Thermoplastic elastomer-based foams
A composition of thermoplastic polyurethane, styrene polymer, and impact modifier enhances the processability and mechanical properties of bead foams, addressing adhesive bonding issues and reducing density for improved shoe components.
Patent Information
- Application Number
- JP2021514417
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-14
- Filing Date
- 2019-09-12
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2039-09-12
AI Technical Summary
Existing bead foams based on thermoplastic polyurethanes face challenges in achieving improved processability and mechanical properties, particularly in applications like shoe components, where insufficient adhesive bonding leads to weakened mechanical properties and increased material requirements due to higher densities.
A composition comprising 60-94% thermoplastic polyurethane, 5-30% styrene polymer, and 1-10% impact modifier is used to create bead foams, optimized with specific ratios and processing methods to enhance adhesive bonding and reduce density.
The solution results in bead foams with improved mechanical properties, reduced density, and efficient manufacturing, suitable for applications requiring minimal material usage and effective cushioning, such as shoe midsoles and inserts.
Smart Images

Figure 0007582936000001 
Figure 0007582936000002 
Figure 0007582936000003
Abstract
Description
[Background technology]
[0001] Bead foams (or foam beads) based on thermoplastic polyurethanes or other elastomers, and moldings produced therefrom, are known (e.g. DE 4126499, WO 94 / 20568, WO 2007 / 082838 A1, WO 2017030835, WO 2013 / 153190 A1, WO 2010010010) and can be used in many applications.
[0002] For the purposes of the present invention, the term "bead foam" or "foam beads" refers to foam in bead form, the foam beads having an average diameter of 0.5 to 30 mm, preferably 1 to 15 mm, and in particular 3 to 12 mm. In the case of non-spherical, e.g. elongated or cylindrical, foam beads, the diameter refers to the longest dimension.
[0003] In principle, there is a need for bead foams with improved processability and advantageous mechanical properties in order to obtain the corresponding moldings at the lowest possible temperatures. This is particularly relevant for the currently widely used melting processes, in which the energy for melting the bead foam is introduced via an auxiliary medium such as steam, since here better adhesive bonds are achieved and at the same time damage to the material or foam structure is reduced.
[0004] Proper adhesive bonding or melting of the foam beads is essential to obtain favorable mechanical properties of the molded article produced therefrom. If the foam beads are not adhesively bonded or melted sufficiently, the properties of the foam beads cannot be fully utilized, and the overall mechanical properties of the resulting molded article are adversely affected. Similar considerations apply if the molded article has weak spots. In such cases, the mechanical properties will be disadvantageous at the weak spots, with the same results as above.
[0005] The expression "advantageous mechanical properties" is to be interpreted in relation to the intended application. The most important applications for the subject matter of the present invention are those in the footwear field, where the bead foams can be used for shoe components where damping and / or cushioning are relevant, such as moldings for midsoles and inserts.
[0006] For the above-mentioned applications in the field of footwear or sports shoes, it is necessary not only to obtain advantageous tensile and bending properties of the moldings made from bead foams, but also to have the ability to produce moldings with advantageous resilience and compression properties for the specific application and with a minimum density. Here, there is a relationship between density and compression properties, since the compression properties are a measure of the minimum achievable density in a molding to comply with the requirements of the application. Moldings made from bead foams with a low level of compression properties will in principle require a higher density. Thus, more material will be required to produce similar final properties than moldings made from bead foams with a high level of compression properties. This relationship determines the usefulness of the bead foams for the specific application. In this context, bead foams that are particularly advantageous for applications in the field of footwear are those in which the compression properties of the moldings made from the bead foams are at a fairly low level to be exposed to small forces, while at the same time showing sufficient deformation for the wearer in the use area of the shoe.
[0007] Another problem is that in large-scale industrial production of bead foams by extrusion, it is desirable to maximize the throughput of material in order to produce the required quantities in the shortest possible time. However, rapid processing of the material here leads to a deterioration in the quality of the material, ranging from instability and / or collapse of the resulting bead foam. Thus, there remains a need to provide bead foams with minimal production time. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] DE4126499 [Patent Document 2] WO94 / 20568 [Patent Document 3] WO2007 / 082838A1 [Patent Document 4] WO2017030835 [Patent Document 5] WO2013 / 153190A1 [Patent Document 6] WO2010010010 Summary of the Invention [Problem to be solved by the invention]
[0009] It is therefore an object of the present invention to provide a bead foam suitable for the stated purposes. [Means for solving the problem]
[0010] The purpose of this is to a) 60 to 94% by weight of a thermoplastic polyurethane as component I, b) 5 to 30% by weight of a styrene polymer as component II, c) 1 to 10% by weight of an impact modifier as component III and the total of components I, II and III is 100% by mass; This was achieved by the bead foam made from composition (Z). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The thermoplastic polyurethanes used as component I are well known. They are prepared by reacting (a) isocyanates with (b) isocyanate-reactive compounds, for example polyols (b1) having a number-average molar mass of 500 g / mol to 100 000 g / mol, and optionally chain extenders (b2) having a molar mass of 50 g / mol to 499 g / mol, optionally in the presence of (c) catalysts and / or (d) conventional auxiliaries and / or additional substances.
[0012] For the purposes of the present invention, preference is given to thermoplastic polyurethanes which are obtainable by reaction of (a) isocyanates with (b) isocyanate-reactive compounds, such as polyols (b1) having a number-average molar mass of 500 g / mol to 100 000 g / mol and chain extenders (b2) having a molar mass of 50 g / mol to 499 g / mol, optionally in the presence of (c) catalysts and / or (d) conventional auxiliaries and / or additional substances.
[0013] The components (a) isocyanates, (b) isocyanate-reactive compounds, such as polyols (b1), and optionally chain extenders (b2), individually or together, are also defined as structural components, which together with catalysts and / or customary auxiliaries and / or additional substances are also defined as starting materials.
[0014] The molar ratio of the amount of structural component (b) used can be changed to adjust the hardness and melt index of the thermoplastic polyurethane. The hardness and melt viscosity increase with increasing content of chain extender in component (b) at a constant molecular weight of TPU, but the melt index decreases.
[0015] For the preparation of thermoplastic polyurethanes, structural components (a) and (b) (in a preferred embodiment (b) also comprises a chain extender) are reacted in the presence of catalyst (c) and optionally auxiliaries and / or additional substances in amounts such that the equivalent ratio of the NCO groups of diisocyanate (a) to the total hydroxy groups of component b) is in the range from 1:0.8 to 1:1.3.
[0016] Another variable that describes this ratio is the index. The index is defined by the ratio of all isocyanate groups used in the reaction to the isocyanate-reactive groups, i.e., the reactive groups of the polyol components and the chain extenders in particular. When the index is 1000, there is one active hydrogen atom for each isocyanate group. When the index is greater than 1000, there are more isocyanate groups than isocyanate-reactive groups.
[0017] Here, an equivalence ratio of 1:0.8 corresponds to an index of 1250 (index 1000=1:1), and a ratio of 1:1.3 corresponds to an index of 770.
[0018] In a preferred embodiment, the index in the reaction of the above components is in the range of 965-1110, preferably in the range of 970-1110, particularly preferably in the range of 980-1030 and very particularly preferably in the range of 985-1010.
[0019] In the present invention, the mass average molar mass (M w Particularly preferred is the production of thermoplastic polyurethanes having a mass average molar mass of at least 60000 g / mol, preferably at least 80000 g / mol, and particularly preferably greater than 100000 g / mol. The upper limit of the mass average molar mass of the thermoplastic polyurethane is very generally determined by the processability and by the desired property profile. The number average molar mass of the thermoplastic polyurethane is preferably 80000 to 300000 g / mol. The above average molar masses for the thermoplastic polyurethanes and for the structural components (a) and (b) are weight averages determined by gel permeation chromatography (for example according to DIN 55672-1, March 2016, or a similar method).
