Composite coated positive electrode material and preparation method thereof, positive electrode plate, lithium ion battery and electric device
By forming a composite cladding layer on the surface of lithium nickel manganese oxide, the problem of poor circulation performance of nickel lithium manganese oxide is solved, the battery capacity and circulation retention rate are improved, and the impedance growth is reduced.
Patent Information
- Application Number
- CN202411266040.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-29
AI Technical Summary
The poor circulation performance of nickel-manganate materials in lithium-ion batteries limits its further application.
By using composite coating technology, the surface structure and ionic conductivity of the material are enhanced by forming phosphate and aluminum oxide coatings on the surface of lithium nickel manganese oxide, absorbing acidic substances in the electrolyte, and reducing the between positive and negative electrode materials. crosstalk effect.
It significantly improves the capacity and cycle retention rate of the material, reduces the impedance growth in cycles, and improves the cycle performance of the battery.
Smart Images

Figure CN119050320A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a composite-coated positive electrode material and a preparation method thereof, a positive electrode sheet, a lithium-ion battery and an electrical device. Background Art
[0002] Lithium-ion batteries are one of the most widely used rechargeable batteries and are widely used in mobile devices, electric vehicles, energy storage systems and other fields. Positive electrode materials play an important role in the performance, safety and cost of lithium-ion batteries. The theoretical discharge capacity of spinel-structured lithium nickel manganese oxide materials can reach 146.7 mA·h / g, and they have the advantages of high voltage platform, fast three-dimensional lithium ion diffusion channels, and abundant and relatively cheap prices. Therefore, they have become one of the most promising high-voltage positive electrode materials.
[0003] However, lithium nickel manganese oxide materials have the problem of poor cycle performance during application, which limits their further application. Summary of the invention
[0004] Based on this, the present application provides a composite coated positive electrode material and its preparation method, a positive electrode plate, a lithium ion battery and an electrical device to improve the cycle performance of the material.
[0005] The first aspect of the present application provides a composite coated positive electrode material, comprising:
[0006] a core comprising lithium nickel manganese oxide;
[0007] A first coating layer coated on at least a portion of the surface of the core, the first coating layer comprising a first coating material, the first coating material comprising one or more of nickel phosphate, manganese phosphate, lithium phosphate, lithium nickel phosphate and lithium manganese phosphate, the first coating material further comprising aluminum, at least a portion of the aluminum occupies the nickel element position and / or the manganese element position of the crystal structure of the lithium nickel manganese oxide; and
[0008] The second coating layer is coated on at least a portion of the surface of the first coating layer, wherein the second coating layer comprises a second coating material, wherein the second coating material comprises (1) lithium phosphate and (2) at least one of lithium aluminate and aluminum oxide.
[0009] In some embodiments, the first coating material is coated on at least a portion of the surface of the lithium nickel manganese oxide, and the second coating material is coated on at least a portion of the surface of the first coating material.
[0010] In some embodiments, the mass ratio of aluminum element to phosphorus element contained in the first coating material is 3-10; and / or
[0011] The total mass of aluminum and phosphorus elements contained in the first coating material accounts for 0.05% - 0.5% of the mass of the lithium nickel manganese oxide contained in the core; and / or
[0012] The first coating material further contains one or more elements selected from Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb, and Bi.
[0013] In some embodiments, the total mass of aluminum and phosphorus elements contained in the second coating material accounts for 0.2% - 1.5% of the mass of the lithium nickel manganese oxide contained in the core; and / or
[0014] The second coating material further contains one or more elements selected from Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb, and Bi.
[0015] In some embodiments, the chemical formula of the lithium nickel manganese oxide is Li a Ni b Mn c M1 d M2 e O 4-f , where 0.95 ≤ a ≤ 1.1, 0.45 < b < 0.55, 1.4 < c < 1.6, 0 ≤ d + e ≤ 0.1, 0 ≤ f ≤ 0.1, the M1 element includes one or more elements selected from S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, and La, and the M2 element includes one or more elements selected from V, Nb, Mo, W, Ta, B, Sb, and Bi.
[0016] In some embodiments, the composite-coated cathode material has one or more of the following characteristics (1) - (8):
[0017] (1) The volume average particle size Dv50 of the core is 4 μm - 8 μm;
[0018] (2) The specific surface area of the core is 0.3 m 2 / g - 0.7 m 2 / g;
[0019] (3) The specific surface area of the composite-coated cathode material is 0.3 m 2 / g - 0.8 m 2 / g;
[0020] (4) The voltage difference between the two main peaks of the capacity differential curve of the electrochemical distribution curve of the composite-coated cathode material charged at 0.33C > 50 mV;
[0021] (5) The capacity of the 0.33C charging electrochemical distribution curve of the composite coated positive electrode material at the 4.3V to 3.8V platform accounts for 5%-9% of the total discharge capacity.
[0022] (6) The 0.33C discharge capacity of the composite coated positive electrode material is greater than 130 mAh / g;
[0023] (7) The peak intensity ratio coefficient I in the XRD diffraction spectrum of the composite coated positive electrode material 311 2 / (I 400 I 111 )<0.5, where I 311 is the diffraction intensity of the crystal plane (311) in the XRD diffraction pattern, I 400 is the diffraction intensity of the crystal plane (400) in the XRD diffraction pattern, I 111 is the diffraction intensity of the crystal plane (111) in the XRD diffraction pattern;
[0024] (8) The composite coated positive electrode material is single crystal particles and / or quasi-single crystal particles.
[0025] The second aspect of the present application provides a method for preparing a composite coated positive electrode material, comprising the following steps:
[0026] After immersing the kernel in a solution containing a first aluminum source and a first phosphorus source for a preset time, filtering, and subjecting the obtained solid to a first calcination treatment to form a first coating layer on at least a portion of the surface of the kernel to prepare an intermediate; or after mixing the solution containing a first aluminum source and a first phosphorus source with the kernel for a preset time, volatilizing and removing the solvent, and subjecting the remaining solid to a first calcination treatment to form a first coating layer on at least a portion of the surface of the kernel to prepare an intermediate;
[0027] Performing a second calcination treatment on a mixture comprising the intermediate, a second aluminum source, and a second phosphorus source to form a second coating layer on at least a portion of the surface of the first coating layer, thereby preparing the composite coated positive electrode material;
[0028] The core comprises lithium nickel manganese oxide; the first coating layer comprises a first coating material, the first coating material comprises one or more of nickel phosphate, manganese phosphate, lithium phosphate, lithium nickel phosphate and lithium manganese phosphate, the first coating material also comprises aluminum element, at least part of the aluminum element occupies the nickel element position and / or the manganese element position of the crystal structure of the lithium nickel manganese oxide; the second coating layer comprises a second coating material, the second coating material comprises (1) lithium phosphate, and (2) at least one of lithium aluminate and aluminum oxide.
[0029] In some embodiments, the preparation method includes at least one of the following conditions:
[0030] (1) The first aluminum source includes one or more of aluminum nitrate and its hydrate, aluminum dihydrogen phosphate and its hydrate, aluminum lactate and its hydrate, aluminum triethoxide, aluminum orthophosphate and aluminum pyrophosphate; and may be one or more of aluminum nitrate and its hydrate and aluminum triethoxide;
[0031] (2) the first phosphorus source includes one or more of phosphoric acid, ammonium dihydrogen phosphate, ammonium monohydrogen phosphate, phosphorus pentoxide, lithium dihydrogen phosphate, potassium dihydrogen phosphate, manganese dihydrogen phosphate and its hydrate, lithium monohydrogen phosphate, sodium monohydrogen phosphate, potassium monohydrogen phosphate, triethyl phosphate, trimethyl phosphate, aluminum dihydrogen phosphate and pyrophosphate, and can be one or more of phosphoric acid and trimethyl phosphate;
[0032] Optionally, the pyrophosphate includes one or more of lithium pyrophosphate, sodium pyrophosphate, potassium pyrophosphate and aluminum pyrophosphate;
[0033] (3) the solvent used to prepare the solution containing the first aluminum source and the first phosphorus source includes one or more of ethanol, methanol, dimethyl phthalate and water;
[0034] (4) The temperature of the first calcination treatment is 600°C-900°C, the time is 2h-12h, the heating rate is 1°C / min-5°C / min, and the cooling rate is >2°C / min;
[0035] Optionally, the temperature of the first calcination treatment is 700°C-800°C, and the time is 6h-8h;
[0036] (5) the raw materials for the first calcination process further include a first additive, the first additive and the filtered solid are subjected to the first calcination process together, and the first additive includes one or more elements selected from the group consisting of Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb and Bi;
[0037] (6) The voltage difference between the two main peaks of the capacity differential curve of the electrochemical distribution curve of the intermediate at 0.33C charging is greater than 50 mV;
[0038] (7) The second aluminum source includes one or more compounds containing Al-O bonds;
[0039] Optionally, the second aluminum source includes one or more of aluminum hydroxide, aluminum oxide, lithium metaaluminate and sodium aluminate;
[0040] (8) the second phosphorus source includes one or more compounds containing PO bonds;
[0041] Optionally, the second phosphorus source includes one or more of lithium phosphate, lithium monohydrogen phosphate, lithium dihydrogen phosphate, and lithium pyrophosphate;
[0042] (9) The temperature of the second calcination treatment is 200°C - 450°C, the time is 0h - 12h, and the heating rate is 1°C / min - 5°C / min;
[0043] Optionally, the time of the second calcination treatment is 1h - 12h;
[0044] (10) The mixed material for the second calcination treatment further includes a second additive, and the second additive contains one or more elements of Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb, and Bi.
