Circular polarizing plate, organic electroluminescence display device, display device

The circularly polarizing plate addresses color unevenness in oblique views by using a retardation film with controlled water content and optimized lamination, achieving stable performance in curved and high aspect ratio displays.

JP7583051B2Active Publication Date: 2024-11-13FUJIFILM CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022545667
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-10
Filing Date
2021-08-25
Publication Date
2024-11-13
Estimated Expiration
2041-08-25

AI Technical Summary

Technical Problem

Existing polarizing plates exhibit color unevenness when viewed from oblique directions, particularly in curved and high aspect ratio displays, due to the use of polymerizable liquid crystal compounds with reverse wavelength dispersion, leading to increased reflectance at certain azimuth angles.

Method used

A circularly polarizing plate is designed with a retardation film having a water content of 1.8% or less, laminated with an aluminum sheet, and optimized to maintain chromaticity and reflectance within specific ranges at various angles, incorporating a retardation film with optically anisotropic layers to suppress color unevenness.

Benefits of technology

The solution effectively reduces color unevenness in diagonal directions, ensuring stable performance over time in organic EL display devices, especially in curved and high aspect ratio displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583051000050
    Figure 0007583051000050
  • Figure 0007583051000051
    Figure 0007583051000051
  • Figure 0007583051000052
    Figure 0007583051000052
Patent Text Reader

Abstract

Provided is a circularly polarizing plate in which color unevenness in the oblique direction can be suppressed and color unevenness in the oblique direction is unlikely to occur over time in application to an organic EL display device (in particular, a curved display and an in-vehicle display having a high aspect ratio), and also provided are an organic electroluminescence display device and an optical device. The circularly polarizing plate according to the present invention includes a polarizing element and a retardation film laminated on one surface side of the polarizing element, wherein the water content of the retardation film is 1.8% or less; the circularly polarizing plate and an aluminum sheet are bonded together so that the retardation film in the circularly polarizing plate faces the aluminum sheet; where a chromaticity a* and a chromaticity b* are measured at all azimuth angles and a polar angle of 40° from the normal direction of the circularly polarizing plate of the obtained laminated body, the absolute value of the chromaticity a* and the absolute value of the chromaticity b* are 10 or less at any of the azimuth angles; and where a reflectance is measured at all azimuth angles and a polar angle of 40° from the normal direction of the circularly polarizing plate of the laminated body, the reflectance is 3.0% or less at any of the azimuth angles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a circular polarizing plate, an organic electroluminescent display device, and a display device. [Background technology]

[0002] In recent years, progress has been made in the development of polarizing plates (so-called broadband polarizing plates) that can provide the same effect for all wavelengths of light, including white light, which is a composite wave that contains a mixture of light rays in the visible light range. In particular, due to the demand for thinner devices in which polarizing plates are used, there is a demand for thinner retardation layers included in polarizing plates as well. In response to such demands, for example, Example 9 of Patent Document 1 discloses a retardation plate in which a polymerizable liquid crystal compound with reverse wavelength dispersion is used as a polymerizable compound used to form an optically anisotropic layer, and further in which different types of optically anisotropic layers exhibiting predetermined optical properties are laminated. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2018 / 216812 Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors have studied a polarizing plate having an optically anisotropic layer obtained by polymerizing a polymerizable liquid crystal composition containing a compound (polymerizable liquid crystal compound) described in Patent Document 1, and have confirmed that when a device to which this polarizing plate is applied is observed from an oblique direction, a color change occurs depending on the azimuth angle, in other words, color unevenness occurs (hereinafter, the occurrence of color unevenness when observed from an oblique direction and the azimuth angle is changed as described above will be simply described as "color unevenness occurs in an oblique direction"). In particular, when the polarizing plate is applied to a curved display or a high aspect ratio in-vehicle display, the above problem was noticeable. In addition, in consideration of long-term use of various devices, it is also required that color unevenness does not occur over time when observed from an oblique direction.

[0005] The present invention aims to provide a circular polarizing plate that, when applied to an organic EL display device (particularly, a curved display and a high aspect ratio in-vehicle display), can suppress color unevenness in an oblique direction and is unlikely to cause color unevenness in the oblique direction even over time. Another object of the present invention is to provide an organic electroluminescence display device and a display device. [Means for solving the problem]

[0006] The present inventors have found that the above problems can be solved by the following configuration.

[0007] (1) A circular polarizing plate including a polarizer and a retardation film laminated on one surface side of the polarizer, The moisture content of the retardation film is 1.8% or less, The circular polarizing plate and the aluminum sheet are laminated together so that the retardation film in the circular polarizing plate faces the aluminum sheet. The chromaticity a of the obtained laminate at all azimuth angles of 40° polar angle from the normal direction of the circular polarizing plate is * and chromaticity b * When measuring the chromaticity a * Absolute value and chromaticity b * The absolute value of is 10 or less, A circular polarizing plate having a reflectance of 3.0% or less at all azimuth angles when the reflectance is measured at a polar angle of 40° from the normal direction of the laminate circular polarizing plate. (2) The circularly polarizing plate according to (1), wherein the retardation film comprises an optically anisotropic layer (B) having fixed therein rod-like liquid crystal compounds which are twisted and aligned with the thickness direction as a helical axis. (3) The circularly polarizing plate according to (1) or (2), wherein the retardation film comprises a negative uniaxial optically anisotropic layer (A). (4) The circularly polarizing plate according to any one of (1) to (3), wherein the retardation film has a thickness of 30 μm or less. (5) The circularly polarizing plate according to any one of (1) to (4), wherein the retardation film is formed by laminating three optically anisotropic layers. (6) The circularly polarizing plate according to any one of (1) to (5), wherein the retardation film is formed by laminating three optically anisotropic layers each having an aligned liquid crystal compound fixed therein. (7) The polarizer is formed using a composition containing a polymerizable liquid crystal compound, The circularly polarizing plate according to any one of (1) to (6), wherein the polarizer has a thickness of 8 μm or less. (8) An organic electroluminescence display device having the circular polarizing plate according to any one of (1) to (7). (9) A display device having the circular polarizing plate according to any one of (1) to (7), A display device, in which a circular polarizing plate is disposed so as to follow a curved surface of the display device. Effect of the Invention

[0008] According to the present invention, it is possible to provide a circular polarizing plate that, when applied to an organic EL display device (e.g., a curved display and a high aspect ratio in-vehicle display), can suppress color unevenness in an oblique direction and is unlikely to cause color unevenness in the oblique direction over time. Moreover, according to the present invention, an organic electroluminescence display device and a display device can be provided. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating an example of an embodiment of a circularly polarizing plate of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view illustrating an example of an embodiment of a circularly polarizing plate of the present invention. [Diagram 3] FIG. 2 is a diagram for explaining the definitions of polar angles and azimuth angles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. In this specification, a numerical range expressed using "to" means a range including the numerical values ​​before and after "to" as the lower and upper limits. First, the terms used in this specification will be described.

[0011] The in-plane slow axis is defined at 550 nm unless otherwise specified.

[0012] In the present invention, Re(λ) and Rth(λ) respectively represent the in-plane retardation and the retardation in the thickness direction at a wavelength λ, which is set to 550 nm unless otherwise specified. In the present invention, Re(λ) and Rth(λ) are values ​​measured at a wavelength λ using an AxoScan (manufactured by Axometrics). By inputting the average refractive index ((nx+ny+nz) / 3) and the film thickness (d(μm)) into AxoScan, Slow axis direction (°) Re(λ)=R0(λ) Rth(λ)=((nx+ny) / 2-nz)×d is calculated. Note that R0(λ) is displayed as a numerical value calculated by AxoScan, but it means Re(λ).

[0013] In this specification, the refractive indices nx, ny, and nz are measured using an Abbe refractometer (NAR-4T, manufactured by Atago Co., Ltd.) and a sodium lamp (λ=589 nm) as a light source. In addition, when measuring wavelength dependency, it can be measured using a multi-wavelength Abbe refractometer DR-M2 (manufactured by Atago Co., Ltd.) in combination with an interference filter. In addition, values ​​from the Polymer Handbook (JOHN WILEY & SONS, INC.) and catalogs of various optical films can be used. The average refractive index values ​​of major optical films are shown below as examples: cellulose acylate (1.48), cycloolefin polymer (1.52), polycarbonate (1.59), polymethyl methacrylate (1.49), and polystyrene (1.59).

[0014] In this specification, "light" refers to actinic rays or radiation, such as the emission line spectrum of a mercury lamp, far ultraviolet rays represented by excimer lasers, extreme ultraviolet rays (EUV light: Extreme Ultraviolet), X-rays, ultraviolet rays, and electron beams (EB). Among these, ultraviolet light is preferable.

[0015] In this specification, "visible light" refers to light having a wavelength of 380 to 780 nm. In addition, in this specification, unless otherwise specified, the measurement wavelength is 550 nm. In this specification, the angular relationship (e.g., "perpendicular", "parallel", etc.) is assumed to include the range of error permitted in the technical field to which the present invention pertains. Specifically, this means that the angle is within a range of less than ±10° from the exact angle, and the error from the exact angle is preferably within a range of ±5° or less, and more preferably within a range of ±3° or less.

[0016] In this specification, the vertical alignment of rod-like liquid crystal compounds refers to a state in which the major axes of the rod-like liquid crystal compounds are aligned perpendicular to and in the same direction as the layer surface. Here, the term "vertical" does not necessarily mean strictly vertical, but means an orientation in which the inclination angle between the average molecular axis of the rod-like liquid crystal compound in the layer and the layer surface is 70° or more. In addition, the same orientation does not require the orientation to be strictly the same, but rather means that when the orientations of the slow axes are measured at any 20 positions, the maximum difference between the slow axis orientations at the 20 positions (the difference between the two slow axis orientations with the largest difference among the 20 slow axis orientations) is less than 10°.

[0017] In this specification, the vertical alignment of a discotic liquid crystal compound refers to a state in which the disc axis of the discotic liquid crystal compound is aligned perpendicular to and in the same direction as the layer surface. Here, the term "vertical" does not necessarily mean strictly vertical, but means an orientation in which the inclination angle between the discotic plane of the discotic liquid crystal compound in the layer and the layer surface is 70 to 90°. In addition, the same orientation does not require the orientation to be strictly the same, but rather means that when the orientations of the in-plane slow axes are measured at any 20 positions within the plane, the maximum difference between the in-plane slow axis orientations among the orientations of the in-plane slow axes at the 20 positions (the difference between the two in-plane slow axis orientations with the largest difference among the 20 in-plane slow axis orientations) is less than 10°.

[0018] In this specification, the optically anisotropic layer may be any layer that exhibits predetermined optical properties, and is preferably, for example, a layer in which the alignment state of aligned liquid crystal compounds is fixed. The "fixed" state is a state in which the alignment of the liquid crystal compound is maintained. Specifically, it is more preferable that the layer has no fluidity in a temperature range of usually 0 to 50° C., or under more severe conditions, −30 to 70° C., and that the alignment state is not changed by an external field or external force, and the fixed alignment state can be stably maintained.

[0019] <<Circular polarizing plate>> The circular polarizing plate of the present invention is characterized in that, when a laminate obtained by laminating the circular polarizing plate on an aluminum sheet is observed from a predetermined direction, the chromaticity a * , chromaticity b * and the reflectance is within a predetermined range. The polymerizable liquid crystal compound exhibiting reverse wavelength dispersion used in Patent Document 1 has excellent front reflection performance, but has a problem that the reflectance becomes high at a specific azimuth angle in an oblique direction, causing color unevenness in the oblique direction. In contrast, the circular polarizer of the present invention solves the above problem by using a retardation film that satisfies predetermined characteristics.

[0020] (One embodiment of the circular polarizing plate) As shown in Fig. 1, a circularly polarizing plate 10 according to an embodiment of the present invention includes a polarizer 3 and a retardation film 1. The retardation film 1 includes an optically anisotropic layer (A) 1a, an optically anisotropic layer (B) 1b, and an optically anisotropic layer (C) 1c, in this order. The polarizer 3 is disposed on the side of the retardation film 1 opposite to the optically anisotropic layer (C) 1c. The optically anisotropic layer (A) 1a is an optically anisotropic layer exhibiting negative uniaxiality, and will be described in detail later. The optically anisotropic layer (B) 1b is a layer in which rod-like liquid crystal compounds are fixed and twisted in a helical axis along the thickness direction, and will be described in detail later. The optically anisotropic layer (C) 1c is a layer in which vertically aligned rod-like liquid crystal compounds or horizontally aligned discotic liquid crystal compounds are fixed, and will be described in detail later.

[0021] (Different embodiment of circularly polarizing plate) 2, a circularly polarizing plate 20 according to another embodiment of the present invention includes a polarizer 3 and a retardation film 2. The retardation film 2 includes an optically anisotropic layer (A) 2a, an optically anisotropic layer (C) 2c, and an optically anisotropic layer (B) 2b, in this order. The polarizer 3 is disposed on the side of the retardation film 2 opposite to the optically anisotropic layer (B) 2b. The optically anisotropic layer (A) 2a is an optically anisotropic layer exhibiting negative uniaxiality, and will be described in detail later. The optically anisotropic layer (B) 2b is a layer in which rod-like liquid crystal compounds are fixed and twisted in a helical axis along the thickness direction, and will be described in detail later. The optically anisotropic layer (C) 2c is a layer in which vertically aligned rod-like liquid crystal compounds or horizontally aligned discotic liquid crystal compounds are fixed, and will be described in detail later.

[0022] The thickness of the circular polarizing plate is not particularly limited, but is preferably 80 μm or less, more preferably 60 μm or less, and even more preferably 40 μm or less. The lower limit of the thickness of the circular polarizing plate is not particularly limited, but is preferably 1 μm or more.

[0023] The circular polarizing plate and the aluminum sheet are laminated together so that the retardation film in the circular polarizing plate faces the aluminum sheet. The chromaticity a of the resulting laminate (hereinafter, also simply referred to as the "specific laminate") at all azimuth angles of a polar angle of 40° from the normal direction of the circular polarizing plate is * and chromaticity b * When measuring the chromaticity a * Absolute value and chromaticity b * The absolute value of is equal to or less than 10. The above characteristics will be explained with reference to the drawings. 3 shows a specific laminate 40 formed by laminating a circular polarizing plate 10 and an aluminum sheet 30. As shown in FIG. 3, the circular polarizing plate 10 is composed of a polarizer 3 and a retardation film 1, and is disposed so that the retardation film 1 faces the aluminum sheet 30.

[0024] Next, first, the polar angle and the azimuth angle will be described with reference to FIG. In FIG. 3, the plane (principal surface, perpendicular to the thickness direction) of the circular polarizer 10 is the xy plane, and the y-axis direction is the absorption axis of the polarizer 3. Therefore, in FIG. 3, the y-axis direction is the reference for an azimuth angle of 0°. As shown in FIG. 3, each θ between the vector v1 and the z-axis is defined as a polar angle (angle with respect to the normal direction of the circular polarizer 10), and the angle φ between the projection of the vector v1 onto the xy plane and the y-axis (absorption axis of the polarizer 3) is defined as an azimuth angle. In other words, the polar angle means the angle with respect to the normal direction of the circular polarizer 10. The azimuth angle refers to the angle with respect to the absorption axis of the polarizer 3. Therefore, a polar angle of 40° means an angle where θ in Fig. 3 is 40°. Also, for example, an azimuth angle of 45° means an angle where φ in Fig. 3 is 45°. In the present invention, when expressing an azimuth angle, a positive value is expressed in a counterclockwise direction based on the absorption axis direction of the polarizer 3 when viewed from the circular polarizing plate side of the specific laminate. Therefore, in Fig. 3, an azimuth angle of 45° means an orientation rotated 45° counterclockwise from the y-axis as a reference.

