Inkjet recording method and image recording material

The inkjet recording method improves hot water resistance by using a two-liquid system with thermally decomposable flocculants and organic amines in the inkjet recording method, addressing the inadequacies of existing methods in high-temperature environments.

JP7582213B2Active Publication Date: 2024-11-13KONICA MINOLTA INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021575684
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-04
Filing Date
2021-01-14
Publication Date
2024-11-13
Estimated Expiration
2041-01-14

AI Technical Summary

Technical Problem

Existing inkjet recording methods for forming images on precoat films lack sufficient hot water resistance, particularly in high-temperature environments required for flexible packaging and boil retort processes, due to inadequate ink fixability and pigment flocculant deterioration.

Method used

An inkjet recording method using a two-liquid system with an aqueous precoat composition containing a flocculant, polymer dispersant, and resin fine particles, where the flocculant is thermally decomposable, and a neutralizing agent like organic amines is used to improve hot water resistance by decomposing the flocculant during drying at temperatures above its thermal decomposition point.

Benefits of technology

The method enhances the hot water resistance of the image recording material, ensuring high ink fixability and durability even in boiling conditions, suitable for packaging materials like canned food and retort foods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582213000005
    Figure 0007582213000005
  • Figure 0007582213000006
    Figure 0007582213000006
  • Figure 0007582213000007
    Figure 0007582213000007
Patent Text Reader

Abstract

The present invention addresses the problem of providing: a two-part inkjet-recording method that is for forming an image on a pre-coat applied film, and that provides improved hot water resistance; and an image-recorded article obtained by using the inkjet-recording method. The inkjet-recording method according to the present invention includes: a step for applying an aqueous pre-coat composition to a base material or a step for applying the aqueous pre-coat composition to the base material and drying the aqueous pre-coat composition; and a step for subsequently applying and drying an aqueous ink composition, the steps being carried out in that order. The inkjet recording method is characterized in that: the aqueous pre-coat composition contains at least a flocculant; the aqueous ink composition contains at least a pigment, a polymer dispersing agent, and fine resin particles; the flocculant is selected from pyrolytic cation resins, organic acids, or multivalent metal salts; a neutralizer for the polymer dispersing agent is selected from organic amines; and step for setting the temperature at which the aqueous ink composition is dried to be equal to or higher than the pyrolytic temperature of the flocculant is included.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an inkjet recording method and an image recorded matter, and more particularly to an inkjet recording method having improved hot water resistance in a two-liquid inkjet recording method in which an image is formed on a precoat coating film, and an image recorded matter using the same. [Background technology]

[0002] In the inkjet method aimed at high-speed printing, a two-liquid inkjet recording method is known in which an image is formed on a precoat coating film containing a pigment flocculant (see, for example, Patent Document 1). Since the pigment dispersion is anionic, the pigment flocculant is generally selected from cationic resins, organic acids, polyvalent metal salts, and the like.

[0003] On the other hand, image recording materials may require hot water resistance. For example, in the field of flexible packaging, the boiling and retorting fields require a process of high-temperature sterilization of the packaging, and are therefore in need of products with a higher level of hot water resistance. Specifically, they are required to have high ink fixation properties and boiling and retorting suitability, which provides excellent fixation to recording media even in high-temperature water environments.

[0004] For example, it has been proposed to improve the lamination strength and image abrasion resistance by selecting a nonionic resin as the resin type of the precoat liquid (see, for example, Patent Document 2), but hot water resistance is still insufficient. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-202596 A [Patent Document 2] JP 2018-94902 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide an inkjet recording method having improved hot water resistance in a two-liquid inkjet recording method in which an image is formed on a precoat coating film, and an image recorded using the same. [Means for solving the problem]

[0007] In the course of investigating the causes of the above problems in order to solve the above problems, the present inventors discovered that the hot water resistance of the pigment dispersant can be improved by selecting an organic amine as a neutralizing agent for the pigment dispersant and utilizing amine elimination by heating, and further discovered that the hot water resistance of the image recording material can be improved by thermally decomposing the pigment aggregating agent, which is also a cause of deterioration of the hot water resistance, during drying.

[0008] That is, the above-mentioned problems of the present invention are solved by the following means.

[0009] 1. An inkjet recording method comprising the steps of applying an aqueous precoat composition onto a substrate, or applying and drying the aqueous precoat composition, and then applying and drying the aqueous ink composition, in that order, The aqueous precoat composition contains at least a flocculant, The aqueous ink composition contains at least a pigment, a polymer dispersant, A neutralizer for the polymer dispersant and resin fine particles, the flocculant is selected from a thermally decomposable cationic resin, an organic acid, or a polyvalent metal salt; The neutralizing agent for the polymeric dispersant is selected from an organic amine, and The inkjet recording method according to claim 1, further comprising a step of drying the aqueous ink composition at a temperature equal to or higher than a thermal decomposition temperature of the aggregating agent.

[0010] 2. The ink-jet recording method described in item 1, wherein the step of applying the aqueous precoat composition is a step using an ink-jet method.

[0011] 3. The inkjet recording method described in item 1 or 2, wherein the content of the coagulant is 5% by mass or less based on the aqueous precoat composition.

[0012] 4. The inkjet recording method described in any one of items 1 to 3, wherein the temperature for drying the aqueous ink composition is 220° C. or lower.

[0013] 5. The inkjet recording method described in any one of items 1 to 4, characterized in that the resin of the resin microparticles of the aqueous ink composition is selected from a polyurethane resin, a polyacrylic resin, or a composite resin of a polyurethane resin and a polyacrylic resin.

[0014] 6. The inkjet recording method described in any one of items 1 to 5, wherein the aqueous precoat composition further contains resin fine particles, and the resin of the resin fine particles is selected from a polyester resin, a polyurethane resin, a polyacrylic resin, or a composite resin of a polyurethane resin and a polyacrylic resin.

[0015] 7. An image recording material having at least four layers laminated on a metal substrate, The first layer and the fourth layer contain a thermosetting resin; The second layer is at least Thermal decomposition product of The flocculant is selected from a thermally decomposable cationic resin, an organic acid, or a polyvalent metal salt; The third layer is at least a pigment and a polymer dispersant. A neutralizer for the polymer dispersant and resin fine particles, and a neutralizer for the polymer dispersant is selected from organic amines. R 1. An image recording material comprising:

[0016] 8. The flocculant Thermal decomposition product of 8. The image recorded matter described in item 7, wherein the content of said compound is 5% by mass or less relative to said second layer.

[0017] 9. The image recording material described in item 7 or 8, wherein the resin of the resin particles contained in the third layer is selected from polyurethane resins, polyacrylic resins, and composite resins of polyurethane resins and polyacrylic resins.

[0018] 10. An image recording material described in any one of items 7 to 9, characterized in that the second layer further contains resin microparticles, and the resin of the resin microparticles is selected from a polyurethane-based resin, a polyacrylic-based resin, or a composite resin of a polyurethane-based resin and a polyacrylic-based resin. Effect of the Invention

[0019] According to the above-mentioned means of the present invention, it is possible to provide an inkjet recording method having improved hot water resistance in a two-liquid inkjet recording method for forming an image on a precoat coating film, and an image recorded using the same.

[0020] The mechanism by which the effects of the present invention are expressed or the mechanism of action is presumed to be as follows.

[0021] The inkjet recording method of the present invention includes a step of applying an aqueous precoat composition onto a substrate, or a step of applying and drying the aqueous precoat composition, and then applying and drying the aqueous ink composition, in this order. The aqueous precoat composition contains at least a coagulant, and the aqueous ink composition contains at least a pigment, a polymer dispersant, A neutralizer for the polymer dispersant and resin fine particles, the aggregating agent being selected from a thermally decomposable cationic resin, an organic acid, or a polyvalent metal salt, a neutralizing agent for the polymer dispersant being selected from an organic amine, and the method further comprises a step of drying the aqueous ink composition at a temperature equal to or higher than the thermal decomposition temperature of the aggregating agent.

[0022] That is, in the present invention, an organic amine is selected as a neutralizing agent for the pigment dispersant, and the hot water resistance of the pigment dispersant is improved by utilizing amine elimination by heating, and further, the hot water resistance of the image recording material is improved by thermally decomposing the pigment aggregating agent, which is a cause of deterioration of the hot water resistance, during drying. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a schematic diagram showing an example of a precoat / inkjet recording device preferred in the present invention. [Diagram 2] FIG. 1 is a cross-sectional view showing a schematic configuration of an image recording material of the present invention. [Diagram 3] Cross-section of packaging material for canned food DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The inkjet recording method of the present invention is an inkjet recording method having a step of applying an aqueous precoat composition onto a substrate, or a step of applying and drying the aqueous precoat composition, and then a step of applying and drying the aqueous ink composition, in this order, wherein the aqueous precoat composition contains at least a coagulant, and the aqueous ink composition contains at least a pigment, a polymer dispersant, A neutralizer for the polymer dispersant and resin fine particles, the aggregating agent being selected from a thermally decomposable cationic resin, an organic acid, or a polyvalent metal salt, a neutralizing agent for the polymer dispersant being selected from an organic amine, and a step of drying the aqueous ink composition at a temperature equal to or higher than the thermal decomposition temperature of the aggregating agent is included. This feature is a technical feature common to or corresponding to the following embodiments.

[0025] As an embodiment of the present invention, from the viewpoint of realizing the effects of the present invention, it is preferable that the step of applying the aqueous precoat composition is a step using an inkjet method, since this eliminates the need to apply a coagulant to areas where the ink is not applied, and therefore from the viewpoint of improving the overall hot water resistance.

[0026] From the viewpoint of balancing image quality and hot water resistance, it is preferable that the content of the coagulant is 5% by mass or less based on the aqueous precoat composition. The content of the coagulant is preferably in the range of 0.1 to 3% by mass.

[0027] The temperature for drying the water-based ink is preferably 220°C or lower from the viewpoint of suppressing thermal decomposition, because if the ink drying temperature is too high, thermal decomposition of the resin in the ink begins and the hot water resistance deteriorates.

[0028] The resin of the resin fine particles of the aqueous ink composition is preferably selected from polyurethane resins, polyacrylic resins, and composite resins of polyurethane resins and polyacrylic resins, from the viewpoint of improving the hot water resistance of the ink image on the substrate.

