Polymer tubes with controlled orientation
By employing planar stretching and annular positioning of crystalline biodegradable polymers with adhesive materials, the method addresses the limitations of conventional techniques, achieving enhanced molecular orientation and mechanical properties in polymer tubes for biomedical applications.
Patent Information
- Application Number
- JP2022076718
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-09-08
- Filing Date
- 2022-05-06
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2038-09-07
AI Technical Summary
Conventional methods for producing polymer tubes, particularly those used in biomedical applications, are limited in controlling molecular orientation throughout the tube wall, leading to imbalanced orientation and reduced mechanical properties.
A method involving planar stretching and annular positioning of crystalline biodegradable polymers, combined with adhesive materials, to achieve controlled molecular orientation and enhanced mechanical properties in the polymer tubes.
The method results in polymer tubes with consistent molecular orientation across the wall thickness, providing higher strength, improved heat shrinkability, and tailored mechanical properties suitable for biomedical applications.
Smart Images

Figure 0007582993000002 
Figure 0007582993000003 
Figure 0007582993000004
Abstract
Description
[Technical field]
[0001] The present application is directed to polymer tubes with specific molecular orientation for application in various fields. [Background technology]
[0002] Polymeric tubes are widely used in many applications. Polymeric bioabsorbable tubes can be designed for implantation in the body (e.g., in blood vessels and arteries), particularly to serve as scaffolding to replace traditional metal stents. Some polymeric bioabsorbable tubes find use as nerve guide tubes and / or as alternatives in the body to regenerate nerve tissue. Other polymeric bioabsorbable tubes can be designed as drains to evacuate fluids and / or gases from body cavities or wounds, for example, to promote healing. Advantageously, polymeric bioabsorbable tubes are prepared using biodegradable polymers and thus can be dissolved or absorbed by the body over time, thereby eliminating the need to surgically remove the tube after use.
[0003] Polymeric biodegradable tubes are generally made of, but are not limited to, poly(L-lactide) (PLLA), poly(D-lactide) (PDLA), poly(D,L-lactide) (PDLLA), poly(ε-caprolactone) (PCL), polyglycolic acid (PGA), poly(para-dioxanone (PDO), poly(trimethylene carbonate) (PTMC), poly(hydroxybutyrate), poly(hydroxyvalerate), poly(tetramethyl carbonate), poly(ethylene oxide) ( The bioabsorbable tube may comprise one or more biodegradable polymers, including poly(ethylene glycol) (PEO), poly(ethylene glycol) (PEG), poly(propylene glycol) (PPG), and copolymers, blends, and derivatives thereof. The selection of the polymer or polymers to produce the polymeric bioabsorbable tube may have an impact on both the biocompatibility / toxicity properties of the resulting tube, and the physical / mechanical properties of the resulting tube, such as degradation rate, strength (e.g., radial strength), and recoil rate.
[0004] One common means for producing such polymer tubes (and particularly single-layer thick-walled polymer tubes) involves extrusion and annular expansion processes. Using such methods, a polymer is extruded into a tubular formation and the resulting tubular formation is annularly stretched / expanded to provide a polymer tube. Molecular orientation within the polymer tube wall, as provided by annular expansion, is generally advantageous as it results in high strength and / or heat shrink properties. However, known extrusion and annular expansion processes are inherently limited in terms of the degree of possible molecular orientation throughout the wall thickness of the polymer tube. Furthermore, due to the tubular structure, a gradient of molecular orientation may exist throughout the wall thickness, and as with annular expansion, the inner diameter of the tube is generally subjected to greater stretching / molecular orientation than the outer diameter of the tube. It would therefore be beneficial to provide a method for controlling molecular orientation within a polymer tube wall, and to provide a polymer tube with a wall that exhibits such controlled molecular orientation. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] “Understanding biaxially and monoaxially oriented films,” Packaging World, October 20, 2013. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention generally relates to a method for producing polymer tubes and polymer tubes produced by such a method. Polymer tubes for use in, for example, biomedical applications are generally expanded / drawn in some manner to induce molecular orientation in the tube wall, which provides high strength (e.g., resistance to radial compression). The novel method disclosed herein, which involves producing polymer tubes and molecularly orienting the polymers herein to obtain oriented polymer tubes, advantageously uses a planar drawing and / or multilayer annular expansion process. As disclosed herein, by modifying the way molecules are oriented in the polymer tube (with respect to the typical extrusion / annular expansion method that provides such oriented polymer tubes), it is possible to provide tubes that exhibit modified crystallinity characteristics and, in some embodiments, corresponding high strength (e.g., high resistance to radial compression) and / or controlled heat shrink properties. [Means for solving the problem]
[0007] In one aspect, the present disclosure provides a method for producing an oriented polymer tube, comprising: subjecting a polymeric material comprising a crystalline biodegradable polymer and having a first dimension to planar stretching to increase the first dimension to obtain an oriented polymeric material exhibiting at least partial molecular orientation; forming the oriented polymeric material and the adhesive polymeric material into a tubular article (which may also be referred to as a tube or an oriented polymeric tube). As an example, the adhesive polymeric material causes adjacent layers of the oriented polymeric material to adhere to themselves or to other layers within the tubular article. The polymeric material may be a polymeric film in some embodiments, and may be a polymeric profile in some embodiments.
[0008] In certain embodiments, the polymeric material has a second dimension, and the subjecting step further comprises stretching the polymeric material to increase the second dimension to obtain a biaxially oriented polymeric material. The adhesive polymeric material may also be associated with a crystalline biodegradable polymer at various stages of the disclosed method. For example, in one embodiment, the method further comprises combining the adhesive polymeric material with a crystalline biodegradable polymer prior to the subjecting step to obtain a polymeric material that is a composite polymeric material having a crystalline biodegradable polymer and an adhesive polymeric material in a hierarchical morphology. In another embodiment, the method further comprises combining the adhesive polymeric material with a stretched polymeric material prior to the forming step.
[0009] The forming step, in certain embodiments, includes winding the polymeric material and the adhesive polymeric material around a cylindrically formed article. In some embodiments, such winding includes winding the polymeric material and the adhesive polymeric material multiple times around the cylindrically formed article to obtain a tube that includes multiple layers of the stretched polymeric material and multiple layers of the adhesive polymeric material. The cylindrically formed article can be modified, for example, a mandrel, where the method further includes removing the tube from the mandrel. In some embodiments, the cylindrically formed article includes a device.
[0010] In another aspect, the present disclosure provides a method for producing an oriented polymer tube, comprising: obtaining at least two polymer tubes, each of which comprises a crystalline biodegradable polymer; annularly expanding the at least two polymer tubes to produce at least two oriented polymer tubes; and combining the at least two oriented polymer tubes and one or more adhesive polymer materials into a multi-layer tubular article. In some embodiments, the annular expansion step is performed before the combining step. In some embodiments, the combining step is performed before the annular expansion step, and in some embodiments, the combining step is performed during the annular expansion step (i.e., the at least two oriented polymer tubes and the adhesive polymer materials are combined during the annular expansion of the at least two polymer tubes).
[0011] The method, in some embodiments, may further include combining the adhesive polymeric material with one or more of the at least two polymeric tubes prior to the annular expansion step to obtain one or more polymeric tubes that are composite polymeric tubes having a crystalline biodegradable polymer and an adhesive polymeric material in a hierarchical form. The method, in some embodiments, further includes combining the adhesive polymeric material with one or more of the at least two polymeric tubes (before or after the annular expansion step) to obtain one or more polymeric tubes that are composite polymeric tubes having a crystalline biodegradable polymer and an adhesive polymeric material in a hierarchical form. In certain embodiments, the method described above and in more detail herein below further includes fusing the multi-layered tubular article by exposing the multi-layered tubular article to heat, pressure, or both heat and pressure. The pressure may be either positive or negative, including, for example, drawing a vacuum (such as by applying a vacuum through a perforated mandrel) to form a tube. The fusion step may, for example, include applying a shrink tube or shrink film around the tubular article / hierarchical structure prior to exposing the tubular article to heat, pressure, or both heat and pressure to obtain the hierarchical structure. For example, the composition of the shrink tube or shrink film may vary and may include, for example, one or more materials selected from the group consisting of fluoropolymers (e.g., poly(tetrafluoroethylene), polyolefins (e.g., low density polyethylene (LLDPE)), polyurethanes, and / or silicone polymers (e.g., polydimethylsiloxane (PDMS)), and combinations thereof.
[0012] In the context of any of the methods disclosed herein, the crystalline biodegradable polymer in certain embodiments is selected from the group consisting of poly(L-lactide) (PLLA), poly(D-lactide) (PDLA), poly(ε-caprolactone) (PCL), polyglycolic acid (PGA), poly(para-dioxanone (PDO), poly(hydroxybutyrate), poly(hydroxyvalerate), poly(tetramethylcarbonate), poly(ethylene oxide) (PEO), poly(ethylene glycol) (PEG), poly(propylene glycol) (PPG), and copolymers, blends, and derivatives thereof. Adhesive polymeric materials can be, for example, poly(ε-caprolactone), poly(trimethylene carbonate), poly(D,L-lactide) (PDLLA), poly(L-lactide-co-ε-caprolactone) poly(L-lactide-co-trimethylene carbonate), The adhesive polymer is selected from the group consisting of poly(ε-caprolactone-co-trimethylene carbonate), poly(ethylene glycol), poly(L-lactide-co-poly(ethylene glycol), and copolymers, derivatives, and combinations thereof. It should be noted that this list is not intended to be exhaustive, i.e., the same polymer or polymers may be present as both the crystalline biodegradable polymer and the adhesive polymer in the resulting product, and may differ in terms of molecular orientation (e.g., a polymer may have greater molecular orientation as the crystalline biodegradable polymer component and less molecular orientation as the adhesive polymer component). Thus, the present disclosure encompasses, in certain embodiments, methods and products in which the crystalline biodegradable polymer and the adhesive polymer material comprise the same polymer with different orientations (e.g., different amounts of orientation).
[0013] The present disclosure further provides an oriented polymer tube prepared according to any of the methods disclosed herein. Some such oriented polymer tubes comprise primarily crystalline biodegradable polymers with minimal amounts of adhesive polymeric material. In some embodiments, such oriented polymer tubes are characterized by a molecular orientation of the crystalline biodegradable polymer that is essentially consistent throughout the wall of the oriented polymer tube.
