Electrode layer

The electrode layer with specific active material and solid electrolyte configuration addresses the need for lower battery resistance by enhancing ionic conductivity through increased contact area.

JP7582270B2Active Publication Date: 2024-11-13TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022113385
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-07-14
Publication Date
2024-11-13
Estimated Expiration
2042-07-14

AI Technical Summary

Technical Problem

There is a demand for batteries with even lower resistance.

Method used

An electrode layer is designed with an active material having openings on the surface with a diameter of 0.25 μm or less and voids inside, along with a particle size of 0.15 μm or less and a BET specific surface area of 25 m²/g, and a solid electrolyte filling rate of 30% by volume or more, achieved through kneading and heating.

Benefits of technology

The electrode layer reduces battery resistance by increasing the contact area between the active material and the solid electrolyte, thereby improving ionic conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582270000001
    Figure 0007582270000001
Patent Text Reader

Abstract

To provide an electrode layer capable of reducing the resistance of the battery.SOLUTION: The electrode layer is obtained by kneading active material with openings with an opening diameter of 0.25 μm or less on the surface and has a void inside and a solid electrolyte with a particle size of 0.15 μm or less and a BET-specific surface product of 25 m2 / g or more, and heating the same. In the electrode layer, the filling ratio of the solid electrolyte to the active material is 30% by volume or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an electrode layer. [Background technology]

[0002] Patent Document 1 proposes an active material having voids inside primary particles, and the surfaces of the active material in the voids are covered with a sulfide solid electrolyte, and an electrode layer containing the active material. Patent Document 2 proposes a method for producing an electrode for a metal ion battery, which includes the steps of (i) sintering silicon-containing porous particles at a temperature of 500° C. to 1200° C. in an oxygen-free atmosphere, and (ii) disposing the sintered silicon-containing particles obtained from step (i) on a current collector. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-080285 A [Patent Document 2] Special Publication No. 2017-503308 Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, there has been a demand for further reducing the resistance of batteries. An object of the present disclosure is to provide an electrode layer that reduces the resistance of a battery. [Means for solving the problem]

[0005] Means for solving the above problems include the following means. <1> An active material having openings on its surface with a diameter of 0.25 μm or less and voids inside, and a particle diameter of 0.15 μm or less and a BET specific surface area of ​​25 m 2% or more by volume, and a solid electrolyte having a molecular weight of 1.0 or more. Effect of the Invention

[0006] According to the present disclosure, an electrode layer is provided that reduces the resistance of a battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] Hereinafter, an embodiment that is an example of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the invention. Each component may contain multiple types of the corresponding substance.

[0008] <Electrode layer> The electrode layer according to the present disclosure comprises an active material having openings on its surface with a diameter of 0.25 μm or less and voids inside, and a porous material having a particle diameter of 0.15 μm or less and a BET specific surface area of ​​25 m 2 / g or more, and a solid electrolyte having a packing ratio of the solid electrolyte to the active material of 30 volume % or more.

[0009] The electrode layer according to the present disclosure has the above-mentioned configuration and reduces the resistance of the battery. The reason for this is presumed to be as follows. An active material having openings on its surface with a diameter of 0.25 μm or less and voids inside, and a particle diameter of 0.15 μm or less and a BET specific surface area of ​​25 m 2 By kneading and heating the active material with a solid electrolyte having a surface area of ​​100 μm or more and a solid electrolyte having a surface area of ​​100 μm or more, the filling rate of the solid electrolyte relative to the active material becomes 30% by volume or more, thereby increasing the contact area between the active material and the solid electrolyte and improving the ionic conductivity. Therefore, the electrode layer according to the present disclosure reduces the resistance of the battery.

[0010] (active material) The electrode layer according to the present disclosure includes an active material having openings on its surface with a diameter of 0.25 μm or less and having voids inside.

[0011] The active material has openings on its surface, the openings having a diameter of 0.25 μm or less, where the openings are holes that open on the surface of the active material. The opening diameter is measured by a scanning electron microscope (SEM). Specifically, a certain amount of active material is observed by SEM, the diameters (circle equivalent diameters) of the openings on the surface of the active material are measured, and the average value is taken as the opening diameter.

[0012] The particle size of the active material is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 6 μm or less. The particle size of the active material is measured by a scanning electron microscope (SEM). Specifically, the particle size of a certain amount of the active material is measured and the average value is calculated.

[0013] The BET specific surface area of ​​the active material is 0.1 m 2 / g or more 25m 2 / g or less, and 0.5m 2 / g or more 10m 2 / g or less is more preferable, and 0.8m 2 / g or more 5m 2 It is more preferable that the molecular weight is not more than 1 / g. The BET specific surface area of ​​the active material is measured by the method described in

[0036] of JP 2021-166198 A.

