intermediate phase before the formation of LFR, and after 1 hour, nanoplatelets (nanodisks) with a particle form of 7 nm size and layer spacing of 1.2 nm begin to form in the intermediate phase, and adjacent nanoplatelets are observed to be attached at different angles.
[0169] After 3 to 5 hours, the ferrihydrite mesophase is completely consumed to grow LFR, and the SAED pattern shows a strong diffraction pattern at d = 1.2 nm due to the wide layer spacing of LFR.
[0170] The nanoplatelets grow as building blocks on the LFR, growing over time in both thickness and stacking directions and reaching a plateau in size after about 8 hours.
[0171] FIG. 30 shows a transmission electron microscope (TEM) image of layered ferric rust according to an embodiment of the present invention depending on the solvent (H2O) content, FIG. 31 shows a powder X-ray diffraction (XRPD) graph of layered ferric rust according to an embodiment of the present invention depending on the solvent (H2O) content, and FIG. 32 is a graph showing the ratio of phases that change from magnetite to layered ferric rust according to an embodiment of the present invention depending on the solvent (H2O) content.
[0172] The formation of LFR is influenced by the conditions of the chemical materials mentioned in the synthesis method. The role of excess water in the crystallization process of magnetite and ferry hydrate is important. The iron ion precursor reacts with acetate and hydrogen ions supplied from water and ethylene glycol (EG) to form the Fe of ferry hydrate.3+ is produced, but then a dehydration process and reduction with ethylene glycol (EG) can occur to produce ferric hydroxide (Fe2O3·H2O) and magnetite.
[0173] Referring to Figures 30 to 32, when the iron ion precursor was fixed at 3 mmol, CH3COONa (sodium acetate) was fixed at 15 mmol, EG was fixed at 50 ml, and the amount of water was increased from 150 mmol to 400 mmol, the final phase after the reaction changed from magnetite to LFR.
[0174] This is because the hydroxyl / iron ratio depending on the amount of water is an important factor in the crystallization process of magnetite and LFR; the more the amount of water increases, the more the dehydration and reduction reactions necessary for the transformation into magnetite are inhibited, making the formation of LFR more stable than that of magnetite.
[0175] The iron hydroxide nanoparticles according to an embodiment of the present invention may be included in at least one of a pollutant adsorbent, a battery catalyst, an oxygen evolution reaction (OER) catalyst, a thermotherapy material, a bioplastic, a construction material, a pigment, and a dye.
[0176] Hereinafter, an arsenic adsorbent containing iron hydroxide nanoparticles according to one embodiment of the present invention will be described as a representative example.
[0177] The arsenic adsorbent according to one embodiment of the present invention can reduce the bioavailability of arsenic through strong arsenic adsorption using organic-inorganic composite iron hydroxide nanoparticles.
[0178] FIG. 33 is a schematic diagram showing an arsenic adsorbent according to one embodiment of the present invention, and FIG. 34 is a schematic diagram showing the adsorption mechanism of arsenic in soil (As in soil) using the arsenic adsorbent according to one embodiment of the present invention.
[0179] The arsenic adsorbent according to one embodiment of the present invention includes organic-inorganic composite iron hydroxide nanoparticles 210, which include at least two or more layers of nanoplatelets 211 (211-1, 211-2) each including at least one FeO6 octahedral structure, and organic ligands 212-1, 212-2 inserted between the at least two or more layers of nanoplatelets 211.
[0180] Therefore, the arsenic adsorbent according to one embodiment of the present invention can have a layer spacing 213 that is relatively wide compared to the size of the nanoparticles, since the organic ligands 212-1 and 212-2 are inserted between the layers of the nanoplatelets 211.
[0181] The organic-inorganic composite iron hydroxide nanoparticles 210 included in the arsenic adsorbent according to an embodiment of the present invention have a layered ferric rust crystal structure, which is different from other FeOOH (Green Rust, Lepidocrocite) materials having an existing layered structure. Therefore, the organic-inorganic composite iron hydroxide nanoparticles 210 are a new pathway and intermediate for forming Fe3O4, and can adsorb and remove arsenic by using the wide layer spacing 213 through the layer structure.
[0182] The nanoplatelet 211 and the organic ligands 212-1 and 212-2 can be connected by bidentate bridging. Thus, the nanoplatelet 211 can have a zigzag structure due to edge sharing and corner sharing between adjacent FeO6 octahedral structures by the organic ligands 212-1 and 212-2.
[0183] For example, the a-axis direction is similar to other FeOOH having an existing layered structure due to edge sharing of Fe atoms in the FeO6 octahedron, but the c-axis direction of the organic-inorganic composite iron hydroxide nanoparticles 210 has a wide layer spacing 213 due to distortion caused by organic ligands 212-1, 212-2, the edge sharing is cut, and the Fe atoms are attached to each other by corner sharing, so that the organic-inorganic composite iron hydroxide nanoparticles 210 can have a crystal structure different from other FeOOH having an existing layered structure.
[0184] The layer spacing 213 of the at least two layers of nanoplatelets 211 may be 1.14 nm to 1.19 nm.
[0185] The number of layers of the at least two or more nanoplatelets 211 is not particularly limited, but preferably, the number of layers of the at least two or more nanoplatelets 211 may be 2 to 16.
[0186] In addition, the layer spacing 213 of the at least two layers of nanoplatelets 211 and the number of layers of the at least two layers of nanoplatelets 211 are proportional to the synthesis time, so the longer the time for heating the synthesis solution, the more the number of layers increases, and after 8 hours, the rate at which the particle size increases gradually slows down, and the critical point can be reached in about 8 hours (average number of layers: 16).