[0029] It is preferable that the aqueous precoat composition further contains resin fine particles, and it is more preferable that the resin of the resin fine particles is selected from polyester resin, polyurethane resin, polyacrylic resin, or composite resin of polyurethane resin and polyacrylic resin, from the viewpoint of improving the hot water resistance of the ink image on the substrate. The selection of the resin particles is also influenced by the acid value of the resin, and a lower acid value is better, but polyurethane resin or polyacrylic resin has higher hot water resistance and is preferable compared to polyester resin, which is prone to hydrolysis of the resin itself.

[0030] The image recording material of the present invention is an image recording material having at least four layers laminated on a metal substrate, the first layer and the fourth layer containing a thermosetting resin, and the second layer containing at least a coagulant. Thermal decomposition product of The flocculant is selected from a thermally decomposable cationic resin, an organic acid, or a polyvalent metal salt, and the third layer contains at least a pigment, a polymer dispersant, A neutralizer for the polymer dispersant and resin fine particles, and a neutralizer for the polymer dispersant is selected from organic amines. R It is characterized by:

[0031] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values ​​before and after the symbol "to" are included as the lower limit and upper limit.

[0032] <Outline of the inkjet recording method of the present invention> The inkjet recording method of the present invention (hereinafter also referred to as the inkjet method) is an inkjet recording method having a step of applying an aqueous precoat composition onto a substrate or a step of applying and drying the aqueous precoat composition, and then a step of applying and drying the aqueous ink composition, in this order, wherein the aqueous precoat composition contains at least a flocculant, and the aqueous ink composition contains at least a pigment, a polymer dispersant, A neutralizer for the polymer dispersant and resin fine particles, the aggregating agent being selected from a thermally decomposable cationic resin, an organic acid, or a polyvalent metal salt, a neutralizing agent for the polymer dispersant being selected from an organic amine, and the method further comprises a step of drying the aqueous ink composition at a temperature equal to or higher than the thermal decomposition temperature of the aggregating agent.

[0033] In the inkjet recording method of the present invention, the aqueous ink composition may be applied continuously after the aqueous precoat composition is applied without drying, in which case the aqueous precoat composition and the aqueous ink composition are dried together.

[0034] The inkjet recording method of the present invention is not particularly limited in its application, but it is possible to record a high-quality image on a non-absorbent substrate by forming a precoat layer on the non-absorbent substrate using the aqueous precoat composition of the present invention and recording an ink image thereon using the aqueous ink composition. In particular, since the inkjet recording method has excellent hot water resistance, it is possible to provide an image recording material suitable for packaging materials for canned foods and retort foods.

[0035] In the present invention, the term "aqueous precoat composition and aqueous ink composition" refers to a "precoat composition and ink composition" that use at least "water" as a solvent. In both cases, 60% by mass or more of the solvent used is "water".

[0036] "Pyrolysis" refers to the chemical decomposition of organic compounds by heating them in the absence of oxygen, halogens, etc.

[0037] The "thermal decomposition temperature of the flocculant" according to the present invention can be measured by a thermogravimetric differential thermal analyzer (TG-DTA), and the "thermal decomposition temperature" means the temperature at which mass loss due to thermal decomposition begins when the temperature is raised from room temperature (heating speed: 10°C / min). Here, the temperature at which mass loss begins is the temperature at the intersection of the tangent at the time when the mass is most greatly reduced and the tangent before mass loss, when a graph is drawn with the mass loss rate plotted on the vertical axis and the temperature on the horizontal axis. Specifically, the decomposition temperature of each flocculant is measured according to the above definition using STA7200 manufactured by Hitachi High-Tech Science Corporation.

[0038] [1] Base material The substrate that can be used in the present invention is not particularly limited, but is preferably a non-absorbent substrate. In the present invention, the term "non-absorbent" refers to non-absorbency to water.

[0039] Examples of non-water-absorbent substrates include known plastic films. Specific examples include polyester films such as polyethylene terephthalate, polyethylene films, polypropylene films, polyamide films such as nylon, polystyrene films, polyvinyl chloride films, polycarbonate films, polyacrylonitrile films, polylactic acid films, and other biodegradable films. In addition, in order to impart gas barrier properties, moisture resistance, and aroma retention, films coated with polyvinylidene chloride on one or both sides of the film, and films vapor-deposited with metal oxides can also be preferably used. Non-water-absorbent films can be used preferably in the form of unstretched or stretched films. In the case of plastic films, the thickness of the substrate is preferably in the range of 10 to 120 μm, more preferably in the range of 12 to 60 μm.

[0040] In addition, metal substrates such as tinplate for three-piece cans and tin-free steel plates (TFS plates, thickness 0.1 to 0.6 μm) are also preferably used as non-absorbent substrates, and can be suitably used as packaging materials for canned foods, for example, with a coating layer of a thermosetting resin. In the packaging materials for canned foods, for example, epoxy-phenol-based paints or polyester-based laminating agents are generally used on the food side to block air, moisture, and light and seal the food inside, and polyester-based or acrylic-based thermosetting paints are generally used on the outside.

[0041] [2] Aqueous precoat composition When an image is recorded on a substrate by inkjet printing, the aqueous precoat composition according to the present invention (hereinafter also referred to as "precoat liquid") can be used to accelerate ink image formation, improve the physical properties of the precoat layer and ink layer, and impart functions of improving image quality. Specifically, in the present invention, the precoat layer according to the present invention is applied in advance to the substrate on the surface to be inkjet printed and dried, and then the aqueous ink composition according to the present invention (hereinafter also referred to as "inkjet ink", "ink liquid", or simply "ink") is printed, thereby enabling recording with excellent image quality, water resistance, and hot water resistance, and excellent adhesion between the non-absorbent substrate and the precoat layer, even if the substrate is non-absorbent.

[0042] The aqueous precoat composition according to the present invention is characterized by containing at least a flocculant and water as a solvent, and preferably further contains resin fine particles from the viewpoint of hot water resistance.

[0043] (Flocculant) The precoat liquid according to the present invention contains a material that generates aggregates when it comes into contact with an inkjet ink containing a pigment, i.e., an aggregating agent, which enhances the interaction with the inkjet ink and enables dots of the aqueous ink composition to be more firmly fixed.

[0044] The flocculant preferably contains any one of a thermally decomposable cationic resin, an organic acid, or a polyvalent metal salt, and more preferably contains an organic acid or a polyvalent metal salt. As described above, the "thermal decomposition temperature of the flocculant" can be measured by a thermogravimetric differential thermal analyzer (TG-DTA), and the "thermal decomposition temperature" means the temperature at which mass loss due to thermal decomposition begins when the temperature is raised from room temperature (heating speed: 10°C / min). Here, the temperature at which mass loss begins is the temperature at the intersection of the tangent when the mass is most greatly reduced and the tangent before mass loss, when a graph is drawn with the mass loss rate plotted on the vertical axis and the temperature on the horizontal axis. Specifically, the decomposition temperature of each flocculant is measured according to the above definition using STA7200 manufactured by Hitachi High-Tech Science Corporation.

[0045] The cationic resin and polyvalent metal salt can aggregate anionic components (usually coloring materials, pigments, etc.) in the inkjet ink by salting out, and the organic acid can aggregate anionic components in the inkjet ink by changing the pH.

[0046] Examples of the cationic resin include polyallylamine, polyvinylamine, polyethyleneimine, polydiallyldimethylammonium chloride, etc. Examples of commercially available cationic resins include KHE100L and FPA100L manufactured by Senka Corporation, and PAS-92A, PAS-M-1A, and PAS-21CL manufactured by Nittobo Medical Co., Ltd.

[0047] The organic acid is capable of aggregating the pigment contained in the inkjet ink, and preferably has a first dissociation constant of 3.5 or less, preferably in the range of 1.5 to 3.5. When in this range, liquid shifting in low-density areas where the printing rate is low is further prevented, and beading in high-density areas where the printing rate is high is further improved.

[0048] It is preferable to use an organic acid that is not completely neutralized by a base. Neutralization by a base means that the acidic group of these acids is ionic-bonded with other positively charged elements or compounds (e.g., inorganic compounds such as metals). Also, not completely neutralized means that among the acidic groups of the organic acid, there are acidic groups that do not form the above-mentioned ionic bonds. By using an organic acid having an acidic group that does not form an ionic bond, compatibility with the composite resin particles having a polyurethane structure contained in the precoat liquid is high, and a transparent precoat layer can be formed, so that the color tone of the formed image is considered to be brighter than when a polyvalent metal salt or the like is used. In addition, by using an organic acid, the storage stability of the precoat liquid is easily maintained, and blocking is less likely to occur after the precoat liquid is applied and dried. From the above viewpoint, preferred organic acids include formic acid, acetic acid, propionic acid, isobutyric acid, oxalic acid, fumaric acid, malic acid, citric acid, malonic acid, succinic acid, maleic acid, benzoic acid, 2-pyrrolidone-5-carboxylic acid, lactic acid, acrylic acid and derivatives thereof, methacrylic acid and derivatives thereof, compounds having a carboxy group including acrylamide and derivatives thereof, sulfonic acid derivatives, and phosphoric acid and derivatives thereof.

[0049] The content of the organic acid in the precoat liquid may be an amount that adjusts the pH of the precoat liquid to less than the first dissociation constant of the organic acid. By adding an organic acid to the precoat liquid in an amount that adjusts the pH of the precoat liquid to less than the first dissociation constant of the organic acid, bleeding during high-speed printing can be effectively suppressed.

[0050] Examples of the polyvalent metal salt include water-soluble salts such as calcium salts, magnesium salts, aluminum salts and zinc salts.

[0051] The coagulant is preferably contained in the precoat liquid in an amount of 5% by mass or less, and is preferably contained in an amount of 0.1 to 3% by mass from the viewpoints of effectively coagulating the anionic components in the inkjet ink and of achieving a balance between image quality and hot water resistance.

[0052] The content of the flocculant in the aqueous solution can be measured by a known method. For example, when the flocculant is a polyvalent metal salt, the content can be measured by ICP emission spectrometry, and when the flocculant is an acid, the content can be measured by high performance liquid chromatography (HPLC).

[0053] When an organic acid is used, the amount of the organic acid applied is preferably an amount that adjusts the pH of the precoat liquid to be equal to or less than the neutralization equivalent of the anionic component contained in the inkjet ink. When the anionic component is a compound having a carboxy group, the first dissociation constant of the organic acid is preferably 3.5 or less, from the viewpoint of preventing image bleeding.

