Electrochemical device and electronic device including said electrochemical device

By distributing low-melting point polymer particles in the nanofiber substrate, the safety and self-discharge problems of lithium-ion batteries are solved, mechanical strength is enhanced, and the safety and circulation performance of the battery are improved.

JP7581364B2Active Publication Date: 2024-11-12AMPEREX TECH
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022558291
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-27
Publication Date
2024-11-12
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

The existing separator materials have insufficient hot melt closing function in lithium-ion batteries, which leads to the inability to cut off the current when the car is hot, which poses safety risks. At the same time, large pore diameters and uneven pore distribution lead to self-discharge problems, and insufficient mechanical strength, which is easy to penetrate by the electrode material and cause short circuits.

Method used

The separator layer is formed by distributing low-melting polymer particles in the nanofiber substrate. The low-melting polymer melts and seals the pores when hot cars, blocks current, and fills large pores to improve mechanical strength.

Benefits of technology

Effectively prevent current conduction during hot sports cars, reduce self-discharge phenomenon, enhance the mechanical strength of the diaphragm, prevent electrode material from penetrating, and improve battery safety and cycling performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581364000008
    Figure 0007581364000008
  • Figure 0007581364000009
    Figure 0007581364000009
  • Figure 0007581364000010
    Figure 0007581364000010
Patent Text Reader

Abstract

The present invention relates to an electrochemical device and an electronic device including the electrochemical device. The electrochemical device includes an electrode piece and a separation layer (10) on at least one surface of the electrode piece. The separation layer (10) includes a porous nanofiber substrate (101) and polymer particles (102) distributed in the porous nanofiber substrate (101). The melting temperature of the polymer particles (102) is 70°C to 150°C. Compared to conventional technologies, the separation layer (10) has low-melting-point polymer particles (102) distributed in the porous nanofiber substrate (101), which gives the separation layer (10) a low-temperature thermal pore-closing function and shuts down current in the event of thermal runaway, improving the safety performance of the electrochemical device. The low-melting-point polymer particles (102) are filled into the "macropores" of the porous substrate made of fibers, and by reducing the number of macropores, the self-discharge problem of the electrochemical device is further improved, the K value is lowered, and the problem of internal short-circuiting that occurs inside the electrochemical device when positive electrode active material particles or negative electrode active material particles penetrate the separation layer is reduced, which is also advantageous in improving the electrical performance, such as the cycle performance, of the electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of electrochemistry, more specifically the present invention relates to electrochemical devices and electronic devices comprising said electrochemical devices. [Background technology]

[0002] Lithium-ion batteries have many advantages, such as high energy density, long cycle life, high nominal voltage (>3.7V), and low self-discharge rate, and are widely used in consumer electronics. In recent years, with the rapid development of electric vehicles and mobile electronic devices, related needs such as battery energy density (>700Wh / L), safety, and cycle performance (>500 cycles) are increasing, and new lithium-ion batteries that comprehensively improve overall performance are expected. Among them, separatorless lithium-ion batteries are a new lithium-ion battery that has attracted attention.

[0003] Separatorless lithium-ion batteries adopt a method of preparing a separation layer on the surface of the electrode piece instead of the traditional separator. In separatorless lithium-ion batteries, the separation layer is directly integrated on the surface of the electrode piece, so there is no need to manufacture a separator separately. In addition, the manufacturing process is changed from a three-assembly of pole piece-separator-pole piece to a laminate / wound body of two assemblies of (integrated) pole piece-(integrated) pole piece, simplifying the battery production process and reducing the difficulty of preparing the battery. And the thinner separation layer improves the battery energy density. In addition, separatorless battery technology has many other advantages, such as improving the porosity of the separation layer, improving the liquid retention capacity, and accelerating the reaction kinetics, and has been widely paid attention.

[0004] Conventional separator-less lithium-ion batteries generally use a nonwoven fabric separator. The nonwoven fabric separator is formed by the orientation or random bonding of nanofibers or microfibers. The random overlap between each fiber forms a large number of pores, which are used for ion transport. The fibers themselves are used as the support structure of the separator. However, such a fiber layer does not have a thermal pore-closing function, and when thermal runaway occurs (e.g., overcharging of the battery, hot box, vibration, collision, drop, internal short circuit, external short circuit, etc.), it cannot cut off the current by melting it to shut down the lithium ion passage, which poses a great risk to the safety performance of the lithium ion battery. In addition, the fiber layer of the nonwoven fabric separator itself has low mechanical strength, so when it resists the penetration of the positive electrode particles or negative electrode particles, it is penetrated by the positive electrode particles or negative electrode particles, causing an internal short circuit in the electrochemical device. In addition, the nonwoven fabric separator has a large fiber pore size and a non-uniform distribution, and the presence of some "macropores" causes the lithium ion battery to have a serious self-discharge problem. Summary of the Invention

[0005] Based on the shortcomings of the prior art, a first aspect of the present invention first provides an electrochemical device comprising an electrode piece and a separation layer on at least one surface of the electrode piece, the separation layer comprising a porous substrate made of nanofibers and polymer particles distributed in the porous substrate, and the melting temperature of the polymer particles is 70°C to 150°C.

[0006] In some preferred embodiments of the first aspect of the present invention, the number of the polymer particles in the separating layer is greater than or equal to 1×10 8 / m 2 ~1×10 18 / m 2 It is.

[0007] In some preferred embodiments of the first aspect of the present invention, the polymer particles have an average particle size of 40 nm to 10 μm.

[0008] In some preferred embodiments of the first aspect of the present invention, the nanofibers have a diameter of 10 nm to 5 μm, and the porous substrate has a pore size of 40 nm to 10 μm.

[0009] In some preferred embodiments of the first aspect of the present invention, a portion of the polymer particles protrudes from the surface of the porous substrate by a height of 0.1 nm to 5 μm, and a surface area of ​​the surface of the porous substrate occupied by the portion of the polymer particles is 0.1% to 60% of a total surface area of ​​the porous substrate.

[0010] In some preferred embodiments of the first aspect of the present invention, the polymer of the polymer particles comprises at least one selected from the group consisting of polystyrene, polyethylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, acrylonitrile-butadiene-styrene, polylactic acid, polyvinyl chloride, polyvinyl butyral, and polyacrylate.

[0011] In some preferred embodiments of the first aspect of the present invention, the nanofibers comprise a polymer, the polymer comprising at least one selected from the group consisting of polyvinylidene fluoride, polyimide, polyamide, polyacrylonitrile, polyethylene glycol, polyethylene oxide, polyphenylene ether, polypropylene carbonate, polymethyl methacrylate, polyethylene terephthalate, poly(vinylidene fluoride-hexafluoropropylene), poly(vinylidene fluoride-co-chlorotrifluoroethylene), and derivatives thereof, preferably at least one selected from the group consisting of polyvinylidene fluoride, polyimide, polyamide, polyacrylonitrile, polyethylene glycol, polyethylene oxide, polyphenylene ether, polypropylene carbonate, polymethyl methacrylate, polyethylene terephthalate, and derivatives thereof.

[0012] In some preferred embodiments of the first aspect of the present invention, the ratio β / α of the cross-sectional porosity β of the separating layer to the surface open area α of the separating layer is 95% or less.

[0013] In some preferred embodiments of the first aspect of the present invention, the surface porosity α is 35% to 90%.

[0014] In some preferred embodiments of the first aspect of the present invention, the cross-sectional porosity β is 30% to 85%.

[0015] A second aspect of the present invention provides an electronic device, comprising an electrochemical device according to any of the above technical solutions.

[0016] The electronic devices according to the present invention include any electronic devices known in the art, such as notebook computers, mobile phones, electric motorcycles, electric cars, electric toys, and the like.

[0017] Compared with the prior art, the separation layer of the present invention has a low-melting-point polymer particle distributed in a porous substrate made of nanofibers, so that the separation layer has a low-temperature thermal pore-closing function, and when thermal runaway occurs, the current can be shut down to improve the safety performance of the electrochemical device. In addition, the separation layer of the present invention has a low-melting-point polymer particle filled in the "macropores" of the porous substrate made of fibers, so that the macropores in the pure heat-resistant spun separation layer can be reduced, which further improves the self-discharge problem of the electrochemical device, reduces the K value, and improves the mechanical strength of the separation layer, thereby reducing the internal short circuit problem that occurs when the positive electrode active material particles or negative electrode active material particles penetrate the separation layer inside the electrochemical device, which is also advantageous in improving the electrochemical performance such as the cycle performance of the electrochemical device. [Brief description of the drawings]

[0018] In order to more clearly explain the technical solutions of the embodiments of the present invention and the prior art, the following briefly introduces drawings that need to be used in the embodiments and the prior art. Obviously, the following drawings are only some embodiments of the present invention, and those skilled in the art can obtain other drawings based on these drawings without any inventive work. [Figure 1]FIG. 1 is a schematic diagram of the configuration of an electrode assembly according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of the configuration of an electrode assembly according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic diagram of the configuration of an electrode assembly according to one embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram of the configuration of an electrode assembly according to one embodiment of the present invention. [Diagram 5] FIG. 5 is a schematic diagram showing the configuration of a separation layer in one embodiment of the present invention. [Figure 6] FIG. 6 is a schematic diagram showing the configuration of a separation layer in one embodiment of the present invention. [Figure 7] FIG. 7 is a schematic diagram of an embodiment of preparing a separating layer of the present invention. [Figure 8] FIG. 8 is a schematic diagram of an embodiment of preparing a separating layer of the present invention.

