Fiber coating rubber composition and marine hose
A coating rubber composition with natural rubber, styrene-butadiene rubber, butadiene rubber, a tackifier, sulfur, and a bismaleimide compound addresses adhesion issues in rubber products by ensuring strong bonding to fiber reinforcing materials even after long-term vulcanization, enhancing uniformity and processability.
Patent Information
- Application Number
- JP2020089456
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-22
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-05-22
AI Technical Summary
Existing rubber products, particularly large-diameter hoses like marine hoses, face issues with decreased adhesion between fiber reinforcing materials and coated rubber due to prolonged vulcanization times, and existing compositions struggle with uniform mixing and adhesiveness.
A coating rubber composition comprising natural rubber, styrene-butadiene rubber, butadiene rubber, a tackifier, sulfur, and a bismaleimide compound, with specific ratios and types of components to enhance adhesion to fiber reinforcing materials even after long-term vulcanization.
The composition achieves excellent adhesion to fiber reinforcing materials, maintaining strong bonding even after prolonged vulcanization, with improved uniformity and processability.
Smart Images

Figure 0007583241000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a fiber coating rubber composition and a marine hose. [Background technology]
[0002] Conventionally, rubber products are generally reinforced with a reinforcing material such as a fiber reinforcing material (a reinforcing material made of fiber) in order to improve their mechanical strength. Examples of the fiber reinforcing material include polyester fiber and polyamide fiber. For example, Patent Document 1 proposes a fiber-reinforced rubber product in which a rubber body is reinforced with polyester fibers and the rubber composition containing 1.0 to 5.0 PHR of a maleimide-based vulcanizing agent is molded and vulcanized, with the aim of providing a high-quality fiber-reinforced rubber product by preventing a decrease in strength and adhesiveness of polyester fibers due to vulcanization in a rubber product reinforced with polyester fibers.
[0003] Rubber products also include large-sized products such as large-diameter hoses. A specific example of a large-diameter hose is a marine hose. Marine hoses are used on the sea to transport oil and the like. When manufacturing a large product (such as a marine hose) having a rubber layer and a reinforcing layer made of a fiber reinforcing material and a coating rubber, it is necessary to extend the vulcanization time of the rubber layer. On the other hand, by extending the vulcanization time as described above, there is a problem that the adhesion between the fiber reinforcing material and the coating rubber in the reinforcing layer is reduced.
[0004] In response to the above-mentioned problems, for example, Patent Document 2 proposes a method for manufacturing a fluid transport hose in which an inner rubber layer is coated around the outer periphery of a mandrel, at least one reinforcing layer group is arranged around the outer periphery of the inner rubber layer, and a reinforcing layer made of a coating rubber containing butadiene rubber and an organic fiber cord is laminated, and an outer rubber layer is coated on the outside of the arranged reinforcing layer group to form a hose body, and the hose body is then steam vulcanized, in which the organic fiber of the organic fiber cord constituting the reinforcing layer is made of polyketone fiber or a composite fiber of polyketone fiber and other fiber. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 11-269276 [Patent Document 2] JP 2010-173110 A Summary of the Invention [Problem to be solved by the invention]
[0006] In this situation, the present inventors prepared a fiber-coated rubber composition with reference to Patent Document 1, applied it to a fiber reinforcing material, and evaluated it. As a result, it became clear that such a composition may have low adhesion (hereinafter, this may be simply referred to as "adhesion") between the fiber reinforcing material and the coating rubber (obtained by vulcanizing the above composition) after long-term vulcanization (Comparative Example 2). It has become clear that the composition prepared with reference to Patent Document 2 may not satisfy the recently required level of adhesiveness (Comparative Example 1). In addition, since a ternary rubber composition containing natural rubber, styrene-butadiene rubber, and butadiene rubber as rubber components is a ternary system, it is difficult to make the rubber composition into a homogeneous mixed state. It was presumed that if a bismaleimide compound is further added to the ternary rubber composition and the rubber composition is not homogeneous, the required level of adhesion cannot be achieved.
