CATALYST AND METHOD FOR PRODUCING SAME, AND METHOD FOR PRODUCING UNSATURATED HYDROCARBON

A catalyst with fibrous carbon support for transition metals on carriers like alumina enhances the selectivity and conversion of alkanes to unsaturated hydrocarbons, addressing low selectivity in existing methods.

JP7582623B2Active Publication Date: 2024-11-13MITSUBISHI CHEM CORP +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021556132
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-24
Filing Date
2020-11-11
Publication Date
2024-11-13
Estimated Expiration
2040-11-11

AI Technical Summary

Technical Problem

Existing methods for producing unsaturated hydrocarbons from alkanes suffer from low selectivity and productivity, necessitating the development of a catalyst and method that can enhance the production of unsaturated hydrocarbons with higher selectivity.

Method used

A catalyst is developed by supporting transition metals, such as molybdenum, tungsten, chromium, nickel, iron, noble metals, vanadium, or manganese, on a carrier like silica, alumina, or titania, with fibrous carbon added to prevent metal aggregation, and using a carbon-containing gas to form the catalyst, followed by contact with a mixed gas containing alkanes and carbon dioxide for dehydrogenation.

Benefits of technology

The catalyst achieves high selectivity and conversion rates of alkanes to unsaturated hydrocarbons, maintaining active sites and preventing metal aggregation through the use of fibrous carbon support.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582623000002
    Figure 0007582623000002
  • Figure 0007582623000003
    Figure 0007582623000003
  • Figure 0007582623000001
    Figure 0007582623000001
Patent Text Reader

Abstract

Provided is a catalyst with which it is possible to manufacture an unsaturated hydrocarbon at a higher selectivity in the dehydrogenation of an alkane, a method for manufacturing the catalyst, and a method for manufacturing an unsaturated hydrocarbon. A catalyst, characterized in that a transition metal and carbon are supported on a carrier and the carbon contains fibrous carbon. The catalyst is brought into contact with a mixed gas containing an alkane and carbon dioxide, and an unsaturated hydrocarbon is manufactured from the alkane.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst and a method for producing the same, and a method for producing unsaturated hydrocarbons. [Background technology]

[0002] Methods for producing alkenes by dehydrogenating alkanes are generally known, and various catalysts for this dehydrogenation have been investigated.

[0003] For example, Patent Document 1 describes a dehydrogenation catalyst in which nickel and tin are supported on a composite carrier made of a specific γ-alumina carrier and a specific amount of zinc oxide supported thereon, and describes an example in which isobutane is dehydrogenated to produce isobutylene (isobutene) using this dehydrogenation catalyst.

[0004] Patent Document 2 describes a catalyst in which zinc and a metal of Group VIIIA of the periodic table are supported on a specific zeolite carrier. It also describes a method for producing unsaturated hydrocarbons by dehydrogenating hydrocarbons in the presence of this catalyst. As an example, it describes an example in which n-butane is dehydrogenated using this catalyst to produce butenes (1-butene, 2-butene, isobutene).

[0005] Patent Document 3 describes a method for producing an oxidative dehydrogenation catalyst, which includes a step (a) of dispersing a silicate in water, a step (b) of adding chromium element, a step (c) of adding a surfactant after step (a) or step (b) and a step (d) of heat-treating at a temperature of 50 to 150°C for 1 to 20 hours, and a step (d) of heat-treating at a temperature of 200 to 700°C for 1 to 10 hours. The method describes a method for producing an alkene from an alkane by contacting the obtained catalyst with a mixed gas containing an alkane and oxygen in a specific mixture ratio. As an example, the method describes an example of producing isobutylene (isobutene) from isobutane using this catalyst.

[0006] Furthermore, Patent Document 4 describes that in a hydrocarbon conversion process, a catalyst in which a transition metal is supported on a carrier is pretreated. However, the pretreatment time is short, from 30 to 90 minutes, and is not capable of suppressing the aggregation of the transition metal, and therefore is not capable of realizing high selectivity. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 9-75732 [Patent Document 2] JP 2013-163647 A [Patent Document 3] JP 2014-140827 A [Patent Document 4] Special Publication No. 2018-520858 Summary of the Invention [Problem to be solved by the invention]

[0008] In a process for producing unsaturated hydrocarbons by dehydrogenation of alkanes, high productivity is desirable, and therefore high selectivity is required.

[0009] Therefore, an object of the present invention is to solve the problems in view of the above circumstances, that is, to provide a catalyst capable of producing unsaturated hydrocarbons with high selectivity in the dehydrogenation of alkanes, a production method thereof, and a production method for unsaturated hydrocarbons. [Means for solving the problem]

[0010] According to one aspect of the present invention, there is provided a catalyst comprising a transition metal and carbon supported on a support, the carbon including fibrous carbon.

[0011] According to another aspect of the present invention, mixing a solution containing a transition metal compound with a support, and heating to remove the solvent to obtain a catalyst precursor; contacting the catalyst precursor with a carbon-containing gas to form a transition metal and carbon supported catalyst; A method for producing a catalyst, comprising: In the step of forming the catalyst, the catalyst precursor is contacted with a carbon-containing gas to form and support fibrous carbon.

[0012] According to another aspect of the present invention, There is provided a method for producing unsaturated hydrocarbons, which comprises contacting the above catalyst with a mixed gas containing an alkane and carbon dioxide to produce unsaturated hydrocarbons from the alkane.

