Thermoelectric conversion materials and thermoelectric conversion elements
A polymer-based thermoelectric conversion material with cation-trapping ability and conductive components addresses conductivity and stability issues, offering enhanced performance under high temperature and humidity.
Patent Information
- Application Number
- JP2021121694
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-07-26
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-11-26
AI Technical Summary
Conventional thermoelectric conversion materials using organic compounds suffer from poor conductivity and stability under high temperature and high humidity conditions, limiting their practical application.
A thermoelectric conversion material comprising a polymer with monomer units derived from (meth)acrylonitrile and having cation-trapping ability, combined with a conductive material, enhances conductivity and stability by trapping cations, thereby improving thermoelectric performance.
The material achieves both high thermoelectric conversion performance and stability under harsh conditions, with improved conductivity and resistance to degradation.
Smart Images

Figure 0007582109000001 
Figure 0007582109000002 
Figure 0007582109000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoelectric conversion material and a thermoelectric conversion element. [Background technology]
[0002] Thermoelectric conversion technology, which converts heat into electricity using thermoelectric conversion materials, has been attracting attention as a clean energy source that can effectively utilize minute thermal energy such as body heat and exhaust heat from factories, cars, and homes, as well as various types of heat in nature, as electricity. There are various thermoelectric effects that are used in thermoelectric conversion technology, but the mainstream system uses the Seebeck effect, in which an electromotive force is generated by an electron gradient that occurs within a material in response to the temperature difference when two different temperatures are applied to both ends of the material, which is made up of a combination of semiconductors and metals.
[0003] Thermoelectric materials that can convert between thermal energy and electrical energy are used in thermoelectric conversion elements such as thermoelectric power generation elements and Peltier elements. Thermoelectric conversion elements are elements that convert heat into electricity and are made up of a combination of semiconductors and metals. Representative thermoelectric conversion elements are classified into p-type semiconductors alone, n-type semiconductors alone, and combinations of p-type and n-type semiconductors. To obtain a larger potential difference, thermoelectric conversion elements generally use a combination of p-type and n-type semiconductors as materials.
[0004] Thermoelectric conversion elements, such as Peltier elements, are used as thermoelectric modules that combine a number of elements into a plate or cylinder. Because they can directly convert thermal energy into electricity, they can be used, for example, as a power source for wristwatches that operate with body heat, and for power generation on the ground and in artificial satellites. The performance of a thermoelectric conversion element depends on the performance of the thermoelectric conversion material and the durability of the module.
[0005] As described in Non-Patent Document 1, the dimensionless thermoelectric figure of merit ZT is used as an index representing the performance of a thermoelectric conversion material. In addition, the power factor PF (=S 2·σ) may also be used. The dimensionless thermoelectric figure of merit ZT is expressed by the following formula (1). ZT=((S 2 ·σ) / к)·T Equation (1) Here, S is the Seebeck coefficient (V / K), σ is the electrical conductivity (S / m), T is the absolute temperature (K), and κ is the thermal conductivity (W / (m K)). Thermal conductivity κ is expressed by the following formula (2). к=α·ρ·C Equation (2) where α is the thermal diffusivity (m 2 / s), ρ is density (kg / m 3 ), and C is the specific heat capacity (J / (kg K)). That is, in order to improve the thermoelectric conversion performance (hereinafter also referred to as thermoelectric properties), it is important to improve the Seebeck coefficient or electrical conductivity while decreasing the thermal conductivity.
[0006] In recent years, research has been conducted on thermoelectric conversion elements using organic materials instead of conventional inorganic materials. Organic materials are lightweight, have excellent moldability, and are more flexible than inorganic materials, so they are highly versatile within the temperature range in which they do not decompose. In addition, they are more advantageous than inorganic materials in terms of manufacturing energy and costs, as printing technology can be easily used.
[0007] For example, Patent Document 1 discloses a thermoelectric conversion material containing a polymer dispersant having an organic dye skeleton and carbon nanotubes (CNTs) and a thermoelectric conversion element using the same. Patent Document 2 discloses a substitution compound containing a polycyclic aromatic ring and an alkyl group having carrier transport properties. A thermoelectric conversion material containing a conductive compound bonded with a substituent and a thermoelectric conversion element using the same are disclosed. However, the invention of Patent Document 1 does not provide sufficient performance as a thermoelectric conversion element. In addition, the invention of Patent Document 2 has a conductivity of 10 -8 ~10 -7The thermal conductivity of the thermoelectric conversion element is as low as 1.0 S / cm, which is not practical for use as a thermoelectric conversion element. In addition to the performance required as a thermoelectric conversion element, conventional thermoelectric conversion elements have the problem of poor stability over time under high temperature and high humidity conditions. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2015 / 050113 [Patent Document 2] International Publication No. 2015 / 129877 [Non-patent literature]
[0009] [Non-Patent Document 1] Takenobu Kajikawa, "Thermoelectric Conversion Technology Handbook (First Edition)", NTS Publishing, p. 19 Summary of the Invention [Problem to be solved by the invention]
[0010] The problem to be solved by the present invention is to provide a thermoelectric conversion material that can achieve both thermoelectric conversion performance and electrical conductivity, and to provide a thermoelectric conversion element that has excellent thermoelectric conversion performance and excellent stability over time under high temperature and high humidity conditions. [Means for solving the problem]
[0011] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention. That is, the present invention relates to a thermoelectric conversion material comprising a polymer (A) and a conductive material (B), wherein the polymer (A) is a copolymer comprising a monomer unit derived from (meth)acrylonitrile and a monomer unit having a cation trapping ability.
[0012] The present invention also relates to the above thermoelectric conversion material, wherein the monomer having a cation trapping ability comprises a monomer having one or more structures selected from the group consisting of a poly(oxyalkylene) structure, an epoxide structure, and a carbonate structure.
