Manufacturing method of platinum nanoparticles

A room-temperature synthesis of platinum nanoparticles using a silicon compound and titania nanoparticles addresses the limitations of high-temperature and organic-substance-based methods, resulting in highly active and transparent materials with antibacterial and antiviral properties.

JP7581112B2Active Publication Date: 2024-11-12OSAKA GAS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021060687
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-31
Publication Date
2024-11-12
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

Existing methods for synthesizing platinum nanoparticles require high temperatures, organic substances that inhibit photocatalyst activity, or involve difficult-to-remove reducing agents, leading to low crystallinity, reduced specific surface area, and aggregation issues.

Method used

A method using a silicon compound with a specific structure and stirring in water at room temperature to produce platinum nanoparticles, combined with titania nanoparticles, to achieve high activity and transparency without the need for organic substances or metal salts.

Benefits of technology

The method enables the production of highly active and transparent platinum nanoparticles with antibacterial and antiviral properties, suitable for use in photocatalysts, without the drawbacks of previous methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581112000001
    Figure 0007581112000001
  • Figure 0007581112000002
    Figure 0007581112000002
  • Figure 0007581112000003
    Figure 0007581112000003
Patent Text Reader

Abstract

To provide a method for producing a platinum nanoparticle that makes it possible to: synthesize a platinum nanoparticle having a very small particle size and high activity and allowing transparent coating, without using a hard-to-remove reductant such as organic materials and metal salts; and to combine the platinum nanoparticle with a photocatalyst to readily prepare an antibacterial-antiviral material having high transparency and high activity.SOLUTION: A method for producing a platinum nanoparticle includes the step of mixing a silicon compound represented by general formula (1): HSi(R1)(R2)(R3) (1) (where R1, R2, and R3 are the same or different to represent an alkyl group, an alkoxy group, a hydrogen atom, a hydroxy group, an acyloxy group, a halogen atom, or -O-Si bond) with a platinum precursor.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing platinum nanoparticles. [Background technology]

[0002] Platinum nanoparticles are used as catalysts in various applications, such as fuel cells, solar cells, chemical synthesis, etc. Platinum chloride (H2PtCl6) is often used as a precursor of platinum, and platinum (Pt) can be easily obtained by heating (Non-Patent Documents 1 to 4).

[0003] Titania (titanium oxide) is used as a photocatalyst to decompose harmful substances and dirt, and as a hydrophilic film. Titania (titanium oxide) is also considered to have various applications such as synthesis of hydrogen and oxygen, corrosion prevention, resin additive, anode of dye-sensitized solar cells, artificial photosynthesis, antibacterial and antiviral. [Prior art documents] [Non-patent literature]

[0004] [Non-Patent Document 1] Nobuyuki Kamiya, Kenichi Hoshino, and Kenichiro Ohta. "Thermal decomposition of platinum chloride and its application to platinum-coated electrodes." Journal of the Chemical Society of Japan (Chemistry and Industrial Chemistry) 1987.2 (1987): 140-146. [Non-Patent Document 2] Farrell, Brendan P., Igor V. Sevonkaev, and Dan V. Goia. "Preparation of dispersed spherical platinum particles with controlled size and internal structure." Platinum Metals Rev 57.3 (2013): 161-168. [Non-Patent Document 3] Xiao, YaoMing, et al. "Low temperature fabrication of high performance and transparent Pt counter electrodes for use in flexible dye-sensitized solar cells." Chinese Science Bulletin 57.18 (2012): 2329-2334. [Non-Patent Document 4] Yuichi Negishi. "Establishment of a precise synthesis method for highly active catalytic platinum nanoparticles." Hosokawa Powder Technology Foundation Annual Report 23 (2015): 136-141. Summary of the Invention [Problem to be solved by the invention]

[0005] However, the above-mentioned conventional techniques have the following problems.

[0006] The technology disclosed in Non-Patent Document 1 is a method for synthesizing platinum nanoparticles that relies on a typical thermal reduction process, which requires heating to 530°C. Even when the reduction is assisted by alcohol or the like, heating to 400°C or higher is still required.

[0007] The technology disclosed in Non-Patent Document 2 attempts to synthesize platinum nanoparticles at temperatures below 500° C., but generally, crystallinity is low at low temperatures, and the specific surface area decreases dramatically at high temperatures.

[0008] The technology disclosed in Non-Patent Document 3 attempts to synthesize platinum nanoparticles at 120°C for use as positive electrode catalysts in dye-sensitized solar cells. However, this requires long periods of heating and a vacuum state, and the produced platinum nanoparticles are aggregated.

[0009] In recent years, the polyol reduction method has been used as a method for synthesizing ultrafine platinum particles with high activity at low temperatures. However, the polyol reduction method requires the addition of organic substances, sodium hydroxide, etc., and when combined with a photocatalyst, the organic substances inhibit the activity of the photocatalyst, and sodium cannot be removed by heating.

[0010] The technique disclosed in Non-Patent Document 4 requires heating to 100° C. or higher for the reaction to obtain platinum particles, and the solvent is ethylene glycol, which has a high boiling point, so high-temperature heating is also required to remove the ethylene glycol.

[0011] To date, there has been no known method for easily synthesizing platinum nanoparticles that have a very small particle size and are highly active, without using reducing agents that inhibit catalytic activity, such as organic substances, or reducing agents that are difficult to remove, such as metal salts, at room temperature.

[0012] Therefore, the present invention aims to provide a method for producing platinum nanoparticles that is very small in particle size, highly active, and capable of being transparently coated, without using reducing agents that are difficult to remove, such as organic substances or metal salts.

[0013] Photocatalysts do not exhibit antibacterial or antiviral properties unless they are exposed to ultraviolet light. Highly crystalline photocatalysts have a high refractive index, which causes a lot of light scattering and makes it difficult to achieve transparency.

[0014] Therefore, an object of the present invention is to easily obtain a highly transparent and active antibacterial and antiviral material by combining the platinum nanoparticles with a photocatalyst. [Means for solving the problem]

[0015] Means for Solving the Problems The present inventors conducted intensive research in light of the above-mentioned objectives and discovered that, in a method for producing platinum nanoparticles, platinum nanoparticles can be obtained by using a silicon material having a specific structure and stirring in water at room temperature, thereby solving the above-mentioned problems.

[0016] After further research, the present invention was completed.

[0017] That is, the present invention includes the following configurations.

[0018] Section 1. A method for producing platinum nanoparticles, comprising the steps of: General formula (1): HSi(R 1 )(R 2 )(R 3 ) (1) (In the formula, R 1 , R 2 , and R 3 are the same or different and each represents an alkyl group, an alkoxy group, a hydrogen atom, a hydroxyl group, an acyloxy group, a halogen atom, or an -O-Si bond. A silicon compound represented by the formula: a platinum precursor; Manufacturing method.