[0187] The nanoplatelet 211 may be in the shape of a disk.
[0188] The nanoplatelets 211 can include FeOOH (Iron(III) oxide-hydroxide).
[0189] The organic ligands 212-1 and 212-2 are not particularly limited, but are preferably acetate (CHCOO - ) type compounds.
[0190] For example, the acetate-based compound may include at least one of sodium acetate, potassium acetate, and ammonium acetate.
[0191] The arsenic adsorbent according to one embodiment of the present invention includes organic-inorganic composite iron hydroxide nanoparticles 210 having a layered ferric iron hydroxide crystal structure in which organic ligands 212-1, 212-2 are inserted between at least two layers of nanoplatelets 211 and the layered spacing 213 is relatively wide compared to the particle size. This allows the arsenic adsorption efficiency to be significantly improved by using a primary adsorption mechanism in which arsenic is adsorbed through chemisorption on the surface of the nanoplatelets 211 and a secondary adsorption mechanism in which arsenic is adsorbed through electrostatic layered intercalation through the layered spacing 213 between the nanoplatelets 211.
[0192] Specifically, in the organic-inorganic composite iron hydroxide nanoparticles 210, the first arsenic 221 is chemically adsorbed by the first organic ligand 212-1 and the second organic ligand 212-2 formed on the surfaces of the first nanoplatelet 211-1 and the second nanoplatelet 211-2, and at the same time, the second arsenic 222 is electrostatically intercalated and adsorbed through the layer-like space 213 formed by the second organic ligand 212-2 between the first nanoplatelet 211-1 and the second nanoplatelet 211-2.
[0193] The primary mechanism is chemisorption, H2AsO4 -1 However, the organic ligands 212-1 and 212-2 (eg, acetate) bonded to the Fe layer are removed, and the organic ligands 212-1 and 212-2 (eg, acetate) can be chemically bonded to and adsorbed at the sites from which the organic ligands 212-1 and 212-2 (eg, acetate) have been removed.
[0194] The second mechanism is layer intercalation, H2AsO4 -1The complex itself may be physically adsorbed in the wide interlamellar spaces between the layers.
[0195] For example, the secondary mechanism is that, in the arsenic adsorbent according to one embodiment of the present invention, the nanoplatelets 211 are stacked in the b-axis direction with the octahedrons distorted by the organic ligands 212-1 and 212-2, so that the layer spacing 213 is wide and arsenic can more easily flow into the wide layer spacing 213, thereby improving the arsenic removal efficiency by electrostatic layer insertion.
[0196] Therefore, the arsenic adsorbent according to one embodiment of the present invention is an arsenic adsorbent comprising organic-inorganic composite iron hydroxide nanoparticles 210 that maintains the soil ecosystem from the viewpoint of a sustainable environment and has an increased degree of adsorption of arsenic (221, 222), and is synthesized based on the structural reconstruction of naturally occurring hydroxides, thereby improving the arsenic adsorption efficiency while maintaining the soil environment.
[0197] As a result, the arsenic adsorbent according to one embodiment of the present invention can be used as a soil amendment.
[0198] Hereinafter, the bonding structure between the nanoplatelets 211 and the organic ligands 212-1 and 212-2 of the organic-inorganic composite iron hydroxide nanoparticles 210 contained in the arsenic adsorbent according to one embodiment of the present invention will be described in more detail.
[0199] The FeO6 octahedral structures of the organic-inorganic composite iron hydroxide nanoparticles 210 are connected by edge sharing in the a-axis direction, and in the c-axis direction, the edge sharing is broken by organic ligands 212-1 and 212-2, allowing corner sharing.
[0200] In this manner, nanoplatelets 211 comprising FeO6 octahedral structures can be formed in the ac plane and stacked with a large layer spacing 213 along the b-axis direction.
[0201]
[0100] When viewed from the domain direction, the corner-sharing FeO6 octahedral structure pairs can form a zigzag layer arrangement together with the edge-sharing.
[0202] The organic ligands 212-1 and 212-2 can form an FeO6 octahedral structure pair through bidentate ligand bridging, and can also participate as building blocks of the FeO6 octahedral structure together with the carboxylate itself.
[0203] The zigzag arrangement of FeO6 octahedral pairs and the b-axis stacking induced by the organic ligands 212-1, 212-2 can determine the crystal structure of iron oxyhydroxide.
[0204] Therefore, the organic-inorganic composite iron hydroxide nanoparticles 210 can have an atomic arrangement that is completely different from other iron hydroxides having a layered structure.
[0205] Specifically, γ-FeOOH and green rust may have boehmite arranged in a zigzag arrangement along the ac plane and brucite with a planar FeO3(OH)3 arrangement along the ab plane, respectively.
[0206] However, the organic-inorganic composite iron hydroxide nanoparticles 210 can have a completely different crystal structure, in that the FeO6 octahedral structure is connected by edge sharing in the a-axis direction by the organic ligands, and in the c-axis direction, the edge sharing is broken at the organic ligands 212-1 and 212-2, and corner sharing occurs to form a layered ferric iron hydroxide crystal structure.
[0207] FIG. 35 is a schematic diagram showing a method for producing an arsenic adsorbent according to one embodiment of the present invention, and FIG. 36 is a schematic diagram showing a specific example of the method for producing an arsenic adsorbent according to one embodiment of the present invention.
[0208] The method for producing an arsenic adsorbent according to one embodiment of the present invention includes the same components as the arsenic adsorbent according to one embodiment of the present invention, and therefore a description of the same components will be omitted.