[0054] The amount of the precoat liquid of the present invention to be applied is not particularly limited and can be appropriately adjusted. For example, when the coagulant is a polyvalent metal salt, the amount of the polyvalent metal salt to be applied is 0.1 to 20 g / m 2 In addition, when the aggregating agent is an organic acid, the amount of the organic acid added is preferably equal to or less than the neutralization equivalent of an anion component in the aqueous ink composition.

[0055] (Resin fine particles) The aqueous precoat composition according to the present invention preferably further contains resin fine particles. The resin fine particles are preferably water-insoluble resin fine particles, and the water-insoluble resin fine particles used in the present invention are water-insoluble resin fine particles that can receive ink and have solubility or affinity for the ink.

[0056] Water-insoluble resin microparticles are essentially water-insoluble, but have a form in which the resin disperses in an aqueous medium as microscopic microparticles, and are water-insoluble resins that are forcibly emulsified and dispersed in water using an emulsifier or the like, or water-insoluble resins that are self-emulsifiable to form a stable aqueous dispersion by themselves without using an emulsifier or dispersion stabilizer by introducing a hydrophilic functional group into the molecule. These resins are usually used in a state of being emulsified and dispersed in water or a water / alcohol mixed solvent.

[0057] In the present invention, "water-insoluble" refers to a resin that, when dried at 105° C. for 2 hours and then dissolved in 100 g of water at 25° C., dissolution amount is 10 g or less, preferably 5 g or less, and more preferably 1 g or less. However, when the resin has a salt-forming group, the dissolution amount is the dissolution amount when the salt-forming group of the resin is 100% neutralized with acetic acid or sodium hydroxide depending on the type of the resin.

[0058] The resin fine particles used in the aqueous precoat composition preferably have cationic or nonionic ionic properties.

[0059] The water-insoluble resin microparticles according to the present invention are preferably at least polyester resin, polyurethane resin, polyacrylic resin, or composite resin microparticles of polyurethane resin and polyacrylic resin, and more preferably polyurethane resin, polyacrylic resin, or composite resin microparticles of polyurethane resin and polyacrylic resin.

[0060] The water-insoluble resin fine particles are preferably contained in the precoat liquid in an amount of 1 to 30 mass % relative to the total mass (100 mass %) of the precoat liquid, and more preferably contained in an amount of 2 to 20 mass % from the viewpoints of storage stability of the precoat liquid and suppression of blooming (a phenomenon in which a resin or a flocculant precipitates or crystallizes on the image surface).

[0061] (Polyester resin) The polyester-based resin having a polyester skeleton as the water-insoluble resin fine particles can be obtained by using a polyhydric alcohol component and a polycarboxylic acid component such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester.

[0062] The polyhydric alcohol component is, specifically, a dihydric alcohol (diol), specifically, an alkylene glycol having 2 to 36 carbon atoms (ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, etc.), an alkylene ether glycol having 4 to 36 carbon atoms (diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol, etc.), an alicyclic diol having 6 to 36 carbon atoms, Examples of the alkylene oxide include alicyclic diols (1,4-cyclohexanedimethanol, hydrogenated bisphenol A, etc.), adducts of the above-mentioned alicyclic diols with alkylene oxides having 2 to 4 carbon atoms (ethylene oxide (hereinafter abbreviated as EO), propylene oxide (hereinafter abbreviated as PO), butylene oxide (hereinafter abbreviated as BO)) (number of moles added is in the range of 1 to 30), and adducts of bisphenols (bisphenol A, bisphenol F, bisphenol S, etc.) with alkylene oxides having 2 to 4 carbon atoms (EO, PO, BO, etc.) (number of moles added is in the range of 2 to 30). These may be used alone or in combination of two or more.

[0063] Examples of the polyvalent carboxylic acid component include divalent carboxylic acids (dicarboxylic acids), specifically alkane dicarboxylic acids having 4 to 36 carbon atoms (succinic acid, apidic acid, sebacic acid, etc.), alkenyl succinic acids (dodecenyl succinic acid, etc.), alicyclic dicarboxylic acids having 4 to 36 carbon atoms (dimer acids (dimerized linoleic acid), etc.), alkene dicarboxylic acids having 4 to 36 carbon atoms (maleic acid, fumaric acid, citraconic acid, mesaconic acid, etc.), and aromatic dicarboxylic acids having 8 to 36 carbon atoms (phthalic acid, isophthalic acid, terephthalic acid or derivatives thereof, naphthalenedicarboxylic acid, etc.). These may be used alone or in combination of two or more.

[0064] The number average molecular weight (Mn) of the polyester resin is preferably in the range of 1,000 to 50,000, and more preferably in the range of 2,000 to 20,000.

[0065] As the polyester resin, a commercially available product may be used, and examples of the commercially available product include PESRESIN A-110F, A-640, and A-647GEX manufactured by Takamatsu Oil Co., Ltd., Vylonal MD-1100, MD-1200, MD-1335, MD-1480, MD-1930, and MD-2000 manufactured by Toyobo Co., Ltd., and Z-1100 manufactured by GOO Chemical Co., Ltd. These may be used alone or in combination of two or more types.

[0066] (Polyurethane resin) As the polyurethane-based resin for the water-insoluble resin particles, those having a hydrophilic group can be used.

[0067] The polyurethane resin is preferably an aqueous dispersion of a self-emulsifying polyurethane having a water-soluble functional group in its molecule, or an aqueous dispersion of a forced-emulsifying polyurethane emulsified under strong mechanical shearing force in combination with a surfactant. The polyurethane resin in the aqueous dispersion can be obtained by reacting a polyol with an organic polyisocyanate and a hydrophilic group-containing compound.

[0068] Examples of polyols that can be used in preparing the aqueous dispersion of the polyurethane resin include polyester polyols, polyether polyols, polycarbonate polyols, and polyolefin polyols.

[0069] Examples of polyester polyols include low molecular weight polyols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2- and 1,3-propylene glycol, neopentyl glycol, 1,3- and 1,4-butanediol, 3-methylpentanediol, hexamethylene glycol, 1,8-octanediol, 2-methyl-1,3-propanediol, bisphenol A, hydrogenated bisphenol A, trimethylolpropane, and cyclohexanedimethanol; and condensates with polyvalent carboxylic acids such as succinic acid, glutaric acid, adipic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, tetrahydrofuran acid, endomethinetetrahydrofuran acid, and hexahydrophthalic acid.

[0070] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polyethylene polytetramethylene glycol, polypropylene polytetramethylene glycol, and polytetramethylene glycol.

[0071] Examples of polycarbonate polyols include those obtained by reacting carbonic acid derivatives such as diphenyl carbonate, dimethyl carbonate, or phosgene with diols. Examples of the diols include ethylene glycol, diethylene glycol, triethylene glycol, 1,2- and 1,3-propylene glycol, neopentyl glycol, 1,3- and 1,4-butanediol, 3-methylpentanediol, hexamethylene glycol, 1,8-octanediol, 2-methyl-1,3-propanediol, bisphenol A, hydrogenated bisphenol A, trimethylolpropane, and cyclohexanedimethanol.

[0072] Examples of organic polyisocyanates that can be used to prepare aqueous dispersions of polyurethane resins include aromatic isocyanates such as tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), polymeric MDI, xylylene diisocyanate (XDI), and tetramethylxylylene diisocyanate (TMXDI); aliphatic isocyanates such as hexamethylene diisocyanate (HMDI); and alicyclic isocyanates such as isophorone diisocyanate (IPDI) and 4,4'-dicyclohexylmethane diisocyanate (hydrogenated MDI, H12MDI). These may be used alone or in combination of two or more.

[0073] Examples of hydrophilic group-containing compounds that can be used in preparing an aqueous dispersion of a polyurethane resin include carboxylic acid-containing compounds such as 2,2-dimethylolpropionic acid, 2,2-dimethylolbutanoic acid, 2,2-dimethylolbutyric acid, 2,2-dimethylolvaleric acid, and glycine, and derivatives thereof such as sodium salts, potassium salts, and amine salts; and sulfonic acid-containing compounds such as taurine (i.e., aminoethylsulfonic acid) and ethoxypolyethylene glycol sulfonic acid, and derivatives thereof such as sodium salts, potassium salts, and amine salts.

[0074] The polyurethane resin can be obtained by a known method. For example, the above-mentioned polyol, organic polyisocyanate, and hydrophilic group-containing compound are mixed and reacted at a temperature of 30 to 130° C. for 30 minutes to 50 hours to obtain a urethane prepolymer.

[0075] The urethane prepolymer is polymerized by extending the chain with a chain extender to become a polyurethane resin having a hydrophilic group. The chain extender is preferably water and / or an amine compound. By using water or an amine compound as the chain extender, the chain extender reacts with free isocyanate in a short time, and the isocyanate-terminated prepolymer can be efficiently extended.

[0076] Examples of the amine compound as a chain extender include aliphatic polyamines such as ethylenediamine and triethylenediamine, aromatic polyamines such as metaxylenediamine and toluylenediamine, polyhydrazino compounds such as hydrazine and adipic acid dihydrazide, etc. The amine compound may contain, together with the polyamine, a monovalent amine such as dibutylamine, methyl ethyl ketoxime, etc. as a reaction terminator to the extent that the polymerization is not significantly inhibited.

[0077] In addition, in the synthesis of the urethane prepolymer, a solvent that is inactive with isocyanate and can dissolve the urethane prepolymer may be used. Examples of such solvents include dioxane, methyl ethyl ketone, dimethylformamide, tetrahydrofuran, N-methyl-2-pyrrolidone, toluene, and propylene glycol monomethyl ether acetate. These hydrophilic organic solvents used in the reaction step are preferably finally removed.

[0078] In addition, in the synthesis of the urethane prepolymer, a catalyst such as an amine catalyst (e.g., triethylamine, N-ethylmorpholine, triethyldiamine, etc.), a tin-based catalyst (e.g., dibutyltin dilaurate, dioctyltin dilaurate, tin octoate, etc.), or a titanium-based catalyst (e.g., tetrabutyl titanate, etc.) may be added to promote the reaction.

