Porous carbon material and its manufacturing method, precursor of porous carbon material, and electrode material using porous carbon material

A cost-effective method for producing porous carbon materials through a zinc acetate and polyvinyl alcohol reaction followed by high-temperature firing addresses the high costs and safety issues of conventional activation methods, resulting in materials suitable for low-resistance electrodes.

JP7582917B2Active Publication Date: 2024-11-13SEIWA ELECTRIC MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021129202
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-05
Publication Date
2024-11-13
Estimated Expiration
2041-08-05

AI Technical Summary

Technical Problem

Conventional methods for producing porous materials like activated carbon require costly activation treatments, such as gas and chemical activation, which involve hazardous chemicals and increase disposal costs, making the process expensive and unsafe.

Method used

A method to produce porous carbon materials using a synthetic reaction between polyvinyl alcohol and zinc acetate in water, followed by firing at high temperatures to create pores without the need for activation steps, utilizing a precursor that forms zinc oxide during firing, which leaves voids and creates a porous structure.

Benefits of technology

This method allows for the production of porous carbon materials with high specific surface area and mesopore volume, reducing production costs by eliminating the need for hazardous chemicals and complex activation processes, and enabling the use of the material as a low-resistance electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582917000002
    Figure 0007582917000002
  • Figure 0007582917000003
    Figure 0007582917000003
  • Figure 0007582917000004
    Figure 0007582917000004
Patent Text Reader

Abstract

To provide a porous carbon material which can be manufactured by a simple work process without an activation process and a manufacturing method thereof and an electrode material using the porous carbon material.SOLUTION: In a manufacturing method of a porous carbon material, a precursor is prepared by a synthetic reaction of polyvinyl alcohol and zinc acetate, followed by firing the precursor at a high temperature until a peak (2θ) of diffraction angles of 31.8, 34.5, and 36.3 by X-ray diffraction (each peak has an error range of ±0.3) is no longer detected.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a porous carbon material that can be obtained through simple work steps that omit an activation step, a method for producing the same, and an electrode material that uses the porous carbon material. [Background technology]

[0002] In general, a porous material such as activated carbon is used as the polarizable electrode of an electric double layer capacitor because of its large surface area and excellent electrical conductivity.

[0003] Conventionally, in the process of producing such porous materials such as activated carbon, activation treatment such as gas activation or chemical activation has been necessary (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-142967 A [Patent Document 2] WO2007 / 034873 publication Summary of the Invention [Problem to be solved by the invention]

[0005] However, when activation treatment such as gas activation or chemical activation is required as in the conventional methods for producing porous materials described above, the costs of procuring the gas and chemicals, disposal costs, and manufacturing costs of the activation process itself increase. In particular, in the case of chemical activation, strong acids such as hydrofluoric acid and concentrated hydrochloric acid are used, which increases disposal costs, and consideration must be given to the safety of the work, resulting in an expensive product.

[0006] An object of the present invention is to provide a porous carbon material that can be produced through simple work steps without an activation step, a production method thereof, and an electrode material using the porous carbon material. [Means for solving the problem]

[0007] The method for producing a porous carbon material according to the present invention for solving the above problems is to use a polyvinyl alcohol Aqueous solution of polyvinyl alcohol dissolved in water by heating and zinc acetate Aqueous solution of zinc acetate dissolved in water by heating By the synthesis reaction with In surface analysis by X-ray photoelectron spectroscopy, the Zn2p peak appearing at 1020-1030 (eV), the O1s peak appearing at 530-540 (eV), and the C1s peak appearing at 280-300 (eV) are all detected. A precursor is prepared, and then the precursor is baked at a high temperature until peaks at diffraction angles (2θ) of 31.8, 34.5, and 36.3 (each peak has an error of ±0.3) by X-ray diffraction are no longer detected. Many Method for producing porous carbon material When the weight ratio of zinc acetate to polyvinyl alcohol used corresponds to 0.5, 1.0, 1.5, 2.0, 2.5, and 3.0, the specific surface area of ​​the porous carbon material after firing is 338, 377, 1078, 1395, 1740, and 2498 m 2 By utilizing this relationship, the weight ratio of zinc acetate to polyvinyl alcohol is determined to prepare a porous carbon material having a desired specific surface area. It is something.

