Display device and manufacturing method thereof

The use of an undercut structure with a double layer of fluoropolymer material and photoresist pattern addresses the mask sagging issue in FMM, enabling finer sub-pixel patterns on large-area panels, thus improving image quality and reliability in organic light emitting display devices.

JP7581311B2Active Publication Date: 2024-11-12LG DISPLAY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022207747
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-28
Filing Date
2022-12-26
Publication Date
2024-11-12
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

Existing organic light emitting display devices face challenges in forming fine sub-pixel patterns on large-area panels due to mask sagging issues with fine metal masks (FMM), limiting their application to smaller panels and hindering improved image quality.

Method used

A display device utilizing a patterning method with an undercut structure consisting of a double layer, specifically using a fluoropolymer material for the protective layer and photoresist pattern, allows for the formation of finer sub-pixel patterns even on large-area panels, reducing leakage current and preventing damage to the organic material.

Benefits of technology

The method enables the formation of finer sub-pixel patterns, enhances image quality, and improves the reliability and performance of large-area organic light emitting display devices by reducing leakage current and preventing organic material damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581311000001
    Figure 0007581311000001
  • Figure 0007581311000002
    Figure 0007581311000002
  • Figure 0007581311000003
    Figure 0007581311000003
Patent Text Reader

Abstract

To improve a quality of a video image.SOLUTION: A display device according to a present specification, contains: a substrate in which a plurality of pixels containing a plurality of sub-pixels is arranged; a first electrode that is arranged in each sub-pixel, and is connected to a transistor for emitting a light by driving the plurality of sub-pixels; and a bank that divides a light emission region of the plurality of sub-pixels, and contains a bank hole exposing one part of the first electrode. Each of the plurality of sub-pixels is arranged at a bottom surface of a bank hole and is contacted to a front surface of which the first electrode is exposed, and contains a sub-pixel pattern continuously extended along a side wall of the bank hole and an upper front surface of an upper outer side edge of the bank. A thickness of the sub-pixel pattern is gradually reduced along the upper front surface of the upper outer side edge of the bank while being extended to a direction directed to the sub-pixel to which the sub-pixel pattern is adjacent.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a display device, and more particularly to a display device in which an organic light-emitting layer can be formed using an undercut structure made of a double layer, and a method for manufacturing the same. [Background technology]

[0002] An organic light emitting display is a self-emissive device in which the device itself is a light emitter, and the time required for converting an electrical signal into light is short, and the generated light spreads uniformly without directionality. Organic light emitting display devices have the advantages of excellent color realization, viewing angle, and light-dark contrast ratio, as well as fast response speed, making it possible to manufacture display devices that realize high-quality moving images. In addition, organic light emitting display devices have a thin overall thickness, and in particular, it is possible to manufacture display devices that are thinner than liquid crystal displays (LCDs) and plasma display panels (PDPs), and so they are being developed as next-generation displays with large areas and high quality.

[0003] The organic material that is the light-emitting body of these organic light-emitting display devices is formed in each sub-pixel on a substrate using a fine metal mask (FMM). However, due to the thinness of the fine metal mask, a drooping phenomenon occurs in the center of the mask, which makes it difficult to apply to large-area panels, although it is possible to manufacture small and medium-sized panels. Summary of the Invention [Problem to be solved by the invention]

[0004] In a display device, a plurality of sub-pixel patterns are arranged in a matrix, and in order to form these sub-pixel patterns, a method of forming a white light-emitting layer using a fine metal mask (FMM) or an open mask is used. However, fine metal masks (FMMs) are difficult to apply to large-area panels due to the mask sagging phenomenon, and are also difficult to form fine patterns.

[0005] As the demand for panels having a large area increases and the need to form sub-pixel patterns in fine patterns to improve image quality increases, research is being conducted into methods for forming sub-pixel patterns.

[0006] The present specification is intended to solve the above-mentioned problems, and aims to provide a display device including a sub-pixel pattern formed by a patterning method using an undercut structure consisting of a double layer, and a manufacturing method thereof.

[0007] In addition, the present invention aims to realize a finer pattern than that formed using a fine metal mask (FMM) by forming a sub-pixel pattern using a patterning method that uses a double-layer undercut structure.

[0008] Another object of the present invention is to form sub-pixel patterns in large area panels by using a patterning method using a double-layer undercut structure.

[0009] The object of the present specification is not limited to the above-mentioned objects, and other objects not mentioned herein will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]

[0010] A display device according to an embodiment of the present specification includes a substrate on which a plurality of pixels, each of which includes a plurality of subpixels, are disposed; a first electrode disposed in each of the subpixels and connected to a transistor for driving the plurality of subpixels to emit light; and a bank including a bank hole that divides light-emitting regions of the plurality of subpixels and exposes a portion of the first electrode, each of the subpixels including a subpixel pattern disposed on a bottom surface of the bank hole, in contact with an exposed surface of the first electrode, and extending continuously along a sidewall of the bank hole and an upper surface of an upper outer edge of the bank, the thickness of the subpixel pattern decreasing stepwise as the subpixel pattern extends along the upper surface of the upper outer edge of the bank in a direction toward an adjacent subpixel.

[0011] A display device according to another embodiment of the present specification includes a substrate on which a plurality of pixels are disposed, each of the pixels including a plurality of subpixels; a first electrode disposed in each of the subpixels and connected to a transistor for driving the plurality of subpixels to emit light; and a bank including a bank hole that divides light-emitting regions of the plurality of subpixels and exposes a portion of the first electrode, each of the subpixels including a subpixel pattern disposed on a bottom surface of the bank hole, in contact with an exposed surface of the first electrode, and extending continuously along a sidewall of the bank hole and an upper surface of an upper outer edge of the bank, each of the subpixel patterns extending continuously along the upper surface of the outer edge of the bank and terminating in a tail portion away from the substrate.

[0012] According to yet another embodiment of the present disclosure, a method for manufacturing a display device includes the steps of: forming a first electrode electrically connected to a thin film transistor on a substrate; forming a bank having a bank hole exposing the first electrode; forming a protective layer on the bank; forming a photoresist pattern exposing a portion of a surface of the protective layer; removing the protective layer to form an undercut structure consisting of a double layer of the protective layer pattern and the photoresist pattern while forming an undercut region under the photoresist pattern; forming a subpixel pattern on a sidewall of the bank hole, the subpixel pattern being located at a bottom surface of the bank hole, contacting an exposed surface of the first electrode, and extending continuously into the undercut region along a surface of an upper outer edge of the bank, removing the undercut structure; and forming a second electrode located on the subpixel pattern. Effect of the Invention

[0013] According to the embodiments of the present specification, by forming a sub-pixel pattern by a patterning method using an undercut structure made of a double layer, it is possible to realize a finer pattern than when a sub-pixel pattern is formed using a fine metal mask (FMM).

[0014] In addition, by using an undercut structure consisting of a double layer of a protective layer pattern made of a fluoropolymer material and a photoresist pattern, and a lift-off method, a plurality of sub-pixel patterns can be easily formed even in a large area panel.

[0015] In addition, by using a patterning method using an undercut structure consisting of a double layer of a protective layer pattern made of a fluoropolymer material and a photoresist pattern, damage to the organic material constituting the sub-pixel pattern can be prevented, which has the advantage of improving the performance and reliability of the display device.

[0016] In addition, by introducing an undercut structure consisting of a double layer of a protective layer pattern made of a fluoropolymer material and a photoresist pattern, it is possible to advantageously adjust the depth of the undercut region in order to control the shape of the sub-pixel pattern.

[0017] Furthermore, by forming the sub-pixel pattern using a patterning method using an undercut structure, the thickness of the sub-pixel pattern becomes thinner toward the outer periphery of the sub-pixel pattern, thereby reducing leakage current.

[0018] Incidentally, according to the embodiment of the present specification, in a patterning process using an undercut structure, by controlling the depth of the undercut region and deforming the shape of the sub-pixel pattern, it is possible to disconnect the charge generation layer in the organic light-emitting layer of a tandem structure that emits white light, which has an advantage of preventing the occurrence of leakage current. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is a plan view showing a schematic view of a display area of ​​the display device. [Diagram 2] FIG. 2 is a cross-sectional view taken along the II' direction in FIG. [Diagram 3] FIG. 2 is a diagram for explaining one sub-pixel pattern. [Figure 4] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Diagram 5] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 6] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 7] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 8] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 9]1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 10] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 11] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 12] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 13] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 14] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 15] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 16] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 17] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 18] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 19] 1 is a diagram illustrating an organic light emitting display device according to a first embodiment of the present specification; [Figure 20] FIG. 4 is a diagram illustrating an organic light emitting display device according to a second embodiment of the present specification. [Figure 21] FIG. 4 is a diagram illustrating an organic light emitting display device according to a second embodiment of the present specification. [Figure 22] FIG. 4 is a diagram illustrating an organic light emitting display device according to a second embodiment of the present specification. [Figure 23] FIG. 4 is a diagram illustrating an organic light emitting display device according to a second embodiment of the present specification. [Figure 24] FIG. 4 is a diagram illustrating an organic light emitting display device according to a second embodiment of the present specification. [Diagram 25]FIG. 4 is a diagram illustrating an organic light emitting display device according to a second embodiment of the present specification. [Figure 26] FIG. 4 is a diagram illustrating an organic light emitting display device according to a second embodiment of the present specification. [Figure 27] FIG. 4 is a diagram illustrating an organic light emitting display device according to a second embodiment of the present specification. [Figure 28a] FIG. 11 is a diagram for explaining defects caused by adjusting the depth of the undercut region in the second embodiment of the present specification. [Figure 28b] FIG. 11 is a diagram for explaining defects caused by adjusting the depth of the undercut region in the second embodiment of the present specification. [Figure 28c] FIG. 11 is a diagram for explaining defects caused by adjusting the depth of the undercut region in the second embodiment of the present specification. [Figure 29] FIG. 11 is a diagram shown for explaining a third embodiment of the present specification. [Diagram 30] FIG. 11 is a diagram shown for explaining a third embodiment of the present specification. [Diagram 31] FIG. 11 is a diagram shown for explaining a third embodiment of the present specification. [Diagram 32] FIG. 11 is a diagram shown for explaining a third embodiment of the present specification. [Diagram 33] FIG. 11 is a diagram shown for explaining a third embodiment of the present specification. [Diagram 34] FIG. 11 is a diagram shown for explaining a third embodiment of the present specification. [Diagram 35] FIG. 11 is a diagram shown for explaining a third embodiment of the present specification. [Diagram 36] FIG. 11 is a diagram shown for explaining a third embodiment of the present specification. [Figure 37] FIG. 11 is a diagram illustrating an organic light emitting display device according to a fourth embodiment of the present specification. [Figure 38] FIG. 11 is a diagram illustrating an organic light emitting display device according to a fourth embodiment of the present specification. [Figure 39] FIG. 11 is a diagram illustrating an organic light emitting display device according to a fourth embodiment of the present specification. [Diagram 40]FIG. 11 is a diagram illustrating an organic light emitting display device according to a fourth embodiment of the present specification. [Diagram 41] FIG. 11 is a diagram illustrating an organic light emitting display device according to a fourth embodiment of the present specification. [Diagram 42] FIG. 11 is a diagram illustrating an organic light emitting display device according to a fourth embodiment of the present specification. [Diagram 43] FIG. 11 is a diagram illustrating an organic light emitting display device according to a fourth embodiment of the present specification. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The advantages and features of the present specification, and the methods for achieving them, will become clear from the detailed description of the embodiments described below in conjunction with the accompanying drawings. However, the present specification is not limited to the embodiments disclosed below, and may be configured in various different forms. However, the present embodiments are provided to complete the disclosure of the specification and to fully inform those skilled in the art of the present specification of the scope of the invention.

