Electrolytic capacitor and method for manufacturing the same

By optimizing the static friction coefficient of the carbon layer and using a specific welding technique, the electrolytic capacitor achieves improved connectivity and reduced resistance between the cathode body and lead terminal, addressing the connectivity issues in existing capacitors.

JP7581709B2Active Publication Date: 2024-11-13NIPPON CHEMI CON CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020144770
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-28
Publication Date
2024-11-13
Estimated Expiration
2040-08-28

AI Technical Summary

Technical Problem

The connectivity between the cathode body with a carbon layer and the lead-out terminal in electrolytic capacitors is compromised due to reduced physical connection strength and increased electrical resistance, primarily because of the poor stretchability of the carbon layer and slippage during cold pressure welding.

Method used

The electrolytic capacitor design includes a cathode body with a carbon layer having a maximum static friction coefficient of 0.6 or more, and a cold pressure welding process using a pressing member with a side surface inclined at 120 degrees or more to ensure proper bonding.

Benefits of technology

This approach enhances the connectivity and reduces stress concentration, improving the connection strength and minimizing electrical resistance between the cathode body and the lead terminal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581709000007
    Figure 0007581709000007
  • Figure 0007581709000008
    Figure 0007581709000008
  • Figure 0007581709000009
    Figure 0007581709000009
Patent Text Reader

Abstract

To provide an electrolytic capacitor improved in the connectability between a negative electrode body including a carbon layer and a lead terminal, and a method for manufacturing the electrolytic capacitor.SOLUTION: An electrolytic capacitor 1 comprises: an anode body 2 with a dielectric oxide coating 5 formed on its surface; a cathode body 3 having cathode foil 31 and a carbon layer 32 formed on the cathode foil 31; a liquid electrolyte 6 interposed between the anode body 2 and the cathode body 3; and lead terminals 7 cold pressure welded to the anode body 2 and the cathode body 3. The maximum static friction coefficient of the surface of the carbon layer 32 of the cathode body 3 is 0.6 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolytic capacitor and a method for manufacturing an electrolytic capacitor. [Background technology]

[0002] An electrolytic capacitor has an anode foil and a cathode foil made of valve metal such as tantalum or aluminum. The anode foil is enlarged by forming the valve metal into a sintered or etched foil, etc., and has a dielectric oxide film layer on the enlarged surface. An electrolyte is interposed between the anode foil and the cathode foil. The electrolyte is in close contact with the uneven surface of the anode foil and functions as a true cathode. This electrolytic capacitor obtains its anode capacitance by the dielectric polarization action of the dielectric oxide film layer.

[0003] An electrolytic capacitor can be considered a series capacitor with capacitance appearing on the anode and cathode sides. Therefore, the cathode capacitance is also very important for efficient use of the anode capacitance. The cathode foil also has an increased surface area through etching, but there is a limit to how much the cathode foil can be enlarged from the viewpoint of its thickness.

[0004] Therefore, an electrolytic capacitor has been proposed in which a film of a metal nitride such as titanium nitride is formed on the cathode foil (see Patent Document 1). In a nitrogen gas environment, titanium is evaporated by vacuum arc deposition, a type of ion plating method, and titanium nitride is deposited on the surface of the cathode foil. Metal nitrides are inactive, and a natural oxide film is unlikely to form. In addition, the deposited film has fine irregularities, which increases the surface area of ​​the cathode. However, the deposition process of metal nitrides is complicated, which increases the cost of electrolytic capacitors.

[0005] Therefore, the inventors have come up with the idea of ​​forming a carbon layer on the cathode foil. The carbon layer is located on the outermost surface of the cathode body. The cathode capacitance of this electrolytic capacitor is generated by the charge storage action of the electric double layer formed at the interface between the polarizable electrode and the electrolyte. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 4-61109 Summary of the Invention [Problem to be solved by the invention]

[0007] The electrolytic capacitor has lead-out terminals that are electrically connected to a circuit. The lead-out terminals are, for example, tab-shaped and include flat portions made of aluminum. The flat portions are connected to the anode and cathode of the capacitor element by various connection methods, and the lead-out terminals are led out from the electrolytic capacitor body.

[0008] Cold pressure welding is known as a method for connecting a lead terminal to an anode body or a cathode body. In cold pressure welding, the anode body or cathode body and the flat part of the lead terminal are overlapped, and pressure is applied in the lamination direction between the anode body or cathode body and the flat part of the lead terminal in an unheated state. This is said to cause atomic bonding between the anode body or cathode body and the flat part of the lead terminal.

[0009] It was confirmed that when a cathode body having a carbon layer formed on a cathode foil was connected to a draw-out terminal by this cold pressure welding, the connection was poorer than when a cathode body without a carbon layer was cold pressure welded to a draw-out terminal, i.e., the physical connection strength between the cathode body and the draw-out terminal was lowered and the electrical resistance between the cathode body and the draw-out terminal was higher.

[0010] The present invention has been proposed to solve the above-mentioned problems, and an object of the present invention is to provide an electrolytic capacitor having improved connectivity between a cathode body including a carbon layer and a lead terminal, and a method for manufacturing the electrolytic capacitor. [Means for solving the problem]

[0011] In order to solve the above-mentioned problems, an electrolytic capacitor according to an embodiment includes an anode body having a dielectric layer formed on a surface thereof, a cathode body having a cathode foil and a carbon layer formed on the cathode foil, an electrolyte interposed between the anode body and the cathode body, and lead terminals of each electrode cold-pressed to the anode body and the cathode body, and wherein the maximum static friction coefficient of the surface of the carbon layer of the cathode body is 0.6 or more.