[0008] The method for producing the porous carbon material includes the steps of: When the weight ratio of zinc acetate to polyvinyl alcohol used was 0.5, 1.0, 1.5, 2.0, 2.5, and 3.0, the mesopore specific surface areas of the calcined porous carbon materials were 64, 78, 147, 189, 358, and 869 m. 2 By utilizing this relationship, the weight ratio of zinc acetate to polyvinyl alcohol is determined to prepare a porous carbon material having a desired mesopore specific surface area. It may also be something.

[0009] The method for producing the porous carbon material includes the steps of: When the weight ratio of zinc acetate to polyvinyl alcohol used is 0.5, 1.0, 1.5, 2.0, 2.5, and 3.0, the recovery rates of the porous carbon material after firing are 9.10, 8.05, 3.46, 2.16, 0.87, and 0.37%. By utilizing this relationship, the weight ratio of zinc acetate to polyvinyl alcohol used is determined to prepare a porous carbon material with a desired recovery rate. It may also be something.

[0013] The porous carbon material of the present invention for solving the above problems is a porous carbon material obtained by the above-mentioned method for producing a porous carbon material, in which no peaks (2θ) at diffraction angles of 31.8, 34.5, or 36.3 (all peaks have an error of ±0.3) are detected by X-ray diffraction. ,ratio Surface area 1395m 2 / g or more.

[0014] The porous carbon material is a porous carbon material obtained by the method for producing a porous carbon material, and no peaks (2θ) at diffraction angles of 31.8, 34.5, or 36.3 (each peak has an error of ±0.3) are detected by X-ray diffraction. , M Pore ​​specific surface area 189m 2 / g or more.

[0018] In order to solve the above problems, an electrode material of the present invention contains the above porous carbon material.

[0019] In the above-mentioned method for producing a porous carbon material, the synthesis reaction between polyvinyl alcohol and zinc acetate is carried out using only water as a solvent, without using an organic solvent, and using an aqueous solution of polyvinyl alcohol dissolved by heating and an aqueous solution of zinc acetate dissolved by heating in the same manner. In this case, the concentration of each aqueous solution is not particularly limited, and an aqueous solution prepared as appropriate can be used. However, since there is a relationship in which the specific surface area of ​​the completed porous carbon material increases as the amount of zinc acetate used relative to the amount of polyvinyl alcohol used increases, it is desirable to determine the mass ratio of the amounts of zinc acetate and polyvinyl alcohol used according to the specific surface area required for the porous carbon material to be produced.

[0020] A precursor of a porous carbon material can be prepared by carrying out a synthesis reaction between the above-mentioned aqueous polyvinyl alcohol solution dissolved by heating and the aqueous zinc acetate solution dissolved by heating. In this case, by carrying out a synthesis reaction between the above-mentioned aqueous polyvinyl alcohol solution dissolved by heating and the aqueous zinc acetate solution dissolved by heating, the precursor has a Zn2p peak appearing at 1020 to 1030 (eV), an O1s peak appearing at 530 to 540 (eV), and a C1s peak appearing at 280 to 300 (eV) all detected in a surface analysis by X-ray photoelectron spectroscopy, as shown in FIG. 1, and the entire precursor contains Zn bonds and Zn elements.