[0019] The acyloxy group (RCOO-) is, for example, an acetoxy group (CH3COO-).

[0020] Section 2. The platinum precursors are hexachloroplatinic acid (H2PtCl6) and hexachloroplatinic acid (IV) hexahydrate (H2PtCl6·6H2O); The method for producing the same according to item 1.

[0021] Section 3. The mixing step is carried out using a solvent, The solvent contains 80% by mass or more of water. 3. The method according to item 1 or 2.

[0022] Section 4. The mixing step is carried out using a solvent, The solvent comprises an organic acid. 4. The method according to any one of items 1 to 3.

[0023] Section 5. The organic acid is acetic acid. Item 5. The method for producing the same according to item 4.

[0024] Section 6. The mixing step is carried out at a reaction temperature of 100° C. or less. 6. The method according to any one of items 1 to 5.

[0025] Section 7. In the silicon compound represented by the general formula (1), 1 , R 2 and the R 3 are the same or different and each is an alkoxy group having 1 to 4 carbon atoms or an acyloxy group having 1 to 4 carbon atoms. 7. The method according to any one of items 1 to 6.

[0026] Section 8. In the silicon compound represented by the general formula (1), 1 , R 2 and the R 3 are the same or different and each is a methoxy group, an ethoxy group, or an acetoxy group; The method according to any one of items 1 to 7.

[0027] Section 9. The mixing step is carried out in the presence of titania nanoparticles. The method for producing the same according to any one of items 1 to 8.

[0028] Section 10. The titania nanoparticles are anatase titania nanoparticles. Item 10. The method for producing the same according to Item 9.

[0029] Section 11. The titania nanoparticles have acyloxy groups bonded to at least some of the titanium atoms present on the surface, The titania nanoparticles have a weight loss of 5% by mass or more at 200°C or higher when heated to 600°C using a thermogravimetric and differential thermal analyzer; The titania nanoparticles are a photocatalyst; The mixing step is carried out in the presence of the photocatalyst. 11. The method according to item 9 or 10.

[0030] Section 12. The titania nanoparticles have an average particle size of 30 nm or less, and the acyloxy group is an acetoxy group. Item 12. The method for producing the same according to Item 11.

[0031] Section 13. The titania nanoparticles have an average particle diameter of 1 nm to 6 nm and a specific surface area of ​​150 m 2 / g~500m 2 / g, 13. The method according to any one of items 9 to 12.

[0032] Section 14. A photocatalyst comprising: Platinum nanoparticles, titania nanoparticles, and General formula (1): HSi(R 1 )(R 2 )(R 3 ) (1) (In the formula, R 1 , R 2 , and R 3 are the same or different and each represents an alkyl group, an alkoxy group, a hydrogen atom, a hydroxyl group, an acyloxy group, a halogen atom, or an -O-Si bond. The silicon compound represented by the formula: Specific surface area is 150m 2 / g~500m 2 / g, Photocatalyst.

[0033] Section 15. An antibacterial and / or antiviral material, Platinum nanoparticles, titania nanoparticles, and General formula (1): HSi(R 1 )(R 2 )(R 3 ) (1) (In the formula, R 1 , R 2 , and R 3 are the same or different and each represents an alkyl group, an alkoxy group, a hydrogen atom, a hydroxyl group, an acyloxy group, a halogen atom, or an -O-Si bond. The silicon compound represented by the formula: Specific surface area is 150m 2 / g~500m2 / g, have antibacterial and / or antiviral activity under visible light or in the dark; Antibacterial and / or antiviral materials.

[0034] Section 16. An antiviral coating solution, The antibacterial and / or antiviral material according to item 15, and Contains water Antiviral coating liquid. Effect of the Invention

[0035] According to the present invention, a method for producing platinum nanoparticles can be used to synthesize platinum nanoparticles that have a very small particle size, are highly active, and can be transparently coated, without using reducing agents that are difficult to remove, such as organic substances or metal salts.

[0036] According to the present invention, in the method for producing platinum nanoparticles, a silicon material having a specific structure is used and platinum nanoparticles can be obtained in a short time by stirring at room temperature in water, which is inexpensive and easy to remove.

[0037] According to the present invention, the reaction (stirring in water at room temperature) is carried out in the presence of titania nanoparticles, thereby making it possible to obtain a highly dispersible composite of platinum and titania.

[0038] According to the present invention, the material containing the composite of platinum nanoparticles and titania can be used as a transparent and highly active antibacterial and antiviral material. [Brief description of the drawings]

[0039] [Figure 1] 1 shows the results of an embodiment of the present invention, and is a TEM image of Example 5. It can be seen that Pt particles of about 5 nm (black particles in the center) are generated in titania primary particles of 3 nm to 5 nm. [Diagram 2]2 is a diagram showing the results of an embodiment of the present invention. Fig. 2 shows a TEM image of Example 5. It can be seen that Pt particles of about 3 nm (black particles in the center) were produced. [Diagram 3] 3 shows the results of an embodiment of the present invention. Figure 3 shows a TEM image of Example 5. Particle A of about 4 nm is a Pt nanoparticle, and overlapping particle B is a TiO2 nanoparticle. [Figure 4] 4 is a diagram showing the results of an embodiment of the present invention. Fig. 4 is a TEM-EDS spectrum of particle A in Fig. 3. Although Ti was partially detected, Pt was mainly detected. [Diagram 5] 5 is a diagram showing the results of an embodiment of the present invention. Fig. 5 shows the peaks of particle B in Fig. 3. Although a small amount of Pt was detected, Ti and O were mainly detected. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0040] In this specification, the term "containing" is a concept that encompasses all of "comprise," "consist essentially of," and "consist only of."

[0041] In this specification, when a numerical range is expressed as A to B, it indicates A or more and B or less.

[0042] In this specification, "titanium oxide" or "titania" does not only refer to titanium dioxide (TiO2), but also includes titanium trioxide (Ti2O3); titanium monoxide (TiO); and titanium dioxide having an oxygen deficiency, such as Ti4O7 and Ti5O9.

[0043] In this specification, "titanium oxide" or "titania" may contain groups other than Ti-O-Ti resulting from the synthesis of titanium oxide, such as terminal Ti-OH groups, TiOCH3 groups, TiOCH2CH3 groups, TiOCH2CH2CH3 groups, TiOCH(CH3)CH3 groups, TiOCH2CH2CH2CH3 groups, TiOCOCH3 groups, etc.

[0044] In this specification, "titanium oxide" or "titania" also includes those having an organic acid or the like bonded to a terminal OH group.

[0045] 1. Manufacturing method of platinum nanoparticles The method for producing platinum nanoparticles of the present invention comprises the steps of: General formula (1): HSi(R 1 )(R 2 )(R 3 ) (1) (In the formula, R 1 , R 2 , and R 3 are the same or different and each represents an alkyl group, an alkoxy group, a hydrogen atom, a hydroxyl group, an acyloxy group, a halogen atom, or an -O-Si bond. A silicon compound represented by the formula: The method includes mixing the platinum precursor with the platinum precursor.

