Polyimide resin and negative type photosensitive resin composition containing the same

A ring-closed polyimide resin with specific terminal groups and a photocurable compound in a negative photosensitive composition addresses swelling and solubility issues, enabling precise pattern formation with improved mechanical properties and reduced costs in electronics and information industries.

JP7582573B2Active Publication Date: 2024-11-13LG CHEM LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020511360
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-07-20
Filing Date
2019-07-19
Publication Date
2024-11-13
Estimated Expiration
2039-07-19

AI Technical Summary

Technical Problem

Existing negative photosensitive resins experience swelling during development and have inadequate solubility, making it difficult to form ultra-fine patterns and increasing process costs in precision electronics and information industries.

Method used

A ring-closed polyimide resin with specific terminal groups containing photopolymerizable unsaturated groups is used in a negative photosensitive composition, along with a photocurable polyfunctional acrylic compound and a photopolymerization initiator, to prevent swelling and enhance solubility, allowing for ultra-fine pattern formation.

Benefits of technology

The polyimide resin composition maintains solubility during development, achieves high adhesion to substrates with lower light intensity, and forms precise patterns with excellent mechanical properties, reducing process costs and improving pattern resolution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582573000013
    Figure 0007582573000013
  • Figure 0007582573000014
    Figure 0007582573000014
  • Figure 0007582573000001
    Figure 0007582573000001
Patent Text Reader

Abstract

The present invention relates to a polyimide resin having a structure of Chemical Formula 1, a negative-type photosensitive resin composition including the polyimide resin, and an electronic device including an organic insulating film or a photosensitive pattern formed from the negative-type photosensitive resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2018-0085003, filed with the Korean Intellectual Property Office on July 20, 2018, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a photosensitive resin composition, and more particularly to a negative type ring-closed polyimide resin having excellent solubility and not swelling during development, and a negative type photosensitive resin composition containing the same. [Background technology]

[0003] Photosensitive resins are representative functional polymer materials that have been put to practical use in the production of various precision electronic and information industry products, and are currently being used in the high-tech industry, especially in the production of semiconductors and displays. In general, photosensitive resins refer to polymer compounds that undergo chemical changes in molecular structure in a short time when irradiated with light, resulting in changes in physical properties such as solubility in a specific solvent, coloring, and hardening. Photosensitive resins enable fine precision processing, can significantly reduce energy and raw materials compared to thermal reaction processes, and can be used quickly and accurately in a small installation space, making them widely used in various precision electronic and information industry fields such as cutting-edge printing, semiconductor production, display production, and photocurable surface coating materials.

[0004] Such photosensitive resins are broadly divided into negative and positive types. Negative photosensitive resins are those in which the parts irradiated with light become insoluble in a developer, while positive photosensitive resins are those in which the parts irradiated with light become soluble in a developer.

[0005] Polymers used in negative photosensitive resins must have high solubility in the developer after selective exposure, and the unexposed parts must have low or no solubility in the developer. This requirement is becoming more and more prevalent in the precision electronics and information industry so that extremely fine patterns can be formed. Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention provides a polyimide having a closed ring structure, which is free from swelling during development when a pattern is formed using a negative type photosensitive composition and has excellent solubility, and a negative type photosensitive resin composition containing the same.

[0007] The present invention also provides an electronic device including an organic insulating film or a photosensitive pattern formed from the negative type photosensitive resin composition. [Means for solving the problem]

[0008] One embodiment of the present invention provides a polyimide resin comprising the structure of Formula 1 below: [Chemical formula 1] [ka] In the above Chemical Formula 1, X is a tetravalent organic group; Y is a divalent to hexavalent organic group; R3 to R6 are the same or different and each independently represents hydrogen; or a C1-C10 organic group containing a photopolymerizable unsaturated group; m1, m2, k1 and k2 are each 0 or 1, and 0≦m1+m2+k1+k2≦2; L1 is a divalent organic group, which is an aromatic group, an aliphatic group, or a combination of an aromatic group and an aliphatic group, and at least one carbon can be replaced by C(=O), SO2, NR, S, or O; R is an aryl group or an alkyl group; L1 can be substituted by a halogen group, a hydroxyl group, a carboxyl group, a thiol group, a sulfonic acid group, or an alkyl group; R1 is -S-, -O-, -CO2- or -SO2-; R2 is represented by the following chemical formula 2. [Chemical formula 2] [ka] In the above Chemical Formula 2, R7 is hydrogen; or an alkyl group having 1 to 4 carbon atoms; and p is an integer from 1 to 10; In Chemical Formula 1, * is a moiety that is linked to the main chain or an end group of the polyimide resin, and in Chemical Formula 2, * is a moiety that is linked to R1, and n is an integer of 1 or more.

[0009] Another embodiment of the present invention provides a negative type photosensitive resin composition comprising the polyimide resin; a photocurable polyfunctional acrylic compound; and a photopolymerization initiator.

