METHOD FOR PRODUCING METAL CARBIDE AND HYDROCARBON, AND CARBON-CONTAINING COMPONENT

By employing molten salts to deposit carbon on electrodes and electrolyzing at lower temperatures, the method efficiently produces metal carbides and hydrocarbons, addressing the inefficiencies and emissions of traditional high-temperature processes.

JP7583418B2Active Publication Date: 2024-11-14DAIKIN INDUSTRIES LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024048291
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-03-25
Publication Date
2024-11-14
Estimated Expiration
2044-03-25

AI Technical Summary

Technical Problem

Existing methods for producing metal carbides and hydrocarbons require high temperatures, leading to low energy efficiency and significant CO2 emissions, and existing carbon sources yield low metal carbide production efficiency.

Method used

A method involving the use of molten salts containing alkali or alkaline earth metal ions and carbonate ions to deposit carbon on an electrode, followed by electrolysis at relatively low temperatures to produce metal carbides, which can then be hydrolyzed to generate hydrocarbons.

Benefits of technology

The method enables efficient production of metal carbides and hydrocarbons at lower temperatures, reducing energy consumption and CO2 emissions while increasing yield and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583418000009
    Figure 0007583418000009
  • Figure 0007583418000010
    Figure 0007583418000010
  • Figure 0007583418000011
    Figure 0007583418000011
Patent Text Reader

Abstract

To provide a manufacturing method capable of efficiently obtaining a metal carbide through a prompt progress of a reaction at a comparatively low temperature, a method of manufacturing hydrocarbon from the obtained metal carbide, and a carbon-containing member carrying the metal carbide.SOLUTION: A manufacturing method of a metal carbide includes: an electrode manufacturing process including preparing a first molten salt containing a carbonate ion and at least one kind of first metal ion selected from a group consisting an alkali metal ion and an alkaline earth metal ion, and applying a voltage to the first molten salt to deposit a deposition containing carbon at a first electrode so as to obtain a second electrode; and an electrolysis process including applying a voltage using the second electrode to a second molten salt containing at least one kind of second metal ion selected from a group consisting an alkali metal ion and an alkaline earth metal ion to obtain a carbide composition containing a carbide of the second metal.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing metal carbides and hydrocarbons, and to a carbon-containing component. [Background technology]

[0002] Acetylene is an industrially important substance as a raw material for various organic compounds. Acetylene is usually obtained by the reaction of metal carbide (mainly calcium carbide) with water.

[0003] Calcium carbide is generally obtained by heating a mixture of quicklime (calcium oxide) and coke to a high temperature in an electric furnace (for example, Patent Document 1). Patent Document 2 proposes, with regard to the production of calcium carbide, to previously briquette coke and mix it with quicklime. Patent Document 3 proposes a method for producing lithium carbide by reacting metallic lithium obtained by melt electrolysis of lithium chloride with carbon powder such as carbon black. Non-Patent Document 1 proposes a method for producing lithium carbide by reacting metallic lithium obtained by molten salt electrolysis of lithium hydroxide with a carbon source such as carbon dioxide. Non-Patent Document 2 proposes a method for producing lithium carbide by reacting metallic lithium with carbon. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 178412 / 1983 [Patent Document 2] JP 2018-35328 A [Patent Document 3] Japanese Patent Application Publication No. 2-256626 [Non-patent literature]

[0005] [Non-Patent Document 1] McEnaney JM, Rohr BA, Nielander AC, Singh AR, King LA, Norskov JK, Jaramillo TF, “A cyclic electrochemical strategy to produce acetylene from CO2, CH4, or alternative carbon sources.”, Sustain Energy Fuels 4:2, 752-2759 (2020) [Non-Patent Document 2] Uwe Ruschewitz, “Binary and ternary carbides of alkali and alkaline-earth metals”, Coordination Chemistry Reviews 244, 115-136 (2003) Summary of the Invention [Problem to be solved by the invention]

[0006] To produce metal carbide, it is usually necessary to heat the raw material to 2000°C or higher. Therefore, there is a problem that the energy efficiency is low and a large amount of carbon dioxide is generated. In addition, in Patent Documents 1 to 3, carbon itself is used as the carbon source of metal carbide. In Non-Patent Document 1, it is described that when carbon dioxide is used as the carbon source, the yield of lithium carbide does not exceed 20% in theory, but the yield of lithium carbide can be increased by using carbon as the carbon source. However, no experimental data supporting this is shown. In Non-Patent Document 2, it is described that amorphous carbon or graphite is used as the carbon source, but in order to produce crystalline lithium carbide, it is necessary to contact metallic lithium vapor at 800°C to 900°C or to contact metallic lithium in an arc melting furnace at approximately 3500°C or higher.

[0007] The present disclosure aims to provide a production method in which a reaction proceeds quickly at a relatively low temperature (for example, 800° C. or lower) and metal carbide can be efficiently obtained. The present disclosure further provides a method for producing hydrocarbons from the obtained metal carbide. In addition, the present disclosure provides a carbon-containing member carrying metal carbide. [Means for solving the problem]

[0008] The present disclosure includes the following aspects. [1] Preparing a first molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions and carbonate ions; and an electrode preparation step including applying a voltage to the first molten salt to cause a carbon-containing precipitate to precipitate on a first electrode, thereby obtaining a second electrode; applying a voltage to a second molten salt containing at least one type of second metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions, using the second electrode, to obtain a carbide composition containing carbide of the second metal.

[0009] [2] The method for producing metal carbide according to [1] above, wherein the first electrode contains at least one selected from the group consisting of transition metals and alloys containing transition metals.

[0010] [3] The method for producing metal carbide according to [1] or [2] above, wherein the first electrode comprises an alloy containing iron.

[0011] [4] The method for producing metal carbide according to any one of the above [1] to [3], wherein the first electrode comprises SUS304.

[0012] [5] The method for producing metal carbide according to any one of the above [1] to [4], wherein the second molten salt is substantially free of carbonate ions.

[0013] [6] The method for producing metal carbide according to any one of the above [1] to [5], wherein in the electrolysis step, the first molten salt used in the electrode preparation step is used as the second molten salt as it is.

[0014] [7] The method for producing metal carbide according to any one of the above [1] to [6], wherein the second molten salt contains, as an anion, at least one selected from the group consisting of a halide ion and an oxide ion.

[0015] [8] The method for producing metal carbide according to any one of the above [1] to [7], wherein the first metal ion and the second metal ion are the same.

[0016] [9] The method for producing a metal carbide according to any one of the above [1] to [8], wherein the carbide composition further contains at least one selected from the group consisting of carbon, an elemental substance, a halide, a carbonate, an oxide, a hydride, and a peroxide of the second metal, and an elemental substance, a halide, a carbonate, an oxide, and a carbide of the first metal.

[0017]

[10] The method for producing metal carbide according to any one of the above [1] to [9], wherein the second molten salt contains, as the second metal ions, at least one selected from the group consisting of sodium ions, lithium ions, and potassium ions, and calcium ions.

[0018]

[11] Preparing a first molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions and a carbonate ion derived from carbon dioxide; and an electrode preparation step including applying a voltage to the first molten salt to cause a precipitate containing carbon to be deposited on a first electrode to obtain a second electrode; an electrolysis step including applying a voltage to a second molten salt containing at least one second metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions, using the second electrode, to obtain a carbide composition containing a carbide of the second metal; and a gas generating step including hydrolyzing the carbide of the second metal to obtain a gas containing a hydrocarbon.