[0209] First, in the method for preparing an arsenic adsorbent according to an embodiment of the present invention, a step of preparing a mixed solution by mixing an iron ion precursor, a reducing agent, an organic ligand precursor, and a solvent (S210) is performed.
[0210] The iron ion precursor is not particularly limited, but may be preferably FeCl3·6H2O (iron chloride hexahydrate).
[0211] The reducing agent can function not only as a reducing agent but also as a solvent. The reducing agent is not particularly limited, but may be preferably ethylene glycol (EG), and specifically may include at least one of ethylene glycol, diethylene glycol, triethylene glycol, and tetraethylene glycol.
[0212] The solvent may be water (H2O).
[0213] The organic ligand precursor is not particularly limited, but preferably, the organic ligand precursor is acetate (CHCOO - The acetate-based compound may include at least one of sodium acetate, potassium acetate, and ammonium acetate.
[0214] Thereafter, in the method for producing an arsenic adsorbent according to an embodiment of the present invention, a step of heating the mixed solution to grow organic-inorganic composite iron hydroxide nanoparticles (S220) is performed.
[0215] The step (S220) of heating the mixed solution to grow organic-inorganic composite iron hydroxide nanoparticles may include a first heat treatment step (S221) of heating the mixed solution to 200°C for 15 minutes, and a second heat treatment step (S222) of heating the mixed solution at 200°C for 8 hours.
[0216] The first heat treatment step (S221) is a process for reaching the temperature of the second heat treatment step (S222), and the mixed solution can be heated up to 200° C. for 15 minutes.
[0217] The second heat treatment step (S222) is a process for forming iron hydroxide FeOOH from ferrihydrite, and the mixed solution can be heated at 200° C. for 8 hours to grow crystals.
[0218] In general, the synthesis process of iron hydroxide nanoparticles is initiated by heat treatment, and thermodynamically stable iron oxides such as hematite and magnetite are formed by iron ion precursors, and metastable iron hydroxide phases such as green rust and ferrihydrite can be formed.
[0219] However, in the method for producing an arsenic adsorbent according to an embodiment of the present invention, an iron ion precursor can form ferrihydrite by reacting with acetate (organic ligand) provided from ethylene glycol, which is a reducing agent, and hydroxide ions provided from water (solvent).
[0220] Then, ferrihydrite and magnetite are formed through a dehydration and reduction reaction with ethylene glycol. At this time, by adjusting the content of the solvent, organic-inorganic composite iron hydroxide nanoparticles having an intermediate layered ferric iron hydroxide crystal structure can be produced.
[0221] For example, the iron ion precursor reacts with acetate and the hydroxyl group (OH -) to form ferrihydrite, then it changes from iron hydroxide (FeOOH) to magnetite through dehydration and reduction processes, but if too much water is added, it will hinder the dehydration and reduction processes that lead to magnetite, and the material will stay in the FeOOH phase instead of going to magnetite. For example, even if hydroxyl groups are released by water during the dehydration process, you can add enough water to replenish the hydroxyl groups that disappear.
[0222] That is, in the method for producing an arsenic adsorbent according to an embodiment of the present invention, excessive water molecules in the synthesis of hydroxide are involved in the dehydration process in the chemical reaction from ferrihydrite, which is a metastable phase, to magnetite, which is a stable phase, and play a crucial role in the formation of a new crystal structure together with acetate. Therefore, the method for producing an arsenic adsorbent according to an embodiment of the present invention can have a new crystal structure that is completely different from lepidocrocite and green rust, which are layered structures of ferric hydroxide currently known.
[0223] Therefore, in the method for producing an arsenic adsorbent according to an embodiment of the present invention, the hydroxyl group / iron (OH - / Fe) ratio can be adjusted.
[0224] For example, hydroxyl group / iron (OH - The ratio of hydroxyl groups / iron (OH / Fe) is an important factor in the transformation process from iron hydroxide to magnetite, but as the solvent content increases, the ratio of hydroxyl groups / iron (OH / Fe) - / Fe ratio increases, hindering the dehydration and reduction reactions required to convert ferric oxyhydroxide to magnetite, and forming organic-inorganic composite iron hydroxide nanoparticles (OH - / Fe=1) is magnetite (OH - / Fe=0).
[0225] The content of the solvent may be 150 mmol to 400 mmol. If it is outside the above range, there is a problem that organic-inorganic composite iron hydroxide nanoparticles (eg, layered ferric rust, LFR) are not produced.
[0226] In addition, the amount of the organic-inorganic composite iron hydroxide nanoparticles produced can be adjusted depending on the content of the solvent.
[0227] The second heat treatment step (S222) may include a step of forming ferrihydrite nanocrystals in the mixed solution (S222-1), a step of forming nanoplatelets on the surfaces of the ferrihydrite nanocrystals (S222-2), and a step of growing at least two layers of nanoplatelets at different angles to each other into a layered ferric iron hydroxide crystal structure (S222-3).
[0228] For example, when the time of the second heat treatment step (S222) reaches 30 minutes, ferrihydrite crystals having low crystallinity, which are an intermediate phase before magnetite, may be produced (S122-1).
[0229] When the time of the second heat treatment step (S222) reaches 1 hour, nanoplatelets of 7 nm size begin to be generated on the surface of the ferrihydrite and grow through the process of alignment and attachment with other adjacent nanoplatelets, thereby forming organic-inorganic composite iron hydroxide nanoparticles (S222-2).