[0021] The shapes, sizes, ratios, angles, numbers, etc. disclosed in the drawings to explain the embodiments of this specification are illustrative, and this specification is not limited to the matters shown. The same reference symbols throughout the specification refer to the same components. In addition, in explaining this specification, if a specific description of related publicly known technology is deemed to make the gist of this specification unclear, the detailed description will be omitted. When "includes," "has," "is," etc. are used in this specification, other parts may be added unless "only" is used. When a component is expressed in the singular, it also includes a case where it includes a plural, unless otherwise explicitly stated.

[0022] When interpreting elements, they are interpreted as including a range of error, even if there is no explicit statement to the contrary.

[0023] When describing a positional relationship between two parts, for example, using "on", "at the top", "below", "to the side", etc., one or more other parts may be located between the two parts, unless "immediately" or "directly" is used.

[0024] When describing a temporal relationship, for example, when using "after", "following", "next to", "before", etc., non-consecutive cases can also be included, unless "immediately" or "directly" is used.

[0025] Although the terms "first", "second", etc. are used to describe various components, these components are not limited by these terms. These terms are used merely to distinguish one component from another. Thus, the first component referred to below may be the second component within the technical concept of this specification.

[0026] The phrase "substantial amount of fluorine" in embodiments herein can mean that the number of fluorine atoms is 50% or more, or up to 60%, 70%, 80%, or 90% or more of the total number of atoms in a molecule, polymer, substance, or functional group.

[0027] The individual features of the embodiments of this specification may be partially or wholly combined or combined with each other, may be technically interlocked and driven in various ways, and each embodiment may be implemented independently of each other, or may be implemented together in a linked relationship.

[0028] Hereinafter, a display device formed using a double-layer undercut structure and a manufacturing method thereof according to an embodiment of the present disclosure will be described with reference to the drawings.

[0029] Fig. 1 is a plan view showing a schematic display area of ​​a display device, Fig. 2 is a cross-sectional view taken along the II' direction of Fig. 1, and Fig. 3 is a diagram for explaining one pixel pattern.

[0030] 1 to 3, a display area (AA) of the display device is an area for displaying an image and includes a plurality of pixels (PX). The plurality of pixels (PX, pixels) are arranged in a matrix (PX1 to PX2) along a first direction (X) and a second direction (Y) intersecting the first direction (X) on the display area (AA; active area). m , P.X. n , m and n are natural numbers). Each pixel (PX) includes a plurality of sub-pixels (SP). A sub-pixel (SP) is a basic color element that actually emits light, and can be understood as the smallest light-emitting unit area. Each sub-pixel (SP) can include an organic light-emitting element that is a self-emitting element, and a thin-film transistor (TR) for driving the organic light-emitting element.

[0031] In one example, referring to an enlarged portion of one pixel (PX) in FIG. 1, adjacent sub-pixels (SP) may configure one pixel (PX) including a first sub-pixel (SP_1), a second sub-pixel (SP_2), a third sub-pixel (SP_3), and an auxiliary electrode pixel (SUB_E). Here, when the display area (AA) displays a color image, the first sub-pixel (SP_1), the second sub-pixel (SP_2), and the third sub-pixel (SP_3) may emit light of a wavelength region corresponding to one of a plurality of different hues. Here, the plurality of hues may include red, green, and blue. Or, the plurality of hues may further include white.

[0032] The auxiliary electrode pixel (SUB_E) may be disposed in each of the pixels (PX) to prevent imbalance in the driving voltage. The wiring for applying the driving voltage to the pixel (PX) is disposed in a non-display area located on the outer edge of the display area (AA). For this reason, the driving voltage may be applied unbalanced due to the generation of a separation distance between the pixels (PX) arranged in a matrix and the wiring disposed in the non-display area, and a defect in which the brightness varies depending on the position of the pixel (PX) may occur. In order to prevent the brightness variation due to the imbalance in the driving voltage, the auxiliary electrode pixel (SUB_E) may be included in each pixel (PX). The auxiliary electrode pixel (SUB_E) may be configured so that the second electrode 190 and the first electrode 122 are in direct contact with each other as shown in FIG. 2. The auxiliary electrode pixel (SUB_E) may be disposed on the display area (AA) to have a mesh shape in a plan view. In FIG. 2, the first electrode 122 of the auxiliary electrode pixel (SUB_E) is connected to the thin film transistor (TR) in the display area (AA), but this is not limited to this and the first electrode 122 of the auxiliary electrode pixel (SUB_E) does not have to be connected to the thin film transistor (TR) in the display area (AA).

[0033] Further referring to FIG. 2, the display device according to an embodiment of the present specification may include, on the substrate 100, a light-blocking layer 102, a buffer layer 104, a thin film transistor (TR), an interlayer insulating film 112, a planarization film 116, a first electrode 122, a bank 124, a plurality of pixel patterns 145a, 165a, 185a, a second electrode 190, and an encapsulation layer 197.

[0034] The light blocking layer 102 is disposed on the substrate 100 so as to overlap the thin film transistor (TR), and the buffer layer 104 is positioned so as to cover the light blocking layer 102. The thin film transistor (TR) is disposed on the buffer layer 104. The thin film transistor (TR) may include an active region 106, a gate electrode 110, a source electrode 114, and a drain electrode 115. The active region 106 includes a source region (SA) and a drain region (DA) disposed with a channel region (CH) overlapping with the gate electrode 110 therebetween. The gate electrode 110 is disposed on the active region 106 with a gate insulating film 108 interposed therebetween.

[0035] The interlayer insulating film 112 may include a first contact hole 113 that covers the entire active region 106 and the gate electrode 110 and exposes a part of the surface of the active region 106. A source electrode 114 and a drain electrode 115 may be disposed to contact the source region (SA) and the drain region (DA) through the first contact hole 113, respectively.

[0036] A planarization film 116 including a second contact hole 120 exposing a portion of a surface of the drain electrode 115 may be disposed on the interlayer insulating film 112. A first electrode 122 may be disposed on the planarization film 116, and the first electrode 122 may be in contact with the drain electrode 115 exposed through the second contact hole 120 and electrically connected to the gate electrode 110. The first electrode 122 may also be referred to as an anode electrode or a pixel electrode. The first electrode 122 may be disposed on each of a plurality of sub-pixels (SP-1, SP-2, SP-3).

[0037] A plurality of banks 124 are disposed on the planarization film 116 to define light-emitting regions of the plurality of sub-pixels (SP-1, SP-2, SP-3) and to separate the sub-pixels (SP-1, SP-2, SP-3) from one another. A bank hole 125 formed in the bank 124 may expose a portion of the surface of the first electrode 122 of each of the sub-pixels (SP-1, SP-2, SP-3).

[0038] The sub-pixel patterns 145a, 165a, and 185a are disposed on the exposed surfaces of the first electrodes 122 of the plurality of sub-pixels (SP-1, SP-2, and SP-3) and on the sidewalls and top surface of the bank 124. The sub-pixel patterns 145a, 165a, and 185a may include a first sub-pixel pattern 145a disposed in the first sub-pixel (SP-1), a second sub-pixel pattern 165a disposed in the second sub-pixel (SP-2), and a third sub-pixel pattern 185a disposed in the third sub-pixel (SP-3). Here, the first to third sub-pixel patterns 145a to 185a may each emit light in a wavelength region corresponding to one of red, green, and blue hues, but are not limited thereto.

[0039] 3, the first to third subpixel patterns 145a to 185a may have a rectangular shape including a edge portion (BD) and a trench portion (TC) disposed inward of the edge portion (BD) in a plan view. The edge portion (BD) of the first subpixel may be located on the top surface of the bank 124, and the trench portion (TC) may be located inside the edge portion (BD) and overlap with the bank hole 125 disposed between the adjacent banks 124. Although only the first subpixel pattern 145a is shown in FIG. 3 for the sake of explanation, the second subpixel pattern 165a and the third subpixel pattern 185a may also have the same shape.

[0040] Also, each of the sub-pixel patterns 145a, 165a, and 185a may be formed to have a thickness (th1, th2, th3) ​​that increases toward the bank hole 125. In other words, each of the sub-pixel patterns 145a, 165a, and 185a may be formed to have a thickness that decreases toward the adjacent sub-pixel pattern while covering the trench portion (TC) defined by the bank hole 125 and extending toward the upper surface of the bank 124. Thus, the sub-pixel patterns 145a, 165a, and 185a may have a first thickness (th1) that is the thickest at the edge portion (BD) connected to the trench portion (TC) and a third thickness (th3) that is the thinnest at the outermost portion of the edge portion (BD).

[0041] The edge (BD) of each of these sub-pixel patterns 145a, 165a, and 185a has a shape in which rings are repeatedly arranged in the direction of the adjacent sub-pixel patterns in a plan view. The rings may have a stepped shape by being formed so that they become thinner in the direction of the adjacent sub-pixel patterns.

[0042] In this way, the thickness of the edge (BD) of the sub-pixel patterns 145a, 165a, and 185a becomes thinner toward the outer periphery, so that the leakage current can be reduced. In one example, the thinnest third thickness (th3) formed at the outermost portion of the edge (BD) has a thin thickness that makes it difficult for charges to move, so that the leakage current can be reduced. In addition, the edge (BD) of each of the sub-pixel patterns 145a, 165a, and 185a has a stepped shape in which rings are repeatedly arranged in a plan view, so that stepped portions where the resistance increases rapidly are repeatedly arranged, so that the leakage current can be further effectively reduced.

[0043] A second electrode 190 may be disposed on the bank 124, which is in common contact with the first subpixel pattern 145a, the second subpixel pattern 165a, and the third subpixel pattern 185a. The second electrode 190 may also be referred to as a cathode electrode, and supplies electrons to the individual subpixel patterns 145a, 165a, and 185a. In one example, the second electrode 190 may be in direct contact with the first electrode 122 on the auxiliary electrode pixel (SUB_E) to form an auxiliary electrode 195. This allows the first subpixel pattern 145a, the second subpixel pattern 165a, the third subpixel pattern 185a, and the auxiliary electrode 195 to form one group.

[0044] An encapsulation layer 197 may be disposed on the second electrode 190. The encapsulation layer 197 serves to improve the reliability of the display device by blocking the penetration of moisture or oxygen from the outside. To this end, the encapsulation layer 197 may be formed as a single layer of at least one inorganic film or organic film, or a multi-layer in which inorganic films and organic films are stacked.

[0045] The subpixel pattern arranged on the display device according to the first embodiment of the present specification may include a rectangular shape including a trench portion at the edge and inside when viewed from above. Also, each subpixel pattern may be formed to have an increasingly thicker thickness toward the bank hole. In other words, each subpixel pattern may be formed to have an increasingly thinner thickness extending from the exposed surface of the bank hole to the upper surface of the bank toward the outer periphery where the adjacent other subpixel patterns are arranged. In this way, the leakage current may be reduced by having an increasingly thinner thickness toward the outer periphery of the subpixel pattern.

[0046] Methods of manufacture according to embodiments herein will be described with reference to the following drawings.

[0047] 4 to 19 are views for explaining a method for manufacturing an organic light emitting display device according to the first embodiment of the present specification. Here, Fig. 4 to Fig. 19 are cut along the II' direction of Fig. 1, and therefore, description thereof will be omitted below.