[0045] In some embodiments, the chemical formula of the lithium nickel manganese oxide is Li a Ni b Mn c M1 d M2 e O 4-f , 0.95 ≤ a ≤ 1.1, 0.45 < b < 0.55, 1.4 < c < 1.6, 0 ≤ d + e ≤ 0.1, 0 ≤ f ≤ 0.1, the M1 element includes one or more elements of S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, and La, and the M2 element includes one or more elements of V, Nb, Mo, W, Ta, B, Sb, and Bi.
[0046] In some embodiments, the preparation method of the core includes:
[0047] Mixing the nickel manganese precursor and the lithium salt and then performing a third calcination treatment; or mixing the nickel manganese precursor, the lithium salt, and a third additive and then performing a third calcination treatment;
[0048] Optionally, the chemical formula of the nickel manganese precursor is Ni 0.25 Mn 0.75 (OH) 2 、Ni 0.25 Mn 0.75 C 2 O 4 和Ni 0.25 Mn 0.75 CO 3 中的一种或多种;
[0049] Optionally, the nickel manganese precursor includes one or more of nickel manganese hydroxide, nickel manganese oxalate, and nickel manganese carbonate, and may be nickel manganese hydroxide;
[0050] Optionally, the third additive comprises one or more elements of S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb and Bi;
[0051] Optionally, the lithium source includes LiOH, Li 2 CO 3 , Li 2 SO 4 , LiCl and LiNO 3 One or more of, optionally LiOH and Li 2 CO 3 One or more of;
[0052] Optionally, the molar ratio of the total metal contained in the nickel-manganese precursor to the lithium element contained in the lithium source is 1:(0.5-0.55);
[0053] Optionally, the temperature of the third calcination treatment is 600°C-1000°C, the time is 5h-30h, the heating rate is 1°C / min-5°C / min, and the oxygen partial pressure in the calcination atmosphere is ≥10000Pa;
[0054] Optionally, the temperature of the third calcination treatment is 850°C-950°C and the time is 6h-12h
[0055] Optionally, the voltage difference between two main peaks of the capacity differential curve of the electrochemical distribution curve of the core at 0.33C charge is less than 40 mV or greater than 50 mV.
[0056] The third aspect of the present application provides a positive electrode plate, comprising the composite coated positive electrode material of the first aspect of the present application or the composite coated positive electrode material prepared by the preparation method of the second aspect of the present application.
[0057] The fourth aspect of the present application provides a lithium-ion battery, comprising the positive electrode sheet of the third aspect of the present application.
[0058] The fifth aspect of the present application provides an electrical device, comprising the lithium-ion battery of the fourth aspect of the present application.
[0059] The above-mentioned composite coated positive electrode material includes a composite coating layer composed of a first coating layer and a second coating layer. The aluminum element contained in the coating material of the first coating layer at least partially occupies the nickel element position and / or manganese element position of the crystal structure of the lithium nickel manganese oxide, thereby slightly doping the surface of the lithium nickel manganese oxide and enhancing its surface structure; the phosphate contained in the coating material of the first coating layer forms a phosphate coating on the surface of the inner core, which can ensure a certain ion conductivity while isolating the electrolyte. The lithium phosphate contained in the coating material of the second coating layer can absorb acidic substances in the electrolyte, prevent acidic substances from reacting with the surface of the positive electrode material, and reduce the crosstalk effect between the positive and negative electrode materials; and the lithium aluminate and / or aluminum oxide contained in the coating material of the second coating layer can strongly absorb acidic substances in the electrolyte system. Therefore, the composite coated positive electrode material provided in the present application effectively improves the capacity and cycle retention rate of the material by adopting a composite coating layer, and greatly reduces the impedance growth in the cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0061] Figure 1 This is a scanning electron microscope image of the positive electrode material prepared in Example 1.
[0062] Figure 2 This is a scanning electron microscope image of the positive electrode material prepared in Comparative Example 1. DETAILED DESCRIPTION
[0063] For ease of understanding of the present invention, the application will be described more fully below with reference to relevant embodiments. The following provides preferred embodiments of the application. However, the application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive.
[0064] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0065] The terms "and / or", "or / and", and "and / or" used herein include any one of two or more related listed items, and also include any and all combinations of the related listed items, wherein the any and all combinations include any combination of two related listed items, any more related listed items, or all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in the present application, the technical solution undoubtedly includes technical solutions connected by "logical and", and also undoubtedly includes technical solutions connected by "logical or".
[0066] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0067] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0068] Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and likewise any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.
[0069] The temperature parameters in this application, unless otherwise specified, allow both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0070] In this application, unless otherwise specified, the size, particle size, and diameter generally refer to the average value. In this application, "particle size" and "particle size" have the same definition, both representing the average particle size of a sphere or a spheroid.
[0071] Herein, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc., shall be based on the ability to implement the technical solution of this application, solve the technical problems of this application, and achieve the expected technical effects of this application.
[0072] In the present application, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present application.
[0073] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0074] In the description of the application, "plurality" means at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0075] If there is no special description, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution. If there is no special description, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.
[0076] If there is no special explanation, all the steps of the present application can be performed sequentially or randomly, preferably sequentially.
[0077] The basic chemical formula of the spinel structured lithium nickel manganese oxide material mentioned in this article is LiNi 0.5 Mn 1.5 O 4 (LNMO) is a lithium-ion battery positive electrode material with a spinel structure, which is mainly composed of nickel, manganese, lithium and oxygen elements.
[0078] The spinel structured lithium nickel manganese oxide material is one of the most promising high voltage cathode materials. The inventors found that the lithium nickel manganese oxide material also encountered many problems in further application, such as the dissolution of transition metals, Mn 3+The Jahn-Teller effect caused by the disproportionation of, the irreversible phase change on the surface, and the side reactions with the electrolyte at the interface under high voltage, etc., all limit the further application of lithium nickel manganese oxide positive electrode materials. The intrinsic structural stability of spinel materials is very strong, and the attenuation in the full battery mainly comes from the positive and negative electrode crosstalk caused by the dissolution of metals in the electrolyte. Based on the above problems, the present application uses phosphorus-containing substances and aluminum-containing substances to composite-coat the lithium nickel manganese oxide material. The aluminum-containing substance can be micro-doped on the surface under roasting to enhance the surface structure, and at the same time dispersed on the surface of the particles to absorb hydrofluoric acid decomposed by the electrolyte. The phosphorus-containing substance can form a phosphate coating on the surface, and the phosphate dispersed on the surface can absorb hydrofluoric acid and transition metal ions dissolved in the electrolyte. Through the composite coating, the generation of HF in the electrolyte and the dissolution of transition metals are suppressed, and the crosstalk effect between the positive and negative electrode materials is reduced.
[0079] One or more embodiments of the present application provide a composite coated positive electrode material, comprising a core, a first coating layer coated on at least a portion of the surface of the core, and a second coating layer coated on at least a portion of the surface of the first coating layer; the core comprises lithium nickel manganese oxide, the first coating layer comprises a first coating material, the first coating material comprises one or more of nickel phosphate, manganese phosphate, lithium phosphate, lithium nickel phosphate and lithium manganese phosphate, the first coating material also comprises aluminum element, at least part of the aluminum element occupies the nickel element position and / or manganese element position of the crystal structure of the lithium nickel manganese oxide; the second coating layer comprises a second coating material, the second coating material comprises (1) lithium phosphate, and (2) at least one of lithium aluminate and aluminum oxide.
[0080] It should be noted that the "lithium nickel manganese oxide" and "lithium nickel manganese oxide" in this context are not limited to LiNi 0.5 Mn 1.5 O 4 As long as it is an oxide containing lithium, nickel and manganese, for example, an oxide containing lithium, nickel and manganese doped with other metal elements (such as transition metal elements), it is within the protection scope of this application.
[0081] The "first coating layer", "second coating layer", "first coating material", "second coating material" and the like mentioned in the context are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second" and the like only serve the purpose of non-exhaustive enumeration description, and it should be understood that they do not constitute a closed limitation on quantity. It is understandable that at least part of the aluminum element in the first coating layer occupies the nickel element position and / or manganese element position of the crystal structure of the lithium nickel manganese oxide to form an Al-O bond.
[0082] The composite coated positive electrode material provided in the embodiment of the present application includes a composite coating layer composed of a first coating layer and a second coating layer. The aluminum element contained in the coating material of the first coating layer at least partially occupies the nickel element position and / or manganese element position of the crystal structure of the lithium nickel manganese oxide, thereby slightly doping the surface of the lithium nickel manganese oxide and enhancing its surface structure; the phosphate contained in the coating material of the first coating layer forms a phosphate coating on the surface of the inner core, which can ensure a certain ion conductivity while isolating the electrolyte. The lithium phosphate contained in the coating material of the second coating layer can absorb acidic substances in the electrolyte, prevent acidic substances from reacting with the surface of the positive electrode material, and reduce the crosstalk effect between the positive and negative electrode materials; and the lithium aluminate and / or aluminum oxide contained in the coating material of the second coating layer can strongly absorb acidic substances in the electrolyte system. Therefore, the composite coated positive electrode material provided in the present application effectively improves the capacity and cycle retention rate of the material by adopting a composite coating layer, and greatly reduces the impedance growth in the cycle.
[0083] It is not difficult to understand that the technical solution of the present application does not exclude the situation where the core and / or the first coating layer and / or the second coating layer include other materials, especially the situation where the core further includes other positive electrode materials and / or the first coating layer further includes other coating materials and / or the second coating layer further includes other coating materials.
[0084] It should be noted that the core and / or the first coating layer and / or the second coating layer may further include other materials, but their content should not make them the main component, so as to avoid affecting the coating of the first coating material on the lithium nickel manganese oxide, and the coating of the second coating material on the first coating material.