[0079] The number average molecular weight (Mn) of the urethane resin is preferably as large as possible by introducing a branched structure or an internal crosslinked structure, and the number average molecular weight is preferably in the range of 50,000 to 10,000,000. By setting the molecular weight within the above range, the urethane resin becomes less soluble in a solvent, so that a coating film with excellent weather resistance and water resistance can be obtained. The number average molecular weight (Mn) is a value measured by gel permeation chromatography (GPC), and can be determined from a calibration curve prepared with a polystyrene standard sample using, for example, Shimadzu Corporation's "RID-6A" (column: Tosoh Corporation's "TSK-GEL", solvent: tetrahydrofuran (THF), column temperature: 40°C).

[0080] The urethane resin may be a commercially available product. Examples of commercially available urethane resins include WBR-016U (manufactured by Taisei Fine Chemical Co., Ltd.), Superflex 620, Superflex 650, Superflex 500M, Superflex E-2000 (all manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Superflex" is a registered trademark of the company), Permarine UC-20 (manufactured by Sanyo Chemical Industries, Ltd., "Permarine" is a registered trademark of the company), and Parasurf UP-22 (manufactured by Ohara Palladium Chemical Co., Ltd.).

[0081] (Polyacrylic resin) The polyacrylic resin as the water-insoluble resin particles can be obtained by using a copolymer with an acrylic acid ester component, a methacrylic acid ester component, or a styrene component.

[0082] Examples of the acrylic acid ester component and the methacrylic acid ester component include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, blue (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, 4-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, 4-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-hydroxyethyl ... -hydroxybutyl, benzyl (meth)acrylate, glycidyl (meth)acrylate, (meth)acrylic acid, (di)ethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerin di(meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and acrylamide.

[0083] Examples of the styrene component include styrene, 4-methylstyrene, 4-hydroxystyrene, 4-acetoxystyrene, 4-acetylstyrene, and styrenesulfonic acid, etc. These components may be used alone or in combination of two or more kinds.

[0084] The number average molecular weight (Mn) of the polyacrylic resin is preferably in the range of 1000 to 50000, and more preferably in the range of 2000 to 20000. When the number average molecular weight (Mn) of the polyacrylic resin is 1000 or more, the cohesive force of the coating film is strong and the adhesion is improved, whereas when it is 50000 or less, the solubility in organic solvents is good, and miniaturization of the particle size of the emulsion dispersion is promoted.

[0085] The polyacrylic resin may be a commercially available product. Examples of commercially available polyacrylic resins include RKW-620, UW-319SX, UW-600, and UW-550CS manufactured by Taisei Fine Chemical Co., Ltd., and acrylic emulsions such as 2682, 2680, 2684, 2685, and 2687 manufactured by Nissin Chemical Industry Co., Ltd.

[0086] (Composite resin fine particles) The composite resin particles that can be contained in the precoat liquid are preferably composite resin particles in which a polyacrylic resin is emulsified in a polyurethane resin, i.e., the composite resin particles have an inner layer made of a polyacrylic resin and a surface layer made of a polyurethane resin.

[0087] Here, the polyurethane resin is present at the interface between the polyacrylic resin as the water-insoluble resin particles and the water as the continuous phase, and functions as a water-insoluble resin particle layer different from the resin that protects the water-insoluble resin particles.

[0088] By emulsifying the polyacrylic resin with the polyurethane resin to form composite resin particles, unlike the use of the polyacrylic resin alone, it is possible to suppress the decrease in compatibility with the polyurethane resin and the pigment flocculant. Also, compared to the case where the polyacrylic resin and the polyurethane resin are emulsified and mixed, it is possible to improve the physical properties of the image (coating film) and the stability of the precoat liquid.

[0089] In the composite resin microparticles obtained by emulsifying the polyacrylic resin in the polyurethane resin, the mass ratio (U / A) of the polyurethane resin (U) to the polyacrylic resin (A) is preferably in the range of 40 / 60 to 95 / 5. When the content of the polyurethane resin (U) is within the above range, compatibility with the dispersant is improved, and solvent resistance is also improved. Furthermore, when the content of the polyacrylic resin (A) is within the above range, adhesion to acrylic films is excellent. In the above content ratios, the mass ratio (U / A) of the polyurethane resin (U) to the polyacrylic resin (A) is preferably in the range of 40 / 60 to 80 / 20.

[0090] The total resin concentration of the polyacrylic resin and the polyurethane resin in the composite resin particles is not particularly limited, but is preferably 5.0% by mass or more, and more preferably in the range of 10.0 to 70.0% by mass. When the resin concentration is within the above range, the fixation of the ink to the substrate is good.

[0091] In addition, in emulsifying the polyacrylic resin with the polyurethane resin, a surfactant acting as an emulsifier can be used together with the polyurethane resin. By adding the emulsifier, the storage stability of the composite resin particles can be improved.

[0092] As the emulsifier, an anionic surfactant and a nonionic surfactant can be used. In the present invention, it is preferable to use either one of the anionic surfactant and the nonionic surfactant, and it is more preferable to use both. Here, the total amount of the anionic surfactant and the nonionic surfactant is preferably in the range of 1.0 to 20.0 parts by mass with respect to 100 parts by mass of the total resin. In addition, by making the total amount of the anionic surfactant and the nonionic surfactant 20.0 parts by mass or less, it is possible to improve water resistance and solvent resistance.

[0093] The blending mass ratio (X / Y) of the anionic surfactant (X) to the nonionic surfactant (Y) is preferably in the range of 100 / 0 to 50 / 50. By setting the blending amount of the anionic surfactant in the above range, emulsifiability and storage stability can be further improved.

[0094] Examples of anionic surfactants that can be used for emulsification include alkyl sulfates, polyoxyethylene alkyl ether sulfates, sulfosuccinates, alpha-olefin sulfonates, N-acylamino acid salts, carboxylates, and phosphates, etc. Among these, sulfosuccinates and alpha-olefin sulfonates are preferred.

[0095] Examples of the types of salts include, but are not limited to, metal salts such as sodium salts, potassium salts, and magnesium salts, and triethanolamine salts.

[0096] Examples of nonionic surfactants that can be used for emulsification include polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene alkylamine ethers, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, etc. Among these, polyoxyethylene alkyl ethers and polyoxyethylene alkyl phenyl ethers are preferred.

[0097] The average particle size of the composite resin microparticles is not particularly limited, but is preferably 10 to 500 nm, more preferably 10 to 300 nm, and even more preferably 10 to 200 nm. The average particle size can be measured by a commercially available particle size measuring device using a dynamic light scattering method, an electrophoresis method, or the like, but the measurement by the dynamic light scattering method is simple and can measure the particle size range with high accuracy.

[0098] By using composite resin particles in which a polyacrylic resin is emulsified in a polyurethane resin, the fixation of an image (coating film) to a low-absorbent substrate or a non-absorbent substrate can be improved.

[0099] The above-mentioned composite resin particles are preferably those obtained by the following production method (I) or (II) of composite resin particles using a polyacrylic resin and a polyurethane resin.

[0100] The precoat liquid according to the present invention may further contain antioxidants, light stabilizers, plasticizers, foaming agents, thickeners, colorants, flame retardants, other water-insoluble resin particles, and various fillers.

[0101] Furthermore, various crosslinking agents such as epoxy-based, carbodiimide-based, oxazolidine-based, blocked isocyanate-based, and isocyanate-based crosslinking agents may be added to the precoat liquid according to the present invention in order to impart higher durability.

[0102] (Method of producing composite resin microparticles) The method for producing the composite resin microparticles according to the present invention will be described below.

[0103] The above-mentioned composite resin fine particles can be prepared by the production method (I) or (II) described below.

[0104] <Manufacturing method (I)> The production method (I) is a method in which a polyacrylic resin is emulsified in water with a urethane prepolymer having a hydrophilic group, and an amine compound or an aqueous solution thereof is added as a chain extender to extend the chain of the urethane prepolymer (to increase the molecular weight).

[0105] In the production method (I), first, a resin solution obtained by dissolving a polyacrylic resin in a solvent is mixed with a solution of a urethane prepolymer having a hydrophilic group, and water is added to the mixture and emulsified by stirring to obtain an emulsion.

[0106] Examples of the solvent include organic solvents such as hexane, isohexane, pentane, cyclohexane, methylcyclohexane, heptane, isooctane, methyl ethyl ketone, xylene, toluene, benzene, etc., and solvents other than water such as carbon dioxide in a supercritical state. Of these solvents, only one type may be used, or two or more types may be used in combination.

[0107] As the emulsification method, known methods such as forced emulsification, phase inversion emulsification, D-phase emulsification, and gel emulsification can be used. As the equipment that can be used in this method, for example, single stirring using a stirring blade, a disperser, a homogenizer, etc., and combined stirring using these, a sand mill, a multi-screw extruder, etc. In addition, in the emulsification, the above-mentioned surfactant may be mixed together with the urethane prepolymer.

[0108] Next, the emulsion is diluted with water, and then an amine compound is added as a chain extender to crosslink the remaining isocyanate groups of the urethane prepolymer with the chain extender, thereby increasing the molecular weight of the polyacrylic resin. The organic solvent is then distilled off to obtain a composite resin particle dispersion (a dispersion in which water-insoluble resin particles are dispersed) containing the polyacrylic resin inside the polyurethane resin.

[0109] <Manufacturing method (II)> The production method (II) is described below. The production method (II) is a method in which a urethane prepolymer having a hydrophilic group is emulsified in water, an amine compound or an aqueous solution thereof is added as a chain extender to extend the chain of the urethane prepolymer, thereby preparing an aqueous dispersion of a polyurethane resin, and a polyacrylic resin is emulsified in the aqueous dispersion of the polyurethane resin.

[0110] In production method (II), water is added to a solution of a urethane prepolymer having hydrophilic groups to emulsify it, and an amine compound is added as a chain extender to the resulting emulsion to crosslink the remaining isocyanate groups of the urethane prepolymer with the chain extender, thereby preparing an aqueous dispersion of a highly molecular weight polyurethane resin.

[0111] Then, the resin solution obtained by dissolving the polyacrylic resin in a solvent is mixed with the aqueous dispersion of the above-mentioned polyurethane resin having hydrophilic groups to emulsify the polyacrylic resin with the polyurethane resin having hydrophilic groups. After diluting with water, the organic solvent can be distilled off to obtain a composite resin microparticle dispersion (a dispersion in which water-insoluble resin microparticles are dispersed) containing the polyacrylic resin inside the polyurethane resin.

