Biaxially oriented polyester film
The biaxially oriented polyester film addresses smoothness and winding issues by controlling protrusion heights and frequencies, enhancing winding properties and reducing signal loss for high-density recording.
Patent Information
- Application Number
- JP2020142669
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-02
- Filing Date
- 2020-08-26
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-08-26
AI Technical Summary
Existing biaxially oriented polyester films used in ultra-high density recording media face challenges in achieving smooth surfaces, leading to air entrapment and wrinkle formation during manufacturing, which affects winding properties and causes signal loss due to protrusion transfer to magnetic layers.
The film is designed with controlled protrusion heights and frequencies on one surface, satisfying relational expression y≦ -24.9X+3.8, where X is the protrusion height, and a specific 0.4% area height in the bearing curve, ensuring smoothness and reducing protrusion transfer.
The film exhibits excellent winding properties and reduced signal loss, enabling high-density recording with improved electromagnetic conversion characteristics.
Smart Images

Figure 0007583356000002 
Figure 0007583356000003 
Figure 0007583356000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a biaxially oriented polyester film, which is useful in applications requiring extremely smooth surfaces, such as base films for ultra-high density recording media exceeding 5 TB (Tera Bytes). [Background technology]
[0002] In recent years, with the increase in the amount of data that needs to be handled in computer systems and the like, there has been a demand for a significant increase in the recording capacity of magnetic recording media. In order to achieve high-density recording by making the surface of the magnetic recording medium highly smooth, it is desirable to also make the surface of the base film smooth. However, the smoother the surface of the base film is, the more difficult it becomes to remove air between the layers of the rolled film in the base film manufacturing process, which leads to problems such as wrinkles easily occurring when the product is wound up, resulting in a decrease in productivity.
[0003] For this reason, a rough surface with a certain degree of roughness is formed on one surface of a base film, a flat surface with a small degree of roughness is formed on the other surface, and a magnetic layer is formed on the flat surface side. For example, Patent Document 1 proposes forming a two-layer polyester film to form a rough surface and a flat surface, controlling the average particle size and content of inactive particles contained in the polyester film for each layer, and setting particle-containing voids in a specific range for the surface of each layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-116093 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, it was found that when attempting to achieve high density recording by making the surface of the magnetic recording medium highly smooth, the effect of the surface shape of the rough side of the base film also becomes significant, and protrusions from the rough surface can be transferred to the surface of the magnetic layer, causing signal loss.
[0006] In particular, it has been found that in applications requiring extremely smooth surfaces, such as base films for ultra-high density recording media exceeding 5TB, it is necessary to precisely control the protrusion height and frequency of the rough surface. However, the polyester film of Patent Document 1 only controls the density of voids that cause protrusions, and is therefore insufficient as a method for precisely controlling the protrusion height and frequency of the rough surface.
[0007] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a biaxially oriented polyester film which has excellent winding properties in the base film manufacturing process, excellent electromagnetic conversion characteristics when made into a magnetic recording tape, and little signal loss. [Means for solving the problem]
[0008] As a result of intensive research conducted by the inventors to solve the above problems, they discovered that by controlling the frequency of each of the multiple protrusion heights and the height of the 0.4% area in the bearing curve based on the distribution of protrusion heights when the rough surface is measured with a non-contact surface profiler, it is possible to achieve both electromagnetic conversion characteristics and minimal signal dropout when made into a magnetic recording tape (hereinafter collectively referred to as "magnetic recording characteristics"), as well as ease of winding in the base film manufacturing process, and thus arrived at the present invention.
[0009] That is, the present invention includes the following.
[0010] (1) A biaxially oriented polyester film, characterized in that when at least one surface is measured with a non-contact surface profiler, where X is 0.075 μm, 0.100 μm, and 0.125 μm, the logarithmic value y of the protrusion frequency of protrusions equal to or greater than X satisfies the following relational expression (1), and the protrusion height corresponding to 0.4% area in a bearing curve based on the protrusion height distribution is 65 nm or more and less than 90 nm.
[0011] y≦-24.9X+3.8 (1) (Here, X is the protrusion height (μm), and y is the logarithm to the base 10 of the number of protrusions with a protrusion height of X or more in a field of view of 282 μm × 211 μm.)
[0012] (2) The biaxially oriented polyester film according to (1), wherein the polyester contained in the biaxially oriented polyester film has ethylene terephthalate or ethylene-2,6 naphthalene dicarboxylate as a main repeating unit.
[0013] (3) A biaxially oriented polyester film according to either (1) or (2), in which, when the one surface and the other surface of the biaxially oriented polyester film are measured using a non-contact surface profiler, the centerline average surface roughness of the one surface is 1 nm or more rougher than the centerline average surface roughness of the other surface.
[0014] (4) The biaxially oriented polyester film according to any one of (1) to (3), wherein the biaxially oriented polyester film contains inert particles.
[0015] (5) The biaxially oriented polyester film according to any one of (1) to (4), which is a laminate of two or more different polyester layers. Effect of the Invention
[0016] The biaxially oriented polyester film of the present invention, when used as a base film for ultra-high density recording media of 5 TB or more, has excellent winding properties in the base film manufacturing process, and when used as a magnetic recording tape, has excellent electromagnetic conversion characteristics and little signal loss. Therefore, when the biaxially oriented polyester film of the present invention is used for a magnetic recording tape, high density recording can be achieved, and a data storage device with a large storage capacity can be provided. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a graph showing the relationship between projection height and frequency when the rough surfaces of the biaxially oriented polyester films obtained in Example 1, Comparative Example 1, and Comparative Example 2 were measured with a non-contact surface profilometer. [Diagram 2] FIG. 2 is a graph showing the bearing curves of the rough surfaces of the biaxially oriented polyester films obtained in Example 1, Comparative Example 1, and Comparative Example 2, measured with a non-contact surface profiler. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will be described in detail below. For convenience of explanation, the film-forming direction of the film may be referred to as the machine axis direction, longitudinal direction, longitudinal direction, or MD direction, and the direction perpendicular to the film-forming direction and the thickness direction may be referred to as the width direction, transverse direction, or TD direction.