[0020] The organic isocyanates (a) which can be used are aliphatic, cycloaliphatic, araliphatic and / or aromatic isocyanates.
[0021] The aliphatic diisocyanates used are customary aliphatic and / or cycloaliphatic diisocyanates, such as, for example, tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethyltetramethylene 1,4-diisocyanate, hexamethylene 1,6-diisocyanate (HDI), pentamethylene 1,5-diisocyanate, butylene 1,4-diisocyanate, trimethylhexamethylene 1,6- Diisocyanates, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), cyclohexane 1,4-diisocyanate, 1-methylcyclohexane 2,4- and / or 2,6-diisocyanate, methylenecyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI).
[0022] Suitable aromatic diisocyanates are in particular naphthylene 1,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), 3,3'-dimethyl-4,4'-diisocyanatobiphenyl (TODI), p-phenylene diisocyanate (PDI), diphenylethane 4,4'-diisocyanate (EDI), methylene diphenyl diisocyanate (MDI), where the term MDI means diphenylmethane 2,2', 2,4'- and / or 4,4'-diisocyanate, 3,3'-dimethyldiphenyl diisocyanate, 1,2-diphenylethane diisocyanate and / or phenylene diisocyanate, or H12MDI (methylene dicyclohexyl 4,4'-diisocyanate).
[0023] Mixtures can also be used in principle. An example of a mixture is a mixture that contains at least further methylene diphenyl diisocyanate alongside methylene diphenyl 4,4'-diisocyanate. Here, the term "methylene diphenyl diisocyanate" means diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate, or a mixture of two or three isomers. It is therefore possible to use, for example, diphenylmethane 2,2'- or 2,4'-diisocyanate, or a mixture of two or three isomers as further isocyanates. In this embodiment, the polyisocyanate composition can also contain other of the above-mentioned polyisocyanates.
[0024] Other examples of mixtures are: 4,4'-MDI and 2,4'-MDI, or 4,4'-MDI and 3,3'-dimethyl-4,4'-diisocyanatobiphenyl (TODI) or 4,4'-MDI and H12MDI (4,4'-methylenedicyclohexyl diisocyanate) or 4,4'-MDI and TDI; or 4,4'-MDI and 1,5-naphthylene diisocyanate (NDI) A polyisocyanate composition comprising:
[0025] In particular, three or more isocyanates may be used according to the invention. The polyisocyanate composition typically comprises 4,4'-MDI in an amount of 2 to 50%, based on the total polyisocyanate composition, and a further isocyanate in an amount of 3 to 20%, based on the total polyisocyanate composition.
[0026] Furthermore, crosslinking agents such as, for example, the aforementioned highly functional polyisocyanates or polyols or other highly functional molecules having several isocyanate-reactive functional groups can also be used. Within the scope of the present invention, it is also possible to crosslink the product by using an excess of isocyanate groups in relation to the hydroxyl groups. Examples of highly functional isocyanates are triisocyanates, for example triphenylmethane 4,4',4"-triisocyanate, and isocyanurates and cyanurates of the aforementioned diisocyanates, and oligomers obtainable by partial reaction of diisocyanates with water, for example biurets of the aforementioned diisocyanates, and oligomers obtainable by controlled reaction of semiblocked diisocyanates with polyols having, on average, more than two, preferably three or more hydroxyl groups.
[0027] Here, the amount of the crosslinking agent, i.e., the high-functional isocyanate (a) and the high-functional polyol (b), should not exceed 3% by weight, preferably 1% by weight, based on the entire mixture of components (a) to (d).
[0028] The polyisocyanate composition may include one or more solvents. Suitable solvents are known to those skilled in the art. Suitable examples are non-reactive solvents such as ethyl acetate, methyl ethyl ketone, and hydrocarbons.
[0029] The isocyanate-reactive compound (b1) preferably has a molar mass of 500 g / mol to 8000 g / mol, more preferably 500 g / mol to 5000 g / mol, in particular 500 g / mol to 3000 g / mol. The molar mass is in particular in the range of 500 g / mol to 8000 g / mol.
[0030] The statistical average number of hydrogen atoms exhibiting Zerewitinoff activity in the isocyanate-reactive compound (b) is at least 1.8, at most 2.2, preferably 2; this number is also defined as the functionality of the isocyanate-reactive compound (b) and represents the amount of isocyanate-reactive groups in the molecule theoretically calculated for one molecule on a molar basis.
[0031] The isocyanate-reactive compound is preferably substantially linear and is one isocyanate-reactive material or a mixture of various materials, and the mixture meets the described requirements.
[0032] The ratio of components (b1) and (b2) is varied to obtain the desired hard segment content, which can be calculated by the formula disclosed in PCT / EP2017 / 079049.
[0033] Suitable hard segment contents here are less than 60%, preferably less than 40%, particularly preferably less than 25%.
[0034] The isocyanate-reactive compound (b1) preferably has reactive groups selected from hydroxy, amino, mercapto and carboxylic acid groups, where hydroxy groups are preferred and where primary hydroxy groups are very particularly preferred. It is particularly preferred that the isocyanate-reactive compound (b) is selected from the group of polyesterols, polyetherols and polycarbonate diols, which are also encompassed by the term "polyol".
[0035] Suitable polymers in the present invention are homopolymers such as polyetherols, polyesterols, polycarbonate diols, polycarbonates, polysiloxane diols, polybutadiene diols, and block copolymers, and hybrid polyols such as poly(ester / amide).Preferred polyetherols in the present invention are polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polytetrahydrofuran (PTHF), polytrimethylene glycol.Preferred polyester polyols are polyadipates, polysuccinates, and polycaprolactones.
[0036] In another embodiment, the present invention provides the above thermoplastic polyurethane, wherein the polyol composition comprises a polyol selected from the group consisting of polyetherols, polyesterols, polycaprolactones, and polycarbonates.
[0037] Examples of suitable block copolymers are those with ether and ester blocks, such as polycaprolactone with polyethylene oxide or polypropylene oxide end blocks, and polyether with polycaprolactone end blocks. Preferred polyetherols in the present invention are polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polytetrahydrofuran (PTHF) and polytrimethylene glycol. Polycaprolactone is more preferred.
[0038] In a particularly preferred embodiment, the molar mass Mn of the polyol used is in the range from 500 g / mol to 4000 g / mol, preferably in the range from 500 g / mol to 3000 g / mol.
[0039] Therefore, another embodiment of the present invention provides the above thermoplastic polyurethane, wherein the molar mass Mn of at least one polyol contained in the polyol composition is in the range of 500 g / mol to 4000 g / mol.
[0040] In particular, it is also possible in the present invention to use mixtures of different polyols.
[0041] In one embodiment of the present invention, at least one polyol composition comprising at least polytetrahydrofuran is used for the preparation of thermoplastic polyurethanes. The polyol composition of the present invention can also comprise other polyols in addition to polytetrahydrofuran.
[0042] Suitable materials for the other polyol in the present invention are, for example, polyethers, and polyesters, block copolymers, and hybrid polyols, such as poly(ester / amide). Examples of suitable block copolymers are those with ether blocks and ester blocks, such as polycaprolactone with polyethylene oxide or polypropylene oxide end blocks, and polyether with polycaprolactone end blocks. Preferred polyetherols in the present invention are, in particular, polyethylene glycol and polypropylene glycol. As the other polyol, polycaprolactone is further preferred.