[0025] Chromaticity a at all azimuth angles (0 to 360°) of 40° polar angle from the normal direction of the circular polarizer in the specific laminate described above * When measuring the chromaticity a * The absolute value of chromaticity a at each azimuth angle position is 10 or less. In other words, when observed from the circular polarizing plate side of the specific laminate, the chromaticity a at each azimuth angle position is measured while changing the azimuth angle in the range of 0 to 360 degrees at a polar angle of 40 degrees from the normal direction of the circular polarizing plate in the specific laminate. * When measuring the chromaticity a * This means that the absolute values ​​of are all 10 or less. Above chromaticity a *In terms of the advantageous effects of the present invention, the absolute value of is preferably 9 or less, and more preferably 8 or less. There is no particular lower limit, but an example of the lower limit is 0.

[0026] In addition, the chromaticity b at all azimuth angles (0 to 360°) of 40° polar angle from the normal direction of the circular polarizer in the specific laminate described above is * When measuring the chromaticity b * The absolute value of chromaticity b at each azimuth angle position is 10 or less. In other words, when observed from the circular polarizing plate side of the specific laminate, the chromaticity b at each azimuth angle position is measured while changing the azimuth angle in the range of 0 to 360 degrees at a polar angle of 40 degrees from the normal direction of the circular polarizing plate in the specific laminate. * When measuring the chromaticity b * This means that the absolute values ​​of are all 10 or less. Chromaticity b above * In terms of the advantageous effects of the present invention, the absolute value of is preferably 9 or less, and more preferably 8 or less. There is no particular lower limit, but an example of the lower limit is 0.

[0027] Above chromaticity a * and chromaticity b * is the L standardized by the International Commission on Illumination (CIE). * a * b * In the color system, it represents chromaticity, which indicates hue and saturation. Above chromaticity a * and chromaticity b * The measurement method is to place a spectrophotometer (manufactured by Konica Minolta) at a specified position (specified polar angle, specified azimuth angle) on the circular polarizing plate side of a specific laminate and measure the chromaticity a * and chromaticity b * Examples of methods for measuring the above include:

[0028] Furthermore, when the reflectance of the specific laminate described above is measured at all azimuth angles (0 to 360°) at a polar angle of 40° from the normal direction of the circular polarizer, the reflectance is 3.0% or less at all azimuth angles. In other words, when observing from the circular polarizer side in the specific laminate, and measuring the reflectance at each azimuth angle while changing the azimuth angle in the range of 0 to 360° at a polar angle of 40° from the normal direction of the circular polarizer in the specific laminate, all of the obtained reflectances are 3.0% or less. The reflectance is preferably 2.5% or less, and more preferably 2.0% or less, in terms of obtaining a better effect of the present invention. The lower limit is not particularly limited, but may be 0%.

[0029] The method for measuring the reflectance is to place a detector at a polar angle of 40° from the normal direction of the circular polarizing plate of the specific laminate, and to allow incident light to enter from a direction of a polar angle of 40° at an azimuth angle that is 180° different from the azimuth angle at which the detector is placed, and to measure the reflectance with the detector. This procedure is carried out over an azimuth angle range of 0 to 360°, and the reflectance at each azimuth angle is measured. The reflectance mentioned above means a luminosity-corrected reflectance in the wavelength range of 400 to 750 nm, more specifically, a luminosity-corrected reflectance according to JIS Z 8701. In the above measurement, the reflectance is calculated based on the reflected light measured by the above procedure using a standard plate (white calibration plate CS-A5 manufactured by Konica Minolta) instead of the specific laminate.

[0030] The aluminum sheet used to form the laminate with the above-mentioned characteristics is a sheet having aluminum foil as the outermost layer, and may be composed of aluminum foil alone, or may be a laminate including a support and aluminum foil disposed on the support. When the aluminum sheet is a laminate including a support and an aluminum foil disposed on the support, the type of the support is not particularly limited, and examples thereof include a resin substrate. The reflectance of the aluminum sheet alone is preferably 80 to 90%.

[0031] <Polarizer> The polarizer may be any member capable of converting natural light into a specific linearly polarized light, and an example of the polarizer is an absorptive polarizer. The type of polarizer is not particularly limited, and any commonly used polarizer can be used, such as an iodine-based polarizer, a dye-based polarizer using a dichroic dye, and a polyene-based polarizer. Iodine-based polarizers and dye-based polarizers are generally produced by adsorbing iodine or a dichroic dye to polyvinyl alcohol and stretching it. A protective film may be disposed on one or both sides of the polarizer.

[0032] Furthermore, as described in WO2019 / 131943 and JP2017-083843A, a coating-type polarizer may be used that is prepared by coating a liquid crystal compound and a dichroic organic dye (for example, a dichroic azo dye used in the light-absorbing anisotropic film described in WO2017 / 195833A) without using polyvinyl alcohol as a binder as a polarizer. This coating type polarizer is a technology that utilizes the orientation of a liquid crystal compound to align a dichroic organic dye. As described in JP2012-083734A, it is preferable that the polymerizable liquid crystal compound exhibits smectic properties in terms of increasing the degree of orientation. Alternatively, as described in WO2018 / 186503A, it is also preferable to crystallize the dye in terms of increasing the degree of orientation. WO2019 / 131943A describes a structure of a polymer liquid crystal that is preferable for increasing the degree of orientation.

[0033] A polarizer in which a dichroic organic dye is oriented by utilizing the orientation of liquid crystals without stretching has the following characteristics: It has many advantages, such as the ability to make the film extremely thin, with a thickness of about 0.1 to 8 μm, the fact that cracks are unlikely to occur when the film is bent and thermal deformation is small, as described in JP 2019-194685 A, and the fact that the film has excellent durability even in polarizing plates with a high transmittance of over 50%, as described in JP 6483486 A. Taking advantage of these advantages, the polarizer can be applied to applications requiring high brightness, small size and light weight, fine optical systems, molding applications to curved surfaces, flexible applications, etc. Of course, when a polarizer is prepared on a support, it is also possible to transfer the polarizer onto a predetermined transfer target and peel off the support to use only the polarizer. Because of the above-mentioned characteristics, the circular polarizing plate of the present invention preferably uses a polarizer formed using a composition containing a polymerizable liquid crystal compound and having a thickness of 8 μm or less. More specifically, the composition preferably contains a polymerizable liquid crystal compound and a dichroic organic dye. The type of the polymerizable liquid crystal compound is not particularly limited, and examples thereof include polymerizable liquid crystal compounds (e.g., rod-shaped liquid crystal compounds having a polymerizable group) used when preparing a retardation film described later.

[0034] From the viewpoint of power saving, the transmittance (luminosity-corrected single transmittance) of the polarizer is preferably 40% or more, more preferably 44% or more, and even more preferably 50% or more.

[0035] <Retardation film> The moisture content of the retardation film in the circular polarizing plate of the present invention is 1.8% or less. If the moisture content of the retardation film is within the above range, the desired effect can be obtained. In particular, in terms of the superior effect of the present invention, it is preferably 1.5% or less, and more preferably 1.0% or less. The lower limit is not particularly limited, but is often 0% or more. The moisture content of the retardation film is a value measured after conditioning for 24 hours or more in an environment of a temperature of 25° C. and a relative humidity of 60%, and the moisture content is measured by the Karl Fischer method.

[0036] The configuration of the retardation film in the circular polarizing plate of the present invention is not particularly limited as long as the retardation film is a circular polarizing plate in which the above-mentioned chromaticity a*, chromaticity b* and reflectance satisfy the predetermined ranges. In particular, in terms of the superior effect of the present invention, it is preferable that the retardation film includes an optically anisotropic layer (corresponding to the optically anisotropic layer (B) shown in Figures 1 and 2) in which a rod-shaped liquid crystal compound is fixed and twisted and aligned with the thickness direction as the helical axis. In order to obtain a more excellent effect of the present invention, the retardation film preferably includes an optically anisotropic layer exhibiting negative uniaxiality (corresponding to the optically anisotropic layer (A) shown in FIGS. 1 and 2). In addition, in terms of obtaining a more excellent effect of the present invention, the retardation film is preferably a retardation film formed by laminating three optically anisotropic layers, and more preferably a retardation film formed by laminating three optically anisotropic layers in which an oriented liquid crystal compound is fixed. In particular, as shown in the above-mentioned FIGS. 1 and 2, the retardation film preferably includes three optically anisotropic layers: an optically anisotropic layer (A), an optically anisotropic layer (B), and an optically anisotropic layer (C). In the following, specific examples of the configurations of the optically anisotropic layers (A) to (C) will be mainly described.

[0037] In the retardation film, at least one of the optically anisotropic layer (A) and the optically anisotropic layer (B) is directly laminated to the optically anisotropic layer (C), and it is preferred that the optically anisotropic layer (C) contains a photoalignable polymer having a photoalignable group, and that the photoalignable polymer having a photoalignable group is present on the surface of the optically anisotropic layer (C) on the side in contact with the optically anisotropic layer (A) or the optically anisotropic layer (B). Here, the surface of the optically anisotropic layer (C) in contact with the optically anisotropic layer (A) or the optically anisotropic layer (B) refers to the surface region up to 20 nm in the thickness direction of the optically anisotropic layer (C) from the interface between the optically anisotropic layer (C) and the optically anisotropic layer (A) or the optically anisotropic layer (B), and hereinafter is also abbreviated as "surface layer C". The presence of the photoalignable polymer in the surface layer C of the optically anisotropic layer (C) can be confirmed, for example, by time-of-flight secondary ion mass spectrometry (TOF-SIMS). The TOF-SIMS method can be the method described in "Surface Analysis Techniques Selection: Secondary Ion Mass Spectroscopy" edited by the Japan Surface Science Society and published by Maruzen Co., Ltd. (1999). Specifically, when a photoalignable polymer having a photoalignable group is present on the surface of the optically anisotropic layer (C) that contacts the optically anisotropic layer (A) or the optically anisotropic layer (B), fragments derived from the photoalignable group will be detected near the interface between the optically anisotropic layer (C) and the optically anisotropic layer (A) or the optically anisotropic layer (B). The composition distribution in the thickness direction of the optically anisotropic layer (C) and the optically anisotropic layer (A) or the optically anisotropic layer (B) is analyzed by repeatedly irradiating an ion beam and measuring with TOF-SIMS from the air interface side of either of the optically anisotropic layers. Note that the ion beam irradiation and TOF-SIMS measurement are performed by first analyzing the components of a region from the surface to 1 to 2 nm in the thickness direction, and then digging further in the thickness direction by 1 to several hundreds of nm to analyze the components of the next surface region, and then repeating a series of operations. The distribution of the photoalignable polymer in the thickness direction of the optically anisotropic layer (C) is analyzed by measuring the secondary ion intensity derived from the unit having a photoalignable group. The type of ion beam includes, for example, an ion beam produced by an argon gas cluster ion gun (Ar-GCIB gun).

[0038] (Optical anisotropic layer (A)) The optically anisotropic layer (A) is an optically anisotropic layer exhibiting negative uniaxiality. The in-plane retardation of the optically anisotropic layer (A) at a wavelength of 550 nm is preferably from 140 to 220 nm, and more preferably from 150 to 200 nm in terms of better effects of the present invention.

[0039] The angle between the in-plane slow axis of the optically anisotropic layer (A) and the absorption axis of the polarizer is not particularly limited, but in terms of better effects of the present invention, in one preferred embodiment, the angle is preferably 40 to 100°, more preferably 50 to 85°, and even more preferably 65 to 85°. In another preferred embodiment, the angle is preferably 5 to 60°, more preferably 5 to 50°, and even more preferably 5 to 25°. In one embodiment when the optically anisotropic layer (A) is formed in a long shape, the angle θ1 between the longitudinal direction and the in-plane slow axis of the optically anisotropic layer (A) is not particularly limited, but is preferably 40 to 85°, more preferably 50 to 85°, and even more preferably 65 to 85°. Furthermore, from the viewpoint of making it possible to reduce the thickness of the optically anisotropic layer (A), it is preferable that the optically anisotropic layer (A) is a layer formed using a liquid crystal compound, and it is more preferable that the optically anisotropic layer is an optically anisotropic layer formed by fixing an oriented liquid crystal compound. More specifically, the optically anisotropic layer (A) is preferably a layer formed using a discotic liquid crystal compound, and more preferably a layer formed by fixing a vertically aligned discotic liquid crystal compound.

[0040] The type of liquid crystal compound is not particularly limited. Generally, liquid crystal compounds can be classified into rod-shaped type (rod-shaped liquid crystal compounds) and disk-shaped type (discotic liquid crystal compounds) based on their shape. Furthermore, liquid crystal compounds can be classified into low molecular weight type and polymer type. Polymer generally refers to a compound with a degree of polymerization of 100 or more (Polymer Physics, Phase Transition Dynamics, Masao Doi, page 2, Iwanami Shoten, 1992). In the present invention, any liquid crystal compound can be used, but it is preferable to use a rod-shaped liquid crystal compound. Two or more rod-shaped liquid crystal compounds, or a mixture of a rod-shaped liquid crystal compound and a discotic liquid crystal compound, may be used. As the rod-like liquid crystal compound, for example, those described in claim 1 of JP-T-11-513019 and paragraphs 0026 to 0098 of JP-A-2005-289980 can be preferably used. As the discotic liquid crystal compound, for example, those described in paragraphs 0020 to 0067 of JP-A No. 2007-108732 and paragraphs 0013 to 0108 of JP-A No. 2010-244038 can be preferably used.

[0041] The liquid crystal compound preferably has a polymerizable group. The type of polymerizable group possessed by the liquid crystal compound is not particularly limited, and is preferably a functional group capable of an addition polymerization reaction, more preferably a polymerizable ethylenically unsaturated group or a ring-polymerizable group, and further preferably a (meth)acryloyl group, a vinyl group, a styryl group, or an allyl group.

[0042] The liquid crystal compound may be a liquid crystal compound with forward wavelength dispersion or a liquid crystal compound with reverse wavelength dispersion. When the liquid crystal compound is a liquid crystal compound with forward wavelength dispersion, the production cost of the film is reduced and durability is improved, which is preferable. In this specification, a liquid crystal compound with forward wavelength dispersion is one in which, when the in-plane retardation (Re) value in the visible light range of an optically anisotropic layer prepared using this liquid crystal compound is measured, the Re value decreases as the measured wavelength increases, whereas a liquid crystal compound with reverse wavelength dispersion is one in which, when the Re value is similarly measured, the Re value increases as the measured wavelength increases.

[0043] The optically anisotropic layer (A) may be a polymer film containing a resin having negative intrinsic birefringence. A resin with negative intrinsic birefringence is one whose slow axis is perpendicular to the stretching direction, in other words, a resin with negative intrinsic birefringence is one whose refractive index in the stretching direction is smaller than the refractive index in the direction perpendicular thereto. Resins with negative intrinsic birefringence include homopolymers of styrene or styrene derivatives (e.g., polystyrene, fluorinated polystyrene), polystyrene-based polymers including copolymers of styrene or styrene derivatives with any monomer, polyacrylonitrile polymers, (meth)acrylic polymers such as polymethyl methacrylate, polyester-based resins, or multicomponent copolymers thereof, and cellulose compounds such as cellulose esters. More specifically, there are polymethyl methacrylate polystyrene, fluorinated polystyrene, polyvinyl naphthalene, and fumaric acid ester-based resins.