[0007] Therefore, an object of the present invention is to provide a fiber coating rubber composition which has excellent adhesion to fiber reinforcing materials even after long-term vulcanization. Another object of the present invention is to provide a marine hose. [Means for solving the problem]
[0008] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems and have found that a composition containing a rubber component including natural rubber, styrene-butadiene rubber, and butadiene rubber, a tackifier, sulfur, and a bismaleimide compound has excellent adhesion to fiber reinforcing materials even after long-term vulcanization, thereby completing the present invention. The present invention is based on the above findings and has the following specific configuration to solve the above problems.
[0009] [1] A rubber component including natural rubber, styrene-butadiene rubber, and butadiene rubber; A tackifier; Sulfur and A fiber coating rubber composition comprising a bismaleimide compound. [2] The fiber coating rubber composition according to [1], wherein the content of the butadiene rubber is 15 parts by mass or more and 30 parts by mass or less in 100 parts by mass of the rubber component. [3] The fiber coating rubber composition according to [1] or [2], wherein the content of the bismaleimide compound is 0.2 parts by mass or more and 1.5 parts by mass or less per 100 parts by mass of the rubber component. [4] The fiber coating rubber composition according to any one of [1] to [3], wherein the tackifier comprises at least one selected from the group consisting of an aliphatic petroleum resin, an aromatic petroleum resin, an alkylphenol resin, a terpene resin, a rosin resin, and a coumarone-indene resin. [5] The fiber coating rubber composition according to any one of [1] to [4], wherein the content of the tackifier is 2.0 parts by mass or more and 6.0 parts by mass or less per 100 parts by mass of the rubber component. [6] A marine hose formed using the fiber coating rubber composition according to any one of [1] to [5]. Effect of the Invention
[0010] The fiber-coating rubber composition of the present invention has excellent adhesion to fiber reinforcing materials even after long-term vulcanization. The marine hose of the present invention has excellent adhesion between the coating rubber and the fiber reinforcing material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this specification, unless otherwise specified, each component may be used alone or in combination of two or more substances corresponding to that component. When a component contains two or more substances, the content of the component means the total content of the two or more substances. In this specification, better adhesion (also simply referred to as "adhesion") between the coating rubber and the fiber reinforcing material after long-term vulcanization may be referred to as better effects of the present invention.
[0012] [Fiber Coating Rubber Composition] The fiber coating rubber composition of the present invention (the composition of the present invention) is a rubber component including natural rubber, styrene-butadiene rubber, and butadiene rubber; A tackifier; Sulfur and and a bismaleimide compound. Each component contained in the composition of the present invention will be described in detail below.
[0013] <<Rubber component>> In the present invention, the rubber component contains natural rubber (NR), styrene butadiene rubber (SBR), and butadiene rubber (BR). The rubber component may further contain a rubber other than NR, SBR, and BR. The rubber other than NR etc. is not particularly limited. It is preferable that the rubber components consist of only NR, SBR and BR, from the viewpoints of excellent ease of production of the rubber composition and superior effects of the present invention.
[0014] <Natural rubber> In the present invention, the natural rubber (NR) as the rubber component is not particularly limited, and examples thereof include conventionally known rubbers.
[0015] NR content The content of the NR is preferably from 40 to 70 parts by mass, and more preferably from 50 to less than 60 parts by mass, per 100 parts by mass of the rubber component, from the viewpoints of obtaining excellent effects of the present invention, the balance between the initial elongation at break, high adhesive strength to the fiber (fiber reinforcing material) (e.g., after initial vulcanization) and heat aging resistance, and processability of the composition (e.g., mixing processability of the composition; the same applies below).
[0016] <Styrene butadiene rubber> In the present invention, the styrene-butadiene rubber (SBR) as the rubber component is not particularly limited as long as it is a copolymer of styrene and butadiene. For example, conventionally known ones can be mentioned.