[0043] Examples of suitable polyols are polyetherols such as polytrimethylene oxide and polytetramethylene oxide.
[0044] Thus, another embodiment of the present invention provides a thermoplastic polyurethane as described above, wherein the polyol composition comprises at least one polytetrahydrofuran (PTHF) and at least one other polyol selected from the group consisting of another polytetramethylene oxide, polyethylene glycol, polypropylene glycol, and polycaprolactone.
[0045] In a particularly preferred embodiment, the number average molar mass Mn of polytetrahydrofuran is in the range from 500 g / mol to 5000 g / mol, more preferably in the range from 550 to 2500 g / mol, particularly preferably in the range from 650 to 2000 g / mol and very particularly preferably in the range from 650 to 1400 g / mol.
[0046] The composition of the polyol composition can vary widely for the purposes of the present invention. For example, the content of the first polyol, preferably polytetrahydrofuran, can be in the range of 15% to 85%, preferably in the range of 20% to 80%, more preferably in the range of 25% to 75%.
[0047] The polyol composition of the invention may also comprise, for example, a solvent. Suitable solvents are known per se to the person skilled in the art.
[0048] As long as polytetrahydrofuran is used, the number average molar mass Mn of polytetrahydrofuran is, for example, in the range of 500 g / mol to 5000 g / mol, preferably in the range of 500 g / mol to 3000 g / mol. It is more preferable that the number average molar mass Mn of polytetrahydrofuran is in the range of 500 to 1400 g / mol.
[0049] The number-average molar mass Mn here can be determined as described above by gel permeation chromatography.
[0050] Another embodiment of the present invention also provides the above thermoplastic polyurethane, wherein the polyol composition comprises a polyol selected from the group consisting of polytetrahydrofurans having a number average molar mass Mn ranging from 500 g / mol to 5000 g / mol.
[0051] In the context of the invention, it is also possible, for example, to use mixtures of different polytetrahydrofurans, ie mixtures of polytetrahydrofurans of different molar masses.
[0052] The chain extenders (b2) used are preferably aliphatic, araliphatic, aromatic and / or cycloaliphatic compounds with a molar mass of 50 g / mol to 499 g / mol, preferably having two isocyanate-reactive groups, also defined as functional groups. Preferred chain extenders are diamines and / or alkanediols, more preferably alkanediols with 2 to 10 carbon atoms, preferably 3 to 8 carbon atoms, in the alkylene part, more preferably having only primary hydroxy groups. In a preferred embodiment, chain extenders (b2) are used, which are preferably aliphatic, araliphatic, aromatic and / or cycloaliphatic compounds with a molar mass of 50 g / mol to 499 g / mol, preferably having two isocyanate-reactive groups, also defined as functional groups.
[0053] It is preferred that the chain extender is at least one selected from the group consisting of ethylene 1,2-glycol, propane-1,2-diol, propane-1,3-diol, butane-1,4-diol, butane-2,3-diol, pentane-1,5-diol, hexane-1,6-diol, diethylene glycol, dipropylene glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, neopentyl glycol, and hydroquinone bis(beta-)ether (HQEE). Particularly suitable chain extenders are those selected from the group consisting of 1,2-ethanediol, propane-1,3-diol, butane-1,4-diol and hexane-1,6-diol, and mixtures of the above chain extenders. Examples of specific chain extenders and mixtures are disclosed, inter alia, in PCT / EP2017 / 079049.
[0054] In a preferred embodiment, catalysts (c) are used together with the structural components. These are in particular catalysts which promote the reaction between the NCO groups of the isocyanate (a) and the hydroxy groups of the isocyanate-reactive compounds (b) and, if used, the chain extenders.
[0055] Further examples of suitable catalysts are organometallic compounds selected from the group consisting of organyl compounds of tin, organyl compounds of titanium, organyl compounds of zirconium, organyl compounds of hafnium, organyl compounds of bismuth, organyl compounds of zinc, organyl compounds of aluminum and organyl compounds of iron, such as organyl compounds of tin, preferably dialkyltin compounds, such as dimethyltin or diethyltin of aliphatic carboxylic acids, or tin-organyl compounds, preferably tin diacetate, tin dilaurate, dibutyltin diacetate, dibutyltin dilaurate, bismuth compounds, such as alkylbismuth compounds, or iron compounds, preferably iron(III) acetylacetonate, or metal salts of carboxylic acids, such as tin(II) isoctanoate, tin dioctanoate, titanium ester or bismuth(III) neodecanoate. Particularly preferred catalysts are tin dioctanoate, bismuth decanoate and titanium ester. The amount of catalyst (c) preferably used is 0.0001 to 0.1 parts by weight per 100 parts by weight of isocyanate-reactive compound (b). Other compounds which can be added to the structural components (a) to (b) alongside the catalyst (c) are conventional auxiliaries (d). Examples include surface-active substances, fillers, flame retardants, nucleating agents, oxidation stabilizers, lubricants and release agent auxiliaries, dyes and pigments, and optionally, preferably stabilizers with respect to hydrolysis, light, heat or discoloration, inorganic and / or organic fillers, reinforcing agents and / or plasticizers.
[0056] Suitable dyes and pigments are described below in a later section.
[0057] Stabilizers for the purposes of the present invention are additives that protect plastics or plastic mixtures from harmful environmental influences, such as primary and secondary antioxidants, sterically hindered phenols, hindered amine light stabilizers, UV absorbers, hydrolysis stabilizers, quenchers and flame retardants. Examples of commercially available stabilizers can be found in Plastics Additives Handbook, 5th edn., H. Zweifel, ed., Hanser Publishers, Munich, 2001 ([1]), pages 98 to 136.
[0058] Thermoplastic polyurethanes may be produced batchwise or continuously by known processes, for example using a reactive extruder or a belt process by the "one-shot" method, or by a prepolymer process, preferably by the "one-shot" method. In the "one-shot" method, the components (a), (b) to be reacted, and in a preferred embodiment also the chain extenders in components (b), (c) and / or (d), are mixed with each other, either continuously or simultaneously, and the polymerization reaction is immediately initiated. The TPU can then be pelletized directly or converted into lenticular pellets by extrusion. In this process, it is possible to achieve the simultaneous incorporation of other adjuvants or other polymers.
[0059] In the extruder process, structural components (a), (b), and in a preferred embodiment also (c) and / or (d), are introduced individually or in the form of a mixture into an extruder and reacted at a temperature preferably between 100° C. and 280° C., preferably between 140° C. and 250° C. The resulting polyurethane is extruded, cooled and pelletized or directly pelletized by an underwater pelletizer into the form of lenticular pellets.
[0060] In a preferred process, the thermoplastic polyurethane is produced in a first step from the structural components isocyanate (a), isocyanate-reactive compounds including chain extenders (b), and in a preferred embodiment other raw materials (c) and / or (d), and additional substances or auxiliaries are incorporated in a second extrusion step.
[0061] The use of a twin screw extruder is preferred because it operates in a force conveying mode, allowing for more precise regulation of the temperature in the extruder and quantitative output. The production and expansion of the TPU can also be achieved in a single step in a reactive extruder or using a tandem extruder, as known to those skilled in the art.
[0062] The styrene polymers mentioned as component II are standard polystyrenes, where the expression "standard polystyrene" preferably includes atactic, syndiotactic or isotactic polystyrene, particularly preferably atactic polystyrene.
[0063] The glass transition temperature of the inventive atactic polystyrene, which is amorphous, is in the range of 100° C.±20° C. (DIN EN ISO11357-1, February 2017 / DIN EN ISO11357-2, July 2014, determined by the inflection point method). The inventive syndiotactic and isotactic polystyrenes, respectively, are semi-crystalline and have melting points in the region of 270° C. and 240° C., respectively (DIN EN ISO11357-1; February 2017 / DIN EN ISO11357-3, April 2013, W-peak melting temperature).