[0021] As shown in FIG. 2, when the relative intensity ratio of the three main peaks (2θ) confirmed by X-ray diffraction is focused on, as the amount of zinc acetate used relative to the amount of polyvinyl alcohol used increases, the peak (2θ) at a diffraction angle of about 12 degrees by X-ray diffraction tends to become larger than the other two peaks (2θ). When the zinc acetate used in the synthesis reaction of the precursor is changed to zinc oxide, as shown in FIG. 3, only the peaks (2θ) of polyvinyl alcohol and zinc oxide are confirmed, and no trace of reaction is observed. From this, it can be confirmed that when the synthesis reaction is performed using polyvinyl alcohol and zinc oxide, as described above, as the amount of zinc acetate used relative to the amount of polyvinyl alcohol used increases, the synthesis reaction proceeds with a tendency for the peak (2θ) at a diffraction angle of about 12 degrees by X-ray diffraction to become relatively larger than the other two peaks (2θ).

[0022] The precursor is calcined to form a porous carbon material. At this time, as shown in FIG. 4, the three main peaks (2θ) confirmed in FIG. 2 disappear as the calcination temperature increases, and zinc oxide (ZnO) is generated in their place during the calcination process. At this time, it can be confirmed that peaks (2θ) with diffraction angles of 31.8, 34.5, and 36.3 (each peak has an error of ±0.3) are generated by X-ray diffraction. These zinc oxide (ZnO) peaks are reduced and disappear when the temperature is further increased and calcined at a high temperature. As a result, the Zn bonds and Zn elements of the precursor generate zinc oxide (ZnO) during the calcination process, and voids are formed in the places where the zinc oxide (ZnO) disappears by calcining at a high temperature, resulting in a calcined body with a porous structure. This can be confirmed by the weight loss around 900°C, which is the boiling point of zinc, as shown in FIG. 5(a), and the endothermic reaction caused by the reduction of zinc oxide around 900°C, as shown in FIG. 5(b). The firing is performed at a high temperature until these zinc oxide (ZnO) peaks are no longer detected, while observing the appearance and disappearance of these zinc oxide (ZnO) peaks. This observation may be to observe the zinc oxide (ZnO) peaks in each temperature range as shown in FIG. 4, to observe the weight loss around 900°C, which is the boiling point of zinc, as shown in FIG. 5(a), to observe the endothermic reaction caused by the reduction of zinc oxide around 900°C, as shown in FIG. 5(b), or to observe a plurality of observations selected from these.

[0023] It is preferable to perform the calcination at a high temperature until these zinc oxide (ZnO) peaks are no longer detectable, but it is also possible not to perform the calcination until they completely disappear. In this case, if the calcination is performed at 907°C or higher, which is the boiling point of zinc, pores can be reliably formed to make the material porous, but even if the temperature is lower than the boiling point of zinc, pores can be formed in the traces of zinc oxide or zinc that had entered, making the material porous, if the calcination is performed for a long period of time. It has been confirmed that when the calcination is performed at 850°C or higher, the above-mentioned peaks can be eliminated by the long-term calcination, and pores can be formed to make the material porous. Therefore, the calcination conditions are not particularly limited as long as the conditions are such that the zinc oxide can be decomposed and the zinc can be evaporated, and as a guideline, it is preferable to perform the calcination for 30 minutes to 8 hours, or 3.84 hours to 61.6 hours per 1 g of precursor. If the calcination time exceeds 30 hours or 2 hours per 1 g of precursor, zinc oxide or zinc starts to disappear exponentially or n-th order (n>1) and pores are formed in their places, so that the above-mentioned peaks can be eliminated by calcining for 30 hours or more or 2 hours or more per 1 g of precursor at 850° C. or higher. Furthermore, if the temperature is 907° C. or higher, which is the boiling point of zinc, not only can the above-mentioned peaks be eliminated, but also amorphous zinc oxide and zinc that were not detected as the above-mentioned peaks can be eliminated, so that pores can be formed in the places where the amorphous zinc oxide and zinc have disappeared, and a porous carbon material with a higher porousness and a higher non-surface area can be obtained.