[0019] [Biaxially oriented polyester film] The biaxially oriented polyester film of the present invention contains polyester as the main resin component, and the polymer has biaxial orientation due to biaxial stretching of the film, etc. The term "main resin component" means that the resin component contains polyester in an amount of 50% by mass or more, preferably 70% by mass, more preferably 80% by mass, and most preferably 90% by mass.
[0020] When the biaxially oriented polyester film of the present invention is measured on at least one surface using a non-contact surface profiler, and the protrusion height X is set to 0.075 μm, 0.100 μm, and 0.125 μm, the logarithmic value y of the protrusion frequency of protrusions having a protrusion height X or more satisfies the following relational formula (1):
[0021] y≦-24.9X+3.8 (1) Here, X is the protrusion height (μm), and y is the logarithm with base 10 of the number of protrusions with a protrusion height of X or more in a visual field of an area of 282 μm × 211 μm. The non-contact surface shape measuring device used was a ZYGO product name: New View 7300, and the measurement conditions were a measurement magnification of 25 times with a zoom magnification of 0.5 times using a 50x objective lens, and a measurement area of 282 μm × 211 μm (= 0.0595 mm 2 ) can be used. The protrusion frequency is calculated by tallying the protrusion height in increments of 0.005 μm to find the number of protrusions, and integrating the number of protrusions that are equal to or greater than the protrusion height X to find the protrusion frequency.
[0022] In other words, y is the projection height X 1 = 0.075 μm, X 2 = 0.100 μm, X 3 For each of =0.125 μm, 1 That's all, X 2 Above or X 3 Protrusion frequency of protrusions with height of Y or more 1 , Y 2 , or Y 3 and calculate the base 10 logarithm y 1 =logY 1 , y 2 =logY 2 , or y 3 =logY 3 The relationship (1) is satisfied if X 1 andy 1 , X 2 andy 2 , X 3 andy 3 For each of the relationships above, the following condition is satisfied: y≦ -24.9X+3.8 (1).
[0023] When the relationship between X and y does not satisfy the relational formula (1), that is, when the frequency of the number of protrusions with protrusion heights of 0.075 μm, 0.100 μm, and 0.125 μm is high, the signal loss is likely to occur due to the transfer of the protrusions to the magnetic layer surface when the magnetic recording medium is used. In other words, in particular, in applications requiring extremely smooth surface properties, such as base films used in ultra-high density recording media exceeding 5 TB, it is necessary to highly control the protrusion height and its frequency, and it is considered that the signal loss due to the transfer of the protrusions to the magnetic layer surface when the magnetic recording medium is used can be effectively suppressed by controlling the frequency of each of the multiple protrusion heights based on the distribution of the protrusion heights when the rough surface side surface is measured with a non-contact surface profiler, as in the present invention.
[0024] In controlling the frequency of each of the multiple protrusion heights, the relationship of a linear inequality between the logarithmic value y of each frequency and the protrusion height X is specified because this is a desirable condition for effectively preventing the protrusions from being transferred to the magnetic layer surface and causing a deterioration in characteristics when the magnetic tape is made. For example, as shown in Figure 1, the relationship when the logarithmic value of each frequency is on the vertical axis and the protrusion height is on the horizontal axis becomes important.
[0025] From this viewpoint, it is preferable to satisfy the relational formula (1') instead of the relational formula (1), and it is more preferable to satisfy the relational formula (1'').
[0026] y≦-24.9X+3.7 (1') -24.9X+2.0 ≦y≦ -24.9X+3.5 (1'')
[0027] In addition, the biaxially oriented polyester film of the present invention has a protrusion height equivalent to 0.4% of the area in the bearing curve based on the protrusion height distribution when measured with a non-contact surface profiler (i.e., when measuring the frequency of each of the above-mentioned multiple protrusion heights) of 65 nm or more and less than 90 nm (hereinafter, this characteristic, together with the characteristic resulting from satisfying relational formula (1), will be collectively referred to as the "surface characteristic of the present invention"). If this height is below the lower limit, wrinkles will occur during product winding, resulting in reduced productivity. On the other hand, if this height is above the upper limit, when the film is made into a magnetic recording medium, the transfer of the protrusions to the magnetic layer surface will make it easier for signals to be lost or output to be reduced.
[0028] The "bearing curve", also known as the "load curve", is a curve that shows the cumulative frequency up to each height as a percentage, from the highest protrusion crest to the deepest protrusion valley (or the smallest protrusion height), based on the protrusion height distribution measured by a non-contact surface profiler or the like, as shown in Figure 2. The total frequency is set to 100, and the cumulative frequency up to each height is expressed as a percentage. Furthermore, "protrusion height equivalent to 0.4% area" refers to the protrusion height in the bearing curve where the percentage (the percentage from the side with the highest protrusion crest) is equivalent to 0.4%.
[0029] Such a protrusion height indicates the lower limit of the protrusion height that exists at a certain frequency rate in the highest part of the protrusion peak among all protrusion heights. In addition to relational formula (1), which controls the absolute value of each frequency of multiple protrusion heights, control of the protrusion height based on the bearing curve provides an index of protrusion height based on relative frequency, allowing for more advanced control of the surface shape.
[0030] From this point of view, the height of the 0.4% area in the bearing curve is preferably in the range of 67 to 87 nm.