[0013] The present invention also relates to the above thermoelectric conversion material, in which the polymer (A) contains 1% by mass or more and less than 100% by mass of units derived from the (meth)acrylonitrile.
[0014] The present invention also relates to the above thermoelectric conversion material, wherein the polymer (A) contains from 1% by mass to 99% by mass of monomer units having a cation trapping ability.
[0015] The present invention also relates to the above thermoelectric conversion material, which further comprises an ionic compound consisting of an anion (C) and a cation (D).
[0016] The present invention also relates to a compound in which the anion (C) is OH - , R 1 O - , R 2 S - , R 3 COO - , S.H. - , BH4 - , I - , Br - and Cl - The above heat treatment method includes at least one selected from the group consisting of However, R 1 , R 2 , and R 3 is an aliphatic or aromatic hydrocarbon group. It is a hydrogen group.
[0017] The present invention also relates to the above thermoelectric conversion material, wherein the cation (D) contains a metal cation or a cation derived from an organic base.
[0018] The present invention also relates to the above thermoelectric conversion material, wherein the content of the polymer (A) is 5 to 100 mass % based on the total amount of the conductive material (B).
[0019] The present invention also relates to a thermoelectric conversion element comprising a thermoelectric conversion film containing the above-mentioned thermoelectric conversion material and electrodes, the thermoelectric conversion film and the electrodes being electrically connected to each other. Effect of the Invention
[0020] The present invention provides a thermoelectric conversion material that can achieve both thermoelectric conversion performance and electrical conductivity. In addition, the material can be used to provide a thermoelectric conversion element that has excellent thermoelectric conversion performance and excellent stability over time under high temperature and high humidity conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, an embodiment of the present invention will be described. In this specification, unless otherwise specified, the terms "(meth)acrylic", "(meth)acrylo", "(meth)acrylic acid", "(meth)acrylate", and "(meth)acryloyloxy" refer to "acrylic or methacrylic", "acrylo or methacrylo", "acrylic acid or methacrylic acid", "acrylate or methacrylate", and "acryloyloxy or methacryloyloxy", respectively.
[0022] <Thermoelectric conversion materials> The thermoelectric conversion material of the present invention is a thermoelectric conversion material comprising a polymer (A) and a conductive material (B), and is characterized in that the polymer (A) is a copolymer comprising a monomer unit derived from (meth)acrylonitrile and a monomer unit having a cation trapping ability. Hereinafter, an embodiment of the present invention will be described in detail.
[0023] <Polymer (A)> The polymer (A) is a copolymer containing a monomer unit derived from (meth)acrylonitrile and a monomer unit having a cation trapping ability. The polymer (A) may be a copolymer with other monomers as long as it contains a monomer unit derived from (meth)acrylonitrile and a monomer unit having a cation trapping ability. The polymer (A) may be in the form of either a random copolymer or a block copolymer. It is presumed that the strong polarity of the cyano group in the (meth)acrylonitrile in the polymer (A) enhances the adsorption to the conductive material (B) and suppresses the aggregation of the conductive material (B). In addition, when the thermoelectric conversion material contains a cation (C), it is presumed that the monomer unit having a cation trapping ability in the polymer (A) can capture the cation (C) in the material, thereby allowing it to be present stably in the thermoelectric conversion material.
[0024] Of the constituent units of the polymer (A), the unit derived from (meth)acrylonitrile is preferably contained in an amount of 1% by mass to 99% by mass, more preferably 50% by mass to 90% by mass, even more preferably 60% by mass to 90% by mass, and particularly preferably 75% by mass to 90% by mass. By containing the unit derived from (meth)acrylonitrile in the above range, good adsorption to the conductive material (B) can be obtained.
[0025] Of the constituent units of polymer (A), the monomer unit having cation trapping ability is preferably contained in an amount of 1 mass % or more and 99 mass % or less, more preferably 1 mass % or more and 50 mass % or less, and even more preferably 1 mass % or more and 20 mass % or less.
[0026] Among the constituent units of the polymer (A), the monomer unit having a cation trapping ability refers to a monomer unit having a structure capable of forming a coordinate bond with a cation (D). An example of a monomer having a structure capable of forming a coordinate bond with a carboxylic acid is a monomer having an ether-like structure. Examples of the ether-like structure include, but are not limited to, a poly(oxyalkylene) structure, a carbonate structure, and an epoxide structure.
[0027] Examples of monomers having a repeating unit of a poly(oxyalkylene) structure include polyethylene glycol monomethacrylate, polypropylene glycol monomethacrylate, polyethylene glycol monoacrylate, polypropylene glycol monoacrylate, methoxypolyethylene glycol methacrylate, methoxypolyethylene glycol acrylate, and triethylene glycol diacrylate. From the viewpoint of cation trapping ability, the repeating unit of the oxyalkylene structure is preferably 6 or more, more preferably 9 or more, and even more preferably 20 or more. In addition, from the viewpoint of cation trapping ability, polyethylene glycol monomethacrylate, polyethylene glycol monoacrylate, methoxypolyethylene glycol methacrylate, and methoxypolyethylene glycol methacrylate are preferred.
[0028] An example of the monomer having a carbonate structure is 4-vinyl-1,3-dioxolan-2-one. An example of the monomer having an epoxide structure is glycidyl methacrylate.
[0029] Other monomers with cation trapping ability include monomers with a calixarene structure, such as 5-vinylcalix[4]arene (MVC4), 5-vinylcalix[6]arene (MVC6), and 5-acryloyloxycalix[4]arene.
[0030] Other examples of monomers having a cation trapping structure include monomers having a crown ether structure. Examples of monomers having a crown ether structure include macrocyclic α-(a Examples of the macrocyclic α-(alkoxymethyl)acrylic acid ester derivatives include compounds having the following structure: can be.