[0019] Explanation of symbols 10 separation layer 101 Porous substrate made of nanofibers 102 Polymer particles 103 Inorganic particles 20 Current collector 201 Positive electrode current collector 202 Negative electrode current collector 30 Active material layer 301 Positive electrode active material layer 302 Negative electrode active material layer 40 Conductive Layer 401 Positive electrode conductive layer 402 Negative electrode conductive layer 50 Spinning equipment 60 Electrodeposition equipment 70 Voltage Regulator DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] In order to make the objectives, technical solutions and advantages of the present invention clearer, the present invention will be described in more detail below with reference to the drawings and embodiments. Obviously, the described embodiments are only some of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments in the present invention, all other embodiments that a person skilled in the art can obtain without creative labor are also within the scope of the protection claims of the present invention.

[0021] The electrochemical device described in the present invention is not particularly limited and may be any electrochemical device in which the present invention can be used, such as a lithium ion battery, a supercapacitor, etc. In the following, for the convenience of explanation, a lithium ion battery will be described as an example, but this does not mean that the electrochemical device of the present invention is limited to a lithium ion battery.

[0022] One aspect of the present invention provides an electrochemical device, the electrochemical device comprising an electrode piece and a separation layer on at least one surface of the electrode piece, the separation layer comprising a nanofiber porous substrate and polymer particles distributed in the porous substrate, the melting temperature of the polymer particles being 70°C to 150°C, preferably 80°C to 140°C, more preferably 90°C to 130°C, and most preferably 100°C to 120°C.

[0023] In some embodiments of the present invention, the porous substrate is formed by the orientation or random bonding of nanofibers. The random overlap between each nanofiber forms a large number of pores, which are used for the transport of ions. The nanofibers themselves are used as the support skeleton of the separation layer. The polymer particles are filled into the porous substrate. Since the melting temperature of the polymer particles is low, when the electrochemical device experiences thermal runaway, such as overcharging, hot boxing, vibration, collision, dropping, internal short circuiting, external short circuiting, etc., the temperature of the electrochemical device rises and reaches the melting point of the polymer particles, after which the polymer particles melt and close the pores of the separation layer, reducing or blocking the conduction of lithium ions, reducing or stopping the charging and discharging of the electrochemical device, and greatly improving the safety of the electrochemical device. In addition, the porous substrate made of nanofibers itself has a high melting temperature, and in the case of thermal abuse such as overcharging / hot boxing, the separation layer retains its original structure and does not cause film rupture due to melting shrinkage, thereby avoiding the occurrence of internal short circuit phenomenon. In addition, since the polymer particles are distributed in the pores of the porous substrate, the macropores in the porous substrate are filled, which can effectively reduce the self-discharge phenomenon. In addition, since the polymer particles are distributed in the porous substrate, the penetration resistance strength of the porous substrate can be improved, and the positive and negative active material particles can be effectively prevented from penetrating the separation layer and causing a short circuit in the electrochemical device. In addition, since the porous substrate made of nanofibers has a relatively good adhesive force between the electrode pieces, the separation layer can be effectively prevented from being scoured by the electrolyte and folded back during the dropping process of the electrochemical device, and the safety performance of the electrochemical device can be greatly improved.

[0024] The number of polymer particles in the separation layer is not particularly limited as long as the object of the present invention can be achieved. In some embodiments of the present invention, the number of polymer particles in the separation layer is 1×10 8 / m 2 ~1×10 18 / m 2 and preferably 1×10 9 / m 2 ~1×10 16 / m 2 and more preferably 1×10 10 / m 2~1×10 14 / m 2 and most preferably 1×10 11 / m 2 ~1×10 13 / m 2 By limiting the number of polymer particles to the above range, when thermal runaway occurs in the electrochemical device, it is possible to quickly respond, shorten the time from melting to pore closure, block the ion passage, and improve the safety performance of the electrochemical device. In addition, it is possible to better improve the penetration resistance of the separation layer, prevent the positive electrode active material particles and the negative electrode active material particles from penetrating the separation layer, and effectively reduce the macropores in the porous substrate, reduce the self-discharge phenomenon, and lower the K value.

[0025] The particle size of the polymer particles is not particularly limited as long as the object of the present invention can be achieved. In some embodiments of the present invention, the average particle size of the polymer particles is 40 nm to 10 μm, preferably 100 nm to 5 μm, more preferably 200 nm to 2 μm, and most preferably 500 nm to 1.5 μm. When the average particle size of the polymer particles is within the above range, the macropores in the porous substrate can be reduced or eliminated better, and the self-discharge phenomenon can be reduced. In addition, when the average particle size of the polymer particles is within the above range, when thermal runaway occurs in the electrochemical device, the pores in the separation layer can be sufficiently and quickly closed, the ion conduction path can be blocked, an insulating layer can be formed, and the ignition or explosion of the battery can be prevented.

[0026] The diameter of the nanofibers or microfibers is not particularly limited as long as the object of the present invention can be achieved. In some embodiments of the present invention, the diameter of the nanofibers is 10 nm to 5 μm, preferably 20 nm to 2 μm, more preferably 50 nm to 1 μm, and most preferably 80 nm to 400 nm. When the diameter of the nanofibers is within the above range, the separation layer has an appropriate porosity, the liquid retention capacity of the separation layer is improved, and the porous substrate has an appropriate strength, and the mechanical strength of the separation layer is improved synergistically with the polymer particles distributed in the porous substrate, and the resistance of the separation layer against the penetration of the positive electrode active material particles and the negative electrode active material particles can be increased. In the separation layer, the pore size of the porous substrate is not particularly limited as long as the object of the present invention can be achieved. In some preferred embodiments of the present invention, the pore size of the porous substrate is 40 nm to 10 μm, preferably 80 nm to 5 μm, more preferably 130 nm to 1 μm, and most preferably 150 nm to 500 nm. Without being limited by any theory, the present inventor believes that the pore size of the porous substrate within the above range can accelerate the transport of lithium ions, improve the reaction kinetics, and effectively reduce the probability of the positive electrode active material particles and the negative electrode active material particles penetrating the separation layer, thereby reducing the risk of self-discharge phenomenon and internal short circuit. In addition, during the thermal runaway of the electrochemical device, the molten polymer particles can quickly fill the pores of the separation layer, close the separation layer, block the transport of ions, and improve the safety performance of the electrochemical device.

[0027] In one preferred embodiment of the present invention, a part of the polymer particles protrudes from the surface of the porous substrate at a height of 0.1 nm to 5 μm, preferably at a height of 1 nm to 1 μm, more preferably at a height of 2 nm to 500 nm, and most preferably at a height of 5 nm to 100 nm. Without being limited to any theory, the present inventor believes that the polymer particles protrude from the porous substrate at a certain height, thereby reducing the acting force of the positive electrode active material particles and the negative electrode active material particles on the porous substrate itself, and further preventing the penetration of the separation layer by the positive electrode particles and the negative electrode particles. The surface area of ​​the surface of the porous substrate occupied by a part of the polymer particles is 0.1% to 60%, preferably 0.5% to 45%, more preferably 2% to 30%, and most preferably 5% to 15% of the total surface area of ​​the porous substrate. Without being limited to any theory, the present inventors believe that when the surface area of ​​the surface of the porous substrate occupied by the polymer particles protruding from the surface is within the above range, the separation layer can have higher strength and the ability to resist penetration by positive electrode active material particles and negative electrode active material particles.

[0028] In the present invention, the "surface of the porous substrate" refers to the surface of the separation layer on the side away from the active material layer after the separation layer is applied to the active material layer.

[0029] The type of polymer in the polymer particles used in the present invention is not particularly limited as long as the melting point is 70 to 150° C. In some embodiments of the present invention, the polymer particles contain at least one selected from the group consisting of polystyrene (PS), polyethylene (PE), ethylene-propylene copolymer, polypropylene (PP), ethylene-vinyl acetate copolymer (EVA), acrylonitrile-butadiene-styrene (ABS), polylactic acid (PLA), polyvinyl chloride (PVC), polyvinyl butyral (PVB), and polyacrylate (PA).

[0030] The shape of the polymer particles used in the present invention is not particularly limited, and may be at least one of a spherical shape, an olive shape, an elongated shape, a flat shape, a ring shape, a doughnut shape, a rod shape, a hollow shape, a spiral shape, a core-shell shape, a gourd shape, a cylinder, a cone shape, a rectangular parallelepiped, a cube, a pyramid, a prism, and any other shape.