[0085] In some embodiments, the inner core mainly includes or contains only lithium nickel manganese oxide, the first coating layer mainly includes or contains only a first coating material, and the second coating layer mainly includes or contains only a second coating material.
[0086] In some embodiments, the first coating material of the first coating layer is directly coated on at least a portion of the surface of the lithium nickel manganese oxide of the inner core, and the second coating material of the second coating layer is directly coated on at least a portion of the surface of the first coating material of the first coating layer.
[0087] In some embodiments, the mass ratio of aluminum to phosphorus in the first coating material is 3-10; for example, it may be, but is not limited to, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10 or a range between any two of the above ratios. When the mass ratio of aluminum to phosphorus in the first coating material is within the above range, phosphorus will preferentially combine with lithium, and aluminum will not be combined with phosphorus to form aluminum phosphate, so that aluminum can effectively enter the lattice.
[0088] As a possible implementation, the total mass of aluminum and phosphorus contained in the first coating material accounts for 0.05%-0.5% of the mass of the lithium nickel manganese oxide contained in the core; for example, it can be but not limited to 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5% or a range between any two of the above values. When the content of aluminum and phosphorus in the first coating material is within the above range, it can avoid the corrosion of the surface caused by excessive addition of phosphorus.
[0089] In some optional embodiments, the first coating material also contains one or more elements of Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb and Bi.
[0090] As a possible implementation, the total mass of aluminum and phosphorus contained in the second coating material accounts for 0.2%-1.5% of the mass of the lithium nickel manganese oxide contained in the core; for example, it may be, but is not limited to, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1.0%, 1.05%, 1.1%, 1.15%, 1.2%, 1.25%, 1.3%, 1.35%, 1.4%, 1.45%, 1.5% or the range between any two of the above values. When the content of aluminum and phosphorus in the second coating material is within the above range, it is beneficial for the second coating material to absorb acidic substances in the electrolyte, and at the same time, the surface resistance of the material will not increase or the capacity will not decrease due to the addition of too much inactive substance.
[0091] In some of the embodiments, the second coating material further comprises one or more elements of Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb and Bi.
[0092] In some embodiments, the lithium nickel manganese oxide has a chemical formula of Li a Ni b Mn c M1 d M2 e O 4-f, 0.95 ≤ a ≤ 1.1, 0.45 < b < 0.55, 1.4 < c < 1.6, 0 ≤ d + e ≤ 0.1, 0 ≤ f ≤ 0.1. The M1 element includes one or more elements among S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, and La. The M2 element includes one or more elements among V, Nb, Mo, W, Ta, B, Sb, and Bi.
[0093] Doping with the M1 element is beneficial to improving the stability of the crystal structure of lithium nickel manganese oxide, and doping with the M2 element is beneficial to the crystal growth of lithium nickel manganese oxide into a single crystal or near-single crystal morphology.
[0094] It should be noted that lithium nickel manganese oxide may also contain any possible impurity elements with a mass fraction less than 400 ppm, which are not specifically defined herein.
[0095] In some embodiments, the volume-average particle size Dv50 of the core is 4 μm - 8 μm; for example, it can be, but is not limited to, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, or the range between any two of the above particle sizes, etc. When the volume-average particle size of the core is within the above range, it is beneficial to achieve a better balance between the electrochemical kinetic performance and the electrochemical stability of the material.
[0096] It should be noted that the volume-average particle size Dv50 refers to the particle size corresponding to when the cumulative volume particle size distribution percentage of the sample reaches 50%. It can be measured by a particle size distribution analyzer.
[0097] As a possible embodiment, the specific surface area of the core is 0.3 m 2 / g - 0.7 m 2 / g; for example, it can be, but is not limited to, 0.3 m 2 / g, 0.35 m 2 / g, 0.4 m 2 / g, 0.45 m 2 / g, 0.5 m 2 / g, 0.55 m 2 / g, 0.6 m 2 / g, 0.65 m 2 / g, 0.7 m 2 / g, or the range between any two of the above specific surface areas, etc. When the specific surface area of the core is within the above range, it is beneficial to achieve a better balance between the electrochemical kinetic performance and the electrochemical stability of the material.
[0098] In some exemplary embodiments, the specific surface area of the composite-coated cathode material is 0.3 m 2 / g - 0.8 m 2 / g; for example, it can be, but is not limited to, 0.3 m2 / g, 0.35m 2 / g, 0.4m 2 / g, 0.45m 2 / g, 0.5m 2 / g, 0.55m 2 / g, 0.6m 2 / g, 0.65m 2 / g, 0.7m 2 / g, 0.75m 2 / g, 0.8m 2 / g or the range between any two of the above specific surface areas, etc. When the specific surface area of the composite coated positive electrode material is within the above range, it is beneficial to achieve a better balance between the electrochemical kinetics and electrochemical stability of the material.
[0099] In some embodiments, the voltage difference between the two main peaks of the capacity differential curve of the electrochemical distribution curve of the composite coated positive electrode material at 0.33C charging is greater than 50 mV; thus, the positive electrode material has a well-crystalline structure and a higher electronic conductivity.
[0100] In some embodiments, the capacity of the 0.33C charged electrochemical distribution curve of the composite coated positive electrode material at the 4.3V to 3.8V platform accounts for 5%-9% of the total discharge capacity; for example, it can be but not limited to 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9% or the range between any two of the above values, etc. Thus, the positive electrode material has a higher electronic conductivity and a higher reversible capacity.
[0101] In some embodiments, the 0.33C discharge capacity of the composite coated positive electrode material is greater than 130 mAh / g; thus, the positive electrode material has a relatively high reversible capacity and is suitable for application in various electrochemical energy storage devices.
[0102] As a possible implementation method, the peak intensity ratio coefficient I in the XRD diffraction spectrum of the composite coated positive electrode material is 311 2 / (I 400 I 111 )<0.5, where I 311 is the diffraction intensity of the crystal plane (311) in the XRD diffraction pattern, I 400 is the diffraction intensity of the crystal plane (400) in the XRD diffraction pattern, I 111 is the diffraction intensity of the crystal plane (111) in the XRD diffraction pattern; therefore, the positive electrode material has a lower ion mixing degree and better structural order.
[0103] In some embodiments, the composite coated positive electrode material is a single crystal particle and / or a quasi-single crystal particle. When the positive electrode material is a single crystal particle and / or a quasi-single crystal particle, the positive electrode material has high electrochemical stability and rarely cracks due to volume deformation between grain boundaries.
[0104] It should be noted that the “quasi-single crystal particles” mentioned in this context refer to crystal particles formed by the aggregation of several or dozens of single crystal particles, and the number of their grain boundaries is far less than that of polycrystalline particles.
[0105] One or more embodiments of the present application provide a method for preparing a composite coated positive electrode material, comprising the following steps:
[0106] The inner core is immersed in a solution containing a first aluminum source and a first phosphorus source for a preset time, filtered, and the solid obtained by filtration is subjected to a first calcination treatment to form a first coating layer on at least a portion of the surface of the inner core to prepare an intermediate; a mixed material containing the intermediate, a second aluminum source and a second phosphorus source is subjected to a second calcination treatment to form a second coating layer on at least a portion of the surface of the first coating layer to prepare a composite coated positive electrode material; wherein the inner core comprises lithium nickel manganese oxide; the first coating layer comprises a first coating material, the first coating material comprises one or more of nickel phosphate, manganese phosphate, lithium phosphate, lithium nickel phosphate and lithium manganese phosphate, the first coating material also comprises aluminum element, at least part of the aluminum element occupies the nickel element position and / or manganese element position of the crystal structure of the lithium nickel manganese oxide; the second coating layer comprises a second coating material, the second coating material comprises lithium phosphate and at least one of lithium aluminate and aluminum oxide.
[0107] It should be noted that the "first roasting treatment", "second roasting treatment", "third roasting treatment", "first aluminum source", "second aluminum source", "first phosphorus source", "second phosphorus source" and the like mentioned in the context are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third" and the like only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0108] Understandably, in the preparation method provided by the embodiment of the present application, wet chemistry is used for coating before the first roasting treatment, which greatly enhances the uniformity of the dispersion of the coating material (the first aluminum source and the first phosphorus source) on the surface. When the first roasting treatment is performed, the first aluminum source can be slightly doped on the surface of the lithium nickel manganese oxide under roasting, thereby enhancing its surface structure. During the roasting process, the first phosphorus source can form a phosphate coating on the surface of the kernel, isolating the electrolyte while ensuring a certain ion conductivity. When the second roasting treatment is performed, the second aluminum source and the second phosphorus source are added by dry mixing. After roasting, the phosphate dispersed on the surface of the intermediate can absorb the acidic substances in the electrolyte, prevent the acidic substances from reacting with the surface of the positive electrode material, and reduce the crosstalk effect between the positive and negative electrode materials, and the lithium aluminate and / or aluminum oxide dispersed on the surface of the intermediate can strongly absorb the acidic substances in the electrolyte system. Therefore, the composite coated positive electrode material prepared by the preparation method, by adopting a composite coating layer, effectively improves the capacity and cycle retention rate of the material, and greatly reduces the impedance growth in the cycle.
[0109] It should be noted that the finished product obtained by the above preparation method can also be used as an intermediate for further processing and optimization, and the processing is not limited to adding other additives for further roasting, mixing other positive electrode materials or more other treatments. Further processing optimization can also be added between the above first roasting treatments, and the processing is not limited to adding other additives for further roasting, mixing other positive electrode materials or more other treatments. Further processing optimization can also be added between the above second roasting treatments, and the processing is not limited to adding other additives for further roasting, mixing other positive electrode materials or more other treatments.
[0110] The inner core is immersed in a solution containing the first aluminum source and the first phosphorus source for a preset time and then filtered, which is beneficial for filtering out soluble impurities along with the solvent and improving the purity of the reaction materials.
