Formation of organic electrografted coatings on conductive or semiconductive surfaces.
The electrografting method using diazonium salts and monomers addresses the challenges of adhesion and thickness control in organic coatings on conductive surfaces by forming stable, reproducible polymeric films on diverse substrates, from nanometers to micrometers thick, enhancing adhesion and versatility.
Patent Information
- Application Number
- JP2020180291
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2006-02-28
- Filing Date
- 2020-10-28
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2027-02-28
AI Technical Summary
Existing methods for forming organic coatings on conductive or semiconductive surfaces face limitations in achieving effective adhesion and control over coating thickness, particularly in ultrathin layers, due to the dependence on specific chemical interactions between precursor molecules and surfaces, which are often unstable and difficult to reproduce.
A method involving electrografting using a solution containing diazonium salts and chain-polymerizable monomers, where a time-dependent electrode potential is applied to form stable organic coatings by electroreduction, allowing for the formation of adhesive polymeric films on various surfaces.
This method enables the reproducible deposition of coatings ranging from nanometers to micrometers thick, providing strong adhesion and control over film thickness, suitable for diverse conductive or semiconductive substrates, and allowing for the use of a variety of polymers, including biodegradable and hydrophilic/hydrophobic coatings.
Smart Images

Figure 0007582839000010 
Figure 0007582839000011 
Figure 0007582839000012
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of organic surface coatings in the form of organic coatings on surfaces, more particularly to the use of appropriately selected solutions for the simple and reproducible formation of organic coatings on conductive or semiconductive surfaces or on parts or portions of surfaces by electrochemical or electrografting. [Background technology]
[0002] There are several prior art techniques for depositing thin organic coatings on substrates, each of which relies on a specific group or class of precursor molecules. The methods of forming coatings by centrifugation or "spin coating", immersion ("dipping"), or evaporation ("spraying") do not require that the molecules deposited have a particular affinity with the substrate in question. In fact, the method itself only forms a coating on the surface, whose cohesion is mainly due to the cohesive energy of the coating, which can be reinforced by post-treatment, e.g. cross-linking, to improve the stability of the coating.
[0003] It is possible to increase the stability of the interfaces in these processes by using special molecules that can self-assemble on the surface. In the prior art, these molecules are called molecules that give self-assembled monolayers or SAMs (Ulman A., "Year introduction to ultrathin organic films from Langmuir-Blodgett films to coil-assembly", 1991, Boston, Academic Press). There is usually no direct relationship between self-assembly, which essentially describes the lateral interactions between adjacent molecules in a more or less close-packed arrangement, and the overall "close-packed" layer having an affinity for the underlying surface. In many instances, such close-packed monolayers have also been obtained with mono- or bifunctional molecules that have a strong affinity at one end for the surface, i.e., monolayer brushes are obtained with a high density of molecules on the surface, even though these molecules have limited lateral interactions and therefore are not considered to be self-assembling. Even though the underlying mechanisms explaining the formation of the monolayer are different in these two cases, there seems to be a tendency to refer to the ultrathin layers (sometimes monolayers) that are actually formed with dense bonding on the surface as SAMs due to the strong bonding on the surface. A "true" SAM, with only lateral interactions, does little (if any) to improve adhesion at the interface, but mono- or bifunctional molecules added to the dip or spray formulation can have a definite effect by strengthening the interface via the anchoring points. Since the bonding of the mono- or bifunctional molecules is important for this strengthening, it will be necessary to consider the precursor-surface bond as a whole. As an example, it is known that sulfur-containing molecules have a strong affinity for gold, silver or copper, trihalogenosilanes for oxides such as silica or alumina, polyaromatic molecules for graphite or carbon nanotubes, etc. In all cases, the formation of the coating relies on specific physicochemical interactions that cause a chemical reaction between a part of the molecular precursor (e.g., the sulfur atom in the case of thiols) and a specific "receptor" site on the surface. In preferred cases, ultrathin layers (<10 nm) can be obtained at room temperature by spraying or dipping.
[0004] However, the formation of interfacial bonds is very much related to both the precursor and the surface, so that favorable bonds are in practice limited to almost "ideal" situations. Silanes give interfacial Si-O-Si interfacial bonds, which are probably the strongest of all chemical reactions, but these bonds are easily hydrolyzed in water at room temperature. Thiols give fairly strong bonds on gold surfaces, but are easily desorbed at 60° C., or at room temperature in good solvents, or on contact with liquid media containing oxidized forms of thiol groups. Overall, the possibilities for obtaining good adhesion on metal and / or semiconducting surfaces using self-assembly and / or mono- or bifunctional molecules are very limited. This is all the more true when the surfaces are obtained by certain special techniques, such as sputtering, or by physical or chemical vapor deposition, because the obtained surfaces are usually non-stoichiometric and of non-standard composition.
[0005] Nevertheless, these spray and immersion techniques are very versatile, applicable to most types of surfaces and extremely reproducible, provided that favorable cases can be taken into account. However, these techniques do not promote an effective bond between the coating and the substrate (apart from mere physical absorption) and the thickness of the coating is hardly controllable, especially when ultrathin layers (<20 nanometers) are the goal. Moreover, the technique of spin-coating can only deposit uniformly if the surface to be coated is mainly planar (see French patent application FR2843757). The quality of the coating obtained by spray-coating (in terms of homogeneity and conformality) is related to the wetting of the substrate by the sprayed liquid, since the deposit becomes substantially filmogenic only if the droplets coalesce on the surface. Thus, for a given polymer, there are generally only a few organic solvents that can give satisfactory results, in terms of control of both the homogeneity and conformality of the coating.
[0006] Other techniques for forming organic coatings on the surface of a support, such as those described in the article "Film deposition by plasma techniques" by Konuma M, (1992) Springer Verlag, Berlin, or in the article "Plasma polymerization process" by Biederman H. and Osada Y., 1992, Elsevier, Amsterdam, plasma deposition, or photochemical activation, are based on a similar principle, generating unstable derivatives of precursor molecules near the surface, which ultimately form a coating on said surface. Plasma deposition does not usually require that the precursors have special chemical properties, whereas photoactivation requires the use of photosensitive precursors, the structure of which is modified under irradiation.
[0007] These techniques typically produce adherent coatings on the treated surfaces, but it is generally difficult, if at all, to distinguish whether this adhesion is due to cross-linking of the coating structurally closed around the object or due to the formation of an actual bond at the interface between the coating and the surface.
[0008] Polymer electrografting is another technique based on forming a polymer layer on a surface in situ, i.e. from a bath of precursors, rather than from a prefabricated polymer. The surface to be coated is electrically polarized, which acts as a polymerization initiator and causes surface polymerization by a propagation chain reaction (S. Palacin and Al, "Molecule-to-metal bonds: electrografting polymers on conducting surfaces", ChemPhysChem, 2004, 10, 1468).
[0009] It is interesting to note that the reaction of the polarized surface with the first monomer is a step that creates a chemical bond that is then stabilized by polymerization propagation. Thus, the presence of a coating at the end of the process is a direct evidence or footprint of a chemical bond existing between the coating and the surface. According to this reaction mechanism, there can be no polymer coating on the surface without charge transfer and bond formation with the first monomer.
[0010] Electron-poor "vinyl-based" molecules, i.e., molecules that contain electron-withdrawing functional groups (eg, acrylonitrile, acrylates, vinylpyridines), are particularly suited to this process, which proceeds via an anionic propagation mechanism.
[0011] The reaction mechanism of electrografting is described inter alia in C. Bureau et al., Macromolecules, 1997, 30, 333, C. Bureau and J. Delhalle, Journal of Surface Analysis, 1999, 6(2), 159, and C. Bureau et al., Journal of Adhesion, 1996, 58, 101.
[0012] The growth of the polymer layer proceeds via anionic propagation in cathodic electrografting. This growth is in particular terminated by protons, and it has even been shown that the proton content constitutes the main parameter controlling the polymer formation in solution, information which is obtained during the synthesis and in particular in the shape and characteristics of the voltammograms recorded during the synthesis (see in particular the article by C. Bureau, Journal of Electroanalytical Chemistry, 1999, 479, 43).
[0013] Traces of water, and more generally the sensitive protons of protic solvents, constitute a source of protons that are detrimental to the anionic growth of polymer chains both in solution and on the surface. However, as described in patent FR2860523, it is preferable to optimize the thickness of the electrografted coating and to carry out the electrografting of vinyl monomers in a bath containing at least 50 ppm of water, ideally about 1000 ppm of water, i.e. an electrolytic bath containing approximately as much water as the electrolyte support. This unexpected result follows from the fact that in electrografting, two types of polymerization are competing: (i) chain growth starting from the initiator on the surface, i.e., growth associated with the grafting itself, and (ii) chain growth resulting from the dimerization of desorbed radical anions (C. Bureau, Journal of Electroanalytical Chemistry, 1999, 479, 43), which takes place in solution and independent of the surface, and which can form a coating if the local concentration of the polymer formed in the solution exceeds the local threshold of solubility near the surface. This coating is generally not adherent and can be removed from the surface by simple washing with a good solvent for the polymer (if electrografting is carried out in a good solvent for the polymer, the solvent is not even visible on the final surface, which only supports the electrografted layer). The competition between these two types of polymerization reactions generally favors, kinetically, the homogeneous solution reactions compared to the heterogeneous surface reactions. Near the surface, there is a shortage of monomer in the medium due to the solution polymerization, which "suffocates" the polymerization, especially by grafting. It is believed that protons added to the reaction medium by adding water can limit this imbalance by "killing" the main reaction, i.e. the solution polymerization, and thus favoring the surface reactions by maintaining a higher local concentration of monomer near the surface than would be the case in the complete absence of water. This "more water is better" mechanism, which is rather counterintuitive for anion-driven polymerizations, can explain all the observations, including the very strange voltammograms obtained with these "aprotic" modes of electrografting.
[0014] However, this process is only observed for proton concentrations not exceeding a few hundred or a few thousand ppm in water, above which the growth starting from the surface is itself killed and no electrografted coating is formed on the surface at all. In practice, it is more difficult to maintain a solution at a particular water content than it is to maintain a very low water content, as for example is the case when the above solution is kept in contact with freshly prepared molecular sieves.
[0015] Overall, even if chemical bonding can be achieved on conductive or semiconducting substrates by electrografting of various precursors starting from organic solutions, the formation of such coatings starting from easily prepared and controllable solutions remains difficult due to these reactions, since the underlying reaction mechanism (anionic polymerization) makes it impossible to work with solutions having any water content.
[0016] So far, only aryldiazonium salts offer a solution to this problem. For example, as described in French Patent Application No. FR2804973, electrografting of precursors such as positively charged aryldiazonium salts is carried out by a cation reduction followed by a cleavage reaction to give chemically absorbed radicals on the surface. Just as in the case of electrografting of polymers, the electrografting reaction of aryldiazonium salts is electrically initiated, leading to the formation of interfacial chemical bonds. Unlike the electrografting of vinyl monomers, the electrografting of aryldiazonium salts does not require a chemical reaction coupled with a charge transfer to stabilize the chemically absorbed species, since this species is electrically neutral. Thus, the electrografting of aryldiazonium salts directly forms stable surface / aryl bonds. In particular, in French Patent Application No. FR2829046, aryldiazonium salts form very thin, electrically conductive, and therefore organic coatings that can grow by themselves. That is, it has been shown that if the initial aryl coating grafting occurs by electrocleavage + chemisorption on the initial surface, the coating grows by an electrosustained reaction, i.e., more polymer coating is formed as more current flows through the electrode. As a result, such coatings are usually more difficult to control, especially with regard to their thickness.