[0010] In another embodiment of the present invention, there is provided an electronic device including an organic insulating film or a photosensitive pattern formed from the negative type photosensitive resin composition. Effect of the Invention

[0011] According to the embodiments described herein, when a pattern is formed using the photosensitive resin composition, the polyimide resin does not swell even during the process of development after selective exposure, and has excellent solubility. In addition, according to the embodiments described herein, it is possible to provide a photosensitive resin composition that exhibits high adhesion to a substrate used in a display device with a lower light dose than existing positive photosensitive polyimides, and that can form an ultrafine pattern while having excellent mechanical properties, and an electronic device including an organic insulating film or a photosensitive pattern formed from the negative type photosensitive resin composition. [Brief description of the drawings]

[0012] [Figure 1] 1 shows a line pattern formed by Example 1. [Diagram 2] 1 shows a photograph of a hole pattern formed by Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The polyimide resin, photosensitive resin composition, and electronic device according to specific examples of the present invention will be described in detail below.

[0014] One embodiment of the present invention provides a polyimide resin comprising a unit of Formula 1 and an end group of Formula 2.

[0015] The present inventors have confirmed through experiments that a photosensitive resin including a polyimide resin having the specific structure can achieve high adhesion and bonding to substrates used in semiconductor devices or display devices, for example, metal substrates such as Au, Cu, Ni, Ti, and inorganic substrates such as SiO2, SiNx, and has improved mechanical properties such as excellent heat resistance and chemical resistance, and can easily form ultra-fine patterns, thereby completing the invention.

[0016] In particular, the negative type photosensitive resin composition does not require a polyimide precursor that requires a high-temperature heat curing process (imidization process), but uses a polyimide resin that can be solution-processed at a low temperature, thereby making it possible to omit the high-temperature imidization process.

[0017] The present inventors also revealed that when a structure in which a photopolymerizable unsaturated group is bonded to the side chain of a polyimide having a closed ring structure is used as an existing polyimide, the side chain is closed during development, causing swelling or a decrease in solubility. In addition, when a closed ring polyimide and a monomer having a photopolymerizable multifunctional group are used together, the polymer itself does not have a photopolymerizable group, so high energy is generated during the curing process by exposure, making precise patterning difficult and increasing process costs. Furthermore, attempts have been made to introduce a polyamic ester structure by opening the closed ring structure of an acid anhydride of a closed ring polyimide and then attaching a photopolymerizable group (R) to the opened position, but it has been revealed that this has problems such as unstable dimensional stability and gas generation due to the detachment of the photopolymerizable group (R) during ring closure. [ka]

[0018] However, the polyimide resin according to the above-mentioned embodiment of the present invention has a structure of Chemical Formula 2 containing a photopolymerizable unsaturated group in the R2 portion of the terminal group, so that the terminal group does not undergo a ring-closing reaction with the main chain or a side chain bonded thereto during development, and therefore no swelling phenomenon occurs during development.

[0019] The polyimide resin may contain an unreacted hydroxyl group (OH), carboxyl group (COOH), thiol group, or sulfonic acid group at the end group, and such groups may provide excellent solubility.

[0020] According to one example, the polyimide resin may contain R2 of Formula 2 in an amount of 5 to 30% based on the equivalent weight. For example, when an amine end group is included, it may be included in an amount of 5 to 30% based on the anhydride, and when an anhydride end group is included, it may be included in an amount of 5 to 30% based on the amine.

[0021] According to one embodiment, in the above Chemical Formula 1, X is not particularly limited as long as it is a tetravalent organic group, and may be, for example, a tetravalent aromatic organic group, a tetravalent aliphatic organic group, or a tetravalent organic group in which an aromatic group and an aliphatic group are linked to each other, at least one carbon may be replaced by C(=O), SO2, NR, S, or O, and R is an aryl group or an alkyl group. Specific examples of X include the following structural formulas. [ka]

[0022] In the above formula 1, Y is a divalent to hexavalent organic group, which may be a divalent to hexavalent aromatic organic group, a divalent to hexavalent aliphatic organic group, or a divalent to hexavalent organic group in which an aromatic group and an aliphatic group are linked to each other, at least one carbon may be replaced with C(=O), SO2, NR, S, or O, R is an aryl group or an alkyl group, and Y may be replaced with a halogen group, a hydroxyl group, a carboxyl group, a thiol group, a sulfonic acid group, or an alkyl group. Specifically, [ka] The following structural formulas are available. [ka]

[0023] Among the above structural formulas, examples of Z include the following structural formulas. [ka]

[0024] When m1+m2+k1+k2 is 1 or 2 and contains an OH or COOH group, as in the above structure, the structure of Chemical Formula 2 is present not only at the terminals of the polyimide resin but also in the side chains, which is advantageous in improving the surface condition when a photosensitive film is formed.