[0013] According to another aspect of the present invention, There is provided a method for producing unsaturated hydrocarbons, which comprises producing a catalyst by the above-mentioned method for producing a catalyst, and then contacting the obtained catalyst with a mixed gas containing an alkane and carbon dioxide to produce unsaturated hydrocarbons from the alkane.

[0014] According to another aspect of the present invention, a step of contacting a catalyst precursor having a transition metal compound supported on a carrier with a carbon-containing gas to support carbon containing fibrous carbon on the catalyst precursor, thereby forming a catalyst having a transition metal and carbon containing fibrous carbon supported thereon; There is provided a method for producing unsaturated hydrocarbons, which comprises contacting a mixed gas containing an alkane and carbon dioxide with the obtained catalyst to produce unsaturated hydrocarbons from the alkane. Effect of the Invention

[0015] According to the present invention, it is possible to provide a catalyst capable of producing unsaturated hydrocarbons with high selectivity in the dehydrogenation of alkanes, a method for producing the same, and a method for producing unsaturated hydrocarbons. [Brief description of the drawings]

[0016] [Figure 1]1 is a SEM image of the catalyst of Example 2 of the present invention. [Diagram 2] This is an SEM image showing grid-like parting lines in the SEM image of Figure 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, a catalyst according to an embodiment of the present invention, a method for producing the catalyst, and a method for producing an unsaturated hydrocarbon (preferably an alkene) from an alkane will be described in detail.

[0018] (catalyst) The catalyst according to an embodiment of the present invention is a catalyst in which carbon is supported on a transition metal-supported support. This catalyst is a solid catalyst having catalytic activity in a reaction of forming an unsaturated hydrocarbon by dehydrogenation of an alkane, and is suitable as a catalyst for a reaction of forming an unsaturated hydrocarbon (preferably an alkene) by dehydrogenation of an alkane in a method for producing an unsaturated hydrocarbon from an alkane, which will be described later.

[0019] In this catalyst, the support on which the transition metal and carbon are supported is not particularly limited, and for example, at least one selected from the group consisting of silica, alumina, zirconia, and titania can be used. These may be used alone or in combination of two or more. Among these, alumina is preferred, and γ-alumina is particularly preferred.

[0020] The particle size of the carrier can be appropriately selected, but it is preferable to adjust the particle size so that the pressure loss in the catalyst layer of the reactor (e.g., reaction tube) filled with the obtained catalyst is not excessively large. In order to secure the surface area of ​​the catalyst while suppressing the pressure loss in the catalyst layer, it is preferable that the particle size of the carrier is as small as possible. When a mesh according to the Japanese Industrial Standards (JIS) is used, it is preferable that it is 3.5 mesh (mesh opening 5.6 mm) or more, and particularly preferable that it is 8.6 mesh (mesh opening 2.0 mm) or more. On the other hand, fine particles are difficult to handle, and from the viewpoint of the influence on reactivity due to the increase in pressure loss when packed in a reactor, it is preferable that it is 635 mesh (mesh opening 20 μm) or less, and particularly preferable that it is 280 mesh (mesh opening 53 μm) or less.

[0021] The catalyst according to the embodiment of the present invention can be filled in a reactor (e.g., a reaction tube) in a powder state. In this case, it is preferable to adjust the particle size so that the pressure loss in the catalyst layer does not become excessively large. In order to secure the surface area of ​​the catalyst while suppressing the pressure loss in the catalyst layer, it is preferable that the particle size of the catalyst is as small as possible. In addition, in order to suppress the pressure loss in the catalyst layer, the catalyst may be mixed with other materials, or may be filled after molding. As the other materials, a filler (silica balls, alumina balls) that is inactive to the catalyst and does not deteriorate the catalytic performance can be used. In addition, molding can be performed by adding a binder that does not deteriorate the catalytic performance to the obtained catalyst, kneading, and heating to sinter. Examples of binders (sintering agents) include silica-based, alumina-based, zirconia-based, and diatomaceous earth-based. In addition, examples of shapes after molding include tablets, pellets, spheres, and extrusions. By molding, strength and handleability can be increased.

[0022] The transition metal supported on the carrier may be at least one selected from the group consisting of molybdenum, tungsten, chromium, nickel, iron, precious metals (Au, Ag, Pt, Pd, Rh, Ir, Ru, Os), vanadium, manganese, and zinc, or a combination of these metals may be used. Among these, nickel (Ni) is preferred from the standpoint of cost and catalytic performance.

[0023] The amount of the transition metal supported on the carrier is preferably 1.0% by mass or more and 30.0% by mass or less with respect to the carrier in order to exhibit good catalytic activity. By setting the amount of the transition metal supported on the carrier to 1.0% by mass or more, the transition metal particles present as active sites are easily retained on the carrier surface, so that the conversion rate of the alkane can be increased. In addition, by setting the amount of the transition metal supported on the carrier to 30.0% by mass or less, the aggregation of the transition metal particles supported on the carrier can be further suppressed, the surface area of ​​the active sites can be kept large, and the conversion rate of the alkane and the selectivity of the alkene corresponding to the alkane can be increased. Among the above, the amount of the transition metal supported on the carrier is more preferably 3.0% by mass or more, even more preferably 5.0% by mass or more, particularly preferably 10.0% by mass or more, and most preferably 15.0% by mass or more, while it is more preferably 28.0% by mass or less, even more preferably 25.0% by mass or less, and particularly preferably 23.0% by mass or less. In the present invention, the amount of the transition metal supported on the carrier can be measured by fluorescent X-ray analysis.