[0046] (1) Platinum nanoparticles and platinum precursors The platinum precursor of the present invention (platinum compound serving as a platinum source) is preferably chloroplatinic acid (tetrachloroplatinic acid), sodium chloroplatinic acid (VI), potassium chloroplatinic acid (VI), ammonium chloroplatinic acid (VI), ammonium bromide platinic acid (VI), bromoplatinic acid (tetrachloroplatinic acid), sodium bromide platinic acid (VI), potassium bromide platinic acid (VI), ammonium bromide platinic acid (VI), chloroplatinic acid (tetrachloroplatinic acid), sodium chloroplatinic acid (II), potassium chloroplatinic acid (II), ammonium chloroplatinic acid (II), bis(acetylacetonato)platinum (II), platinum chloride (II), platinum chloride (IV), platinum bromide (II), platinum bromide (IV), platinum iodide (II), platinum iodide (IV), platinum oxide (VI), tetraammine platinum (II) nitrate, These include potassium tetracyanoplatinate(II), dichloro(1,5-cyclooctadiene)platinum(II), diiodo(1,5-cyclooctadiene)platinum(II), dimethyl(1,5-cyclooctadiene)platinum(II), (trimethyl)cyclopentadienylplatinum(IV), tetraamineplatinum(II), tetrachloroplatinic acid, iodotrimethylplatinum(IV), dichlorobis(pyridine)platinum(II), tetraamineplatinum(II) hydroxide, platinum sulfite, platinum hexafluoroacetylacetonate(II), hexahydroxoplatinic acid, sodium hexahydroxoplatinate(IV), potassium hexahydroxoplatinate(IV), ammonium hexahydroxoplatinate(IV), tetraammineplatinum(II) hydrogen carbonate, and tetraammineplatinum(II) hydrogen phosphate solution.

[0047] Among these, those which are water-soluble and do not contain any metal elements other than platinum are preferred.

[0048] More preferred are chloroplatinic acid (VI) and ammonium chloroplatinate (VI).

[0049] In the method for producing platinum nanoparticles of the present invention, the platinum precursor is preferably hexachloroplatinic (IV) acid (H2PtCl6) and hexachloroplatinic (IV) acid hexahydrate (H2PtCl6·6H2O).

[0050] These platinum precursors (platinum sources) are reduced to obtain platinum nanoparticles.

[0051] (2) Silicon compounds (reducing agents) In the present invention, a compound having a SiH group is used as the reducing agent.

[0052] The compound having a SiH group has the general formula (1): HSi(R 1 )(R 2 )(R 3 ) (1) (In the formula, R 1 , R 2 , and R 3 are the same or different and each represents an alkyl group, an acyloxy group, a hydrogen atom, a hydroxyl group, an acyloxy group, a halogen atom, or an -O-Si bond. It is a silicon compound represented by the formula:

[0053] Since the compound can be used by suspending it in a solvent, it is not necessarily required to dissolve it in a solvent.

[0054] From the viewpoint of not impairing the activity of platinum nanoparticles or photocatalysts, it is preferable that the silicon compound, after acting as a reducing agent, becomes a substance close to silica through oxidation, hydrolysis, etc., and HSiCl3, H2SiCl2, polysilazanes or cyclosilazanes -(H2Si-NH)n-, alkoxysilanes having a SiH group SiH(OR)3 or SiH2(OR)2, carboxysilanes having a SiH group, SiH(OCOR)3, or SiH2(OCOR)2 are preferred.

[0055] In the method for producing platinum nanoparticles of the present invention, preferably, in the silicon compound represented by the general formula (1), 1 , R 2 and the R 3 are the same or different and each is an alkoxy group having 1 to 4 carbon atoms or an acyloxy group having 1 to 4 carbon atoms.

[0056] In the method for producing platinum nanoparticles of the present invention, preferably, in the silicon compound represented by the general formula (1), 1 , R 2 and the R 3 are the same or different and each is a methoxy group, an ethoxy group, or an acetoxy group.

[0057] In particular, SiH(OR)3, SiH2(OR)2, SiH(OCOCH3)3, or SiH2(OCOCH3)2, which are water-soluble or can be made water-soluble by contact with an organic acid, are preferred.

[0058] When SiH(OR)3 or SiH2(OR)2 comes into contact with an organic acid such as acetic acid, all or part of the alkoxy groups become acyloxy groups, making them more hydrophilic, dissolving or dispersing in water and more likely to participate in reactions.

[0059] If the amount of silicon compound (reducing agent) is too small relative to the platinum precursor (platinum source), the reaction is difficult to occur, whereas if the amount is too large, silica, which is a solid component, is likely to be produced.

[0060] During the reaction, other reducing agents may be added in addition to the above substances.

[0061] Preferred examples of the other reducing agent include hydrazine, oxalic acid, formic acid, gallic acid, gallic acid esters, hydroquinone, methoquinone, lithium aluminum hydride, iron (II) ions, sodium borohydride, tin (II) ions, polyphenols, tannic acid, hyposulfite, hyposulfite salts, ascorbic acid, and sodium ascorbate.

[0062] When the reaction is carried out in the presence of titania nanoparticles, a photocatalytic reduction reaction caused by irradiation with ultraviolet light may be used in combination.

[0063] (3) Titania nanoparticles In the method for producing platinum nanoparticles of the present invention, the mixing step is preferably carried out in the coexistence of titania nanoparticles.

[0064] In the present invention, titania nanoparticles may be present and reacted together.

[0065] The coexistence of titania nanoparticles is expected to have the following benefits: 1) the photocatalytic reduction reaction can be used in combination, 2) the hydrophilic titania contributes to the dispersion of the generated platinum nanoparticles, 3) a synergistic effect between the photocatalyst and platinum, such as antibacterial and antiviral properties, can be expected, and 4) contamination on the platinum surface can be decomposed by the photocatalyst.

[0066] However, the coexistence of titania nanoparticles is not essential, and platinum production occurs even without the addition of titania nanoparticles.

[0067] When titania nanoparticles are used together, those having a large specific surface area and high dispersibility in water are preferred.

[0068] The specific surface area of ​​titania nanoparticles is 10m 2 / g~500m 2 / g is preferred, 45m 2 / g~400m 2 / g is more preferable, and 90m 2 / g~350m 2 / g is more preferred.

[0069] The diameter of the titania nanoparticles is preferably from 1 nm to 150 nm, more preferably from 1 nm to 30 nm, further preferably from 1 nm to 16 nm, and most preferably from 1 nm to 6 nm.

[0070] In particular, the titania nanoparticles of the present invention are preferably those that are uniformly dispersed in water, and can be produced, for example, by the following production method.