[0017] It has been observed that the electroreduction of a solution containing an aryldiazonium salt and a vinyl monomer can result in the formation of a polymeric coating of the monomer on a surface, but that the polymer is insoluble in the solvent used for electrosynthesis (see X. Zhang and JP Bell, Journal of Applied Polymer Science, 73, 2265, 1999). One advantage of a mixture of aryldiazonium and vinyl monomers is that, as claimed in this document, the polymer can be obtained by electrosynthesis without the need to apply a high cathodic voltage necessary to achieve electroreduction of the vinyl monomer, i.e., it is sufficient to reduce the aryldiazonium salt, which is then used as an initiator for radical-type polymerization. Zhang et al. (supra) have in fact reported that the aryldiazonium salt is dissolved in about 10 -2By polarizing aqueous solutions of acrylamide at a concentration of about 5.10 mol / l at a constant potential (-0.8 V / SCE), they observed that no film formed on the surface of the steel coupons, but a large amount of polymer formed in the solution. They interpreted this data by considering that polyacrylamide is water soluble. In contrast, they found that aryl diazonium salts at a concentration of about 5.10 mol / l were -3 The formation of a whitish, very thick coating on the surface of similar steel coupons has been observed by polarization at constant potential (-1.0 V / SCE) of aqueous solutions of acrylonitrile and methyl methacrylate in moles / l and mixtures of acrylonitrile and methyl methacrylate in concentrations of 0.24 and 0.36 moles / l, respectively. After 30 minutes of electrolysis, the thickness of the coating was estimated to be 1 micrometer, which is much greater than can be achieved by simple electrografting of vinyl monomers. They interpret this result by showing that the copolymer formed (whose structure is confirmed by variable angle reflection-absorption infrared spectroscopy) is completely insoluble in water and precipitates on the surface.
[0018] These results are of interest to those skilled in the art who wish to form polymeric coatings on metal substrates. However, the grafting or strong bond formation reaction, which constitutes one of the prominent features of the electrografting reaction, disappears under the operating conditions chosen by Zhang et al. to form the coating by deposition on the surface. Summary of the Invention
[0019] The present invention starts from precursor solutions that are easy to prepare and control, in particular (i) the application of an electrode potential to force the grafting reaction; (ii) the use of an electrolytic medium which is at least a good swelling agent for the polymer formed or which is a good solvent for the polymer; This provides a facile operating procedure for the actual electrografting of the polymer.
[0020] The aim of the present invention is to propose a method by which organic coatings, in particular polymeric coatings, can be electrografted onto any conductive or semiconductive substrate or onto any such portion of a composite surface, with a thickness of nanometers to a few microns, preferably from about 10 nanometers to 1 micron.
[0021] Such organic coatings are useful for their intrinsic properties or, if desired, as underlayers or interfacial layers to which other materials can be attached by other means such as dipping, spray coating or spin coating.
[0022] As described in French Patent FR 2843757, the adhesion of a functional, for example organic, functional layer is effectively reinforced by a grafted organic, in particular polymeric, underlayer, if said underlayer has a thickness of at least a few tens or hundreds of nanometers, this length being of the order of the radius of gyration of most of the known polymers, such that an underlayer having a thickness of at least this length is theoretically sufficient to combine the polymer of the functional layer into the grafted underlayer, i.e. to form at least one loop of the polymer of the functional layer in the grafted underlayer. It is therefore believed that a better adhesion can be obtained by thin or ultrathin underlayers grafted onto the surface, compared to the relatively thick layers described in the prior art.
[0023] As described in FR2837842, it is also important to obtain non-vinyl electrografted polymers (polyethylene glycol PEG, poly(dimethylsiloxane) PDMS, etc.) of non-polymeric macromolecules (dextrans, proteins, ADN, etc.) or of non-macromolecular macroobjects (carbon nanotubes, fullerenes, inorganic aggregates, etc.). It goes without saying that the same vinyl precursors as those described in FR2837842 can be used in the present invention, and all precursors that comply with the conditions of monomers or vinyl monomers will be used without any further strictness, although said monomers can be chosen from all the types of precursors already mentioned in FR2837842.
[0024] The invention is based on the fact that when a time-dependent electrode potential procedure is applied, which procedure includes a cathodic excursion at a potential above a certain threshold, an electrode can be immersed in an electrolytic bath comprising at least one diazonium salt and at least one chain-polymerizable group to form, after washing, a polymeric coating containing said groups.
[0025] The first object of the present invention is a method for grafting an organic coating onto a conductive or semiconductive surface by electroreduction of a solution, comprising the steps of: a) preparing a solution containing at least one diazonium salt and one monomer having at least one chain polymerizable functional group, which is a precursor of the organic coating; b) forming a grafted coating of an organic film on the surface by applying at least one procedure consisting of electrolyzing said solution in an electrolytic cell, using the conductive or semiconductive surface to be coated as working electrode and at least one counter electrode, and electrically polarizing the surface by applying a variable potential spanning at least a range of values that are more cathodic than the reduction or peak potential of all diazonium salts present in said solution; The method comprises:
[0026] Advantageously, at least one of the procedures is carried out in cyclic voltammetry scanning (CVS) mode.
[0027] In at least one procedure it is advantageous to apply a variable working current to the surface.
[0028] In the present invention, a monomer is a compound having at least one chain-polymerizable functional group. The polymerizable group can include various polymerizable moieties, such as a double bond, a ring (polymerization by ring opening), or a functional group. In a preferred embodiment, the monomer is a vinyl monomer. In another preferred embodiment, the monomer is a polymerizable cyclic compound, such as a lactone.
[0029] The threshold value of interest in the present invention is the reduction potential of the aryl diazonium in solution.
[0030] As will be explained in detail in the examples below, adhesion coatings of poly-hydroxyethyl methacrylate (poly-HEMA) were prepared by 100% solubility in 4-nitrobenzenediazonium tetrafluoroborate. -2 The surface can be obtained by voltametric scanning at a scan rate of 100 mV / s over the potential range of -0.1 V / CES to -1.2 V / CES in a solution containing 100 mol / l of HEMA and 2 mol / l of HEMA (solvent=DMF / water). Although P-HEMA is a highly hydrophilic polymer with high water solubility, electrochemical impedance spectroscopy (EIS) data show that the poly-HEMA layer obtained by the method of the invention remains completely swollen in water and is capable of ionically conducting. This is one evidence that the coating is almost, if at all, devoid of crosslinking and that its adhesion on the surface is the result of bond formation with the underlying metal. For this reason, in the following, the term electrografting of polymers is used, even though it currently means a grafting obtained by electroreduction of a solution containing both a monomer capable of undergoing a chain propagation reaction and a diazonium salt, preferably present in low concentration.
[0031] It is a major achievement of the present invention that the same method can also be applied to monomers that normally undergo almost exclusively anionic propagation, e.g., monomers that can undergo ring opening (e.g., lactones such as ε-caprolactone, or lactides, e.g., lactic acid or glycolic acid). These monomers, like the vinyl systems, undergo chain propagation reactions and therefore can be described as "chain polymerizable" monomers, but unlike the vinyl systems, they have been found to be susceptible to anionic propagation as well, if not exclusively.
[0032] Nevertheless, 316L stainless steel coupons were treated with 4-nitrophenyldiazonium tetrafluoroborate for 10 min. -2 Polylactic acid (PLA) coatings with a thickness of nearly 1.1 μm were observed to be formed on the surface of stainless steel coupons by voltammetric scanning polarization over the potential range of -0.2 V / ECS to -2.8 V / ECS at a scan rate of 100 mV / s in an aqueous solution containing 0.5 mol / L L-di-lactide. The coatings survived washing in water and under ultrasonic treatment, indicating strong adhesion was obtained by grafting. This type of coating is of great importance in biomedicine, since PLA is a biodegradable coating.
[0033] It can thus be seen that the invention is based on the fact that the application of a time-dependent electrode potential procedure, which procedure includes a cathodic excursion at a potential above a certain threshold, makes it possible to form, after washing, an adherent polymeric coating based on a monomer, by immersing an electrode in an electrolytic bath comprising at least a diazonium salt and at least one monomeric compound, i.e. a molecular compound having at least one chain-polymerizable functional group.
[0034] The following examples illustrate the main advantages obtained by using the method of the present invention. (i) The method of the present invention is applicable to any conductive or semi-conductive surface, such as 316L stainless steel, cobalt chromium alloys, titanium surfaces, titanium nitride, etc. (ii) The process of the present invention allows the production of a wide variety of homopolymer layers with the required properties, i.e. hydrophilic layers containing HEMA (hydroxyethyl methacrylate) as a monomer, hydrophobic layers containing BUMA (butyl methacrylate) as a monomer, etc. (iii) The method of the present invention allows the preparation of a wide variety of copolymer layers with the required properties, i.e. hydrophilic or hydrophobic layers containing copolymers of BUMA and MPC (2-methacryloyloxyethyl phosphorylcholine) as monomers in various ratios. (iv) The method of the present invention allows the preparation of a wide variety of organic layers made from non-vinyl polymers, i.e., PEG (polyethylene glycol) or PDMS (poly(dimethylsiloxane)) made from the methacrylate telechelic monomers of PEG and PDMS. (v) The process of the present invention enables the production of a wide variety of polymers resulting from the ring-opening polymerization of cyclic monomers such as lactic acid, glycolic acid, ε-caprolactone, and the like. (vi) The method involves the actual grafting of a polymer layer onto the surface, which is evidenced by the fact that the poly-HEMA layer obtained according to the invention is completely swollen by water and therefore insoluble on the surface, rather than simply crosslinked; electrochemical impedance spectroscopy (EIS) measurements show that the electrochemical impedance of the TiN surface in NaCl medium is only slightly changed by a 100 nm poly-HEMA layer obtained by electrografting, which indicates that the ionic currents through the coating are still active and that the polymer layer is permeable and does not constitute a water-insoluble barrier layer. (vii) The method of the present invention allows the formation of thin grafted polymer layers which can be used as an adhesion primer for much thicker layers sprayed on top of it. This is demonstrated with a 150 nm poly-BUMA layer electrografted onto a 316L stainless steel coupon which does not delaminate a 5 μm PLA layer sprayed on top of it when the steel coupon is pulled apart. (viii) The method of the present invention allows the formation of grafted layers that are composed essentially of the desired polymer. Contrary to expectations, the electroreduction of the diazonium and propagation on the nitrophenylene does not in itself inhibit the initiation of polymerization of the monomer.