[0024] As described above, the catalyst of the present embodiment supports carbon containing fibrous carbon in addition to the transition metal. By supporting carbon containing fibrous carbon on the catalyst, the conversion rate of the alkane and the selectivity of the alkene corresponding to the alkane can be improved in the dehydrogenation reaction of the alkane. The reason for this is not clear, but the following reasons are considered.

[0025] In a typical metal-supported catalyst, metal particles on the support generally aggregate and become coarse particles as the reaction proceeds, which reduces the surface area of ​​the active sites, resulting in a decrease in reactivity, and a decrease in selectivity due to a change in the structure of the active sites. However, by supporting a specific amount of carbon containing fibrous carbon in advance in addition to the transition metal, the presence of carbon containing fibrous carbon can suppress the aggregation of transition metals caused by heat or vibration during the reaction, so that good active sites can be maintained, and the selectivity of alkanes, the selectivity of alkenes corresponding to the alkanes, and the selectivity of unsaturated hydrocarbons are thought to be improved. In the present invention, carbon that is stretched in a fibrous shape (carbon that exists in a so-called elongated shape) when observed with a scanning electron microscope (SEM) is referred to as fibrous carbon. The cross-sectional shape of the carbon stretched in a fibrous shape (the cross-sectional shape perpendicular to the longitudinal direction) may be any of circular, elliptical, triangular, rectangular, polygonal, etc., may be amorphous, or may be thin and plate-like. There is also no particular limitation on the ratio of the length of the fibrous carbon to the average diameter of the cross section. The fibrous carbon may be bent, extend linearly, or may be branched.

[0026] The amount of carbon containing fibrous carbon supported on the support is preferably 510% by mass or more, and preferably 2500% by mass or less, based on the transition metal supported. If the amount of carbon containing fibrous carbon supported on the support is 550% by mass or more based on the transition metal supported, the effect of immobilizing the transition metal particles is easily obtained, and the aggregation of the transition metal particles during the reaction is easily suppressed. As a result, the conversion rate of the alkane and the selectivity of the alkene corresponding to the alkane can be increased. The carbon supported on the support only needs to contain fibrous carbon, and if the amount of carbon containing fibrous carbon is within such a range, the above effect can be more sufficiently obtained. The presence of fibrous carbon in the carbon supported on the support (the presence of fibrous carbon supported on the support) can be confirmed by a scanning electron microscope (SEM). It is preferable that the fibrous carbon is formed on the support to such an extent that the observation image obtained by SEM is divided into 12 equal lattices and the presence of fibrous carbon can be confirmed in each lattice. On the other hand, if the amount of carbon, including fibrous carbon, supported on the support is 2,500 mass% or less relative to the supported transition metal, it is possible to more effectively prevent the transition metal particles from being covered with an excessive amount of carbon, thereby preventing the catalytic activity from being hindered, and to increase the conversion rate of the alkane and the selectivity of the alkene corresponding to the alkane. Among the above, the amount of carbon, including fibrous carbon, supported on the support is more preferably 700 mass% or more, and particularly preferably 1000 mass% or more, relative to the supported transition metal, while being more preferably 2300 mass% or less, and particularly preferably 2000 mass% or less. In the present invention, the amount of carbon, including fibrous carbon, supported on the carrier can be measured by heating to 1000° C. using simultaneous thermogravimetry and differential thermal analysis (TG-DTA) and measuring the amount of carbon supported from the weight loss at that time. In the examples described later, the weight loss when heated to 200° C. is due to the desorption of adsorbed water, so the weight loss during the heating process from 200° C. to 1000° C. was calculated as being due to the carbon, including the supported fibrous carbon.

[0027] The fibrous carbon supported on the transition metal-supported carrier preferably has an average diameter of 20 nm or more and 100 nm or less. If the average diameter of the fibrous carbon is 20 nm or more, the aggregation of transition metal particles during the reaction can be more effectively prevented, and the conversion rate of the alkane and the selectivity of the alkene corresponding to the alkane can be more effectively improved. On the other hand, if the average diameter of the fibrous carbon is 100 nm or less, the covering of the transition metal particles with the fibrous carbon can be more effectively suppressed, and there is a tendency that the decrease in catalytic activity can be easily prevented. Among them, the average diameter of the fibrous carbon is more preferably 25 nm or more, and particularly preferably 30 nm or more, while it is more preferably 95 nm or less, and particularly preferably 90 nm or less. In the present invention, the average diameter of the fibrous carbon is determined by dividing an observation image obtained by a scanning electron microscope (SEM) into 12 equal grids, selecting from each grid the point with the largest diameter and the point with the smallest diameter of the fibrous carbon, determining these as representative diameter values, and averaging the representative diameter values ​​of the fibrous carbon as the average diameter of the fibrous carbon.

[0028] (Catalyst manufacturing method) A method for producing a catalyst according to an embodiment of the present invention includes a step of mixing a solution containing a transition metal compound with a support, and heating the mixture to remove the solvent to obtain a catalyst precursor, and a step of contacting the catalyst precursor with a carbon-containing gas to form a catalyst in which a transition metal and carbon are supported. By contacting the catalyst precursor with a carbon-containing gas, fibrous carbon can be formed and supported.

[0029] The step of obtaining the catalyst precursor can include a step of mixing a solution in which a transition metal compound is dissolved with a support, heating the mixture to evaporate the solvent to obtain a solid, and pulverizing the solid to obtain a powdered catalyst precursor.