[0031] The nanofibers used in the present invention are not particularly limited as long as they can achieve the object of the present invention, and any material known to those skilled in the art can be used. In some embodiments of the present invention, the nanofibers comprise a polymer, the polymer comprising at least one selected from the group consisting of polyvinylidene fluoride (PVDF), polyimide (PI), polyamide (PA), polyacrylonitrile (PAN), polyethylene glycol (PEG), polyethylene oxide (PEO), polyphenylene ether (PPO), polypropylene carbonate (PPC), polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), poly(vinylidene fluoride-co-chlorotrifluoroethylene) (PVDF-PCTFE), and derivatives thereof, preferably at least one selected from the group consisting of polyvinylidene fluoride, polyimide, polyamide, polyacrylonitrile, polyethylene glycol, polyethylene oxide, polyphenylene ether, polypropylene carbonate, polymethyl methacrylate, polyethylene terephthalate, and derivatives thereof. Preferably, in some embodiments of the present invention, the melting point of the polymer is 170° C. or higher. By using the nanofibers containing a polymer having a melting point of 170° C. or higher, when thermal runaway occurs, the polymer particles begin to melt at a relatively low temperature, for example, 70-150° C., and close the ion transport path of the separation layer, but the nanofiber framework does not melt at this temperature and maintains the original structure of the separation layer without melting and shrinking, ensuring that internal short circuits of the battery due to shrinkage or rupture of the separation layer do not occur, and improving the safety of the electrochemical device.

[0032] The nanofibers may further include inorganic particles, which are not particularly limited and may be any inorganic particles known to those skilled in the art. For example, the inorganic particles may include at least one selected from the group consisting of HfO2, SrTiO3, SiO2, Al2O3, MgO, CaO, NiO, BaO, ZnO, TiO2, ZrO2, SnO2, CeO2, boehmite, magnesium hydroxide, and aluminum hydroxide. The size of the inorganic particles is not particularly limited and may be, for example, 10 nm to 10 μm. The content of the inorganic particles is not particularly limited and may be, for example, 0.1% to 80%. By adding inorganic particles, the mechanical strength of the separation layer can be further improved, the self-discharge phenomenon of the electrochemical device can be reduced, and the safety performance of the electrochemical device can be improved.

[0033] In some preferred embodiments of the present invention, the surface porosity α of the separation layer is 35% to 90%, preferably 45% to 87%, more preferably 60% to 85%, and most preferably 75% to 82%. The cross-sectional porosity β of the separation layer is 30% to 85%, preferably 40% to 80%, more preferably 50% to 75%, and most preferably 55% to 65%. The ratio β / α of the cross-sectional porosity β of the separation layer to the surface porosity α of the separation layer is 95% or less, preferably 20% to 90%, more preferably 40% to 85%, and most preferably 65% ​​to 80%.

[0034] By controlling the surface porosity and cross-sectional porosity of the separation layer within the above ranges, the separation layer can be provided with high liquid retention capacity, appropriate strength, and rapid reaction kinetics.

[0035] The thickness of the separation layer according to the present invention is not particularly limited and can be selected by a person skilled in the art according to the specific situation, and is preferably 1 μm to 20 μm, preferably 2 μm to 18 μm, more preferably 5 μm to 15 μm, and most preferably 6 μm to 12 μm. The thickness of the separation layer refers to the thickness of the entire separation layer that includes the porous substrate made of nanofibers and the polymer particles.

[0036] The electrochemical device of the present invention may be a lithium ion battery. The present invention is not limited to the type of lithium ion battery, and may be any type of lithium ion battery, such as a button type, cylindrical type, soft pack type lithium ion battery, etc.

[0037] The lithium ion battery of the present invention comprises a positive electrode piece, a negative electrode piece, an electrolyte and the separator according to any one of the above aspects of the present invention.

[0038] In one embodiment of the present invention, the separator layer is formed on one side of a positive electrode piece and one side of a negative electrode piece, and the layers are stacked in the order of negative electrode piece + separator layer, positive electrode piece + separator layer to form a lithium ion battery stack.

[0039] In another embodiment of the present invention, the separator may be formed on both sides of the positive electrode piece, and the negative electrode piece may be stacked in the order of separator + positive electrode piece + separator to form a lithium ion battery stack, where there is no separator on the surface of the negative electrode piece.

[0040] In another embodiment of the present invention, the separators are formed on both sides of the negative electrode piece, and the positive electrode piece is laminated in the order of separator + negative electrode piece + separator to form a lithium ion battery stack, where there is no separator on the surface of the positive electrode piece.

[0041] The stack formed in the above embodiment may be further stacked in the above order, or may be directly wound to form a multi-layer lithium ion battery stack. The present invention is not limited to the stacking method, and those skilled in the art may select it according to the specific situation.

[0042] 1 is a schematic diagram of the configuration of an electrode assembly according to one embodiment of the present invention. Here, a separation layer is provided on one side of an electrode piece. The separation layer 10 covers the surface of an electrode active material layer 30 provided on one side of a current collector 20.

[0043] 2 is a schematic diagram of the configuration of an electrode assembly according to one embodiment of the present invention, in which a separator 10 is disposed between a positive electrode active material layer 301 and a negative electrode active material layer 302, the positive electrode active material layer 301 being disposed on one side of a positive electrode current collector 201, and the negative electrode active material layer 302 being disposed on one side of a negative electrode current collector 202.

[0044] 3 is a schematic diagram of an electrode assembly configuration according to one embodiment of the present invention, in which the electrode assembly further includes a conductive layer 40, which is located between an electrode active material layer 30 and a current collector 20, and a separation layer 10 covering the surface of the electrode active material layer 30.

[0045] 4 is a schematic diagram of the configuration of an electrode assembly according to one embodiment of the present invention, where the electrode assembly further includes a positive electrode conductive layer 401 and a negative electrode conductive layer 402, where the positive electrode conductive layer 401 is located between the positive electrode current collector 201 and the positive electrode active material layer 301, and the negative electrode conductive layer 402 is located between the negative electrode current collector 202 and the negative electrode active material layer 302.

[0046] Figure 5 is a schematic diagram of a separation layer configuration according to one embodiment of the present invention, in which polymer particles 102 are located within a porous substrate 101 made of nanofibers.

[0047] 6 is a schematic diagram of the configuration of a separation layer according to one embodiment of the present invention, in which polymer particles 102 and inorganic particles 103 are located in a porous substrate 101 made of nanofibers.

[0048] In an embodiment of the present invention, the positive electrode piece is not particularly limited as long as it can achieve the object of the present invention. For example, the positive electrode piece usually includes a positive electrode current collector and a positive electrode active material. Here, the positive electrode current collector is not particularly limited and may be any positive electrode current collector known in the art, such as aluminum foil, aluminum alloy foil, or a composite current collector. The positive electrode active material is not particularly limited and may be any positive electrode active material in the prior art. The active material includes at least one selected from the group consisting of NCM811, NCM622, NCM523, NCM111, NCA, lithium iron phosphate, lithium cobalt oxide, lithium manganate, lithium iron manganese phosphate, and lithium titanate.

[0049] The positive electrode piece may further include a conductive layer located between the positive electrode current collector and the positive electrode active material. The composition of the conductive layer is not particularly limited and may be any conductive layer commonly used in the art. For example, the conductive layer may include a conductive agent and an adhesive.

[0050] In an embodiment of the present invention, the negative electrode piece is not particularly limited as long as it can achieve the object of the present invention. For example, the negative electrode piece usually includes a negative electrode current collector and a negative electrode active material. Here, the negative electrode current collector is not particularly limited, and any negative electrode current collector known in the art, such as copper foil, copper alloy foil, or a composite current collector, may be used. The negative electrode active material is not particularly limited, and any negative electrode active material known in the art may be used. The negative electrode active material may include at least one selected from the group consisting of graphite, hard carbon, soft carbon, silicon, silicon carbide, and silicon oxide.

[0051] The negative electrode piece may further include a conductive layer located between the negative electrode current collector and the negative electrode active material. The composition of the conductive layer is not particularly limited and may be any conductive layer commonly used in the art. For example, the conductive layer may include a conductive agent and an adhesive. The conductive agent is not particularly limited, and any conductive agent known in the art can be used as long as the object of the present invention can be achieved. The conductive agent may include at least one selected from the group consisting of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fiber, graphene, and the like. The conductive agent may include, for example, conductive carbon black (Super P). The adhesive is not particularly limited, and any adhesive known in the art can be used as long as the object of the present invention can be achieved. The adhesive may include, for example, at least one selected from the group consisting of styrene butadiene rubber (SBR), polyvinyl alcohol (PVA), polytetrafluoroethylene (PTFE), and sodium carboxymethyl cellulose (CMC-Na). The adhesive may include, for example, styrene butadiene rubber (SBR).