[0035] According to the method of the present invention, the monomers suitable for the present invention are preferably selected from activated vinyl monomers and cyclic molecules that can be cleaved by nucleophilic attack, having formulae (I) and (II), respectively. [ka] (In the formula, A, B, R1 and R2 may be the same or different and are each a hydrogen atom, a C1-C4 alkyl group, a nitrile group, a hydroxyl, an amine, i.e., -NH x (x=1 or 2), ammonium, thiol, carboxylic acid and their salts, esters, amides, i.e., C(=O)NH y (where y=1 or 2), imides, imide-esters, acid halides, i.e., C(=O)X (where X represents a halogen atom selected from fluorine, chlorine, bromine and iodine), acid anhydrides, i.e., C(=O)OC(=O), amino acids, phosphoric acids and their salts, phosphoric acids and their salts, phosphonylcholines and their derivatives, sulfonic acids and their salts, sulfuric acids and their salts, nitriles, succinimides, phthalimides, isocyanates, epoxies, siloxanes, i.e., -Si(OH) z(z being an integer between 1 and 3), benzoquinone, carbonyl-diimidazole, para-toluenesulfonyl, para-nitrophenyl chloroformiate, ethylene and vinyl, aromatics, in particular toluene, benzene, halogeno-benzenes, pyridine, pyrimidine, styrene or halogeno-styrene and their substituted equivalents, functional groups capable of complexing with cations, in particular reducing cations of metals, for example copper, iron and nickel, molecular structures substituted and / or functionalized starting from these functional groups, groups which can be thermally or photochemically cleaved (for example diazonium, salts, peroxides, nitrenes, azides, nitrosoanilides, alkoxyamines, in particular 2,2,6,6-tetramethyl-1-piperidinyloxy (TEMPO), benzophenone and its derivatives, dithioesters, dithiocarbamates, trithiocarbonates), electroactive groups and in particular conductive polymer precursors (e.g. aniline, thiophene, methylthiophene, bisthiophene, pyrrole, ethylenedioxothiophene (EDOT) and analogues, and electrocleavable groups (e.g. diazonium, sulfonium, phosphonium and iodonium salts), as well as mixtures of monomers containing the above groups, The straight line in formula (II) represents a C3-C10 alkyl group; n, m and p may be the same or different and represent an integer of 0 to 20, with the proviso that n, m and p are not all 0 at the same time.
[0036] Other cyclic molecules that can be cleaved by nucleophilic attack can also be used. For example, the monomer can be a cyclic compound that contains an amine and / or an amide, such as a lactam.
[0037] In the above symbols, R1 and R2 are unconditionally radicals differing by an index i not shown above, i being 0 to n. This means that the R1 and R2 radicals may in fact be (C(R1)R2) different from the others in the structure of the cyclic molecule of formula (II), i.e. the notation (C(R1)R2) nrepresents a sequence of (C(R1)R2) type groups, where R1 and R2 are included in the list above, rather than a repetition of the same element (C(R1)R2).
[0038] Among the functional groups of the activated vinyl monomers of formula (I) above that are capable of complexing with cations, mention may be made in particular of amides, ethers, carbonyls, carboxyls and carboxylates, phosphines, phosphine oxides, thioethers, disulfides, ureas, ether-crowns, aza-crowns, thio-crowns, cryptands, sepulcrats, podands, porphyrins, calixarenes, bipyridines and terpyridines, quinolines, orthophenanthroline compounds, naphthols, iso-naphthols, thioureas, siderophores, antibiotics, ethylene glycol and cyclodextrins.
[0039] Among the activated vinyl monomers of formula (I) mentioned above, particular mention may be made of acrylonitrile, methacrylonitrile, methyl, ethyl, propyl and butyl methacrylates, hydroxyethyl hydroxypropyl glycidyl methacrylate, acrylamide and in particular amino-ethyl, propyl, butyl, pentyl and hexyl methacrylamide, cyanoacrylates, di- or di-methacrylates, tri- or tri-methacrylates, tetra- or tetra-methacrylates (e.g. pentaerythritol tetramethacrylate), acrylic acid and methacrylic acid, styrene and its derivatives, parachlorostyrene, pentafluorostyrene, N-vinylpyrrolidone, 2-vinylpyridine, vinyl acryloyl, methacryloyl halides, divinylbenzene (DVB) and more generally vinyl reticulating or methacrylate-based agents and their derivatives.
[0040] Among the cleavable cyclic molecules of formula (II) above, mention may be made in particular of epoxies, lactones and in particular butyrolactone, ε-caprolactone and its derivatives, lactic acid, glycolic acid, oxiranes, polyaspartates, mixtures thereof and derivatives thereof.
[0041] Another object of the invention is a method for grafting an organic coating onto a conductive or semiconductive surface by electroreduction of a solution comprising at least one diazonium salt and one cyclic monomer of formula (II) which is polymerized by nucleophilic attack cleavage, the polymer being chosen in particular from the group consisting of lactic acid, glycolic acid and ε-caprolactone.
[0042] Another subject of the invention is a method for attaching macroscopic objects to conductive or semiconductive surfaces by electrografting. For the purposes of the invention, the term "macroscopic object" means a polymeric or non-polymeric macrostructure functionalized with at least one group capable of participating in a chain propagation reaction, i.e. a group belonging to the group of vinylic or cleavable cyclic molecules, such as those mentioned above. Such groups will hereinafter be called "chain polymerizable" groups, similar to the chain polymerizable monomers mentioned above.
[0043] In this embodiment, the object of the invention is a method for grafting an organic coating onto a conductive or semiconductive surface by electroreduction of a solution, comprising the steps of: a) preparing a solution containing at least one diazonium salt and one macro-object which is a precursor of the organic coating; b) forming a grafted coating of said organic film on said surface by applying at least one procedure consisting of electrolyzing said solution in an electric field layer with a conductive or semiconductive surface coated as a working electrode and at least one counter electrode, and electrically polarizing said surface by applying a variable potential over at least a range of values that are more cathodic than the reduction or peak potential of all diazonium salts in said solution; The method comprises:
[0044] The object may be, for example, a crosslinked or uncrosslinked polymer, functionalized at the chain ends or along the chain, or at other crosslinked sections, or a fully or partially functionalized macromolecule, or an object of nanometer or micrometer size or larger, the surface of which may be functionalized with at least one chain-polymerizable group capable of undergoing or participating in a surface-initiated polymerization reaction according to the present invention.
[0045] The macroscopic objects of the present invention may be, for example, crosslinked or uncrosslinked polymers, or fully or partially functionalized macromolecules, or objects of nanometer or micrometer size or larger, whose surfaces may be functionalized with electron-withdrawing groups, such as methacrylates, acrylates, vinyl chloride, acrylonitrile, methacrylonitrile, 4-vinylpyridine, 2-vinylpyridine, N-vinylpyrrolidone, etc., or other cyclic groups, such as epoxy groups or more generally, vinyl groups activated with oxiranes or lactones, such as ε-caprolactone.
[0046] These macroscopic objects can be used to obtain electrografted coatings containing macrostructural moieties. Grafting occurs due to the presence of electron-withdrawing or nucleophilic groups on the macrostructural moieties, which are attached to the macrostructural moieties and thus electrografted onto their surfaces.
[0047] Due to the presence of their chain-polymerizable functional groups, the macroscopic entities that can be used in the present invention can themselves act as monomers and can be electrografted like "standard" monomers. In some cases, the molecular structures attached to the chain-polymerizable groups are so large that the chain-polymerizable groups become powerless, i.e., they do not have sufficient mobility to propagate and actually be the sole agents of electrografting the macroscopic entities to the surface. In that case, one may need to consider co-electrografting the macro-objects with some small monomer, such as an efficient vinyl monomer (e.g., butyl methacrylate or hydroxyethyl methacrylate), to achieve electrografting onto the surface and achieve chain propagation and film growth, possibly propagating through the chain-polymerizable groups of the macro-objects.
[0048] The macroscopic entities that can be used according to the method of the invention are preferably selected from compounds of the following formulae: AP APB P(A)n M(A) n A-[M(B)] n A-[M(B)] n -C AP-[M(B)] n AP-[M(B)]-C (In the formula, (i) P is a macrostructure selected from organic or inorganic oligomers and polymers, polymers obtained by polycondensation of one or more reagents, polysiloxanes, poly(ortho-esters), polyphosphates, parylene and substituted parylene-based polymers, conductive polymers, oligopeptides and proteins, nucleic acid molecules, polysaccharides, substituted or unsubstituted porphyrins, substituted or unsubstituted phthalocyanines, polymers formed from substituted monomers or substituted macromolecules selected from the above list, prepolymers, macromers or telechelics based on monomers and / or macromolecules selected from the above list, substituted or unsubstituted copolymers and / or mixtures which may be formed from these polymers, from their constituent monomers or from the above mentioned macromolecules, macrostructures which are neither polymeric nor strictly macromolecular, for example structures obtained by crosslinking two- or three-dimensional networks, such as rubbers, mineral aggregates, liquid vesicles such as liposomes and niosomes, and living cells, objects comprising at least one surface which can be functionalized with at least one electroactive group, in particular an electrograftable group, (ii) n is an integer equal to or greater than 1; (iii) M, when the structure is polymeric, is a constituent monomer unit of type P as defined above; (iv) A, B and C, which may be the same or different, are selected from chain polymerizable groups selected from vinylic groups or cleavable cyclic molecules, e.g., lactones, lactides, oxiranes, and A, B and C are bonded to the macrostructural moiety P or to the monomeric moiety M by covalent, ionic or coordinate bonds or by hydrogen bonds.
[0049] Among the polymers defined for P, mention may in particular be made of crosslinked or uncrosslinked vinyl polymers, such as acrylonitrile, methacrylonitrile, methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, cyanoacrylate, acrylic acid, methacrylic acid, styrene and its derivatives, N-vinylpyrrolidone, polymers of vinyl halides, and also polyacrylamides, isoprene, ethylene, propylene, ethylene oxide, molecules containing a cleavable ring, such as lactones, in particular ε-caprolactone, lactide, glycolic acid, polymers of ethylene glycol, polyamides, polyurethanes, poly(orthoesters) and polyaspartates.
[0050] Among the conductive polymers, mention may in particular be made of polymers based on aniline, thiophene or ethylenedioxythiophene (EDOT), pyrrole, their analogues or their substituted derivatives.
[0051] Among the proteins, mention may in particular be made of antigens, enzymes, growth factors, antibodies and collagen.
[0052] Among the nucleic acid molecules, particular mention may be made of single- and double-stranded DNA, single- and double-stranded RNA.
[0053] Among the polysaccharides, mention may in particular be made of, for example, cellulose and substituted celluloses, chitosan and substituted or functionalized chitosans, dextran and substituted or functionalized dextran, amylose, pectin, starch and heparin.
[0054] Among the mineral aggregates, mention may in particular be made of beads of silica, and more generally of oxides, and of nano-objects of any nature (nano-beads, nano-tubes, fullerenes, etc.).
[0055] Among the objects having at least one surface that can be functionalized with at least one electroactive group, mention may be made of non-liquid and non-gaseous objects having at least one conductive, semiconductive or insulating surface selected from metallic, organic or mineral surfaces, for example wood, glass, plastics, plant fibres, keratinous materials, organic or mineral gels, composites thereof or mixtures thereof.
[0056] The maximum number that can be specified for n is not critical to the present invention and will vary depending on the number of functional groups present on the macrostructural portion that can be functionalized with a chain polymerizable group.
[0057] This functionalization can be carried out, for example, by reacting these hydroxyl groups with methacryloyl chloride (MAC) to form methacrylic acid esters, which introduce methacrylate-chain polymerizable-groups into the macrostructure and can be electrografted by the method of the invention.
[0058] The same type of reaction can be carried out with, for example, glycidyl methacrylate instead of methacryloyl chloride.
[0059] It is also conceivable to use molecules that can be used as spacer elements, such as diisocyanates, epichlorohydrin and more generally all bifunctional molecules, to form covalent bonds between the vinyl monomers and the macrostructures. The concentration of electrophilic macro-entities in the electrolyte solution is preferably 10 -6 ~5 mol / l.