[0112] In the production method (II), the solvent that can be used can be the same as that in the production method (I). Also, the emulsification method can be the same as that in the production method (I).

[0113] The average particle size of the composite resin microparticles is not particularly limited, but is preferably in the range of 10 to 500 nm, more preferably in the range of 10 to 300 nm, and even more preferably in the range of 10 to 200 nm. The average particle size can be measured by a commercially available particle size measuring device using a dynamic light scattering method, an electrophoresis method, or the like. Among the above measuring methods, the dynamic light scattering method is preferred because it is easy to measure and can accurately measure the particle size range.

[0114] These resins may be copolymers using other monomers.

[0115] The weight-average molecular weight of the composite resin microparticles is preferably in the range of 10,000 to 1,000,000. When the weight-average molecular weight (Mw) of the water-insoluble resin microparticles is 10,000 or more, the cohesive force of the image (coating film) formed on the surface of a low-absorbent substrate or a non-absorbent substrate is increased, and the adhesion of the coating film is improved. When the weight-average molecular weight (Mw) is 1,000,000 or less, the solubility in organic solvents is good, and the particle size of the emulsion dispersion is promoted to be reduced. The weight-average molecular weight (Mw) is a value measured by gel permeation chromatography (GPC), and can be determined from a calibration curve prepared with a polystyrene standard sample using, for example, Shimadzu Corporation's "RID-6A" (column: Tosoh Corporation's "TSK-GEL", solvent: tetrahydrofuran (THF), column temperature: 40°C).

[0116] Although the method for producing the composite resin fine particles has been described as the water-insoluble resin fine particles, the present invention is not limited thereto, and commercially available composite resins may be used. For example, commercially available urethane-acrylic resins include WEM-506C manufactured by Taisei Fine Chemical Co., Ltd. and Mowinyl 6910 manufactured by Japan Coating Resins Co., Ltd.

[0117] (Water, other additives) The water contained in the precoat liquid according to the present invention is not particularly limited, and may be ion-exchanged water, distilled water, or pure water.

[0118] The precoat liquid according to the present invention may contain an organic solvent in addition to water as a solvent, which can be removed when the precoat liquid is dried in the subsequent step.

[0119] The precoat liquid may contain other components, such as surfactants, crosslinking agents, antifungal agents, and bactericides, as appropriate, within the scope of not impairing the effects of the present invention.

[0120] Further, for example, ultraviolet absorbents described in JP-A-57-74193, JP-A-57-87988 and JP-A-62-261476, discoloration inhibitors described in JP-A-57-74192, JP-A-57-87989, JP-A-60-72785, JP-A-61-146591, JP-A-1-95091 and JP-A-3-13376, anions, It is also possible to contain various known additives such as various cationic or nonionic surfactants, fluorescent brightening agents described in JP-A-59-42993, JP-A-59-52689, JP-A-62-280069, JP-A-61-242871, and JP-A-4-219266, antifoaming agents, lubricants such as diethylene glycol, preservatives, thickeners, antistatic agents, etc.

[0121] It is preferable to prepare a precoat layer by directly applying the precoat liquid according to the present invention as a coating liquid onto a substrate and drying it. The additives preferably used in the precoat liquid are preferably thoroughly dispersed before use as a coating liquid.

[0122] The precoat liquid is preferably applied by roll coating, rod bar coating, air knife coating, spray coating, curtain coating, extrusion coating using a hopper as described in U.S. Pat. No. 2,681,294, or ink jet coating.

[0123] [3] Water-based ink composition The aqueous ink composition according to the present invention (hereinafter referred to as "ink liquid" or simply "ink") is characterized by containing at least a pigment, a polymeric dispersant for dispersing the pigment, and resin microparticles, and preferably further contains water.

[0124] (Pigments) The pigment contained in the ink according to the present invention may be an anionic dispersed pigment, such as an anionic self-dispersing pigment or a pigment dispersed with an anionic polymer dispersant, and in particular, a pigment dispersed with an anionic polymer dispersant is preferred.

[0125] As the pigment, any conventionally known pigment can be used without any particular limitation. For example, organic pigments such as insoluble pigments and lake pigments, and inorganic pigments such as titanium oxide can be preferably used.

[0126] In the case of titanium oxide, for which it is generally difficult to ensure both ink ejection stability and adhesion, the present invention is particularly advantageous in that it makes bleeding less likely to occur and also improves adhesion.

[0127] Titanium oxide has three crystal forms: anatase, rutile, and brookite, but the most commonly used are roughly classified into anatase and rutile. Although not particularly limited, rutile is preferred because it has a high refractive index and high hiding power. Specific examples include the TR series from Fuji Titanium Industry Co., Ltd., the JR series from Teika Corporation, and Typeque from Ishihara Sangyo Co., Ltd.

[0128] The insoluble pigment is not particularly limited, but examples thereof include azo, azomethine, methine, diphenylmethane, triphenylmethane, quinacridone, anthraquinone, perylene, indigo, quinophthalone, isoindolinone, isoindoline, azine, oxazine, thiazine, dioxazine, thiazole, phthalocyanine, and diketopyrrolopyrrole.

[0129] Specific examples of organic pigments that can be preferably used include the following pigments.

[0130] Examples of pigments for magenta or red include CI Pigment Red 2, CI Pigment Red 3, CI Pigment Red 5, CI Pigment Red 6, CI Pigment Red 7, CI Pigment Red 15, CI Pigment Red 16, CI Pigment Red 48:1, CI Pigment Red 53:1, CI Pigment Red 57:1, CI Pigment Red 122, CI Pigment Red 123, CI Pigment Red 139, CI Pigment Red 144, CI Pigment Red 149, CI Pigment Red 166, CI Pigment Red 177, CI Pigment Red 178, CI Pigment Red 202, CI Pigment Red 222, and CI Pigment Violet 19.

[0131] Examples of pigments for orange or yellow include CI Pigment Orange 31, CI Pigment Orange 43, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, CI Pigment Yellow 15, CI Pigment Yellow 15:3, CI Pigment Yellow 17, CI Pigment Yellow 74, CI Pigment Yellow 93, CI Pigment Yellow 128, CI Pigment Yellow 94, CI Pigment Yellow 138, and CI Pigment Yellow 155. In particular, CI Pigment Yellow 155 is preferred in terms of the balance between color tone and lightfastness.

[0132] Examples of pigments for green or cyan include CI Pigment Blue 15, CI Pigment Blue 15:2, CI Pigment Blue 15:3, CI Pigment Blue 16, CI Pigment Blue 60, CI Pigment Green 7, and the like.

[0133] Examples of black pigments include CI Pigment Black 1, CI Pigment Black 6, and CI Pigment Black 7.

[0134] (Pigment dispersant) The pigment dispersant used to disperse the pigment is not particularly limited, but is preferably a polymer dispersant having an anionic group, and one having a molecular weight in the range of 5,000 to 200,000 can be suitably used.

[0135] Examples of polymer dispersants include block copolymers and random copolymers having a structure derived from two or more monomers selected from styrene, styrene derivatives, vinylnaphthalene derivatives, acrylic acid, acrylic acid derivatives, maleic acid, maleic acid derivatives, itaconic acid, itaconic acid derivatives, fumaric acid, and fumaric acid derivatives, as well as salts thereof, polyoxyalkylenes, and polyoxyalkylene alkyl ethers.

[0136] The polymer dispersant preferably has an acryloyl group and is preferably neutralized with a neutralizing base before addition. The neutralizing base is not particularly limited, but is preferably an organic base such as ammonia, monoethanolamine, diethanolamine, triethanolamine, morpholine, etc. In particular, when the pigment is titanium oxide, the titanium oxide is preferably dispersed with a polymer dispersant having an acryloyl group.

[0137] The amount of the polymer dispersant added is preferably in the range of 10 to 100% by mass, and more preferably in the range of 10 to 40% by mass, based on the pigment.

[0138] It is particularly preferred that the pigment has a form of a so-called capsule pigment in which the pigment is coated with the polymer dispersant. As a method for coating the pigment with the polymer dispersant, various known methods can be used, and preferred examples thereof include a phase inversion emulsification method, an acid precipitation method, and a method in which the pigment is dispersed in a polymerizable surfactant, a monomer is supplied thereto, and the monomer is coated while being polymerized.

[0139] A particularly preferred method is to dissolve a water-insoluble resin in an organic solvent such as methyl ethyl ketone, partially or completely neutralize the acidic groups in the resin with a base, add a pigment and ion-exchanged water, disperse the pigment, remove the organic solvent, and add water as necessary to prepare the dispersion.

[0140] The average particle size of the pigment in the dispersed state in the ink is preferably 50 nm or more and less than 200 nm. This can improve the dispersion stability of the pigment and the storage stability of the ink. The particle size of the pigment can be measured by a commercially available particle size measuring device using a dynamic light scattering method, an electrophoresis method, or the like, but the measurement by the dynamic light scattering method is simple and can measure the particle size range with high accuracy.

[0141] The pigment can be dispersed in a dispersing machine together with a dispersant and other additives required for various desired purposes.

[0142] As the dispersing machine, a conventionally known ball mill, sand mill, line mill, high-pressure homogenizer, etc. can be used. Among them, dispersing the pigment with a sand mill is preferable because it results in a sharp particle size distribution. The material of the beads used for the sand mill dispersion is not particularly limited, but is preferably zirconia or zircon from the viewpoint of preventing the generation of bead fragments and contamination of ion components. Furthermore, the bead diameter is preferably in the range of 0.3 to 3 mm.

[0143] The content of the pigment in the ink is not particularly limited, but for titanium oxide, the range is preferably 7 to 18 mass %, and for organic pigments, the range is preferably 0.5 to 7 mass %.

[0144] (Resin fine particles) The resin fine particles in the aqueous ink composition according to the present invention are preferably water-insoluble resin fine particles. The water-insoluble resin fine particles used in the present invention are a water-insoluble resin fine particle dispersion that can receive ink and has solubility or affinity for the ink.

[0145] As mentioned above, the water-insoluble resin microparticles are essentially water-insoluble, but have a form in which the resin disperses in an aqueous medium as microscopic microparticles, and are water-insoluble resins that are forcibly emulsified and dispersed in water using emulsifiers, etc., or water-insoluble resins that are self-emulsifiable and form a stable aqueous dispersion by themselves without using emulsifiers or dispersion stabilizers by introducing hydrophilic functional groups into the molecule.These resins are usually used in a state of being emulsified and dispersed in water or a water / alcohol mixed solvent.