[0052] The electrolyte in the lithium ion battery is not particularly limited, and any electrolyte known in the art can be used. The electrolyte may be in any state of gel, solid, or liquid. For example, the liquid electrolyte contains a lithium salt and a non-aqueous solvent.

[0053] The lithium salt is not particularly limited, and any lithium salt known in the art can be used as long as the object of the present invention can be achieved. The lithium salt may include at least one selected from the group consisting of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, and LiPO2F2. The lithium salt may be, for example, LiPF6.

[0054] The non-aqueous solvent is not particularly limited as long as the object of the present invention can be achieved. The non-aqueous solvent may include, for example, at least one selected from the group consisting of carbonate compounds, carboxylate compounds, ether compounds, nitrile compounds, and other organic solvents.

[0055] Examples of the carbonate compound include diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, The fluoroethylene carbonate may contain at least one selected from the group consisting of 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, and trifluoromethylethylene carbonate.

[0056] The present invention is not particularly limited to the preparation method of the electrochemical device, and any preparation method known in the art can be used. For example, nanofibers and polymer particles are deposited on one or both sides of a positive or negative electrode piece to form a porous substrate made of nanofibers and polymer particles filled in the porous substrate.

[0057] Alternatively, nanofibers, polymeric particles and inorganic particles are deposited on one or both sides of a positive or negative electrode piece to form a porous substrate comprised of nanofibers, and polymeric and inorganic particles filled into the porous substrate.

[0058] The method of depositing the nanofibers, polymer particles, and / or inorganic particles is not particularly limited, and any method known in the art can be used. For example, the porous substrate is prepared by electrospinning, air spinning, centrifugal spinning, electroblowing, meltblowing, flash evaporation, or coating. The polymer particles and / or inorganic particles are prepared by electrodeposition, printing, coating, spin coating, or immersion. The order of depositing the nanofibers, polymer particles, and / or inorganic particles is not particularly limited, as long as it is possible to form the separation layer of the present invention, which includes a porous substrate made of nanofibers and polymer particles and / or inorganic particles distributed on the porous substrate. For example, the nanofibers and the polymer particles and / or inorganic particles can be deposited simultaneously or alternately.

[0059] 7 is a schematic diagram of the electrospinning process of the present invention. An electrospinning apparatus 50 deposits nanofibers onto an electrode surface to form a separating layer 10.

[0060] FIG. 8 is a schematic diagram of an embodiment of preparing a separation layer of the present invention, in which an electrospinning device 50 and an electrodeposition device 60 deposit nanofibers and polymer particles onto an electrode surface, respectively, and both the electrospinning device 50 and the electrodeposition device 60 are connected to a voltage regulator 70.

[0061] The porous substrate is not particularly limited, and can be carried out using any spinning device known in the art as long as it can achieve the object of the present invention. The electrospinning method can be carried out using any electrospinning device known in the art, for example, the electrospinning device may be an Elite series manufactured by Yongkang Le Industry. The air spinning method can be carried out using any air spinning device known in the art, for example, the air spinning device may be an air jet spinning machine manufactured by Nanjing Azimuth New Materials. The centrifugal spinning method can be carried out using any centrifugal spinning device known in the art, for example, the centrifugal spinning device may be a centrifugal spinning machine manufactured by Sichuan Riken Science and Technology. The electrodeposition method is not particularly limited, and can be carried out using any device known in the art as long as it can achieve the object of the present invention. The electrospray method can be carried out using any electrospray device known in the art, for example, an electrospray device manufactured by Summer, France.

[0062] The present invention further provides an electronic device comprising an electrochemical device according to the present invention.

[0063] The electronic device described in the present invention refers to common electronic devices in the art, such as notebook computers, mobile phones, electric motorcycles, electric cars, electric toys, and the like.

[0064] The terms used in the present invention are generally those commonly used by those skilled in the art, and in the case of any discrepancy with the commonly used terms, the terms in the present invention shall prevail.

[0065] Specifically, in the present invention, the following terms have the following meanings:

[0066] Cross-sectional porosity: The percentage of the void area in any cross section perpendicular to the surface of the separation layer to the total cross-sectional area.

[0067] Surface Open Area: The percentage of the surface area of ​​the open pores on the surface of the separating layer relative to the total surface area of ​​the surface of the separating layer.

[0068] Number of polymer particles: the total number of polymer particles per unit area of ​​the separating layer.

[0069] Average particle size of polymer particles: The average particle size of polymer particles is indicated by D50, where D represents the diameter of the polymer particles, and D50 is the particle size at which the cumulative particle size distribution percentage of the polymer particles reaches 50% based on the volume distribution, which physically means that particles smaller than this particle size account for 50%, and particles larger than this particle size also account for 50%.

[0070] Measurement method: Method for measuring the pore closing temperature of the separation layer A sample of a positive electrode current collector containing an active material on one side + a separation layer + a negative electrode current collector containing an active material on the other side was wetted with an electrolyte. Here, the active material was adjacent to the separation layer. The contacts of a multi-path temperature measuring instrument were placed on the separation layer. The combination was placed on a measuring fixture plate, a pressure of 10 MPa was applied, and the mixture was connected to an AC impedance measuring instrument, and then placed in an oven at 50°C and heated at a rate of 2°C / min. The temperature at which the resistance reached 1000Ω was recorded as the pore closing temperature of the separation layer.

[0071] Measurement method for the rupture temperature of the separation layer A sample of a positive electrode current collector containing active material on one side + a separation layer + a negative electrode current collector containing active material on the other side was placed on a measurement fixture plate, and the contacts of a multi-path temperature measuring device were placed on the separation layer. Then, a pressure of 10 MPa was applied and connected to an electrical conductivity measuring device. The sample was then placed in a 50°C oven and heated at a rate of 2°C / min. The temperature at which electrical conductivity appeared was the rupture temperature of the separation layer.

[0072] 1C-1.5U (where U is the cut-off voltage) 1h overcharge performance measurement method The lithium-ion battery was discharged to 3.0V, then charged at a constant current of 1C to 1.5U, and then charged at a constant voltage for 1 hour. If the battery did not ignite or explode, it was deemed to have passed the test and was marked as "pass."

[0073] 150℃, 1h Hotbox performance measurement method A fully charged lithium-ion battery was placed in an oven, and the oven was heated to 150°C at a rate of 5±2°C / min. The temperature was then increased for 1 hour and then stopped. If the battery did not ignite or explode, it was deemed to have passed the test and was noted as "pass."

[0074] Method for measuring the porosity ε of the separation layer The porosity ε of the separation layer is calculated by the weight M 分離層 and volume V 分離層 , the mass fraction w of the porous substrate and the polymer particles in the separation layer 多孔質基体 and w 重合体粒子 , and their densities ρ 多孔質基体 and ρ 重合体粒子 It was obtained by converting ε=(V 分離層 -V 多孔質基体 -V 重合体粒子 ) / V 分離層 *100%, where V 多孔質基体 =M 分離層 *w 多孔質基体 / ρ 多孔質基体 , V 重合体粒子 =M 分離層 *w 重合体粒子 / ρ 重合体粒子 .

[0075] Method for measuring cross-sectional porosity β The cross section of the prepared separation layer was observed under a scanning electron microscope with a certain number of lattice standards arranged, a unit area was selected, and the lattices covering the voids were counted. The ratio of the area of ​​the lattices covering the voids to the selected area was the cross-sectional porosity β1 of the separation layer. This method was repeated, and unit areas at different positions of different cross sections of the separation layer were selected to measure the cross-sectional porosity, and the cross-sectional porosities were respectively β2, β3, β4...β n Therefore, the cross-sectional porosity β of the separation layer is β1, β2, β3, β4... β n The average value of β(%)=n / (β1+β2+β3+β4+……+β n ) was.

[0076] Measuring method of surface porosity α The measured separation layer was observed under a scanning electron microscope with a certain number of lattice standards arranged thereon, a unit area was selected, and the lattices covering the pores were counted therein. The ratio of the area of ​​the lattices covering the pores to the selected area was the surface porosity α1 of the separation layer. This method was repeated by selecting unit areas at different positions on the surface of the separation layer to measure the surface porosity, and the surface porosity was calculated as α2, α3, α4...α n Therefore, the surface porosity α of the separation layer is α1, α2, α3, α4...α n The average value of α(%)=n / (α1+α2+α3+α4+……+α n ) was.

[0077] How to measure the self-discharge rate K value of lithium-ion batteries The lithium-ion battery was discharged at 0.5C to 3.0V and left to stand for 5 minutes. The lithium-ion battery was then charged at a constant current of 0.5C to 3.85V, and then charged at a constant voltage of 0.05C at 3.85V, and left to stand for 2 days in an environment of 25°C ± 3°C, and the voltage at that time was measured and recorded as OCV1. The lithium-ion battery was then left to stand for 2 days at room temperature, and the voltage at that time was measured and recorded as OCV2. The K value was obtained by the formula: K(mV / h)=(OCV2-OCV1) / 48h*1000.