[0031] [ka]
[0032] The polymer (A) may contain other monomers as constituent units other than the above monomers. Examples of the other monomers include: Vinyl ethers such as ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, and isobutyl vinyl ether; vinyl acetate, vinyl propionate and other vinyl fatty acids; heterocyclic (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate and 3-methyloxetanyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate; aliphatic unsaturated fatty acids such as (meth)acrylic acid and crotonic acid; Aromatic hydrocarbon compounds such as styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-methoxystyrene, 4-methoxystyrene, 4-isopropenyltoluene, 2-isopropenyltoluene, 4-n-octylstyrene, 1-vinylnaphthalene, m-vinylbenzyl cyanide, and p-vinylbenzyl cyanide; and the like.
[0033] The method for producing the polymer (A) is not particularly limited, and may be any of, for example, a solution polymerization method, a suspension polymerization method, a bulk polymerization method, an emulsion polymerization method, a precipitation polymerization method, etc., with solution polymerization or precipitation polymerization being preferred, and precipitation polymerization being most preferred. The polymer (A) obtained by the precipitation polymerization method can be quickly removed after polymerization from low molecular weight components and residual monomers that dissolve in the solvent used during polymerization, so that it is possible to narrowly control the molecular weight distribution, and the amount of residual monomers can be reduced as much as possible, and a polymer (A) with a molecular weight that functions as a dispersant can be efficiently obtained. As the polymerization reaction system, addition polymerization such as ionic polymerization, free radical polymerization, and living radical polymerization can be used, and free radical polymerization or living radical polymerization is preferred. In addition, as the radical polymerization initiator, a compound selected from peroxides, azo-based initiators, etc., or a mixture thereof can be used, and a molecular weight regulator such as a chain transfer agent may be used as necessary.
[0034] The molecular weight of the polymer (A), in terms of polystyrene equivalent weight average molecular weight, is preferably in the range of 3000 to 500000, more preferably in the range of 4000 to 200000, further preferably in the range of 5000 to 100000, and particularly preferably in the range of 10000 to 100000. By setting the weight average molecular weight within the above range, the adsorption to the conductive material (B) becomes better.
[0035] <Conductive material (B)> The conductive material (B) contributes to improving the conductivity. Therefore, the conductivity can be improved by increasing the content of the conductive material (B). The conductive material (B) is not particularly limited as long as it is a material having conductivity (carbon material, metal material, conductive polymer, etc.), and examples of the carbon material include graphite, carbon nanotubes, carbon black, graphene (including graphene nanoplates), etc. Examples of the metal material include metal powders such as gold, silver, copper, nickel, chromium, palladium, rhodium, ruthenium, indium, silicon, aluminum, tungsten, molybdenum, germanium, gallium, and platinum, as well as ZnSe, CdS, InP, GaN, SiC, SiGe, and alloys thereof, and composite powders thereof. In addition, fine particles coated with a core and a material different from the core material, specifically, for example, silver-coated copper powder in which the core material is copper and the surface is coated with silver, can be mentioned. Examples of the conductive polymer include powders of metal oxides such as silver oxide, indium oxide, tin oxide, zinc oxide, ruthenium oxide, ITO (tin-doped indium oxide), AZO (aluminum-doped zinc oxide), and GZO (gallium-doped zinc oxide), as well as powders surface-coated with these metal oxides. Examples of the conductive polymer include PEDOT / PSS (a composite of poly(3,4-ethylenedioxythiophene) and polystyrene sulfonic acid), polyaniline, polyacetylene, polypyrrole, polythiophene, and polyparaphenylene. The conductive material may be one type or a combination of two or more types. The shape of the conductive material (B) is not particularly limited, and may be amorphous, aggregated, scaly, microcrystalline, spherical, flake, wire, or the like, as appropriate.
[0036] From the viewpoint of achieving both the Seebeck coefficient and electrical conductivity, at least one selected from the group consisting of carbon nanotubes, carbon black, and graphene (including graphene nanoplates) is preferred, more preferably carbon nanotubes, and particularly preferably single-walled carbon. There are nanotubes.
[0037] Examples of carbon materials include flaky graphite such as CMX, UP-5, UP-10, UP-20, UP-35N, CSSP, CSPE, CSP, CP, CB-150, CB-100, ACP, ACP-1000, ACB-50, ACB-100, ACB-150, SP-10, SP-20, J-SP, SP-270, HOP, GR-60, LEP, F#1, and F manufactured by Nippon Graphite Industries Co., Ltd. Examples of the graphite include #2, F#3, BF-3AK, FBF, BF-15AK, CBR, CPB-6S, CPB-3, 96L, 96L-3, K-3, SC-120, SC-60, HLP, CP-150, and SB-1 manufactured by Chuetsu Graphite Industry Co., Ltd., EC1500, EC1000, EC500, EC300, EC100, and EC50 manufactured by Ito Graphite Industry Co., Ltd., and 10099M and PB-99 manufactured by Nishimura Graphite Co., Ltd. Examples of the spherical natural graphite include CGC-20, CGC-50, CGB-20, and CGB-50 manufactured by Nippon Graphite Industry Co., Ltd. Examples of the amorphous graphite include Blue P, AP, AOP, and P#1 manufactured by Nippon Graphite Industry Co., Ltd., and APR, K-5, AP-2000, AP-6, 300F, and 150F manufactured by Chuetsu Graphite Co., Ltd. Examples of artificial graphite include PAG-60, PAG-80, PAG-120, PAG-5, HAG-10W, and HAG-150 manufactured by Nippon Graphite Industries Co., Ltd.; G-4AK, G-6S, G-3G-150, G-30, G-80, G-50, SMF, EMF, SFF, SFF-80B, SS-100, BSP-15AK, BSP-100AK, and WF-15C manufactured by Chuetsu Graphite Co., Ltd.; and SGP-100, SGP-50, SGP-25, SGP-15, SGP-5, SGP-1, SGO-100, SGO-50, SGO-25, SGO-15, SGO-5, SGO-1, SGX-100, SGX-50, SGX-25, SGX-15, SGX-5, and SGX-1 manufactured by SEC Carbon Co., Ltd.