[0044] The thickness of the optically anisotropic layer (A) is not particularly limited. When the optically anisotropic layer (A) is a layer formed using a discotic liquid crystal compound, the thickness is preferably 0.5 to 5 μm, and more preferably 0.5 to 2 μm, from the viewpoint of a balance between thinning and ease of handling.

[0045] (Optical anisotropic layer (B)) The optically anisotropic layer (B) is a layer in which a rod-shaped liquid crystal compound is fixed in a twisted orientation with the thickness direction as the helical axis. It is preferable that the layer is a layer in which a chiral nematic phase having a so-called helical structure is fixed. In addition, when forming the above phase, it is preferable to use a mixture of a liquid crystal compound showing a nematic liquid crystal phase and a chiral agent described later. The meaning of the "fixed" state is as described above.

[0046] The value of the product Δnd of the refractive index anisotropy Δn of the optically anisotropic layer (B) measured at a wavelength of 550 nm and the thickness d of the optically anisotropic layer (B) is not particularly limited, but is preferably 140 to 220 nm, more preferably 150 to 210 nm, and even more preferably 160 to 200 nm, in that color unevenness is further suppressed. The refractive index anisotropy Δn means the refractive index anisotropy of the optically anisotropic layer. The above Δnd is measured using an AxoScan (polarimeter) device manufactured by Axometrics and the device analysis software of the same company.

[0047] The twist angle of the liquid crystal compound (the twist angle of the alignment direction of the liquid crystal compound) is preferably in the range of 90±30° (in the range of 60 to 120°), and in terms of further suppressing color unevenness, is more preferably in the range of 90±20° (in the range of 70 to 110°), and even more preferably in the range of 90±10° (in the range of 80 to 100°). The torsion angle is measured using an AxoScan (polarimeter) device manufactured by Axometrics Inc. and the device analysis software of the same company. The liquid crystal compound is twisted around the thickness direction of the optically anisotropic layer (B) as an axis, from one main surface to the other main surface of the optically anisotropic layer (B). Accordingly, the orientation direction (in-plane slow axis direction) of the liquid crystal compound differs depending on the position in the thickness direction of the optically anisotropic layer (B).

[0048] The thickness of the optically anisotropic layer (B) is not particularly limited, but from the viewpoint of a balance between thinness and ease of handling, it is preferably from 0.5 to 5 μm, more preferably from 0.5 to 2 μm.

[0049] The in-plane slow axis of the optically anisotropic layer (A) is preferably parallel to the in-plane slow axis of the optically anisotropic layer (B) on the surface of the optically anisotropic layer (A). Therefore, when the optically anisotropic layer (A) and the optically anisotropic layer (B) are long, the angle between the in-plane slow axis of the optically anisotropic layer (B) on the surface of the optically anisotropic layer (A) and the longitudinal direction preferably corresponds to the above-mentioned θ1. In addition, the in-plane slow axis of the optically anisotropic layer (B) on the surface on the optically anisotropic layer (A) side and the in-plane slow axis of the optically anisotropic layer (B) on the surface opposite to the optically anisotropic layer (A) side preferably form the above-mentioned twist angle (within the range of 90±30°). In particular, it is preferable that the in-plane slow axis of the optically anisotropic layer (B) on the surface opposite to the optically anisotropic layer (A) side rotates a predetermined angle (within the range of 90±30°) clockwise based on the in-plane slow axis of the optically anisotropic layer (B) on the surface on the optically anisotropic layer (A) side.

[0050] The type of liquid crystal compound used to form the optically anisotropic layer (B) is not particularly limited, and examples thereof include the compounds exemplified as the liquid crystal compound used to form the optically anisotropic layer (A).

[0051] Various known chiral agents can be used to form a twisted alignment of liquid crystal compounds. Chiral agents have the function of inducing a helical structure in liquid crystal compounds. Chiral compounds can be selected according to the purpose, since the sense or pitch of the helix they induce varies depending on the compound. As the chiral agent, known compounds can be used, but it is preferable to have a cinnamoyl group.As examples of chiral agents, the compounds described in Liquid Crystal Device Handbook (Chapter 3, Section 4-3, Chiral Agents for TN and STN, page 199, edited by the 142nd Committee of the Japan Society for the Promotion of Science, 1989) and JP-A-2003-287623, JP-A-2002-302487, JP-A-2002-080478, JP-A-2002-080851, JP-A-2010-181852 and JP-A-2014-034581 can be exemplified.

[0052] The chiral agent generally contains an asymmetric carbon atom, but an axially asymmetric or planarly asymmetric compound that does not contain an asymmetric carbon atom can also be used as the chiral agent. Examples of the axially asymmetric or planarly asymmetric compound include binaphthyl, helicene, paracyclophane and their derivatives. The chiral agent may have a polymerizable group. When both the chiral agent and the liquid crystal compound have a polymerizable group, a polymer having a repeating unit derived from the polymerizable liquid crystal compound and a repeating unit derived from the chiral agent can be formed by the polymerization reaction between the polymerizable chiral agent and the polymerizable liquid crystal compound.In this embodiment, the polymerizable group of the polymerizable chiral agent is preferably the same type of group as the polymerizable group of the polymerizable liquid crystal compound.Therefore, the polymerizable group of the chiral agent is also preferably an unsaturated polymerizable group, an epoxy group or an aziridinyl group, more preferably an unsaturated polymerizable group, and particularly preferably an ethylenically unsaturated polymerizable group. The chiral agent may also be a liquid crystal compound.

[0053] As the chiral agent, preferred are isosorbide derivatives, isomannide derivatives, binaphthyl derivatives, etc. As the isosorbide derivative, a commercially available product such as LC-756 manufactured by BASF may be used. The content of the chiral dopant in the optically anisotropic layer (B) is preferably from 0.01 to 200 mol %, more preferably from 1 to 30 mol %, based on the total molar amount of the liquid crystal compound.

[0054] The optically anisotropic layer (B) may contain materials other than those mentioned above. Examples of the other materials include surfactants, alignment control agents, polymers, and the like that are used in the production method of the optically anisotropic layer (B) described below.

[0055] (Optical anisotropic layer (C)) The optically anisotropic layer (C) is a layer in which vertically aligned rod-like liquid crystal compounds or horizontally aligned discotic liquid crystal compounds are fixed. In view of their usefulness as compensation layers for circular polarizers and display devices, the layer in which vertically aligned rod-shaped liquid crystal compounds are fixed is preferably a positive C plate, and the layer in which horizontally aligned discotic liquid crystal compounds are fixed is preferably a negative C plate.

[0056] Here, the positive C plate and the negative C plate are defined as follows. When the refractive index in the slow axis direction in the film plane (the direction in which the in-plane refractive index is maximum) is nx, the refractive index in the direction perpendicular to the in-plane slow axis is ny, and the refractive index in the thickness direction is nz, the positive C plate satisfies the relationship in formula (C1), and the negative C plate satisfies the relationship in formula (C2). Note that the positive C plate has a negative Rth value, and the negative C plate has a positive Rth value. Formula (C1) nz>nx≒ny Formula (C2) nz <nx≒ny It should be noted that the above "≒" includes not only the case where the two are completely identical, but also the case where the two are substantially identical. The term "substantially the same" means that, for example, the absolute value of (nx-ny) x d (where d is the thickness of the film) is 0 to 10 nm, preferably 0 to 5 nm, is also included in "nx ≈ ny".

[0057] The in-plane retardation of the optically anisotropic layer (C) at a wavelength of 550 nm is not particularly limited, but is preferably 0 to 10 nm, and more preferably 0 to 5 nm in that color unevenness is further suppressed. When the optically anisotropic layer (C) is a layer in which vertically aligned rod-like liquid crystal compounds are fixed, the retardation in the thickness direction of the optically anisotropic layer (C) at a wavelength of 550 nm is preferably −140 to −20 nm, more preferably −130 to −30 nm, and even more preferably −120 to −40 nm. When the optically anisotropic layer (C) is a layer in which a horizontally aligned discotic liquid crystal compound is fixed, the retardation in the thickness direction of the optically anisotropic layer (C) at a wavelength of 550 nm is preferably 20 to 140 nm, more preferably 30 to 130 nm, and even more preferably 40 to 120 nm.

[0058] The upper limit of the thickness of the retardation film is preferably 30 μm or less, more preferably 20 μm or less, even more preferably 10 μm or less, and particularly preferably 5 μm or less. The lower limit of the thickness of the retardation film is preferably 1 μm or more. Note that the thickness of the retardation film refers to the thickness including the adhesive when the optically anisotropic layer is attached with an adhesive or the like.

[0059] <Other materials> The circular polarizer may further include other components. The circular polarizer may include a substrate. The substrate is preferably a transparent substrate. Note that the transparent substrate refers to a substrate having a visible light transmittance of 60% or more, preferably 80% or more, and more preferably 90% or more.

[0060] The retardation value (Rth(550)) in the thickness direction of the substrate at a wavelength of 550 nm is not particularly limited, but is preferably −110 to 110 nm, more preferably −80 to 80 nm. The in-plane retardation value (Re(550)) of the substrate at a wavelength of 550 nm is not particularly limited, but is preferably 0 to 50 nm, more preferably 0 to 30 nm, and further preferably 0 to 10 nm.

[0061] The material for forming the substrate is preferably a polymer having excellent optical performance transparency, mechanical strength, thermal stability, moisture barrier properties, isotropy, and the like. Examples of polymer films that can be used as the substrate include cellulose acylate films (e.g., cellulose triacetate film (refractive index 1.48), cellulose diacetate film, cellulose acetate butyrate film, and cellulose acetate propionate film), polyolefin films such as polyethylene and polypropylene, polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyethersulfone films, polyacrylic films such as polymethyl methacrylate, polyurethane films, polycarbonate films, polysulfone films, polyether films, polymethylpentene films, polyether ketone films, (meth)acrylonitrile films, and films of polymers having an alicyclic structure (norbornene-based resins (Arton: product name, manufactured by JSR Corporation, amorphous polyolefins (Zeonex: product name, manufactured by Zeon Corporation))). Among these, the material for the polymer film is preferably triacetyl cellulose, polyethylene terephthalate, or a polymer having an alicyclic structure, and more preferably triacetyl cellulose.

[0062] The substrate may contain various additives (for example, an optical anisotropy adjusting agent, a wavelength dispersion adjusting agent, fine particles, a plasticizer, an ultraviolet protection agent, an anti-degradation agent, and a release agent).

[0063] The thickness of the substrate is not particularly limited, but is preferably 10 to 200 μm, more preferably 10 to 100 μm, and even more preferably 20 to 90 μm. The substrate may be made of a laminate of multiple sheets. In order to improve adhesion with a layer provided thereon, the surface of the substrate may be subjected to a surface treatment (e.g., glow discharge treatment, corona discharge treatment, ultraviolet (UV) treatment, flame treatment). In addition, an adhesive layer (undercoat layer) may be provided on the substrate. In addition, in order to impart slipperiness to the substrate during the transport process and to prevent sticking between the front and back surfaces after winding, a polymer layer containing inorganic particles having an average particle size of about 10 to 100 nm at a solid content ratio of 5 to 40 mass % may be placed on one side of the substrate.

[0064] The substrate may be a so-called temporary support, that is, the substrate may be peeled off from the optically anisotropic layer after carrying out the production method of the present invention.

[0065] In addition, the surface of the substrate may be directly subjected to rubbing treatment. In other words, a substrate that has been subjected to rubbing treatment may be used. The direction of the rubbing treatment is not particularly limited, and an optimal direction is appropriately selected depending on the direction in which the liquid crystal compound is desired to be aligned. The rubbing treatment can be a treatment method that is widely used as a liquid crystal alignment treatment process for LCDs (liquid crystal displays), in which the surface of the substrate is rubbed in a certain direction with paper, gauze, felt, rubber, nylon fiber, polyester fiber, or the like to obtain alignment.

[0066] An alignment film may be disposed on the substrate. The alignment layer can be formed by such means as rubbing an organic compound (preferably a polymer), oblique deposition of an inorganic compound, formation of a layer with microgrooves, or deposition of an organic compound (e.g., ω-tricosanoic acid, dioctadecylmethylammonium chloride, methyl stearate) by the Langmuir-Blodgett technique (LB film). Furthermore, an alignment film is also known that exhibits an alignment function when an electric field is applied, a magnetic field is applied, or light (preferably polarized light) is irradiated.

[0067] The circularly polarizing plate may have an adhesive layer disposed between each of the layers. Examples of the adhesive layer include a known pressure-sensitive adhesive layer and adhesive layer.

[0068] As described in JP-A-11-149015, generally, it is preferable to adjust the refractive index of the adhesive or pressure-sensitive adhesive of each layer forming a laminated wave plate or a circular polarizing plate from the viewpoint of suppressing reflection by adjusting the refractive index between layers. The difference in refractive index between the layer and the object to be adhered is preferably 0.1 or less, more preferably 0.08 or less, even more preferably 0.06 or less, and most preferably 0.03 or less.

[0069] When the optically anisotropic layer using a polymerizable liquid crystal is disposed between the layers, a highly refractive adhesive or pressure sensitive adhesive may be used. In order to increase the refractive index, it is also preferable to use a highly refractive monomer or highly refractive metal particles. The highly refractive monomer preferably has a benzene ring skeleton in the molecule. Examples of monofunctional monomers having a benzene ring skeleton in the molecule include ethoxylated O-phenylphenol (meth)acrylate, O-phenylphenol glycidyl ether (meth)acrylate, paracumylphenoxyethylene glycol (meth)acrylate, 2-methacryloyloxyethyl phthalate, 2-acryloyloxyethyl phthalate, 2-acryloyloxyethyl-2-hydroxyethyl phthalate, 2-acryloyloxypropyl phthalate, phenoxyethyl (meth)acrylate, EO-modified phenol (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, EO-modified nonylphenol (meth)acrylate, PO-modified nonylphenol (meth)acrylate, phenyl glycidyl ether (meth)acrylate, neopentyl glycol benzoate (meth)acrylate, nonylphenoxy polyethylene glycol (meth)acrylate, ECH-modified phenoxy (meth)acrylate, benzyl (meth)acrylate, and vinyl carbazole. Examples of components constituting inorganic particles include metal oxides, metal nitrides, metal oxynitrides, and simple metals. Examples of metal atoms contained in the above-mentioned metal oxides, metal nitrides, metal oxynitrides, and simple metals include titanium atoms, silicon atoms, aluminum atoms, cobalt atoms, and zirconium atoms. Specific examples of inorganic particles include inorganic oxide particles such as alumina particles, alumina hydrate particles, silica particles, zirconia particles, and clay minerals (e.g., smectite). From the viewpoint of refractive index, fine particles of zirconium oxide are preferred. The refractive index can be adjusted to a predetermined value by changing the amount of inorganic fine particles. When zirconium oxide is used as the main component, the average particle size of the inorganic fine particles in the layer is preferably 1 to 120 nm, more preferably 1 to 60 nm, and even more preferably 2 to 40 nm.