[0025] In the formula 1, L1 is a divalent organic group, which is an aromatic group, an aliphatic group, or a combination of an aromatic group and an aliphatic group, and at least one carbon can be replaced by C(=O), SO2, NR, S, or O, R is an aryl group or an alkyl group, and L1 can be replaced by a halogen group, a hydroxyl group, a carboxyl group, a thiol group, a sulfonic acid group, or an alkyl group. Here, the aromatic group can be a C6-C20 arylene group, and the aliphatic group can be a C1 to C20 alkylene group or a C3 to C20 cycloalkylene group. The arylene group can be a phenylene group, etc. The halogen group can be F, etc.

[0026] According to one embodiment, L1 may be a phenylene group.

[0027] According to one embodiment, the structure of Formula 1 may be represented by Formula 11 or 12 below. [Chemical formula 11] [ka] [Chemical formula 12] [ka] In the above formulas 11 and 12, L2 is a divalent organic group, and the remaining substituents are as previously described.

[0028] According to one example, L2 may be an alkylene or arylene, specifically a C1 to C12 alkylene or phenylene.

[0029] In one embodiment, R1 is -S-, -O- or -CO2-.

[0030] In one embodiment, R1 is -S-.

[0031] In one embodiment, R1 is -O-.

[0032] In one embodiment, R1 is -CO2-.

[0033] In one embodiment, L2 is phenylene.

[0034] According to one embodiment, the polyimide resin may contain two or more types of units represented by Chemical Formula 1, and may further contain units other than the units of Chemical Formula 1, as necessary. However, the polyimide resin preferably contains 50 mol % or more of the units of Chemical Formula 1.

[0035] The other end of the polyimide resin may also have the end of Chemical Formula 2, or may have the diamine or dianhydride used in the production of the polyimide as an end group.

[0036] According to one embodiment, the polyimide resin may have a weight average molecular weight of 1,000 to 500,000, preferably 5,000 to 200,000. If the weight average molecular weight is less than 1,000, it may be difficult to achieve the desired coating properties and mechanical properties when applying the polyimide copolymer, and if it exceeds 500,000, it may be difficult to apply it as a photosensitive material due to its low solubility in a developer. The weight average molecular weight may be a value measured by gel permeation chromatography, i.e., GPC.

[0037] The polyimide resin can be prepared using a dianhydride compound and a diamine compound, and the materials and polymerization methods for forming the polyimide can be those known in the art. However, in order to have the end group of the above formula 1, a compound having at least one group selected from a hydroxyl group, a carboxyl group, a thiol group, and a sulfonic acid group and having one anhydride group or one amine group is used during polymerization of the polyimide to prepare a polyimide having at least one group selected from a hydroxyl group, a carboxyl group, a thiol group, and a sulfonic acid group, and an isocyanate compound is reacted therewith to prepare the end group of the above formula 1.

[0038] Another embodiment of the present invention provides a negative type photosensitive resin composition comprising the polyimide resin, a photocurable polyfunctional acrylic compound, and a photopolymerization initiator. The negative type photosensitive resin composition may further comprise a solvent. If necessary, the negative type photosensitive resin composition may further comprise an epoxy resin.

[0039] In the negative-type photosensitive resin composition of the embodiment, the photocurable polyfunctional acrylic compound is a compound having at least two or more photocurable acrylic structures in the molecule, and specifically, may include one or more acrylic compounds selected from the group consisting of acrylate-based compounds, polyester acrylate-based compounds, polyurethane acrylate-based compounds, epoxy acrylate-based compounds, and caprolactone-modified acrylate-based compounds.

[0040] For example, the acrylate compounds include hydroxyl group-containing acrylate compounds such as pentaerythritol triacrylate and dipentaerythritol pentaacrylate; water-soluble acrylate compounds such as polyethylene glycol diacrylate and polypropylene glycol diacrylate, and the polyester acrylate compounds include trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate. Examples of the polyurethane acrylate compounds include isocyanate-modified products of the hydroxyl group-containing acrylate compounds, examples of the epoxy acrylate compounds include bisphenol A diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, and (meth)acrylic acid adducts of phenol novolac epoxy resins, and examples of the caprolactone-modified acrylate compounds include caprolactone-modified ditrimethylolpropane tetraacrylate, ε-caprolactone-modified dipentaerythritol acrylate, and caprolactone-modified hydroxypivalic acid neopentyl glycol ester diacrylate.

[0041] In addition, in the negative type photosensitive resin composition of the embodiment, the epoxy resin can help to exhibit high adhesion and bonding properties to a substrate used in a semiconductor device or a display device, and the epoxy resin can be cured at a low temperature, which can improve the economy of the process.

[0042] Such epoxy resins may include, for example, one or more selected from the group consisting of bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, novolac type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, N-glycidyl type epoxy resins, bisphenol A novolac type epoxy resins, bixylenol type epoxy resins, biphenol type epoxy resins, chelate type epoxy resins, glyoxal type epoxy resins, amino group-containing epoxy resins, rubber-modified epoxy resins, dicyclopentadiene phenolic type epoxy resins, diglycidyl phthalate resins, heterocyclic epoxy resins, tetraglycidyl xylenoyl ethane resins, silicone-modified epoxy resins, and ε-caprolactone-modified epoxy resins, and preferably include liquid type N-glycidyl epoxy resins.