[0012] In order to solve the above-mentioned problems, a manufacturing method for an electrolytic capacitor according to an embodiment is a manufacturing method for an electrolytic capacitor in which an anode body having a dielectric layer formed on a surface thereof and a cathode body are opposed to each other with an electrolyte sandwiched therebetween, and is characterized by including a cold pressure welding step of cold pressure welding a lead terminal to the cathode body having a carbon layer formed on a cathode foil and having a maximum static friction coefficient of 0.6 or more on the surface thereof.

[0013] When the lead terminal and the cathode body are cold-welded, the cathode foil of the cathode body is made of metal such as aluminum foil and is therefore highly extensible, and is easily stretched by pressing. On the other hand, the carbon layer is originally less extensible than the cathode foil, and when the maximum static friction coefficient becomes 0.6 or more, it gets caught by the pressing member and becomes increasingly unable to follow the stretching of the cathode foil during cold welding. This makes it easier for multiple cracks to form in the carbon layer, and the cathode foil is exposed through the cracks. Therefore, the flat part of the lead terminal and the surface of the cathode foil can be pressure-welded through the cracks in the carbon layer, improving the connection between the lead terminal and the cathode body.

[0014] In addition, if the frictional force of the carbon layer surface is low, the pressing member surface and the carbon layer surface slip during cold welding. During cold welding, a pressing area is generated in the carbon layer and the cathode foil that is in contact with the pressing member and receives pressure, but in the outer area of ​​this pressing area, a force that moves outward from the pressing area acts due to the sliding between the pressing member surface and the carbon layer surface. Therefore, the outer area of ​​the pressing area does not become thinner in response to the pressing force, and the pressing area is likely to have a shape in which the thickness of the outer area and the other central area changes suddenly. In this shape, stress is likely to concentrate in the part where the thickness changes suddenly, and the connection between the cathode body and the draw-out terminal may be insufficient. However, if the maximum static friction coefficient of the carbon layer surface is set to 0.6 or more, the pressing member does not slip on the surface of the carbon layer surface, and the entire pressing area of ​​the carbon layer and the cathode foil becomes thinner in response to the pressing force. Therefore, a structure in which stress is unlikely to concentrate is obtained, and the connection force between the cathode body and the draw-out terminal can be improved.

[0015] The carbon layer may contain graphite at a ratio of 18 wt% or less, including no additive, relative to the total amount of all carbon materials in the carbon layer. Since graphite has a sliding property, if the graphite content is no additive or 18 wt% or less, the maximum static friction coefficient of the surface of the carbon layer can be increased to 0.6 or more. The carbon layer may contain spherical carbon as the carbon material.

[0016] In the cold welding step, the cathode body and the pull-out terminal are overlapped and pressed by a pressing member, and the pressing member may have a flat surface and a side surface inclined at an angle of 120 degrees or more with the flat surface. Also, a cold-welded region may be provided at a boundary surface between the cathode body and the pull-out terminal, and the cold-welded region may have a flat surface and an inclined surface which forms an angle of 120 degrees or more with the flat surface.

[0017] When the cathode body and the lead terminal are pressed by a pressing member having a side surface inclined at 120 degrees or more, the cathode body is less likely to be sheared, improving the connection between the cathode body and the lead terminal. In addition, the cold pressure welding area has a flat surface and an inclined surface of 120 degrees or more, making it a wide area, and the bonding area is increased, improving the connection between the cathode body and the lead terminal. Effect of the Invention

[0018] According to the present invention, the connectivity between the cathode body including the carbon layer and the lead-out terminal is improved. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a model diagram of an electrolytic capacitor. [Diagram 2] FIG. 2 is a schematic diagram showing a cross section of a cathode body. [Diagram 3] FIG. 2 is a schematic diagram showing a connection process using cold welding. [Figure 4] 1 is a graph showing connection strength for each maximum static friction coefficient when cold welding is performed using a trapezoidal pressing member having a side surface with an inclination angle of 120 degrees. [Diagram 5] 1 is a graph showing contact resistance for each maximum static friction coefficient when cold welding is performed using a trapezoidal pressing member having a side surface with an inclination angle of 120 degrees. [Figure 6] 1 is a graph showing connection strength for each maximum static friction coefficient when cold welding is performed using a trapezoidal pressing member having a side surface with an inclination angle of 150 degrees. [Figure 7] 1 is a graph showing contact resistance for each maximum static friction coefficient when cold welding is performed using a trapezoidal pressing member having a side surface with an inclination angle of 150 degrees. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The electrode body according to the embodiment of the present invention and an electrolytic capacitor using this electrode body as a cathode will be described. In this embodiment, a wound-type electrolytic capacitor having an electrolytic solution will be described as an example, but is not limited to this. The present invention can be applied to any electrolytic capacitor having various electrolytes, such as an electrolytic solution, a solid electrolyte layer such as a conductive polymer, a gel electrolyte, or an electrolyte in which an electrolyte solution is used in combination with a solid electrolyte layer and a gel electrolyte, and can also be applied to, for example, a stacked-type electrolytic capacitor.

[0021] (Electrolytic capacitor overview) 1 is a model diagram of an electrolytic capacitor according to this embodiment. This electrolytic capacitor 1 is a passive element that stores and discharges electric charge according to the electrostatic capacitance. This electrolytic capacitor 1 includes an anode body 2 having a dielectric oxide film 5 formed on its surface, a cathode body 3 formed by forming a carbon layer 32 on the surface of a cathode foil 31, and a separator 4. The carbon layer 32 is formed on both sides of the cathode foil 31. The anode body 2 and the cathode body 3 are strip-shaped and disposed opposite each other with the separator 4 therebetween, and are wound so that the strip length direction forms a spiral.

