Magnetic heat exchange material, heat exchange device, and magnetic heat exchange apparatus using the same
A NaZn13-based magnetic heat exchange material with controlled composition and hydrogenation addresses cracking and powder issues, ensuring efficient and durable refrigeration performance.
Patent Information
- Application Number
- JP2021002927
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-12
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2041-01-12
AI Technical Summary
Conventional magnetic refrigeration materials face issues such as cracking and powder generation due to hydrogenation, leading to increased pressure loss and reduced refrigeration capacity in heat exchange devices.
A magnetic heat exchange material with a NaZn13 crystal structure, represented by formulas La1-aRaNi1-b-cSi bTcHe, where R is Sm or Y, T is V, Cr, Mn, Ni, or Cu, and specific atomic ratios, combined with hydrogen, providing high magnetic refrigeration effects and durability.
The material exhibits high magnetic heat exchange characteristics, mechanical strength, and corrosion resistance, enabling efficient and durable heat exchange devices with reduced pressure loss.
Smart Images

Figure 0007583439000004 
Figure 0007583439000005 
Figure 0007583439000006
Abstract
Description
[Technical Field]
[0001] The present invention relates to a magnetic heat exchange material that has a large magnetocaloric effect and is usable in a room temperature range suitable for practical use, a heat exchange device equipped with the material, and a magnetic heat exchange apparatus using the material. [Background technology]
[0002] Most room-temperature refrigeration technologies closely related to daily life, such as refrigerators, freezers, and room heaters and coolers, use the gas compression-expansion cycle. However, refrigeration technologies based on the gas compression-expansion cycle have become a major issue due to the environmental damage caused by the emission of specific fluorocarbon gases, and there are concerns about the environmental impact of alternative fluorocarbon gases. Against this background, efforts are being made to use natural refrigerants (such as CO2 and ammonia) and isobutane, which pose less environmental risk. In other words, there is a need for practical application of safe, clean, and highly efficient refrigeration technologies that do not involve the environmental damage caused by the disposal of working gases.
[0003] Expectations are rising for magnetic refrigeration as one such environmentally friendly and highly efficient refrigeration technology, and research and development of magnetic refrigeration technology targeting room temperature is progressing. Magnetic refrigeration technology is based on the magnetocaloric effect of Fe. The magnetocaloric effect is a phenomenon in which the temperature of a magnetic material changes when an external magnetic field is applied to the magnetic material in an adiabatic state. Gd2(SO4)3·8H2O and Gd3Ga5O, which have the magnetocaloric effect, 12 Refrigeration systems using paramagnetic salts and paramagnetic compounds, such as those listed above, have been developed. However, these systems are mainly applicable to cryogenic temperatures below 20 K, and require a magnetic field of around 10 T using a superconducting magnet.
[0004] Since then, research has been actively conducted on utilizing the magnetic transition between the paramagnetic and ferromagnetic states in ferromagnetic materials in order to realize magnetic refrigeration in the high-temperature range. As a result, magnetic materials such as lanthanide rare-earth elements such as Pr, Nd, Dy, Er, Tm, and Gd, alloys of two or more rare-earth elements such as Gd-Y and Gd-Dy, and rare-earth intermetallic compounds such as RAl2 and RNi2 (R: rare-earth element), and GdPd have been discovered.
[0005] In 1982, Barclay in the United States proposed the AMR ("Active Magnetic Regenerative Refrigeration") method, a magnetic refrigeration system intended for room temperature ranges, which uses magnetic refrigeration materials to simultaneously perform heat storage effects in addition to magnetocaloric effects (Patent Document 1). This AMR method actively utilizes lattice entropy, which has traditionally been considered an obstacle to magnetic refrigeration in the room temperature range.
[0006] AMR magnetic refrigeration is carried out in the following steps: (1) A magnetic field is applied to the magnetic refrigeration material. (2) The heat generated by (1) is transported from one end to the other by a refrigerant. (3) Remove the magnetic field from the magnetic refrigeration material. (4) The cold generated by (3) is transported to the end opposite to the end where the heat was transported by (2). By repeating the thermal cycles (1) to (4), the heat generated in the magnetic refrigeration material in the heat exchange device (inside the magnetic refrigeration chamber) is transported in one direction via the heat transport medium, creating a temperature gradient in the direction of the heat flow, and a large temperature difference occurs at both ends, resulting in refrigeration.
[0007] Subsequently, it was reported that continuous operation of the magnetic refrigeration cycle was achieved by using Gd (gadolinium) as a magnetic refrigeration material in the room temperature range and applying a high magnetic field of up to 5 T using a superconducting magnet to a magnetic refrigerator using the above-mentioned AMR method.