[0043] In addition, in the negative type photosensitive resin composition of the embodiment, the photo-initiator may be any photo-initiator that is known to be generally usable in photosensitive resin compositions, and may be appropriately selected in consideration of the wavelength of ultraviolet light to be used. As the photo-initiator, for example, an acetophenone-based compound, a biimidazole-based compound, a triazine-based compound, an oxime-based compound, or a mixture thereof may be used.

[0044] Specific examples of the photopolymerization initiator include 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)-phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexylphenyl ketone, benzoin methyl ether, benzoin ethyl ether, benzoin isobutyl ether, benzoin butyl ether, 2,2-dimethoxy-2-phenylacetophenone, 2-methyl-(4-methylthio)phenyl-2-morpholino-1-propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, acetophenone compounds such as 2,2-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetrakis(3,4,5-trimethoxyphenyl)-1,2'-biimidazole, 2,2'-bis(2,3-dichlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, or 2,2'-bis(o-chlorophenyl)-4,4,5,5'-tetraphenyl-1,2'-biimidazole;3-{4-[2,4-bis(trichloromethyl)-s-triazin-6-yl]phenylthio}propionic acid, 1,1,1,3,3,3-hexafluoroisopropyl-3-{4-[2,4-bis(trichloromethyl)-s-triazin-6-yl]phenylthio}propionate, ethyl-2-{4-[2,4-bis(trichloromethyl)-s-triazin-6-yl]phenylthio}acetate, 2-epoxyethyl-2-{4-[2,4-bis(trichloromethyl)-s-triazin-6-yl]phenylthio}acetate, cyclohexyl-2-{4-[2,4-bis(trichloromethyl)-s-triazin-6-yl]phenylthio}acetate, benzyl-2-{4-[2,4-bis(trichloromethyl)-s triazine compounds such as 2,4-bis(trichloromethyl)-s-triazin-6-yl]phenylthio}acetate, 3-{chloro-4-[2,4-bis(trichloromethyl)-s-triazin-6-yl]phenylthio}propionic acid, 3-{4-[2,4-bis(trichloromethyl)-s-triazin-6-yl]phenylthio}propionamide, 2,4-bis(trichloromethyl)-6-p-methoxystyryl-s-triazine, 2,4-bis(trichloromethyl)-6-(1-p-dimethylaminophenyl)-1,3,-butadienyl-s-triazine, or 2-trichloromethyl-4-amino-6-p-methoxystyryl-s-triazine; and oxime compounds such as CGI-242 and CGI-124 from Ciba Corporation of Japan.

[0045] The negative type photosensitive resin composition according to the embodiment may include 10 to 50 parts by weight of the photocurable multifunctional acrylic compound and 0.1 to 10 parts by weight of the photopolymerization initiator, based on 100 parts by weight of polyimide resin. The composition may further include 10 to 100 parts by weight of epoxy resin, based on 100 parts by weight of polyimide resin.

[0046] The negative type photosensitive resin composition may further include one or more curing accelerators selected from the group consisting of imidazole compounds, phosphine compounds, and tertiary amine compounds. The imidazole compounds may be, for example, 2-phenylimidazole, 2-phenyl-4-methylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole, and the phosphine compounds may be, for example, triphenylphosphine, diphenylphosphine, phenylphosphine, and tetraphenylphosphonium tetraphenylborate, and the tertiary amine compounds may be, for example, dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine. Such curing accelerators may be included in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the polyimide resin.

[0047] Meanwhile, the negative type photosensitive resin composition may further include a solvent, an adhesion promoter, a surfactant, a defoamer, a leveling agent, an anti-gelling agent, or a mixture thereof.

[0048] The solvent may be any organic solvent known to be usable in the negative type photosensitive resin composition without any particular limitation. Preferably, the solvent is selected from the group consisting of ethyl acetate, butyl acetate, diethylene glycol dimethyl ether, diethylene glycol dimethyl ether, methyl methoxypropionate, ethyl ethoxypropionate (EEP), ethyl lactate, propylene glycol methyl ether acetate (PGMEA), propylene glycol methyl ether, propylene glycol propyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol methyl acetate, diethylene glycol ethyl acetate, acetone, methyl isobutyl ketone, cyclohexanone, dimethyl methyl acetate (DMF), N,N-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), γ Solvents selected from the group consisting of 1-butyrolactone (GBL), diethyl ether, ethylene glycol dimethyl ether, diglyme, tetrahydrofuran (THF), methanol, ethanol, propanol, isopropanol, methyl cellosolve, ethyl cellosolve, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol methyl ethyl ether, dipropylene glycol methyl ether, toluene, xylene, hexane, heptane and octane can be used alone or in combination. The organic solvent can be included in an amount of 100 to 400 parts by weight based on 100 parts by weight of the polyimide resin.

