Polyphenylene-based semipermeable membrane and method for producing same
A partially sulfonated polyphenylene resin membrane addresses the balance of chemical resistance, mechanical strength, and water permeability in nanofiltration, ensuring high performance and ion rejection.
Patent Information
- Application Number
- JP2020060684
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-30
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-03-30
AI Technical Summary
Existing nanofiltration membranes face challenges in achieving a balance between chemical resistance, mechanical strength, and water permeability, particularly in applications requiring resistance to chemicals and high processing flow rates.
A semipermeable membrane made of polyphenylene resin with a sulfonated layer ratio of 50% or less, specifically 5% to 40%, and a non-sulfonated second surface, is produced by partial sulfonation using sulfuric acid under controlled conditions.
The membrane achieves both chemical resistance, including chlorine, acid, and alkali resistance, along with high membrane strength and performance, while maintaining effective water permeability and ion rejection.
Smart Images

Figure 0007581642000002 
Figure 0007581642000003 
Figure 0007581642000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyphenylene-based semipermeable membrane and a method for producing the same. [Background technology]
[0002] Nanofiltration is a pressurized membrane separation process that excels at capturing dissolved molecules, heavy metal ions, and other small particles. Nanofiltration is one of the membrane separation techniques included in reverse osmosis, but it is a general term for membrane separation techniques that perform reverse osmosis using semipermeable membranes with solute permeability intermediate between reverse osmosis and ultrafiltration membranes.
[0003] Many nanofiltration membranes developed to date are organic membranes or organic and inorganic mixed membranes. In particular, most organic membranes are composite semipermeable membranes, and there are known ones having a separation functional layer in which a gel layer and a polymer are crosslinked on a porous support membrane, and ones having a separation functional layer in which a monomer is polycondensed on a porous support membrane. Among them, composite semipermeable membranes obtained by coating a separation functional layer made of a crosslinked polyamide obtained by an interfacial polycondensation reaction between a polyfunctional amine and a polyfunctional acid halide on a porous support membrane are widely used as separation membranes with high permeability and selective separation. For example, Patent Document 1 (JP Patent Publication 55-147106) discloses a sheet-like composite in which a thin film of polyamide crosslinked by an interfacial polycondensation reaction is formed on the surface of a porous support membrane. Furthermore, as a composite nanofiltration membrane exhibiting high water permeability and high fouling resistance, for example, Patent Document 2 (International Publication No. 1997 / 34686) discloses a nanofiltration membrane consisting of a support material having a layer made of polyamide and a separation layer in which the support material is coated with polyvinyl alcohol. Polyamide-based organic membranes such as those disclosed in Patent Documents 1 and 2 are widely used in seawater desalination, wastewater treatment, and other applications.
[0004] As a nanofiltration membrane with excellent resistance to alkali and chlorine, for example, Patent Document 3 (JP Patent Publication No. 2013-31836 A) discloses a separation membrane using a sulfonated polyarylene ether sulfone polymer. In Patent Document 3, it has been found that by using a sulfonated polyarylene ether sulfone polymer as the material of the nanofiltration membrane and controlling the position of the peak top derived from the bound water in the hydrated state of this membrane to a specific chemical shift value region, the sulfonic acid group in the membrane and the bound water interact well, thereby achieving both high levels of salt removal and water permeability. It has been shown that the separation membrane of the polymer has strong resistance to both alkaline and chlorine chemicals. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 55-147106 [Patent Document 2] International Publication No. 1997 / 34686 [Patent Document 3] JP 2013-31836 A Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, in the fields of industrial wastewater (wastewater) treatment, organic solvent recovery, pharmaceutical manufacturing, and the like, attempts have been made to reduce costs and improve productivity by using membrane separation technology. When using membrane separation for such purposes, emphasis is placed not only on separation characteristics and processing flow rate, but also on resistance to chemicals and mechanical strength. An object of the present invention is to provide a separation membrane that can solve the above-mentioned problems. [Means for solving the problem]
[0007] As a result of extensive investigations, the present inventors have found that the above problems can be solved by the means described below, and have arrived at the present invention.