[0014] A further aspect provides a method for producing an oriented polymer tube, the method comprising: determining a desired geometry and molecular orientation profile for the oriented polymer tube; selecting one or more polymer tube precursors comprising a biodegradable crystalline polymer; positioning the one or more polymer tube precursors; and forming the one or more polymer tube precursors into an oriented polymer tube exhibiting a desired final tubular geometry and molecular orientation profile. The geometry and molecular orientation profile can be determined, for example, based on one or more of: (i) the desired mechanical properties of the oriented polymer tube to be formed; (ii) the desired thermodynamic properties of the oriented polymer tube to be formed; and (iii) the desired chemical properties of the oriented polymer tube to be formed.
[0015] In some embodiments, at least one of the one or more polymer precursors is selected based at least in part on (i) the composition of the one or more polymer precursors, (ii) the geometry of the one or more polymer precursors, (iii) the mechanical properties of the one or more polymer precursors, (iv) the thermodynamic properties of the one or more polymer precursors, (v) the chemical properties of the one or more polymer precursors, (vi) the degree of molecular orientation of the one or more polymer precursors, (vii) the molecular orientation profile about one or more axes of the one or more polymer precursors, (viii) a predetermined method of forming the one or more polymer precursors into a final polymer tube, and any combination thereof. In some embodiments, the one or more polymer precursors are selected from the group consisting of (i) one or more films, (ii) one or more tubes, and (iii) one or more profiles.
[0016] In certain embodiments, the one or more polymer precursors are one or more films or one or more tubes, where the film or tube is specifically selected to impart one or more of the following to the oriented polymer tube: (i) one or more specific mechanical properties, (ii) one or more specific thermodynamic properties, (iii) one or more specific chemical properties, and (iv) one or more specific degradation rates. In other certain embodiments, the one or more polymer precursors are one or more profiles, where the one or more profiles have cross-sectional shapes including, but not limited to, circular, rectangular, triangular, elliptical, and tubular. In some embodiments, the one or more polymer precursors are one or more profiles, where the profiles are specifically selected to impart one or more of the following to the oriented polymer tube: (i) one or more specific mechanical properties, (ii) one or more specific thermodynamic properties, (iii) one or more specific chemical properties, and (iv) one or more specific degradation rates. Advantageously, in some of these embodiments, the one or more polymer precursors further include a tie layer.
[0017] Positioning the one or more polymer precursors, in some embodiments, includes one or more of: (i) positioning the one or more polymer precursors around a mandrel (or other support as described herein below); and (ii) positioning the one or more polymer precursors inside a mold (which in certain embodiments may be expandable, e.g., includes a balloon). For example, positioning around the mandrel can include positioning around the mandrel using a technique selected from the group consisting of wrapping, sheathing, wrapping, braiding, and combinations thereof. The mandrel can, in some embodiments, include a device. Positioning one or more polymer precursors within the mold includes (i) positioning one or more polymer precursors on a mandrel, then inserting the one or more polymer precursors on the mandrel into the mold and removing the mandrel, (ii) positioning one or more polymer precursors on a mandrel, then removing the mandrel and inserting the one or more polymer precursors into the mold, or (iii) positioning one or more polymer precursors within the mold during one or more production steps of the precursors.
[0018] The one or more producing steps are, for example, selected from the group consisting of tube expansion, blow molding, injection stretch blow molding, die drawing, and mandrel drawing. Positioning, for example, includes positioning two or more polymer precursors, where the positioning of each polymer precursor occurs simultaneously or sequentially. Forming, in certain embodiments, can further include fusing the one or more polymer precursors by exposing the one or more polymer precursors to heat, pressure, or both heat and pressure. Such fusing can, for example, include applying a shrink tube or shrink film around the one or more polymer precursors before exposing the one or more polymer precursors to heat, pressure, or both heat and pressure. Such fusing can, for example, include exposing the one or more polymer precursors to heat, pressure, or both heat and pressure using a mold and a balloon. In some such embodiments, the mold is lined with one or more polymer precursors, and a portion of the balloon will constitute a portion of the final polymer tube. In such embodiments, the forming step can occur, for example, during or after the positioning step. In some embodiments, the two or more positioning steps and the two or more forming steps occur simultaneously or sequentially. Advantageously, in some embodiments, the one or more polymer precursors comprise a biocompatible, biodegradable polymer, such as a polymer including one or more polymers selected from the group consisting of, but not limited to, poly(L-lactide) (PLLA), poly(D-lactide) (PDLA), poly(ε-caprolactone) (PCL), polyglycolic acid (PGA), poly(para-dioxanone) (PDO), poly(hydroxybutyrate), poly(hydroxyvalerate), poly(tetramethylcarbonate), poly(ethylene oxide) (PEO), poly(ethylene glycol) (PEG), poly(propylene glycol) (PPG), and copolymers, blends, and derivatives thereof.
[0019] The present disclosure further provides an oriented polymer tube prepared according to any of the methods outlined herein. The tube of the present disclosure can be characterized, for example, by a molecular orientation profile that is essentially consistent through the wall of the oriented polymer tube, a molecular orientation profile that is essentially consistent through a predefined portion of the wall of the oriented polymer tube, a molecular orientation profile characterized by varying levels of orientation through a predefined portion of the wall of the oriented polymer tube, a molecular orientation profile characterized by varying axes of orientation through a predefined portion of the wall of the oriented polymer tube, a molecular orientation profile characterized by an increasing gradient of molecular orientation through the wall from the inner diameter to the outer diameter of the oriented polymer tube, a molecular orientation profile characterized by a decreasing gradient of molecular orientation through the wall from the inner diameter to the outer diameter of the oriented polymer tube, a molecular orientation profile that is essentially consistent through the length of the oriented polymer tube, a molecular orientation profile that is essentially consistent through a predefined portion of the length of the oriented polymer tube, a molecular orientation profile characterized by varying levels of orientation through a predefined portion of the length of the oriented polymer tube, and / or a molecular orientation profile characterized by varying axes of orientation through a predefined portion of the length of the oriented polymer tube.
[0020] Tubes of the present disclosure can be characterized, for example, by a compositional profile that is essentially consistent through the wall of the oriented polymer tube, a compositional profile that is essentially consistent through a predefined portion of the wall of the oriented polymer tube, a compositional profile characterized by a variation in composition through a predefined portion of the wall of the oriented polymer tube, a compositional profile that is essentially consistent through the length of the oriented polymer tube, a compositional profile that is essentially consistent through a predefined portion of the length of the oriented polymer tube, and / or a compositional profile characterized by a variation in composition through a predefined portion of the length of the oriented polymer tube. The tubes of the present disclosure can be characterized, for example, by a degradation rate profile that is essentially consistent through the wall of the oriented polymer tube, a degradation rate profile that is essentially consistent through a predefined portion of the wall of the polymer tube, a degradation rate profile characterized by a variety of degradation rates through a predefined portion of the wall of the oriented polymer tube, a degradation rate profile characterized by an increasing degradation rate gradient through the wall from the inner diameter to the outer diameter of the oriented polymer tube, a degradation rate profile characterized by a decreasing degradation rate gradient through the wall from the inner diameter to the outer diameter of the oriented polymer tube, a degradation rate profile that is essentially consistent through the length of the oriented polymer tube, a degradation rate profile that is essentially consistent through a predefined portion of the length of the oriented polymer tube, a degradation rate profile characterized by a variety of orientation degradation rates through a predefined portion of the length of the oriented polymer tube, and / or a degradation rate profile characterized by a degradation rate gradient along the length of the oriented polymer tube.
[0021] The present disclosure further provides a method for producing an oriented polymer tube, the method including: determining a desired tubular geometry and at least one of a desired composition profile and a desired molecular orientation profile; selecting one or more polymer precursors; positioning the one or more polymer precursors; and forming the one or more polymer precursors into an oriented polymer tube exhibiting the desired tubular geometry and at least one of the desired composition profile and the desired molecular orientation profile.
[0022] Certain specific embodiments are as follows:
[0023] Embodiment 1: A method for producing an oriented polymer tube, comprising obtaining at least one stretched polymer material exhibiting at least partial molecular orientation, where obtaining the at least one stretched polymer material comprises stretching the at least one polymer material, the at least one polymer material having a first dimension, and at least one crystalline biodegradable polymer material, the at least one polymer material being stretched in a manner that increases the first dimension; and using the at least one stretched polymer material to form an oriented polymer tube.
[0024] Embodiment 2: The method of the previous embodiment, wherein the stretching comprises planar stretching.
[0025] Embodiment 3: The method of any of the previous embodiments, wherein one or more of the at least one polymeric material is one or more of a polymeric film, a polymeric monofilament, a polymeric ribbon, a polymeric tape, and a polymeric rod.
[0026] Embodiment 4: The method of any of the previous embodiments, wherein the at least one polymeric material has a second dimension, and stretching the at least one polymeric material comprises stretching the at least one polymeric material to increase the second dimension, and the at least one stretched polymeric material comprises a biaxially stretched polymeric material.
[0027] Embodiment 5: The method of any of the previous embodiments, wherein forming comprises using at least one stretched polymeric material, and at least one adhesive polymeric material.
[0028] Embodiment 6: The method according to the previous embodiment, further comprising obtaining the at least one polymeric material at least in part based on combining at least one adhesive polymeric material with at least one crystalline biodegradable polymeric material.
[0029] Embodiment 7: The method according to the previous embodiment, wherein the at least one polymeric material is a composite polymeric material comprising at least one crystalline biodegradable polymeric material and at least one adhesive polymeric material in a hierarchical morphology.
[0030] Embodiment 8: The method of embodiment 6, wherein the at least one adhesive polymeric material and the at least one crystalline biodegradable polymeric material are combined before, during, or after the at least one polymeric material is stretched.
[0031] Embodiment 9: The method of embodiment 6, wherein forming the tube comprises winding at least one expanded polymeric material and at least one adhesive polymeric material around a support.
[0032] Embodiment 10: The method according to the previous embodiment, wherein the support has one or more of a cylindrical, circular, rectangular, triangular, elliptical, polygonal, and tubular shape.
[0033] Embodiment 11: The method of embodiment 9 or 10, wherein the winding comprises winding at least one stretched polymeric material and at least one adhesive polymeric material multiple times around the support such that the tube comprises multiple layers of at least one stretched polymeric material and multiple layers of at least one adhesive polymeric material.