[0017] Weight average molecular weight of SBR The weight average molecular weight of the SBR is preferably 300,000 to 1,000,000, and more preferably 400,000 to 800,000, from the viewpoints of achieving superior effects of the present invention and superior physical properties (for example, tensile properties; the same applies below) or processability of the composition. The weight average molecular weight of the SBR can be measured by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent and converted into standard polystyrene.
[0018] Styrene content of SBR, etc. The styrene content of the SBR (the content of styrene structural units in the entire SBR) is preferably 20.0 to 35.0 mass %, more preferably 22.5 to 24.5 mass %, from the viewpoints of obtaining superior effects of the present invention and superior physical properties or processability of the composition. The styrene content of the SBR is 1 It can be measured by H-NMR.
[0019] The value obtained by subtracting the above styrene amount from 100% by mass can be regarded as the content of structural units based on butadiene in the entire SBR. The greater the content of butadiene structural units in the entire SBR, the greater the possibility of there being more reaction sites with the bismaleimide compound described below, and the greater the effects of the present invention, which is preferable.
[0020] SBR content From the viewpoint of achieving superior effects of the present invention and excellent physical properties or processability of the composition, the content of the SBR is preferably 15 parts by mass or more and 30 parts by mass or less, and more preferably 20 to 30 parts by mass, per 100 parts by mass of the rubber component.
[0021] <Butadiene rubber> In the present invention, the butadiene rubber (BR) as the rubber component is not particularly limited, and examples thereof include those that are conventionally known. The effects of the present invention are excellent when BR is used in combination with a bismaleimide compound described below. As the butadiene rubber, for example, a homopolymer of butadiene can be mentioned as one preferred embodiment.
[0022] Weight average molecular weight of BR The weight average molecular weight of the BR is preferably from 300,000 to 1,000,000, and more preferably from 400,000 to 800,000, from the viewpoints of obtaining superior effects of the present invention and superior physical properties or processability of the composition. The weight average molecular weight of the BR can be measured by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent and converted into standard polystyrene.
[0023] BR cis 1,4-bond The cis 1,4-bond amount in the BR (the content of structural units formed by cis 1,4-bonds of butadiene in the entire BR) is preferably 90 to 98%, and more preferably 95 to 98%, from the viewpoints of increasing the number of reaction sites with the bismaleimide compound described later and achieving better effects of the present invention and better physical properties. The amount of cis 1,4-bonds in the BR can be measured by FT-IR.
[0024] Butadiene rubber content The content of the butadiene rubber is preferably 15 parts by mass or more and 30 parts by mass or less, and more preferably 20 to 30 parts by mass, per 100 parts by mass of the rubber component, from the viewpoints of achieving excellent effects of the present invention, a balance between initial elongation at break, high adhesive strength (after initial vulcanization, for example) with fibers (fiber reinforcing materials) and heat aging resistance, and excellent processability of the composition. The heat aging resistance can be evaluated by the retention of elongation at break after heat aging relative to the elongation at break before heat aging for a cured rubber obtained from the rubber composition. In the present invention, when the retention of elongation at break is 80% or more, it is preferable that the rubber has excellent heat aging resistance.
[0025] <Tackifier> The tackifier contained in the composition of the present invention is not particularly limited as long as it is a substance that can impart tackiness to the fiber-coating rubber composition. By containing a tackifier, the composition of the present invention has excellent processability when applied to fibers (fiber reinforcing materials) (e.g., ease of adhesion between the composition of the present invention and fibers (fiber reinforcing materials) during calendar processing, etc.).
[0026] From the viewpoints of achieving superior effects of the present invention and excellent processability when applying the composition of the present invention to fibers (fiber reinforcing materials), the tackifier preferably contains at least one selected from the group consisting of aliphatic petroleum resins, aromatic petroleum resins, alkylphenol resins, terpene resins, rosin resins, and coumarone-indene resins, and more preferably contains an aliphatic petroleum resin. Examples of the aliphatic petroleum resin include C5 petroleum resins (for example, resins obtained by polymerizing fractions of isoprene, 1,3-pentadiene, cyclopentadiene, methylbutene, pentene, and the like).