[0048] 4, a light blocking layer 102 is formed on a substrate 100, and a buffer layer 104 is formed on the light blocking layer 102 to cover the front surface of the substrate 100. The substrate 100 may be a light-transmitting substrate. The substrate 100 may be made of a hard material such as glass or tempered glass, or a flexible material such as a plastic material, but is not limited thereto.

[0049] The light-blocking layer 102 is disposed to overlap the active region 106 located thereover to protect the thin film transistor (Tr) from external light and prevent an off current from being generated in the thin film transistor (TR).

[0050] The buffer layer 104 protects the thin film transistor (TR) from ions or impurities by blocking the penetration of moisture or oxygen from the substrate 100 toward the organic light emitting element above. The buffer layer 104 also plays a role in insulating the light blocking layer 102. The buffer layer 104 may be formed as a single layer of an inorganic insulating film or an organic insulating film including silicon oxide (SiOx), silicon nitride (SiNx), or silicon oxynitride (SiON), or may be formed as a multilayer structure of an inorganic insulating film and an organic insulating film.

[0051] A thin film transistor (TR) may be disposed on the buffer layer 104. The thin film transistor (TR) in the first embodiment of the present specification may include an active region 106, a gate electrode 110, a source electrode 114, and a drain electrode 115. The gate electrode 110 is positioned to overlap a channel region (CH) of the active region 106. A gate insulating film 108 is disposed between the gate electrode 110 and the channel region (CH) of the active region 106. The gate electrode 110 may be made of any one of the group consisting of molybdenum (Mo), aluminum (Al), chromium (Cr), gold (Au), titanium (Ti), nickel (Ni), neodymium (Nd), or copper (Cu), or an alloy thereof.

[0052] The active region 106 includes a source region (SA) and a drain region (DA) that face each other with a channel region (CH) interposed therebetween. The active region 106 may be formed of at least one of amorphous silicon, polycrystalline silicon, and an oxide semiconductor.

[0053] An interlayer insulating film 112 may be formed on the thin film transistor (TR). The interlayer insulating film 112 may be formed over the entire surface of the substrate 100 including the gate electrode 110 and the active region 106, and may be formed to a thickness that covers the entire upper surface of the gate electrode 110. The interlayer insulating film 112 may be formed of a single layer of an inorganic insulating film, or may be formed of multiple layers of an inorganic insulating film and an organic insulating film.

[0054] The interlayer insulating film 112 has a first contact hole 113 formed therein that penetrates the interlayer insulating film 112 and exposes a portion of the surface of the active region 106, and the first contact hole 113 may be filled with a source electrode 114 and a drain electrode 115.

[0055] The source electrode 114 is electrically connected to a source region (SA) of the active region 106, and the drain electrode 115 is electrically connected to a drain region (DA) of the active region 106. The source electrode 114 and the drain electrode 115 may be arranged spaced apart from each other via the gate electrode 110. The source electrode 114 and the drain electrode 115 may be formed to fill all of the open regions of the first contact holes 113 and extend to partially cover the upper surface of the interlayer insulating film 112.

[0056] A planarization film 116 having a second contact hole 120 may be disposed on the interlayer insulating film 112. The planarization film 116 may have a thickness sufficient to cover the front surface of the substrate 100 and to provide a flat surface on the substrate 100. The second contact hole 120 penetrating the planarization film 116 may be formed to expose a portion of the surface of the drain electrode 115.

[0057] The first electrode 122 is formed on the planarization film 116. The first electrode 122 may be electrically connected to the gate electrode 110 through the drain electrode 115 exposed by the second contact hole 120. The first electrode 122 may be made of a transparent metal oxide such as indium tin oxide (ITO) or indium zinc oxide (IZO). The first electrode 122 may also be referred to as an anode electrode or a pixel electrode. The first electrodes 122 may be disposed spaced apart from each other for each sub-pixel.

[0058] A bank 124 having a bank hole 125 is formed on the planarization film 116. The bank 124 serves to divide each sub-pixel into a boundary region that defines a light-emitting region 126 of the pixel. The bank 124 also serves as a barrier to prevent lights of different colors from adjacent pixels from being mixed together and output. The bank 124 can space the first electrodes 122 for each sub-pixel.

[0059] The bank 124 may be formed using an inorganic insulating material such as silicon nitride (SiNx), silicon oxide (SiOx), etc., or an organic insulating material such as polyimide, etc. The bank 124 may be formed to cover the other regions except for the exposed portion of the first electrode 122 in the light emitting region 126 defined by the bank hole 125. The bank hole 125 may have a trench shape.

[0060] 5, a first shielding layer 130 and a first photoresist layer 135 are formed on the front surface of the substrate 100 including the bank 124. The first shielding layer 130 serves to prevent damage, for example damage caused by an etching material, that may occur during a process step of the organic light-emitting layer to be formed subsequently. The first shielding layer 130 is formed to have a first thickness (T1) on the surface of the bank 124 while filling all of the bank holes 125.

[0061] In one example, the first protective layer 130 may be made of a fluoropolymer material in which carbon-carbon bonds are continuously formed in a chain structure and functional groups contain a large amount of fluorine (F). The first protective layer 130 has orthogonality due to the inclusion of a large amount of fluorine (F). An orthogonal property can be understood as a property in which two things exist independently of each other. As a result, the first protective layer 130 has both hydrophobic properties, which have low affinity for water, and oleophobic properties, which have low affinity for oil. Due to these orthogonal properties, the first protective layer 130 can be separated from moisture or repel moisture. In addition, the first protective layer 130 is less affected by a developer containing an organic solvent used in the process steps.

[0062] The first photoresist layer 135 formed on the first protective layer 130 may be formed of either a positive type or a negative type photoresist material, and may be formed of a positive type photoresist material in the embodiment of the present invention. The first photoresist layer 135 is preferably formed to a first thickness (P1) that can prevent defects such as sagging or crumbling in a process of forming an undercut region thereafter.

[0063] Referring to FIG. 6, a first photoresist pattern 135a is formed including an opening region 136 that defines a region where a first pixel pattern of an organic light-emitting layer is to be formed. To this end, a photomask having an opening is positioned on a portion of the first photoresist layer 135 (see FIG. 5) where the opening region 136 is to be formed, and an exposure process is performed on the first photoresist layer 135 exposed through the opening, exposing it to light such as ultraviolet light (UV). Next, a development process is performed to remove the first photoresist layer 135 using a developer, and only the portion of the first photoresist layer 135 exposed to the ultraviolet light (UV) is selectively removed. Then, a first photoresist pattern 135a is formed including an opening region 136 that defines a region where a first sub-pixel pattern of an organic light-emitting layer is to be formed. A part of the surface of the first protective layer 130 may be exposed through the opening region 136 of the first photoresist pattern 135a.

[0064] 7 and 8, a patterning process is performed using the first photoresist pattern 135a as an etching mask to form a first undercut structure (UC1). The first undercut structure (UC1) is composed of a double layer of the first protective layer pattern 130a and the first photoresist pattern 135a. The first undercut region 140 may be formed on the first protective layer pattern 130a.

[0065] The first undercut structure (UC1) may have an undercut shape with respect to the first photoresist pattern 135a. The undercut can be understood as a phenomenon in which the first protective layer pattern 130a is further removed below the first photoresist pattern 135. In other words, the first undercut structure (UC1) is not vertically removed in alignment with the end portion (ed1) of the first photoresist pattern 135a, but is further removed inward from both ends (ed1) of the first photoresist pattern 135a by a first depth (d1). As a result, a second width (W2) between both ends (ed2) of adjacent first undercut structures (UC1) is formed to be relatively wider than a first width (W1) between both ends (ed1) of the first photoresist pattern 135a.

[0066] The patterning process for forming the first undercut structure (UC1) can be performed using a lift-off method. The lift-off process can be performed using a fluorine (F)-based organic solvent. The fluorine (F)-based organic solvent may be made of a polymeric material having a large amount of fluorine (F) in its functional group (or functional group) while carbon-carbon bonds are continuously formed in a chain structure. The fluorine (F)-based organic solvent containing a large amount of fluorine (F) in its functional group can also penetrate into the first protective layer 130 made of a fluoropolymeric material containing a large amount of fluorine (F) in its functional group, and selectively remove only the first protective layer 130 without affecting the first photoresist pattern 135a, thereby allowing patterning.

[0067] In the patterning process using the lift-off method, the amount of the first protective layer 130 removed can be adjusted by adjusting the time for which the first protective layer 130 made of a fluoropolymer material containing a large amount of fluorine (F) in the functional group is exposed to a fluorine (F)-based organic solvent, and the depth (d1) of the first undercut region 140 of the first undercut structure (UC1) can be controlled.

[0068] For example, Figure 8 is a photograph showing undercut regions formed after protective layers (SL1, SL2) and photoresist patterns (PR1, PR2) are disposed on substrates (SUB1, SUB2) and the protective layers (SL1, SL2) are exposed to a fluorine (F)-based organic solvent for different periods of time.

[0069] 8, when the protective layer (SL1) is exposed to the fluorine (F)-based organic solvent for a first time (10 seconds), the depth (UCW1) of the undercut region formed in FIG. 8(a) is a first depth, while when the protective layer (SL2) is exposed to the fluorine (F)-based organic solvent for a second time (45 seconds) that is longer than the first time, the depth (UCW2) of the undercut region formed in FIG. 8(b) is a second depth that is larger than the first depth. In other words, the longer the protective layers (SL1, SL2) are exposed to the fluorine (F)-based organic solvent, the larger the depth of the undercut region is.

[0070] By utilizing the characteristics of these protective layers, as shown in FIG. 7, the first depth (d1) of the first undercut region 140 of the first undercut structure (UC1) is formed to have a size greater than the thickness (T1) of the first protective layer pattern 130a (d1>T1).

[0071] Referring to FIG. 9, a first organic light emitting layer 145 including a first sub-pixel pattern 145a and a first organic material layer 145b is formed on a substrate 100. The first organic light emitting layer 145 includes a first sub-pixel pattern 145a and a first organic material layer 145b.

[0072] To this end, first, a plasma treatment is performed on the substrate 100 on which the first undercut region 140 is formed. The plasma treatment serves to remove foreign matter or residues generated during the previous process. In one example, the plasma treatment can be performed by generating plasma from nitrogen (N2), oxygen (O2), or argon (Ar) alone or in combination.

[0073] After the plasma treatment, a first organic light-emitting layer 145 is formed on the substrate 100. The first organic light-emitting layer 145 may be formed on the exposed surface of the first electrode 122 and the surface of the first photoresist pattern 135a.

[0074] The first subpixel pattern 145a may be formed on the bank 124, passing through the first undercut region 140 of the first undercut structure (UC1). Thus, the first subpixel pattern 145a may be formed to extend to the upper surface of the bank 124 along the shape of the sidewall of the bank 124 exposed by the bank hole 125, while covering the exposed surface of the first electrode 122. The first organic material layer 145b may be formed on the exposed surface of the first photoresist pattern 135a.

[0075] 10, the first sub-pixel pattern 145a may be formed to have a thickness that increases toward the bank hole 125. Specifically, when a deposition process for forming the first organic light emitting layer 145 is performed in a state in which the first undercut structure UC1 is formed, the organic material may be deposited non-uniformly due to the first undercut structure UC1.