[0034] Embodiment 12: The method of any of embodiments 9 to 11, wherein the at least one stretched polymeric material has multiple units of stretched polymeric material, the multiple units of stretched polymeric material having different polymeric materials or the same polymeric materials; and forming includes arranging the multiple units of stretched polymeric material in at least one of a stacked manner and a staggered manner, and winding the arranged multiple units of stretched polymeric material at a bias angle.
[0035] Embodiment 13: The method of any of embodiments 9 to 12, wherein the support is a mandrel, and the method further comprises removing the tube from the mandrel.
[0036] Embodiment 14: The method of any one of embodiments 9 to 12, wherein the support comprises a device.
[0037] Embodiment 15: The method of embodiment 14, further comprising forming a resulting composite based at least in part on the oriented polymer tubes and the support, wherein the resulting composite is a medical device.
[0038] Embodiment 16: The method of any of the preceding embodiments, further comprising forming a medical device based at least in part on the oriented polymer tubes.
[0039] Embodiment 17: The method of any of the preceding embodiments, wherein forming the medical device comprises cutting the tube into a stent.
[0040] Embodiment 18: The method of the previous embodiment, further comprising applying one or more of a therapeutic agent, a covering, and a coating to the stent.
[0041] Embodiment 19: The method of any of the preceding embodiments, wherein forming comprises exposing the at least one stretched polymeric material to at least one of heat and pressure.
[0042] Embodiment 20: The method of any of the preceding embodiments, wherein forming comprises applying a shrink tube or shrink film around at least a portion of the at least one stretched polymeric material to obtain a hierarchical structure, and forming comprises exposing the hierarchical structure to at least one of heat and pressure.
[0043] Embodiment 21: The method of any of the previous embodiments, wherein forming comprises inserting at least a portion of the at least one stretched polymeric material into a mold; positioning the at least one stretched polymeric material on an expandable support; and exposing the at least one stretched polymeric material to at least one of heat and pressure.
[0044] Embodiment 22: The method of any of the previous embodiments, wherein one or more of the at least one crystalline, biodegradable polymeric material is selected from the group consisting of poly(L-lactide) (PLLA), poly(D-lactide) (PDLA), poly(ε-caprolactone) (PCL), polyglycolic acid (PGA), poly(para-dioxanone) (PDO), poly(hydroxybutyrate), poly(hydroxyvalerate), poly(tetramethylcarbonate), poly(ethylene oxide) (PEO), poly(ethylene glycol) (PEG), poly(propylene glycol) (PPG), copolymers thereof, derivatives thereof, and combinations thereof.
[0045] Embodiment 23: The method of any of the previous embodiments, wherein the forming comprises using at least one stretched polymeric material and at least one adhesive polymeric material, the adhesive polymeric material being selected from the group consisting of poly(ε-caprolactone), poly(trimethylene carbonate), poly(D,L-lactide), poly(L-lactide)-co-ε-caprolactone), poly(L-lactide-co-trimethylene carbonate), poly(ε-caprolactone-co-trimethylene carbonate), poly(ethylene glycol), poly(L-lactide-co-poly(ethylene glycol)), copolymers thereof, derivatives thereof, and combinations thereof.
[0046] Embodiment 24: The method of any of embodiments 5 to 23, wherein forming comprises using at least one stretched polymeric material and at least one adhesive polymeric material, and wherein the at least one crystalline biodegradable polymeric material and the at least one adhesive polymeric material comprise the same polymeric material.
[0047] Embodiment 25: The method of any of the preceding embodiments, wherein the at least one stretched polymeric material is stretched by at least 10 percent of the maximum stretch ratio respectively corresponding to the at least one polymeric material.
[0048] Embodiment 26: The method of any of the previous embodiments, wherein stretching the at least one polymeric material comprises controlling one or more of the mechanical properties, thermodynamic properties, chemical properties, electrical properties, and degradation rates of the at least one polymeric material during stretching.
[0049] Embodiment 27: The method of any of the previous embodiments, wherein the at least one polymeric material is stretched between 300 percent and 1000 percent of the original dimension of the at least one polymeric material.
[0050] Embodiment 28: A method comprising obtaining at least one stretched polymeric material exhibiting at least partial molecular orientation, the at least one stretched polymeric material corresponding to at least one polymeric material having a first dimension and at least one crystalline biodegradable polymeric material, the at least one polymeric material being stretched to increase the first dimension; and forming a tube using the at least one stretched polymeric material.
[0051] Embodiment 29: A tube comprising at least one stretched polymeric material exhibiting at least partial molecular orientation, the at least one stretched polymeric material being obtained at least in part based on stretching at least one polymeric material, the at least one polymeric material having a first dimension and at least one crystalline biodegradable polymeric material, the at least one polymeric material being stretched in an increasing first direction.
[0052] Embodiment 30: A tube having at least one crystalline biodegradable polymeric material and an exterior surface having a normal perpendicular to the length of the tube, the tube exhibiting a maximum stress value of about 20 MPa or more measured based on a first compression cycle; and the tube being deformed by at least 17% of a first dimension after the first compression cycle.
[0053] Embodiment 31: A tube as described in the previous embodiment, wherein the first compression cycle includes: obtaining an initial distance between two parallel plates between which the tube is placed, wherein the two parallel plates are in contact with an outer surface of the tube such that the two parallel plates essentially do not impose a load on the tube; compressing the plates to a distance of 50% of the initial distance at a rate of 50% of the initial distance of the two parallel plates per minute, wherein the tube is deformed in a first direction, the first direction being the direction in which the plates are compressed; and releasing the compression of the plates against the tube at a rate of 50% of the initial distance of the two parallel plates per minute.
[0054] Embodiment 32: A tube according to embodiment 30 or 31, wherein the total energy value under the engineering stress-strain curve corresponding to the tube after the first compression is at least 138 kgf·mm / cm.
[0055] Embodiment 33: A tube according to any of the preceding embodiments, wherein the tube has one or more of a therapeutic agent, a cover, and a coating applied thereto.
[0056] Embodiment 34: A tube having at least one crystalline biodegradable polymeric material and an exterior surface having a normal perpendicular to the length of the tube, the tube exhibiting a maximum stress value of about 20 MPa or more as measured based on a first compression cycle; and a total energy value under an engineering stress-strain curve corresponding to the tube after the first compression of at least 138 kgf·mm / cm.
[0057] These and other features, aspects, and advantages of the present disclosure will become apparent upon reading the following detailed description in conjunction with the accompanying drawings, which are briefly described below. The present invention includes any combination of two, three, or more of the above-mentioned embodiments, as well as any combination of two, three, or more of the features or elements described in the present disclosure, regardless of whether such features or elements are expressly combined in the description of a specific embodiment herein. The present disclosure is intended to be read holistically such that any separable features or elements of the disclosed invention are deemed to be intended to be combinable in any of its various aspects and embodiments, unless the context clearly dictates otherwise. Other aspects and advantages of the present invention will become apparent from the following.
[0058] To provide an understanding of embodiments of the present invention, reference is made to the accompanying drawings, which are not necessarily drawn to scale, and in which reference numerals refer to components of exemplary embodiments of the present invention. The drawings are merely illustrative and should not be construed as limiting the present invention. [Brief description of the drawings]
[0059] [Figure 1] FIG. 1 is a background (prior art) schematic diagram of a typical extrusion / expansion process for producing a single layer oriented polymer tube. [Diagram 2] FIG. 1 is a schematic diagram of the method disclosed herein for producing oriented polymer tubes by planar orientation and annular positioning. [Diagram 3] 1A-1D are schematic diagrams of various techniques for winding a polymer film to form a polymer tube. [Figure 4] 1 is a schematic diagram of a method for aligning adjacent polymer films to form a polymer tube. [Figure 5A] FIG. 2 is a schematic diagram of a particular method disclosed herein for producing an oriented polymer tube by multi-layer annular orientation and annular positioning. [Figure 5B] FIG. 2 is a schematic diagram of another method disclosed herein for producing an oriented polymer tube by multi-layer annular orientation and annular positioning. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0060] The present invention will now be described more fully hereinafter with reference to the accompanying drawings, in which some, but not all, embodiments of the invention are shown. Indeed, these inventions may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will satisfy applicable legal requirements. Like numbers refer to like elements throughout.
[0061] The present disclosure relates to methods for producing polymer tubes (e.g., biodegradable polymer tubes) and the polymer tubes produced thereby. In particular, the present disclosure relates to methods for producing polymer tubes comprising crystalline polymers, which involve a molecular orientation step that aligns / orients at least some of the molecules of the crystalline polymer within the wall of the tube (yielding an oriented polymer tube). In various embodiments, the methods disclosed herein provide control over the crystalline molecular orientation within the polymer tube wall, e.g., with respect to all three axes of a cylindrical coordinate system. The methods disclosed herein, in certain embodiments, involve selecting a predetermined final tubular geometry and an associated predetermined molecular orientation profile, and thus selecting materials and method steps, e.g., by positioning and forming one or more precursors to achieve the desired final tubular geometry and molecular orientation profile. The disclosed methods can advantageously provide oriented polymer tubes that exhibit sufficient strength / resistance to radial compression to make them useful in a wide range of applications, including, for example, but not limited to, biomedical applications. The disclosed methods can also advantageously provide oriented polymer tubes that exhibit more controlled and improved heat shrink properties relative to tubes (e.g., oriented polymer tubes) produced by conventional extrusion and cyclic expansion.
[0062] As mentioned above, a conventional method for producing oriented polymer tubes involves extrusion and annular expansion to provide a monolayer tube. In such a method, a polymer tube is extruded by conventional methods and then subjected to annular expansion as shown diagrammatically in Figure 1 (Prior Art). As shown in Figure 1, an extruded tube 10 has an OD of 2 x r il The inner radius (r il For a given inner diameter (ID) and OD=2×r o1 According to the formula, the outer radius (r o1The extruded tube 10 is produced with a given outside diameter (OD) for a given ID (r based on the above formula) to produce the polymer tube 12. i2 ) and a larger OD (r based on the above formula o2 (with respect to T) (optionally under conditions of heat and pressure as indicated by T and P, respectively). In such an expansion process, the ID of the extruded tube undergoes a higher degree of stretching than the OD of the extruded tube. The difference in the rate and amount of expansion the ID and OD experience during such a process leads to an imbalance in the degree of molecular orientation across the tube wall (i.e., from the ID to the OD). As noted above, typical annular expansion processes are limited in terms of the degree of orientation across the final wall thickness, which results in a reduced orientation gradient from the ID to the OD.