[0230] When the time of the second heat treatment step (S222) reaches 3 to 5 hours, all the ferrihydrite present in the mixed solution is converted into nanoplatelets, which are attached to adjacent nanoplatelets and spread in the a-axis and c-axis directions while being stacked in the b-axis direction, thereby growing into organic-inorganic composite iron hydroxide nanoparticles (S222-3).
[0231] When the time of the second heat treatment step (S222) reaches 8 hours, the size of the organic-inorganic composite iron hydroxide nanoparticles can be stabilized. At this time, the attachment method of the nanoplatelets can be roughly divided into three types: axial, lateral, and axial+lateral.
[0232] Therefore, in the method for producing an arsenic adsorbent according to an embodiment of the present invention, even if the mixing ratio of the synthesis solution is the same, the synthesis can be controlled by the second heat treatment time.
[0233] In one embodiment, the step of preparing a mixed solution by mixing the iron ion precursor, the reducing agent, the organic ligand precursor, and the solvent (S210) may further include adjusting the pH of the mixed solution.
[0234] Referring to FIG. 36, ferrihydrite is synthesized at pH 7 using an iron ion precursor (preferably FeCl3·6H2O (iron chloride hexahydrate)), and then goethite is formed through a classical crystallization method without a reducing agent and an organic ligand. However, even if goethite is formed, a reducing agent and an organic ligand precursor are mixed with the goethite, the pH is adjusted to 1.5 or less, and then the goethite can be grown into organic-inorganic composite iron hydroxide nanoparticles through a first heat treatment and a second heat treatment method.
[0235] In addition, ferrihydrite synthesized at pH 7 can be grown into organic-inorganic composite iron hydroxide nanoparticles through particle attachment growth by heat treatment using a reducing agent and organic ligands in the pH range of 1 to 2.
[0236] That is, in the method for preparing an arsenic adsorbent according to an embodiment of the present invention, even if goethite is used as an iron ion precursor, organic-inorganic composite iron hydroxide nanoparticles can be prepared by adjusting the pH of the mixed solution and then performing heat treatment.
[0237] For example, when FeCl3·6H2O (iron chloride hexahydrate) is used as an iron ion precursor, organic-inorganic composite iron hydroxide nanoparticles can be produced by the particle attachment growth method when the pH is adjusted to 2 or less. Even if goethite is formed through classical crystallization at pH 7, organic-inorganic composite iron hydroxide nanoparticles can be produced by the particle attachment growth method through a heat treatment method when a reducing agent and an organic ligand precursor are mixed with the goethite and the pH is adjusted to 1.5 or less.
[0238] Therefore, the pH of the mixed solution may be 1-2.
[0239] Thereafter, in the method for producing an arsenic adsorbent according to an embodiment of the present invention, a step of cooling the heated mixed solution (S230) is performed.
[0240] In the method for producing an arsenic adsorbent according to an embodiment of the present invention, the process of forming the layered structure may be terminated by cooling the mixed solution.
[0241] Finally, the method for preparing an arsenic adsorbent according to an embodiment of the present invention includes a step of washing the cooled mixture solution to obtain organic-inorganic composite iron hydroxide nanoparticles (S240).
[0242] Therefore, the method for producing an arsenic adsorbent according to one embodiment of the present invention synthesizes organic-inorganic composite iron hydroxide nanoparticles using iron hydroxide, a clay mineral that is abundant on Earth, and reconstructs naturally occurring ferric oxyhydroxide (ferrihydrite) and hydroxide polymorph (goethite) to produce an environmentally friendly and economical nanomaterial capable of immobilizing arsenic.
[0243] [Comparative example 1: Gt] The synthesis was carried out by mixing 180 mL of 5 M (molar concentration) KOH with 100 mL of 1 M Fe(NO3)3 (iron ion precursor) and reacting them in an oven at 70°C for 60 hours.
[0244] Oxyhydroxide (ferrihydrite): Synthesized by adding 0.1 M Fe(NO3)3 to 30 mL of 1 M KOH until the pH was in the range of 7 to 8.
[0245] [Comparative example 2: Control] The control was a soil sample that did not contain goethite (Gt) and organic-inorganic composite iron hydroxide nanoparticles.
[0246] [Example 2: r-FAN] Organic-inorganic composite iron hydroxide nanoparticles were prepared by chemically reacting FeCl3·6H2O, ethylene glycol, and the surface ligand acetate under acidic conditions (pH<2) using pathway 1 in Figure 4.
[0247] First, for chemical synthesis, FeCl3·6H2O was reacted with acetate in a mixture of water and ethylene glycol at 200 °C for 8 h.
[0248] FIG. 37 is an image showing a manufacturing process of the arsenic adsorbent according to Example 2 of the present invention.
[0249] Referring to FIG. 37, it can be seen that the arsenic adsorbent according to Example 2 of the present invention allows for large-scale synthesis capable of producing 40 g of nanoparticles per batch.
[0250] FIG. 38 is a scanning electron microscopy (SEM) and a transmission electron microscopy (TEM) image showing the hierarchical structure of the arsenic adsorbent according to Example 2 of the present invention.
[0251] Referring to Figure 38, it can be seen that the length of the organic-inorganic composite iron hydroxide nanoparticles contained in the arsenic adsorbent of Example 2 of the present invention is 22.4 ± 2.59 nm, the thickness is 16.3 ± 3.35 nm, and the spacing between layers is 1.14 nm.
[0252] FIG. 39 is an image showing a selected area electron diffraction (SAED) pattern of the arsenic adsorbent according to Example 2 of the present invention, and a graph showing the results of powder X-ray diffraction (XRPD).
