Anion exchange membrane and method for producing same
A 4VP-based anion exchange membrane with polyethylene woven fabric and vinyl chloride resin reinforcement addresses shrinkage issues, achieving high stability and permeability for efficient electrodialysis.
Patent Information
- Application Number
- JP2021051340
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-25
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-03-25
AI Technical Summary
Existing 4VP-based anion exchange membranes suffer from shrinkage upon contact with water, leading to poor dimensional stability, reduced current efficiency, and decreased water permeability when used in electrodialysis applications.
An anion exchange membrane with a pyridinium group as the anion exchange group, reinforced with a polyethylene woven fabric and vinyl chloride resin as a thickener, is developed, with specific parameters for the resin's degree of polymerization, thickness, and aperture ratio to enhance stability and permeability.
The membrane exhibits low shrinkage rates, high current efficiency, and improved water permeability, ensuring stable electrodialysis performance over time, particularly in acid concentration processes.
Smart Images

Figure 0007582662000004 
Figure 0007582662000001 
Figure 0007582662000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an anion exchange membrane having protonated pyridinium groups as anion exchange groups, and a method for producing the same. [Background technology]
[0002] Anion exchange membranes are formed from an anion exchange resin layer having a base sheet functioning as a reinforcing material as a core material, and are widely used in combination with cation exchange membranes or bipolar membranes for applications such as salt production, desalination, and electrodialysis for producing acids and alkalis from neutral salts.
[0003] As such an anion exchange membrane, one having a pyridinium group as the anion exchange group (hereinafter, sometimes referred to as 4VP-based anion exchange membrane) is known. This 4VP-based anion exchange membrane can be easily obtained by acid treatment of a precursor having a pyridyl group as a functional group. That is, by placing the pyridyl group in an acidic environment, a pyridinium group that functions as an anion exchange membrane is quickly generated. When such a 4VP-based anion exchange membrane is combined with a bipolar membrane and a cation exchange membrane to perform desalting by electrodialysis, acid is highly efficiently concentrated (see Patent Document 1). That is, the protons (H + This is because the anion exchange membrane prevents leakage of the anion salts into the desalting compartment.
[0004] However, 4VP-based anion exchange membranes have the drawback that they shrink when they come into contact with water. That is, 4VP-based anion exchange membranes function as ion exchange membranes by coordinating protons to the N atoms of the pyridine rings, but the pKa value is low and protons are coordinated only in an acidic environment. For this reason, deprotonation occurs when the membrane comes into contact with water, and at the same time as the protons are discharged, counterions are discharged and hydrated ions are released, which is thought to result in the entire membrane shrinking.
[0005] In addition, the dimensional stability of 4VP-based anion exchange membranes can be improved by using polyethylene powder as a thickening agent, but in this case, there is a problem that the current efficiency of the membrane decreases and the water permeability also decreases. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 5-184877 Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, an object of the present invention is to provide a 4VP-based anion exchange membrane in which membrane shrinkage due to contact with water is suppressed and which has excellent dimensional stability, and a method for producing the same. Another object of the present invention is to provide an anion exchange membrane which has high current efficiency and good water permeability in addition to dimensional stability, and a method for producing the same. [Means for solving the problem]
[0008] According to the present invention, in an anion exchange membrane having an anion exchange resin layer reinforced by a base sheet, the anion exchange resin layer contains an anion exchange resin containing a pyridinium group obtained by protonating a pyridyl group as an anion exchange group, and a vinyl chloride resin as a thickener; The anion exchange membrane is characterized in that the base sheet is made of a polyethylene woven fabric.
[0009] In the anion exchange membrane of the present invention (that is, the 4VP-based anion exchange membrane), the following aspects are preferably adopted. (1) The vinyl chloride resin has an average degree of polymerization of 700 to 1,200. (2) The vinyl chloride resin is contained in the anion exchange membrane in an amount of 5 to 30% by mass. (3) The polyethylene woven fabric base sheet has a thickness of 120 to 160 μm. (4) The base sheet made of the woven polyethylene fabric has an opening ratio of 35 to 55%. (5) The shrinkage rate of the membrane when immersed in a 0.5N HCl aqueous solution and then in pure water for three days is 2.3% or less. (6) Current efficiency is 55% or more and water permeability is 1000ml / m 2 -Be lower than Hr.