[0008] That is, the present invention comprises the following configuration. 1. A semipermeable membrane made of a material containing a polyphenylene resin, The semipermeable membrane has at least a portion of a first surface that is sulfonated; A polyphenylene-based semipermeable membrane, in which, when the concentration distribution of sulfur element derived from sulfonic acid groups is measured by elemental analysis on a cross section in the thickness direction of the semipermeable membrane, the ratio of a sulfonated layer obtained by the following formula is 50% or less. Ratio of sulfonated layer (%) = thickness of sulfonated layer / (thickness of sulfonated layer + thickness of non-sulfonated layer) × 100 2. The polyphenylene-based semipermeable membrane according to 1, wherein the ratio is 5% or more and 40% or less. 3. A polyphenylene-based semipermeable membrane according to 1 or 2, wherein the second surface of the semipermeable membrane is not sulfonated. 4. The polyphenylene-based semipermeable membrane according to any one of 1 to 3, wherein the second surface of the semipermeable membrane has a sulfur element ratio of less than 0.1 atm %. 5. Sulfonation degree is 0.1×10 4 meq. / m 3 ~9.0×10 4 meq. / m 3 5. The polyphenylene-based semipermeable membrane according to any one of 1 to 4, 6. A method for producing a polyphenylene-based semipermeable membrane according to any one of 1 to 5, comprising contacting a first surface of a semipermeable membrane substrate produced from a material containing a polyphenylene-based resin with sulfuric acid for sulfonation treatment. 7. The method for producing a polyphenylene-based semipermeable membrane according to 6, wherein the sulfuric acid has a concentration of 90 to 98 wt %. 8. The method for producing a polyphenylene-based semipermeable membrane according to 6 or 7, wherein sulfuric acid is brought into contact with the first surface of the semipermeable membrane substrate while pressure is applied to the second surface side. Effect of the Invention
[0009] According to the present invention, by sulfonating a polyphenylene-based semipermeable membrane substrate under specific conditions, it is possible to obtain a semipermeable membrane that has both chemical resistance (chlorine resistance, acid resistance, alkali resistance), membrane performance and membrane strength. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a schematic diagram showing a sulfonated layer and a non-sulfonated layer. [Diagram 2] FIG. 2 is a schematic diagram showing a method for determining yield strength from a stress-strain curve in a tensile test. [Diagram 3] FIG. 2 is a schematic cross-sectional view in the thickness direction of the semipermeable membrane of the present invention. [Figure 4] 1 is an example of a cross-sectional SEM image in the thickness direction of a semipermeable membrane of the present invention. [Diagram 5] 1 is a graph showing an example of an analysis result by elemental analysis. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Below, a form for carrying out the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and it should be understood that design changes, improvements, etc. may be made as appropriate based on the ordinary knowledge of a person skilled in the art without departing from the spirit of the present invention.
[0012] In order to impart chemical resistance to the semipermeable membrane, it is desirable that the resin used as the raw material itself has excellent chemical resistance. Examples of such resins include polyphenylene-based resins such as polyphenylene ether resins, polyphenylene oxide resins, and polyphenylene sulfide resins. In the present invention, it is preferable to use a material containing a polyphenylene oxide resin in terms of excellent heat resistance, impact resistance, strength, and chemical resistance. However, since polyphenylene-based resins are hydrophobic, a membrane manufactured from a single polyphenylene-based resin has a problem of very low water permeability.
[0013] In order to improve the above problems, a hydrophilization treatment is required for the polyphenylene-based semipermeable membrane. Possible hydrophilization treatments include the introduction of hydrophilic groups (e.g., sulfonic acid groups) into the semipermeable membrane and hydrophilization treatment using alcohol. However, the introduction of hydrophilic groups into the semipermeable membrane has a drawback in that the mechanical strength is reduced if hydrophilic groups are introduced into the entire membrane. Therefore, it has been found that by sulfonating a part of the semipermeable membrane, the mechanical strength can be maintained and the water permeability can be improved.