[0253] Referring to FIG. 39, it can be seen that the organic-inorganic composite iron hydroxide nanoparticles contained in the arsenic adsorbent according to Example 2 of the present invention have a structure different from other naturally occurring hydroxide polymorphs.
[0254] FIG. 40 is a schematic diagram showing the arsenic (As) adsorption mechanism, FIG. 41 is a graph showing the results of inductively coupled plasma mass spectrometry (ICP-MS) showing the adsorption capacity of the arsenic adsorbent of Comparative Example 1 and the arsenic adsorbent of Example 2 of the present invention, and FIG. 42 is a graph showing the electrokinetic potential before and after arsenic adsorption.
[0255] 40 to 42, when the adsorption capacities of the arsenic adsorbent according to Comparative Example 1, which is made of goethite (Gt) used as an existing arsenic adsorbent, and the arsenic adsorbent according to Example 2 of the present invention are compared using inductively coupled plasma mass spectrometry (ICP-MS), it can be seen that the arsenic adsorbent according to Example 2 of the present invention adsorbs 6.7 times more arsenic than the arsenic adsorbent according to Comparative Example 1.
[0256] In the case of surface potential measurement (Zeta potential), the potential of the arsenic adsorbent according to Comparative Example 1 decreased from 39.3 mV to -14.2 mV before and after arsenic adsorption, whereas the potential of the arsenic adsorbent according to Example 2 of the present invention decreased from 12.1 mV to 32.1 mV.
[0257] However, when compared with the results of inductively coupled plasma mass spectrometry (ICP-MS), the arsenic adsorbent according to Example 2 of the present invention had a higher potential than that of Comparative Example 1, despite having adsorbed 6.7 times more arsenic than the arsenic adsorbent according to Comparative Example 1. This shows that the surface coordination and adsorption mechanism of the arsenic adsorbent according to Comparative Example 1 and the arsenic adsorbent according to Example 2 of the present invention are different.
[0258] Specifically, the arsenic adsorbent according to Comparative Example 1 adsorbs arsenic through a primary mechanism of chemically binding arsenic only to the outer surface, whereas the arsenic adsorbent according to Example 2 of the present invention, in addition to the primary mechanism of chemically binding arsenic to the outer surface like the arsenic adsorbent according to Comparative Example 1, also includes a secondary mechanism in which arsenic is chemically bound to the surface between the wide layers and arsenic is physically inserted into the spaces between the layers.
[0259] FIG. 43 is a graph showing the results of X-ray photoelectron spectroscopy (XPS) of the arsenic adsorbent according to Comparative Example 1 before arsenic adsorption, FIG. 44 is a graph showing the results of X-ray photoelectron spectroscopy of the arsenic adsorbent according to Comparative Example 1 after arsenic adsorption, FIG. 45 is a graph showing the results of X-ray photoelectron spectroscopy of the arsenic adsorbent according to Example 2 of the present invention before arsenic adsorption, FIG. 46 is a graph showing the results of X-ray photoelectron spectroscopy of the arsenic adsorbent according to Example 2 of the present invention after arsenic adsorption, FIG. 47 is a graph showing the results of Fourier transform infrared spectroscopy (FT-IR) of the arsenic adsorbent according to Example 2 of the present invention before and after arsenic adsorption, and FIG. 48 is a graph showing the results of Fourier transform infrared spectroscopy of the arsenic adsorbent according to Comparative Example 1 before and after arsenic adsorption.
[0260] 43 to 48, after arsenic was adsorbed, the peak of the As-O bond was detected as the main bond with the highest intensity in the arsenic adsorbent of Example 2 of the present invention, whereas in the case of the arsenic adsorbent of Comparative Example 1, Fe-OH remained as the main bond after arsenic was adsorbed.
[0261] This means that in the arsenic adsorbent of Comparative Example 1, since the Fe-OH peak is maintained, only arsenic that is chemically bound to the outer surface of the arsenic adsorbent of Comparative Example 1 is present, whereas in the arsenic adsorbent of Example 2 of the present invention, arsenic is adsorbed by AsO insertion and the formation of Fe-As-O bonds.
[0262] Furthermore, the AsO4 insertion and chemically bonded Fe-As-O bonds of the arsenic adsorbent according to Example 2 of the present invention can be confirmed by FT-IR analysis.
[0263] Specifically, since the strength of the As-O bond is relatively higher than the strength of the Fe-As-O bond in the arsenic adsorbent according to Example 2 of the present invention, it can be seen that a large amount of arsenic is inserted between the layers of the organic-inorganic composite iron hydroxide nanoparticles contained in the arsenic adsorbent according to Example 2 of the present invention in the form of AsO4.
[0264] FIG. 49 is a graph showing the results of a bioassay of A. kimi in the absence of arsenic in artificial soil, and FIG. 50 is a graph showing the results of a bioassay of B. juncea in artificial soil that was not treated with arsenic.
[0265] Figures 49 and 50 show that the treatment with the arsenic adsorbent according to Comparative Example 1 and the arsenic adsorbent according to Example 2 of the present invention significantly affected the decrease in the bioavailability of As, and the reproduction and phytotoxicity analyses were performed in the artificial soil contaminated with arsenic to investigate the suitability of biological indicator species in the soil ecosystem, and a control experiment was performed in advance in the artificial soil without arsenic contamination to explain the effect of the addition of the arsenic adsorbent according to Comparative Example 1 and the arsenic adsorbent according to Example 2 of the present invention on the test group of Allonychiurus kimi and Brassica juncea in uncontaminated soil.