[0019]

[12] The method for producing hydrocarbons according to the above

[11] , wherein the hydrocarbon is acetylene.

[0020]

[13] The method for producing hydrocarbons according to

[11] or

[12] above, wherein the gas contains acetylene as the hydrocarbon and further contains at least one selected from the group consisting of ethylene, ethane, methane, methylacetylene, propylene, butene, and hydrogen.

[0021]

[14] A substrate; a metal carbide composition supported on the substrate, the metal carbide composition including a carbide of at least one second metal selected from the group consisting of alkali metals and alkaline earth metals.

[0022]

[15] A substrate; a metal carbide layer covering at least a portion of the substrate and including at least one second metal carbide selected from the group consisting of alkali metals and alkaline earth metals; a carbon layer covering at least a portion of the metal carbide layer, the carbon layer comprising carbon and being substantially free of the second metal carbide. Effect of the Invention

[0023] According to the present disclosure, it is possible to provide a production method in which a reaction proceeds quickly at a relatively low temperature and metal carbide can be efficiently obtained, a method for producing hydrocarbons from the obtained metal carbide, and a carbon-containing member supporting metal carbide. [Brief description of the drawings]

[0024] [Figure 1] 1 is a flow chart illustrating a method for producing metal carbide according to the present disclosure. [Diagram 2]1 is a flow chart illustrating a method for producing a hydrocarbon according to the present disclosure. [Figure 3A] 1 is a photograph showing the appearance of a working electrode before an electrolysis step in Example 6-1. [Figure 3B] 1 is a photograph showing the appearance of a working electrode after an electrolysis step in Example 6-1. [Figure 3C] 1 is a cross-sectional photograph of a deposit deposited on a working electrode after an electrolysis step in Example 6-1. [Figure 4A] 1 is a photograph showing the appearance of the working electrode after the electrolysis step in Example 6-2. [Figure 4B] 1 is an optical microscope photograph of a cross section of a deposit deposited on a working electrode after the electrolysis step in Example 6-2, observed using a micro-Raman spectroscopic analyzer. [Figure 4C] 1 is a graph showing the results of Raman spectroscopy of the precipitate obtained in Example 6-2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] First embodiment In the method for producing metal carbide according to the present embodiment, a voltage is applied to a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions and carbonate ions derived from carbon dioxide to cause a first precipitate containing carbon to precipitate on a first electrode made of SUS304, thereby obtaining a second electrode (electrode preparation step). Next, metal carbide is obtained by electrolysis using the first molten salt used in the electrode preparation step as it is, with the carbon precipitated on the second electrode as a carbon source (electrolysis step).

[0026] This allows metal carbide to be obtained efficiently at a relatively low temperature of 800°C or less. Furthermore, CO2, which is said to be a cause of global warming, can be effectively used as a carbon source. In addition, the first molten salt used in the electrode preparation process is used as is in the next electrolysis process, that is, the electrode preparation process and the electrolysis process are performed in the same electrolytic bath, so productivity is high.

[0027] This embodiment includes obtaining hydrocarbons by hydrolyzing the metal carbide obtained by the above-mentioned method. According to this method, it is possible to obtain high-purity hydrocarbons efficiently.

[0028] The present embodiment includes a carbon-containing component having a metal carbide supported thereon, the carbon-containing component being capable of being utilized in the production of hydrocarbons.

[0029] [Metal carbide manufacturing method] The method for producing metal carbide according to the present disclosure includes an electrode preparation step including preparing a first molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions and carbonate ions, and applying a voltage to the first molten salt to cause a deposit containing carbon to be deposited on the first electrode to obtain a second electrode, and an electrolysis step including applying a voltage to a second molten salt containing at least one second metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions using the second electrode to obtain a carbide composition containing carbide of the second metal. Fig. 1 is a flow chart showing the method for producing metal carbide according to the present disclosure.

[0030] (I) Electrode preparation process In the electrode preparation process, a carbon-containing deposit is deposited on a first electrode to prepare a second electrode. The carbon on the second electrode is used as a carbon source for producing metal carbide in the electrolysis process. The carbon-containing deposit is deposited on the surface of the electrode with a lower potential (cathode). Hereinafter, the first electrode may be referred to as the "cathode" and the other electrode as the "anode."

[0031] The electrode preparation process includes preparing a first molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions and carbonate ions, and applying a voltage to the first molten salt to cause a first precipitate containing carbon to precipitate on the first electrode, thereby obtaining a second electrode.

[0032] (i) Preparation of first molten salt (S11) A first molten salt containing a first metal ion and a carbonate ion derived from carbon dioxide is prepared. The first metal ion is generated by ionizing the salt of the first metal. The carbonate ion is generated by adding a gas containing carbon dioxide to the electrolytic bath. In the first molten salt, it is not necessary that the first metal salt and the carbon dioxide are all ionized. In this embodiment, for convenience, the salt of the first metal contained in the electrolytic bath is referred to as the first metal salt even if it is completely ionized, and the molten salt prepared from the first metal salt and carbon dioxide is referred to as the first molten salt even if they are not completely ionized.

[0033] (First metal ion) The first metal ion is at least one selected from the group consisting of alkali metal ions and alkaline earth metal ions. The alkali metal ions and alkaline earth metal ions have excellent electrolyte functions.

[0034] The alkali metal may be at least one selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs) and francium (Fr). The alkali metal may be at least one selected from the group consisting of Li, Na, K, Rb and Cs. The alkali metal may in particular be at least one selected from the group consisting of Li, Na, K and Cs.

[0035] The alkaline earth metal may be at least one selected from the group consisting of beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba) and radium (Ra). The alkaline earth metal may be at least one selected from the group consisting of Mg, Ca, Sr and Ba.

[0036] (other metal ions) The first molten salt may contain a metal ion (a third metal ion) other than the first metal ion. It is preferable that the salt of the third metal ion ionizes at a temperature of 800° C. or lower.

[0037] The third metal may be at least one selected from the group consisting of rare earth elements, aluminum (Al), gallium (Ga), indium (In), thallium (Tl), zinc (Zn), cadmium (Cd), gold (Au), silver (Ag) and copper (Cu). The rare earth elements may be scandium (Sc), yttrium (Y), lanthanide elements and actinide elements.

[0038] (carbonate ion derived from carbon dioxide) Carbonate ions are generated by adding a gas containing carbon dioxide to the electrolytic bath. A gas containing carbon dioxide (hereinafter, sometimes referred to as CO2 gas) is brought into contact in a gaseous state with the first metal salt in a liquid state. The CO2 gas may be blown into the gas phase of the electrolytic bath to bring it into contact with the liquid surface of the first metal salt, or the CO2 gas may be blown into the first metal salt. The CO2 gas may be a mixed gas of CO2 and an inert gas (typically argon). A sufficient amount of CO2 gas may be added to the first metal salt before the voltage is applied, or the CO2 gas may be added to the first metal salt while the voltage is being applied.

[0039] The amount of CO2 gas to be blown in may be appropriately set depending on the amount of the first metal ion. For example, the amount of CO2 gas to be blown in is equal to or greater than the equivalent amount of the first metal salt, taking into account the efficiency of absorption of the gas into the first metal salt.

[0040] In order to promote dissolution of CO2 into the first metal salt, it is desirable that the bubble diameter of the CO2 gas to be blown in is small. The bubble diameter of the CO2 gas is preferably 10 mm or less, more preferably 1 mm or less. The bubble diameter of the CO2 gas may be 100 nm or more, and may be 1 μm or more. The bubble diameter of the CO2 gas can be made fine by, for example, bubbling through a porous material made of quartz glass or high-purity alumina, stirring with a stirrer, applying vibration, or irradiating with ultrasonic waves.