[0022] An electrolyte 6 is filled between the anode body 2 and the cathode body 3. The electrolyte 6 is in close contact with the dielectric oxide film 5 of the anode body 2 and also with the carbon layer 32 of the cathode body 3. In this electrolytic capacitor 1, a cathode-side capacitance is generated by the electric double layer effect generated at the interface between the carbon layer 32 of the cathode body 3 and the electrolyte 6, and an anode-side capacitance is generated in the anode body 2 by the dielectric polarization effect.

[0023] Fig. 2 is a cross-sectional view of the cathode body 3. As shown in Fig. 2, a lead-out terminal 7 is electrically and mechanically connected to the cathode body 3 by cold pressure welding. Similarly, another lead-out terminal 7 is electrically and mechanically connected to the anode body 2 by cold pressure welding. Via this lead-out terminal 7, the electrolytic capacitor 1 is mounted on an electric circuit or electronic circuit.

[0024] The draw-out terminal 7 is a metal member having a flat portion 71, is made of aluminum, for example, and has a flat plate shape or a rectangular wire shape. One end side of the draw-out terminal 7 is brought into contact with the cathode body 3 so that the flat portion 71 is in surface contact with one side of the cathode body 3. The draw-out terminal 7 is caused to protrude from the cathode body 3 so as to be perpendicular to the band long side of the cathode body 3. The draw-out terminal 7 and the cathode body 3 are then connected by cold pressure welding. The anode body 2 and the other draw-out terminal 7 are connected in the same manner. Note that it is sufficient for the draw-out terminal 7 to have the flat portion 71, and it may be one in which one end of a round bar portion is crushed by press working to form the flat portion 71, and a metal wire is connected to the other end of the round bar portion by arc welding or the like.

[0025] (cathode body) The cathode body 3 has a laminated structure of a cathode foil 31 and a carbon layer 32. The cathode foil 31 serves as a current collector, and preferably has a surface-expanding layer formed on its surface. The carbon layer 32 contains a carbon material as a main material. The carbon layer 32 is in close contact with the surface-expanding layer, thereby forming a laminated structure of the cathode foil 31 and the carbon layer 32. The carbon layer 32 is located on the outermost surface of the cathode body 3.

[0026] The cathode foil 31 is a long foil made of a valve metal. The valve metal is aluminum, tantalum, niobium, titanium, hafnium, zirconium, zinc, tungsten, bismuth, antimony, etc. The purity is preferably about 99% or more, but impurities such as silicon, iron, copper, magnesium, and zinc may be contained. For example, the cathode foil 31 may be made of an aluminum material having a temper symbol H as specified by JIS standard H0001, that is, a so-called H material, or an aluminum material having a temper symbol O as specified by JIS standard H0001, that is, a so-called O material. If a metal foil made of an H material having high rigidity is used, deformation of the cathode foil 31 due to press working can be suppressed.

[0027] The cathode foil 31 is a metal foil made of an elongated valve metal that has been subjected to a surface enlargement process. The surface enlargement layer is formed by electrolytic etching, chemical etching, sandblasting, or the like, or by depositing or sintering metal particles or the like on the metal foil. Examples of electrolytic etching include direct current etching and alternating current etching. In chemical etching, the metal foil is immersed in an acid solution or an alkaline solution. The formed surface enlargement layer is a layer region having tunnel-shaped etching pits or spongy etching pits dug from the foil surface toward the foil core. The etching pits may be formed to penetrate the cathode foil 31.

[0028] An oxide film may be formed on the surface-expanding layer either intentionally or naturally. A natural oxide film is formed by the reaction of the cathode foil 31 with oxygen in the air, while a chemical conversion film is an oxide film formed intentionally by a chemical conversion treatment in which a voltage is applied in a solution that does not contain halogen ions, such as an aqueous solution of adipic acid or boric acid. When the metal foil is, for example, an aluminum foil, the oxide film formed by this method is aluminum oxide formed by oxidation of the surface-expanding layer.

[0029] Carbon layer 32 contains, as a main material, a carbon material that generates an electric double layer action. The surface of this carbon layer 32 is adjusted so that the maximum static friction coefficient is 0.6 or more. By making the maximum static friction coefficient of the surface of carbon layer 32 0.6 or more, the connectivity between cathode body 3 having carbon layer 32 and pull-out terminal 7 is improved. The following mechanism is speculation and is not limited to this mechanism, but it is believed that the connectivity between cathode body 3 having carbon layer 32 and pull-out terminal 7 is improved for the following reason.

[0030] That is, when the lead terminal 7 and the cathode body 3 are pressed by cold welding, the cathode foil 31 of the cathode body 3 is highly extensible because it is made of a metal such as an aluminum foil, and is easily stretched by pressing. On the other hand, the carbon layer 32 is originally less extensible than the cathode foil 31, but when the maximum static friction coefficient becomes 0.6 or more, it gets caught by the pressing member, and becomes increasingly unable to follow the stretching of the cathode foil 31 during cold welding. Then, many cracks are generated in the carbon layer 32, and the cathode foil 31 is exposed as if peeking through the cracks in the carbon layer 32. Therefore, the flat portion 71 of the lead terminal 7 and the surface of the cathode foil 31 can be joined through the cracks in the carbon layer 32, and the connection between the lead terminal 7 and the cathode body 3 is improved. In this way, in order to make the surface of the carbon layer 32 easily catch on the lead terminal 7, the carbon layer 32 is adjusted so that the maximum static friction coefficient of the surface of the carbon layer 32 is 0.6 or more.