[0031] The surface characteristics of the present invention as described above may be satisfied on at least one surface of the biaxially oriented polyester film, but it is preferable to satisfy them on one surface rather than on both surfaces of the biaxially oriented polyester film, from the viewpoint of controlling the shape of the rough surface to achieve both winding properties and magnetic recording properties in the manufacturing process, and from the viewpoint of enhancing the smoothness of the other surface.
[0032] From the viewpoint of achieving both winding ease in the manufacturing process and magnetic recording properties, the center line average surface roughness (Ra) of the biaxially oriented polyester film is preferably 3 to 9 nm, and more preferably 4 to 8 nm, at least on the surface that satisfies the surface properties of the present invention.
[0033] From the viewpoint of achieving both windability in the manufacturing process and magnetic recording properties, it is preferable to change the center line average surface roughness (Ra) between the surface satisfying the surface properties of the present invention and the other surface. Specifically, when one surface and the other surface of a biaxially oriented polyester film are measured with a non-contact surface profiler, the center line average surface roughness of one surface is preferably 1 nm or more rougher, more preferably 2 nm or more rougher, than the center line average surface roughness of the other surface.
[0034] [polyester] The polyester contained in the biaxially oriented polyester film of the present invention is preferably a polyester having a dibasic acid and a glycol as constituents. For example, the aromatic dibasic acid may be terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, diphenylsulfone dicarboxylic acid, diphenylether dicarboxylic acid, diphenylketone dicarboxylic acid, phenylindanedicarboxylic acid, sodium sulfoisophthalic acid, dibromoterephthalic acid, 4,4'-diphenyldicarboxylic acid, 6,6'-(ethylenedioxy)di-2-naphthoic acid, etc. In addition, the alicyclic dibasic acid may be oxalic acid, succinic acid, adipic acid, azelaic acid, sebacic acid, dimer acid, etc.
[0035] As the glycol, as the aliphatic diol, ethylene glycol, propylene glycol, tetramethylene glycol, hexamethylene glycol, neopentyl glycol, diethylene glycol, etc. can be used, as the aromatic diol, naphthalenediol, 2,2-bis(4-hydroxydiphenyl)propane, 2,2-bis(4-hydroxyethoxyphenyl)propane, bis(4-hydroxyphenyl)sulfone, hydroquinone, etc. can be used, as the alicyclic diol, cyclohexanedimethanol, cyclohexanediol, etc. As the polyester in the present invention, those having ethylene terephthalate or ethylene-2,6 naphthalenedicarboxylate as the main repeating unit are particularly preferred.
[0036] Furthermore, the polyester in the present invention is preferably substantially linear from the viewpoint of forming a film, and within the range of being substantially linear, a polyfunctional compound having three or more functional groups, such as glycerin, trimethylolpropane, pentaerythritol, trimellitic acid, trimesic acid, pyromellitic acid, tricarballylic acid, gallic acid, etc., may be copolymerized, or a monofunctional compound, such as o-benzoylbenzoic acid, naphthoic acid, etc., may be added and reacted. Also, a polyether such as polyethylene glycol, a polyether such as polytetramethylene glycol, or an aliphatic polyester typified by polycaprolactone may be copolymerized.
[0037] The polyester in the present invention may be used as a composition in which two or more kinds are blended. For example, as long as the resin component contains 50% by mass or more of polyester, a resin other than polyester may be blended.
[0038] The intrinsic viscosity (measured in orthochlorophenol at 25° C.) of the polyester used in the present invention is preferably 0.50 dl / g, more preferably 0.51 dl / g, and most preferably 0.52 dl / g in terms of melt-kneadability, film-forming property, decomposition property during melt extrusion, etc. In particular, when other resins such as polyetherimide described below are blended, it is preferable from the viewpoint of melt-kneadability that the intrinsic viscosity is equal to or higher than the lower limit.
[0039] As described above, the biaxially oriented polyester film of the present invention may be formed of a composition in which two or more kinds are blended, and one of the preferred embodiments contains at least one selected from the group consisting of polyimide, polyetherimide, polyetherketone, polyetheretherketone, and polyarylate. In particular, it is preferable to contain either polyetherimide or polyarylate. Polyetherimide is a polymer containing an aliphatic, alicyclic, or aromatic ether unit and a cyclic imide group as a repeating unit, and is not particularly limited as long as it is a polymer having melt moldability. As long as the effects of the present invention are not impaired, the main chain of polyetherimide may contain structural units other than cyclic imide and ether units, such as aromatic, aliphatic, or alicyclic ester units, oxycarbonyl units, etc.
[0040] Polyarylate is a synthetic resin that belongs to the category of amorphous thermoplastic resins, and its basic composition is the polycondensation of dihydric phenols and dibasic acids such as phthalic acid and carboxylic acid.
[0041] [Inert particles] In the biaxially oriented polyester film of the present invention, in order to set the protrusion frequency at a specific protrusion height on at least one surface and the height that results in a specific bearing area within an appropriate range, it is preferable that inactive particles are contained in the polyester resin that forms the biaxially oriented polyester film.
[0042] As the type of inactive particles, inorganic particles such as spherical silica, aluminum silicate, titanium dioxide, calcium carbonate, etc., and other organic polymer particles such as crosslinked polystyrene particles, crosslinked silicone resin particles, crosslinked acrylic resin particles, crosslinked styrene-acrylic resin particles, crosslinked polyester particles, polyimide particles, melamine resin particles, etc. are preferred. The particles may be hollow or not. One or more of these may be selected and used.