[0030] In the step of obtaining a catalyst precursor, a transition metal compound containing the transition metal to be supported is dissolved in a solvent to prepare a solution, and the support is added to this solution to obtain a mixed solution containing the transition metal compound and the support. Note that, in the present invention, "adding" is a type of "mixing," but this means that further mixing may be performed after adding.

[0031] The carrier used in the step of obtaining the catalyst precursor can be at least one selected from the group consisting of silica, alumina, zirconia, and titania. Among these, alumina is preferred, and γ-alumina is particularly preferred.

[0032] The mixture containing the transition metal compound and the carrier is then heated to evaporate the solvent, thereby obtaining a solid catalyst precursor in which the transition metal is supported on the carrier. The resulting catalyst precursor (solid) can be pulverized to obtain a powdered catalyst precursor.

[0033] The obtained catalyst precursor can be subjected to a drying treatment, for example, at 20° C. to 200° C., for example, for 1 hour to 20 hours. The temperature of this drying treatment is more preferably 60° C. or higher, even more preferably 100° C. or higher, and more preferably 120° C. or lower. The time of this drying treatment is more preferably 5 hours or longer, and more preferably 15 hours or shorter.

[0034] The obtained catalyst precursor may be subjected to a heat treatment (calcination) at a high temperature of, for example, 300° C. to 1000° C. for, for example, 2 hours to 30 hours. The temperature of this heat treatment (calcination) is more preferably 400° C. or higher, and more preferably 800° C. or lower. The time of this heat treatment (calcination) is more preferably 3 hours or longer, and more preferably 12 hours or shorter.

[0035] The obtained powdered catalyst precursor can be filled in a reactor (e.g., a reaction tube) in a powder state. In this case, it is preferable to adjust the particle size so that the pressure loss in the catalyst precursor phase does not become excessively large. In order to ensure the surface area of ​​the catalyst precursor while suppressing the pressure loss in the catalyst precursor phase, it is preferable that the particle size of the catalyst precursor is as small as possible. In order to suppress pressure loss in the catalyst precursor phase, the catalyst precursor may be mixed with other materials, or may be molded and then filled. As the other materials, fillers (silica balls, alumina balls) that are inactive to the catalyst and do not deteriorate the catalyst performance can be used. In addition, molding can be performed by adding a binder that does not deteriorate the performance of the finally obtained catalyst to the catalyst precursor, kneading, and heating to sinter. Examples of binders (sintering agents) include silica-based, alumina-based, zirconia-based, and diatomaceous earth-based. In addition, examples of the shape after molding include tablets, pellets, spheres, and extrusions. By molding, strength and handleability can be increased.

[0036] Next, the obtained catalyst precursor is contacted with a carbon-containing gas. As a result, the carbon-containing gas is carbonized by an oxidation reaction. At the same time, the transition metal (transition metal oxide) present in an oxidized state on the catalyst precursor is reduced, so that carbon is supported at the same time as the reduction of the transition metal oxide, and a catalyst (catalyst for alkane dehydrogenation) in which the transition metal and carbon are supported can be formed. At this time, since the reduction of the transition metal oxide and the support of carbon can be performed simultaneously, carbon is generated between the transition metal oxide during the reduction of the transition metal oxide, and the aggregation of the transition metal crystallites can be suppressed.

[0037] The crystallite size of the transition metal supported on the catalyst (support), as the ratio of the crystallite size of the transition metal after contact with carbon-containing gas to the crystallite size when carbon-containing gas is not contacted, or the ratio of the crystallite size of the transition metal supported on the support when the carbon supported on the support does not contain fibrous carbon to the crystallite size of the transition metal when the carbon supported on the support does not contain fibrous carbon, is preferably 0.80 or less, more preferably more than 0.00 and 0.60 or less, more preferably 0.20 or more and 0.50 or less.The conditions shown below can be appropriately adjusted so as to fall within this range. In addition, in measuring the transition metal crystallite size supported on the carrier, the catalyst is subjected to powder X-ray analysis, and the obtained results can be used to calculate the diameter from the Scherrer formula using the peaks attributable to the transition metal crystallites. In the present invention, the powder X-ray analysis was performed using SmartLab / R / INP / DX (manufactured by Rigaku Corporation). The measurement conditions were Cu-Kα radiation as the X-ray source, tube voltage 45 kV, and tube current 150 mA. In addition, for example, when Ni is used as the transition metal, the diameter can be calculated using the peak attributable to the (112) plane at 2θ=44°. The standard of the ratio of the crystallite size of the transition metal supported on the catalyst (support) can be the crystallite size of the transition metal when the catalyst precursor is not contacted with a carbon-containing gas, or the crystal particle size of the transition metal supported on the support when the supported carbon does not contain fibrous carbon, as described above. The crystallite size used as the standard is preferably the crystallite size of the transition metal when the catalyst precursor is subjected to hydrogen reduction treatment (contact with a pretreatment gas containing hydrogen that does not contain a carbon-containing gas). In particular, it is preferable to use the crystal particle size of the transition metal supported on the support after the catalyst precursor is subjected to hydrogen reduction treatment (contact with a pretreatment gas containing hydrogen that does not contain a carbon-containing gas) under the conditions of Comparative Example 3 described later as the standard.