[0010] According to the present invention, there is also provided a method for producing a medicament for a medicament comprising the steps of: preparing a polymerizable composition comprising 4-vinylpyridine as a monomer component and a vinyl chloride resin as a thickener; impregnating a polyethylene woven substrate sheet with the polymerizable composition to produce a polymerizable sheet; overlapping the polymerizable sheet with a release sheet and winding it up into a roll; a polymerization step of heating the polymerizable sheet wound around the roll to polymerize the sheet; a release sheet peeling step of peeling the release sheet from the polymer sheet to obtain an ion exchange precursor membrane; a protonation step of immersing the ion exchange precursor membrane in an acid solution to protonate the pyridyl groups to obtain an anion exchange membrane; A method for producing an anion exchange membrane is provided, comprising:
[0011] In the production method of the present invention, it is preferable that the vinyl chloride resin is blended in the polymerizable composition so that the vinyl chloride resin is contained in an amount of 5 to 30% by mass in the resulting anion exchange membrane. Effect of the Invention
[0012] The anion exchange membrane of the present invention is called a 4VP-based anion exchange membrane, as can be understood from the fact that an anion exchange resin containing a protonated pyridinium group is used as the anion exchange group, but it has the characteristic that a specific base sheet (polyethylene woven fabric) is used and a specific thickener (vinyl chloride resin) is distributed in the anion exchange resin layer, which results in excellent dimensional stability and effective suppression of membrane shrinkage when contacted with water. For example, as shown in the examples described below, when a membrane treated with a 0.5N HCl aqueous solution is immersed in pure water for 3 days and then the shrinkage rate of the membrane is measured (see Examples for detailed conditions), the shrinkage rate of the conventionally known 4VP-based anion exchange membrane (Comparative Example 1; polyvinyl chloride woven fabric is used as the base sheet and NBR is used as the thickener) is 2.8%, while the shrinkage rate of the 4VP-based anion exchange membrane of the present invention (Examples 1 to 3) is suppressed to about 1.4 to 2.3%. In addition, the current efficiency is greater than 55%, and the water permeability is 1000 ml / m 2 ·Hr and has excellent current efficiency and water permeability. Furthermore, in Comparative Examples 2 and 3, in which polyethylene powder was used as a thickener instead of polyvinyl chloride resin, the shrinkage rate was kept low at 1.0 to 1.1%, but the current efficiency was low at 54% or less and the water permeability was 40,000 ml / m 2 ·Hr, and both are inferior to the present invention.
[0013] Thus, the 4VP-based anion exchange membrane of the present invention is excellent not only in dimensional stability but also in current efficiency and water permeability, and therefore can be used in electrodialysis in combination with a cation exchange membrane or a bipolar membrane, preventing breakage of the 4VP-based anion exchange membrane due to dimensional changes during cleaning of the inside of the apparatus and preventing the membrane from being reassembled due to dimensional changes during disassembly and reassembly, and allowing stable electrodialysis over a long period of time. In particular, the 4VP-based anion exchange membrane is most suitably used in electrodialysis for concentrating an acid in combination with a bipolar membrane and a cation exchange membrane. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view showing the structure of the 4VP-based anion exchange membrane of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] <4VP-based anion exchange membrane> With reference to FIG. 1, the 4VP-based anion exchange membrane of the present invention generally designated by 1 has a basic structure in which an anion exchange resin layer 3 is reinforced by a substrate sheet 5 .
[0016] The anion exchange resin used to form the anion exchange resin layer 3 contains a pyridinium group as an anion exchange group. That is, this anion exchange resin contains a repeating unit of 4-vinylpyridine, and as shown in the following formula, a proton (H + ) functions as an anion exchange group. [ka]
[0017] Incidentally, the Pka value of pyridine is as low as 5.25, and therefore the pyridyl group becomes a pyridinium that functions as an anion exchange group when protons are coordinated only in an acidic environment. In general anion exchange resins, the nitrogen atoms of the amino groups are thoroughly methylated to form a quaternary ammonium base that functions as an anion exchange group. That is, the present invention does not require any troublesome treatment or reaction to generate an anion exchange group, which is different from general quaternary ammonium salt-based anion exchange membranes.
[0018] Although the above-mentioned 4VP-based anion exchange membranes can easily be protonated by acid, they are easily deprotonated when in contact with water (or when the pH is increased). As mentioned above, when the membranes are deprotonated, counterions are expelled and hydrated ions are also released, resulting in a large shrinkage of the membrane. In order to overcome such drawbacks, in the present invention, vinyl chloride resin that functions as a thickener is dispersed in the anion exchange resin layer 3, and a polyethylene woven fabric is used as the base sheet 5. As shown in Fig. 1, this woven fabric is woven using warp threads 5a and weft threads 5b, and may be any of plain weave, twill weave, and satin weave, but plain weave is most suitable from the viewpoint of setting the opening ratio within a certain range, etc.