[0043] The size of the inactive particles is preferably 0.01 μm or more and 0.8 μm or less, more preferably 0.05 μm or more and 0.6 μm or less, and particularly preferably 0.1 μm or more and 0.4 μm or less. The average particle diameter of the inactive particles as a whole is preferably 0.05 μm or more and 0.6 μm or less, more preferably 0.1 μm or more and 0.4 μm or less. Within this range of the average particle diameter of the inactive particles as a whole, it is preferable that the inactive particles at least partially contain inactive particles having an average particle diameter of 0.25 μm or more and 0.35 μm or less. In other words, it is preferable to include inactive particles having an average particle diameter of 0.25 μm or more and 0.35 μm or less and inactive particles having an average particle diameter of 0.05 μm or more and less than 0.25 μm.
[0044] There are several methods for adding inactive particles to polyester resin, including polymerization addition, in which the particles are added to a portion of the raw material components constituting the resin to form a slurry, which is then polymerized as is, kneading, in which the particles are added to the polymerized resin using a twin-screw extruder or the like, and further, preparing a master polymer with a high content of inactive particles and diluting this with resin to achieve the desired content.
[0045] The preferred amount of inactive particles is 0.001% by mass or more and 2% by mass or less, more preferably 0.01% by mass or more and 1% by mass or less, particularly preferably 0.1% by mass or more and 0.8% by mass or less, based on the mass of the polyester layer forming one of the surfaces. When the inactive particles having an average particle size of 0.25 μm or more and 0.35 μm or less are contained, the content of the inactive particles having an average particle size of 0.25 μm or more and 0.35 μm or less is preferably 0.02% by mass or more and 0.07% by mass or less. In addition, the inactive particles having an average particle size of 0.05 μm or more and less than 0.25 μm are preferably contained in an amount of 0.03% by mass or more and 0.5% by mass or less.
[0046] [Layer composition] The biaxially oriented polyester film of the present invention may have a single layer structure, or may have two or more polyester layers laminated together so that the surface roughness of the front and back sides is different. In particular, when the film is used as a substrate for a magnetic recording medium, it is preferable to have a layer structure of two or more layers. When the film has a two or more layer structure, particles may not be added to the resin constituting the outermost layer.
[0047] The biaxially oriented polyester film of the present invention may be provided with a coating layer for the purpose of improving adhesion to the magnetic layer and improving the slipperiness of the film itself, as long as the effect of the present invention is not impaired. In this case, it is sufficient that the surface of the coating layer or the surface on the side on which the coating layer is not provided satisfies the surface characteristics of the present invention, but it is preferable that the surface on the side on which the coating layer is not provided satisfies the surface characteristics of the present invention.
[0048] [Manufacturing method of biaxially oriented polyester film] The biaxially oriented polyester film of the present invention can be produced by a method known per se, for example by extruding a polymer into a sheet form from a die using a single extruder, or by laminating different polymers in a molten state using two or more extruders and then extruding them into a sheet form from a die, and cooling and solidifying the resulting sheet to form a monolayer or laminated unstretched film, and then stretching the resulting unstretched film preferably in one direction or in two perpendicular directions, and further heat treating the film.
[0049] The temperature in the process of extruding in a molten state is not particularly limited as long as there is no unmelted material and the temperature does not excessively deteriorate the resin. For example, it is preferable to extrude the resin at a temperature between the melting point of the resin (Tm:°C) and (Tm+70)°C.
[0050] Next, regarding cooling, in order to maintain the flatness of the resulting unstretched film while also reducing thickness unevenness, it is preferable to use a rotating cooling drum installed below the die along the film production direction and cool the sheet-like material by contacting it closely to the drum.
[0051] In this case, in order to realize the surface characteristics of the present invention, it is preferable to increase the smoothness of the surface of the cooling drum, and it is preferable to make the surface finish of the cooling drum 1.0S or less, and it is more preferable to make it 0.5S or less from the viewpoint of precisely controlling the height of the 0.4% area in the bearing curve.
[0052] It is not impossible to leave the film as an unstretched film if the desired thickness and Young's modulus can be achieved, but in order to achieve better processability at high temperatures, it is preferable to subject the unstretched film to a stretching operation to produce a film having the desired thickness and Young's modulus.
[0053] There are various stretching methods, such as longitudinal uniaxial stretching, transverse uniaxial stretching, sequential biaxial stretching, and simultaneous biaxial stretching, and there is no particular restriction. Here, sequential biaxial stretching will be described. Longitudinal uniaxial stretching is sequential biaxial stretching without transverse stretching, transverse uniaxial stretching is sequential biaxial stretching without longitudinal stretching, and simultaneous biaxial stretching is performed simultaneously in longitudinal and transverse stretching. In sequential biaxial stretching, an unstretched film is stretched in a uniaxial direction (usually the longitudinal direction) at a temperature of (Tg-10)°C to (Tg+60)°C at a ratio of 2 times or more, preferably 2.5 times or more, based on the glass transition temperature (Tg:°C) of the resin, and then preferably stretched in a direction perpendicular to the stretching direction at a temperature of Tg to (Tg+60)°C at a ratio of 2 times or more, preferably 2.5 times or more. If necessary, the film may be further stretched again in the longitudinal and / or transverse directions.
[0054] In particular, it is preferable to perform the transverse stretching in two stages in order to set the projection frequency in the specific projection height range and the height in the 0.4% area of the bearing curve in the specific range in the present invention. Furthermore, the resin film after stretching can be heat-set at a temperature of (Tm-70)°C to (Tm-10)°C, where Tm is the melting point of the resin. The heat-setting time is preferably 0.1 to 60 seconds.
[0055] [Magnetic recording tape] The biaxially oriented polyester film of the present invention is preferably used as a base film for a magnetic recording tape, more preferably a high-density magnetic recording tape, particularly a digital recording magnetic recording tape. That is, the magnetic recording tape contains the biaxially oriented polyester film of the present invention as a base film. Hereinafter, the magnetic recording tape using the biaxially oriented polyester film of the present invention will be further described.