[0064] The polystyrenes used have a tensile modulus of greater than 2500 (DIN EN ISO 527-1 / 2, June 2012). The modulus of elasticity of the polystyrenes used (styrene polymers as component II) is preferably in the range from 2500 MPa to 4000 MPa, more preferably in the range from 2800 MPa to 3700 MPa, particularly preferably in the range from 3000 MPa to 3500 MPa and very particularly preferably 3317 MPa.
[0065] The preparation and processing of the polystyrene of the present invention has been widely described in the literature, for example in Becker / Braun (1996), Kunststoff-Handbuch Band 4, "Polystyrol" [Plastics Handbook, Vol. 4, "Polystyrene"].
[0066] It is also possible to use commercially available materials such as PS158K (BASF SE), PS148H Q (BASF SE), STYROLUTION PS156F, STYROLUTION PS158N / L, STYROLUTION PS168N / L, STYROLUTION PS153F, SABIC PS125, SABIC PS155, and SABIC PS160.
[0067] The impact modifiers that can be used as component III are characterized by accumulating in the styrene polymer phase or at the interface between the thermoplastic polyurethane phase and the styrene polymer phase. The impact modifiers as component III preferably accumulate in the styrene polymer phase.
[0068] A preferred impact modifier is a styrene block copolymer based on a styrene monomer and at least one other monomer. A particularly preferred impact modifier based on a styrene block copolymer is selected from the group of styrene-based thermoplastic elastomers and high impact polystyrene (HIPS). HIPS is a term used specifically for high impact polystyrene. HIPS is particularly impact resistant.
[0069] HIPS preferably includes SEBS, SBS, SEPS, SEPS-V, and acrylonitrile-butadiene-styrene copolymer (ABS). SEBS is the term used specifically for styrene-ethylene-butylene-styrene block copolymers. SBS is the term used specifically for styrene-butadiene-styrene block copolymers. SEPS is the term used specifically for styrene-ethylene-propylene-styrene block copolymers. SIBS is the term used specifically for styrene-isoprene-butadiene-styrene block copolymers. SEPS-V is the term used specifically for styrene-ethylene-propylene-styrene block copolymers that have been converted from thermoplastic to elastomeric by vulcanization.
[0070] It is particularly preferred to use high impact polystyrene (HIPS) as the impact modifier of component III.SEBS, SBS, SEPS are particularly preferred HIPS for component III.
[0071] For the purposes of the present invention, high impact polystyrene (HIPS) specifically does not contain maleic acid as a polymer component. It is preferred that neither the polymer of component II nor the polymer of component III contain any maleic acid as a monomer.
[0072] The composition of the invention in particular comprises two different styrene polymers as component II and component III. Component II is in particular atactic, syndiotactic or isotactic polystyrene. Component III is in particular high impact polystyrene (HIPS, high impact polystyrene) as impact modifier selected from the group consisting of SEBS, SBS, SEPS, SEPS-V, SIBS and acrylonitrile-butadiene-styrene copolymer (ABS). Component II and component III in particular do not comprise polymers derived from maleic acid monomers.
[0073] The tensile modulus of the high impact polystyrene (HIPS) used is less than 2700 MPa (DIN EN ISO 527-1 / 2, June 2012). The modulus of the high impact polystyrene (HIPS, impact modifier as component III) used is preferably in the range of 1000 MPa to 2700 MPa, more preferably in the range of 1500 MPa to 2000 MPa, even more preferably in the range of 1600 MPa to 1700 MPa and very particularly preferably 1650 MPa.
[0074] The production and processing of styrene polymers has been widely described in the literature, for example in Becker / Braun (1996), Kunststoff-Handbuch Band 4, "Polystyrol" [Plastics Handbook, Vol. 4, "Polystyrene"].
[0075] Commercially available materials can be used here, such as, for example, Styron A-TECH1175, Styron A-TECH1200, Styron A-TECH1210, Styrolution PS495S, Styrolution PS485N, Styrolution PS486N, Styrolution PS542N, Styrolution PS454N, Styrolution PS416N, Roechling PS HI, SABIC PS325, SABIC PS330.
[0076] As mentioned above, composition Z is in particular 60 to 94% by weight of a thermoplastic polyurethane as component I, 5 to 30% by weight of a styrene polymer as component II, 1 to 10% by weight of an impact modifier as defined above as component III The total of Components I, II and III amounts to 100 mass %.
[0077] Composition Z preferably comprises 72 to 86% by weight of a thermoplastic polyurethane as component I, 10 to 20% by weight of a styrene polymer as component II, 4 to 8 weight percent of an impact modifier as defined above as component III The total of Components I, II and III amounts to 100 mass %.
[0078] Composition Z is more preferably 72 to 94% by weight of a thermoplastic polyurethane as component I, 5 to 20% by weight of a styrene polymer as component II, 1 to 8 weight percent of an impact modifier as defined above as component III The total of Components I, II and III amounts to 100 mass %.
[0079] Composition Z is more preferably 80 to 98% by weight of a thermoplastic polyurethane as component I, 1 to 10% by weight of a styrene polymer as component II, 1 to 10% by weight of an impact modifier as defined above as component III The total of Components I, II and III amounts to 100 mass %.
[0080] For the purposes of the present invention, composition (Z) may, for example, comprise 1 to 10% by weight of a styrene polymer as component II, preferably 2.5 to 7.5% by weight of a styrene polymer as component II, or more preferably 5% by weight of a styrene polymer as component II.
[0081] For the purposes of the present invention, composition (Z) may, for example, comprise 1 to 10% by weight of an impact modifier as component III, preferably 2.5 to 7.5% by weight of an impact modifier as component III, or more preferably 4% by weight of an impact modifier as component III.
[0082] For the purposes of the present invention, composition (Z) may, for example, comprise 80-95% by weight of a thermoplastic polyurethane as component I, 2.5-10% by weight of a styrene polymer as component II, and 2.5-10% by weight of an impact modifier as component III, preferably 85-92.5% by weight of a thermoplastic polyurethane as component I, 3.75-7.5% by weight of a styrene polymer as component II, and 3.75-7.5% by weight of an impact modifier as component III, more preferably 87.5-95% by weight of a thermoplastic polyurethane as component I, 2.5-6.25% by weight of a styrene polymer as component II, and 2.5-6.5% by weight of an impact modifier as component III, the total of components I, II and III always adding up to 100% by weight.
[0083] For the purposes of the present invention, composition (Z) more preferably comprises, for example, 91% by weight of a thermoplastic polyurethane as component I, 5% by weight of a styrene polymer as component II, and 4% by weight of an impact modifier as component III, the total of components I, II and III always adding up to 100% by weight.
[0084] The bead foam is preferably a) 60 to 94% by weight of a thermoplastic polyurethane as component I, b) 5 to 30% by weight of a styrene polymer as component II, c) 1 to 10% by weight of an impact modifier as component III The composition (Z) is made from The total of components I, II and III equals 100% by weight.
[0085] The bead foam is more preferably a) 72 to 94% by weight of a thermoplastic polyurethane as component I, b) 5 to 20% by weight of a styrene polymer as component II, c) 1 to 8% by weight of an impact modifier as component III The composition (Z) is made from The total of components I, II and III equals 100% by weight.
[0086] The bead foam is more preferably a) 80 to 98% by weight of a thermoplastic polyurethane as component I, b) 1 to 10% by weight of a styrene polymer as component II, c) 1 to 10% by weight of an impact modifier as component III The composition (Z) is made from The total of components I, II and III equals 100% by weight.