[0060] The concentration of chain polymerizable groups or monomers in the electrolytic solution according to the method of the invention may vary from monomer to monomer, but this concentration is preferably between 0.1 and 10 mol / l, more preferably between 0.1 and 5 mol / l.
[0061] The concentration of the diazonium salt in the electrolyte solution according to the method of the present invention is preferably 1 to 10 -4 mol / l, more preferably 10 -2 ~10-3 It is in moles / l.
[0062] In particular embodiments of the present invention, the electrolytic solution may contain at least one additional liquid (solvent), primarily as a bystander (i.e., not participating in the electropolymerization reaction), to solubilize and tailor the water-insoluble or poorly water-soluble chain-polymerizable monomers. However, it is important to note that the presence of such a liquid is not always necessary, since one can imagine situations in which the monomers used are used in pure form, or some of the monomers of the monomer mixture are used as solvents, or all the monomers of the monomer mixture are in miscible ratios. When these solvents are used, they are preferably selected from among dimethylformamide, dimethylsulfoxide, ethyl acetate, acetonitrile, tetrahydrofuran, propylene carbonate and other solvents commonly used in electrochemistry, dichloroethane and, more generally, chlorinated solvents. The solvents can also be selected from the group consisting of water and alcohols. The process of the invention has the advantage that these solvents can be used directly, without prior distillation to remove the water contained therein or without strict control of the water content of the atmosphere above the reaction medium. The process of the invention can therefore be easily carried out on an industrial scale.
[0063] In a preferred embodiment of the invention, the electrolyte solution comprises dimethylformamide, either alone or mixed with water or dimethylsulfoxide.
[0064] Likewise, in another embodiment of the method of the invention, the electrolytic solution may also contain at least one supporting electrolyte to ensure and / or improve the passage of electric current in the electrolytic solution. However, the use of a supporting electrolyte is not absolutely necessary, for example, when the chain-polymerizable monomer used comprises a group that is itself ionic (such as, for example, aminohexyl methacrylate ammonium chloride), in which case this ionic group ensures that the resistance drop of the electric circuit is maintained at an acceptable value. If used, the supporting electrolyte is preferably selected from among quaternary ammonium salts, such as perchlorates, tosylates, tetrafluoroborates, hexafluorophosphates, quaternary ammonium halides, sodium nitrate and sodium chloride. Among these quaternary ammonium salts, mention may in particular be made by way of example of tetraethylammonium perchlorate (TEAP), tetrabutylammonium perchlorate (TBAP), tetrapropylammonium perchlorate (TPAP), benzyltrimethylammonium perchlorate (BTMAP).
[0065] The electrolyte solution may further comprise agents that improve the homogeneity of the coating (surfactants), such as glycerol.
[0066] According to the invention, the conductive or semiconductive surfaces are preferably surfaces of stainless steel, cobalt and its alloys (e.g. Co-Cr-Mo, Co-Cr-W), titanium and its alloys (e.g. Nitinol, NiTi), materials particularly preferred according to the invention in biomedicine, iron, copper, nickel, niobium, aluminium (especially when freshly brushed), silver, silicon (doped or not), silicon carbide, titanium nitride, tungsten, tungsten nitride, tantalum, tantalum nitride or platinum-iridium or of precious metals selected from iridium, platinum, gold.
[0067] In the method of the invention, the electrolysis of the electrolytic solution can be carried out by polarization of the surface to be coated under voltammetric conditions and by a potential- or current-controlled procedure in which the potential (current) is time-dependent. The invention is based on the fact that, when a time-dependent electrode potential procedure is applied, which procedure includes a cathodic excursion at a potential higher than a certain threshold, the immersion of the electrode in an electrolytic bath comprising at least a diazonium salt and at least one monomer can result in the formation of an adherent polymeric coating of said monomer after rinsing. The threshold in question in the present invention is at least the reduction potential of the diazonium present in the solution, i.e. it is necessary that, over at least a part of the potential (or current) procedure applied to the substrate, the potential of the surface is higher than that of the highest diazonium salt present in the solution.
[0068] In a preferred embodiment, the threshold value of interest in the present invention is at least the reduction potential of the aryldiazonium in solution, i.e., the potential of the surface must be higher than that of the highest aryldiazonium salt present in solution over at least part of the potential (or current) sequence applied to the substrate. Without wishing to be bound by theory, this actually allows grafting of aryl groups onto the surface, followed by attachment of polymers to the surface via said aryl groups by radical aromatic substitution. In such a scheme, polymers will be formed by some non-grafted or chemisorbed aryl groups that can act as initiators, or by some other radicals derived, for example, from the reduction of protons and / or from the solvent itself. Preferred experimental conditions include, for example, polarization from the resting potential of the substrate in solution under voltammetric conditions.
[0069] For Example 15, the best polymeric coatings (consisting essentially of polymer and low in diazonium salt content) are obtained with cathodic excursions approximately in the potential range for reducing the monomer.
[0070] These results demonstrate that the best polymer coatings are obtained at potentials higher than the reduction potential of the diazonium salt, and that although the diazonium salt is important in providing an operational method for electrografting the polymer layer, the best working potential is much more cathodic, closer to the reduction potential of the diazonium and / or the substituents on the monomer itself.
[0071] In a preferred embodiment, the applied potential has an excursion within a potential range that is the most cathodic potential that can be reached within the solvent window before the so-called "solvent wall". This solvent wall is very easily identified in a voltammogram, since it usually corresponds to the potential at which a very steep rise (in absolute value) in the electrochemical current is observed, well above the maximum of the current peak resulting from the electroreduction of the diazonium salt. The nature of the electrochemical reaction that accompanies this steep increase in cathodic current may vary from electrochemical medium to electrochemical medium, but usually corresponds to the reduction of the supporting electrolyte, or the solvent, or dissolved water (if water is not the solvent), or all of these. Typically, according to this embodiment, the potential applied in the present invention is -2 to -3 V / ECS, ie, 1 to 2 V or more more cathodic than the reduction peak of the diazonium.
[0072] When the solvent is or contains water, one skilled in the art will appreciate that the applied potential must be less than the proton reduction potential.
[0073] The choice of potential value can be an important feature of the method (see Examples 12 and 13).
[0074] In a preferred embodiment of the invention, the coating is obtained by successively applying several independently selected sequences of sequences of applying different action potentials and sequences of applying different action currents, each sequence being applied to the surface for a specific duration that is the same or different from the other sequences.
[0075] The present invention also aims to produce conductive or semiconductive areas of surfaces coated with electrografted coatings as described above. Typically, these coatings have a thickness of 10 nm to 10 μm, preferably 10 nm to 1 μm.
[0076] Diazonium salts have the general formula R'-N 2+ ,X - where R' contains one or more aromatic rings and / or one or more unsaturated groups, and X- is a counter ion.
[0077] R' preferably comprises an organic or mineral group selected from the group consisting of nitro, fluoro, bromo, chloro, iodo, thiocyano, sulfate, sulfonate, sulfonium salt, phosphate, phosphonate, phosphonium salt, diazonium salt, amine, ammonium, alcohol, aldehyde, ketone, carboxylic acid, ester, amide, nitrile, acid anhydride, acid halide, alkyl, alkenyl, alkynyl, aryl, naphthyl, anthryl, pyrryl and higher polyaromatic groups, which include groups selected from the group consisting of nitro, fluoro, bromo, chloro, iodo, thiocyano, sulfate, sulfonate, sulfonium salt, phosphate, phosphonate, phosphonium salt, diazonium salt, amine, ammonium, alcohol, aldehyde, ketone, carboxylic acid, ester, amide, nitrile, acid anhydride, acid halide, alkyl, alkenyl, alkynyl, aryl, naphthyl, anthryl, pyrryl and higher polyaromatic groups.
[0078] According to a preferred mode of accomplishment, the process of the invention comprises the step of: 2+ X - wherein Ar represents an aromatic group and X represents an anion selected from halogen, sulfate, phosphate, perchlorate, tetrafluoroborate, hexafluorophosphate, and carboxylate.
[0079] The anion may be a substituent of an aryl group, such as a sulfonate group, in which case an amphiphilic molecule comprising a diazonium salt is obtained.
[0080] The aromatic group may contain one or more aromatic groups, either linked or fused. The aromatic group may be a C6-C14 aromatic moiety, optionally substituted with one or more functional substituents, or a heteroaromatic moiety having 4 to 14 atoms, optionally substituted with one or more functional substituents, and comprising one or more heteroatoms selected from oxygen, nitrogen, sulfur, or phosphorus. The aromatic group may further comprise one or more linear or branched, having 1 to 20 carbon atoms, optionally containing one or more double or triple bonds, optionally substituted with a carboxyl group, NO2, protected, di- and mono-substituted amino groups, cyano, diazonium, alkoxy containing 1 to 20 carbon atoms, alkoxycarbonyl containing 1 to 20 carbon atoms, alkylcarbonyloxy containing 1 to 20 carbon atoms, optionally fluorinated vinyl or allyl, aliphatic groups substituted with halogen atoms; optionally a carboxyl group, NO2, cyano, diazonium, an alkoxy group containing 1 to 20 carbon atoms, an alkoxycarbonyl group containing 1 to 20 carbon atoms, an alkylcarbonyloxy group containing 1 to 20 carbon atoms, an optionally fluorinated vinyl or allyl group, an aryl group substituted with a halogen atom; Carboxyl groups, NO2, protected, disubstituted and monosubstituted amino groups, amido, cyano, diazonium, sulfonic, phosphonic, alkoxy containing 1 to 20 carbon atoms, alkoxycarbonyl containing 1 to 20 carbon atoms, alkylcarbonyloxy containing 1 to 20 carbon atoms, optionally fluorinated vinyl, halogen atoms, The alkyl group may comprise a substituent selected from the group consisting of:
[0081] In a preferred mode of achievement, the method of the invention is characterized in that the aromatic group comprises one or more substituents which are likely to react directly with an organic resin, a biological molecule, a chemical molecule or a complexing agent, or one or more precursor substituents which are likely to react after conversion with an organic resin, a biological molecule, a chemical molecule or a sequestering agent. The expression "substituents likely to react directly with a polymer, a chemical or biological molecule" means a substituent of the aromatic group which bears a reactive functional group which is likely to react with a chemical functional group carried by another molecule, fixed to the surface. Examples of reactive functional groups carried by aromatic groups are allyl or vinyl or acetylenic functional groups, halogens, alcohols, e.g. -(CH2) n Alcohols of the -CH2-OH type, carboxylic acids, e.g. -(CH2) n Carboxylic acids of the -COOH type, acid anhydrides or acid halides, nitriles, isocyanates, amines, e.g. -(CH2) n -NH2 type amines (n is an integer from 0 to 10), sulfonic acids or sulfonates, phosphonic acids or phosphonates. The expression "precursor substituents likely to react with a polymer, chemical or biological molecule after transformation" means a substituent likely to react with a polymer, chemical or biological molecule after one or more transformations. Precursor substituents likely to react after transformation are, for example, NO2, N 2+ , -(CH2) n -CN, -(CH2) n -CHO, -(CH2) n -COOPr (where Pr is a protecting group), -(CH n -NHP'R, -(CH2) n -N(P'r)2, -(CH2) n -N=P"R, where P'R, P"R are protecting groups, and n is an integer from 1 to 10. Phenacylsulfonyl chloride or acetyl chloride are examples of amine protecting groups.
[0082] The method may comprise the separate step of applying an outer coating, which may be applied by electrodeposition or other means such as dipping, spray coating or spin coating.