[0008] On the other hand, materials other than Gd for room temperature magnetic refrigeration have been developed, such as (Hf,Ta)Fe2, (Ti,Sc)Fe2, (Nb,Mo)Fe2, and La(Fe,Si). 13 Magnetic materials such as these systems exhibit large magnetic entropy changes, contain inexpensive Fe as their main constituent element, and are characterized by small hysteresis during heating and cooling of magnetic phase transitions, and their development has been progressing.
[0009] Magnetic refrigeration devices using such magnetic refrigeration materials generate low temperatures by utilizing the magnetocaloric effect of the materials. For example, in the case of ferromagnetic materials, applying an external magnetic field near the ferromagnetic phase transition temperature (Curie temperature; Tc) causes the electron magnetic spin to transition from a paramagnetic state to a ferromagnetic state, resulting in a change in entropy, which is utilized to achieve low temperatures.
[0010] Among these magnetic materials, NaZn is particularly well known, which is formed by substituting part of Fe with Si. 13 La(Fe) 1-x Si x ) 13 It is known that shows a particularly large magnetic entropy change. In materials with this crystal structure, the site corresponding to Zn is mainly occupied by Fe, and the site corresponding to Na is mainly occupied by rare earth elements such as La.
[0011] In order to apply magnetic materials to magnetic refrigeration such as AMR, they must be processed into small pieces such as spherical particles for practical heat exchange. For example, Patent Document 2 discloses a spherical La(Fe 1-x Si x ) 13 The publication discloses a technique for performing hydrogenation treatment to increase the Curie temperature of the alloy. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] U.S. Patent No. 4,332,135 [Patent Document 2] Japanese Patent Application Laid-Open No. 2003-96547 Summary of the Invention [Problem to be solved by the invention]
[0013] However, the above-mentioned conventional techniques have the following problems. In the technique disclosed in Patent Document 2, during hydrogenation, the lattice expands due to hydrogen entering the interstitial spaces, and in some cases, cracks may occur. Therefore, in such a state, La(Fe 1-x Si x ) 13 When magnetic material particles are filled into the heat exchange device of a magnetic refrigeration device and heat exchange occurs between the particles and a refrigerant to achieve refrigeration, the magnetic material particles may vibrate in accordance with the frequency of the refrigerant flow and the application and removal of a magnetic field during heat exchange.
[0014] If this state continues for a relatively long time, the vibrations described above will cause collisions and friction between magnetic materials, resulting in the destruction of the magnetic materials and the generation of fine particles. The generation of fine particles increases the pressure loss of the refrigerant, which reduces the efficiency of heat exchange and causes a decrease in refrigeration capacity.
[0015] In view of the above problems, the present invention aims to provide a magnetic heat exchange material that combines magnetic heat exchange properties, including a high magnetic refrigeration effect, with durability, i.e., crack resistance and corrosion resistance, as well as a heat exchange device equipped with the magnetic heat exchange material and a magnetic heat exchanger using the same. [Means for solving the problem]
[0016] In order to achieve the above objective, we conducted extensive research into magnetic materials used in magnetic heat exchange materials that combine magnetic heat exchange properties, including a high magnetic refrigeration effect, with durability. As a result, we discovered that materials containing at least rare earth elements, iron, silicon, and hydrogen can achieve high magnetic heat exchange properties and durability, leading to the development of the present invention.
[0017] That is, the magnetic heat exchange material according to the present invention, which was developed to solve the above problems and achieve the above objects, has a main phase of NaZn 13 The magnetic heat exchange material has a crystalline structure represented by the following general formula (1): La 1-a R a (Fe 1-b-c Si b T c ) e H f ···(1) Here, in the above formula (1), R: at least one selected from Sm and Y; T: at least one selected from V, Cr, Mn, Ni and Cu; Also, the subscripts a, b, c, e and f 0 <a≦0.30、 0.09≦b≦0.14, 0 <c≦0.04、 12.5≦e≦13.5, 1.3≦f≦2.3 Meet the conditions.
[0018] The magnetic heat exchange material of the present invention, which was developed to solve the above problems and achieve the above objects, has a main phase of NaZn 13 The magnetic heat exchange material has a crystalline structure represented by the following general formula (2): La 1-a R a (Fe 1-b-c-d Si b T c Co d ) e H f ···(2) Here, in the above formula (2), R: at least one selected from Sm and Y; T: at least one selected from V, Cr, Mn, Ni and Cu; Also, the subscripts a, b, c, d, e and f 0 <a≦0.30、 0.09≦b≦0.14, 0 <c≦0.05、 0 <d≦0.03、 12.5≦e≦13.5, 1.3≦f≦2.3 Meet the conditions.