[0056] The magnetic recording tape can be produced by forming a magnetic layer on the biaxially oriented polyester film of the present invention. In this case, it is preferable to form a magnetic layer on the back side of the surface that satisfies the surface characteristics of the present invention. In addition, in order to improve the adhesion with the magnetic layer, etc., a coating layer having a known adhesive function may be formed on the surface of the biaxially oriented polyester film of the present invention as described above, within a range that does not impair the effects of the present invention.
[0057] The magnetic layer forming the magnetic recording tape is not particularly limited, but is formed by uniformly dispersing iron or iron-based acicular fine magnetic powder or barium ferrite in a binder such as polyvinyl chloride or vinyl chloride-vinyl acetate copolymer, and applying the resulting coating liquid. As described above, by using the biaxially oriented polyester film of the present invention, a magnetic recording tape with excellent dimensional stability, electromagnetic conversion characteristics, and error rate performance can be obtained.
[0058] As mentioned above, in order to increase recording density, it is necessary to make the magnetic material finer. This makes it difficult to remove solvents from the coating liquid, and in order to maintain processability, it has become necessary to dry the material at higher temperatures.
[0059] The magnetic layer is preferably coated to a thickness of 1 μm or less, more preferably 0.02 to 0.5 μm, from the viewpoint of obtaining a coated magnetic recording tape for high-density recording with excellent electromagnetic conversion characteristics, particularly in the short wavelength region, such as output, S / N, C / N, and low dropout and error rate. If necessary, it is also preferable to coat a non-magnetic layer containing fine titanium oxide particles or the like as an underlayer for the coated magnetic layer, by dispersing the non-magnetic layer in the same organic binder as the magnetic layer.
[0060] In addition, a protective layer such as diamond-like carbon (DLC) and a fluorine-containing carboxylic acid-based lubricant layer may be provided on the surface of the magnetic layer in this order depending on the purpose, use and necessity, and further a known backcoat layer may be provided on the other surface.
[0061] The coated magnetic recording tape thus obtained is extremely useful as a magnetic recording tape for data applications such as LTO, enterprise, etc. In particular, according to the present invention, a smooth magnetic layer surface can be realized by suppressing transfer, which makes it possible to dramatically improve the recording density in linear tapes, and the tape can be suitably used in ultra-high density recording media, particularly those with a storage capacity of more than 5 TB. EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples and comparative examples. In the present invention, the properties were measured and evaluated by the following methods. In the following, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0063] (1) Film thickness Ten sheets of film were stacked to prevent dust from entering, and the thickness was measured with a dot-type electronic micrometer to calculate the film thickness per sheet.
[0064] (2) Surface roughness A non-contact surface shape measuring instrument (ZYGO: New View7300) was used, and the measurement magnification was 25x with a zoom magnification of 0.5x using a 50x objective lens, and the measurement area was 282μm×211μm (=0.0595mm 2 ) was measured ten times at different locations, and the average value was taken as the center line average surface roughness (Ra). In the examples, the surface with the larger center line average surface roughness (Ra) is referred to as the rough surface, and the surface with the smaller center line average surface roughness (Ra) is referred to as the flat surface.
[0065] (3) Protrusion frequency For the measurement data of the surface with a large Ra (rough surface) obtained by the above surface roughness measurement, the Reference Band was set to 10 nm in the analysis software Metro Pro built into the surface shape measuring instrument, and the peaks at a slice level of 5 nm were extracted as protrusions. The protrusion heights were counted every 0.005 μm to obtain the number of protrusions, and the number of protrusions was integrated from the highest protrusion, and the average value of N = 10 was taken as the protrusion frequency. Here, the logarithmic value with the base 10 was calculated for the protrusion frequency at protrusion heights of 0.075 μm, 0.100 μm, and 0.125 μm. In addition, the protrusion frequency at protrusion heights of 0.075 μm, 0.100 μm, and 0.125 μm means the protrusion frequency at protrusion heights of 0.075 μm or more, 0.100 μm or more, and 0.125 μm or more, respectively. FIG. 1 is a graph showing the relationship between protrusion height and frequency when the rough surfaces of the biaxially oriented polyester films obtained in Example 1, Comparative Example 1, and Comparative Example 2 were measured using a non-contact surface profilometer.
[0066] (4) Bearing curve 0.4% height A bearing curve was created using analysis software (SPIP, manufactured by Image Metrology) from the measurement data of the surface with large Ra (rough surface) obtained in the above surface roughness measurement, and the slice level where the bearing area in this bearing curve is 0.4% was read as the height, and the average value was calculated for N = 10. Note that Fig. 2 shows the bearing curves of the rough surfaces of the biaxially oriented polyester films obtained in Example 1, Comparative Example 1, and Comparative Example 2, measured with a non-contact surface profiler.
[0067] (5) Film winding properties After the biaxially oriented polyester film was produced and wound up, it was slit into pieces measuring 1 m wide and 10,000 m long, and 100 rolls were wound up at a speed of 80 m / min. The percentage of non-defective products free of defects such as wrinkles, edge misalignment, or surface protrusions was judged. ◎: The rate of non-defective products is 95% or more ○: The rate of non-defective products is 90% or more ×: The rate of non-defective products is less than 90%.