[0024] In addition, the precursor used in this firing is formed by a synthesis reaction between an aqueous polyvinyl alcohol solution obtained by dissolving polyvinyl alcohol in water by heating, and an aqueous zinc acetate solution obtained by dissolving zinc acetate in water by heating, so that zinc elements are uniformly dispersed in the matrix of the precursor containing zinc bonds. Therefore, when these zinc bonds and zinc elements are released from the precursor during firing via zinc oxide and zinc, zinc and carbon are consumed, and many voids are formed in the places where they are released, resulting in a porous fired body.

[0025] The firing may be performed in an inert gas atmosphere (nitrogen gas or argon gas atmosphere). In this case, the firing atmosphere may be replaced with the inert gas atmosphere at a gas flow rate of 0.1 to 1.0 liters / minute. The firing may be performed by increasing the temperature from a predetermined temperature at a rate of about 5 to 10°C / minute to a predetermined temperature. Furthermore, the firing may be performed under a reduced pressure atmosphere. The firing furnace may be a furnace tube type, a box furnace, a rotary kiln furnace, or the like.

[0026] The porous carbon material thus constructed is a precursor in which the Zn2p peak appearing at 1020-1030 (eV), the O1s peak appearing at 530-540 (eV), and the C1s peak appearing at 280-300 (eV) are all detectable, i.e., a precursor in which Zn elements are uniformly dispersed in a precursor in which the skeleton is formed with a three-dimensional network structure in which Zn bonds, O bonds, and C bonds are firmly formed. By baking this, the Zn bonds and Zn of the Zn elements contained in the precursor become zinc oxide (ZnO), and then by baking at a higher temperature, the zinc oxide (ZnO) disappears, resulting in a porous carbon material in which peaks (2θ) at diffraction angles of 31.8, 34.5, and 36.3 (all peaks with an error of ±0.3) are not detectable by X-ray diffraction. In this way, the zinc ions of the precursor pass through zinc oxide (ZnO) during the firing process and then escape, and by making the porous carbon material in which the diffraction angle peak (2θ) caused by these is not detected, pores are generated at the traces of the zinc ions that have escaped, making it possible to make the material porous. In addition, by going through such a process, it is possible to form many mesopores (2 to 50 nm) defined by IUPAC, and the ratio of the specific surface area of ​​the mesopores to the total specific surface area can be increased. Specifically, this ratio can be made 13.5% or more. If the ratio of the specific surface area occupied by the mesopores is increased, it becomes possible to more smoothly take in and out the electrolyte ions, making it suitable as an electrode material with low electrical resistance.

[0027] Moreover, the porous carbon material thus constructed can be made porous by a single firing process, and since it does not contain impurities such as metal oxides that inhibit the formation of pores, acid treatment and the like are not required. Therefore, the fired body obtained after the firing process can be used as is, and the porous carbon material can be obtained through a simple work process.

[0028] In addition, this porous carbon material has a relationship in which the specific surface area of ​​the completed porous carbon material increases as the amount of zinc acetate used relative to the amount of polyvinyl alcohol used increases. As shown in FIG. 6, when the amount of zinc acetate used relative to polyvinyl alcohol increases, the specific surface area of ​​the obtained porous carbon material increases, but at the same time, the recovery rate also decreases. Therefore, when an absolute specific surface area is required, the amount of zinc acetate used is reduced to give priority to the recovery rate of the porous carbon material even if the specific surface area is somewhat reduced, and the porous carbon material is produced by prioritizing the specific surface area of ​​the porous carbon material, even if the recovery rate is somewhat reduced, and when a relative specific surface area is required, the amount of zinc acetate used is increased to give priority to the specific surface area of ​​the porous carbon material, even if the recovery rate is somewhat reduced, and thus it is possible to produce a porous carbon material suited to the application and needs. The specific surface area of ​​the mesopores also increases as the amount of zinc acetate used increases, so it is possible to produce a porous carbon material suited to the application and needs in the same way. Effect of the Invention