[0019] The magnetic heat exchange material according to the present invention is (a) In X-ray diffraction measurements using Cu-Kα radiation as an X-ray source, NaZn 13 La(Fe) 1-x Si x ) 13 the ratio of the diffraction intensity of the (110) plane of the Fe phase to the diffraction intensity of the (422) plane of the Fe phase is 7% or less; (b) In X-ray diffraction measurements using Cu-Kα radiation as an X-ray source, NaZn 13 La(Fe) 1-x Si x ) 13 the ratio of the diffraction intensity of the (101) plane of the LaFeSi phase having a CeFeSi type crystal structure to the diffraction intensity of the (422) plane of the LaFeSi phase is 7% or less; (c) the magnetic heat exchange material is a spherical particle having an aspect ratio of 2 or less; (d) the average particle size of the magnetic heat exchange material is 0.05 mm or more and 1 mm or less; This is thought to be a more preferable solution.
[0020] Furthermore, the heat exchange device of the present invention, which has been developed to solve the above problems and achieve the above objects, is characterized in that it is equipped with any of the magnetic heat exchange materials described above.
[0021] The magnetic heat exchanger according to the present invention, which has been developed to solve the above problems and achieve the above objects, is characterized by comprising the above heat exchange device. [Effects of the Invention]
[0022] As described above, the present invention provides a magnetic heat exchange material that exhibits high magnetic heat exchange properties, as well as high mechanical strength and practical corrosion resistance. Furthermore, by using the magnetic heat exchange material of the present invention, it is possible to provide a heat exchange device that is suitable for practical use and has high heat exchange efficiency, and a highly efficient magnetic heat exchanger that uses the same. [Brief explanation of the drawings]
[0023] [Figure 1] 1 is a cross-sectional view showing an embodiment of a magnetic heat exchange device using a magnetic heat exchange material according to the present invention. [Figure 2] 4 is a cross-sectional view showing an outline of the operation of the magnetic heat exchanger according to the embodiment. FIG. [Figure 3] FIG. 1 is a conceptual diagram showing another embodiment of a magnetic heat exchange device using a magnetic heat exchange material according to the present invention. [Figure 4] FIG. 10 is a detailed view of the magnetic heat exchanger according to the other embodiment. [Figure 5] 2 is a graph showing an example of the results of X-ray diffraction measurement of the magnetic heat exchange material according to the present invention. DETAILED DESCRIPTION OF THE INVENTION
[0024] Other features and advantages of the present invention will be described below based on the embodiments.
[0025] The magnetic heat exchange material of the present invention has a main phase of NaZn 13 The magnetic heat exchange material has a crystalline structure and is represented by the following general formula (1). La 1-a R a (Fe 1-b-c Si b T c ) e H f ···(1) Here, in the above formula (1), R: at least one selected from Sm and Y; T: at least one selected from V, Cr, Mn, Ni and Cu; Also, the subscripts a, b, c, e and f 0 <a≦0.30、 0.09≦b≦0.14, 0 <c≦0.04、 12.5≦e≦13.5, 1.3≦f≦2.3 Meet the conditions.
[0026] In addition, the magnetic heat exchange material of the present invention has a main phase of NaZn 13 The magnetic heat exchange material has a crystalline structure and is represented by the following general formula (2). La 1-a R a (Fe 1-b-c-d Si b T c Co d ) e H f ···(2) Here, in the above formula (2), R: at least one selected from Sm and Y; T: at least one selected from V, Cr, Mn, Ni and Cu; Also, the subscripts a, b, c, d, e and f 0 <a≦0.30、 0.09≦b≦0.14, 0 <c≦0.05、 0 <d≦0.03、 12.5≦e≦13.5, 1.3≦f≦2.3 Meet the conditions.
[0027] The reasons for limiting the component compositions of the magnetic heat exchange materials of the present invention represented by general formulas (1) and (2) will be explained below.
[0028] R: R is a rare earth element that substitutes for La, and is at least one element selected from Sm and Y. The atomic ratio a of R to the total of R and La is in the range of more than 0 and 0.30 or less. The magnetic heat exchange material used in the present invention is NaZn 13It has a type structure as the main phase and contains rare earth elements as elements at the Na site. The rare earth element is based on La, but by substituting a part of it with at least one element selected from Sm and Y, durability is improved. Therefore, it is effective in improving reliability when actually installed in a heat exchanger, for example, a refrigerator, and operated. The amount is such that at least a part of La is substituted with these elements, with the upper limit being 0.30. When the substitution ratio a exceeds 0.30, NaZn 13 Phases other than the crystalline structure, such as α-Fe phase and R-Fe phase, are likely to form, resulting in a reduced magnetocaloric effect. The ratio is preferably 0.25 or less. While rare earth elements such as Pr and Nd are not actively used, they may be included at the level of unavoidable impurities.