[0049] In addition, the adhesion promoter may be a silane coupling agent having a functional group such as epoxy, carboxyl or isocyanate, and specific examples thereof include trimethoxysilyl benzoic acid, triethoxysilyl benzoic acid, gamma-isocyanatopropyltrimethoxysilane, gamma-isocyanatopropyltriethoxysilane, gamma-glycidoxypropyltrimethoxysilane, gamma-glycidoxypropyltriethoxysilane, or a mixture thereof. The adhesion promoter may be included in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the polyimide resin.

[0050] The surfactant may be any surfactant known to be usable in photosensitive resin compositions without any particular limitations, but it is preferable to use a fluorine-based surfactant or a silicone-based surfactant, which may be included in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of the polyimide resin.

[0051] Meanwhile, according to another embodiment of the present invention, there is provided an electronic device including an organic insulating film or a photosensitive pattern formed from the negative type photosensitive resin composition of the one embodiment.

[0052] The organic insulating film or photosensitive pattern may include a polyimide having a specific structure and an acrylic compound having two or more photocurable acrylic functional groups, and may have improved mechanical properties such as excellent heat resistance, insulating properties, or chemical resistance while achieving high adhesion to substrates used in semiconductor devices or display devices, for example, metal substrates such as Au, Cu, Ni, and Ti, and inorganic substrates such as SiO2 and SiNx.

[0053] Therefore, an electronic device including an organic insulating film or a photosensitive pattern formed from the negative type photosensitive resin composition can realize excellent performance such as high resolution and high sensitivity, and can exhibit excellent film characteristics and high mechanical properties as well as excellent heat resistance characteristics, for example, the adhesion of the organic insulating film or the photosensitive pattern can be maintained firmly without being deteriorated even when used for a long time or exposed to high temperature conditions for a long time.

[0054] The organic insulating film may include various insulating films of a semiconductor device or a display device, for example, an interlayer insulating film, a surface protective film, a substrate electrode protective layer, a buffer coat film, a passivation film, etc. And, the electronic device may include various components of a semiconductor device or a display device.

[0055] Meanwhile, the organic insulating film or the photosensitive pattern can be formed through the steps of: applying the negative type photosensitive resin composition onto a supporting substrate and drying to form a resin film; exposing the resin film; developing the exposed resin film with a developer; and heat-treating the developed photosensitive resin film.

[0056] By using the negative type photosensitive resin composition, a patterned photosensitive resin film can be easily formed on a substrate such as glass or a silicon wafer. In this case, the negative type photosensitive resin composition can be applied by spin coating, bar coating, screen printing, etc.

[0057] The supporting substrate that can be used in the process of forming the photosensitive resin film can be any substrate that is known to be commonly used in the fields of electronics and communications, semiconductors, and displays, without any particular limitations. Specific examples of the supporting substrate include a silicon wafer, a glass substrate, a metal substrate, a ceramic substrate, and a polymer substrate.

[0058] In the drying process after the coating, a prebaked film can be formed by prebaking at 50° C. to 150° C. for 1 to 20 minutes to evaporate the solvent. If the drying temperature is too low, the amount of remaining solvent is too large, and the film may be lost in the non-exposed area during development, resulting in a low remaining film. If the drying temperature is too high, the curing reaction may be accelerated, and the non-exposed area may not be developed.

[0059] In the step of exposing the resin film, ultraviolet rays or visible light having a wavelength of 200 to 500 nm can be irradiated using a photomask having a pattern to be processed, and the exposure dose during irradiation is 10 mJ / cm. 3 to 4,000 mJ / cm 3 The exposure time is not particularly limited and can be appropriately changed depending on the exposure device used, the wavelength of the irradiated light, or the exposure dose, and specifically, the exposure time can be changed within a range of 5 to 250 seconds.

[0060] In the step of forming the photosensitive resin film, an alkaline aqueous developer that is generally known to be usable in the production step of semiconductors or displays can be used without any particular limitation.

[0061] The present invention will be described in more detail with reference to the following examples. However, the following examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples.

[0062] Synthesis Example 1 16.02g (43.75mmol) of 2,2'-Bis(3-amino-4-hydroxyphenyl)-hexafluoropropane (BisAPAF) was dissolved in 60g of gammabutyroloactone (GBL) while passing nitrogen into a three-neck flask equipped with a stirrer, temperature controller, nitrogen gas injector, Dean-Stark distillation apparatus, and condenser. 10.58g (34.12mmol) of 4,4'-oxydiphthalic dianhydride (ODPA) and 3.67g (19.25mmol) of trimeristic anhydride were added to the solution, and the mixture was stirred for 4 hours. Then, 20g of toluene, 20g of GBL, 0.84g of acetic anhydride, and 2.12g of aniline were added, and the reaction temperature was raised to 160℃, and the reaction was continued for 20 hours after removing water through a Dean-Stark distillation apparatus for 5 hours. After the reaction was completed, 104g of SPI-1 was obtained. 3g (21mmol) of 2-acryloyloxyethyl isocyanate was slowly added to 100g of the obtained SPI-1, and the reaction temperature was raised to 60℃ and stirred for 12 hours. As a result of 1H-NMR analysis, SPI-A-1 was obtained, which was calculated to have an average of 0.20 equivalents per hydroxyl group (-OH) in the polyimide replaced with AOI. The molecular weight of the polyimide resin was measured by gel permeation chromatography (GPC) in a dimethylformamide (DMF) solvent, and the weight average molecular weight was 14,000.