[0041] It is preferable to preheat the CO2 gas to a temperature close to that of the first metal salt, which makes it easier to prevent the first metal salt from being solidified due to a drop in temperature.

[0042] (other anions) The first molten salt may contain anions other than carbonate ions. Examples of the other anions include halide ions, sulfate ions, phosphate ions, nitrate ions, acetate ions, carboxylate ions, and oxide ions (O 2- ) The other anion may include a halide ion derived from a halide of the first metal. The halide of the first metal is generally used as a molten salt and is excellent as an electrolyte.

[0043] (ii) Application of voltage (S12) Next, a voltage is applied to the first molten salt. This causes the CO3 2- is reduced to obtain a precipitate containing carbon (Equation 1). The carbon contained in the precipitate may be polycrystalline, and may be polycrystalline with a high degree of crystallinity (e.g., polycrystalline like carbon nanotubes). Carbide of the first metal may also be precipitated on the cathode. O 2- is oxidized to produce oxygen (Equation 2). (Formula 1) 2CO3 2- +8e - → 2C+6O 2- (Formula 2) 2O 2- → O2+4e -

[0044] When the first metal is Ca, calcium carbide (CaC2) may be precipitated on the cathode (Formula 3). Metallic calcium may also be produced on the cathode (Formula 4). Some or all of the metallic lithium produced in this side reaction may further react to become calcium carbide (Formula 5). Alternatively, metallic calcium may react with carbon dioxide physically dissolved in the first molten salt to become calcium carbide (Formula 6). Fine carbon powder may be produced, causing the molten salt to become black and turbid (Formula 7). The CaO produced in (Formula 6) and (Formula 7) above immediately dissolves in the molten salt to produce calcium ions and oxide ions (Formula 8). (Formula 3) Ca 2+ +2CO3 2- +10e - → CaC2+6O 2- (Formula 4) Ca 2+ +2e - → Ca (Formula 5) Ca+2C → CaC2 (Formula 6) 2CO2+5Ca → CaC2+4CaO (Formula 7) 2Ca+CO2→ C+2CaO (Formula 8) CaO → Ca 2+ +O 2-

[0045] When the first metal is Na, K or Li, a similar reaction occurs to precipitate sodium carbide (Na2C2), potassium carbide (K2C2) or lithium carbide (LiC2) along with carbon. The same is true for other first metals.

[0046] On the anode, O 2- is oxidized to produce oxygen. The oxygen produced on the anode is released into the gas phase. This oxygen gas can be collected and used for other purposes.

[0047] The voltage is applied at a temperature at which the first molten salt can be maintained in a molten state. The temperature of the electrolytic bath may be, for example, 350° C. or higher, or 400° C. or higher. The temperature of the electrolytic bath may be, for example, 800° C. or lower, or 700° C. or lower. According to the present disclosure, the reaction proceeds at such a relatively low temperature, and therefore the energy efficiency is high.

[0048] The applied voltage is set so that the potential of the first electrode (cathode) is equal to or lower (lower) than the potential (Ec) at which carbon is deposited. The current value may be appropriately set according to the supply amount of CO2 per unit time. For example, the current value is set to the ratio of the CO3 2- The amount of CO3 consumed per unit time at the cathode so that the concentration does not decrease 2- Therefore, CO2 and O2 in the first molten salt - CO3 produced by reaction with 2- is set so that

[0049] In this embodiment, a cathode made of SUS304 is used. This significantly improves the Faraday efficiency. In addition, SUS304 is relatively easy to obtain, inexpensive, and has excellent heat resistance, making it desirable. SUS304 is an austenitic stainless steel, and its components are described in JIS G 4303 and the like.

[0050] The material of the cathode is not limited to SUS304. Examples of the material of the cathode include metals such as Ag, Cu, Ni, Pb, Hg, Tl, Bi, In, Sn, Cd, Au, Zn, Ga, Ge, Fe, Pt, Pd, Ru, Ti, Cr, Mo, W, V, Nb, Ta, Zr, and alloys thereof. Specific examples of alloys include ferritic stainless steel such as SUS430.

[0051] In particular, from the viewpoint of Faraday efficiency, the cathode may include at least one selected from the group consisting of transition metals and alloys containing transition metals. Among the transition metals, Ni, Fe, Mo, and Ti may be used. The cathode may include, in particular, an iron alloy (typically, stainless steel) or may be formed from an iron alloy. The cathode may include, in particular, SUS304 or may be formed from SUS304.

[0052] The material of the anode is not particularly limited. Examples of the material of the anode include Pt, conductive metal oxide, glassy carbon, natural graphite, isotropic graphite, pyrolytic graphite, plastic formed carbon, and boron-doped diamond. Examples of electrodes made of conductive metal oxide include transparent conductive electrodes called ITO electrodes in which a mixed oxide of indium and tin is formed on glass, electrodes called DSA electrodes (trademark of De Nora Permelec Electrodes, Inc.) in which oxides of platinum group metals such as ruthenium and iridium are formed on a substrate such as titanium, and La 1-x Sr x FeO 3-δ (0≦x≦0.5 (particularly, 0.1≦x≦0.5), 0≦δ≦0.5), etc. Among them, conductive metal oxide anodes are preferred because they are less likely to be consumed due to oxidation reactions.

[0053] The electrode preparation step provides a second electrode carrying a deposit containing carbon.

[0054] (II) Electrolysis process (S2) In the electrolysis step, a second molten salt containing at least one second metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions is electrolyzed using the second electrode obtained in the electrode preparation step, whereby a carbide composition containing carbide of the second metal is obtained using the carbon supported on the second electrode as a carbon source.

[0055] (Second metal ion) The second metal ion is at least one selected from the group consisting of alkali metal ions and alkaline earth metal ions. The second metal ion is a metal source for the target metal carbide. Carbides of alkali metals and alkaline earth metals, also called acetylides, are easy to produce acetylene by hydrolysis and are of high industrial value. In addition, as described above, alkali metal ions and alkaline earth metal ions have excellent functions as electrolytes.

[0056] In terms of industrial value, the second metal ion may include an alkaline earth metal ion, and may include a Ca ion. The second metal ion may include an alkali metal ion together with an alkaline earth metal ion. The alkali metal ion has an excellent function as an electrolyte, such as facilitating the ionization of an alkaline earth metal salt, promoting the generation of an alkaline earth metal ion, lowering the melting point of the molten salt, and enabling electrolysis at a lower temperature. The first metal ion may include at least one selected from the group consisting of Li, Na, K, Rb, and Cs ions as an alkali metal ion, and at least one selected from the group consisting of Be, Mg, Ca, Sr, and Ba ions as an alkaline earth metal ion. In particular, it may include at least one of Li, Na, and K ions, and Ca ions.

[0057] The amount of the second metal ion contained in the second molten salt is not particularly limited. Since the second metal ion is a metal source of the target metal carbide, it is desirable that a sufficient amount is contained. The number of moles of the second metal ion may be 1 mol% or more, 2 mol% or more, or 3 mol% or more, based on the total number of moles of cations in the electrolytic bath. The number of moles of the second metal ion may be 20 mol% or less, 15 mol% or less, or 10 mol% or less, based on the total number of moles of cations in the electrolytic bath. In one embodiment, the number of moles of the second metal ion is 1 mol% or more and 20 mol% or less, based on the total number of moles of cations in the electrolytic bath.