[0068] (6) Preparation of magnetic recording tape The film is slit to a width of 1m and tensioned at 2kg / mm 2 The support is conveyed at a speed of 100 rpm, and one surface of the support is coated with a magnetic paint and a non-magnetic paint, and the other surface is coated with a backcoat layer according to the following description, and the support is slit to a width of 12.65 mm to prepare a pancake (cut roll). Next, a length of 900 m from the pancake is assembled into a cassette to prepare a magnetic recording tape. <Coating liquid for forming magnetic layer> Barium ferrite magnetic powder 100 parts (Plate diameter: 20.5 nm, plate thickness: 7.6 nm, plate aspect ratio: 2.7, Hc: 191 kA / m (≒ 2400 Oe) Saturation magnetization: 44Am 2 / kg, BET specific surface area: 60m 2 / g) Polyurethane resin 12 parts Weight average molecular weight 10,000 Sulfonic acid functional group 0.5meq / g α-alumina HIT60 (Sumitomo Chemical Co., Ltd.) 8 parts Carbon black #55 (Asahi Carbon Co., Ltd.) Particle size 0.015μm 0.5 parts Stearic acid 0.5 parts Butyl stearate 2 parts Methyl ethyl ketone 180 parts Cyclohexanone 100 parts <Coating liquid for forming non-magnetic layer> Non-magnetic powder α-iron oxide 85 parts Average major axis length 0.09μm, specific surface area by BET method 50m 2 / g pH 7 DBP oil absorption 27~38ml / 100g Surface treatment layer Al 2 O 3 8% by mass Carbon black 15 parts "Conductex" (registered trademark) SC-U (manufactured by Columbian Carbon Co., Ltd.) Polyurethane resin UR8200 (manufactured by Toyobo Co., Ltd.) 22 parts Phenylphosphonic acid 3 parts Cyclohexanone 140 parts Methyl ethyl ketone 170 parts Butyl stearate 1 part Stearic acid 2 parts Methyl ethyl ketone 205 parts Cyclohexanone 135 parts The above coating liquids (magnetic layer coating liquid, non-magnetic layer coating liquid) were kneaded with each component in a kneader. The coating liquid was pumped through a horizontal sand mill containing 1.0 mmφ zirconia beads in an amount that filled the dispersion section at 65% by volume, and dispersed at 2,000 rpm for 120 minutes (time spent substantially in the dispersion section). 5.0 parts of polyisocyanate were added to the non-magnetic layer coating material and 2.5 parts to the magnetic layer coating material, and 3 parts of methyl ethyl ketone were further added. The mixture was filtered using a filter with an average pore size of 1 μm to prepare coating liquids for forming the non-magnetic layer and the magnetic layer, respectively.
[0069] The obtained coating liquid for forming a non-magnetic layer was coated and dried on the flat surface of the film so that the dried thickness would be 0.6 μm, and then the coating liquid for forming a magnetic layer was coated so that the dried thickness would be 0.07 μm. While the magnetic layer was still wet, it was oriented using a cobalt magnet with a magnetic force of 6,000 G (600 mT) and a solenoid with a magnetic force of 6,000 G (600 mT) and dried.
[0070] Thereafter, a backcoat layer (100 parts of carbon black, average particle size: 17 nm, 80 parts of calcium carbonate, average particle size: 40 nm, 5 parts of α-alumina, average particle size: 200 nm, dispersed in polyurethane resin and polyisocyanate) was applied onto the rough surface of the film so that the thickness after calendering was 0.4 μm. Next, calendering was performed using a calender at a temperature of 90° C. and a linear pressure of 300 kg / cm (294 kN / m), and then curing was performed at 70° C. for 48 hours. Furthermore, the nonwoven fabric and razor blade were attached to a device having a device for feeding and winding the slit product so that they were pressed against the magnetic surface, and the surface of the magnetic layer was cleaned using a tape cleaning device, to obtain a magnetic recording tape.
[0071] (7) Electromagnetic conversion characteristics The recording head (MIG, gap 0.15μm, 1.8T) and the GMR head for reproduction were attached to a drum tester to measure the output of the magnetic recording tape obtained by (6) above. The head / tape relative speed was 15m / sec, and a signal with a track density of 16KTPI and a linear recording density of 400Kbpi was recorded, after which the ratio of output to noise was taken as the electromagnetic conversion characteristic. Example 1 was taken as 0dB, and +2dB or more was taken as ◎, less than +2dB to 0dB was taken as ◯, and less than 0dB was taken as ×.
[0072] (8) Dropout The magnetic recording tape obtained in (6) above was loaded into an IBM LTO8 drive, and 14 GB of data signals were recorded and then played back. A signal with an amplitude (PP value) of 50% or less of the average signal amplitude was considered a missing pulse, and four or more consecutive missing pulses were detected as a dropout. Dropouts were evaluated over one 900 m long roll, converted into the number per meter, and judged according to the following criteria. ◎: Dropouts less than 3 / m ○: Dropouts: 3 or more / m, less than 9 / m ×: Dropouts: 9 or more / m.
[0073] [Example 1] Using two extruders, an extruder 1 for forming a polyester layer on the rough surface side and an extruder 2 for forming a polyester layer on the flat surface side, a laminated unstretched film was produced by co-extrusion as follows. In the extruder 1, 0.06% by mass of crosslinked polystyrene particles having an average particle size of 0.3 μm and 0.12% of spherical silica particles having a size of 0.1 μm were added to polyethylene-2,6-naphthalenedicarboxylate having an intrinsic viscosity (orthochlorophenol, 35° C.) of 0.60 dl / g to produce a PEN resin composition 1. This PEN resin composition 1 was dried at 180° C. for 5 hours in the form of chips and then supplied. In the extruder 2, 0.1% by mass of spherical silica having an average particle size of 0.1 μm was added to polyethylene-2,6-naphthalenedicarboxylate having an intrinsic viscosity of 0.60 dl / g to produce a PEN resin composition 2. This PEN resin composition 2 was dried in the same manner as PEN resin composition 1 and then fed so that the thickness ratio of resins 1 and 2 was 55 / 45. It was then extruded from a T-shaped extrusion die so that the PEN resin composition 1 was in contact with a casting drum maintained at a surface finish of 0.3S and a surface temperature of 60°C, and rapidly cooled and solidified to obtain a laminated unstretched film.