[0027] The content of the tackifier is preferably 2.0 parts by mass or more and 6.0 parts by mass or less per 100 parts by mass of the rubber component, from the viewpoints of achieving superior effects of the present invention and excellent processability when applying the composition of the present invention to fibers (fiber reinforcing materials).
[0028] <Sulfur> The sulfur contained in the composition of the present invention is not particularly limited as long as it can be used for vulcanizing diene rubber. For example, conventionally known sulfur can be used. In the present invention, the sulfur can function as a vulcanizing agent.
[0029] Sulfur content The amount of sulfur is preferably 1.0 to 3.0 parts by mass, and more preferably 1.5 parts by mass or more and less than 2.5 parts by mass, per 100 parts by mass of the rubber component, from the viewpoint of obtaining superior effects of the present invention.
[0030] The amount of sulfur per 100 parts by mass of the rubber component is preferably greater than the amount of a bismaleimide compound, which will be described later, per 100 parts by mass of the rubber component, from the viewpoint of obtaining superior effects of the present invention.
[0031] <Bismaleimide compounds> The bismaleimide compound contained in the composition of the present invention is not particularly limited as long as it is a compound having two maleimide groups. The maleimide group of the bismaleimide compound can react (for example, undergo a radical reaction) with a diene rubber (for example, NR, SBR, BR). In the present invention, the bismaleimide compound can function as a vulcanizing agent or a crosslinking agent.
[0032] The bismaleimide compound may, for example, be a compound in which the nitrogen atom of each maleimide group is bonded to a divalent hydrocarbon group. The divalent hydrocarbon group is not particularly limited. For example, it may be an aliphatic hydrocarbon, an aromatic hydrocarbon, or a combination thereof. Among them, from the viewpoint of obtaining superior effects of the present invention, a divalent aromatic hydrocarbon group is preferable, and a phenylene group is more preferable.
[0033] Examples of the bismaleimide compound include N,N'-ethylene bismaleimide, N,N'-cyclohexylene bismaleimide, N,N'-phenylene bismaleimide, and N,N'-naphthylene bismaleimide. From the viewpoint of obtaining superior effects of the present invention, the bismaleimide compound is preferably N,N'-phenylene bismaleimide, and more preferably N,N'-m-phenylene bismaleimide (N,N'-m-phenylene dimaleimide).
[0034] Bismaleimide compound content The amount of the bismaleimide compound is preferably 0.2 parts by mass or more and 1.5 parts by mass or less per 100 parts by mass of the rubber component, from the viewpoints of achieving superior effects of the present invention and excellent heat aging resistance.
[0035] Combination of sulfur content and bismaleimide compound content As for the combination of the sulfur content and the bismaleimide compound content, when the sulfur content is less than 2.0 parts by mass per 100 parts by mass of the rubber component, the bismaleimide compound content is preferably 0.5 to 1.5 parts by mass, more preferably 0.8 to 1.2 parts by mass, per 100 parts by mass of the rubber component, from the viewpoint of achieving superior effects of the present invention and excellent heat aging resistance. The above combination of the sulfur content and the bismaleimide compound content is referred to as "combination SB1". In the above combination SB1, the content of sulfur is preferably greater than the content of the bismaleimide compound, from the viewpoint of achieving superior effects of the present invention.
[0036] When the sulfur content is 2.0 parts by mass or more per 100 parts by mass of the rubber component, the bismaleimide compound content is preferably 0.2 to 0.8 parts by mass, more preferably 0.2 to 0.4 parts by mass, per 100 parts by mass of the rubber component, from the viewpoints of obtaining superior effects of the present invention and excellent heat aging resistance. The above combination of the sulfur content and the bismaleimide compound content is referred to as "combination SB2".