[0063] Synthesis Example 2 Polyimide resin SPI-3 was prepared in the same manner as in Synthesis Example 1, except that 15.16 g (34.12 mmol) of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA) was used instead of 4,4'-oxydiphthalic dianhydride (ODPA). 3 g (21 mmol) of 2-acryloyloxyethyl isocyanate was slowly added to 100 g of the obtained SPI-3, and the reaction temperature was raised to 60°C and stirred for 12 hours. As a result of 1H-NMR analysis, SPI-A-2 was obtained, which was calculated to have an average of 0.21 equivalents per hydroxyl group (-OH) in the polyimide substituted with AOI. The molecular weight of the polyimide resin was measured by gel permeation chromatography (GPC) in a dimethylformamide (DMF) solvent, and the weight average molecular weight was 16,000.

[0064] Synthesis Example 3 Polyimide resin SPI-4 was prepared in the same manner as in Synthesis Example 1, except that 10.04 g (34.12 mmol) of biphenyltetracarboxylic dianhydride (BPDA) was used instead of 4,4'-oxydiphthalic dianhydride (ODPA). 3 g (21 mmol) of 2-acryloyloxyethyl isocyanate was slowly added to 100 g of the obtained SPI-4, and the reaction temperature was raised to 60°C and stirred for 12 hours. As a result of 1H-NMR analysis, SPI-A-3 was obtained, which was calculated to have an average of 0.25 equivalents per hydroxyl group (-OH) in the polyimide substituted with AOI. The molecular weight of the polyimide resin was measured by gel permeation chromatography (GPC) in a dimethylformamide (DMF) solvent, and the weight average molecular weight was 15,000.

[0065] Synthesis Example 4 Polyimide resin SPI-2 was prepared in the same manner as in Synthesis Example 1, except that 3.69 g (19.25 mmol) of 1,2-cyclohexanedicarboxylic anhydride (CHA) was used instead of trimeristic anhydride. 3 g (21 mmol) of 2-acryloyloxyethyl isocyanate was slowly added to 100 g of the obtained SPI-2, and the reaction temperature was raised to 60° C. and stirred for 12 hours. SPI-A-4 was obtained, which was calculated to have an average of 0.23 equivalents per hydroxyl group (-OH) in the polyimide substituted with AOI as a result of 1H-NMR analysis. The molecular weight of this polyimide resin was measured by Gel Permeation Chromatography (GPC) in a dimethylformamide (DMF) solvent, and the weight average molecular weight was 13,000.

[0066] Synthesis Example 5 The same method as in Synthesis Example 1 was used to prepare polyimide resin SPI-5, except that 19.43 g (43.75 mmol) of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA) was used instead of 4,4'-oxydiphthalic dianhydride (ODPA), 13.46 g (36.75 mmol) of 2,2'-bis(3-amino-4-hydroxyphenyl)-hexafluoropropane (BisAPAF) was used instead of 16.02 g (43.75 mmol), and 1.53 g (14.00 mmol) of 4-aminophenol was used instead of trimeristic anhydride. 3g (21mmol) of 2-acryloyloxyethyl isocyanate was slowly added to 100g of the obtained SPI-5, and the reaction temperature was raised to 60℃ and stirred for 12 hours. As a result of 1H-NMR analysis, SPI-A-5 was obtained, which was calculated to have an average of 0.23 equivalents per hydroxyl group (-OH) in the polyimide substituted with AOI. The molecular weight of this polyimide resin was measured through GPC (Gel Permeation Chromatography) in dimethylformamide (DMF) solvent, and the weight average molecular weight was 12,000.

[0067] Synthesis Example 6 Polyimide resin SPI-6 was prepared in the same manner as in Synthesis Example 5, except that 1.75 g (14.00 mmol) of 4-aminobenzenethiol was used instead of 4-aminophenol. 100 g of the obtained SPI-6 was slowly added with 3 g (21 mmol) of 2-acryloyloxyethyl isocyanate, and the reaction temperature was raised to 60° C. and stirred for 12 hours. As a result of 1H-NMR analysis, SPI-A-6 was obtained, which was calculated to have an average of 0.23 equivalents per hydroxyl group (-OH) in the polyimide substituted with AOI. The molecular weight of this polyimide resin was measured by Gel Permeation Chromatography (GPC) in a dimethylformamide (DMF) solvent, and the weight average molecular weight was 13,000.