[0266] Referring to Figures 49 and 50, it can be seen that there is no significant difference between the control groups.
[0267] Figure 51 is a graph showing the results of a bioassay of A. kimi in arsenic-treated artificial soil (circles are adults, bars are larvae), Figure 52 is a graph showing the arsenic content in the arsenic-treated artificial soil, Figure 53 is an image of A. kimi in the arsenic-treated artificial soil, Figure 54 is a graph showing B. juncea in the artificial soil, Figure 55 is a graph showing the arsenic content of B. juncea in the artificial soil, and Figure 56 is a graph showing an image of B. juncea in the artificial soil.
[0268] Referring to FIG. 51, in a springtail reproduction test using artificial soil contaminated with arsenic, the number of surviving adult specimens treated with the arsenic adsorbent of Comparative Example 1 and the arsenic adsorbent of Example 2 of the present invention (9.2±0.8) was significantly higher than the number of surviving adult specimens treated with Comparative Example 2 (5.6±0.9).
[0269] In the treatment of Comparative Example 2, the adults of A. kimi produced a small number of larvae (1.4±2.2), whereas in the treatment of the arsenic adsorbent of Comparative Example 1, they produced a slight increase (27.8±13.4), but this increase was not statistically significant.
[0270] On the other hand, treatment with the arsenic adsorbent according to Example 2 of the present invention showed significantly higher juvenile production of 113.6±39.7.
[0271] Referring to FIG. 52, it can be seen that after 28 days of exposure of A. kimi specimens, the arsenic concentrations in the bodies were 22.3±10.1 mg / kg, 37.2±21.2 mg / kg, and 5.1±2.9 mg / kg in the treatments with the arsenic adsorbent of Comparative Example 1, Comparative Example 2, and the arsenic adsorbent of Example 2 of the present invention, respectively.
[0272] 53, the arsenic concentration in the body of A. kimi was significantly lower in the arsenic adsorbent according to Example 2 of the present invention. In addition, the adult A. kimi produced significantly more offspring in the arsenic adsorbent according to Example 2 of the present invention than in the arsenic adsorbent according to Comparative Example 1 and Comparative Example 2 (white points).
[0273] Referring to FIG. 54, in a phytotoxicity test using artificial soil contaminated with arsenic, the average weights of the roots and shoots changed from 0.008±0.002 to 0.13±0.02 and from 0.1±0.01 to 0.36±0.02, respectively, and it can be seen that the weights increased significantly upon treatment with the arsenic adsorbent according to Example 2 of the present invention.
[0274] Referring to FIG. 55, the concentrations of accumulated arsenic in B. juncea were 5.29±1.10, 5.13±1.39, and 0.34±0.04 mg / kg for the treatments with the arsenic adsorbent of Comparative Example 1, Comparative Example 2, and Example 2 of the present invention, respectively.
[0275] Referring to FIG. 56, the concentration of accumulated arsenic in B. juncea was significantly lower when treated with the arsenic adsorbent according to Example 2 of the present invention compared to other treatments, and the specimens also grew significantly faster.
[0276] Therefore, the results of the bioanalysis in arsenic-contaminated artificial soil show that the arsenic adsorbent of Example 2 of the present invention can reduce the bioavailability of arsenic in A. kimi and B. juncea in arsenic-contaminated soil, thereby improving their fitness.
[0277] 57 to 62 are graphs and images showing the results of biological tests to examine the treatment of the arsenic adsorbent of Comparative Example 1 (Gt), Comparative Example 2 (Control), and the arsenic adsorbent of Example 2 of the present invention (r-FAN) as an amendment to As-contaminated mine soil in Collembolan propagation (A. kimi) and phytotoxicity (B. juncea) tests.
[0278] Figures 57-62 show that because the results for the artificial soils are not representative of all arsenic-contaminated soils at the site, including old mine sites, biological tests were performed with A. kimi and B. juncea on arsenic-contaminated mine soils.
[0279] FIG. 57 is a graph showing the number of A. kimi adults (circles) and larvae (bars) surviving after 28 days of exposure to As-contaminated mine soil.
[0280] Referring to FIG. 57, in the springtail reproduction test, the numbers of adults surviving in the soils treated with the arsenic adsorbent of Comparative Example 1, Comparative Example 2, and Example 2 of the present invention were 8.0±0.0, 6.8±1.3, and 8.75±1.0, respectively, and the numbers of offspring produced were 50.8±24.5, 56.5±8.9, and 97.0±21.1, respectively.
[0281] FIG. 58 is a graph showing the mean As concentration (mg / kg) of surviving adult worms after exposure to arsenic.
[0282] 58, the soil treated with the arsenic adsorbent according to Example 2 of the present invention had the largest number of surviving adults and the largest offspring production. In addition, after 28 days of exposure, the arsenic concentrations in the body of A. kimi were 70.1±25.1, 62.5±9.5, and 41.0±14.5 mg / kg in the treatments with the arsenic adsorbent according to Comparative Example 1, Comparative Example 2, and Example 2 of the present invention, respectively.
[0283] Figure 59 is an image of a larval specimen produced after exposure to arsenic.
[0284] 59, although there was no statistically significant difference, the lowest arsenic concentration was observed in the bodies of adult A. kimi in the soil treated with the arsenic adsorbent according to Example 2 of the present invention. In addition, the adult A. kimi treated with the arsenic adsorbent according to Example 2 of the present invention gave birth to significantly more offspring.