[0058] When the first molten salt used in the electrode preparation step is used as the second molten salt as is, as in this embodiment, a second metal ion may be further added to the electrolytic bath before the electrolysis step.

[0059] (anion) Examples of the counter ion (anion) of the second metal ion include a halide ion, a sulfate ion, a phosphate ion, a nitrate ion, an acetate ion, a carboxylate ion, and an oxide ion (O 2- ) is at least one selected from the group consisting of:

[0060] The second molten salt may contain at least one of halide ions and oxide ions as anions. In particular, the second molten salt may contain both halide ions and oxide ions. While oxides of the second metal are easy to obtain, their melting temperature tends to be high. Halides of the second metal are commonly used as molten salts. However, halide ions may generate halogen gas at the anode, which has a high oxidizing power (and may cause corrosion). When the molten salt contains both halide ions and oxide ions, it is possible to lower the melting temperature of the molten salt while suppressing the generation of halogen gas.

[0061] The halogen includes at least one selected from the group consisting of fluorine (F), chlorine (Cl), bromine (Br), iodine (I) and astatine (At). The halogen may be at least one selected from the group consisting of F, Cl, Br and I, and may be, in particular, F and / or Cl.

[0062] The second molten salt is carbonate ions (CO3 2- ) is preferably substantially free of carbonate ions. If the second molten salt contains carbonate ions, it will react with electrons generated by the discharge of the second metal (Formula 7) and carbon will be easily produced. This will decrease the yield of the second metal carbide. If the second molten salt is substantially free of carbonate ions, such side reactions are suppressed and the yield of the second metal carbide will increase. (Formula 7) 2CO32- +8e - → 2C+6O 2-

[0063] "Substantially free of carbonate ions" allows the presence of carbonate ions to an extent that they are not involved in the electrolytic reaction. The second molten salt may contain, for example, about 1.0 mol% or less of carbonate ions. The carbonate ion concentration in the second molten salt may be 0.5 mol% or less, 0.3 mol% or less, or 0 mol%.

[0064] Specific examples of second metal salts containing alkaline earth metal ions include CaO, CaCl2, CaF2, CaBr2, CaI2, CaH2, and Ca3P2.Specific examples of second metal salts containing alkali metal ions include LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI.

[0065] The second metal ion may be the same as or different from the first metal ion. The first metal ion and the second metal ion may be the same. In this embodiment, the first molten salt used in the electrode preparation step is used as the second molten salt in the electrolysis step, so the second metal ion may contain the same type of metal ion as the first metal ion.

[0066] The material of the other electrode (anode) is not particularly limited. The material of the anode may be the same as that used in the electrode preparation process. In this embodiment, the anode used in the electrode preparation process may be used in the electrolysis process as it is.

[0067] When a voltage is applied to the second molten salt, the second metal ions are reduced on the carbon constituting the cathode (second electrode) to produce the second metal, which immediately reacts with the carbon constituting the cathode (second electrode) to produce a composition containing the second metal carbide (metal carbide composition). If there is a second metal salt that has not been ionized in the second molten salt, the application of a voltage can also promote ionization of the second metal salt.

[0068] When the second metal is Ca, calcium carbide (CaC2) is produced (Equation 8). Calcium metal may also be produced on the cathode through a side reaction (Equation 9). Some or all of the calcium metal produced in this side reaction may further react to form calcium carbide. (Formula 8) Ca 2+ +2C +2e - → CaC2 (Formula 9) Ca 2+ +2e - → Ca

[0069] The voltage is applied at a temperature at which the molten salt can be maintained in a molten state. The temperature of the electrolytic bath may be, for example, 350° C. or higher, or 400° C. or higher. The temperature of the electrolytic bath may be, for example, 800° C. or lower, or 700° C. or lower. According to the present disclosure, the reaction proceeds at such a relatively low temperature, and therefore the energy efficiency is high.

[0070] The applied voltage is set so that the cathode potential is lower (more noble) than the potential (Emc) at which the second metal is deposited on the cathode. This can further improve the selectivity of the second metal carbide. If the cathode potential is too high (more noble), the amount of the target second metal carbide produced is likely to decrease. If the cathode potential is too low (more noble), the second metal carbide is produced, but the metal with the most noble redox potential in the molten salt is mainly deposited among the metals contained in the molten salt. If multiple metals with similar redox potentials are present in the molten salt, an alloy of multiple metals may be deposited. The potential Emc can be determined by performing cyclic voltammetry measurements in the molten salt to be used, using a metal electrode to be used, for example, a SUS304 electrode.

[0071] The set current value when constant current electrolysis is performed may be appropriately set so that the cathode potential during electrolysis falls within the above-mentioned potential range.

[0072] The metal carbide composition is usually obtained in a state supported on the cathode (strictly speaking, on the substrate derived from the first (second) electrode used as the cathode). When a molten salt having excellent solubility for the second metal carbide is used, the second metal carbide is obtained in a state where it is partially or entirely dissolved in the molten salt. If the second metal carbide is dissolved in the molten salt in advance, the second metal carbide obtained by electrolysis is easily precipitated on the cathode, and is easily obtained in a state where it is supported on the substrate derived from the first electrode.

[0073] The metal carbide composition includes a carbide of a second metal. The second metal carbide is a main component of the metal carbide composition. The main component is a component that occupies 50 mass% or more of the total mass of the metal carbide composition. The content ratio of the second metal carbide may be 80 mass% or more, or 90 mass% or more, of the mass of the metal carbide composition. The content ratio of the second metal carbide may be 99.9 mass% or less, or 99 mass% or less, of the mass of the metal carbide composition. In one embodiment, the content ratio of the second metal carbide is 80 mass% or more and 99.9 mass% or less of the mass of the metal carbide composition.

[0074] The metal carbide composition may include at least one selected from the group consisting of carbon, an elemental product, a halide, a carbonate, an oxide, a hydride, and a peroxide of the second metal as a by-product. The metal carbide composition may further include at least one selected from the group consisting of an elemental product, a halide, a carbonate, an oxide, and a carbide of the first metal.

[0075] The metal carbide composition may further include at least one selected from the group consisting of solidified electrolytes (other metal salts), halides, oxides, metals, and hydrates of the materials constituting the device.

[0076] The carbon contained in the metal carbide composition is at least one selected from the group consisting of nanocarbon materials such as graphite, amorphous carbon, glassy carbon, carbon nanotube, diamond, nanodiamond, graphene, etc. By continuing the electrolysis of the above method, a second metal carbide can be further obtained from the carbon contained in the metal carbide composition. In this case, the yield can be further increased.

[0077] The presence and quantification of the second metal carbide, the second metal itself, compounds containing the second metal, and other by-products can be performed, for example, by Raman spectroscopy and X-ray diffraction (XRD) analysis of the composition.

[0078] [Carbon-containing materials] The present disclosure encompasses a carbon-containing component comprising a substrate and a metal carbide composition supported on the substrate, the metal carbide composition comprising at least one second metal carbide selected from the group consisting of alkali metals and alkaline earth metals. The carbon-containing component according to the present disclosure can be utilized in the production of hydrocarbons.

[0079] The carbon-containing member can be obtained by, for example, the above-mentioned method for producing a metal carbide. That is, the carbon-containing member can correspond to the second electrode used in the electrolysis of the second molten salt. In this case, the substrate is derived from the second electrode.