[0068] Synthesis Example 7 Polyimide resin SPI-7 was prepared in the same manner as in Synthesis Example 5, except that 2.63 g (14.00 mmol) of N-(4-aminophenyl)maleimide was used instead of 4-aminophenol. 3 g (21 mmol) of 2-acryloyloxyethyl isocyanate was slowly added to 100 g of the obtained SPI-7, and the reaction temperature was raised to 60° C. and stirred for 12 hours. SPI-A-7 was obtained, which was calculated to have an average of 0.23 equivalents per hydroxyl group (-OH) in the polyimide substituted with AOI as a result of 1H-NMR analysis. The molecular weight of this polyimide resin was measured by Gel Permeation Chromatography (GPC) in a dimethylformamide (DMF) solvent, and the weight average molecular weight was 13,000.

[0069] Synthesis Example 8 Polyimide resin SPI-8 was prepared in the same manner as in Synthesis Example 5, except that 1.64 g (14.00 mmol) of 4-ethylaniline was used instead of 4-aminophenol. 3 g (21 mmol) of 2-acryloyloxyethyl isocyanate was slowly added to 100 g of the obtained SPI-8, and the reaction temperature was raised to 60° C. and stirred for 12 hours. SPI-A-8 was obtained, which was calculated to have an average of 0.23 equivalents per hydroxyl group (-OH) in the polyimide substituted with AOI as a result of 1H-NMR analysis. The molecular weight of this polyimide resin was measured by Gel Permeation Chromatography (GPC) in a dimethylformamide (DMF) solvent, and the weight average molecular weight was 12,000.

[0070] Synthesis Example 9 1 mol of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB) was dissolved in 80 g of diethylformamide (DEF), to which 1.1 mol of 4,4'-oxydiphthalic dianhydride (ODPA) was added, and the mixture was added to 50 g of diethylformamide (DEF) and polymerized at 50°C for 24 hours to produce a solution containing polyamic acid. 40 g of toluene was added to the solution produced, and the solution was refluxed at 180°C for 12 hours after being placed in a Dean-Stark distillation apparatus to remove water. The prepared polyimide solution was precipitated in methanol solvent, dried, and then the dried polyimide was dissolved in 50g of diethylformamide (DEF), and 3mol of 2-methacryloyloxyethyl isocyanate was added, and 30g of diethylformamide (DEF) was added, and the mixture was reacted at room temperature for 24 hours, and then precipitated in methanol and dried to obtain PI-M-1. The molecular weight was measured by GPC (Gel Permeation Chromatography) in dimethylformamide (DMF) solvent, and the weight average molecular weight was 17,000.

[0071] Example 1 10.0g of polyimide resin SPI-A-1 of Synthesis Example 1, 0.45g of photopolymerization initiator Irgacure369 (Ciba Specialty Chemical Co.), and 2.0g of photocurable multifunctional acrylic compound Kayalado DPHA (Nippon Kayaku Co.) were dissolved in 20g of organic solvent MEDG (Diethyleneglycol methylethyl ether), and then 0.05g of DC-190 (Toray Dow Corning Co.) was mixed and stirred at room temperature for 1 hour. After stirring, the resultant was filtered through a filter with pores of 0.45μm to prepare a photosensitive resin composition.

[0072] Example 2 A photosensitive resin composition was prepared in the same manner as in Example 1, except that 10 g of SPI-A-2 was used instead of the polyimide resin SPI-A-1.

[0073] Example 3 A photosensitive resin composition was prepared in the same manner as in Example 1, except that 10 g of SPI-A-3 was used instead of the polyimide resin SPI-A-1.

[0074] Example 4 A photosensitive resin composition was prepared in the same manner as in Example 1, except that 10 g of SPI-A-5 was used instead of the polyimide resin SPI-A-1.

[0075] Example 5 A photosensitive resin composition was prepared in the same manner as in Example 1, except that 10 g of SPI-A-6 was used instead of the polyimide resin SPI-A-1.

[0076] Comparative Example 1 A photosensitive resin composition was prepared in the same manner as in Example 1, except that 10 g of SPI-A-4 was used instead of the polyimide resin SPI-A-1.

[0077] Comparative Example 2 A photosensitive resin composition was prepared in the same manner as in Example 1, except that 10 g of SPI-1, which had no urethane acrylic functional group, was used instead of the polyimide resin SPI-A-1.

[0078] Comparative Example 3 A photosensitive resin composition was prepared in the same manner as in Example 1, except that 10 g of SPI-2, which had no urethane acrylic functional group, was used instead of the polyimide resin SPI-A-1.

[0079] Comparative Example 4 A photosensitive resin composition was prepared in the same manner as in Example 1, except that 10 g of SPI-A-7 was used instead of the polyimide resin SPI-A-1.