[0063] In accordance with the present disclosure, various methods are provided for producing oriented polymer tubes comprising crystalline polymers (e.g., biodegradable crystalline polymers providing the resulting biodegradable oriented polymer tubes). In some embodiments, such tubes may exhibit modified molecular orientation characteristics, as well as corresponding modified mechanical and / or thermodynamic properties, with respect to oriented polymer tubes produced by conventional extrusion and cyclic expansion. In this regard, modified molecular orientation characteristics may refer to a greater proportion of molecular orientation in the crystalline regions of the oriented polymer tube and / or a greater regularity in the distribution of molecular orientation within the crystalline regions of the oriented polymer tube. For example, in some embodiments, the molecular orientation throughout the wall thickness of the disclosed oriented polymer tubes is more uniform (leading to such improved mechanical and thermodynamic properties) than the walls of oriented polymer tubes produced by conventional methods such as those shown in FIG. 1. Modified mechanical properties may refer to higher strength, higher modulus, higher toughness, and / or greater elasticity. Modified thermomechanical properties may also refer to modified heat shrink properties, including, but not limited to, controlled shrink activation temperature, shrink force, and shrink ratio.
[0064] Planar orientation and annular positioning One method provided herein involves using uniaxially or biaxially oriented polymer films as oriented precursors for forming oriented polymer tubes (referred to herein as "planar orientation and annular positioning"). It is known that orienting polymer molecules by stretching them into uniaxially or biaxially oriented films improves properties such as tensile strength and toughness. See, for example, "Understanding biaxially and monoaxially oriented films," Packaging World, October 20, 2013.
[0065] One embodiment of the presently disclosed method is shown diagrammatically in Figure 2. According to this method, a polymer film comprising a crystalline polymer having a given dimension x1 (herein considered as the film length) is stretched in a planar direction to obtain a stretched polymer film having a corresponding dimension x2 that is longer than x1 (i.e., the stretched polymer film has an increased length). The stretched polymer film is referred to herein as an "oriented" polymer film because the stretching process imparts at least some molecular orientation within the crystalline regions of the polymer film.
[0066] The polymer film may come in a variety of sizes and thicknesses, with the amount of stretching (for x1 and x2 values) being determined in some embodiments based on the desired thickness (z, not shown in FIG. 2) of the stretched / oriented film relative to the initial thickness of the (unstretched / unoriented) film. In some embodiments, the amount of stretching (for x1 and x2 values) can be determined based on the desired mechanical and / or thermodynamic properties of the stretched / oriented film. The embodiment illustrated in FIG. 2 provides for uniaxial stretching (only stretching / increasing the dimension x); however, in some embodiments, the disclosed method involves biaxial stretching (stretching / increasing both dimensions x and y, i.e., length and width). In such embodiments, the stretch rate and / or amount in both the x and y directions may be modified independently of each other. Planar stretching (either in only one dimension, i.e. uniaxial, or in two dimensions, i.e. biaxial) is advantageously carried out in a controlled manner so that the stretch ratio, i.e. dx / dt (FIG. 2), represented by "k", is constant, and the resulting stretched / oriented polymer film is essentially homogeneous (e.g., in terms of thickness). When the planar stretching is uniaxial as shown in FIG. 2, it is understood that the stretch ratio dy / dt with respect to another axis (here along the y-axis) is equal to 0 (i.e., there is no stretching along the y-axis). Those skilled in the art will recognize that dy / dt is not 0 when stretching along the y-axis.
[0067] The polymeric film subjected to stretching can be produced by any of a number of methods, including, but not limited to, extrusion, extrusion coating, injection / blow molding, melt casting, solution casting, or compression molding (the latter two processes allow the use of higher molecular weight polymers than extrusion). In some embodiments, materials such as fillers can be dispersed into the polymeric film prior to the stretching step. In certain embodiments, the tie layer material is associated with the polymeric film prior to stretching (so that both the polymeric film and the tie layer material are stretched together), as described in more detail below. It should be noted that although the application is specifically described in the context of stretched polymeric films (and polymeric profiles, as referenced below), the present disclosure is not intended to be so limited. For example, in other embodiments, polymeric materials in the form of polymeric monofilaments, polymeric ribbons, polymeric tapes, or polymeric rods are used. Those skilled in the art are familiar with these terms and will understand, for example, that a polymer monofilament is a synthetic fiber such as a thread (the fiber can have a variety of diameters), a polymer tape is a flattened piece of polymer material (the tape may have a variety of lengths and widths), and a polymer rod is a three-dimensional structure (circular in diameter, but not limited to such). As an example, the polymer rod may be a cylindrical structure. As another example, the polymer rod may be a tubular structure.
[0068] As mentioned above, there are many methods known in the art for stretching polymeric materials in one or two dimensions. In machine direction (MD) stretching, the extruded film is cast onto a chill roll, then reheated and passed through nips and tensioning rollers at a speed exceeding the speed of extrusion casting to stretch the material. Subsequent transverse direction (TD) stretching is accomplished by gripping the sides of the film in clamps and pulling the clamps perpendicular to the machine direction through a heated oven in a tenter. Alternatively, MD and TD stretching can be accomplished simultaneously in a tenter capable of simultaneous biaxial stretching, such as the LISIM line manufactured by Bruckner. The line speed, temperature, and stretch ratio are controlled to achieve the desired degree of stretching without tearing the film. Simultaneous stretching of polymeric materials can also be achieved by using a blown film line, which extrudes the polymeric material through an annular die and then expands the extrudate with air to create a bubble that helps stretch the material in both the TD and MD directions. If additional MD or TD stretching is required, the blown film line can be modified to provide a second bubble to achieve a higher degree of stretching in either or both MD and TD. There are many manufacturers of industrial blown film and double bubble lines, such as Hosokawa Alpine, GAP srl. or Kuhne Group. In addition to the continuous process outlined herein, batch stretching can be achieved in some embodiments by clamping the polymer film on all sides and stretching it in one or both MD and TD, either sequentially or simultaneously, in an oven. The Karo IV stretcher manufactured by Bruckner provides one example of a batch film stretcher.
[0069] The extent to which the polymer film is stretched can be varied as described above. In some embodiments, the polymer film is stretched at least 10 percent of the maximum stretch ratio corresponding to at least one polymer material. As used herein, "maximum stretch ratio" is intended to mean the maximum possible stretch before material tearing occurs.
[0070] Using the stretched and oriented polymer film as a precursor for forming a tubular article, the stretched and oriented polymer film is positioned in an annular configuration (e.g., by rolling or winding the stretched and oriented polymer film) and, optionally, further processed to provide an oriented polymer tube (e.g., an oriented biodegradable polymer tube). While the present disclosure focuses on positioning the stretched and oriented polymer film in an annular configuration by rolling / winding the film to provide a tubular article, other means for positioning are also encompassed herein.
[0071] The stretched and oriented polymeric film may optionally be further processed prior to this step, for example, by cutting the film into individual desired sizes and / or associating a tie layer therewith, as described in more detail below. While not intended to be limiting, one means for positioning the stretched and oriented polymeric film in a circular configuration includes winding / rolling the film around a forming mandrel. It is noted that the shape of the forming mandrel is not particularly limited. Thus, it is understood that a polymeric "tube" as used herein is not limited to a cylindrical tube. Rather, a polymeric "tube" produced according to the disclosed method is any hollow elongated structure, where the cross-sectional shape of the hollow elongated structure may be, but is not limited to, a circle.
[0072] The disclosed method is further not limited to winding / rolling the film around a mandrel; rather, the film can be wrapped around various types of supports. Suitable supports include, but are not limited to, supports having one or more of cylindrical, circular, rectangular, triangular, elliptical, polygonal, and tubular configurations. In some embodiments, the support is a device or a component of a device (e.g., but not limited to, a stent). In certain such embodiments, the methods disclosed herein provide a composite including the support and the positioned and oriented polymer film, which may be in the form of a medical device. Particularly when the support is a device, and when the disclosed method provides a medical device, the composite can, in some embodiments, be further processed. For example, in some embodiments, one or more of a therapeutic agent, a cover, and a coating are applied to the composite. In some embodiments, the composite is cut to an appropriate size for a stent. Various methods are known for cutting stents, including, but not limited to, laser cutting.
[0073] The oriented polymer film can be positioned, in some embodiments, by rolling / wrapping as described above to provide a single layer oriented polymer tube with little to no overlap of one end of the polymer film with the opposite end of the film (e.g., with only a slight seam where the two film ends meet), or by rolling / wrapping the film multiple times to produce a multi-layer tube. More preferably, a multi-layer tube having any number of layers (e.g., a tube having a "hierarchical structure") is formed, where the number of layers is not particularly limited. An exemplary such multi-layer tube has 2-20 layers of oriented polymer film, which preferably includes a single oriented polymer film that is rolled / wrapped to obtain a desired number of layers (e.g., to achieve a desired wall thickness of the resulting multi-layer oriented polymer tube). In such embodiments, it is understood that a greater number of layers / wrappings will provide a polymer tube with a thicker wall (assuming that oriented polymer films with the same thickness are used). Therefore, the number of layers / wrappings may dictate the wall thickness of the resulting oriented polymer tube. The axis along which the polymer film is rolled / wound can be varied relative to the axis / axes along which the polymer film is stretched / oriented, as shown in Figures 3A-3C, where the circular arrow indicates the direction of rolling.
[0074] Typically, to provide sufficient adhesion between adjacent oriented polymer film layers of such multi-layer polymer tubes (e.g., produced by positioning and forming multiple wrappings of one or more films), a tie layer (e.g., "adhesive polymer material") as described herein below is included in the oriented polymer tube. In some embodiments, the tie layer is incorporated by associating a tie layer material with a (non-stretched / non-oriented) polymer film as described herein above to provide a composite polymer film, and subjecting the composite polymer film to planar expansion as described above. This association can be done, for example, by aligning a tie layer material film with the (non-stretched / non-oriented) polymer film, or by coating the (non-stretched / non-oriented) polymer film with the tie layer material, such as by extrusion coating or solution coating onto the polymer film. This method provides both the crystalline polymer film and the tie layer in a stretched form (and in some such embodiments, this method could provide molecular orientation not only in the polymer film, but also in the tie layer).
