Radio wave permeable metallic member and its manufacturing method
By orienting metal particles vertically with a high aspect ratio and using a polymer coating, the metallic member maintains metallic luster and radio wave transparency, addressing the issues of conventional methods that lose luster and are costly or difficult to control.
Patent Information
- Application Number
- JP2022066684
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-04-14
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-04-14
AI Technical Summary
Conventional methods for producing radio wave transparent metallic members result in loss of metallic luster and are costly or difficult to control, leading to surface plasmon resonance and absorption of specific wavelengths.
A metallic member is constructed with a substrate, an ion exchange resin layer, and a metal particle layer where metal particles are oriented vertically with a high aspect ratio, having gaps between them, and coated with a polymer to maintain metallic luster and radio wave transparency.
The solution achieves a metallic member with inherent color and luster while maintaining radio wave transparency by shifting the absorption peak due to surface plasmon resonance, ensuring no specific absorption in the visible light region.
Smart Images

Figure 0007582243000002 
Figure 0007582243000003 
Figure 0007582243000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a radio wave transparent metallic member and a method for producing the same. [Background technology]
[0002] Metallic parts are used in various products because they can impart a high-brightness metallic luster to the surface of the product, giving it a luxurious feel. In addition to having excellent metallic luster, metallic parts are required to have various properties depending on the product in which they are used. One of such properties is radio wave transparency. For example, a millimeter wave radar mounted on an automobile or the like is a device that irradiates radio waves in the millimeter wave band (radio waves with a wavelength of 1 to 10 mm) and measures the time it takes for the radio waves to reflect off an obstacle and return, thereby measuring the distance to the obstacle. When a metallic part is used in this millimeter wave radar, the metallic part is required to have excellent metallic luster and millimeter wave transparency.
[0003] As an example of a metallic member having radio wave transparency, Patent Document 1 discloses an electromagnetic wave transparent metallic gloss member produced by sputtering a metal onto a substrate to form a discontinuous film. However, sputtering is a vacuum batch process, and therefore the cost is high.
[0004] Patent Document 2 also discloses a method for producing an electromagnetic wave-transmitting metal composite material, including a step of forming a metal coating on a resin substrate and a step of removing a part of the formed metal coating to form regular island-shaped metal regions. Patent Document 2 also discloses that the metal coating is formed by sputtering or vacuum deposition, and that the part of the metal coating is removed by masking and etching the part of the metal coating that corresponds to the metal region. However, this production method involves many complicated steps, and furthermore, etching is difficult to control, making it difficult to obtain the desired structure.
[0005] Moreover, Patent Document 3 discloses a metallic film produced by a method other than sputtering or vapor deposition.
[0006] However, in metallic components produced by conventional manufacturing methods, surface plasmon resonance occurs, causing the metal film to strongly absorb light of specific wavelengths in the visible light range, which can damage the original color and luster of the metal. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2018-69462 A [Patent Document 2] JP 2010-251899 A [Patent Document 3] JP 2021-155844 A Summary of the Invention [Problem to be solved by the invention]
[0008] As described above, in conventional radio wave transparent metallic components, the color and luster inherent to the metal may be impaired. Therefore, an object of the present invention is to provide a radio wave transparent metallic component having excellent metallic luster. [Means for solving the problem]
[0009] The inventors have investigated various means for solving the above problems and have found that by orienting high aspect ratio metal particles vertically relative to a substrate, it is possible to obtain a metallic component that has no peculiar absorption in the visible light region and combines excellent metallic luster and radio wave transmittance, thereby completing the present invention.
[0010] That is, the gist of the present invention is as follows. (1) A metallic component having a substrate, an ion exchange resin layer formed on the substrate, and a metal particle layer formed on the ion exchange resin layer, In the metal particle layer, there are gaps between the metal particles, In a cross section of the metallic component, a maximum horizontal length a (nm) of the metal particle, a maximum vertical length b (nm) of the metal particle, and a vertical length c (nm) of a portion of the metal particle embedded in the ion exchange resin layer satisfy 1.5 nm≦a≦200 nm, b / a≧1.25, and c≧0, A metallic member, wherein an inclination θ(°) of the metal particles with respect to a bottom surface of the ion exchange resin layer satisfies 60°≦θ≦90°. (2) The metallic member according to (1) above, wherein the metal of the metal particles is one or more metals selected from Ag, Al, Au, Ti, Cr, Mn, Fe, Ni, Cu, Zn, Zr, Nb, Mo, In, Co and Sn. (3) The metallic member according to (2) above, wherein the metal of the metal particles is Ag. (4) The metallic member according to any one of (1) to (3) above, wherein the ion exchange resin of the ion exchange resin layer is a resin having a carboxyl group and / or a sulfo group. (5) The metallic member according to (4) above, wherein the ion exchange resin of the ion exchange resin layer is a polyamic acid. (6) The metallic member according to any one of (1) to (5) above, wherein at least a part of the surface of the metal particle is coated with a polymer that is adsorbed to the metal surface. (7) The metallic member according to (6) above, wherein the polymer adsorbed on the metal surface has a weight average molecular weight of 10,000 to 360,000. (8) The metallic member according to (6) or (7) above, wherein the polymer adsorbed to the metal surface is at least one selected from the group consisting of polyvinyl polymers, polyethylene glycol polymers, and polyacrylic acid polymers. (9) A method for producing a metallic component according to any one of (1) to (8), forming an ion exchange resin layer on a surface of a substrate; treating the ion exchange resin layer with a solution containing metal ions to introduce the metal ions into the ion exchange resin layer; The ion exchange resin layer into which the metal ions have been introduced is treated with a solution containing 0.1 mM to 500 mM of a polymer adsorbed to a metal surface and 0.01 mM to 10 mM of a reducing agent, thereby reducing the metal ions and precipitating metal particles on the surface of the ion exchange resin layer. The method for producing a metallic member includes the steps of: Effect of the Invention
[0011] According to the present invention, it is possible to provide a radio wave transparent metallic component having excellent metallic luster. [Brief description of the drawings]
[0012] [Figure 1] Fig. 1A is a schematic cross-sectional view of one embodiment of the metallic member of the present invention, and Fig. 1B is a partially enlarged schematic cross-sectional view of one embodiment of the metallic member of the present invention. [Diagram 2] 2A shows a TEM image of a cross section of the metallic member of Example 3. FIG. 2B shows a TEM image of a cross section of the metallic member of Comparative Example 1. [Diagram 3] FIG. 3 shows a 3D-TEM image of the metallic member of Example 3. [Figure 4] FIG. 4 shows the absorption spectra of the metallic members of Examples 2 and 3 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Preferred embodiments of the present invention will now be described in detail.