[0076] For example, as shown by the arrow in FIG. 10, the first undercut region 140 of the first undercut structure (UC1) may be deposited with a relatively small amount of organic material due to the first photoresist pattern 135a located at the top. As a result, the first undercut region 140 may be formed to have the thinnest third thickness (th3). Also, the closer to the bank hole 125, the less the structure that is obstructed by the deposition process, so the thickest first thickness (th1) may be formed. And, the portion disposed relatively close to the first undercut structure (UC1) may be formed to have a second thickness (th2) that is relatively thicker than the third thickness (th3) but is relatively thinner than the first thickness (th1) because the organic material accumulates at the end of the first photoresist pattern 135a.

[0077] Although not shown in the drawings, the first organic light emitting layer 145 may include a stacked structure of a hole transport layer (HTL), an emission layer (EML), and an electron transport layer (ETL). The first organic light emitting layer 145 may further include a hole blocking layer (HBL), a hole injecting layer (HIL), an electron blocking layer (EBL), and an electron injecting layer (EIL) in addition to the hole transport layer (HTL), the emission layer (EML), and the electron transport layer (ETL). The emission layer (EML) of the first organic light emitting layer 145 is a layer that emits light by recombination of holes injected from the first electrode 122 and electrons injected from a second electrode formed thereafter, and may emit red light in the embodiment of the present invention.

[0078] Referring to FIG. 11, a full lift-off process is performed to expose the first electrode 122 in other regions except the first sub-pixel pattern 145a. The full lift-off process can be performed using a fluorine (F)-based organic solvent. The fluorine (F)-based organic solvent can also penetrate into the first protective layer pattern 130a made of a polymer material containing a large amount of fluorine (F) to remove the first protective layer pattern 130a. Then, the first photoresist pattern 135a disposed on the first protective layer pattern 130a and the first organic material layer 145b formed on the surface of the first photoresist pattern 135a can be removed together during the process of removing the first protective layer pattern 130a.

[0079] Here, the organic material constituting the first sub-pixel pattern 145a is resistant to fluorine (F)-based organic solvents and therefore does not deteriorate or change in quality. As a result, the first sub-pixel pattern 145a is not damaged during the full lift-off process. When the above-mentioned full lift-off process is performed, the surfaces of the first electrode 122 and the bank 124 in areas other than the first sub-pixel pattern 145a are exposed, and the portion where the first sub-pixel pattern 145a is formed can be defined as the first sub-pixel (SP-1).

[0080] 3, the first sub-pixel pattern 145a may have a rectangular shape including a edge portion (BD) and a trench portion (TC) arranged inward of the edge portion (BD) in a plan view. The edge portion (BD) of the first sub-pixel pattern 145a may have a stepped shape in which rings are repeatedly arranged in a plan view.

[0081] Referring to FIG. 12, a second protective layer 150 and a second photoresist layer 155 are sequentially formed on the front surface of the substrate 100 on which the first sub-pixel pattern 145a is formed. The second protective layer 150 may be formed to have a sufficient thickness to cover the entire exposed surface of the first sub-pixel pattern 145a to prevent damage to the organic light-emitting layer to be formed later. The second protective layer 150 may be formed of the same material and with the same first thickness (T1) as the first protective layer 130 (see FIG. 5). For example, the second protective layer 150 may be made of a fluoropolymer material in which carbon-carbon bonds are continuously formed in a chain structure and a large amount of fluorine (F) is contained in the functional group (or functional group). As a result, the second protective layer 150 has orthogonal properties including both hydrophobic and oleophobic properties.

[0082] The second photoresist layer 155 formed on the second protective layer 150 may be formed of either a positive type or a negative type photoresist material, and may be formed of a positive type photoresist material in the embodiment of the present invention. The second photoresist layer 155 is preferably formed to a first thickness (P1) that can prevent defects such as sagging or crumbling in a process of forming an undercut region thereafter.

[0083] Referring to FIG. 13, a second photoresist pattern 155a is formed including an opening region 156 that defines a region where a second pixel pattern of the organic light emitting layer is to be formed. To this end, a photomask having an opening is positioned on a portion of the second photoresist layer 155 where the opening region 156 is to be formed, and an exposure process is performed on the second photoresist layer 155 exposed through the opening to light such as ultraviolet (UV). Then, a development process is performed using a developer, whereby only the portion of the second photoresist layer 155 exposed to ultraviolet (UV) light is selectively removed. Then, a second photoresist pattern 155a is formed including an opening region 156 that defines a region where a second sub-pixel pattern of the organic light emitting layer is to be formed. A portion of the surface of the second protective layer 150 may be exposed through the opening region 156 of the second photoresist pattern 155a.

[0084] 14, a patterning process is performed using the second photoresist pattern 155a as an etching mask to form a second undercut structure (UC2). The second undercut structure (UC2) is composed of a double layer of the second protective layer pattern 150a and the second photoresist pattern 155a. A second undercut region 160 may be formed on the second protective layer pattern 150a.

[0085] The second undercut structure (UC2) may have an undercut shape with respect to the second photoresist pattern 155a. The second undercut structure (UC2) is not vertically removed in alignment with the end portion (ed3) of the second photoresist pattern 155a, but is further removed inward from both ends (ed3) of the second photoresist pattern 155a by a predetermined depth (d1). As a result, the width (W4) between both ends (ed4) of the second undercut structure (UC2) is formed to be relatively wider than the width (W3) between both ends (ed3) of the second photoresist pattern 155a.

[0086] The patterning process for forming the second undercut structure (UC2) can be performed using a lift-off method. The lift-off process can be performed using a fluorine (F)-based organic solvent. The fluorine (F)-based organic solvent, which contains a large amount of fluorine (F) in the functional group, penetrates into the second protective layer 150, selectively removing only the second protective layer 150, and the second undercut region 160 can be formed.

[0087] The depth (d1) of the second undercut region 160 may be controlled by adjusting the time for which the second protective layer 150 is exposed to the fluorine (F)-based organic solvent. In one example, the depth (d1) of the second undercut region 160 of the second undercut structure (UC2) may be similar to the depth of the first undercut region 140 (see FIG. 7). Thus, the depth (d1) of the second undercut region 160 is formed to have a size (d1>T1) greater than the thickness (T1) of the second protective layer pattern 150a.

[0088] Referring to FIG. 15, a second organic light emitting layer 165 including a second sub-pixel pattern 165a and a second organic material layer 165b is formed on a substrate 100. The second organic light emitting layer 165 includes a second sub-pixel pattern 165a and a second organic material layer 165b.

[0089] For this purpose, first, a plasma treatment is performed on the substrate 100 on which the second undercut region 160 is formed to remove foreign matter or residues generated during the previous process. In one example, the plasma treatment can be performed by generating plasma from nitrogen (N2), oxygen (O2), or argon (Ar) alone or in combination.

[0090] After the plasma treatment, a second organic light-emitting layer 165 is formed on the substrate 100. The second organic light-emitting layer 165 may be formed on the exposed surface of the first electrode 122 and the surface of the second photoresist pattern 155a.

[0091] The second subpixel pattern 165a may be formed on the bank 124, passing through the second undercut region 160 of the second undercut structure (UC2). Thus, the second subpixel pattern 165a may be formed to cover the exposed surface of the first electrode 122 and extend to the upper surface of the bank 124 along the shape of the sidewall of the bank 124 exposed by the bank hole 125. In one example, the second subpixel pattern 165a may be formed to have a thickness that increases toward the bank hole 125, as shown in FIG. 3, similar to the first subpixel pattern 145a. In addition, the edge portion (BD, see FIG. 3) of the second subpixel pattern 165a may have a stepped shape in which rings are repeatedly arranged in a plan view.

[0092] Although not shown in the drawing, the second organic light emitting layer 165 may include a stacked structure of a hole transport layer (HTL), an emission layer (EML), and an electron transport layer (ETL). The second organic light emitting layer 165 may further include a hole blocking layer (HBL), a hole injection layer (HIL), an electron blocking layer (EBL), and an electron injection layer (EIL).

[0093] The light emitting layer (EML) of the second organic light emitting layer 165 is a layer that emits light by recombination of holes injected from the first electrode 122 and electrons injected from a second electrode that is formed subsequently, and in an embodiment of the present invention, can emit green light.

[0094] 16, a full lift-off process is performed to expose the first electrode 122 in other regions except the first sub-pixel pattern 145a and the second sub-pixel pattern 165a. The full lift-off process can be performed using a fluorine (F)-based organic solvent. The fluorine (F)-based organic solvent can penetrate into the second protective layer pattern 150a and peel off and remove the bank 124 and the first electrode 122. Then, the second photoresist pattern 155a and the second organic material layer 165b disposed on the second protective layer pattern 150a can be removed together during the process of peeling off and removing the second protective layer pattern 150a.

[0095] Here, the organic material constituting the first sub-pixel pattern 145a and the second sub-pixel pattern 165a is resistant to a fluorine (F)-based organic solvent and is therefore not deteriorated or altered. As a result, the first sub-pixel pattern 145a and the second sub-pixel pattern 165a are not damaged during the full lift-off process. The first sub-pixel pattern 145a and the second sub-pixel pattern 165a may be spaced apart from each other by a predetermined distance (s1). The portion where the second sub-pixel pattern 165a is formed may be defined as the second sub-pixel (SP-2).

[0096] Next, as described above, a process for forming an undercut structure is performed to form the first sub-pixel pattern 145a or the second pixel pattern 145a, thereby forming a third undercut structure UC3.

[0097] Specifically, a protective layer and a photoresist layer are formed on the substrate 100, and an exposure and development process is performed on the photoresist layer to form a third photoresist pattern 175a defining an area where a third pixel pattern is to be formed, as shown in FIG. 17. Then, a patterning process is performed using the third photoresist pattern 175a as an etching mask to form a third undercut structure (UC3) consisting of a double layer of the third protective layer pattern 170a and the third photoresist pattern 175a. Here, the third protective layer pattern 170a may be made of the same material as the first protective layer 130 or the second protective layer 150, for example, a polymer material containing a large amount of fluorine (F). In addition, the third protective layer 170a may be formed to have the same thickness (T1) as the first protective layer 130 or the second protective layer 150, and the third photoresist pattern 170a may have the same thickness (P1) as the first photoresist pattern 135a or the second photoresist pattern 155a.

[0098] Thus, the patterning process for forming the third undercut structure (UC3) can be performed using a lift-off method using a fluorine (F)-based organic solvent. The third undercut structure (UC3) formed by these patterning processes is composed of a double layer of a third protective layer pattern 170a and a third photoresist pattern 175a. The third protective layer pattern 170a can include a third undercut region 180. The depth (d1) of the third undercut region 180 can be formed to have a size (d1>T1) greater than the thickness (T1) of the third protective layer pattern 170a.

[0099] Subsequently, a plasma treatment is performed to remove foreign matter or residual matter before forming the third organic light emitting layer 185. Then, as further shown in Fig. 17, the third organic light emitting layer 185 is formed on the substrate 100. The third organic light emitting layer 185 may include a third sub-pixel pattern 185a formed on the exposed surface of the first electrode 122, and a third organic material layer 185b formed on the surface of the third photoresist pattern 175a.