[0037] As for the combination of the sulfur content and the bismaleimide compound content, from the viewpoints of obtaining a superior effect of the present invention and excellent heat aging resistance, the above combination SB1 or the above combination SB2 is preferred. In the above combination SB1 (sulfur content less than 2.0 parts by mass), from the viewpoint of achieving a superior effect of the present invention, it is more preferable that the sulfur content is greater than the bismaleimide compound content and the bismaleimide compound content is 0.8 to 1.2 parts by mass per 100 parts by mass of the rubber component. In the above combination SB2 (sulfur content of 2.0 parts by mass or more), from the viewpoint of achieving a superior effect of the present invention and excellent initial elongation at break, it is more preferable that the content of the bismaleimide compound is 0.2 to 0.4 parts by mass per 100 parts by mass of the rubber component.
[0038] Additives In addition to the above components, the composition of the present invention may further contain additives as necessary within the range that does not impair the effects of the present invention. Examples of the additives include fillers such as carbon black, zinc oxide, stearic acid, antioxidants, plasticizers, vulcanization accelerators, etc. The type and content of each of the additives may be appropriately selected.
[0039] The carbon black is not particularly limited, and examples thereof include conventionally known carbon blacks. The amount of the carbon black is preferably 10 to 80 parts by mass based on 100 parts by mass of the rubber component, from the viewpoint of obtaining superior effects of the present invention.
[0040] The composition of the present invention can be produced, for example, by mixing the above-mentioned components and the above-mentioned additives that can be used as necessary.
[0041] The composition of the present invention can be used as a rubber composition for coating fibers. In the present invention, the above-mentioned fibers are not particularly limited as long as they are a material (fiber reinforcing material) capable of reinforcing rubber products. In this specification, the fiber to which the composition of the present invention is applied may be referred to as a "fiber reinforcing material." The composition of the present invention can be applied to fibers (fiber reinforcement) and used to form a coated rubber. The composition of the present invention, after being applied to a fiber reinforcing material and vulcanized, can become a coating rubber that covers the fiber reinforcing material.
[0042] Examples of the fiber reinforcement include continuous fiber reinforcement (i.e., fiber reinforcement having sufficient length) and discontinuous fiber reinforcement (i.e., short fiber, usually fiber having a length of 1 cm or less). The fiber reinforcement is preferably continuous fiber reinforcement from the viewpoint of excellent reinforcing properties of the obtained rubber product. The continuous fiber reinforcing material is not particularly limited in terms of fiber diameter, fiber length, shape, etc., so long as it is a continuous fiber reinforcing material that can be generally used in rubber products (for example, marine hoses, etc.).
[0043] Examples of fiber reinforcing materials to which the composition of the present invention can be applied include polyester fibers (eg, polyethylene terephthalate (PET) fibers, polyethylene naphthalate (PEN) fibers), polyamide fibers, and polyketone fibers. The fiber reinforcing material is preferably polyester fiber, from the viewpoint of obtaining superior effects of the present invention.
[0044] The fiber reinforcement material may be, for example, dip-treated. The dip treatment is not particularly limited. For example, a conventionally known dip treatment may be used. Specific examples of the dip treatment include a dip treatment using a combination of epoxy system / RFL (resorcinol-formaldehyde-latex), a dip treatment using a combination of chlorophenol system / RFL (resorcinol-formaldehyde-latex), and the like.
[0045] The fiber reinforcement may be, for example, in the form of a blind. An example of the fiber reinforcement in the blind shape is one having a plurality of warp threads arranged in parallel. The plurality of warp threads may be bundled (cords), and the plurality of bundles may be arranged in parallel. In the plurality of bundles, adjacent bundles may be in contact with each other, or adjacent bundles may be separated from each other. A plurality of weft threads may be incorporated so as to cross the plurality of warp threads (or the plurality of bundles).
[0046] The method of applying the composition of the present invention to a fiber reinforcement material is not particularly limited. For example, the composition of the present invention and the fiber reinforcement material are extruded to form a laminate, the composition of the present invention is molded into a sheet and then laminated with the fiber reinforcement material to form a laminate, and a calendar molding method can be used.