[0071] (A) a step of mixing a titanium-containing substance, an organic acid, and water to obtain a dispersion; (B) stirring the dispersion obtained in the step (A) for 5 minutes or more; and (C) a step of heating the dispersion obtained in the step (B) at 70° C. or higher for 1 hour or more. and In the step (A), the mixture ratio of the titanium-containing substance and the organic acid is such that the amount of acyloxy groups in the organic acid is 0.4 mol or more per mol of titanium in the titanium-containing substance.

[0072] In the case of acetic acid, 2 moles or more is preferable, but in the case of lactic acid or citric acid, highly transparent titania nanoparticles can be obtained even with 0.5 moles or less.

[0073] <Process (A)> In step (A), a specific amount of a substance containing titanium, a specific amount of an organic acid, and water are mixed to obtain a dispersion.

[0074] The titanium-containing substance to be used is not particularly limited as long as it is a substance that becomes titanium oxide by heating. The titanium-containing substance is preferably titanium oxide and / or a titanium oxide precursor, and specifically includes titanium oxide; titanium hydroxide; titanium alkoxide; titanium halide such as titanium trichloride and titanium tetrachloride (particularly those neutralized with a base); metallic titanium, etc. Also, only one of these may be used, or two or more may be used in combination.

[0075] Among these, from the viewpoint of dispersibility of the obtained titania, titanium alkoxide, titanium hydroxide or titanium halide, particularly those neutralized with a base, are preferred, and titanium alkoxide is more preferred from the viewpoint of purity and dispersibility.

[0076] Examples of titanium alkoxides include titanium tetraisopropoxide, titanium tetra n-butoxide, titanium tetra n-propoxide, and titanium tetraethoxide. From the viewpoints of cost and water solubility of by-products, titanium tetraisopropoxide is preferred.

[0077] Depending on the combination of titanium alkoxide and organic acid, the resulting titania may act as a catalyst to liberate ester compounds that are poorly soluble in water, but the titania itself is not a problem. For example, when titanium tetra-n-butoxide and acetic acid are combined, butyl acetate is produced and liberated when they are mixed and heated.

[0078] From the viewpoint of obtaining a uniform dispersion, it is preferable to employ a combination of an organic acid and a titanium alkoxide that can provide an organic acid alkoxide having excellent water solubility.

[0079] Titanium halides (titanium tetrachloride, titanium trichloride, etc.) are preferably neutralized with a base and the precipitate washed from the viewpoints of impurities (halogens), corrosion of the reactor during mass production, and crystallinity control. In that case, it is preferable to use the titanium halides without drying from the viewpoint of dispersibility of the obtained titania.

[0080] When using a solid such as titanium oxide or metallic titanium, the average particle size is preferably 100 nm or less, more preferably 50 nm or less. The lower limit is not particularly set, but is usually about 1 nm. When the particle size is large, it may be ground in a dry or wet manner using a planetary ball mill, paint shaker, or the like. The average particle size can be measured, for example, by observation with an electron microscope (SEM or TEM).

[0081] The concentration of the titanium-containing substance in the dispersion is preferably 0.01 mol / L to 5 mol / L, and more preferably 0.05 mol / L to 3 mol / L, from the viewpoints of productivity and viscosity of the reaction liquid.

[0082] In the method for producing platinum nanoparticles of the present invention, the mixing step is preferably carried out using a solvent, and the solvent preferably contains an organic acid.

[0083] The acid used in the reaction is an organic acid, represented by the chemical formula C n H 2n+1 Monocarboxylic acids represented by COOH (n = 0-11), HOOCC m H 2m Examples thereof include dicarboxylic acids represented by COOH (m=0 to 8) and hydroxycarboxylic acids having 1 to 6 carbon atoms.

[0084] Of the monocarboxylic acids, acetic acid (n=1) is preferred from the viewpoints of solubility in water (particularly, those with n=4 or less are easily soluble in water) and odor (particularly, those with n=2 to 4 have a strong odor).

[0085] For the dicarboxylic acid, m is preferably 0 to 2 from the viewpoint of solubility in water, but m is more preferably 1 or 2 in consideration of dispersibility in titania.

[0086] Examples of hydroxycarboxylic acids include glycolic acid, lactic acid, malic acid, tartaric acid, and citric acid.

[0087] Of these, acetic acid and lactic acid are particularly preferred as the organic acid, from the viewpoint of being able to be removed later by volatilization.

[0088] In the method for producing platinum nanoparticles of the present invention, the organic acid is preferably acetic acid.

[0089] These organic acids may be used alone or in combination of two or more.

[0090] From the viewpoints of dispersibility and cost, the amount of organic acid used is preferably adjusted so that the COOH group is contained in the titanium-containing substance in an amount of 0.4 mol or more, preferably 0.5 mol to 10 mol, per mol of titanium in the titanium-containing substance. The more organic acid is used, the more improved the dispersibility becomes.

[0091] The concentration of the organic acid in the dispersion is preferably from 0.005 mol / L to 10 mol / L, and more preferably from 0.02 mol / L to 7 mol / L, from the viewpoints of dispersibility and cost.

[0092] In the method for producing platinum nanoparticles of the present invention, the mixing step is preferably carried out using a solvent, and the solvent preferably contains 80 mass % or more of water.

[0093] As the reaction solvent, it is preferable to use an aqueous solvent such as water as the main component (specifically, for example, 50% by weight or more), but alcohols or esters may be contained during the reaction.

[0094] For example, when titanium tetraisopropoxide is used as a raw material, it reacts with an organic acid to produce isopropanol, and may also produce isopropyl esters of organic acids upon heating.

[0095] Alcohols or esters may be added to the dispersion obtained in step (A) or may be generated in the system. The alcohols or esters may be removed by heating in an open system at 100° C. or less, or may remain in the reaction liquid.

[0096] When an alcohol is contained in the dispersion liquid, the particle size tends to become small, and therefore, in order to control the particle size, an alcohol may be intentionally added.

[0097] In the present invention, inorganic acids (particularly strong inorganic acids) such as nitric acid, hydrochloric acid, and sulfuric acid, which are usually used in hydrothermal synthesis reactions of titania nanoparticles, may be used.

[0098] Carboxylic acid is preferred because the resulting titania nanoparticles have low adhesion to the substrate, and in addition, from the viewpoints of equipment corrosion, impurities, wastewater, and the like.

[0099] Inorganic and organic acids can be used supplementarily to improve the dispersibility and uniformity of the raw material and to facilitate handling, without impairing the effect, for example, in the range of 0.01 mol / L or less. In this case, the concentrations of N, Cl, and S elements in the dispersion liquid are all 0.01 mol / L.

[0100] In the method for producing platinum nanoparticles of the present invention, the titania nanoparticles are preferably anatase type titania nanoparticles.