[0029] As described above, according to the present invention, the precursor is prepared by a synthetic reaction between polyvinyl alcohol and zinc acetate, and then the precursor is calcined, which is a simple process. This eliminates the need to use an organic solvent when preparing the precursor, and when preparing the calcined body, calcination is performed at a high temperature until peaks (2θ) at diffraction angles of 31.8, 34.5, and 36.3 (all peaks have an error of ±0.3) by X-ray diffraction are no longer detected, eliminating the need for gas activation or chemical activation after carbonization. This eliminates the disposal costs of organic solvents, acids, etc., and simplifies unnecessary work steps, allowing a porous carbon material to be obtained easily and at low cost. Moreover, the resulting porous carbon material is When the weight ratio of zinc acetate to polyvinyl alcohol used was 0.5, 1.0, 1.5, 2.0, 2.5, and 3.0, the specific surface area of ​​the porous carbon material after firing was 338, 377, 1078, 1395, 1740, and 2498 m 2 By utilizing this relationship, the weight ratio of zinc acetate to polyvinyl alcohol is determined, Since it is possible to obtain a porous carbon material with a desired specific surface area, it is possible to produce a porous carbon material according to the application or needs. [Brief description of the drawings]

[0030] [Figure 1] (a) is the overall data of the surface analysis by X-ray photoelectron spectroscopy of the precursor used in the manufacturing method of the porous carbon material according to the present invention, (b) is the data of the zinc peak portion, (c) is the data of the oxygen peak portion, and (d) is the data of the carbon peak portion. [Diagram 2] FIG. 1 is a graph showing diffraction data of powder X-ray diffraction of a precursor used in a method for producing a porous carbon material according to the present invention, and showing the correlation between each diffraction data when the amount of zinc acetate used relative to the amount of polyvinyl alcohol used is changed. [Diagram 3] FIG. 3 is a graph showing diffraction data of powder X-ray diffraction of a precursor according to a comparative example in which the zinc acetate in FIG. 2 is changed to zinc oxide, and showing the correlation between each diffraction data when the amount of zinc oxide used relative to the amount of polyvinyl alcohol used is changed. [Figure 4] 1 is a graph showing diffraction data by powder X-ray diffraction of a precursor used in a method for producing a porous carbon material according to the present invention, in each temperature range during the process of calcining the precursor to obtain a calcined body. [Diagram 5] FIG. 1(a) is a graph showing the results of differential thermal analysis in the process of calcining a precursor used in the production method for a porous carbon material according to the present invention to obtain a calcined body, and FIG. 1(b) is a graph showing the results of thermogravimetric analysis of the same. [Figure 6] 1 is a graph showing the relationship between the specific surface area and recovery rate of the obtained porous carbon material when the amount of zinc acetate used relative to the amount of polyvinyl alcohol used is changed in the production method of a porous carbon material according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] Hereinafter, an embodiment of the present invention will be described.

[0032] (Preparation of Precursor) [Example 1] 1.0 g of polyvinyl alcohol was placed in a beaker containing 30 g of water, and the mixture was heated and stirred at 70° C. for 1 hour. 0.5 g of zinc acetate was placed in a beaker containing 30 g of water, subjected to ultrasonic cleaning for 10 minutes, and then heated and stirred at 70° C. for 1 hour. The polyvinyl alcohol aqueous solution obtained above and an aqueous zinc acetate solution were mixed and heated with stirring at 70° C. for 2 hours. The liquid obtained above was then dried at 80° C. for 24 hours. The solid thus obtained was pulverized in a crusher (mixer) and further dried under reduced pressure at 100° C. for 24 hours to obtain a precursor.

[0033] [Examples 2-6, Comparative Examples 1-5] Each precursor of Examples 2 to 6 was prepared in the same manner as in Example 1 above, except that the amount of zinc acetate was changed to 1.0 g, 1.5 g, 2.0 g, 2.5 g, and 3.0 g. Each precursor of Comparative Examples 1-5 was prepared in the same manner as in Example 1 above, except that zinc oxide was used instead of zinc acetate, and the amounts were 0.5 g, 1.0 g, 1.5 g, 2.0 g, and 2.5 g.