[0285] FIG. 60 is a graph showing the weight (g) of root and shoot of B. juncea after exposure to arsenic.
[0286] Referring to FIG. 60, in the phytotoxicity test, the average root weights of the groups treated with the arsenic adsorbent of Comparative Example 1, Comparative Example 2, and the arsenic adsorbent of Example 2 of the present invention were 0.08±0.01, 0.06±0.01, and 0.10±0.01 g, respectively, and the group treated with the arsenic adsorbent of Example 2 of the present invention showed significantly higher root weights.
[0287] In addition, the average sprout weight was in the range of 0.39±0.04 for the group treated with the arsenic adsorbent of Comparative Example 1 and 0.49±0.03 for the control group of Comparative Example 2, with the weight of the sprouts in the group treated with the arsenic adsorbent of Comparative Example 1 being the lowest.
[0288] However, there was no significant difference between the groups treated with the arsenic adsorbent according to Comparative Example 2 and Example 2 of the present invention.
[0289] FIG. 61 is a graph showing the mean As concentration (mg / kg) of B. juncea after exposure to arsenic.
[0290] Referring to FIG. 61, in the treatment with the arsenic adsorbent of Comparative Example 1, Comparative Example 2, and Example 2 of the present invention, the arsenic accumulation concentrations of B. juncea were 6.6±0.5, 8.7±1.1, and 6.3±0.3 mg / kg, respectively.
[0291] Figure 62 is a growth image of B. juncea after exposure to arsenic.
[0292] 62, the arsenic accumulation concentration of B. juncea was much lower in the treatment groups of the arsenic adsorbent according to Comparative Example 1 and the arsenic adsorbent according to Example 2 of the present invention than in the treatment of Comparative Example 2. Despite the considerable difference in root weight and accumulated arsenic concentration in B. juncea after exposure to arsenic, there was no noticeable change in the external shape of the shoots between the treatment groups.
[0293] Therefore, referring to Figures 57 to 62, it can be seen that the arsenic adsorbent according to Example 2 of the present invention significantly reduces the bioavailability of arsenic in old mine soils with high arsenic concentrations.
[0294] FIG. 63 is an image showing the morphological characteristics of the arsenic adsorbent according to Example 2 of the present invention in artificial soil (a) and arsenic-contaminated soil (b).
[0295] 63, the shape and phase of the arsenic adsorbent according to Example 2 of the present invention were maintained for 28 days. However, the treatment with the arsenic adsorbent according to Comparative Example 1 and the arsenic adsorbent according to Example 2 of the present invention did not significantly change the pH and EC of the soil to an extent that would affect soil microorganisms and plants.
[0296] Table 4 shows the pH and EC of arsenic-contaminated mine soil and artificial soil 28 days after the addition of the arsenic adsorbent according to Comparative Example 1 and the arsenic adsorbent according to Example 2 of the present invention.
[0297] [Table 5]
[0298] Referring to Table 4, the soil treated with the arsenic adsorbent according to Example 2 of the present invention showed the lowest pH and EC because the ionic strength of the pore water was reduced by the adsorption and intercalation of a significant amount of bioavailable arsenic in the amendment.
[0299] FIG. 64 is a graph showing the results of Olsen extraction for arsenic-contaminated artificial soil (a) and arsenic-contaminated mine soil (b) treated with the arsenic adsorbent of Comparative Example 1 (Gt), Comparative Example 2 (Control), and the arsenic adsorbent of Example 2 of the present invention (r-FAN).
[0300] FIG. 64 shows that Olsen extractable arsenic was measured after an exposure interval of 28 days to observe the immobilization effect of the arsenic adsorbent according to Example 2 of the present invention on bioavailable arsenic.
[0301] Referring to FIG. 64, in both arsenic-contaminated artificial and mine soils, the arsenic adsorbent according to Example 2 of the present invention showed 3 times greater arsenic immobilization than the arsenic adsorbent according to Comparative Example 1.
[0302] Using Wenzel's sequential extraction process (SEP), the arsenic fractions (F1-F5) in equilibrium with other components of soil were evaluated for the arsenic adsorbent according to Comparative Example 1 and the arsenic adsorbent according to Example 2 of the present invention. The results are shown in Table 5.
[0303] [Table 6]
[0304] In the arsenic-contaminated artificial soil, the ratio of fraction 1 (F1; non-specific absorption) was greatly reduced in both the arsenic adsorbent of Comparative Example 1 and the arsenic adsorbent of Example 2 of the present invention.
[0305] Treatment with the arsenic adsorbent according to Example 2 of the present invention rapidly reduced F1 from 63.4±4.4 to 2.4±0.6%. At the same time, the ratio of F1 reduced by the arsenic adsorbent according to Comparative Example 1 and the arsenic adsorbent according to Example 2 of the present invention shifted the equilibrium state of As fractionation to the stronger chemical adsorption side, increasing F2 (especially chemically adsorbed As).
[0306] In addition, in the soil treated with the arsenic adsorbent according to Example 2 of the present invention, the ratio of F3 (poorly crystalline hydrous metal oxides) increased to a level similar to that of F2, indicating two states of arsenic species bound to the arsenic adsorbent according to Example 2 of the present invention with different binding strengths.
[0307] Besides surface adsorption, the arsenic adsorbent according to Example 2 of the present invention also converted F1 into F3 species by integrating additional arsenic into the crystal structure through an insertion mechanism.
[0308] This immobilized arsenic more strongly than the arsenic adsorbent of Comparative Example 1, which relies only on surface chemical adsorption.