[0111] In some embodiments, the filtering method includes one or more of centrifugal filtration, pressure filtration and suction filtration.
[0112] One or more embodiments of the present application provide a method for preparing a composite coated positive electrode material, comprising the following steps:
[0113] After mixing a solution containing a first aluminum source and a first phosphorus source with the inner core for a preset time, the solvent is evaporated and removed, and the remaining solid is subjected to a first roasting treatment to form a first coating layer on at least a portion of the surface of the inner core to prepare an intermediate; a mixed material containing the intermediate, a second aluminum source, and a second phosphorus source is subjected to a second roasting treatment to form a second coating layer on at least a portion of the surface of the first coating layer to prepare a composite coated positive electrode material; wherein the inner core contains lithium nickel manganese oxide; the first coating layer contains a first coating material, the first coating material includes one or more of nickel phosphate, manganese phosphate, lithium phosphate, lithium nickel phosphate and lithium manganese phosphate, the first coating material also includes aluminum element, at least part of the aluminum element occupies the nickel element position and / or manganese element position of the crystal structure of the lithium nickel manganese oxide; the second coating layer contains a second coating material, the second coating material includes lithium phosphate and at least one of lithium aluminate and aluminum oxide.
[0114] Understandably, in the preparation method provided by the embodiment of the present application, wet chemistry is used for coating before the first roasting treatment, which greatly enhances the uniformity of the dispersion of the coating material (the first aluminum source and the first phosphorus source) on the surface. When the first roasting treatment is performed, the first aluminum source can be slightly doped on the surface of the lithium nickel manganese oxide under roasting, thereby enhancing its surface structure. During the roasting process, the first phosphorus source can form a phosphate coating on the surface of the kernel, isolating the electrolyte while ensuring a certain ion conductivity. When the second roasting treatment is performed, the second aluminum source and the second phosphorus source are added by dry mixing. After roasting, the phosphate dispersed on the surface of the intermediate can absorb the acidic substances in the electrolyte, prevent the acidic substances from reacting with the surface of the positive electrode material, and reduce the crosstalk effect between the positive and negative electrode materials, and the lithium aluminate and / or aluminum oxide dispersed on the surface of the intermediate can strongly absorb the acidic substances in the electrolyte system. Therefore, the composite coated positive electrode material prepared by the preparation method, by adopting a composite coating layer, effectively improves the capacity and cycle retention rate of the material, and greatly reduces the impedance growth in the cycle.
[0115] It should be noted that the finished product obtained by the above preparation method can also be used as an intermediate for further processing and optimization, and the processing is not limited to adding other additives for further roasting, mixing other positive electrode materials or more other treatments. Further processing optimization can also be added between the above first roasting treatments, and the processing is not limited to adding other additives for further roasting, mixing other positive electrode materials or more other treatments. Further processing optimization can also be added between the above second roasting treatments, and the processing is not limited to adding other additives for further roasting, mixing other positive electrode materials or more other treatments.
[0116] The method of mixing the solution containing the first aluminum source and the first phosphorus source with the inner core may include adding the solution to the inner core under stirring, spraying the solution on the inner core under stirring, or washing the inner core with a flowing solution, which is not specifically limited.
[0117] The composition and properties of lithium nickel manganese oxide, the first coating material and the second coating material, as well as the structure and properties of the core and the prepared positive electrode material are respectively as described above and will not be repeated in the method.
[0118] In some exemplary embodiments, the preset time mentioned in the context may be 30s-300s, for example, but not limited to, 30s, 60s, 120s, 180s, 240s, 300s, or a range between any two of the above times.
[0119] As a possible implementation, the first aluminum source includes one or more of aluminum nitrate and its hydrate, aluminum dihydrogen phosphate and its hydrate, aluminum lactate and its hydrate, aluminum triethoxide, aluminum orthophosphate and aluminum pyrophosphate.
[0120] In some optional embodiments, the first aluminum source includes one or more of aluminum nitrate and its hydrate and aluminum triethoxide.
[0121] In some exemplary embodiments, the first phosphorus source includes one or more of phosphoric acid, ammonium dihydrogen phosphate, ammonium monohydrogen phosphate, phosphorus pentoxide, lithium dihydrogen phosphate, potassium dihydrogen phosphate, manganese dihydrogen phosphate and hydrates thereof, lithium monohydrogen phosphate, sodium monohydrogen phosphate, potassium monohydrogen phosphate, triethyl phosphate, trimethyl phosphate, aluminum dihydrogen phosphate and pyrophosphate.
[0122] In some optional embodiments, the first phosphorus source includes one or more of phosphoric acid and trimethyl phosphate.
[0123] As a possible implementation, the pyrophosphate includes one or more of lithium pyrophosphate, sodium pyrophosphate, potassium pyrophosphate and aluminum pyrophosphate.
[0124] In some embodiments, the solvent used to prepare the solution comprising the first aluminum source and the first phosphorus source includes one or more of ethanol, methanol, dimethyl phthalate, and water.
[0125] In some embodiments, the temperature of the first calcination treatment is 600°C-900°C; for example, it can be but not limited to 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C or a range between any two of the above temperatures.
[0126] In some optional embodiments, the time of the first calcination treatment is 2h-12h; for example, it can be but not limited to 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h or a range between any two of the above times.
[0127] In some optional embodiments, the temperature of the first calcination treatment is 700° C.-800° C., and the time is 6 h-8 h.
[0128] As a possible implementation manner, the heating rate of the first roasting treatment is 1°C / min-5°C / min; for example, it can be but not limited to 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min or a range between any two of the above heating rates.
[0129] It should be noted that the temperature, time and heating rate of the first calcination treatment can be combined in any appropriate manner, and the three can be selected from any temperature, time and heating rate of the first calcination treatment described in this document.
[0130] When the temperature, time and heating rate of the first calcination treatment are respectively within the above ranges, the gas generated by the lithium salt or precursor can be effectively dissipated while ensuring that the temperature rises in a relatively short time.
[0131] In some exemplary embodiments, the cooling rate of the first calcination process is greater than 2° C. / min.
[0132] In some embodiments, the raw materials for the first calcination treatment also include a first additive, and the first additive and the filtered solid are subjected to the first calcination treatment together, and the first additive includes one or more elements of Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb and Bi.
[0133] In some embodiments, the voltage difference between the two main peaks of the capacity differential curve of the electrochemical distribution curve of the intermediate at 0.33C charge is greater than 50 mV; thus, the material has a better crystalline structure and higher electronic conductivity.
[0134] In some embodiments, the second aluminum source includes one or more compounds containing Al—O bonds.
[0135] As a possible implementation, the second aluminum source includes one or more of aluminum hydroxide, aluminum oxide, lithium metaaluminate and sodium aluminate.
[0136] In some embodiments, the second phosphorus source includes one or more compounds containing PO bonds.
[0137] In some optional embodiments, the second phosphorus source includes one or more of lithium phosphate, lithium monohydrogen phosphate, lithium dihydrogen phosphate and lithium pyrophosphate.
[0138] In some embodiments, the temperature of the second calcination treatment is 200°C-450°C; for example, it can be but not limited to 200°C, 250°C, 300°C, 350°C, 400°C, 450°C or a range between any two of the above temperatures.
[0139] As a possible implementation manner, the time of the second roasting treatment is 0h-12h; for example, it can be but not limited to 0h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h or a range between any two of the above times, etc. It should be noted that when the time of the second roasting treatment is 0h, it means that the mixture of the intermediate, the second aluminum source and the second phosphorus source is only mixed without roasting, which also has a certain improvement effect.
[0140] In some optional embodiments, the second calcination treatment time is 1 hour to 12 hours.
[0141] In some exemplary embodiments, the heating rate of the second calcination treatment is 1°C / min-5°C / min; for example, it can be but not limited to 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min or a range between any two of the above heating rates.
[0142] It should be noted that the temperature, time and heating rate of the second calcination treatment can be combined in any appropriate manner, and the three can be selected from any temperature, time and heating rate of the second calcination treatment described in this document.
[0143] When the temperature, time and heating rate of the second calcination treatment are respectively within the above ranges, the coating additive can effectively combine with the material surface without having a negative impact on the electrochemical performance.
[0144] In some optional embodiments, the mixed material subjected to the second calcination treatment further includes a second additive, and the second additive includes one or more elements selected from the group consisting of Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb and Bi.
[0145] In some embodiments, the lithium nickel manganese oxide has a chemical formula of Li a Ni b Mn c M1 d M2 e O 4-f, 0.95 ≤ a ≤ 1.1, 0.45 < b < 0.55, 1.4 < c < 1.6, 0 ≤ d + e ≤ 0.1, 0 ≤ f ≤ 0.1. The M1 element includes one or more elements of S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, and La. The M2 element includes one or more elements of V, Nb, Mo, W, Ta, B, Sb, and Bi.
[0146] In some embodiments, the method for preparing the core includes: mixing a nickel-manganese precursor and a lithium salt and then performing a third calcination treatment; or mixing a nickel-manganese precursor, a lithium salt, and a third additive and then performing a third calcination treatment.
[0147] In some embodiments, the chemical formula of the nickel-manganese precursor is Ni 0.25 Mn 0.75 (OH) 2 、Ni 0.25 Mn 0.75 C 2 O 4 and Ni 0.25 Mn 0.75 CO 3 or more of them.
[0148] In some embodiments, the nickel-manganese precursor includes one or more of nickel-manganese hydroxide, nickel-manganese oxalate, and nickel-manganese carbonate.
[0149] As a possible embodiment, the nickel-manganese precursor is nickel-manganese hydroxide.