[0087] The bead foam is more preferably a) 80 to 91% by weight of a thermoplastic polyurethane as component I, b) 5 to 10% by weight of a styrene polymer as component II, c) 4 to 10% by weight of an impact modifier as component III The composition (Z) is made from The total of components I, II and III equals 100% by weight.
[0088] The unexpanded polymer mixture of composition Z required for the production of the bead foam is prepared in a known manner from the individual components and, optionally, other components, such as processing aids, stabilizers, compatibilizers or pigments. Examples of suitable processes are conventional mixing processes using kneaders, in continuous or batch mode, or using extruders, such as co-rotating twin-screw extruders.
[0089] If compatibilizers or auxiliaries are used, such as stabilizers, they can also be incorporated into the components before the end of the production of the components. The individual components are usually combined or metered into the mixing equipment before the mixing process. If an extruder is used, all of the components are metered into the inlet and conveyed together into the extruder, or the individual components are added by an auxiliary feeding system.
[0090] The processing is carried out at a temperature at which the components are in a plasticized state. The temperature depends on the softening or melting range of the components, but must be below the decomposition temperature of each component. Additives, such as pigments or fillers, or other conventional auxiliaries as mentioned above (d), are incorporated in the solid state, not in the molten state.
[0091] There are other possible embodiments using widely used methods, where the processes used to produce the starting materials can be directly integrated into the manufacturing procedure. For example, when using a belt process, the styrene polymer, the impact modifier, and also the fillers or dyes could be introduced directly into the end of the belt where the material is fed into the extruder to obtain lenticular pellets.
[0092] Some of the conventional auxiliaries (d) mentioned above can be added to the mixture at this stage.
[0093] The bulk density of the bead foam according to the invention is generally 50 g / l to 200 g / l, preferably 60 g / l to 180 g / l, particularly preferably 80 g / l to 150 g / l. The bulk density of the bead foam is more preferably in the range of 100 g / l to 180 g / l, preferably in the range of 130 g / l to 150 g / l. The bulk density is measured by a method based on DIN ISO 697, but the determination of said value differs from the standard in that a container with a volume of 10 l is used instead of a container with a volume of 0.5 l, because the measurement using a volume of only 0.5 l is too inaccurate especially for foam beads with low density and high mass.
[0094] As mentioned above, the diameter of the foam beads is between 0.5 and 30 mm, preferably between 1 and 15 mm, and in particular between 3 and 12 mm. In the case of non-spherical, e.g. elongated or cylindrical, foam beads, the diameter refers to the longest dimension.
[0095] The diameter of the foam beads is in particular in the range from 0.5 to 30 mm, preferably in the range from 1 to 15 mm and particularly preferably in the range from 3 to 12 mm. In the case of non-spherical, e.g. elongated or cylindrical, foam beads, the diameter means the longest dimension.
[0096] The bead foam can be produced by known processes widely used in the prior art. i. providing a composition (Z) of the present invention; ii. impregnating the composition with a blowing agent under pressure; iii. Expanding the composition by reducing the pressure. It can be produced via:
[0097] The amount of the foaming agent is preferably 0.1 to 40 parts by mass, particularly preferably 0.5 to 35 parts by mass, and particularly preferably 1 to 30 parts by mass, based on 100 parts by mass of the composition (Z) used.
[0098] One embodiment of the above process comprises: i. providing a composition (Z) of the present invention in pellet form; ii. impregnating the pellets with a blowing agent under pressure; iii. Expanding the pellets by reducing the pressure Includes.
[0099] Another embodiment of the above process comprises the additional steps: i. providing a composition (Z) of the present invention in pellet form; ii. impregnating the pellets with a blowing agent under pressure; iii. Reducing the pressure to atmospheric pressure, optionally by prior reduction of the temperature, without expanding the pellets; iv. A step of expanding the pellets by increasing the temperature. Includes.
[0100] It is preferred that the unexpanded pellets have an average minimum diameter of 0.2-10 mm (as determined by 3D evaluation of the pellets, for example by dynamic image analysis using Microtrac's PartAn3D optical measurement instrument).
[0101] The average mass of the individual pellets is generally in the range of 0.1 to 50 mg, preferably in the range of 4 to 40 mg, and particularly preferably in the range of 7 to 32 mg. This average mass of the pellets (particle mass) is determined as the arithmetic mean via three weighing procedures using 10 pellets each.
[0102] One embodiment of the above process includes the steps of impregnating the pellets with a blowing agent under pressure followed by expanding the pellets in steps (ii) and (iii): ii. impregnating the pellets in the presence of a blowing agent in a suitable closed reaction vessel (e.g. an autoclave) at elevated temperature and pressure; iii. Sudden pressure reduction without cooling.
[0103] The impregnation in step (ii) here can be carried out in the presence of water and optionally a suspending aid, or in the presence of only a blowing agent and in the absence of water.
[0104] Examples of suitable suspending aids are water-insoluble inorganic stabilizers such as tricalcium phosphate, magnesium pyrophosphate, metal carbonates, and polyvinyl alcohol, and surfactants such as sodium dodecylarylsulfonate, the usual amounts of which are 0.05 to 10% by weight based on the composition of the present invention.
[0105] The impregnation temperature depends on the selected pressure and is in the range of 100-200° C., the pressure in the reaction vessel is in particular in the range of 2-150 bar, preferably in the range of 5-100 bar, particularly preferably in the range of 20-60 bar, and the impregnation time is generally in the range of 0.5-10 hours. The pressure in the reaction vessel is in particular in the range of 2-150 bar, preferably in the range of 5-100 bar, particularly preferably in the range of 20-60 bar.
[0106] The performance of processes in suspension is known to the person skilled in the art and is extensively described, for example, in WO2007 / 082838.
[0107] When the process is carried out in the absence of a blowing agent, care must be taken to avoid agglomeration of the polymer pellets.
[0108] Suitable blowing agents for carrying out the process in a suitable closed reaction vessel are, for example, organic liquids and organic gases, such as hydrocarbons, which are in the gaseous state under the treatment conditions, or inorganic gases, or mixtures of organic liquids or organic gases, respectively, with inorganic gases, which can likewise be combined.
[0109] Examples of suitable hydrocarbons are halogenated or non-halogenated, saturated or unsaturated aliphatic hydrocarbons, preferably non-halogenated, saturated or unsaturated aliphatic hydrocarbons.
[0110] Preferred organic blowing agents are saturated aliphatic hydrocarbons, especially those having 3 to 8 C atoms, such as butane or pentane.
[0111] Suitable inorganic gases are nitrogen, air, ammonia or carbon dioxide, preferably nitrogen or carbon dioxide, or a mixture of the abovementioned gases.
[0112] In another embodiment, the step of impregnating the pellets in a blowing agent under pressure comprises a process followed by expanding the pellets in steps (ii) and (iii): ii. impregnating the pellets in an extruder under pressure and at elevated temperature in the presence of a blowing agent; iii. Pelletizing the melt exiting the extruder under conditions which prevent uncontrolled foaming.
[0113] Suitable blowing agents in this version of the process are volatile organic compounds with a boiling point of −25 to 150° C., in particular −10 to 125° C., at atmospheric pressure of 1013 mbar. Good compatible materials are hydrocarbons (preferably halogen-free), in particular C4-10-alkanes, such as the isomers of butane, isomers of pentane, isomers of hexane, isomers of heptane and isomers of octane, particularly preferably isopentane. Other possible blowing agents are further bulkier compounds, such as alcohols, ketones, esters, ethers and organic carbonates.