[0070] <Method of manufacturing a circularly polarizing plate and a method of manufacturing a retardation film> The method for producing the circularly polarizing plate is not particularly limited, and a known method can be used. For example, a method of laminating a polarizer and a retardation film can be used. When laminating, an adhesive layer can be used as necessary. The method for producing the retardation film is not particularly limited, and any known method can be used. In particular, the method for producing the retardation film can be carried out continuously by roll-to-roll. For example, a retardation film can be produced by preparing optically anisotropic layers (A) to (C) each exhibiting a predetermined optical property, and bonding the optically anisotropic layers to a substrate (e.g., a long substrate) in a predetermined order via an adhesive layer (e.g., a pressure-sensitive adhesive layer or a bonding layer). Alternatively, the retardation film may be produced by successively preparing the optically anisotropic layer (A) to the optically anisotropic layer (C) on a substrate using the polymerizable liquid crystal composition described later. For example, the polymerizable liquid crystal composition may be applied onto the substrate to form the optically anisotropic layer (C), and then the polymerizable liquid crystal composition may be applied onto the optically anisotropic layer (C) to form the optically anisotropic layer (B), and the polymerizable liquid crystal composition may be further applied onto the optically anisotropic layer (B) to form the optically anisotropic layer (A). In addition, the above-mentioned method of laminating optically anisotropic layers and the method of forming an optically anisotropic layer using a polymerizable liquid crystal composition may be combined. More specifically, a method of forming an optically anisotropic layer (C) by applying a polymerizable liquid crystal composition onto a substrate, forming an optically anisotropic layer (B) by applying a polymerizable liquid crystal composition onto the optically anisotropic layer (C) to obtain a laminate, and then laminating the laminate with a separately prepared optically anisotropic layer (A) to produce a retardation film, etc., may be mentioned. The manufacturing method for each layer will be described in detail below. Each component will be described in detail below.

[0071] The optically anisotropic layer (A) to the optically anisotropic layer (C) contained in the retardation film are preferably layers in which aligned liquid crystal compounds are fixed. The optically anisotropic layer produced in the present invention is preferably a layer formed by fixing a liquid crystal compound having a polymerizable group (a rod-shaped liquid crystal compound or a discotic liquid crystal compound having a polymerizable group) by polymerization or the like.

[0072] The optically anisotropic layers (A) to (C) are preferably formed using a polymerizable liquid crystal composition. More specifically, it is preferable to form a composition layer by applying a polymerizable liquid crystal composition, align the liquid crystal compound in the composition layer, and then perform a curing treatment to form a predetermined optically anisotropic layer. The polymerizable liquid crystal composition is a composition containing a liquid crystal compound having a polymerizable group. Various components contained in the polymerizable liquid crystal composition will be described in detail later. The above procedure will now be described in detail.

[0073] The procedure for forming the composition layer is not particularly limited, and for example, a method of applying a polymerizable liquid crystal composition onto a substrate and, if necessary, carrying out a drying treatment can be mentioned. The coating method is not particularly limited, and examples thereof include wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, and die coating.

[0074] The thickness of the composition layer is not particularly limited, but is preferably from 0.1 to 20 μm, more preferably from 0.2 to 15 μm, and even more preferably from 0.5 to 10 μm.

[0075] Next, the formed composition layer is subjected to an alignment treatment to align the polymerizable liquid crystal compound in the composition layer. The alignment treatment can be carried out by drying the coating film at room temperature or by heating the coating film. In the case of a thermotropic liquid crystal compound, the liquid crystal phase formed by the alignment treatment can generally be transitioned by a change in temperature or pressure. In the case of a lyotropic liquid crystal compound, the transition can also be caused by the composition ratio of the amount of solvent, etc. The conditions for heating the composition layer are not particularly limited, but the heating temperature is preferably 50 to 250° C., more preferably 50 to 150° C., and the heating time is preferably 10 seconds to 10 minutes. After the composition layer is heated, the coating film may be cooled, if necessary, before the curing treatment (light irradiation treatment) described later. The cooling temperature is preferably 20 to 200°C, and more preferably 30 to 150°C.

[0076] Next, the composition layer in which the polymerizable liquid crystal compound is aligned is subjected to a curing treatment. The method of hardening treatment performed on the composition layer in which the polymerizable liquid crystal compound is aligned is not particularly limited, and examples thereof include light irradiation treatment and heat treatment. Among them, from the viewpoint of manufacturability, light irradiation treatment is preferred, and ultraviolet irradiation treatment is more preferred. The irradiation conditions for the light irradiation treatment are not particularly limited, but are preferably 50 to 1000 mJ / cm 2 is preferred. The atmosphere during the light irradiation treatment is not particularly limited, but a nitrogen atmosphere is preferred.

[0077] Although the method of forming a composition layer by applying a polymerizable liquid crystal composition has been described above, a composition layer may be formed separately and then transferred onto a predetermined substrate.

[0078] The polymerizable liquid crystal composition used above contains the liquid crystal compound having the above-mentioned polymerizable group, and other components used as necessary (e.g., a chiral agent, a polymerization initiator, a polymerizable monomer, a surfactant, a polymer, a photoaligned polymer, and a solvent, etc.).

[0079] The content of the liquid crystal compound in the polymerizable liquid crystal composition is not particularly limited, but is preferably 60% by mass or more, more preferably 70% by mass or more, based on the total solid content in the polymerizable liquid crystal composition, in terms of ease of controlling the alignment state of the liquid crystal compound. The upper limit is not particularly limited, but is preferably 99% by mass or less, more preferably 97% by mass or less. The solid content means a component capable of forming an optically anisotropic layer from which the solvent has been removed, and even if the component is in a liquid state, it is considered to be a solid content.

[0080] As described above, the polymerizable liquid crystal composition may contain components other than the liquid crystal compound. For example, the polymerizable liquid crystal composition may contain a polymerization initiator. When the polymerizable liquid crystal composition contains a polymerization initiator, the polymerization of the liquid crystal compound having a polymerizable group proceeds more efficiently. The polymerization initiator may be a known polymerization initiator, such as a photopolymerization initiator or a thermal polymerization initiator, with a photopolymerization initiator being preferred. The content of the polymerization initiator in the polymerizable liquid crystal composition is not particularly limited, but is preferably from 0.01 to 20% by mass, and more preferably from 0.5 to 10% by mass, based on the total solid content in the polymerizable liquid crystal composition.

[0081] The polymerizable liquid crystal composition may contain a chiral dopant. The type of chiral agent is not particularly limited, and examples thereof include known chiral agents. The content of the chiral dopant in the polymerizable liquid crystal composition is not particularly limited, but is preferably from 0.01 to 20 mass %, more preferably from 0.3 to 10 mass %, based on the total solid content in the polymerizable liquid crystal composition.

[0082] The polymerizable liquid crystal composition may contain a polymerizable monomer different from the liquid crystal compound having a polymerizable group. The polymerizable monomer may be a radical polymerizable compound or a cationic polymerizable compound, and a polyfunctional radical polymerizable monomer is preferable. The polymerizable monomer may be, for example, the polymerizable monomer described in paragraphs 0018 to 0020 of JP-A-2002-296423. The content of the polymerizable monomer in the polymerizable liquid crystal composition is not particularly limited, but is preferably from 1 to 50% by mass, and more preferably from 5 to 30% by mass, based on the total mass of the liquid crystal compound.

[0083] The polymerizable liquid crystal composition may contain a surfactant. Examples of the surfactant include conventionally known alkyl ether compounds, silicone compounds, and fluorine compounds, and fluorine compounds are preferred. Specifically, for example, the compounds described in paragraphs 0028 to 0056 of JP-A No. 2001-330725 and the compounds described in paragraphs 0069 to 0126 of JP-A No. 2003-295212 are included.

[0084] The polymerizable liquid crystal composition may contain a polymer. Examples of the polymer include cellulose esters. Examples of the cellulose esters include those described in paragraph 0178 of JP-A-2000-155216. The content of the polymer in the polymerizable liquid crystal composition is not particularly limited, but is preferably from 0.1 to 10% by mass, and more preferably from 0.1 to 8% by mass, based on the total mass of the liquid crystal compound.

[0085] In addition to the above, the polymerizable liquid crystal composition may contain an additive (alignment control agent) that promotes horizontal or vertical alignment in order to bring the liquid crystal compound into a horizontal or vertical alignment state.

[0086] The polymerizable liquid crystal composition may contain a photo-alignable polymer. The photo-alignable polymer is a polymer having a photo-alignable group. When the photo-alignable polymer has a repeating unit having a fluorine atom or a silicon atom represented by the formula (1) or formula (2) described later, or when the photo-alignable polymer is a cleavage-type photo-alignable polymer, the photo-alignable polymer is likely to be unevenly distributed on the surface of the composition layer when a composition layer is formed using the polymerizable liquid crystal composition. In the optically anisotropic layer formed using such a composition layer, the photo-alignable polymer is unevenly distributed near the surface, so that when the photo-alignment treatment is performed, a surface shape having a predetermined alignment control force is formed. As a result, a desired optically anisotropic layer can be manufactured by further applying a polymerizable liquid crystal composition on the optically anisotropic layer without providing a separate alignment film.

[0087] The photo-alignable group possessed by a photo-alignable polymer refers to a group having a photo-alignment function in which rearrangement or an anisotropic chemical reaction is induced when irradiated with anisotropic light (e.g., plane polarized light, etc.). Photo-alignable groups that undergo at least one of dimerization and isomerization due to the action of light are preferred because they provide excellent alignment uniformity and good thermal and chemical stability.

[0088] Specific examples of the group that dimerizes by the action of light preferably include groups having a skeleton of at least one derivative selected from the group consisting of cinnamic acid derivatives, coumarin derivatives, chalcone derivatives, maleimide derivatives, and benzophenone derivatives. On the other hand, specific examples of groups that are isomerized by the action of light preferably include groups having a skeleton of at least one compound selected from the group consisting of an azobenzene compound, a stilbene compound, a spiropyran compound, a cinnamic acid compound, and a hydrazono-β-ketoester compound.

[0089] Of these photoalignable groups, a group selected from the group consisting of a cinnamoyl group, an azobenzene group, a chalconyl group, and a coumarin group is preferred, because this provides better liquid crystal alignment in the optically anisotropic layer formed on top of the optically anisotropic layer containing a photoalignable polymer even with a small amount of exposure.

[0090] The photoalignable polymer is preferably a photoalignable polymer containing a repeating unit having a photoalignable group and a repeating unit having a fluorine atom or a silicon atom. In addition, because the optically anisotropic layer formed on top of an optically anisotropic layer containing a photoalignable polymer has better liquid crystal alignment properties, it is preferable that the photoalignable polymer has a repeating unit A containing a cleavage group that decomposes to produce a polar group by the action of at least one selected from the group consisting of light, heat, acid and base, and that the repeating unit A has a cleavage group in its side chain and has a fluorine atom or a silicon atom on the terminal side of the cleavage group in the side chain (hereinafter also referred to as "cleavage-type photoalignable polymer"). Here, the "polar group" contained in the repeating unit A refers to a group having at least one heteroatom, and specific examples thereof include a hydroxyl group, a carbonyl group, a carboxyl group, an amino group, a nitro group, an ammonium group, and a cyano group. Among these, a hydroxyl group, a carbonyl group, or a carboxyl group is preferred. Furthermore, the term "cleavable group that generates a polar group" refers to a group that generates the above-mentioned polar group upon cleavage, but in the present invention also includes a group that reacts with an oxygen molecule after radical cleavage to generate a polar group.

[0091] Examples of such cleavable photo-alignable polymers include the photo-alignable polymers described in paragraphs 0014 to 0049 of Patent Document 1 (International Publication No. 2018 / 216812), the contents of which are incorporated herein by reference.

[0092] For example, by incorporating a photo-aligned polymer in the optically anisotropic layer (C), the polymerizable liquid crystal composition forming the optically anisotropic layer (B) can be applied onto the optically anisotropic layer (C) without applying a separate alignment film, thereby forming the optically anisotropic layer (B) in which the liquid crystal compound is aligned. In other words, the optically anisotropic layer (C) and the optically anisotropic layer (A) or (B) can be directly laminated.

[0093] Other examples of photoalignable polymers containing a repeating unit having a fluorine atom or a silicon atom include copolymers (hereinafter also referred to as "specific copolymers") having a repeating unit having a fluorine atom or a silicon atom, represented by the following formula (1) or formula (2), and a repeating unit having a photoalignable group. The repeating unit having a fluorine atom or a silicon atom represented by the following formula (1) or formula (2) is a repeating unit containing a cleavable group that is decomposed by the action of at least one selected from the group consisting of light, heat, acid and base to generate a polar group.

[0094] [ka]

[0095] In the above formulas (1) and (2), r and s each independently represent an integer of 1 or more. Also, R B1 and R B2 each independently represents a hydrogen atom or a substituent. Also, Y 1 and Y 2 each independently represents -O- or -NR Z -, where R Z represents a hydrogen atom or a substituent. Also, L B1 represents a linking group having a valence of r+1. Also, L B2 represents a linking group having a valence of s+1. In addition, B1 represents a group represented by the following formula (B1): B1and when r is an integer of 2 or more, multiple B1's may be the same or different. In addition, B2 represents a group represented by the following formula (B2): B2 and when s is an integer of 2 or more, multiple B2's may be the same or different.

[0096] [ka]

[0097] In the above formulas (B1) and (B2), * represents a bonding position. Furthermore, n represents an integer of 1 or greater, provided that multiple n's may be the same or different. Additionally, m represents an integer of 2 or more. Also, R b1 represents a hydrogen atom or a substituent. Also, R b2 , R b3 , and R b4 Each independently represents a hydrogen atom or a substituent. b3 may be bonded to each other to form a ring, and multiple R b2 may be the same or different, and multiple R b3 may be the same or different, and multiple R b4 may be the same or different. Also, L b1 represents a n+1-valent linking group. b1 may be the same or different. Also, L b2 represents a linking group having a valence of m+1. Furthermore, Z represents an aliphatic hydrocarbon group having a fluorine atom or an organosiloxane group, provided that the aliphatic hydrocarbon group may have an oxygen atom, and multiple Z's may be the same or different.

[0098] In the above formula (1), R B1 Examples of the substituent represented by include known substituents. Among them, an alkyl group having 1 to 12 carbon atoms is preferable, and a methyl group is more preferable.

[0099] In the above formula (1), Y 1 each independently represents -O- or -NR Z - represents R Z represents a hydrogen atom or a substituent. Z The substituent of Y may be a known substituent, and a methyl group is preferable. 1 preferably represents -O- or -NH-, and more preferably represents -O-.

[0100] In the above formula (1), L B1 represents an r+1 valent linking group. The r+1 valent linking group is preferably an r+1 valent hydrocarbon group having 1 to 24 carbon atoms which may have a substituent, in which some of the carbon atoms constituting the hydrocarbon group may be substituted with a heteroatom, and more preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may contain an oxygen atom or a nitrogen atom. The r+1 valent linking group is preferably a divalent or trivalent linking group, and more preferably a divalent linking group.

[0101] In the above formula (1), r represents an integer of equal to or greater than 1. Among them, from the viewpoint of suitability for synthesis, an integer of 1 to 3 is preferable, an integer of 1 to 2 is more preferable, and 1 is even more preferable.

[0102] In the above formula (2), R B2 Examples of the substituent represented by include known substituents. Among them, an alkyl group having 1 to 12 carbon atoms is preferable, and a methyl group is more preferable.