[0029] Si: Si replaces Fe and becomes NaZn 13 It is an essential element for the stable formation of the NaZn structure and also provides a large magnetocaloric effect. The atomic ratio b of Si substituting for Fe is in the range of 0.09 to 0.14. When the substitution ratio b is less than 0.09, NaZn 13 On the other hand, if the ratio exceeds 0.14, it becomes difficult to form the NaZn type structure and obtain a large magnetocaloric effect. 13 Although the type structure is maintained, the magnetocaloric effect becomes small and it becomes impractical. The preferable range is 0.10 or more and 0.13 or less. Note that a part of Si can be replaced with Al up to 1 / 2 in atomic ratio.
[0030] T: T is a transition metal element that is effective in substituting Fe to control the magnetic transition temperature, and is at least one element selected from V, Cr, Mn, Ni, and Cu. Depending on the element, it can also improve corrosion resistance. The atomic ratio c of T substituting Fe is in the range of more than 0 and not more than 0.04 in the case of formula (1) where Co is not used, and in the case of formula (2) where Co is used, it is in the range of more than 0 and not more than 0.05. If the substitution ratio c exceeds the upper limit, the magnetic transition temperature may become too low. Preferably, it is 0.03 or less.
[0031] Co: Co is used in formula (2) as a transition metal element to substitute for Fe and is effective in controlling the magnetic transition temperature, particularly in setting it to a high temperature. The atomic ratio d of Co substituting for Fe is in the range of more than 0 and not more than 0.03. If the upper limit is exceeded, the contribution of the second-order phase transition becomes large, the magnetocaloric effect begins to decrease, and the magnetic transition temperature may become too high. A preferable range is 0.005 or more and not more than 0.025. Furthermore, the presence of Co makes it relatively easy to introduce hydrogen, making it an effective element in this respect as well.
[0032] The atomic ratio e of rare earth elements to transition metal elements is 12.5 or more and 13.5 or less. 13 Below the lower limit, the structure is stable. 12 Structure, Th2Zn 17 On the other hand, if the upper limit is exceeded, the Fe phase formed before the heat treatment is difficult to disappear, and NaZn 13 Since it becomes difficult to achieve a single phase, the magnetocaloric effect decreases. The preferable range is 12.6 or more and 13.4 or less.
[0033] H: H (hydrogen) is an element that controls the magnetic transition temperature to be near room temperature and is effective in increasing the magnetocaloric effect. The atomic ratio f of H to the total rare earth elements is in the range of 1.3 to 2.3, resulting in an appropriate magnetic transition temperature. Preferably, it is in the range of 1.5 to 2.2.
[0034] The magnetic heat exchange material of this embodiment has little temperature hysteresis due to the magnetocaloric effect, so even when used as a material for configuring a heat exchange cycle in a magnetic heat exchange device, it can operate stably. In addition, since the main component is Fe, the manufacturing cost is significantly lower than that of conventional magnetic heat exchange materials, and it can be widely used.
[0035] Furthermore, the magnetic heat exchange material preferably has a spherical particle shape. Here, "spherical" refers not only to a perfect sphere but also to an approximately spherical shape such as an ellipse, or to shapes with irregularities on their surfaces. This shape prevents the generation of fine powder due to particle breakage, suppresses the increase in pressure loss of the heat exchange medium, and maintains heat exchange efficiency. Specifically, it is preferable that 80% by mass or more of the magnetic heat exchange material have an aspect ratio (ratio of major axis to minor axis) of 2 or less. This is because, in an experiment in which irregular-shaped particles with an aspect ratio of 2 or more were mixed with approximately spherical particles, when the amount of irregular-shaped particles mixed was 20% or more, fine powder was generated by long-term exposure to the heat exchange medium flow, increasing the pressure loss of the heat exchange medium.
[0036] To achieve high heat exchange capacity when using the above-mentioned magnetic heat exchange material in a magnetic heat exchange device such as the one described below, it is important to ensure sufficient heat exchange between the magnetic heat exchange material filled inside the heat exchange device and the heat exchange medium. To achieve this, it is preferable to increase the specific surface area of the magnetic heat exchange material. To increase the specific surface area of the magnetic heat exchange material, it is effective to granulate the magnetic heat exchange material and set the particle size small. On the other hand, if the particle size is too small, the pressure loss of the heat exchange medium increases. Furthermore, factors such as the viscosity (surface tension) of the heat exchange medium, the capacity and pressure loss of the pump installed in the magnetic heat exchange device, and the size of the heat exchange device also affect the particle size of the magnetic heat exchange material. Taking these points into consideration, the volume-average particle size (major axis) is preferably in the range of 0.05 mm to 1 mm, and more preferably in the range of 0.08 mm to 0.8 mm.
[0037] The magnetic heat exchange material of this embodiment can be obtained using commonly known methods. Specifically, it can be obtained by producing an alloy using an arc melting method, casting method, or the like, and then heat treating the alloy. Furthermore, by using an alloy production method with a fast cooling rate, such as roll quenching or atomization, the heat treatment time can be significantly shortened, and the material can also be made into a thin ribbon or spheroidized.