[0038] The carbon-containing gas preferably contains a hydrocarbon as a source of carbon (carbon source) to be supported on the catalyst precursor. The hydrocarbon is preferably an alkane having 2 to 5 carbon atoms. Examples of the alkane having 2 to 5 carbon atoms include ethane, propane, n-butane, isobutane, n-pentane, and isopentane. These may be used alone or in combination of two or more. When the step of producing a catalyst and the step of dehydrogenating an alkane using the obtained catalyst to produce an unsaturated hydrocarbon are performed continuously, the carbon source for carbon support and the alkane raw material for the dehydrogenation reaction may be different or the same hydrocarbon, but from the viewpoint of process simplification, it is preferable that they are the same hydrocarbon. In this case, the carbon source and the alkane raw material are preferably the above-mentioned alkanes having 2 to 5 carbon atoms (e.g., ethane, propane, n-butane, isobutane, n-pentane, isopentane), and more preferably isobutane.

[0039] The carbon-containing gas may contain an inert gas such as helium or nitrogen in addition to a carbon source.

[0040] The concentration of the carbon source (preferably a hydrocarbon) contained in the carbon-containing gas (volume ratio of the carbon source to the carbon-containing gas) is 1 capacity % or more and 30% or less by volume, and among these, 5 capacity % or more is particularly preferred, while 20 capacity % or less is particularly preferred. By setting the carbon source concentration to 1% by volume or more, a sufficient amount of carbon can be supported more satisfactorily, and the selectivity of unsaturated hydrocarbons can be further increased. Furthermore, by setting the carbon source concentration to 30% by volume or less, the support of excess carbon can be more easily controlled, and the decrease in the alkane conversion rate and the selectivity of unsaturated hydrocarbons can be more sufficiently suppressed.

[0041] The temperature in the step of supporting carbon on the catalyst precursor (the temperature when the catalyst precursor is contacted with a carbon-containing gas) is preferably 300°C or higher and 1000°C or lower, particularly preferably 400°C or higher, more preferably 700°C or lower, and particularly preferably 600°C or lower. By setting the temperature of this carbon supporting step to 300°C or higher, a more sufficient amount of carbon can be supported. In addition, by setting the temperature of this carbon supporting step to 1000°C or lower, the decrease in the amount of carbon supported and the decrease in catalytic activity due to the thermal decomposition reaction of the alkane of the carbon source can be more sufficiently suppressed.

[0042] The pressure in the step of supporting carbon on the catalyst precursor (the pressure when the catalyst precursor is contacted with the carbon-containing gas) can be appropriately selected depending on the type of carbon-containing gas used, but is preferably 0.01 MPa or more and 1 MPa or less. By setting the pressure to 0.01 MPa or more, it is possible to easily suppress the desorption of components on the carrier under reduced pressure. In addition, by setting the pressure to 1 MPa or less, it is possible to more sufficiently prevent the increase in reactivity due to pressurization, and it is possible to prevent the amount of carbon supported on the carrier from becoming excessive. Among the above, it is more preferable that it is 0.8 MPa or less, and particularly preferable that it is 0.5 MPa or less, while it is even more preferable that it is 0.05 MPa or more. The pressure may be atmospheric pressure (0.101 MPa).

[0043] The method for contacting the catalyst precursor with a carbon-containing gas can be a fixed-bed flow reaction method in which a carbon-containing gas is passed through a reactor (for example, a reaction tube) filled with the catalyst precursor.

[0044] The W / F ratio when the carbon-containing gas is brought into contact with the catalyst precursor is preferably 0.03 g·min / ml or more and 0.5 g·min / ml or less. Here, W is the mass (g) of the catalyst precursor packed in the reaction tube, and F is the flow rate (ml / min) of the carbon-containing gas flowing through the reaction tube packed with the catalyst precursor. That is, W / F is the mass of the catalyst precursor packed in the reaction tube relative to the flow rate of the carbon-containing gas flowing through the reactor, and is expressed by the following formula.

[0045] W / F = (amount of catalyst precursor packed in the reaction tube [g]) / (flow rate of carbon-containing gas flowing in the reaction tube [ml / min])

[0046] By setting the W / F to 0.03 g min / ml or more, it is possible to prevent the amount of carbon supported from becoming insufficient. Also, by setting the W / F to 0.5 g min / ml or less, it is possible to prevent the amount of carbon supported from becoming excessive. Among the above, it is particularly preferable that the W / F is 0.05 g min / ml or more, while it is particularly preferable that the W / F is 0.2 g min / ml or less.

[0047] (Method for Producing Unsaturated Hydrocarbons from Alkanes) In the method for producing unsaturated hydrocarbons according to an embodiment of the present invention, the catalyst according to the present invention is contacted with a mixed gas containing an alkane and carbon dioxide (hereinafter also referred to as a "reaction gas") to produce unsaturated hydrocarbons from an alkane.

[0048] The alkane raw material used in the dehydrogenation reaction of an alkane is not particularly limited, but an alkane having 2 to 5 carbon atoms is preferred. By using an alkane having 5 or less carbon atoms, it is possible to suppress the generation of by-products having a low carbon number due to a decomposition reaction. Examples of alkanes having 2 to 5 carbon atoms include ethane, propane, n-butane, isobutane, n-pentane, and isopentane. These may be used alone or in combination of two or more. Through the dehydrogenation reaction, ethylene is mainly produced from ethane, propylene from propane, butadiene from n-butane, isobutene from isobutane, pentene from n-pentane, and isoprene from isopentane.