[0047] When the composition of the present invention and the above-mentioned fiber reinforcing material are formed into a laminate, the fiber reinforcing material may be formed in a single layer or multiple layers in the laminate. The same applies to the composition of the present invention. The composition of the present invention is preferably disposed so as to cover the fiber reinforcing material, and more preferably disposed so as to cover the entire fiber reinforcing material. When the fiber reinforcement is in the form of a layer or a blind, the composition of the present invention is preferably disposed above and below the fiber reinforcement. When the fiber reinforcement material has a plurality of layers, it is preferable to further place the composition of the present invention between adjacent layers of the fiber reinforcement material.
[0048] · Vulcanization The laminate having the composition of the present invention and a fiber reinforcing material as described above can be vulcanized, for example, under conditions of 120 to 160° C. Pressure may be applied during the vulcanization. The time required for vulcanization is not particularly limited. For example, it can be 30 to 400 minutes. Since the composition of the present invention has excellent adhesion to fiber reinforcing materials even after long-term vulcanization, the vulcanization time can be extended.
[0049] Reinforcement layer The reinforcing layer obtained by vulcanizing the laminate may have a coating rubber formed by vulcanizing the composition of the present invention and a fiber reinforcing material. The coating rubber preferably covers at least a part of the fiber reinforcing material, and more preferably covers the entire fiber reinforcing material. The reinforcing layer is formed using the composition of the present invention, and therefore has excellent adhesion to the fiber reinforcing material even after long-term vulcanization.
[0050] Applications of the composition of the present invention include, for example, large diameter hoses such as marine hoses, conveyor belts, and the like.
[0051] [Marine hose] The marine hose of the present invention is a marine hose formed using the fiber coating rubber composition of the present invention. The fiber-coating rubber composition used for the marine hose of the present invention is not particularly limited as long as it is the fiber-coating rubber composition of the present invention. The components constituting the marine hose of the present invention are not particularly limited. From the viewpoint that the fiber coating rubber composition of the present invention has excellent adhesion to the fiber reinforcement even after long-term vulcanization, the marine hose of the present invention preferably has a reinforcing layer having a coating rubber formed by the fiber coating rubber composition and a fiber reinforcement. The fiber reinforcement that the marine hose of the present invention can have is the same as described above. In the reinforcing layer, the coating rubber preferably covers at least a part of the fiber reinforcement, and more preferably covers the entire fiber reinforcement. The marine hose of the present invention may have the above-mentioned reinforcing layer in a single layer or in multiple layers. The method for producing the marine hose of the present invention is not particularly limited, except that the fiber-coating rubber composition of the present invention is used. For example, a conventionally known method may be used. It is preferable to use the fiber-coating rubber composition as a coating rubber composition for coating a fiber reinforcing material. EXAMPLES
[0052] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these.
[0053] <Production of Composition> The vulcanization components in Table 1 below, except for the vulcanization accelerator DM and sulfur, were mixed in the compositions (parts by mass) shown in the same table using a stirrer (kneading A). The vulcanization components (vulcanization accelerator DM and sulfur) were then added to the rubber obtained by kneading A in the compositions (parts by mass) shown in the same table, and these were further mixed to produce each composition (fiber coating rubber composition).
[0054] <Evaluation> The compositions prepared as described above were subjected to the following evaluations, and the results are shown in Table 1.
[0055] Initial tensile properties (initial breaking strength, initial breaking elongation) Each of the compositions produced as described above was vulcanized under conditions of 150° C. for 45 minutes and a surface pressure of 2.0 MPa to obtain an initial rubber sheet with a thickness of 2 mm. JIS No. 3 dumbbells were punched out from the above initial rubber sheet, and a tensile test was conducted in accordance with JIS K6251:2017 at a tensile speed of 500 mm / min and 23°C to measure the initial breaking strength [MPa] and initial breaking elongation (%). The initial breaking strength is preferably large, and the same is true for the initial breaking elongation.
[0056] Heat aging test Using each of the initial rubber sheets obtained as described above, a heat aging test was conducted in accordance with JIS K6257:2017 in which each No. 3 dumbbell punched out from each initial rubber sheet was placed under a condition of 70°C for 96 hours. For each dumbbell after the heat aging test, a tensile test similar to the initial tensile properties test was carried out to measure the breaking strength [MPa] and elongation at break (%) after the heat aging test.