[0038] For example, the magnetic heat exchange material can be produced by the following method. First, the raw materials are blended in a predetermined ratio of each constituent element and then homogenized by melting. The type and blending ratio of the raw materials are determined taking into account the composition ratio (content of each element) of the desired magnetic heat exchange material.
[0039] Next, these materials are melted in a high-frequency induction furnace under an inert atmosphere and then cast into a master alloy. At this stage, the alloy contains a large amount of Fe phase, a small amount of LaFeSi phase, and La(Fe 1-x Si x ) 13 phase, which is then heat-treated at 1000-1300°C for 100-500 hours in an inert atmosphere to form La(Fe 1-x Si x ) 13 (NaZn 13 It is possible to create a nearly single phase (type crystal structure).
[0040] On the other hand, by controlling the cooling rate after melting, the time required to achieve the single phase can be shortened. Specifically, by cooling using a roll quenching method or an atomization method, the structure can be refined, and the time required for the subsequent heat treatment to achieve the single phase can be significantly shortened. For example, a nearly single phase can be achieved in about 5 to 24 hours at 1100 to 1300°C.
[0041] Before the heat treatment, the Fe phase was the most abundant constituent phase, and LaFeSi phase was also present. However, due to atomic diffusion during the heat treatment, the phase was mostly La(Fe 1-x Si x ) 13 The amount of the Fe phase and LaFeSi phase remaining was measured by X-ray diffraction using Cu-Kα radiation as an X-ray source. 13 La(Fe) 1-x Si x ) 13It is preferable that the ratio of the diffraction intensity of the (110) plane of the Fe phase to the diffraction intensity of the (422) plane of the LaFeSi phase is 7% or less, and that the ratio of the diffraction intensity of the (101) plane of the LaFeSi phase having a CeFeSi type crystal structure is 7% or less. If either of these exceeds the upper limit, the magnetocaloric effect decreases. The remainder is the main phase, NaZn 13 La(Fe 1-x Si x ) 13 phase, including other phases at unavoidable impurity levels that do not affect the magnetocaloric effect.
[0042] When a magnetic heat exchange material is placed in a heat exchange device and heat is exchanged using a liquid heat exchange medium, if the volume average particle size is 50 μm or less, pressure loss increases and heat exchange efficiency decreases. On the other hand, if the volume average particle size exceeds 1 mm, pressure loss decreases, but the surface area of the magnetic heat exchange material decreases, reducing the heat exchange area and tending to reduce heat exchange efficiency. From the perspective of pressure loss, the magnetic heat exchange material is preferably spherical particles with an aspect ratio (ratio of major axis to minor axis) of 2 or less. There are no particular restrictions on the manufacturing method, and it can be produced by gas atomization, rotating disk method, rotating electrode method, etc.
[0043] In particular, when gas atomization is used, spherical powder can be produced, which not only shortens the time required to create a single phase by making the structure finer, but also results in a structure that is suitable for efficient heat exchange when actually used, as described above.
[0044] On the other hand, a similar fine structure can be obtained by roll quenching, and a single phase can be obtained relatively easily. However, when actually using it as a heat exchange device, it is too costly to obtain a spherical sample from this type of sample, so in this case it is preferable to sinter it into a block, then process it into grooves, etc., to use it as a heat exchanger.
[0045] The introduction of hydrogen into magnetic heat exchange materials is 13 La(Fe) 1-x Si x ) 13The sample can be hydrogenated by treating it in a hydrogen atmosphere at a temperature range of 250 to 400°C and a pressure of 0.01 to 1 MPa for 1 to 10 hours.
[0046] An example of a magnetic heat exchanger using the magnetic heat exchange material of the present invention is an AMR-type magnetic heat exchanger using a liquid heat exchange medium. This device comprises a heat exchange device filled with a magnetic heat exchange material, a magnetic field generating means for applying and removing a magnetic field to the magnetic heat exchange material, a low-temperature heat exchange section, and a high-temperature heat exchange section. Furthermore, the device comprises a heat exchange circuit formed by connecting the heat exchange device, the low-temperature heat exchange section, and the high-temperature heat exchange section, and circulating the liquid heat exchange medium. At least a portion of the magnetic heat exchange material filled in the heat exchange device is the magnetic heat exchange material of the present invention. While the magnetic heat exchange material of the present invention may be loaded into a heat exchange device with only one magnetic transition temperature, loading multiple magnetic heat exchange materials with multiple magnetic transition temperatures results in a heat exchange device with high heat exchange efficiency.