[0049] In the production method according to the embodiment of the present invention, the above-mentioned dehydrogenation reaction of alkanes is carried out to produce the corresponding unsaturated hydrocarbons. This dehydrogenation reaction is carried out by contacting a mixed gas (reaction gas) containing alkanes and carbon dioxide with the catalyst according to the present invention. The molar ratio of carbon dioxide to alkanes contained in this mixed gas (reaction gas) is preferably 0.1 to 1.9, more preferably 0.25 or more, and more preferably 1.6 or less. When this molar ratio is less than 0.1, the concentration of carbon dioxide is low, and therefore the reactivity tends to decrease. On the other hand, when this molar ratio is more than 1.9, the concentration of carbon dioxide is high, and therefore the selectivity tends to decrease.

[0050] This mixed gas (reactive gas) may contain, in addition to alkanes and carbon dioxide, inert gases such as helium and nitrogen, water vapor (water), methane, hydrogen, etc., to the extent that the effects of the present invention are not impaired.

[0051] The concentration of the alkane in this mixed gas (reaction gas) is preferably 1% by volume or more and 30% by volume or less, more preferably 1% by volume or more, even more preferably 5% by volume or more, and more preferably 20% by volume or less. By having the concentration of the alkane be 1% by volume or more, it is possible to further suppress the decrease in the selectivity of the unsaturated hydrocarbons due to the improvement of the conversion rate of the alkane. In addition, by having the concentration of the alkane be 30% by volume or less, it is possible to further suppress the decrease in the conversion rate of the alkane.

[0052] The temperature of the dehydrogenation reaction of alkanes (the temperature when the mixed gas is contacted with the catalyst) is preferably 300° C. or higher and 1000° C. or lower, more preferably 400° C. or higher, and more preferably 700° C. or lower, and even more preferably 600° C. or lower. By setting the temperature of this dehydrogenation reaction to 300° C. or higher, more sufficient catalytic activity can be obtained. Furthermore, by setting the temperature of this dehydrogenation reaction to 1000° C. or lower, the decrease in the selectivity of unsaturated hydrocarbons and the decrease in catalytic activity due to the thermal decomposition reaction of alkanes can be further suppressed.

[0053] The pressure in the dehydrogenation reaction of an alkane can be appropriately selected depending on the type of alkane used in the reaction, but can usually be set to 1 MPa or less, and is preferably 0.01 MPa or more and 1 MPa or less. Among these, the pressure is more preferably 0.8 MPa or less, and even more preferably 0.5 MPa or less, while more preferably 0.05 MPa or more, and even more preferably 0.1 MPa or more. The pressure may be atmospheric pressure (0.101 MPa). By setting the pressure to 0.01 MPa or more, the contact between the active sites on the catalyst and the alkane during the reaction is more appropriately carried out, and the selectivity of the alkane is likely to be improved. In addition, by setting the pressure to 1 MPa or less, it is possible to further suppress a runaway reaction caused by excessive contact of the alkanes in the reaction gas and the generated unsaturated hydrocarbons with the active sites on the catalyst, and to increase the selectivity of the corresponding alkene.

[0054] The reaction type used in the method for producing unsaturated hydrocarbons according to the embodiment of the present invention is not particularly limited, and a typical type used in catalytic reactions can be adopted. For example, reaction types such as a fixed bed, a moving bed, and a fluidized bed can be mentioned. Among these, a fixed bed type can be preferably adopted because the apparatus is relatively simple and the process design is easy. That is, in the method for producing unsaturated hydrocarbons according to the embodiment of the present invention, the dehydrogenation reaction of an alkane can be carried out by a fixed bed flow type reaction type in which a mixed gas (reaction gas) containing the raw alkane, carbon dioxide, etc. is flowed through a reactor (e.g., a reaction tube) filled with the catalyst according to the present invention.

[0055] The W / F in the dehydrogenation reaction of an alkane is preferably 0.001 g min / ml or more and 1000 g min / ml or less, more preferably 0.01 g min / ml or more, and more preferably 100 g min / ml or less. Here, W is the mass (g) of the catalyst packed in the reaction tube, and F is the flow rate (ml / min) of the mixed gas (reaction gas) containing alkanes and carbon dioxide that is passed through the reaction tube packed with the catalyst. In other words, W / F is the mass of the catalyst packed in the reaction tube relative to the flow rate of the mixed gas (reaction gas) flowing through the reaction tube, and is expressed by the following formula.

[0056] W / F = (amount of catalyst packed in the reaction tube [g]) / (flow rate of mixed gas flowing in the reaction tube [ml / min])

[0057] By setting the W / F to 0.001 g min / ml or more, the reaction time of the alkane with the catalyst can be secured, and the conversion rate of the alkane can be improved. Also, by setting the W / F to 1000 g min / ml or less, the reaction time of the alkane with the catalyst can be prevented from becoming excessive, and further, the generated alkene can be prevented from reacting on the catalyst to become carbon dioxide, which can reduce the selectivity. EXAMPLES

[0058] EXAMPLES The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0059] Example 1 First, a catalyst (Ni-C / γ-Al2O3 catalyst) was prepared as follows. An aqueous solution was obtained by adding and dissolving 3.89 parts by mass of nickel nitrate hexahydrate (Wako Pure Chemical Industries, Ltd.) in 15 parts by mass of water so that the amount of Ni charged relative to γ-Al2O3 was 20% by mass. Then, 4 parts by mass of γ-Al2O3 (Nippon Light Metals Co., Ltd.) was added to this aqueous solution and mixed. Next, this mixture was heated to evaporate the water to obtain a solid. The obtained solid was pulverized and vacuum dried at 110°C for 12 hours. The crushed solid was further calcined at 550° C. for 1 hour (heating rate: 1° C. / min). The obtained solid was crushed again to obtain a powdered catalyst precursor 1 (γ-Al2O3 carrying nickel).