[0014] In the semipermeable membrane of the present invention, the thickness of the sulfonated layer is preferably 50% or less of the entire membrane thickness. If the thickness of the sulfonated layer exceeds 50% of the entire membrane thickness, hydrophilization progresses, and the balance between water permeability and ion rejection rate may become poor. In order to exert the separation function as a semipermeable membrane, the thickness of the sulfonated layer is more preferably in the range of 40% or less of the entire membrane thickness. On the other hand, the thickness of the sulfonated layer is preferably 5% or more. If the thickness of the sulfonated layer is thin, problems such as a decrease in water permeability may occur, so the thickness of the sulfonated layer is more preferably 10% or more. The thickness of the sulfonated layer is measured by photographing a cross section of the sulfonated semipermeable membrane embedded in a resin piece using a scanning electron microscope (SEM) and detecting elemental sulfur by EDS mapping, as described below.
[0015] In the present invention, the degree of sulfonation of the entire semipermeable membrane is 0.1×10 4 meq. / m 3 ~9.0×10 4 meq. / m 3 If the degree of sulfonation is low, the formation of the sulfonated layer becomes insufficient, and the separation function (particularly the ion rejection rate) tends to decrease. If the degree of sulfonation is high, the strength of the membrane decreases, and the stability of the separation performance may not be ensured. That is, in order to ensure the strength of the membrane as a semipermeable membrane while also ensuring sufficient separation function, the degree of sulfonation is preferably 0.5×10 4 meq. / m 3 ~4.0×10 4 meq. / m 3It is more preferable that the sulfonation degree of the semipermeable membrane is in the range of 100 to 200. The sulfonation degree of the semipermeable membrane can be measured by a titration method as described later.
[0016] In the present invention, as long as the degree of sulfonation of the entire semipermeable membrane satisfies the above range, both surfaces of the semipermeable membrane may be sulfonated, but it is more preferable that the first surface of the semipermeable membrane is sulfonated and the second surface is not sulfonated (FIG. 1). Specifically, it is preferable that the second surface has a sulfur element ratio of less than 0.1 atm%. Here, the sulfur element ratio can be measured to a depth of about 10 nm from the membrane surface by X-ray photoelectron spectroscopy, which will be described later. If the sulfur element ratio is high, the strength of the semipermeable membrane may decrease.
[0017] A semipermeable membrane having the above-mentioned properties has an excellent balance between water permeability and ion rejection rate, and can also exhibit high membrane strength (yield strength).
[0018] In the present invention, the production of a hollow fiber type semipermeable membrane substrate includes a step of dissolving a polyphenylene resin in an aprotic solvent to obtain a membrane-forming stock solution (dissolving step), a step of extruding the membrane-forming stock solution from a spinning nozzle into a hollow fiber shape at a temperature equal to or higher than the temperature-induced phase separation point (extruding step), a step of contacting (immersing) the membrane-forming stock solution extruding into a hollow fiber shape with a mixed solution of water and an organic solvent to solidify it (solidifying step), a step of washing the solidified hollow fiber shape with warm water to remove excess solvent, etc. (washing step), and a step of drying it (drying step).
[0019] In the present invention, the flat semipermeable membrane substrate is produced by spreading the membrane forming solution on a glass plate or the like using an applicator or the like so as to have a uniform thickness, immersing the glass plate together with the membrane forming solution in a coagulating liquid, and then recovering the semipermeable membrane substrate from the glass plate. The recovered semipermeable membrane substrate is washed and, if necessary, dried.