[0080] The metal carbide composition may be supported on at least a portion of the surface of the substrate. The surface of the substrate typically corresponds to the portion that was in contact with the second metal ion of the second electrode. Supported includes a state in which at least a portion of the surface of the substrate is covered with the metal carbide composition.

[0081] When an elemental analysis is performed by energy dispersive X-ray analysis (EDX) on a cross section passing through the center (or center of gravity) of the carbon-containing member, the second metal and carbon are detected in the cross section. Since the substrate (second electrode) does not usually contain the second metal, the detection of the second metal and carbon can be safely taken as indicating the presence of the second metal carbide.

[0082] [Method of producing hydrocarbons] The present disclosure includes a method for producing hydrocarbons from a second metal carbide. That is, the method for producing hydrocarbons according to the present disclosure includes the above-mentioned electrode preparation step, electrolysis step, and hydrolysis of the second metal carbide to obtain a gas containing hydrocarbons. Figure 2 is a flowchart showing the method for producing hydrocarbons according to the present disclosure.

[0083] (1) Electrode preparation process (S11, S12) A second electrode is produced in the same manner as in the electrode production steps (S11 and S12) in the above-mentioned method for producing metal carbide.

[0084] (2) Electrolysis process (S2) A voltage is applied to the second molten salt in the same manner as in the electrolysis step in the above-mentioned method for producing a metal carbide, thereby obtaining a composition containing the second metal carbide.

[0085] (3) Hydrolysis of metal carbides (S3) Next, the second metal carbide is brought into contact with water and hydrolyzed. This results in the production of a gas containing the target hydrocarbon. According to the present disclosure, the Faraday efficiency e for the production of hydrocarbons is improved. Hydrocarbons usually have low solubility in water. Therefore, the produced hydrocarbons are quickly discharged into the gas phase and collected.

[0086] The second metal carbide may be isolated from the metal carbide composition and then hydrolyzed. For example, the isolation is performed by a method of crushing the metal carbide composition and utilizing the difference in specific gravity. Alternatively, the metal carbide composition may be hydrolyzed as it is. For example, an electrode on which the metal carbide composition has been precipitated (which may be the "carbon-containing member" according to the present disclosure) is brought into contact with water as it is.

[0087] Examples of the obtained hydrocarbons include methane, ethane, ethylene, acetylene (C2H2), methylacetylene, propane, propylene, butane, and butene. When an isolated first metal carbide is used or when the amount of by-products (particularly, elemental metals) contained in the composition is small, acetylene is obtained as the main component. The main component is a component that accounts for 50% by mass or more of the total mass of the gas recovered. Acetylene is an industrially important hydrocarbon.

[0088] The gas obtained may contain water vapor, hydrogen, nitrogen, and oxygen as by-products in addition to hydrocarbons. The amount of by-products is preferably 10% by mass or less, more preferably 1% by mass or less, of the gas recovered. The amount of by-products may be 0.0001% by mass or more, or may be 0.001% by mass or more, of the gas recovered. In one embodiment, the amount of by-products is 0.0001% by mass or more and 1% by mass or less of the gas recovered.

[0089] The resulting gas contains acetylene as a hydrocarbon, and may further contain at least one selected from the group consisting of ethylene, ethane, methane, methylacetylene, propylene, butene, and hydrogen.

[0090] The presence of hydrocarbons and by-products can be confirmed and their quantity determined, for example, by gas chromatography mass spectrometry (GC-MS analysis) of the recovered gas, Fourier transform infrared absorption spectrometry (FT-IR analysis) equipped with a gas cell, or ultraviolet-visible absorption spectrometry (UV-Vis analysis).

[0091] The amount of water to be brought into contact with the composition is appropriately set according to the mass of the composition. The amount of water is, for example, an amount equal to or more than the amount required for hydrolysis of the metal carbide and metal contained in the composition. In addition, it is desirable to use an amount of water that allows the entire composition to be immersed and that takes into consideration evaporation due to heat generated during hydrolysis.

[0092] Hydrolysis of the second metal carbide produces the hydroxide of the second metal along with hydrocarbons. For example, the hydrolysis of calcium carbide produces calcium hydroxide along with acetylene (Equation 10). (Formula 10) CaC2+2H2O → C2H2+Ca(OH)2

[0093] Second embodiment This embodiment differs from the first embodiment in that the electrolytic bath used in the electrode preparation step and the electrolysis step is different. This difference will be described below. In this embodiment, the other configurations of the method for producing metal carbide are the same as those in the first embodiment, so their description will be omitted. In this embodiment, the method for producing hydrocarbons and the configuration of the carbon-containing member are the same as those in the first embodiment, so their description will be omitted.

[0094] In this embodiment, a second molten salt prepared separately from the first molten salt used in the electrode preparation step is used in the electrolysis step. The first molten salt used in the electrode preparation step may contain carbonate ions, which were a carbon source. In this embodiment, a second molten salt that is substantially free of carbonate ions can be prepared, thereby suppressing side reactions and further improving the yield and faradaic efficiency of the second metal carbide.

[0095] Third embodiment This embodiment differs from the first embodiment in the material of the first electrode. This difference will be described below. In this embodiment, other configurations of the method for producing metal carbide are the same as those of the first embodiment, so their description will be omitted. In this embodiment, the method for producing hydrocarbons and the configuration of the carbon-containing member are the same as those of the first embodiment, so their description will be omitted.

[0096] In this embodiment, an Fe plate is used as the first electrode. In this case, a carbon-containing member can be formed that includes a substrate, a metal carbide layer that covers at least a part of the substrate and contains at least one carbide of a second metal selected from the group consisting of alkali metals and alkaline earth metals, and a carbon layer that covers at least a part of the metal carbide layer, contains carbon, and is substantially free of the second metal carbide. Such a carbon-containing member can suppress decomposition of carbide even when stored in a humid atmosphere. The presence or absence of the second metal carbide can be confirmed, for example, by Raman spectroscopy.

[0097] "Substantially free of second metal carbide" allows the presence of the second metal carbide to an extent that it does not contribute to the generation of hydrocarbons. The carbon layer may contain, for example, about 10,000 ppm or less of the second metal carbide. The concentration of the second metal carbide in the carbon layer may be 1000 ppm or less, 500 ppm or less, or 0 ppm.

[0098] Although the embodiments of the present disclosure have been described in detail above, the present disclosure is not limited to these, and design changes are possible without departing from the gist of the present disclosure.

[0099] In the above embodiment, carbon dioxide is used as the carbonate ion source, but the carbonate ion source is not limited to this. The carbonate ion source may be any metal carbonate. When a carbonate of a first metal is used, a first metal ion and a carbonate ion are generated by ionization. The carbonate of the first metal can be synthesized, for example, by reacting a hydroxide of the first metal with carbon dioxide.

[0100] In the above embodiment, an electrode made of SUS304 or Fe is used as the first electrode (cathode), but is not limited thereto. The first electrode may contain other metal materials and may be formed of a carbon material. The first electrode may also contain carbon materials such as glassy carbon, natural graphite, isotropic graphite, pyrolytic graphite, plastic formed carbon, and conductive diamond, and may be formed of a carbon material.

[0101] In the first embodiment, the carbon-containing member obtained includes a substrate and a metal carbide composition containing a carbide of a second metal supported on the substrate, but is not limited thereto. The carbon-containing member obtained by the method shown in the first embodiment may include a substrate, a metal carbide layer, and a carbon layer.