[0060] The obtained catalyst precursor 1 was packed into a quartz reaction tube with a diameter of 9 mm and a length of 35 mm installed in a fixed-bed flow-type reactor, and heated to 550°C while flowing helium. After that, the pretreatment gas containing 85.8 vol% helium and 14.2 vol% isobutane was set so that the W / F was 0.12 g min / ml. In this way, the pretreatment gas was flowed through the reaction tube for 3 hours, and a Ni-C / γ-Al2O3 catalyst with carbon supported on the catalyst precursor 1 was obtained. In addition, the obtained catalyst (Ni-C / γ-Al2O3 catalyst) was subjected to powder X-ray analysis. The X-ray analysis was performed using a SmartLab / R / INP / DX (Rigaku Corporation). The measurement conditions were Cu-Kα radiation as the X-ray source, a tube voltage of 45 kV, and a tube current of 150 mA. The Ni crystallite size was calculated using the peak at 2θ=44° that belongs to the (112) plane.

[0061] Next, this catalyst was used to produce isobutene from isobutane as follows. The catalyst obtained as above was packed in a reactor as it was, and a reaction gas adjusted to 73.7% by volume of helium, 14.2% by volume of isobutane, and 12.1% by volume of carbon dioxide was passed through the reactor, with each condition set so that the W / F was 0.017 g min / ml. Six hours after the start of the reaction gas flow, the gas at the outlet of the reaction tube was measured by gas chromatography to determine the isobutane conversion, isobutene selectivity, and isobutene yield. The results are shown in Table 1.

[0062] The "W / F" is expressed by the following formula. W / F = amount of catalyst precursor or catalyst packed in the reaction tube (g) / supply rate of carbon-containing gas or reaction gas supplied into the reaction tube (ml / min)

[0063] The isobutane conversion, isobutene selectivity and isobutene yield are expressed by the following formulas. Isobutane conversion (%) = (number of moles of isobutane reacted) / (number of moles of isobutane fed) Isobutene selectivity (%) = (moles of isobutene produced) / (moles of isobutane reacted) Isobutene yield (%) = (moles of isobutene produced) / (moles of isobutane fed)

[0064] Example 2 A catalyst (Ni-C / γ-Al2O3 catalyst) was prepared in the same manner as in Example 1, except that the flow time of the pretreatment gas was changed to 5 hours. Then, isobutene was produced in the same manner as in Example 1. The catalyst (Ni-C / γ-Al2O3 catalyst) was heated to 1000°C using simultaneous thermogravimetry and differential thermal analysis (TG-DTA), and the amount of supported carbon was measured from the weight loss at that time. In the weight change at this time, the weight loss when heated to 200°C was due to the desorption of adsorbed water, so the weight loss during the heating process from 200°C to 1000°C was calculated as being due to the supported carbon. Next, it was confirmed that the carbon in the catalyst was fibrous carbon using a scanning electron microscope (SEM) (SEM images are shown in Figures 1 and 2). The average diameter of the fibrous carbon was 41.9 nm. The results are shown in Table 1.

[0065] Example 3 Except for changing the flow time of the pretreatment gas to 7 hours, a catalyst (Ni-C / γ-Al2O3 catalyst) was prepared in the same manner as in Example 1, and then isobutene was produced in the same manner as in Example 1. The results are shown in Table 1.

[0066] Comparative Example 1 Except for not passing the pretreatment gas, a Ni / γ-Al2O3 catalyst was prepared in the same manner as in Example 1, and then isobutene was produced in the same manner as in Example 1. The results are shown in Table 1.

[0067] Comparative Example 2 Except for changing the pretreatment gas to a gas containing 80.0 vol% helium and 20.0 vol% hydrogen, setting the W / F to 0.0042 g min / ml, and changing the pretreatment gas flow time to 1 hour, a Ni / γ-Al2O3 catalyst was prepared in the same manner as in Example 1, and then isobutene was produced in the same manner as in Example 1. The results are shown in Table 1.

[0068] Comparative Example 3 A Ni / γ-Al2O3 catalyst was prepared in the same manner as in Comparative Example 2, except that the flow time of the pretreatment gas was changed to 5 hours. Then, isobutene was produced in the same manner as in Example 1. The results are shown in Table 1.

[0069] Comparative Example 4 A Ni / γ-Al2O3 catalyst was prepared in the same manner as in Example 1, except that the flow time of the pretreatment gas was changed to 1 hour. Then, isobutene was produced in the same manner as in Example 1. The results are shown in Table 1.

[0070] [Table 1]

Claims

1. A catalyst comprising a transition metal and carbon supported on a support, the carbon comprising fibrous carbon, The catalyst is an alkane dehydrogenation catalyst, the transition metal is Ni; A catalyst characterized in that the amount of the carbon relative to the transition metal is 1000 mass % or more and 2500 mass % or less.

2. The catalyst according to claim 1 , wherein the amount of the carbon relative to the transition metal is 1000% by mass or more and 2300% by mass or less.

3. 3. The catalyst according to claim 1, wherein the support is at least one selected from the group consisting of silica, alumina, zirconia, and titania.

4. 3. The catalyst according to claim 1 or 2, wherein the support is gamma-alumina.