[0100] The third subpixel pattern 185a may be formed on the bank 124, passing through the third undercut region 180 of the third undercut structure (UC3). Thus, the third subpixel pattern 185a may be formed to cover the exposed surface of the first electrode 122 and extend to the upper surface of the bank 124 along the shape of the sidewall of the bank 124 exposed by the bank hole 125. In one example, the third subpixel pattern 185a may be formed to have a thickness that increases toward the bank hole 125, as shown in FIG. 3, similar to the first subpixel pattern 145a. In addition, the edge (BD) of the third subpixel pattern 185a may have a stepped shape in which rings are repeatedly arranged in a plan view. Since the edges (BD) of the first to third sub-pixel patterns 145a, 165a, 185a have a stepped shape in which rings are repeatedly arranged in a plan view, step portions where the resistance increases suddenly are repeatedly arranged, making it possible to further effectively reduce the leakage current.

[0101] The third organic light-emitting layer 185 may include a stacked structure of a hole-transporting layer (HTL), an emitting layer (EML), and an electron-transporting layer (ETL), and may further include a hole-blocking layer (HBL), a hole-injecting layer (HIL), an electron-blocking layer (EBL), and an electron-injecting layer (EIL).

[0102] The light-emitting layer (EML) of the third organic light-emitting layer 185 is a layer that emits light by recombination of holes injected from the first electrode 122 and electrons injected from the second electrode that is formed subsequently, and in an embodiment of the present invention, can emit blue light.

[0103] 18, a full lift-off process is performed on the substrate 100 including the third sub-pixel pattern 185a. The full lift-off process is performed using a fluorine (F)-based organic solvent, and the third protective layer pattern 170a may be peeled off and removed from the bank 124 and the first electrode 122. Then, the third photoresist pattern 175a and the third organic material layer 185b disposed on the third protective layer pattern 170a may be removed together during the process in which the third protective layer pattern 170a is peeled off and removed.

[0104] Here, the organic materials constituting the first sub-pixel pattern 145a, the second sub-pixel pattern 165a, and the third sub-pixel pattern 185a are resistant to fluorine (F)-based organic solvents and therefore do not deteriorate or change in quality. As a result, the third sub-pixel pattern 185a is not damaged during the full lift-off process. Furthermore, the organic materials constituting the first sub-pixel pattern 145a and the second sub-pixel pattern 165a are not damaged during the full lift-off process.

[0105] The first sub-pixel pattern 145a, the second sub-pixel pattern 165a, and the third sub-pixel pattern 185a formed by the full lift-off process may be spaced apart from each other by a predetermined distance (s1). A portion where the third sub-pixel pattern 185a is formed may be defined as a third sub-pixel (SP-3). And, a portion where the sub-pixel patterns 145a, 165a, and 185a are not arranged and the first electrode 122 is exposed may be an auxiliary electrode pixel (SUB_E).

[0106] 19, a second electrode 190 is formed on the front surface of the substrate 100. The second electrode 190 may be formed as a common electrode that is in common contact with the first subpixel pattern 145a, the second subpixel pattern 165a, and the third subpixel pattern 185a and applies a voltage to the first subpixel pattern 145a, the second subpixel pattern 165a, and the third subpixel pattern 185a. The second electrode 190 may also be referred to as a cathode electrode, and supplies electrons to the individual subpixel patterns 145a, 165a, and 185a.

[0107] The second electrode 190 may be formed including a transparent metal material capable of transmitting light. In one example, the second electrode 190 may be made of a transparent metal oxide such as indium-tin-oxide (ITO) or indium-zinc-oxide (IZO). Alternatively, the second electrode 190 may be formed of a semi-transparent metal material made of molybdenum (Mo), tungsten (W), silver (Ag), aluminum (Al), or an alloy containing at least one of these. Also, the second electrode 190 in the auxiliary electrode pixel (SUB_E) may be formed of an auxiliary electrode 195 in direct contact with the first electrode 122. The auxiliary electrode 195 serves to prevent imbalance in driving voltage.

[0108] The first sub-pixel pattern 145a, the second sub-pixel pattern 165a, the third sub-pixel pattern 185a, and the auxiliary electrode 195 form one group to configure one pixel. The pixel may have a structure in which a plurality of pixels are arranged in a matrix. As a result, the auxiliary electrode pixel (SUB_E) may be arranged in a mesh shape in a plan view.

[0109] An encapsulation layer 197 is formed on the substrate 100 on which the second electrode 190 is formed. The encapsulation layer 197 serves to improve the reliability of the display device by blocking the penetration of moisture or oxygen from the outside. To this end, the encapsulation layer 197 may be formed of at least one inorganic or organic single layer, or a multi-layer in which inorganic and organic layers are stacked.

[0110] In the display device according to the first embodiment of the present specification, a plurality of sub-pixel patterns can be formed by using a patterning method using an undercut structure consisting of a double layer of a protective layer made of a fluoropolymer material containing a large amount of fluorine (F) and a photoresist pattern. By forming the sub-pixel pattern using the patterning method, a finer pattern can be realized than when the sub-pixel pattern is formed using a fine metal mask (FMM). In addition, the fine metal mask (FMM) is difficult to apply to a large area panel due to a mask sagging phenomenon, while the patterning method can easily form a plurality of sub-pixel patterns even in a large area panel.

[0111] In addition, by using a patterning method using an undercut structure consisting of a double layer of a protective layer made of a fluoropolymer material and a photoresist pattern, damage to the organic material constituting the sub-pixel pattern can be prevented, thereby improving the performance and reliability of the display device.

[0112] Furthermore, since the edges of each subpixel pattern have a stepped shape in which rings are repeatedly arranged in a planar view, step portions where the resistance increases suddenly are repeatedly arranged, and leakage current can be further effectively reduced.

[0113] Meanwhile, by introducing an undercut structure consisting of a double layer of a protective layer made of a fluoropolymer material and a photoresist pattern, the depth of the undercut region can be adjusted to control the shape of the sub-pixel pattern, which will be described below with reference to the drawings.

[0114] 20 to 27 are views for explaining a method for manufacturing a display device according to a second embodiment of the present specification. And, Figs. 28a to 28c are views for explaining defects caused by adjusting the depth of the undercut region in the second embodiment of the present specification. Here, components that are the same or similar to those in Figs. 4 to 19 will be briefly described using the same reference numerals.

[0115] Referring to FIG. 20, a light blocking layer 102, a buffer layer 104, a thin film transistor (TR), an interlayer insulating film 112, a source electrode 114, a drain electrode 115, a planarization film 116, a first electrode 122, and a bank 124 may be provided on a substrate 100.

[0116] The light blocking layer 102 may be disposed on the substrate 100 so as to overlap the thin film transistor (TR), and a buffer layer 104 may be formed to cover the light blocking layer 102. The thin film transistor (TR) is disposed on the buffer layer 104. The thin film transistor (TR) may include an active region 106, a gate electrode 110, a source electrode 114, and a drain electrode 115.

[0117] A gate electrode 110 is disposed on the active region 106 via a gate insulating film 108, and a source electrode 114 and a drain electrode 115 may be disposed so as to be in direct contact with a source region (SA) and a drain region (DA) of the active region 106, respectively, but is not limited to this.

[0118] The interlayer insulating film 112 may be formed to cover the active region 106 and the gate electrode 110. The interlayer insulating film 112 may include a first contact hole 113 exposing a portion of a surface of the active region 106 so that the source electrode 114 and the drain electrode 115 can contact the active region 106. The source electrode 114 and the drain electrode 115 may be spaced apart from each other via the gate electrode 110. The source electrode 114 and the drain electrode 115 may be formed to fill the entire first contact hole 113 formed in the interlayer insulating film 112 and may extend to cover a portion of an upper surface of the interlayer insulating film 112.

[0119] A planarization film 116 having a second contact hole 120 may be disposed on the interlayer insulating film 112. The second contact hole 120 penetrating the planarization film 116 exposes a portion of a surface of the drain electrode 115. A first electrode 122 is disposed on the planarization film 116. The first electrode 122 may be electrically connected to the gate electrode 110 via the drain electrode 115. The first electrode 122 may also be referred to as an anode electrode or a pixel electrode. The first electrodes 122 may be disposed spaced apart from each other for each sub-pixel.

[0120] A plurality of banks 124 may be disposed on the planarization film 116. The banks 124 may define a light-emitting region of a pixel and separate individual sub-pixels. The banks 124 are disposed spaced apart from each other and separate the first electrodes 122 into individual sub-pixels.

[0121] A first protective layer 200 and a first photoresist layer 205 are formed on the front surface of the substrate 100 on which the above-mentioned structures are formed. The first protective layer 200 is formed to have a first thickness (T1) on the surface of the bank 124 while filling all of the bank holes 125. The first protective layer 200 is made of a fluoropolymer material containing a large amount of fluorine (F) in its functional group (or functional group) and has orthogonal properties. The first photoresist layer 205 formed on the first protective layer 200 is preferably formed to a first thickness (P1) to prevent defects such as sagging or crumbling downwards in the process of forming an undercut region thereafter.

[0122] 21, an exposure process using a photomask and a development process are performed on the first photoresist layer 205 (see FIG. 20) to form a first photoresist pattern 205a. The exposure process is selectively performed on the first photoresist layer 205 in the area where the first sub-pixel pattern is to be formed, and a development process is performed to remove the first photoresist layer 205 in the area where the exposure process was performed.

[0123] As a result, a first photoresist pattern 205a is formed in which the surface of the first protective layer 200 is exposed by the opening regions 207 that define the regions in which the first sub-pixel patterns are to be formed.

[0124] Referring to FIG. 22, a patterning process is performed using the first photoresist pattern 205a as an etching mask to form a first undercut structure (UC1). The first undercut structure (UC1) is composed of a double layer of the first protective layer pattern 200a and the first photoresist pattern 205a. The first undercut region 210 may be formed on the first protective layer pattern 200a.

[0125] The first undercut structure (UC1) may have an undercut shape with respect to the first photoresist pattern 205a. In one example, the first undercut structure (UC1) is not vertically removed in alignment with the end portions (ed1) of the first photoresist pattern 205a, but is further removed inward by a predetermined depth (d2) from both end portions (ed1) of the first photoresist pattern 205a.

[0126] The patterning process for forming the first undercut structure (UC1) can be performed by a lift-off method using a fluorine (F)-based organic solvent. The fluorine (F)-based organic solvent penetrates into the interior through the exposed surface of the first protective layer 200 (see FIG. 21), does not affect the first photoresist pattern 205a, and selectively removes only the first protective layer 200 to form an undercut shape. In the lift-off patterning process, the depth (d2) of the first undercut region 210 of the first undercut structure (UC1) is controlled by adjusting the time for which the first protective layer 200 made of a fluoropolymer material is exposed to the fluorine (F)-based organic solvent to adjust the amount of the first protective layer 200 removed.

[0127] The depth (d2) of the first undercut region 210 according to the second embodiment of the present specification is formed to have a size (d2 < T1) that is even smaller than the thickness (T1) of the first protective layer pattern 200a.

[0128] Referring to FIG. 23, a first organic light-emitting layer 215 including a first sub-pixel pattern 215a and a first organic material layer 215b is formed on a substrate 100.

[0129] For this purpose, first, plasma treatment is performed on the substrate 100 on which a first undercut region 210 (see FIG. 22) is formed. The plasma treatment serves to remove foreign substances or residues generated in the process of performing the previous steps before forming the organic light-emitting layer. In one example, the plasma treatment can be performed by plasmaizing a single or mixed gas of nitrogen (N2), oxygen (O2), or argon (Ar).

[0130] Next, a first organic light-emitting layer 215 is formed on the substrate 100. The first organic light-emitting layer 215 may be formed on the exposed surface of the first electrode 122 and the surface of the first photoresist pattern 205a using a vapor deposition method.