[0034] (Surface analysis of precursors by X-ray photoelectron spectroscopy) The precursors prepared in Examples 1 to 6 were used to carry out surface analysis of the precursors by X-ray photoelectron spectroscopy (XPS). The measuring equipment and measuring conditions are as follows. The results of Example 1 are shown in FIG. Measurement model: ULVAC-PHI ESCA5700 Measurement conditions: X-ray source: Mg, accelerating voltage: 400 W (15 kV)

[0035] From the results in FIG. 1, in the precursor of Example 1, all of the following peaks were detected: a Zn2p peak appearing at 1020 to 1030 (eV) where a Zn-related bond is present, an O1s peak appearing at 530 to 540 (eV) where an O-related bond is present, and a C1s peak appearing at 280 to 300 (eV) where a C-related bond is present. Although not shown, similar results were also confirmed for Examples 2-6.

[0036] (Powder X-ray diffraction of precursor) Approximately 0.02 g of the precursor powder prepared by the above method was placed on a sample holder, leveled, and diffraction was performed. The measurement equipment and measurement conditions are as follows. The results of Examples 1-4 are shown in Figure 2, and the results of Comparative Examples 1-5 are shown in Figure 3. Measurement model: X-ray diffraction device SmartLab SE (manufactured by Rigaku Corporation) Measurement conditions: Measurement angle range is 2θ=2°~60° Scan speed 10° / min X-ray source;Cu(Kα)

[0037] As shown in FIG. 2, in the precursor according to the embodiment, a peak of zinc element derived from zinc acetate and a peak derived from zinc bonds formed by the reaction of the zinc acetate with polyvinyl alcohol can be confirmed, whereas in the precursor according to the comparative example, as shown in FIG. 3, only a peak resulting from the mixture of zinc oxide and polyvinyl alcohol can be confirmed, and no trace of reaction was confirmed.

[0038] (Baking of precursor) A part of the precursor according to Example 1 above was used as a sample, and the sample was heated in a nitrogen gas atmosphere at a gas flow rate of 0.2 liters / min from room temperature 25°C at a temperature increase rate of 10°C / min up to 1100°C to obtain a porous carbon material.

[0039] (X-ray diffraction during the firing process) X-ray diffraction was performed on the sample during the firing process of the precursor according to the above-mentioned Example 1. The measuring device and measuring conditions are as follows. The results are shown in FIG. Measurement model: smartlab SE (Rigaku Corporation), multipurpose high-temperature device Measurement conditions: 0.02g of sample is placed in a platinum holder and inserted into the multipurpose high temperature unit of the SmartLab SE. The temperature rise program is to raise the temperature at 10°C / min in a nitrogen gas atmosphere (0.2 liters / min), and to 50°C, 100°C, 150°C, ..., 1100°C, and when each temperature is reached in 50°C increments, X-ray measurement begins. The measurement angle range is 2θ=2°~40°. Scan speed 10° / min X-ray source;Cu(Kα)

[0040] (Differential thermal analysis and thermogravimetric analysis during firing) In the precursor firing step according to the above-mentioned Example 1, a differential thermal analysis and a thermogravimetric analysis were performed on the sample. The measuring equipment and measuring conditions are as follows. The results are shown in FIG. Measurement model: DTG-60 (Shimadzu Corporation) Measurement conditions: Approximately 5 mg of the sample was placed in a platinum holder and heated at 10°C / min in a nitrogen gas atmosphere (0.2 liters / min). The temperature was raised to 30-38°C (2θ) and the sample was fired at a high temperature until the zinc oxide reflection planes (Miller indices) (100), (002), and (101) could no longer be confirmed from the low-angle side. Measurement model: Same as above Measurement conditions: Same as above