[0014] The present invention relates to a metallic component having a substrate having an ion exchange resin layer on its surface and a metal particle layer formed on the ion exchange resin layer side of the substrate. That is, the metallic component of the present invention has a substrate, an ion exchange resin layer formed on the substrate, and a metal particle layer formed on the ion exchange resin layer.
[0015] FIG. 1A shows a schematic cross-sectional view of one embodiment of the metallic component of the present invention. As shown in FIG. 1A, the metallic component 10 has a base 11, an ion exchange resin layer 12 formed on the base 11, and a layer of metal particles 13 formed on the ion exchange resin layer 12. That is, the metallic component 10 has the base 11, the ion exchange resin layer 12, and the layer of metal particles 13 laminated in this order from the bottom. In a preferred embodiment, the metallic component 10 is composed of the base 11, the ion exchange resin layer 12 laminated directly on the base 11, and the layer of metal particles 13 laminated directly on the ion exchange resin layer 12. In the metal particle layer, there are gaps between the metal particles. The metallic component may have an ion exchange resin layer and a metal particle layer on both sides of the base.
[0016] The substrate is not particularly limited, and may be a substrate film, a resin molded substrate, a glass substrate, or an article to which a metallic luster should be imparted.
[0017] For example, a resin film can be used as the base film. As the resin film, a transparent film is preferable, and examples thereof include polyethylene terephthalate, polycarbonate, polymethyl methacrylate, and acrylic, with polycarbonate and acrylic being preferable. In addition, as the resin film, a resin having a group that can be converted into an ion exchange group such as a carboxyl group and / or a sulfo group may be used. Examples of such resins include polycarbonate, acrylic, polyimide, and polystyrene, with polyimide having a high functional group density being preferable.
[0018] Examples of the resin molding substrate include resins for automobile emblems, etc. Examples of the articles to which metallic luster should be imparted include door knobs for automobiles equipped with smart keys, mobile phone housings, personal computer housings, refrigerators, etc.
[0019] The thickness of the substrate is usually 10 μm to 10 mm, and preferably 10 μm to 5 mm.
[0020] The ion exchange resin layer is formed on the surface of the substrate. The ion exchange resin may be any resin having an ion exchange group capable of ion-exchanging with a metal ion, and may be, for example, a resin having a carboxyl group and / or a sulfo group. As the ion exchange resin, polyamic acid and styrene-divinylbenzene copolymer are preferred, and polyamic acid is more preferred. The ion exchange resin may be in a form in which the ion exchange group is converted into any form by heat treatment or the like. For example, polyamic acid is dehydrated and converted into polyimide by heat treatment.
[0021] The thickness of the ion exchange resin layer is usually 0.5 μm to 10 μm, and preferably 0.7 μm to 1.5 μm.
[0022] The metal particle layer is formed on the surface of the ion-exchange resin layer. The metal of the metal particles is preferably Ag, Al, Au, Ti, Cr, Mn, Fe, Ni, Cu, Zn, Zr, Nb, Mo, In, Co, or Sn, more preferably Ag, Al, or Cr, and particularly preferably Ag, from the viewpoint of high brightness.
[0023] In the metal particle layer, the metal particles are formed, for example, in an island shape, and there are gaps between the metal particles. That is, the metal particle layer is a discontinuous film of metal particles. The gaps between the metal particles may exist between at least some of the metal particles, but preferably, there are gaps between each metal particle. The gaps between the metal particles are usually 1 nm to 1000 nm, and preferably 1 nm to 100 nm. The gaps between the metal particles refer to the average length of the linear gaps measured using image analysis software ImageJ, by randomly extracting, for example, 100 particles from an image of the surface of the metallic member obtained by a field emission scanning electron microscope (FE-SEM) (50,000 times magnification), drawing straight lines between the centers of adjacent particles, and measuring the linear gaps. The presence of gaps between the metal particles gives the metallic member excellent radio wave permeability.
[0024] The metallic component of the present invention is characterized in that metal particles with a high aspect ratio are oriented vertically with respect to the ion exchange resin layer and the substrate, which allows the absorption peak due to surface plasmon resonance to be shifted, resulting in a metal film that has no specific absorption in the visible light region and has the original color and luster of the metal.
[0025] FIG. 1B shows a partially enlarged schematic cross-sectional view of one embodiment of the metallic member of the present invention. As shown in FIG. 1B, in one embodiment, metal particles 13 are embedded in an ion exchange resin layer 12. The metal particles 13 have a high aspect ratio and are vertically oriented with respect to the ion exchange resin layer 12 and the substrate (not shown). In one embodiment, a part of the surface of the metal particles 13 is covered with a polymer 14 that adsorbs to the metal surface. In FIG. 1B, a represents the maximum horizontal length (nm) of the metal particles, b represents the maximum vertical length (nm) of the metal particles, and c represents the vertical length (nm) of the part where the metal particles are embedded in the ion exchange resin layer. Also, in FIG. 1B, θ represents the inclination (°) of the metal particles with respect to the bottom surface of the ion exchange resin layer.