[0038] Examples of commercially available conductive carbon fibers and carbon nanotubes include vapor grown carbon fibers such as VGCF manufactured by Showa Denko K.K.; single-walled carbon nanotubes such as EC1.5 and EC1.5-P manufactured by Meijo Nano Carbon Co., Ltd., TUBALL manufactured by Kusumoto Chemicals Co., Ltd., and ZEONANO manufactured by Zeon Nano Technology Inc.; FloTube9000, FloTube7000, and FloTube2000 manufactured by CNano Corporation; NC7000 manufactured by Nanocyl Corporation; and 100T and 200P manufactured by Knano Corporation.
[0039] Examples of commercially available carbon black include Tokai Carbon's Tokablack #4300, #4400, #4500, and #5500; Degussa's Printex L; and Colombian's Raven7000, 5750, 5250, 5000ULTRAIII, and 500. Examples of the black include furnace blacks such as #2350, #2400B, #2600B, #3050B, #3030B, #3230B, #3350B, #3400B, and #5400B manufactured by Mitsubishi Chemical Corporation, MONARCH1400, 1300, and 900, VulcanXC-72R, and BlackPearls2000 manufactured by Cabot Corporation, Ensaco250G, Ensaco260G, Ensaco350G, and SuperP-Li manufactured by TIMCAL Corporation, Ketjen blacks such as EC-300J and EC-600JD manufactured by Lion Corporation, and acetylene blacks such as Denka Black, Denka Black HS-100, and FX-35 manufactured by Denki Kagaku Kogyo Co., Ltd., but are not particularly limited thereto.
[0040] When the monomer units derived from acrylonitrile in polymer (A) form a cyclic structure, the dispersibility, fluidity, and storage stability of the thermoelectric conversion material are improved. For example, when polymer (A) is treated with alkali, the monomer units derived from acrylonitrile are converted to a cyclic structure such as a hydrogenated naphthyridine ring, thereby improving dispersibility. In addition, although the detailed mechanism is unknown, the formation of a cyclic structure also improves the thermoelectric performance of the thermoelectric conversion material. The presence of a cyclic structure increases the adsorption to conductive material (B), and carrier transfer from polymer (A) to conductive material (B) is facilitated. This is thought to be because movement is now more likely to occur.
[0041] <Ionic compounds> The thermoelectric conversion material of the present invention may contain an ionic compound consisting of an anion (C) and a cation (D). Examples of the ionic compound include, but are not limited to, inorganic bases, inorganic metal salts, organic salts other than onium salts, onium salts, etc.
[0042] Examples of inorganic bases include metal hydroxides. Examples of metal hydroxides include hydroxides of alkali metals and hydroxides of alkaline earth metals. Examples of alkali metal hydroxides include lithium hydroxide, sodium hydroxide, potassium hydroxide, etc. Examples of alkaline earth metal hydroxides include calcium hydroxide, magnesium hydroxide, etc. Among these, hydroxides of alkali metals are preferred, and sodium hydroxide and potassium hydroxide are more preferred.
[0043] Examples of inorganic metal salts include metal carbonates. Examples of metal carbonates include alkali metal carbonates and alkaline earth metal carbonates. Examples of alkali metal carbonates include lithium carbonate, lithium hydrogen carbonate, sodium carbonate, sodium hydrogen carbonate, potassium carbonate, and potassium hydrogen carbonate. Examples of alkaline earth metal carbonates include calcium carbonate and magnesium carbonate. Among these, alkali metal carbonates are preferred, and lithium carbonate and sodium carbonate are more preferred. The metal in the inorganic base or inorganic metal salt may be a transition metal.
[0044] Examples of organic salts other than onium salts include carboxylates, sulfonates, phenolates, and metal alkoxides. Examples of carboxylates include sodium acetate and sodium benzoate. Examples of sulfonates include sodium p-toluenesulfonate. Examples of phenolates include sodium phenolate. Examples of metal alkoxides include sodium methoxide, sodium ethoxide, sodium tert-butoxide, potassium methoxide, potassium ethoxide, and potassium tert-butoxide.
[0045] Examples of the onium salt include ammonium salt, oxonium salt, sulfonium salt, iodonium salt, bromonium salt, etc. Examples of the ammonium salt include ammonium hydroxide, ammonium fluoride, ammonium chloride, ammonium bromide, ammonium iodide, etc.
[0046] Examples of the ammonium hydroxide include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and benzyltrimethylammonium hydroxide. Examples of ammonium fluoride include tetramethylammonium fluoride tetrahydrate, tetraethylammonium fluoride hydrate, and tetrabutylammonium fluoride. Examples of ammonium chloride include acetylcholine chloride, triethylmethylammonium chloride, tetraethylammonium chloride, tetrapropylammonium chloride, and decyltrimethylammonium chloride. Examples of ammonium bromides include acetylcholine bromide, tetramethylammonium bromide, tetraethylammonium bromide, trimethylphenylammonium bromide, 1-butyl-1-methylpiperidinium bromide, and hexyldimethyloctylammonium bromide. Ammonium iodides include acetylcholine iodide and tetramethylammonium iodide. ammonium iodide, tetraethylammonium iodide, tetrapropylammonium iodide, tetrabutylammonium iodide, tetraamylammonium iodide, trimethylphenylammonium iodide, and the like.
[0047] Examples of the oxonium salt include trimethyloxonium tetrafluoroborate and triethyloxonium tetrafluoroborate. Examples of the sulfonium salt include dimethyl(methylthio)sulfonium tetrafluoroborate, trimethylsulfonium bromide, and the like. Examples of iodonium salts include bis(2,4,6-trimethylpyridine)iodonium hexafluorophosphate, diphenyliodonium perchlorate, and the like. Bromonium salts include bis(2,4,6-trimethylpyridine)bromonium hexafluorophosphate and the like.