[0031] Furthermore, if the frictional force of the surface of the carbon layer 32 is low, the pressing member surface and the surface of the carbon layer 32 slip during cold welding. During cold welding, a pressing region that is in contact with the pressing member and receives pressure is generated in the carbon layer 32 and the cathode foil 31, and a force that moves the pressing region outward acts on the outer region of the pressing region due to the sliding between the pressing member surface and the surface of the carbon layer 32. Therefore, the outer region of the pressing region does not become thinner in response to the pressing force, and the pressing region tends to have a shape in which the thickness of the outer region and the other central region changes abruptly. In this shape, stress tends to concentrate in the part where the thickness changes abruptly, and the connection between the cathode body 3 and the lead-out terminal 7 may become insufficient. However, if the maximum static friction coefficient of the surface of the carbon layer 32 is set to 0.6 or more, the pressing member does not slip on the surface of the carbon layer 32, and the pressing region of the carbon layer 32 and the cathode foil 31 becomes thinner in response to the pressing force. This results in a structure in which stress is less likely to concentrate, and the connection strength between cathode body 3 and extraction terminal 7 can be improved.

[0032] The carbon material contained in the carbon layer 32 is fibrous carbon, carbon powder, or a mixture thereof. It may be fibrous carbon or carbon powder that has been subjected to a porous treatment such as activation treatment or opening treatment to form holes. The fibrous carbon is carbon nanotubes, carbon nanofibers, etc. The carbon nanotubes may be single-walled carbon nanotubes with one graphene sheet, or multi-walled carbon nanotubes (MWCNTs) with two or more graphene sheets rolled coaxially to form multiple tube walls. The carbon powder may be activated carbon made from natural plant tissue such as coconut shells, synthetic resins such as phenol, fossil fuels such as coal, coke, and pitch, carbon black such as ketjen black, acetylene black, and channel black, carbon nanohorns, amorphous carbon, mesoporous carbon, etc. In the electrolytic capacitor 1 using the electrolytic solution 6 as the electrolyte, the carbon material is preferably one that exhibits an electric double layer effect.

[0033] As the carbon material, spherical carbon is particularly preferred. It is preferable to include one or more types of spherical carbon as the carbon material in the carbon layer 32. The spherical carbon has a small particle diameter and easily penetrates deeper into the surface-expanding layer formed on the cathode foil 31, so that the carbon layer 32 adheres closely to the cathode foil 31. An example of the spherical carbon is carbon black. Examples of carbon black include ketjen black, acetylene black, channel black, and thermal black, and preferably have an average primary particle diameter of 100 nm or less and a specific surface area calculated according to the BET theory (hereinafter referred to as BET specific surface area) of 200 m 2 / g or less. BET specific surface area is 200m 2 An example of carbon black having a carbon black content of less than 1000 ppm is acetylene black.

[0034] As the carbon material, graphite may be added to the carbon layer 32 together with other carbon materials. As the other carbon material to be added together with the graphite, spherical carbon is preferable. As the graphite, it is preferable that the graphite is flaky or scaly and the aspect ratio of the minor axis to the major axis is in the range of 1:5 to 1:100. When the carbon layer 32 containing this combination of carbon materials is laminated on the cathode foil 31, the spherical carbon is easily rubbed into the pores of the surface-expanding layer by the graphite. The graphite is easily deformed along the uneven surface of the surface-expanding layer and is easily piled up on the uneven surface. Then, the graphite acts as a pressing lid to hold down the spherical carbon rubbed into the pores. Therefore, the adhesion and fixation between the carbon layer 32 and the cathode foil 31 are further improved.

[0035] Here, since graphite has high sliding performance, the maximum static friction coefficient of the surface of the carbon layer 32 can be adjusted by adjusting the graphite content. No graphite is added to the carbon layer 32, or the graphite content is at least 18 wt% relative to the total amount of all carbon materials contained in the carbon layer 32. This makes the maximum static friction coefficient of the surface of the carbon layer 32 0.6 or more.

[0036] Such a cathode body 3 is produced by a cathode body production process. In the cathode body production process, a slurry containing the material of the carbon layer 32 is produced, a surface expansion layer is formed on the cathode foil 31, and the slurry is applied to the surface expansion layer, followed by drying and pressing. For the carbon layer 32, a carbon material is dispersed in a solvent, and a binder is added to produce a slurry. Before producing the slurry, the average particle size of the carbon material may be adjusted by pulverizing it with a pulverizing means such as a bead mill or a ball mill. The solvent may be an alcohol such as methanol, ethanol, or 2-propanol, a hydrocarbon solvent, an aromatic solvent, an amide solvent such as N-methyl-2-pyrrolidone (NMP) or N,N-dimethylformamide (DMF), water, or a mixture thereof. As a dispersion method, a mixer, jet mixing (jet collision), ultracentrifugation, ultrasonic treatment, or the like is used. In the dispersion process, the graphite, spherical carbon, and binder in the mixed solution are finely divided and homogenized, and dispersed in the solution. The binder may be, for example, styrene butadiene rubber, polyvinylidene fluoride, or polytetrafluoroethylene.

[0037] The slurry is applied to the cathode foil 31 by a slurry casting method, a doctor blade method, a spray atomization method, or the like. After application, the solvent is evaporated by drying. Alternatively, the carbon layer 32 is formed into a sheet by papermaking and placed on the cathode foil 31. The papermaking sheet is produced by dispersing the carbon material to be contained in the carbon layer 32 in a dispersion solvent, adding a binder as necessary, filtering under reduced pressure, drying, and then peeling off the deposit from the filter paper.