[0014] When the active material is used as a positive electrode active material, an oxide active material is used. Examples of oxide active materials include LiCoO2, LiMnO2, LiNiO2, LiVO2, and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, etc., rock salt layered active materials, LiMn2O4, Li(Ni 0.5 Mn 1.5 )O4 and the like, and olivine type active materials such as LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, etc. In addition, a coating layer containing a Li ion conductive oxide may be formed on the surface of the positive electrode active material. When the active material is used as a negative electrode active material, an example of the active material is a Si (silicon)-based active material. Examples of the Si-based active material include simple Si, Si alloys, and Si oxides.

[0015] (solid electrolyte) The electrode layer according to the present disclosure includes a solid electrolyte. The particle size of the solid electrolyte is 0.15 μm or less, preferably 0.13 μm or less, and more preferably 0.12 μm or less. The method for measuring the particle size of the solid electrolyte is the same as the method for measuring the particle size of the active material.

[0016] The BET specific surface area of ​​the solid electrolyte is 25m 2 / g or more, 28m 2 / g or more, and 2 It is more preferable that the molecular weight is 1 / g or more. The BET specific surface area of ​​the solid electrolyte is measured by the same method as that for the BET specific surface area of ​​the active material.

[0017] As the solid electrolyte, for example, a sulfide solid electrolyte can be used. As the sulfide solid electrolyte, for example, a Li2S-P2S5-based sulfide solid electrolyte can be used.

[0018] (Filling rate) In the electrode layer according to the present disclosure, the filling rate of the solid electrolyte relative to the active material is 30% by volume or more, and preferably 35% by volume or more and 90% by volume or less. The filling ratio of the solid electrolyte to the active material is measured using a scanning electron microscope (SEM) as follows. The electrode layer is cut, and five random points on the cut surface of the electrode layer are observed by SEM at a magnification of 5000 times to obtain SEM images. The SEM images are imported into the image processing software ImageJ, and the ratio of the area of ​​the solid electrolyte present in the voids of the primary particles of the active material to the area of ​​the voids contained inside the primary particles of the active material is calculated, and this value is taken as the filling rate of the solid electrolyte relative to the active material.

[0019] (Other Ingredients) The electrode layer according to the present disclosure may contain, as necessary, other components such as a binder (e.g., a rubber-based binder, a fluoride-based binder, etc.) and a conductive assistant (e.g., a fibrous carbon material, etc.) in addition to the active material and the solid electrolyte.

[0020] (Method of manufacturing electrode layer) The electrode layer according to the present disclosure comprises an active material having openings on its surface with a diameter of 0.25 μm or less and voids inside, and a porous material having a particle diameter of 0.15 μm or less and a BET specific surface area of ​​25 m 2 / g or more, and a solid electrolyte, and kneading and heating the mixture. Specifically, it is preferable to obtain an electrode composition by kneading an active material, a solid electrolyte, a dispersant, and other components as necessary, and then apply the electrode composition in the form of a film and heat the film-like electrode composition to produce an electrode layer.

[0021] <All-solid-state battery> The all-solid-state battery according to the present disclosure preferably includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer. The all-solid-state battery further preferably includes a positive electrode current collector that collects current from the positive electrode layer and a negative electrode current collector that collects current from the negative electrode layer. Here, the electrode layer according to the present disclosure is applied to at least one of the positive electrode layer and the negative electrode layer. The all-solid-state battery according to the present disclosure is preferably an all-solid-state lithium battery. EXAMPLES

[0022] Examples will be described below, but the present disclosure is not limited to these examples in any way.

[0023] <Preparation of sulfide solid electrolyte> Li2S and P2S5 were weighed out so that the molar ratio was Li2S:P2S5=75:25 to obtain a raw material composition. This raw material composition and tetrahydrofuran in a mass ratio of 20 times that of the raw material composition were placed in a glass container and stirred at 25°C for 72 hours, and then the precipitate was collected as a precursor of a sulfide solid electrolyte. The collected precursor was dried at 25°C under an argon atmosphere and then fired at 100°C for 1 hour under atmospheric pressure. The obtained fired body was vacuum sealed in a quartz tube, and the quartz tube was placed in a muffle furnace and fired at 140°C for 12 hours to obtain a sulfide solid electrolyte. The obtained sulfide solid electrolyte was pulverized to adjust the particle size, to obtain sulfide solid electrolytes 1 to 3.