[0048] The thermoelectric conversion material of the present invention may contain an ionic compound consisting of an anion (C) and a cation (D). The ionic compound is preferably blended in an amount of 1 to 70 parts by mass, more preferably 4 to 60 parts by mass, and even more preferably 4 to 20 parts by mass, per 100 parts by mass of the conductive material (B). By using such an amount, the dispersibility is further improved, and the electrical conductivity and stability over time of the thermoelectric conversion element are further improved.
[0049] <Anion (C)> The anion (C) is OH - , R 1 O - , R 2 S - , R 3 COO - , S.H. - , BH4 - , I - , Br - , Cl - , BF4 - , PF6 -, ClO4 - Among these, OH - , R 1 O - , R 2 S - , R 3 COO - , S.H. - , BH4 - , I - , Br - and Cl - Preferably, the group is at least one selected from the group consisting of OH - or R 1 O - It is more preferable that So, R 1 , R 2 , and R 3 is an aliphatic hydrocarbon group or an aromatic hydrocarbon group.
[0050] Examples of the aliphatic hydrocarbon group include an alkyl group, a cycloalkyl group, an alkenyl group, and an alkynyl group. The alkyl group includes a straight chain alkyl group and a branched alkyl group. Examples of the straight-chain alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, a hexadecyl group, and an icosyl group. Examples of the branched alkyl group include an isopropyl group, an isobutyl group, an isopentyl group, a neopentyl group, a 2-ethylhexyl group, a tertiary butyl group, a tertiary pentyl group, and an isopentadecyl group. Examples of the cycloalkyl group include a cyclopropyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a tricyclodecyl group, a norbornyl group, and an adamantyl group. Examples of the alkenyl group include a vinyl group (ethenyl group), a 1-propenyl group, a 2-propenyl group, a 2-butenyl group, a 1-butenyl group, a 1-hexenyl group, a 2-dodecenyl group, and a pentenyl group. Examples of the alkynyl group include an ethynyl group, a 1-propynyl group, a 2-propynyl group, a 1-butynyl group, a 3-hexynyl group, and a 2-dodecynyl group.
[0051] Examples of the aromatic hydrocarbon group include aryl groups, etc. Examples of the aryl group include a phenyl group, a biphenylyl group, a terphenylyl group, a naphthyl group, and an anthryl group.
[0052] <Cation (D)> Examples of the cation (D) include metal ions and cations derived from organic bases. Metal Examples of the ion include typical metal ions, transition metal ions, etc. Examples of the metal ion include lithium ions, sodium ions, potassium ions, rubidium ions, cesium ions, francium ions, beryllium ions, magnesium ions, calcium ions, strontium ions, barium ions, radium ions, and scandium ions.
[0053] Examples of the cation derived from an organic base include cations derived from primary, secondary, or tertiary amines, and cations derived from other basic nitrogen-containing organic compounds. Examples of the cation derived from a primary, secondary, or tertiary amine include cations derived from ethylamine, butylamine, diethylamine, dibutylamine, triethylamine, tributylamine, etc. Examples of the cation derived from other basic nitrogen-containing organic compounds include cations derived from pyridine, quinoline, isoquinoline, pyrrolidine, piperidine, aziridine, polyethyleneimine, etc.
[0054] From the viewpoints of dispersing the conductive material (B) in the thermoelectric conversion material, improving the Seebeck coefficient, and achieving compatibility with electrical conductivity, the content of the polymer (A) is preferably 400% by mass or less, more preferably 200% by mass or less, even more preferably 120% by mass or less, and particularly preferably 100% by mass or less, based on the total amount of the conductive material (B). In order to exert the effects of the polymer (A), the lower limit of the polymer (A) is preferably 5% by mass or more, more preferably 20% by mass or more, even more preferably 25% by mass or more, and particularly preferably 40% by mass or more, based on the total amount of the conductive material (B).
[0055] The content of polymer (A) in the thermoelectric conversion material is preferably 4 mass% or more and 80 mass% or less, more preferably 20 mass% or more and 60 mass% or less, and even more preferably 40 mass% or more and 50 mass% or less.
[0056] Furthermore, the content of the conductive material (B) in the thermoelectric conversion material is preferably 15 mass% or more and 90 mass% or less, more preferably 30 mass% or more and 80 mass% or less, and even more preferably 50 mass% or more and 60 mass% or less.
[0057] In order to maintain the thermoelectric properties, the thermoelectric conversion material of the present invention preferably does not contain a compound that generates radicals, and more preferably consists of only the polymer (A) and the conductive material (B), or the polymer (A), the conductive material (B) and an ionic compound, but may contain other components as necessary.
[0058] (dispersion medium) The dispersion medium can be used as a medium when mixing the polymer (A) and the conductive material (B). The inclusion of the dispersion medium results in an ink or paste state, which can be used to form a thermoelectric conversion film by printing or coating. The dispersion medium that can be used is preferably one that can dissolve or disperse the polymer (A) and the conductive material (B), and examples of such dispersion medium include organic solvents and water. The dispersion medium may be used alone or in combination of two or more types.
[0059] Examples of organic solvents include alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol methyl ether, terpineol, dihydroterpineol, 2,4-diethyl-1,5-pentanediol, 1,3-butylene glycol, isobornylcyclohexanol, ethylene glycol, 1,3-propanediol, 1,4-butanediol, glycerin, trifluoroethanol, m-cresol, and thiodiglycol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; tetrahydrofuran, dioxane, and ethylene glycol dimethyl. The solvent can be appropriately selected as necessary from ethers such as ether, hydrocarbons such as hexane, heptane, octane, aromatics such as benzene, toluene, xylene, cumene, esters such as ethyl acetate, butyl acetate, N-methylpyrrolidone, etc. From the viewpoint of dispersibility and solubility of the polymer (A) and the conductive material (B), N-methylpyrrolidone is particularly preferable.