[0047] FIG. 1 is a schematic cross-sectional view of a magnetic heat exchanger according to one embodiment of the present invention. This magnetic heat exchanger uses, for example, water as a liquid heat exchange medium. A low-temperature side heat exchange section 21 is provided at the low-temperature end LT of a heat exchange device 10, and a high-temperature side heat exchange section 31 is provided at the high-temperature end HT. A switching means 40 for switching the flow direction of the heat exchange medium is provided between the low-temperature side heat exchange section 21 and the high-temperature side heat exchange section 31. A heat exchange medium pump 50, which serves as a heat exchange medium transport means, is connected to the switching means 40. The heat exchange device 10, the low-temperature side heat exchange section 21, the switching means 40, and the high-temperature side heat exchange section 31 are connected by piping to form a heat exchange circuit that circulates the liquid heat exchange medium.
[0048] The heat exchange device 10 is filled with the magnetic heat exchange material 12 of the present invention, which has a magnetocaloric effect. A horizontally movable permanent magnet 14 is arranged on the outside of the heat exchange device 10 as a magnetic field generating means.
[0049] Next, the operation of the magnetic heat exchanger will be outlined using Figure 2. When a permanent magnet 14 is placed in a position facing the heat exchange device 10 (the position shown in Figure 2), a magnetic field is applied to the magnetic heat exchange material 12 in the heat exchange device 10. As a result, the magnetic heat exchange material 12, which has a magnetocaloric effect, generates heat. At this time, the heat exchange medium pump 50 and switching means 40 operate to circulate the liquid heat exchange medium from the heat exchange device 10 toward the high-temperature side heat exchange section 31. The liquid heat exchange medium, whose temperature has increased due to the heat generated by the magnetic heat exchange material 12, transports heat to the high-temperature side heat exchange section 31. The high-temperature side heat exchange section 31 has a high-temperature side heat exchanger 32 and a high-temperature side water tank 34, and transports heat to a radiator 36.
[0050] Thereafter, the permanent magnet 14 is moved from the position facing the heat exchange device 10, and the magnetic field applied to the magnetic heat exchange material 12 is removed. Removing the magnetic field causes the magnetic heat exchange material 12 to absorb heat. At this time, the heat exchange medium pump 50 and the switching means 40 are operated to circulate the liquid heat exchange medium from the heat exchange device 10 toward the low-temperature side heat exchange section 21. The liquid heat exchange medium is cooled by the heat absorption of the magnetic heat exchange material 12, and cold is transported to the low-temperature side heat exchange section 21. The low-temperature side exchange section 21 has a low-temperature side heat exchanger 22 and a low-temperature side water tank 24, and transports cold to a low-temperature consumer 26.
[0051] By repeatedly moving the permanent magnets 14 and repeatedly applying and removing a magnetic field to the magnetic heat exchange material 12 in the heat exchange device 10, a temperature gradient is generated in the magnetic heat exchange material 12 in the heat exchange device 10. Then, the liquid heat exchange medium moves in synchronization with the application and removal of the magnetic field, thereby continuously cooling the low-temperature side heat exchange section 21.
[0052] The magnetic heat exchange device can achieve high heat exchange efficiency by using a magnetic heat exchange material that has a large magnetocaloric effect at the magnetic heat exchange operating temperature.
[0053] As an example of another magnetic heat exchange device, a schematic diagram is shown in Fig. 3, and the details of the magnetic heat exchange section are shown in Fig. 4. In this diagram, 100 represents a magnetic heat exchange material, 200 represents a heat exchange device, 300 represents a heat exchange medium inlet pipe, 400 represents a heat exchange medium outlet pipe, 500a and 500b represent permanent magnets, 600a and 600b represent rotating disks, 250 represents a low-temperature consumer, and 260 represents a radiator. Water, for example, can be used as the heat exchange medium.
[0054] As shown in Fig. 4, the heat exchange device 200 has a cylindrical shape with a rectangular cross section, and the magnetic heat exchange material 100 inside is, for example, spherical with a volume average particle size of 0.3 mm, and is filled in the heat exchange device 200 at a volume filling rate of 58%. One end of the heat exchange device 200 is connected to an inlet pipe 300 for the heat exchange medium, and the other end is connected to an outlet pipe 400. In this figure, two heat exchange devices 200 of the same shape are provided and arranged parallel to each other.
[0055] A pair of rotating disks 600a, 600b are provided to sandwich the two heat exchange devices 200, and the rotating disks 600a, 600b are supported by a common shaft 700. This shaft 700 is located at the center of the two heat exchange devices 200. Permanent magnets 500a, 500b are installed on the inside near the periphery of the rotating disks 600a, 600b, respectively. The permanent magnets 500a, 500b face each other and are connected to each other via a yoke (not shown). This creates a strong magnetic field space in the gap between the paired permanent magnets 500a, 500b. In this example, two pairs of permanent magnets 500a, 500b are provided to correspond to the two heat exchange devices 200, respectively, and are arranged with the shaft 700 in between.