[0146] The resin used is preferably at least polyester resin, polyurethane resin, polyacrylic resin, or composite resin fine particles of polyurethane resin and polyacrylic resin.

[0147] With regard to the above-mentioned polyester-based resin, polyurethane-based resin, polyacrylic-based resin, or composite resin fine particles of polyurethane-based resin and polyacrylic-based resin, it is preferable to appropriately use those detailed in the above-mentioned precoat liquid section, but the resin fine particles used in the aqueous precoat composition are preferably cationic or nonionic in ionicity, whereas the resin fine particles used in the aqueous ink composition are preferably anionic.

[0148] In particular, it is preferable that the resin particles used in the aqueous ink composition contain an acid structure, which allows the particles to be dispersed in water even with a small amount of surfactant added, improving the water resistance of the ink layer. This is called a self-emulsifying type, and means that the urethane resin can be dispersed and stabilized in water only by molecular ionicity without using a surfactant. Examples of acid structures include a carboxyl group (-COOH), a sulfonic acid group (-SO 3 The acid structure may be present in a side chain or at the end of the resin.

[0149] It is preferable that the acid structure is partially or entirely neutralized. By neutralizing the acid structure, the water dispersibility of the resin can be improved. As an example of a neutralizing agent for neutralizing the acid structure, organic amines are preferable, and it is preferable to use organic amines such as trimethylamine, triethylamine, tripropylamine, tributylamine, N-methyldiethanolamine, and triethanolamine.

[0150] Examples of commercially available resin fine particles that can be used in the aqueous ink composition are given below.

[0151] (polyester) Takamatsu Oil Co., Ltd. PES resin A-110F, A-520, A-613D, A-615GE, A-640, A-645GH, A-647GEX, Unitika Ltd. Elitetel KA-5034, KA-5071S, KA-1449, KA-0134, KA-3556, KA-6137, KZA-6034, KT-8803, KT-8701, KT-9204, KT-8904, KT-0507, KT-9511

[0152] (Urethane type) Kusumoto Chemicals NeoRez R-967, R-600, R-9671, Mitsui Chemicals W-6061, W-5661, WS-4000

[0153] (Acrylic) Japan Coating Resins' Mowinyl 6899D, 6969D, 6800, 6810, Toyochem's TOCRYL W-7146, W-7150, W-7152

[0154] (Organic solvent) The organic solvent contained in the ink may be a water-soluble organic solvent, such as alcohols, polyhydric alcohols, amines, amides, glycol ethers, and 1,2-alkanediols having 4 or more carbon atoms.

[0155] Examples of alcohols include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, t-butanol, 3-methoxy-1-butanol, 3-methoxy-3-methylbutanol, 1-octanol, 2-octanol, n-nonyl alcohol, tridecyl alcohol, n-undecyl alcohol, stearyl alcohol, oleyl alcohol, and benzyl alcohol.

[0156] Examples of polyhydric alcohols include ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycols having 5 or more ethylene oxide groups, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycols having 4 or more propylene oxide groups, butylene glycol, hexanediol, pentanediol, glycerin, hexanetriol, and thiodiglycol.

[0157] Examples of amines include ethanolamine, diethanolamine, triethanolamine, N-methyldiethanolamine, N-ethyldiethanolamine, morpholine, N-ethylmorpholine, ethylenediamine, diethylenediamine, triethylenetetramine, tetraethylenepentamine, polyethyleneimine, pentamethyldiethylenetriamine, and tetramethylpropylenediamine.

[0158] Examples of amides include formamide, N,N-dimethylformamide, and N,N-dimethylacetamide.

[0159] Examples of glycol ethers include ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, propylene glycol monopropyl ether, dipropylene glycol monomethyl ether, and tripropylene glycol monomethyl ether.

[0160] Examples of 1,2-alkanediols having 4 or more carbon atoms include 1,2-butanediol, 1,2-pentanediol, 1,2-hexanediol, and 1,2-heptanediol.

[0161] Particularly preferred organic solvents are polyhydric alcohols, which can effectively suppress bleeding during high-speed printing.Specifically, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, and tripropylene glycol are preferred.

[0162] The ink may contain one or a combination of two or more selected from these organic solvents.

[0163] The content of the organic solvent in the ink is not particularly limited, but is preferably in the range of 10 to 60% by mass.

[0164] (Water, other additives) The water contained in the ink according to the present invention is not particularly limited, and may be ion-exchanged water, distilled water, or pure water.

[0165] The ink according to the present invention may contain various known additives as necessary for the purpose of improving various performances, such as a surfactant, ejection stability, compatibility with print heads and ink cartridges, storage stability, image storage stability, and the like.

[0166] The ink can also contain a surfactant, which can improve the ink ejection stability and control the spread (dot diameter) of the droplets that land on the recording medium.

[0167] The surfactant that can be used in the ink according to the present invention is not particularly limited. However, when the other constituent components of the ink contain an anionic compound, the ionicity of the surfactant is preferably anionic, nonionic or betaine type.

[0168] In the present invention, fluorine-based or silicone-based surfactants having high static surface tension reducing ability, anionic surfactants such as dioctyl sulfosuccinate having high dynamic surface tension reducing ability, and nonionic surfactants such as relatively low molecular weight polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, acetylene glycols, Pluronic (registered trademark) type surfactants, and sorbitan derivatives are preferably used. It is also preferable to use a fluorine-based or silicone-based surfactant in combination with a surfactant having high dynamic surface tension reducing ability.

[0169] The content of the surfactant in the ink is not particularly limited, but is preferably in the range of 0.1 to 5.0% by mass.

[0170] In addition to the above, the ink used in the present invention may contain various known additives, such as polysaccharides, viscosity modifiers, resistivity modifiers, film-forming agents, ultraviolet absorbers, antioxidants, anti-fading agents, antifungal agents, and anti-rust agents, which may be appropriately selected and used according to the purpose of improving ejection stability, compatibility with print heads and ink cartridges, storage stability, image storage stability, and other performances. For example, liquid paraffin, dioctyl phthalate, tricresyl phosphate, silicone oil, and other oil droplet fine particles, 193, 57-87988, 62-261476, etc.; anti-fading agents described in JP-A-57-74192, 57-87989, 60-72785, 61-146591, 1-95091, 3-13376, etc.; fluorescent brightening agents described in JP-A-59-42993, 59-52689, 62-280069, 61-242871, 4-219266, etc.

[0171] The ink used in the present invention having the above constitution preferably has a viscosity at 25°C in the range of 1 to 40 mPa·s, and more preferably in the range of 2 to 10 mPa·s.

[0172] [4] Inkjet recording method The inkjet recording method of the present invention is characterized in that the above-mentioned aqueous precoat composition and aqueous ink composition are combined and used as an inkjet recording liquid set. In the method using this inkjet recording liquid set, for example, one inkjet printer can be used to continuously and efficiently apply the precoat liquid constituting the inkjet recording liquid set of the present invention to the surface of a non-absorbent substrate and print with ink. It is then possible to print characters, patterns, etc. with excellent image quality and with little variation in dot diameter between substrates.

[0173] Specifically, the inkjet recording method of the present invention is an image forming method having a precoat applying step of applying the above-mentioned precoat liquid onto a recording medium made of a low-absorbency substrate or a non-absorbency substrate, a precoat liquid drying step of drying the precoat liquid applied onto the low-absorbency substrate or the non-absorbency substrate to form a precoat layer, an ink applying step of applying the above-mentioned ink onto the precoat layer by an inkjet method, and an ink drying step of drying the ink applied onto the precoat layer to form an ink layer.

[0174] [4.1] Precoat liquid application process In the precoat liquid application step, the precoat liquid is applied onto a recording medium made of a low-absorbency substrate or a non-absorbency substrate.

[0175] The method of applying the precoat liquid to a recording medium made of a low-absorbent or non-absorbent substrate is not particularly limited, and preferred examples include roller coating, curtain coating, spray coating, inkjet, etc. Among them, the roller coating is preferred from the viewpoints that a roller coater or the like can be connected to an inkjet device and can be efficiently applied even when the viscosity is relatively high. In addition, it is preferable from the viewpoint of improving the overall hot water resistance that the inkjet method is used as the step of applying the precoat liquid, since it is not necessary to apply a flocculant to the areas not to be coated with ink. In this case, as described below, when the substrate used is a metal substrate or the like, it is also preferable to place the metal substrate on a transport belt and coat and form a precoat layer while transporting the belt, or to use a flatbed type printer to which the substrate is fixed, to form the precoat layer.

[0176] [4.2] Precoat liquid drying process The precoat liquid drying step is a step of drying the precoat liquid applied onto a recording medium made of a low-absorbency substrate or a non-absorbency substrate to form a precoat layer. However, this step can be omitted, and a step of applying the ink liquid can be performed successively. In that case, the drying of the precoat liquid can be performed together with the drying of the ink liquid.

[0177] The precoat liquid is preferably dried under conditions that remove the solvent components of the precoat liquid, such as water and water-soluble organic solvents, while preventing the resin particles contained in the precoat liquid from completely fusing. The drying temperature of the precoat liquid is preferably in the range of, for example, 50 to 100° C. The drying time of the precoat liquid is preferably in the range of, for example, 3 to 30 seconds.

[0178] The precoat liquid may be dried using a non-contact heating type drying device such as a drying oven or a hot air blower, or may be dried using a contact heating type drying device such as a hot plate or a heated roller.

[0179] The drying temperature can be obtained by measuring any one of the following throughout the entire drying period of the precoat liquid: (a) when a non-contact heating drying device such as a drying oven or a hot air blower is used, the ambient temperature such as the oven temperature or the hot air temperature; (b) when a contact heating drying device such as a hot plate or a hot roller is used, the temperature of the contact heating part; or (c) the surface temperature of the surface to be dried. It is more preferable to measure the surface temperature of the surface to be dried (c) as the measurement location.

[0180] The thickness of the obtained precoat layer is preferably in the range of 0.3 to 3.0 μm, and more preferably in the range of 0.5 to 2.0 μm. When the thickness of the precoat layer is 0.3 μm or more, it is easy to increase the adhesion of the image and the laminate strength while suppressing ink bleeding. When the thickness of the precoat layer is 3.0 μm or less, it is possible to reduce deformation stress due to moisture and heat, so that the adhesion of the image and the laminate strength are less likely to be impaired.