[0102] In the third embodiment, the carbon-containing member obtained includes, but is not limited to, a substrate, a metal carbide layer, and a carbon layer. The carbon-containing member obtained by the method shown in the third embodiment may include a substrate and a metal carbide composition containing a carbide of a second metal supported on the substrate. EXAMPLES

[0103] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited thereto.

[0104] [Example 1-1] (1) Electrode fabrication process 3.0 mol% CaO was mixed with the eutectic composition of LiCl, KCl, and CaCl2 (LiCl / KCl / CaCl2=52.3 mol% / 11.6 mol% / 36.1 mol%) (i.e., LiCl / KCl / CaCl2 / CaO=50.8 mol% / 11.3 mol% / 35.0 mol% / 2.9 mol%) and vacuum dried at 200°C and 100 Pa or less for 24 hours or more. Each of these mixed salts was placed in a quartz container, set in an electric furnace, and heated to 450°C. In this way, a molten salt of LiCl-KCl-CaCl2-CaO was obtained.

[0105] Next, a working electrode (1.0 cm x 1.0 cm, SUS304), a counter electrode (platinum coil), and a reference electrode (Ag + A lid (100 mL / Ag) was attached to the container and the container was sealed with the lid. CO2 was blown into the molten salt in the container at 450°C for more than 30 minutes at a flow rate of 100 mL / min. Next, a voltage was applied for 30 minutes using a potentio-galvanostat while maintaining the potential of the working electrode relative to the reference electrode at 0.9 V. It was confirmed that a precipitate had formed on the working electrode. All experimental operations were performed in a glove box maintained in a high-purity argon atmosphere.

[0106] (2) Electrolysis process Next, electrolysis was performed using the same electrolytic bath and electrodes. Specifically, a voltage was applied for 30 minutes using a potentio-galvanostat while maintaining the potential of the working electrode relative to the reference electrode at 0.3 V. It was confirmed that a deposit was formed on the working electrode. All experimental operations were performed in a glove box maintained in a high-purity argon atmosphere. The potential of the working electrode was maintained at 0.3 V relative to the reference electrode (Ag + The potential between the cathode and the Li-Ca alloy was measured and calibrated based on the Li-Ca alloy deposition potential.

[0107] (3) Hydrocarbon production The precipitate was placed in a sealed test tube. Pure water was added to the test tube in small amounts at room temperature (23°C) to hydrolyze the precipitate. The total amount of water added was 2.5 ml. After confirming that bubbles were being generated in the test tube, the test tube was left to stand until the bubbles were no longer observed. Next, 100 μl (microliters) of gas was collected from the test tube using a gas-tight syringe.

[0108] Using a gas chromatograph (GC), GC-MS analysis of the resulting gas confirmed that C2H2 was produced as the main component. It was also confirmed that methane, ethane, and hydrogen were by-produced. Other components included water, carbon dioxide, nitrogen, oxygen, and argon. The amount of each component produced was also confirmed. The mass ratio of C2H2 in the recovered gas was well above 50 mass%.

[0109] The Faraday efficiency for C2H2 gas generation through the electrode preparation process and the electrolysis process was calculated to be about 2.2%. Since C2H2 gas was generated, it can be understood that the precipitate contains CaC2 as the main component. The higher the Faraday efficiency for hydrocarbon gas generation, the higher the Faraday efficiency for metal carbide generation.

[0110] [Example 1-2] Electrolysis and hydrolysis were carried out in the same manner as in Example 1-1, except that the potential of the working electrode relative to the reference electrode was maintained at 0.6 V in the electrode preparation step and at 0.1 V in the electrolysis step.

[0111] It was confirmed that a deposit was formed on the working electrode. The Faraday efficiency of C2H2 gas generation throughout the electrode preparation process and the electrolysis process was calculated to be approximately 9.1%. Since C2H2 gas was generated, it can be understood that the deposit deposited on the working electrode during the electrolysis process contains CaC2 as the main component.

[0112] [Table 1]

[0113] [Example 2-1] The potential of the working electrode relative to the reference electrode was maintained at 0.3 V in the electrode preparation process, and at 0.1 V in the electrolysis process. In the electrolysis process, the electrode was not changed, and a separately prepared electrolytic bath was used. Other than these, electrolysis and hydrolysis were performed in the same manner as in Example 1-1. The electrolytic bath used in the electrolysis process was prepared in the same manner as in Example 1-1.

[0114] It was confirmed that a deposit was formed on the working electrode. The Faraday efficiency of C2H2 gas generation throughout the electrode preparation process and the electrolysis process was calculated to be approximately 21.5%. Since C2H2 gas was generated, it can be understood that the deposit deposited on the working electrode during the electrolysis process contains CaC2 as the main component.

[0115] [Example 2-2] Electrolysis and hydrolysis were performed in the same manner as in Example 2-1, except that the potential of the working electrode relative to the reference electrode was maintained at 0.1 V in the electrode preparation step and was maintained at 0.1 V in the electrolysis step.

[0116] It was confirmed that a deposit was formed on the working electrode. The Faraday efficiency of C2H2 gas generation throughout the electrode preparation process and the electrolysis process was calculated to be approximately 34.6%. Since C2H2 gas was generated, it can be understood that the deposit deposited on the working electrode during the electrolysis process contains CaC2 as the main component.

[0117] [Table 2]

[0118] [Example 3-1] The potential of the working electrode relative to the reference electrode was maintained at 0.3 V in the electrode preparation step and the electrolysis step. The electrolysis step was carried out in a CO2 atmosphere. Other than these, electrolysis and hydrolysis were carried out in the same manner as in Example 1-1.

[0119] It was confirmed that a deposit was formed on the working electrode. The Faraday efficiency of C2H2 gas generation throughout the electrode preparation process and the electrolysis process was calculated to be approximately 8.4%. Since C2H2 gas was generated, it can be understood that the deposit deposited on the working electrode during the electrolysis process contains CaC2 as the main component.

[0120] [Example 3-2] Electrolysis and hydrolysis were carried out in the same manner as in Example 3-1, except that the potential of the working electrode relative to the reference electrode was maintained at 0.1 V in the electrode preparation step and the electrolysis step.

[0121] It was confirmed that a deposit was formed on the working electrode. Regarding the generation of C2H2 gas, the Faraday efficiency throughout the electrode preparation process and the electrolysis process was calculated to be approximately 10.3%. Since C2H2 gas was generated, it can be understood that the deposit deposited on the working electrode during the electrolysis process contains CaC2 as the main component.

[0122] [Table 3]

[0123] [Example 4-1] The potential of the working electrode relative to the reference electrode was maintained at 0.3 V in the electrode preparation step, and at 0.1 V in the electrolysis step. In addition, electrolysis and hydrolysis were performed in the same manner as in Example 3-1, except that after the electrode preparation step, the electrode was temporarily removed from the electrolysis bath, and after 30 minutes, it was placed in the same bath again to perform the electrolysis step.

[0124] It was confirmed that a deposit was formed on the working electrode. The Faraday efficiency of C2H2 gas generation throughout the electrode preparation process and the electrolysis process was calculated to be approximately 4.5%. Since C2H2 gas was generated, it can be understood that the deposit deposited on the working electrode during the electrolysis process contains CaC2 as the main component.

[0125] [Example 4-2] Electrolysis and hydrolysis were carried out in the same manner as in Example 4-1, except that the potential of the working electrode relative to the reference electrode was maintained at 0.1 V in the electrode preparation step and the electrolysis step.