[0038] Other methods for forming the carbon layer 32 on the cathode foil 31 include vacuum deposition, sputtering, ion plating, CVD, electrolytic plating, and electroless plating. In the case of deposition, a carbon material is evaporated by heating it with electricity in a vacuum, or by irradiating the carbon material with an electron beam in a vacuum, to form a film of the carbon material on the cathode foil. In the case of sputtering, a target made of a carbon material and the cathode foil are placed in a vacuum chamber, and an inert gas is introduced into the vacuum chamber and a voltage is applied to cause the plasmatized inert gas to collide with the target, and particles of the carbon material knocked out from the target are deposited on the cathode foil.

[0039] After carbon layer 32 is formed on cathode foil 31, cathode foil 31 and carbon layer 32 are pressed together with a predetermined press pressure. In the press process, cathode body 3 consisting of carbon layer 32 and cathode foil 31 is sandwiched between press rollers and a linear press pressure is applied. The press pressure is 0.01 to 100 t / cm. 2 It is desirable to press the carbon layer 32 so that the carbon material is graphite and spherical carbon. When the carbon material of the carbon layer 32 is graphite and spherical carbon, the graphite and spherical carbon are closely aligned. In addition, the graphite of the carbon layer 32 is deformed to fit the uneven surface of the surface-expanding layer by pressing. In addition, the graphite deformed to fit the uneven surface of the surface-expanding layer is subjected to a pressure-welding stress by pressing, and the spherical carbon between the graphite and the surface-expanding layer is pushed into the pores. This enhances the adhesion between the carbon layer 32 and the cathode foil 31.

[0040] The obtained cathode body 3 is connected to the pull-out terminal 7 through a cold pressure welding step. Fig. 3 is a schematic diagram showing cold pressure welding of the obtained cathode body 3 and pull-out terminal 7. As shown in Fig. 3, the obtained cathode body 3 is overlapped on the flat portion 71 of the pull-out terminal 7. Then, in an unheated state, a pressing member 200 is pressed against the cathode body 3 and the flat portion 71 of the pull-out terminal 7 from the cathode body 3 side, and the cathode body 3 and the flat portion 71 of the pull-out terminal 7 are pressed by the pressing member 200 in the stacking direction.

[0041] It is preferable that pressing member 200 has a trapezoidal tip. That is, the tip of pressing member 200 is defined by flat surface 210 and side surface 220. Side surface 220 is connected to flat surface 210, inclines outward from pressing member 200, and preferably forms an angle α with flat surface 210 of 120 degrees or more. When side surface 220 is inclined to 120 degrees or more, shear stress on cold welded region 33 against which pressing member 200 is pressed is reduced. That is, cathode body 3 is not broken in part or in whole between cold welded region 33 and its surroundings, and good connectivity between cathode body 3 and lead terminal 7 can be maintained.

[0042] Incidentally, cold pressure welding region 33 is a region of the boundary between cathode body 3 and pull-out terminal 7 that is joined by cold pressure welding, and is a region onto which pressing member 200 is projected.

[0043] This cold pressure welding region 33 has a flat surface 33a and an inclined surface 33b due to pressing member 200 having a trapezoidal shape with an inclination angle of 120 degrees or more. Flat surface 33a is the region formed by contact with flat surface 210 of pressing member 200, and inclined surface 33b is the region formed by contact with side surface 220 of pressing member 200. Therefore, inclined surface 33b leans outward, and the angle it forms with flat surface 33a is angle α of 120 degrees or more, the same as pressing member 200. Therefore, the area of ​​cold pressure welding region 33 is increased, and the connectivity between cathode body 3 and lead terminal 7 is further improved.

[0044] (Anode 2) Next, the anode body 2 is a long foil made of a valve metal. The purity of the anode body 2 is preferably about 99.9% or more. This anode body 2 is formed by etching a stretched foil, or by sintering a valve metal powder, or by depositing a film of metal particles or the like onto the foil. The anode body 2 has an etched layer or a porous structure layer on its surface.

[0045] The dielectric oxide film 5 formed on the anode body 2 is typically an oxide film formed on the surface layer of the anode body 2, and if the anode body 2 is made of aluminum, it is an aluminum oxide layer formed by oxidizing the porous structure region. This dielectric oxide film 5 is formed by chemical conversion treatment in which a voltage is applied in a solution that does not contain halogen ions, such as an acid such as ammonium borate, ammonium phosphate, or ammonium adipate, or an aqueous solution of such an acid.

[0046] (Separator) Examples of materials for the separator 4 include cellulose such as kraft, Manila hemp, esparto, hemp, and rayon, and mixed papers thereof; polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and derivatives thereof; polytetrafluoroethylene-based resins, polyvinylidene fluoride-based resins, vinylon-based resins, polyamide-based resins such as aliphatic polyamides, semi-aromatic polyamides, and fully aromatic polyamides; polyimide-based resins, polyethylene resins, polypropylene resins, trimethylpentene resins, polyphenylene sulfide resins, and acrylic resins. These resins can be used alone or in combination, and can also be used in combination with cellulose.

[0047] (electrolyte) The electrolyte 6 is a mixed solution in which a solute is dissolved in a solvent and an additive is added as necessary. The solvent may be either a protic polar solvent or an aprotic polar solvent. Representative examples of protic polar solvents include monohydric alcohols, polyhydric alcohols, oxyalcohol compounds, water, and the like. Representative examples of aprotic polar solvents include sulfones, amides, lactones, cyclic amides, nitriles, oxides, and the like.