[0078] Measurement method for discharge capacity after 50 charge / discharge cycles / initial discharge capacity η Charge the lithium-ion battery at a constant current of 0.5C to 4.4V, then charge it at a constant voltage of 4.4V until the current reaches 0.05C, leave it at 25℃±3℃ for 10 minutes, then discharge it at a constant current of 0.5C to 3.0V, and measure the initial discharge capacity as Q 1D Repeat this cycle for 50 cycles and record the discharge capacity as Q 50D The capacity retention rate after 50 charge / discharge cycles is η(%)=Q 50D / Q 1D *It was 100%.

[0079] Working Example Preparation Example 1: Preparation of negative electrode pieces The negative electrode active materials, graphite, conductive carbon black (Super P), and styrene butadiene rubber (SBR), were mixed in a weight ratio of 96:1.5:2.5, and deionized water (H2O) was added as a solvent to prepare a slurry with a solid content of 0.7, which was then uniformly stirred. The slurry was uniformly coated on one side of a copper foil with a thickness of 8 μm as a negative electrode current collector, and dried at 110°C to obtain a negative electrode piece with a coating layer of 130 μm thickness on one side of which the negative electrode active material was applied. The above steps were repeated on the other side of the negative electrode piece to obtain a negative electrode piece with the negative electrode active material applied on both sides. The piece was then cut into a size of 41 mm x 61 mm and set aside until it was used in the subsequent step.

[0080] Preparation Example 2: Preparation of Positive Electrode Pieces The positive electrode active materials, lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and polyvinylidene fluoride (PVDF), were mixed in a weight ratio of 97.5:1.0:1.5, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 0.75, which was then uniformly stirred. The slurry was uniformly coated on one side of a 10 μm thick aluminum foil as a positive electrode current collector, and dried at 90 °C to obtain a positive electrode piece with a coating layer thickness of 110 μm. The above steps were repeated on the other side of the aluminum foil as the positive electrode current collector to obtain a positive electrode piece coated on both sides. After coating was completed, the pole piece was cut into a size of 38 mm x 58 mm and set aside until it was used in the subsequent step.

[0081] Preparation example 3: Electrolyte preparation First, in a dry argon gas atmosphere, organic solvents ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a mass ratio of EC:EMC:DEC = 30:50:20, and then lithium hexafluorophosphate (LiPF6) was dissolved in the organic solvent and mixed uniformly to obtain an electrolyte solution with a lithium salt concentration of 1.15 M. The following examples are given to illustrate the preparation of the integrated separation layer of the porous substrate + polymer particles made of nanofibers of the present invention. These examples are described using a positive electrode piece as an example. In these examples, an integrated separation layer is deposited on both sides of the positive electrode piece. It should be understood that the integrated separation layer may be deposited on both sides of the negative electrode piece, and one integrated separation layer may be deposited on one side of the positive electrode piece and one side of the negative electrode piece, respectively. These embodiments can similarly achieve the object of the present invention. Those skilled in the art should understand that these embodiments are also within the scope of protection of the present invention.

[0082] Example 1 Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. On one side of the positive electrode piece obtained in Preparation Example 2, solution A was used as a raw material to prepare a porous substrate made of PVDF fibers by electrospinning. At the same time as spinning, suspension B was used as a raw material to spray-coat low-melting polyethylene (PE) particles by electrospraying to form a 10 μm thick integrated separation layer of the porous substrate made of fibers and the low-melting polymer, and the low-melting polymer particles were distributed in the porous substrate made of fibers by filling. Here, the average diameter of the fibers was 100 nm. The average particle diameter of the selected low-melting polyethylene (PE) particles was 500 nm, the ratio of the average pore diameter of the porous substrate to the average particle diameter of the low-melting polyethylene (PE) particles was 1:2.5, that is, the average pore diameter of the porous substrate made of fibers was 200 nm, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 95:5, and the porosity of the separation layer was 75%. The separation layer had a cross-sectional porosity β of 53%, a surface porosity α of 88%, and a cross-sectional porosity / surface porosity ratio β / α of 60%. The other surface of the positive electrode piece was then subjected to the same steps, and vacuum dried at 40° C. to remove the dispersant and solvent such as DMF, thereby obtaining a positive electrode piece having a separation layer applied on both surfaces.

[0083] Example 2 As shown in Table 1, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 80:20, and the cross-sectional porosity β of the separation layer was 56%, the surface porosity α was 80%, and the cross-sectional porosity / surface porosity ratio β / α was 70%, except for this, the same as in Example 1.

[0084] Example 3 As shown in Table 1, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 65:35, and the cross-sectional porosity β of the separation layer was 60%, the surface porosity α was 75%, and the cross-sectional porosity / surface porosity ratio β / α was 80%, except for which the same procedure was followed as in Example 1.

[0085] Example 4 As shown in Table 1, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 35:65, and the cross-sectional porosity β of the separation layer was 50%, the surface porosity α was 65%, and the cross-sectional porosity / surface porosity ratio β / α was 77%, except for this, the same as in Example 1.

[0086] Example 5 As shown in Table 1, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 5:95, and the cross-sectional porosity β of the separation layer was 35%, the surface porosity α was 40%, and the cross-sectional porosity / surface porosity ratio β / α was 88%, except for which the same procedure was followed as in Example 1.

[0087] Example 6 The same procedure was followed as in Example 3, except that the porous substrate material made of fibers was changed to PI.

[0088] Example 7 The same procedure was followed as in Example 3, except that the porous substrate material made of fibers was changed to PAN.

[0089] Example 8 The same procedure was followed as in Example 3, except that the polymer particle material was ABS.

[0090] Example 9 The same procedure was followed as in Example 3, except that the polymer particle material was changed to PVB.

[0091] Example 10 As shown in Table 1, the same procedures as in Example 3 were carried out except that the average particle size of the polymer particles was 200 nm, the cross-sectional porosity β of the separation layer was 55%, the surface porosity α was 70%, and the cross-sectional porosity / surface porosity ratio β / α was 78%, so that the ratio of the pore size of the porous substrate made of fibers to the average particle size of the polymer particles was 1:1.

[0092] Example 11 As shown in Table 1, the same procedure as in Example 3 was followed except that the average particle size of the polymer particles was 1000 nm, the cross-sectional porosity β of the separation layer was 60%, the surface porosity α was 80%, and the cross-sectional porosity / surface porosity ratio β / α was 75%, so that the ratio of the pore size of the porous substrate made of fibers to the average particle size of the polymer particles was 1:5.

[0093] Example 12 As shown in Table 1, the same procedure as in Example 3 was followed except that the average particle size of the polymer particles was 3000 nm, the cross-sectional porosity β of the separation layer was 65%, the surface porosity α was 85%, and the cross-sectional porosity / surface porosity ratio β / α was 75%, so that the ratio of the pore size of the porous substrate made of fibers to the average particle size of the polymer particles was 1:15.

[0094] Example 13 As shown in Table 1, the pore size of the porous substrate made of fibers was 40 nm, the fiber diameter was 10 nm, the average particle size of the polymer particles was 10,000 nm, and the cross-sectional porosity β of the separation layer was 60%, the surface porosity α was 75%, and the cross-sectional porosity / surface porosity ratio β / α was 80%, except for these, the same as in Example 3.

[0095] Example 14 As shown in Table 1, the pore size of the porous substrate made of fibers was 1000 nm, the fiber diameter was 400 nm, the average particle size of the polymer particles was 5000 nm, and the cross-sectional porosity β of the separation layer was 65%, the surface porosity α was 80%, and the cross-sectional porosity / surface porosity ratio β / α was 81%, except for which the same procedures were followed as in Example 3.

[0096] Example 15 As shown in Table 1, the pore size of the porous substrate made of fibers was 40 nm, the fiber diameter was 20 nm, the average particle size of the polymer particles was 40 nm, and the cross-sectional porosity β of the separation layer was 50%, the surface porosity α was 70%, and the cross-sectional porosity / surface porosity ratio β / α was 71%, except for these, the same as in Example 3.

[0097] Example 16 As shown in Table 1, the same procedure as in Example 11 was used except that the thickness of the separation layer was 5 μm, the cross-sectional porosity β of the separation layer was 65%, the surface porosity α was 80%, and the cross-sectional porosity / surface porosity ratio β / α was 81%.

[0098] Example 17 As shown in Table 1, the same procedure as in Example 11 was followed except that the porosity of the separation layer was 30%, the cross-sectional porosity β of the separation layer was 25%, the surface porosity α was 35%, and the cross-sectional porosity / surface porosity ratio β / α was 71%.

[0099] Example 18 As shown in Table 1, the same procedure as in Example 11 was used except that the porosity of the separation layer was 30%, the cross-sectional porosity β of the separation layer was 80%, the surface porosity α was 85%, and the cross-sectional porosity / surface porosity ratio β / α was 94%.