[0026] In the metallic component of the present invention, the fact that metal particles with a high aspect ratio are oriented vertically relative to the ion exchange resin layer and the substrate is expressed by the ratio b / a of the maximum vertical length b (nm) of the metal particle to the maximum horizontal length a (nm), and the inclination θ (°) of the metal particle.
[0027] The maximum horizontal length a of the metal particles refers to the maximum length in the horizontal direction relative to the surface of the ion exchange resin layer and the base. The maximum vertical length b of the metal particles refers to the maximum length in the vertical direction relative to the surface of the ion exchange resin layer and the base. Note that since the metal particles may be inclined at an inclination θ(°) relative to the bottom surface of the ion exchange resin layer, the vertical direction does not only mean a direction of 90° relative to the surface of the ion exchange resin layer and the base, but may be a direction of 60° to 90° depending on the inclination θ(°).
[0028] The maximum horizontal length a and maximum vertical length b of the metal particles can be determined by obtaining a cross-sectional image of the metallic component using a scanning transmission electron microscope (STEM), randomly selecting, for example, 100 particles present within a 50,000x field of view, calculating the length using the image analysis software ImageJ, and determining the average value (number average). The maximum horizontal length a of the metal particles can also be determined by obtaining a surface image of the metallic component using a field emission scanning electron microscope (FE-SEM) (50,000x) and determining the average value (number average) of the maximum diameter of the particles. It is believed that the maximum horizontal length a of the metal particles will be the same whether measured using STEM or FE-SEM.
[0029] The maximum horizontal length a (nm) of the metal particles is 1.5 nm≦a≦200 nm. When the length a is within this range, the metal particles reflect visible light and transmit millimeter waves, and have radio wave transmittance. The length a (nm) is preferably 5 nm≦a≦150 nm, more preferably 5 nm≦a≦100 nm, and particularly preferably 5 nm≦a<50 nm.
[0030] The maximum length b (nm) of the metal particles in the vertical direction is preferably 1.9 nm≦b≦500 nm, more preferably 10 nm≦b≦100 nm. When the length b is within this range, a metal film having the original color and luster of the metal can be obtained.
[0031] The ratio b / a (also referred to as aspect ratio) of the maximum vertical length b of the metal particle to the maximum horizontal length a is b / a≧1.25, preferably b / a≧1.5, and more preferably b / a≧2.0. When the aspect ratio b / a of the metal particle is 1.25 or more, the absorption peak due to surface plasmon resonance can be shifted to suppress absorption of a specific wavelength in the visible light range, and a metal film having the original color and luster of the metal without specific absorption in the visible light range can be obtained.
[0032] The vertical length c (nm) of the portion where the metal particles are embedded in the ion exchange resin layer satisfies c ≧ 0. That is, the metal particles are in contact with the surface of the ion exchange resin layer (c = 0), or a part of them is embedded in the ion exchange resin layer (c > 0). From the viewpoint of having high durability, the length c (nm) is preferably c > 0. The length c (nm) is smaller than the maximum vertical length b (nm) of the metal particles (c < b), preferably c < 50 nm, more preferably c < 25 nm, and particularly preferably c < 10 nm. Similar to the lengths a and b, the length c of the metal particles can be determined by obtaining a cross-sectional image of the metal-containing member with a scanning transmission electron microscope (STEM), randomly extracting the particles present in a field of view of 50,000 times magnification, and using image analysis software ImageJ. As shown in Fig. 1B, the metal particles are in contact with the surface of the ion exchange resin layer at both ends. The length c of the metal particles is calculated as the vertical (90°) length from the straight line passing through the bottom surface of the particles in the ion exchange resin layer to both ends of the particles in contact with the surface of the ion exchange resin layer in the cross-sectional image, and the average value (number average) is obtained for, for example, 25 to 50 particles.
[0033] The inclination θ (°) of the metal particles with respect to the bottom surface of the ion exchange resin layer (i.e., the surface on the substrate side) satisfies 60° ≦ θ ≦ 90°, preferably 75° ≦ θ ≦ 90°, and more preferably 80° ≦ θ ≦ 90°. By setting the inclination θ of the metal particles within this range, the metal film can have the original color and luster of the metal.
[0034] Similar to the measurement of the length of the metal particles, the inclination θ of the metal particles can be determined by analyzing the TEM image obtained by STEM with ImageJ, randomly extracting, for example, 100 particles present in a field of view of 50,000 times magnification, and calculating the angle formed by the central axis in the vertical direction of the metal particles and the bottom surface of the ion exchange resin layer. The central axis in the vertical direction of the metal particles corresponds to the maximum vertical length b of the metal particles.
[0035] A structure in which metal particles with a high aspect ratio are vertically oriented can be obtained by using a polymer that adsorbs to the metal surface in the manufacturing method of the metallic component described below. Therefore, preferably, at least a part of the surface of the metal particles is coated with a polymer that adsorbs to the metal surface. Since the polymer that adsorbs to the metal surface is adsorbed to a specific crystal plane of the metal, usually a part of the surface of the metal particles is coated with this polymer.
[0036] The weight average molecular weight of the polymer adsorbed to the metal surface is preferably from 10,000 to 360,000, and more preferably from 10,000 to 100,000, from the viewpoint of high adsorption to the metal surface.