[0041] (Considerations on the firing process) From the results of Figures 4 and 5, in the low temperature region, the zinc element peaks from zinc acetate confirmed in the precursor and the zinc bond peaks formed by the reaction of zinc acetate with polyvinyl alcohol can be confirmed, but as the temperature increases, these peaks gradually decrease, and instead, the reflection planes (Miller indices) (100), (002), and (101) of zinc oxide can be confirmed from the low angle side at 30 to 38 degrees (2θ). However, it was confirmed that these zinc oxide peaks also completely disappeared at 1050°C. As shown in Figure 5(a), it can be confirmed that the reduction of zinc oxide begins and zinc disappears with the weight loss around 900°C. In addition, as shown in Figure 5(b), it is shown that an endothermic reaction due to the reduction of zinc oxide occurs around 900°C.

[0042] (Preparation of porous carbon materials) The precursors according to Examples 1 to 6 prepared by the above-mentioned methods were each calcined to obtain a porous carbon material. The calcination conditions were the same as those in Example 1, and the porous carbon material was naturally cooled to obtain the porous carbon material. The recovery rate was calculated from the relationship between the total amount of zinc acetate and polyvinyl alcohol used in the preparation of the precursor and the amount of the porous carbon material obtained by calcination. The results are shown in Table 1.

[0043] (Nitrogen adsorption / desorption measurement (specific surface area / pore distribution measurement)) Each of the porous carbon materials according to Examples 1-6 prepared by the above method was dried under reduced pressure at 200°C for 24 hours, and the moisture adsorbed in the porous carbon material was desorbed in a room temperature atmosphere. Then, 0.02 g of each powder of the porous carbon material was placed in a sample tube, and a nitrogen adsorption / desorption isothermal curve was measured in a liquid nitrogen atmosphere using a specific surface area / pore distribution measuring device (BELLSORP-miniII: manufactured by Microtrack Bell Co., Ltd.). The specific surface area and the specific surface area of ​​mesopores were calculated using an analysis program (I type (ISO9277) BET automatic analysis) of the same device. In addition, the specific surface area and the specific surface area of ​​mesopores were measured in the same manner for the activated carbon according to Comparative Example 6 (YP50F manufactured by Kuraray Chemical Co., Ltd.) and the activated carbon according to Comparative Example 7 (MSP20 manufactured by Kansai Thermochemical Co., Ltd.) as comparative objects for comparing the specific surface area and the specific surface area of ​​mesopores of the porous carbon materials according to Examples 1-6. The results are shown in Table 1. In addition, for the porous carbon materials according to Examples 1-6, the relationship between the specific surface area and the recovery rate depending on the mixing ratio of zinc acetate and polyvinyl alcohol during the preparation of the precursor was determined. The graphed results are shown in FIG.

[0044] [Table 1]

[0045] From the above results, it was confirmed that when the amount of zinc acetate used relative to polyvinyl alcohol was increased, the recovery rate decreased, but a porous carbon material with a high specific surface area was obtained, and when the amount of zinc acetate used relative to polyvinyl alcohol was decreased, the recovery rate increased, but a porous carbon material with a low specific surface area was obtained. It was confirmed that the specific surface area of ​​the porous carbon material can be controlled by the blending ratio of zinc acetate and polyvinyl alcohol. Regarding the specific surface area of ​​the mesopores, it was confirmed that when the amount of zinc acetate used was increased, the specific surface area of ​​the mesopores increased, and when the amount of zinc acetate used was decreased, the specific surface area of ​​the mesopores decreased, and it was confirmed that a porous carbon material with a desired specific surface area could be obtained. In addition, it was confirmed that when a porous carbon material was prepared using the precursor of the comparative example using zinc oxide instead of zinc acetate, it could not be made porous.

[0046] From the above results, it was confirmed that the porous carbon material according to the present invention can provide a porous carbon material in which the ratio of the specific surface area of ​​mesopores to the total specific surface area is 13.5% or more, which is a dramatically higher ratio, compared to the activated carbons according to Comparative Examples 6 and 7. In particular, in the case of the porous carbon material of Example 4-6 in which the amount of zinc acetate used was increased, a porous carbon material can be obtained in which the specific surface area of ​​the mesopores is overwhelmingly larger than the specific surface area of ​​the mesopores of the activated carbons according to Comparative Examples 6 and 7. Therefore, a porous carbon material having a large pore distribution of mesopores through which electrolyte ions can easily enter and exit can be obtained, making the porous carbon material according to the present invention suitable as an electrode material with low electrical resistance.