[0083] Another object is a conductive or semiconductive surface grafted with an organic coating obtained by the method of the invention. The method of the invention allows thick coatings of organic coatings to be obtained. In the examples below it can be seen that organic coatings of 300 nm can be obtained (see for example examples 1 and 9). Example 3 shows that thicker coatings can be obtained using a crosslinking agent. The grafted coatings preferably have a thickness of 1 nm to 10 μm, more preferably 10 nm to 1 μm.
[0084] The surface is a conductive or semiconductive surface. This surface may in particular be stainless steel, steel or a cobalt-chromium alloy. The method thus allows the coating of all conductive or semiconductive surfaces with organic coatings, in particular vinyl polymers.
[0085] The organic coating may be a vinyl polymer or copolymer, particularly poly-BUMA, poly-HEMA, poly-MPC / BUMA and poly-MPC / DMA / TMSPMA. In a preferred embodiment, the organic coating is a biodegradable polymer, particularly polycaprolactone or PLA.
[0086] In the examples below, the organic coating includes the chemical structure of a monomer (one type of monomer or a variety of monomers) and a diazonium salt moiety (when an aryl diazonium salt is used, the aryl moiety is present in the organic coating - see for example Example 1).
[0087] As shown in Example 16, the electrografted polymeric coatings are not homogeneous in the direction perpendicular to the surface; closer to the metal surface the coatings are rich in diazonium and its electroreduction by-products, whereas further from the surface the films are more polymer-rich. This "dual" structure of the coatings is an interesting result for the following reasons: (i) diazonium salts are more easily grafted than monomers on conductive or semiconductive surfaces. In the case of vinylic monomers, this is believed to be because vinylic monomers are reduced to radical anions during their electroreduction and these anions are mainly repelled by (negatively) polarized surfaces when formed, so that electrografting of vinylic monomers is a phenomenon with a very low yield with respect to the electric current. In fact, electrografting of monomers, i.e. vinylic monomers, is difficult on common surfaces, especially when a residual oxide layer is present. Moreover, from a practical point of view, diazonium salts are very compliant and more easily electrografted on common surfaces. Thus, the present invention transfers the docility observed with diazonium salts to monomers, mainly vinylic monomers. Moreover, the electrografting of diazonium salts, as observed in the present invention, is not very sensitive to water content, whereas the direct electrografting of monomers, mainly vinylic monomers, is very sensitive to water content. (ii) The layers obtained by electrografting of diazonium salts are denser than those obtained with monomers (vinylic), and even with a thin oxide layer, as soon as it becomes at least semiconductive, provide good covalent bonding, and good electrografting and adhesion of the polymer is achieved even under conditions where monomers (vinylic monomers) are not electrografted.
[0088] The organic coating obtained by this method is Can be made into a biocompatible coating, It can be made into an adhesive primer, It may be electrically conductive, It may have electrical insulating properties.
[0089] Another object of the invention is an electrolytic composition comprising at least one diazonium salt, one monomer having at least one chain-polymerizable functional group, and one supporting electrolyte. The diazonium salt, the monomer and the supporting electrolyte have the same definition as above. In a particular embodiment, the monomer is selected from the group consisting of butyl methacrylate, hydroxyethyl methacrylate, lactic acid, glycolic acid and ε-caprolactone. Advantageously, the composition further comprises a solvent (as above) and / or a surfactant (glycerol). The electrolytic composition comprises the monomer in a concentration of 1.5-2 mol / l and the diazonium salt in a concentration of 5.10 mol / l. -4 ~10 -1 Supporting electrolyte concentration 10 in mol / l -3 ~5.10 -2 Advantageously, it is comprised in moles per liter.
[0090] The present invention relates to A monomer selected from the group consisting of butyl methacrylate and hydroxyethyl methacrylate, at least one diazonium salt, Supportive electrolytes, and solvent The present invention also relates to an electrolytic composition comprising:
[0091] The electrolytic composition contains monomers at a concentration of 1.5 to 2 mol / l and diazonium salts at a concentration of 5.10 -4 ~10 -1 Supporting electrolyte concentration 10 in mol / l -3 ~5.10 -2 Advantageously, it is comprised in moles per liter.
[0092] In particular, the diazonium salt is an aryl diazonium salt. The supporting electrolyte is advantageously selected from the group consisting of NaNO3 and TEAP. For these polymers, the use of a solvent, in particular DMF, can be recommended.
[0093] Another object of the present invention is to Butyl methacrylate monomer at a concentration of 1.5 to 2 mol / l Glycerol at a concentration of 0.01 to 1 mol / l Dimethylformamide was used as a solvent. 4-Nitrophenyldiazonium tetrafluoroborate at a concentration of 5.10 -4 ~10 -1 Sodium nitrate (NaNO3) at a concentration of 10 in moles / l -3 ~5.10 -2 The electrolytic composition comprises in moles / l.
[0094] The present invention provides a method for making an electrografting formulation, comprising the steps of: a) Butyl methacrylate monomer at a concentration of 1.5 to 2 mol / l; Glycerol (5% of the total volume) at concentrations of 0.01–1 mol / l; Dimethylformamide was used as a solvent. Sodium nitrate (NaNO3) at a concentration of 10 -3 ~5.10 -2 preparing a composition comprising in moles / liter b) Prior to use, the composition is diluted with 4-nitrophenyldiazonium tetrafluoroborate at a concentration of 5.10 -4 ~10 -1 Addition step in moles / l The present invention relates to a method comprising the steps of:
[0095] Another object of the present invention is to Hydroxyethyl methacrylate monomer at a concentration of 1.5 to 2 mol / l, Glycerol at a concentration of 0.01 to 1 mol / l Dimethylformamide was used as a solvent. 4-Nitrophenyldiazonium tetrafluoroborate at a concentration of 5.10 -4 ~10 -1 Sodium nitrate (NaNO3) at a concentration of 10 in moles / l -3 ~5.10 -2 The electrolytic composition comprises in moles / l.
[0096] The present invention provides a method for making an electrografting formulation, comprising the steps of: a) Hydroxyethyl methacrylate monomer at a concentration of 1.5 to 2 mol / l; Glycerol at a concentration of 0.01 to 1 mol / l Dimethylformamide was used as a solvent. Sodium nitrate (NaNO3) at a concentration of 10 -3 ~5.10 -2 preparing a composition comprising in moles / liter b) Prior to use, the composition is diluted with 4-nitrophenyldiazonium tetrafluoroborate at a concentration of 5.10 -4 ~10 -1 Addition step in moles / l The present invention relates to a method comprising the steps of:
[0097] The present invention further provides a method of coating a stent with an electrografted layer of polyhydroxyethyl methacrylate, comprising the steps of: A process of washing with detergent for 10 to 20 minutes at 90% ultrasonic output of 35 kHz; Cleaning with DI water for 10-90 minutes at 90% ultrasonic output of 35 kHz. drying process, contacting the stent with a negative pole of a power source; A step of immersing the metal in the electrolytic solution of claim 25 for 5 to 20 minutes while bubbling with argon; Polarizing the stent by a cyclic voltammetry procedure, scanning 5-75 times from the open circuit potential to -3 V / CE (CE = counter electrode = anode) at a scan rate of 100 mV / s with argon bubbling at 8 l / min; A first cleaning step is performed in DMF with argon bubbling for 5 to 20 minutes. A second cleaning step is performed for 5 to 20 minutes while bubbling with argon. Washing in DI water for 5-20 minutes; Drying in a vacuum oven at 40°C and 10 mbar for 30-180 minutes The present invention relates to a method comprising the steps of:
[0098] The present invention further provides a method of coating a stent with an electrografted layer of polybutylmethacrylate, comprising the steps of: A process of washing with detergent for 10 to 20 minutes at 90% ultrasonic output of 35 kHz; Cleaning with DI water for 10-90 minutes at 90% ultrasonic output of 35 kHz. drying process, contacting the stent with a negative pole of a power source; A step of immersing the metal in the electrolytic solution of claim 23 for 5 to 20 minutes while bubbling with argon; Polarizing the stent by a cyclic voltammetry procedure, scanning 5-75 times from the open circuit potential to -3.2 V / CE (CE = counter electrode = anode) at a scan rate of 50 mV / s with argon bubbling at 8 l / min; A first cleaning step is performed in DMF with argon bubbling for 5 to 20 minutes. A second cleaning step is performed for 5 to 20 minutes while bubbling with argon. Washing in DI water for 5-20 minutes; Drying in a vacuum oven at 40°C and 10 mbar for 30-180 minutes The present invention relates to a method comprising the steps of: EXAMPLES
[0099] experiment All chemicals were obtained from Aldrich Chemical Co. or Acros and used as received. TiN thin films were obtained on SiO2 / Si substrates by MOCVD.
[0100] Typical specimen size is 7 x 1 cm 2 Electropolished stainless steel (316L), cobalt chrome (MP35N), sandblasted and non-sandblasted titanium substrates were ultrasonically cleaned in a 2% Dorex solution at 50°C, followed by distilled water, and dried in a furnace at 100°C for 1 h before use. TiN / SiO2 / Si were used as removed from the MOCVD chamber.
[0101] The composition of the coatings was analyzed using a Brucker Tensor 27 Fourier transform infrared spectrometer (FT-IR) equipped with a SensIR (Durascope) attachment for ATR measurements at a resolution of 4 cm-1. The thickness of the coatings was confirmed by cutting a sharp groove through the coating with a cutter and measuring the groove with a Step IQ profilometer obtained from KLA Tencor. Voltammetry and other time-dependent potential experiments were performed with a potentiostat / galvanostat (CH660A, CH Instruments, USA) where the potential of the working electrode (substrate to be coated) is applied against a calomel reference electrode (ECS). Unless otherwise indicated, all potentials are given in absolute values relative to the ECS reference potential for all experiments. XPS spectra were obtained with an ESCALAB VG XL 220 instrument (source Al, energy 1486.6 eV). ToF-SIMS spectra were obtained on a ToF-SIMS IV (ION-TOF GmbH, Muenster, Germany). The acquisition time was 75 s and the spectrum was measured using a 150 × 150 μm 2 The spectra were acquired with a Au source (25 keV) operating in high mass resolution mode. Both positive and negative spectra were recorded.
[0102] Electrochemical impedance spectroscopy experiments were carried out in a three-electrode electrochemical cell with a large platinum foil as counter electrode and an Ag / AgCl reference electrode. EIS spectra were collected using a multichannel potentiostat VMPII / z computer controlled with Eclab software. Measurements were performed in 0.9 gL NaCl. -1 The open circuit potential in solution is 10 5 ~10 -2 Measurements were made over a frequency range of 10 Hz, with 5 measurement frequencies per 10 and a 10 mV peak-to-peak sinusoidal amplitude signal.
[0103] The present invention will now be described in more detail with reference to the following examples, which, however, are not intended to limit the scope of the present invention.
[0104] Example 1 Deposition of BUMA thin films on stainless steel in the presence of 4-nitrodiazonium tetrafluoroborate Poly-BUMA coatings are known to be important biocompatible coatings to be deposited as coatings on biocompatible substrates for use in prostheses, such as stainless steel, titanium (example 4), CoCr (example 5). Such coatings are obtained as follows: TEAP (tetraethylammonium perchlorate as supporting electrolyte, 2.5 10 -2 In 50 mL of undistilled dimethylformamide (DMF) containing 574 mg (3.5 M), 50 mL of butyl methacrylate and 236 mg (10 M) of 4-nitrobenzenediazonium tetrafluoroborate were added. -2 M) will be introduced. The solution was introduced into a cell with two electrodes, a polished stainless steel coupon as the working electrode and a piece of carbon paper as the counter electrode. The potential of the stainless steel cathode was adjusted from -0.2 V to -3.0 V with argon bubbling (2 L min ) at a rate of 100 mV / s. -1 ) and scan 20 times.