[0037] As a polymer to be adsorbed to a metal surface, for example, a polymer having a lone pair of nitrogen (N), sulfur (S) or oxygen (O) in the molecular chain structure of the polymer can be used, and a polymer having a lone pair of oxygen is preferred. Since the atomic packing rate differs on each crystal face of a metal, the electronic state on the crystal surface differs. In the production of metallic components, a polymer having a lone pair of N, S or O can be adsorbed to a specific crystal face of a metal via the electrons of the lone pair, and the aspect ratio and inclination of the metal particles can be controlled.
[0038] The polymer adsorbed onto the metal surface is not particularly limited, and examples thereof include polyvinyl-based polymers such as polyvinyl acetate, polyvinyl alcohol, poly-N-vinyl acetamide, polyvinylpyrrolidone, etc.; polyethylene glycol-based polymers such as polyethylene glycol, polyepichlorohydrin, polyepibromohydrin, etc.; polyacrylic acid-based polymers such as polyacrylic acid, polymethacrylic acid, sodium polyacrylate, sodium polymethacrylate, etc.; and poly(amidoamine) dendrimers synthesized by alternating addition of ethylenediamine and methyl acrylate. Of these, polyvinyl-based polymers, polyethylene glycol-based polymers, and polyacrylic acid-based polymers are preferred, polyvinyl alcohol, polyvinylpyrrolidone, polyethylene glycol, and sodium polyacrylate are more preferred, and polyvinylpyrrolidone is particularly preferred.
[0039] The L* value of the metallic member is preferably 75 or more, and has high brightness. The L* value of the metallic member can be determined, for example, by measuring with a spectrophotometer using the SCI method (including regular reflection light), determining the spectral reflectance R(λ) as the ratio (JIS Z 8722) between the spectral radiant flux of wavelength λ reflected from an object and the spectral radiant flux of wavelength λ reflected from a perfect diffuse reflecting surface, and calculating the index value L* of the CIE1976 (L*, a*, b*) color system defined by the International Commission on Illumination (CIE) using the spectral reflectance R(λ).
[0040] The a* value of the metallic member is preferably −2 to 2, and there is little change in color tone with respect to red and green hues. The a* value of the metallic member can be measured in the same manner as the L* value.
[0041] The b* value of the metallic member is preferably −5 to 6, and there is little change in color tone for yellow and blue hues. The b* value of the metallic member can be measured in the same manner as the L* value.
[0042] The metallic member preferably has an a* value of −2 to 2 and a b* value of −5 to 6. When the metallic member has an a* value and a b* value within this range, the metal film has the original color and luster of the metal, and has excellent metallic luster.
[0043] The present invention also relates to a method for producing the metallic component. The method for producing the metallic component of the present invention includes forming an ion-exchange resin layer on the surface of a substrate (step 1), treating the ion-exchange resin layer with a solution containing metal ions to introduce metal ions into the ion-exchange resin layer (step 2), and treating the ion-exchange resin layer with the introduced metal ions with a solution containing a polymer adsorbed to a metal surface and a reducing agent to reduce the metal ions and precipitate metal particles on the surface of the ion-exchange resin layer (step 3).
[0044] In step 1, an ion exchange resin layer is formed on the surface of a substrate. As the substrate, those described above for the metallic member can be used.
[0045] In step 1, the ion exchange resin layer can be formed, for example, by applying a solution containing an ion exchange resin (hereinafter also referred to as an ion exchange resin solution) to the surface of the substrate and drying to remove the solvent. The application of the ion exchange resin solution to the surface of the substrate is not particularly limited and can be performed by a known application method, for example, a nozzle flow method, a spray method, a dip method, a roll method, a spin method, etc. can be used. In one embodiment, when the roll method is used, a microgravure coater or a doctor knife coater can be used.
[0046] The ion exchange resin solution may be applied to the surface of the substrate under conditions such that an ion exchange resin layer of a desired thickness is formed.
[0047] The ion exchange resin solution applied to the substrate surface may be dried under conditions that allow the solvent to be sufficiently removed, and is usually dried at 10° C. to 120° C. for 0.5 to 4 hours.
[0048] In another embodiment, the ion exchange resin layer can be formed by modifying the surface of the substrate. In this embodiment, a resin film having a group that can be converted into an ion exchange group can be used as the substrate. As such a resin film, a resin having a hydrolyzable functional group and capable of introducing an ion exchange group into the resin film by hydrolysis can be used. As such a resin film, a resin having a group that can be converted into a carboxyl group and / or a sulfo group by hydrolysis can be used, and examples of such a resin film include polycarbonate, acrylic, polyimide, etc., and polyimide having a high functional group density is preferred. When polyimide is used, a polyamic acid (also called polyamic acid) layer having a carboxyl group as an ion exchange group is formed on the surface by hydrolysis. In addition, polystyrene can be used as the resin film, and for example, a layer having a sulfo group can be formed on the surface by sulfonating the surface with concentrated sulfuric acid.
[0049] In step 2, the ion exchange resin layer is treated with a solution containing metal ions (hereinafter also referred to as a metal ion solution). By this treatment, the ion exchange groups of the ion exchange resin layer are replaced with metal ions by ion exchange, and the metal ions are introduced into the ion exchange resin layer. Note that the ion exchange groups do not have to be completely replaced with metal ions, and a part of the ion exchange groups may remain as ion exchange groups.
[0050] The metal ions are not particularly limited and are ions of the metals described above for the metallic component, for example, Ag, Al, Au, Ti, Cr, Mn, Fe, Ni, Cu, Zn, Zr, Nb, Mo, In, Co, and Sn ions. From the viewpoint of having high brightness, Ag, Al, and Cr ions are preferred, and Ag ions are more preferred.