[0020] The obtained semipermeable membrane substrate can be easily sulfonated by contacting the first surface of the semipermeable membrane substrate with sulfuric acid. At this time, it is preferable to pressurize from the second surface side so that the sulfuric acid does not penetrate into the inside of the membrane. The pressurization is preferably 2 MPa or less using nitrogen gas or the like. If the pressure is high, bubbles may be generated from the first surface, and the sulfonation may be partially insufficient. If the pressure is low, the sulfuric acid may penetrate into the inside of the membrane, and the second surface may be sulfonated. The sulfonation degree of the semipermeable membrane substrate can be adjusted by the concentration and contact time of the sulfuric acid used. The concentration of sulfuric acid is preferably 90 to 98 wt%, more preferably 93 to 95 wt%. In addition, the contact time is preferably 0.5 min to 60 min, more preferably 30 min. If the concentration of sulfuric acid is low, a long time is required to obtain the desired sulfonation degree, or the desired sulfonation degree cannot be achieved. On the other hand, if the concentration of sulfuric acid is high, it becomes difficult to adjust the sulfonation degree. If the contact time is short, uniform sulfonation may not be achieved. On the other hand, if the contact time is long, sulfonation progresses to the inside of the semipermeable membrane, making it impossible to obtain the required membrane strength. EXAMPLES
[0021] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0022] (Measurement of sulfonation degree by titration method) The degree of sulfonation of the entire semipermeable membrane of each of the Examples and Comparative Examples was measured by a titration method. Pretreatment for measurement: A sample of 1.0 g was prepared in terms of dry weight, and the sample was cut into 3 cm pieces. The semipermeable membrane treated with sulfuric acid was washed with pure water at 80°C until there was no change in pH (residual sulfuric acid), and then vacuum dried at 110°C for 5 hours. The sample was then immersed in a 2.0 M NaCl aqueous solution for 24 hours to remove the counter ions of the sulfonic acid groups, H + Na + was replaced with. Titration experiment: The NaCl aqueous solution was titrated with 0.010 M NaOH using an automatic titrator (Hiranuma Sangyo Co., Ltd. COM-1700) to measure the ion exchange capacity (IEC). The sulfonation degree was calculated by the following formula. IEC [meq. / g] = sodium hydroxide concentration [M] x titration amount [ml] / sample amount [g] Sulfonation degree [meq. / m 3 ] = sodium hydroxide concentration [M] × titration amount [ml] / membrane volume [m 3 ]
[0023] (Evaluation of mechanical strength of semipermeable membrane) The mechanical strength of the semipermeable membranes of the examples and comparative examples was evaluated by measuring the prepared semipermeable membranes using a tensile tester (Shimadzu Corporation EZ-SX). As a pretreatment of the measurement sample, the sample was immersed in 25 wt% ethanol for 30 min, and then immersed in pure water for 24 hours. The tensile test was performed by clamping with a load cell of 50 N, an initial gauge length of 50 mm at both ends, and a test speed of 20 mm / min. The average value of 10 measurements was taken as the measured value of the yield strength. In addition, if a clear yield point exists in the stress-strain curve, the value of the yield strength is adopted. In the case where there is no clear yield point peak, the value of the intersection between the straight line used to calculate the initial elastic modulus in the stress-strain curve and the straight line (tangent) in the linear region after yield (elongation: 10 to 30%) was taken as the value of the yield strength (Figure 2).
[0024] (Evaluation of the ratio of sulfonated regions in the membrane cross section) The ratio of sulfonated regions in the cross sections of the semipermeable membranes of the Examples and Comparative Examples was evaluated by SEM-EDS measurement (SEM: S4800 manufactured by Hitachi High-Technologies Corporation, detector: energy dispersive X-ray analysis manufactured by BRUKER). The sample was embedded in epoxy resin (Nacalai Tesku Rubeac 812) and cross-sectioned using a microtome equipped with a glass knife. The sample was fixed to a sample stage, osmium was evaporated, and elemental analysis was performed using the microscope with an accelerating voltage of 10 kV. SEM-EDS measurements were performed, and a line analysis of sulfur element was performed on the membrane cross section (Figure 3-5). The baseline was set to 0.01 or less in relative count number (count number / total count number), and the ratio of sulfonated area was calculated using the following formula. Ratio of sulfonated layer [%] = thickness of sulfonated layer [μm] / (thickness of sulfonated layer (Ts) [μm] + thickness of non-sulfonated layer (Tb) [μm]) × 100