[0150] In some embodiments, the third additive contains one or more elements of S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb, and Bi.
[0151] It should be noted that the "first additive", "second additive", "third additive", etc. mentioned in the context are only for descriptive purposes and should not be understood as indicating or implying relative importance or quantity, nor should they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, the "first", "second", "third", etc. only serve the purpose of non-exhaustive enumeration and description and should be understood not to constitute a closed limitation on quantity.
[0152] In some alternative embodiments, the lithium source includes one or more of LiOH, Li 2 CO 3 、Li 2 SO 4 、LiCl and LiNO 3 and may be optionally LiOH and Li 2 CO 3One or more of .
[0153] In some embodiments, the molar ratio of the total metal contained in the nickel manganese precursor to the lithium element contained in the lithium source is 1:(0.5-0.55); for example, it can be but not limited to 1:0.5, 1:0.51, 1:0.52, 1:0.53, 1:0.54, 1:0.55 or a range between any two of the above molar ratios.
[0154] In some optional embodiments, the temperature of the third calcination treatment is 600°C-1000°C; for example, it can be but not limited to 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C or a range between any two of the above temperatures.
[0155] In some optional embodiments, the temperature of the third calcination treatment is 850°C-950°C.
[0156] As a possible implementation manner, the time of the third roasting treatment is 5h-30h; for example, it can be but not limited to 5h, 8h, 10h, 13h, 15h, 18h, 20h, 23h, 25h, 28h, 30h or a range between any two of the above times.
[0157] In some optional embodiments, the third calcination treatment lasts for 6 hours to 12 hours.
[0158] In some exemplary embodiments, the heating rate of the third calcination treatment is 1°C / min-5°C / min; for example, it can be but not limited to 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min or a range between any two of the above heating rates.
[0159] It should be noted that the temperature, time and heating rate of the third calcination treatment can be combined in any appropriate manner, and the three can be selected from any temperature, time and heating rate of the third calcination treatment described in this document.
[0160] In some embodiments, the oxygen partial pressure in the calcination atmosphere of the third calcination process is ≥10000 Pa.
[0161] In some embodiments, the voltage difference between the two main peaks of the capacity differential curve of the electrochemical distribution curve of the core at 0.33C charge is less than 40 mV or greater than 50 mV. Thus, the core of the material has good crystallinity.
[0162] One or more embodiments of the present application provide a positive electrode plate, including the composite-coated positive electrode material provided in the present application or the composite-coated positive electrode material prepared by the preparation method provided in the present application.
[0163] One or more embodiments of the present application provide a lithium-ion battery, comprising the above-mentioned positive electrode plate.
[0164] The lithium-ion battery of the present application comprises the above-mentioned composite coated positive electrode material, has a high capacity and initial efficiency, and has excellent cycle performance.
[0165] One or more embodiments of the present application provide an electrical device, including the above-mentioned lithium-ion battery. The electrical device can be an electric car, an electric bicycle, an electric two-wheeled vehicle, an electric car power system, an energy storage system or a mobile storage device, etc., without limitation.
[0166] The electric device of the present application includes the lithium-ion battery provided by the present application, and thus has at least the same advantages as the lithium-ion battery.
[0167] The technical scheme of the present invention is described in detail below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods for which specific conditions are not specified in the following embodiments are preferably referred to the guidance given in the present invention, and can also be carried out according to the experimental manual or conventional conditions in the art, or according to the conditions recommended by the manufacturer, or with reference to experimental methods known in the art.
[0168] In the following specific embodiments, the measured parameters of raw material components may have slight deviations within the range of weighing accuracy unless otherwise specified. For temperature and time parameters, acceptable deviations caused by instrument test accuracy or operation accuracy are allowed.
[0169] 1. Preparation of positive electrode materials
[0170] Example 1
[0171] Step S1: Ni 0.25 Mn 0.75 (OH) 2 (nickel manganese precursor, Dv50 is 4μm), Li 2 CO 3 (lithium source) according to the molar ratio of 1:0.2625, and then add 1000ppm Y 2 O 3 、1000ppm Al(OH) 3 、1000ppm SiO 2 、500ppm MoO 3 and 500ppm Ta2 O 5 , mixed in a high-speed mixer at a speed of 1000 rpm / min for 40 min, and a mixture was obtained after sufficient mixing. The mixture was calcined at 600°C in an air atmosphere for 4 h, and then the temperature was raised to 950°C and calcined for 10 h to obtain a calcined product, which was crushed, sieved, washed, and dried to obtain the inner core Li 1.013 Ni 0.496 Mn 1.488 Y 0.002 Al 0.007 Si 0.006 Mo 0.001 Ta 0.0005 O 3.983 .
[0172] Step S2, immersing the core into an ethanol solution of aluminum triethoxide (the first aluminum source) and triethyl phosphate (the first phosphorus source), wherein the addition amounts of Al and P elements are 0.2wt% and 0.05wt% respectively based on the mass of the core, and mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying in vacuum at 60°C for 2h, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0173] Step S3, adding aluminum oxide (a second aluminum source) and lithium phosphate (a second phosphorus source) to the intermediate, wherein the addition amounts of Al and P elements are 0.3wt% and 0.2wt% respectively based on the mass of the intermediate, the speed of the high-speed mixer is 700rpm / min, the mixing time is 20min, and after mixing evenly, calcining at 450°C for 6h to obtain a finished nickel manganese oxide lithium positive electrode material.
[0174] Example 2
[0175] The difference between the preparation method of Example 2 and the preparation method of Example 1 is that the temperature of the calcination treatment in step S2 of Example 2 is 750° C., and the other aspects are the same. Step S2 in Example 2 is specifically as follows:
[0176] Step S2, immersing the core into an ethanol solution of aluminum triethoxide (the first aluminum source) and triethyl phosphate (the first phosphorus source), wherein the addition amounts of Al and P elements are 0.2wt% and 0.05wt% respectively based on the mass of the core, and mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying in vacuum at 60°C for 2h, and then adding 0.05wt% TiO 2, placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 750°C for 6 h to obtain an intermediate.
[0177] Example 3
[0178] The difference between the preparation method of Example 3 and the preparation method of Example 1 is that the addition amounts of Al and P elements in step S2 of Example 3 are 0.4wt% and 0.1wt% respectively, and the others are the same. Step S2 of Example 3 is as follows:
[0179] Step S2, immersing the core into an ethanol solution of aluminum triethoxide (the first aluminum source) and triethyl phosphate (the first phosphorus source), wherein the addition amounts of Al and P elements are 0.4wt% and 0.1wt% respectively based on the mass of the core, and mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying in vacuum at 60°C for 2h, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0180] Example 4
[0181] The difference between the preparation method of Example 4 and the preparation method of Example 1 is that the first phosphorus source and the first aluminum source used in step S2 of Example 4 are different, and the other parts are the same. Step S2 of Example 4 is as follows:
[0182] Step S2, immersing the core into an ethanol solution of aluminum dihydrogen phosphate and aluminum nitrate, wherein the addition amounts of Al and P elements are 0.2wt% and 0.05wt% respectively based on the mass of the core, and mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying in vacuum at 60°C for 2h, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0183] Example 5
[0184] The difference between the preparation method of Example 5 and the preparation method of Example 1 is that the temperature of the calcination treatment in step S1 of Example 5 is 940°C; the method of removing the solvent in step S2 of Example 5 is different, and the other steps are the same. Step S1 and step S2 of Example 5 are respectively as follows:
[0185] Step S1: Ni 0.25 Mn0.75 (OH) 2 (nickel manganese precursor, Dv50 is 4μm), Li 2 CO 3 (lithium source) according to the molar ratio of 1:0.2625, and then add 1000ppm Y 2 O 3 、1000ppm Al(OH) 3 、1000ppm SiO 2 、500ppm MoO 3 and 500ppm Ta 2 O 5 , mixed in a high-speed mixer at a speed of 1000 rpm / min for 40 min, and a mixture was obtained after sufficient mixing. The mixture was calcined at 600°C in an air atmosphere for 4 h, and then the temperature was raised to 940°C and calcined for 10 h to obtain a calcined product, which was crushed, sieved, washed with water, and dried to obtain Li 1.015 Ni 0.496 Mn 1.488 Y 0.002 Al 0.007 Si 0.006 Mo 0.001 Ta 0.0005 O 3.989 .
[0186] Step S2, immersing the core into an ethanol solution of aluminum triethoxide (the first aluminum source) and triethyl phosphate (the first phosphorus source), wherein the addition amounts of Al and P elements are 0.2wt% and 0.05wt% respectively based on the mass of the core, mixing for 15 minutes under strong stirring, and volatilizing the ethanol by vacuum drying at 60°C, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0187] Example 6
[0188] The difference between the preparation method of Example 6 and the preparation method of Example 1 is that in step S2 of Example 6, the addition amounts of Al and P elements are 0.4wt% and 0.1wt% respectively, and in step S3 of Example 6, the addition amounts of Al and P elements are 0.6wt% and 0.4wt% respectively, and the others are the same. Step S2 and step S3 of Example 6 are respectively as follows:
[0189] Step S2, immersing the core into an ethanol solution of aluminum triethoxide (the first aluminum source) and triethyl phosphate (the first phosphorus source), wherein the addition amounts of Al and P elements are 0.4wt% and 0.1wt% respectively based on the mass of the core, and mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying in vacuum at 60°C for 2h, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0190] Step S3, adding aluminum oxide (a second aluminum source) and lithium phosphate (a second phosphorus source) to the intermediate, wherein the addition amounts of Al and P elements are 0.6wt% and 0.4wt% respectively based on the mass of the intermediate, the speed of the high-speed mixer is 700rpm / min, the mixing time is 20min, and after mixing evenly, calcining at 450°C for 6h to obtain a finished nickel manganese oxide positive electrode material.