[0051] The metal ion solution may be any solution containing the metal ion. The metal ion solution is not particularly limited, and a salt solution of the metal ion may be used. Examples of the salt include nitrates, sulfates, chlorides, carbonates, acetates, and phosphates.
[0052] The concentration of the metal ion solution is usually 1 mM (mmol / l) to 500 mM, and preferably 50 mM to 150 mM.
[0053] The treatment with the metal ion solution can be carried out, for example, by immersing a substrate having an ion exchange resin layer formed on its surface in the metal ion solution. The treatment conditions with the metal ion solution are that the treatment temperature is preferably 10° C. to 50° C., more preferably 20° C. to 30° C., and the treatment time is preferably 1 minute to 60 minutes, more preferably 15 minutes to 45 minutes.
[0054] In step 3, the ion exchange resin layer into which the metal ions have been introduced is treated with a solution containing a polymer that adsorbs to the metal surface and a reducing agent. This treatment reduces the metal ions to metal, and metal particles are precipitated on the surface of the ion exchange resin layer. The metal ions diffuse to the surface of the ion exchange resin layer where the reducing agent is present and are reduced to metal, so that the resulting metallic component has a substrate, an ion exchange resin layer formed thereon, and a metal particle layer formed thereon. In one embodiment, at least a portion of the surface of the metal particles is coated with a polymer that adsorbs to the metal surface.
[0055] In step 3, by using a polymer that adsorbs to the metal surface together with a reducing agent, metal particles with a high aspect ratio can be oriented vertically with respect to the ion-exchange resin layer and the substrate. In addition, by using a polymer that adsorbs to the metal surface, the polymer covers at least a part of the surface of the metal particles, and the metal particles can be protected by the polymer. Therefore, for example, when a resin layer or the like is provided to protect the metal particles, pretreatment is not necessary, and the number of steps can be reduced.
[0056] The polymer adsorbed to the metal surface is as described above for the metallic member.
[0057] The concentration of the polymer adsorbed to the metal surface in the solution containing the polymer and the reducing agent is 0.1 mM to 500 mM, preferably 0.1 mM to 30 mM. When the concentration of the polymer adsorbed to the metal surface is 0.1 mM or more, the aspect ratio of the metal particles can be controlled within the specific range of the present invention, and the metal film has excellent metallic luster, and when the concentration is 500 mM or less, the metal ions can be reliably reduced to the metal particles.
[0058] The reducing agent is not particularly limited, and examples thereof include phosphoric acid compounds, boron hydride compounds, and hydrazine derivatives. Examples of phosphoric acid compounds include hypophosphorous acid, phosphorous acid, pyrophosphoric acid, and polyphosphoric acid. Examples of boron hydride compounds include methylhexaborane, dimethylamine borane, diethylamine borane, morpholine borane, pyridine amine borane, piperidine borane, ethylenediamine borane, ethylenediamine bisborane, t-butylamine borane, imidazole borane, methoxyethylamine borane, and sodium borohydride. Examples of hydrazine derivatives include hydrazine salts such as hydrazine sulfate and hydrazine hydrochloride, and hydrazine derivatives such as pyrazoles, triazoles, and hydrazides. Among these, examples of pyrazoles include pyrazole derivatives such as 3,5-dimethylpyrazole and 3-methyl-5-pyrazolone in addition to pyrazole. As the triazoles, 4-amino-1,2,4-triazole, 1,2,3-triazole, etc. can be used. As the hydrazides, adipic acid hydrazide, maleic acid hydrazide, carbohydrazide, etc. can be used. The reducing agent is preferably dimethylamine borane (DMAB).
[0059] The concentration of the reducing agent in the solution containing the polymer adsorbed to the metal surface and the reducing agent is 0.01 mM to 10 mM, and preferably 0.1 mM to 5 mM. When the reducing agent concentration is 0.01 mM or more, the adhesion between the metal particles and the ion exchange resin layer is increased, and the durability and abrasion resistance are increased, and when the reducing agent concentration is 10 mM or less, the metal particle layer can be made into a discontinuous film with gaps between the metal particles, so that the metal film has excellent radio wave transmittance.
[0060] The molar concentration ratio of the reducing agent to the polymer (reducing agent:polymer) in a solution containing the polymer and the reducing agent to be adsorbed onto the metal surface is usually 1:0.01 to 1:50000, and preferably 1:0.05 to 1:500.
[0061] Treatment with a solution containing a polymer adsorbed to the metal surface and a reducing agent can be carried out, for example, by immersing a substrate having an ion-exchange resin layer on its surface in this solution. The treatment conditions are that the treatment temperature is usually 10°C to 60°C, preferably 25°C to 50°C, and the treatment time is usually 10 seconds to 60 minutes, preferably 30 seconds to 30 minutes. By adjusting the treatment time and temperature according to the reducing power of the reducing agent, a metal film can be obtained in which there are gaps between the deposited metal particles and the metal particles have a predetermined length.
[0062] The treatment with the solution containing the polymer adsorbed to the metal surface and the reducing agent is preferably carried out while stirring the solution. In this treatment, the inclination θ of the metal particles can be adjusted by changing the stirring speed of the solution. Specifically, when the stirring speed of the solution is high, the particles tend to grow in the direction along the flow, and the inclination θ of the metal particles tends to become smaller. Therefore, the treatment with the solution containing the polymer adsorbed to the metal surface and the reducing agent can be carried out while stirring the solution so that the inclination θ of the metal particles is 60°≦θ≦90°. In one embodiment, when the solution containing the polymer and the reducing agent is stirred using a stirrer, the inclination θ of the metal particles can be 60°≦θ≦90° when the rotation speed is 0 rpm to 1250 rpm (preferably 0 rpm to 500 rpm). In a preferred embodiment, when the solution containing the polymer and the reducing agent is stirred using a stirrer, the inclination θ of the metal particles can be 80°≦θ≦90° when the rotation speed is 0 rpm to 300 rpm. The stirring conditions of the solution can be appropriately selected so as to achieve the desired inclination θ of the metal particles, taking into consideration other processing conditions.