[0105] FIG. 1 shows the initial (black line) and final (dashed line) cyclic voltammograms of the solution, demonstrating film formation.
[0106] The electrode was then carefully rinsed with DMF, water, and air-dried, resulting in a homogeneous greenish coating 300 nm thick. The IR spectrum of this coating showed that the carbonyl vibration of polybutylmethacrylate was at 1728 cm -1 In the nitrophenyl group, two symmetric and asymmetric vibrations are observed at 1520 and 1350 cm -1 are observed in the following cases.
[0107] It can be seen that a poly-BUMA layer is obtained even though poly-BUMA is readily soluble in DMF, and moreover, the coating can withstand thorough rinsing in DMF under ultrasound for 2 min.
[0108] Example 2 Deposition of BUMA thin films on stainless steel in the presence of 4-nitrodiazonium tetrafluoroborate by pulse train potentials A scanning potential can be used as in Example 1, or a pulse train potential can be used as described in the Experimental Procedures below.
[0109] The same procedure as in Example 1 was used, except that a pulse train potential (Ei=-0.5 V for 0.6 s and Et=-3.0 V for 0.3 s) was used instead of the scanning potential. The number of scans was 2000. A homogeneous greenish coating with a thickness of 300 nm was formed on the electrode, which was then carefully rinsed with DMF, water and air-dried.
[0110] In the IR spectrum of this coating, the carbonyl vibration of polybutyl methacrylate was detected at 1728 cm -1 In the nitrophenyl group, two symmetric and asymmetric vibrations are observed at 1520 and 1350 cm -1 are observed in the following cases.
[0111] Example 3 The influence of a crosslinking agent (pentaerythritol tetraacrylate) on the thickness of films obtained on stainless steel from methyl methacrylate and 4-nitrobenzenediazonium tetrafluoroborate.
[0112] Typically, the thickness of the coating obtained by vinyl / diazo copolymerization is about several hundred nm. Thicker coatings can be obtained by adding a crosslinking agent, such as pentaerythritol tetraacrylate, to the coating deposition bath as described in the procedure below.
[0113] NaNO32 10 mg (2.5 10 mg as supporting electrolyte) -2 In 50 mL of undistilled DMF containing 50 mL (5 M), methyl methacrylate, 236 mg (10 -2 1 mL of pentaerythritol tetraacrylate (1.2 10 -3 M) into a two-electrode cell in which the working electrode is a polished stainless steel coupon and the counter electrode is a piece of carbon paper.
[0114] The potential of the stainless steel cathode was changed from -0.17 V to -2.8 V at a rate of 50 mV / s by bubbling with argon (2 L min -1) while scanning.
[0115] A homogeneous greenish coating was formed on the electrode, which was then carefully rinsed with DMF, water, and air-dried. The thickness of the coating containing pentaerythritol is 1.0 μm. The thickness of the coating without pentaerythritol tetraacrylate is limited to 150 nm.
[0116] In separate experiments with pentaerythritol tetraacrylate, under the same conditions but with 20 and 40 potential scans, respectively, thinner films were obtained, the thickness of which is linear with the number of cycles imposed by voltammetry, as shown in FIG. 2.
[0117] Figure 2 shows the relationship between the increase in thickness of the coating obtained on a stainless steel coupon from MMA and 4-nitrobenzenediazonium tetrafluoroborate in the presence of pentaerythritol tetraacrylate and the number of electrochemical cycles, where the horizontal axis is the number of cycles and the vertical axis is the thickness of the coating (Å).
[0118] In the IR spectrum, the carbonyl vibration of polyester is at 1740 cm -1 In the nitrophenyl group, two symmetric and asymmetric vibrations are observed at 1520 and 1350 cm -1 are observed in
[0119] Example 4 Deposition of poly-BUMA thin films on sandblasted and non-sandblasted titanium substrates in the presence of 4-nitrobenzenediazonium tetrafluoroborate The same procedure as in Example 1 was used, except that sandblasted and non-sandblasted titanium substrates were used instead of stainless steel.
[0120] The IR spectrum of a 300 nm thick coating on bulk Ti shows the carbonyl vibration of polybutyl methacrylate at 1728 cm -1 In the nitrophenyl group, two symmetric and asymmetric vibrations are observed at 1520 and 1350 cm -1 are observed in
[0121] In the case of sandblasted Ti, a change in the hydrophilic / hydrophobic nature of the surface was observed after treatment, with the water droplet contact angle increasing from close to 0° before treatment to almost 90° after coating deposition due to the highly hydrophobic poly-BUMA coating obtained by electrografting.
[0122] Example 5 Deposition of poly-BUMA thin films in the presence of 4-nitrobenzenediazonium tetrafluoroborate on CoCr (MP35N) substrates NaNO32 15 mg (2.5 10 mg as supporting electrolyte) -2 In 50 mL of undistilled DMF containing 50 mL of butyl methacrylate (3.5 M) and 236 mg (10 -2 The solution is introduced into a two-electrode cell in which the working electrode is an electropolished CoCr substrate (MP35N) and the counter electrode is a piece of carbon paper. The potential of the stainless steel cathode is varied from -0.3 V to -3.5 V at a rate of 100 mV / s with argon bubbling (2 L min -1 ) while scanning.
[0123] A homogeneous greenish coating of 300 nm thickness was formed on the electrode, which was then carefully rinsed with DMF, water and air-dried. The IR spectrum of the coating showed that the carbonyl vibration of polybutyl methacrylate was at 1728 cm -1 is observed.
[0124] Example 6 Deposition of poly-BUMA thin films on CoCr(L605) substrates in the presence of 4-nitrobenzenediazonium tetrafluoroborate The same device setup as in Example 5 is used, except that the substrate is an 18 mm L605 cobalt-chromium coronary stent. The composition of the electrolyte solution is as follows: butyl methacrylate (30 wt%), 4-nitrobenzenediazonium tetrafluoroborate (10 -3 M), NaNO3(2.5.10 -2 M), glycerol (5% by weight), DMF (65% by weight), the weight percentages being based on the total weight of the composition.
[0125] After electrografting, the stents are rinsed in DMF and dried at 40° C. under 10 mbar vacuum for 60 min. Prior to electrografting, the stent surface is treated with a 40% solution of NH4F for 1 min. The thickness of the coating obtained using this method is about 150 nm. Electrografting parameters: argon bubbling (2 l.min -1 ) and cyclic voltammetry from open circuit potential to -3.5 V / CE. Number of scans: 50 scans. Scan rate 50 mV / s. TOF-SIMS analysis of the stent shows peaks characteristic of p-BUMA. The same spectrum also demonstrates the absence of peaks characteristic of glycerol.
[0126] Example 7 Deposition of poly-HEMA thin films on stainless steel in the presence of 4-nitrobenzenediazonium tetrafluoroborate Poly-HEMA is another example of a biocompatible polymer. Poly-BUMA is considered hydrophobic, whereas poly-HEMA is considered to be a more hydrophilic polymer due to its hydroxyl groups. Poly-HEMA coatings have been obtained on stainless steel, TiN thin film (Example 7), and Nitinol (Example 8) under the following conditions:
[0127] NaCl 145 mg (2.5.10 as supporting electrolyte) -2 A mixture of 10 mL of nondistilled DMF and 66 mL of deionized water containing 24 mL of hydroxyethyl methacrylate (HEMA, 2 M) and 236 mg (10 mL) of 4-nitrobenzenediazonium tetrafluoroborate was added. -2 M) will be introduced. The solution is introduced into a three-electrode cell in which the working electrode is a polished stainless steel coupon, the counter electrode is a piece of carbon paper, and the reference electrode is Ag / AgCl. The potential of the stainless steel cathode is varied from -0.1 V to -1.2 V at a rate of 100 mV / s with argon bubbling (2 L min -1 ) and scan 100 times.
[0128] In the IR spectrum of the coating, the carbonyl and C-OH vibrations of polyhydroxyethyl methacrylate were detected at 1728 and 1164 cm -1The two vibrations of the nitrophenyl group are barely detectable.
[0129] Example 8 Deposition of poly-HEMA thin films on TiN in the presence of 4-nitrobenzenediazonium tetrafluoroborate The same procedure was used as in Example 7, except that a TiN / SiO2 / Si substrate was used instead of polished stainless steel. FT-IR of the resulting coating identified the carbonyl and C-OH vibrations of polyhydroxyethyl methacrylate at 1704 and 1152 cm -1 are shown in the figures.
[0130] Example 9 Deposition of poly-HEMA thin films on NiTi (Nitinol) in the presence of 4-nitrobenzenediazonium tetrafluoroborate A mixture of 240 mL of deionized water containing 58.5 mg of NaCl (0.1 M as supporting electrolyte) was added to 60 mL of hydroxyethyl methacrylate (HEMA, 20% by volume) and 144 mg of 4-nitrobenzenediazonium tetrafluoroborate (10 -2 The solution is introduced into a two-electrode cell in which the working electrode is a Nitinol coupon and the counter electrode is a piece of carbon paper. The potential of the Nitinol cathode is changed from -0.7 V to -2.5 V at a rate of 100 mV / s with argon bubbling (2 L min -1 ) and scan 100 times.
[0131] In the IR spectrum of the coating, the carbonyl and C-OH vibrations of polyhydroxyethyl methacrylate were detected at 1728 and 1164 cm -1 The two vibrations of the nitrophenyl group are barely detectable. The surface of the electrografted substrate is hydrophilic, as can be seen from the water drop shape.
[0132] Example 10 Deposition of poly-MPC / BUMA copolymer thin films on stainless steel in the presence of 4-nitrobenzenediazonium tetrafluoroborate We used various amounts of 2-methacryloyloxyethyl-2-trimethylammonium methylphosphate (or 2-methacryloyloxyethyl phosphorylcholine, MPC). [ka] The monomer mixtures in solution compositions containing
[0133] This monomer was synthesized as described in Ishihara K, Ueda T, Nakabayashi N, Polym J 1990; 22: 355-360.
[0134] The composition consisted of 210 mL of undistilled DMF, 640 mg of NaNO3, a constant amount of butyl methacrylate (BUMA) at about 30% and an increasing amount of MPC (see Table 9-1), and 72 mg (10 -2 The solution is based on a mixture of 1000 mM sodium chloride and 1000 mM glycerol. The volume of the solution is maintained at 300 mL. The solution is introduced into a two-electrode cell in which the working electrode is a polished stainless steel coupon and the counter electrode is a piece of carbon paper. The potential of the stainless steel cathode is varied from -0.5 V to -3.2 V at a rate of 50 mV / s with argon bubbling (2 L min -1 ) and scan 50 times.
[0135] [Table 1]
[0136] Contact angle measurements for the different layers (samples 1, 3 and 5) show an increase in hydrophobicity.
[0137] An important aspect of this monomer mix is the possibility to adjust the surface energy of the resulting coating with the monomer ratio.