[0191] Example 7
[0192] The difference between the preparation method of Example 7 and the preparation method of Example 1 is that the molar ratio of the nickel-manganese precursor and the lithium source in step S1 of Example 7 is different, and the type of additive is different, and the other parts are the same. Step S1 of Example 7 is as follows:
[0193] Step S1: Ni 0.25 Mn 0.75 (OH) 2 (nickel manganese precursor, Dv50 is 4μm), Li 2 CO 3 (lithium source) were mixed in a molar ratio of 1:0.265, and then 2000ppm ZrO was added based on the mass of the final core. 2 , 1000 ppm TiO 2 、1000ppmLa 2 O 3 , 500 ppm WO 3 and 500 ppm B 2 O 3 , mixed in a high-speed mixer at a speed of 1000 rpm / min for 40 min, and a mixture was obtained after sufficient mixing. The mixture was calcined at 600°C in an air atmosphere for 4 h, and then the temperature was raised to 950°C and calcined for 10 h to obtain a calcined product, which was crushed, sieved, washed, and dried to obtain the inner core Li 1.011 Ni 0.496 Mn 1.488 Zr 0.004 Ti0.004 La 0.001 W 0.0005 B 0.008 O 3.982 .
[0194] Example 8
[0195] The difference between the preparation method of Example 8 and the preparation method of Example 7 is that the temperature of the calcination treatment in step S2 of Example 8 is different, and the other steps are the same. Step S1 and step S2 of Example 8 are respectively as follows:
[0196] Step S2, immersing the core into an ethanol solution of aluminum triethoxide (the first aluminum source) and triethyl phosphate (the first phosphorus source), wherein the addition amounts of Al and P elements are 0.2wt% and 0.05wt% respectively based on the mass of the core, and mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying in vacuum at 60°C for 2h, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 750°C for 6 h to obtain an intermediate.
[0197] Example 9
[0198] The difference between the preparation method of Example 9 and the preparation method of Example 7 is that in step S2 of Example 9, the addition amounts of Al and P elements are 0.4wt% and 0.1wt% respectively, and the others are the same. Step S2 of Example 9 is specifically as follows:
[0199] Step S2, immersing the core into an ethanol solution of aluminum triethoxide (the first aluminum source) and triethyl phosphate (the first phosphorus source), wherein the addition amounts of Al and P elements are 0.4wt% and 0.1wt% respectively based on the mass of the core, and mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying in vacuum at 60°C for 2h, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0200] Example 10
[0201] The difference between the preparation method of Example 10 and the preparation method of Example 7 is that the types of the first phosphorus source and the first aluminum source used in step S2 of Example 10 are different, and the other parts are the same. Step S2 of Example 10 is as follows:
[0202] Step S2, immersing the core into an ethanol solution of aluminum dihydrogen phosphate and aluminum nitrate, wherein the addition amounts of Al and P elements are 0.2wt% and 0.05wt% respectively based on the mass of the core, and mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying in vacuum at 60°C for 2h, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0203] Embodiment 11
[0204] The difference between the preparation method of Example 11 and the preparation method of Example 7 is that the method of removing the solvent in step S2 of Example 11 is different, and the other methods are the same. Step S2 of Example 11 is as follows:
[0205] Step S2, immersing the core into an ethanol solution of aluminum triethoxide (the first aluminum source) and triethyl phosphate (the first phosphorus source), wherein the addition amounts of Al and P elements are 0.2wt% and 0.05wt% respectively based on the mass of the core, mixing for 15 minutes under strong stirring, and volatilizing the ethanol by vacuum drying at 60°C, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0206] Example 12
[0207] The difference between the preparation method of Example 12 and the preparation method of Example 7 is that in step S2 of Example 12, the addition amounts of Al and P elements are 0.4wt% and 0.1wt% respectively, and in step S3 of Example 12, the addition amounts of Al and P elements are 0.6wt% and 0.4wt% respectively, and the others are the same. Step S2 and step S3 of Example 12 are respectively as follows:
[0208] Step S2, immersing the core into an ethanol solution of aluminum triethoxide (the first aluminum source) and triethyl phosphate (the first phosphorus source), wherein the addition amounts of Al and P elements are 0.4wt% and 0.1wt% respectively based on the mass of the core, and mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying in vacuum at 60°C for 2h, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0209] Step S3, adding aluminum oxide (a second aluminum source) and lithium phosphate (a second phosphorus source) to the intermediate, wherein the addition amounts of Al and P elements are 0.6wt% and 0.4wt% respectively based on the mass of the intermediate, the speed of the high-speed mixer is 700rpm / min, the mixing time is 20min, and after mixing evenly, calcining at 450°C for 6h to obtain a finished nickel manganese oxide positive electrode material.
[0210] Embodiment 13
[0211] The difference between the preparation method of Example 13 and the preparation method of Example 1 is that no additive is added when preparing the kernel in step S1 of Example 13, and the other steps are the same. Step S1 of Example 13 is as follows:
[0212] Step S1: Ni 0.25 Mn 0.75 (OH) 2 (nickel manganese precursor, Dv50 is 4μm), Li 2 CO 3 (lithium source) were mixed in a molar ratio of 1:0.2625, placed in a high-speed mixer for mixing, the speed of the high-speed mixer was 1000 rpm / min, the mixing time was 40 min, and the mixture was fully mixed to obtain a mixture. The mixture was placed in an air atmosphere and roasted at 600 ° C for 4 h, and then the temperature was increased to 950 ° C and roasted for 10 h to obtain a roasted product, and the roasted product was crushed, sieved, washed with water, and dried to obtain Li 1.016 Ni 0.5 Mn 1.5 O 3.991
[0213] Comparative Example 1
[0214] The difference between the preparation method of comparative example 1 and the preparation method of embodiment 1 is that in comparative example 1, no phosphorus source and aluminum source are used to prepare the coating layer. The specific steps of comparative example 1 are as follows:
[0215] Step S1: Ni 0.25 Mn 0.75 (OH) 2 (nickel manganese precursor, Dv50 is 4μm), Li 2 CO 3 (lithium source) according to the molar ratio of 1:0.2625, and then add 1000ppm Y 2 O 3 、1000ppm Al(OH) 3 、1000ppm SiO 2 、500ppm MoO 3 and 500ppm Ta2 O 5 , mixed in a high-speed mixer at a speed of 1000 rpm / min for 40 min, and a mixture was obtained after sufficient mixing. The mixture was calcined at 600°C in an air atmosphere for 4 h, and then the temperature was raised to 950°C and calcined for 10 h to obtain a calcined product, which was crushed, sieved, washed with water, and dried to obtain Li 1.013 Ni 0.496 Mn 1.488 Y 0.002 Al 0.007 Si 0.006 Mo 0.001 Ta 0.0005 O 3.983 .
[0216] Step S2: Add 0.05 wt% TiO to the core based on the core mass. 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0217] Step S3, calcining the intermediate at 450° C. for 6 hours to obtain a finished positive electrode material.
[0218] Comparative Example 2
[0219] The difference between the preparation method of Comparative Example 2 and the preparation method of Example 1 is that the first phosphorus source and the first aluminum source are not used in the coating in step S2 of Comparative Example 2, and the other parts are the same. The specific details of Comparative Example 2 are as follows:
[0220] Step S1: Ni 0.25 Mn 0.75 (OH) 2 (nickel manganese precursor, Dv50 is 4μm), Li 2 CO 3 (lithium source) according to the molar ratio of 1:0.2625, and then add 1000ppm Y 2 O 3 、1000ppm Al(OH) 3 、1000ppm SiO 2 、500ppm MoO 3 and 500ppm Ta 2 O 5, mixed in a high-speed mixer at a speed of 1000 rpm / min for 40 min, and a mixture was obtained after sufficient mixing. The mixture was calcined at 600°C in an air atmosphere for 4 h, and then the temperature was raised to 950°C and calcined for 10 h to obtain a calcined product, which was crushed, sieved, washed with water, and dried to obtain Li 1.013 Ni 0.496 Mn 1.488 Y 0.002 Al 0.007 Si 0.006 Mo 0.001 Ta 0.0005 O 3.983 .
[0221] Step S2: Add 0.05 wt% TiO to the core based on the core mass. 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0222] Step S3, adding aluminum oxide (a second aluminum source) and lithium phosphate (a second phosphorus source) to the intermediate, wherein the addition amounts of Al and P elements are 0.3wt% and 0.2wt% respectively based on the mass of the intermediate, the speed of the high-speed mixer is 700rpm / min, the mixing time is 20min, and after mixing evenly, calcining at 450°C for 6h to obtain a finished positive electrode material.
[0223] Comparative Example 3
[0224] The difference between the preparation method of Comparative Example 3 and the preparation method of Example 1 is that the second phosphorus source and the second aluminum source are not used in the coating in step S3 of Comparative Example 3, and the other parts are the same. The specific details of Comparative Example 3 are as follows:
[0225] Step S1: Ni 0.25 Mn 0.75 (OH) 2 (nickel manganese precursor, Dv50 is 4μm), Li 2 CO 3 (lithium source) according to the molar ratio of 1:0.2625, and then add 1000ppm Y 2 O 3 、1000ppm Al(OH) 3 、1000ppm SiO 2 、500ppm MoO 3 and 500ppm Ta 2 O 5, mixed in a high-speed mixer at a speed of 1000 rpm / min for 40 min, and a mixture was obtained after sufficient mixing. The mixture was calcined at 600°C in an air atmosphere for 4 h, and then the temperature was raised to 950°C and calcined for 10 h to obtain a calcined product, which was crushed, sieved, washed with water, and dried to obtain Li 1.013 Ni 0.496 Mn 1.488 Y 0.002 Al 0.007 Si 0.006 Mo 0.001 Ta 0.0005 O 3.983 .