[0080] Comparative Example 5 A photosensitive resin composition was prepared in the same manner as in Example 1, except that 10 g of SPI-A-8 was used instead of the polyimide resin SPI-A-1.

[0081] Comparative Example 6 A photosensitive resin composition was prepared in the same manner as in Example 1, except that 10 g of PI-M-1 was used instead of the polyimide resin SPI-A-1.

[0082] Experimental example: Photosensitivity experiment of photosensitive resin film The photosensitive resin compositions obtained in the examples and comparative examples were applied onto a 10 cm x 10 cm glass substrate using a spin coating method at 800 rpm to 1,200 rpm, and then dried at a temperature of 120°C for 2 minutes to obtain a substrate on which a photosensitive resin film of 5 μm was formed. Then, using a mask having a fine pattern, a broadband aligner exposure device was used to expose the substrate at 40 mJ / cm. 3 The exposed glass substrate was developed with a 2.38 wt% tetramethylammonium hydroxide solution for 100 seconds, washed with ultrapure water, and dried under nitrogen to form a pattern on the photosensitive resin film. The thickness of the exposed and remaining film was measured using Alpha Step.

[0083] The photosensitive resin film was evaluated for the realization of fine hole patterns with a diameter of 3μm or less. The surface condition after coating and development was rated as "good" if there were no pinholes or cracks when observed with an optical microscope and the surface uniformity measured with an AFM (Atomic Force Microscope) was 0.5nm or less, otherwise it was rated as "poor." The realization of hole patterns was rated as "possible" if holes with a diameter of 3μm or less were formed, and "poor" if residual film remained or a pattern was not formed due to non-development.

[0084] The measurement results are shown in the following Table 1. Figure 1 shows the line pattern formed by Example 1. Figure 2 is a photograph showing that a hole pattern with a diameter of 3 μm or less was clearly formed by Example 1. [Table 1]

[0085] Comparative Example 1 had the end group of Chemical Formula 2 only in the side chain, and the surface condition was good, but the hole pattern with a diameter of 3 μm or less was not realized in a good state. Comparative Examples 2 and 3 did not contain the structure of Chemical Formula 2 in either the side chain or the end, and the swelling phenomenon and solubility were low during development, and the surface condition after development was poor, and the hole pattern with a diameter of 3 μm or less was not realized in a good state. Comparative Examples 4 to 6 had the end group of Chemical Formula 2 in the side chain and a photocurable group at the end, and the surface condition was good, but the hole pattern with a diameter of 3 μm or less was not realized in a good state. In particular, Comparative Example 6 was not developed with the developer due to a lack of alkali-soluble groups after photocuring. Meanwhile, Examples 1 to 5 not only had excellent surface conditions after coating and development, but also made it possible to realize a hole pattern with a diameter of 3 μm or less.

Claims

1. A polyimide resin having a structure represented by the following chemical formula 11. [Chemical formula 11] 【Chemistry 3】 In the above Chemical Formula 11, X is a tetravalent organic group; Y is a divalent to hexavalent organic group and has a structure derived from 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane; R 3 From R 6 are the same or different and each independently represents hydrogen; or a C1-C10 organic group containing a photopolymerizable unsaturated group, m 1 , m 2 , k 1 and k 2 are each 0 or 1, and 0≦m 1 +m 2 +k 1 +k 2 ≦2, R 1 is a single bond, R 2 is represented by the following chemical formula 2: [Chemical formula 2] 【Chemistry 2】 In the above Chemical Formula 2, R 7 is hydrogen; or an alkyl group having 1 to 4 carbon atoms, and p is an integer from 1 to 10, The symbol * in Formula 11 represents a moiety that is connected to the main chain or end group of the polyimide resin, and the symbol * in Formula 2 represents R 1 and n is an integer of 1 or more.

2. The polyimide resin according to claim 1 , wherein the polyimide resin has a weight average molecular weight of 1,000 to 500,000.

3. A negative type photosensitive resin composition comprising the polyimide resin according to claim 1 or 2; a photocurable polyfunctional acrylic compound; and a photopolymerization initiator.

4. The negative type photosensitive resin composition according to claim 3 , further comprising an organic solvent.

5. 5. The negative type photosensitive resin composition according to claim 3, wherein the photocurable polyfunctional acrylic compound is contained in an amount of 10 to 50 parts by weight and the photopolymerization initiator is contained in an amount of 0.1 to 10 parts by weight, relative to 100 parts by weight of the polyimide resin.

6. An electronic device comprising an organic insulating film or a photosensitive pattern formed from the negative type photosensitive resin composition according to claim 3 .

Citation Information

Patent Citations

  • Novel photosensitive resin composition, photosensitive resin composition solution obtained therefrom, photosensitive film, insulating film, and printed wiring board with insulating film

    JP2009069664A

  • Modified polyimide and curable resin composition containing the same

    JP2018502931A

  • Photosensitive resin composition

    KR1020160020229A

  • Negative type photosensitive resin composition and organic light emitting device black matrix comprising the same