[0181] [4.3] Ink application process In the ink application step, a precoat layer is formed on a recording medium made of a low-absorbency substrate or a non-absorbency substrate, and then the ink of the inkjet recording liquid set described above is applied by an inkjet method.

[0182] The inkjet method is not particularly limited, and a printer equipped with an inkjet head loaded with ink can be used. Specifically, ink is ejected as droplets from the nozzles of the inkjet head based on a digital signal, and the droplets are deposited on the precoat layer of the film substrate to perform printing.

[0183] The inkjet head may be either an on-demand type or a continuous type. Examples of on-demand type inkjet heads include electro-mechanical conversion types including single cavity type, double cavity type, bender type, piston type, shear mode type and shared wall type, and electro-thermal conversion types including thermal inkjet type and bubble jet type ("Bubble Jet" is a registered trademark of Canon Inc.).

[0184] Of the above inkjet heads, inkjet heads using a piezoelectric element as the electromechanical conversion element used in the electromechanical conversion method (also called a piezo type inkjet head) are preferable.

[0185] The inkjet head may be either a scanning type or a line type inkjet head, but the line type is preferable.

[0186] A line-type inkjet head is an inkjet head that has a length equal to or greater than the width of the printing range. As a line-type inkjet head, a single head that is equal to or greater than the width of the printing range may be used, or multiple heads may be combined to form a head that is equal to or greater than the width of the printing range.

[0187] Furthermore, a plurality of heads may be arranged in parallel so that the nozzles are arranged in a staggered arrangement, thereby increasing the resolution of the heads as a whole.

[0188] The conveying speed of the recording medium made of a low-absorbency substrate or a non-absorbency substrate can be set, for example, in the range of 1 to 120 m / min. The faster the conveying speed, the faster the image formation speed. According to the present invention, a high-definition image with high ink fixation can be obtained even at a very high linear speed in the range of 50 to 120 m / min, which is applicable to a single-pass inkjet image forming method.

[0189] By including the above-mentioned water-insoluble resin microparticles in the precoat liquid, the fixability of the image (coating film) on the recording medium of low absorbency substrate or non-absorbency substrate can be improved.In particular, by using a silicone surfactant (e.g., KF351A (manufactured by Shin-Etsu Silicone Co., Ltd.), etc.), it is possible to make the low absorbency substrate or non-absorbency substrate such as PP, PET, etc., wet and spread easily uniformly, so that the fixability of the image (coating film) on the recording medium of low absorbency substrate or non-absorbency substrate can be improved.

[0190] [4.4] Ink drying process In the ink drying step, the ink applied onto a recording medium having a low absorbency or a non-absorbency substrate is dried.

[0191] The ink is dried by removing the main solvent components of the ink, such as water and water-soluble organic solvents, and at the same time drying the aggregating agent according to the present invention at a temperature equal to or higher than the thermal decomposition temperature to thermally decompose it. The upper limit of the drying temperature is preferably 220°C or lower, from the viewpoint of achieving both the thermal decomposition property of the aggregating agent and the stability of the ink composition. The ink drying time is controlled by at least the time it takes for the aggregating agent to thermally decompose. The decomposition time is appropriately selected depending on the type of aggregating agent selected, and can be appropriately determined from the viewpoint of the degree of thermal decomposition at which the effects of the present invention can be obtained and productivity.

[0192] The ink can be dried in the same manner as the above-mentioned drying of the precoat liquid.

[0193] [5] Inkjet recording device Fig. 1 is a schematic diagram of a precoat / inkjet recording apparatus preferred in the present invention. However, the present invention is not limited thereto, and for example, in the precoat / inkjet recording apparatus 1 shown in Fig. 1, the first drying section 14 may be omitted.

[0194] The precoat / inkjet recording apparatus 1 is mainly composed of a precoat application section 10 and an inkjet printing section 20. In the precoat application section 10, a precoat layer C is formed on a substrate F, and an ink layer R is formed by the inkjet printing section 20.

[0195] Specifically, precoat droplets 13 ejected from a nozzle 12 are applied by a roll coater 11 onto a substrate F fed from a delivery roller 30 to form a precoat layer C. Subsequently, the precoat layer C is dried by a first drying section 14.

[0196] Next, ink droplets 22 are ejected from an inkjet head 21 onto the precoat layer C to form an ink layer R, which is then dried by a second drying section 23 at a temperature equal to or higher than the thermal decomposition temperature of the aggregating agent according to the present invention. The substrate F on which the precoat layer C and the ink layer R are formed is then wound up by a winding roller 40 to obtain an image recording material.

[0197] Although FIG. 1 shows the case where the substrate F is a film substrate, in the case of a metal substrate or the like, the metal substrate can be placed on a conveyor belt, and the precoat layer C and the ink layer R can be coated and formed in one pass while conveying the belt.

[0198] Furthermore, as an apparatus other than the precoat / inkjet recording apparatus shown in Fig. 1, it is also preferable to use a flatbed type printer for applying the precoat liquid and the ink liquid. In a flatbed type printer, the substrate is fixed, and the inkjet head can be moved in the main scanning direction and the sub-scanning direction intersecting the main scanning direction, and printing can be performed without transporting the substrate. For metal substrates such as tinplate, roll-to-roll transport is not possible as with resin film materials, so it is preferable to use a flatbed type printer that does not require transporting the substrate.

[0199] Examples of such flatbed type printers include the printers described in FIG. 1 of JP-A-2015-74161 and FIG. 1 of JP-A-2017-177578.

[0200] [6] Image recordings The image recorded matter of the present invention is characterized by having a substrate, a precoat layer formed on the substrate using a precoat liquid of the inkjet recording liquid set, and an ink layer formed on the precoat layer using an ink.

[0201] 2, the image recording material P is prepared by applying the precoat liquid according to the present invention onto a substrate F using a roll coater or by discharging the liquid from an inkjet head to form a precoat layer C. At the position where the precoat layer C is fixed, an ink liquid is discharged from an inkjet head and fixed to form an image recording layer R.

[0202] The above configuration shows the minimum configuration, and another functional layer may be formed between the substrate and the precoat layer, and a non-absorbent film substrate or the like may be attached to the upper layer of the ink layer via, for example, a laminating adhesive layer. At least, a configuration in which the precoat layer and the ink layer are in contact with each other is essential.

[0203] One example of the image recording material of the present invention is an image recording material that uses at least the aqueous precoat composition and aqueous ink composition of the present invention, in which a first layer containing a thermosetting resin, a second layer containing the aqueous precoat composition, a third layer containing the aqueous ink composition, and a fourth layer containing a thermosetting resin are laminated in this order on a metal substrate.

[0204] That is, the image recording material has at least four layers laminated on a metal substrate, the first layer and the fourth layer contain a thermosetting resin, and the second layer contains at least a coagulant. Thermal decomposition product of The flocculant is selected from a thermally decomposable cationic resin, an organic acid, or a polyvalent metal salt, and the third layer contains at least a pigment, a polymer dispersant, A neutralizer for the polymer dispersant and resin fine particles, and a neutralizer for the polymer dispersant is selected from organic amines. R It is characterized by the above.

[0205] Specific preferred examples of the image-recorded material include packaging materials for packaging canned foods, retort foods, beverages, and the like.

[0206] FIG. 3 shows a cross-sectional view of a packaging material for canned food, which is an example of the image recorded material of the present invention.

[0207] A thermosetting resin (e.g., TW-1407 series, manufactured by T&K TOKA) is roller-coated on a tinplate substrate 51 to form a thermosetting resin layer (base coat) 52, on which an image is formed by a precoat layer 53 and an ink layer 54. Next, a thermosetting resin (e.g., AX-10 series, manufactured by T&K TOKA) is roller-coated to form a thermosetting resin layer (top coat) 55, which is then heated and cured and dried to obtain a packaging material 50 for canned foods. EXAMPLES

[0208] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they represent "parts by mass" or "% by mass" unless otherwise specified.

[0209] The materials used in preparing the aqueous precoat composition were as follows:

[0210] (Flocculant) Cationic polymer: PAS-21CL (Nittobo Medical Co., Ltd.), thermal decomposition temperature: 180℃ Polyvalent metal salt 1: calcium acetate, thermal decomposition temperature: 160℃ Organic acid: malonic acid, thermal decomposition temperature: 140℃ Polyvalent metal salt 2 (comparison example): calcium chloride, boiling point: 1600°C

[0211] (Resin fine particles) Polyester: Z-1100 (Goyo Chemical Co., Ltd.) Acrylic: RKW-620 (Taisei Fine Chemical Co., Ltd.) Urethane: SF650 (Daiichi Kogyo Seiyaku) · Urethane · Acrylic: WEM-506C (Taisei Fine Chemical Co., Ltd.)

[0212] (Surfactant): KF351A (Shin-Etsu Silicone Co., Ltd.)

[0213] The materials used in preparing the aqueous ink composition are as follows:

[0214] (Dispersant neutralizer) Neutralizer 1: N-methyldiethanolamine Neutralizer 2 (comparison): NaOH

[0215] (Resin fine particles) Polyester: PES RESIN A-645GH (Takamatsu Oil Co., Ltd.) Polyacrylic: NeoCryl A-1127 (Kusumoto Chemicals) Polyurethane: W-6061 (Mitsui Chemicals) · Urethane · Acrylic: WEM-041U (Taisei Fine Chemical Co., Ltd.) (Pigment): Pigment Blue 15:3

[0216] (Dispersion resin): Joncryl 819 (BASF)

[0217] (Ink solvent): Ethylene glycol

[0218] (Surfactant): KF351A (Shin-Etsu Silicone Co., Ltd.)

[0219] <Example 1> Preparation of the Precoat Composition 14% by mass of polyester resin Z-1100 (GOO Chemical Co., Ltd.) as resin particles, 5% by mass of cationic polymer PAS-21CL (Nittobo Medical Co., Ltd., thermal decomposition temperature: 180°C) as flocculant, 0.5% by mass of surfactant KF351A (Shin-Etsu Silicone Co., Ltd.), and ion-exchanged water (balance: amount that the total amount is 100% by mass) were added in sequence while stirring, and then filtered through a 5.0 μm filter to obtain a precoat composition. There was no substantial change in composition before and after filtration.