[0047] The present invention can be embodied in various other forms without departing from its spirit or main features. Therefore, the above-described embodiments are merely illustrative in all respects and should not be interpreted as being limiting. The scope of the present invention is defined by the claims and is not limited to the text of the specification. Furthermore, all modifications and changes within the scope of the claims are within the scope of the present invention.

Claims

1. A synthetic reaction between an aqueous solution of polyvinyl alcohol, in which polyvinyl alcohol is dissolved in water by heating, and an aqueous solution of zinc acetate, in which zinc acetate is dissolved in water by heating, is carried out. A precursor is prepared in which a Zn2p peak appearing at 1020 to 1030 (eV), an O1s peak appearing at 530 to 540 (eV), and a C1s peak appearing at 280 to 300 (eV) are all detected in a surface analysis by X-ray photoelectron spectroscopy; Thereafter, the precursor is calcined at a high temperature until peaks at diffraction angles (2θ) of 31.8, 34.5, and 36.3 (each peak has an error of ±0.3) by X-ray diffraction are no longer detected, When the weight ratio of zinc acetate to polyvinyl alcohol used was 0.5, 1.0, 1.5, 2.0, 2.5, and 3.0, the specific surface areas of the porous carbon materials after firing were 338, 377, 1078, 1395, 1740, and 2498 m 2 Using the relationship of / g, A method for producing a porous carbon material, comprising determining a weight ratio of zinc acetate to polyvinyl alcohol to prepare a porous carbon material having a desired specific surface area.

2. When the weight ratio of zinc acetate to polyvinyl alcohol used was 0.5, 1.0, 1.5, 2.0, 2.5, and 3.0, the mesopore specific surface areas of the porous carbon materials after firing were 64, 78, 147, 189, 358, and 869 m. 2 Using the relationship of / g, 2. The method for producing a porous carbon material according to claim 1, wherein a porous carbon material having a desired specific mesopore surface area is prepared by determining the weight ratio of zinc acetate and polyvinyl alcohol used.

3. When the weight ratio of zinc acetate to polyvinyl alcohol used is 0.5, 1.0, 1.5, 2.0, 2.5, and 3.0, the recovery rates of the porous carbon material after firing are 9.10, 8.05, 3.46, 2.16, 0.87, and 0.37%, respectively.

2. The method for producing a porous carbon material according to claim 1, wherein the porous carbon material is prepared with a desired recovery rate by determining the weight ratio of zinc acetate and polyvinyl alcohol used.

4. A porous carbon material obtained by the method for producing a porous carbon material according to claim 1, No peaks (2θ) were detected at diffraction angles of 31.8, 34.5, and 36.3 (all with an error of ±0.3) by X-ray diffraction, and the specific surface area was 1395 m 2 / g or more.

5. A porous carbon material obtained by the method for producing a porous carbon material according to claim 2, No peaks (2θ) were detected at diffraction angles of 31.8, 34.5, and 36.3 (all with an error of ±0.3) by X-ray diffraction, and the mesopore specific surface area was 189 m 2 / g or more.

6. An electrode material comprising the porous carbon material according to claim 4 or 5.

Citation Information

Patent Citations

  • Controllable synthetic method for phosphorus doped graphitization carbon spheres with hollow structures

    CN103183342A

  • Method for preparing nitrogen-doped porous carbon material on the basis of folic acid

    CN105129768A

  • Manufacturing method of nitrogen-containing carbon material

    JP2019218232A

  • Method for producing activated carbon

    JP2020142967A

  • Method for producing porous carbon material

    JP2020189760A