[0101] Of the inorganic acids and organic acids, nitric acid is preferred because it easily produces anatase-type titania, which has high transparency, and is easy to remove.

[0102] The pH of the dispersion obtained in step (A) is preferably 1.5 or more and less than 6, more preferably 2 to 5, from the viewpoints of corrosion of the apparatus, safety in handling, and dispersibility.

[0103] In the step (A), the method for preparing the dispersion is not particularly limited, and the titanium-containing substance, the organic acid and water (solvent) may be mixed simultaneously or successively.

[0104] In particular, from the viewpoint of preventing aggregation and forming large lumps and enabling continuous stirring, it is preferable to mix the organic acid and water (solvent) and then add the titanium-containing substance while stirring. Conversely, if water is added dropwise after mixing the titanium-containing substance and organic acid, aggregation is likely to occur.

[0105] <Process (B)> In the step (B), the dispersion obtained in the step (A) is stirred for 5 minutes or more.

[0106] The stirring method is not particularly limited, and may be performed according to a conventional method. The stirring time is 5 minutes or more, preferably 15 minutes or more, from the viewpoint of sufficiently reacting the titanium-containing substance with the organic acid and water. The upper limit of the stirring time is not particularly limited, but is usually about 240 hours.

[0107] <Process (C)> In the method for producing platinum nanoparticles of the present invention, the mixing step is preferably carried out at a reaction temperature of 100° C. or lower.

[0108] In the step (C), the dispersion obtained in the step (B) is heated at 70° C. or higher for 1 hour or more.

[0109] Step (C) may be carried out under normal pressure or under pressure in a closed vessel.

[0110] When heating is performed under pressure, it may be performed under supercritical conditions. More specifically, the pressure during heating is preferably 0.45 MPa or more, more preferably 1 MPa to 30 MPa, from the viewpoint of increasing the particle size. However, when a small particle size is acceptable, it is easier to perform the heating under normal pressure.

[0111] The heating temperature is 50° C. or higher, preferably 70° C. to 450° C., and more preferably 150° C. to 400° C. If the heating temperature is less than 50° C., highly active titania nanoparticles cannot be obtained.

[0112] When the reaction is carried out under normal pressure, the reaction temperature is preferably 50° C. to 120° C., and more preferably 70° C. to 110° C., from the viewpoint of obtaining titania nanoparticles having a smaller average particle size.

[0113] When the reaction is carried out under pressure (not supercritical), from the viewpoint of obtaining titania nanoparticles having a larger average particle size than those under normal pressure, the temperature is preferably 120° C. to 370° C., more preferably 150° C. to 300° C. In this case, the reaction may be first heated at a low temperature (e.g., 50° C. to 120° C.) and then heated to a high temperature (e.g., 120° C. to 370° C.).

[0114] When the reaction is carried out under supercritical conditions, even under pressure, the dispersion obtained in step (B) can be mixed with supercritical water in a flow reactor, for example, to synthesize titania nanoparticles with uniform particle size and a titania dispersion with extremely high dispersibility in an extremely short time. In this case, it is preferable to mix the dispersion obtained in step (B) at 50°C or less with supercritical water at 374°C or more and hold it at 300°C or more (particularly 375°C to 450°C) for 1 second or more (particularly 5 seconds to 600 seconds). When contacting with supercritical water, the reaction can be completed in an extremely short time.

[0115] The titania nanoparticles of the present invention thus obtained have significantly improved dispersibility compared to conventional titania nanoparticles.

[0116] The titania nanoparticles of the present invention have an average particle size of about 3 nm to 50 nm, and particularly about 4 nm to 40 nm.

[0117] By setting the average particle size of the titania nanoparticles within this range, the metal nanoparticles can be supported appropriately and more firmly, and a film having higher visible light catalytic activity and higher transparency can be formed.

[0118] Normally, when the average particle size is small, the shrinkage during heating is large, which makes it easy for cracks and peeling off from the substrate to occur. However, the metal nanoparticle-supported titania nanoparticles of the present invention are a material with excellent coatability, despite the use of titania nanoparticles with a small average particle size.

[0119] In the present invention, the average particle size of the titania nanoparticles is measured by observation with a transmission electron microscope (TEM).

[0120] The titania nanoparticles of the present invention have a specific surface area of ​​30 m 2 / g~500m 2 / g, especially 40m 2 / g~350m 2 / g is obtained.

[0121] By setting the specific surface area of ​​the titania nanoparticles within this range, the metal nanoparticles can be supported appropriately and more firmly, and the visible light catalytic activity can be easily increased.

[0122] The specific surface area of ​​the titania nanoparticles is measured by the BET method.

[0123] In the method for producing platinum nanoparticles of the present invention, preferably, the titania nanoparticles have an average particle diameter of 1 nm to 6 nm and a specific surface area of ​​150 m 2 / g~500m 2 / g.

[0124] The titania nanoparticles of the present invention have N, Cl, and S element concentrations of 0 to 5,000 ppm, and particularly 0 to 1,000 ppm.

[0125] By setting the concentrations of N, Cl, and S elements in the titania nanoparticles within this range, it is easy to suppress corrosion of the substrate, etc. This condition means that there is no impurity derived from the acidic titania precursor such as TiCl4 or TiOSO4, or there is only a very small amount of it.

[0126] The concentrations of N, Cl, and S elements in the titania nanoparticles are measured by WDX (fluorescent X-ray).

[0127] The crystal form of the titania nanoparticles is preferably anatase type, which can particularly improve the visible light catalytic activity.

[0128] There are no other crystal forms than the anatase type, and it is preferable that the anatase type is 100%.

[0129] Thereafter, the titania nanoparticles of the present invention can be recovered by precipitating and centrifuging the titania nanoparticles of the present invention using a conventional method.

[0130] In this way, the titania nanoparticles of the present invention can be used to adjust the average particle size and specific surface area, and also have excellent dispersibility. Therefore, they can be used not only for photocatalysis (superhydrophilicity, decomposition of organic / inorganic substances, hydrogen production, etc.), but also for a wide variety of applications, such as dye-sensitized solar cells, transparent conductive films, catalyst supports, heat-resistant coatings, high refractive coatings, and heat-shielding coatings.

[0131] The titania dispersion of the present invention can be prepared as a uniform dispersion by using the reaction liquid that has been subjected to the above steps (A) to (C) and adding a dispersion step such as ultrasonic dispersion.

[0132] In the method for producing platinum nanoparticles of the present invention, preferably, the titania nanoparticles have acyloxy groups (RCOO-) bonded to at least some of the titanium atoms present on the surface, the titania nanoparticles show a weight loss of 5 mass % or more at 200°C or higher when heated to 600°C using a simultaneous differential thermal and thermogravimetric analyzer, the titania nanoparticles are a photocatalyst, and the mixing step is carried out in the coexistence of the photocatalyst.