[0226] Step S2, immersing the core into an ethanol solution of aluminum triethoxide (the first aluminum source) and triethyl phosphate (the first phosphorus source), wherein the addition amounts of Al and P elements are 0.2wt% and 0.05wt% respectively based on the mass of the core, and mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying in vacuum at 60°C for 2h, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0227] Step S3, calcining the intermediate at 450° C. for 6 hours to obtain a finished positive electrode material.
[0228] Comparative Example 4
[0229] The difference between the preparation method of Comparative Example 4 and the preparation method of Example 1 is that the first phosphorus source is not used in the coating in step S2 of Comparative Example 4, and the other steps are the same. Step S2 of Comparative Example 4 is specifically as follows:
[0230] Step S2, immersing the core into an ethanol solution of triethoxide aluminum (the first aluminum source), wherein the amount of Al element added is 0.25wt% based on the mass of the core, mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying in vacuum at 60°C for 2h, then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0231] Comparative Example 5
[0232] The difference between the preparation method of Comparative Example 5 and the preparation method of Example 1 is that the first aluminum source is not used in the coating in step S2 of Comparative Example 5, and the other steps are the same. Step S2 of Comparative Example 5 is specifically as follows:
[0233] Step S2, immersing the core into an ethanol solution of triethyl phosphate (the first phosphorus source), wherein the amount of P element added is 0.25wt% based on the mass of the core, mixing for 15min under strong stirring, separating the solid powder by centrifugal filtration, and drying at 60°C in vacuum for 2h, and then adding 0.05wt% TiO 2 , placed in a high-speed mixer for mixing, the speed of the high-speed mixer is 700 rpm / min, the mixing time is 20 min, after mixing evenly, calcined at 700° C. for 6 h to obtain an intermediate.
[0234] Comparative Example 6
[0235] The difference between the preparation method of Comparative Example 6 and the preparation method of Example 1 is that the second aluminum source is not used in the coating in step S3 of Comparative Example 6, and the other steps are the same. The specific steps S3 of Comparative Example 6 are as follows:
[0236] Step S3, adding lithium phosphate (second phosphorus source) to the intermediate, wherein the amount of P element added is 0.5wt% based on the mass of the intermediate, the speed of the high-speed mixer is 700rpm / min, the mixing time is 20min, and after mixing evenly, calcining at 450°C for 6h to obtain a finished positive electrode material.
[0237] Comparative Example 7
[0238] The difference between the preparation method of Comparative Example 7 and the preparation method of Example 1 is that the second phosphorus source is not used in the coating in step S3 of Comparative Example 7, and the other steps are the same. Step S3 of Comparative Example 6 is as follows:
[0239] Step S3, adding aluminum oxide (second aluminum source) to the intermediate, wherein the amount of Al element added is 0.5wt% based on the mass of the intermediate, the speed of the high-speed mixer is 700rpm / min, the mixing time is 20min, and after mixing evenly, calcining at 550°C for 6h to obtain a finished positive electrode material.
[0240] Comparative Example 8
[0241] The difference between the preparation method of Comparative Example 8 and the preparation method of Example 1 is that the wet chemical coating is not used in the coating in step S2 of Comparative Example 8, and the other parts are the same. Step S2 of Comparative Example 8 is as follows:
[0242] Step S2: adding aluminum triethoxide (the first aluminum source), triethyl phosphate (the first phosphorus source) and TiO 2, based on the mass of the core, the addition amounts of Al and P are 0.2wt% and 0.05wt%, respectively, and TiO 2 The addition amount is 0.05wt%, and the mixture is placed in a high-speed mixer for mixing. The speed of the high-speed mixer is 700rpm / min, and the mixing time is 20min. After mixing evenly, the mixture is calcined at 700℃ for 6h to obtain an intermediate.
[0243] Comparative Example 9
[0244] Ni 0.25 Mn 0.75 (OH) 2 (nickel manganese precursor, Dv50 is 4μm), Li 2 CO 3 (lithium source) according to the molar ratio of 1:0.2625, and then add 1000ppm Y 2 O 3 、1000ppm Al(OH) 3 、1000ppmSiO 2 、500ppm MoO 3 and 500ppm Ta 2 O 5 , mixed in a high-speed mixer at a speed of 1000 rpm / min for 40 min, and a mixture was obtained after sufficient mixing. The mixture was calcined at 600°C in an air atmosphere for 4 h, and then the temperature was raised to 950°C and calcined for 10 h to obtain a calcined product, which was crushed, sieved, washed with water, and dried to obtain Li 1.013 Ni 0.496 Mn 1.488 Y 0.002 Al 0.007 Si 0.006 Mo 0.001 Ta 0.0005 O 3.983 .
[0245] The specific surface areas of the positive electrode materials prepared in the above-mentioned embodiments and comparative examples were tested by gas adsorption method. The results are shown in Table 1.
[0246] The positive electrode materials prepared in Example 1 and Comparative Example 1 were observed using a scanning electron microscope. The scanning electron microscope images (SEM images) of the positive electrode materials in Example 1 and Comparative Example 1 were as follows: Figure 1 and Figure 2 shown.
[0247] 2. Battery performance test
[0248] The positive electrode material prepared in Example 1 was mixed with acetylene black and polyvinylidene fluoride in a mass ratio of 90:5:5, and N-methylpyrrolidone was added as a dispersant to grind into a slurry; then the slurry was evenly coated on one side of the aluminum foil, vacuum dried at 120°C for 10 hours, and the dried electrode was rolled with a roller machine. The aluminum foil was cut with a slicer to form a circular electrode with a diameter of 1.2 cm. The loading amount of the active material was controlled at 12 mg / cm 2 The liquid battery was assembled in an argon atmosphere glove box, with a lithium sheet with a diameter of 1.5 cm as the negative electrode, a 12 μm PP / PE film as the separator, and 10 μL of 1 mol / L LiPF added to the interface between the positive electrode sheet, the lithium negative electrode and the electrolyte. 6 The electrolyte is assembled in an environment where the water partial pressure is ≤0.1ppm and the oxygen partial pressure is ≤0.1ppm. The specification is CR2032 button cell.
[0249] The preparation methods of button cells in Examples 2-13 and Comparative Examples 1-9 are the same as those in Example 1.
[0250] The button-type batteries prepared in the above-mentioned embodiments and comparative examples were subjected to metal dissolution test, capacity test and cycle performance test respectively, and the test conditions were LR 2032.
[0251] The cycle performance test method is: at 45°C, charge the button battery at 1C and discharge at 1C for 50 cycles with a voltage range of 3.5V-4.9V.
[0252] The capacity test method is: at 25°C, charge the button battery at 0.33C and discharge at 0.33C for 1 week, with a voltage range of 3.5V-4.9V.
[0253] Metal dissolution test: The metal content in the electrolyte was measured by ICP after standing at 60°C and 4.9V for 7 days.
[0254] The test results of the above embodiments and comparative examples are shown in Table 1.
[0255] Table 1
[0256]
[0257] From the comparison of the results of Example 1-13 and Comparative Example 1-9, it can be seen that compared with Comparative Example 1-9, Example 1-13 has a higher discharge specific capacity and cycle capacity retention rate as a whole, and the total metal dissolution amount is lower. It shows that the composite coating layer of the positive electrode material provided in the present application can effectively adsorb the transition metal ions dissolved in the electrolyte and reduce the crosstalk effect between the positive and negative electrode materials; the positive electrode material of the present application effectively improves the capacity and cycle retention rate of the material by adopting the composite coating layer, and greatly reduces the impedance growth in the cycle.
[0258] By comparing the results of Example 1 and Comparative Example 1 in Table 1 and Figure 1-2 It can be seen that the positive electrode material prepared in comparative example 1 shows no coating, and after the composite coating layer containing Al and P is formed on the surface of the positive electrode material prepared in example 1, the capacity increases significantly, the first coulomb efficiency increases, the capacity retention rate increases significantly, and the metal dissolution amount decreases significantly. This shows that the composite coating has a good effect of increasing capacity, inhibiting cycle attenuation, and inhibiting transition metal dissolution.
[0259] From the comparison of the results of Example 1 and Comparative Examples 1-7, it can be seen that compared with Comparative Examples 1-7, the capacity and cycle retention rate in Example 1 are greatly improved, and the metal dissolution amount is greatly reduced; this shows that by composite coating the lithium nickel manganese oxide, and each coating layer contains aluminum and phosphorus, the composite coating has a good effect of improving capacity, inhibiting cycle attenuation and inhibiting transition metal dissolution.
[0260] By comparing the results of Example 1 and Comparative Example 8, it can be seen that in step S2 of the preparation method provided in the present application, wet chemical coating is performed before calcination, which can greatly enhance the dispersion uniformity of the coating material (phosphorus source and aluminum source) on the surface of the inner core, thereby further improving the performance of the obtained positive electrode material.
[0261] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0262] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A composite coated positive electrode material, characterized in that: include: a core comprising lithium nickel manganese oxide; A first coating layer coated on at least a portion of the surface of the core, the first coating layer comprising a first coating material, the first coating material comprising one or more of nickel phosphate, manganese phosphate, lithium phosphate, lithium nickel phosphate and lithium manganese phosphate, the first coating material further comprising aluminum, at least a portion of the aluminum occupies the nickel element position and / or the manganese element position of the crystal structure of the lithium nickel manganese oxide; and The second coating layer is coated on at least a portion of the surface of the first coating layer, and the second coating layer comprises a second coating material, and the second coating material comprises lithium phosphate and at least one of lithium aluminate and aluminum oxide.