[0131] The first sub-pixel pattern 215a may be formed on the bank 124 through the first undercut region 210 of the first undercut structure (UC1). Here, the depth (d2) of the first undercut region 210 is formed to have a size (d2 < T1) that is even smaller than the thickness (T1) of the first protective layer pattern 200a.

[0132] Thus, the first sub-pixel pattern 215a covers the exposed surface of the first electrode 122 and extends to the top surface of the bank 124 along the shape of the sidewall of the bank 124 exposed by the bank hole 125. Here, the first sub-pixel pattern 215a may be formed including tail portions 215t formed by extending to the exposed sidewall surfaces of the first protective layer pattern 200a by forming the depth (d2) of the first undercut region 210 of the first undercut structure (UC1) to a size smaller than the thickness (T1) of the first protective layer pattern 200a. Here, the first sub-pixel pattern 215a may have tail portions 215t at both ends in a cross-sectional view, but may have tail portions 215t formed to surround the edge portion (BD) shown in FIG. 3 in a plan view.

[0133] The tail portions 215t can define an area in which the first sub-pixel patterns 215a are formed on a plane. These tail portions 215t can function as alignment marks for the first sub-pixel patterns 215a in a subsequent process. For example, when a color filter is formed on the first sub-pixel patterns 215a, the tail portions 215t corresponding to the first sub-pixel patterns 215a can be used to align the color filter formation area.

[0134] The height (h1) of the tail portion 215t of the first sub-pixel pattern 215a may be formed to be thinner than the thickness (T1) of the first protective layer pattern 200a, so that a part of the sidewall surface of the first protective layer pattern 200a may be exposed. Then, the first organic material layer 215b may be formed on the exposed surface of the first photoresist pattern 205a.

[0135] Although not shown in the drawings, the first organic light emitting layer 215 may include a stacked structure of a hole transport layer (HTL), an emission layer (EML), and an electron transport layer (ETL), and may further include a hole blocking layer (HBL), a hole injection layer (HIL), an electron blocking layer (EBL), and an electron injection layer (EIL). The emission layer (EML) of the first organic light emitting layer 215 is a layer that emits light by recombination of holes injected from the first electrode 122 and electrons injected from a second electrode formed thereafter, and in the embodiment of the present invention, it can emit red light.

[0136] Referring to FIG. 24, a full lift-off process is performed to expose the first electrode 122 in the region where the first sub-pixel pattern 215a and other pixel patterns are to be formed. The full lift-off process can be performed using a fluorine (F)-based organic solvent. The fluorine (F)-based organic solvent can penetrate into the exposed surface of the first protective layer pattern 200a made of a polymer material containing fluorine (F) and remove the first protective layer pattern 200a. Then, the first undercut structure (UC1) is removed by the full lift-off process to expose the first sub-pixel pattern 215a. The portion where the first sub-pixel pattern 145a is formed can be defined as the first sub-pixel (SP-1). Here, the organic material constituting the first sub-pixel pattern 215a is resistant to the fluorine (F)-based organic solvent, and is not deteriorated or altered, nor is it damaged.

[0137] Next, a process of forming an undercut structure is performed on the second sub-pixel (SP-1) as described in FIG. 20 to FIG. 24, and the second sub-pixel pattern 225a is formed using the formed undercut structure as shown in FIG. 25. The depth of the undercut region of the undercut structure is formed to be smaller than the thickness of the protective layer of the undercut structure, and the second sub-pixel pattern 225a is formed on the undercut region, so that the second sub-pixel pattern 225a can include tail portions 225t at both ends. Here, the second sub-pixel pattern 225a has tail portions 225t at both ends in a cross-sectional view, but the tail portions 225t can be formed to surround the edge portion (BD) shown in FIG. 3 in a plan view. In the embodiment of the present invention, the second sub-pixel pattern 225a can emit green light.

[0138] Next, a process of forming an undercut structure is performed on the third sub-pixel (SP-3) as described in FIGS. 20 to 24, and the third sub-pixel pattern 235a is formed using the formed undercut structure as shown in FIG. 26. The depth of the undercut region of the undercut structure is formed to be smaller than the thickness of the protection layer of the undercut structure, and the third sub-pixel pattern 235a is formed on this undercut region, so that the third sub-pixel pattern 235a can include tail portions 235t at both ends. In the embodiment of the present invention, the third sub-pixel pattern 235a can emit blue light.

[0139] The tail portions 225t, 235t formed at both ends of each of the second subpixel pattern 225a and the third subpixel pattern 235a may be formed to have a height similar to the height (h1, see Figure 23) of the tail portion 215t of the first subpixel pattern 215a.

[0140] 27, a second electrode 240 is formed on the front surface of the substrate 100. The second electrode 240 may be formed as a common electrode that is in common contact with the first subpixel pattern 215a, the second subpixel pattern 225a, and the third subpixel pattern 235a and applies a voltage to the first subpixel pattern 215a, the second subpixel pattern 225a, and the third subpixel pattern 235a. The second electrode 240 may also be called a cathode electrode, and supplies electrons to the individual subpixel patterns 215a, 225a, and 235a.

[0141] The second electrode 240 may be formed to a thickness sufficient to cover all of the tail portions 215t, 225t, and 235t located at both ends of each of the sub-pixel patterns 215a, 225a, and 235a. The second electrode 240 may be formed by selecting from a transparent metal material or a semi-transparent metal material capable of transmitting light. Also, the second electrode 240 in the auxiliary electrode pixel (SUB_E) may be formed of an auxiliary electrode 245 in direct contact with the first electrode 122. The auxiliary electrode 245 serves to prevent imbalance in driving voltages.

[0142] The first sub-pixel pattern 215a, the second sub-pixel pattern 225a, the third sub-pixel pattern 235a, and the auxiliary electrode 245 can configure one pixel. Since the pixel has a structure in which a plurality of pixels are arranged in a matrix, the auxiliary electrode pixel (SUB_E) may be arranged in a mesh shape in a plan view.

[0143] The encapsulation layer 250 is formed on the substrate 100 on which the second electrode 240 is formed. The encapsulation layer 250 serves to improve the reliability of the display device by blocking the penetration of moisture or oxygen from the outside. To this end, the encapsulation layer 250 may be formed as a single layer of at least one inorganic film or organic film, or a multi-layer in which inorganic films and organic films are stacked.

[0144] According to the second embodiment of the present specification, it is possible to form including tail portions 215t, 225t, 235t at both end portions of each of the plurality of sub-pixel patterns 215a, 225a, 235a. As described above, these tail portions 215t, 225t, 235t can be formed by controlling the depth (d2) of the first undercut region 210 in the first undercut structure (UC1) to have a size (d2 < T1) smaller than the thickness (T1) of the first protective layer pattern 200a. And the depth (d2) of this first undercut region 210 will be controlled by adjusting the time for which the first protective layer 200 is exposed to the fluorine (F)-based organic solvent.

[0145] However, this first protective layer 200 may be exposed to the fluorine (F)-based organic solvent for a time shorter than the target time. Hereinafter, it will be described with reference to the drawings.

[0146] Referring to FIGS. 28a to 28c, in the process of forming a double layer of a protective layer (SL) and a photoresist pattern (PR) on a substrate on which a lower structure (BN1) including a first electrode (AE) or the like is formed, and exposing the protective layer (SL) to a fluorine (F)-based organic solvent to form an undercut structure, if it is exposed for a time shorter than the target time, the end portion (eds) of the protective layer (SL) may protrude from the end portion (edp) of the photoresist pattern (PR), and a part of the surface (a) of the protective layer (SL) may be exposed.

[0147] When plasma treatment is performed before depositing an organic light-emitting layer while the surface (a) of the protective layer (SL) is partially exposed, the exposed surface (a) of the protective layer (SL) can be directly exposed to a plasma treatment material and cured. The cured protective layer (SL) does not need to be removed by a fluorine (F)-based organic solvent in a full lift-off process performed thereafter. When an organic light-emitting layer is deposited to form a sub-pixel pattern (EML-SP) while the end portion (eds) of the protective layer (SL) protrudes from the end portion (edp) of the photoresist pattern (PR), the sub-pixel pattern (EML-SP) can form a tail portion (EML-T) that extends to the sidewall surface of the end portion (eds) of the protective layer (SL) and has a thickness greater than that of the protective layer (SL).

[0148] Furthermore, when a full lift-off process is performed to remove the protective layer (SL) and the photoresist pattern (PR), the protective layer (SL) is not completely removed from one side of the tail portion (EML-T) of the sub-pixel pattern (EML-SP), as shown in part "Y" of Figure 28b, and protective layer remnant (SL-R) remains.

[0149] When the second electrode (CE) is formed on the subpixel pattern (EML-SP) while the protective layer residue (SL-R) remains, the second electrode (CE) in the tail portion (EML-T) of the subpixel pattern (EML-1, EML-2, EML-3) may be disconnected as shown in Fig. 28c. Since the second electrode (CE) is a common electrode that is in common contact with the first subpixel pattern (EML-1), the second subpixel pattern (EML-2), and the third subpixel pattern (EML-3) and applies a voltage, when the second electrode (CE) is disconnected, a defect occurs in which at least one or more hues among the plurality of subpixels (SP-1, SP-2, SP-3) do not emit light, which may reduce the reliability of the display device.

[0150] Therefore, it is preferable to form the depth of the undercut region of the undercut structure consisting of a double layer of the protective layer and the photoresist pattern to have a size at least larger or smaller than the thickness of the protective layer, and to perform a lift-off process so that the protective layer is not directly exposed to the outside from the end of the photoresist pattern.

[0151] Meanwhile, the method of forming a sub-pixel pattern through a patterning process using an undercut structure may also be applied to a display device that emits white light, which will be described below with reference to the accompanying drawings.

[0152] 29 to 36 are drawings for explaining the third embodiment of the present specification. Here, components that are the same as or similar to those in Figs. 4 to 19 will be simply described using the same reference numerals.

[0153] Referring to FIG. 29, a light blocking layer 102, a buffer layer 104, a thin film transistor (Tr), an interlayer insulating film 112, a source electrode 114, a drain electrode 115, a planarization film 116, a first electrode 122, and a bank 124 may be provided on a substrate 100.

[0154] A color filter (CF) is disposed on the interlayer insulating film 112. The color filter (CF) is disposed at a position overlapping the light-emitting region defined by the bank hole 125. When the organic light-emitting layer is made of an organic material that emits white light, the color filter (CF) may exhibit a hue assigned to each sub-pixel. For example, the color filter (CF) may be one of red (R), green (G) and blue (B).

[0155] A protective layer 300 is formed to a first thickness (T1) on the front surface of the substrate 100 on which the above-mentioned components are formed, and a photoresist layer 305 is formed to a first thickness (P1). The protective layer 300 is made of a fluoropolymer material containing a large amount of fluorine (F) in its functional group (or functional group) and has orthogonal properties. The photoresist layer 305 formed on the protective layer 300 is preferably formed to a thickness that can prevent defects such as sagging or crumbling in the process of forming an undercut region thereafter.

[0156] 30, a photomask (M) having openings (OA; open areas) and light-shielding portions (NOA; non-open areas) is positioned on a photoresist layer 305. The openings (OA) of the photomask (M) expose the surface of the photoresist layer 305 in the areas where the sub-pixel patterns are to be formed, and the light-shielding portions shield the surface of the photoresist layer 305 in the areas where the auxiliary electrode pixels are to be formed. Next, an exposure process is performed to expose the photoresist layer 305 to light such as ultraviolet light (UV) through the openings (OA) of the photomask (M).