[0075] In another embodiment, the tie layer is incorporated by associating the tie layer material with a stretched / oriented polymer film. In such an embodiment, the composite film is provided by stretching / orienting a crystalline polymer film and then associating the tie layer material with the stretched and oriented polymer film. The association can be done, for example, by aligning the tie layer material film with the (stretched / oriented) polymer film, or by coating the (stretched / oriented) polymer film with the tie layer material, such as by extrusion coating or solution coating the tie layer material onto the polymer film. The composite polymer film provided according to this embodiment includes the crystalline polymer film in stretched / oriented form, while the tie layer is in non-stretched / non-oriented form. Other modifications to these embodiments are also encompassed, for example, where the polymer film and the tie layer can be stretched independently to obtain a stretched / oriented polymer film and a stretched or stretched / oriented tie layer, which can then be combined to obtain a composite polymer film.
[0076] As briefly mentioned hereinabove, the composition of the oriented polymer film and the composition of the tie layer may be the same or different. Thus, in certain embodiments, the composition of one or more of the oriented polymer films is the same as the composition of one or more tie layers, but the polymers are oriented to a different degree (e.g., the oriented polymer film(s) are oriented to a greater degree than the tie layer(s)).
[0077] The composite polymer film is then formed into an oriented polymer tube as provided herein above, such that the tie layer material is associated with each "layer" (or wrapping) of the oriented polymer film and bonds adjacent layers of the polymer film together. Bonding may, in some embodiments, require treating the final polymer tube by exposing it to heat and / or pressure. In some embodiments, the pressure is negative, i.e., a vacuum is applied to the tube, such as by drawing a vacuum through a mandrel around which the polymer tube is wrapped. In some embodiments, the heat and (positive) pressure are provided by wrapping the polymer tube with a shrink material (e.g., shrink tubing or shrink wrap including linear low density polyethylene, LLDPE) and heating the wrapped polymer tube (e.g., by placing the tube in an oven). The oven temperature, forming time, and applied forming pressure may depend on the components of the polymer tube, and these process variables can each be controlled to tailor the properties of the final oriented polymer tube. In some embodiments, other bonding techniques may be utilized to replace or supplement the heat / pressure method. For example, in some embodiments, the bonding can utilize contact with one or more solvents (e.g., chloroform), and in some embodiments, the bonding can involve the use of radio frequency welding.
[0078] The planar orientation / annular positioning method outlined herein above is disclosed as including three separate steps (planar orientation, e.g., stretching a polymer film; annular positioning, e.g., positioning the oriented polymer film in an annular position, and forming, e.g., forming the positioned and oriented polymer film into an oriented polymer tube), and the disclosed method can be modified to perform two or all three of these steps, often simultaneously. For example, in some embodiments, the polymer film may be provided in an unstretched form and can be stretched (and oriented) by air and / or hydraulic pressure against a cylindrical forming surface to form an oriented polymer tube.
[0079] In some embodiments, rather than utilizing a stretched polymer film as the polymer tube precursor, an oriented composite polymer profile can be positioned and formed into a tube, thus providing a polymer tube precursor. The method involves positioning an oriented composite polymer profile with respect to all three cylindrical axes according to a desired orientation profile. Positioning the composite profile can include, but is not limited to, rolling, sheathing, wrapping, or braiding. The positioned composite profile is exposed to pressure and / or temperature such that the tie layers adhere to adjacent layers of the composite profile, thereby forming a coherent multi-layer oriented polymer tube.
[0080] A polymer profile is a shaped form of polymer (rather than a polymer film as described above), which includes crystalline polymers as disclosed herein. Exemplary polymer profiles include, but are not limited to, cross-sectional profiles in the form of squares, rectangles, polygons, ellipses, or other geometric shapes, which may or may not have regular or intermittent features on one or more surfaces of the shape. A composite profile is a polymer profile (including a crystalline polymer as described above) that further includes a tie layer material.
[0081] In certain embodiments, the tubes produced by positioning and forming the oriented film or profile as outlined in this paragraph exhibit a more consistent degree of molecular orientation across the tube wall thickness than that of the extruded and radially expanded monolayer tube (produced as described above and shown diagrammatically in FIG. 1). Using a cylindrical coordinate system and assuming that two surfaces in full contact (except for a tie layer of negligible thickness) are geometrically continuous, such a tube formed from a circular shaped profile positioned to obtain maximum density would not be geometrically continuous along all three axes. In terms of imposing molecular orientation and geometric continuity, such a tube would be continuous along the θ axis and not continuous along the r and z axes. Such a tube formed from a rectangular shaped profile positioned to obtain maximum density would not be geometrically continuous along all three axes. In terms of imposing molecular orientation and geometric continuity, such a tube would be continuous along all three axes.
[0082] The planar orientation / annular positioning method disclosed herein offers many advantages over conventional extrusion / annular expansion. For example, according to the disclosed method, each polymer film (or profile) can be stretched uniaxially or biaxially as desired and to a desired degree. Multiple polymers can be combined as individual layers in a composite structure in some embodiments and stretched (and oriented) together. In some embodiments, multiple polymers can be provided independently in the form of films or profiles and stretched (and oriented) to various degrees, and then these oriented films and / or profiles can be combined before or during the formation of a polymer tube.
[0083] The manner in which the various polymer films (or profiles) can be combined may be varied to achieve various composite structures and various properties. For example, in some embodiments, multiple films can be stacked (e.g., on a forming mandrel) at a bias angle during the tube forming process to meet the key application requirements. Various configurations of the component layers can be obtained during production. For example, the individual layers may be staggered or stacked on top of each other. In this context, a stacked configuration (e.g., as shown in FIG. 4A) includes different films directly on top of each other, and a staggered configuration (e.g., as shown in FIG. 4B) includes different films placed off-center, so that when they are rolled (or otherwise formed into a tubular form), the initial layer(s) are a single material, followed by one or more layers of the composite film (or profile), followed by one or more layers of the final material. The resulting oriented polymer tube further provides a stacked set of layers and a staggered set of layers.
[0084] In some embodiments, individual films / layers can be selected for highly specific properties such as strength, toughness, drug encapsulation / elution, adhesion, surface functionality, degradability, etc., to impart such properties to the resulting polymer tube. Additional components can be incorporated into the final tube at various stages of the production methods outlined herein (e.g., between films that are subsequently encapsulated by tie layer(s) before or during the forming process), including, but not limited to, braids, fibers, wovens, nonwovens, and / or inserts. In some embodiments, the oriented polymer tubes provided via the methods disclosed herein can be further modified (e.g., by laser cutting, crimping, expansion, etc.) in subsequent steps to produce a medical device.
[0085] Multilayer annular orientation and annular positioning Another aspect of the present disclosure relates to a method involving multi-layer annular orientation and annular positioning, and the oriented polymer tube produced thereby. As mentioned above, one disadvantage of the annular expansion process is that the degree of orientation throughout the final tube wall thickness is limited, which results in a reduced orientation gradient from ID to OD. This concern can be addressed by utilizing an annular orientation approach, which minimizes wall thickness because the limit to the degree of orientation that can be achieved approaches zero as the wall thickness approaches zero. Thus, a multi-layer tube formed from an annularly oriented tube precursor, where the wall thickness of the precursor is additive in forming the wall thickness of the final formed oriented polymer tube, will show a higher degree of orientation throughout the tube wall thickness, and a reduced orientation gradient from ID to OD of the final formed polymer tube.
[0086] In this multi-layer annular orientation and annular positioning approach, multiple polymer tubes (which may be of the same or different compositions) are prepared and subjected to annular expansion, thereby generating an oriented tube precursor having at least some degree of molecular orientation, as shown in FIG. 5A (steps 14 or 18). Such polymer tubes can be made by any method, for example, via extrusion, extrusion coating, and / or injection molding. In one embodiment, the individual oriented tube precursors are positioned in a nested manner, as shown in step 16. In another embodiment, the oriented tube precursors are positioned in a nested manner, as shown in step 20, and then (simultaneously) subjected to additional annular expansion, as shown in step 22. Positioning the oriented tube precursors in such an embodiment is completed via the annular expansion step. The formation of the final tubular geometry (obtaining an oriented multi-layer polymer tube) can be completed via the annular expansion step or after the annular expansion step.
[0087] In another embodiment, the annular expansion of the polymer tubes can be performed one after the other in sequence, as shown in FIG. 5B. Following the annular expansion of the first tube (constituting the outer oriented tube precursor), the annular expansion of each subsequent tube positions the additional oriented tube precursor within the ID of the previous oriented tube precursor, resulting in annular positioning of all oriented tube precursors. The formation of the final tubular geometry (obtaining an oriented multi-layered polymer tube) can be completed via the annular expansion of one or more tube precursors or after the annular expansion of one or more tube precursors. The annular expansion of any of these embodiments can be performed by any known method for annularly expanding a tube.
[0088] Combining multiple unstretched / unoriented polymer tube precursors or stretched / oriented tube precursors using this method can be accomplished in a variety of ways, such as by forming an oriented polymer tube on a mandrel (optionally with heat and / or pressure) or by forming an oriented polymer tube into a mold (again, optionally with heat and / or pressure). It is noted that such forming mandrels and molds need not be circular in cross section, and thus the resulting multi-layered oriented polymer tubes may be in the form of hollow elongated structures that may, but are not limited to, be circular in cross section.
[0089] With the method of multi-layer annular orientation and annular positioning, in order to encapsulate the multiple individual layers, the tie layer is typically again incorporated between adjacent layers to provide sufficient adhesion therebetween. In these embodiments, the encapsulation of the tie layer can be achieved, for example, by associating the tie layer material with one or more polymer tube precursors (to provide a composite polymer tube precursor), so that when the polymer tube precursor is expanded / oriented and combined with other precursors (or combined with other precursors and then expanded / oriented), the tie layer is likewise subjected to such a process as well. Thus, in some embodiments, the tie layer is likewise subjected to annular expansion / orientation. In other embodiments, the tie layer is applied after the individual polymer tubes are expanded / oriented, and in such embodiments, the tie layer is not subjected to annular expansion / orientation. Again, forming the final oriented polymer tube by joining adjacent layers (resulting from combining multiple tube precursors or multiple individually expanded or oriented tubes) may require treating the final oriented polymer tube by exposing the multi-layer oriented polymer tube to heat and / or pressure. In some embodiments, the heat and pressure are provided by wrapping the oriented polymer tube with shrink tubing or shrink wrap and heating, for example, by placing the wrapped oriented polymer tube in an oven. The oven temperature and forming pressure applied can each be controlled to tailor the final tube properties.