[0114] Here, in step (ii), the composition is mixed in an extruder while melted under pressure with a blowing agent introduced in the extruder. The mixture including the blowing agent is extruded under pressure, preferably using a controlled back pressure at a moderate level, and pelletized (e.g., pelletized under water). Here, the molten strands are expanded, and foam beads are obtained by pelletization.
[0115] The performance of the process via extrusion is known to the person skilled in the art and is extensively described, for example, in WO2007 / 082838, and WO2013 / 153190A1.
[0116] Extruders which can be used are any conventional screw-based machines, in particular single- and twin-screw extruders (e.g. ZSK from Werner & Pfleiderer), co-kneaders, Kombiplast machines, MPC kneading mixers, FCM mixers, KEX kneading screw extruders and shear roll extruders of the type described, for example, in Saechtling (ed.), Kunststoff-Taschenbuch [Plastics Handbook], 27th edn., Hanser-Verlag, Munich 1998, chapters 3.2.1 and 3.2.4. The extruder is usually operated at a temperature at which the composition (Z) is in the form of a melt, for example 120°C to 250°C, in particular 150 to 210°C, and at a pressure of 40 to 200 bar, preferably 60 to 150 bar, particularly preferably 80 to 120 bar, after addition of the blowing agent to ensure homogenization of the blowing agent with the melt.
[0117] The process here can be carried out in one extruder or in an arrangement of one or more extruders. Thus, for example, in the first extruder, it is possible to melt and blend the components together with the injection of the blowing agent. In the second extruder, the impregnated melt is homogenized and the temperature and / or pressure is adjusted. It is also possible that the mixing of the components and the injection of the blowing agent are split across two different process components, for example, when three extruders are combined with each other. As is preferred, when only one extruder is used, all process steps of melting, mixing, injection of the blowing agent, homogenization, temperature and / or pressure adjustment are carried out in a single extruder.
[0118] Alternatively, in the method described in WO2014150122 or WO2014150124A1, the corresponding bead foam (optionally already colored in practice) can be produced directly from the corresponding pellets in that the pellets are saturated with a supercritical liquid and removed from the supercritical liquid, which includes: (i) immersing the product in a heated fluid; (ii) irradiating the product with high energy radiation (e.g., infrared radiation or microwave radiation). continues.
[0119] Examples of suitable supercritical liquids are those described in WO2014150122, such as carbon dioxide, nitrogen dioxide, ethane, ethylene, oxygen or nitrogen, preferably carbon dioxide or nitrogen.
[0120] Here, the supercritical liquid may include a polar liquid having a Hildebrand solubility parameter of 9 MPa1 / 2 or more.
[0121] Here, it is also possible that the supercritical liquid or the heated liquid contains a colorant, so that a colored foamed product is obtained.
[0122] The present invention further provides a molded article produced from the bead foam of the present invention.
[0123] The corresponding shaped bodies can be produced by methods known to those skilled in the art.
[0124] A preferred process for producing foamed moulded articles herein comprises the following steps: (i) introducing foam beads into a suitable mold; (ii) melting the foam beads from step (i).
[0125] The melting in step (ii) is preferably carried out in a closed mould where melting can be achieved via steam, hot air (e.g. as described in EP1979401B1), or high energy radiation (microwave or radio wave).
[0126] The temperature during melting of the bead foam is preferably below or close to the melting point of the polymer from which the bead foam is produced. For the widely used polymers, the temperature for melting of the bead foam is correspondingly between 100° C. and 180° C., preferably between 120° C. and 150° C. The temperature for melting of the bead foam is in particular in the range between 100° C. and 180° C., preferably between 120° C. and 150° C.
[0127] Here, the temperature profile / residence time can be determined individually based on the processes described, for example, in US20150337102 or EP2872309B1.
[0128] Melting by high energy radiation is generally carried out in the microwave or radio wave frequency range, optionally in the presence of water or other polar liquids, such as microwave absorbing hydrocarbons bearing polar groups (examples are esters of carboxylic acids, esters of diols or triols, other examples are glycols and liquid polyethylene glycols), and can be achieved by methods based on the processes described in EP3053732A or WO16146537.
[0129] For fusion by high-frequency electromagnetic radiation, the bead foam is preferably wetted with a polar liquid suitable for absorbing radiation, for example in a proportion of 0.1 to 10% by weight, preferably 1 to 6% by weight, based on the bead foam used. For the purposes of the present invention, fusion of the bead foam can also be carried out by the use of high-frequency electromagnetic radiation, without the use of a polar liquid. The thermal bonding of the foam beads is carried out in a mould, for example by means of high-frequency electromagnetic radiation, in particular microwaves. Electromagnetic radiation described as high-frequency has a frequency of at least 20 MHz, for example at least 100 MHz. In general, electromagnetic radiation in the frequency range of 20 MHz to 300 GHz, for example 100 MHz to 300 GHz, is used. It is preferred to use microwaves with frequencies in the range of 0.5 to 100 GHz, in particular in the range of 0.8 to 10 GHz, and irradiation times of 0.1 to 15 minutes. It is preferred to match the frequency range of the microwaves to the absorption behaviour of the polar liquid, or, working inversely, to select a polar liquid based on its absorption behaviour suitable for the frequency range of the microwave device used. Suitable methods are described, for example, in WO2016 / 146537A1.
[0130] As noted above, the bead foam may also include colorants, which may be added in a variety of ways.
[0131] In one embodiment, the produced bead foam can be colored after production. In this case, the corresponding bead foam is contacted with a carrier liquid containing a colorant. The polarity of the carrier liquid (CL) is suitable for the carrier liquid to achieve sorption on the bead foam. This method can be based on the method described in the EP application with application number 17198591.4.
[0132] Examples of suitable colorants are inorganic or organic pigments. Examples of suitable natural or synthetic inorganic pigments are carbon black, graphite, titanium oxide, iron oxide, zirconium oxide, cobalt oxide compounds, chromium oxide compounds, copper oxide compounds. Examples of suitable organic pigments are azo pigments and polycyclic pigments.
[0133] In another embodiment, the colorant can be added during the production of the bead foam. For example, the colorant can be added to the extruder during the production of the bead foam by extrusion. Alternatively, an already colored material can be used as starting material for the production of the bead foam, which is extruded or expanded in a closed container by the above process. Furthermore, in the process described in WO2014150122, it is possible for the supercritical liquid or the heated liquid to contain the colorant.
[0134] As mentioned above, the moulded articles according to the invention have advantageous properties for the above mentioned applications in the field of shoes or sports shoes.
[0135] The tensile and compressive properties of the mouldings produced from the bead foam are characterised by a tensile strength of more than 600 kPa (DIN EN ISO 1798, April 2008), an elongation at break of more than 100% (DIN EN ISO 1798, April 2008) and a compressive stress at 10% compression of more than 15 kPa (based on DIN EN ISO 844, November 2014; deviations from the standard consist of a sample height of 20 mm instead of 50 mm and the resulting test speed being adjusted to 2 mm / min).
[0136] The resilience of mouldings made from bead foam is greater than 55% (according to a method based on DIN 53512, April 2000; the deviation from the standard is the height of the specimen, which should be 12 mm, but in this test is taken to be 20 mm in order to avoid energy transmission beyond the specimen and measurement of the substrate).
[0137] As mentioned above, there is a relationship between the density and the compression properties of the resulting compact. The density of the compact produced is advantageously between 75 and 375 kg / m 3 , preferably 100 to 300 kg / m 3 , particularly preferably 150 to 200 kg / m 3(DIN EN ISO 845, October 2009). The density of the produced moldings is in particular 75 to 375 kg / m 3 in the range of 100 to 300 kg / m 3 In particular, 150 to 200 kg / m 3 (DIN EN ISO845, October 2009). The density of the molded body is more preferably 100 to 180 kg / m 3 and more preferably in the range of 130 to 150 kg / m 3 The range is.