[0133] In the method for producing platinum nanoparticles of the present invention, the titania nanoparticles preferably have an average particle size of 30 nm or less, and the acyloxy group is preferably an acetoxy group.

[0134] In the present invention, the form of titania nanoparticles carrying metal nanoparticles (platinum nanoparticles) is preferably adopted, and metal nanoparticle-carrying titania nanoparticles in which metal nanoparticles are carried on the surfaces of titania nanoparticles are preferred.

[0135] In the present invention, the titania nanoparticles preferably have acyloxy groups bonded to at least some of the titanium atoms present on the surface, and metal nanoparticles are supported on the surface in an amount of 90 mass% or less relative to the titanium oxide in the titania nanoparticles.

[0136] In the present invention, preferably, when the temperature is raised to 600° C. using a thermogravimetric and differential thermal analyzer, the mass loss at 200° C. or higher is 5% by mass or more.

[0137] In the titania nanoparticles carrying metal nanoparticles (platinum nanoparticles) of the present invention, the average particle size and specific surface area of ​​both the titania nanoparticles and the metal nanoparticles can be adjusted, and the titania nanoparticles and the metal nanoparticles are firmly adhered to each other. In addition, the titania nanoparticles and the metal nanoparticles have excellent dispersibility and are not prone to aggregation, so that the coating property and transparency are excellent without using a separate additive such as a dispersant.

[0138] The titania nanoparticles and photocatalyst carrying metal nanoparticles (platinum nanoparticles) of the present invention have sufficient coatability and transparency without the use of a separate dispersant, and therefore can have excellent visible light catalytic activity without the visible light catalytic activity being impaired by additives such as dispersants.

[0139] The metal nanoparticle (platinum nanoparticle)-supporting titania nanoparticle of the present invention is useful as a photocatalyst (particularly, a visible light-responsive photocatalyst).

[0140] Generally, water, inorganic acids, free organic acids, etc. volatilize almost entirely at temperatures below 200°C.

[0141] The titania nanoparticles constituting the metal nanoparticle (platinum nanoparticle)-supporting titania nanoparticles of the present invention have acyloxy groups bonded to at least some of the titanium atoms present on the surface, and therefore the acyloxy groups are gradually eliminated in the range of 200° C. to 600° C. For example, in the case of acetoxy groups, the acetoxy groups are gradually eliminated in the range of 200° C. to 600° C., with a peak at about 260° C.

[0142] The titania nanoparticles constituting the titania nanoparticles supporting metal nanoparticles (platinum nanoparticles) of the present invention have acyloxy groups bonded to at least some of the titanium atoms present on the surface, and therefore, aggregation of the titania nanoparticles with each other during drying or firing can be suppressed, making cracks, peeling, and the like less likely to occur. As a result, the titania nanoparticles are particularly excellent in coatability and transparency, and cracks, peeling, and the like can be suppressed. Furthermore, as a result of easily firmly supporting the metal nanoparticles described below, the visible light catalytic activity is also excellent.

[0143] It is generally known in the art that the presence of acyloxy groups on the surface generally reduces the visible light catalytic activity.

[0144] In the present invention, the aggregation of titania nanoparticles during drying or calcination can be suppressed, and therefore the effect of suppressing cracks, peeling, etc. is particularly excellent. In addition, since metal nanoparticles (platinum nanoparticles) can be easily and firmly supported, visible light catalytic activity can also be improved despite the presence of acyloxy groups.

[0145] Titania nanoparticles preferably have a large number of acyloxy groups bonded to titanium atoms present on the surface. When acyloxy groups are present on at least some of the titanium atoms present on the surface, they are gradually released in the range of 200°C to 600°C, and therefore, when the temperature is increased using a thermogravimetric and differential thermal analyzer (TG-DTA), the mass loss is large at temperatures above 200°C.

[0146] In the present invention, when the temperature is increased using a thermogravimetry-differential thermal analyzer (TG-DTA), the mass loss at 200°C or higher represents an index of the number of acetoxy groups bonded to titanium atoms present on the surface.

[0147] When heated to 600° C. using a thermogravimetry and differential thermal analyzer (TG-DTA), the mass loss at 200° C. or higher is 5% by mass or more, preferably 7% by mass to 20% by mass. The detailed conditions for the thermogravimetry and differential thermal analyzer (TG-DTA) are as follows: atmosphere: air, heating rate: 3° C. / min.

[0148] Titania nanoparticles have acyloxy groups bonded to at least some of the titanium atoms present on the surface, and these acyloxy groups are preferably bonded to the titanium atoms via a group represented by -OCOR (wherein R represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a hydroxyalkyl group having 1 to 2 carbon atoms).The acyloxy group is preferably an acyloxy group derived from an organic acid such as a monocarboxylic acid having 1 to 4 carbon atoms or a hydroxycarboxylic acid having 2 to 3 carbon atoms.

[0149] In the above R, preferred examples of the alkyl group include a methyl group, an ethyl group, and an n-propyl group.

[0150] In the above R, preferred examples of the hydroxyalkyl group include a hydroxymethyl group, a 1-hydroxyethyl group, and a 2-hydroxyethyl group.

[0151] Preferred examples of the monocarboxylic acid include formic acid, acetic acid, propionic acid, and butyric acid. Preferred examples of the hydroxycarboxylic acid include glycolic acid and lactic acid.

[0152] From the viewpoints of volatility, harmfulness and decomposability, R is preferably a hydrogen atom, or a methyl group, a hydroxymethyl group, a 1-hydroxyethyl group, a 2-hydroxyethyl group, or the like, and from the viewpoints of water solubility and odor, a methyl group is preferred.

[0153] From the viewpoints of volatility, harmfulness and decomposability, the monocarboxylic acid is preferably formic acid, acetic acid, etc., and the hydroxycarboxylic acid is preferably glycolic acid, lactic acid, etc.

[0154] Acetic acid is particularly preferred from the viewpoints of water solubility and odor.

[0155] The organic acids can be used alone or in combination of two or more kinds.

[0156] In conventional titania dispersions, a uniform dispersion could not be obtained unless a dispersant was used. Therefore, in the present invention, a dispersant may be added, but even without adding a dispersant, a dispersion with far better dispersibility than that of ordinary titania nanoparticles can be obtained.

[0157] The good dispersibility results in excellent crack resistance of the coating, and the absence of the need for a dispersant makes it possible to produce a dense titania coating.

[0158] In the titania dispersion of the present invention, the content of water as a solvent is preferably 60% by weight or more, particularly preferably 75% by weight or more, from the viewpoints of ease of coating and film properties of the coating.

[0159] It is also possible to take out titania nanoparticles from the reaction solution and change the solvent. Water may be removed from the reaction solution by centrifugation or a filtration membrane, and replaced with an organic solvent. In this case, it is preferable not to dry the titania nanoparticles from the viewpoints of dispersibility, transparency, etc.