[0060] (resin) The thermoelectric conversion material of the present invention may further contain a resin for the purpose of adjusting the film-forming property and film strength. The resin may be used alone or in combination of two or more. The resin may also be a copolymer of these resins. Although not particularly limited, in one embodiment, polyurethane resin, acrylic resin, and acrylamide resin are preferable. From the viewpoint of electrical conductivity, when a resin is contained, the content of the resin is preferably 99 mass% or less, more preferably 50 mass% or less, and even more preferably 20 mass% or less, based on the total mass of the polymer (A) and the conductive material (B).
[0061] (Inorganic thermoelectric conversion materials) The thermoelectric conversion material of the present invention may contain an inorganic thermoelectric conversion material as necessary in order to improve the thermoelectric conversion performance. The inorganic thermoelectric conversion material is not particularly limited, and any material generally known as a thermoelectric conversion material can be used.
[0062] <Thermoelectric conversion element> The thermoelectric conversion element of the present invention has a thermoelectric conversion film formed using the thermoelectric conversion material of the present invention and electrodes, and the thermoelectric conversion film and the electrodes are electrically connected. The thermoelectric conversion film is excellent in heat resistance and flexibility in addition to electrical conductivity and thermoelectric properties. Therefore, a high-quality thermoelectric conversion element can be easily produced.
[0063] The thermoelectric conversion film may be a film obtained by applying a thermoelectric conversion material onto a substrate. Since the thermoelectric conversion material has excellent moldability, it is easy to obtain a good film by application or printing. The method for producing the thermoelectric conversion film is not particularly limited as long as the desired thermoelectric conversion film can be obtained, and can be appropriately selected according to the properties of the thermoelectric conversion material, such as viscosity, and the required film thickness, area, shape, and other conditions. For example, methods using various means such as spin coating, spray coating, roll coating, gravure coating, flexo coating, die coating, lip coating, knife coating, blade coating, comma coating, roll coating, curtain coating, bar coating, dip coating, dispenser, screen coating, and inkjet printing can be mentioned.
[0064] The thickness of the thermoelectric conversion film is not particularly limited and can be set according to the required electric properties such as current value, voltage value, and resistance, and thermoelectric properties, but as described later, it is preferable that the film is formed to have a certain thickness or more so that a temperature difference can be generated and transmitted in the thickness direction or surface direction of the thermoelectric conversion film. From the viewpoint of thermoelectric properties and flexibility, the film thickness of the thermoelectric conversion film is preferably in the range of 0.1 to 200 μm, more preferably in the range of 1 to 100 μm, and particularly preferably in the range of 1 to 60 μm.
[0065] The substrate is not particularly limited, and examples of the substrate that can be used include nonwoven fabric, paper, plastic films made of materials such as polyethylene, polyethylene terephthalate (PET), polyethylene naphthalate, polyethersulfone, polypropylene, polyimide, polycarbonate, and cellulose triacetate, and glass, etc. These substrates may have an aluminum deposition layer or a barrier layer on the substrate surface to prevent deterioration of the thermoelectric conversion material due to the effects of water and oxygen.
[0066] In order to improve the adhesion between the substrate and the thermoelectric conversion film, various treatments are performed on the substrate surface. Specifically, prior to application of the thermoelectric conversion material, a UV ozone treatment, a corona treatment, a plasma treatment, or a treatment for improving adhesion can be performed.
[0067] The thermoelectric conversion film may be laminated with a substrate, or may be a free-standing film without a substrate. When preparing a free-standing film, there is no particular limitation, but for example, the film can be obtained by forming the thermoelectric conversion film on a release sheet and then removing the release coat.
[0068] Examples of the release sheet include release-treated plastic films such as polyester film, polyethylene film, polypropylene film, and polyimide film.
[0069] The thermoelectric conversion element can be constructed by applying techniques well known in the art, except that it is constructed using the above-mentioned thermoelectric conversion material. A more specific configuration of the thermoelectric conversion element and a manufacturing method thereof will be described below.
[0070] In a thermoelectric conversion element, a thermoelectric conversion film and an electrode are electrically connected. Here, "electrically connected" means that they are joined to each other or can be electrically connected via other components such as wires.
[0071] The material of the electrode is not particularly limited as long as it functions as an electrode, and can be selected from metals, alloys, and semiconductors. In one embodiment, metals and alloys are preferred because they have high electrical conductivity and low contact resistance of the thermoelectric conversion film. For example, it is preferred that the electrode contains at least one selected from the group consisting of gold, silver, copper, platinum, nickel, and aluminum. It is more preferred that the electrode contains silver.
[0072] The method for forming the electrodes is not particularly limited, and the electrodes can be formed by a method such as vacuum deposition, thermocompression bonding of an electrode material foil or a film having an electrode material film, application of a paste in which fine particles of the electrode material are dispersed, etc. From the viewpoint of process simplicity, a method using thermocompression bonding of an electrode material foil or a film having an electrode material film, or application of a paste in which the electrode material is dispersed is preferred.
[0073] Typical examples of the structure of a thermoelectric conversion element can be broadly classified into (1) a structure in which electrodes are formed on both ends of the thermoelectric conversion film of the present invention, and (2) a structure in which the thermoelectric conversion film of the present invention is sandwiched between two electrodes, based on the positional relationship between the thermoelectric conversion film and a pair of electrodes. The thermoelectric conversion element having the structure (1) above can be obtained, for example, by forming a thermoelectric conversion film on a substrate, and then applying silver paste to both ends of the film to form the first and second electrodes. In this way, a thermoelectric conversion element having electrodes formed on both ends of the thermoelectric conversion film can easily increase the distance between the two electrodes. Therefore, it is easy to generate a large temperature difference between the two electrodes and perform efficient thermoelectric conversion.