[0090] Thus, in certain embodiments (e.g., as illustrated by steps 16 and 22 in FIG. 5A), at least two oriented tubes (each of which may include one crystalline polymer layer and optionally one tie layer (to obtain a composite oriented tube)) are positioned relative to all three cylindrical axes according to a desired orientation profile. The positioned tubes are exposed to increased pressure and / or temperature such that the tie layers adhere to adjacent layers (i.e., oriented polymer layers on either side of them), thereby forming a coherent multi-layer oriented polymer tube. In some embodiments, the stretched and oriented composite tube is positioned relative to an external and / or internal expanded / oriented tube comprising crystalline polymer (which may or may not include a tie layer).
[0091] In some embodiments (e.g., as illustrated in FIG. 5B), the unoriented composite tube (containing both the crystalline polymer and the tie layer material) is cyclically expanded (e.g., under conditions of high temperature and pressure) to orient at least a portion of the crystalline polymer. Through this cyclic expansion process, the tie layer material can, in some embodiments, be attached to any adjacent layer. For example, in this embodiment, one adjacent layer is the same unoriented crystalline polymer of the composite tube precursor. Another adjacent layer can be an already oriented tube of a second crystalline polymer (which may be the same or different from the crystalline polymer in the composite tube precursor), thereby forming a coherent multi-layer oriented polymer tube. In such an embodiment, the individual layers are positioned with respect to all three cylindrical axes according to a desired orientation profile. The composite tube precursor can also be positioned with respect to an inner tube precursor containing a crystalline polymer.
[0092] There are many methods known in the art for annularly expanding a polymer tube as described above. In conventional blow molding, the extruded polymer tube is placed in a mold, heated to a rubbery state, and pressure is applied to expand the tube into the mold. In some methods, the extruded polymer tube is also longitudinally stretched by applying tension. The longitudinal stretching is completed before or during the annular expansion. The geometry of the final expanded tube is generally determined by the geometry of the mold and process parameters such as temperature and pressure. The properties of the final expanded tube are generally determined by process parameters such as annular expansion ratio, annular expansion rate, longitudinal stretch ratio, longitudinal stretch rate, temperature, and pressure.
[0093] The multi-layer annular orientation and annular positioning methods disclosed herein provide many advantages over conventional extrusion / annular extrusion. For example, each tube precursor can be uniaxially or biaxially oriented to a desired degree as desired before or during the formation of the multi-layer oriented polymer tube to meet application requirements. Multiple polymers can be combined as individual layers in a composite structure in some embodiments and expanded / oriented together. In some embodiments, multiple polymers can be provided independently in tube form and expanded (and thus oriented) to, for example, different degrees, and then the resulting oriented tubes can be combined during positioning and formation of the multi-layer oriented polymer tube. In some embodiments, the individual tubes and tube precursors can be selected for very specific properties, such as strength, toughness, drug encapsulation / elution, adhesion, surface functionality, degradability, etc., to impart such properties to the resulting multi-layer polymer tube. Additional components, such as fillers, can be dispersed in one or more of the tube precursors prior to expansion. Additional components can be incorporated into the final multi-layer polymer tube at various stages of the production methods outlined herein (e.g., between tube layers that are subsequently encapsulated by tie layer(s) material), including, but not limited to, braids, fibers, wovens, non-wovens, and / or inserts. In some embodiments, the multi-layer polymer tubes provided via the methods disclosed herein can be further modified (i.e., by laser cutting, crimping, expansion, etc.) in subsequent steps to produce a medical device.
[0094] Using a cylindrical coordinate system and assuming that the two surfaces in full contact are geometrically continuous, such a tube (formed from the precursor annular geometry) would be geometrically continuous along all three axes. With respect to imposing molecular orientation and geometric continuity, such a tube would be continuous along the z and θ axes, but not along the r axis.
[0095] The method of producing an oriented polymer tube disclosed herein is applicable to a wide range of crystalline polymers. Such methods are particularly applicable, but not limited to, biodegradable polymers. Thus, in a preferred embodiment, the polymer(s) from which an oriented polymer tube is prepared according to the present disclosure are advantageously crystalline biodegradable polymers and can advantageously exhibit high molecular orientation, strain-induced crystallization, and high strength.
[0096] Biodegradable (also commonly referred to as "bioresorbable" and / or "bioresorbable") polymers are those polymers that, under certain biological conditions, undergo degradation or transformation into compounds that are considered harmless / safe as part of normal biological processes. Advantageously, under the biological conditions to which they are exposed, biodegradable polymers gradually degrade and / or erode and are absorbed or resorbed within the body. Typically, applicable biodegradable polymers in the context of the present disclosure are sufficiently stable under biological conditions to remain within the body for a period of time (e.g., including but not limited to, up to about 1 week, up to about 1 month, up to about 3 months, up to about 6 months, up to about 12 months, up to about 18 months, up to about 2 years, or longer) before substantial degradation. Typically, such biodegradable polymers are also biocompatible.
[0097] Exemplary applicable crystalline polymers in the context of the present invention include, but are not limited to, poly(L-lactide) (PLLA), poly(D-lactide) (PDLA), poly(ε-caprolactone) (PCL), polyglycolic acid (PGA), poly(para-dioxanone) (PDO), poly(hydroxybutyrate), poly(hydroxyvalerate), poly(tetramethylcarbonate), poly(ethylene oxide) (PEO), poly(ethylene glycol) (PEG), poly(propylene glycol), polydioxanone, polygluconate, and copolymers, blends, and derivatives thereof. Certain polymers that can be used according to the disclosed methods can be characterized as poly(α-hydroxy acids). Some polymers are modified cellulosic polymers, collagen or other binding proteins, adhesive proteins, hyaluronic acid, polyanhydrides, polyphosphoesters, poly(amino acids), and copolymers, and derivatives thereof. The molecular weight of the polymer processed according to the methods outlined herein can be varied and may affect the properties of the resulting oriented polymer tube. It is generally understood that the mechanical properties (e.g., strength and modulus) of the polymer generally improve as the molecular weight increases, and that the degradation time generally increases as the molecular weight increases (i.e., a tube made with a low molecular weight polymer typically deteriorates faster than a comparable tube made with a higher molecular weight polymer). Thus, the molecular weight of the polymer can be appropriately selected to balance these properties and may vary widely depending on the particular application.
[0098] As noted above, the oriented polymer tubes disclosed herein generally include, in addition to the oriented crystalline polymer, one or more tie layer materials (also referred to herein as "adhesive" layer materials) sufficient to bond the layers together. Such layers can include multiple layers of the same material (e.g., in the case of a multi-layer material produced by rolling) and / or layers of different materials. Advantageously, in some embodiments, the tie layer bonds adjacent layers together such that the oriented polymer tube exhibits little or no delamination during use (e.g., the adhesion between the layers allows the oriented polymer tube to undergo at least partial degradation without exhibiting significant delamination).
[0099] The composition of the tie layer in the final oriented polymer tube can vary. The tie layer typically comprises one or more polymers capable of bonding together two adjacent layers, and therefore a variety of polymers with adhesive properties may be used. Typical adhesive polymers for use as tie layers exhibit some degree of flowability and / or tackiness. The polymer(s) comprising the tie layer are preferably biocompatible biodegradable polymers in some embodiments (e.g., when the final product is designed for implantation within the body). The polymer(s) comprising the tie layer are, in some embodiments, amorphous / essentially amorphous polymers. Exemplary polymers suitable for serving as (or being included within) a tie layer in accordance with the present disclosure include, but are not limited to, poly(ε-caprolactone), poly(trimethylene carbonate), poly(D,L-lactide), poly(L-lactide)-co-ε-caprolactone), poly(L-lactide-co-trimethylene carbonate, poly(ε-caprolactone-co-trimethylene carbonate), poly(ethylene glycol), poly(L-lactide-co-poly(ethylene glycol), and copolymers, and derivatives, and combinations thereof.
[0100] The properties of the tubes produced by the above methods can be varied. For example, the geometric and orientational continuity of oriented polymer tubes prepared by various methods are compared in Table 1 below.
[0101] [Table 1]
[0102] The shape and size of the oriented polymer tubes produced according to the disclosed methods can be varied. As mentioned herein above, such tubes are cylindrical, but not limited thereto. The wall thickness of the oriented polymer tubes can be varied as well, and can be adjusted based on, for example, the thickness of the polymer film (or profile) (for planar orientation and annular positioning methods), the thickness of the tube / tube precursor (for multi-layer annular orientation and annular positioning methods), the amount of elongational force applied thereto, and the number of layers combined to produce the final oriented polymer tube (e.g., the number of turns, or the number of tube precursors or tubes combined to produce a multi-layer tube). The oriented polymer tubes provided according to the present disclosure can be essentially homogeneous in composition (e.g., consisting primarily of a single oriented crystalline polymer component), where multiple layers thereof may be bonded together with a relatively small amount of tie layer material (forming an adhesive / tie layer between adjacent layers of oriented polymer). The specific oriented polymer tubes provided according to the present disclosure can also be non-homogeneous, as the films / profiles / tubes can be combined and compositionally different. (For example, the tubes may comprise different crystalline polymers and / or different tie layer materials (which may be in oriented or unoriented form), may include / exclude fillers or other ingredients, etc.) The methods outlined herein are broadly applicable to the preparation of a wide range of oriented polymer tubes.
[0103] In some embodiments, the oriented polymer tubes prepared according to the disclosed methods can be characterized by the degree of molecular orientation of the crystalline polymer across the cross-section of the tube (i.e., from the ID to the OD of the tube). Preferably, the molecular orientation of the crystalline polymer within the tube wall is essentially invariant across the cross-section of the oriented polymer tube. For example, the molecular orientation is generally in the same direction, with approximately the same amount near the ID of an oriented polymer tube according to the present disclosure as near the OD. Such orientation characteristics can be evaluated, for example, using X-ray diffraction.