[0048] The solute contained in the electrolytic solution 6 includes anion and cation components, and is typically an organic acid or its salt, an inorganic acid or its salt, or a composite compound of an organic acid and an inorganic acid or an ionically dissociable salt thereof, and is used alone or in combination of two or more. An acid that becomes an anion and a base that becomes a cation may be added separately to the electrolytic solution as solute components.

[0049] Furthermore, other additives can be added to the electrolyte. Examples of additives include polyethylene glycol, complex compounds of boric acid and polysaccharides (mannitol, sorbitol, etc.), complex compounds of boric acid and polyhydric alcohols, boric acid esters, nitro compounds (o-nitrobenzoic acid, m-nitrobenzoic acid, p-nitrobenzoic acid, o-nitrophenol, m-nitrophenol, p-nitrophenol, etc.), phosphate esters, colloidal silica, etc. These may be used alone or in combination of two or more.

[0050] The electrolytic capacitor using the electrolytic solution 6 has been described above, but when a solid electrolyte is used, the carbon layer 32 provides electrical continuity with the solid electrolyte, and the capacitance of the electrolytic capacitor is determined by the anode capacitance due to dielectric polarization. When a solid electrolyte is used, examples of the electrolytic capacitor include polythiophenes such as polyethylenedioxythiophene, and conductive polymers such as polypyrrole and polyaniline. EXAMPLES

[0051] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0052] (Examples 1 and 2) (Preparation of cathode body) The cathode bodies 3 for the electrolytic capacitors 1 of Comparative Examples 1 to 3 and Examples 1 and 2 were produced as follows. First, the carbon material contained in the carbon layer 32 was a mixture of graphite and carbon black, which is a type of spherical carbon, or carbon black alone. Graphite powder, carbon black, and styrene butadiene rubber (SBR), which is a binder, were added to an aqueous solution of sodium carboxymethyl cellulose (CMC-Na), which is an aqueous solution containing a dispersant, and kneaded to produce a slurry. The compounding ratio of the carbon material, binder, and aqueous solution containing a dispersant was 84:10:6 by weight.

[0053] Separately, an aluminum foil was prepared as the cathode foil 31, and the slurry was uniformly applied to the cathode foil 31. A surface-expanding layer had been formed on the aluminum foil in advance by applying a voltage in hydrochloric acid. The surface area of ​​the cathode foil 31 was expanded by 22 times due to the surface-expanding layer. The depth of the surface-expanding layer was 4 μm on one side and 8 μm on both sides in total, and the foil core where the surface-expanding layer was not formed remained with a thickness of 12 μm. The depth of the surface-expanding layer is the average depth from the surface of the cathode foil 31 to the deepest part of the etching pit. The thickness of the foil core is the average thickness of the layer not reached by the etching pit.

[0054] A slurry containing graphite and carbon black, or a slurry containing only carbon black, was applied to the cathode foil 31. The slurry was applied to the surface-expanding layer of the cathode foil 31. After the slurry was dried, the cathode foil 31 was subjected to a pressure of 150 kNcm. -2 The carbon layer 32 was fixed onto the cathode foil 31 by applying a vertical press at a pressure of 1000 .mu.m.

[0055] The cathode bodies 3 of Comparative Examples 1 to 3 and Examples 1 and 2 have different mixture ratios of graphite and carbon black, as shown in the following Table 1. Note that the carbon materials contained in the carbon layer 32 of Comparative Examples 1 to 3 and Examples 1 and 2 are only graphite and carbon black, and the numerical values ​​related to graphite in the following Table 1 can be restated as weight percentages based on the total carbon materials contained in the carbon layer 32.

[0056] (Table 1) TIFF0007581709000001.tif61159

[0057] (Measurement of maximum friction coefficient) The maximum static friction coefficient μ of the surface of each carbon layer 32 of the cathode body 3 of Comparative Examples 1 to 3 and Examples 1 and 2 was measured as follows. That is, in accordance with JIS Standard P-8147 "Testing method for friction coefficient of paper and paperboard", the maximum static friction coefficient μ was measured by a horizontal linear reciprocating sliding method. Specifically, a solvent spun rayon (manufactured by Nippon Kodo Paper Industries; TEF (thickness 40 μm and density 0.40 g / cm)) was applied on each cathode body 3. 3 ), felt, and a 200 g weight were placed on the workpiece in that order, and the solvent-spun rayon was pulled at a speed of 100 mm / min. The traction force was gradually increased, and the force at the moment the solvent-spun rayon started to move was taken as the maximum static friction force (N) and was detected by a load cell (Kyowa Electric Industry Co., Ltd.; model number LUX-B). The maximum static friction coefficient of the surface of the carbon layer 32 of each cathode body 3 was calculated by dividing the maximum static friction force (N) by the normal force (N) that the solvent-spun rayon received from the cathode body 3 by the weight.

[0058] The maximum static friction coefficient μ of the surface of each carbon layer 32 of the cathode body 3 in Comparative Examples 1 to 3 and Examples 1 and 2 is shown in Table 2 below. (Table 2) TIFF0007581709000002.tif61159

[0059] As shown in Table 2 above, the maximum static friction coefficient μ of Example 1 and Example 2 is 0.6 or more. The graphite content in Example 1 is the sum of graphite and carbon black, i.e., 18.75 wt% based on the total carbon material, while no graphite is added in Example 2. Therefore, it was confirmed that if the graphite content in carbon layer 32 is 18 wt% or less based on the total carbon material, the maximum static friction coefficient μ of the surface of carbon layer 32 can be made 0.6 or more.