[0063] The method for producing a metallic component of the present invention may further include step 4 of performing heat treatment after step 3. This treatment can convert the ion exchange resin layer into any form. In one embodiment, when the ion exchange resin contains a carboxyl group and / or a sulfo group, these groups are dehydrated by the heat treatment. For example, polyamic acid is converted into polyimide by the heat treatment. The heat treatment temperature is usually 100°C to 300°C.
[0064] The metallic member of the present invention has radio wave transmittance and excellent metallic luster, and therefore can be suitably used as a metallic member for products that require radio wave transmittance. EXAMPLES
[0065] The present invention will be described in more detail below with reference to examples, although the technical scope of the present invention is not limited to these examples.
[0066] Example 1 A surface of a polycarbonate (PC) film (thickness 400 μm, Sumika Acrylic Sales Co., Ltd., Technoloy (registered trademark) C000) was spin-coated with 250 μL of a polyamic acid solution (IST Corporation, Pyre-ML (registered trademark) RC-5019) at 1000 rpm for 15 seconds and then at 3000 rpm for 60 seconds, followed by vacuum drying at 40° C. for 1 hour to form a polyamic acid layer on the surface of the polycarbonate film.
[0067] Silver nitrate (AgNO3) (Nacalai Tesque, 31018-14) was dissolved in pure water to prepare a 100 mM AgNO3 solution. After washing the surface of the film with water, the film was immersed in the AgNO3 solution at room temperature for 30 minutes to introduce Ag ions into the polyamic acid layer by ion exchange.
[0068] Dimethylamine borane (DMAB) (Wako, 028-08401) was dissolved in pure water, and polyvinylpyrrolidone (PVP) with a weight average molecular weight of 10,000 was added to this solution and mixed to prepare a mixed solution of 1.5 mM DMAB and 0.1 mM PVP. A stirrer was placed in the mixed solution of DMAB and PVP, and the mixed solution was stirred at a rotation speed of 200 rpm while the film was immersed in the mixed solution at 30°C for 10 minutes to reduce Ag ions and precipitate Ag particles on the surface of the polyamic acid layer. The film was then washed with water and dried to obtain a metallic part.
[0069] Example 2 A metallic member of Example 2 was obtained in the same manner as in Example 1, except that the PVP concentration in the mixed solution of DMAB and PVP was changed to 1.0 mM.
[0070] Example 3 A metallic member of Example 3 was obtained in the same manner as in Example 1, except that the PVP concentration in the mixed solution of DMAB and PVP was changed to 5.0 mM.
[0071] Example 4 A metallic part of Example 4 was obtained in the same manner as in Example 1, except that the PVP concentration in the mixed solution of DMAB and PVP was changed to 500 mM.
[0072] Example 5 A metallic part of Example 5 was obtained in the same manner as in Example 3, except that the DMAB concentration in the mixed solution of DMAB and PVP was changed to 0.01 mM.
[0073] Example 6 A metallic part of Example 6 was obtained in the same manner as in Example 3, except that the DMAB concentration in the mixed solution of DMAB and PVP was changed to 0.05 mM.
[0074] Example 7 A metallic part of Example 7 was obtained in the same manner as in Example 3, except that the DMAB concentration in the mixed solution of DMAB and PVP was changed to 10 mM.
[0075] Example 8 A metallic member of Example 8 was obtained in the same manner as in Example 3, except that the weight average molecular weight of PVP was changed to 40,000.
[0076] Example 9 A metallic member of Example 9 was obtained in the same manner as in Example 3, except that the weight average molecular weight of PVP was changed to 360,000.
[0077] Example 10 A metallic component of Example 10 was obtained in the same manner as in Example 3, except that the rotation speed of the mixed solution when immersing the film in the mixed solution of DMAB and PVP was changed to 1000 rpm and the inclination θ of the metal particles was changed to 75°.
[0078] Example 11 A metallic part of Example 11 was obtained in the same manner as in Example 3, except that the rotation speed of the mixed solution when immersing the film in the mixed solution of DMAB and PVP was changed to 1250 rpm and the inclination θ of the metal particles was changed to 60°.
[0079] Comparative Example 1 A metallic member of Comparative Example 1 was obtained in the same manner as in Example 1, except that the mixed solution of DMAB and PVP was changed to a DMAB solution.
[0080] Comparative Example 2 A metallic member of Comparative Example 2 was obtained in the same manner as in Example 1, except that the PVP concentration in the mixed solution of DMAB and PVP was changed to 5000 mM.
[0081] Comparative Example 3 A metallic part of Comparative Example 3 was obtained in the same manner as in Example 3, except that the DMAB concentration in the mixed solution of DMAB and PVP was changed to 100 mM.
[0082] Comparative Example 4 A metallic part of Comparative Example 4 was obtained in the same manner as in Example 3, except that the rotation speed of the mixed solution when immersing the film in the mixed solution of DMAB and PVP was changed to 1500 rpm and the inclination θ of the metal particles was changed to 55°.
[0083] The metallic members of Examples 1 to 11 and Comparative Examples 1 to 4 were subjected to the following measurements.
[0084] Color Difference Measurement L*, a*, and b* were measured as follows. Spectral reflectance R(λ) was calculated as the ratio of the spectral radiant flux of wavelength λ reflected from an object to the spectral radiant flux of wavelength λ reflected from a perfect diffuse reflecting surface (JIS Z 8722). The spectrophotometer used was a CMS-35SP manufactured by Murakami Color Research Laboratory, and measurements were performed using the SCI method (specular reflection included).