[0103] In the above formula (2), Y 2 is -O- or -NR Z -, where R Z represents a hydrogen atom or a substituent. Z The substituent of Y may be a known substituent, and a methyl group is preferable. 2preferably represents -O- or -NH-, and more preferably represents -O-.

[0104] In the above formula (2), L B2 represents an s+1 valent linking group. The s+1 valent linking group is an s+1 valent hydrocarbon group having 1 to 24 carbon atoms which may have a substituent, preferably a hydrocarbon group in which some of the carbon atoms constituting the hydrocarbon group may be substituted with a heteroatom, and more preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may contain an oxygen atom or a nitrogen atom. The s+1 valent linking group is preferably a divalent linking group.

[0105] In the above formula (2), s represents an integer of equal to or greater than 1. Among them, from the viewpoint of suitability for synthesis, an integer of 1 to 2 is preferable, and 1 is more preferable.

[0106] In the above formula (B1), R b1 The substituent represented by R is preferably an aliphatic hydrocarbon group having 1 to 18 carbon atoms, more preferably an alkyl group having 1 to 12 carbon atoms, and further preferably a methyl group. b1 is preferably a substituent.

[0107] In the above formula (B1), R b2 The substituent represented by R in the above formula (B1) may be a known substituent. b1 The substituents of R b2 preferably represents a hydrogen atom.

[0108] In the above formula (B1), L b1 represents an n+1 valent linking group, and the n+1 valent linking group is an n+1 valent hydrocarbon group having 1 to 24 carbon atoms which may have a substituent, preferably a hydrocarbon group in which some of the carbon atoms constituting the hydrocarbon group may be substituted with a heteroatom, and more preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may contain an oxygen atom or a nitrogen atom.

[0109] The (n+1)-valent linking group is preferably a divalent to tetravalent linking group, more preferably a divalent to trivalent linking group, and even more preferably a divalent linking group.

[0110] In the above formula (B1), n ​​represents an integer of equal to or greater than 1. Among them, from the viewpoint of suitability for synthesis, an integer of 1 to 5 is preferable, an integer of 1 to 3 is more preferable, and 1 is even more preferable.

[0111] In the above formula (B1) and formula (B2), Z represents an aliphatic hydrocarbon group having a fluorine atom or an organosiloxane group, provided that the aliphatic hydrocarbon group may have an oxygen atom, and multiple Z may be the same or different. Examples of the aliphatic hydrocarbon group having a fluorine atom include a fluorine atom-containing alkyl group, a -CH 2 Examples of the fluorine atom-containing aliphatic hydrocarbon group include a group in which one or more - are substituted with -O-, and a fluorine atom-containing alkenyl group. The number of carbon atoms in the fluorine atom-containing aliphatic hydrocarbon group is not particularly limited, and is preferably 1 to 30, more preferably 3 to 20, and further preferably 3 to 10. The number of fluorine atoms contained in the fluorine atom-containing aliphatic hydrocarbon group is not particularly limited, and is preferably 1-30, more preferably 5-25, and even more preferably 7-20.

[0112] In the above formula (B2), R b3 and R b4 The substituent represented by R in the above formula (B1) may be a known substituent. b1 The substituents represented by R b3 is two Rb 3 are preferably bonded to each other to form a ring, and two Rb 3 More preferably, R are bonded to each other to form a cyclohexane ring. b4 preferably represents a hydrogen atom.

[0113] In the above formula (B2), L b2 represents a linking group having a valence of m+1. The (m+1)-valent linking group is preferably an (m+1)-valent hydrocarbon group having 1 to 24 carbon atoms which may have a substituent, in which some of the carbon atoms constituting the hydrocarbon group may be substituted with a heteroatom, and more preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may contain an oxygen atom or a nitrogen atom. The (m+1)-valent linking group is preferably a trivalent or tetravalent linking group, and more preferably a tetravalent linking group.

[0114] In the above formula (B2), m represents an integer of 2 or greater. Among them, from the viewpoint of synthesis suitability, an integer of 2 to 4 is preferred, and an integer of 2 to 3 is more preferred.

[0115] Specific examples of the repeating unit containing the group represented by formula (B1) above include repeating units represented by the following formulae B-1 to B-22, and specific examples of the repeating unit containing the group represented by formula (B2) above include repeating units represented by the following formulae B-23 to B-24.

[0116] [ka] JPEG0007583051000004.jpg38135JPEG0007583051000005.jpg51141JPEG0007583051000006.jpg38131 JPEG0007583051000007.jpg37137JPEG0007583051000008.jpg4377JPEG0007583051000009.jpg39109JPEG0007583051000010.jpg4474

[0117] The content of the repeating units having fluorine atoms or silicon atoms represented by formula (1) or formula (2) in the photo-alignable polymer is not particularly limited, and is preferably 15 to 75 mass %, more preferably 20 to 50 mass %, and even more preferably 25 to 45 mass %, of the total repeating units of the photo-alignable polymer, because this improves the effect of suppressing wind unevenness.

[0118] The structure of the main chain of the repeating unit having a photoalignable group is not particularly limited, and examples thereof include known structures, and for example, a skeleton selected from the group consisting of (meth)acrylic, styrene, siloxane, cycloolefin, methylpentene, amide, and aromatic ester structures is preferred. Among these, a skeleton selected from the group consisting of a (meth)acrylic, a siloxane, and a cycloolefin skeleton is more preferred, and a (meth)acrylic skeleton is even more preferred.

[0119] Specific examples of the repeating unit having a photoalignable group include the following.

[0120] [ka]

[0121] [ka]

[0122] [ka]

[0123] [ka]

[0124] [ka]

[0125] [ka]

[0126] The content of the repeating units having photoalignable groups in the photoalignable polymer is not particularly limited, and is preferably 5 to 60 mass %, more preferably 10 to 50 mass %, and even more preferably 15 to 40 mass %, of the total repeating units of the photoalignable polymer, because this improves the liquid crystal alignment of the optically anisotropic layer formed on the upper layer.

[0127] The specific copolymer may further have a repeating unit having a crosslinkable group in addition to the repeating unit having a fluorine atom or a silicon atom and the repeating unit having a photoalignable group represented by the above-mentioned formula (1) or formula (2). The type of crosslinkable group is not particularly limited, and examples thereof include known crosslinkable groups, such as an epoxy group, an epoxycyclohexyl group, an oxetanyl group, an acryloyl group, a methacryloyl group, a vinyl group, a styryl group, and an allyl group.

[0128] The structure of the main chain of the repeating unit having a crosslinkable group is not particularly limited, and examples thereof include known structures. For example, a skeleton selected from the group consisting of (meth)acrylic, styrene, siloxane, cycloolefin, methylpentene, amide, and aromatic ester skeletons is preferred. Among these, a skeleton selected from the group consisting of a (meth)acrylic, a siloxane, and a cycloolefin skeleton is more preferred, and a (meth)acrylic skeleton is even more preferred.

[0129] Specific examples of the repeating unit having a crosslinkable group include the following.

[0130] [ka]

[0131] The content of the repeating unit having a crosslinkable group in the specific copolymer is not particularly limited, but is preferably 10 to 60% by mass, more preferably 20 to 50% by mass, based on the total repeating units of the photoalignment polymer, because this improves the liquid crystal alignment properties of the optically anisotropic layer formed on the upper layer.

[0132] Examples of monomers (radical polymerizable monomers) that form other repeating units than those described above include acrylic acid ester compounds, methacrylic acid ester compounds, maleimide compounds, acrylamide compounds, acrylonitrile, maleic anhydride, styrene compounds, and vinyl compounds.

[0133] The method for synthesizing the photo-alignable polymer is not particularly limited, and the photo-alignable polymer can be synthesized, for example, by mixing a monomer that forms a repeating unit having a fluorine atom or a silicon atom represented by the above-mentioned formula (1) or formula (2), a monomer that forms a repeating unit having the above-mentioned photoreactive group, and a monomer that forms any other repeating unit, and polymerizing the mixture in an organic solvent using a radical polymerization initiator.

[0134] The weight average molecular weight (Mw) of the photoalignable polymer is not particularly limited, but is preferably 25,000 or more, more preferably 25,000 to 500,000, even more preferably 25,000 to 300,000, and particularly preferably 30,000 to 150,000, in order to improve the liquid crystal alignment properties of the optically anisotropic layer formed on the upper layer. Here, the weight average molecular weight of the photoalignable polymer and the surfactant is a value measured by gel permeation chromatography (GPC) under the following conditions. Solvent (eluent): THF (tetrahydrofuran) ·Device name: TOSOH HLC-8320GPC Column: Three TOSOH TSKgel Super HZM-H (4.6mm x 15cm) columns connected together Column temperature: 40℃ Sample concentration: 0.1% by mass ·Flow rate: 1.0ml / min Calibration curve: TOSOH TSK standard polystyrene Calibration curve using 7 samples with Mw = 2,800,000 to 1,050 (Mw / Mn = 1.03 to 1.06)

[0135] <<Organic EL display device>> The organic EL display device of the present invention has the above-mentioned circular polarizer. Usually, the circular polarizer is provided on an organic EL display panel of the organic EL display device. That is, the organic EL display device of the present invention has an organic EL display panel and the above-mentioned circular polarizer. An example of an organic EL display device includes an organic EL display panel, a retardation film, and a polarizer in this order.

[0136] An organic EL display panel is a member in which a light-emitting layer or a plurality of organic compound thin films including a light-emitting layer are formed between a pair of electrodes, an anode and a cathode, and may have a hole injection layer, a hole transport layer, an electron injection layer, an electron transport layer, a protective layer, etc. in addition to the light-emitting layer, and each of these layers may have other functions. Various materials can be used to form each layer.

[0137] <<Display device>> The above-mentioned circularly polarizing plate can also be used in various display devices having a curved surface, such as rollable displays, in-vehicle displays, sunglasses lenses, and goggle lenses for image display devices, all of which have a curved surface. The circular polarizing plate of the present invention can be attached to a curved surface or molded integrally with a resin, which contributes to improving design. The organic EL display device using the circular polarizing plate of the present invention can suppress color unevenness in an oblique direction, so it is preferably used for a curved display or an in-vehicle display. It is also preferable to use the circular polarizing plate of the present invention in an in-vehicle display optical system such as a head-up display, an optical system such as AR glasses and VR glasses, an optical sensor such as LiDAR, a face recognition system, and polarization imaging, etc. In addition, the circular polarizing plate of the present invention is also preferably used in a display device having a curved surface by being disposed along the curved surface. EXAMPLES

[0138] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts, ratios, processing contents, and processing procedures shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0139] <Example 1> (Preparation of Cellulose Acylate Film (Substrate)) The following composition was put into a mixing tank, stirred, and heated at 90°C for 10 minutes. The obtained composition was then filtered through a filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to prepare a dope. The solid content concentration of the dope was 23.5% by mass, the amount of the plasticizer added was the ratio relative to the cellulose acylate, and the solvent of the dope was methylene chloride / methanol / butanol = 81 / 18 / 1 (mass ratio).

[0140] ------------------------------------------------------------------ Cellulose Acylate Dope ------------------------------------------------------------------ Cellulose acylate (acetyl substitution degree 2.86, viscosity average polymerization degree 310) 100 parts by mass Sugar ester compound 1 (shown in chemical formula (S4)) 6.0 parts by mass Sugar ester compound 2 (shown in chemical formula (S5)) 2.0 parts by mass Silica particle dispersion (AEROSIL R972, Nippon Aerosil Co., Ltd.) 0.1 part by mass Solvent (methylene chloride / methanol / butanol) ------------------------------------------------------------------

[0141] [ka]

[0142] [ka]

[0143] The dope prepared above was cast using a drum film-forming machine. The dope was cast from a die onto a metal support cooled to 0°C so as to be in contact with the support, and then the resulting web (film) was peeled off from the drum. The drum was made of SUS.

[0144] The web (film) obtained by casting was peeled off from the drum, and then dried for 20 minutes in a tenter apparatus, which clips both ends of the web with clips and transports the web at 30 to 40°C during film transport. The web was then post-dried by zone heating while being transported by rolls. The obtained web was knurled and then wound up. The obtained cellulose acylate film had a thickness of 40 μm, an in-plane retardation Re(550) at a wavelength of 550 nm of 1 nm, and a retardation in the thickness direction Rth(550) at a wavelength of 550 nm of 26 nm.

[0145] (Alkaline saponification treatment) The above-mentioned cellulose acylate film was passed through a dielectric heating roll at a temperature of 60°C to raise the film surface temperature to 40°C, and then an alkaline solution having the composition shown below was applied to the band surface of the film using a bar coater in an amount of 14 ml / m 2 The plate was then conveyed for 10 seconds under a steam-type far-infrared heater manufactured by Noritake Co., Ltd., which had been heated to 110°C. Next, using the same bar coater, pure water was applied at a rate of 3 ml / m 2 Next, the film was washed with water using a fountain coater and then dried with an air knife three times, and then conveyed to a drying zone at 70° C. for 10 seconds to prepare an alkali saponified cellulose acylate film.

[0146] ------------------------------------------------------------------ Alkaline solution ------------------------------------------------------------------ Potassium hydroxide 4.7 parts by mass Water 15.8 parts by mass Isopropanol 63.7 parts by weight Surfactant: C 14 H 29 O(CH 2 CH 2 O) 20 H 1.0 parts by mass Propylene glycol 14.8 parts by weight ------------------------------------------------------------------

[0147] (Formation of alignment film) An alignment layer coating solution having the following composition was continuously coated on the alkaline saponified surface of the cellulose acylate film using a wire bar #14, and then dried with hot air at 60° C. for 60 seconds and then with hot air at 100° C. for 120 seconds.

[0148] ------------------------------------------------------------------ Alignment film coating solution ------------------------------------------------------------------ 10 parts by weight of the following polyvinyl alcohol Water 371 parts by mass Methanol 119 parts by weight Glutaraldehyde (crosslinking agent) 0.5 parts by weight Citric acid ester (manufactured by Sankyo Chemical Co., Ltd.) 0.175 parts by mass ------------------------------------------------------------------

[0149] (Polyvinyl alcohol)

[0150] [ka]

[0151] (Formation of Optically Anisotropic Layer (A)) The above-prepared alignment film was subjected to continuous rubbing treatment. At this time, the longitudinal direction of the long film was parallel to the transport direction, and the angle between the longitudinal direction of the film (transport direction) and the rotation axis of the rubbing roller was 76°. The longitudinal direction of the film (transport direction) was set to 90°, and the clockwise direction was expressed as a positive value with the film width direction as the reference (0°) when observed from the film side, so that the rotation axis of the rubbing roller was at -14°. In other words, the position of the rotation axis of the rubbing roller was a position rotated 76° clockwise with the longitudinal direction of the film as the reference when observed from the film side.