[0074] The laminated unstretched film thus obtained was preheated at 120°C, and further heated between low-speed and high-speed rolls with an infrared heater having a surface temperature of 830°C from 14 mm above, stretched 4.8 times, rapidly cooled, subsequently supplied to a tenter, stretched 4.6 times in the transverse direction at 150°C, then rapidly cooled, and then heated again to 180°C and stretched 1.25 times in the transverse direction, and heat-fixed at 215°C for 3 seconds to obtain a biaxially oriented polyester film having a laminated structure with a thickness of 4.5 μm. The properties of the obtained film are shown in Table 1.
[0075] [Examples 2 to 4] A biaxially oriented polyester film having a laminated structure was obtained in the same manner as in Example 1 except that the type and amount of the added particles and the film thickness were changed as shown in Table 1. The properties of the obtained film are shown in Table 1.
[0076] [Preparation of PET-based raw material] (1-a) Preparation of PET pellets: 194 parts by mass of dimethyl terephthalate and 124 parts by mass of ethylene glycol were charged into a transesterification reactor, and the contents were heated to 140°C to dissolve. Thereafter, 0.3 part by mass of magnesium acetate tetrahydrate and 0.05 part by mass of antimony trioxide were added while stirring the contents, and a transesterification reaction was carried out at 140 to 230°C while distilling off methanol. Next, 0.5 part by mass of a 5 mass% ethylene glycol solution of trimethyl phosphate (0.025 part by mass as trimethyl phosphate) and 0.3 part by mass of a 5 mass% ethylene glycol solution of sodium dihydrogen phosphate dihydrate (0.015 part by mass as sodium dihydrogen phosphate dihydrate) were added.
[0077] When the ethylene glycol solution of trimethyl phosphate is added, the temperature of the reaction contents decreases. Therefore, stirring was continued until the temperature of the reaction contents returned to 230°C while distilling off excess ethylene glycol. After the temperature of the reaction contents in the transesterification reactor reached 230°C in this way, the reaction contents were transferred to a polymerization reactor.
[0078] After the transition, the reaction system was gradually heated from 230°C to 275°C, and the pressure was lowered to 0.1kPa. The time to reach the final temperature and the final pressure was both 60 minutes. After reaching the final temperature and the final pressure, the reaction was continued for 2 hours (3 hours from the start of polymerization), and the stirring torque of the polymerization apparatus showed a predetermined value (the specific value differs depending on the specifications of the polymerization apparatus, but the value shown by polyethylene terephthalate with an intrinsic viscosity of 0.55 in this polymerization apparatus was set as the predetermined value). The reaction system was then purged with nitrogen and returned to normal pressure to stop the polycondensation reaction, and the mixture was discharged into cold water in the form of a strand, and immediately cut to obtain PET pellets of polyethylene terephthalate with an intrinsic viscosity (orthochlorophenol, 35°C) of 0.55 dl / g (raw material-1a).
[0079] Using a rotary vacuum polymerization apparatus, the above PET pellets (raw material-1a) were heat-treated for a long time at a temperature of 230°C under a reduced pressure of 0.1 kPa, and solid-state polymerization was carried out until the intrinsic viscosity (orthochlorophenol, 35°C) reached 0.70 dl / g (raw material-1ak).
[0080] (2) Preparation of particle-containing PET pellets (raw material-2a): 90 parts by mass of the above-mentioned solid-phase polymerization PET pellets (raw material-1ak: processing time 2 hours) and 10 parts by mass of 10% by mass water slurry of cross-linked polystyrene particles with an average particle size of 0.30 μm (1 part by mass as cross-linked polystyrene particles) were fed into a vented twin-screw kneading extruder of the same direction rotation type heated to 280°C, and the vent hole was kept at a reduced pressure of 1 kPa or less to remove moisture, and particle-containing pellets (raw material-2a) containing 1% by mass of cross-linked polystyrene particles and having an intrinsic viscosity (orthochlorophenol, 35°C) of 0.62 dl / g were obtained.
[0081] (3) Preparation of particle-containing PET pellets (raw material-2b): 90 parts by mass of the above-mentioned solid-phase polymerization PET pellets (raw material-1ak: processing time 2 hours) and 10 parts by mass of 10% by mass water slurry of spherical silica particles with an average particle size of 0.10 μm (1 part by mass as spherical silica particles) were fed into a vented twin-screw kneading extruder of the same direction rotation type heated to 280°C, and the vent hole was kept at a reduced pressure of 1 kPa or less to remove moisture, and particle-containing pellets (raw material-2b) containing 1% by mass of spherical silica particles and having an intrinsic viscosity (orthochlorophenol, 35°C) of 0.62 dl / g were obtained.
[0082] (4) Preparation of two-component composition (mass ratio PET / PEI = 50 / 50) pellets (raw material-3): The solid-phase polymerized PET pellets (raw material-1ak: processing time 2 hours) obtained by the above method and pellets of PEI "Ultem" (registered trademark) 1010 manufactured by SABIC Innovative Plastics were fed into a vented twin-screw kneading extruder (manufactured by Japan Steel Works, Ltd., screw diameter 30 mm, screw length / screw diameter = 45.5) of the same direction rotation type equipped with three kneading paddle kneading sections heated to a temperature of 280 ° C., and the pellets were mixed at a shear rate of 100 sec. -1 The mixture was melt-extruded with a residence time of 1 minute to obtain two-component composition pellets containing 50% by mass of PEI. The glass transition temperature of the two-component composition pellets thus produced was 150° C. (raw material-3).