[0024] <Preparation of positive electrode> The positive electrode active material has openings on its surface with the opening diameters shown in Table 1, and has voids inside (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 80.0 g of O2), 9.51 g of the sulfide solid electrolyte shown in Table 1, and 2.5 g of VGCF (Showa Denko K.K.) as a conductive assistant were collected in a Filmix container. Then, a solution containing styrene butadiene rubber as a binder (the concentration of the binder in the solution was 5% by mass relative to the entire solution) and 32.21 g of tetralin as a dispersant were added to the Filmix container to obtain a raw material composition for a positive electrode with a solid content concentration of 69% by mass. Filmix was used as a kneading device, and the raw material composition for a positive electrode was kneaded at the peripheral speed shown in Table 1 to obtain an electrode composition for a positive electrode. A high-shear PC wheel was used for the Filmix. The electrode composition for a positive electrode was applied in a film form to the surface of a positive electrode current collector (aluminum foil) by a blade coat method using an applicator, and the film-like electrode composition was heated at 100 ° C. for 30 minutes to obtain a positive electrode having a positive electrode layer on the positive electrode current collector.

[0025] <Preparation of negative electrode> 18.6 g of simple Si as the negative electrode active material, 0.09 g of the first solid electrolyte (i.e., the sulfide solid electrolyte prepared in the above <Preparation of sulfide solid electrolyte>), 8.6 g of the second solid electrolyte (i.e., the sulfide solid electrolyte prepared in the above <Preparation of sulfide solid electrolyte>), a solution containing styrene butadiene rubber as a binder (the binder concentration in the solution is 5% by mass relative to the entire solution), and diisobutyl ketone as a dispersant were added to a Filmix container to obtain a negative electrode raw material composition with a solid concentration of 43% by mass. The Filmix was used as a kneading device, and the negative electrode raw material composition was kneaded at a peripheral speed in the range of 5 m / s to 30 m / s to obtain an electrode composition for a negative electrode. A high-shear PC wheel was used for the Filmix. The electrode composition for the negative electrode was applied in the form of a film to the surface of the negative electrode current collector (nickel foil) by the blade coating method using an applicator, and the film-like electrode composition was heated at 100°C for 30 minutes to obtain a negative electrode having a negative electrode layer on the negative electrode current collector.

[0026] <Preparation of solid electrolyte layer> 40 g of sulfide solid electrolyte (the sulfide solid electrolyte prepared in the above <Preparation of sulfide solid electrolyte> before pulverization), 8.00 g of a solution containing acrylate butadiene rubber and hexane (the concentration of acrylate butadiene rubber in the solution is 5% by mass relative to the entire solution), 25.62 g of heptane, and 8.00 g of dibutyl ether were mixed and kneaded with an ultrasonic homogenizer to obtain a solid electrolyte layer composition. The solid electrolyte layer composition was applied in a film form on the surface of an aluminum foil by a blade coating method using an applicator, and the film-like solid electrolyte layer composition was heated at 100°C for 30 minutes to prepare a solid electrolyte layer.

[0027] <Battery Construction> The positive electrode, solid electrolyte layer, and negative electrode prepared in the above procedure were stacked in this order. Specifically, the solid electrolyte layer was transferred onto the negative electrode layer of the negative electrode at 20 kN, and then the positive electrode was stacked on the solid electrolyte layer at 20 kN so that the positive electrode layer faced the solid electrolyte layer. This laminate was densified at 4 ton / cm and then laminated and sealed to constrain the entire structure with a force of 5 MPa, producing the desired all-solid-state battery.

[0028] <Battery resistance evaluation> Using the fabricated all-solid-state battery, CCCV charging and discharging was performed at 0.1 C with an upper limit voltage of 4.55 V and a lower limit voltage of 2.5 V. The design capacity of the all-solid-state battery was 0.3 Ah. The battery resistance was calculated from the obtained results.

[0029] [Table 1]

[0030] From the above results, it is understood that the all-solid-state battery of this example has low resistance. In addition, "filling rate of the solid electrolyte" in Table 1 means the filling rate of the solid electrolyte relative to the active material.

Claims

[Claim 1] an active material having openings on its surface with a diameter of 0.25 μm or less and having voids inside; The particle size is 0.15 μm or less and the BET specific surface area is 25 m 2 / g or more, and a solid electrolyte, The electrode layer has a packing ratio of the solid electrolyte to the active material of 30 volume % or more.

Citation Information

Patent Citations

  • Positive electrode for battery and method of manufacturing the same

    JP2010251194A

  • Positive electrode active material for lithium ion secondary battery, method for preparing the same, positive electrode sheet for lithium ion secondary battery, and lithium ion secondary battery

    JP2016526262A

  • Electrodes for metal ion batteries

    JP2017503308A

  • Electrode, secondary battery, battery pack and vehicle

    JP2019169252A

  • Active material

    JP2020080285A