[0138] Example 11 Deposition of poly-MPC / DMA / HPMA / TMSPMA copolymer thin films on stainless steel in the presence of 4-nitrobenzenediazonium tetrafluoroborate More complex copolymers can also be obtained, as shown by the following examples. -22-Methacryloyloxyethyl phosphorylcholine (MPC, 0.1 M), dodecyl methacrylate (DMA, 0.1 M), hydroxypropyl methacrylate (HPMA, 0.1 M), trimethylsilylpropyl methacrylate (TMSPMA, 0.1 M), and 236 mg (10 mL) of 4-nitrobenzenediazonium tetrafluoroborate in 10 mL of undistilled DMF containing 0.1 M -2 The solution is introduced into a three-electrode cell in which the working electrode is a polished stainless steel coupon, the counter electrode is a piece of carbon paper, and the reference electrode is Ag / AgCl. The potential of the stainless steel cathode is varied from -0.0 V to -2.5 V at a rate of 100 mV / s with argon bubbling (2 L min -1 ) and scan 20 times.
[0139] Based on the infrared vibrational signature of each monomer and the mixture, the composition of the resulting coating is MPC=25%, DMA=10%, TMSPMA=21%, HPMA estimated, 4-nitrophenylene estimated.
[0140] [Table 2]
[0141] The complex nature of the structure of the coating is confirmed by the ToF-SIMS analysis, shown in Table 2. The ToF-SIMS spectrum indicates the presence of MPC, DMA and TMSPMA moieties in the copolymer of the resulting coating. The HPMA moiety is more difficult to detect, as is the 4-nitrophenylene residue. This latter result is not specific to this copolymer.
[0142] Example 12 Electrografting of poly(butyl methacrylate) (poly-BUMA) films in the presence of 4-diazophenylcarboxylic acid (DCOOH) tetrafluoroborate Diazo / vinyl film formation is not limited to 4-nitrobenzenetetrafluoroborate. Other examples of diazo derivatives that have been tested and found to be effective are listed below.
[0143] A 100 mL solution was prepared from 50 mL DMF (dimethylformamide) and 50 mL BUMA (butyl methacrylate, 0.31 M), 11 mg NaNO32 (25 mM) and 23.6 mg 4-diazophenylcarboxylic acid (DCOOH) tetrafluoroborate (1 mM). A stainless steel plate, polished as described previously and carefully cleaned, was introduced into the electrochemical cell together with a piece of carbon paper as the counter electrode and an SCE reference electrode. The potential of the stainless steel cathode was scanned 50 times at 100 mV / s between the open circuit potential and -3 V. The coupon was rinsed with water, then acetone, and dried.
[0144] A grey coating was easily observed on the specimen, which could not be rubbed off with a finger after drying, and the height of the coating was 87±5 nm as measured by profilometer.
[0145] The IR spectra are summarized in Table 3. Assuming that the absorption of the C=O bands of BUMA and DCOOH have similar heights, it can be estimated that this film contains about 30% DCOOH and 70% BUMA.
[0146] [Table 3]
[0147] The ToF-SIMS spectra are summarized in Table 4.
[0148] [Table 4]
[0149] Thus, both spectra confirm the presence of polybutyl methacrylate and phenyl carboxyl groups on the coating surface.
[0150] Example 13 Electrografting of poly(butyl methacrylate) (poly-BUMA) films in the presence of 4-diazophenylcarboxylic acid (DCOOH) tetrafluoroborate with a potential limit of -1 V The same procedure as in Example 12 was used, except that the final potential was limited to −1 V. After rinsing with acetone, no film was observed on the surface and its height could not be measured (<10 nm).
[0151] Example 14 Relationship between coating thickness and cathodic potential of polybutyl methacrylate (BUMA) on 316L stainless steel. The same setup as in Example 1 was used. The concentration of BUMA monomer was 3.5 mol / l, and the concentration of 4-nitrophenyldiazonium tetrafluoroborate was 10 -3 and 10 -2 mol / l. These experiments were carried out under a classical hood in DMF as solvent. All reagents were used as delivered without purification or water content adjustment. For each experiment, a new 316L stainless steel coupon was immersed in the electrolyte solution and the electrode potential was scanned 50 times between the open circuit potential and -0.8, -1, -1.5, -2, -2.5 and -3 V / SCE, respectively. The coupon was then rinsed in DMF under ultrasound for 10 min and dried. The thickness of the coupon was then measured with a profilometer. The results are shown in Tables 3 and 4.
[0152] Figure 3 shows the relationship between the thickness of the p-BUMA coating on 316L and the cathodic final potential (DNO2 concentration is 10 -2 mol / l).
[0153] Figure 4 shows the relationship between the thickness of the p-BUMA coating on 316L and the cathodic final potential (DNO2 concentration is 10 -3 mol / l).
[0154] These results show that when the cathodic final potential in the voltammetric experiment is (in absolute value) lower than the reduction potential of the diazonium salt under the same conditions, i.e., about -0.4 V / SCE, which is much more cathodic, -1 V / SCE, practically no polymer coating is formed (i.e. the thickness of the coating is not detectable by profilometer; the sensitivity of the profilometer given by the supplier is about 5 nm). -3 and 10 -2 The results are given in both mol / l, indicating the consistency of the observations.
[0155] In particular, it has been found that coatings of the order of several hundred nanometers associated with the top Velcro layer can only be obtained if the scanning procedure has an excursion at a potential more cathodic than -2 V / SCE.
[0156] Example 15 Relationship between quality of polybutyl methacrylate (Buma) coatings on 316L stainless steel and cathodic potential. The same instrument settings as in Example 14 were used. The polymer coating was analyzed by IRRAS. The IR spectrum showed a C=O band at 1720 cm, which is attributed to the carbonyl group of the Buma polymer. -1 , a small NO2 band at approximately 1345 and 1520 cm -1 As shown in.
[0157] C=O peak at 1345 cm -1 NO 2 By estimating the intensity ratio of the peaks (C=O) / (NO2), a "quality parameter" of the coating can be defined. The higher the cathodic potential, the higher the electroreduction rate of the diazonium salt, which has a much less cathodic reduction potential than any other species in the bath. The content of nitro groups in the coating can therefore be considered as a guide to the electroreduction of the diazonium and the growth of the nitro-phenylene itself versus the initiation of the polymerization reaction of the Buma monomers. This competition is estimated by the (C=O) / (NO2) ratio; the higher this ratio is, when polymeric p-Buma coatings are required, the better the coating.
[0158] This ratio is shown in relation to the cathodic final potential in Figures 5 and 6.
[0159] Figure 5 shows the relationship between (C=O) / (NO2)(IR) and the final cathode potential. -2 It is in moles / l.
[0160] Figure 6 shows the relationship between (C=O) / (NO2)(IR) and the final cathode potential. -3 It is in moles / l.
[0161] These figures show that the best polymeric coatings (in the above sense) are obtained with a cathodic excursion of about -2 V / SCE. This turns out to correspond to the potential range for reducing the vinyl monomer itself. The results also show that the quality of the coatings is poor at low cathodic potentials and very poor at higher cathodic potentials.
[0162] Example 16 Structure of polybutyl methacrylate (Buma) coatings on 316L stainless steel. The same setup as in Example 1 was used. The concentration of BUMA monomer was 3.5 mol / l, and the concentration of 4-nitrophenyldiazonium tetrafluoroborate was 10 -2 The concentrations of the ions in the electrolyte were 100% mol / l. The experiments were carried out under a classical hood in DMF as the solvent. All reagents were used as delivered without purification or adjustment of water content. The substrate was a 316L stainless steel coupon. The coupon was immersed in the electrolyte solution and the electrode potential was scanned three times between the open circuit potential and -3 V / SCE. The coupons were then rinsed in DMF under ultrasound for 10 minutes and dried. Ultrathin films on the order of 15 nm were obtained, allowing a complete analysis of the surface vs. bulk composition of the coating by angle-resolved XPS. N1s and C1s spectra are compared when electrons are collected near normal (15°) and at a grazing angle (60°) to compare the bulk vs. surface chemical structure of the polymer coating, respectively.
[0163] The N1s region of the XPS spectrum shows two main contributions at about 399.7 and 405.8 eV due to the nitrogen atom of the hydroxylamine or amine group and to the nitrogen atom of the nitro group (the hydroxylamine or nitro group is believed to be the result of the reduction of the nitro group during the electrochemical process or under the electron beam during the XPS analysis). The C1s region shows a contribution at 286.2 eV, which is especially attributable to the nitrophenyl group originating from the aromatic carbon bearing the NO2 or NH2 group and thus obtained by reduction of the diazonium salt.
[0164] Comparison of the XPS spectra at normal and elevation angles reveals that (i) aromatic carbons are mostly present at the interface, since their peaks are much weaker at the elevation angle (=surface), and (ii) the overall signal in the N1s region is always much weaker at elevation angles than at normal angles. The ratio between the 399.7 and 405.8 peaks, I(399.7) / I(405.8), is also smaller at elevation angles, indicating a relative paucity of nitro groups near the metal surface compared to the outer surface of the coating. This latter result indicates that the hydroxylamine and amine groups most likely originate from a highly electrochemical process due to their displacement at highly cathodic potentials causing the reduction of NO2 groups.
[0165] In summary, the results of this example show that the electrografted polymeric coating is not homogeneous in the direction perpendicular to the surface: close to the metal surface the coating is enriched in nitrophenyldiazonium and its electroreduction by-products, whereas far from the surface the coating is enriched in poly-BUMA, suggesting that electrografting occurs primarily through electrografting of the diazonium, and that some of its electroreduction by-products actually initiates the polymerization reaction at very cathodic potentials.
[0166] Example 17 Deposition of PEG onto Stainless Steel in the Presence of 4-Nitrodiazonium Tetrafluoroborate Cross-linkable polyethylene glycol dimethacrylate PEG(875) was used as an example for nano-object grafting.
[0167] The same procedure as in Example 1 was used, except that poly(ethylene glycol) dimethacrylate (PEG 875, 50 mL, 0.6 M) was used instead of butyl methacrylate.
[0168] Then, the electrode was carefully rinsed with DMF, water and air-dried, and a homogeneous brownish coating with a thickness of 300 nm was present on the electrode.
[0169] In the IR spectrum of the coating, the carbonyl and CH2-O vibrations of PEG were detected at 1729 and 1146 cm -1The two vibrations of the nitrophenyl group are barely detectable.
[0170] Example 18 Deposition of poly(ε-caprolactone) onto stainless steel in the presence of 4-nitrobenzenediazonium tetrafluoroborate Another class of biopolymers are the biodegradable polymers, many of which are of natural origin, although polylactones and polylactides (see Example 19) constitute an important class of synthetic biodegradable polymers. Coatings obtained from ε-caprolactone and 4-nitrobenzenediazonium tetrafluoroborate can be prepared by the following procedure.
[0171] NaNO32 10 mg (2.5 10 mg as supporting electrolyte) -2 In 100 mL of undistilled DMF containing 55.4 mL (5 M) of ε-caprolactone and 236 mg (10 -2 The solution is introduced into a two-electrode cell in which the working electrode is a polished stainless steel coupon and the counter electrode is a piece of carbon paper. The potential of the stainless steel cathode is varied from -0.15 to -2.8 V at a rate of 100 mV / s with argon bubbling (2 L min -1 ) and scan 40 times.
[0172] The electrode is then carefully rinsed, leaving a thick, homogeneous bluish coating.
[0173] In blank experiments in which no diazonium salt is present, no film is formed.