[0157] 31, a development process is performed to selectively remove only the portions of the photoresist layer 305 exposed to ultraviolet (UV) light, thereby forming a photoresist pattern 305a. The photoresist pattern 305a includes opening regions 310 that define regions in which sub-pixel patterns of an organic light-emitting layer are to be formed. A portion of the surface of the protective layer 300 may be exposed through the opening regions 310 of the photoresist pattern 305a. The region in which auxiliary electrode pixels are to be formed thereafter is covered with the photoresist pattern 305a.

[0158] 32, a patterning process is performed using the photoresist pattern 305a as an etching mask to form an undercut structure (UC). The undercut structure (UC) is composed of a double layer of a protection layer pattern 300a and a photoresist pattern 305a. An undercut region 310 may be disposed under the photoresist pattern 305a.

[0159] The undercut structure (UC) may have an undercut shape with respect to the photoresist pattern 305a. The undercut structure (UC) is further removed from both ends (ed) of the photoresist pattern 305a inwardly by a predetermined depth (d3). The patterning process for forming the undercut structure (UC) may be performed using a lift-off method using a fluorine-based organic solvent. A fluorine (F)-based organic solvent may penetrate into the protective layer 300 and selectively remove it, forming the protective layer pattern 300a.

[0160] The undercut structure (UC) according to the third embodiment of the present specification can collectively form an area in which a plurality of sub-pixel patterns are to be formed thereafter, for example, can expose an area in which a first sub-pixel pattern, a second sub-pixel pattern, and a third sub-pixel pattern are to be formed.

[0161] Referring to FIG. 33, an organic light emitting layer 320 is formed on a substrate 100, the organic light emitting layer 320 including a first sub-pixel pattern 320a, a second sub-pixel pattern 320b, a third sub-pixel pattern 320c, and an organic material layer 320d.

[0162] For this purpose, first, a plasma treatment is performed on the substrate 100 on which the undercut region 315 is formed. After the plasma treatment, an organic light emitting layer 320 is formed on the substrate 100. The organic light emitting layer 320 may be formed on the exposed surface of the first electrode 122 and the surface of the photoresist pattern 305a. Each of the subpixel patterns 320a, 320b, and 320c may be formed on the bank 124 by passing through the undercut region 315 of the undercut structure (UC). As a result, the subpixel patterns 320a, 320b, and 320c may be formed to cover the exposed surface of the first electrode 122 and extend to the upper surface of the bank 124 along the shape of the sidewall of the bank 124 exposed by the bank hole 125. The subpixel patterns 320a, 320b, and 320c may be formed to extend to a position where they contact the sidewall of the protective layer pattern 300a, but are not limited thereto. An organic material layer 340d may be formed on the exposed surface of the photoresist pattern 305a.

[0163] 34, the organic light emitting layer 320 according to the third embodiment of the present specification may be formed in a multi-stack structure, which is a tandem structure in which a plurality of light emitting layer stacks (ST1, ST2) for emitting white light are stacked. The organic light emitting layer 320 may be formed of a stack in which a hole transport layer (HTL), an emission layer (EML), and an electron transport layer (ETL) are sequentially stacked. In one example, the organic light emitting layer 320 may include a structure in which a first light emitting layer stack (ST1) having a structure in which a first hole transport layer (HTL1), a first emission layer (EML1), and a first electron transport layer (ETL1) are stacked, and a second light emitting layer stack (ST2) having a structure in which a second hole transport layer (HTL2), a second emission layer (EML2), and a second electron transport layer (ETL2) are stacked are stacked. Here, the first light-emitting layer stack (ST1) may include a first light-emitting layer (EML1) that emits a first hue, and the second light-emitting layer stack (ST2) may include a second light-emitting layer (EML2) that emits a second hue different from the first hue, but is not limited thereto. In another example, when the light-emitting layer stack has a structure in which three stacks are laminated, each of the light-emitting layers may include two blue light-emitting layers (B-EML) and one orange light-emitting layer (OR-EML).

[0164] Here, a charge generation layer (CGL) may be disposed between the first light emitting layer stack (ST1) and the second light emitting layer stack (ST2). The charge generation layer (CGL) serves to supply charges to each of the first light emitting layer stack (ST1) and the second light emitting layer stack (ST2).

[0165] 35, a full lift-off process is performed on the substrate 100 to remove the undercut structure (UC). The full lift-off process can be performed using a fluorine (F)-based organic solvent. The fluorine (F)-based organic solvent can penetrate into the protective layer pattern 300a to peel and remove the protective layer pattern 300a from the bank 124 and the first electrode 122. Then, the photoresist pattern 305a and the organic material layer 320d disposed on the protective layer pattern 300a can be removed together during the process in which the protective layer pattern 300a is peeled and removed.

[0166] During the full lift-off process, the organic materials constituting the first sub-pixel pattern 320a, the second sub-pixel pattern 320b, and the third sub-pixel pattern 320c are resistant to fluorine (F)-based organic solvents, and therefore are not deteriorated, altered, or damaged.

[0167] The first, second, and third sub-pixel patterns 320a, 320b, and 320c may be spaced apart from each other by a predetermined distance S2. The portions where the first, second, and third sub-pixel patterns 320a, 320b, and 320c are formed may be defined as first, second, and third sub-pixels (SP-1, SP-2, and SP-3), respectively.

[0168] The first to third sub-pixel patterns 320a, 320b, and 320c may have a rectangular shape including a edge portion (BD) and a trench portion (TC) arranged inward of the edge portion (BD) as shown in Fig. 3. In addition, the edge portion (BD) of each of the sub-pixel patterns 320a, 320b, and 320c has a stepped shape in which rings are repeatedly arranged in a plan view, so that stepped portions where the resistance increases suddenly are repeatedly arranged, and the leakage current can be further effectively reduced.

[0169] Furthermore, each of the first to third sub-pixel patterns 320a, 320b, and 320c may be formed to have a thickness that increases toward the bank hole 125. In this manner, the first to third sub-pixel patterns 320a, 320b, and 320c have a thickness that decreases toward the outer periphery of the pattern, and therefore leakage current can be reduced.

[0170] 36, a second electrode 325 is formed on the front surface of the substrate 100. The second electrode 325 may be formed as a common electrode that is in common contact with the first to third sub-pixel patterns 320a, 320b, and 320c and applies a voltage to the first to third sub-pixel patterns 320a, 320b, and 320c. The second electrode 325 may also be called a cathode electrode, and supplies electrons to the individual sub-pixel patterns 320a, 320b, and 320c.

[0171] In one example, the second electrode 325 may be in direct contact with the first electrode 122 on the auxiliary electrode pixel (SUB_E) to form the auxiliary electrode 330. As a result, the first to third sub-pixel patterns 320a, 320b, 320c and the auxiliary electrode 330 form one group to form one pixel. The pixel may have a structure in which a plurality of pixels are arranged in a matrix. As a result, the auxiliary electrode pixel (SUB_E) may be arranged in a mesh shape in a plan view.

[0172] An encapsulation layer 340 may be disposed on the second electrode 325. The encapsulation layer 340 serves to improve the reliability of the display device by blocking the penetration of moisture or oxygen from the outside. To this end, the encapsulation layer 340 may be formed as a single layer of at least one inorganic film or organic film, or a multi-layer in which inorganic films and organic films are stacked.

[0173] The display device according to the third embodiment of the present specification may be configured by forming an organic light-emitting layer in a tandem structure and a multi-stack structure in which a plurality of light-emitting layers for emitting white light are stacked, and including a charge generation layer (CGL). Here, the charge generation layer (CGL) is a layer for generating electrons and holes and stably supplying them to the electron transport layer (ETL) and the hole transport layer (HTL), and it may be an important issue to prevent leakage current from the charge generation layer (CGL).

[0174] Therefore, in the fourth embodiment of the present specification, a structure capable of preventing the occurrence of leakage current due to the charge generation layer (CGL) will be described below with reference to the drawings.

[0175] 37 to 43 are cross-sectional views illustrating a manufacturing method of the display device according to the fourth embodiment of the present specification.

[0176] Referring to FIG. 37, a light blocking layer 102, a buffer layer 104, a thin film transistor (TR), an interlayer insulating film 112, a color filter (CF), a source electrode 114, a drain electrode 115, a planarization film 116, a first electrode 122, and a bank 124 may be provided on a substrate 100.

[0177] A protective layer 300 is formed to a first thickness (T1) on the front surface of the substrate 100 on which the above-mentioned components are formed, and a photoresist layer 305 is formed to a first thickness (P1). The protective layer 300 is made of a fluoropolymer material containing a large amount of fluorine (F) in its functional group, and has orthogonal properties.

[0178] 38, an exposure process and a development process are performed on the photoresist layer to form a photoresist pattern 305a. The photoresist pattern 305a includes an opening region 310 that defines an area where a sub-pixel pattern of an organic light emitting layer is to be formed. A surface of the protective layer 300 may be partially exposed through the opening region 310. Then, an area where an auxiliary electrode pixel is to be formed is covered with the photoresist pattern 305a.

[0179] 39, a patterning process is performed using the photoresist pattern 305a as an etching mask to form a mold structure 306. The patterning process may be a lift-off process in which the protective layer 300 is exposed to a fluorine (F)-based organic solvent.

[0180] The mold structure 306 is composed of a double layer of a protective layer pattern 300a and a photoresist pattern 305a. Here, the protective layer pattern 300a may be formed to protrude from an end of the photoresist pattern 305a by a predetermined area (E). To this end, the lift-off process may be performed by controlling the time for exposing the protective layer 300 to a fluorine (F)-based organic solvent to set the point where the surface of the protective layer pattern 300a is exposed.

[0181] In this case, the width between both ends of adjacent photoresist patterns 305a, which is the opening region 310 of the photoresist pattern 305a, may be formed to have a width wider than the width between both ends of adjacent protective layer patterns 300a.

[0182] 40, on the first to third sub-pixels (SP-1, SP-2, SP-3) of the substrate 100, a first light-emitting layer stack 315 and an organic material layer 315d are formed.

[0183] For this purpose, first, a plasma treatment is performed on the substrate 100 on which the mold structure 306 is formed. When the plasma treatment is performed, the exposed surface of the protective layer pattern 300a may be directly exposed to a plasma treatment material and hardened. Then, when an organic light emitting layer is deposited in a state in which the end portion of the protective layer pattern 300a protrudes from the end portion of the photoresist pattern 305a, the first light emitting layer stacks 315 formed on the first to third sub-pixels (SP-1, SP-2, SP-3) may be formed including tail portions 315t that extend to the sidewall surfaces of the end portions of the protective layer pattern 300a and have a height greater than the thickness of the protective layer pattern 300a.

[0184] 34, a first light emitting layer stack 315 having a structure in which a first hole transport layer (HTL1), a first light emitting layer (EML1), and a first electron transport layer (ETL1) are stacked is formed on the substrate 100 on which the mold structure 306 is formed. Then, the first light emitting layer stack 315 may be formed to include a tail portion 315t by extending to a sidewall surface of an end portion of the protective layer pattern 300a.

[0185] Referring to FIG. 41, a full lift-off process is performed to remove the mold structure 306. The full lift-off process can be performed using a fluorine (F)-based organic solvent. When the full lift-off process is performed, the hardened portion of the protective layer pattern 300a is not removed, and a residual pattern of the protective layer pattern 300a remains as a tail portion side support portion 300r on one side of each tail portion 315t of the first light emitting layer stack 315. Here, the tail portion side support portion 300r has a height lower than the height of the tail portion 315t of the first light emitting layer stack 315.