[0074] The thermoelectric conversion element having the structure of (2) above can be obtained, for example, by applying silver paste onto a substrate to form a first electrode, forming the thermoelectric conversion film of the present invention thereon, and further applying silver paste onto the first electrode to form a second electrode. In this way, a thermoelectric conversion element having the thermoelectric conversion film of the present invention sandwiched between two electrodes can utilize the temperature difference in the film thickness direction of the thermoelectric conversion film, that is, in the direction perpendicular to the substrate, and can be used in a form attached to a heat source. Therefore, it is preferable because it has the advantage of being able to extract heat from a wide range from the heat source. In the thermoelectric conversion element having the structure of (2) above, it is also possible to ensure a temperature difference by increasing the film thickness to widen the distance between the two electrodes.
[0075] Thermoelectric conversion elements can generate high voltages when connected in series, and can generate large currents when connected in parallel. According to the present invention, since the thermoelectric conversion element has excellent flexibility, it is possible to satisfactorily install the element on a heat source having a shape that is not flat. The thermoelectric conversion element may have a heat absorption layer or a heat storage layer for efficient heat transfer from a heat source, and may also have a heat insulation layer or a heat dissipation layer for ensuring a temperature difference. Furthermore, depending on the application and the amount of power required, the extracted electricity can be boosted using a boost circuit, or the extracted electric energy can be temporarily stored in a condenser, a capacitor, a secondary battery, or the like for use. EXAMPLES
[0076] The present invention will be described in more detail below with reference to experimental examples, but the present invention is not limited to these examples. In the examples, "parts" means "parts by mass" and "%" means "% by mass". In addition, "NMP" refers to N-methylpyrrolidone.
[0077] (Method of measuring weight average molecular weight (Mw)) The weight average molecular weight (Mw) was measured by gel permeation chromatography (GPC) equipped with a differential refractive index (RI) detector. The instrument used was an HLC-8320GPC (manufactured by Tosoh Corporation), with three separation columns connected in series, and the packing materials used were Tosoh Corporation's "TSK-GELSUPERAW-4000", "AW-3000" and "AW-2500", respectively. The oven temperature was 40°C, and an N,N-dimethylformamide solution of 30 mM triethylamine and 10 mM LiBr was used as the eluent, at a flow rate of 0.6 mL / min. The measurement sample was adjusted to a concentration of 1% in the dispersion medium consisting of the above eluent, and 20 μL was injected. The molecular weight is a polystyrene equivalent value.
[0078] <Production of Polymer (A)> (Production Example 1) (Production of Polymer (A-1)) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 100 parts of acetonitrile, 99 parts of acrylonitrile, 1 part of PME400, and 1 part of 3-mercapto-1,2-propanediol, and substituted with nitrogen gas. The reaction vessel was heated to 70°C, and a mixture consisting of 10 parts of acetonitrile and 0.4 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.: V-65) was dropped into the reaction vessel over 6 hours to carry out a polymerization reaction. After the dropwise addition, the reaction was carried out at 70°C for 1 hour, and then 0.1 parts of V-65 was added, and the reaction was continued at 70°C for another 1 hour to obtain the target product as a precipitate. Thereafter, it was confirmed that the conversion rate exceeded 98% by measuring the nonvolatile content. The product was filtered out by vacuum filtration, washed with 100 parts of acetonitrile, and the solvent was completely removed by vacuum drying to obtain a polymer (A-1).
[0079] (Examples 2 to 21) (Production of Polymers (A-2) to (A-21)) Polymers (A-2) to (A-21) were produced in the same manner as in Production Example 1, except that the types and amounts of monomers were changed as shown in Table 1. The Mw of each polymer is shown in Table 1. In the synthesis of polymers (A-2) to (A-21), the Mw was adjusted by adding a chain transfer agent, adjusting the amount of polymerization initiator, and appropriately changing reaction conditions, etc. In addition, 3-mercapto-1,2-propanediol was used as a chain transfer agent.
[0080] In Table 1, unless otherwise specified, the numerical values represent "parts", and blank spaces mean that no ingredient was blended. The abbreviations used in this specification are as follows. HEA: Hydroxyethyl acrylate BA: Butyl acrylate PME400: (NOF Corp. "Blenmer PME400" methoxypolyethylene glycol methacrylate, polyethylene glycol repeating units are approximately 9) AME400: (NOF Corp. "Blenmer AME400" methoxypolyethylene glycol acrylate, polyethylene glycol repeating units are approximately 9) PME1000: (NOF Corp. "Blenmar PME1000" methoxypolyethylene glycol methacrylate, polyethylene glycol repeating units are approximately 23) PP800: (NOF Corp. "Blenmer PP800" polypropylene glycol monomethacrylate) GMA: glycidyl methacrylate 3EG-A: (Kyoeisha Light Acrylate 3EG-A: Triethylene Glycol Diacrylate) Macrocyclic α-alkoxymethyl acrylate ester (compound with the following structure)
[0081] [ka]
[0082] <Production of Dispersion Containing Thermoelectric Conversion Material> [Example 1] (Dispersion 1) 0.3 parts of polymer (A-1), 0.4 parts of SWCNT (OCSiAl's single-walled carbon nanotube "TUBALL"), 79.3 parts of NMP, 0.036 parts of sodium hydroxide as an ionic compound, and 〇 parts of DB15C5 as a cation capture agent (E) were weighed and mixed. Beads were further added, and the mixture was shaken with a Scandex for 4 hours, and then filtered to remove the beads, to obtain a dispersion liquid 1 of a thermoelectric conversion material.
[0083] [Examples 2 to 34, Comparative Examples 1 to 2] (Dispersion 2~34, 101~102) Except for changing the types and amounts of materials as shown in Table 2, the same production method as for Dispersion 1 was used to obtain Dispersions 2 to 34 and 101 to 102 of thermoelectric conversion materials, respectively.