[0019] That is, although vinyl chloride resin sheets are known as substrate sheets for ion exchange membranes, the vinyl chloride resin used in the present invention is not used as a substrate sheet but as a thickener, and is therefore distributed in the anion exchange resin layer 3 in the form of particles (i.e., it is not in a sheet shape but is dispersed in the form of islands), and only polyethylene woven fabric is used as the substrate sheet 5. By employing such a combination, the shrinkage of the membrane seen in the conventionally known 4VP-based anion exchange membrane is suppressed, and not only is high dimensional stability obtained, but also current efficiency and water permeability are excellent.
[0020] In the present invention, the reason why the use of the polyvinyl chloride resin (thickener) and the polyethylene woven fabric as described above suppresses membrane shrinkage and improves current efficiency and water permeability has not been precisely elucidated, but the inventors presume it to be as follows. That is, the thickener is blended into the polymerizable composition (containing 4-vinylpyridine) for producing the anion exchange resin, and is used to increase the viscosity of the polymerizable composition to a level that allows it to be applied to a substrate sheet (woven fabric). Since it is used in the form of a powder or granule, it exists in the obtained anion exchange membrane (anion exchange resin layer 3) in a state of being dispersed in the matrix (sea) of the anion exchange resin in the form of islands. The polyvinyl chloride resin powder (PVC powder) used as such a thickener has a high affinity with the monomer contained in the polymerizable composition, and the monomer component is easily impregnated into the PVC powder. For this reason, it is considered that the PVC powder is well blended with the obtained ion exchange resin, and gaps are unlikely to be formed. Moreover, the polyethylene woven fabric used as the substrate has a high strength compared to porous films, nonwoven fabrics, or polyvinyl chloride resin woven fabrics. Therefore, by using the polyethylene woven fabric and polyvinyl chloride resin powder (PVC powder) in combination, a membrane that is not only high in dimensional stability (low shrinkage rate) but also excellent in current efficiency and water permeability can be obtained.
[0021] For example, when polyethylene powder is used instead of polyvinyl chloride resin powder, the monomer component does not easily penetrate the polyethylene powder, improving the dimensional stability, but the monomer component of the ion exchange resin does not easily penetrate the polyethylene powder, so gaps tend to form in the ion exchange resin, resulting in unsatisfactory current efficiency and water permeability. Furthermore, when a polyvinyl chloride resin sheet or a polyolefin porous sheet is used as the base sheet, either has a low reinforcing effect as a base sheet, and in particular in the case of a polyolefin porous sheet, the openings in the sheet are small, so the thickener particles do not penetrate into the openings, and the reinforcing effect of the thickener is not expressed.
[0022] In the 4VP-based anion exchange membrane of the present invention, the vinyl chloride resin used as a thickener preferably has an average degree of polymerization in the range of 650 to 1200 in order to ensure the coatability of the polymerizable composition when producing the anion exchange membrane. This is because the lower the degree of polymerization of vinyl chloride, the greater the thickening effect, and the higher the degree of polymerization, the smaller the thickening effect. This range is desirable in the present invention. In addition, from the viewpoint of ensuring coatability by thickening and at the same time obtaining a shrinkage suppression effect of the membrane without impairing the basic composition of the exchange membrane (anion exchange capacity, electrical resistance, etc.), it is preferable that the vinyl chloride resin is present in an amount of 5 to 25 mass %, particularly 6 to 20 mass %, in the anion exchange membrane 1.
[0023] Furthermore, the polyethylene woven fabric used as the base sheet 5 in the present invention is preferably one having a form that does not impair strength and avoids an increase in electrical resistance due to the use of vinyl chloride resin. For example, the thickness d of the polyethylene woven fabric (base sheet 5) is preferably in the range of 120 to 160 μm, and the opening ratio is preferably in the range of 35 to 55%. That is, it is considerably thinner than the thickness of various woven fabrics conventionally used as base sheets, and the opening ratio is in a relatively large range. Moreover, the diameter of polyethylene monofilament yarn is relatively thin, in the range of about 60 to 80 μm.