[0309] Unlike the behavior observed in the artificial soils, the distribution of As fractions in the mine soils contained a small proportion of bioavailable F1-F2 and a high proportion of crystallized As in the F3-F5 forms.
[0310] It was unclear whether the treatment with the arsenic adsorbent according to Comparative Example 1 and the arsenic adsorbent according to Example 2 of the present invention had a significant effect on the ratio of F2-F5 in the mine soil samples. However, the arsenic adsorbent according to Example 2 of the present invention reduced the ratio of F1 by 33%, while the arsenic adsorbent according to Comparative Example 1 did not induce any change in F1.
[0311] Overall, the arsenic adsorbent according to Example 2 of the present invention effectively reduced F1, the most harmful bioavailable form for plants and animals, by maintaining arsenic in suspended forms corresponding to F2 and F3, demonstrating the mechanism of restoring ecological health in both soil types.
[0312] FIG. 65 is a graph showing the average percentage of arsenic by form in artificial soils, and FIG. 66 is a graph showing the average percentage of arsenic by form in actual mine soils.
[0313] F1 is a non-specifically bound form of arsenic, F2 is a specifically chemically bound form of arsenic, and F3 is an amorphous form of arsenic hydroxide.
[0314] Table 6 shows the results of FIGS. 65 and 66.
[0315] [Table 7]
[0316] Referring to Figures 65, 66 and Table 6, since there is a lot of bioavailable arsenic in artificial soil, the arsenic adsorbent (r-FAN) according to Example 2 of the present invention and the arsenic adsorbent (Gt) according to Comparative Example 1 have high F1 removal amounts, and therefore the amount of arsenic adsorption in the form of F2 is also high.
[0317] Furthermore, in the case of the arsenic adsorbent (r-FAN) according to Example 2 of the present invention, unlike the arsenic adsorbent (Gt) according to Comparative Example 1, the adsorption amount of arsenic in the form of F3 is significantly high, which indicates that the arsenic adsorbent includes an arsenic adsorption mechanism based on layered intercalation, which is a mechanism different from that of the arsenic adsorbent (Gt) according to Comparative Example 1.
[0318] In addition, since there is almost no bioavailable arsenic in actual mine soil, the F1 value is low, but it can be seen that the arsenic adsorbent (r-FAN) according to Example 2 of the present invention removes 33% more arsenic than the arsenic adsorbent (Gt) according to Comparative Example 1.
[0319] As described above, even if the present invention has been described with reference to limited embodiments and drawings, the present invention is not limited to the above embodiments, and various modifications and variations are possible from such descriptions by those skilled in the art to which the present invention pertains. Therefore, the scope of the present invention should not be limited to the described embodiments, but should be determined not only by the claims below, but also by equivalents to the claims. [Explanation of symbols]
[0320] 110 Nanoplatelets 111 FeO6 octahedral structure 120 Layer Spacing 121 Organic Anions 210 Organic-inorganic composite iron hydroxide nanoparticles 211 Nanoplatelets 211-1 First Nanoplatelet 211-2 Second Nanoplatelet 212-1 First organic ligand 212-2 Second organic ligand 221 Arsenic I 222 Arsenic
Claims
1. Layered ferric rust having a novel crystal structure that satisfies the following conditions (a) to (c): (a) The crystal system is monoclinic; (b) The space group belongs to Pn (No. 7); (c) the unit cell parameters are a=3.854±0.002 Å, b=11.491±0.007 Å, c=9.818±0.004 Å, and β=88.47±0.005°, where b is the distance between layers along the [010] axis; At least two layers of nanoplatelets including at least one FeO 6 octahedral structure; and an organic anion inserted between the at least two layers of nanoplatelets; The at least two layers of nanoplatelets have a distance between the layers determined by the organic anion; The nanoplatelets and the organic anions are linked by bidentate bridging; The nanoplatelets are layered iron rusts, characterized in that the adjacent FeO 6 octahedral structures include zigzag corner sharing and edge sharing due to the organic anion.
2. The layered iron rust according to claim 1, wherein the atomic coordinates and equivalent isotropic displacement parameters of the elements in the lattice of the layered iron rust satisfy the following Table 1. 【Table 1】
3. The layered iron rust according to claim 1, wherein the layered iron rust is represented by the following chemical formula 1: FeO x C y H z (Chemical formula 1) (In the above Chemical Formula 1, x is a number between 3 and 3.5 (3≦x≦3.5), y is a number between 0.67 and 1 (0.67≦y≦1), and z is a number between 1.94 and 3.5 (1.94≦z≦3.5).)
4. The layered iron rust according to claim 1, characterized in that the layer spacing of the at least two layers of nanoplatelets is 1.14 nm to 1.19 nm.
5. The layered iron rust according to claim 1, wherein the number of nanoplatelets in the at least two layers is 2 to 16.
6. The layered iron rust according to claim 1, wherein the nanoplatelets comprise FeOOH (Iron (III) oxide-hydroxide).
7. The organic anion is acetate (CH 3 COO - The layered iron rust according to claim 1, comprising a Cd-type compound.
8. 2. Iron hydroxide nanoparticles comprising the layered iron rust according to claim 1.
9. The iron hydroxide nanoparticles according to claim 8, which are included in at least one of a pollutant adsorbent, a battery catalyst, an oxygen evolution reaction (OER) catalyst, a thermotherapy material, a bioplastic, a construction material, a pigment, and a dye.
Citation Information
Patent Citations
Green rust, production method thereof, pigment, and anion exchanger
JP2022080364A
KR10-1771005、
KR10-2019-0085902、