[0186] 42, a charge generation layer 315G and a second light-emitting layer stack 317 are formed on a first light-emitting layer stack 315. The charge generation layer 315G may be formed to have a thickness smaller than the thickness of a tail portion 315t (see FIG. 41t) of the first light-emitting layer stack 315. As a result, the charge generation layer 315G may be arranged to have a shape separated from each of the first to third sub-pixels (SP-1, SP-2, SP-3).

[0187] The second light-emitting layer stack 317 is formed on the charge generation layer 315G separated by the tail portion 315t of the first light-emitting layer stack 315, and may have a structure that extends from the first sub-pixel (SP-1) to the second sub-pixel (SP-2), the third sub-pixel (SP-3), and the auxiliary electrode pixel (SUB_E) without being cut off and connected. As shown in FIG. 34, the second light-emitting layer stack 317 may include a second hole transport layer (HTL2), a second light-emitting layer (EML2) that is a different hue from the first light-emitting layer (EML1), and a second electron transport layer (ETL2). The charge generation layer (CGL) serves to supply charges to the first light-emitting layer stack 315 and the second light-emitting layer stack 317, respectively.

[0188] This may result in the formation of a first subpixel pattern 320a, a second subpixel pattern 320b, and a third subpixel pattern 320c, each including a first light-emitting layer stack 315, a charge generation layer 315G, and a second light-emitting layer stack 317, in the first to third subpixels (SP-1, SP-2, SP-3).

[0189] When the organic light-emitting layer is made of an organic material that emits white light, the organic light-emitting layer is formed in a structure that extends from the first sub-pixel pattern to the third sub-pixel pattern without any breaks. In this case, the charge generation layer is also formed without any breaks from the first sub-pixel pattern to the third sub-pixel pattern, which may cause a leakage current to flow to an adjacent sub-pixel pattern and may cause an unintended sub-pixel to be driven. If an unintended sub-pixel is driven, a defect that reduces the image quality may occur.

[0190] In this regard, according to the fourth embodiment of the present specification, the first light-emitting layer stack 315 formed in each subpixel (SP-1, SP-2, SP-3) is formed including the tail portion 315t, so that the charge generation layer 315G having a thickness smaller than the tail portion 315t may be arranged to have a shape separated from each of the first to third subpixels (SP-1, SP-2, SP-3). As a result, the charge generation layer 315G arranged between the first light-emitting layer stack 315 and the second light-emitting layer stack 317 between the adjacent subpixel patterns can be physically disconnected by the tail portion 315t. In other words, by physically disconnecting the path of the leakage current caused by the charge generation layer 315G, the leakage current can be prevented and the image quality can be improved.

[0191] 43, a second electrode 325 is formed on the front surface of the substrate 100. The second electrode 325 may be formed as a common electrode that is in common contact with the first subpixel pattern 320a, the second subpixel pattern 320b, and the third subpixel pattern 320c and applies a voltage to the first subpixel pattern 320a, the second subpixel pattern 320b, and the third subpixel pattern 320c. The second electrode 325 may also be called a cathode electrode, and supplies electrons to the individual subpixel patterns 320a, 320b, and 320c.

[0192] Also, the second electrode 325 may be formed as an auxiliary electrode by directly contacting the first electrode 122 in the auxiliary electrode pixel (SUB_E). The auxiliary electrode serves to prevent imbalance in driving voltages.

[0193] The encapsulation layer 340 is formed on the substrate 100 on which the second electrode 325 is formed. The encapsulation layer 340 serves to improve the reliability of the display device by blocking the penetration of moisture or oxygen from the outside. To this end, the encapsulation layer 340 may be formed as a single layer of at least one inorganic film or organic film, or a multi-layer in which inorganic films and organic films are stacked.

[0194] The manufacturing method of the display device according to the fourth embodiment of the present specification can improve image quality by physically disconnecting the charge generation layer (CGL) when forming an organic light-emitting layer in a tandem structure in which a plurality of light-emitting layers for emitting white light are stacked, thereby preventing leakage current from occurring. [Explanation of symbols]

[0195] 100 Substrates 102 Light blocking layer 104 Buffer Layer T Thin-film transistor 106 Active region 110 Gate electrode 112 Interlayer insulating film 114 Source Electrode 115 Drain electrode 116 Planarization film 122 1st electrode 124 Bank 145a, 215a, 320a First subpixel pattern 165a, 225a, 320b Second subpixel pattern 185a, 235a, 320c Third subpixel pattern 215t, 225t, 235t, 315t tail section 190, 240, 325 2nd electrode 195, 245, 330 auxiliary electrode 197, 250, 340 Sealing layer

Claims

1. A substrate on which a plurality of pixels are arranged, each of the pixels including a plurality of sub-pixels; a first electrode disposed in each of the sub-pixels and connected to a transistor for driving the sub-pixels to emit light; a bank that divides light-emitting regions of the plurality of sub-pixels and includes a bank hole that exposes a portion of the first electrode; each of the sub-pixels includes a sub-pixel pattern disposed on a bottom surface of the bank hole, in contact with an exposed surface of the first electrode, and extending continuously along a sidewall of the bank hole and a surface of an upper outer edge of the bank; the sub-pixel pattern functions as an organic light-emitting layer; the thickness of the subpixel pattern decreases stepwise along a surface of an upper outer edge of the bank in a direction toward another subpixel pattern adjacent to the subpixel pattern; a step portion is provided by decreasing a thickness of the sub-pixel pattern in a step-like manner, and an electrical resistance increases suddenly in the step portion; Display device.

2. each of the sub-pixel patterns extends continuously along a surface of an upper outer edge of the bank and terminates in a tail portion away from the substrate; The display device according to claim 1 .

3. the tails are located at each end of the sub-pixel pattern and surround an outer portion of the sub-pixel pattern. The display device according to claim 2 .

4. the tail portion defines an area of ​​the sub-pixel pattern and serves as an alignment mark for the sub-pixel pattern. The display device according to claim 2 .

5. further comprising a second electrode disposed on the tail portion. The display device according to claim 2 .

6. a tail portion side support portion in contact with an outer surface portion of the tail portion; The height of the tail portion side support portion is lower than the height of the tail portion. The display device according to claim 2 .

7. Each of the subpixel patterns comprises a first light-emitting layer stack including a first hole transport layer, a first light-emitting layer, and a first electron transport layer; a charge generating layer overlying the first light emitting layer stack and having a thickness less than the tail; a second light emitting layer stack comprising a second hole transport layer overlying the charge generating layer, a second light emitting layer that emits a different hue than the first light emitting layer, and a second electron transport layer; Including, the charge generation layer is located lower than the height of the tail portion and is separated from the charge generation layers of other adjacent sub-pixels among the plurality of sub-pixels; The display device according to claim 2 .

8. The plurality of sub-pixels include a first sub-pixel emitting a first color; a second sub-pixel emitting a second color; a third sub-pixel emitting a third color; and an auxiliary sub-pixel in which the first electrode and the second electrode are in direct contact with each other without the sub-pixel pattern; The display device according to claim 1 .

9. The sub-pixel pattern comprises: an edge extending along an upper outer corner surface of the bank; a trench pattern disposed on a bottom surface and a side wall of the bank hole; Including, The display device according to claim 1 .

10. the edge portion has a step and includes a plurality of annular patterns arranged horizontally in a plan view, and a thickness of an innermost annular pattern of the plurality of annular patterns is thicker than a thickness of an outermost annular pattern; The display device according to claim 9.

11. A substrate on which a plurality of pixels are arranged, each of the pixels including a plurality of sub-pixels; a first electrode disposed in each of the sub-pixels and connected to a transistor for driving the sub-pixels to emit light; a bank that divides light-emitting regions of the plurality of sub-pixels and includes a bank hole that exposes a portion of the first electrode; Including, each of the sub-pixels includes a sub-pixel pattern disposed on a bottom surface of the bank hole, in contact with an exposed surface of the first electrode, and extending continuously along a sidewall of the bank hole and a surface of an upper outer edge of the bank; the sub-pixel pattern functions as an organic light-emitting layer; each of the subpixel patterns extends continuously along a surface of an upper outer edge of the bank and terminates in a tail portion extending upwardly away from the substrate; the subpixel pattern has a maximum thickness at the tail portion; Display device.

12. the tails are located at each end of the sub-pixel pattern and surround an outer portion of the sub-pixel pattern. The display device according to claim 11.

13. the tail portion defines an area of ​​the sub-pixel pattern and serves as an alignment mark for the sub-pixel pattern. The display device according to claim 11.

14. further comprising a second electrode disposed on the tail portion. The display device according to claim 11.

15. a tail portion side support portion in contact with an outer surface portion of the tail portion; The height of the tail portion side support portion is lower than the height of the tail portion. The display device according to claim 11.

16. the thickness of the subpixel pattern decreases stepwise as it extends along a surface of an upper outer edge of the bank in a direction toward other subpixel patterns adjacent to the subpixel pattern; The display device according to claim 11.

17. 1. A method for manufacturing a display device, comprising the steps of: forming a plurality of pixels on a substrate, each pixel including a plurality of sub-pixels; forming a first electrode in each of the sub-pixels connected to a transistor for driving the plurality of sub-pixels to emit light; forming a bank having a bank hole that divides the light emitting regions of the plurality of sub-pixels and exposes a portion of the first electrode; forming a protective layer on the bank; forming a photoresist pattern exposing a portion of a surface of the protective layer; removing a portion of the protective layer to form an undercut structure consisting of a double layer of the protective layer pattern and the photoresist pattern, the double layer forming an undercut region under the photoresist pattern; forming a sub-pixel pattern located at a bottom surface of the bank hole, contacting an exposed surface of the first electrode, and extending continuously into the undercut region along a sidewall of the bank hole and a surface of an upper outer edge of the bank, the sub-pixel pattern functioning as an organic light-emitting layer; removing the undercut structure; forming a second electrode located on the sub-pixel pattern; Including, forming the subpixel pattern includes decreasing a thickness of the subpixel pattern in a stepwise manner as the subpixel pattern extends into the undercut region; a step portion is provided by decreasing a thickness of the sub-pixel pattern in a step-like manner, and an electrical resistance increases suddenly in the step portion; A method for manufacturing a display device.

18. forming the subpixel pattern includes forming individual subpixel patterns extending continuously along a surface of an upper outer edge of the bank and terminating in tails extending in a direction away from the substrate; The method for manufacturing the display device according to claim 17 .

19. The protective layer contains a fluoropolymer material in which carbon-carbon bonds are continuously formed in a chain structure and a certain amount of fluorine (F) is contained in a functional group. The method for manufacturing the display device according to claim 17 .

20. The step of forming the undercut structure includes supplying a fluorine (F)-based organic solvent onto an exposed surface of the protective layer to selectively remove the protective layer except for the photoresist pattern, thereby forming the undercut region. The method for manufacturing the display device according to claim 17 .

21. forming a tail portion side support in contact with an outer surface of the tail portion, the tail portion side support including a protective layer residual pattern supporting the tail portion; The method for manufacturing the display device according to claim 18 .

Citation Information

Patent Citations

  • Light-emitting device

    JP2007258163A

  • Method for manufacturing organic el element, organic el element, and organic el system

    JP2009181932A

  • Light-emitting device and method for manufacturing the same

    JP2014123527A

  • Organic light-emitting display apparatus and method of manufacturing the same

    JP2019133921A