[0025] (Calculation of sulfur element ratio on film surface) XPS measurement (Thermo Fisher Scientific K-Alpha + The sulfur element ratio was calculated by analyzing the sulfur element of the semipermeable membrane by the method described above. In the case of a hollow fiber type semipermeable membrane, the outer surface side was measured as it was, and the inner surface side was measured by opening the hollow fiber membrane with a knife to expose the inner surface side. XPS can measure the sulfur element ratio from the surface to a depth of about 10 nm. Measurement conditions Excitation X-ray: Monochromatic Al Kα radiation X-ray output: 12kV 2.5mA Photoelectron escape angle: 90° Spot size: approx. 200 μmφ Pass energy: 50 eV Step: 0.1eV
[0026] (Membrane performance evaluation) Four hundred semipermeable membranes (hollow fiber semipermeable membranes) of the examples and comparative examples were looped, the tips of the loops were glued with two-component epoxy resin, and the open end side of the hollow fiber semipermeable membrane was inserted into a 5 cm polycarbonate sleeve, after which the two-component epoxy resin was injected into the sleeve and cured to seal it. The end of the hollow fiber semipermeable membrane cured with the thermosetting resin was cut to obtain the open surface of the hollow fiber semipermeable membrane, thereby producing an evaluation module. The membrane performance was evaluated by mounting the evaluation module on a hollow fiber water permeability tester and using a 1500 ppm NaCl aqueous solution at an operating pressure of 0.5 MPa. The electrical conductivity of the membrane permeate water collected in the permeability test and the supplied aqueous solution was measured using an electrical conductivity meter (DS-70, Horiba, Ltd.), and the ion rejection rate was calculated using the following formula. Ion rejection rate [%] = (1 - filtrate conductivity [μS / cm] / feed aqueous solution conductivity [μS / cm]) × 100 In addition, the pure water flux was measured at an operating pressure of 0.5 MPa using pure water. The pure water flux was calculated using the following formula. Pure water Flux[L / (m 2 ·day)]=permeated water amount [L] / membrane area [m 2 ] / Collection time [days]
[0027] Example 1 N-methyl-2-pyrrolidone (Nacalai Tesque, Extra Pure Reagent) was added to polyphenylene oxide (SABIC Innovative Plastics, PPO646) to make a 30 wt% suspension, which was then kneaded to prepare a uniform suspension, and heated at 100°C while kneading to obtain a uniform spinning dope. The obtained spinning dope was extruded in a fixed amount from the slit of the double cylindrical nozzle. From the inner hole of the double cylindrical nozzle, a fixed amount of RO water was discharged as the inner liquid, and while inducing phase separation in the inner layer part of the spinning dope extruded in a hollow shape, the surface layer of the spinning dope was dried in an air gap, and then the phase separation was completely promoted in a coagulation bath. The solidified hollow fiber-like product was thoroughly washed with water and then wound up while still containing water.
[0028] The obtained hollow fiber-like product was cut to a length of 100 cm, immersed and washed in pure water at 60° C., and air-dried overnight. An evaluation module was produced using the obtained semipermeable membrane substrate.
[0029] While the inner cavity side of the hollow fiber membrane of the module was pressurized with nitrogen gas (1.5 MPa), the outer side of the hollow fiber membrane was contacted with a 92.5% sulfuric acid solution for 30 minutes to obtain the semipermeable membrane of Example 1. The inner diameter of the semipermeable membrane was 240 μm.
[0030] Example 2 Except for contacting with the 93.5% sulfuric acid solution for 30 minutes, the semipermeable membrane of Example 2 was obtained in the same manner as in Example 1. The inner diameter of the semipermeable membrane was 240 μm.
[0031] Example 3 Except for contacting with the 94.5% sulfuric acid solution for 30 minutes, the semipermeable membrane of Example 3 was obtained in the same manner as in Example 1. The inner diameter of the semipermeable membrane was 240 μm.
[0032] Example 4 Except for contacting with the 94.5% sulfuric acid solution for 1 minute, the semipermeable membrane of Example 4 was obtained in the same manner as in Example 1. The inner diameter of the semipermeable membrane was 240 μm.
[0033] Example 5 Except for contacting with the 94.5% sulfuric acid solution for 5 minutes, the semipermeable membrane of Example 5 was obtained in the same manner as in Example 1. The inner diameter of the semipermeable membrane was 240 μm.
[0034] Example 6 Except for contacting with the 94.5% sulfuric acid solution for 10 minutes, the semipermeable membrane of Example 6 was obtained in the same manner as in Example 1. The inner diameter of the semipermeable membrane was 240 μm.