[0138] Here, the ratio of the density of the molded article to the bulk density of the bead foam of the present invention is generally 1.5 to 2.5, preferably 1.8 to 2.0, and more preferably 1.8 to 2.0. The ratio is particularly in the range of 1.5 and 2.5.
[0139] The invention further provides the use of the bead foams according to the invention for the production of moldings for shoe midsoles, shoe insoles, shoe combisoles, bicycle saddles, bicycle tyres, damping elements, cushioning, mattresses, underlays, grips, protective films, components in the automotive interior or exterior sectors, in balls and sports equipment or as floor coverings, in particular for sports surfaces, running tracks, sports halls, children's play areas and walkways.
[0140] The bead foams according to the invention are preferably used for the production of moldings for shoe midsoles, shoe insoles, shoe combisoles or cushioning elements for shoes, where the shoes are preferably outdoor shoes, sports shoes, sandals, boots or safety shoes, particularly preferably sports shoes.
[0141] The invention therefore further provides a moulding, which is a combi-sole for a shoe, preferably for an outdoor shoe, a sports shoe, a sandal, a boot or a safety shoe, particularly preferably for a sports shoe.
[0142] The invention therefore further provides a molding, which is a midsole for a shoe, preferably for an outdoor shoe, a sports shoe, a sandal, a boot or a safety shoe, particularly preferably for a sports shoe.
[0143] The invention therefore further provides a moulding, which is an insert for a shoe, preferably for an outdoor shoe, a sports shoe, a sandal, a boot or a safety shoe, particularly preferably for a sports shoe.
[0144] The invention therefore further provides a molding, which is a cushioning element for a shoe, preferably for an outdoor shoe, a sports shoe, a sandal, a boot or a safety shoe, particularly preferably for a sports shoe.
[0145] Here, the cushioning element can be used, for example, in the heel area or in the forefoot area.
[0146] The invention therefore provides a shoe in which the inventive molding is used as a midsole, intermediate sole or cushioning, for example in the heel area or forefoot area, preferably an outdoor shoe, a sports shoe, a sandal, a boot or a safety shoe, particularly preferably a sports shoe.
[0147] The following are exemplary embodiments of the present invention, but are not intended to limit the present invention. In particular, the present invention also encompasses embodiments resulting from the dependencies described below and therefore combinations.
[0148] 1. a) 60 to 94% by weight of a thermoplastic polyurethane as component I; b) 5 to 30% by weight of a styrene polymer as component II, c) 1 to 10% by weight of an impact modifier as component III and the total of components I, II and III is 100% by mass; A bead foam made from composition (Z).
[0149] 2. a) 72 to 89% by weight of a thermoplastic polyurethane as component I; b) 10 to 20% by weight of a styrene polymer as component II, c) 1 to 8% by weight of an impact modifier as component III and the total of components I, II and III is 100% by mass; 2. The bead foam of embodiment 1.
[0150] 3. A bead foam according to any one of embodiments 1 and 2, wherein the styrene polymer is atactic polystyrene.
[0151] 4. A bead foam according to any one of embodiments 1 and 2, wherein the impact modifier is a styrene block copolymer.
[0152] 5. A bead foam according to any one of embodiments 1 and 2, wherein the impact modifier is a styrene-based thermoplastic elastomer.
[0153] 6. A bead foam according to any one of embodiments 1 and 2, wherein the impact modifier is impact resistant polystyrene.
[0154] 7. A bead foam according to any one of the preceding embodiments, wherein the average diameter of the foam beads is in the range of 0.5 to 20 mm, preferably 0.5 to 20 mm.
[0155] 8. A bead foam according to any one of the preceding embodiments, wherein the average diameter of the foam beads is in the range of 0.5 to 15 mm, preferably 0.5 to 15 mm.
[0156] 9. A method for producing a bead foam according to any one of the preceding claims, comprising: i. providing a composition (Z) of the present invention; ii. impregnating the composition with a blowing agent under pressure; iii. Expanding the composition by reducing the pressure. The method includes:
[0157] 10. A molded body made from the bead foam according to any one of the preceding claims.
[0158] 11. A molded body made from the bead foam of embodiment 10, wherein the molded body has a tensile strength of greater than 600 kPa. The tensile strength of the molded body is preferably at least 600 kPa.
[0159] 12. The molded body according to embodiment 10 or 11, having an elongation at break of more than 100%. The elongation at break is preferably at least 100%.
[0160] 13. The molded body according to any one of embodiments 10 to 12, having a compressive stress at 10% compression of more than 15 kPa. The compressive strength at 10% compression is preferably at least 15 kPa.
[0161] 14. Density of the compact is 75-375kg / m 3 Preferably, the density is 75 to 375 kg / m 3 14. The molded body according to any one of embodiments 10 to 13, wherein the average molecular weight of the molded body is in the range of 0.1 to 0.5.
[0162] 15. Density of the compact is 100-300kg / m 3 Preferably, it is 100 to 300 kg / m 3 14. The molded body according to any one of embodiments 10 to 13, wherein the average molecular weight of the molded body is in the range of 0.1 to 0.5.
[0163] 16. The density of the compact is 150-200kg / m 3 Preferably, it is 150 to 200 kg / m 3 14. The molded body according to any one of embodiments 10 to 13, wherein the average molecular weight of the molded body is in the range of 0.1 to 0.5.
[0164] 17. The molded body according to any one of embodiments 10 to 16, wherein the molded body has a rebound resilience of more than 55% (measured according to DIN 53512, April 2000). The rebound resilience of the molded body is preferably at least 55%.
[0165] 18. The molded body according to any one of embodiments 10 to 17, wherein the ratio of the density of the molded body to the bulk density of the bead foam is in the range of 1.5 to 2.5, preferably between 1.5 and 2.5.
[0166] 19. A molded body made from the bead foam according to any one of embodiments 10 to 17, wherein the ratio of the density of the molded body to the bulk density of the bead foam is in the range of 1.8 to 2.0, preferably 1.8 to 2.0.
[0167] 20. The molded article of any one of embodiments 10 to 19, wherein the molded article is a midsole of a shoe.
[0168] 21. The molded article of any one of embodiments 10 to 19, wherein the molded article is a shoe insert.
[0169] 22. The molded body according to any one of embodiments 10 to 19, wherein the molded body is a cushioning element for a shoe.
[0170] 23. The molded body according to any of embodiments 21 and 22, wherein the shoe is an outdoor shoe, a sports shoe, a sandal, a boot, or a safety shoe.
[0171] 24. A molded body according to any one of embodiments 21 and 22, wherein the shoe is a sports shoe.
[0172] 25. For producing the molded body according to any one of embodiments 10 to 24, (i) introducing foam beads into a suitable mold; (ii) melting the foam beads from step (i). The method includes:
[0173] 26. The method of embodiment 25, wherein the melting in step (ii) is accomplished in a closed mold.
[0174] 27. The method of embodiment 25 or 26, wherein the melting in step (ii) is achieved by steam, hot air or high-energy radiation.
[0175] 28. A shoe comprising a molding according to any one of embodiments 20 and 21.
[0176] 29. The shoe of embodiment 28, wherein the shoe is an outdoor shoe, a sports shoe, a sandal, a boot, or a safety shoe.
[0177] 30. The shoe of embodiment 28, wherein the shoe is a sports shoe.
[0178] 31. Use of the bead foam according to any one of the embodiments 1 to 8 for the production of a molding according to any one of the embodiments 10 to 19 for shoe midsoles, shoe insoles, shoe combisoles, shoe cushioning elements, bicycle saddles, bicycle tires, damping elements, cushioning, mattresses, underlays, grips, protective films, components in the automotive interior or automotive exterior sector, in balls and sports goods or as floor coverings.