[0085] The calculated spectral reflectance R(λ) was used to calculate the index values L*, a*, and b* of the CIE1976 (L*, a*, b*) color system defined by the International Commission on Illumination (CIE). Here, the L* value is an index that describes the lightness of a color. A larger L* value indicates a brighter color. The a* value is an index that describes the intensity of a color relative to red and green hues. A larger a* value (positive value) indicates a redder hue, and a smaller a* value (negative value) indicates a greener hue. The b* value is an index that describes the intensity of a color relative to yellow and blue hues. A larger b* value (positive value) indicates a yellower hue, and a smaller b* value (negative value) indicates a bluer hue.
[0086] Measurement of absorption spectrum The absorption spectrum was measured in the visible light region of 380 nm to 780 nm using the formula: absorptivity (%) = 100% - (transmittance (%) + reflectance (%)). The absorption spectrum was measured using a spectrophotometer (Shimadzu Corporation, UV-3600i Plus) with a spectral bandwidth of 2 nm and a wavelength scan speed of 1000 nm / min. The transmittance was measured by placing the spectrophotometer on the opposite side of the light source (through the sample), and the reflectance was measured by placing the spectrophotometer on the light source side.
[0087] Metal particle length a, b The maximum horizontal length a (nm) and maximum vertical length b (nm) of Ag particles were measured using a scanning transmission electron microscope (STEM) as follows: Specifically, an image of the cross section of the metallic component was acquired using a scanning transmission electron microscope (JEM-ARM300F, manufactured by JEOL Ltd.), 100 particles present within a 50,000x field of view were randomly selected, the outer edge of each particle was surrounded by an oval, and the maximum horizontal length a (nm) and maximum vertical length b (nm) were calculated using the image analysis software ImageJ, and the average value was calculated.
[0088] Length of the buried metal particle c The vertical length c of the part where the Ag particles are buried in the polyamic acid layer was measured using a scanning transmission electron microscope (STEM) as follows. The surface of the polyamic acid layer was confirmed from the TEM image of the cross section of the metallic member, and a straight line was drawn passing through both ends of the particle in contact with the surface of the polyamic acid layer. In the TEM image, the polyamic acid layer and the Ag particles have different contrasts, so the surface of the polyamic acid layer can be seen, but if the surface is difficult to find, the boundary can be made clear by adjusting the contrast by image processing or detecting N atoms with EDX. Next, a straight line was drawn passing through the bottom surface of the Ag particle in the polyamic acid layer, and a line was drawn perpendicular (90°) from this straight line to one end of the particle in contact with the surface of the polyamic acid layer, and the length (length c) was measured, and the length was measured in the same way for the other end of the particle. This was performed at random for 50 to 100 points, and the average value was calculated.
[0089] Metal particle inclination θ The angle that the metal particles (Ag particles) make with the bottom surface of the ion exchange resin layer (polyamic acid layer) was measured as the inclination θ of the metal particles. In the same manner as for the lengths a and b of the metal particles, the TEM image of the cross section of the metallic component obtained by STEM was analyzed with ImageJ, 100 particles present within the 50,000x field of view were randomly selected, and the angle between the bottom surface of the polyamic acid layer and the central axis of the particle in the vertical direction was calculated. Here, the central axis of the particle refers to the axis drawn so as to pass through the center of the top and bottom of the particle, and corresponds to the maximum length b of the metal particle in the vertical direction.
[0090] 3D-TEM The cross section of the metallic component was rotated by 1 degree at a time using a scanning transmission electron microscope (Talos F200X, manufactured by Thermo Fisher Scientific), and images were acquired and synthesized to obtain an image.
[0091] Millimeter wave attenuation The millimeter wave attenuation of the metallic component was measured to evaluate its millimeter wave transmittance. The millimeter wave attenuation was determined by measuring the one-way attenuation using a millimeter wave characteristic measuring device with a horn antenna and doubling the measured value. Specifically, the measurement sample was irradiated with millimeter waves from the transmitting horn antenna, and the intensity of the millimeter waves passing through the sample and entering the receiving horn antenna was measured to determine the one-way attenuation. The distance between the transmitting and receiving horn antennas was 95 cm. The sample was installed with an elevation angle of 17° relative to the transmitting horn antenna, and the distance between the sample and the transmitting horn antenna was approximately 40 mm. The measurement was performed at 77 GHz, which is the applicable frequency for automotive millimeter wave radar.
[0092] Fig. 2A shows a TEM image of a cross section of the metallic member of Example 3, and Fig. 2B shows a TEM image of a cross section of the metallic member of Comparative Example 1. Fig. 3 shows a 3D-TEM image of the metallic member of Example 3. As shown in Figs. 2A, 2B and 3, in the metallic member of Example 3, Ag particles with a high aspect ratio compared to the metallic member of Comparative Example 1 were oriented vertically with respect to the polyamic acid layer and the PC film thereunder, and there were gaps between each Ag particle.
[0093] Table 1 shows the manufacturing conditions and evaluation results for the metal conditioning members of Examples 1 to 11 and Comparative Examples 1 to 4. In Table 1, for the millimeter-wave permeability, when the millimeter-wave attenuation amount was 0.2 dB or less for the round trip, it was judged as good (〇), and when it exceeded 0.2 dB, it was judged as bad (×). Also, in Table 1, the judgment was that when the millimeter-wave permeability was good (〇), and all of 75≦L*, -2<a*<2, and -5<b*≦6 were satisfied and the change in hue was sufficiently small, it was judged as good (〇), and when at least one of these was not satisfied, it was judged as bad (×). Note that in Comparative Example 2, since the Ag particle layer was not formed, it was judged as bad.