[0126] It was confirmed that a deposit was formed on the working electrode. The Faraday efficiency for C2H2 gas generation throughout the electrode preparation process and the electrolysis process was calculated to be approximately 2.8%. Since C2H2 gas was generated, it can be understood that the deposit deposited on the working electrode during the electrolysis process contains CaC2 as the main component.

[0127] [Table 4]

[0128] [Examples 5-1 to 5-49] Except for changing the composition of the molten salt, the material of the cathode, and the electrolysis conditions as shown in Tables 5 and 6, the electrode preparation step and hydrolysis were performed in the same manner as in Example 1-1.

[0129] In Examples 5-23 to 5-49, the potential of the working electrode was measured using a reference electrode (Ag + The potential between the electrode (Ag) and the cathode was measured and calibrated based on the Na-K-Ca alloy deposition potential. In Examples 5-31 to 5-49, 7.0 mol % of CaC2 was added to the molten salt in advance.

[0130] It was confirmed that a precipitate was deposited on the working electrode. Hydrolysis was performed on the precipitate deposited on the working electrode (corresponding to the second electrode) prepared in the electrode preparation process. The Faraday efficiency in the table is a value related to the generation of C2H2 gas by the precipitate deposited in the electrode preparation process. The larger this Faraday efficiency, the greater the amount of CaC2 precipitated in the electrode preparation process. It can be said that if the Faraday efficiency related to the generation of C2H2 gas in the electrode preparation process is large, the Faraday efficiency related to the generation of C2H2 gas through the electrode preparation process and the electrolysis process will also be large. Since C2H2 gas is generated, it can be understood that the precipitate deposited on the working electrode by the electrolysis process contains CaC2 as the main component.

[0131] [Table 5]

[0132] [Table 6]

[0133] [Example 6-1] Electrolysis and hydrolysis were carried out in the same manner as in Example 5-45, except that the accumulated amount of electricity was set to 2000C.

[0134] XRD analysis confirmed that the deposit formed on the working electrode during the electrode preparation process contained polycrystalline C as the main component and CaC2 as a by-product.

[0135] FIG. 3A is a photograph showing the appearance of the working electrode before the electrolysis process in Example 6-1. FIG. 3B is a photograph showing the appearance of the working electrode after the electrolysis process in Example 6-1. A black precipitate can be confirmed on the surface of the working electrode, and it can be seen that it has swelled to more than double its size. FIG. 3C is a cross-sectional photograph of the precipitate precipitated on the working electrode after the electrolysis process in Example 6-1. From FIG. 3C, it was confirmed that the precipitate has a layer structure. Furthermore, as a result of Raman spectroscopy analysis, it was confirmed that gas was generated only from the inner layer when water was poured on the cross section, and that ignition was confirmed when fire was brought close to the precipitate, so that it was confirmed that the inner layer was a metal carbide layer mainly composed of calcium carbide, and the outer layer was a carbon layer that contained carbon but did not substantially contain calcium carbide.

[0136] [Example 6-2] Electrolysis and hydrolysis were carried out in the same manner as in Example 6-1, except that the accumulated amount of electricity was set to 500C. FIG. 4A is a photograph showing the appearance of the working electrode after the electrolysis process of Example 6-2. FIG. 4B is an optical microscope photograph of a cross section of the precipitate deposited on the working electrode after the electrolysis process of Example 6-2, observed using a micro-Raman spectroscopic analyzer. FIG. 4B also shows a schematic cross-sectional view of the working electrode after the electrolysis process. The optical microscope photograph corresponds to the part surrounded by a square in the schematic cross-sectional view. In FIG. 4B, point A indicates the black part outside the precipitate, point B indicates the gray part inside the precipitate, and point C indicates the Fe substrate of the working electrode. It was confirmed from FIG. 4B that the precipitate has a layer structure.

[0137] 4C is a graph showing the results of Raman spectroscopy performed at points A to C. From this result, it was confirmed that the inside of the precipitate (point B) was a metal carbide layer mainly composed of calcium carbide, and the outside of the precipitate (point A) was a carbon layer that contained carbon but was substantially free of calcium carbide.

[0138] [Example 7-1] (1) Electrode fabrication process 3.0 mol% CaO was mixed with NaCl, KCl, and CaCl2 (NaCl / KCl / CaCl2=33.4 mol% / 11.6 mol% / 55.0 mol%) (i.e., NaCl / KCl / CaCl2 / CaO=32.4 mol% / 11.3 mol% / 53.4 mol% / 2.9 mol%) and vacuum dried at 200°C and 100 Pa or less for 24 hours or more. Each of these mixed salts was placed in a Ni container, set in an electric furnace, and heated to 550°C. In this way, a molten salt of NaCl-KCl-CaCl2-CaO was obtained.

[0139] Next, a working electrode (1.0 cm x 1.0 cm, Fe), a counter electrode (platinum) and a reference electrode (Ag + A lid (Ag / Ag) was attached to the container and the container was sealed. CO2 was blown into the molten salt in the container at 550°C for more than 60 minutes at a flow rate of 100 mL / min. While maintaining the CO2 atmosphere in the gas phase of the container, a voltage was applied for 30 minutes while maintaining the potential of the working electrode with respect to the reference electrode at 0.3 V using a potentio-galvanostat. The potential of the working electrode was measured by the voltage of the reference electrode (Ag + The potential between the electrode and the cathode was measured and calibrated using the Na-K-Ca alloy deposition potential as the standard.

[0140] It was confirmed that a deposit was formed on the working electrode. All experimental operations were carried out in a glove box maintained in a high-purity argon atmosphere.

[0141] (2) Electrolysis process Next, electrolysis was performed using a separately prepared electrolytic bath having the same composition as above and the electrode obtained in the above electrode preparation process. Specifically, a voltage was applied for 30 minutes using a potentio-galvanostat while maintaining the potential of the working electrode relative to the reference electrode at 0.3 V. It was confirmed that a deposit was deposited on the working electrode. All experimental operations, including the gas phase in the container, were performed in a glove box that maintained a high-purity argon atmosphere.

[0142] (3) Hydrocarbon production The precipitate was placed in a sealed test tube. Pure water was added to this test tube in small amounts at room temperature (23°C) to hydrolyze the precipitate. The total amount of water added was 2.5 ml. After confirming that bubbling had occurred in the test tube, the test tube was left to stand until bubbling was no longer observed. Next, 100 μl (microliters) of gas was collected from the test tube using a gas-tight syringe. The volume of the generated gas was measured by the water displacement method.

[0143] Using a gas chromatograph (GC), GC-MS analysis of the obtained gas confirmed that C2H2 was produced as the main component. Since C2H2 gas was produced, it can be understood that the deposit deposited on the working electrode by the electrolysis process contains CaC2 as the main component. Furthermore, it was confirmed that methane, ethane, and hydrogen were by-produced. In addition, it contained water, carbon dioxide, nitrogen, oxygen, and argon. The amount of each component produced was also confirmed. The mass ratio of C2H2 in the recovered gas was well above 50 mass%.

[0144] Regarding the generation of C2H2 gas, the Faraday efficiency throughout the electrode preparation process and the electrolysis process was calculated to be about 42.8%. Since C2H2 gas was generated, it can be understood that the precipitate contains CaC2 as the main component.

[0145] [Examples 7-2 to 7-6] Electrolysis and hydrolysis were carried out in the same manner as in Example 7-1, except that the electrolysis conditions were changed as shown in Table 7.

[0146] It was confirmed that a deposit was formed on the working electrode. Regarding the generation of C2H2 gas, the Faraday efficiency throughout the electrode preparation process and the electrolysis process is shown in Table 7. Since C2H2 gas is generated, it can be understood that the deposit deposited on the working electrode by the electrolysis process contains CaC2 as the main component.