[0056] Every time the turntables 600a, 600b are rotated by 90 degrees, the permanent magnets 500a, 500b repeatedly approach and move away from the heat exchange device 200. When each pair of permanent magnets 500a, 500b is closest to the side wall of each heat exchange device 200, the heat exchange device 200 enters the magnetic field space formed between the permanent magnets 500a, 500b, and a magnetic field is applied to the magnetic heat exchange material 100 contained therein.
[0057] When the magnetic heat exchange material 100 switches from a state in which a magnetic field is applied to a state in which it is removed, the entropy of the electron magnetic spin system increases, and entropy transfer occurs between the lattice system and the electron magnetic spin system. This causes the temperature of the magnetic heat exchange material 100 to decrease, which is then transferred to the heat exchange medium, causing the temperature of the heat exchange medium to decrease. The heat exchange medium whose temperature has decreased in this way is discharged from the heat exchange device 200 through the discharge pipe 400 and supplied to an external low-temperature consumer (250: Figure 4) as a heat exchange medium.
[0058] In the above embodiment, the magnetic heat exchange material 12 in the heat exchange device 10 or the magnetic heat exchange material 100 in the magnetic heat exchange working chamber (heat exchange device) 200 may be filled uniformly with one type of magnetic heat exchange material of the same composition, or may be filled with magnetic heat exchange materials having two or more different compositions.
[0059] For example, the magnetic heat exchange material may be a mixture of multiple magnetic materials packed in a heat exchange device, or multiple magnetic materials may be packed in layers in a heat exchange device.
[0060] A magnetic heat exchange device using the above-mentioned magnetic heat exchange material can, for example, reduce the size of a refrigeration system, and can therefore be applied to refrigeration systems such as household refrigerator-freezers, air conditioners, industrial refrigerator-freezers, large refrigerated warehouses, and freezers for storing and transporting liquefied gas, or heating systems. [Example]
[0061] After preparing alloys with the composition ratios shown in Tables 1-1 and 1-2, they were melted in a vacuum induction melting furnace. The obtained alloys were then remelted and spherical powders were produced using the gas atomization method. All alloys had an aspect ratio of 2 or less and were produced into spherical particles with a volume average particle size in the range of 100 to 150 μm. The spherical powders produced were heat-treated at 1150°C for 12 hours to produce NaZn 13 La(Fe 1-x Si x ) 13 The phase ratio was increased while the Fe phase and LaFeSi phase were decreased. After this, hydrogen was absorbed in a hydrogen atmosphere of 0.5 MPa at 300°C for 5 hours, and then cooled to room temperature. Samples Nos. 1 to 22 are inventive examples, and samples Nos. 23 to 32 are comparative examples.
[0062] The hydrogenated sample was taken out and subjected to X-ray diffraction measurement and hydrogen content analysis. In the X-ray diffraction measurement using Cu-Kα radiation as the X-ray source, NaZn 13 La(Fe) 1-x Si x ) 13 Table 1 shows the ratio of the diffraction intensity of the (110) plane of the Fe phase to the diffraction intensity of the (422) plane of the LaFeSi phase, and the ratio of the diffraction intensity of the (101) plane of the LaFeSi phase, which has a CeFeSi type crystal structure. The hydrogen storage capacity is also expressed by the composition formula. As an example, Figure 5 shows the X-ray diffraction pattern of sample No. 3. In the figure, ● indicates La(Fe 1-x Si x ) 13 The triangles indicate the (422) plane of the LaFeSi phase, the crosses indicate the (101) plane of the LaFeSi phase, and the crosses indicate the (110) plane of the Fe phase.
[0063] Furthermore, 50 spherical powders, roughly 100 μm in diameter, obtained by hydrogen treatment were examined for the number of cracks in the spherical powder caused by hydrogen absorption. Samples with two or fewer cracks out of the 50 were marked "absent," while samples with three or more cracks were marked "present." These samples were loaded into a designated jig designed to simulate a heat exchange device, and subjected to vibration for a set period of time. After that, the degree of cracking was examined, and cracks in the spherical powder were confirmed in the same number as the number of cracks that had been introduced.
[0064] For the hydrogenated samples, the Curie temperature (Tc) was measured from the temperature characteristics of the magnetization curve, and the magnetic field dependence of the magnetization was measured at each temperature. From the magnetization values when the externally applied magnetic field was changed between 0 and 2 T, the entropy change ΔS of the electron magnetic spin system was calculated using the following formula 1.
[0065]
number
[0066] The results are shown in Tables 1-1 and 1-2 as relative values, with sample No. 23 set to 1. As is clear from this table, the entropy change ΔS of the electron magnetic spin system in all of the inventive examples was roughly equivalent to or even greater than that of No. 23, confirming their superiority in terms of practical performance of magnetic heat exchange.