[0104] In particular, the molecular orientation profile of certain embodiments is essentially consistent through the wall of the oriented polymer tube or is essentially consistent through a predefined portion of the wall of the oriented polymer tube. In some embodiments, the tube has a molecular orientation profile characterized by varying levels of orientation through a predefined portion of the wall of the oriented polymer tube and / or varying axes of orientation through a predefined portion of the wall of the oriented polymer tube. Some tubes provided herein exhibit other profiles, such as a gradient of molecular orientation that increases through the wall from the inner diameter to the outer diameter of the oriented polymer tube, or a gradient of molecular orientation that decreases through the wall from the inner diameter to the outer diameter of the oriented polymer tube. In some embodiments, the molecular orientation profile is essentially consistent along the length of the oriented polymer tube or it is essentially consistent along a predefined portion of the length of the oriented polymer tube. In some embodiments, the tube has a molecular orientation profile characterized by varying levels of orientation along the length of the oriented polymer tube and / or varying axes of orientation along the length of the oriented polymer tube.
[0105] The composition profile of an oriented polymer tube as provided herein, in certain embodiments, is essentially consistent through the wall of the oriented polymer tube, or is essentially consistent through a predefined portion of the wall of the oriented polymer tube. In other embodiments, the composition profile can be characterized by a variation in composition through a predefined portion of the wall of the oriented polymer tube. Similarly, the composition profile of an oriented polymer tube as provided herein, in certain embodiments, is essentially consistent along the length of the oriented polymer tube, or is essentially consistent along the length of the oriented polymer tube. In other embodiments, the composition profile can be characterized by a variation in composition along the length of the oriented polymer tube.
[0106] In certain embodiments, the degradation rate profile may also be influenced by the specific method used to form the oriented polymer tube. For example, oriented polymer tubes are provided herein that are characterized by a degradation rate profile that is essentially consistent through the wall of the oriented polymer tube, or that is essentially consistent through a predefined portion of the wall of the polymer tube, or that is characterized by a degradation rate profile that is varied through a predefined portion of the wall of the oriented polymer tube, including a degradation rate profile that is characterized by a gradient of degradation rate that increases through the wall from the inner diameter to the outer diameter of the oriented polymer tube, and a degradation rate profile that is characterized by a gradient of degradation rate that decreases through the wall from the inner diameter to the outer diameter of the oriented polymer tube. In some embodiments, oriented polymer tubes are provided herein that are characterized by a degradation rate profile that is essentially consistent through the length of the oriented polymer tube, or that is essentially consistent along the length of the oriented polymer tube, or that is characterized by a degradation rate profile that is characterized by a gradient of degradation rate along the length of the oriented polymer tube.
[0107] Advantageously, the oriented polymer tubes provided according to the present disclosure can exhibit sufficient strength for use in vivo, for example. Such tubes can be characterized as having sufficient compressive strength / resistance to radial compression to function in desired situations. For example, in some embodiments, the oriented polymer tubes provided according to the disclosed methods may find use, for example, as stents, or components of stents. Stents, for example, are exposed to large loads when inserted and left in a blood vessel, and should exert sufficient radial force to ensure that the stent remains at the narrowed point and prevents constriction of the blood vessel. Oriented polymer tubes prepared according to the aforementioned methods have been tested (e.g., to evaluate repeated compression), and the relevant findings of this testing are described herein below. Certain oriented polymer tubes prepared according to the planar orientation / annular positioning method have demonstrated higher energy absorption (normalized to wall thickness) than comparative materials (prepared by conventional extrusion / expansion methods as described herein). All of the oriented polymer tubes tested, prepared according to the planar orientation / annular positioning method, exhibited improved hysteretic behavior as measured by the x-intercept at the beginning of each cycling period.
[0108] It has also been found that various parameters of the disclosed methods (and properties of the disclosed materials) lead to differences in the physical properties of the resulting oriented polymer tubes, allowing for flexible processing. For example, the physical properties of the oriented polymer tubes may be modified according to the present disclosure, for example, by selecting polymers (including, for example, copolymers) with different molecular weights and / or compositions, modifying the orientation style of the film (e.g., uniaxial vs. biaxial) in the planar orientation / annular positioning method, wrapping the polymer film / profile at different angles (e.g., axially or at a bias angle) around the forming mandrel, utilizing different polymer films / profiles wrapped together on the mandrel, wrapping such polymer films / profiles in different ways (e.g., staggered vs. stacked), etc. In some embodiments, the disclosed methods include arranging a plurality of units of stretched polymeric material (e.g., stretched films / profiles, etc.) in at least one of a stacked and staggered manner, and wrapping the arranged plurality of units of stretched polymeric material at a bias angle, where the bias angle can be varied (including 0°).
[0109] The end use of the tubes provided according to the present disclosure can vary. As referenced herein, the molecular orientation imparted by the disclosed methods can advantageously provide tubes of relatively high strength (e.g., radial / compressive strength), making these tubes particularly useful where such high strength is important. One such use is in the context of medical implants, such as stents. The size of the stents provided according to certain embodiments of the disclosed methods can vary and can be designed for one or more specific uses. For example, in some embodiments, the length L of the stent can be from about 20 mm to about 200 mm. For example, for some uses, the stent can have a length L of about 40 mm to 100 mm, or any value between, for example, at least about 50 mm, 60 mm, 70 mm, 80 mm, or 90 mm. In some uses, the stent can have a length L of about 25 mm to 150 mm, or any value between, for example, at least about 50 mm, 75 mm, 100 mm, or 125 mm. In other stent applications, the stent may also be longer or shorter than these exemplary values. Similarly, in some embodiments, the strut thickness of the stent may be from about 0.7 mm to about 0.4 mm. For example, for some applications, the stent may have a strut thickness of about 0.08 mm to 0.15 mm, or any value between, for example, at least about 0.09 mm, 0.1 mm, 0.12 mm, 0.13 mm, or 0.14 mm. In some applications, the stent may have a strut thickness of about 0.15 mm to 0.4 mm, or any value between, for example, at least about 0.2 mm, 0.25 mm, 0.3 mm, or 0.35 mm. The stent may also have a strut thickness higher or lower than these exemplary values for other stent applications. Similarly, the stent may be formed in a variety of diameters.In some embodiments, the central diameter of the stent (the diameter of the stent at a point equidistant from each end) may be a central inner diameter of about 1.5 mm to about 40 mm, e.g., about 2.5 mm to 16 mm, or any distance within this range, e.g., between about 3 mm and 14 mm, or between about 5 mm and about 10 mm.
[0110] Stents are cylindrically shaped devices that are often used in the treatment of arterial disease. Arterial disease involves the deposition of lipids within arteries and subsequent plaque formation along the arterial wall. These plaque lesions may be soft or may harden and calcify, reducing the luminal space within the blood vessel over time, a process known as stenosis. To treat stenosis, stents are generally placed at the treatment site and help maintain luminal patency in the diseased portion of the blood vessel. Stents must have adequate radial strength to provide adequate radial support to the blood vessel to maintain vascular patency.
[0111] Stents are generally manufactured by laser cutting a tube into a radially expandable geometry that includes interconnected structural elements or struts. During conventional deployment, similar to angioplasty balloon catheters, the struts of the stent undergo high local deformation, requiring the material to be manufactured so that the stent is highly deformable while maintaining high strength and stiffness (e.g., the material must exhibit high toughness). In many clinical treatment applications, stents are only needed temporarily, for example, to maintain patency during a critical treatment phase or to deliver an active agent or drug to a target site.
[0112] Thus, the tubes described herein may find particular use as stents, since they, in various embodiments, exhibit high compressive / radial strength as well as biodegradability / bioabsorbability. The ability to tailor the composition and physical properties of the layers that comprise each tube, as disclosed herein, allows for the production of tubes that exhibit sufficient compressive / radial strength as well as biodegradability, e.g., that can be completely absorbed after their clinical usefulness has expired. The tubes disclosed herein can be appropriately processed / modified in this regard to serve the desired purpose, e.g., by cutting into appropriate sizes / geometry.
[0113] In other embodiments, the tubes provided according to the present disclosure can be used in other contexts, including, for example, but not limited to, serving as heat shrink tubing disposed around other tubes / tubular constructs to, for example, aid in fusing components of such tubular constructs. In some embodiments, such heat shrink tubing prepared according to the disclosed methods exhibits enhanced thermodynamic properties, including, but not limited to, improved heat shrink functionality.
[0114] Although the present disclosure focuses on embodiments that include at least one crystalline (e.g., crystalline and biodegradable) polymer, it should be noted that the principles described herein are not so limited. Although the techniques outlined herein are advantageously applied in the context of such crystalline polymers to orient the molecules to enhance the strength of the resulting tubular morphology in that context, these principles can provide other benefits as well, which are not limited to crystalline polymers (and may be applicable to amorphous macromolecules, including, for example, but not limited to, biodegradable amorphous polymers). Thus, in some embodiments, the present disclosure provides methods for subjecting polymeric materials, including amorphous biodegradable polymers, to planar stretching and annular orientation, or to multilayer annular expansion and annular positioning, generally as disclosed herein. Typically, products containing such amorphous polymers do not exhibit the high strength values discussed herein above relative to products containing crystalline polymers (e.g., reinforced by molecular orientation) and therefore may also find use, for example, in fabricating other tubes (including, for example, but not limited to, serving as heat shrink materials for fusing other multi-layer tubes as discussed above) and as components of various devices where they are reinforced, for example, by one or more additional components.
[0115] Many modifications and other embodiments of the invention will come to mind to one skilled in the art to which this invention pertains having the benefit of the teachings presented in the foregoing description. It is to be understood, therefore, that the invention is not limited to the specific embodiments disclosed, and that modifications and other embodiments are intended to be included within the scope of the appended claims. Although specific terms are employed herein, they are used in a generic and descriptive sense only and not for purposes of limitation. EXAMPLES
[0116] Plaques made of PL32, a polylactide resin purchased from Corbion Purac, were made by compression molding to a thickness of 125 μm using a Carver Press. The PL32 plaques were then uniaxially stretched in a Bruckner Lab Stretcher to a final thickness of approximately 25 μm. Plaques made of PLC 7015, a copolymer resin of lactide and caprolactone obtained from Corbion Purac, were made by compression molding to a thickness of approximately 40 μm using a Carver Press. The PLC7015 plaques were then biaxially stretched in a Bruckner Lab Stretcher to a final thickness of approximately 15 μm.