[0100] Example 19 The same procedure was followed as in Example 11, except that the low-melting point polymer particle material was changed to EVA with a melting point of 70°C, and the cross-sectional porosity β of the separation layer was 65%, the surface open area α was 80%, and the cross-sectional porosity / surface open area ratio β / α was 81%.

[0101] Example 20 The same procedure was followed as in Example 11, except that the low-melting point polymer particle material was changed to PP with a melting point of 150°C, and the cross-sectional porosity β of the separation layer was 65%, the surface porosity α was 80%, and the cross-sectional porosity / surface porosity ratio β / α was 81%.

[0102] Example 21 Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. On one side of the positive electrode piece obtained in Preparation Example 2, solution A was used as a raw material to prepare a porous substrate made of PVDF fibers by electrospinning. At the same time as spinning, suspension B was used as a raw material to spray-coat low-melting polyethylene (PE) particles on the same surface of the positive electrode piece by electrospraying to form a 10 μm thick integrated separation layer of the porous substrate made of fibers + low-melting polymer, and the low-melting polymer particles were distributed in the porous substrate made of fibers in a filling manner. Here, the average diameter of the fibers was 100 nm. The average particle diameter of the selected low-melting polyethylene (PE) particles was 10000 nm, the ratio of the average pore diameter of the porous substrate made of fibers to the average particle diameter of the low-melting polyethylene (PE) particles was 1:50, that is, the average pore diameter of the porous substrate made of fibers was 200 nm, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 95:5, and the porosity of the separation layer was 90%. The number of the polymer particles per unit area of ​​the porous substrate is 1×10 8 / m 2 The cross-sectional porosity β of the separation layer was 75%, the surface porosity α was 90%, and the cross-sectional porosity / surface porosity ratio β / α was 83%. The other surface of the positive electrode piece was then subjected to the same steps, and then vacuum dried at 40° C. to remove the dispersant and solvent such as DMF, thereby obtaining a positive electrode piece having a separation layer applied on both surfaces.

[0103] Example 22 Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. A porous substrate made of PVDF fibers was prepared on one side of the positive electrode piece obtained in Preparation Example 2 by electrospinning using solution A as a raw material. At the same time as spinning, low melting point polyethylene (PE) particles were spray-coated by electrospray using suspension B as a raw material to form a 20 μm thick integrated separation layer of the porous substrate made of fibers and the low melting point polymer, and the low melting point polymer particles were distributed in the porous substrate made of fibers by filling. Here, the average diameter of the fibers was 10 nm. The average particle diameter of the selected low melting point polyethylene (PE) particles was 40 nm, and the ratio of the average pore diameter of the fiber substrate to the average particle diameter of the low melting point polyethylene (PE) particles was 1:1, that is, the average pore diameter of the porous substrate made of fibers was 40 nm, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 5:95, and the porosity of the separation layer was 30%. The number of the polymer particles per unit area of ​​the porous substrate was 4×10 17 / m 2 The cross-sectional porosity β of the separation layer was 25%, the surface porosity α was 45%, and the cross-sectional porosity / surface porosity ratio β / α was 56%. The other surface of the positive electrode piece was then subjected to the same steps, and then vacuum dried at 40° C. to remove the dispersant and solvent such as DMF, thereby obtaining a positive electrode piece having a separation layer applied on both surfaces.

[0104] Example 23 Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. A porous substrate made of PVDF fibers was prepared on one side of the positive electrode piece obtained in Preparation Example 2 by electrospinning using solution A as a raw material. At the same time as spinning, low melting point polyethylene (PE) particles were spray-coated by electrospray using suspension B as a raw material to form a 1 μm thick integrated separation layer of the porous substrate made of fibers and the low melting point polymer, and the low melting point polymer particles were distributed in the porous substrate made of fibers by filling. Here, the average diameter of the fibers was 100 nm. The average particle diameter of the selected low melting point polyethylene (PE) particles was 1000 nm, the ratio of the average pore diameter of the fiber substrate to the average particle diameter of the low melting point polyethylene (PE) particles was 1:5, that is, the average pore diameter of the porous substrate made of fibers was 200 nm, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 95:5, and the porosity of the separation layer was 90%. The weight of the polymer particles per unit area of ​​the porous substrate was 0.004 g / m 2 The cross-sectional porosity β of the separation layer was 70%, the surface porosity α was 85%, and the cross-sectional porosity / surface porosity ratio β / α was 82%. The other surface of the positive electrode piece was then subjected to the same steps, and then vacuum dried at 40° C. to remove the dispersant and solvent such as DMF, thereby obtaining a positive electrode piece having a separation layer applied to both surfaces.

[0105] Example 24 Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. A porous substrate made of PVDF fibers was prepared on one side of the positive electrode piece obtained in Preparation Example 2 by electrospinning using solution A as a raw material. At the same time as spinning, low melting point polyethylene (PE) particles were spray-coated by electrospray using suspension B as a raw material to form a 20 μm thick integrated separation layer of the porous substrate made of fibers and the low melting point polymer, and the low melting point polymer particles were distributed in the porous substrate made of fibers by filling. Here, the average diameter of the fibers was 10 nm. The average particle diameter of the selected low melting point polyethylene (PE) particles was 40 nm, and the ratio of the average pore diameter of the fiber substrate to the average particle diameter of the low melting point polyethylene (PE) particles was 1:1, that is, the average pore diameter of the porous substrate made of fibers was 40 nm, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 5:95, and the porosity of the separation layer was 30%. The weight of the polymer particles per unit area of ​​the porous substrate was 20 g / m 2 The cross-sectional porosity β of the separation layer was 25%, the surface porosity α was 45%, and the cross-sectional porosity / surface porosity ratio β / α was 56%. The other surface of the positive electrode piece was then subjected to the same steps, and then vacuum dried at 40° C. to remove the dispersant and solvent such as DMF, thereby obtaining a positive electrode piece having a separation layer applied on both surfaces.

[0106] Example 25 Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. On one side of the positive electrode piece obtained in Preparation Example 2, solution A was used as a raw material to prepare a porous substrate made of PVDF fibers by electrospinning. At the same time as spinning, suspension B was used as a raw material to spray-coat low-melting polyethylene (PE) particles by electrospraying to form a 20 μm thick integrated separation layer of the porous substrate made of fibers + low-melting polymer, and the low-melting polymer particles were distributed in the porous substrate made of fibers by filling. Here, the average diameter of the fibers was 100 nm. The average particle diameter of the selected low-melting polyethylene (PE) particles was 10000 nm, and the ratio of the average pore diameter of the fiber substrate to the average particle diameter of the low-melting polyethylene (PE) particles was 1:1, that is, the average pore diameter of the porous substrate made of fibers was 10000 nm, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 65:35, and the porosity of the separation layer was 75%. The cross-sectional porosity β of the separation layer was 60%, the surface porosity α was 80%, and the cross-sectional porosity / surface porosity ratio β / α was 75%. Here, the height of the polymer particles protruding from the surface of the porous substrate made of fibers was 5000 nm. The above steps were then repeated on the other side of the positive electrode piece, and then vacuum dried at 40°C to remove the dispersant and solvent such as DMF, thereby obtaining a positive electrode piece with a separation layer applied on both sides.

[0107] Example 26 Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. On one side of the positive electrode piece obtained in Preparation Example 2, solution A was used as a raw material to prepare a porous substrate made of PVDF fibers by electrospinning. At the same time as spinning, suspension B was used as a raw material to spray-coat low-melting polyethylene (PE) particles by electrospraying to form a 20 μm thick integrated separation layer of the porous substrate made of fibers + low-melting polymer, and the low-melting polymer particles were distributed in the porous substrate made of fibers by filling. Here, the average diameter of the fibers was 1000 nm. The average particle diameter of the selected low-melting polyethylene (PE) particles was 10000 nm, the ratio of the average pore diameter of the fiber substrate to the average particle diameter of the low-melting polyethylene (PE) particles was 1:5, that is, the average pore diameter of the porous substrate made of fibers was 2000 nm, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 5:95, and the porosity of the separation layer was 30%. The cross-sectional porosity β of the separation layer was 25%, the surface porosity α was 35%, and the cross-sectional porosity / surface porosity ratio β / α was 71%. Here, the surface area of ​​the surface of the separation layer occupied by the polymer particles was 60%. The above steps were then repeated on the other side of the positive electrode piece, and then vacuum dried at 40°C to remove the dispersant and solvent such as DMF, thereby obtaining a positive electrode piece with a separation layer applied on both sides.