[0152] On the above-mentioned rubbed alignment film, a composition for forming an optically anisotropic layer (1a) containing a discotic liquid crystal compound of the following composition was applied using a Giesser coater to form a composition layer. Thereafter, the obtained composition layer was heated with hot air at 110°C for 2 minutes to dry the solvent and ripen the alignment of the discotic liquid crystal compound. Next, the obtained composition layer was irradiated with UV light (500 mJ / cm2) at 80°C. 2 ) was carried out to fix the alignment of the liquid crystal compound, thereby forming an optically anisotropic layer (1a) corresponding to the optically anisotropic layer (A). The thickness of the optically anisotropic layer (1a) was 1.1 μm. The in-plane retardation at a wavelength of 550 nm was 168 nm. The average inclination angle of the discotic surface of the discotic liquid crystal compound with respect to the film surface was 90°, and it was confirmed that the compound was oriented perpendicularly to the film surface. The angle of the in-plane slow axis of the optically anisotropic layer (1a) was parallel to the rotation axis of the rubbing roller, and the in-plane slow axis was -14° when viewed from the optically anisotropic layer (1a) side, assuming that the width direction of the film is 0° (the longitudinal direction is 90° counterclockwise and -90° clockwise).

[0153] ------------------------------------------------------------------ Composition for forming optically anisotropic layer (1a) ------------------------------------------------------------------ 80 parts by weight of the following discotic liquid crystal compound 1 20 parts by weight of the following discotic liquid crystal compound 2 0.55 parts by weight of the following alignment film interface alignment agent 1 0.1 parts by mass of the following fluorine-containing compound A 0.05 parts by mass of the following fluorine-containing compound B 0.21 parts by mass of the following fluorine-containing compound C Ethylene oxide modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 10 parts by mass Photopolymerization initiator (Irgacure 907, manufactured by BASF) 3.0 parts by mass Methyl ethyl ketone 200 parts by mass ------------------------------------------------------------------

[0154] Discotic Liquid Crystal Compound 1

[0155] [ka]

[0156] Discotic Liquid Crystal Compound 2

[0157] [ka]

[0158] Alignment film interface alignment agent 1

[0159] [ka]

[0160] Fluorine-containing compound A

[0161] [ka]

[0162] The above a and b represent the content (mass %) of each repeating unit relative to all repeating units, with a representing 90 mass % and b representing 10 mass %.

[0163] Fluorine-containing compound B (the numerical value in each repeating unit indicates the content (mass%) relative to all repeating units, the content of the repeating unit on the left side was 32.5 mass%, and the content of the repeating unit on the right side was 67.5 mass%).

[0164] [ka]

[0165] Fluorine-containing compound C (the numerical value in each repeating unit indicates the content (mass%) relative to all repeating units, the content of the repeating unit on the left was 25 mass%, the content of the repeating unit in the middle was 25 mass%, and the content of the repeating unit on the right was 50 mass%).

[0166] [ka]

[0167] (Formation of a laminate of an optically anisotropic layer (C) and an optically anisotropic layer (B)) (Formation of Optically Anisotropic Layer (1c)) On the cellulose acylate film prepared above, a composition for forming an optically anisotropic layer (1c) containing a rod-shaped liquid crystal compound having the following composition was applied using a Giesser coater to form a composition layer. Then, both ends of the film were held, a cooling plate (9°C) was placed on the side of the film on which the composition layer was formed so as to be 5 mm away from the film, and a heater (75°C) was placed on the side opposite to the side on which the composition layer was formed so as to be 5 mm away from the film, and the film was dried for 2 minutes. Next, the sample was heated to 60°C for 1 minute with hot air, and then irradiated with a 365 nm UV-LED at a dose of 100 mJ / cm while purging with nitrogen to keep the oxygen concentration in the atmosphere at 100 ppm or less. 2 After that, it was annealed with hot air at 120° C. for 1 minute to form an optically anisotropic layer (1c). The obtained optically anisotropic layer (1c) was irradiated with UV light (ultra-high pressure mercury lamp; UL750; manufactured by HOYA) at room temperature at 7.9 mJ / cm through a wire grid polarizer. 2 By irradiating the film with light (wavelength: 313 nm), an optically anisotropic layer (1c) having an alignment control ability was formed on the surface. The thickness of the optically anisotropic layer (1c) formed was 0.5 μm. The in-plane retardation Re at a wavelength of 550 nm was 0 nm, and the retardation Rth in the thickness direction at a wavelength of 550 nm was −68 nm. The average tilt angle of the long axis direction of the rod-like liquid crystal compound with respect to the film surface was 90°, and it was confirmed that the compound was aligned perpendicular to the film surface. In this manner, an optically anisotropic layer (1c) corresponding to the optically anisotropic layer (C) was formed.

[0168] ------------------------------------------------------------------ Composition for forming optically anisotropic layer (1c) ------------------------------------------------------------------ 100 parts by weight of the following rod-shaped liquid crystal compound (A) Polymerizable monomer (A-400, manufactured by Shin-Nakamura Chemical Co., Ltd.) 4.0 parts by mass 5.0 parts by mass of the following polymerization initiator S-1 (oxime type) 3.0 parts by weight of the following photoacid generator D-1 2.0 parts by weight of the following polymer M-1 2.0 parts by weight of the vertical alignment agent S01 listed below 2.0 parts by mass of the photo-alignable polymer A-1 shown below 0.2 parts by weight of the following surfactant B-1 Methyl ethyl ketone 42.3 parts by mass Methyl isobutyl ketone 627.5 parts by mass ------------------------------------------------------------------

[0169] Rod-shaped liquid crystal compound (A) (hereinafter, a mixture of compounds)

[0170] [ka]

[0171] Polymerization initiator S-1

[0172] [ka]

[0173] Photoacid generator D-1

[0174] [ka]

[0175] Polymer M-1

[0176] [ka]

[0177] Vertical alignment agent S01

[0178] [ka]

[0179] Photoalignable polymer A-1 (the numerical value in each repeating unit indicates the content (mass%) of each repeating unit relative to the total repeating units, and the repeating units from the left were 43 mass%, 27 mass%, and 30 mass%. The weight average molecular weight was 69,800.)

[0180] [ka]

[0181] Surfactant B-1 (weight average molecular weight was 2200)

[0182] [ka]

[0183] (Formation of Optically Anisotropic Layer (1b)) Next, on the optically anisotropic layer (1c) prepared above, a composition for forming an optically anisotropic layer (1b) containing a rod-shaped liquid crystal compound having the following composition was applied using a Giesser coater, and heated with hot air at 80°C for 60 seconds. Next, the obtained composition layer was irradiated with UV (500 mJ / cm2) at 80°C. 2 ) was carried out to fix the alignment of the liquid crystal compound, thereby forming an optically anisotropic layer (1b) corresponding to the optically anisotropic layer (B). The optically anisotropic layer (1b) had a thickness of 1.2 μm, a Δnd at a wavelength of 550 nm of 164 nm, and a twist angle of the liquid crystal compound of 81°. When viewed from the optically anisotropic layer (1b) side, assuming that the width direction of the film is 0° (the longitudinal direction is 90°), the alignment axis angle of the liquid crystal compound was 14° on the air side and 95° on the side in contact with the optically anisotropic layer (1c). The alignment axis angle of the liquid crystal compound contained in the optically anisotropic layer is expressed as negative when clockwise (right-handed) and positive when counterclockwise (left-handed), with the width direction of the substrate being taken as the reference 0°, when observing the substrate from the surface side of the optically anisotropic layer. In addition, the twist angle of the liquid crystal compound is expressed by observing the substrate from the surface side of the optically anisotropic layer, and taking the orientation axis direction of the liquid crystal compound on the surface side (front side) as the reference, when the orientation axis direction of the liquid crystal compound on the substrate side (rear side) is clockwise (right-handed), it is negative, and when it is counterclockwise (left-handed), it is positive.

[0184] ------------------------------------------------------------------ Composition for forming optically anisotropic layer (1b) ------------------------------------------------------------------ The above rod-shaped liquid crystal compound (A) 100 parts by mass Ethylene oxide modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 4 parts by mass Photopolymerization initiator (Irgacure 819, manufactured by BASF) 3 parts by weight 0.60 parts by mass of the following left-twisted chiral agent (L1) 0.08 parts by mass of the above fluorine-containing compound C Methyl ethyl ketone 156 parts by mass ------------------------------------------------------------------

[0185] Left-twisted chiral agent (L1)

[0186] [ka]

[0187] By the above procedure, a laminate (1c-1b) was prepared in which the optically anisotropic layer (1c) and the optically anisotropic layer (1b) were directly laminated on a long cellulose acylate film. When the surface of the optically anisotropic layer (1c) in contact with the optically anisotropic layer (1b) was confirmed by the above method, the presence of a photoalignable polymer was confirmed.

[0188] (Formation of a laminate of an optically anisotropic layer (A), an optically anisotropic layer (B) and an optically anisotropic layer (C)) The surface side of the optically anisotropic layer (1a) formed on the long-length cellulose acylate film prepared above and the surface side of the optically anisotropic layer (1b) of the laminate (1c-1b) formed on the long-length cellulose acylate film prepared above were bonded to a continuous machine using an ultraviolet-curing adhesive. Subsequently, the cellulose acylate film on the optically anisotropic layer (1a) side was peeled off to expose the surface of the optically anisotropic layer (1a) that had been in contact with the cellulose acylate film. In this way, a retardation film (1c-1b-1a) was obtained in which the optically anisotropic layer (1c), the optically anisotropic layer (1b), and the optically anisotropic layer (1a) were laminated in this order on the long cellulose acylate film. The thickness of the retardation film (1c-1b-1a) was 4.0 μm. The water content of the obtained retardation film (1c-1b-1a) was 0.8%. The in-plane slow axis of the surface of the optically anisotropic layer (1a) side of the optically anisotropic layer (1b) was parallel to the in-plane slow axis of the optically anisotropic layer (1a).

[0189] (Preparation of Linear Polarizing Plate 1) The surface of the support of cellulose triacetate film TJ25 (manufactured by Fujifilm Corporation: thickness 25 μm) was subjected to an alkali saponification treatment. Specifically, the support was immersed in a 1.5N sodium hydroxide aqueous solution at 55° C. for 2 minutes, then washed in a water washing bath at room temperature, and further neutralized with 0.1N sulfuric acid at 30° C. After neutralization, the support was washed in a water washing bath at room temperature, and further dried with hot air at 100° C. to obtain a polarizer protective film. A rolled polyvinyl alcohol (PVA) film with a thickness of 60 μm was continuously stretched in the longitudinal direction in an iodine aqueous solution and dried to obtain a polarizer with a thickness of 13 μm. The luminous efficiency corrected single transmittance of the polarizer was 43%. At this time, the absorption axis direction of the polarizer coincided with the longitudinal direction. The above polarizer protective film was attached to one surface of the above polarizer using the following PVA adhesive to prepare a linear polarizing plate 1.

[0190] (Preparation of PVA adhesive) A PVA adhesive was prepared by dissolving 100 parts by mass of a polyvinyl alcohol resin having acetoacetyl groups (average degree of polymerization: 1200, degree of saponification: 98.5 mol%, degree of acetoacetylation: 5 mol%) and 20 parts by mass of methylol melamine in pure water at a temperature of 30°C to prepare an aqueous solution with a solids concentration of 3.7% by mass.

[0191] (Preparation of circular polarizing plate) The surface of the optically anisotropic layer (1a) of the long-sized retardation film (1c-1b-1a) prepared above and the surface of the polarizer (the surface opposite to the polarizer protective film) of the long-sized linear polarizing plate 1 prepared above were continuously bonded together using an ultraviolet-curable adhesive. Then, the cellulose acylate film on the optically anisotropic layer (1c) side was peeled off to expose the surface of the optically anisotropic layer (1c) that had been in contact with the cellulose acylate film. In this way, a circular polarizing plate (P1) consisting of a retardation film (1c-1b-1a) and a linear polarizing plate was produced. At this time, the polarizer protective film, the polarizer, the optically anisotropic layer (1a), the optically anisotropic layer (1b), and the optically anisotropic layer (1c) were laminated in this order, and the angle between the absorption axis of the polarizer and the slow axis of the optically anisotropic layer (1a) was 76°. In addition, the alignment axis angle of the liquid crystal compound on the optically anisotropic layer (1b) side of the optically anisotropic layer (1a) was 14°, with the width direction being taken as 0° as the reference, and was consistent with the slow axis direction of the optically anisotropic layer (1a). The thickness of the circular polarizing plate was 43 μm. The alignment axis angle of the liquid crystal compound contained in the optically anisotropic layer is expressed as negative when clockwise (right-handed) and positive when counterclockwise (left-handed) when observed from the surface side of the polarizing plate, with the width direction of the linear polarizing plate being taken as the reference 0°.

[0192] <Example 2> (Formation of alignment film) The photo-alignment film-forming material described in Example 1 of WO2016 / 002722 was applied onto the long cellulose acylate film prepared above. The coating film was then heated to 125° C. with hot air to harden it. The coating film was then irradiated with 313 nm polarized ultraviolet light to prepare a photo-alignment film.

[0193] (Formation of Optically Anisotropic Layer (B)) On the photo-alignment film prepared above, the composition for forming an optically anisotropic layer (1b) containing the rod-shaped liquid crystal compound having the above composition was applied using a Giesser coater, and heated with hot air at 80°C for 60 seconds. Subsequently, the obtained composition layer was irradiated with UV (500 mJ / cm2) at 80°C. 2 ) was carried out to fix the alignment of the liquid crystal compound, thereby forming an optically anisotropic layer (2b) corresponding to the optically anisotropic layer (B). The optically anisotropic layer (2b) had a thickness of 1.2 μm, a Δnd at a wavelength of 550 nm of 164 nm, and a twist angle of the liquid crystal compound of 81°. When viewed from the optically anisotropic layer (2b) side, assuming that the width direction of the film is 0° (the longitudinal direction is 90°), the alignment axis angle of the liquid crystal compound was −76° on the air side and 5° on the side in contact with the cellulose acylate film. The alignment axis angle of the liquid crystal compound contained in the optically anisotropic layer is expressed as negative when clockwise (right-handed) and positive when counterclockwise (left-handed), with the width direction of the substrate being taken as the reference 0°, when observing the substrate from the surface side of the optically anisotropic layer. In addition, the twist angle of the liquid crystal compound is expressed by observing the substrate from the surface side of the optically anisotropic layer, and taking the orientation axis direction of the liquid crystal compound on the surface side (front side) as the reference, when the orientation axis direction of the liquid crystal compound on the substrate side (rear side) is clockwise (right-handed), it is negative, and when it is counterclockwise (left-handed), it is positive.

[0194] (Formation of a laminate of an optically anisotropic layer (C) and an optically anisotropic layer (A)) (Formation of Optically Anisotropic Layer (2c)) An optically anisotropic layer (2c) having an alignment control ability on its surface was formed in the same manner as in the formation of the optically anisotropic layer (1c) of Example 1, except that the thickness of the composition layer was changed. The thickness of the optically anisotropic layer (2c) formed was 0.7 μm. The in-plane retardation Re at a wavelength of 550 nm was 0 nm, and the retardation Rth in the thickness direction at a wavelength of 550 nm was −96 nm. The average tilt angle of the long axis direction of the rod-like liquid crystal compound with respect to the film surface was 90°, and it was confirmed that the compound was aligned perpendicular to the film surface. In this manner, an optically anisotropic layer (2c) corresponding to the optically anisotropic layer (C) was formed.