2. The composite coated positive electrode material according to claim 1, characterized in that: The mass ratio of aluminum element to phosphorus element contained in the first coating material is 3-10; and / or The total mass of the aluminum element and the phosphorus element contained in the first coating material accounts for 0.05%-0.5% of the mass of the lithium nickel manganese oxide contained in the core; and / or The first coating material also contains one or more elements of Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb and Bi.
3. The composite coated positive electrode material according to claim 1, characterized in that: The total mass of the aluminum element and the phosphorus element contained in the second coating material accounts for 0.2%-1.5% of the mass of the lithium nickel manganese oxide contained in the core; and / or The second coating material also contains one or more elements of Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb and Bi.
4. The composite coated positive electrode material according to any one of claims 1 to 3, characterized in that: The composite coated positive electrode material has one or more of the following characteristics (1)-(10): (1) The first coating material is coated on at least a portion of the surface of the lithium nickel manganese oxide, and the second coating material is coated on at least a portion of the surface of the first coating material; (2) The chemical formula of the lithium nickel manganese oxide is Li a Ni b Mn c M1 d M2 e O 4-f , 0.95 ≤ a ≤ 1.1, 0.45 < b < 0.55, 1.4 < c < 1.6, 0 ≤ d + e ≤ 0.1, 0 ≤ f ≤ 0.1, the M1 element includes one or more elements of S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F and La; the M2 element includes one or more elements of V, Nb, Mo, W, Ta, B, Sb and Bi; (3) The volume average particle size Dv50 of the core is 4 μm-8 μm; (4) The specific surface area of the inner core is 0.3 m 2 / g-0.7m 2 / g; (5) The specific surface area of the composite coated positive electrode material is 0.3 m 2 / g-0.8m 2 / g; (6) The voltage difference between the two main peaks of the capacity differential curve of the electrochemical distribution curve of the composite coated positive electrode material at 0.33C charging is greater than 50 mV; (7) The capacity of the 0.33C charging electrochemical distribution curve of the composite coated positive electrode material at the 4.3V to 3.8V platform accounts for 5% to 9% of the total discharge capacity; (8) The 0.33C discharge capacity of the composite coated positive electrode material is greater than 130 mAh / g; (9) The peak intensity ratio coefficient I in the XRD diffraction spectrum of the composite coated positive electrode material 311 2 / (I 400 I 111 )<0.5, where I 311 is the diffraction intensity of the crystal plane (311) in the XRD diffraction pattern, I 400 is the diffraction intensity of the crystal plane (400) in the XRD diffraction pattern, I 111 is the diffraction intensity of the crystal plane (111) in the XRD diffraction pattern; (10) The composite coated positive electrode material is a single crystal particle and / or a quasi-single crystal particle.
5. A method for preparing a composite coated positive electrode material, characterized in that: The following steps are involved: After immersing the core in a solution containing a first aluminum source and a first phosphorus source for a preset time, filtering, and subjecting the filtered solid to a first calcination treatment to form a first coating layer on at least a portion of the surface of the core to prepare an intermediate; Alternatively, after mixing a solution containing a first aluminum source and a first phosphorus source with the inner core for a preset time, the solvent is volatilized and removed, and the remaining solid is subjected to a first calcination treatment to form a first coating layer on at least a portion of the surface of the inner core to prepare an intermediate; Performing a second calcination treatment on a mixture comprising the intermediate, a second aluminum source, and a second phosphorus source to form a second coating layer on at least a portion of the surface of the first coating layer, thereby preparing the composite coated positive electrode material; Wherein, the core comprises lithium nickel manganese oxide; the first coating layer comprises a first coating material, the first coating material comprises one or more of nickel phosphate, manganese phosphate, lithium phosphate, lithium nickel phosphate and lithium manganese phosphate, the first coating material also comprises aluminum element, at least part of the aluminum element occupies the nickel element position and / or manganese element position of the crystal structure of the lithium nickel manganese oxide; the second coating layer comprises a second coating material, the second coating material comprises lithium phosphate and at least one of lithium aluminate and aluminum oxide.
6. The preparation method according to claim 5, characterized in that: The preparation method comprises at least one of the following conditions: (1) The first aluminum source includes one or more of aluminum nitrate and its hydrate, aluminum dihydrogen phosphate and its hydrate, aluminum lactate and its hydrate, aluminum triethoxide, aluminum orthophosphate and aluminum pyrophosphate; and may be one or more of aluminum nitrate and its hydrate and aluminum triethoxide; (2) the first phosphorus source includes one or more of phosphoric acid, ammonium dihydrogen phosphate, ammonium monohydrogen phosphate, phosphorus pentoxide, lithium dihydrogen phosphate, potassium dihydrogen phosphate, manganese dihydrogen phosphate and its hydrate, lithium monohydrogen phosphate, sodium monohydrogen phosphate, potassium monohydrogen phosphate, triethyl phosphate, trimethyl phosphate, aluminum dihydrogen phosphate and pyrophosphate, and can be one or more of phosphoric acid and trimethyl phosphate; Optionally, the pyrophosphate includes one or more of lithium pyrophosphate, sodium pyrophosphate, potassium pyrophosphate and aluminum pyrophosphate; (3) the solvent used to prepare the solution containing the first aluminum source and the first phosphorus source includes one or more of ethanol, methanol, dimethyl phthalate and water; (4) The temperature of the first calcination treatment is 600°C-900°C, the time is 2h-12h, the heating rate is 1°C / min-5°C / min, and the cooling rate is >2°C / min; Optionally, the temperature of the first calcination treatment is 700°C-800°C, and the time is 6h-8h; (5) the raw materials for the first calcination process further include a first additive, the first additive and the filtered solid are subjected to the first calcination process together, and the first additive includes one or more elements selected from the group consisting of Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb and Bi; (6) The voltage difference between the two main peaks of the capacity differential curve of the electrochemical distribution curve of the intermediate at 0.33C charging is greater than 50 mV; (7) The second aluminum source includes one or more compounds containing Al-O bonds; Optionally, the second aluminum source includes one or more of aluminum hydroxide, aluminum oxide, lithium metaaluminate and sodium aluminate; (8) the second phosphorus source includes one or more compounds containing PO bonds; Optionally, the second phosphorus source includes one or more of lithium phosphate, lithium monohydrogen phosphate, lithium dihydrogen phosphate and lithium pyrophosphate; (9) The temperature of the second calcination treatment is 200°C-450°C, the time is 0h-12h, and the heating rate is 1°C / min-5°C / min; Optionally, the second calcination treatment time is 1h-12h; (10) The mixed material subjected to the second calcination treatment further includes a second additive, wherein the second additive comprises one or more elements selected from the group consisting of Li, S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb and Bi.
7. The preparation method according to any one of claims 5 to 6, characterized in that: The chemical formula of the lithium nickel manganese oxide is Li a Ni b Mn c M1 d M2 e O 4-f , 0.95 ≤ a ≤ 1.1, 0.45 < b < 0.55, 1.4 < c < 1.6, 0 ≤ d + e ≤ 0.1, 0 ≤ f ≤ 0.
1. The M1 element includes one or more elements among S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, and La. The M2 element includes one or more elements among V, Nb, Mo, W, Ta, B, Sb, and Bi; Optionally, the method for preparing the inner core comprises: A third calcination treatment is performed after mixing a nickel-manganese precursor and a lithium salt; or a third calcination treatment is performed after mixing a nickel-manganese precursor, a lithium salt and a third additive; Optionally, the chemical formula of the nickel-manganese precursor is Ni 0.25 Mn 0.75 (OH)2、Ni 0.25 Mn 0.75 C2O4 and Ni 0.25 Mn 0.75 One or more of CO3; Optionally, the nickel manganese precursor includes one or more of nickel manganese hydroxide, nickel manganese oxalate and nickel manganese carbonate, and may be nickel manganese hydroxide; Optionally, the third additive comprises one or more elements of S, Y, Mg, Al, Ti, Zr, P, Sr, Si, F, La, V, Nb, Mo, W, Ta, B, Sb and Bi; Optionally, the lithium source includes one or more of LiOH, Li2CO3, Li2SO4, LiCl and LiNO3, and may be one or more of LiOH and Li2CO3; Optionally, the molar ratio of the total metal contained in the nickel-manganese precursor to the lithium element contained in the lithium source is 1:(0.5-0.55); Optionally, the temperature of the third calcination treatment is 600°C-1000°C, the time is 5h-30h, the heating rate is 1°C / min-5°C / min, and the oxygen partial pressure in the calcination atmosphere is ≥10000Pa; Optionally, the temperature of the third calcination treatment is 850°C-950°C and the time is 6h-12h Optionally, the voltage difference between two main peaks of the capacity differential curve of the electrochemical distribution curve of the core at 0.33C charge is less than 40 mV or greater than 50 mV.
8. A positive electrode sheet, characterized in that: A composite coated positive electrode material comprising the composite coated positive electrode material as described in any one of claims 1 to 4 or a composite coated positive electrode material prepared by the preparation method as described in any one of claims 5 to 7.
9. A lithium ion battery, characterized in that: Comprising the positive electrode sheet as described in claim 8.
10. An electrical device, characterized in that: Comprising the lithium ion battery as claimed in claim 9.
Citation Information
Cited By
Detection method and device for testing crosstalk characteristic of lithium battery
CN119758110A
Positive electrode active material, positive plate and lithium ion battery
CN120376597A
Positive electrode material and preparation method thereof, electrochemical device and electronic equipment
CN120674482A
Positive pole piece, battery and energy storage device
CN121506879A
Composite-coated positive electrode material and preparation method therefor, positive electrode sheet, lithium-ion battery and electric device
WO2026056714A1