[0057] - Breaking strength retention rate after heat aging test The initial breaking strength and the breaking strength after the heat aging test were applied to the following formula to determine the breaking strength retention after the heat aging test. Breaking strength retention rate after heat aging test (%) = (breaking strength after heat aging test / initial breaking strength) x 100
[0058] -Elongation retention at break after heat aging test The initial elongation at break and the elongation at break after the heat aging test were applied to the following formula to determine the retention of elongation at break after the heat aging test. Elongation retention rate at break after heat aging test (%) = (elongation at break after heat aging test / initial elongation at break) x 100 Evaluation criteria In the present invention, when the retention of elongation at break after the heat aging test is 80% or more, it is preferable because the heat aging resistance is excellent.
[0059] (Adhesion evaluation after vulcanization) - Preparation of evaluation samples Layer 1 (thickness 3.0 mm) of each composition prepared as above, Fiber reinforcement material 1 (Chlorophenol / RFL dip-treated (dip-treated with a combination of chlorophenol compounds and resorcin-formaldehyde-latex): manufactured by Gyosei Co., Ltd. The polyester fiber is in the form of a blind. In the polyester fiber, 45 to 50 warp bundles are arranged in parallel. The thickness of the polyester fiber: 1.0 mm. The same applies below), Layer 2 (thickness 0.8 mm) of the composition prepared as above, Fiber reinforcement 2 (similar to fiber reinforcement 1 above), and Three layers (3.0 mm thick) of the composition prepared above were laminated in the above order to prepare a 5-ply laminate, the width of the laminate being 1 inch. The compositions used in layers 1, 2, and 3 of one laminate are all the same composition. Fiber reinforcement 1 was also arranged so that the warp yarns of fiber reinforcement 1 were perpendicular to the 1-inch width of the laminate. Fiber reinforcement 2 was also arranged in the same direction as fiber reinforcement 1. Each laminate had 25 warp yarn bundles for fiber reinforcements 1 and 2 per inch width.
[0060] · Vulcanization The laminate was vulcanized at 150° C. under pressure (surface pressure 2.0 MPa) for 45 minutes or 300 minutes to prepare evaluation samples for evaluating the adhesion of the reinforcing layer after long-term vulcanization. Layers 1 to 3 (layers of the fiber coating rubber composition) in the laminate before vulcanization become the coating rubber in the evaluation sample after vulcanization. The obtained evaluation samples had a total thickness of 6 mm. Fiber reinforcing materials 1 and 2 were embedded inside each evaluation sample in the thickness direction and width direction.
[0061] Peel test Using each evaluation sample prepared as described above, a peel test was performed in accordance with JIS K6256:2013 to peel fiber reinforcement 1 from a 1-inch-wide end of the vulcanized evaluation sample, and the peel force (N / inch) was measured. The rubber adhesion (rubber coverage area (%) on the peeled surface after the peel test) was visually observed.
[0062] Evaluation criteria for adhesion after initial vulcanization (vulcanization time 45 minutes) When the vulcanization time was 45 minutes (initial vulcanization), and the peel force was 260 N / inch or more and the rubber adhesion was 90% or more, the adhesion between the fiber reinforcement and the coating rubber after the initial vulcanization was evaluated as excellent. When the peel strength was 260 N / inch or more and the rubber adhesion was 90% or more, it was evaluated that the greater the peel strength, the better the adhesion between the fiber reinforcement and the coating rubber after the initial vulcanization. On the other hand, when the peel force was less than 260 N / inch or the rubber adhesion was less than 90%, the adhesion between the fiber reinforcing material and the coating rubber after the initial vulcanization was evaluated as poor.
[0063] [Adhesion evaluation criteria after long-term vulcanization (300 minutes vulcanization)] In the present invention, when the vulcanization time was 300 minutes (long-term vulcanization), if the peel force was 245 N / inch or more and the rubber adhesion was 80% or more, the adhesion between the fiber reinforcement material and the coating rubber after long-term vulcanization was evaluated as excellent. When the peel strength was 245 N / inch or more and the rubber adhesion was 80% or more, it was evaluated that the greater the peel strength, the better the adhesion between the fiber reinforcement and the coating rubber after long-term vulcanization. On the other hand, when the peel force was less than 245 N / inch or the rubber adhesion was less than 80%, the adhesion between the fiber reinforcement and the coating rubber after long-term vulcanization was evaluated as poor.