[0179] 32. The use according to embodiment 31 for a shoe midsole, a shoe insole, a shoe combi-sole or a shoe cushioning element.
[0180] 33. The use of embodiment 31, wherein the shoe is a sports shoe.
[0181] The following examples serve to illustrate the invention but are not limiting in any way with respect to the subject matter. EXAMPLES
[0182] Expanded beads made of thermoplastic polyurethane and styrene polymer were produced using a twin-screw extruder with a screw diameter of 44 mm and a length-to-diameter ratio of 42, fitted with a melt pump, a diverter valve with a screen changer, a pelletizing die and an underwater pelletizing system. In accordance with processing guidelines, the thermoplastic polyurethane was dried at 80° C. for 3 hours before use to a residual moisture content of less than 0.02% by weight. To prevent moisture being introduced via the styrene polymer and the impact modifier, a similarly significant amount was dried at 80° C. for 3 hours to a residual moisture content of less than 0.05% by weight. Thermoplastic polyurethane in which diphenylmethane 4,4′-diisocyanate with an average functionality of 2.05 had been mixed in a separate extrusion process was added to each test specimen in addition to the above two components at 0.9% by weight based on the thermoplastic polyurethane used.
[0183] The thermoplastic polyurethane used was an ether-based TPU (Elastollan 1180A) from BASF, with a Shore hardness of 80A according to the datasheet. The styrene polymer used was PS158K Q from BASF, with a modulus of elasticity measured in a tensile test of 3317 MPa according to the datasheet. The impact modifier used was an impact-modified polystyrene (Styrolution PS485N) from Ineos, with a modulus of elasticity measured in a tensile test of 1650 MPa according to the datasheet.
[0184] The thermoplastic polyurethane, polystyrene, impact modified polystyrene, and the thermoplastic polyurethane that had been mixed with diphenylmethane 4,4'-diisocyanate were each separately metered into the inlet of a twin screw extruder by a mass metering device.
[0185] Table 1 shows the mass proportions of the thermoplastic polyurethane containing the thermoplastic polyurethane mixed with diphenylmethane 4,4'-diisocyanate and polystyrene.
[0186] [Table 1]
[0187] The materials were metered into the inlet of the twin screw extruder and then melted and mixed together. After mixing, a mixture of CO2 and N2 was added as blowing agents. During the remaining length of the extruder, the blowing agent and polymer melt were mixed together to form a homogenous mixture. The total throughput of the extruder was 80 kg / h, including TPU, polystyrene, and blowing agent, to which diphenylmethane 4,4'-diisocyanate with an average functionality of 2.05 had been added in a separate extrusion process.
[0188] The molten mixture was then forced into a pelletizing die (PD) through a diverter valve with a screen changer (DV) using a gear pump (GP), where the mixture was chopped into pellets in the cutting chamber of an underwater pelletizing system (UP) and conveyed with temperature-controlled pressurized water for expansion. A centrifugal dryer was used to ensure separation of the expanded beads from the process water.
[0189] The plant component temperatures used are listed in Table 2. Table 3 shows the amounts of blowing agents (CO2 and N2) used. The amounts were adjusted in each case to obtain the lowest possible bulk density. The blowing agent quantitative data is based on the total throughput of the polymer.
[0190] [Table 2]
[0191] [Table 3]
[0192] Table 4 lists the bulk density of the expanded pellets obtained from each experiment.
[0193] [Table 4]
Claims
1. a) 60 to 94% by weight of a thermoplastic polyurethane as component I, b) 5 to 30% by weight of a styrene polymer as component II, where the styrene polymer is atactic polystyrene; c) 1 to 10% by weight of an impact modifier as component III, wherein the impact modifier is a styrene block copolymer or a high impact polystyrene; wherein components II and III do not contain any structure derived from maleic acid or maleic anhydride, and the total of components I, II and III is 100 mass%; A bead foam made from composition (Z).
2. 2. The bead foam according to claim 1, wherein the foam beads have an average diameter of 0.5 to 20 mm.
3. i. Providing a composition (Z) of the present invention; ii. impregnating the composition with a blowing agent under pressure; iii. Expanding the composition by reducing pressure. A method for producing the bead foam according to claim 1 or 2, comprising:
4. A molded article made from the bead foam according to claim 1 or 2.
5. The molded article according to claim 4, wherein the molded article has a tensile strength of greater than 600 kPa.
6. The molded article according to claim 4 or 5, having a breaking elongation of more than 100%.
7. The molded article according to claim 4, 5 or 6, which has a compressive stress of more than 15 kPa when compressed by 10%.
8. The density of the molded body is 75 to 375 kg / m 3 The molded body according to any one of claims 4 to 7,
9. The molded article according to claim 4 , wherein the molded article has a rebound resilience of more than 55%.
10. 10. The molding according to any one of claims 4 to 9, wherein the molding is a midsole, an insert or a cushioning element of a shoe, the shoe being an outdoor shoe, a sports shoe, a sandal, a boot or a safety shoe.
11. (i) introducing the foam beads into a suitable mold; (ii) melting the foam beads from step (i); A method for producing the molded body according to claim 4 , comprising:
12. A shoe comprising the molding according to any one of claims 4 to 9.
13. 12. The use of the bead foams according to claim 1 or 2 for the production of moldings according to claim 6 to 11 for shoe midsoles, shoe insoles, shoe combisoles, shoe cushioning elements, bicycle saddles, bicycle tyres, damping elements, cushioning, mattresses, underlays, grips, protective films, components in the automotive interior or exterior sector, balls and sports equipment or as floor coverings.
14. The bead foam according to claim 1 or 2, wherein the composition (Z) comprises 80 to 94% by weight of a thermoplastic polyurethane as component I.
15. a. 72 to 94% by weight of a thermoplastic polyurethane as component I; b. 5 to 20% by weight of a styrene polymer as component II; c. 1 to 8% by weight of an impact modifier as component III. The bead foam according to claim 1 or 2, comprising a composition (Z) made of the above, in which the total of components I, II and III is 100% by mass.
16. a. 72 to 86% by weight of a thermoplastic polyurethane as component I; b. 10 to 20% by weight of a styrene polymer as component II; c. 4 to 8% by weight of an impact modifier as component III. The bead foam according to claim 1 or 2, comprising a composition (Z) made of the above, in which the total of components I, II and III is 100% by mass.
17. a. 91% by weight of a thermoplastic polyurethane as component I; b. 5% by weight of a styrene polymer as component II; c. 4% by weight of an impact modifier as component III 3. The bead foam according to claim 1 or 2, comprising a composition (Z) made of the above formula (1), in which the total of components I, II and III always amounts to 100% by weight.
18. 16. The bead foam of claim 15, wherein the styrene polymer as component II has a tensile modulus of greater than 2500 MPa (DIN EN ISO 527-1 / 2, June 2012).
19. 3. Bead foam according to claim 1 or 2, wherein the impact modifier as component III has a tensile modulus of less than 2700 MPa (DIN EN ISO 527-1 / 2, June 2012).
Citation Information
Patent Citations
Extruded and foamed thermoplastic polyurethane elastomer particle and preparation method thereof
CN108239386A
Flatting agents for thermoplastic polyurethane elastomers - comprise non-polar homo- or co-polyolefin(s) which are incompatible with the elastomers and provide improved anti-blocking properties
DE4126499A1
Foams based on thermoplastic elastomers
JP2021522368A
Thermoplastic polyurethane-based foamed materials
WO1994020568A1
Foams based on thermoplastic polyurethanes
WO2007082838A1