[0160] Examples of the organic solvent used in the dispersion include alcohols, etc. Examples of the alcohols include aliphatic alcohols having 1 to 6 carbon atoms, such as methanol, ethanol, and isopropanol, as well as non-aliphatic alcohols, such as α-terpineol, glycol solvents, such as butyl carbitol (diethylene glycol monobutyl ether), hexylene glycol (2-methyl-2,4-pentanediol), ethylene glycol-2-ethylhexyl ether, ethylene glycol monomethyl ether, and propylene glycol monomethyl ether, and diols, such as 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol.

[0161] The organic solvent used in the dispersion may not have an OH group, as long as it has affinity with titania and other solvents (water, alcohol, etc.), and examples of the organic solvent include diethylene glycol butyl methyl ether, tripropylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol dibutyl ether, triethylene glycol butyl methyl ether, tetraethylene glycol dimethyl ether, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol diacetate, triethylene glycol diacetate, tetraethylene glycol diacetate, etc. Among these, diethylene glycol monobutyl ether acetate, tetraethylene glycol dimethyl ether, etc. are preferred from the viewpoint of boiling point, etc.

[0162] (4) Other additives The viscosity of the platinum nanoparticles of the present invention is preferably adjusted to improve uniformity during synthesis or according to the application during use. For example, when used for spin coating, dip coating, spraying, etc., the viscosity is adjusted to a low value, when used for brush coating, squeegee method, etc., the viscosity is adjusted to a higher value, and when used for screen printing, the viscosity is adjusted to an even higher value to suppress fluidity.

[0163] For example, from the viewpoint of being less likely to inhibit catalytic activity, metal oxides other than silica and titania, or water-soluble cellulose derivatives are mentioned.

[0164] Examples of the water-soluble cellulose derivatives include sodium carboxymethylcellulose, ammonium carboxymethylcellulose, hydroxypropylcellulose, hydroxyethylcellulose, hydroxypropylmethylcellulose, hydroxypropylethylcellulose, and methylcellulose.

[0165] 2. Photocatalysts, antibacterial materials, antiviral materials, and antiviral coating solutions The photocatalyst of the present invention is Platinum nanoparticles, titania nanoparticles, and General formula (1): HSi(R1 )(R 2 )(R 3 ) (1) (In the formula, R 1 , R 2 , and R 3 are the same or different and each represents an alkyl group, an alkoxy group, a hydrogen atom, a hydroxyl group, an acyloxy group, a halogen atom, or an -O-Si bond. The silicon compound represented by the formula: Specific surface area is 150m 2 / g~500m 2 / g.

[0166] The antibacterial and / or antiviral material of the present invention comprises: Platinum nanoparticles, titania nanoparticles, and General formula (1): HSi(R 1 )(R 2 )(R 3 ) (1) (In the formula, R 1 , R 2 , and R 3 are the same or different and each represents an alkyl group, an alkoxy group, a hydrogen atom, a hydroxyl group, an acyloxy group, a halogen atom, or an -O-Si bond. The silicon compound represented by the formula: Specific surface area is 150m 2 / g~500m 2 / g, It has antibacterial and / or antiviral activity in visible light or in the dark.

[0167] The antiviral coating liquid of the present invention contains the antibacterial and / or antiviral material and water.

[0168] The viscosity of the antiviral coating liquid of the present invention is adjusted depending on the application. For example, when it is used for spin coating, dip coating, spraying, or the like, it is adjusted to a low viscosity.

[0169] When the antiviral coating liquid of the present invention is used for brush application, squeegee method, or the like, the viscosity is adjusted to be higher.

[0170] When the antiviral coating liquid of the present invention is used for screen printing, it is preferable to adjust the viscosity to be higher and suppress the fluidity.

[0171] The coating of the present invention is a dense coating. EXAMPLES

[0172] The present invention will now be described in detail with reference to examples.

[0173] The present invention is not limited to these.

[0174] [Example 1] Water was added to 2.655 g of chloroplatinic (VI) acid hexahydrate to make up to 100 g (1 g of Pt atoms dissolved in 100 g).

[0175] When 5 g of this solution, 5 g of a 10 wt % solution of hydroxypropyl cellulose, 35.75 g of water, and 3 g of acetic acid were mixed at room temperature (25° C.), a pale yellow solution was obtained.

[0176] 1.25 g of HSi(OEt)3 was added to this solution and stirred. Within 30 minutes, the liquid turned dark brown and the formation of platinum nanoparticles was confirmed, so stirring was stopped.

[0177] [Example 2] 120 g (2 mol) of acetic acid was added to 142.1 g (0.5 mol) of titanium tetraisopropoxide and stirred for 15 minutes, and then 550 g of water was added. The pH of this dispersion was 2.5.

[0178] A large amount of translucent precipitate was generated, but after stirring for 60 minutes and heating at 60°C, the precipitate was completely dissolved.

[0179] Thereafter, the reaction solution was stirred at normal pressure (0.1 MPa) at 80° C. for 5 hours, and then water was added to the reaction solution to adjust the total weight to 800 g.

[0180] By applying ultrasonic waves, a semi-transparent uniform titania dispersion was obtained without using a strong inorganic acid.

[0181] 500 g of water was added to 500 g of the titania dispersion to make up to 1,000 g.

[0182] Water was added to 2.655 g of chloroplatinic (VI) acid hexahydrate to make up to 100 g (1 g of Pt atom dissolved in 100 g), and 75 g was added per 1,000 g of the titania dispersion.

[0183] Furthermore, 60 g of HSi(OEt)3 was added and stirred, and the liquid immediately turned dark gray, forming a composite of platinum nanoparticles and titania.

[0184] [Example 3] The experiment was carried out in the same manner as in Example 2, except that 6.0 g of HSi(OEt)3 was added.

[0185] After 20 minutes, the liquid turned dark gray, indicating that a composite of platinum nanoparticles and titania had formed.

[0186] [Example 4] The experiment was carried out in the same manner as in Example 2, except that 50 g of chloroplatinic (VI) acid hexahydrate solution and 4.0 g of HSi(OEt)3 were added.

[0187] After 30 minutes, the color turned dark gray, indicating that a composite of platinum nanoparticles and titania was formed.

[0188] [Example 5] The experiment was carried out in the same manner as in Example 2, except that 25 g of chloroplatinic (VI) acid hexahydrate solution and 2.0 g of HSi(OEt)3 were added.

[0189] After 30 minutes, the color turned dark gray, indicating that a composite of platinum nanoparticles and titania was formed.

[0190] Figures 1 to 5 1 shows a TEM image of Example 5. It can be seen that Pt particles of about 5 nm (black particles in the center) are generated in titania primary particles of 3 nm to 5 nm.

[0191] Figure 2 shows a TEM image of Example 5. It can be seen that Pt particles of about 3 nm (black particles in the center) were produced.