[0094]
Table 1
[0095] As shown in Table 1, in Comparative Example 1 where PVP was not used, b / a<1.25, the a* value of the metal film was 6.5, the b* value was 8, and the hue was reddish and yellowish, and the metal film did not have the original color and luster of the metal. On the other hand, in Examples 1 to 11 where PVP was used, b / a≧1.25, the change in the hue of the metal film was small, the metal film had the original color and luster of the metal, and had excellent metallic luster. From Comparative Example 1 and Examples 1 to 11, it was shown that in order to obtain a metal film with little change in hue, in the reduction step, it is necessary for the metal particles to have a high aspect ratio satisfying b / a≧1.25 by using PVP adsorbed on the metal surface.
[0096] From Examples 1 to 4 and Comparative Example 2, when the PVP concentration in the mixed solution of DMAB and PVP was 0.1 mM to 500 mM (Examples 1 to 4), Ag ions were surely reduced to Ag particles, but when the PVP concentration was 5000 mM (Comparative Example 2), Ag ions were not reduced to Ag particles and the Ag particle layer was not formed. From Examples 3, 8, and 9, it was shown that in the range of the weight-average molecular weight of PVP from 10000 to 360000, the Ag particles had a high aspect ratio and the metal film had excellent metallic luster.
[0097] Examples 3, 5 to 7 and Comparative Example 3 show that when the DMAB concentration in the mixed solution of DMAB and PVP is 0.01 mM to 10 mM (Examples 3, 5 to 7), the reducing power of the reducing agent is within an appropriate range, so the Ag particle layer forms a discontinuous film and the metallic component has excellent millimeter wave transmittance. However, when the DMAB concentration is 100 mM (Comparative Example 3), the reducing power of the reducing agent is too strong, so the Ag particle layer forms a continuous film and the millimeter wave transmittance of the metallic component deteriorates.
[0098] Examples 3, 10, and 11 and Comparative Example 4 showed that when the inclination θ of the metal particles is in the range of 60° to 90°, the b* value of the metal film is 6 or less, the hue is less yellowish, and the metal retains its original color and luster.
[0099] Figure 4 shows the absorption spectra of the metallic members of Examples 2 and 3 and Comparative Example 1. As shown in Figure 4, in Comparative Example 1, the metal film strongly absorbs light of a specific wavelength (380 nm to 480 nm) in the visible light range, causing a change in the color of the metal film, but the metallic members of Examples 2 and 3 did not have any specific absorption in the visible light range, had little change in the color of the metal film, and retained the original color and luster of the metal. [Explanation of symbols]
[0100] 10: metallic member, 11: substrate, 12: ion exchange resin layer, 13: metal particle, 14: polymer adsorbed to metal surface, a: maximum horizontal length of metal particle (nm), b: maximum vertical length of metal particle (nm), c: vertical length of part of metal particle buried in ion exchange resin layer (nm), θ: inclination of metal particle with respect to bottom surface of ion exchange resin layer (°)
Claims
1. A metallic component having a substrate, an ion exchange resin layer formed on the substrate, and a metal particle layer formed on the ion exchange resin layer, In the metal particle layer, there are gaps between the metal particles, In a cross section of the metallic component, a maximum horizontal length a (nm) of the metal particle, a maximum vertical length b (nm) of the metal particle, and a vertical length c (nm) of a portion of the metal particle embedded in the ion exchange resin layer satisfy 1.5 nm≦a≦200 nm, b / a≧1.25, and c≧0, The inclination θ (°) of the metal particles with respect to the bottom surface of the ion exchange resin layer satisfies 60°≦θ≦90°. Metallic parts.
2. 2. The metallic member according to claim 1, wherein the metal of the metal particles is one or more metals selected from Ag, Al, Au, Ti, Cr, Mn, Fe, Ni, Cu, Zn, Zr, Nb, Mo, In, Co, and Sn.
3. The metallic member according to claim 2 , wherein the metal of the metal particles is Ag.
4. 2. The metallic component according to claim 1, wherein the ion exchange resin of the ion exchange resin layer is a resin having a carboxyl group and / or a sulfo group.
5. The metallic component according to claim 4, wherein the ion exchange resin of the ion exchange resin layer is a polyamic acid.
6. The metallic component according to claim 1 , wherein at least a part of the surface of the metal particle is coated with a polymer that is adsorbed to the metal surface.
7. 7. The metallic component according to claim 6, wherein the polymer adsorbed on the metal surface has a weight average molecular weight of 10,000 to 360,000.
8. 8. The metallic component according to claim 6, wherein the polymer adsorbed to the metal surface is at least one selected from the group consisting of polyvinyl polymers, polyethylene glycol polymers, and polyacrylic acid polymers.
9. A method for producing the metallic component according to claim 1, forming an ion exchange resin layer on a surface of a substrate; treating the ion exchange resin layer with a solution containing metal ions to introduce the metal ions into the ion exchange resin layer; The ion exchange resin layer into which the metal ions have been introduced is treated with a solution containing 0.1 mM to 500 mM of a polymer adsorbed on a metal surface and 0.01 mM to 10 mM of a reducing agent to reduce the metal ions and precipitate metal particles on the surface of the ion exchange resin layer. The method for producing a metallic member includes the steps of:
Citation Information
Patent Citations
Manufacturing method of metallic film and metallic film
CN113445034A
Sensing method and sensing device
JP2007071667A
Metal composite material of electromagnetic wave transparency and method for manufacturing the same
JP2010251899A
Immersion tin-silver plating in the manufacture of electronic devices
JP2013517375A
Electromagnetic wave transmissive metallic sheen member, article using the same and thin metallic film
JP2018069462A