[0195] (Formation of Optically Anisotropic Layer (2a)) Next, on the optically anisotropic layer (2c) prepared above, a composition for forming an optically anisotropic layer (2a) containing a rod-shaped liquid crystal compound having the following composition was applied using a Giesser coater, and heated with hot air at 80°C for 60 seconds. Next, the obtained composition layer was irradiated with UV (500 mJ / cm2) at 80°C. 2 ) was carried out to fix the alignment of the liquid crystal compound, thereby forming an optically anisotropic layer (2a) corresponding to the optically anisotropic layer (A). The thickness of the optically anisotropic layer (2a) was 1.2 μm. The retardation at a wavelength of 550 nm was 168 nm. The average tilt angle of the long axis direction of the rod-like liquid crystal compound with respect to the film surface was 0°, and it was confirmed that the compound was aligned horizontally with respect to the film surface. When the width direction of the film was 0° (the longitudinal direction was 90°), the slow axis was −76° when viewed from the optically anisotropic layer (2a) side.

[0196] ------------------------------------------------------------------ Composition for forming optically anisotropic layer (2a) ------------------------------------------------------------------ The above rod-shaped liquid crystal compound (A) 100 parts by mass Ethylene oxide modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 4 parts by mass Photopolymerization initiator (Irgacure 819, manufactured by BASF) 3 parts by weight 0.08 parts by mass of the above fluorine-containing compound C Methyl ethyl ketone 156 parts by mass ------------------------------------------------------------------

[0197] By the above procedure, a laminate (2c-2a) was prepared in which the optically anisotropic layer (2c) and the optically anisotropic layer (2a) were directly laminated on a long cellulose acylate film. When the surface of the optically anisotropic layer (2c) in contact with the optically anisotropic layer (2a) was confirmed by the above method, the presence of a photoalignable polymer was confirmed.

[0198] (Formation of a laminate of an optically anisotropic layer (A), an optically anisotropic layer (C) and an optically anisotropic layer (B), and preparation of a circularly polarizing plate) The surface of the optically anisotropic layer (2a) of the laminate (2c-2a) formed on the long cellulose acylate film prepared above was continuously bonded to the surface of the polarizer (the surface opposite to the polarizer protective film) of the long linear polarizing plate 1 prepared above using an ultraviolet-curable adhesive. Then, the cellulose acylate film on the optically anisotropic layer (2c) side was peeled off to expose the surface of the optically anisotropic layer (2c) that had been in contact with the cellulose acylate film. The exposed surface of the optically anisotropic layer (2c) and the surface of the optically anisotropic layer (2b) formed on the long cellulose acylate film prepared above were attached to a continuous machine using an ultraviolet-curing adhesive. Then, the cellulose acylate film on the optically anisotropic layer (2b) side was peeled off to expose the surface of the optically anisotropic layer (2b) that had been in contact with the cellulose acylate film. In this way, a circular polarizing plate (P2) consisting of the optical retardation film (2b-2c-2a) and the linear polarizing plate 1 was produced. The thickness of the retardation film (2b-2c-2a) was 4.0 μm. The water content of the obtained retardation film (2b-2c-2a) was 0.8%. At this time, the polarizer protective film, the polarizer, the optically anisotropic layer (2a), the optically anisotropic layer (2c), and the optically anisotropic layer (2b) were laminated in this order, and the angle between the absorption axis of the polarizer and the slow axis of the optically anisotropic layer (2a) was 14°. In addition, the alignment axis angle of the liquid crystal compound on the optically anisotropic layer (2c) side of the optically anisotropic layer (2b) was 76°, with the width direction being taken as the reference angle of 0°, which coincided with the slow axis direction of the optically anisotropic layer (2a). The thickness of the circular polarizing plate was 43 μm. The alignment axis angle of the liquid crystal compound contained in the optically anisotropic layer is expressed as negative when clockwise (right-handed) and positive when counterclockwise (left-handed) when observed from the surface side of the polarizing plate, with the width direction of the linear polarizing plate being taken as the reference 0°.

[0199] <Comparative Example 1> In the same manner as in Example 1, an optically anisotropic layer (1c) was formed on a long cellulose acylate film. Next, on the optically anisotropic layer (1c) prepared above, an optically anisotropic layer (1h) containing a reverse wavelength dispersion liquid crystal compound was formed using the composition A-1 described in Example 9 of Patent Document 1. The retardation at a wavelength of 550 nm was 138 nm. It was confirmed that the average tilt angle of the long axis direction of the reverse wavelength dispersion liquid crystal compound with respect to the film surface was 0°, and that the compound was aligned horizontally with respect to the film surface. In addition, when the width direction of the film was 0° (the longitudinal direction was 90°), the slow axis was 45° when viewed from the optically anisotropic layer (1h) side. In this way, a laminate was prepared in which an optically anisotropic layer (1c) containing a vertically aligned rod-like liquid crystal compound and an optically anisotropic layer (1h) containing a horizontally aligned reverse wavelength dispersion liquid crystal compound were directly laminated together.

[0200] The linear polarizing plate 1 prepared in the same manner as in Example 1 and the laminate including the optically anisotropic layer (1c) and the optically anisotropic layer (1h) prepared above were continuously bonded together using an ultraviolet-curable adhesive so that the surface of the optically anisotropic layer (1h) faced the surface of the polarizer (the surface opposite to the polarizer protective film) of the linear polarizing plate 1. Then, the cellulose acylate film on the optically anisotropic layer (1c) side was peeled off to expose the surface of the optically anisotropic layer (1c) that had been in contact with the cellulose acylate film. In this way, a circular polarizing plate composed of a linear polarizing plate was produced. At this time, the polarizer protective film, the polarizer, the optically anisotropic layer (1h), and the optically anisotropic layer (1c) were laminated in this order, and the angle between the absorption axis of the polarizer and the slow axis of the optically anisotropic layer (1h) was 45°.

[0201] <Comparative Example 2> In the same manner as in Example 1, an optically anisotropic layer (1c) was formed on a long cellulose acylate film. Next, the optically anisotropic layer (2h) was formed on the optically anisotropic layer (1c) prepared above using the optically anisotropic layer forming composition (2a). The retardation at a wavelength of 550 nm was 138 nm. It was confirmed that the average tilt angle of the long axis direction of the rod-shaped liquid crystal compound with respect to the film surface was 0°, and that the compound was aligned horizontally with respect to the film surface. In addition, when the width direction of the film was 0° (the longitudinal direction was 90°), the slow axis was 45° when viewed from the optically anisotropic layer (2h) side. In this manner, a laminate was prepared in which an optically anisotropic layer (1c) containing a vertically aligned rod-like liquid crystal compound and an optically anisotropic layer (2h) containing a horizontally aligned rod-like liquid crystal compound were directly laminated together.

[0202] The linear polarizing plate 1 prepared in the same manner as in Example 1 and the laminate including the optically anisotropic layer (1c) and the optically anisotropic layer (2h) prepared above were continuously bonded together using an ultraviolet-curable adhesive so that the surface of the optically anisotropic layer (2h) faced the surface of the polarizer (the surface opposite to the polarizer protective film) of the linear polarizing plate 1. Then, the cellulose acylate film on the optically anisotropic layer (1c) side was peeled off to expose the surface of the optically anisotropic layer (1c) that had been in contact with the cellulose acylate film. In this way, a circular polarizing plate composed of a linear polarizing plate was produced. At this time, the polarizer protective film, the polarizer, the optically anisotropic layer (2h), and the optically anisotropic layer (1c) were laminated in this order, and the angle between the absorption axis of the polarizer and the slow axis of the optically anisotropic layer (2h) was 45°.

[0203] <Comparative Example 3> (Formation of Optically Anisotropic Layer (3h)) The alignment film disposed on the cellulose acylate film used in the preparation of the optically anisotropic layer A in Example 1 was subjected to continuous rubbing treatment. At this time, the longitudinal direction of the long film was parallel to the transport direction, and the angle between the longitudinal direction of the film (transport direction) and the rotation axis of the rubbing roller was 75°. The longitudinal direction of the film (transport direction) was set to 90°, and the rotation axis of the rubbing roller was at 165°, with the film width direction as the reference (0°) and the clockwise direction as a positive value when observed from the film side.

[0204] Onto the above-mentioned rubbed alignment film, the same optically anisotropic layer coating solution (1a) as in Example 1 was applied using a Giesser coater to form an optically anisotropic layer (3h) corresponding to the optically anisotropic layer (A). The thickness of the optically anisotropic layer (3h) was 2.0 μm. The retardation at a wavelength of 550 nm was 250 nm. The average inclination angle of the disc surface of the discotic liquid crystal compound with respect to the film surface was 90°, and it was confirmed that the compound was oriented perpendicularly to the film surface. The angle of the slow axis of the optically anisotropic layer (3h) was parallel to the rotation axis of the rubbing roller, and the slow axis was 165° when viewed from the optically anisotropic layer (3h) side, assuming that the width direction of the film was 0° (the longitudinal direction was 90° counterclockwise and -90° clockwise).

[0205] (Formation of Optically Anisotropic Layer (4h)) A continuous rubbing treatment was performed on the alignment film disposed on the cellulose acylate film used in the preparation of the optically anisotropic layer A in Example 1. At this time, the longitudinal direction of the long film was parallel to the transport direction, and the angle between the longitudinal direction of the film (transport direction) and the rotation axis of the rubbing roller was 75°.

[0206] If the longitudinal direction of the film (transport direction) is 90° and the width direction of the film as observed from the film side is expressed as the reference (0°) and clockwise directions are expressed as positive values, the rotation axis of the rubbing roller is at 165°.

[0207] Onto the above-mentioned rubbed alignment film, the same optically anisotropic layer forming composition (1a) as in Example 1 was applied using a Giesser coater to form an optically anisotropic layer (4h) corresponding to the optically anisotropic layer (A). The thickness of the optically anisotropic layer (4h) was 0.8 μm. The retardation at a wavelength of 550 nm was 120 nm. The average tilt angle of the long axis of the rod-shaped liquid crystal compound with respect to the film surface was 0°, and it was confirmed that the compound was aligned horizontally with respect to the film surface. The angle of the slow axis of the optically anisotropic layer (4h) was parallel to the rotation axis of the rubbing roller, and the slow axis was 105° when viewed from the optically anisotropic layer (4h) side, assuming that the width direction of the film was 0° (the longitudinal direction was 90° counterclockwise and -90° clockwise).

[0208] The linear polarizing plate 1 prepared in the same manner as in Example 1 and the cellulose acylate film on which the optically anisotropic layer (3h) was arranged were continuously laminated together using an ultraviolet-curing adhesive so that the surface of the optically anisotropic layer (3h) and the surface of the polarizer of the linear polarizing plate 1 (the surface opposite to the polarizer protective film) faced each other. Then, the cellulose acylate film on the optically anisotropic layer (3h) side was peeled off to expose the surface of the optically anisotropic layer (3h) that had been in contact with the cellulose acylate film. The exposed surface of the optically anisotropic layer (3h) and the surface side of the optically anisotropic layer (4h) formed on the long cellulose acylate film prepared above were laminated to a continuous machine using an ultraviolet-curing adhesive. Then, the cellulose acylate film on the optically anisotropic layer (4h) side was peeled off to expose the surface of the optically anisotropic layer (4h) that had been in contact with the cellulose acylate film. In this way, a circular polarizing plate composed of a linear polarizing plate was produced. At this time, the polarizer protective film, the polarizer, the optically anisotropic layer (3h), and the optically anisotropic layer (4h) were laminated in this order, and the angle between the absorption axis of the polarizer and the slow axis of the optically anisotropic layer (3h) was 75°.

[0209] <Comparative Example 4> Instead of the optically anisotropic layer (1c) of Example 1, a cellulose acylate film (3c) was prepared according to the same procedure as in Example 15 of JP-A-2006-265309, except that the stretching was not performed. Re and Rth were equal to those of the optically anisotropic layer (1c). The cellulose acylate film (3c) was subjected to an alkali saponification treatment to form an alignment film, and then the optically anisotropic layer (3b) was formed. The optically anisotropic layer (3b) was produced in the same manner as the optically anisotropic layer (1b) in Example 1, except that the optically anisotropic layer (1c) in Example 1 was changed to the above-mentioned cellulose acylate film (3c). The surface side of the optically anisotropic layer (1a) prepared in Example 1 and the surface side of the optically anisotropic layer (3b) prepared above were laminated in a continuous machine using an ultraviolet curing adhesive. Then, the cellulose acylate film on the optically anisotropic layer (1a) side was peeled off to obtain a retardation film (3c-3b-1a). The moisture content of the obtained retardation film was 2.1%, and the thickness was 303 μm.

[0210] The surface of the optically anisotropic layer (1a) of the long-sized retardation film (3c-3b-1a) prepared above and the surface of the polarizer of the long-sized linear polarizing plate 1 prepared above (the surface opposite to the polarizer protective film) were continuously bonded together using an ultraviolet-curing adhesive. In this way, a circular polarizing plate consisting of the retardation film (3c-3b-1a) and the linear polarizing plate was produced. At this time, the polarizer protective film, the polarizer, the optically anisotropic layer (1a), the optically anisotropic layer (3b), and the optically anisotropic layer (3c) were laminated in this order, and the angle between the absorption axis of the polarizer and the slow axis of the optically anisotropic layer (1a) was 76°. In addition, the alignment axis angle of the liquid crystal compound on the optically anisotropic layer (1a) side of the optically anisotropic layer (3b) was 14°, with the width direction being taken as the reference angle of 0°, which coincided with the slow axis direction of the optically anisotropic layer (1a). The thickness of the circular polarizing plate was 342 μm.

[0211] <Color and reflectance measurements> A reflective substrate was prepared by attaching aluminum foil to a 100 μm thick PET film using an adhesive sheet. The circularly polarizing plate produced in the Examples and Comparative Examples was placed on the aluminum foil side of the obtained reflective substrate to obtain a laminate (corresponding to a specific laminate). The reflective substrate and the circularly polarizing plate were laminated so that the retardation film of the circularly polarizing plate and the aluminum foil faced each other. The obtained laminate was observed from the circularly polarizing plate side using a spectrophotometer (manufactured by Konica Minolta), and the chromaticity a at all azimuth angles (0 to 360°) of a polar angle of 40° from the normal direction of the circularly polarizing plate of the laminate was measured. * and chromaticity b * In addition, the reflectance of the laminate was measured at all azimuth angles (0 to 360°) with a polar angle of 40° from the normal direction of the circularly polarizing plate, according to the procedure described above. The azimuth angle is expressed as an angle between the absorption axis of the polarizer and the polarizer, and is expressed as a positive value in the counterclockwise direction with respect to the absorption axis direction of the polarizer when viewed from the circular polarizing plate side of the obtained laminate.

[0212] <Fabrication of organic EL display device> (Mounting to a display device) A Royole FlexPai equipped with an organic EL display panel (organic EL display element) was disassembled, and the circular polarizer was peeled off from the organic EL display device. Next, the circular polarizer prepared above was attached to the isolated organic EL display panel using a pressure-sensitive adhesive so that the protective film was placed on the outside, thereby producing an organic EL display device.

[0213] (Display performance evaluation) (Front direction) The organic EL display device thus produced was made to display black, and the display was unfolded and observed from the front under bright light, and the color unevenness was evaluated according to the following criteria. The results are shown in Table 1. A: No visible color unevenness at all (acceptable) B: Slight color unevenness is visible, but does not affect use (tolerable) C: Color unevenness is visible, and there is a problem in use.

[0214] (Diagonal) The fabricated organic EL display device was black-displayed, and in the state where the display was bent, it was observed from an oblique direction over the full azimuth angle under bright light, and the color unevenness was evaluated according to the following criteria. The results are shown in Table 1. A: No color unevenness is visually recognized (acceptable) B: Slight color unevenness is visually recognized, but there is no problem in use (acceptable) C: Color unevenness is visually recognized and there is a problem in use.