[0084] The abbreviations for the materials listed in Table 2 are as follows. Conductive material (B) SWCNT: OCSiAl's single-walled carbon nanotube "TUBALL" MWCNT: (Kumho Petrochemical's multi-walled carbon nanotubes "Knanos100P") CB: (Lion Ketjen Black "EC-300J") Polymer that is not polymer (A) PVA: Exeval RS-2117 (Kuraray) Ionic Compounds TBAOH: Tetrabutylammonium hydroxide
[0085] <Evaluation of Thermoelectric Conversion Materials> The obtained dispersions 1 to 34, 101 to 102 were each applied to a 75 μm thick PET film, which was a sheet-like substrate, using an applicator, and then dried at 120° C. for 30 minutes to obtain a laminate having a thermoelectric conversion film with a thickness of 5 μm. The obtained laminates having thermoelectric conversion films (hereinafter also referred to as coating films) were evaluated for electrical conductivity, Seebeck coefficient, and stability over time in an environment of 85° C. and 85% humidity according to the following method. The results are shown in Table 2.
[0086] (Electrical conductivity (resistivity)) Immediately after production, the laminate was cut into a size of 2.5 cm × 5 cm, and the conductivity was measured by the four-probe method using Loresta GX MCP-T700 (manufactured by Mitsubishi Chemical Analytech Co., Ltd.) in accordance with JIS-K7194. The conductivity is shown in Table 2 as a relative value when the conductivity of Comparative Example 1 is set to 1.
[0087] (Seebeck coefficient) Immediately after production, the laminate was cut into a size of 3 mm × 10 mm, and the Seebeck coefficient (μV / K) at 80° C. was measured using a ZEM-3LW manufactured by Advance Riko Co., Ltd. Table 2 shows the relative values when the Seebeck coefficient of Comparative Example 1 was set to 1.
[0088] (Stability over time under high temperature and humidity conditions) The Seebeck coefficient of the laminate immediately after preparation was measured after leaving it for 10 days in an environment of 85°C and 85% humidity. The rate of change in the Seebeck coefficient of the laminate immediately after preparation (the Seebeck coefficient listed in Table 2) was determined and evaluated based on the following criteria. ◎: The change in the Seebeck coefficient is 10% or less. (Very good) ○: The rate of change in the Seebeck coefficient is greater than 10% and less than 20% (good). △: The rate of change in the Seebeck coefficient is greater than 20% and less than 50%. (Usable) ×: The rate of change in the Seebeck coefficient is greater than 50%. In the case of an n-type thermoelectric element, this also includes cases where a negative Seebeck coefficient turns to a positive one (defective).
[0089] As shown in Table 2, the thermoelectric conversion material of the present invention exhibited high electrical conductivity and Seebeck coefficient. Furthermore, it was confirmed that the thermoelectric conversion material had excellent stability over time under high temperature and high humidity conditions. This is believed to be because polymer A (A) has a cation trapping ability, and thus was able to trap cations in the film and prevent oxidation from oxygen and other substances in the system.
[0090] <Manufacturing of thermoelectric conversion elements> The above dispersions were applied onto a PET film having a thickness of 50 μm, and five thermoelectric conversion layers each having a thickness of 20 μm and a shape of 5 mm×30 mm were prepared at intervals of 10 mm. Next, four silver circuits (electrodes) having a thickness of 10 μm and a shape of 5 mm×33 mm were prepared using silver paste so that each thermoelectric conversion layer was connected in series, and thermoelectric conversion elements were manufactured. As the above silver paste, REXALPHA RA-FS 074 manufactured by Toyo Ink Co., Ltd. was used. When the electromotive force of each thermoelectric conversion element was measured, it was confirmed that the thermoelectric conversion elements manufactured using the dispersions manufactured in Examples 1 to 34 had a superior Seebeck coefficient to the thermoelectric conversion elements manufactured using the dispersions manufactured in Comparative Examples 1 and 2.
[0091] [Table 1]
[0092] [Table 2]
Claims
1. A thermoelectric conversion material comprising a polymer (A) and a conductive material (B), wherein the polymer (A) is a copolymer comprising a monomer unit derived from (meth)acrylonitrile and a monomer unit having a cation trapping ability, wherein the monomer having a cation trapping ability comprises a monomer having an epoxide structure, and the polymer (A) contains 40 mass % or more and less than 100 mass % of the unit derived from (meth)acrylonitrile, except for those in which the monomer having a cation trapping ability in the polymer (A) comprises a monomer having one or more structures selected from the group consisting of a poly(oxyalkylene) structure and a carbonate structure.
2. 2. The thermoelectric conversion material according to claim 1, wherein the polymer (A) contains from 1% by mass to 60% by mass of a monomer unit having a cation trapping ability.
3. 3. The thermoelectric conversion material according to claim 1, further comprising an ionic compound comprising an anion (C) and a cation (D).
4. The anion (C) is OH - , R 1 O - , R 2 S - , R 3 COO - , S.H. - , B.H. 4 - , I - , B - and Cl - The thermoelectric conversion material according to claim 3, characterized in that it contains at least one selected from the group consisting of: 1 , R 2 , and R 3 is an aliphatic hydrocarbon group or an aromatic hydrocarbon group.
5. 5. The thermoelectric conversion material according to claim 3, wherein the cation (D) includes a metal cation or a cation derived from an organic base.
6. 6. The thermoelectric conversion material according to claim 1, wherein the content of the polymer (A) is 5 to 100 mass % based on the total amount of the conductive material (B).
7. A thermoelectric conversion element comprising a thermoelectric conversion film comprising the thermoelectric conversion material according to any one of claims 1 to 6, and electrodes, the thermoelectric conversion film and the electrodes being electrically connected to each other.
Citation Information
Patent Citations
Thermoelectric conversion material, composition for thermoelectric conversion element, thermoelectric conversion film, and thermoelectric conversion element using them
JP2014199837A
Film-like connecting material, connected structure production method and connected structure
JP2015108060A
Thermoelectric conversion element
JP2016058475A
Thermoelectric conversion material and thermoelectric conversion element
WO2015050113A1
Thermoelectric conversion material and thermoelectric conversion element
WO2015129877A1