[0035] Comparative Example 1 A semipermeable membrane of Comparative Example 1 was obtained in the same manner as in Example 1, except that no contact with the sulfuric acid solution was carried out.
[0036] Comparative Example 2 A semipermeable membrane of Comparative Example 2 was obtained in the same manner as in Example 1, except that the 95.5% sulfuric acid solution was contacted for 30 minutes.
[0037] Comparative Example 3 A semipermeable membrane of Comparative Example 3 was obtained in the same manner as in Example 1, except that the 96.5% sulfuric acid solution was contacted for 30 minutes.
[0038] Comparative Example 4 A semipermeable membrane of Comparative Example 4 was obtained in the same manner as in Example 1, except that a membrane was formed using PPO that had been subjected to a sulfonation treatment at the raw material stage, and no sulfonation treatment was performed after membrane formation.
[0039] [Table 1]
[0040] As is clear from Table 1, the semipermeable membranes of Examples 1 to 6 have an appropriate ratio of sulfonated regions, and therefore have an excellent balance of water permeability, separation properties, and mechanical strength. In contrast, the semipermeable membrane of Comparative Example 1 has high mechanical strength because it has not been subjected to sulfonation treatment, but has a salt rejection rate of only 5%, and therefore has low functionality as a separation membrane. In addition, the semipermeable membranes of Comparative Examples 2 to 3 have low mechanical strength because the entire membrane is sulfonated, resulting in an unbalanced water permeability and separation properties. In addition, the semipermeable membrane of Comparative Example 4 has very high water permeability, but is not well balanced with the ion rejection rate, and has very low mechanical strength. [Industrial Applicability]
[0041] As described above in detail, according to the present invention, by sulfonating a polyphenylene-based porous substrate membrane under specific conditions, only a portion of the membrane is sulfonated, making it possible to achieve both chemical resistance (chlorine resistance, acid resistance, alkali resistance), membrane performance, and membrane strength. [Explanation of symbols]
[0042] 1. Sulfonated layer 2. Non-sulfonated layer
Claims
1. A semipermeable membrane made of a material containing a polyphenylene resin, the polyphenylene resin is a polyphenylene oxide resin, The semipermeable membrane is a hollow fiber membrane, The hollow fiber membrane has an outer first surface and a lumen-side second surface, The first surface is formed by sulfonating at least a portion of the polyphenylene oxide resin, the second surface is not sulfonated and has an elemental sulfur ratio of less than 0.1 atm %, A polyphenylene-based semipermeable membrane, in which, when a concentration distribution of sulfur element derived from sulfonic acid groups is measured by elemental analysis on a cross section in a thickness direction of the semipermeable membrane, the ratio of a sulfonated layer obtained by the following formula is 50% or less. Ratio of sulfonated layer (%)=thickness of sulfonated layer / (thickness of sulfonated layer+thickness of non-sulfonated layer)×100
2. The polyphenylene-based semipermeable membrane according to claim 1 , wherein the ratio is 5% or more and 40% or less.
3. Sulfonation degree is 0.1 x 10 4 meq. / m 3 ~9.0 x 10 4 meq. / m 3 3. The polyphenylene-based semipermeable membrane according to claim 1 or 2,
4. A method for producing the polyphenylene-based semipermeable membrane according to any one of claims 1 to 3, comprising the steps of: a sulfonation treatment is carried out by contacting a first surface of a semipermeable membrane substrate made of a material containing the polyphenylene resin with sulfuric acid; The semipermeable membrane substrate is a hollow fiber membrane, The sulfuric acid has a concentration of 92.5 to 95 wt %, The method for producing a polyphenylene-based semipermeable membrane comprises contacting the first surface with the sulfuric acid while applying pressure to the second surface side.
Citation Information
Patent Citations
Osmotic membrane synthesized on interface
JP1980147106A
Sulfonated porous material and production thereof
JP1988054452A
Hollow yarn composite membrane for separation of organic material
JP1990014725A
Production of separation membrane
JP1994000350A
Separation membrane for nanofiltration
JP2013031836A