[0215] (Evaluation over time) After leaving the fabricated organic EL display device standing for 72 hours in an environment of 25°C and a relative humidity of 10%, the organic EL display device was black-displayed, and in the state where the display was bent, the color unevenness was evaluated according to the following criteria under bright light. The results are shown in Table 1. A: No change over time B: There was a change over time

[0216] In Table 1, in the column of "liquid crystal compound type", "discotic" means that the optically anisotropic layer is a layer formed using a discotic liquid crystal compound, "rod-like liquid crystal" means that the optically anisotropic layer is a layer formed using a rod-like liquid crystal compound, and "inverse dispersion liquid crystal" means that the optically anisotropic layer is a layer formed using a liquid crystal compound with inverse wavelength dispersion. In the column of "orientation state", "horizontal" means that the liquid crystal compound is horizontally oriented. "Twisted" means that the liquid crystal compound is twisted and oriented. "Vertical" means that the liquid crystal compound is vertically oriented. In Table 1, the column of "reflectivity" represents the reflectivity at the full azimuth angle measured in the above <chromaticity and reflectivity measurement>. "<X%" means that the reflectivity at any azimuth angle is less than X%, and ">Y%" means that the reflectivity at any azimuth angle is more than Y%. In Table 1, "a * " column represents the absolute value of the chromaticity a * at the full azimuth angle measured in the above <chromaticity and reflectivity measurement>. "<X" means that the absolute value of the chromaticity a * at any azimuth angle is less than X, and ">Y" means that the absolute value of the chromaticity a *It means that the absolute value of In Table 1, the column of "b * " represents the absolute value of chromaticity b at all azimuth angles measured by the above <Chromaticity and Reflectance Measurement>, and "<X" means that the absolute value of chromaticity b at any azimuth angle * is less than X, and ">Y" means that the absolute value of chromaticity b at any azimuth angle * is greater than Y. * It means that the absolute value of

[0217]

Table 1

[0218] From the results shown in Table 1 above, it was confirmed that the circular polarizing plate of the present invention can suppress color unevenness in the front direction and the diagonal direction when used in an organic EL display device. Also, the occurrence of color unevenness over time was suppressed. On the other hand, the circular polarizing plate of the comparative example did not obtain the desired effect when used in an organic EL display device.

[0219] <Example 3> In the same manner as in Example 1, a retardation film (1c-1b-1a) in which an optically anisotropic layer (1c), an optically anisotropic layer (1b), and an optically anisotropic layer (1a) were laminated in this order was obtained on a long cellulose acetate film. Next, as the linear polarizing plate 3, a polarizer using a dichroic organic dye and a polymerizable liquid crystal was prepared. A coating liquid PA1 for forming an alignment layer described later was continuously coated on a cellulose triacetate film TJ40 (manufactured by Fuji Film: thickness 40 μm) with a wire bar. The support on which the coating film was formed was dried with warm air at 140 °C for 120 seconds, and then, the coating film was irradiated with polarized ultraviolet rays (10 mJ / cm 2 , using an ultra-high pressure mercury lamp) to form an optical alignment layer PA1, and a TAC film with the optical alignment layer PA1 was obtained. The film thickness of the optical alignment layer PA1 was 0.3 μm.

[0220] ――――――――――――――――――――――――――――――――― Coating solution for forming alignment layer PA1 ------------------------------------------------------------------ 100.00 parts by weight of the following polymer PA-1 5.00 parts by weight of the following acid generator PAG-1 0.005 parts by weight of the following acid generator CPI-110TF Xylene 1220.00 parts by mass Methyl isobutyl ketone 122.00 parts by weight ------------------------------------------------------------------

[0221] Polymer PA-1

[0222] [ka]

[0223] Acid generator PAG-1

[0224] [ka]

[0225] Acid generator CPI-110F

[0226] [ka]

[0227] On the obtained photoalignment layer PA1, the following composition for forming an optically absorptive anisotropic layer P2 was continuously applied with a wire bar to form a coating film P2. Next, the coating film P2 was heated at 140° C. for 30 seconds, after which the coating film P2 was cooled to room temperature (23° C.). The resulting coating film P2 was then heated at 90° C. for 60 seconds and cooled again to room temperature. Then, an LED (light emitting diode) lamp (center wavelength 365 nm) was used to illuminate the specimen at an intensity of 200 mW / cm 2An optically absorptive anisotropic layer P2 was formed on the photo-alignment layer PA1 by irradiating the layer for 2 seconds under the irradiation conditions of: The molar content of the radical polymerizable group was 1.17 mmol / g. The optically absorptive anisotropic layer P2 had a thickness of 1.3 μm.

[0228] ---------------------------------------------------------------------------------- Optically absorptive anisotropic layer forming composition P2 ---------------------------------------------------------------------------------- 0.25 parts by weight of the following dichroic dye D-4 0.36 parts by weight of the following dichroic dye D-5 0.59 parts by weight of the following dichroic dye D-6 2.21 parts by weight of the following polymer liquid crystal compound P-1 1.36 parts by weight of the following low molecular weight liquid crystal compound M-1 Polymerization initiator IRGACUREOXE-02 (BASF) 0.150 parts by mass 0.026 parts by weight of the following surfactant F-1 Cyclopentanone 46.00 parts by mass Tetrahydrofuran 46.00 parts by weight Benzyl alcohol 3.00 parts by weight ----------------------------------------------------------------------------------

[0229] Dichroic dye D-4

[0230] [ka]

[0231] Dichroic dye D-5

[0232] [ka]

[0233] Dichroic dye D-6

[0234] [ka]

[0235] Polymer liquid crystal compound P-1

[0236] [ka]

[0237] Low molecular liquid crystal compound M-1

[0238] [ka]

[0239] Surfactant F-1

[0240] [ka]

[0241] Onto the obtained light absorption anisotropic layer P2, the following composition for forming a cured layer K1 was continuously applied with a wire bar to form a coating film. The coating is then dried at room temperature and then illuminated with a high-pressure mercury lamp at an illumination intensity of 28 mW / cm 2 By irradiating for 15 seconds under the irradiation conditions above, a hardened layer K1 was formed on the light absorption anisotropic layer P2. The thickness of the hardened layer K1 was 0.05 μm. ---------------------------------------------------------------------------------- Composition K1 for forming hardened layer ---------------------------------------------------------------------------------- 2.61 parts by weight of the mixture L1 of the following rod-shaped liquid crystal compounds 0.11 parts by weight of the following modified trimethylolpropane triacrylate 0.05 parts by weight of the following photopolymerization initiator I-1 0.21 parts by weight of the following surfactant F-3 Methyl isobutyl ketone 297 parts by weight ----------------------------------------------------------------------------------

[0242] Mixture L1 of rod-shaped liquid crystal compounds (the numerical values ​​in the formula below represent mass %, and R represents a group bonded via an oxygen atom).

[0243] [ka]

[0244] Modified Trimethylolpropane Triacrylate [ka]

[0245] Photopolymerization initiator I-1

[0246] [ka]

[0247] Surfactant F-3

[0248] [ka]

[0249] The following oxygen barrier layer-forming composition B2 was continuously applied onto the cured layer K1 with a wire bar, and then dried for 2 minutes with hot air at 100°C to form an oxygen barrier layer B2 with a thickness of 1.0 μm on the cured layer K1, thereby producing a polarizing film including a light absorption anisotropic layer P2. The luminous efficiency corrected single transmittance of the polarizing film was 43%. ---------------------------------------------------------------------------------- Composition B2 for forming oxygen barrier layer ---------------------------------------------------------------------------------- 3.80 parts by weight of the following modified polyvinyl alcohol Initiator Irg2959 0.20 parts by weight ·Water 70 parts by mass Methanol 30 parts by weight ----------------------------------------------------------------------------------

[0250] Modified Polyvinyl Alcohol

[0251] [ka]

[0252] The oxygen barrier layer B2 side of the polarizing film and the polarizing plate protective film were attached using an adhesive sheet. Then, only TJ40 of the polarizing film was peeled off, and the peeled surface was continuously attached to the surface of the optically anisotropic layer (1a) of the long retardation film (1c-1b-1a) using an ultraviolet-curing adhesive. Next, the cellulose acylate film of the optically anisotropic layer (1c) was peeled off, and the surface of the optically anisotropic layer (1c) that had been in contact with the cellulose acylate film was exposed. In this way, a circular polarizing plate was produced. The thickness of the circular polarizing plate was 38 μm.

[0253] <Example 4> A circular polarizing plate was produced in the same direction as in Example 3, except that the thickness of the light absorption anisotropic layer P2 in Example 3 was 0.8 μm. The luminous efficiency corrected single transmittance of the polarizing film was 45%. The thickness of the circular polarizing plate was 37 μm.

[0254] (Display performance evaluation) When the circular polarizing plate of Example 3 or 4 was mounted on an organic EL display device in the same manner as in Example 1, the display performance was confirmed to be equivalent to that of Example 1. Furthermore, the overall thickness of the circular polarizing plate could be reduced, improving the yield rate during processing into irregular shapes such as curved displays.

[0255] <Example 5> (Fabrication of circular polarizers using highly refractive adhesives) The surface side of the optically anisotropic layer (1a) formed on the long cellulose acylate film prepared in the same manner as in Example 1 and the surface side of the optically anisotropic layer (1b) of the laminate (1c-1b) formed on the long cellulose acylate film prepared above were continuously bonded together using an ultraviolet-curing adhesive. As the ultraviolet-curing adhesive, an adhesive was used in which a high refractive index monomer was added to an acrylic compound to control the refractive index after curing to 1.53. The refractive index difference between the averaged refractive index in the axial direction of the adjacent optically anisotropic layers and the adhesive was both within 0.08. A circularly polarizing plate was prepared in the same manner as in Example 1, except that the refractive index was controlled.

[0256] <Example 6> A circularly polarizing plate was produced in the same manner as in Example 1, using an ultraviolet-curable adhesive whose refractive index after curing was controlled to 1.58 in the same manner as in Example 5. The difference in the average refractive index in the axial direction of adjacent optically anisotropic layers and the refractive index of the adhesive were both within 0.05.

[0257] <Example 7> A UV-curable adhesive with a refractive index controlled to 1.53 was prepared in the same manner as in Example 5. The surface of the optically anisotropic layer (1a) of the long retardation film (1c-1b-1a) prepared in Example 5 and the surface of the polarizer of the long linear polarizing plate 1 prepared above (the surface opposite to the polarizer protective film) were continuously bonded together using a UV-curable adhesive with a refractive index controlled to 1.53 after curing. A circular polarizing plate was prepared in the same manner as in Example 5 except for the above. The difference in the average refractive index of the polarizer and the refractive index of the adhesive were both within 0.05.

[0258] (Display performance evaluation) When the polarizing plates of Examples 5, 6, and 7 were mounted on an organic EL display device in the same manner as in Example 1, display performance equivalent to that of Example 1 was confirmed. [Explanation of symbols]

[0259] 1, 2 Phase difference film 10, 20 Circular polarizer 1a, 2a Optically anisotropic layer (A) 1b, 2b Optically anisotropic layer (B) 1c, 2c Optically anisotropic layer (C) 3 Polarizer 30 Aluminum Sheet 40 Specific laminate

Claims

1. A circular polarizing plate comprising a polarizer and a retardation film laminated on one surface side of the polarizer, The moisture content of the retardation film is 1.8% or less, The circularly polarizing plate and the aluminum sheet are laminated together so that the retardation film in the circularly polarizing plate faces the aluminum sheet, and the chromaticity a of the obtained laminate at all azimuth angles of a polar angle of 40° from the normal direction of the circularly polarizing plate is * and chromaticity b * When measuring the chromaticity a * Absolute value and chromaticity b * The absolute value of is 10 or less, When the reflectance of the laminate is measured at all azimuth angles of a polar angle of 40° from the normal direction of the circularly polarizing plate, the reflectance is 3.0% or less at all azimuth angles, The retardation film includes an optically anisotropic layer (A), an optically anisotropic layer (B), and an optically anisotropic layer (C), the optically anisotropic layer (A) is an optically anisotropic layer exhibiting negative uniaxiality, the optically anisotropic layer (B) is an optically anisotropic layer in which a rod-like liquid crystal compound is fixed and twisted and aligned with a helical axis in the thickness direction, the optically anisotropic layer (C) is a layer in which vertically aligned rod-like liquid crystal compounds or horizontally aligned discotic liquid crystal compounds are fixed, The in-plane retardation of the optically anisotropic layer (A) at a wavelength of 550 nm is 140 to 220 nm, the value of the product Δnd of the refractive index anisotropy Δn of the optically anisotropic layer (B) measured at a wavelength of 550 nm and the thickness d of the optically anisotropic layer (B) is 140 to 220 nm; The twist angle of the twisted rod-like liquid crystal compound is in the range of 90±30°, an in-plane slow axis of the optically anisotropic layer (A) is parallel to an in-plane slow axis of the optically anisotropic layer (B) on the surface thereof facing the optically anisotropic layer (A); A circular polarizing plate in which, when the optically anisotropic layer (C) is a layer formed by fixing vertically aligned rod-like liquid crystal compounds, the retardation in the thickness direction of the optically anisotropic layer (C) at a wavelength of 550 nm is −140 to −20 nm, and, when the optically anisotropic layer (C) is a layer formed by fixing horizontally aligned discotic liquid crystal compounds, the retardation in the thickness direction of the optically anisotropic layer (C) at a wavelength of 550 nm is 20 to 140 nm. The moisture content of the retardation film is a value measured after conditioning for 24 hours or more in an environment of a temperature of 25° C. and a relative humidity of 60%, and the moisture content is measured by the Karl Fischer method. The chromaticity a * and the chromaticity b * is the L standardized by the International Commission on Illumination (CIE). * a * b * Represents chromaticity in a color system. The reflectance refers to the luminosity-corrected reflectance in the wavelength range of 400 to 750 nm. The reflectance of the aluminum sheet is 80 to 90%, and any reflectance within this range satisfies the above-mentioned chromaticity and reflectance conditions.

2. The circular polarizing plate according to claim 1 , wherein the retardation film has a thickness of 30 μm or less.

3. 3. The circularly polarizing plate according to claim 1, wherein the retardation film is formed by laminating three optically anisotropic layers.

4. 4. The circularly polarizing plate according to claim 1, wherein the retardation film is formed by laminating three optically anisotropic layers each having an aligned liquid crystal compound fixed therein.

5. the polarizer is formed using a composition containing a polymerizable liquid crystal compound, 5. The circularly polarizing plate according to claim 1, wherein the polarizer has a thickness of 8 μm or less.

6. An organic electroluminescence display device comprising the circular polarizer according to any one of claims 1 to 5.

7. A display device having the circular polarizer according to any one of claims 1 to 5, The display device, wherein the circular polarizing plate is disposed so as to conform to a curved surface of the display device.

Citation Information

Patent Citations

  • Optical compensation sheet, polarizing plate and liquid crystal display

    JP2005037809A

  • Polarizing plate with optical compensation layer and image display device using the same

    JP2007140480A

  • Optically anisotropic body, and manufacturing method of the same

    JP2021001972A

  • Polymerizable liquid crystal composition, optically anisotropic substance, and manufacturing method therefor

    JP2021002026A

  • Flexible display device

    US20180149786A1