[0192] Figure 3 shows a TEM image of Example 5. Particle A, approximately 4 nm in size, is a Pt nanoparticle, and overlapping particle B is a TiO2 nanoparticle.

[0193] Figure 4 shows the TEM-EDS spectrum of particle A in Figure 3. Although some Ti was detected, Pt was the main component.

[0194] Fig. 5 shows the peaks of particle B in Fig. 3. Although a small amount of Pt was detected, Ti and O were mainly detected.

[0195] [Example 6] The experiment was carried out in the same manner as in Example 2, except that 12.5 g of chloroplatinic (VI) acid hexahydrate solution and 1.0 g of HSi(OEt)3 were added.

[0196] After 60 minutes, the color turned dark gray, indicating that a composite of platinum nanoparticles and titania was formed.

[0197] The solutions obtained in Examples 3 to 6 were spin-coated three times on a 50 mm square glass substrate at 1,000 rpm for 60 seconds to obtain a transparent coating film.

[0198] The antiviral properties of this test piece were evaluated according to a method in accordance with JIS R 1756 (conditions: visible light illuminance 2,000 Lx x 7 hours).

[0199] As a result, the antiviral activity value was 5.3 or higher (inactivation of 99.9995% or more), confirming high antiviral properties.

[0200] In addition, when the antiviral activity was evaluated in a dark place, the antiviral activity value was 5.0 or higher (99.999% or more inactivated), confirming high antiviral activity.

[0201] [Comparative Example 1] The experiment was carried out in the same manner as in Example 6, except that HSi(OEt)3 was not added.

[0202] Even after stirring for 24 hours, no change was observed in the solution, it remained pale yellow, and no platinum nanoparticles were produced.

[0203] [Comparative Example 2] The experiment was carried out in the same manner as in Example 6, except that HSi(OEt)3 was not added and the mixture was heated to 80°C.

[0204] Even after stirring for 10 hours, no change was observed in the solution, it remained pale yellow, and platinum nanoparticles were not produced.

[0205] [Comparative Example 3] The experiment was carried out in the same manner as in Example 6, except that 8 g of formic acid was added instead of HSi(OEt)3.

[0206] Even after stirring for 24 hours, no change was observed in the solution, it remained pale yellow, and no platinum nanoparticles were produced.

[0207] There was no change even after heating to 80°C.

[0208] [Comparative Example 4] The experiment was carried out in the same manner as in Example 6, except that 8 g of acetaldehyde was added instead of HSi(OEt)3.

[0209] Even after stirring for 24 hours, no change was observed in the solution, it remained pale yellow, and no platinum nanoparticles were produced.

[0210] There was no change even after heating to 80°C.

[0211] [Comparative Example 5] The experiment was carried out in the same manner as in Example 6, except that 0.4 g of hydroquinone was added instead of HSi(OEt)3.

[0212] Even after stirring for 24 hours, no change was observed in the solution, it remained pale yellow, and no platinum nanoparticles were produced.

[0213] There was no change even after heating to 80°C.

[0214] [Comparative Example 6] The experiment was carried out in the same manner as in Example 6, except that 0.4 g of tannic acid was added instead of HSi(OEt)3.

[0215] Even after stirring for 24 hours, no change was observed in the liquid; it remained orange in color due to tannic acid, and no platinum nanoparticles were produced.

[0216] There was no change even after heating to 80°C.

Claims

1. A method for producing platinum nanoparticles, comprising the steps of: General formula (1): HSi(R 1 )(R 2 )(R 3 ) (1) (In the formula, R 1 , R 2 , and R 3 are the same or different and each represents a methoxy group, an ethoxy group, or an acetoxy group.) A silicon compound represented by the formula: a platinum precursor; Manufacturing method.

2. The platinum precursor is hexachloroplatinic acid (IV) (H 2 PtCl 6 ), and hexachloroplatinic acid (IV) hexahydrate (H 2 PtCl 6 ・6H 2 O) The method of claim 1.

3. The mixing step is carried out using a solvent, The solvent contains 80% by mass or more of water. The method according to claim 1 or 2.

4. The mixing step is carried out using a solvent, The solvent comprises an organic acid. The method according to any one of claims 1 to 3.

5. The organic acid is acetic acid. The method of claim 4.

6. The mixing step is carried out at a reaction temperature of 100° C. or less. The method according to any one of claims 1 to 5.

7. The mixing step is carried out in the presence of titania nanoparticles. The method according to any one of claims 1 to 6.

8. The titania nanoparticles are anatase titania nanoparticles. The method of claim 7.

9. The titania nanoparticles have acyloxy groups bonded to at least some of the titanium atoms present on the surface, The titania nanoparticles have a weight loss of 5% by mass or more at 200°C or higher when heated to 600°C using a thermogravimetric and differential thermal analyzer; The titania nanoparticles are a photocatalyst; The mixing step is carried out in the presence of the photocatalyst. The method according to claim 7 or 8.

10. The titania nanoparticles have an average particle size of 30 nm or less, and the acyloxy group is an acetoxy group. The method of claim 9.

11. The titania nanoparticles have an average particle size of 1 nm to 6 nm and a specific surface area of ​​150 m 2 / g~500m 2 / g, The method according to any one of claims 7 to 10.

12. A photocatalyst comprising: Platinum nanoparticles, titania nanoparticles, and General formula (1): HSi(R 1 )(R 2 )(R 3 ) (1) (In the formula, R 1 , R 2 , and R 3 are the same or different and each represents a methoxy group, an ethoxy group, or an acetoxy group.) The silicon compound represented by the formula: Specific surface area is 150m 2 / g~500m 2 / g, Photocatalyst.

13. An antibacterial or antiviral material, Platinum nanoparticles, titania nanoparticles, and General formula (1): HSi(R 1 )(R 2 )(R 3 ) (1) (In the formula, R 1 , R 2 , and R 3 are the same or different and each represents a methoxy group, an ethoxy group, or an acetoxy group.) The silicon compound represented by the formula: Specific surface area is 150m 2 / g~500m 2 / g, An antimicrobial material that has antimicrobial activity under visible light or in the dark, or An antiviral material that has antiviral activity under visible light or in the dark.

14. An antiviral coating solution, The antiviral material according to claim 13, and Contains water Antiviral coating liquid.

Citation Information

Patent Citations

  • SiO2-precious metal nano composite material of core-shell structure and preparation method of SiO2-precious metal nano composite material

    CN111141726A

  • Metal colloid particle, metal colloid, and use of metal colloid

    JP2006124826A

  • Composition containing metal fine particle and inorganic fine particle and method for producing the same

    JP2006307084A

  • Platinum-carrying titanium oxide carrier

    JP2012214373A

  • Electrostatic Coating with Metallic Nanoparticles by Intrinsic Particle to Surface Interaction

    US20150194242A1