[0174] In the IR spectrum of the film, the carbonyl vibration of polyester was detected at 1725 cm -1 The two symmetric and asymmetric vibrations of the nitrophenyl group are observed at 1522 and 1346 cm -1 From the intensity of the bands, the amount of poly-ε-caprolactone present in the coating is estimated to be about 50%.
[0175] Example 19 Deposition of polylactide thin films on stainless steel in the presence of 4-nitrobenzenediazonium tetrafluoroborate A coating made from polylactide and 4-nitrobenzenediazonium tetrafluoroborate can be prepared by the following procedure.
[0176] Prepare a solution from 100 mL of DMSO, 50 g of L-lactide (L-lactide, (3S)cis-3,6-dimethyl 1,4-dioxane 2,5-dione, 3.47 M), 236 mg of 4-nitrobenzenediazonium tetrafluoroborate (0.01 M), and 10 mg of NaNO3 (0.025 M). This solution is deoxygenated and used for electrolysis with weak nitrogen bubbling (2 L min). -1 ) in the solution while scanning the stainless steel cathode from -0.2 to -2.8 V at 0.1 V / s.
[0177] A yellow, homogeneous, iridescent coating is observed that is adherent to finger rubbing and has a thickness of 1.1±0.3 μm measured by profilometer.
[0178] In the IR spectrum of the coating, 1758 cm -1 The carbonyl band at 1519 and 1346 cm -1 Both symmetric and asymmetric bands in the spectrum show the signature of 4-nitropolyphenylene. From this spectrum, a polylactide content of 55% can be estimated in the coating.
[0179] The structures are confirmed by ToF-SIMS analysis as shown in Table 1.
[0180] [Table 5]
[0181] The ToF-SIMS spectrum shows both the presence of polylactide and the presence of 4-nitrophenylene.
[0182] Example 20 Electrochemical impedance spectroscopy (EIS) measurements of (water-soluble) poly-HEMA coatings electrografted onto TiN showing that the coatings are swollen by water. EIS spectra are interpreted using a simple model consisting of a double layer capacitance in parallel with the polarization resistance in addition to the electrical resistance. This model can be represented by the equivalent electrical circuit shown in Figure 7, where Rs is the electrolyte resistance and Rp is the polarization resistance of the sample in the electrolyte. Q is a constant phase element, which is used instead of capacitance to account for the non-ideal capacitive response resulting from diffusion phenomena near the electrode (see, for example, C. Gabrielli. Technical Report. Intro Elect. Imp. Tech. CSB / AO1 (1990), Edt. Schlumberger Technologies Instrument Division Farnborough. Hampshire. England.).
[0183] Both the constant phase element and the polarization resistance features give an indication of the extent to which diffusion, and hence ionic conduction, is modified near the surface when the surface is covered with an electrografted HEMA layer. We find it more expedient to pursue this quest by assessing the extent to which the polarization resistance is modified by grafting.
[0184] Typical spectra giving the modulus (Z) and phase angle versus sampling frequency are shown in Figures 8 and 9. Figure 8 shows a comparison of the impedance modulus of a bare TiN specimen with that of a specimen coated with a layer of HEMA / 4-nitrophenyldiazonium tetrafluoroborate and of the same coated specimen after drying under vacuum at 30°C for 24 hours. The horizontal axis is frequency (Hertz) and the vertical axis is modules (Ohms.cm2). Figure 9 shows a comparison of the phase angle of a bare TiN coupon with that of a coupon coated with a layer of HEMA / 4-nitrophenyldiazonium tetrafluoroborate, and the phase angle of the same coated coupon after drying under vacuum at 30° C. for 24 hours. The horizontal axis is frequency (Hertz) and the vertical axis is phase angle (degrees).
[0185] These clearly demonstrate the fact that coating the TiN surface with a HEMA / 4-nitrophenyldiazonium tetrafluoroborate polymer layer has only a small effect on the overall impedance of the electrode. It can be seen that the same spectra were also recorded after drying the coated electrode at 30° C. for 24 hours under a vacuum of 700 mbar, i.e., Figures 8 and 9 show that the impedance remains comparable, which is evidence that the swelling of the HEMA / 4-nitrophenyldiazonium tetrafluoroborate coating on the electrode is reversible.
[0186] To quantify this comparison, we extracted the electrical parameters in Figure 8 by performing a mathematical nonlinear least-squares fit of the experimental data in Figure 9. Typical results of the spectral fit are shown in Table 6.
[0187] [Table 6]
[0188] The percentage change in polarization resistance is
number
[0189] After coating the TiN electrode by electrografting with HEMA / 4-nitrophenyldiazonium tetrafluoroborate film according to the present invention, the low polarization resistance is only slightly different from that of the bare TiN specimen. This observation indicates that the polymer is not an electrical insulator, i.e., it is permeable to ions and therefore completely swollen by the electrolyte.
[0190] Although completely swollen by the electrolyte, the HEMA / 4-nitrophenyldiazonium tetrafluoroborate coating is insoluble in water, which is well-indicated to be due to the strong grafting of the coating onto the TiN surface.
[0191] Example 21 The grafted polymer layer can be used as an adhesion primer for a much thicker layer that is sprayed on top of it. Electropolished dog-bone shaped 316L stainless steel coupons measuring 7 x 1 cm x 1 mm are homogeneously coated with a poly-BUMA electrografted layer by the procedure described in Example 1. The specific film thickness is 150 nm.
[0192] The central (narrow) part of the coupon is spray coated on one side with 5 μm of PLA (polylactide acid). This is achieved by covering the two wide ends of the dog-bone coupon and spraying a solution of PLA in chloroform (3% w / w). The coupon is vacuum dried to a constant weight. Four dots are written on the PLA layer with an ink pen.
[0193] The specimen was then placed in an INSTRON (5 kN capacity, ε' = 10 -3 s -1 ) machine and pull it apart at both ends. The deformation of a point on the surface is recorded by a video camera and it is verified that the deformation speed of the point is equal to the speed imposed by the INSTRON machine. If it is not, this means that some delamination has occurred in the sandwich layers.
[0194] Figure 10 shows and compares the corrected strain / stress response of coupons with and without a poly-BUMA electrografted underlayer in the INSTRON machine. The black curves are comparable for all tests, with and without an electrografted underlayer, and show the elastic, inelastic and fracture behavior of the metal coupon itself, which is generally largely unaffected by the 5 μm coating.
[0195] The numbered points on the curves indicate the information provided by the camera during the test, and more particularly, when the camera detected the onset of delamination.
[0196] The results of the tests show that in the absence of an electrografted underlayer, the PLA layer delaminates at low stress and strain on 316 L stainless steel (points #15 and #18 in Figure 10), whereas when an electrografted layer of BUMA is used as the underlayer, the sandwich structure never delaminates until metal fracture (points #11, 12, 13, 14, 16, 17 in Figure 17-2).
[0197] This demonstrates the significant improvement achieved by the electrografted layer of the present invention, even though the layer is very thin compared to the overlying 5 μm layer. [Brief description of the drawings]
[0198] [Figure 1] Initial (black line) and final (dashed line) cyclic voltammograms of the solution demonstrating film formation. [Diagram 2] The increase in thickness of the coating obtained on a stainless steel coupon from MMA and 4-nitrobenzenediazonium tetrafluoroborate in the presence of pentaerythritol tetraacrylate versus the number of electrochemical cycles. The horizontal axis is the number of cycles, and the vertical axis is the thickness of the coating (Å). [Diagram 3] The relationship between the thickness of the p-BUMA coating on 316L and the cathodic final potential is shown (DNO2 concentration is 10-2 mol / l). [Figure 4] The relationship between the thickness of the p-BUMA coating on 316L and the cathodic final potential is shown (DNO2 concentration is 10-3 mol / l). [Diagram 5] The relationship between (C=O) / (NO2)(IR) and the cathodic final potential is shown. The DNO2 concentration is 10-2 mol / l. [Figure 6] The relationship between (C=O) / (NO2)(IR) and the final cathode potential is shown. The DNO2 concentration is 10-3 mol / l. [Figure 7] The equivalent electrical circuit is shown. [Figure 8]A comparison of the impedance modulus of a bare TiN specimen with that of a specimen coated with a layer of HEMA / 4-nitrophenyldiazonium tetrafluoroborate and of the same coated specimen after drying for 24 hours at 30°C under vacuum is shown. The horizontal axis is frequency (Hertz) and the vertical axis is modules (Ohms.cm2). [Figure 9] A comparison is shown of the phase angle of a bare TiN coupon, a coupon coated with a layer of HEMA / 4-nitrophenyldiazonium tetrafluoroborate, and the phase angle of the same coated coupon after drying under vacuum at 30° C. for 24 hours. The horizontal axis represents frequency (Hertz) and the vertical axis represents phase angle (degrees). [Figure 10] 1 shows the compensated strain / stress response of the specimen in the INSTRON machine, with and without the poly-BUMA electrografted sublayer. Horizontal axis is true deformation, horizontal axis is true strain / stress (MPa).
Claims
1. An object comprising a conductive or semiconductive surface, having an organic coating grafted to said surface or a portion thereof, said organic coating comprising a chemical structure derived from at least one monomer or macro-object having a chain polymerizable functional group and being a precursor of said organic coating, and a chemical structure derived from an aryl diazonium salt or an electroreduction by-product thereof; the monomer is selected from methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, dodecyl methacrylate, hydroxypropyl methacrylate, trimethylsilylpropyl methacrylate, 2-methacryloyloxyethyl phosphorylcholine, cyanoacrylate, acrylic acid, methacrylic acid, isoprene, ethylene, propylene, ethylene oxide, and lactide; The organic coating has a thickness of 10 nm to 10 μm; The organic coating is formed on the surface or a portion thereof by a covalent bond, and 1. An object comprising a conductive or semiconductive surface, wherein the composition of said organic coating is not uniform in a direction perpendicular to said surface.
2. 10. The article of claim 1, wherein the organic coating is richer in diazonium and its electrochemical reduction byproducts near the surface, while being richer in polymer away from the surface.
3. The at least one polymerizable compound having a chain polymerizable functional group and being a precursor of the organic coating.
10. The article of claim 1, wherein the at least one monomer is selected from ethylene and propylene.
4. 4. The object according to claim 1, wherein the surface is a surface of stainless steel, cobalt and its alloys, titanium and its alloys, iron, copper, nickel, niobium, aluminium, silver, silicon (doped or not), silicon carbide, titanium nitride, tungsten, tungsten nitride, tantalum, tantalum nitride or platinum-iridium or a precious metal selected from iridium, platinum and gold.
5. The object according to any one of claims 1 to 3, wherein the macro object is a nanometer or micrometer sized object, and the macro object surface is functionalized with vinyl groups activated by electron-withdrawing groups or cyclic groups.
6. The object according to any one of claims 1 to 5, wherein the organic coating is not crosslinked.
7. 6. The article of claim 1, wherein the aryl diazonium salt is nitrophenyl diazonium and the monomer is BUMA, and the organic coating is not uniform perpendicular to the surface, being richer in nitrophenyl diazonium and its electrochemical reduction byproducts near the surface while being richer in polyBUMA away from the surface.
8. The object of claim 1 , wherein the object is biocompatible.
9. 2. The article of claim 1, wherein the conductive surface is 316L stainless steel, the polymer layer electrically grafted onto the 316L stainless steel is a 150 nm thick layer of PolyBUMA, and a 5 micrometer thick layer of PLA is spray formed onto the PolyBUMA layer.
10. The object of claim 8 or 9, wherein the object is a stent.