[0024] By selecting the substrate sheet 5 as described above, the electrical resistance of the 4VP-based anion exchange membrane 1 is 5.0 Ω cm when measured in 0.5 mol / l hydrochloric acid at 25° C. 2 It is preferable that the resistance be set in the range below, and more preferably 4.5 Ω cm 2 The range is as follows:
[0025] The thickness D of the 4VP-based anion exchange resin layer 3 is preferably in the range of about 100 to 200 μm in terms of strength and ease of handling, and the anion exchange groups (cationized pyridyl groups) of the 4VP-based anion exchange resin are desirably introduced into the resin at a ratio that ensures an ion exchange capacity of about 0.9 to 1.4 meq / g-dry mass. If more anion exchange groups than necessary are introduced, the shrinkage rate may increase during deprotonation, and if the amount of anion exchange groups is small, the ion exchange capacity will not be fully exerted.
[0026] As will be apparent from the examples described later, the 4VP-based anion exchange membrane 1 of the present invention has a shrinkage rate (dimensional change) of less than 2.5% and a current efficiency of 55% or more, and more preferably has a shrinkage rate (dimensional change) of less than 2.3% and a current efficiency of 60% or more, and a water permeability of 1000 ml / m 2 ·Hr. The moisture content is about 13 to 21%, and the burst strength is about 1.0 to 1.1 MPa. The measurement method for each parameter is described in the Examples.
[0027] <Production of 4VP-based anion exchange membrane 1> The 4VP-based anion exchange membrane 1 of the present invention as described above is produced through a polymerizable composition preparation step, a polymerizable sheet preparation step, a roll winding step, a polymerization step, a release sheet peeling step, and a protonation step. Each step will be described below in order.
[0028] Polymerizable composition preparation step; This step is a step for preparing a polymerizable composition for obtaining a polymer (anion exchange resin precursor) that becomes an anion exchange resin by protonation. Therefore, it is essential that the monomer component contains 4-vinylpyridine. However, since the use of 4-vinylpyridine alone results in significant shrinkage, other monomers, crosslinkable monomers, and polymerization initiators are used to adjust the physical properties. In addition, since 4-vinylpyridine is a compound that serves as a source of anion exchange groups, it is used in the polymerizable composition in an amount that will provide the above-mentioned ion exchange capacity. For example, it is used in an amount of 15 to 35 parts by mass, particularly 18 to 30 parts by mass, per 100 parts by mass of the total amount of the polymerizable composition (corresponding to 100 parts by mass of the anion exchange resin).
[0029] Examples of other monomers copolymerizable with 4-vinylpyridine include styrene, vinyltoluene, vinylxylene, α-methylstyrene, vinylnaphthalene, acrylonitrile, etc. In principle, conventionally used monomers having an anion exchange group, such as nitrogen-containing vinyl compounds such as vinylimidazole, vinylbenzyltrimethylamine, and vinylbenzyltriethylamine, can also be used.
[0030] The crosslinkable monomer is used to densify the anion exchange resin and to increase the swelling inhibition property and membrane strength, and is not particularly limited. Examples of the crosslinkable monomer include divinyl compounds such as divinylbenzene, divinyl sulfone, butadiene, chloroprene, divinyl biphenyl, trivinylbenzenes, divinyl naphthalene, diallylamine, divinyl pyridine, 1,2-bis(vinylphenyl)ethane, ethylene glycol dimethacrylate, and N,N-methylene bisacrylamide. Such a crosslinkable monomer is generally used in an amount of 0.1 to 50 parts by mass, particularly 1 to 40 parts by mass, per 100 parts by mass of the total amount of 4-vinylpyridine and other monomers copolymerizable therewith (hereinafter referred to as the basic monomer component).
[0031] The polymerization initiator may be any known one without any particular limitation.Specific examples of the polymerization initiator include organic peroxide-based polymerization initiators such as octanoyl peroxide, lauroyl peroxide, t-butyl peroxy-2-ethylhexanoate, benzoyl peroxide, t-butyl peroxyisobutyrate, t-butyl peroxylaurate, t-hexyl peroxybenzoate, and di-t-butyl peroxide, and azo-based polymerization initiators such as azobisisobutyronitrile. The amount of such a polymerization initiator is preferably 0.1 to 20 parts by mass, and more preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the basic monomer component.
[0032] Furthermore, in the present invention, a vinyl chloride resin is used as a thickener for the polymerizable composition containing the above-mentioned various components to ensure a viscosity that allows coating without causing sagging. The vinyl chloride resin preferably has the above-mentioned average degree of polymerization and is used in the form of a powder or granules. This average particle size varies due to heating during polymerization, and does not coincide with the dispersed particle size of the vinyl chloride resin in the anion exchange resin. However, it is preferable that the average particle size is determined by the 50% particle size (D ) calculated by volume, measured by a laser diffraction scattering method, for example. 50 ) in the range of 0.1 to 50 μm. If the particle size is too large, it becomes difficult for the particles to penetrate into the openings in the polyethylene woven fabric (base sheet 5), which may reduce the shrinkage suppression effect of the film. If the particle size is too small, the particles will be difficult to handle and difficult to obtain. As mentioned above, the amount of vinyl chloride resin used as such a thickener is within the range of 5% by mass to 25% by mass, particularly 6% by mass to 20% by mass, present in the final anion exchange membrane 1, and is used in an amount such that the polymerizable composition exhibits appropriate coatability (usually about 5 to 30 parts by mass per 100 parts by mass of the polymerizable composition).