[0060] (Cold Welding) Next, a pull-out terminal 7 was connected by cold pressure welding to the cathode bodies 3 of Comparative Examples 1 to 3 and Examples 1 and 2. The cathode body 3 and flat portion 71 of the pull-out terminal 7 were overlapped, and pressure was applied in the stacking direction from the cathode body 3 side with a pressing member 200. The pressing member 200 has a trapezoidal tip, and the angle formed between the flat surface 210 and the side surface 220 is 120 degrees.

[0061] (Connection strength test) The cathode body 3 was fixed with the pull-out terminal 7 on the upper side, and the tip side of the pull-out terminal 7 protruding from the cathode body 3 was pulled up. The maximum tensile stress generated until the flat portion 71 of the pull-out terminal 7 was peeled off from each cathode body 3 was measured as the connection strength using a load cell (Kyowa Electric Industry Co., Ltd.; model number LUX-B). The position of the point of force was the same for all of the pull-out terminals.

[0062] The results of this connection strength test are shown in Table 3 below. The average values ​​of Table 3 below are also shown in the graph of Figure 4. Three cathode bodies 3 were produced and each was subjected to a connection strength test, and the average value of the three tests was also calculated. In Table 3 below, an x ​​mark indicates that the connection was not possible.

[0063] (Table 3) TIFF0007581709000003.tif70159

[0064] First, in the cathode body 3 of Comparative Example 1 having a maximum static friction coefficient of 0.33, the cathode body 3 was completely sheared during cold welding by pressing member 200 having side surface 220 inclined at 120 degrees, and could not be connected to pull-out terminal 7. In the cathode bodies 3 of Comparative Example 2 having a maximum static friction coefficient of 0.41, only one out of three could be connected to pull-out terminal 7 without being sheared.

[0065] 4, it was confirmed that the connection strength is completely different between Comparative Examples 1 to 3, in which the maximum static friction coefficient is 0.51 or less, and Examples 1 and 2, in which the maximum static friction coefficient is 0.6 or more. When the maximum static friction coefficient is at least 0.51 or less, no improvement in connection strength is observed even if the maximum static friction coefficient is increased, but when the maximum static friction coefficient is at least 0.6 or more, the connection strength is greatly improved compared to when the maximum static friction coefficient is at least 0.51 or less.

[0066] (Contact resistance test) The electrode terminals of a resistance meter were connected to the portion of the pull-out terminal 7 protruding from the cathode body 3 and to the cathode body 3. The pull-out terminal 7 was placed on the upper side, the cathode body 3 was fixed, and the contact resistance was measured in a state where the pull-out terminal 7 was lifted 0.8 mm and a state where the pull-out terminal 7 was lifted 0.0 mm, i.e., in a state where the pull-out terminal 7 was not lifted. A model RM3545 resistance meter manufactured by Hioki E.E. Corporation was used. The measurement results show the total value of the resistance value of the cathode body 3, the resistance value of the pull-out terminal 7, and the connection resistance. The resistance value of the cathode body 3 and the resistance value of the pull-out terminal 7 are the same in Comparative Examples 1 to 3 and Examples 1 and 2.

[0067] The results of this contact resistance test are shown in Table 4 below. The average values ​​of Table 4 below are also shown in the graph of Figure 5. Three cathode bodies 3 were produced for each, and a contact resistance test was carried out for each one when it was lifted 0.0 mm and 0.8 mm, and the average value of the three runs was also calculated. In Table 3 below, an x ​​mark indicates that the connection could not be made due to shearing, and the individual values ​​are the resistance values ​​(mΩ) obtained in the test.

[0068] (Table 4) TIFF0007581709000004.tif80166

[0069] The resistance value of the cathode body 3 and the resistance value of the lead-out terminal 7 are the same in Comparative Examples 1 to 3 and Examples 1 and 2, so the difference in the measurement results shown in Table 4 and FIG. 5 is the difference in contact resistance. As shown in Table 4 and FIG. 5, up to Comparative Example 3, where the maximum static friction coefficient is 0.51 or less, the difference in connection resistance is large between the state where the electrode is lifted 0.0 mm and the state where the electrode is lifted 0.8 mm. However, it was confirmed that when the maximum static friction coefficient becomes 0.6 or more, the contact resistance when the electrode is lifted 0.8 mm decreases, and the difference with the contact resistance when the electrode is lifted 0.0 mm becomes small. In this way, when the maximum static friction coefficient of the surface of the carbon layer 3 is 0.6 or more, the contact resistance is greatly improved compared to when the maximum static friction coefficient is at least 0.51 or less.

[0070] (Modification of the pressing member) The cathode bodies 3 of the electrolytic capacitor 1 of Comparative Examples 1 to 3 and Examples 1 and 2 were connected to the lead-out terminal 7 by cold pressure welding using pressing members 200 having different inclination angles of the side surfaces 220. The cathode body 3 and the flat portion 71 of the lead-out terminal 7 were overlapped, and pressure was applied in the stacking direction from the cathode body 3 side with the trapezoidal pressing member 200 in which the angle between the flat surface 210 and the side surface 220 was 150 degrees.