5. mixing a solution containing a transition metal compound with a support, and heating to remove the solvent to obtain a catalyst precursor; contacting the catalyst precursor with a carbon-containing gas to form a transition metal and carbon supported catalyst; A method for producing the catalyst according to any one of claims 1 to 4, comprising: the catalyst is a catalyst for producing unsaturated hydrocarbons by contacting a mixed gas containing an alkane and carbon dioxide with the catalyst to produce unsaturated hydrocarbons from the alkane, In the step of forming the catalyst, a carbon-containing gas is contacted with the catalyst precursor to form fibrous carbon, and a catalyst is formed in which the carbon containing the fibrous carbon and the transition metal are supported.

6. 6. The method for producing a catalyst according to claim 5, wherein the step of obtaining a catalyst precursor comprises the steps of: mixing a solution in which a transition metal compound is dissolved with a support, and heating the mixture to evaporate the solvent to obtain a solid; and pulverizing the solid to obtain a powdered catalyst precursor.

7. The method for producing a catalyst according to claim 5 or 6, wherein the carbon-containing gas comprises a hydrocarbon.

8. The method for producing a catalyst according to claim 7, wherein the hydrocarbon is an alkane having 2 to 5 carbon atoms.

9. The method for producing a catalyst according to claim 7, wherein the hydrocarbon is isobutane.

10. The method for producing a catalyst according to any one of claims 7 to 9, wherein a volume ratio of the hydrocarbon to the carbon-containing gas is 1 vol% or more and 30 vol% or less.

11. The method for producing a catalyst according to claim 5 , wherein the temperature when the carbon-containing gas is brought into contact with the catalyst precursor is 300° C. or more and 1000° C. or less.

12. 12. The method for producing a catalyst according to claim 5, wherein a ratio (W / F) of an amount of the catalyst precursor to a supply rate of the carbon-containing gas when the carbon-containing gas is contacted with the catalyst precursor is 0.03 g min / ml or more and 0.5 g min / ml or less.

13. 13. The method for producing a catalyst according to claim 5, wherein a ratio of a crystallite size of the transition metal supported on the catalyst to a crystallite size of the transition metal on the catalyst precursor after a hydrogen reduction treatment is performed by contacting the catalyst precursor with a gas containing hydrogen that does not contain a carbon-containing gas, instead of contacting the catalyst precursor with the carbon-containing gas, is 0.80 or less.

14. In the hydrogen reduction treatment, The hydrogen-containing gas without carbon-containing gas is a gas containing 80% by volume of helium and 20% by volume of hydrogen, the ratio (W / F) of the amount of catalyst precursor to the supply rate of the gas when the catalyst precursor is contacted with the gas is 0.0042 g min / ml; The method for producing a catalyst according to claim 13, wherein the gas flow time is 5 hours.

15. A method for producing unsaturated hydrocarbons, comprising contacting a mixed gas containing an alkane and carbon dioxide with the catalyst according to any one of claims 1 to 4 to produce unsaturated hydrocarbons from the alkane.

16. The method for producing unsaturated hydrocarbons according to claim 15, wherein in the mixed gas, a molar ratio of the carbon dioxide to the alkane is 0.1 or more and 1.9 or less.

17. The method for producing unsaturated hydrocarbons according to claim 15 or 16, wherein the alkane is an alkane having 2 to 5 carbon atoms.

18. The method for producing unsaturated hydrocarbons according to claim 15 or 16, wherein the alkane is isobutane.

19. The method for producing unsaturated hydrocarbons according to any one of claims 15 to 18, wherein the temperature when the mixed gas is contacted with the catalyst is 300°C or higher and 1000°C or lower.

20. 20. The method for producing unsaturated hydrocarbons according to any one of claims 15 to 19, wherein a ratio (W / F) of the amount of catalyst to a supply rate of the mixed gas when the mixed gas is contacted with the catalyst is 0.001 g min / ml or more and 1000 g min / ml or less.

21. A method for producing unsaturated hydrocarbons, comprising producing a catalyst by the production method according to any one of claims 5 to 14, and subsequently contacting the resulting catalyst with a mixed gas containing an alkane and carbon dioxide to produce unsaturated hydrocarbons from the alkane.

22. A step of forming the catalyst according to any one of claims 1 to 4, in which a catalyst precursor having a transition metal compound supported on a carrier is contacted with a carbon-containing gas to support carbon containing fibrous carbon on the catalyst precursor, and a transition metal and carbon containing fibrous carbon are supported on the catalyst precursor; A method for producing unsaturated hydrocarbons, comprising the step of contacting a mixed gas containing an alkane and carbon dioxide with the obtained catalyst to produce unsaturated hydrocarbons from the alkane.

23. 23. The method for producing unsaturated hydrocarbons according to claim 21 or 22, wherein in the mixed gas, a molar ratio of the carbon dioxide to the alkane is 0.1 or more and 1.9 or less.

24. The method for producing unsaturated hydrocarbons according to claim 22 or 23, wherein the temperature when the carbon-containing gas is contacted with the catalyst precursor is 300° C. or higher and 1000° C. or lower.

Citation Information

Patent Citations

  • Removal of nitrogen oxide from gas stream

    JP1983076129A

  • Dehydrogenation catalyst

    JP1997075732A

  • Method for producing unsaturated hydrocarbon and dehydrogenation catalyst used for the method

    JP2013163647A

  • Catalyst for synthesizing hydrocarbons from CO and H2 and method for producing the same

    JP2013509290A

  • Method for producing oxidative dehydrogenation catalyst and alkene

    JP2014140827A