[0067] [Table 1-1]
[0068] [Table 1-2]
[0069] The present invention has been described in detail above based on the embodiments of the invention, citing specific examples. However, the present invention is not limited to the above content, and any modifications or changes are possible as long as they do not deviate from the scope of the present invention. [Explanation of symbols]
[0070] 10 Heat Exchange Devices 12 Magnetic heat exchange materials 14 Permanent magnets 21 Low temperature side heat exchange section 22 Low temperature side heat exchanger 24 Low temperature water tank 26 Low temperature consumer 31 High temperature side heat exchange section 32 High temperature side heat exchanger 34 High temperature water tank 36 Heat sink 40 Switching Methods 50 Heat exchange medium pump 100 Magnetic Heat Exchange Materials 200 Heat Exchange Device 250 Low temperature consumer 260 Heatsink 300 Heat exchange medium introduction piping 400 Heat exchange medium discharge piping 500a, 500b permanent magnets 600a, 600b turntable 700 rotation axis HT High temperature field LT Low temperature field
Claims
1. In an X-ray diffraction measurement using Cu-Kα radiation as an X-ray source, the ratio of the diffraction intensity of the (110) plane of the Fe phase to the diffraction intensity of the (422) plane of the La(Fe1-xSix)13 phase having a NaZn13 type crystal structure is 7% or less, the ratio of the diffraction intensity of the (101) plane of the LaFeSi phase having a CeFeSi type crystal structure to the diffraction intensity of the (422) plane of the La(Fe1-xSix)13 phase having a NaZn13 type crystal structure is 7% or less, and the remainder is NaZn 13 A magnetic heat exchange material having a La(Fe 1-x Si x ) 13 phase and an unavoidable impurity level phase, A magnetic heat exchange material represented by the following general formula (1): La 1-a R a (Fe 1-b-c Si b T c ) e H f ・・・(1) Here, in the above formula (1), R: at least one selected from Sm and Y; T: at least one selected from V, Cr, Mn, Ni and Cu; The subscripts a, b, c, e, and f represent 0.1≦a≦0.30, 0.09≦b≦0.14, 0.01≦c≦0.04, 12.5≦e≦13.5, 1.3≦f≦2.3 Meet the conditions.
2. In an X-ray diffraction measurement using Cu-Kα radiation as an X-ray source, the ratio of the diffraction intensity of the (110) plane of the Fe phase to the diffraction intensity of the (422) plane of the La(Fe1-xSix)13 phase having a NaZn13 type crystal structure is 7% or less, the ratio of the diffraction intensity of the (101) plane of the LaFeSi phase having a CeFeSi type crystal structure to the diffraction intensity of the (422) plane of the La(Fe1-xSix)13 phase having a NaZn13 type crystal structure is 7% or less, and the remainder is NaZn 13 A magnetic heat exchange material having a La(Fe 1-x Si x ) 13 phase and an unavoidable impurity level phase, A magnetic heat exchange material represented by the following general formula (2): Lạ 1-a R a (Fe1-b-c-dSi b T c Co d ) e H f ・・・(2) Here, in the above formula (2), R: at least one selected from Sm and Y; T: at least one selected from V, Cr, Mn, Ni and Cu; The subscripts a, b, c, d, e, and f represent 0.05≦a≦0.30, 0.09≦b≦0.14, 0<c≦0.05, 0.01≦d≦0.03, 12.5≦e≦13.5, 1.3≦f≦2.3 Meet the conditions.
3. The magnetic heat exchange material according to claim 1 or 2, characterized in that the magnetic heat exchange material is a spherical particle having an aspect ratio of 2 or less.
4. The magnetic heat exchange material according to any one of claims 1 to 3, characterized in that the volume average particle size of the magnetic heat exchange material is 0.05 mm or more and 1 mm or less.
5. A heat exchange device comprising the magnetic heat exchange material according to any one of claims 1 to 4.
6. A magnetic heat exchange apparatus comprising the heat exchange device according to claim 5.
Citation Information
Patent Citations
Metal-bonded hydrogenated La(Fe,Si)13-based magnetic refrigeration sheet, preparation method thereof and application thereof
CN109524189A
Magnetic refrigeration material and producing method thereof
JP2003096547A
Method of producing rare earth-containing alloy, rare earth-containing alloy, method of producing rare earth-containing alloy powder, rare earth-containing alloy powder, method of producing rare earth-containing alloy sintered compact, rare earth-containing alloy sintered compact, magnetostriction element, and magnetic refrigeration working substance
JP2005036302A
Magnetic alloy and its manufacturing method
JP2005226124A
Magnetic grain and method for producing the same
JP2006124783A