[0064] [Table 1]
[0065] Details of each component shown in Table 1 are as follows. ·NR: Natural rubber. SIR-20 ·SBR: Styrene butadiene rubber. Styrene butadiene rubber. Product name: NIPOL1502, manufactured by Zeon Corporation. Weight average molecular weight: 490,000, styrene content: 23.5% by mass. BR: Butadiene rubber, product name "NIPOL BR1220", manufactured by Zeon Corporation. Weight average molecular weight: 520,000, cis-1,4-bond content: 98%
[0066] CB: GPF grade carbon black, product name "Niteron #GN", manufactured by Nippon Steel Carbon Co., Ltd.
[0067] Zinc oxide: Three types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. Stearic acid: Beads made by NOF Corporation, Stearic Acid YR
[0068] Tackifier (aliphatic petroleum resin): Product name Quinton A100, manufactured by Zeon Corporation
[0069] Vulcanization accelerator DM: Di-2-benzothiazolyl disulfide (Noccela DM-PO(DM), manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)
[0070] Sulfur: Powdered sulfur, produced by Karuizawa Refinery Bismaleimide compound (N,N'-m-phenylenedimaleimide): Trade name: Valnoc PM, manufactured by Ouchi Shinko Chemical Co., Ltd.
[0071] As is clear from the results shown in Table 1, Comparative Examples 1 and 3, which did not contain a bismaleimide compound, had poor adhesion to fiber reinforcing materials after long-term vulcanization. Comparative Example 2, which did not contain butadiene rubber, had poor adhesion to the fiber reinforcing material after long-term vulcanization. Comparative Example 4, which did not contain butadiene rubber or a bismaleimide compound, had poor adhesion to the fiber reinforcing material after long-term vulcanization.
[0072] In contrast, the fiber-coating rubber composition of the present invention exhibited excellent adhesion to fiber reinforcing materials even after long-term vulcanization. Each of the compositions (fiber-coating rubber compositions) produced in Examples 1 to 8 was visually uniform, and the mixability of the fiber-coating rubber compositions was good.
Claims
1. a rubber component including natural rubber, styrene-butadiene rubber, and butadiene rubber; A tackifier; Sulfur and A bismaleimide compound is contained, The fiber coating rubber composition has a content of the butadiene rubber of 20 parts by mass or more and 30 parts by mass or less based on 100 parts by mass of the rubber component.
2. The fiber coating rubber composition according to claim 1, wherein the content of the bismaleimide compound is from 0.2 parts by mass to 1.5 parts by mass based on 100 parts by mass of the rubber component.
3. 3. The fiber coating rubber composition according to claim 1, wherein the tackifier comprises at least one selected from the group consisting of aliphatic petroleum resins, aromatic petroleum resins, alkylphenol resins, terpene resins, rosin resins, and coumarone-indene resins.
4. The fiber coating rubber composition according to any one of claims 1 to 3, wherein the content of the tackifier is 2.0 parts by mass or more and 6.0 parts by mass or less based on 100 parts by mass of the rubber component.
5. a rubber component including natural rubber, styrene-butadiene rubber, and butadiene rubber; A tackifier; Sulfur and A bismaleimide compound is contained, A marine hose formed using the fiber coating rubber composition, wherein the content of the butadiene rubber is 15 parts by mass or more and 30 parts by mass or less based on 100 parts by mass of the rubber component.
Citation Information
Patent Citations
Amine free vulcanizable rubber
EP1676876A1
Fiber-reinforced rubber article
JP1999269276A
Method for manufacturing fluid carrying hose
JP2010173110A
Rubber composition, vulcanized rubber, belt coating rubber, intermediate rubber, and tire