[0117] Rectangles were cut from each of the two films, placed one on top of the other, and wrapped around a metal mandrel with OD=2.8 mm, with the PL32 film in contact with the mandrel. The film was wrapped such that the stretch direction of the PL32 film was aligned in the circumferential direction. The wrapped mandrel was then tightly covered with a linear low density polyethylene (LLDPE) film, Cortuff® shrink film, obtained from Sealed Air Corporation, and taped in place. The assembly was then placed in a circulating hot air oven set at 80° C. for 30 minutes. After removing the assembly from the oven, the shrink film was removed, and the now fused composite tube was removed from the mandrel. The final average wall thickness of the composite tube was approximately 130 μm. EXAMPLES
[0118] The procedure of Example 1 was repeated starting with a 125 μm plaque made from PL65 polylactide purchased from Corbion Purac, uniaxially stretched to a final thickness of approximately 30 μm, and a 40 μm plaque made from PLC 7015, biaxially stretched to a final thickness of approximately 15 μm. The pressure-formed tube had a wall thickness of approximately 140 μm. EXAMPLES
[0119] The procedure of Example 1 was repeated using an oven temperature of 120°C. EXAMPLES
[0120] The procedure of Example 2 was repeated using an oven temperature of 120°C. EXAMPLES
[0121] The procedure of Example 1 was repeated using an oven temperature of 160°C. EXAMPLES
[0122] The procedure of Example 2 was repeated using an oven temperature of 160°C. EXAMPLES
[0123] The procedure of Example 1 was repeated using an oven temperature of 180°C. EXAMPLES
[0124] The procedure of Example 2 was repeated using an oven temperature of 180°C.
[0125] Repeated compression test The composite tubes of Examples 1-8 were tested in compression on an Instron testing machine equipped with a 10 lb load cell. The tube was positioned so that its length axis was perpendicular to the movement of the jaws. During the test, a disk clamped to the jaws was lowered onto the tube surface. The tube was compressed at 50% of its initial diameter per minute until it deformed to 50% of its initial diameter, after which the jaws returned to their starting position at the same rate. The force required to compress the sample was measured by the load cell and converted to stress. The procedure was repeated five times per tube without dwelling between cycles. Values reported were the maximum stress, the energy absorbed by the tube over five cycles normalized to the wall thickness, and the recovery of the tube as a percentage of the extent of compression. This last quantity is an indication of the history between compression cycles for the tube.
[0126] Figures 6A, 6B, and 6C show the maximum stress, normalized energy, and X-intercept of cyclic compression tests for tubes of Examples 3 and 4 compared to a control tube. The control tube was fabricated by extruding and expanding an input tube made of PL38 PLLA from Corbion Purac to a final dimension of 2.8 mm ID with a wall thickness of 100 μm. The tube was then annealed at 120°C for 30 minutes to match the pressure building time of the composite tubes of Examples 3 and 4. From Figures 6A, 6B, and 6C, the tube of Example 4 shows a clear advantage over the control tube in the maximum stress, normalized energy, and history between cycles for all compression cycles. The tube of Example 3 has a lower maximum stress value but improved normalized energy and history between cycles.
[0127] 7A, 7B, and 7C show the maximum stress, normalized energy, and X-intercept of cyclic compression tests for the tubes of Examples 1, 3, 5, and 7. The effect of forming temperature on these properties is readily apparent. For the PL32 / PLC7015 composite structures disclosed in the examples, the optimal forming temperature for maximizing maximum stress and energy is 160° C.
[0128] 8A, 8B, 8C show the maximum stress, normalized energy, and X-intercept of cyclic compression tests for the tubes of Examples 2, 4, 6, and 8. For the PL65 / PLC7015 composite structures disclosed in the examples, the optimal forming temperature for maximizing the maximum stress and energy is 120° C. EXAMPLES
[0129] The procedure of Example 3 was repeated starting with a 125 μm plaque made from PL32, biaxially stretched to a final thickness of about 10 μm, and a 40 μm plaque made from PLC 7015, biaxially stretched to a final thickness of approximately 15 μm. The average wall thickness of the finished composite tube was approximately 120 μm. EXAMPLES
[0130] The procedure of Example 3 was repeated starting with a 125 μm plaque made from PL32, biaxially stretched to a final thickness of about 10 μm, and a 125 μm plaque made from PLC8516, a polylactide-co-caprolactone copolymer purchased from Corbion Purac, biaxially stretched to a final thickness of about 7 μm. The average wall thickness of the finished composite tube was approximately 50 μm. EXAMPLES
[0131] The procedure of Example 4 was repeated starting with a 125 μm plaque made from PLC8516, uniaxially stretched to a final thickness of about 25 μm, and a 125 μm plaque made from PLC8516, a polylactide-co-caprolactone copolymer purchased from Corbion Purac, biaxially stretched to a final thickness of about 7 μm. The average wall thickness of the finished composite tube was approximately 95 μm. EXAMPLES
[0132] The procedure of Example 3 was repeated using a 125 μm plaque made from PLC8516, biaxially stretched to a final thickness of about 7 μm, and a 45 μm plaque made from PC12, a polycaprolactone purchased from Corbion Purac, biaxially stretched to a final thickness of about 25 μm. The average wall thickness of the finished composite tube was approximately 100 μm. EXAMPLES
[0133] A 125 μm plaque made from PLC8516 was biaxially stretched to a final thickness of about 7 μm. Rectangles were cut from the film and wrapped around a metal mandrel with OD=2.8 mm. The wrapped mandrel was then tightly wrapped with LLDPE shrink film and taped in place. The assembly was then placed in a circulating hot air oven set at 120° C. for 30 minutes. After removing the assembly from the oven, the shrink film was removed and the now fused composite tube was removed from the mandrel. The final average wall thickness of the composite tube was approximately 90 μm. EXAMPLES
[0134] A plaque made of PL32 was cast to a thickness of 125 μm and biaxially stretched in a Bruckner Lab Stretcher to obtain a final thickness of approximately 15 μm. A plaque made of PLC7015 was cast to obtain a thickness of 40 μm, which was then biaxially stretched to result in a final thickness of approximately 15 μm. A 125 μm plaque made of PLC8516 was biaxially stretched to a final thickness of approximately 7 μm. Rectangles were cut from each of the films, stacked in the order PL32 / PLC7015 / PLC8516, and wrapped around a metal mandrel with OD=2.8 mm. The PL32 film was in contact with the mandrel. The wrapped mandrel was then tightly covered with LLDPE film and taped in place. The assembly was then placed in a circulating hot air oven set at 120° C. for 30 minutes. After the assembly was removed from the oven, the shrink film was removed and the now fused composite tube was removed from the mandrel The final average wall thickness of the composite tube was approximately 80 μm. EXAMPLES
[0135] A 30 μm wall, 2.8 mm ID extruded and expanded tube made from PL32 resin (PLA) was slid onto the mandrel, and the biaxially oriented PL32 film of Example 9 and the PLC7015 film were wrapped around the PLA tube, with the PLC7015 film in contact with the outer circumference of the PLA tube. The wrapped mandrel was then tightly wrapped with LLDPE film and taped in place. The assembly was then placed in a circulating hot air oven set at 120° C. for 30 minutes. After removing the assembly from the oven, the shrink film was removed, and the now fused composite tube was removed from the mandrel. The final average wall thickness of the composite tube was approximately 130 μm.
Claims
1. A multi-layer tube comprising at least one oriented polymeric material and at least one adhesive polymeric material, or at least one oriented polymeric material and at least one stretch adhesive polymeric material, The multi-layer tube has an orientation profile that is consistent through the wall of the multi-layer tube.
2. The multi-layer tube of claim 1 , wherein the at least one oriented polymeric material exhibits a controlled level of orientation.
3. The multilayer tube of claim 1, wherein the at least one oriented polymeric material comprises at least one crystalline biodegradable polymeric material.
4. A multi-layer tube having an exterior surface with a normal perpendicular to a length of the multi-layer tube, exhibiting a maximum stress value of 20 MPa or more measured based on a first compression cycle; being deformed by at least 17% of the first dimension after the first compression cycle; The multi-layer tube according to claim 1 .
5. The multi-layer tube of claim 4, wherein the maximum stress value is measured based on the first compression cycle in a direction perpendicular to the length of the multi-layer tube, and the first compression cycle is repeated five times per tube without stopping between compression cycles.
6. The first compression cycle comprises: obtaining an initial distance between two parallel plates between which the multi-layer tube is disposed, the two parallel plates contacting an outer surface of the multi-layer tube such that the two parallel plates provide essentially no load on the multi-layer tube; compressing the plates to a distance of 50% of the initial distance of the two parallel plates at a rate of 50% of the initial distance per minute, deforming the multi-layer tube in a first direction, the first direction being the direction in which the plates are compressed; releasing the compression of the plates against the multi-layer tube at a rate of 50% of the initial distance between the two parallel plates per minute; The multi-layer tube of claim 4 comprising:
7. 5. The multi-layer tube of claim 4, wherein a total energy value under an engineering stress-strain curve corresponding to said multi-layer tube after said first compression is at least 138 kgf·mm / cm.
8. The multi-layer tube of claim 4 , wherein the multi-layer tube has one or more of a therapeutic agent, a cover, and a coating applied thereto.
9. the multi-layer tube having an exterior surface with a normal perpendicular to the length of the tube; exhibiting a maximum stress value of 20 MPa or greater as measured on a first compression cycle; 5. The multi-layer tube of claim 4, wherein the total energy value under the engineering stress-strain curve corresponding to the tube after the first compression is at least 138 kgf·mm / cm.
10. A stent comprising the multi-layer tube of claim 1.
11. 2. The multi-layer tube of claim 1, wherein the average wall thickness is less than or equal to 50 μm.
12. 2. The multi-layer tube of claim 1, wherein the average wall thickness is less than or equal to 100 μm.
13. 2. The multi-layer tube of claim 1, wherein the average wall thickness is less than or equal to 85 μm.
14. 2. The multi-layer tube of claim 1, wherein the average wall thickness is less than or equal to 130 μm.
15. 2. The multi-layer tube of claim 1, wherein the inner diameter is less than 3 mm.
16. 10. The multi-layer tube of claim 1, wherein the multi-layer tube is between 40 mm and 100 mm in length.
17. 10. The multi-layer tube of claim 1, wherein the multi-layer tube is between 20 mm and 200 mm in length.
Citation Information
Patent Citations
Thermal curing of medical tubing
JP1999510446A
Biological duct stent
JP2002200175A
low profile absorbable stent
JP2007515249A
Method for manufacturing a tube for use in forming a stent and such tube
JP2015530157A
Polymer scaffold with enhanced axial fatigue properties
JP2016514007A