[0108] Example 27 Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. On one side of the positive electrode piece obtained in Preparation Example 2, solution A was used as a raw material to prepare a porous substrate made of PVDF fibers by electrospinning. At the same time as spinning, suspension B was used as a raw material to spray-coat low-melting polyethylene (PE) particles by electrospraying to form a 10 μm thick integrated separation layer of the porous substrate made of fibers + low-melting polymer, and the low-melting polymer particles were distributed in the porous substrate made of fibers by filling. Here, the average diameter of the fibers was 100 nm. The average particle diameter of the selected low-melting polyethylene (PE) particles was 1000 nm, and the ratio of the average pore diameter of the fiber substrate to the average particle diameter of the low-melting polyethylene (PE) particles was 1:5, that is, the average pore diameter of the porous substrate was 200 nm. The ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 65:35, the porosity of the separation layer was 50%, the cross-sectional porosity β of the separation layer was 45%, the surface porosity α was 60%, and the cross-sectional porosity / surface porosity ratio β / α was 75%. The other side of the positive electrode piece was then subjected to the same steps, and vacuum dried at 40°C to remove the dispersant and solvent such as DMF, thereby obtaining a positive electrode piece having a separation layer applied to both sides.

[0109] Example 28 Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. On one side of the positive electrode piece obtained in Preparation Example 2, solution A was used as a raw material to prepare a porous substrate made of PVDF fibers by electrospinning. At the same time as spinning, suspension B was used as a raw material to spray-coat low-melting polyethylene (PE) particles by electrospraying to form a 20 μm thick integrated separation layer of the porous substrate made of fibers and the low-melting polymer, and the low-melting polymer particles were distributed in the porous substrate made of fibers by filling. Here, the average diameter of the fibers was 100 nm. The average particle diameter of the selected low-melting polyethylene (PE) particles was 10000 nm, and the ratio of the average pore diameter of the fiber substrate to the average particle diameter of the low-melting polyethylene (PE) particles was 1:2.5, that is, the average pore diameter of the porous substrate was 4000 nm, and the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 95:5. The porosity of the separation layer was 90%. The cross-sectional porosity β of the separation layer was 85%, the surface porosity α was 90%, and the cross-sectional porosity / surface porosity ratio β / α was 94%. The above steps were then repeated on the other side of the positive electrode piece, followed by vacuum drying at 40° C. to remove the dispersant and solvent such as DMF, thereby obtaining a positive electrode piece coated with a separation layer on both sides.

[0110] Example 29 Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. On one side of the positive electrode piece obtained in Preparation Example 2, solution A was used as a raw material to prepare a porous substrate made of PVDF fibers by electrospinning. At the same time as spinning, suspension B was used as a raw material to spray-coat low-melting polyethylene (PE) particles by electrospraying to form a 10 μm thick integrated separation layer of the porous substrate made of fibers and the low-melting polymer, and the low-melting polymer particles were distributed in the porous substrate made of fibers by filling. Here, the average diameter of the fibers was 100 nm. The average particle diameter of the selected low-melting polyethylene (PE) particles was 1000 nm, the ratio of the average pore diameter of the fiber substrate to the average particle diameter of the low-melting polyethylene (PE) particles was 1:2.5, that is, the average pore diameter of the porous substrate was 400 nm, the ratio of the content of the porous substrate material made of fibers to the polymer particles was 65:35, and the porosity of the separation layer was 75%. Here, the cross-sectional porosity β of the separation layer was 40%, the surface porosity α was 80%, and the cross-sectional porosity / surface porosity ratio β / α was 50%. The above steps were then repeated on the other side of the positive electrode piece, followed by vacuum drying at 40°C to remove the dispersant and solvent such as DMF, thereby obtaining a positive electrode piece with a separation layer applied on both sides.

[0111] Example 30 Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, obtaining solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, obtaining suspension B with a mass fraction of 40%. Inorganic particles, alumina (Al2O3) and polyvinylidene fluoride (PVDF) were mixed in a weight ratio of 90:10, and N-methylpyrrolidone (NMP) was added as a solvent to prepare slurry C with a solid content of 40%. On one side of the positive electrode piece obtained in Preparation Example 2, solution A was used as a raw material to prepare a porous substrate made of PVDF fibers by electrospinning, and at the same time, suspension B and slurry C were used as raw materials to spray coat low-melting polyethylene (PE) particles and inorganic particles, alumina (Al2O3), by electrospraying, to form an integrated separation layer of 10 μm thick of the porous substrate made of PVDF fibers + low-melting polymer + inorganic particles, and the low-melting polymer particles and inorganic particles were embedded in the pores of the porous substrate made of fibers. Here, the average diameter of the fibers was 100 nm. The average particle size of the selected low melting polyethylene (PE) particles was 1000 nm, the ratio of the average pore size of the fiber substrate to the average particle size of the low melting polyethylene (PE) particles was 1:5, that is, the average pore size of the porous substrate was 200 nm, the average particle size of the selected inorganic ceramic (Al2O3) particles was 400 nm, the weight ratio of the porous substrate material made of fibers to the polymer particles and the inorganic particles was 60:30:10, and the porosity of the separation layer was 70%. The cross-sectional porosity β of the separation layer was 55%, the surface porosity α was 70%, and the cross-sectional porosity / surface porosity ratio β / α was 79%. Then, the above steps were repeated on the other side of the positive electrode piece, and then vacuum dried under a condition of 40°C to remove the dispersant and solvent such as DMF, to obtain a positive electrode piece coated with a separation layer on both sides.

[0112] Example 31 Preparation of positive electrode pieces Conductive carbon black (Super P) and styrene butadiene rubber (SBR) were mixed in a weight ratio of 97:3, deionized water (H2O) was added as a solvent, and a slurry with a solid content of 0.85 was prepared and stirred uniformly. The slurry was uniformly applied to an aluminum foil positive electrode current collector and dried at 110°C to obtain a positive electrode undercoating layer. The positive electrode active materials, lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and polyvinylidene fluoride (PVDF), were mixed in a weight ratio of 97.5:1.0:1.5, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 0.75, which was then uniformly stirred. The slurry was uniformly applied to an aluminum foil positive electrode current collector coated with an undercoating layer, and dried at 90°C to obtain a positive electrode piece. After coating was completed, the piece was cut into pieces of 38 mm x 58 mm and set aside for use in the subsequent steps. Polyvinylidene fluoride (PVDF) was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. Low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. On one side of the positive electrode piece prepared in this embodiment, solution A is used as raw material to prepare a porous substrate made of PVDF fiber by electrospinning, and at the same time, suspension B is used as raw material to spray-coat low-melting polyethylene (PE) particles by electrospraying to form a 10 μm thick integrated separation layer of the porous substrate made of fiber + low-melting polymer, and the low-melting polymer particles are distributed in the porous substrate made of fiber by filling. Here, the average diameter of the fiber is 100 nm. The average particle size of the selected low melting polyethylene (PE) particles was 1000 nm, the ratio of the average pore size of the fiber substrate to the average particle size of the low melting polyethylene (PE) particles was 1:5, that is, the average pore size of the porous substrate was 200 nm, the ratio of the content of the porous substrate material made of fibers to the content of the polymer particles was 65:35, the cross-sectional porosity β of the separation layer was 65%, the surface porosity α was 80%, and the cross-sectional porosity / surface porosity ratio β / α was 81%.Then, the above steps were repeated on the other side of the positive electrode piece, and then vacuum dried under a condition of 40°C to remove the dispersant and solvent such as DMF, to obtain a positive electrode piece coated with a separation layer on both sides.

[0113] Preparation of Li-ion batteries As shown in Figure 2, the negative electrode piece prepared in Preparation Example 1 and the positive electrode piece with a separator prepared in each Example were stacked facing each other. After fixing the four corners of the entire laminate structure with tape, it was placed in an aluminum plastic film, and the electrolyte obtained in Preparation Example 3 was injected through a top and side seal, and then sealed to obtain a lithium ion laminate battery. The data and measurement results of each example are shown in Tables 1, 2 and 3.

[0114] Comparative Example 1 A 15 μm thick polyethylene (PE) was selected as a separator and placed between the negative electrode pieces and the positive electrode pieces prepared in Preparation Examples 1 and 2. The negative electrode pieces, the positive electrode pieces, and the separator were stacked facing each other. After fixing the four corners of the entire laminate structure with tape, it was placed in an aluminum plastic film, and the electrolyte obtained in Preparation Example 3 was injected through a top side seal and sealed, and then a lithium ion laminate battery was obtained.

[0115] Comparative Example 2 PVDF was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent, and stirred uniformly until the viscosity of the slurry stabilized, to obtain a solution A with a mass fraction of 25%. On one side of the positive electrode piece prepared in Preparation Example 2, solution A was used as a raw material to prepare a single layer of PVDF nonwoven fabric fiber layer with a thickness of 10 μm by electrospinning, the fiber layer had a diameter of 100 nm, an average pore size of 200 nm, and a porosity of 75%. The above steps were then repeated on the other side of the positive electrode piece, and the dispersant of the polymer coating layer was dried under a condition of 90° C. to obtain a positive electrode piece with a PVDF nonwoven fabric fiber layer on both sides. As shown in Fig. 2, the positive electrode piece was placed opposite the negative electrode piece prepared in Preparation Example 1 and overlapped. After fixing the four corners of the entire laminate structure with tape, it was placed in an aluminum plastic film, and the electrolyte solution obtained in Preparation Example 3 was injected through a top and side seal, and then sealed to obtain a lithium-ion laminate battery.