[0147] [Examples 8-1 to 8-6] The electrolysis conditions were changed as shown in Table 7, and electrolysis and hydrolysis were performed in the same manner as in Example 7-1, except that CaC2 was added to the molten salt in an amount of 1.0 mol% relative to the molten salt during the electrolysis process.

[0148] It was confirmed that a deposit was formed on the working electrode. The Faraday efficiency for C2H2 gas generation throughout the electrode preparation process and the electrolysis process is shown in Table 7. Since C2H2 gas was generated, it can be understood that the deposit formed on the working electrode during the electrolysis process contains CaC2 as the main component.

[0149] [Examples 9-1 to 9-6] The electrolysis conditions were changed as shown in Table 7, and electrolysis and hydrolysis were performed in the same manner as in Example 7-1, except that CaC2 was added to the molten salt in an amount of 7.0 mol% relative to the molten salt during the electrolysis process.

[0150] It was confirmed that a deposit was formed on the working electrode. The Faraday efficiency for C2H2 gas generation throughout the electrode preparation process and the electrolysis process is shown in Table 7. Since C2H2 gas was generated, it can be understood that the deposit formed on the working electrode during the electrolysis process contains CaC2 as the main component.

[0151] [Examples 10-1 to 10-3] After the electrode preparation process, the electrodes were removed from the bath, and after 30 minutes, they were placed back in the same bath to carry out the electrolysis process. Except for this, electrolysis and hydrolysis were carried out in the same manner as in Examples 7-1, 7-3, and 7-5. The electrolysis conditions were as shown in Table 7, and the electrolysis process was carried out in a CO2 atmosphere.

[0152] It was confirmed that a deposit was formed on the working electrode. The Faraday efficiency for C2H2 gas generation throughout the electrode preparation process and the electrolysis process is shown in Table 7. Although the amount of C2H2 gas generated was not measured, the Faraday efficiency was 0.1% or more in both cases, so it can be understood that the deposit formed on the working electrode during the electrolysis process contains CaC2 as the main component.

[0153] [Table 7]

[0154] The faradaic efficiency e for C2H2 production was calculated as follows: First, the volume ratio of C2H2 contained in the collected gas was calculated from the total area of ​​the peaks obtained from the GC-MS analysis and the calibration curve. Next, the volume of C2H2 generated was calculated from the volume of the gas phase in the collection vessel and the calculated volume ratio of C2H2 in the gas. Finally, the Faraday efficiency e (%) was calculated using the following formula, assuming that the generated C2H2 was in standard conditions (0°C, 101 kPa).

number

[0155] As can be seen from Tables 1 and 4, the desired second metal carbide was obtained with high faradaic efficiency by any of the electrolysis methods. In particular, the series of Examples 2, 3, and 4 had higher faradaic efficiency. This indicates that carbon was sufficiently precipitated because the potential in the electrode preparation step was base. In particular, the series of Example 2 had a very high faradaic efficiency. This is believed to be because the electrolysis step was performed in an Ar atmosphere and the electrolytic bath was changed between the electrode preparation step and the electrolysis step, resulting in a low carbonate ion concentration in the second molten salt.

[0156] As can be seen from Tables 5 and 6, especially when SUS304 was used as the working electrode, hydrocarbons could be obtained from the precipitate with high Faraday efficiency. This indicates that the amount of CaC2 precipitated in the electrode preparation process was large. It can be understood that a large amount of CaC2 also means a large amount of carbon precipitated.

[0157] As can be seen from Table 7, by using the NaCl-KCl-CaCl2 molten salt, it was possible to obtain hydrocarbons from the precipitate with higher faradaic efficiency. 2-It is desirable from the viewpoint of faradaic efficiency that the electrolysis process is carried out in an Ar atmosphere and that the electrolysis process is carried out in an Ar atmosphere. It is desirable from the viewpoint of faradaic efficiency that CaC2 is added to the molten salt as an additive. This is considered to be because the CaC2 formed on the working electrode is prevented from dissolving in the molten salt. [Industrial Applicability]

[0158] The production method of the present disclosure is useful in various fields because the reaction proceeds quickly at a relatively low temperature and metal carbide can be efficiently obtained.

Claims

1. preparing a first molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions and carbonate ions; an electrode preparation step including applying a voltage to the first molten salt to cause a carbon-containing precipitate to precipitate on a first electrode, thereby obtaining a second electrode; applying a voltage to a second molten salt containing at least one type of second metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions, using the second electrode, to obtain a carbide composition containing a carbide of the second metal.

2. The method for producing metal carbide according to claim 1 , wherein the first electrode contains at least one selected from the group consisting of transition metals and alloys containing transition metals.

3. The method of claim 1 , wherein the first electrode comprises an alloy including iron.

4. The method for producing metal carbide according to claim 1 , wherein the first electrode comprises SUS304.

5. The method for producing metal carbide according to claim 1 , wherein the second molten salt is substantially free of carbonate ions.

6. 2. The method for producing metal carbide according to claim 1, wherein the first molten salt used in the electrode preparation step is used as the second molten salt in the electrolysis step.

7. 2. The method for producing metal carbide according to claim 1, wherein the second molten salt contains, as an anion, at least one selected from the group consisting of a halide ion and an oxide ion.

8. The method for producing metal carbide according to claim 1 , wherein the first metal ion and the second metal ion are the same.

9. 2. The method for producing metal carbide according to claim 1, wherein the carbide composition further comprises at least one selected from the group consisting of carbon, an elemental form, a halide, a carbonate, an oxide, a hydride, and a peroxide of the second metal, and an elemental form, a halide, a carbonate, an oxide, and a carbide of the first metal.

10. 2. The method for producing metal carbide according to claim 1, wherein the second molten salt contains, as the second metal ions, at least one selected from the group consisting of sodium ions, lithium ions, and potassium ions, and calcium ions.

11. preparing a first molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions and carbonate ions derived from carbon dioxide; and an electrode preparation step including applying a voltage to the first molten salt to cause a precipitate containing carbon to be deposited on a first electrode to obtain a second electrode; an electrolysis step including applying a voltage to a second molten salt containing at least one second metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions, using the second electrode, to obtain a carbide composition containing a carbide of the second metal; and a gas generating step of hydrolyzing the carbide of the second metal to obtain a gas containing a hydrocarbon.

12. The method for producing hydrocarbons according to claim 11, wherein the hydrocarbon is acetylene.

13. 13. The method for producing hydrocarbons according to claim 11 or 12, wherein the gas contains acetylene as the hydrocarbon, and further contains at least one selected from the group consisting of ethylene, ethane, methane, methylacetylene, propylene, butene, and hydrogen.

14. A substrate; a metal carbide layer covering at least a portion of the substrate, the metal carbide layer including at least one second metal carbide selected from the group consisting of alkali metals and alkaline earth metals; a carbon layer covering at least a portion of the metal carbide layer, the carbon layer comprising carbon and being substantially free of the second metal carbide.

Citation Information

Patent Citations

  • Method for preparing calcium carbide through electrolysis

    CN116288415A

  • Production of calcium carbide by blast furnace process

    JP1986178412A

  • Production of high-purity acetylene gas

    JP1990256626A

  • Manufacturing method of briquette and manufacturing method of calcium carbide

    JP2018035328A

  • Electrolytic preparation of calcium carbide

    US2952591A