[0033] In the present invention, thickeners other than vinyl chloride resins can also be used as long as they are small enough not to inhibit the film shrinkage suppression effect of the vinyl chloride resin described above. Examples of such thickeners include ethylene-propylene copolymers, saturated aliphatic hydrocarbon polymers such as polybutylene, styrene-based polymers such as styrene-butadiene copolymers, nitrile butadiene rubber, hydrogenated nitrile butadiene rubber, epichlorohydrin rubber, chlorinated polyethylene rubber, or copolymers of these with various comonomers (for example, vinyl toluene, vinyl xylene, chlorostyrene, chloromethylstyrene, α-methylstyrene, α-halogenated styrene, α,β,β'-trihalogenated styrene, and other styrene monomers, monoolefins such as ethylene and butylene, and conjugated diolefins such as butadiene and isoprene).
[0034] Furthermore, in order to impart flexibility to the film-like material after polymerization, the above-mentioned polymer composition may be mixed with an appropriate amount of plasticizer as necessary. Examples of the plasticizer include phthalates such as dioctyl phthalate and dibutyl phthalate, adipic esters such as dioctyl adipate and diisononyl adipate, epoxies such as styrene oxide, and ethers such as diphenyl ether and dibenzyl ether.
[0035] The above-mentioned components are mixed uniformly in a typical liquid stirring blade type tank, thereby preparing a polymerizable composition.
[0036] Polymerizable sheet preparation process; The polymerizable composition prepared as described above is applied to a polyethylene woven fabric, which is a base sheet 5, and the openings of the woven fabric are filled with the polymerizable composition to produce a polymerizable sheet. This polymerizable sheet is the source of the anion exchange resin layer 3 in Fig. 1, and the above-mentioned polyethylene woven fabric having a reinforcing effect as a core material is present inside the polymerizable sheet.
[0037] The method for applying the polymerizable composition to the polyethylene woven fabric is not particularly limited, and generally, a method of immersing the polyethylene woven fabric in the polymerizable composition by brush coating or roll coating is employed, but a method such as spraying can also be employed. Depending on the viscosity of the polymerizable composition, a method of contacting the polymerizable composition with the polyethylene woven fabric under reduced pressure can also be employed. The thickness of the polymerizable sheet thus produced (the coating thickness of the polymerizable composition) is set so that the thickness after polymerization and curing becomes the thickness of the anion exchange resin layer 3 described above (about 100 to 200 μm).
[0038] Roll winding process; In the present invention, the polymerizable sheet prepared as described above is overlapped with a release sheet and wound up into a roll. The roll body obtained in this manner is for efficient heating in the subsequent polymerization step. That is, if the polymerizable sheet is heated as it is, a large oven is required, which increases the production cost, but if the polymerizable sheet is heated in the form of a roll body, it can be heated in a compact oven. If the release sheet is not superimposed, the coated layers of the polymerizable composition will adhere to each other and become integrated, making it impossible to wind the coated layers around a roll.
[0039] That is, the release sheet used above is unnecessary as an anion exchange membrane, and is peeled off after polymerization. Therefore, as such a release sheet, various materials can be used as long as they do not adversely affect the polymerization of the polymerizable composition and can be easily peeled off from the polymer. Usually, a polyethylene terephthalate (PET) film, which is easily available, is used.
[0040] Polymerization process; As will be understood from the above description, the roll of the polymerizable sheet superimposed on the release sheet obtained above is heated, thereby obtaining a polymer of the polymerizable composition.
[0041] The heating temperature for polymerization is set within an appropriate range depending on the type of monomer component and polymerization initiator used in combination with 4-vinylpyridine, but it should naturally be lower than the melting points of the polyethylene used as the base sheet 5 and the polyvinyl chloride resin used as the thickener, and is generally set in the range of 70 to 90°C. The polymerization is carried out using an oven or the like, and although it can be carried out in an air atmosphere, it is preferable to carry out the polymerization in a nitrogen atmosphere since the polymerization may be inhibited by oxygen in the air. The polymerization time varies depending on the polymerization temperature, etc., but is generally about 2 to 5 hours.