[0071] The cathode body 3 and the lead-out terminal 7 were connected by cold welding using the pressing member 200 having the side surface 220 inclined at 150 degrees, and then a connection strength test and a contact resistance test were performed. The connection strength test and the contact resistance test were performed using the same methods and conditions as those used for cold welding using the pressing member 200 having the side surface 220 inclined at 120 degrees. The results of the connection strength test are shown in Table 5 below, and the average results of the contact resistance test are shown in Table 6 below. The average results of Table 5 below are shown in the graph of FIG. 6, and the results of Table 6 below are shown in the graph of FIG. 7. In Tables 5 and 6 below, an x ​​mark indicates that the connection could not be made due to shearing and therefore the measurement could not be made, and in Table 6 below, each value is the resistance value (mΩ) obtained in the test.

[0072] (Table 5) TIFF0007581709000005.tif70159

[0073] (Table 6) TIFF0007581709000006.tif80166

[0074] When cold welding was performed using pressing member 200 having side surface 220 inclined at 120 degrees, some of the cathode bodies 3 were sheared in Comparative Example 2, but shearing did not occur in three out of three cathode bodies 3 and they were able to be connected to the lead-out terminal 7. Also, when cold welding was performed using pressing member 200 having side surface 220 inclined at 120 degrees, shearing did not occur in two out of three cathode bodies 3 and they were able to be connected to the lead-out terminal 7.

[0075] Meanwhile, an attempt was made to connect lead terminal 7 to cathode bodies 3 of Comparative Examples 1 to 3 and Examples 1 and 2 by cold pressure welding using pressing member 200 in which side surface 220 and flat surface 210 form an angle of 90 degrees. However, in each of the three individuals of Comparative Examples 1 to 3 and Examples 1 and 2, cathode body 3 was sheared, and cathode body 3 and lead terminal 7 could not be connected.

[0076] In other words, it was confirmed that by cold welding with a pressing member 200 having a side surface 220 inclined at 120 degrees or more, the cathode body 3 having a maximum static friction coefficient of 0.6 or more on the surface of the carbon layer 32 can be connected to the lead-out terminal 7 without shearing.

[0077] 6, when the pressing member 200 having the side surface 220 inclined at 150 degrees is used, the connection strength is improved even in Comparative Examples 1 to 3 having a maximum static friction coefficient of 0.51 or less. Moreover, in Examples 1 and 2 having a maximum static friction coefficient of 0.6 or more, the connection strength is further improved compared to the case where the pressing member 200 having the side surface 220 inclined at 120 degrees is used.

[0078] 7, when using a pressing member 200 having side surfaces 220 inclined at 150 degrees, it can be confirmed that the difference in connection resistance between the state lifted 0.0 mm and the state lifted 0.8 mm becomes smaller as the maximum static friction coefficient increases. Also, when using a pressing member 200 having side surfaces 220 inclined at 150 degrees and the maximum static friction coefficient is 0.6 or more, there is almost no difference in connection resistance between the state lifted 0.0 mm and the state lifted 0.8 mm. [Explanation of symbols]

[0079] 1. Electrolytic capacitor 2 Anode body 3 Cathode body 31 Cathode foil 32 Carbon layer 33 Cold Welding Area 33a flat surface 33b Slope 4. Separator 5 Dielectric oxide film 6 Electrolyte 7 Output terminal 71 Flat area 200 Pressing member 210 Flat surface 220 Side

Claims

1. an anode body having a dielectric layer formed on a surface thereof; a cathode body having a cathode foil and a carbon layer formed on the cathode foil; an electrolyte interposed between the anode body and the cathode body; Lead terminals of the anode body and the cathode body are cold-welded to each other; Equipped with the maximum static friction coefficient of the surface of the carbon layer of the cathode body is 0.6 or more; An electrolytic capacitor characterized by:

2. the carbon layer contains graphite in an amount of 18 wt % or less, including no additive, based on the total amount of all carbon materials in the carbon layer; 2. The electrolytic capacitor according to claim 1 .

3. the carbon layer contains spherical carbon as the carbon material; 3. The electrolytic capacitor according to claim 2 .

4. a cold-welded region at an interface between the cathode body and the lead terminal; The cold pressure welding region has a flat surface and an inclined surface that forms an angle with the flat surface of 120 degrees or more; 4. The electrolytic capacitor according to claim 1, wherein

5. A method for manufacturing an electrolytic capacitor in which an anode body having a dielectric layer formed on a surface thereof and a cathode body are opposed to each other with an electrolyte interposed therebetween, comprising the steps of: a cold pressure welding step of cold pressure welding a lead terminal to the cathode body having a carbon layer formed on a cathode foil and having a maximum static friction coefficient of 0.6 or more on the surface thereof; containing, A method for manufacturing an electrolytic capacitor comprising the steps of:

6. In the cold pressure welding step, the cathode body and the lead terminal are overlapped and pressed by a pressing member, the pressing member has a flat surface and a side surface that is inclined with respect to the flat surface at an angle of 120 degrees or more; The method for producing an electrolytic capacitor according to claim 5,

7. The method further comprises a cathode body preparation step in which graphite is included in a proportion of 18 wt % or less, including no additives, relative to the total amount of all carbon materials in the carbon layer.

7. The method for producing an electrolytic capacitor according to claim 5 or 6,

8. In the cathode body preparation step, spherical carbon is contained in the carbon layer as the carbon material; The method for producing an electrolytic capacitor according to claim 7,

Citation Information

Patent Citations

  • Cathode material for electrolytic capacitor

    JP1992061109A

  • Aluminum electrolytic capacitor and its manufacturing method

    JP2006080111A

  • Manufacturing method of electrolytic capacitor and electrolytic capacitor

    JP2012069829A

  • Electrolytic capacitor

    WO2016174807A1

  • Electrode body, electrolytic capacitor including electrode body, and method of manufacturing electrode body

    WO2020059609A1