[0116] Comparative Example 3 A 15 μm thick polyethylene (PE) was selected as the separator. Low melting point polyethylene (PE) particles were dispersed in N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, to obtain suspension B with a mass fraction of 40%. A 5 μm thick low melting point polyethylene (PE) particle coating layer was prepared on the surface of the polyethylene separator by electrospraying, where the average particle diameter of the particles was 500 nm. The total thickness of the separation layer was 20 μm, and the porosity of the entire separation layer was 30%. The integrated separation layer containing the prepared low melting point polymer particle coating layer was placed between the negative electrode pieces and the positive electrode pieces prepared in Preparation Examples 1 and 2. The negative electrode pieces, the positive electrode pieces, and the separation layer were stacked facing each other. After fixing the four corners of the entire laminate structure with tape, it was placed in an aluminum plastic film, and the electrolyte obtained in Preparation Example 3 was injected through a top side seal and sealed, and then a lithium ion laminate battery was obtained.

[0117] Comparative Example 4 PVDF was dispersed in a dimethylformamide (DMF) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a solution A with a mass fraction of 25%. At the same time, low-melting-point polyethylene (PE) particles were dispersed in an N-methylpyrrolidone (NMP) / acetone (7:3) solvent and stirred uniformly until the viscosity of the slurry stabilized, yielding a suspension B with a mass fraction of 40%. On one side of the positive electrode piece prepared in Preparation Example 2, solution A was used as a raw material to prepare a single layer of PVDF nonwoven fiber layer having a thickness of 10 μm by electrospinning, the average diameter of the fibers was 100 nm, and the average pore size of the porous substrate made of fibers was 200 nm. After spinning, suspension B was used as a raw material to prepare low-melting polyethylene (PE) particles on the surface of the porous substrate made of fibers by electrospraying, the average particle size of the selected low-melting polyethylene (PE) particles was 500 nm, the ratio of the average pore size of the porous substrate made of fibers to the average particle size of the low-melting polyethylene (PE) particles was 1:2.5, and the porosity of the entire separation layer was 75%. Then, the above steps were repeated on the other side of the positive electrode piece, and the dispersant such as DMF was removed, to obtain a positive electrode piece with separation layers on both sides. As shown in Fig. 2, the positive electrode piece was placed opposite the negative electrode piece prepared in Preparation Example 1 and overlapped. After fixing the four corners of the entire laminate structure with tape, it was placed in an aluminum plastic film, and the electrolyte solution obtained in Preparation Example 3 was injected through a top and side seal, and then sealed to obtain a lithium-ion laminate battery. The data and measurement results of Comparative Examples 1 to 4 are shown in Tables 1, 2 and 3.

[0118] [Table 1-1] [Table 1-2] [Table 1-3]

[0119] [Table 2-1] [Table 2-2]

[0120] [Table 3-1] [Table 3-2]

[0121] As can be seen from Tables 1, 2 and 3, compared with conventional separators, the integrated separation layer in which low melting point polymer particles are filled into a porous substrate made of nanofibers can reduce the thickness of the separation layer to improve energy density, improve the porosity of the separation layer to improve liquid retention capacity, accelerate reaction kinetics to improve electrical performance, improve the adhesion between the separation layer and the pole pieces to improve the mechanical abuse performance of the lithium ion battery, such as resistance to dropping, reduce the pore closing temperature of the separation layer, and improve the heat shrinkage resistance of the separation layer in high temperature environments, thereby improving the safety and stability of the lithium ion battery.

[0122] Compared with the heat-resistant spun separation layer, the separation layer of the present invention has a low-melting point polymer particle distributed in a porous substrate made of nanofibers, so that the separation layer of the present invention has a low-temperature thermal pore-closing function, and when thermal runaway occurs, the current can be cut off to improve the safety performance of the lithium-ion battery. In addition, the separation layer of the present invention has a low-melting point polymer particle filled in the "macropores" of the porous substrate made of fibers, so that the macropores in the pure heat-resistant spun separation layer are reduced, which further improves the self-discharge problem of the lithium-ion battery, reduces the K value, and improves the mechanical strength of the separation layer, thereby reducing the internal short circuit problem that occurs when the positive electrode active material particles or negative electrode active material particles penetrate the separation layer inside the lithium-ion battery, which is also advantageous for improving the cycle performance of the lithium-ion battery.

[0123] Compared with a two-layer structure such as a normal separator + a separation layer made of low melting point polymer particles, the integrated structure design reduces the thickness of the separation layer by half, greatly improving the volumetric energy density of the lithium-ion battery. At the same time, the porous substrate made of fibers has a high melting point and excellent high-temperature stability, which reduces the risk of the separation layer shrinking and even bursting at high temperatures, providing lithium-ion batteries with excellent safety performance. In addition, the integrated separation layer has a higher porosity, which accelerates the transport of ions, improves reaction kinetics, and improves the electrical performance of lithium-ion batteries.

[0124] Compared with a two-layer structure such as a heat-resistant spun layer + low-melting polymer particles, the integrated structure design effectively reduces the thickness of the separation layer, so that the lithium-ion battery has a higher volumetric energy density. At the same time, the low-melting polymer is filled into the porous fiber substrate, so that the response speed of melting and closing the pores is faster when thermal runaway occurs. In addition, the low-melting polymer fills the "macropores" in the porous fiber substrate, so the pore size distribution is optimized, the self-discharge problem of the lithium-ion battery is improved, the K value is reduced, and the mechanical strength of the porous fiber substrate is improved, and the resistance ability of the separation layer against the penetration of the positive and negative electrode particles is enhanced.

[0125] The above is merely a preferred embodiment of the present invention, and does not limit the scope of protection of the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention shall be included in the scope of protection of the present invention.

Claims

1. an electrode piece and a separation layer on at least one surface of the electrode piece, the separation layer comprising a porous substrate made of nanofibers and polymer particles distributed in the porous substrate, the melting temperature of the polymer particles being 70° C. to 150° C.; The average particle size of the polymer particles is 40 nm to 2 μm, a portion of the polymer particles protrudes from the surface of the porous substrate by a height of 0.1 nm to 20 nm, and a surface area of ​​the surface of the porous substrate occupied by the portion of the polymer particles is 5% to 60% of a total surface area of ​​the porous substrate; the ratio β / α of the cross-sectional porosity β of the separation layer to the surface porosity α of the separation layer is 71% or more and 90% or less, and the surface porosity α is 70% to 90%, The electrochemical device, wherein the separation layer has a thickness of 6 μm to 20 μm.

2. The number of the polymer particles in the separation layer is 1×10 8 / m 2 ~1×10 18 / m 2 2. The electrochemical device of claim 1 ,

3. 2. The electrochemical device of claim 1, wherein the nanofibers have a diameter of 10 nm to 400 nm, and the pore size of the porous substrate is 40 nm to 10 μm.

4. 2. The electrochemical device according to claim 1, wherein the polymer of the polymer particles includes at least one selected from the group consisting of polystyrene, polyethylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, acrylonitrile-butadiene-styrene, polylactic acid, polyvinyl chloride, polyvinyl butyral, and polyacrylate.

5. 2. The electrochemical device of claim 1, wherein the nanofibers comprise a polymer, the polymer comprising at least one selected from the group consisting of polyvinylidene fluoride, polyimide, polyamide, polyacrylonitrile, polyethylene glycol, polyethylene oxide, polyphenylene ether, polypropylene carbonate, polymethyl methacrylate, polyethylene terephthalate, poly(vinylidene fluoride-hexafluoropropylene), poly(vinylidene fluoride-co-chlorotrifluoroethylene), and derivatives thereof.

6. 2. The electrochemical device of claim 1, wherein the nanofibers comprise a polymer, the polymer comprising at least one selected from the group consisting of polyvinylidene fluoride, polyimide, polyamide, polyacrylonitrile, polyethylene glycol, polyethylene oxide, polyphenylene ether, polypropylene carbonate, polymethyl methacrylate, polyethylene terephthalate, and derivatives thereof.

7. The nanofibers further include inorganic particles, the inorganic particles being HfO 2 , SrTiO 3 , SiO 2 , Al 2 O 3 , MgO, CaO, NiO, BaO, ZnO, TiO 2 , ZrO 2 , SnO 2 , CeO 2 2. The electrochemical device according to claim 1, comprising at least one selected from the group consisting of boehmite, magnesium hydroxide and aluminum hydroxide.

8. The electrochemical device according to claim 1 , wherein the cross-sectional porosity β is between 50% and 80%.

9. An electronic device comprising an electrochemical device according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Composite lithium ion battery diaphragm and preparation method thereof

    CN104766938A

  • Separator for battery, and lithium secondary cell

    JP2008004438A

  • Heat-resistant ultrafine fibrous separation membrane and secondary battery utilizing the same

    JP2010500717A

  • Lithium ion secondary battery

    JP2011181195A

  • Separator and battery having the same

    JP2013004336A