[0083] [Example 5] Using two extruders, extruder 1 for forming the polyester layer on the rough surface side and extruder 2 for forming the polyester layer on the flat surface side, a laminated unstretched film was produced by co-extrusion as follows: 74 parts by mass of PET pellets (raw material-1ak), 4 parts by mass of particle-containing PET pellets (raw material-2a), 12 parts by mass of particle-containing PET pellets (raw material-2b), and 10 parts by mass of two-component composition pellets (raw material-3) were fed to extruder 1 after drying at 170°C for 3 hours, and 84 parts by mass of PET pellets (raw material-1ak), 6 parts by mass of particle-containing PET pellets (raw material-2b), and 10 parts by mass of two-component composition pellets (raw material-3) were fed to extruder 2 after drying at 170°C for 3 hours. After molten in each extruder, the two layers of resin were merged in the molten state so that the layer thickness ratio was rough side / flat side = 10 / 90, and extruded from the extrusion die so that the rough side was in contact with a casting drum maintained at a surface finish of 0.3S and a surface temperature of 20°C, where it was rapidly cooled and solidified to obtain a laminated unstretched film.
[0084] The laminated unstretched film thus obtained was preheated at 70°C, and then stretched 3 times by heating it between low-speed and high-speed rolls from 14 mm above with an infrared heater having a surface temperature of 800°C, quenched, and then fed to a tenter, stretched 4.5 times in the transverse direction at 100°C, and heat-set at 205°C for 3 seconds to obtain a film with a thickness of 4.5 μm. The properties of the obtained film are shown in Table 1.
[0085] [Comparative Examples 1 to 2, Comparative Example 4] A film was obtained in the same manner as in Example 1, except that the type and amount of particles added were changed as shown in Table 1. The properties of the obtained film are shown in Table 1.
[0086] [Comparative Example 3] The same operation as in Example 1 was repeated to obtain a laminated unstretched film. The laminated unstretched film thus obtained was preheated at 120°C, and further heated between low-speed and high-speed rolls from 14 mm above with an infrared heater having a surface temperature of 830°C to be stretched 4.8 times, quenched, and then fed to a tenter, stretched 5.75 times in the transverse direction at 170°C, and heat-set at 215°C for 3 seconds to obtain a film having a thickness of 4.5 μm. The properties of the obtained film are shown in Table 1.
[0087] [Table 1]
[0088] In Table 1, PEN means polyethylene-2,6-naphthalenedicarboxylate, PET means polyethylene terephthalate, PEI means polyetherimide, cross-linked Pst means cross-linked polystyrene particles, and spherical silica means spherical silica particles.
[0089] As shown in Table 1, the biaxially oriented polyester films of Examples 1 to 5 satisfied the relational formula (1) and had a height of 0.4% area in the bearing curve of 65 nm or more and less than 90 nm, and therefore had excellent winding properties in the base film manufacturing process, excellent electromagnetic conversion characteristics when made into a magnetic recording tape, and little signal dropout.
[0090] In contrast, Comparative Example 1, which does not satisfy the relational expression (1) and in which the height of the 0.4% area in the bearing curve is too large, had good winding properties but poor properties when used as a magnetic recording tape, and Comparative Example 2, in which the height of the 0.4% area in the bearing curve is too small, had good magnetic recording tape properties but poor winding properties. Comparative Example 3, which does not satisfy the relational expression (1) and in which the height of the 0.4% area in the bearing curve is too large, had high surface roughness and poor properties when used as a magnetic recording tape. Comparative Example 4, in which the height of the 0.4% area is too large, had good winding properties but poor tape properties. [Industrial Applicability]
[0091] The biaxially oriented polyester film of the present invention can be suitably used as a base film for magnetic recording tapes, particularly for high-capacity data storage, and can be suitably used as a data storage device having a large storage capacity, which can realize high-density recording.
Claims
1. A biaxially oriented polyester film characterized in that, when measured on at least one surface with a non-contact surface profiler, where X is 0.075 μm, 0.100 μm, and 0.125 μm, the logarithmic value y of the protrusion frequency of protrusions that are equal to or greater than the protrusion height X satisfies the following relational expression (1), and the protrusion height corresponding to 0.4% area in a bearing curve based on the protrusion height distribution is 65 nm or more and less than 90 nm. -24.9X+2.50≦y≦-24.9X+3.8 (1) (Here, X is the protrusion height (μm), and y is the logarithm to the base 10 of the number of protrusions that are equal to or greater than the protrusion height X in a visual field of an area of 282 μm × 211 μm.)
2. 2. The biaxially oriented polyester film according to claim 1, wherein the polyester contained in said biaxially oriented polyester film has ethylene terephthalate or ethylene-2,6-naphthalene dicarboxylate as a main repeating unit.
3. 3. The biaxially oriented polyester film according to claim 1, wherein when the one surface and the other surface of the biaxially oriented polyester film are measured using a non-contact surface profile measuring device, the centerline average surface roughness of the one surface is 1 nm or more rougher than the centerline average surface roughness of the other surface.
4. The biaxially oriented polyester film according to any one of claims 1 to 3, which contains inert particles.
5. The biaxially oriented polyester film according to any one of claims 1 to 4, wherein the biaxially oriented polyester film is a laminate of two or more different polyester layers.
Citation Information
Patent Citations
Composite film
JP2008290365A
Polyester film and data storage using the same
JP2010205321A
Laminated polyester film and coated magnetic recording tape using this polyester film
JP2012153100A
Biaxially oriented laminated polyester film and coating type magnetic recording tape using the same
JP2015003408A
Two-axially oriented polyester film and magnetic recording medium
JP2016079410A