[0042] Release sheet removal process; After polymerization, the roll is unwound and the release sheet is peeled off to remove the polymer sheet obtained by polymerization of the polymerizable composition. This polymer sheet is called an ion exchange precursor membrane.
[0043] Protonation step; This step is a step in which a proton is coordinated to the nitrogen atom of the pyridyl group contained in the ion exchange precursor membrane obtained above to produce a pyridinium capable of functioning as an anion exchange group. Such protonation is carried out by contacting the ion-exchange precursor membrane with an acid, and generally can be easily carried out by immersing the ion-exchange precursor membrane in an aqueous acid solution.
[0044] Various acids can be used, but generally, hydrochloric acid, sulfuric acid, and phosphoric acid are preferably used, and the acid concentration is preferably about 1 to 3N.
[0045] After the protonation step is completed, the membrane is washed with water, cut into pieces of an appropriate size, and used as an anion exchange membrane.
[0046] The 4VP-based anion exchange membrane 1 of the present invention obtained in this manner can be applied to various electrodialysis methods, and is most preferably used in electrodialysis devices in combination with a bipolar membrane or a cation exchange membrane for concentrating acids. EXAMPLES
[0047] EXAMPLES The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The base materials and thickeners used in the examples and comparative examples are shown below.
[0048] 1) Base material; Polyolefin-based woven fabric High density polyethylene monofilament woven fabric (PE-33D-120: NBC Meshtec Co., Ltd.) Warp: 76μm diameter - 120 threads per inch (33 denier) Weft: 76μm diameter - 120 threads per inch (33 denier) Thickness: 132μm Opening ratio: 41% Polyvinyl chloride woven fabric, manufactured by Teijin Ltd. Product name: V-7275 Warp: 274μm - 86 threads per inch (84dtex) Weft: 213μm - 73 threads per inch (84dtex) Thickness: 86μm Opening ratio: 3%
[0049] 2) Thickener PVC powder PQB-83: Manufactured by Shin-Daiichi Vinyl Corporation (Particle size 10~50μm, average degree of polymerization: 700) P-22: Manufactured by Shin-Daiichi Vinyl Corporation (Particle size 0.1~10μm, average degree of polymerization: 1050) PE powder LE-1080: Manufactured by Sumitomo Seika Chemicals Co., Ltd. (particle size 0.1~10μm) EA-209: Sumitomo Seika Chemicals Co., Ltd. (particle size 0.1~15μm)
[0050] Other thickening agents H-NBR: Hydrogenated nitrile butyl rubber (Manufactured by Zeon Corporation, product name: zetpol2000L) NBR: Nitrile butyl rubber (JSR Corporation, product name: N230SH)
[0051] The characteristics of the ion exchange membranes shown in the examples and comparative examples were measured by the following methods.
[0052] <1: Opening ratio of filament substrate> The calculation was made according to the following formula (1) from the wire diameter (μm) and mesh number of the thread constituting the substrate. Opening rate (%) = (Opening) 2 / (opening + wire diameter) 2 (1) The coefficients in the above formula (1) are as follows: Opening (μm) = 25400 / mesh number-wire diameter (μm) Mesh count = number of threads per inch (average value)
[0053] <2: Shrinkage rate> The ion exchange membrane was immersed in a 0.5 mol / L-HCl aqueous solution for 12 hours or more, and then the dimensions of the ion exchange membrane were measured (L0). The ion exchange membrane was then thoroughly washed with ion exchange water, and immersed in ion exchange water for 72 hours, after which the dimensions of the membrane were measured (L1), and the shrinkage rate was calculated using the following formula (2). Shrinkage rate (%) = (1 - L1 / L0) × 100 (2)
[0054] <3: Current efficiency> A two-chamber cell having the following configuration was used. Cathode (silver chloride plate); (0.5mol / L-hydrochloric acid) / anion exchange membrane / (3mol / L-hydrochloric acid) Anode (silver plate); Liquid temperature 25℃, current density 10A / dm 2After passing a current at 1000 V for 1 hour, the solution on the cathode side was collected. The hydrochloric acid concentrations of the collected solution and the initial solution were quantified using an aqueous sodium hydroxide solution with a potentiometric titrator (AutoTitrator manufactured by KEM), and the current efficiency was calculated using the following formula (3). Current efficiency (%) = {1-(C S -C B ) / (I × t / F)} × 100 (3) The coefficients in the above formula (3) are as follows: C B : Initial solution concentration C S : Concentration of liquid recovered after energization I: Current value (A) t: Energization time (sec) F: Faraday constant (96500C / mol)
[0055] <4: Burst strength of ion exchange membrane> The ion exchange membrane was immersed in a 0.01 mol / L-HCl aqueous solution for 4 hours or more, and then thoroughly washed with ion exchange water. Then, without drying the membrane, the burst strength was measured in accordance with JIS-P812 using a Mullen burst tester (manufactured by Toyo Seiki Co., Ltd.).