[0220] (Preparation of Ink Composition) A mixture of 18% by mass of pigment (Pigment Blue 15:3), 31.5% by mass of pigment dispersant (acrylic dispersant having a carboxyl group neutralized with sodium hydroxide (BASF's "Joncryl 819", acid value 75 mg KOH / g, solid content 20% by mass), 20% by mass of ethylene glycol, and ion-exchanged water (balance; amount that makes the total amount 100% by mass) was premixed, and then dispersed using a sand grinder filled with 0.5 mm zirconia beads at a volume ratio of 50%, to prepare pigment dispersion G-2 with a pigment content of 18% by mass. The average particle size of the pigment particles contained in this pigment dispersion was 110 nm. The average particle size was measured using a "Zetasizer 1000HS" manufactured by Marballoon Co., Ltd.

[0221] To the pigment dispersion liquid 27.8% by mass (5% by mass as solid content), 5% by mass of resin fine particles PESRESIN A-645GH (Takamatsu Oil Co., Ltd.), 0.4% by mass of dispersant neutralizer N-methyldiethanolamine, 30% by mass of ethylene glycol, 0.5% by mass of surfactant KF351A (Shin-Etsu Silicone Co., Ltd.) and ion-exchanged water (balance; total amount is 100% by mass) were added while stirring, and the resulting mixture was filtered through a 1 μm filter to obtain an ink composition. There was no substantial change in composition before and after filtration.

[0222] <Preparation of precoat compositions and ink compositions of Examples 2 to 17 and Comparative Examples 1 to 3> The precoat compositions and ink compositions of Examples 2 to 17 and Comparative Examples 1 to 3 were prepared in the same manner as the precoat composition and ink composition of Example 1, except that the precoat composition materials and ink composition materials were changed as shown in Tables I to IV.

[0223] <Formation of precoat layer and ink layer> The aqueous precoat composition was applied to the tinplate substrate by roller coating at a resin solid content of 1.5 g / m 2 After coating to a wet film thickness of 9 μm, the substrate was prepared by drying for 5 minutes with hot air at 60° C. In Examples 4 and 17, the aqueous precoat composition was coated by the inkjet method.

[0224] Next, two independently driven inkjet heads (360 dpi, ejection volume 14 pL) manufactured by Konica Minolta were arranged side by side with the nozzles staggered to create a head module capable of printing a 720 dpi x 720 dpi solid image in a single pass. Two such head modules were prepared and arranged side by side along the transport direction of the transport stage that transports the recording medium. Each head module was installed so that it intersected with the transport direction (movement axis of the transport stage). In this way, a printing rate of 200%, that is, the amount of ink applied for two colors (22.5 cc / m2) was achieved during one pass of the recording medium. 2 ) can now be printed.

[0225] The recording medium was placed on a transport stage with the surface coated with the aqueous precoat composition facing up, and transported at a speed of 60 m / min. As the recording medium passed under the head, the aqueous ink composition was printed using a single pass method.

[0226] After printing by the inkjet method, the recording medium was placed in a dryer and dried for 15 minutes at each of the set temperatures shown in Tables I to IV to obtain a laminate having a precoat layer and an ink layer.

[0227] In Examples 16 and 17, a base coat liquid (TW-1407 series, manufactured by T&K TOKA) made of a thermosetting resin was applied to the tinplate substrate at a rate of 160 mg / 100 cm by roller coating. 2 After coating so as to obtain the above, the coating was dried in a dryer at 190° C. for 10 minutes. Next, the precoat layer and the ink layer were formed as described above.

[0228] Furthermore, a topcoat liquid made of thermosetting resin (AX-10 series, manufactured by T&K TOKA) was applied to the ink-coated surface at a rate of 160 mg / 100 cm by roller coating. 2 After coating, the mixture was dried in a dryer at 180° C. for 10 minutes.

[0229] Evaluation (1) Measurement of the thermal decomposition temperature of the coagulant The thermal decomposition temperature of the flocculant was measured using a thermogravimetric differential thermal analyzer (TG-DTA).

[0230] "Thermal decomposition temperature" means the temperature at which mass loss due to thermal decomposition begins when the temperature is increased from room temperature (heating rate: 10°C / min). The temperature at which mass loss begins is determined by plotting the mass loss rate on the vertical axis and temperature on the horizontal axis, and the temperature at which the tangent at the time of the greatest mass loss intersects with the tangent before mass loss. The decomposition temperature of each flocculant was measured according to the above definition using a measuring device STA7200 manufactured by Hitachi High-Tech Science Corporation.

[0231] (2) Hot water resistance The solid images formed above for evaluation of Examples 1 to 17 and Comparative Examples 1 to 3 were stored at 40°C for 3 days, and then cut into strips of 10 cm x 1 cm so that the image portion was the cut edge to prepare test pieces. The test pieces were boiled in a pressure cooker for 30 minutes, and the condition of the test pieces after boiling was visually confirmed, and the hot water resistance of the images made with each ink was evaluated according to the following criteria. A rating of 2 or higher is within the practical acceptable range.

[0232] 4: There is no peeling in either the cut end or solid area images. 3: There is some peeling on the cut edge image, but there is no peeling on the solid image 2: Image of cut edge, part of the solid part of the image is peeled off 1: Image of cut edge, most of the solid part of the image has peeled off The configurations of the above precoat layer and ink layer, and the evaluation results are shown in Tables I to IV.

[0233] [Table 1]

[0234] [Table 2]

[0235] [Table 3]

[0236] [Table 4]

[0237] It is clear from Tables I to IV that the ink jet recording methods of Examples 1 to 17 using the precoat composition and ink composition of the present invention are superior in hot water resistance to Comparative Examples 1 to 3.

[0238] In comparison with Example 3, in Examples 6 to 8, it was found that hot water resistance was improved when the drying temperature was set to 220° C. or less. Similarly, in Examples 9 to 11, it was found that hot water resistance was improved when the polyester resin was changed to a polyurethane resin, a polyacrylic resin, or a composite resin particle of a polyurethane resin and a polyacrylic resin as the resin particle of the ink composition.

[0239] In addition, in Examples 16 and 17, a metal substrate was used, and a precoat layer and an ink layer were sandwiched between thermosetting resin layers (base coat and top coat) to form a canned food packaging material. A similar evaluation was performed, and the image recording material had excellent hot water resistance. [Industrial Applicability]

[0240] The inkjet recording method of the present invention is a two-liquid inkjet recording method in which an image is formed on a precoat coating film, and since it has improved hot water resistance, it is suitable for use in inkjet recording on packaging materials for packaging canned foods, retort foods, beverages, and the like. [Explanation of symbols]

[0241] 1 Pre-coat / inkjet recording device 10 Precoat application section 11 Roll coater 12 Nozzles 13 Precoat droplets 14 1st drying section 20 Inkjet Printing Section 21 Inkjet head 22 Ink Droplets 23 2nd drying section 30 Delivery roller 40 Winding roller C Precoat layer F Base material P Image recording R ink layer 50 Canned food packaging materials 51 Tinplate substrate 52 Thermosetting resin layer (base coat) 53 Precoat layer 54 Ink Layer 55 Thermosetting resin layer (top coat)

Claims

1. An inkjet recording method comprising the steps of applying an aqueous precoat composition onto a substrate, or applying and drying the aqueous precoat composition, and then applying and drying an aqueous ink composition onto the substrate, in this order, The aqueous precoat composition contains at least a flocculant, the aqueous ink composition contains at least a pigment, a polymer dispersant, a neutralizer for the polymer dispersant, and resin fine particles; the flocculant is selected from a thermally decomposable cationic resin, an organic acid, or a polyvalent metal salt; The neutralizing agent for the polymeric dispersant is selected from an organic amine, and The inkjet recording method according to claim 1, further comprising a step of drying the aqueous ink composition at a temperature equal to or higher than a thermal decomposition temperature of the aggregating agent.

2. 2. The ink-jet recording method according to claim 1, wherein the step of applying the aqueous precoat composition is a step using an ink-jet method.

3. 3. The inkjet recording method according to claim 1, wherein the content of the coagulant is 5% by mass or less based on the weight of the aqueous precoat composition.

4. 4. The inkjet recording method according to claim 1, wherein the aqueous ink composition is dried at a temperature of 220[deg.] C. or less.

5. 5. The inkjet recording method according to claim 1, wherein the resin of the resin fine particles of the aqueous ink composition is selected from the group consisting of polyurethane resins, polyacrylic resins, and composite resins of polyurethane resins and polyacrylic resins.

6. 6. The inkjet recording method according to claim 1, wherein the aqueous precoat composition further contains resin fine particles, and the resin of the resin fine particles is selected from a polyester resin, a polyurethane resin, a polyacrylic resin, or a composite resin of a polyurethane resin and a polyacrylic resin.

7. An image recording material having at least four layers laminated on a metal substrate, the first layer and the fourth layer contain a thermosetting resin; The second layer contains at least a thermal decomposition product of a flocculant, and the flocculant is selected from a thermally decomposable cationic resin, an organic acid, or a polyvalent metal salt; 1. An image recording material, wherein the third layer contains at least a pigment, a polymeric dispersant, a neutralizer for the polymeric dispersant, and resin fine particles, and the neutralizer for the polymeric dispersant is selected from organic amines.

8. 8. The image recorded matter according to claim 7, wherein the content of the thermal decomposition product of the flocculant is 5% by mass or less with respect to the second layer.

9. 9. The image recorded matter according to claim 7, wherein the resin of the resin particles contained in the third layer is selected from the group consisting of polyurethane resins, polyacrylic resins, and composite resins of polyurethane resins and polyacrylic resins.

10. The image recording material according to any one of claims 7 to 9, characterized in that the second layer further contains resin microparticles, and the resin of the resin microparticles is selected from a polyurethane-based resin, a polyacrylic-based resin, or a composite resin of a polyurethane-based resin and a polyacrylic-based resin.

Citation Information

Patent Citations

  • Inkjet recording method, pretreatment liquid for inkjet recording and ink composition

    JP2009202596A

  • Inkjet ink set and image forming method

    JP2015034277A

  • Image formation set, image formation method and image formation apparatus

    JP2017137461A

  • Liquid composition for surface treatment of printed matter, ink set, recording method and recording device

    JP2018094902A

  • Ink set, and manufacturing method of printed material

    JP2019019315A