[0056] <5: Electrical resistance> An ion exchange membrane was sandwiched between a two-chamber cell with platinum black electrodes, and 0.5 m The electrodes were filled with an ion exchange membrane and the resistance between the electrodes was measured at 25°C using an AC bridge (frequency 1000 cycles / sec). The difference between the electrode resistance and the resistance between the electrodes without the ion exchange membrane was used to determine the membrane resistance (Ω cm 2 The ion exchange membrane used in the above measurement was previously equilibrated in a 0.5 mol / L HCl aqueous solution.
[0057] <6: Film thickness> The ion exchange membrane was immersed in 0.5 mol / L-HCl solution for more than 4 hours, and then wiped with tissue paper. Wipe off the moisture on the surface of the membrane with paper and measure it with a micrometer MED-25PJ (Micrometer Corporation) The measurements were performed using a meter (manufactured by Tsutoyo Corporation).
[0058] <7:Water permeability> When an ion exchange membrane is placed in a cylindrical cell, 50 ml of water is poured into the top, and a pressure of 0.1 MPa is applied from above, the amount of water W that permeates the ion exchange membrane in one hour is pw The effective area of the membrane was 12.6 m. 2 It is. Water permeability (mL / (m 2 hr))=W pw / (S × T) · · · (4) The coefficients in the above formula (4) are as follows: S: effective area of the membrane (m 2 ) T: Test time (hr)
[0059] <8: Ion exchange capacity and water content> The ion exchange membrane was immersed in a 1 mol / L HCl aqueous solution for 10 hours or more. After that, the counter ions were replaced from chloride ions to nitrate ions with a 1 mol / L NaNO3 aqueous solution, and the liberated chloride ions were quantified using a potentiometric titrator (COMTITE-900, Hiranuma Sangyo Co., Ltd.) with a silver nitrate aqueous solution (quantified value is expressed in Amol). Next, the same ion exchange membrane was immersed in a 1 mol / L-NaCl aqueous solution for more than 4 hours to remove ions. The membrane was thoroughly washed with exchanged water. The surface moisture was then wiped off with tissue paper, and the mass W of the membrane when wet was measured. The membrane was then dried under reduced pressure at 60°C for 5 hours, and its weight D when dry was measured. Based on the above measurements, the ion exchange capacity and water content of the ion exchange membrane were calculated using the following formulas (5) and (6). Ion exchange capacity [meq / g-dry mass] = A × 1000 / D (5) Moisture content [%]=100×(WD) / D···(6)
[0060] <9: Calculation method for PVC content> The ion exchange precursor membrane and the substrate sheet were cut into 10 cm squares and weighed, and the PVC content was calculated using the following formula (7). PVC content in ion exchange membrane [%] = T × (MB) × 100 (7) The coefficients in the above formula (7) are as follows: M: Weight of 10 cm square ion exchange precursor (g) B: Weight of 10 cm square base sheet (g) T: Proportion of PVC in the polymerizable composition
[0061] <Example 1> A mixture of the following formulation was prepared: Styrene (St) 50 parts by mass 57% divinylbenzene (DVB) (other component is ethylvinylbenzene) 21 parts by weight 4-Vinylpyridine 29 parts by mass Benzoyl peroxide (BW) (Niper BW, manufactured by Nippon Oil & Fats Co., Ltd.) 5.3 parts by mass
[0062] To this mixture was added 30 parts by mass of polyvinyl chloride powder (PQB-83) to obtain a homogeneous polymerizable composition. Next, a high-density polyethylene monofilament woven fabric (PE-33D-120) was prepared as a polyolefin-based woven fabric.
[0063] The polymerizable composition obtained above was applied onto the above-mentioned high-density polyethylene monofilament woven fabric (PE-33D-120), and both sides were covered with polyester film as a release material, followed by polymerization at 75° C. for 3 hours. The resulting polymer membrane was then immersed in 2 mol / L hydrochloric acid at 35° C. for 23 hours to obtain a pyridinium-modified anion exchange membrane. The structure of the anion exchange membrane is shown in Table 1. The properties of the anion exchange membrane obtained are shown in Table 2.
[0064] <Examples 2 to 3, Comparative Examples 1 to 3> An anion exchange membrane was prepared in the same manner as in Example 1, except that the mixture was mixed in the amount shown in Table 1 and the base material and thickener were used as shown in Table 1. The membrane properties of the obtained anion exchange membrane are shown in Table 2.
[0065] [Table 1]
[0066] [Table 2]
[0067] As is clear from the above Examples and Comparative Examples, when a membrane treated with a 0.5N HCl aqueous solution was immersed in pure water for 3 days and then the shrinkage rate of the membrane was measured (see Examples for detailed conditions), the shrinkage rate of the conventionally known 4VP-based anion exchange membrane (Comparative Example 1; using a polyvinyl chloride woven fabric as a base sheet and NBR as a thickener) was 2.8%, while the shrinkage rate of the 4VP-based anion exchange membrane of the present invention (Examples 1 to 3) was suppressed to about 2.1 to 2.3%. In addition, the current efficiency was greater than 55%, and the water permeability was 1000 ml / m 2 ·Hr and has excellent current efficiency and water permeability. Furthermore, in Comparative Examples 2 and 3, in which polyethylene powder was used as a thickener instead of polyvinyl chloride resin, the shrinkage rate was kept low at 1.6 to 1.9%, but the current efficiency was low at 54% or less and the water permeability was 40,000 ml / m 2 ·Hr, both of which are inferior to the present invention. [Explanation of symbols]
[0068] 1:4VP anion exchange membrane 3: Anion exchange resin layer 5: Base sheet (polyethylene woven fabric)
Claims
1. In an anion exchange membrane having an anion exchange resin layer reinforced by a substrate sheet, the anion exchange resin layer contains an anion exchange resin containing a pyridinium group obtained by protonating a pyridyl group as an anion exchange group, and a vinyl chloride resin as a thickener in an amount of 5 to 25% by mass in the anion exchange membrane; The anion exchange membrane, wherein the base sheet is made of a polyethylene woven fabric.
2. The anion exchange membrane according to claim 1, wherein the vinyl chloride resin has an average degree of polymerization of 650 to 1,200.
3. The anion exchange membrane described in claim 1 or 2, which does not contain polyethylene powder.
4. The anion exchange membrane according to any one of claims 1 to 3, wherein the substrate sheet made of the polyethylene woven fabric has a thickness of 120 to 160 µm.
5. 5. The anion exchange membrane according to claim 4, wherein the substrate sheet made of the polyethylene woven fabric has an opening ratio of 35 to 55%.
6. The anion exchange membrane according to any one of claims 1 to 5, wherein the membrane is immersed in a 0.5N-HCl aqueous solution, the membrane dimensions are measured (L 0 ), and then the membrane is immersed in pure water for 3 days, the membrane dimensions are measured (L 1 ), and the membrane shrinkage rate calculated by the following formula (2) is 2.3% or less. Shrinkage rate (%)=(1−L 1 / L 0 )×100 (2)
7. The current efficiency is 55% or more, and the water permeability is 1000 ml / m 2 The anion exchange membrane according to any one of claims 1 to 6, wherein the anion exchange membrane has a melting point of 1000 to 2000 mmHr.
8. preparing a polymerizable composition comprising 4-vinylpyridine as a monomer component and a vinyl chloride resin as a thickener; A step of impregnating a polyethylene woven substrate sheet with the polymerizable composition to produce a polymerizable sheet; winding the polymerizable sheet onto a roll over a release sheet; a polymerization step of heating the polymerizable sheet wound around the roll to polymerize the sheet; a release sheet peeling step for peeling the release sheet from the polymer sheet to obtain an ion exchange precursor membrane; a protonation step of immersing the ion exchange precursor membrane in an acid solution to protonate the pyridyl groups to obtain an anion exchange membrane; The method for producing the anion exchange membrane according to claim 1, comprising:
9. The method for producing an anion exchange membrane according to claim 8, wherein the vinyl chloride resin is blended in the polymerizable composition so that the vinyl chloride resin is contained in an amount of 5 to 25% by mass in the resulting anion exchange membrane.
Citation Information
Patent Citations
Ion exchange membranes and their manufacturing methods
CN106536051B
Production of acid
JP1993184877A
Bipolar membrane and method for producing the same
JP2010132829A
Ion exchanger
JP2012176373A
Ion-exchange membrane for water electrolysis, and method for manufacturing the ion-exchange membrane
JP2018127506A